Secondary battery
By incorporating carbon nanotubes in the positive electrode layer and controlling the thickness and fluidity of both electrode layers, the secondary battery addresses electrolyte leakage and uneven salt concentration issues, enhancing its high-rate performance.
Patent Information
- Application Number
- JP2023060222
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-16
AI Technical Summary
Secondary batteries experience performance deterioration during high-rate charging and discharging due to electrolyte leakage and uneven salt concentration between positive and negative electrodes, leading to increased internal resistance.
The secondary battery design includes a configuration where the positive electrode composite material layer contains carbon nanotubes to create fine voids, ensuring high fluidity of the electrolyte, and the thickness and fluidity index values of both positive and negative electrode layers are controlled to balance electrolyte flow, reducing uneven salt concentration.
This design effectively suppresses performance deterioration during high-rate energization by maintaining consistent electrolyte distribution, thereby improving the battery's high-rate characteristics.
Smart Images

Figure 2024147299000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a secondary battery. [Background technology]
[0002] Conventionally, there is a secondary battery equipped with an electrode assembly formed by winding up positive and negative electrode sheets stacked with a separator sandwiched therebetween. In a secondary battery equipped with such an electrode assembly, during high-rate charging and discharging in which a large current flows, the electrolyte and the electrode mixture constituting the electrode sheet expand due to heat generation, and the electrolyte impregnated in the electrode assembly flows out. Furthermore, this causes unevenness in the salt concentration of the electrolyte impregnated in the electrode assembly, which increases the internal resistance. As a result, there is a problem that the charge and discharge performance deteriorates.
[0003] In order to solve such a problem, attention is paid to the fact that the amount of electrolyte flowing out from the electrode mixture during high-rate current application is likely to be greater on the negative electrode side than on the positive electrode side. Then, as shown in, for example, Patent Documents 1 to 4, etc., by balancing the difference in the amount of electrolyte flowing out on the positive electrode side and the negative electrode side, it is possible to suppress the deterioration of charge / discharge performance due to high-rate current application. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-174648 A [Patent Document 2] JP 2017-10882 A [Patent Document 3] JP 2017-123236 A [Patent Document 4] JP 2016-66461 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in applications requiring high levels of battery performance, such as electric vehicles, further improvements in performance are always being sought, and therefore further improvements in the effects of the above-mentioned high-rate current application on the charge / discharge performance of secondary batteries, that is, improvements in so-called high-rate characteristics, are also being sought. [Means for solving the problem]
[0006] Various aspects of the secondary battery that solves the above problems will be described below. A first aspect is a secondary battery comprising an electrode body formed by winding positive and negative electrode sheets stacked with a separator in between, and each of the electrode sheets is formed by laminating an electrode mixture layer on a substrate that serves as a current collector, and when pressure is applied to the electrode mixture layer in the wound state for a predetermined time, if the weight of electrolyte flowing out from the electrode mixture layer per unit volume of the electrode mixture layer per unit pressure applied to the electrode mixture layer is defined as a fluidity index value of the electrolyte impregnated in the electrode mixture layer, the predetermined time for applying the pressure to the electrode mixture layer is 3 minutes and the fluidity index value of the electrolyte is expressed in "grams (@3 minutes) / kilopascal cubic millimeter", the fluidity index value of the positive electrode mixture layer minus the fluidity index value of the negative electrode mixture layer is 0.48 x 10^-6 or more.
[0007] According to the above configuration, even during high-rate current application, the salt concentration of the electrolyte is unlikely to be uneven between the positive electrode side and the negative electrode side. As a result, deterioration of the charge / discharge performance due to high-rate current application is suppressed. This makes it possible to improve the high-rate characteristics.
[0008] A second aspect of the secondary battery is the one according to the first aspect, wherein the flowability index value of the positive electrode mixture layer is 7.8×10^-7 or more and 8.8×10^-6 or less. A third aspect of the secondary battery is the battery according to the first aspect, wherein the positive electrode mixture layer has a thickness of 0.034 millimeters or more and 0.050 millimeters or less.
[0009] A fourth aspect of the secondary battery is the one according to the first aspect, wherein the fluidity index value of the negative electrode mixture layer is not less than 2.4×10^-6 and not more than 1.1×10^-5. A fifth aspect is the secondary battery according to the first aspect, wherein the negative electrode mixture layer has a thickness of 0.060 millimeters or more and 0.080 millimeters or less.
[0010] According to each of the above configurations, the high rate characteristics can be effectively improved. A sixth aspect of the present invention is the secondary battery according to any one of the first to fifth aspects, wherein the positive electrode mixture layer contains a conductive fibrous carbon material.
