Laminate, electrode structure, battery, aircraft, method for manufacturing laminate, and method for manufacturing electrode structure

The laminate structure with thermoplastic resin support layers and integrated metal layers stabilizes metal layers, reducing electrical resistance variations and enhancing battery safety and energy density for high-performance applications.

JP2024149278AActive Publication Date: 2024-10-18SOFTBANK CORPORATION
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023063059
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-18
Estimated Expiration
2043-04-07

AI Technical Summary

Technical Problem

Existing methods for integrating metal layers in laminates used in battery electrodes result in high electrical resistance variations and potential breakage, leading to reduced battery performance and safety concerns.

Method used

A laminate structure with thermoplastic resin support layers and metal layers featuring bellows-like or wrinkled shapes, integrated with conductive members, to stabilize the metal layers and reduce electrical resistance variations.

Benefits of technology

The laminate structure enhances battery safety by preventing thermal runaway and improves energy density, making it suitable for high-performance applications such as aircraft batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149278000001_ABST
    Figure 2024149278000001_ABST
Patent Text Reader

Abstract

To provide a laminate for realizing a rechargeable battery capable of improving the amount of energy per weight and storing more power with less weight.SOLUTION: A laminate is provided that includes a plurality of stacked sheet materials. In the laminate, each of the plurality of sheet materials has a support layer including a thermoplastic resin material, and a first metal layer and a second metal layer formed on both sides of the support layer. In some of the plurality of sheet materials, the plurality of first metal layers and the plurality of second metal layers included in the plurality of sheet materials are integrated, and each of the plurality of first metal layers and the plurality of second metal layers includes an uneven region in which each metal layer has a bellows-like shape or a wrinkled shape.SELECTED DRAWING: Figure 11
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate, an electrode structure, a battery, an aircraft, a method for producing a laminate, and a method for producing an electrode structure. [Background technology]

[0002] Patent documents 1 and 2 disclose methods for welding materials containing resin and metal. Patent document 3 discloses a current collector having a through hole with a conductive material disposed in it. (Prior art document) (Patent Documents) (Patent Document 1) JP 2004-130331 A (Patent Document 2) JP 2006-305591 A (Patent Document 3) JP 2019-186204 A Summary of the Invention [Means for solving the problem]

[0003] In a first aspect of the present invention, a laminate is provided. The laminate includes, for example, a plurality of laminated sheet materials. In the laminate, each of the plurality of sheet materials has, for example, a support layer including a thermoplastic resin material. Each of the plurality of sheet materials has, for example, a first metal layer and a second metal layer formed on both sides of the support layer. According to the laminate, for example, in a portion of the plurality of sheet materials, the plurality of first metal layers and the plurality of second metal layers included in the plurality of sheet materials are integrated. In the laminate, each of the plurality of first metal layers and the plurality of second metal layers includes, for example, an uneven region in which each metal layer has a bellows-like shape or a wrinkled shape.

[0004] In the laminate, the first metal layers and the second metal layers may not be integrated in the concave-convex region. In the laminate, each metal layer may include a plurality of peaks and at least one valley arranged in the in-plane direction of each metal layer. In the laminate, the concave-convex region may be arranged adjacent to an integrated region where the first metal layers and the second metal layers are integrated.

[0005] In the laminate, the ratio of the volume of resin contained in the integrated region to the volume of metal contained in the integrated region, which is a region where the multiple first metal layers and the multiple second metal layers are integrated, may be 5 to 50%.In the laminate, the ratio of the volume of voids contained in the integrated region to the volume of metal contained in the integrated region, which is a region where the multiple first metal layers and the multiple second metal layers are integrated, may be 10% or less.

[0006] In the above laminate, the multiple sheet materials may have a first sheet material arranged on the outermost side of one side of the multiple sheet materials, and a second sheet material arranged on the outermost side of the other side of the multiple sheet materials. The above laminate may further include a first support member that supports the first sheet material, and a second support member that supports the second sheet material. In the above laminate, the first support member and the second support member may include metal. In a portion of the multiple sheet materials, the first support member, the second support member, the multiple first metal layers, and the multiple second metal layers may be integrated together.

