Method for manufacturing solid-state secondary battery
The method of press-bonding the negative and intermediate layers at lower pressures and the solid electrolyte and positive electrode layers at higher pressures in solid-state secondary batteries addresses defects in the electrolyte layer, enhancing adhesion and cycle characteristics, thus improving battery performance.
Patent Information
- Application Number
- JP2023059660
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Solid-state secondary batteries with a stacked structure face issues of defects such as cracks and short circuits in the solid electrolyte layer due to non-uniform stress when an intermediate layer is provided, which affects cycle characteristics.
A method for manufacturing solid-state secondary batteries involves press-bonding the negative electrode and intermediate layers at a lower pressure, followed by press-bonding the solid electrolyte and positive electrode layers at higher pressures, with specific pressure ranges and directions to minimize stress on the electrolyte layer.
This method reduces defects in the solid electrolyte layer, enhances adhesion, and improves cycle characteristics by maintaining the integrity of the electrolyte layer, resulting in reduced internal resistance and improved battery performance.
Smart Images

Figure 2024146636000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a solid secondary battery. [Background technology]
[0002] In recent years, research and development into secondary batteries that contribute to energy efficiency has been conducted to ensure that more people have access to affordable, reliable, sustainable, and advanced energy. Among secondary batteries, solid-state secondary batteries using solid electrolytes have attracted particular attention because of their superiority in terms of improved safety due to the non-flammability of the solid electrolyte and higher energy density.
[0003] In order to improve the energy density of solid-state secondary batteries, a solid-state secondary battery having a laminated structure in which multiple positive electrode layers and negative electrode layers are alternately stacked has been studied. This type of laminated solid-state secondary battery is generally manufactured by press-bonding a positive electrode layer, a solid electrolyte layer, and a negative electrode layer (Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6790919 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in solid secondary batteries, the improvement of cycle characteristics is an issue. In order to improve the cycle characteristics of solid secondary batteries, the provision of an intermediate layer between the anode layer and the solid electrolyte layer or between the cathode layer and the solid electrolyte layer has been considered. However, the provision of the intermediate layer may cause uneven stress on the solid electrolyte layer during press bonding, which may cause defects such as cracks and fissures in the solid electrolyte layer, resulting in a short circuit inside the battery. According to the study by the present inventors, in particular, when an intermediate layer having a smaller Young's modulus than the solid electrolyte layer is provided between the anode layer and the solid electrolyte layer, defects tend to occur in the solid electrolyte layer during press bonding.
[0006] The present invention has been made in view of the above, and aims to provide a method for manufacturing a solid secondary battery in which defects are unlikely to occur in the solid electrolyte layer even when an intermediate layer is provided between the negative electrode layer and the solid electrolyte layer, thereby contributing to energy efficiency. [Means for solving the problem]
[0007] The present inventors have found that the above-mentioned problems can be solved by, in the manufacture of a solid secondary battery, first press-bonding the anode layer and the intermediate layer to obtain an intermediate layer-anode layer laminate, then press-bonding the intermediate layer and the solid electrolyte layer of the intermediate layer-anode layer laminate at a bonding pressure lower than the bonding pressure of the anode layer and the intermediate layer, and then press-bonding the solid electrolyte layer and the cathode layer at a bonding pressure higher than the bonding pressure of the anode layer and the intermediate layer, or press-bonding the intermediate layer, the solid electrolyte layer and the cathode layer of the intermediate layer-anode layer laminate at a bonding pressure higher than the bonding pressure of the anode layer and the intermediate layer, and have thus completed the present invention. Therefore, the present invention provides the following method for manufacturing a solid secondary battery.
[0008] (1) A method for manufacturing a solid secondary battery including an electrode laminate in which an anode layer, an intermediate layer, a solid electrolyte layer, and a cathode layer are laminated in this order, the method comprising: a 1A step of press-bonding the anode layer and the intermediate layer to obtain an intermediate layer-anode layer laminate; a 1B step of press-bonding the intermediate layer and the solid electrolyte layer of the intermediate layer-anode layer laminate to obtain a solid electrolyte layer-intermediate layer-anode layer laminate; and a 1C step of press-bonding the solid electrolyte layer and the positive electrode layer of the solid electrolyte layer-intermediate layer-anode layer laminate to obtain the electrode laminate, wherein the bonding pressure in the 1B step is lower than the bonding pressure in the press bonding in the 1A step, and the bonding pressure in the 1C step is higher than the bonding pressure in the press bonding in the 1A step.
[0009] In the manufacturing method of the solid secondary battery of (1), in step 1A, the negative electrode layer and the intermediate layer are press-bonded to obtain an intermediate layer-negative electrode layer laminate, in step 1B, the intermediate layer and the solid electrolyte layer of the intermediate layer-negative electrode layer laminate are press-bonded to obtain a solid electrolyte layer-intermediate layer-negative electrode layer laminate, and in step 1C, the solid electrolyte layer and the positive electrode layer of the solid electrolyte layer-intermediate layer-negative electrode layer laminate are press-bonded to obtain an electrode laminate. Since the bonding pressure in step 1B is lower than the bonding pressure in the press bonding in step 1A, defects such as cracks and fissures are unlikely to occur in the solid electrolyte layer in step 1B. Furthermore, since the solid electrolyte layer is supported by the intermediate layer and the negative electrode layer in step 1C, defects are unlikely to occur in the solid electrolyte layer even if the bonding pressure in the press bonding in step 1C is higher than the bonding pressure in the press bonding in step 1A. Therefore, according to the manufacturing method of the solid secondary battery of (1), defects are unlikely to occur in the solid electrolyte layer even if an intermediate layer is provided between the negative electrode layer and the solid electrolyte layer.
[0010] (2) The method for producing the solid secondary battery according to (1), further comprising, after the step 1C, a step 1D of applying a pressure higher than the joining pressure in the press joining in the step 1C in a stacking direction of the electrode stack.
[0011] According to the method for manufacturing a solid secondary battery in (2), in step 1D, a pressure higher than the bonding pressure in the press bonding in step 1C is applied in the stacking direction of the electrode laminate, so that the electrode laminate is densified and the adhesion between the layers of the electrode laminate is increased. As a result, the internal resistance of the obtained solid secondary battery is reduced, and characteristics such as cycle characteristics are improved.
[0012] (3) The method for producing a solid secondary battery according to (1) or (2), wherein the Young's modulus of the anode layer, the intermediate layer, the solid electrolyte layer, and the cathode layer is the highest for the cathode layer, the second highest for the solid electrolyte layer, the second highest for the anode layer, and the lowest for the intermediate layer.
[0013] According to the method for producing a solid secondary battery of (3), even if the Young's modulus of the intermediate layer is lower than those of each of the positive electrode layer, the solid electrolyte layer, and the negative electrode layer, defects are unlikely to occur in the solid electrolyte layer.
[0014] (4) The method for producing a solid secondary battery according to any one of (1) to (3), wherein the joining pressure in the press bonding in the step 1A is within a range of 300 to 500 MPa, the joining pressure in the press bonding in the step 1B is within a range of 50 to 100 MPa, and the joining pressure in the step 1C is 800 MPa or less.
[0015] According to the method for producing a solid secondary battery in (4), the bonding pressure in steps 1A, 1B and 1C is within the above range, so that defects in the solid electrolyte layer are less likely to occur.
[0016] (5) The method for producing a solid secondary battery according to any one of (1) to (4), wherein the intermediate layer has a porosity greater than a porosity of the solid electrolyte layer.
[0017] According to the method for producing a solid secondary battery in (5), the porosity of the intermediate layer is larger than the porosity of the solid electrolyte layer, so that non-uniform metal deposition at the negative electrode layer interface can be suppressed, and the cycle characteristics of the obtained solid secondary battery are improved.
[0018] (6) The method for producing a solid secondary battery according to (2), wherein in the first step C and the first step D, a roll press device is used for press bonding, and a conveying direction of the solid electrolyte layer-intermediate layer-negative electrode layer stack conveyed to the roll press device in the first step C is different from a conveying direction of the electrode stack conveyed to the roll press device in the first step D.
