Composition and method for producing the same
A composition of polylactic acid, citric acid ester, and plant food residue addresses moldability and sensory issues in plant food residue-thermoplastic resin blends, maintaining high tensile properties and biodegradability.
Patent Information
- Application Number
- JP2023060553
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-17
AI Technical Summary
Existing compositions containing plant food residues and thermoplastic resins suffer from poor moldability, color issues, odor problems, and reduced elastic modulus, while polylactic acid compositions with plasticizers have improved flexibility but compromised rigidity.
A composition comprising polylactic acid, citric acid ester, and plant food residue, with a specific extrusion pressure difference ΔP of 25 bar or less, enhances moldability, sensory properties, and maintains high tensile modulus and elongation.
The composition achieves excellent moldability, biodegradability, and improved sensory properties, with a high tensile modulus and large tensile elongation, suitable for forming films or sheets.
Smart Images

Figure 2024147865000001 
Figure 2024147865000002
Abstract
Description
[Technical Field]
[0001] The present invention relates to a composition and a method for producing the composition, and in particular to a composition containing plant food residue and polylactic acid and a method for producing the composition. [Background technology]
[0002] Plastic molded products manufactured from petroleum resources and other raw materials are used in a wide range of applications, including food and beverage containers, various packaging materials such as sheets and films, cushioning materials, household goods, agricultural products, and other industrial materials. However, the mass consumption of plastic materials has led to global warming due to greenhouse gas emissions and the depletion of petroleum resources, which are important long-term issues that need to be addressed on a global scale.
[0003] Therefore, the use of biomass materials has been studied to reduce the amount of plastic materials used. For example, Patent Document 1 below discloses a thermoplastic starch composition obtained by blending a mixture containing 45 to 70% by weight of starch-containing agricultural waste based on the total composition, wherein the agricultural waste contains less than 50% starch by dry weight, 25 to 50% by weight of a thermoplastic synthetic polymer based on the total composition, 1 to 10% by weight of a plasticizer based on the total composition, and 1 to 5% by weight of a coupling agent based on the total composition; and the blending is carried out at a first temperature higher than room temperature. Furthermore, plastic materials are difficult to decompose in the natural environment after disposal, making them a cause of environmental pollution. In recent years, biodegradable plastics that decompose in the natural environment after disposal have been attracting attention. Polylactic acid has been investigated as such a biodegradable plastic. However, although polylactic acid has a high tensile modulus (rigidity), it has properties such as low flexibility and impact resistance, and its applications have been limited. Patent Document 2 listed below discloses the addition of a plasticizer to polylactic acid as a method of improving flexibility. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2015-511648 [Patent Document 2] Japanese Patent Publication No. 2020-117692 Summary of the Invention [Problem to be solved by the invention]
[0005] One example of biomass materials is vegetable food waste. One method for utilizing vegetable food waste is to mix it with a thermoplastic resin, such as polyester or polyolefin, to produce a thermoplastic composition. However, compositions containing vegetable food waste and a thermoplastic resin can have poor moldability and often have problems such as color or odor. Furthermore, when a plasticizer is mixed into polylactic acid, flexibility (tensile elongation) is improved, but the modulus of elasticity is significantly reduced, which limits the range of applications.
[0006] An object of the present invention is to provide a composition that has excellent moldability and excellent sensory properties such as color and odor, and further has excellent biodegradability, and that has a high tensile modulus and large tensile elongation. [Means for solving the problem]
[0007] This technology is Polylactic acid and Citrate esters, Plant food residues, A composition comprising: The composition may have a difference ΔP between the extrusion start pressure and the extrusion end pressure measured using a pressure increase tester under the following conditions of 25 bar or less. <Conditions for measurement using the above-mentioned pressure increase tester> Extruder diameter: 25mm Temperature: 200℃ Mesh: 100 mesh Amount of composition subjected to test: 200 g The citrate ester may include at least triethyl acetyl citrate or tributyl acetyl citrate. The plant food residue may be residue of a food material selected from the group consisting of vegetables, fruits, grains, coffee, and tea. The plant food residue may be a starch extract residue from vegetables or grains, a juice extract residue from fruits, a coffee or tea beverage extract residue, or a grain milling residue. The plant food residue may be primarily composed of residue pieces having a size of 5 mm or less. The plant food residue may include ground plant food residue. The composition may be a thermoplastic composition. The composition may be a composition that can be formed into a film or sheet. The composition may further contain at least a polyester-based resin or a polyolefin-based resin. The composition may contain the polylactic acid in an amount of 90% by mass or less relative to the mass of the composition. In addition, this technology: Polylactic acid and Citrate esters, Plant food residues, Also provided is a molded article comprising: The molded article may be a film or a sheet. In addition, this technology: dispersing vegetable food residue in a citric acid ester to produce a composite material containing the citric acid ester and the vegetable food residue; kneading the composite material with polylactic acid to produce a composition; Also provided is a method for making a composition comprising: The difference ΔP between the extrusion start pressure and the extrusion end pressure measured when the composition is measured using a pressure increase tester under the following conditions may be 25 bar or less. <Conditions for measurement using the above-mentioned pressure increase tester> Extruder diameter: 25mm Temperature: 200℃ Mesh: 100 mesh Amount of composition subjected to test: 200 g [Effects of the Invention]
[0008] The composition according to the present invention has excellent moldability and excellent sensory properties such as color and odor. Therefore, the composition according to the present invention is suitable for promoting the utilization of plant-based food residues. Furthermore, the composition according to the present invention can be molded into molded articles with high tensile modulus and large tensile elongation. Furthermore, since polylactic acid and plant-based food residues are biodegradable, the composition according to the present invention is also biodegradable and can contribute to the achievement of the SDGs. [Brief explanation of the drawings]
[0009] [Figure 1] FIG. 10 is a diagram for explaining an extrusion pressure difference ΔP. [Figure 2] FIG. 1 is a schematic diagram of a pressure rise tester used to measure the extrusion pressure difference ΔP. DETAILED DESCRIPTION OF THE INVENTION
[0010] Preferred embodiments for carrying out the present invention will be described below. Note that the embodiments described below are representative embodiments of the present invention, and the scope of the present invention is not limited to these embodiments.