[0007] In the laminate, each of the plurality of sheet materials may have a region in which a plurality of through holes are formed penetrating each sheet material near an integrated region where the plurality of first metal layers and the plurality of second metal layers are integrated. The laminate may further include a conductive member that electrically connects the first metal layer and the second metal layer disposed on each of the plurality of sheet materials.

[0008] In a second aspect of the present invention, an electrode structure is provided. The electrode structure includes, for example, a first electrode and a second electrode. The electrode structure includes, for example, a third electrode. The electrode structure includes, for example, a first separator and a second separator. In the electrode structure, for example, a first electrode, a first separator, a third electrode, a second separator, and a second electrode are laminated in this order. In the electrode structure, each of the first electrode and the second electrode includes, for example, a current collector and an active material layer disposed on at least one surface of the current collector. In the electrode structure, the current collector includes, for example, a support layer including a thermoplastic resin material, and a first metal layer and a second metal layer formed on both surfaces of the support layer. According to the electrode structure, for example, the first metal layer and the second metal layer of the first electrode and the first metal layer and the second metal layer of the second electrode are integrated in the vicinity of the ends of the first electrode and the second electrode. In the above electrode structure, the first metal layer and the second metal layer of the first electrode, and the first metal layer and the second metal layer of the second electrode each include an uneven region in which, for example, each metal layer has a bellows-like shape or a wrinkled shape.

[0009] The electrode structure may further include a fourth electrode and a third separator. In the electrode structure, the first electrode, the first separator, the third electrode, the second separator, the second electrode, the third separator, and the fourth electrode may be laminated in this order. In the electrode structure, each of the first electrode, the second electrode, the third electrode, and the fourth electrode may have a current collector and an active material layer. In the vicinity of the ends of the third electrode and the fourth electrode, the first metal layer and the second metal layer of the third electrode and the first metal layer and the second metal layer of the fourth electrode may be integrated. Each of the first metal layer and the second metal layer of the third electrode and the first metal layer and the second metal layer of the fourth electrode may include an uneven region in which each metal layer has a bellows-like shape or a wrinkled shape.

[0010] In a third aspect of the present invention, a battery is provided. The battery includes, for example, any of the electrode structures of the second aspect. The battery includes, for example, a case that houses the electrode structure.

[0011] In a fourth aspect of the present invention, an aircraft is provided. The aircraft includes, for example, any of the batteries according to the third aspect. The aircraft includes, for example, a thrust generating device that generates thrust using the electrical energy stored in the battery.

[0012] The above summary of the invention does not list all of the necessary features of the present invention. Also, subcombinations of these features may also be inventions. [Brief description of the drawings]

[0013] [Figure 1] 1 shows a schematic diagram of an example of the system configuration of an aircraft 100. [Diagram 2] An example of a power storage cell 112 is shown diagrammatically. [Diagram 3] Another example of a power storage cell 112 is shown diagrammatically. [Figure 4] An example of a current collector 400 is shown diagrammatically. [Diagram 5] An example of a current collector 500 is shown diagrammatically. [Figure 6] An example of a current collector 600 is shown diagrammatically. [Figure 7] An example of a laminate structure 760 is shown diagrammatically. [Figure 8] An example of the electrical connection relationship of the electrodes of the laminated structure 760 is shown roughly. [Figure 9] An example of a method for manufacturing the power storage cell 112 is shown in schematic form. [Figure 10] An example of a method for manufacturing the positive electrode 220 is shown in schematic form. [Figure 11] An example of a welding procedure using welding device 1120 is shown. [Figure 12] 1 shows an example of a plurality of through holes 620 arranged in a current collector 1102. [Figure 13] 1 shows an example of a plurality of through holes 620 arranged in a current collector 1102. [Figure 14] An example of a procedure for producing the laminated structure 760 will be described. [Figure 15]An example of a top view of the positive electrode connector 820 is shown diagrammatically. [Figure 16] An example of a cross section of a positive electrode connector 820 is shown diagrammatically. [Figure 17] An example of a cross section of a positive electrode connector 820 is shown diagrammatically. [Figure 18] An example of a positive electrode current collector 222 including a roughened region 1600 is shown generally. [Figure 19] An example of a rough area 1900 is shown diagrammatically. [Figure 20] Another example of a cross section of the positive electrode connector 820 is shown diagrammatically. [Figure 21] 13 shows yet another example of a cross section of a positive electrode connector 820. [Figure 22] 1 shows an example of an X-ray CT observation result of the welded portion and its surroundings in Example 1. [Diagram 23] An example of an X-ray CT observation result of an observation area 2200 is shown. [Figure 24] An example of an X-ray CT observation result of an observation area 2300 is shown. [Diagram 25] 1 shows an example of an SEM image of a cross section of a welded portion and its surroundings in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] According to one embodiment (sometimes referred to as the present embodiment) illustrated in this specification, a laminate is produced by welding a portion of a plurality of stacked welding objects. Each of the plurality of welding objects includes a support layer containing a resin material, and a first metal layer and a second metal layer formed on both sides of the support layer. The welding object may be a sheet-like material (sometimes referred to as a sheet material). The welding object may be a current collector used in an electrode of a battery.