[0019] According to the method for producing a solid secondary battery of (6), the transport direction of the solid electrolyte layer-intermediate layer-negative electrode layer laminate in step 1C is different from the transport direction of the electrode laminate in step 1D. Therefore, compared with the case where steps 1C and 1D are performed by roll-to-roll, layers with a low Young's modulus, such as the negative electrode layer and the intermediate layer, are extended in one direction, which pulls the solid electrolyte layer, making it less likely that defects will occur in the solid electrolyte layer.
[0020] (7) A method for manufacturing a solid secondary battery including an electrode laminate in which an anode layer, an intermediate layer, a solid electrolyte layer, and a cathode layer are laminated in this order, the method comprising: a 2A step of press-bonding the anode layer and the intermediate layer to obtain an intermediate layer-anode layer laminate; and a 2B step of arranging a solid electrolyte layer and a cathode layer in this order on the intermediate layer of the intermediate layer-anode layer laminate and press-bonding them to obtain the electrode laminate, wherein the bonding pressure in the 2B step is higher than the bonding pressure in the press bonding in the 2A step.
[0021] In the manufacturing method of a solid secondary battery of (7), in step 2A, the negative electrode layer and the intermediate layer are press-bonded to obtain an intermediate layer-negative electrode layer laminate, and in step 2B, the solid electrolyte layer and the positive electrode layer are arranged in this order on the intermediate layer of the intermediate layer-negative electrode layer laminate and press-bonded to obtain an electrode laminate. In step 2B, the solid electrolyte layer is supported in a sandwiched state between the positive electrode layer and the intermediate layer-negative electrode layer laminate, so that even if the bonding pressure in the press bonding in step 2B is higher than the bonding pressure in the press bonding in step 2A, defects are unlikely to occur in the solid electrolyte layer. Therefore, according to the manufacturing method of a solid secondary battery of (7), even if an intermediate layer is provided between the negative electrode layer and the solid electrolyte layer, defects are unlikely to occur in the solid electrolyte layer.
[0022] (8) The method for producing a solid secondary battery according to (7), wherein the intermediate layer has a porous substrate therein.
[0023] According to the method for producing a solid secondary battery of (8), since the solid electrolyte layer has a porous substrate therein, it is less likely to deform when press-joined in step 2B. Therefore, defects are less likely to occur in the solid electrolyte layer.
[0024] (9) The method for producing a solid secondary battery according to (7) or (8), further comprising, after the step 2B, applying a pressure higher than the joining pressure in the press joining in the step 2B in a stacking direction of the electrode stack.
[0025] According to the method for producing a solid secondary battery in (9), in the 2C step, a pressure higher than the bonding pressure in the press bonding in the 2B step is applied in the stacking direction of the electrode laminate, so that the electrode laminate is densified and the adhesion between the layers of the electrode laminate is increased. As a result, the internal resistance of the obtained solid secondary battery is reduced, and characteristics such as cycle characteristics are improved.
[0026] (10) The method for producing a solid secondary battery according to any one of (7) to (9), wherein the Young's modulus of the anode layer, the intermediate layer, the solid electrolyte layer, and the cathode layer is the highest for the cathode layer, the second highest for the solid electrolyte layer, the second highest for the solid electrolyte layer, the anode layer, and the lowest for the intermediate layer.
[0027] According to the method for producing a solid secondary battery of (10), even if the Young's modulus of the intermediate layer is lower than those of each of the positive electrode layer, the solid electrolyte layer, and the negative electrode layer, defects are unlikely to occur in the solid electrolyte layer.
[0028] (11) The method for producing a solid secondary battery according to any one of (7) to (10), wherein a joining pressure in the press bonding in the step 2A is within a range of 300 to 500 MPa, and a joining pressure in the press bonding in the step 2B is 800 MPa or less.
[0029] According to the method for producing a solid secondary battery of (11), since the bonding pressure in steps 2A and 2B is within the above range, defects in the solid electrolyte layer are less likely to occur.
[0030] (12) The method for producing a solid secondary battery according to any one of (7) to (11), wherein the intermediate layer has a porosity greater than a porosity of the solid electrolyte layer.
[0031] According to the method for producing a solid secondary battery of (12), the porosity of the intermediate layer is larger than the porosity of the solid electrolyte layer, so that non-uniform deposition of metal at the negative electrode layer interface can be suppressed, and the cycle characteristics of the obtained solid secondary battery are improved.
[0032] (13) In the method for producing a solid secondary battery according to (9), in the step 2B and the step 2C, a roll press device is used for the press bonding, and a conveying direction of the intermediate layer-negative electrode layer stack conveyed to the roll press device in the step 2B is different from a conveying direction of the electrode stack conveyed to the roll press device in the step 2C.
[0033] According to the manufacturing method of a solid secondary battery of (13), the conveying direction of the intermediate layer-negative electrode layer laminate in the 2B step is different from the conveying direction of the electrode laminate in the 2C step. Therefore, compared with the case where the 2B step and the 2C step are performed by roll-to-roll, layers having a low Young's modulus, such as the negative electrode layer and the intermediate layer, are extended in one direction, which pulls the solid electrolyte layer, making it less likely that defects will occur in the solid electrolyte layer. Effect of the Invention
[0034] According to the present invention, it is possible to provide a method for producing a solid secondary battery in which defects are unlikely to occur in the solid electrolyte layer even when an intermediate layer is provided between the negative electrode layer and the solid electrolyte layer. [Brief description of the drawings]
[0035] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a solid secondary battery that can be manufactured using the manufacturing method for a solid secondary battery of the present invention. [Diagram 2] 1A to 1C are process diagrams illustrating a method for manufacturing a solid secondary battery according to a first embodiment of the present invention. [Diagram 3] 5A to 5C are process diagrams showing a method for manufacturing a solid secondary battery according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0036] Hereinafter, embodiments of the present invention will be described with reference to the drawings. However, the embodiments described below are merely examples of the present invention, and the present invention is not limited to the following.
[0037] <Solid secondary battery> A solid secondary battery that can be manufactured using the method for manufacturing a solid secondary battery of the present invention will be described below. Fig. 1 is a cross-sectional view showing an example of a solid secondary battery that can be manufactured using the method for manufacturing a solid secondary battery of the present invention.
[0038] As shown in FIG. 1, a solid secondary battery 100 includes an electrode laminate 1 and an exterior body 50 that houses the electrode laminate 1. The electrode laminate 1 is a laminate in which a positive electrode layer 10, a solid electrolyte layer 20, an intermediate layer 30, and a negative electrode layer 40 are laminated in this order. The positive electrode layer 10 includes a positive electrode collector 11 and a positive electrode active material layer 12 laminated on both sides of the positive electrode collector 11. The outer periphery of the positive electrode active material layer 12 is surrounded by an insulating frame 13. The positive electrode collector 11 is connected to a positive electrode terminal 16 via a positive electrode lead wire 15. An intermediate layer 30 and a negative electrode layer 40 are laminated on each of the positive electrode active material layers 12 laminated on both sides of the positive electrode collector 11. The negative electrode layer 40 has a negative electrode collector 41 and a metal layer 42 laminated on the surface of the negative electrode collector 41 on the solid electrolyte layer 20 side. The negative electrode collector 41 is connected to a negative electrode terminal 46 via a negative electrode lead wire 45. A portion of the positive electrode terminal 16 and the negative electrode terminal 46 are exposed from the exterior body 50. The electrode laminate 1 shown in Fig. 1 is in a discharged state. In the negative electrode layer 40 in a charged state, metal ions serving as a charge transfer medium are precipitated on the surface of the metal layer 42 to form a metal precipitate layer. The metal precipitate layer acts as a negative electrode active material layer, and releases metal ions during discharge.