[0011] The present invention will be described in the following order. 1. First embodiment (composition) 2. Second embodiment (method for producing the composition) 3. Working Example
[0012] 1. First embodiment (composition)
[0013] As mentioned above, a composition containing polylactic acid and a plasticizer has improved flexibility (tensile and physical properties), but may have a problem in terms of physical properties, such as a significant decrease in elastic modulus. Furthermore, compositions containing plant-based food residues and thermoplastic resins may have problems with moldability, color, odor, etc. These problems are particularly likely to occur when the content of plant-based food residues is increased.
[0014] The present inventors have found that by including polylactic acid, a citric acid ester, and vegetable food residue, it is possible to increase tensile elongation while maintaining a high tensile modulus (rigidity), and also to improve moldability and sensory properties such as color or odor. In one embodiment, the composition of the present invention includes polylactic acid, a citric acid ester, and vegetable food residue. Furthermore, when the composition of the present invention is measured using a pressure increase tester under specified conditions, the difference ΔP between the extrusion start pressure and the extrusion end pressure is 25 bar or less.
[0015] The composition of the present invention will be described in more detail below.
[0016] (1) Composition
[0017] (1-1) Polylactic acid
[0018] The composition of the present invention contains polylactic acid. Polylactic acid is a type of aliphatic polyester in which lactic acid is the basic unit and multiple lactic acid units are linked together to form a high molecular weight. Examples of such polylactic acid include poly(L-lactic acid) whose structural unit is L-lactic acid, poly(D-lactic acid) whose structural unit is D-lactic acid, poly(DL-lactic acid) whose structural units are L-lactic acid and D-lactic acid, mixtures of these, and random copolymers of L-lactic acid and D-lactic acid.
[0019] The polylactic acid contained in the composition of the present invention may be not only a polylactic acid homopolymer obtained by condensation polymerization of only a lactic acid component as a raw material monomer, but also a polylactic acid copolymer obtained by condensation polymerization of a lactic acid component and another monomer component copolymerizable with the lactic acid component as a raw material monomer.
[0020] Polylactic acid can be produced by a method of dehydrating polymerization of only a lactic acid component as a raw material monomer using an appropriate catalyst and an initiator, a method of dehydrating polymerization of a lactic acid component as a raw material monomer using an initiator and another monomer component copolymerizable with the lactic acid component, or a synthesis method utilizing an enzymatic reaction using lipase, etc. The other monomer component copolymerizable with the lactic acid component is not particularly limited, and examples thereof include oxyacids, dihydric alcohols or trihydric or higher polyhydric alcohols, aromatic hydroxy compounds, dicarboxylic acids or trivalent or higher polycarboxylic acids, and lactones.
[0021] Examples of hydroxy acids include glycolic acid, hydroxypropionic acid, hydroxybutyric acid, hydroxyvaleric acid, hydroxypentanoic acid, hydroxycaproic acid, hydroxybenzoic acid, and hydroxyheptanoic acid, and among these, glycolic acid and hydroxycaproic acid are preferred.
[0022] Examples of dihydric alcohols include ethylene glycol, propylene glycol, propanediol, butanediol, heptanediol, hexanediol, octanediol, nonanediol, decanediol, 1,4-cyclohexanedimethanol, neopentyl glycol, diethylene glycol, triethylene glycol, polyethylene glycol, and polytetramethylene glycol. Examples of trihydric or higher polyhydric alcohols include glycerin, trimethylolpropane, and pentaerythritol.
[0023] Examples of aromatic hydroxy compounds include hydroquinone, resorcinol, bisphenol A, and the like.
[0024] Examples of dicarboxylic acids include oxalic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, dodecanedioic acid, malonic acid, glutaric acid, cyclohexanedicarboxylic acid, terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid, bis(4-carboxyphenyl)methane, anthracenedicarboxylic acid, bis(4-carboxyphenyl)ether, and sodium 5-sulfoisophthalate. Examples of trivalent or higher polyvalent carboxylic acids include trimellitic acid and pyromellitic acid.
[0025] Examples of lactones include caprolactone, valerolactone, propiolactone, undecalactone, and 1,5-oxepan-2-one.
[0026] In addition, components other than lactic acid contained in polylactic acid can be copolymerized within a range that does not impair the inherent biodegradability of polylactic acid, but the amount ratio is preferably 20 mol % or less of all constituent components, more preferably 0 to 10 mol %, and even more preferably 0 to 5 mol %.
