Solid secondary battery

By using an insulating frame and high-porosity intermediate layer, the solid-state secondary battery addresses metal ion precipitation issues, improving cycle characteristics and storage performance.

JP2024146635APending Publication Date: 2024-10-15HONDA MOTOR CO LTD

Patent Information

Application Number
JP2023059659
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Solid-state secondary batteries face issues with capacity increase and cycle characteristics due to metal ion precipitation at the ends of the solid electrolyte and intermediate layers, leading to short circuits and resistance increases.

Method used

Surrounding the positive electrode active material layer and solid electrolyte layer with an insulating frame having specific volume resistivity and porosity, and incorporating an intermediate layer with higher porosity to prevent metal ion deposition at the ends, ensuring uniform metal deposition and reducing short circuits.

Benefits of technology

The solution enhances cycle characteristics and storage performance by preventing metal ion deposition at critical interfaces, maintaining structural integrity, and reducing resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146635000001_ABST
    Figure 2024146635000001_ABST
Patent Text Reader

Abstract

To provide a solid secondary battery that has an excellent cycle characteristics in which a thickness of a negative electrode layer changes greatly due to charging and discharging, and in which metal ions are less likely to precipitate at an end of a solid electrolyte layer or an intermediate layer even after repeated charging and discharging.SOLUTION: A solid secondary battery includes an electrode laminate and an exterior body that houses the electrode laminate. The electrode laminate includes a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer. The positive electrode layer includes a positive electrode current collector and a positive electrode active material layer. The outer periphery of the positive electrode active material layer and the solid electrolyte layer is surrounded by an insulating frame having a volume resistivity of 1×1012 Ω cm or more at 20°C and a porosity of 40% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solid secondary battery. [Background technology]

[0002] In recent years, research and development into secondary batteries that contribute to energy efficiency has been conducted to ensure that more people have access to affordable, reliable, sustainable, and advanced energy. Among secondary batteries, solid-state secondary batteries using solid electrolytes have attracted particular attention because of their superiority in terms of improved safety due to the non-flammability of the solid electrolyte and higher energy density.

[0003] In a solid-state secondary battery, repeated charging and discharging may cause the precipitation of metal ions such as lithium ions used as a charge transfer medium between the solid electrolyte layer and the negative electrode layer. The precipitation of the metal may cause a decrease in the adhesion of the interface, which may result in a decrease in the performance of the solid-state secondary battery. In response to this problem, a technology is known in which a layer on which lithium metal can be precipitated is provided to cover the negative electrode current collector, and the lithium metal is precipitated approximately uniformly on the surface of the coating layer, thereby making it difficult for dead lithium to be generated (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-129159 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in solid secondary batteries, the challenge is to increase the capacity and improve the cycle characteristics. In order to increase the capacity of solid secondary batteries, the use of metallic lithium as the negative electrode active material has been considered. However, in solid secondary batteries using metallic lithium as the negative electrode active material, the thickness of the negative electrode layer changes greatly due to charging and discharging. In addition, in solid secondary batteries, if the dimensions, structural design, and process conditions are inappropriate, metal ions, which are charge transfer media, may be easily precipitated at the end of the solid electrolyte layer. In particular, when an intermediate layer is provided between the solid electrolyte layer and the negative electrode current collector, metal ions may also be easily precipitated at the end of the intermediate layer. If metal ions are precipitated at the end of the solid electrolyte layer or the intermediate layer, the precipitated metal may accumulate, causing a short circuit between the positive electrode layer and the negative electrode layer, or a side reaction may occur locally, causing an increase in resistance, which may result in a decrease in cycle characteristics.

[0006] The present invention has been made in view of the above, and aims to provide a solid secondary battery that has excellent cycle characteristics, in which the thickness of the negative electrode layer changes significantly due to charging and discharging, and in which metal ions are unlikely to precipitate at the ends of the solid electrolyte layer and intermediate layer even after repeated charging and discharging, and which ultimately contributes to energy efficiency. [Means for solving the problem]

[0007] The present inventors have found that the above-mentioned problems can be solved by surrounding the outer periphery of the positive electrode active material layer and the solid electrolyte layer of the positive electrode layer with an insulating frame having a predetermined volume resistivity and porosity, and have completed the present invention. Therefore, the present invention provides the following.

[0008] (1) An electrode laminate comprising: an electrode laminate; and an exterior body that houses the electrode laminate; the electrode laminate having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer; the positive electrode layer having a positive electrode current collector and a positive electrode active material layer; and a volume resistivity at 20° C. of 1×10 12 A solid-state secondary battery surrounded by an insulating frame with a capacitance of Ω·cm or more and a porosity of 40% or less.

[0009] In the solid secondary battery of (1), the outer periphery of the positive electrode active material layer and the solid electrolyte layer is surrounded by an insulating frame having the above-mentioned volume resistivity and porosity, so that metal ions released from the positive electrode layer and the negative electrode layer are unlikely to precipitate at the end of the solid electrolyte layer during charging and discharging. Therefore, the positive electrode layer and the negative electrode layer are unlikely to short-circuit. Therefore, the solid secondary battery of (1) has excellent cycle characteristics.

[0010] (2) The solid secondary battery according to (1), wherein the insulating frame has a porosity of 20% or less.

[0011] In the solid secondary battery of (2), the porosity of the insulating frame is low at 20% or less, so that the diameter of the voids in the insulating frame is small and the structure of the insulating frame can be easily maintained, and therefore, during charging and discharging, metal ions released from the positive electrode layer and the negative electrode layer are less likely to deposit at the ends of the solid electrolyte layer, making it possible to make the positive electrode layer and the negative electrode layer less likely to short-circuit.