[0039] There is no particular limitation on the material or shape of the positive electrode current collector 11 as long as it has the function of collecting current from the positive electrode layer 10. Examples of the material of the positive electrode current collector 11 include aluminum, aluminum alloy, stainless steel, nickel, iron, and titanium, and among these, aluminum, aluminum alloy, and stainless steel are preferable. Examples of the shape of the positive electrode current collector 11 include a foil shape, a plate shape, and the like.
[0040] The positive electrode active material layer 12 contains at least one type of positive electrode active material. There are no particular limitations on the positive electrode active material, and any material that is used in the positive electrode layers of general solid secondary batteries can be used. As the positive electrode active material, for example, a layered active material containing lithium, a spinel type active material, an olivine type active material, or the like can be used. A specific example of the positive electrode active material is lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), LiNi p Mn q Co r O 2 (p+q+r=1), LiNi p Al q Co r O 2 (p+q+r=1), lithium manganate (LiMn 2 O 4 ), Li 1+x Mn 2-x-y MO 4 Li-Mn spinel substituted with different elements represented by the formula (x+y=2, M=at least one selected from Al, Mg, Co, Fe, Ni, and Zn), lithium titanate (oxide containing Li and Ti), lithium metal phosphate (LiMPO 4 , M=at least one selected from Fe, Mn, Co, and Ni).
[0041] The positive electrode active material layer 12 may optionally contain a solid electrolyte in order to improve the charge transfer medium conductivity. It may also optionally contain a conductive assistant in order to improve the conductivity. Furthermore, it may also optionally contain a binder in order to achieve flexibility. There are no particular limitations on the solid electrolyte, conductive assistant, and binder, and those used in the positive electrode layer of a general solid secondary battery may be used.
[0042] The insulating frame 13 has a volume resistivity of 1×10 12 It may be 1×10 Ω cm or more. 12 ~1×10 17 It may be in the range of Ω cm, 1×10 14 ~1×10 17 The insulating frame 13 has a porosity of 40% or less. The porosity may be 20% or less, or may be in the range of 1 to 20%. If the porosity is too high, it may be difficult to maintain the structure of the insulating frame 13 when high pressure is applied in the battery production process, and there may be an increased risk of the deposited metal physically penetrating into the insulating frame 13 during charging and discharging, causing a short circuit.
[0043] The insulating frame 13 may be an organic material or an inorganic material. Examples of insulating materials contained in the insulating frame 13 include rubber, glass, resin (polyimide, polybenzimidazole, polyamideimide, polyetherimide, polyacetal, polyphenylene sulfide, polyetheretherketone, tetrafluoroethylene, 6-polyamide (6-nylon), ultra-high molecular weight polyethylene, polyethylene, polypropylene, polyvinyl chloride resin, polystyrene, polyethylene terephthalate, ABS resin, etc.), and ceramics (alumina, zirconia, silicon nitride, aluminum nitride, mullite, steatite, magnesia, sialon, macerite, etc.). The insulating material may be a single type, or a composite material in which two or more types of materials are combined. The insulating frame 13 may also contain a small amount of a binder or additive. The insulation breakdown voltage per unit thickness of the insulating frame 13 is preferably 10 kV / mm or more, and more preferably 100 kV / mm or more.
[0044] The material of the positive electrode lead wire 15 may be the same as the material of the positive electrode collector 11, or may be different from the material of the positive electrode collector 11. The positive electrode lead wire 15 may be integrally connected to the positive electrode collector 11. In this embodiment, the positive electrode lead wire 15 is formed by extending the positive electrode collector 11, and is integrally connected to the positive electrode collector 11. The material of the positive electrode terminal 16 may be the same as the material of the positive electrode lead wire 15, or may be different from the material of the positive electrode lead wire 15. The positive electrode terminal 16 may be integrally connected to the positive electrode lead wire 15. In this embodiment, the positive electrode terminal 16 and the positive electrode lead wire 15 are separate members and are electrically connected.
[0045] The solid electrolyte layer 20 is a layer laminated between the positive electrode layer 10 and the negative electrode layer 40. The solid electrolyte layer 20 contains at least one type of solid electrolyte material. The solid electrolyte layer 20 can conduct a charge transfer medium between the positive electrode layer 10 and the negative electrode layer 40 via the solid electrolyte material contained in the solid electrolyte layer 20.
[0046] The solid electrolyte material is not particularly limited as long as it has charge transfer medium conductivity. For example, a sulfide solid electrolyte material, an oxide solid electrolyte material, a nitride solid electrolyte material, a halide solid electrolyte material, etc. can be used.
[0047] Examples of sulfide solid electrolyte materials include Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -LiI, etc. 2 SP 2 S 5 " The statement is from Li 2 S and P 2 S 5 The sulfide solid electrolyte material may have an argyrodite-type crystal structure.
[0048] Examples of oxide solid electrolyte materials include NASICON-type oxides, garnet-type oxides, perovskite-type oxides, etc. Examples of NASICON-type oxides include oxides containing Li, Al, Ti, P, and O (e.g., Li 1.5 Al 0.5 Ti 1.5 (PO 4 ) 3 Examples of garnet-type oxides include oxides containing Li, La, Zr, and O (e.g., Li 7 La 3 Zr 2 O 12 Examples of perovskite oxides include oxides containing Li, La, Ti, and O (e.g., LiLaTiO 3 ) are mentioned.
[0049] The solid electrolyte layer 20 may contain a binder. There are no particular limitations on the binder, and any binder that is used in solid electrolyte layers of general solid secondary batteries can be used.
[0050] The porosity of the solid electrolyte layer 20 is lower than that of the intermediate layer 30 described later, for example, less than 10%. The particle size of the solid electrolyte material constituting the solid electrolyte layer 20 is, for example, 0.5 to 10 μm in median size (D50), and is preferably larger than that of the particles constituting the intermediate layer 30 described later.
[0051] The porosity of the solid electrolyte layer 20 can be calculated, for example, by the following formula (1): In formula (1), the "packing ratio" refers to the percentage of the density of the solid electrolyte layer after molding relative to the true density. Porosity (%) = (100-Filling rate (%)) …(1) The intermediate layer 30 is a layer laminated between the solid electrolyte layer 20 and the negative electrode layer 40. The intermediate layer 30 has the function of suppressing non-uniform deposition of metal ions at the interface of the negative electrode layer 40 and improving the interface adhesion.
[0052] The solid electrolyte layer 20 may have a porous substrate therein. The porous substrate may be, for example, a woven fabric or a nonwoven fabric. A solid electrolyte having a porous substrate therein has high strength.
[0053] The intermediate layer 30 preferably has electron conductivity and voids through which metal ions (e.g., lithium ions) serving as a charge transfer medium can pass. When the intermediate layer 30 has voids, when the solid secondary battery 100 is charged, the metal ions moving from the solid electrolyte layer 20 toward the negative electrode layer 40 pass through the intermediate layer 30 and are precipitated on the surface of the negative electrode current collector 41 of the negative electrode layer 40 on the intermediate layer 30 side, forming a metal precipitate layer (a layer of metallic lithium). By passing through the intermediate layer 30, a metal precipitate layer can be uniformly formed on the surface of the metal layer 42. In addition, by having voids, the intermediate layer 30 has flexibility that can follow the change in thickness of the negative electrode layer 40 accompanying charging and discharging. Therefore, even when the solid secondary battery 100 is repeatedly charged and discharged, the interfacial adhesion can be maintained, and the durability of the solid secondary battery 100 can be improved.
[0054] The porosity of the intermediate layer 30 is preferably higher than that of the solid electrolyte layer 20. This allows many voids through which metal ions can pass to be formed inside the intermediate layer 30, so that a metal deposit layer can be more uniformly formed on the surface of the metal layer 42. In addition, the intermediate layer 30 becomes more flexible, so that the ability to follow changes in the thickness of the negative electrode layer 40 is improved. The porosity of the intermediate layer 30 can be, for example, 40 to 70%. The porosity of the intermediate layer 30 can be calculated in the same manner as the porosity of the solid electrolyte layer 20.