[0027] The melting point of polylactic acid is in the range of 160° C. to 170° C., and the glass transition temperature is in the range of 60° C. to 70° C. Furthermore, polylactic acid is biodegradable and can be composted, making it an environmentally friendly material.
[0028] The content of polylactic acid is preferably 75% by mass or more, more preferably 80% by mass or more, and even more preferably 85% by mass or more, based on the mass of the composition.
[0029] The content of polylactic acid is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 88% by mass or less, based on the mass of the composition.
[0030] (1-2) Citric acid ester
[0031] The composition of the present invention contains a citrate ester. Examples of the citrate ester include triethyl citrate (TEC), tributyl citrate (TBC), tris(2-ethylhexyl) acetyl citrate, triethyl acetyl citrate (ATEC), and tributyl acetyl citrate (ATBC). One citrate ester may be used alone, or two or more citrate esters may be used in combination. In the composition of the present invention, the citrate ester can function as a plasticizer. Preferably, the citrate ester contains at least triethyl acetyl citrate (ATEC) or tributyl acetyl citrate (ATBC).
[0032] In the composition of the present invention, from the viewpoint of lowering the temperature during extrusion such as twin-screw extrusion, the content of acetyl triethyl citrate (ATEC) is preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 11% by mass or more, relative to the mass of the composition.
[0033] In the composition of the present invention, from the viewpoint of lowering the temperature during extrusion such as twin-screw extrusion, the content of acetyl triethyl citrate (ATEC) is preferably 20% by mass or less, more preferably 18% by mass or less, and even more preferably 16% by mass or less, relative to the mass of the composition.
[0034] In the composition of the present invention, from the viewpoint of lowering the temperature during extrusion such as twin-screw extrusion, the content of acetyl tributyl citrate (ATBC) is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, relative to the mass of the composition.
[0035] In the composition of the present invention, from the viewpoint of lowering the temperature during extrusion such as twin-screw extrusion, the content of acetyl tributyl citrate (ATBC) is preferably 30% by mass or less, more preferably 28% by mass or less, and even more preferably 26% by mass or less, relative to the mass of the composition.
[0036] The citrate ester contained in the composition of the present invention may be a mixture of acetyl triethyl citrate (ATEC) and acetyl tributyl citrate (ATBC). In the case of a mixture of acetyl triethyl citrate (ATEC) and acetyl tributyl citrate (ATBC), the mixing ratio of acetyl tributyl citrate (ATBC) to acetyl triethyl citrate (ATEC) is preferably 12:1 to 12:5, more preferably 12:1.5 to 12:4, and even more preferably 12:2 to 12:3.
[0037] In the composition of the present invention, from the viewpoint of lowering the temperature during extrusion such as twin-screw extrusion, the content of the mixture of acetyl triethyl citrate (ATEC) and acetyl tributyl citrate (ATBC) is preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, based on the mass of the composition.
[0038] In the composition of the present invention, from the viewpoint of lowering the temperature during extrusion such as twin-screw extrusion, the content of the mixture of acetyl triethyl citrate (ATEC) and acetyl tributyl citrate (ATBC) is preferably 40% by mass or less, more preferably 37% by mass or less, and even more preferably 35% by mass or less, relative to the mass of the composition.
[0039] (1-3) Plant food residue
[0040] The composition of the present invention contains a plant food residue. The plant food residue may be a residue containing plant fiber. For example, the plant food residue may contain, for example, 10 g or more, preferably 15 g or more, more preferably 20 g or more, and even more preferably 30 g or more, 40 g or more, 50 g or more, or even 60 g or more, or 70 g or more, of dietary fiber per 100 g of dry weight of the residue. The dietary fiber content may be, for example, 99 g or less, 97 g or less, or 95 g or less, or even 90 g or less, 85 g or less, or 80 g or less, per 100 g of dry weight of the residue. Food residues with such high dietary fiber content are often difficult to mix with thermoplastic resins, but the use of plasticized starch allows them to be well dispersed in the composition, improving the quality of the composition.
[0041] The dietary fiber content per 100 g of dry weight of plant food residues is determined by freeze-drying the plant food residues, grinding them in a mill, and passing the ground material through a 0.8 mm mesh. Dietary fiber is extracted from the resulting product and measured according to the Prosky method (Prosky L et al., Determination of total dietary fiber in foods and food products, Collaborative study. J Assoc Off Anal Chem. 58:677-679, 1985).
[0042] The plant food residue may be, for example, residue of a food material selected from the group consisting of vegetables, fruits, grains, coffee, and tea. Various plant food residues may be used in the present invention.
[0043] In one embodiment, the plant food residue may be vegetable food residue, such as potato, root, legume, leafy, fruit, cruciferous, or leafy vegetable residue. Examples of the potatoes include potatoes, sweet potatoes, taro, and mountain potatoes. Examples of the root vegetables include sugar beets, radishes, carrots, and turnips. Examples of the pulses include soybeans, adzuki beans, broad beans, and green soybeans. Thus, the present invention can be applied to a variety of vegetable food waste.
[0044] In another embodiment, the plant food residue may be fruit food residue, which may be citrus, pome fruit, stone fruit, or berry residue. Citrus fruits include, for example, mandarins, grapefruits, and oranges. Pome fruits include apples and pears. Stone fruits include peaches and plums. Berries include grapes and blueberries. Thus, the present invention can be applied to various fruit food wastes.