[0012] (3) The solid secondary battery according to (1) or (2), further comprising an intermediate layer disposed between the negative electrode layer and the solid electrolyte layer, the intermediate layer having a porosity greater than a porosity of the solid electrolyte layer.

[0013] According to the solid secondary battery of (3), even if an intermediate layer is provided, the outer periphery of the positive electrode active material layer and the solid electrolyte layer are surrounded by the insulating frame, so that the positive electrode layer and the negative electrode layer are unlikely to short-circuit. In addition, since the porosity of the intermediate layer is larger than that of the solid electrolyte layer, non-uniform metal deposition at the interface of the negative electrode layer can be suppressed, and the cycle characteristics can be further improved.

[0014] (4) The solid secondary battery according to (3), wherein the insulating frame extends to an outer periphery of the intermediate layer.

[0015] In the solid secondary battery of (4), since the insulating frame extends to the outer periphery of the intermediate layer, metal ions are less likely to precipitate at the end of the intermediate layer, making it more difficult for the positive electrode layer and the negative electrode layer to short-circuit.

[0016] (5) The solid secondary battery according to (3) or (4), wherein the intermediate layer has a thickness of 5 μm or less in the stacking direction of the electrode stack.

[0017] According to the solid-state secondary battery of (5), since the thickness of the intermediate layer is 5 μm or less, the deposition position of the metal, which is the charge transfer medium during charging, can be between the intermediate layer and the negative electrode layer. This can greatly reduce the frequency of direct contact between the electrolyte layer and the deposited metal, suppressing local deterioration of the electrolyte layer and current concentration, and improving cycle characteristics and storage characteristics. In addition, a relatively elastic intermediate layer can be arranged between the hard electrolyte layer and the deposited metal, making it easier to follow the expansion and contraction caused by the deposition and dissolution of the metal, allowing for a uniform reaction in the in-plane and thickness directions, resulting in reduced resistance and improved cycle characteristics.

[0018] (6) The solid secondary battery according to any one of (3) to (5), wherein the intermediate layer contains metal nanoparticles and amorphous carbon.

[0019] According to the solid secondary battery of (6), the electronic conductivity of the intermediate layer can be ensured, and the particles constituting the intermediate layer and the charge transfer medium can be prevented from reacting with each other to form an alloy.

[0020] (7) The solid secondary battery according to any one of (1) to (6), wherein the negative electrode active material is metallic lithium.

[0021] According to the solid secondary battery of (7), the negative electrode active material is metallic lithium, so that a high capacity can be achieved. Effect of the Invention

[0022] According to the present invention, it is possible to provide a solid secondary battery having excellent cycle characteristics in which the thickness of the negative electrode layer changes greatly due to charging and discharging, and in which metal ions are less likely to precipitate at the ends of the solid electrolyte layer or intermediate layer even after repeated charging and discharging. [Brief description of the drawings]

[0023] [Figure 1]FIG. 2 is a top view of an electrode stack of a solid secondary battery according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view taken along line II-II in FIG. [Diagram 3] 3 is a cross-sectional view showing a charged state of the electrode stack shown in FIG. 2. [Figure 4] FIG. 1 is a cross-sectional view of a solid secondary battery according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, embodiments of the present invention will be described with reference to the drawings. However, the embodiments described below are merely examples of the present invention, and the present invention is not limited to the following.

[0025] Fig. 1 is a top view of an electrode laminate of a solid secondary battery according to one embodiment of the present invention. Fig. 2 is a cross-sectional view taken along line II-II in Fig. 1, and Fig. 3 is a cross-sectional view showing the charged state of the electrode laminate shown in Fig. 2. Fig. 4 is a cross-sectional view of a solid secondary battery having the electrode laminate shown in Figs. 1 to 3. In Figs. 1 to 4, the X direction indicated by the arrow X is a direction parallel to the upper surface of the electrode laminate when viewed from above. The Y direction indicated by the arrow Y is a direction parallel to the upper surface of the electrode laminate when viewed from above and perpendicular to the X direction. The Z direction indicated by the arrow Z is the stacking direction of the electrode laminate.

[0026] The solid secondary battery 100 of this embodiment includes an electrode laminate 1, as shown in FIG. As shown in FIGS. 1 to 3, the electrode laminate 1 is a laminate in which a positive electrode layer 10, a solid electrolyte layer 20, an intermediate layer 30, and a negative electrode layer 40 are laminated in this order. The positive electrode layer 10 includes a positive electrode current collector 11 and a positive electrode active material layer 12. The outer peripheries of the positive electrode active material layer 12, the solid electrolyte layer 20, and the intermediate layer 30 are surrounded by an insulating frame 35. The negative electrode layer 40 includes a negative electrode current collector 41. Note that the electrode laminate 1 shown in FIGS. 1 and 2 is in a discharged state, and the electrode laminate 1 shown in FIG. 3 is in a charged state. The negative electrode layer 40 in the charged state has a metal deposition layer 42 formed by deposition of metal ions, which are charge negative electrode active materials, on the surface of the negative electrode current collector 41 on the intermediate layer 30 side. The metal deposition layer 42 acts as a negative electrode active material layer and releases metal ions during discharge. The thickness of the negative electrode layer 40 of the electrode laminate 1 changes during charge and discharge.

[0027] As shown in FIG. 1, the electrode laminate 1 has a rectangular shape in a top view in which the X direction is longer than the Y direction. The electrode laminate 1 may be square or circular in a top view.