[0055] The thickness of the intermediate layer 30 may be 5 μm or less. By making the thickness of the intermediate layer 30 5 μm or less, the deposition position of the metal, which is the charge transfer medium during charging, can be between the intermediate layer 30 and the negative electrode layer 40. This can greatly reduce the frequency of direct contact between the solid electrolyte layer 20 and the deposited metal, suppressing local deterioration and current concentration of the solid electrolyte layer 20, and improving cycle characteristics and storage characteristics. In addition, the relatively elastic intermediate layer 30 can be disposed between the hard solid electrolyte layer 20 and the deposited metal, making it easier to follow the expansion and contraction caused by the deposition and dissolution of the metal, allowing a uniform reaction in the in-plane and thickness directions, thereby obtaining the effects of reducing resistance and improving cycle characteristics. In order to obtain the effects of further reducing resistance and improving cycle characteristics, the thickness of the intermediate layer may be 3 μm or less, or may be within the range of 1 to 3 μm.
[0056] The intermediate layer 30 preferably contains amorphous carbon and metal nanoparticles. The intermediate layer 30 may further contain a binder as a binding material to maintain the structure.
[0057] Unlike graphite, amorphous carbon is less likely to react with metals such as lithium and form an alloy, and therefore can suppress the formation of dendrites and improve the cycle characteristics of solid secondary batteries. The amorphous carbon may be either easily graphitized carbon (soft carbon) or difficultly graphitized carbon (hard carbon). In addition, the amorphous carbon may be any carbon allotrope that does not show a clear crystalline state, and may be an aggregate of fine graphite crystals. Specific examples of amorphous carbon include carbon blacks such as acetylene black, furnace black, and ketjen black, coke, activated carbon, CNT (carbon nanotube), fullerene, and graphene.
[0058] Examples of metal nanoparticles include metal nanoparticles of tin (Sn), silicon (Si), zinc (Zn), magnesium (Mg), gold (Au), platinum (Pt), palladium (Pd), silver (Ag), aluminum (Al), bismuth (Bi), and antimony (Sb). The content of the metal nanoparticles in the intermediate layer 30 is preferably more than 0 mass% and 30 mass% or less. When the intermediate layer 30 contains metal nanoparticles, the electronic conductivity of the intermediate layer 30 can be increased, and a metal precipitate layer can be generated more uniformly. In addition, since the metal nanoparticles have a higher Young's modulus than amorphous carbon, the structure of the intermediate layer 30 can be maintained even when high-pressure pressing is performed when manufacturing the solid secondary battery 100.
[0059] The particle diameter of the amorphous carbon and metal nanoparticles is preferably smaller than that of the solid electrolyte material. This allows the intermediate layer 30 to enter the gaps between the solid electrolyte materials constituting the interface of the solid electrolyte layer 20, thereby increasing the contact area between the solid electrolyte layer 20 and the intermediate layer 30 and improving adhesion. The particle diameter of the amorphous carbon may be, for example, in the range of 0.04 to 0.05 μm in median diameter (D50). The particle diameter of the metal nanoparticles may be, for example, about 0.07 μm in median diameter (D50).
[0060] The binder is preferably one that can improve the adhesion between the particles constituting the intermediate layer 30 and between the intermediate layer 30 and the solid electrolyte layer 20. There are no particular limitations on the binder, and it is possible to use binders that are generally used in solid secondary batteries. Examples of binders include acrylic acid-based polymers, cellulose-based polymers, styrene-based polymers, vinyl acetate-based polymers, urethane-based polymers, fluoroethylene-based polymers, and PVDF-based polymers.
[0061] The material and shape of the negative electrode current collector 41 are not particularly limited as long as it has the function of collecting current from the negative electrode layer 40. Examples of materials for the negative electrode current collector 41 include nickel, copper, and stainless steel. Examples of the shape of the negative electrode current collector 41 include a foil shape, a plate shape, and the like.
[0062] The metal layer 42 is not particularly limited in material or shape as long as it has the function of densely precipitating a charge transfer medium such as lithium ions. When the charge transfer medium is lithium ions, the metal layer 42 can be a metallic lithium layer or a layer of a metal that forms an alloy with lithium. Examples of metals that form an alloy with lithium include Mg, Si, Au, Ag, In, Ge, Sn, Pb, Al, and Zn. The metal that forms the metal layer 42 may be in the form of a powder or a thin film. By using the negative electrode layer 40 having this metal layer 42, a uniform metal precipitate layer can be formed on the surface of the metal layer 42. The metal layer 42 may be omitted.
[0063] The material of the negative electrode lead wire 45 may be the same as the material of the negative electrode current collector 41, or may be different from the material of the negative electrode current collector 41. The negative electrode lead wire 45 may be integrally connected to the negative electrode current collector 41. In this embodiment, the negative electrode lead wire 45 is formed by extending the negative electrode current collector 41, and is integrally connected to the negative electrode current collector 41. The material of the negative electrode terminal 46 may be the same as the material of the negative electrode lead wire 45, or may be different from the material of the negative electrode lead wire 45. The negative electrode terminal 46 may be integrally connected to the negative electrode lead wire 45. In this embodiment, the negative electrode terminal 46 and the negative electrode lead wire 45 are separate members and are electrically connected to each other.
[0064] The exterior body 50 is expandable and contractable in accordance with the change in thickness of the negative electrode due to charging and discharging. A laminate film can be used as the material of the exterior body 50. As the laminate film, a laminate film having a three-layer structure in which an inner resin layer, a metal layer, and an outer resin layer are laminated in this order from the inside can be used. The outer resin layer is, for example, a polyamide (nylon) layer or a polyethylene terephthalate (PET) layer, the metal layer is, for example, an aluminum layer, and the inner resin layer may be, for example, a polyethylene layer or a polypropylene layer.
[0065] In the solid secondary battery 100, the Young's modulus of the anode layer 40, intermediate layer 30, solid electrolyte layer 20, and cathode layer 10 may be the highest in the cathode layer 10, the second highest in the solid electrolyte layer 20, the second highest in the solid electrolyte layer 20, the anode layer 40, and the lowest in the intermediate layer 30. The Young's modulus of each layer varies depending on the material and porosity contained in each layer. For example, the Young's modulus of the cathode layer 10 is 100% when the cathode active material is LiCoO 2 The Young's modulus of the solid electrolyte layer 20 may be within a range of 190 to 200 GPa when the solid electrolyte is an oxide, and 198 GPa when the solid electrolyte is a sulfide. The Young's modulus of the negative electrode layer 40 may be within a range of 6 to 8 GPa when the negative electrode current collector 41 is copper and the metal layer 42 is lithium (4 to 5 GPa when lithium is the elemental lithium). The intermediate layer 30 may be 1 GPa or less, within a range of approximately 700 to 800 MPa.
[0066] <Method of manufacturing solid secondary battery> [First embodiment] The method for producing a solid secondary battery according to the present embodiment includes steps 1A, 1B, 1C, and 1D. Fig. 2 is a process chart showing the method for producing a solid secondary battery according to the first embodiment of the present invention.
[0067] As shown in FIG. 2 (1A), the 1A step is a step of press-bonding the negative electrode layer 40 and the intermediate layer 30 of the lead-wire-attached negative electrode layer 110 to obtain an intermediate layer-negative electrode layer laminate 120. In this embodiment, the lead-wire-attached negative electrode layer 110 is used as the negative electrode layer 40. The lead-wire-attached negative electrode layer 110 has the negative electrode layer 40 and the negative electrode lead wire 45 connected to the negative electrode current collector 41 of the negative electrode layer 40. The negative electrode layer 40 includes the negative electrode current collector 41 and a metal layer 42 laminated on the surface of the negative electrode current collector 41. In this embodiment, the intermediate layer 30 is disposed on the metal layer 42 of the lead-wire-attached negative electrode layer 110, and the obtained laminate is press-bonded to obtain the intermediate layer-negative electrode layer laminate 120. There is no particular restriction on the bonding pressure in the press bonding in the 1A step, as long as the layers of the negative electrode layer 40 and the intermediate layer 30 are not excessively deformed and can be bonded without peeling in a subsequent step. The joining pressure in the press joining in step 1A is, for example, within a range of 300 to 500 MPa.