[0011] That is, by containing the fibrous conductive carbon material, many fine voids are formed in the positive electrode mixture layer, and this makes it possible to ensure high fluidity of the electrolyte impregnated in the positive electrode mixture layer. Effect of the Invention
[0012] According to the present invention, the high-rate characteristics can be improved. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a perspective view of a secondary battery. [Diagram 2] FIG. [Diagram 3] FIG. 2 is a side view of the secondary battery. [Figure 4] 2 is a schematic diagram showing the structure of a positive electrode mixture layer in the secondary battery of the present embodiment. FIG. [Diagram 5] FIG. 2 is a schematic diagram showing the structure of a positive electrode mixture layer in a secondary battery of a reference example. [Figure 6] FIG. 2 is a schematic diagram showing the arrangement of positive and negative electrodes and separators. [Figure 7] FIG. 2 is an explanatory diagram showing a process for preparing a sample used for measuring a liquid flow rate. [Figure 8] FIG. 2 is an explanatory diagram showing a process for preparing a sample used for measuring a liquid flow rate. [Figure 9]FIG. 4 is an explanatory diagram showing a method for measuring a liquid flow rate. [Figure 10] 1 is a flowchart showing a method for measuring the amount of electrolyte outflow. [Figure 11] FIG. 4 is an explanatory diagram showing a method for measuring a liquid flow rate. [Figure 12] FIG. 4 is an explanatory diagram showing the distribution of lithium ions in a secondary battery of a reference example in a non-energized state. [Figure 13] FIG. 4 is an explanatory diagram showing the distribution of lithium ions in a secondary battery of a reference example in a high-rate current-carrying state. [Figure 14] FIG. 4 is an explanatory diagram showing the distribution of lithium ions in a secondary battery of a reference example in a high-rate current-carrying state. [Figure 15] FIG. 2 is an explanatory diagram showing the distribution of lithium ions in the secondary battery of the present embodiment in a non-energized state. [Figure 16] FIG. 4 is an explanatory diagram showing the distribution of lithium ions in the secondary battery of the present embodiment in a high-rate current-carrying state. [Figure 17] FIG. 4 is an explanatory diagram showing the distribution of lithium ions in the secondary battery of the present embodiment in a high-rate current-carrying state. [Figure 18] 1 is a table showing the effect of the amount of liquid flow in the positive and negative electrode mixture layers on the high-rate characteristics of a secondary battery. [Figure 19] 1 is a graph showing the effect of the amount of liquid flow in the positive and negative electrode mixture layers on the high-rate characteristics of a secondary battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of a secondary battery and an electrode assembly thereof will be described with reference to the drawings. (Secondary battery) 1, the secondary battery 1 includes an electrode assembly 10 in which a positive electrode 3, a negative electrode 4, and a separator 5 are integrated, and a case 20 that houses the electrode assembly 10. The secondary battery 1 of this embodiment has a configuration as a lithium ion secondary battery in which the electrode assembly 10 in the case 20 is impregnated with a non-aqueous electrolyte solution (not shown).
[0015] More specifically, in the secondary battery 1 of this embodiment, the positive electrode 3, the negative electrode 4, and the separator 5 are laminated with a sheet-like outer shape. Then, by winding up the laminate of the positive electrode 3, the negative electrode 4, and the separator 5, an electrode body 10 is formed in which the positive and negative electrodes and the separators 5 are alternately arranged in the radial direction with the separator 5 sandwiched between the positive electrode 3 and the negative electrode 4.
[0016] The case 20 of this embodiment includes a case body 21 having a flat, substantially rectangular box shape, and a lid member 22 that closes an open end 21x of the case body 21. The electrode body 10 of this embodiment has a flat outer shape that corresponds to the box shape of the case 20.
[0017] (Electrode sheet and electrode body) More specifically, as shown in FIG. 2, in the secondary battery 1 of this embodiment, the positive electrode 3 and the negative electrode 4 each have a configuration as an electrode sheet 35 including a current collector 31 having a sheet-like outer shape and an electrode mixture layer 32 laminated on this current collector 31.
[0018] Specifically, for the electrode sheet 35P for the positive electrode 3, a composite paste 37P containing a lithium transition metal oxide serving as a positive electrode active material is applied onto a substrate 36P made of aluminum or the like that constitutes the positive electrode current collector 31P. For the electrode sheet 35N for the negative electrode 4, a slurry-like composite paste 37N containing a carbon-based material serving as a negative electrode active material is applied onto a substrate 36N made of copper or the like that constitutes the negative electrode current collector 31N. Furthermore, each of these composite pastes 37P and 37N contains a binder. In the secondary battery 1 of this embodiment, the composite pastes 37P and 37N are dried to form the corresponding positive electrode composite layer 32P and negative electrode composite layer 32N for the positive and negative electrode sheets 35P and 35N, respectively.
[0019] Furthermore, in the secondary battery 1 of this embodiment, the positive and negative electrode sheets 35P, 35N are each shaped into a belt-like shape. The electrode body 10 of this embodiment is configured such that the positive and negative electrode sheets 35P, 35N, which are stacked with the separator 5 sandwiched therebetween, are wound around a winding axis 10x extending in the width direction of the belt-like shape (the left-right direction in FIG. 2).
[0020] 2, the separator 5 and each electrode sheet 35 are wound in such a manner that the electrode sheet 35P constituting the positive electrode 3 is wound inward. However, this figure is one example showing the structure of the electrode body 10, and the separator 5 and each electrode sheet 35 may be wound in such a manner that the electrode sheet 35N constituting the negative electrode 4 is wound inward. This determines whether the electrode sheet 35 arranged on the outermost shell of the electrode body 10 is the electrode sheet 35P constituting the positive electrode 3 or the electrode sheet 35N constituting the negative electrode 4.
[0021] 1 to 3, the cover member 22 of the case 20 is provided with a positive electrode terminal 38P and a negative electrode terminal 38N that protrude to the outside of the case 20. Furthermore, each electrode sheet 35 has an uncoated portion 39 where the electrode mixture layer 32 is not formed on the current collector 31. The secondary battery 1 of this embodiment is configured such that the electrode sheet 35P constituting the positive electrode 3 and the positive electrode terminal 38P are electrically connected, and the electrode sheet 35N constituting the negative electrode 4 and the negative electrode terminal 38N are electrically connected, utilizing these uncoated portions 39.