[0015] The first metal layer and the second metal layer of each of the plurality of welding targets are electrically connected to each other, so that the first metal layer and the second metal layer can be welded to each other by, for example, resistance welding.

[0016] The type of the resin material is not particularly limited, and any thermoplastic resin material can be used as the resin material. The support layer may be substantially made of a thermoplastic resin material, or the support layer may be a thermoplastic resin material.

[0017] By using a thermoplastic resin material as the main component of the support layer, for example, when the laminate is used as an electrode of a battery, the safety of the battery is improved. More specifically, when the battery experiences thermal runaway, the thermoplastic resin material is melted by the heat. As a result, the thermal runaway can be terminated.

[0018] In addition, the thermoplastic resin material softens and becomes more fluid when its temperature rises. As a result, in a welding process for multiple welding objects, when pressure is applied to the heated welding objects, the resin material disposed between the first metal layer and the second metal layer moves easily, and the first metal layer and the second metal layer come close to each other or come into contact with each other. In this state, the first metal layer and the second metal layer are integrated by applying energy to the first metal layer and the second metal layer.

[0019] According to one example of this embodiment, a plurality of welding objects are welded by the following procedure. First, energy is applied to a softened region disposed in a portion of the plurality of welding objects. As described above, the support layer of the welding object in this embodiment mainly contains, for example, a thermoplastic resin material. When an appropriate energy is applied to the softened region of the welding object, the temperature of the thermoplastic resin material contained in the support layer increases, and the resin material softens.

[0020] Next, a welding region disposed in at least a part of the softened region of the welding object is pressed. This applies pressure to the resin material of the support layer disposed between the first metal layer and the second metal layer. The resin material present inside the welding region is softened and has a suitable degree of fluidity. Therefore, when an appropriate amount of pressure is applied to the resin material of the support layer, the resin material moves inside the welding object.

[0021] When welding the first metal layer and the second metal layer, applying pressure to the first metal layer and the second metal layer to bring the first metal layer and the second metal layer into close proximity or contact with each other causes the resin material disposed between the first metal layer and the second metal layer to be pushed out to the periphery of the welded portion. The present inventors have found that, depending on the thickness of the first metal layer and the second metal layer, the volume of the resin material pushed out to the periphery of the welded portion, the viscosity or ease of movement of the resin material, and the like, when the resin material disposed at the welded portion is pushed out to the periphery of the welded portion, the first metal layer and the second metal layer disposed around the welded portion may be broken by the resin material.