[0068] In the 1B step, as shown in FIG. 2(1B), the intermediate layer 30 and the solid electrolyte layer 20 of the intermediate layer-negative electrode layer laminate 120 are press-bonded to obtain a solid electrolyte layer-intermediate layer-negative electrode layer laminate 130. A solid electrolyte layer transfer sheet can be used as the solid electrolyte layer 20. The solid electrolyte layer transfer sheet is a sheet in which the solid electrolyte layer 20 is peelably laminated on the surface of a support sheet. When the solid electrolyte layer transfer sheet is used, the solid electrolyte layer 20 of the solid electrolyte layer transfer sheet is placed on the intermediate layer 30 of the intermediate layer-negative electrode layer laminate 120, the obtained laminate is press-bonded, the solid electrolyte layer 20 is transferred onto the intermediate layer 30 of the intermediate layer-negative electrode layer laminate 120, and the support sheet is peeled off and collected to obtain the solid electrolyte layer-intermediate layer-negative electrode layer laminate 130. The bonding pressure in the press bonding in step 1B is preferably a pressure that can bond the negative electrode layer 40, the intermediate layer 30, and the solid electrolyte layer 20 without excessively deforming them and preventing them from peeling off in a subsequent step. For this reason, in this embodiment, the bonding pressure in the press bonding in step 1B is set to a pressure lower than the bonding pressure in step 1A. The bonding pressure in the press bonding in step 1B may be, for example, within a range of 1 / 10 to 1 / 2 of the bonding pressure in step 1A. The bonding pressure in the press bonding in step 1B is, for example, within a range of 50 to 100 MPa.
[0069] In the 1C step, as shown in FIG. 2 (1C), the solid electrolyte layer 20 and the positive electrode layer 10 of the solid electrolyte layer-intermediate layer-negative electrode layer laminate 130 are press-bonded to obtain an electrode laminate (positive electrode layer-solid electrolyte layer-intermediate layer-negative electrode layer laminate) 150. In this embodiment, a positive electrode layer 140 with a lead wire is used as the positive electrode layer 10. The positive electrode layer 140 with a lead wire has the positive electrode layer 10 and a positive electrode lead wire 15 connected to the positive electrode current collector 11 of the positive electrode layer 10. The positive electrode layer 10 includes the positive electrode current collector 11, a positive electrode active material layer 12 laminated on both sides of the positive electrode current collector 11, and an insulating frame 13 surrounding the outer periphery of the positive electrode active material layer 12. In this embodiment, the positive electrode active material layer 12 of the positive electrode layer 140 with lead wire is placed on the solid electrolyte layer 20 of the solid electrolyte layer-intermediate layer-negative electrode layer laminate 130, and the resulting laminate is press-bonded. As a result, an electrode laminate 150 is obtained in which the negative electrode layer 40, the intermediate layer 30, the solid electrolyte layer 20, and the positive electrode layer 10 are laminated in this order (see FIG. 2(1D)). The solid electrolyte layer 20, the intermediate layer 30, and the negative electrode layer 40 may be further laminated on the positive electrode active material layer 12 on the upper side of the electrode laminate 150. The bonding pressure in the press bonding in the 1C step is preferably a pressure that can bond the negative electrode layer 40, the intermediate layer 30, the solid electrolyte layer 20, and the positive electrode layer 10 without excessively deforming them and without peeling them off when the battery is used. For this reason, in this embodiment, the bonding pressure in the press bonding in the 1C step is set to a pressure higher than the bonding pressure in the press bonding in the 1A step. The bonding pressure in the press bonding in step 1C may be, for example, within a range of 1.5 to 3.0 times the bonding pressure in the press bonding in step 1A. The bonding pressure in the press bonding in step 1C is, for example, within a range of 500 to 800 MPa.
[0070] As shown in FIG. 2 (1D), the 1D step is a step of pressing the electrode laminate 150 in the lamination direction. The bonding pressure in the press bonding in the 1D step is preferably a pressure that does not excessively deform each of the negative electrode layer 40, the intermediate layer 30, the solid electrolyte layer 20, and the positive electrode layer 10, and can increase the density of the electrode laminate 150. For this reason, in this embodiment, the bonding pressure in the press bonding in the 1D step is set to a pressure higher than the bonding pressure in the press bonding in the 1C step. The bonding pressure in the press bonding in the 1D step may be, for example, 1.05 times or more the bonding pressure in the press bonding in the 1C step, and may be in the range of 1.10 to 2.00 times. The bonding pressure in the press bonding in the 1B step may be, for example, more than 800 MPa, and is in the range of 850 to 1500 MPa.
[0071] In steps 1A to 1D, the press bonding apparatus is not particularly limited, and a roll press apparatus or a flat plate press apparatus can be used. When the press bonding in steps 1A to 1D is performed using a roll press apparatus, the conveying direction of the objects to be press bonded to the roll press apparatus in steps 1A to 1C may be the same or different. It is preferable that the conveying direction of the objects to be press bonded to the roll press apparatus in steps 1C and 1D is different. That is, it is preferable that the conveying direction of the solid electrolyte layer-intermediate layer-negative electrode layer laminate conveyed to the roll press apparatus in step 1C is different from the conveying direction of the electrode laminate 150 conveyed to the roll press apparatus in step 1D. For example, in the 1C step, the solid electrolyte layer-intermediate layer-negative electrode layer laminate 130 and the lead-wire-attached positive electrode layer 140 are press-bonded by a roll press device to obtain the electrode laminate 150, and in the 1D step, the electrode laminate 150 is pressed by the roll press device. In this case, the direction of the electrode laminate 150 to the roll press device in the 1D step may be perpendicular to the direction of the solid electrolyte layer-intermediate layer-negative electrode layer laminate 130 to the roll press device in the 1C step. As a result, the direction in which the metal layer 42 and the intermediate layer 30 of the solid electrolyte layer-intermediate layer-negative electrode layer laminate 130 are pressurized and extended in the 1C step is perpendicular to the direction in which the metal layer 42 and the intermediate layer 30 of the electrode laminate 150 are pressurized and extended in the 1D step. For this reason, layers with a low Young's modulus, such as the metal layer 42 and the intermediate layer 30, are extended in one direction, which pulls the solid electrolyte layer 20, making it difficult for defects to occur in the solid electrolyte layer 20.
[0072] The solid secondary battery 100 can be manufactured using the electrode laminate 150 obtained as described above as follows. A positive electrode terminal 16 is connected to the positive electrode lead wire 15 of the electrode laminate 150, and a negative electrode terminal 46 is connected to the negative electrode lead wire 45. Next, the electrode laminate 150 with the positive electrode terminal 16 and the negative electrode terminal 46 connected is housed in an exterior body 50, and the exterior body 50 is sealed.
[0073] According to the manufacturing method of the solid secondary battery of the first embodiment configured as described above, the bonding pressure in the 1B step is lower than the bonding pressure in the press bonding in the 1A step, so that in the 1B step, defects such as cracks and fissures are unlikely to occur in the solid electrolyte layer 20. In addition, in the 1C step, since the solid electrolyte layer 20 is supported by the intermediate layer 30 and the negative electrode layer 40, even if the bonding pressure in the press bonding in the 1C step is higher than the bonding pressure in the press bonding in the 1A step, defects are unlikely to occur in the solid electrolyte layer 20. Furthermore, in the 1D step, a pressure higher than the bonding pressure in the press bonding in the 1C step is applied in the stacking direction of the electrode stack 150, so that the electrode stack 150 is densified and the adhesion of each layer of the electrode stack 150 is increased. Therefore, according to the manufacturing method of the solid secondary battery of the first embodiment, the obtained solid secondary battery is unlikely to have defects such as cracks and fissures in the solid electrolyte layer 20, the internal resistance is reduced, and characteristics such as cycle characteristics are improved.