[0045] In yet another embodiment, the plant food residue may be a cereal residue. The cereal residue may be rice, corn, barley (e.g., wheat, barley, or rye), or buckwheat residue. An example of the cereal residue is rice bran. In yet another embodiment, the plant food residue may be coffee or tea residue, such as coffee extract residue (e.g., coffee grounds) or tea extract residue (e.g., tea leaves). Thus, the present invention can also be applied to plant food residues other than vegetables or fruits.
[0046] In one embodiment, the plant food residue may be a starch extract residue derived from vegetables or grains, a juice extract residue derived from fruit, a coffee or tea beverage extract residue, or a grain milling residue (e.g., rice or wheat milling residue). In this embodiment, the vegetable may be any of the vegetables mentioned above, and may in particular be potatoes, root vegetables, or beans. In this embodiment, the grain may in particular be rice, corn, or wheat. In this embodiment, the fruit may be a citrus fruit, pome fruit, stone fruit, or berry, and in particular may be an apple or grape. The residue may include, for example, a skin portion. For example, if the residue is a potato residue, the residue may or may not include potato skin. Furthermore, if the residue is a fruit, the residue may or may not include fruit skin. These residues are generated in particularly large amounts during food manufacturing processes, and the compositions of the present invention are particularly suitable from the perspective of upcycling, as they can utilize such residues.
[0047] Preferably, the plant food residue may be a residue primarily composed of residue pieces having a size of 5 mm or less. Using a residue primarily composed of residue pieces having such a size contributes to improving the physical properties of the composition. In this specification, the term "residue primarily composed of residue pieces" may mean that, for example, 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, or 90% by weight or more of the total weight of the residue has a size of 5 mm or less. The residue primarily composed of residue pieces may be obtained, for example, by grinding the residue raw material. The type of grinding process may be appropriately selected by those skilled in the art depending on, for example, the type of residue raw material. That is, the plant-based food residue may include ground plant-based food residue. Grinding may result in the above-mentioned residue primarily composed of residue pieces having a size of 5 mm or less.
[0048] The plant food residue may preferably be a residue that has not been dried. The moisture content of the residue may be, for example, preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and even more preferably 30% by mass or more. In certain embodiments, the moisture content may be 50% by mass or more. The moisture content is measured by loss on drying. Using the plant food residue in this moist state to produce a composition (particularly a residue-containing composite material (masterbatch) containing polylactic acid, a citric acid ester, and the plant food residue) is particularly preferable because it allows the polylactic acid and the plant food residue to be mixed and improves the moldability and sensory properties of the composition. Furthermore, because the plant food residue is not dried, no drying treatment is required, thereby reducing thermal energy and other factors. That is, the plant food residue may be used to produce the masterbatch using a wet method. The lower limit of the moisture content of the residue is not particularly limited, but may be, for example, preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 80% by mass or less.
[0049] (1-4)Thermoplastic resin
[0050] The composition may contain a thermoplastic resin. The thermoplastic resin may contain at least a polyester-based resin or a polyolefin-based resin. The composition according to the present invention may contain a polyester-based resin, a polyolefin-based resin, or both. The thermoplastic resin may also be a polystyrene-based resin. The thermoplastic resin may also contain a biodegradable material so as not to reduce biodegradability.
[0051] The composition may contain the thermoplastic resin in an amount, for example, preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, relative to the mass of the composition, and preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 8% by mass or more, relative to the mass of the composition.
[0052] In the present embodiment, the type of thermoplastic resin may be appropriately selected by a person skilled in the art depending on, for example, the application of the molded article to be molded from the composition, and a thermoplastic resin with a low processing temperature is preferred. For example, in the case of a sheet used for food packaging containers, the thermoplastic resin may be, for example, preferably a polyolefin resin, more preferably a polyethylene resin or a polypropylene resin.
[0053] In this embodiment, the melting point of the thermoplastic resin is preferably 170°C or lower, and more preferably 165°C or lower. By using a thermoplastic resin with a lower melting point, the molding temperature can be lowered. The melting point of the thermoplastic resin is preferably 90°C or higher, and more preferably 95°C or higher.
[0054] (1-5) Other ingredients
[0055] The composition of the present invention may further contain other components, such as high-melting point additives.
[0056] The composition of the present invention may also contain a high-melting additive having a melting point lower than that of the thermoplastic resin and higher than that of a low-melting additive that melts at a relatively low temperature. Such a high-melting additive may have a melting point preferably in the range of 100 to 150°C and lower than that of the thermoplastic resin. Examples of such high-melting additives include fatty acid metal salts, hydrocarbons, higher alcohols, aliphatic amides, and fatty acid esters. Specific examples of such high-melting additives include magnesium stearate, zinc stearate, calcium stearate, aluminum stearate, sodium lauryl sulfate, magnesium lauryl sulfate, potassium benzoate, sodium benzoate, and sodium stearyl fumarate.
[0057] The high-melting point additive may be contained, for example, in an amount of preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 6% by mass or less, relative to the mass of the composition. The high-melting point additive may be contained, for example, in an amount of preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more, relative to the mass of the composition.