[0022] Specifically, the electrode body 10 of this embodiment is housed in the case 20 with its winding axis 10x aligned along the longitudinal direction (left-right direction in FIG. 1) of the cover member 22, which is an elongated, generally rectangular plate. Furthermore, in this state, an uncoated portion 39P of an electrode sheet 35P constituting the positive electrode 3 is connected to a positive electrode terminal 38P via a connecting member 40P. Similarly, an uncoated portion 39N of an electrode sheet 35N constituting the negative electrode 4 is connected to a negative electrode terminal 38N via a connecting member 40N.
[0023] Furthermore, an electrolyte solution 50 is poured into the case 20. That is, the electrolyte solution 50 of the secondary battery 1 having a configuration as a lithium ion secondary battery is one in which a lithium salt serving as a supporting salt is dissolved in an organic solvent. Thus, the secondary battery 1 of this embodiment is configured such that the electrolyte solution 50 is impregnated into the electrode body 10 sealed in the case 20.
[0024] (High rate characteristics) As shown in Fig. 4, in the secondary battery 1 of this embodiment, the positive electrode composite layer 32P forming the electrode body 10 contains carbon nanotubes (CNT) as conductive fibrous carbon material 51. That is, the carbon nanotubes (CNT) are applied in the form of a composite paste 37P together with the positive electrode active material 52P onto the substrate 36P for the positive electrode 3 (see Fig. 2). As a result, the secondary battery 1 of this embodiment is configured such that the carbon nanotubes (CNT) dispersed in the positive electrode composite layer 32P function as a conductive material that forms a conductive path for the positive electrode active material 52P located in the vicinity thereof.
[0025] In addition, for example, when a granular material such as carbon black CB is contained as the conductive material in positive electrode mixture layer 32BP of the reference example shown in Fig. 5, positive electrode mixture layer 32BP has a dense structure, which tends to reduce the fluidity of electrolyte 50 impregnated in positive electrode mixture layer 32BP.
[0026] In contrast, in the secondary battery 1 of the present embodiment, many fine voids are formed in the positive electrode mixture layer 32P by containing fibrous carbon nanotubes CNT as shown in Fig. 4. As a result, the secondary battery 1 of the present embodiment has a configuration in which the electrolyte solution 50 impregnated in the positive electrode mixture layer 32P has high fluidity.
[0027] 6, in the secondary battery 1 of this embodiment, the positive electrode mixture layer 32P constituting the positive electrode 3 and the negative electrode mixture layer 32N constituting the negative electrode 4 each have their own thicknesses Dp, Dn. Furthermore, the positive electrode mixture layer 32P and the negative electrode mixture layer 32N each have their own fluidity index value indicating the fluidity of the impregnated electrolyte 50. The secondary battery 1 of this embodiment is configured to improve its high-rate characteristics by managing the thicknesses Dp, Dn of the positive electrode mixture layer 32P and the negative electrode mixture layer 32N and managing the fluidity index value of the impregnated electrolyte 50.
[0028] In detail, the secondary battery 1 of this embodiment has a so-called double-sided laminated structure in which the electrode mixture layer 32 is laminated on both sides of the sheet-shaped substrate 36 constituting the positive and negative electrode sheets 35. That is, in the secondary battery 1 of this embodiment, the one-side portion laminated on one of the two sides of the substrate 36 becomes the one-side thickness Dhp of the positive electrode mixture layer 32P and the one-side thickness Dhn of the negative electrode mixture layer 32N. Furthermore, the values obtained by multiplying each of these one-side thicknesses Dhp and Dhn become the two-side portions of the electrode mixture layer 32 laminated on the substrate 36, that is, the two-side thickness Ddp of the positive electrode mixture layer 32P and the two-side thickness Ddn of the negative electrode mixture layer 32N. The secondary battery 1 of this embodiment is configured to manage the values of each of these two-side thicknesses Ddp and Ddn as the thickness Dp of the positive electrode mixture layer 32P and the thickness Dn of the negative electrode mixture layer 32N, respectively.
[0029] Specifically, in the secondary battery 1 of this embodiment, the thickness Dp of the positive electrode composite layer 32P is controlled by adjusting the pressing pressure, speed, etc., when applying the composite paste 37P to the carbon nanotubes CNT, which serve as the conductive material, and the base material 36P.
[0030] For example, the secondary battery 1 of this embodiment uses carbon nanotubes CNTs having a specific surface area value of 150 or more and 300 or less using the BET method. The unit of this so-called BET specific surface area value is [m^2 / g] (square meters / gram). The pressing pressure is set to, for example, 40 kN or more and 100 kN or less. Furthermore, the coating speed is set to, for example, a range of 6 m or more and 120 m or less per minute. Thus, the secondary battery 1 of this embodiment is configured such that the thickness Dp of the positive electrode composite layer 32P is controlled to, for example, 0.034 mm or more and 0.050 mm or less.
[0031] In addition, in the secondary battery 1 of this embodiment, the thickness Dn of the negative electrode composite layer 32N is controlled by adjusting the binder and thickener added to the composite paste 37N together with the carbon-based material such as graphite, as well as the pressing pressure, coating speed, etc.
[0032] For example, in the secondary battery 1 of this embodiment, the binder added to the composite paste 37N is styrene-butadiene copolymer (SBR), styrene-acrylic copolymer (SAR), or the like, and the thickener is carboxymethyl cellulose (CMC), or the like.
[0033] The pressing pressure is set to, for example, 10 kN or more and 50 kN or less. Furthermore, the coating speed is set to, for example, 6 m or more and 120 m or less per minute. Thus, the secondary battery 1 of this embodiment is configured such that the thickness Dn of the negative electrode composite layer 32N is controlled to, for example, 0.060 mm or more and 0.080 mm or less.