[0028] The positive electrode layer 10, the solid electrolyte layer 20, the intermediate layer 30, and the negative electrode layer 40 are laminated so that their centers C overlap. When the area of the positive electrode active material layer 12 in a top view is Sp, the area of the solid electrolyte layer 20 in a top view is Ss, the area of the intermediate layer 30 in a top view is Sm, and the area of the negative electrode layer 40 in a top view is Sn, Sp = Sm = Ss < Sn. In a top view of the electrode laminate 1, the positive electrode active material layer 12, the solid electrolyte layer 20, and the intermediate layer 30 have the same shape, and the end portion of the insulating frame 35 on the negative electrode layer 40 side is outside the end portion of the positive electrode active material layer 12. The ratio Sn / Sp of the area Sn of the negative electrode layer 40 to the area Sp of the positive electrode active material layer 12 may be, for example, within the range of 1.05 to 1.45.

[0029] There are no particular limitations on the material or shape of the positive electrode current collector 11 as long as it has the function of collecting current from the positive electrode layer 10. The area of ​​the positive electrode current collector 11 in a top view is preferably equal to or larger than that of the positive electrode active material layer 12. Examples of materials for the positive electrode current collector 11 include aluminum, aluminum alloys, stainless steel, nickel, iron, and titanium, and among these, aluminum, aluminum alloys, and stainless steel are preferred. Examples of the shape of the positive electrode current collector 11 include a foil shape, a plate shape, and the like.

[0030] The positive electrode active material layer 12 contains at least one type of positive electrode active material. There are no particular limitations on the positive electrode active material, and any material that is used in the positive electrode layers of general solid-state secondary batteries can be used. As the positive electrode active material, for example, a layered active material containing lithium, a spinel type active material, an olivine type active material, etc. can be used. Specific examples of the positive electrode active material include lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), LiNi p Mn q Co r O2(p+q+r=1), LiNi p Al q Co r O2(p+q+r=1), lithium manganese oxide (LiMn2O4), Li 1+x Mn 2-x-y Examples of such materials include Li-Mn spinel substituted with different elements represented by MO4 (x+y=2, M=at least one selected from Al, Mg, Co, Fe, Ni, and Zn), lithium titanate (oxide containing Li and Ti), and lithium metal phosphate (LiMPO4, M=at least one selected from Fe, Mn, Co, and Ni).

[0031] The positive electrode active material layer 12 may optionally contain a solid electrolyte in order to improve the charge transfer medium conductivity. It may also optionally contain a conductive assistant in order to improve the conductivity. Furthermore, it may also optionally contain a binder in order to achieve flexibility. There are no particular limitations on the solid electrolyte, conductive assistant, and binder, and those used in the positive electrode layer of a general solid secondary battery may be used.

[0032] The solid electrolyte layer 20 is a layer laminated between the positive electrode layer 10 and the negative electrode layer 40. The solid electrolyte layer 20 contains at least one type of solid electrolyte material. The solid electrolyte layer 20 can conduct a charge transfer medium between the positive electrode layer 10 and the negative electrode layer 40 via the solid electrolyte material contained in the solid electrolyte layer 20.

[0033] The solid electrolyte material is not particularly limited as long as it has charge transfer medium conductivity. For example, a sulfide solid electrolyte material, an oxide solid electrolyte material, a nitride solid electrolyte material, a halide solid electrolyte material, etc. can be used.

[0034] Examples of sulfide solid electrolyte materials include Li2S-P2S5, Li2S-P2S5-LiI, etc. The above description of "Li2S-P2S5" means a sulfide solid electrolyte material made using a raw material composition containing Li2S and P2S5, and the same applies to other similar descriptions. The sulfide solid electrolyte material may have an argyrodite-type crystal structure.

[0035] Examples of oxide solid electrolyte materials include NASICON-type oxides, garnet-type oxides, perovskite-type oxides, etc. Examples of NASICON-type oxides include oxides containing Li, Al, Ti, P, and O (e.g., Li 1.5 Al 0.5 Ti 1.5 (PO4)3). Examples of garnet-type oxides include oxides containing Li, La, Zr, and O (e.g., Li7La3Zr2O 12 Examples of perovskite oxides include oxides containing Li, La, Ti, and O (for example, LiLaTiO3).

[0036] The solid electrolyte layer 20 may contain a binder. There are no particular limitations on the binder, and any binder that is used in solid electrolyte layers of general solid secondary batteries can be used.

[0037] The porosity of the solid electrolyte layer 20 is lower than that of the intermediate layer 30 described later, for example, less than 10%. The particle size of the solid electrolyte material constituting the solid electrolyte layer 20 is, for example, 0.5 to 10 μm in median size (D50), and is preferably larger than that of the particles constituting the intermediate layer 30 described later.

[0038] The porosity of the solid electrolyte layer 20 can be calculated, for example, by the following formula (1): In formula (1), the "packing ratio" refers to the percentage of the density of the solid electrolyte layer after molding relative to the true density. Porosity (%)=(100-Filling rate (%)) …(1)

[0039] The solid electrolyte layer 20 may have a moisture content of 700 mass ppm or less, or 500 mass ppm or less, after drying at 110° C. for 1 hour in a vacuum state of less than 100 Pa. By using a solid electrolyte layer 20 with a low moisture content, it is possible to suppress a decrease in the ionic conductivity of the solid electrolyte layer, and also to suppress deterioration of the positive electrode layer 10, the intermediate layer 30, and the negative electrode layer 40 due to moisture, thereby further improving the cycle characteristics of the solid secondary battery 100. The moisture content after drying was measured using the Karl Fischer method.