[0058] As another additive, a compatibilizer may be included in the composition of the present invention to improve the compatibility of the polylactic acid, citric acid ester, vegetable food residue, and thermoplastic resin. The compatibilizer may be selected depending on the type of thermoplastic resin. Examples of such compatibilizers include acid-modified polyolefins, acid-modified nylons, acid-modified polystyrenes, acid-modified EVAs, acid-modified ethylene copolymers, acid-modified acrylates, acrylic acid-modified EVAs, and modified ethylene acrylates.
[0059] When the thermoplastic resin is a polyolefin-based resin, the compatibilizer is preferably an acid-modified polyolefin, in particular a carboxylic acid anhydride-modified polyolefin or an olefin-based comonomer.
[0060] The carboxylic acid anhydride constituting the carboxylic acid anhydride-modified polyolefin may preferably be maleic anhydride. The compatibilizer may be, for example, a maleic anhydride-grafted polyolefin resin, more particularly, one or a combination of two or more selected from the group consisting of maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, and maleic anhydride-modified ethylene-propylene copolymer. A rubber component may be dispersed in the compatibilizer.
[0061] The compatibilizer may be contained in the composition at a content of, for example, preferably 0.5% by mass to 5% by mass, more preferably 1% by mass to 4.5% by mass, and even more preferably 1.5% by mass to 4% by mass, relative to the mass of the composition.
[0062] As other additives, colorants may be used.
[0063] Colorants may be used to impart color to the composition and may include, for example, titanium dioxide, carbon black, dyes, and pigments.
[0064] Furthermore, the other components may include, for example, an antioxidant, a crosslinking agent, an ultraviolet absorber, a foaming agent, an impact resistance agent, etc. Commercially available additives may be used as these additives.
[0065] (2) Physical properties
[0066] (2-1) The difference ΔP between the extrusion start pressure and the extrusion end pressure measured using a pressure rise tester
[0067] The composition of the present invention may have a difference ΔP between the extrusion start pressure and the extrusion end pressure measured when the composition is measured using a pressure increase tester under the following conditions, of preferably 25 bar or less, more preferably 20 bar or less, even more preferably 18 bar or less, 14 bar or less, or 12 bar or less, and particularly preferably 10 bar or less, 8 bar or less, or 6 bar or less. The difference ΔP may be, for example, -1 bar or more, -0.5 bar or more, -0.3 bar or more, or 0 bar or more. The measurement method will be described below.
[0068] When the extrusion pressure of a composition is measured using a pressure increase tester described below, a graph such as that shown in Figure 1 can be obtained. This graph is a schematic example of a graph in which pressure is plotted against time. The extrusion pressure difference ΔP measured for the composition is the extrusion start pressure P when the extrusion pressure of the base polylactic acid (trade name "REVODE110", manufactured by Zhejiang Hishi Biomaterials Co., Ltd.) reaches equilibrium (pressure change in the last 5 minutes is within ±0.5%). start and the extrusion end pressure P 600 seconds after the start of extrusion endIt is an index that shows the pressure difference between the mesh and the surface. It is expressed in units of bar. In other words, it can be used as an index to show the level of particles contained in the composition. The lower this value, the less likely it is that the mesh will become clogged.
[0069] The extrusion pressure difference ΔP is measured using a pressure rise tester "LFT44-GP" (manufactured by Labotec Co., Ltd.).
[0070] The extrusion pressure difference ΔP is measured by the following procedure. FIG. 2 is a schematic diagram showing an example of a pressure increase tester used to measure the extrusion pressure difference ΔP for the composition according to this embodiment. The pressure increase tester 40 shown in FIG. 2 includes a single-screw extruder 43, a gear pump 42, and a mesh 41. In the pressure increase tester 40, the gear pump inlet pressure P1 and the gear pump outlet pressure P2 are measured. When measuring the extrusion pressure difference ΔP, the rotation speed of the gear pump 42 is set to a constant 30 RPM, the gear pump inlet pressure P1 is set to 50 bar, and the rotation speed of the single-screw extruder 43 is controlled in conjunction with the above to maintain P1 at 50 bar, and the gear pump outlet pressure P2 is measured. The extrusion pressure difference ΔP is measured by the following procedure. (i) As shown in FIG. 2, a 100-mesh (nominal mesh size: 0.154 mm, void ratio: 37%) mesh 41 is installed, and a pressure increase tester 40 capable of monitoring the extrusion pressure is used to extrude the base polylactic acid. After the extrusion pressure reaches equilibrium (a state in which the pressure change over the last 5 minutes is within ±0.5%) at the gear pump outlet pressure P2 of the pressure increase tester 40, the pressure increase tester 40 capable of monitoring the extrusion pressure is set at a temperature of 200°C, and extrusion of 200 g of the composition is initiated. (ii) The extrusion start pressure P2 at the gear pump outlet side pressure of the pressure increase tester 40 shown in FIG. 2 when the extrusion pressure reaches an equilibrium state (a state in which the pressure change in the last 5 minutes is ±0.5% or less). start Measure. (iii) After all 200 g of the composition is extruded from the pressure increase tester 40, the base polylactic acid is used. The extrusion end pressure P2 is measured at the time when the pressure at the gear pump outlet side P2 reaches an equilibrium state (a state in which the pressure change in the last minute is ±0.5% or less). end Measure. (iv) Calculate the extrusion pressure difference ΔP using the following formula. Extrusion pressure difference ΔP=P end -P start
[0071] (2-2) Tensile properties
[0072] The molded article obtained by molding the composition according to the present invention has a tensile modulus, which is a tensile property, of preferably 1.5 GPa or more, more preferably 1.7 GPa or more, and even more preferably 2.0 GPa or more. The upper limit of the tensile modulus is not particularly limited, but the tensile modulus is preferably 3 GPa or less, more preferably 2.8 GPa or less, and even more preferably 2.5 GPa or less.