[0034] Furthermore, in the secondary battery 1 of this embodiment, the thickness Dp of the positive electrode mixture layer 32P and the thickness Dn of the negative electrode mixture layer 32N are controlled, as well as their respective densities and porosities. For example, the density of the positive electrode mixture layer 32P is controlled to be 2.2 g / cc or more and 2.9 g / cc or less. The density of the negative electrode mixture layer 32N is controlled to be 0.9 g / cc or more and 1.2 g / cc or less. The porosity of the positive electrode mixture layer 32P is controlled to be 37% or more and 51% or less, for example. The porosity of the negative electrode mixture layer 32N is controlled to be 45% or more and 55% or less, for example.
[0035] In addition, for example, ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), etc. are used for the electrolytic solution 50 of this embodiment. Furthermore, the composition ratios of these are set, for example, as follows: EC=1, 1≦EMC≦1.5, 1≦DMC≦1.5. In this case, the specific gravity of the electrolytic solution 50 is in the range of 1.1 or more and 1.3 or less. Thus, the electrolytic solution 50 of this embodiment has a viscosity based on its composition.
[0036] In the secondary battery 1 of this embodiment, the liquid flow amount Q is used as the fluidity index value of the electrolyte 50 impregnated in the electrode mixture layer 32. Specifically, the liquid flow amount Q indicates the weight of the electrolyte 50 flowing out from the electrode mixture layer 32 per unit volume per unit pressure applied by applying pressure to the electrode mixture layer 32 in a state of being wound as the electrode sheet 35 for a predetermined time. Furthermore, in the secondary battery 1 of this embodiment, the liquid flow amount Q is expressed as [g(@3min) / kPa·mm^3] ("gram(@3min) / kilopascal·cubic millimeter"), assuming that the predetermined time for applying pressure to the electrode mixture layer 32 is 3 minutes. As a result, in the secondary battery 1 of this embodiment, the liquid flow amount Qp on the positive electrode 3 side has a value of 7.8×10^-7 or more and 8.8×10^-6 or less. In addition, "×10^-7" is "10 to the power of -7", and "×10^-6" is "10 to the power of -6" (hereinafter the same). The secondary battery 1 of this embodiment is configured so that the amount of liquid flow Qn on the negative electrode 4 side is 2.4×10^-6 or more and 1.1×10^-5 or less.
[0037] More specifically, the secondary battery 1 of this embodiment is configured so that the liquid flow rate Q, which is a fluidity index value of the electrolyte 50 impregnated in the electrode mixture layer 32, is larger on the positive electrode 3 side than on the negative electrode 4 side, as shown in the following formula.
[0038] Qp>Qn (1) Specifically, it is preferable that the value obtained by subtracting the amount of liquid flow Qn on the negative electrode 4 side from the amount of liquid flow Qp on the positive electrode 3 side satisfies the following formula (2).
[0039] Qp-Qn≧0.48×10^-6 (2) Furthermore, it is more preferable that the value obtained by subtracting the amount of liquid flow Qn on the negative electrode 4 side from the amount of liquid flow Qp on the positive electrode 3 side satisfies the following formula (3).
[0040] Qp-Qn≧0.66×10^-6 (3) Thus, the secondary battery 1 of this embodiment is configured to improve its high-rate characteristics.
[0041] (Method of measuring liquid flow rate) As shown in Figures 7 and 8, when measuring the liquid flow rate Q, samples 60 used for measuring the liquid flow rate Q are prepared from the positive and negative electrode sheets 35 that constitute the electrode body 10 of the secondary battery 1, respectively.
[0042] Specifically, first, a strip-shaped sample sheet 62 having a predetermined length L and a predetermined width W is cut out from the actual electrode sheet 35. Next, this sample sheet 62 is wound around a rod-shaped member 63, and the wound shape is fixed with a winding stop tape (not shown). Then, in this state, the rod-shaped member 63 around which the sample sheet 62 is wound is removed, thereby forming a measurement sample 60 having a wound body configuration similar to the electrode body 10 of the secondary battery 1.
[0043] 9, in the secondary battery 1 of this embodiment, the sample 60 formed as described above is placed in a measurement case 64 configured as a sealed container. In this state, pressure P is applied to the sample 60 for a predetermined time, and the weight of the electrolyte solution 50 flowing out from the electrode mixture layer 32 is measured.
[0044] Specifically, as shown in FIG. 10, first, the electrolyte 50 is filled in the case 64 containing the sample 60, so that the electrolyte 50 is impregnated into the sample 60, specifically, the electrode mixture layer 32 is impregnated with the electrolyte 50 (step 101). The hole of the sample 60 formed by removing the rod-shaped member 63 as described above is liquid-tightly sealed, for example, by inserting a rod-shaped rubber plug 65. Next, the electrolyte 50 in the case 64 is discharged, so that only the sample 60 impregnated with the electrolyte 50 is placed in the case 64 (step 102). Then, in this state, the inside of the case 64 is pressurized to a predetermined pressure P using a pressurizing device 66 connected to the case 64 (step 103).
[0045] Next, this pressurized state is maintained for a predetermined time t (step 104: NO). As described above, in the secondary battery 1 of this embodiment, the predetermined time t is "3 minutes." Furthermore, after the predetermined time t has elapsed (step 104: YES), the weight of the electrolyte 50 accumulated in the case 64, that is, the electrolyte 50 that has flowed out of the sample 60 due to the pressurization, is measured as the electrolyte outflow amount Fw (step 105). Then, in the secondary battery 1 of this embodiment, the liquid flow amount Qs per sample 60 is calculated based on the electrolyte outflow amount Fw measured in step 105.