[0040] The intermediate layer 30 is a layer laminated between the solid electrolyte layer 20 and the negative electrode layer 40. The intermediate layer 30 has the function of suppressing non-uniform deposition of metal ions at the interface of the negative electrode layer 40 and improving the interface adhesion.

[0041] The intermediate layer 30 preferably has electron conductivity and voids through which metal ions (e.g., lithium ions) serving as a charge transfer medium can pass. When the intermediate layer 30 has voids, when the solid secondary battery 100 is charged, the metal ions moving from the solid electrolyte layer 20 toward the negative electrode layer 40 pass through the intermediate layer 30 and are precipitated on the surface of the negative electrode current collector 41 of the negative electrode layer 40 on the intermediate layer 30 side, forming a metal precipitate layer 42 (a layer of metallic lithium). By passing through the intermediate layer 30, the metal precipitate layer 42 can be uniformly formed on the surface of the negative electrode current collector 41. In addition, by having voids, the intermediate layer 30 has flexibility capable of following the change in thickness of the negative electrode layer 40 accompanying charging and discharging. Therefore, even when the solid secondary battery 100 is repeatedly charged and discharged, the interfacial adhesion can be maintained, and the durability of the solid secondary battery 100 can be improved.

[0042] The porosity of the intermediate layer 30 is preferably higher than that of the solid electrolyte layer 20. This allows many voids through which metal ions can pass to be formed inside the intermediate layer 30, so that the metal deposit layer 42 can be more uniformly formed on the surface of the negative electrode current collector 41. In addition, the intermediate layer 30 becomes more flexible, so that the ability to follow changes in the thickness of the negative electrode layer 40 is improved. The porosity of the intermediate layer 30 can be, for example, 40 to 70%. The porosity of the intermediate layer 30 can be calculated in the same manner as the porosity of the solid electrolyte layer 20.

[0043] The thickness of the intermediate layer 30 may be 5 μm or less. By making the thickness of the intermediate layer 30 5 μm or less, the deposition position of the metal, which is the charge transfer medium during charging, can be between the intermediate layer 30 and the negative electrode layer 40. This can greatly reduce the frequency of direct contact between the solid electrolyte layer 20 and the deposited metal, suppressing local deterioration and current concentration of the solid electrolyte layer 20, and improving cycle characteristics and storage characteristics. In addition, the relatively elastic intermediate layer 30 can be disposed between the hard solid electrolyte layer 20 and the deposited metal, making it easier to follow the expansion and contraction caused by the deposition and dissolution of the metal, allowing a uniform reaction in the in-plane and thickness directions, thereby obtaining the effects of reducing resistance and improving cycle characteristics. In order to obtain the effects of further reducing resistance and improving cycle characteristics, the thickness of the intermediate layer may be 3 μm or less, or may be within the range of 1 to 3 μm.

[0044] The intermediate layer 30 preferably contains amorphous carbon and metal nanoparticles. The intermediate layer 30 may further contain a binder as a binding material to maintain the structure.

[0045] Unlike graphite, amorphous carbon is less likely to react with metals such as lithium and form an alloy, and therefore can suppress the formation of dendrites and improve the cycle characteristics of solid secondary batteries. The amorphous carbon may be either easily graphitized carbon (soft carbon) or difficultly graphitized carbon (hard carbon). In addition, the amorphous carbon may be any carbon allotrope that does not show a clear crystalline state, and may be an aggregate of fine graphite crystals. Specific examples of amorphous carbon include carbon blacks such as acetylene black, furnace black, and ketjen black, coke, activated carbon, CNT (carbon nanotube), fullerene, and graphene.

[0046] Examples of metal nanoparticles include metal nanoparticles of tin (Sn), silicon (Si), zinc (Zn), magnesium (Mg), gold (Au), platinum (Pt), palladium (Pd), silver (Ag), aluminum (Al), bismuth (Bi), and antimony (Sb). The content of the metal nanoparticles in the intermediate layer 30 is preferably more than 0 mass% and 30 mass% or less. When the intermediate layer 30 contains metal nanoparticles, the electronic conductivity of the intermediate layer 30 can be increased, and the metal precipitate layer 42 can be generated more uniformly. In addition, since the metal nanoparticles have a high Young's modulus compared to amorphous carbon, the structure of the intermediate layer 30 can be maintained even when high-pressure pressing is performed when manufacturing the solid secondary battery 100.

[0047] The particle diameter of the amorphous carbon and metal nanoparticles is preferably smaller than that of the solid electrolyte material. This allows the intermediate layer 30 to enter the gap between the solid electrolyte materials constituting the interface of the solid electrolyte layer 20, thereby increasing the contact area between the solid electrolyte layer 20 and the intermediate layer 30 and improving the adhesion. The particle diameter of the amorphous carbon may be, for example, in the range of 0.02 to 0.10 μm in terms of median diameter (D50). The particle diameter of the metal nanoparticles may be, for example, in the range of 0.02 to 0.20 μm in terms of median diameter (D50).

[0048] The binder is preferably one that can improve the adhesion between the particles constituting the intermediate layer 30 and between the intermediate layer 30 and the solid electrolyte layer 20. There are no particular limitations on the binder, and it is possible to use binders that are generally used in solid secondary batteries. Examples of binders include acrylic acid-based polymers, cellulose-based polymers, styrene-based polymers, vinyl acetate-based polymers, urethane-based polymers, fluoroethylene-based polymers, and PVDF-based polymers.