[0073] The molded article has a tensile property of preferably 8% or more, more preferably 50% or more, and even more preferably 80% or more. The upper limit of the tensile elongation is not particularly limited, but the tensile elongation is preferably 200% or less, more preferably 180% or less, and even more preferably 150% or less.
[0074] The molded article has a tensile strength, which is a tensile property, of preferably 30 MPa or more, more preferably 40 MPa or more, and even more preferably 50 MPa or more. Although there is no particular upper limit to the tensile strength, the tensile strength is preferably 60 MPa or less, more preferably 58 MPa or less, and even more preferably 55 MPa or less.
[0075] The tensile properties can be measured, for example, according to JIS K 7161. Carrot residue is dispersed in citric acid ester, and polylactic acid is added to the dispersion. The resulting mixture is fed into a twin-screw extruder (model PCM30, manufactured by Ikegai Corporation) and melt-kneaded (the melting temperature is appropriately set within the range of 115 to 155°C depending on the sample) to produce pellets. The pellets are heat-pressed at 180°C using a heat press machine (manufactured by LAB TECH Engineering Co., Ltd.) to produce a sheet. The tensile properties are measured according to JIS K 7161 using a Tensilon universal testing machine (manufactured by A&D Co., Ltd.).
[0076] (2-3) Formability
[0077] The composition according to the present invention may be a composition that can be molded into a film or sheet. A molded body formed by molding the composition according to the present invention comprises polylactic acid, a citric acid ester, and a plant food residue. In particular, the composition according to the present invention may be a thermoplastic composition, i.e., a composition that can be molded when heat is applied. The composition according to the present invention may be molded into, for example, a film or sheet shape. The composition according to the present invention may also be in the form of pellets.
[0078] 2. Second embodiment (method for producing the composition)
[0079] The composition of the present invention can be produced through a dispersion step and a kneading step as follows. By producing the composition through these two steps, a composition having a pressure difference ΔP within the above-mentioned numerical range can be obtained.
[0080] (1) Dispersion process
[0081] In the dispersion step, wet vegetable food residue is dispersed in a citric acid ester to produce a composite material containing vegetable food residue and a citric acid ester. The dispersion method is not particularly limited, and examples include media mills such as ball mills, bead mills, and sand grinders, pressure-type dispersers such as high-pressure homogenizers and ultra-high-pressure homogenizers, and ultrasonic dispersers. Dispersion conditions such as dispersion temperature, dispersion time, and rotation speed can also be appropriately set.
[0082] (2) Mixing process
[0083] In the kneading step, the plant food residue dispersed in the citric acid ester (the composite material) is mixed with polylactic acid. The plant food residue dispersed in the citric acid ester and polylactic acid may be mixed using a mixer such as a high-temperature stirrer, a Henschel mixer, a tumbler mixer, a Barbary mixer, or a kneader mixer. The mixing may be performed at room temperature.
[0084] The mixture obtained by the mixing is subjected to a heat treatment. The heat treatment may be carried out as a kneading treatment using an extruder. The kneading treatment may be carried out using, for example, a single-screw kneading extruder or a twin-screw kneading extruder. As these kneading extruders, devices known in the technical field may be used. Preferably, the mixing and heating step includes at least heating and kneading treatment using a twin-screw kneading extruder. As the twin-screw kneading extruder, a co-rotating twin-screw kneading extruder or a counter-rotating twin-screw kneading extruder may be used. By performing the kneading treatment using a twin-screw kneading extruder, a composition can be obtained as a kneaded product in which the raw materials are more uniformly dispersed. In the mixing and heating step, the mixture is heat-treated at a temperature of 130°C or less. The temperature condition may be appropriately selected by a person skilled in the art depending on the type and content of the citric acid ester used.
[0085] In the kneading step, for example, when the citric acid ester is acetyl triethyl citrate (ATEC), the heat treatment is preferably carried out at 100° C. or higher, more preferably 110° C. or higher, even more preferably 115° C. or higher, and even more preferably 120° C. or higher. The heat treatment is also preferably carried out at 130° C. or lower, preferably 125° C. or lower, and more preferably 123° C. or lower.
[0086] In the kneading step, for example, when the citrate ester is acetyl tributyl citrate (ATBC), the heat treatment may be carried out at preferably 100° C. or higher, more preferably 110° C. or higher, even more preferably 115° C. or higher, and even more preferably 120° C. or higher. The heat treatment may be carried out at 130° C. or lower, preferably 125° C. or lower, and more preferably 123° C. or lower.
[0087] In the kneading step, for example, when the citrate ester is a mixture of acetyl triethyl citrate (ATEC) and acetyl tributyl citrate (ATBC), the heat treatment is preferably carried out at 100° C. or higher, more preferably 110° C. or higher, even more preferably 115° C. or higher, and even more preferably 120° C. or higher. The heat treatment is also preferably carried out at 130° C. or lower, preferably 125° C. or lower, and more preferably 123° C. or lower.