[0046] More specifically, as shown in FIG. 11, in the secondary battery 1 of this embodiment, the measurement of the electrolyte outflow amount Fw by pressurization as described above is performed by changing the predetermined pressure P applied to the sample 60 in the case 64. For example, the first predetermined pressure P1 is set to "37 kPa", the second predetermined pressure P2 is set to "104 kPa", and the third predetermined pressure P3 is set to "165 kPa", and the measurement of the electrolyte outflow amount Fw by pressurization is performed for each of the pressures P1, P2, and P3, for example, without replacing the sample 60, and the pressurization measurements are performed for three minutes for each of the pressures P1, P2, and P3 in ascending order of pressure P. Then, the electrolyte outflow amounts Fw1, Fw2, and Fw3 obtained for each of the pressures P1, P2, and P3 are plotted on the XY coordinate system in association with each of the pressures P1, P2, and P3.
[0047] That is, the electrolyte outflow amount Fw, which is the weight of the electrolyte 50 that flows out of the sample 60 due to pressure, is a value corresponding to the predetermined pressure P applied to the sample 60. Therefore, as described above, by plotting the measurement results on the XY coordinate, a linear approximation (y=ax+b) showing this relationship is obtained. Then, in the secondary battery 1 of this embodiment, the liquid flow amount Qs per sample 60 expressed in [g(3min) / kPa] is calculated from the slope of this linear approximation.
[0048] Also, as shown in Figures 7 and 8, in the secondary battery 1 of this embodiment, the volume V of the electrode mixture layer 32 in the sample 60 is determined by the length L and width W of the sample sheet 62 constituting this sample 60, and the thickness D of the electrode mixture layer 32, as shown in the following formula.
[0049] V = D × L × W (4) Specifically, in the secondary battery 1 of this embodiment, the length L of the sample sheet 62 is set to "500 mm" and the width W is set to "55 mm". Furthermore, as described above, the liquid flow amount Q as a fluidity index value of the electrolyte 50 impregnated in the electrode mixture layer 32 constituting the electrode body 10 of the secondary battery 1 is expressed in "grams (@3 minutes) / kilopascals·cubic millimeters". In other words, the liquid flow amount Q is a value indicating the weight of the electrolyte 50 flowing out from the electrode mixture layer 32 per unit pressure and per unit volume when a pressure P is applied to the electrode mixture layer 32 in a state of being wound as the electrode sheet 35 for a predetermined time t. Therefore, the liquid flow amount Q as a fluidity index value is a value obtained by dividing the liquid flow amount Qs per sample 60 by the volume V of the electrode mixture layer 32 in the sample 60 as shown in the following formula.
[0050] Q = Qs / V (5) In the secondary battery 1 of this embodiment, by utilizing this, the liquid flow rate Q is measured as a fluidity index value of the electrolyte 50 impregnated in the electrode mixture layer 32 constituting the electrode body 10 of the secondary battery 1 through the steps shown in Figures 7 to 11 as described above.
[0051] (action) As in the secondary battery 1B of the reference example shown in Figs. 12 to 14, during high-rate current application, the salt concentration of the electrolyte 50 tends to vary between the positive electrode 3 and the negative electrode 4. That is, during high-rate discharge as shown in Fig. 13, the lithium ion concentration on the negative electrode 4 tends to be high. Also, during high-rate charging as shown in Fig. 14, the lithium ion concentration on the negative electrode 4 tends to be low. The resulting salt concentration variation increases the internal resistance, resulting in deterioration of the charge / discharge performance.
[0052] In this regard, in the secondary battery 1 of the present embodiment, as described above, the thicknesses Dp, Dn are managed for the positive electrode mixture layer 32P and the negative electrode mixture layer 32N constituting the electrode body 10. Furthermore, the liquid flow rates Qp, Qn, which are fluidity index values of the impregnated electrolyte 50, are managed for each of the positive electrode mixture layer 32P and the negative electrode mixture layer 32N.
[0053] 15 to 17, even during high-rate current application, the salt concentration of the electrolyte 50 is less likely to vary between the positive electrode 3 and the negative electrode 4. This in turn suppresses deterioration of the charge / discharge performance due to high-rate current application.
[0054] Next, the effects of this embodiment will be described. (1) The secondary battery 1 includes an electrode body 10 formed by winding an electrode sheet 35P for a positive electrode 3 and an electrode sheet 35N for a negative electrode 4, which are stacked with a separator 5 sandwiched therebetween. Each electrode sheet 35P, 35N is formed by stacking an electrode mixture layer 32 on a substrate 36 that serves as a current collector 31. When a pressure P is applied to the electrode mixture layer 32 for a predetermined time t in a wound state as the electrode sheet 35, the weight of the electrolyte 50 flowing out of the electrode mixture layer 32 per unit volume per unit pressure acting on the electrode mixture layer 32 is defined as a liquid flow rate Q. Furthermore, this liquid flow rate Q is defined as a fluidity index value of the electrolyte 50 impregnated in the electrode mixture layer 32. The liquid flow rate Q is expressed in "grams (@3 minutes) / kilopascals·cubic millimeters" assuming that the predetermined time t for applying the pressure P to the electrode mixture layer 32 is 3 minutes. Secondary battery 1 is configured so that the value (Qp-Qn) obtained by subtracting the liquid flow rate Qn of negative electrode mixture layer 32N from the liquid flow rate Qp of positive electrode mixture layer 32P is 0.48×10^-6 or more.
[0055] According to the above configuration, it is possible to suppress unevenness in the salt concentration that occurs in the electrolyte 50 impregnated in the electrode body 10 due to high-rate current application, and this makes it possible to improve the high-rate characteristics.