[0074] [Second embodiment] The method for producing a solid secondary battery according to the present embodiment includes a step 2A, a step 2B, and a step 2C. Fig. 3 is a process diagram showing the method for producing a solid secondary battery according to the second embodiment of the present invention. Note that the materials used in the method for producing a solid secondary battery according to the second embodiment are the same as those used in the method for producing a solid secondary battery according to the first embodiment, so in Fig. 3, the same materials as those in Fig. 2 are denoted by reference characters and detailed descriptions thereof are omitted.
[0075] The 2A step is a step of pressing the negative electrode layer 40 of the lead-wire-attached negative electrode layer 110 and the intermediate layer 30 to obtain an intermediate layer-negative electrode layer laminate 120, as shown in FIG. 3(2A). In the 1A step, the negative electrode layer 40 of the lead-wire-attached negative electrode layer 110 and the intermediate layer 30 are pressed together to obtain a pair of intermediate layer-negative electrode layer laminates 120, as shown in FIG. 2(1A). In this embodiment, the negative electrode layer 110 with the lead wire is used as the negative electrode layer 40, and the negative electrode layer 40 of the lead-wire-attached negative electrode layer 110 and the intermediate layer 30 are pressed together to obtain a pair of intermediate layer-negative electrode layer laminates 120. There are no particular limitations on the conditions of the pressing pressure in the 2A step, as long as the negative electrode layer 40 and the intermediate layer 30 can be pressed together without excessively deforming them and without peeling them off in a subsequent step. The pressing pressure in the 1A step is, for example, within the range of 300 to 500 MPa.
[0076] In the 2B step, as shown in FIG. 3(2B), the solid electrolyte layer 20 and the positive electrode layer 10 are arranged in this order on the intermediate layer 30 of the intermediate layer-negative electrode layer laminate 120, and press-bonded to obtain an electrode laminate 160. In this embodiment, a lead-wire-attached positive electrode layer 140 is used as the positive electrode layer 10. The solid electrolyte layer 20 may have a porous substrate inside. The solid electrolyte layer having a porous substrate inside has high strength, so it is not easily deformed when press-bonded in the 2B step. In this embodiment, a pair of intermediate layer-negative electrode layer laminates 120 are arranged so that the respective intermediate layers 30 face each other, a solid electrolyte layer 20 is arranged on each intermediate layer 30 of the pair of intermediate layer-negative electrode layer laminates 120, and a lead-wire-attached positive electrode layer 140 is arranged between the solid electrolyte layers 20 so that the positive electrode active material layer 12 of the lead-wire-attached positive electrode layer 140 faces each other, and the obtained laminate is press-bonded. As a result, an electrode laminate 150 is obtained in which the negative electrode layer 40, the intermediate layer 30, the solid electrolyte layer 20, the positive electrode layer 10, the solid electrolyte layer 20, the intermediate layer 30, and the negative electrode layer 40 are laminated in this order (see FIG. 3(1C)). The bonding pressure in the press bonding in the 2B step is preferably a pressure that can bond the negative electrode layer 40, the intermediate layer 30, the solid electrolyte layer 20, and the positive electrode layer 10 without excessively deforming them and preventing them from peeling off when the battery is used. For this reason, in this embodiment, the bonding pressure in the press bonding in the 2B step is set to a pressure higher than the bonding pressure in the press bonding in the 2A step. The bonding pressure in the press bonding in the 2B step may be, for example, within a range of 1.5 to 3.0 times the bonding pressure in the press bonding in the 1A step. The bonding pressure in the press bonding in the 1C step is, for example, within a range of 500 to 800 MPa.
[0077] As shown in FIG. 2(1C), the 2C step is a step of applying pressure in the lamination direction of the electrode laminate 160. The bonding pressure in the press bonding in the 2C step is preferably a pressure that does not excessively deform each of the negative electrode layer 40, the intermediate layer 30, the solid electrolyte layer 20, and the positive electrode layer 10, and can increase the density of the electrode laminate 150. For this reason, in this embodiment, the bonding pressure in the press bonding in the 2C step is set to a pressure higher than the bonding pressure in the press bonding in the 2B step. The bonding pressure in the press bonding in the 2C step may be, for example, 1.05 times or more the bonding pressure in the press bonding in the 2B step, and may be in the range of 1.10 to 2.00 times. The bonding pressure in the press bonding in the 1B step may be, for example, more than 800 MPa, and is in the range of 850 to 1500 MPa.
[0078] In the steps 2A to 2C, the press bonding apparatus is not particularly limited, and a roll press apparatus or a flat plate press apparatus can be used. When the press bonding in the steps 2A to 2C is performed using a roll press apparatus, the conveying direction of the objects to be press bonded to the roll press apparatus in the steps 2A and 2B may be the same or different. It is preferable that the conveying direction of the objects to be press bonded to the roll press apparatus in the steps 2B and 2C is different. That is, it is preferable that the conveying direction of the intermediate layer-negative electrode layer laminate 120 conveyed to the roll press apparatus in the step 2BC is different from the conveying direction of the electrode laminate 160 conveyed to the roll press apparatus in the step 2C. For example, in the case where the intermediate layer-negative electrode layer laminate 120, the solid electrolyte layer 20, and the positive electrode layer 140 with lead wires are press-bonded by a roll press device to obtain the electrode laminate 160 in the 2B step, and the electrode laminate 160 is pressed by the roll press device in the 2C step, the direction of the electrode laminate 160 to the roll press device in the 2C step may be perpendicular to the direction of the intermediate layer-negative electrode layer laminate 120 to the roll press device in the 2B step. As a result, the direction in which the metal layer 42 and the intermediate layer 30 of the intermediate layer-negative electrode layer laminate 120 are pressed and extended in the 2B step is perpendicular to the direction in which the metal layer 42 and the intermediate layer 30 of the electrode laminate 160 are pressed and extended in the 2C step. For this reason, the layers with a low Young's modulus, such as the metal layer 42 and the intermediate layer 30, are extended in one direction, which pulls the solid electrolyte layer 20, making it difficult for defects to occur in the solid electrolyte layer 20.
[0079] The solid secondary battery 100 can be manufactured using the electrode laminate 160 obtained as described above as follows. A positive electrode terminal 16 is connected to the positive electrode lead wire 15 of the electrode laminate 160, and a negative electrode terminal 46 is connected to the negative electrode lead wire 45. Next, the electrode laminate 150 with the positive electrode terminal 16 and the negative electrode terminal 46 connected is housed in an exterior body 50, and the exterior body 50 is sealed.
[0080] According to the manufacturing method of the solid secondary battery of the second embodiment configured as described above, in the 2B step, the solid electrolyte layer 20 is supported by the intermediate layer 30 and the negative electrode layer 40, so that even if the joining pressure in the press joining in the 2B step is higher than the joining pressure in the press joining in the 2A step, defects are unlikely to occur in the solid electrolyte layer 20. In addition, in the 2C step, a pressure higher than the joining pressure in the press joining in the 2B step is applied in the stacking direction of the electrode stack 160, so that the electrode stack 160 is densified and the adhesion of each layer of the electrode stack 160 is increased. Therefore, according to the manufacturing method of the solid secondary battery of the second embodiment, the obtained solid secondary battery is unlikely to have defects such as cracks and fissures in the solid electrolyte layer 20, the internal resistance is reduced, and characteristics such as cycle characteristics are improved.
[0081] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment. For example, in this embodiment, the negative electrode layer 110 with a lead wire is used as a member for forming the negative electrode layer 40, and the positive electrode layer 140 with a lead wire is used as a member for forming the positive electrode layer 10, but the members for forming the negative electrode layer 40 and the positive electrode layer 10 may not have lead wires. For example, after producing the electrode laminate, the positive electrode lead wire 15 may be connected to the positive electrode current collector 11, and the negative electrode lead wire 45 may be connected to the negative electrode current collector 41.