[0049] The insulating frame 35 has a volume resistivity of 1×10 at 20°C. 12 The volume resistivity is 1×10 12 ~1×10 17 It may be in the range of Ω cm, 1×10 14 ~1×1017 The insulating frame 35 has a porosity of 40% or less. The porosity may be 20% or less, or may be in the range of 1 to 20%. If the porosity is too high, it may be difficult for the insulating frame 35 to maintain its structure when high pressure is applied in the battery production process, and there may be an increased risk of the deposited metal physically penetrating into the insulating frame 35 during charging and discharging, causing a short circuit.

[0050] The insulating frame 35 may be an organic material or an inorganic material. Examples of insulating materials contained in the insulating frame 35 include rubber, glass, resin (polyimide, polybenzimidazole, polyamideimide, polyetherimide, polyacetal, polyphenylene sulfide, polyetheretherketone, tetrafluoroethylene, 6-polyamide (6-nylon), ultra-high molecular weight polyethylene, polyethylene, polypropylene, polyvinyl chloride resin, polystyrene, polyethylene terephthalate, ABS resin, etc.), and ceramics (alumina, zirconia, silicon nitride, aluminum nitride, mullite, steatite, magnesia, sialon, macerite, etc.). The insulating material may be a single type, or may be a composite material combining two or more types of materials. The insulating frame 35 may also contain a small amount of a binder or additive. The insulation breakdown voltage per unit thickness of the insulating frame 35 is preferably 10 kV / mm or more, and more preferably 100 kV / mm or more.

[0051] The negative electrode current collector 41 is a laminate having a current collecting substrate 41a and a metal layer 41b laminated on the surface of the current collecting substrate 41a. There are no particular limitations on the material or shape of the current collecting substrate 41a as long as it has the function of collecting current from the negative electrode layer 40. Examples of materials for the current collecting substrate 41a include nickel, copper, and stainless steel. Examples of the shape of the current collecting substrate 41a include a foil shape, a plate shape, and the like.

[0052] The metal layer 41b is not particularly limited in material or shape as long as it has a function of densely precipitating a charge transfer medium such as lithium ions. When the charge transfer medium is lithium ions, the material of the metal layer 41b can be metallic lithium or a metal that forms an alloy with lithium. Examples of metals that form an alloy with lithium include Mg, Si, Au, Ag, In, Ge, Sn, Pb, Al, and Zn. The metal that forms the metal layer 41b may be in the form of a powder or a thin film. By using the negative electrode current collector 41 having this metal layer 41b, a uniform metal deposition layer 42 can be formed on the surface of the negative electrode current collector 41. The metal layer 41b may be omitted and lithium ions may be directly deposited on the current collector substrate 41a.

[0053] 4, the electrode laminate 1 is housed in an exterior body 50. A pair of restraining members 60 for applying a restraining force to the electrode laminate 1 are disposed on the outer surface of the exterior body 50. The solid secondary battery 100 has a positive electrode tab (not shown) having one end connected to the positive electrode current collector 11 and the other end protruding outward, and a negative electrode tab (not shown) having one end connected to the negative electrode current collector 41 and the other end protruding outward.

[0054] The exterior body 50 is expandable and contractable in accordance with the change in thickness of the negative electrode due to charging and discharging. A laminate film can be used as the material of the exterior body 50. As the laminate film, a laminate film having a three-layer structure in which an inner resin layer, a metal layer, and an outer resin layer are laminated in this order from the inside can be used. The outer resin layer may be, for example, a polyamide (nylon) layer or a polyethylene terephthalate (PET) layer, the metal layer may be, for example, an aluminum layer, and the inner resin layer may be, for example, a polyethylene layer or a polypropylene layer. In addition, an adhesive layer may be included between each layer, and the layers may be integrated by heat, pressure, or the like.

[0055] In order to ensure clearance inside the exterior body 50, the ratio of the thickness of the positive electrode layer 10 to the thickness of the negative electrode layer 40 (the thickness of the negative electrode current collector 41) in a discharged state (thickness of the positive electrode layer 10 / thickness of the negative electrode layer 40) may be 1.9 or more.

[0056] The restraining member 60 is intended to apply a restraining force in the stacking direction of the electrode laminate 1. When the area of ​​the restraining member 60 in a top view is Sr and the area of ​​the negative electrode layer 40 in a top view is Sn, it is preferable that the relationship Sn≦Sr is satisfied. When the area Sr of the restraining member 60 satisfies this relationship, the restraining force acts uniformly on the surface of the negative electrode layer 40. Therefore, during charging, metal ions can be uniformly precipitated on the surface of the negative electrode layer 40, so that metal is less likely to accumulate at the ends of the solid electrolyte layer 20 and the intermediate layer 30. There is no particular restriction on the material of the restraining member 60, and a material generally used for solid-state batteries can be used. The restraining force of the restraining member 60 on the electrode laminate 1 may be within a range of, for example, 0.1 to 10 MPa. Next, a method for manufacturing the solid secondary battery 100 of this embodiment will be described. The electrode laminate 1 can be produced, for example, by a method including a positive electrode active material layer forming step, an insulating frame arranging step, a solid electrolyte layer forming step, an intermediate layer forming step, and a negative electrode layer forming step.

[0057] The positive electrode active material layer forming step is a step of forming a positive electrode active material layer 12 on the surface of a positive electrode current collector 11. A method of applying a positive electrode active material layer slurry and drying it can be used as a method of forming the positive electrode active material layer 12. As the positive electrode active material layer slurry, a dispersion of a positive electrode active material containing a solvent, a positive electrode active material, and optionally a conductive assistant and a binder can be used.