[0088] In the kneading step, for example, when an extruder is used, the composition is discharged from the extruder. The composition may have, for example, a columnar shape (particularly, a cylindrical shape). The cross-sectional dimension of the columnar shape (particularly, the cross-sectional diameter of the cylindrical shape) may be, for example, 2 mm to 10 mm, particularly 3 mm to 8 mm, and more particularly 4 mm to 6 mm. The composition may be, for example, in the form of strands. The composition may be, for example, transparent or translucent. The columnar composition may be cut into pellets, for example, using a pelletizer. That is, the composition may have a pellet shape. Alternatively, the composition does not necessarily have to have a columnar shape, but may have, for example, a cake shape, especially a wet cake shape. The composition may also be optionally ground for combination with a thermoplastic resin.
[0089] (3) Molding process
[0090] The production method may or may not include a molding step of molding the composition obtained through the above (1) dispersion step and (2) kneading step. The molding method used in the molding step may be appropriately selected by those skilled in the art depending on the shape or type of the desired molded product. For example, the molding step may involve processing to obtain a film or sheet-like molded product. To obtain the molded product, for example, inflation molding, injection molding, extrusion molding, or stretch molding may be performed.
[0091] 3. Working Example
[0092] The present invention will be described in more detail below with reference to examples. Note that the examples described below are representative examples of the present invention, and the scope of the present invention is not limited to these examples.
[0093] The evaluation methods used in the examples are described below, followed by a description of each composition.
[0094] (1) Evaluation method
[0095] (1-1) Pressure increase test
[0096] Each composition was fed into a pressure rise tester (LABTECH ENGINEERING, extruder diameter 25 mm, temperature 200°C) and a pressure rise test was carried out. The pressure rise test was carried out at 200°C using a 100 mesh, and the pressure difference ΔP between the start and end of the measurement was measured. The pressure difference ΔP was measured as described in "(2) Physical Properties" in 1 above.
[0097] (1-2) Tensile properties
[0098] The tensile properties were measured as described in 1. "(2) Physical Properties" above.
[0099] (1-3) Moldability (blowing)
[0100] Each composition was fed to an inflation molding machine (Placo Corporation, die Φ65, extruder diameter 55 mm, temperature 150°C) and inflation molding was carried out. The inflation molding was carried out at 150°C to 160°C. A film with a thickness of 50 μm was obtained by the inflation molding. The films obtained by the inflation molding were evaluated according to the following criteria. <Evaluation criteria> A: Inflation molding was possible, and the resulting film had no tears and a uniform appearance. B: Inflation molding was possible and the resulting film had no breaks, but agglomerates were observed in some parts of the film. C: Inflation molding was not possible due to factors such as holes.
[0101] Test Example 1: Production of composition (first embodiment)
[0102] [Example 1]
[0103] Carrot residue was prepared. The carrot residue was a pomace produced during the extraction of carrot starch, i.e., a residue of starch extraction derived from carrots. The carrot residue was pulverized to a size of 5 mm or less. The carrot residue was moist because it was not dried. The carrot residue was moist enough that moisture adhered to the hand when touched.
[0104] The components were prepared so that the carrot residue content was 10% by mass (content of dried carrot residue) and the acetyl tributyl citrate content (manufactured by Taoka Chemical Co., Ltd.) was 22.2% by mass in the composition. These two components were mixed, and the carrot residue was dispersed in the acetyl tributyl citrate. Polylactic acid (trade name "REVODE110", manufactured by Zhejiang Haizheng Biomaterials Co., Ltd.) was dry-blended so that the polylactic acid content was 67.8% by mass. The dry-blending was carried out at room temperature.
[0105] The mixture obtained by the dry blending was fed into a twin-screw extruder (PCM30, Ikegai Corporation), and these components were subjected to a kneading treatment. The cylinder temperature during the kneading treatment was 120°C.
[0106] The mixture was extruded through the die of the extruder, and elongated, roughly cylindrical pellets were obtained. Through this kneading process, pellets of a composition (hereinafter also referred to as "the composition of Example 1") were obtained.
[0107] The composition of Example 1 was supplied to a pressure rise tester (LABTECH ENGINEERING, extruder diameter 25 mm, temperature 200°C), and a pressure rise test was carried out as described above to measure the pressure difference ΔP. ΔP was 20.1 bar.
[0108] Pellets of the composition of Example 1 were fed into a heat press (manufactured by LAB TECH Engineering Co., Ltd.) and then heat pressed. The heat pressing was carried out at 180° C. A sheet having a thickness of 500 μm was obtained by the heat pressing.
[0109] The tensile modulus, tensile elongation, and tensile strength of the obtained sheet were measured according to the methods described in Embodiment 1. The obtained sheet had a tensile modulus of 1.5 GPa, a tensile elongation of 86.7%, and a tensile strength of 20.8 MPa. The moldability was rated A.
[0110] [Example 2]
[0111] Pellets of the composition (hereinafter also referred to as "the composition of Example 2") were obtained in the same manner as in Example 1, except that the content of carrot residue in the composition was 15 mass% (content of dried carrot residue) and the content of polylactic acid (product name "REVODE110", manufactured by Zhejiang Haizheng Biomaterials Co., Ltd.) was 62.8 mass%.