[0056] (2) The positive electrode mixture layer 32P has a liquid flow rate Qp of 7.8×10^-7 or more and 8.8×10^-6 or less. The positive electrode mixture layer 32P has a thickness Dp of 0.034 millimeters or more and 0.050 millimeters or less. The negative electrode mixture layer 32N has a liquid flow rate Qn of 2.4×10^-6 or more and 1.1×10^-5 or less, and the negative electrode mixture layer 32N has a thickness Dn of 0.060 millimeters or more and 0.080 millimeters or less. This can effectively improve the high-rate characteristics.
[0057] (3) Positive electrode mixture layer 32P contains carbon nanotubes CNT as conductive fibrous carbon material 51. That is, by containing fibrous carbon nanotubes CNT, many fine voids are formed in positive electrode mixture layer 32P, and this makes it possible to ensure high fluidity of electrolyte solution 50 impregnated in positive electrode mixture layer 32P.
[0058] The above embodiment can be modified as follows: The above embodiment and the following modifications can be combined with each other to the extent that no technical contradiction occurs.
[0059] In the above embodiment, the secondary battery 1 has a so-called double-sided laminated structure in which the electrode mixture layer 32 is laminated on both sides of the sheet-shaped substrate 36 constituting the positive and negative electrode sheets 35. For this reason, the double-sided thicknesses Ddp and Ddn of the positive electrode mixture layer 32P and the negative electrode mixture layer 32N are set to the thickness Dp of the positive electrode mixture layer 32P and the thickness Dn of the negative electrode mixture layer 32N, respectively. However, the present invention is not limited to this, and the positive and negative electrode sheets 35 may be applied to a configuration having a so-called single-surface layer structure in which the electrode mixture layer 32 is laminated only on one side of the substrate 36. In this case, the single-sided thickness Dhp of the positive electrode mixture layer 32P and the single-sided thickness Dhn of the negative electrode mixture layer 32N may be set to the thicknesses Dp and Dn of the positive electrode mixture layer 32P and the negative electrode mixture layer 32N.
[0060] In the above embodiment, the liquid flow rate Q, which is the fluidity index value of the electrolyte 50, is expressed in [g(@3min) / kPa·mm^3] ("gram(@3min) / kilopascal·cubic millimeter"). In this case, the positive electrode mixture layer 32P has a liquid flow rate Qp of 7.8×10^-7 or more and 8.8×10^-6 or less. The negative electrode mixture layer 32N has a liquid flow rate Qn of 2.4×10^-6 or more and 1.1×10^-5 or less. Furthermore, the positive electrode mixture layer 32P has a thickness Dp of 0.034 mm or more and 0.050 mm or less. And the negative electrode mixture layer 32N is set to be 0.060 mm or more and 0.080 mm or less. However, without being limited thereto, these values may be arbitrarily changed within a range that satisfies the relationship of the above formula (2). It is preferable that the range is within a range that satisfies the relationship of the above formula (3).
[0061] Furthermore, depending on the required level of high-rate characteristics, the range may be expanded to the extent that the relationship of the above formula (1) is satisfied. In other words, a configuration may be adopted in which "the fluidity index value of the electrolyte solution 50 impregnated in the electrode mixture layer 32 is greater on the positive electrode 3 side than on the negative electrode 4 side." In this case, for example, as the fluidity index value, an index value other than the liquid flow rate Q detailed in the above embodiment, such as a value including the concept of outflow rate, may be used.
[0062] The density and porosity of positive electrode mixture layer 32P and negative electrode mixture layer 32N may also be changed as desired. The pressing pressure, speed, and the like used when applying mixture paste 37 to substrate 36 may also be changed as desired. The conductive material, binder, and thickener may also be changed as desired.
[0063] In the above embodiment, the positive electrode mixture layer 32P contains carbon nanotubes CNT as the conductive fibrous carbon material 51. However, the present invention is not limited to this, and other conductive fibrous carbon materials such as carbon nanofibers (CNF) may be used as the conductive material. Furthermore, the specifications, such as the so-called BET specific surface area, may also be changed arbitrarily. In addition, the positive electrode mixture layer 32P does not necessarily contain such conductive fibrous carbon material 51.
[0064] In the above embodiment, the sample 60 used for measuring the liquid flow rate Q is formed using a sample sheet 62 having a length L of "500 mm" and a width W of "55 mm." However, this is not limiting, and the size of the sample sheet 62, i.e., the volume V of the electrode mixture layer 32 in the sample 60 formed using this sample sheet 62, may be changed arbitrarily.
[0065] In the above embodiment, when the amount of liquid flow Q is measured, the predetermined time t for applying pressure to the electrode mixture layer 32 is set to 3 minutes, and the amount of electrolyte outflow Fw, which is the weight of the electrolyte 50 that flows out of the sample 60 due to the pressure, is measured. However, the predetermined time t is not limited to this, and may be changed arbitrarily.
[0066] In the above embodiment, the first predetermined pressure P1 is set to "37 kPa", the second predetermined pressure P2 is set to "104 kPa", and the third predetermined pressure P3 is set to "165 kPa", and the electrolyte outflow amount Fw due to the pressurization is measured. The electrolyte outflow amounts Fw1, Fw2, and Fw3 obtained for the predetermined pressures P1, P2, and P3 are plotted on the XY coordinate system in association with the respective predetermined pressures P1, P2, and P3, thereby calculating the liquid flow amount Qs per sample 60. However, the present invention is not limited to this, and the electrolyte outflow amount Fw due to the pressurization may be measured twice, or four or more times. The value of the pressure P applied to the electrode mixture layer 32 of the sample 60 in each measurement may be changed arbitrarily.
[0067] In the above embodiment, the secondary battery 1 is configured as a lithium ion secondary battery, but the present invention is not limited to this and may be applied to a secondary battery 1 other than a lithium ion secondary battery.