[0058] The insulating frame arrangement step is a step of arranging an insulating frame 35 on the outer periphery of the positive electrode active material layer 12. As a method for arranging the insulating frame 35, for example, a method can be used in which an insulating frame slurry is applied to the outer periphery of the positive electrode active material layer 12 and dried to form an insulating frame. As the insulating frame slurry, for example, a dispersion liquid of an insulating material containing a solvent, an insulating material, and an optionally included binder can be used.

[0059] The solid electrolyte layer forming step is a step of forming a solid electrolyte layer 20 on the surface of the positive electrode active material layer 12 of the positive electrode layer 10. As a method for forming the solid electrolyte layer 20, a method of directly applying the solid electrolyte layer slurry to the surface of the positive electrode active material layer 12 and drying it, or a method of applying the solid electrolyte layer slurry to the surface of a separately prepared support sheet and drying it to form a solid electrolyte layer 20, and transferring the solid electrolyte layer 20 to the surface of the positive electrode active material layer 12 at a predetermined pressure can be used. As the solid electrolyte layer slurry, for example, a dispersion liquid of a solid electrolyte containing a solvent, a solid electrolyte, and an optional binder can be used. As a method for forming the solid electrolyte layer 20, a method of integrating the solid electrolyte layer with a substrate, making it independent, and then arranging it on the positive electrode layer can be used. As the substrate, for example, a nonwoven fabric or a woven fabric can be used. As the material of the substrate, a polyester resin such as PET can be used.

[0060] The intermediate layer forming step is a step of forming an intermediate layer 30 on the surface of the solid electrolyte layer 20 opposite to the positive electrode active material layer 12 side. The intermediate layer 30 can be formed by directly applying an intermediate layer slurry to the surface of the solid electrolyte layer 20 and drying it, or by applying the intermediate layer slurry to the surface of a separately prepared support sheet, drying it, and transferring the intermediate layer 30 to the surface of the solid electrolyte layer 20 at a predetermined pressure. As the intermediate layer slurry, for example, a dispersion of an intermediate layer forming material containing a solvent, metal nanoparticles, amorphous carbon, and an optional binder can be used.

[0061] The negative electrode layer forming step is a step of forming the negative electrode layer 40 on the surface of the intermediate layer 30 opposite to the solid electrolyte layer 20 side. As a method for forming the negative electrode layer 40, a method in which a previously prepared negative electrode current collector 41 is disposed on the surface of the intermediate layer 30 can be used.

[0062] The intermediate layer forming step and the negative electrode layer forming step may be performed simultaneously. For example, the intermediate layer 30 of an intermediate layer-negative electrode layer laminate in which the intermediate layer 30 and the negative electrode layer 40 are integrated and made independent in advance may be disposed on the surface of the solid electrolyte layer 20. The intermediate layer-negative electrode layer laminate can be obtained, for example, by applying an intermediate layer slurry to the surface of the negative electrode current collector 41 and drying it to form the intermediate layer 30.

[0063] In this manner, an electrode laminate 1 is obtained in which the positive electrode layer 10, the solid electrolyte layer 20, the intermediate layer 30, and the negative electrode layer 40 are laminated in this order. The obtained electrode laminate 1 may be optionally pressed to be integrated.

[0064] The solid secondary battery 100 can be fabricated as follows. One end of the positive electrode tab is connected to the positive electrode current collector 11 of the obtained electrode laminate 1, and one end of the negative electrode tab is connected to the negative electrode current collector 41. Next, the electrode laminate 1 is housed in an exterior body 50 so that the other ends of the positive electrode tab and the negative electrode tab protrude, and the exterior body 50 is sealed. Then, a restraining member 60 is disposed on the outer surface of the exterior body 50, and the electrode laminate 1 is restrained with a predetermined restraining force.

[0065] According to the solid secondary battery 100 of the present embodiment configured as described above, the outer periphery of the positive electrode active material layer 12, the solid electrolyte layer 20, and the intermediate layer 30 are surrounded by the insulating frame 35 having the above-mentioned volume resistivity and porosity, so that metal ions released from the positive electrode layer 10 and the negative electrode layer 40 are unlikely to precipitate at the ends of the solid electrolyte layer 20 and the intermediate layer 30 during charging and discharging. Therefore, the positive electrode layer 10 and the negative electrode layer 40 are unlikely to short-circuit. Therefore, the solid secondary battery 100 of the present embodiment has excellent cycle characteristics.

[0066] In addition, according to the solid secondary battery 100 of this embodiment, when the porosity of the insulating frame is low, 20% or less, the pore diameter in the insulating frame 35 is small and the structure of the insulating frame 35 is easily maintained, so that metal ions released from the positive electrode layer 10 and the negative electrode layer 40 are more unlikely to precipitate at the ends of the solid electrolyte layer 20 and the intermediate layer 30 during charging and discharging. Therefore, the positive electrode layer 10 and the negative electrode layer 40 are more unlikely to short-circuit. In addition, in the solid secondary battery 100 of this embodiment, when the porosity of the intermediate layer 30 is larger than the porosity of the solid electrolyte layer 20, non-uniform metal precipitation at the interface of the negative electrode layer 40 can be suppressed, and the cycle characteristics can be further improved. In addition, in the solid secondary battery 100 of this embodiment, when the intermediate layer 30 contains metal nanoparticles and amorphous carbon, the electronic conductivity of the intermediate layer 30 can be ensured, and the particles constituting the intermediate layer 30 and the charge transfer medium can be prevented from reacting with each other to form an alloy. Furthermore, in the solid secondary battery 100 of this embodiment, when the negative electrode active material is metallic lithium, a high capacity can be achieved.