[0022] The inventors have also found that when the above-mentioned metal layer breaks, the variation in the measured electrical resistance between the integrated sheet materials becomes greater than a predetermined threshold value. For example, consider a case where a part of sheet material A, sheet material B, and sheet material C are integrated by welding. As described above, each sheet material includes a support layer containing a resin material, and a first metal layer and a second metal layer formed on both sides of the support layer. Sheet material A, sheet material B, and sheet material C are laminated such that the second metal layer of sheet material A contacts the first metal layer of sheet material B, and the second metal layer of sheet material B contacts the first metal layer of sheet material C. Also, a part of the laminated sheet materials is welded according to the above-mentioned procedure.

[0023] In this case, the first metal layer and the second metal layer included in the sheet material A, the sheet material B, and the sheet material C are integrated at the welded portions, and all of the metal layers are electrically connected. Therefore, it was thought that the variation in electrical resistance between the multiple metal layers was sufficiently small.

[0024] However, the inventors have found that when they measured (i) the electrical resistance between an arbitrary point on the first metal layer of sheet material A and an arbitrary point on the second metal layer of sheet material A or an arbitrary point on the first metal layer of sheet material B, (ii) the electrical resistance between an arbitrary point on the first metal layer of sheet material A and an arbitrary point on the second metal layer of sheet material B or an arbitrary point on the first metal layer of sheet material C, (iii) the electrical resistance between an arbitrary point on the first metal layer of sheet material A and an arbitrary point on the second metal layer of sheet material C, (iv) the electrical resistance between an arbitrary point on the first metal layer of sheet material B and an arbitrary point on the B metal layer of sheet material A or an arbitrary point on the first metal layer of sheet material C, (v) the electrical resistance between an arbitrary point on the first metal layer of sheet material B and an arbitrary point on the second metal layer of sheet material C, and (vi) the electrical resistance between an arbitrary point on the first metal layer of sheet material C and an arbitrary point on the second metal layer of sheet material C, the measured values ​​may vary. Although the cause is not entirely clear, it is speculated that at least a portion of the first metal layer and the second metal layer arranged around the welded area were fractured, resulting in a complex conductive path around the welded area.

[0025] In addition, the inventors have found that when the first metal layer and the second metal layer have a region (sometimes referred to as an uneven region) having a bellows-like or wrinkled shape around the welded portion, the above-mentioned variation is smaller than when more than half of the first metal layer and the second metal layer included in the laminate near the welded portion are broken. Although the reason why the above-mentioned variation is smaller when the uneven region is formed in the first metal layer and the second metal layer is not necessarily clear, it is presumed that when the resin material arranged at the welded portion is pushed out around the welded portion, the first metal layer and the second metal layer move or deform, thereby suppressing the breakage of the first metal layer and the second metal layer.

[0026] By obtaining a laminate with small variations, for example, when the multiple metal layers constituting the laminate are used as a member constituting a part of the current collector of the stacked battery, the variations in the electrode reactions in the layers of the stacked battery are also suppressed, and as a result, the life characteristics of the stacked battery are improved.

[0027] The present inventors have also found that the uneven region can be formed, for example, when the support layer contains a thermoplastic resin having a melting point lower than that of polyimide as a main component. Examples of the main component of the support layer include a component whose content in the support layer is more than 50% by mass, and a component whose content in the support layer is 51% by mass or more. Furthermore, the present inventors have found that the uneven region can be formed when one or more through holes penetrating the support layer, the first metal layer, and the second metal layer are formed at and / or near the welding location of the welding target before welding.

[0028] As described above, the welding object is, for example, a current collector used in an electrode of a battery, and the method for producing the laminate or the method for welding a plurality of laminated welding objects can be applied to the manufacture of an electrode structure disposed inside a housing of a battery (particularly, a secondary battery). Also, according to this embodiment, a part of the current collector is formed of a material (typically, air or a resin material) having a lower density than aluminum foil or copper foil.

[0029] As a result, a storage cell having excellent energy density per unit mass and / or capacity per unit mass of active material can be provided. For example, according to this embodiment, a storage cell having an energy density per unit mass of 350 [Wh / kg-storage cell] or more can be provided. In addition, a battery including the storage cell according to this embodiment has a high energy density per unit mass, and is therefore particularly suitable for use in aircraft.