[0068] The terminal shapes of the positive electrode terminal 38P and the negative electrode terminal 38N are not limited to the shapes shown in Fig. 1 and may be changed as desired. The shape of the case 20 that defines the outer shape of the secondary battery 1 is also not necessarily limited to a flat rectangular box shape and may be changed as desired, for example, to a cylindrical shape.
[0069] Next, the technical ideas that can be understood from the above embodiment and modified examples will be described. (i) An electrode body formed by winding positive and negative electrode sheets stacked with a separator in between, each of the electrode sheets being formed by stacking an electrode mixture layer on a substrate serving as a current collector, and in which the fluidity index value of the electrolyte impregnated in the electrode mixture layer is greater on the positive electrode side than on the negative electrode side. EXAMPLES
[0070] Examples will be described below to more specifically explain the configuration and effects of the present invention, but the present invention is not limited to these examples. 18 and 19 are a table and a graph listing test results regarding the effects of the liquid flow rates Qp, Qn of the positive electrode mixture layer 32P and the negative electrode mixture layer 32N that constitute the electrode body 10 on the high-rate characteristics of the secondary battery 1.
[0071] More specifically, columns (1) and (2) in the table show the liquid flow rates Qsp and Qsn on the positive electrode 3 side and the negative electrode 4 side for each sample 60 described in detail in the above embodiment. That is, in this characteristic test, the liquid flow rates Qsp and Qsn for each sample 60 are measured by the method described in detail in the above embodiment for each of "Example 1" to "Example 4" and "Comparative Example 1" to "Comparative Example 7". As a result, the liquid flow rates Qsp and Qsn for each sample 60 shown in columns (1) and (2) in the table are expressed in units of [g(3min) / kPa].
[0072] More specifically, in this characteristic test, the electrode mixture layer 32 of each sample 60 corresponding to "Example 1" to "Example 4" and "Comparative Example 1" to "Comparative Example 7" has its own thickness Dp, Dn. In the table, the thickness Dp of the positive electrode mixture layer 32P and the thickness Dn of the negative electrode mixture layer 32N shown in the specifications column (3) and (4) are both-side thicknesses Ddp, Ddn, respectively. In addition, each of these samples 60 is formed using a sample sheet 62 whose length L is "500 mm" and whose width W is "55 mm". That is, the electrode mixture layer 32 of each sample 60 in "Example 1" to "Example 4" and "Comparative Example 1" to "Comparative Example 7" has its own volume V based on the difference in its thickness D, as shown in formula (4) in the above embodiment. Furthermore, the values shown in columns (5) and (6) in the table are the liquid flow rates Qp, Qn per unit volume obtained by dividing the liquid flow rates Qsp, Qsn per sample 60 by the volume V specific to the electrode mixture layer 32 of each sample 60 using formula (5) above. As a result, the unit of each of these liquid flow rates Qp, Qn is [g(3min) / kPa mm^3].
[0073] Moreover, column (7) in the table is the value obtained by subtracting the value in column (6) from the value in column (5), i.e., the value obtained by subtracting the amount of liquid flow Qn on the negative electrode 4 side from the amount of liquid flow Qp on the positive electrode 3 side (Qp-Qn). Furthermore, the "resistance increase rate" was used as the evaluation index of the high-rate characteristics shown in column (8) in the table. That is, this resistance increase rate is the increase rate [%] of the internal resistance (CD-IR) after a charge-discharge cycle test was conducted in which charging and discharging were repeated for a certain period of time at a large current (several tens of amperes or more) corresponding to high-rate current. Therefore, the smaller the value of the high-rate characteristics shown in each figure, the smaller the deterioration of the charge-discharge performance due to high-rate current. In other words, it indicates that the battery has better high-rate characteristics.
[0074] As shown in FIGS. 18 and 19, in all of "Example 1" to "Example 4", the values shown in column (7) of the table are "positive". That is, the value obtained by subtracting the liquid flow rate Qn on the negative electrode 4 side from the liquid flow rate Qp on the positive electrode 3 side is "positive" (Qp - Q>0). That is, when comparing the liquid flow rates Qp and Qn, which are the fluidity index values of the electrolytic solution 50, the positive electrode 3 side is larger than the negative electrode 4 side (Qp>Qn). And in these "Example 1" to "Example 4", the "resistance increase rate (%)", which is the evaluation index value of the high rate characteristics, is respectively "107", "100", "107", "108", and all are excellent values.
[0075] In contrast, except for "Comparative Example 1", in all of "Comparative Example 2" to "Comparative Example 7", the value obtained by subtracting the liquid flow rate Qn on the negative electrode 4 side from the liquid flow rate Qp on the positive electrode 3 side is "negative" (Qp - Qn<0). That is, when comparing the liquid flow rates Qp and Qn, the positive electrode 3 side is smaller than the negative electrode 4 side (Qp<Qn). And in these "Comparative Example 2" to "Comparative Example 7", when the required level of the "resistance increase rate (%)", which is the evaluation index value of the high rate characteristics, is set to "114", all of their values are larger than the required level value. That is, as a result, a remarkable improvement effect on the high rate characteristics cannot be obtained. Incidentally, for "Comparative Example 1", although the value obtained by subtracting the liquid flow rate Qn on the negative electrode 4 side from the liquid flow rate Qp on the positive electrode 3 side is slightly "positive", its "resistance increase rate (%)" is "114".
[0076] Also, when comparing "Example 1" to "Example 4", "Example 1", "Example 3", and "Example 4" show particularly excellent high rate characteristics. Furthermore, when comparing these "Example 1" to "Example 4", the value shown in column (7) of the table is the smallest for "Example 2". And the value was "0.48×10^-6".