[0067] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment. For example, in the solid secondary battery 100 of the present embodiment, the metal precipitate layer 42 is used as the negative electrode active material layer, but the negative electrode active material layer is not limited thereto. The negative electrode active material layer may be a layer containing a negative electrode active material capable of absorbing and releasing a charge transfer medium such as lithium ions. In this case, the negative electrode active material layer may be disposed on the surface of the current collecting substrate 41a. As the negative electrode active material, a material used in the negative electrode of a general solid secondary battery can be used. When the charge transfer medium is lithium ions, examples of the negative electrode active material include lithium transition metal oxides such as lithium titanate, transition metal oxides such as TiO2, Nb2O3, and WO3, Si, SiO, metal sulfides, metal nitrides, and carbon materials such as artificial graphite, natural graphite, graphite, soft carbon, and hard carbon. The negative electrode active material layer may optionally contain a solid electrolyte from the viewpoint of improving the conductivity of the charge transfer medium. In addition, it may optionally contain a conductive assistant to improve the conductivity. Furthermore, it may optionally contain a binder from the viewpoint of expressing flexibility, etc. As for the solid electrolyte, the conductive assistant, and the binder, those generally used in solid-state batteries can be used.

[0068] Furthermore, the solid secondary battery 100 of this embodiment has the intermediate layer 30, and the insulating frame 35 extends to the outer periphery of the intermediate layer 30, but the present invention is not limited to this. In the solid secondary battery 100 of this embodiment, metal ions are unlikely to precipitate at the end of the solid electrolyte layer 20, so that even if the insulating frame 35 is not extended to the outer periphery of the intermediate layer 30, the positive electrode layer 10 and the negative electrode layer 40 are unlikely to short-circuit.

[0069] The present invention will be described in detail below using examples, but the present invention is not limited to these examples.

[0070] <Example 1> [Preparation of positive electrode active material layer] As a positive electrode current collector, a rectangular aluminum foil having a length of 30.0 mm in the X direction, a length of 30.0 mm in the Y direction, and a thickness of 15.0 μm was prepared. A mixture of 80 parts by mass of lithium nickel cobalt manganese composite oxide (NCM622) as the positive electrode active material, 17 parts by mass of an argyrodite-type sulfide solid electrolyte as the solid electrolyte, 2 parts by mass of carbon black as a conductive assistant, and 1 part by mass of an SBR (styrene butadiene rubber) binder as the binding material was used. The mixture was dispersed in 43 parts by mass of butyl butyrate to prepare a positive electrode active material layer slurry. The obtained positive electrode active material layer slurry was applied to the center of the positive electrode current collector in a size of 20.0 mm in the X direction, 20.0 mm in the Y direction, and 27 mg / cm2 in weight per unit area after drying. 2 The mixture was applied using a bar coater so as to obtain a positive electrode active material layer having a thickness of 80.0 μm, and then dried.

[0071] [Making an insulating frame] Alumina (Al2O3) particles (median diameter: 0.4 μm) as an insulating material and 10 parts by mass of SBR-based binder as a binding material were mixed in a ratio of 90 parts by mass. The obtained mixture was dispersed in 120 parts by mass of butyl butyrate to prepare an insulating frame slurry. The obtained insulating frame slurry was applied to the part of the positive electrode current collector where the positive electrode active material layer was not formed, so that the basis weight after drying was 20 mg / cm. 2 The coating was applied using a spray coater so that the coating became as shown in FIG.

[0072] [Preparation of solid electrolyte layer] A dispersion of an argyrodite-type sulfide solid electrolyte (median diameter: 3.0 μm) was applied to a support sheet and dried to form an argyrodite-type sulfide solid electrolyte layer having a length of 27.0 mm in the X direction and a length of 27.0 mm in the Y direction. The argyrodite-type sulfide layer formed on the support sheet was transferred to the center of the positive electrode active material layer to produce a solid electrolyte layer.

[0073] [Creation of intermediate layer] A total of 95 parts by mass of Sn particles (median diameter: 0.07 μm) as metal nanoparticles, acetylene black (median diameter: 0.05 μm) as amorphous carbon, and 5 parts by mass of a PVDF-based binder as a binding material were mixed. The resulting mixture was dispersed in 1000 parts by mass of NMP (N-methyl-2-pyrrolidone) to prepare an intermediate layer slurry. The obtained intermediate layer slurry was applied to the base foil with a basis weight of 0.4 mg / cm. 2 The layer was coated and dried using a gravure coater so that the thickness of the layer was 22.0 mm. The layer was then placed at the center of the solid electrolyte layer and transferred under a predetermined pressure to produce an intermediate layer having a length of 22.0 mm in the X direction, a length of 22.0 mm in the Y direction, and a thickness of 3.0 μm after pressing. In this manner, a positive electrode layer, a solid electrolyte layer, and an intermediate layer were laminated in this order, and an insulating frame-attached positive electrode layer-solid electrolyte layer-intermediate layer laminate was obtained in which the outer periphery of the layer was surrounded by an insulating frame.

[0074] [Preparation of negative electrode current collector] A laminated metal foil (total thickness: 50 μm) was prepared by laminating a copper foil having a thickness of 10 μm and a lithium foil having a thickness of 40 μm. This laminated metal foil was cut into a size of 21.0 mm in the Y direction × 21.0 mm in the Y direction to prepare a negative electrode current collector.