[0030] As described above, according to the present embodiment, for example, the amount of energy per weight in a rechargeable battery can be improved, and a rechargeable battery that is lighter and can store more power can be realized. The rechargeable battery can be brought to a disaster site, for example, and used to supply energy to disaster victims. Therefore, the laminate, electrode structure, and battery according to the present embodiment, as well as the manufacturing method thereof, can contribute to the achievement of Goal 7 "Affordable and clean energy" or Goal 13 "Take urgent action to combat climate change" of the Sustainable Development Goals (SDGs).

[0031] The present invention will be described below through embodiments of the invention, but the following embodiments do not limit the scope of the invention according to the claims. Furthermore, not all of the combinations of features described in the embodiments are necessarily essential to the solution of the invention.

[0032] In this specification, when a numerical range is expressed as "A to B", the expression means A or more and B or less. In addition, "substituted or unsubstituted" means "substituted with any substituent or not substituted with any substituent". The type of the above-mentioned substituent is not particularly limited unless otherwise stated in the specification. In addition, the number of the above-mentioned substituents is not particularly limited unless otherwise stated in the specification.

[0033] (Overview of the Aircraft 100) 1 illustrates an example of a system configuration of an aircraft 100. In this embodiment, the aircraft 100 includes a storage battery 110, a power control circuit 120, one or more electric motors 130, one or more propellers 140, one or more sensors 150, and a control device 160. In this embodiment, the storage battery 110 includes one or more storage cells 112.

[0034] In this embodiment, the flying object 100 flies using electrical energy stored in the storage battery 110. Examples of the flying object 100 include an airplane, an airship or a balloon, a helicopter, a drone, and the like.

[0035] In this embodiment, the storage battery 110 receives electric energy from an external charging device (not shown) via the power control circuit 120, and stores the electric energy in one or more storage cells 112. In addition, the storage battery 110 supplies the electric energy stored in the one or more storage cells 112 to the electric motor 130 via the power control circuit 120.

[0036] In this embodiment, the storage cell 112 stores electric energy (sometimes referred to as charging the storage cell 112). Also, the storage cell 112 releases the stored electric energy (sometimes referred to as discharging the storage cell 112). The storage cell 112 may be a secondary battery.

[0037] The storage cell 112 may be an all-solid-state battery. The storage cell 112 may be an all-solid-state secondary battery. The all-solid-state secondary battery is a secondary battery that does not substantially contain the above-mentioned electrolytic solution or gel electrolyte, and includes, for example, a pair of electrodes and a solid electrolyte layer disposed between the pair of electrodes.

[0038] The secondary battery being substantially free of electrolytic solution or gel electrolyte means not only the case where the secondary battery does not contain electrolytic solution or gel electrolyte, but also the case where the secondary battery contains a small amount of electrolytic solution or gel electrolyte. Even if the constituent materials of the secondary battery dissolve in the solvent contained in the electrolytic solution or gel electrolyte, if the amount of the solvent contained in the secondary battery is small, the effect on the battery performance of the constituent materials of the secondary battery dissolving in the solvent can be ignored.

[0039] In one embodiment, the energy storage cell 112 does not include at least one of (i) an electrolyte solution containing a supporting electrolyte salt and a solvent, and (ii) a gel electrolyte containing a supporting electrolyte salt, an organic polymer compound, and an organic solvent. In another embodiment, the ratio of the mass [kg] of the electrolyte solution and the gel electrolyte to the mass [kg] of the organic compound used as the active material is less than 5%.

[0040] Examples of carrier ions in secondary batteries include lithium, sodium, potassium, magnesium, calcium, etc. Examples of secondary batteries include sodium ion secondary batteries, lithium ion secondary batteries, lithium metal secondary batteries, lithium air secondary batteries, lithium sulfur secondary batteries, magnesium ion secondary batteries, etc.

[0041] For example, a material that can store a large amount of charge per unit volume is often selected as an active material for a secondary battery mounted on a vehicle. On the other hand, in this embodiment, the storage cell 112 is mounted on the aircraft 100. Therefore, it is preferable that the active material used for the storage cell 112 is a material that can store a large amount of charge per unit mass.