[0077] From the above test results, the relationship of formula (2) shown as the preferred numerical range in the above embodiment is derived. In other words, when the liquid flow rate Q is expressed in "grams (@3 min) / kilopascal·cubic millimeters", it can be confirmed that the preferred numerical range should be "Qp-Qn≧0.48×10^-6".
[0078] Furthermore, the test results of "Example 1" to "Example 4" also reveal the change in the effect of improving the high-rate characteristics when the value obtained by subtracting the liquid flow amount Qn on the negative electrode 4 side from the liquid flow amount Qp on the positive electrode 3 side is "positive."
[0079] In detail, in FIG. 19, an auxiliary line m1 is drawn based on the point where the "resistance increase rate (%)" which is an evaluation index of the high-rate characteristics is "114" and the value obtained by subtracting the liquid flow amount Qn on the negative electrode 4 side from the liquid flow amount Qp on the positive electrode 3 side is "0", and the point showing the test result of "Example 2". As a result, as the value obtained by subtracting the liquid flow amount Qn on the negative electrode 4 side from the liquid flow amount Qp on the positive electrode 3 side increases, a region where the high-rate characteristics are improved relatively sharply is confirmed. Also, in the same figure, a region where high high-rate characteristics are obtained is confirmed, as represented by the auxiliary line m2 based on each point showing the test results of "Example 1", "Example 3", and "Example 4". Furthermore, the intersection of these two auxiliary lines m1 and m2 shows the change point of the improvement effect of the high-rate characteristics. This change point is located at a position where, when the liquid flow rate Q is expressed in "grams (@3 minutes) / kilopascals·cubic millimeters", the value obtained by subtracting the liquid flow rate Qn on the negative electrode 4 side from the liquid flow rate Qp on the positive electrode 3 side is "0.66 x 10^-6".
[0080] From the above test results, the relationship of formula (3) shown as a more preferable numerical range in the above embodiment is derived. That is, it can be confirmed that the numerical range of "Qp-Qn≧0.66×10^-6" is appropriate. And, when the required level of high-rate characteristics is relatively loose, it is presumed that the preferable numerical range can be expanded to the range (Qp-Qn>0) shown in formula (1) by excluding "Comparative Example 1" by taking into account the measurement error.
[0081] In addition, in all of "Example 1" to "Example 4", the liquid flow amount Qp on the positive electrode 3 side is in the range of "7.8 x 10^-7" or more and "8.8 x 10^-6" or less. In all of "Example 1" to "Example 4", the thickness Dp of the positive electrode mixture layer 32P is in the range of "0.034 mm" or more and "0.050 mm" or less. In all of "Example 1" to "Example 4", the liquid flow amount Qn on the negative electrode 4 side is in the range of "2.4 x 10^-6" or more and "1.1 x 10^-5" or less. In all of "Example 1" to "Example 4", the thickness Dn of the negative electrode mixture layer 32N is in the range of "0.060 mm" or more and "0.080 mm" or less.
[0082] From the above, it can be confirmed that the liquid flow rate Qp and thickness Dp of the positive electrode mixture layer 32P, and the liquid flow rate Qn and thickness Dn of the negative electrode mixture layer 32N shown as preferred numerical ranges in the above embodiment are all appropriate. [Explanation of symbols]
[0083] 1…Secondary battery 3...Positive electrode 4...Negative electrode 5…Separator 10...Electrode body 31...Current collector 32…Electrode composite material layer 35P…Electrode sheet 35N…Electrode sheet 36...Base material 50...Electrolyte Q, Qp, Qn: Liquid flow rate (fluidity index value) t...Predetermined time P…pressure
Claims
1. The battery has an electrode body formed by winding positive and negative electrode sheets stacked with a separator sandwiched therebetween, Each of the electrode sheets is formed by laminating an electrode mixture layer on a substrate serving as a current collector, When pressure is applied to the electrode mixture layer for a predetermined time in a wound state as the electrode sheet, the weight of the electrolyte flowing out from the electrode mixture layer per unit volume of the electrode mixture layer per unit pressure applied to the electrode mixture layer is defined as a fluidity index value of the electrolyte impregnated in the electrode mixture layer, The predetermined time for applying the pressure to the electrode mixture layer is set to 3 minutes, When the fluidity index value of the electrolyte is expressed in "grams (@3 minutes) / kilopascals / cubic millimeter", A secondary battery in which a value obtained by subtracting the fluidity index value of the negative electrode mixture layer from the fluidity index value of the positive electrode mixture layer is 0.48×10^-6 or more.
2. The fluidity index value of the positive electrode mixture layer is 7.8×10^-7 or more and 8.8×10^-6 or less The secondary battery according to claim 1 .
3. 2. The secondary battery according to claim 1, wherein the positive electrode mixture layer has a thickness of 0.034 mm or more and 0.050 mm or less.
4. The fluidity index value of the negative electrode mixture layer is 2.4×10^-6 or more and 1.1×10^-5 or less The secondary battery according to claim 1 .
5. 2. The secondary battery according to claim 1, wherein the negative electrode mixture layer has a thickness of 0.060 mm or more and 0.080 mm or less.
6. The positive electrode mixture layer contains a conductive fibrous carbon material. The secondary battery according to any one of claims 1 to 5.
Citation Information
Patent Citations
Lithium secondary battery and process for producing same
WO2011036759A1
Lithium ion secondary battery
JP2016066461A
Secondary battery system
JP2017010882A
Nonaqueous electrolyte secondary battery
JP2017123236A
Power storage device
JP2017174648A