[0112] The composition of Example 2 was subjected to a pressure rise test in the same manner as in Example 1 to measure the pressure difference ΔP, which was 6.0 bar.
[0113] Pellets of the composition of Example 2 were hot pressed in the same manner as in Example 1 to obtain a sheet having a thickness of 500 μm.
[0114] The tensile modulus, tensile elongation, and tensile strength of the obtained sheet were measured by the same methods as in Example 1. The tensile modulus, tensile elongation, and tensile strength of the obtained sheet were 2.6 GPa, 8.3%, and 29.8 MPa. The moldability was rated A.
[0115] [Comparative Example 1]
[0116] Carrot residue was prepared. The carrot residue was the pomace produced during the carrot starch extraction process, i.e., the residue of starch extraction derived from carrots. The carrot residue was pulverized to a size of 5 mm or less and dried. In this way, a dry powder of carrot residue was prepared.
[0117] Pellets of the composition (hereinafter also referred to as "composition of Comparative Example 1") were obtained in the same manner as in Example 1, except that the content of dried carrot residue in the composition was 10% by mass, the content of polylactic acid (product name "REVODE110", manufactured by Zhejiang Haizheng Biomaterials Co., Ltd.) was 90% by mass, and the content of citric acid ester was 0% by mass.
[0118] The composition of Comparative Example 1 was subjected to a pressure rise test in the same manner as in Example 1 to measure the pressure difference ΔP, which was 49.8 bar.
[0119] Pellets of the composition of Comparative Example 1 were hot pressed in the same manner as in Example 1 to obtain a sheet having a thickness of 500 μm.
[0120] The tensile modulus, tensile elongation, and tensile strength of the obtained sheet were measured by the same methods as in Example 1. The obtained sheet had a tensile modulus of 3.5 GPa, a tensile elongation of 1.0%, and a tensile strength of 27.6 MPa.
[0121] (2) Evaluation results
[0122] As shown in the evaluation results for Comparative Example 1, the composition containing no citrate ester had poor moldability due to a high pressure difference ΔP.
[0123] In Examples 1 and 2, the pressure difference ΔP was high, and therefore the moldability was excellent.
[0124] The configurations, methods, steps, shapes, materials, and values given in the above-described embodiments and examples are merely examples, and different configurations, methods, steps, shapes, materials, and values may be used.
[0125] Furthermore, the configurations, methods, steps, shapes, materials, numerical values, etc. of the above-described embodiments and examples can be combined with one another without departing from the spirit of the present invention.
[0126] Furthermore, in this specification, a numerical range indicated using "to" indicates a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively. In numerical ranges described in stages in this specification, the upper or lower limit of a numerical range in a certain stage may be replaced with the upper or lower limit of a numerical range in another stage. Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more types.
Claims
1. Polylactic acid, Citrate esters, Plant food residues; A composition comprising:
2. The composition according to claim 1, wherein the difference ΔP between the extrusion start pressure and the extrusion end pressure measured when the composition is measured using a pressure increase tester under the following conditions is 25 bar or less. <Conditions for measurement using the voltage boost tester> Extruder diameter: 25 mm Temperature: 200℃ Mesh: 100 mesh Amount of composition subjected to test: 200 g
3. 2. The composition of claim 1, wherein the citrate ester comprises at least acetyl triethyl citrate or acetyl tributyl citrate.
4. 2. The composition of claim 1, wherein the plant-based food residue is a residue of a food material selected from the group consisting of vegetables, fruits, grains, coffee, and tea.
5. 2. The composition of claim 1, wherein the plant-based food residue is a starch extract residue from vegetables or cereals, a juice extract residue from fruit, a coffee or tea beverage extract residue, or a grain milling residue.
6. The composition of claim 1 , wherein the plant food residue is comprised primarily of residue pieces having a size of 5 mm or less.
7. The composition of claim 1 , wherein the plant food residue comprises ground plant food residue.
8. The composition of claim 1 , wherein the composition is a thermoplastic composition.
9. The composition of claim 1 , wherein the composition is a composition that can be formed into a film or sheet.
10. The composition according to claim 1 , further comprising at least a polyester-based resin or a polyolefin-based resin.
11. The composition according to claim 1 , comprising the polylactic acid in an amount of 90% by mass or less based on the mass of the composition.
12. Polylactic acid, Citrate esters, Plant food residues; A molded body comprising:
13. The molded article according to claim 12, which is a film or a sheet.
14. Dispersing a vegetable food residue in a citric acid ester to produce a composite material containing the citric acid ester and the vegetable food residue; kneading the composite material with polylactic acid to produce a composition; A method for producing a composition comprising:
15. The method for producing a composition according to claim 14, wherein the difference ΔP between the extrusion start pressure and the extrusion end pressure measured when the composition is measured using a pressure increase tester under the following conditions is 25 bar or less. <Conditions for measurement using the voltage boost tester> Extruder diameter: 25 mm Temperature: 200℃ Mesh: 100 mesh Amount of composition subjected to test: 200 g
Citation Information
Patent Citations
Thermoplastic starch composition obtained from agricultural waste
JP2015511648A
Resin composition and tubular molded body obtained by molding the same
JP2020117692A