[0075] [Preparation of electrode laminate] The insulating frame-equipped positive electrode layer-solid electrolyte layer-intermediate layer laminate obtained above was isostatically pressed at a heating temperature of 120°C and a pressure of 980 MPa for 5 minutes to densify each layer. Next, the insulating frame-equipped positive electrode layer-solid electrolyte layer-intermediate layer laminate obtained above was placed so that the lithium foil was in contact with the surface of the intermediate layer of the insulating frame-equipped positive electrode layer-solid electrolyte layer-intermediate layer laminate, and then pressed to produce an electrode laminate in which the positive electrode layer, solid electrolyte layer, intermediate layer, and negative electrode current collector were laminated in this order.

[0076] [Preparation of solid-state secondary batteries] After tabs were attached to the positive and negative current collectors of the electrode laminate obtained above, the electrode laminate was housed in a bag-shaped laminate pack, and the laminate pack was then sealed in an argon atmosphere.

[0077] A restraining member having a length of 21.0 mm in the X direction and a length of 21.0 mm in the Y direction was prepared. This restraining member was placed so as to face the negative electrode current collector of the electrode laminate from the surface of the laminate pack, and a restraining force of 3 MPa was applied to the electrode laminate to produce a solid secondary battery.

[0078] <Examples 2 to 4, Comparative Examples 1 to 2> A solid secondary battery was produced in the same manner as in Example 1, except that the heating temperature and pressing pressure during the densification treatment of the electrode laminate were set to the temperatures and pressures shown in Table 1 below.

[0079] <Physical properties of insulating frame> An insulating frame was taken out from the electrode laminate produced in Examples 1 to 3 and Comparative Examples 1 and 2. The volume resistivity (20°C) and true density of the obtained insulating frame were measured. In addition, the apparent density and true density of the insulating frame were measured, and the porosity (=apparent density / true density×100) was calculated from the obtained true density and apparent density. The apparent density was calculated from the weight and size of the insulating frame.

[0080] <Battery characteristics> For the solid secondary batteries prepared in Examples 1 to 3 and Comparative Examples 1 to 3, cycle tests were conducted in which charging and discharging were repeated at a charging upper limit voltage of 4.3V, a discharging lower limit voltage of 2.65V, and a C rate of 1 / 3C. The ratio of the first discharge capacity to the first charge capacity (first discharge capacity / first charge capacity×100) was taken as the initial charge / discharge efficiency. In addition, when the ratio of the first discharge capacity to the second charge capacity (second charge capacity / first discharge capacity×100) exceeded 105%, the short circuit behavior during the second charge was considered to be "present", and when the ratio of the first discharge capacity to the second charge capacity was 105% or less, the short circuit behavior during the second charge was considered to be "absent". The results are shown in Table 1.

[0081] [Table 1]

[0082] From the results shown in Table 1, it was confirmed that the solid secondary batteries obtained in Examples 1 to 3 having an insulating frame according to the present invention had high initial charge / discharge efficiency and were less likely to short circuit. In contrast, it was confirmed that the solid secondary battery obtained in Comparative Example 1, in which the porosity of the insulating frame was larger than the range of the present invention, and the solid secondary batteries in Comparative Examples 1 and 2, in which the porosity of the insulating frame was larger than the range of the present invention and the volume resistivity was smaller than the range of the present invention, had low initial charge / discharge efficiency and were more likely to short circuit. This was because lithium was precipitated in the voids in the insulating frame during charging. [Explanation of symbols]

[0083] 1 Electrode laminate 10 Positive electrode layer 11 Positive electrode current collector 12 Cathode active material layer 20 Solid electrolyte layer 30 Middle Class 35 Insulation frame 40 Negative electrode layer 41 Negative electrode current collector 41a Current collector substrate 41b Metal layer 42 Metal deposit layer 50 Exterior body 60 Restraint member 100 Solid state secondary battery

Claims

1. The electrode stack includes an electrode laminate and an exterior body that houses the electrode laminate. the electrode stack includes a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer; The positive electrode layer includes a positive electrode current collector and a positive electrode active material layer, The outer periphery of the positive electrode active material layer and the solid electrolyte layer has a volume resistivity of 1×10 at 20° C. 12 A solid-state secondary battery surrounded by an insulating frame having a resistance of Ω·cm or more and a porosity of 40% or less.

2. The solid secondary battery according to claim 1 , wherein the insulating frame has a porosity of 20% or less.

3. an intermediate layer disposed between the negative electrode layer and the solid electrolyte layer; The solid secondary battery according to claim 1 , wherein the porosity of the intermediate layer is greater than the porosity of the solid electrolyte layer.

4. The solid secondary battery according to claim 3 , wherein the insulating frame extends to an outer periphery of the intermediate layer.

5. The solid secondary battery according to claim 3 , wherein the intermediate layer has a thickness of 5 μm or less in the stacking direction of the electrode stack.

6. The solid state secondary battery according to claim 3 , wherein the intermediate layer comprises metal nanoparticles and amorphous carbon.

7. The solid secondary battery according to claim 1 , wherein the negative electrode active material is metallic lithium.

Citation Information

Patent Citations

  • All-solid battery and its manufacturing method

    JP2009193728A

  • All-solid power storage device and method for manufacturing the same

    JP2017117672A

  • All-solid-state secondary battery and method of manufacturing the same

    JP2019139892A

  • Battery

    JP2019207873A

  • Solid-state battery manufacturing method and solid state battery

    WO2010131321A1

Cited By

  • All-solid-state battery

    WO2026182013A1

  • Electrode laminate, and production method of electrode laminate

    WO2026197246A1

  • Method for manufacturing solid-state battery

    WO2026210688A1