[0082] In this embodiment, the negative electrode layer 40 includes the metal layer 42, and a metal precipitate layer is formed on the surface of the metal layer 42 during charging, but the negative electrode layer 40 is not limited to this. Instead of the metal layer 42, a layer including a negative electrode active material capable of absorbing and releasing a charge transfer medium such as lithium ions may be used. In this case, the negative electrode active material layer may be disposed on the surface of the current collecting substrate 41a. As the negative electrode active material, a material used in the negative electrode of a general solid secondary battery may be used. When the charge transfer medium is lithium ions, examples of the negative electrode active material include lithium transition metal oxides such as lithium titanate, TiO 2 , Nb 2 O 3 and WO 3Examples of the material include transition metal oxides such as silicon, silicon dioxide, metal sulfides, metal nitrides, and carbon materials such as artificial graphite, natural graphite, graphite, soft carbon, and hard carbon. The negative electrode active material layer may optionally contain a solid electrolyte from the viewpoint of improving the charge transfer medium conductivity. In addition, it may optionally contain a conductive assistant to improve the conductivity. Furthermore, it may optionally contain a binder from the viewpoint of expressing flexibility. As for the solid electrolyte, conductive assistant, and binder, those generally used in solid batteries can be used. EXAMPLES
[0083] <Example 1> [Preparation of positive electrode layer] An aluminum foil having a thickness of 15.0 μm was prepared as a positive electrode current collector. A mixture of 80 parts by mass of lithium nickel cobalt manganese composite oxide (NCM622) as the positive electrode active material, 17 parts by mass of an argyrodite-type sulfide solid electrolyte as the solid electrolyte, 2 parts by mass of carbon black as the conductive assistant, and 1 part by mass of an SBR (styrene butadiene rubber) binder as the binding material was used. The mixture was dispersed in 43 parts by mass of butyl butyrate to prepare a positive electrode active material layer slurry. The obtained positive electrode active material layer slurry was applied to one surface of a positive electrode current collector so that the surface area after drying was 27 mg / cm. 2 The positive electrode layer was prepared by applying the positive electrode active material layer having a thickness of 80.0 μm using a bar coater so as to obtain a positive electrode layer.
[0084] [Preparation of solid electrolyte layer transfer sheet] A dispersion of an argyrodite-type sulfide solid electrolyte (median diameter: 3.0 μm) was applied to a support sheet and dried to form an argyrodite-type sulfide solid electrolyte layer, thereby producing a solid electrolyte layer transfer sheet.
[0085] [Preparation of intermediate layer transfer sheet] A total of 95 parts by mass of Sn particles (median diameter: 0.07 μm) as metal nanoparticles, acetylene black (median diameter: 0.05 μm) as amorphous carbon, and 5 parts by mass of PVDF-based binder as a binding material were mixed. The resulting mixture was dispersed in 1000 parts by mass of NMP (N-methyl-2-pyrrolidone) to prepare an intermediate layer slurry. The resulting intermediate layer slurry was applied to a support sheet and dried to produce an intermediate layer transfer sheet with a final thickness of 3.0 μm.
[0086] [Creation of negative electrode layer] As a negative electrode current collector, a copper foil having a thickness of 10 μm was prepared. A 40 μm-thick metallic lithium foil was laminated on the surface of the copper foil to prepare a negative electrode layer.
[0087] [Preparation of electrode laminate] The intermediate layer of the intermediate layer transfer sheet was transferred onto the metallic lithium foil of the negative electrode layer, and then the negative electrode layer and the intermediate layer were press-bonded at a bonding pressure of 300 MPa to produce an intermediate layer-negative electrode layer laminate (step I). Next, the solid electrolyte layer of the solid electrolyte layer transfer sheet was placed on the intermediate layer of the intermediate layer-negative electrode layer laminate, and then the intermediate layer and the solid electrolyte layer transfer sheet were press-bonded at a bonding pressure of 50 MPa, and then the support sheet of the solid electrolyte layer transfer sheet was peeled off to produce a solid electrolyte layer-intermediate layer-negative electrode layer laminate (step II). Next, the positive electrode active material layer of the positive electrode layer was placed on the solid electrolyte layer of the solid electrolyte layer-intermediate layer-negative electrode layer laminate, and then the solid electrolyte layer and the positive electrode layer were press-bonded at a bonding pressure of 500 MPa to produce an electrode laminate (positive electrode layer-solid electrolyte layer-intermediate layer-negative electrode layer laminate) (step III). A multi-stage press machine was used to apply a pressure of 980 MPa in the lamination direction of the obtained electrode laminate, thereby densifying the electrode laminate (step IV).In this manner, an electrode laminate was produced.
[0088] [Preparation of solid-state secondary batteries] After attaching tabs to the positive and negative current collectors of the electrode laminate obtained above, the electrode laminate was housed in a bag-shaped laminate pack. The laminate pack was then sealed under an argon atmosphere. A restraining member was placed on the surface of the laminate pack so as to face the negative current collector of the electrode laminate, and a restraining force of 3 MPa was applied to the electrode laminate to produce a solid secondary battery.
[0089] <Example 2> A solid secondary battery was produced in the same manner as in Example 1, except that the joining pressure in the III step was set to 550 MPa.
[0090] <Example 3> A solid secondary battery was produced in the same manner as in Example 1, except that the joining pressure in the III step was set to 600 MPa.
[0091] <Example 4> The intermediate layer of the intermediate layer transfer sheet was transferred onto the metallic lithium foil of the negative electrode layer, and then the metallic lithium foil and the intermediate layer were press-bonded at a bonding pressure of 400 MPa to produce an intermediate layer-negative electrode layer laminate (step I). Next, a solid electrolyte layer was disposed on the intermediate layer of the intermediate layer-negative electrode layer laminate, and then the positive electrode active material layer of the positive electrode layer was disposed on the solid electrolyte layer, and then the intermediate layer, the solid electrolyte layer, and the positive electrode layer were press-bonded at a bonding pressure of 500 MPa to produce an electrode laminate (positive electrode layer-solid electrolyte layer-intermediate layer-negative electrode layer laminate) (step II). Next, a pressure of 900 MPa was applied in the stacking direction of the obtained electrode laminate using a multi-stage press device to densify the electrode laminate (step III). A solid secondary battery was produced in the same manner as in Example 1 except for the above.
[0092] <Example 5> A solid secondary battery was produced in the same manner as in Example 4, except that the joining pressure in step I was 430 MPa and the joining pressure in step III was 950 MPa.
[0093] <Example 6> A solid secondary battery was produced in the same manner as in Example 1, except that the joining pressure in step IV was 950 MPa.
[0094] <Example 7> A solid secondary battery was produced in the same manner as in Example 1, except that the joining pressure in step III was 600 MPa and the joining pressure in step IV was 950 MPa.
[0095] <Comparative Example 1> A solid secondary battery was produced in the same manner as in Example 1, except that the electrode laminate was produced as follows. The solid electrolyte layer of the solid electrolyte layer transfer sheet was placed on the positive electrode active material layer of the positive electrode layer, and then the positive electrode layer and the solid electrolyte layer transfer sheet were press-bonded with a bonding pressure of 300 MPa, and then the support sheet of the solid electrolyte layer transfer sheet was peeled off to produce a positive electrode layer-solid electrolyte layer laminate (step I). Next, the intermediate layer of the intermediate layer transfer sheet was transferred onto the solid electrolyte layer of the positive electrode layer-solid electrolyte layer laminate, and then the solid electrolyte layer and the intermediate layer were press-bonded with a bonding pressure of 500 MPa to produce a positive electrode layer-solid electrolyte layer-intermediate layer laminate (step II). Next, the positive electrode layer-solid electrolyte layer-intermediate layer laminate was densified by applying a pressure of 800 MPa using a multi-stage press machine in the stacking direction (step III). A metallic lithium foil of the negative electrode layer was placed on the intermediate layer of the densified positive electrode layer-solid electrolyte layer-intermediate layer laminate, and then the solid electrolyte and the negative electrode layer were press-bonded with a bonding pressure of 300 MPa to produce an electrode laminate (positive electrode layer-solid electrolyte layer-intermediate layer-negative electrode layer laminate) (Step IV).
[0096] <Comparative Example 2> A solid secondary battery was produced in the same manner as in Comparative Example 1, except that the joining pressure in step III was set to 900 MPa.
[0097] <Comparative Example 3> A solid secondary battery was produced in the same manner as in Comparative Example 1, except that the bonding pressure in step I was 80 MPa, the bonding pressure in step II was 120 MPa, and the bonding pressure in step IV was 120 MPa.
[0098] <Comparative Example 4> A solid secondary battery was produced in the same manner as in Comparative Example 1, except that the joining pressure in step IV was set to 120 MPa.
[0099] The steps for producing the electrode laminates of Examples 1 to 7 and Comparative Examples 1 to 4 are shown in Table 1 below.
[0100] <Evaluation> The Young's modulus was measured for the negative electrode, intermediate layer, solid electrolyte layer, and positive electrode layer used in Examples 1 to 7 and Comparative Examples 1 to 4. In addition, the porosity was measured for the intermediate layer and solid electrolyte layer. The results are shown in Table 2.
[0101] For the solid secondary batteries produced in Examples 1 to 7 and Comparative Examples 1 to 4, cycle tests were conducted in which charging and discharging were repeated at a charging upper limit voltage of 4.3V, a discharging lower limit voltage of 2.65V, and a C rate of 1 / 3C. The ratio of the discharge capacity to the first charging capacity (discharging capacity / charging capacity×100) was taken as the initial charging and discharging efficiency. In addition, the presence or absence of a short circuit in the solid secondary battery was confirmed from the second charging capacity. In addition, when the ratio of the first discharging capacity to the second charging capacity (second charging capacity / first discharging capacity×100) exceeded 105%, the short circuit behavior during the second charging was taken as "present", and when the ratio of the first discharging capacity to the second charging capacity was 105% or less, the short circuit behavior during the second charging was taken as "absent". These results are shown in Table 2.
[0102] [Table 1]
[0103] [Table 2]
[0104] From the results of Tables 1 and 2, it can be seen that the solid secondary batteries obtained in Examples 1 to 7 have high initial charging efficiency, are less likely to short circuit, and can be charged and discharged at 25°C, even if an intermediate layer with a low Young's modulus is provided between the negative electrode layer and the solid electrolyte layer. In contrast, the solid secondary batteries obtained in Comparative Examples 1, 2, 4, and 5, in which the negative electrode layer was joined to the positive electrode layer-solid electrolyte layer-intermediate layer laminate, had low initial charging efficiency, short circuit occurred in the second cycle, and could not be charged and discharged at 25°C. In addition, as a result of disassembling the solid secondary batteries after evaluating the battery characteristics, the solid secondary batteries obtained in Comparative Examples 1 to 4 had cracks and fissures in the solid electrolyte layer. [Explanation of symbols]
[0105] 1 Electrode laminate 10 Positive electrode layer 11 Positive electrode current collector 12 Cathode active material layer 13 Insulation frame 20 Solid electrolyte layer 30 Middle Class 40 Negative electrode layer 41 Negative electrode current collector 42 Metal layer 50 Exterior body 100 Solid state secondary battery 110 Negative electrode layer with lead wire 120 Intermediate layer-negative electrode layer laminate 130 Solid electrolyte layer-intermediate layer-negative electrode layer laminate 140 Positive electrode layer with lead wire 150, 160 Electrode laminate
Claims
1. A method for producing a solid-state secondary battery including an electrode stack in which a negative electrode layer, an intermediate layer, a solid electrolyte layer, and a positive electrode layer are stacked in this order, comprising: A first step A of press-bonding the negative electrode layer and the intermediate layer to obtain an intermediate layer-negative electrode layer laminate; a first step B of press-bonding the intermediate layer and the solid electrolyte layer of the intermediate layer-negative electrode layer laminate to obtain a solid electrolyte layer-intermediate layer-negative electrode layer laminate; a first step C of press-joining the solid electrolyte layer and the positive electrode layer of the solid electrolyte layer-intermediate layer-negative electrode layer laminate to obtain the electrode laminate, a bonding pressure in the first step B being lower than a bonding pressure in the press bonding in the first step A, and a bonding pressure in the first step C being higher than a bonding pressure in the press bonding in the first step A.
2. 2. The method for producing a solid secondary battery according to claim 1, further comprising, after the first step C, a first step D of applying a pressure higher than a joining pressure in the press joining in the first step C in a stacking direction of the electrode stack.
3. 2. The method for producing a solid secondary battery according to claim 1, wherein the Young's modulus of the negative electrode layer, the intermediate layer, the solid electrolyte layer, and the positive electrode layer is the highest for the positive electrode layer, the second highest for the solid electrolyte layer, the second highest for the solid electrolyte layer, the negative electrode layer, and the lowest for the intermediate layer.
4. The method for producing a solid secondary battery according to claim 1, wherein the joining pressure in the press joining in the first A step is within a range of 300 to 500 MPa, the joining pressure in the press joining in the first B step is within a range of 50 to 100 MPa, and the joining pressure in the first C step is 800 MPa or less.
5. The method for producing a solid secondary battery according to claim 1 , wherein the porosity of the intermediate layer is greater than the porosity of the solid electrolyte layer.
6. 3. The method for producing a solid secondary battery according to claim 2, wherein in the first C step and the first D step, a roll press device is used for press bonding, and a conveying direction of the solid electrolyte layer-intermediate layer-negative electrode layer stack conveyed to the roll press device in the first C step is different from a conveying direction of the electrode stack conveyed to the roll press device in the first D step.
7. A method for producing a solid-state secondary battery including an electrode stack in which a negative electrode layer, an intermediate layer, a solid electrolyte layer, and a positive electrode layer are stacked in this order, comprising: A second step A of press-bonding the negative electrode layer and the intermediate layer to obtain an intermediate layer-negative electrode layer laminate; a second step B of disposing a solid electrolyte layer and a positive electrode layer in this order on the intermediate layer of the intermediate layer-negative electrode layer laminate and press-bonding them to obtain the electrode laminate, The method for manufacturing a solid secondary battery, wherein the bonding pressure in the second step B is higher than the bonding pressure in the press bonding in the second step A.
8. The method for producing a solid secondary battery according to claim 7 , wherein the intermediate layer has a porous substrate therein.
9. 8. The method for producing a solid secondary battery according to claim 7, further comprising, after the step 2B, a step 2C of applying a pressure higher than a joining pressure in the press joining in the step 2B in a stacking direction of the electrode stack.
10. 8. The method for producing a solid secondary battery according to claim 7, wherein the Young's modulus of the negative electrode layer, the intermediate layer, the solid electrolyte layer, and the positive electrode layer is the highest for the positive electrode layer, the second highest for the solid electrolyte layer, the second highest for the solid electrolyte layer, the negative electrode layer, and the lowest for the intermediate layer.
11. 8. The method for producing a solid secondary battery according to claim 7, wherein the joining pressure in the press joining in the second A step is within a range of 300 to 500 MPa, and the joining pressure in the press joining in the second B step is 800 MPa or less.
12. The method for producing a solid secondary battery according to claim 7 , wherein the porosity of the intermediate layer is greater than the porosity of the solid electrolyte layer.
13. 10. The method for producing a solid secondary battery according to claim 9, wherein in the second B step and the second C step, a roll press device is used for press bonding, and a conveying direction of the intermediate layer-negative electrode layer laminate conveyed to the roll press device in the second B step is different from a conveying direction of the electrode laminate conveyed to the roll press device in the second C step.
Citation Information
Patent Citations
Manufacturing method for all-solid battery
JP2012069248A
Method of manufacturing battery
JP2014207104A
Method for manufacturing solid battery
JP2015153647A
Method of manufacturing all-solid battery
JP2017010816A
Manufacturing method of all-solid battery
JP2018147621A
Cited By
Method for producing solid-state battery
WO2026210684A1
Method for manufacturing solid-state battery
WO2026210688A1