[0042] The mass energy density of the storage cell 112 is preferably 350 [Wh / kg-storage cell] or more, more preferably 400 Wh / kg-storage cell] or more, more preferably 500 Wh / kg-storage cell] or more, even more preferably 600 Wh / kg-storage cell] or more, and even more preferably 700 Wh / g-storage cell] or more. This provides a storage cell that is particularly suitable for use as a power source for an aircraft.

[0043] The volumetric energy density of the storage cell 112 is 300 [Wh / m 3 - Storage cell] 1200 [Wh / m 3 - Storage cell] or less, 400 [Wh / m 3 - Storage cell] 1000 [Wh / m 3 When the storage cell 112 is mounted on the aircraft 100 as part of the power source of the aircraft 100, the volumetric energy density of the storage cell 112 may be 600 [Wh / m 3 - Storage cell] or less, 800 [Wh / m 3 -storage cell] or less.

[0044] The storage cell 112 may have a mass energy density within the above numerical range and a volume energy density within the above numerical range. This allows the storage cell, which is relatively difficult to use as a power source for a vehicle, to be used as a power source for an aircraft. The details of the storage cell 112 will be described later.

[0045] In this embodiment, the power control circuit 120 controls the input and output of power of the storage battery 110. The power control circuit 120 may control the input and output of power of the storage battery 110 based on an instruction from the control device 160. The power control circuit 120 includes, for example, a plurality of switching elements that operate based on a control signal from the control device 160.

[0046] In this embodiment, the electric motor 130 receives electric energy from the storage battery 110 via the power control circuit 120. The electric motor 130 rotates the propeller 140 using the electric energy received from the storage battery 110. In this way, the electric motor 130 can generate propulsion force for the flying object 100 using the electric energy stored in the storage cell 112.

[0047] In this embodiment, the sensor 150 measures various physical quantities related to the position and attitude of the flying object 100. Examples of sensors for measuring various physical quantities related to the position and attitude of the flying object 100 include a GPS signal receiver, an acceleration sensor, an angular acceleration sensor, and a gyro sensor. The sensor 150 may measure various physical quantities related to the state of the storage battery 110. Examples of sensors for measuring various physical quantities related to the state of the storage battery 110 include a temperature sensor, a current sensor, and a voltage sensor.

[0048] In this embodiment, the control device 160 controls the flying object 100. The control device 160 may control the input and output of power to the storage battery 110 by controlling the power control circuit 120. For example, the control device 160 controls the output current, output voltage, input current, input voltage, etc. of the storage battery 110. This allows the control device 160 to control the position and attitude of the flying object 100. The control device 160 may control the position and attitude of the flying object 100 by controlling the power control circuit 120 based on the output from the sensor 150.

[0049] The storage battery 110 may be an example of a secondary battery. The power storage cell 112 may be an example of a secondary battery. The electric motor 130 may be an example of a propulsion force generating device. The secondary battery may be an example of a battery.

[0050] (Outline of storage cell 112) 2 is a schematic diagram of an example of the storage cell 112. In this embodiment, the details of the storage cell 112 will be described using as an example a case where the storage cell 112 is a coin-type all-solid-state secondary battery. However, it should be noted that the storage cell 112 is not limited to a coin-type all-solid-state secondary battery.

[0051] (Energy storage cell) In this embodiment, the energy storage cell 112 includes a positive electrode case 212, a negative electrode case 214, a sealant 216, and a metal spring 218. The energy storage cell 112 also includes a positive electrode 220, a separator 230, and a negative electrode 240. In this embodiment, the positive electrode 220 includes a positive electrode current collector 222 and a positive electrode active material layer 224. In this embodiment, the negative electrode 240 includes a negative electrode current collector 242 and a negative electrode active material layer 244.

[0052] In this embodiment, the energy storage cell 112 includes a structure 260 having a positive electrode 220, a separator 230, and a negative electrode 240. As shown in FIG. 2, the positive electrode 220, the separator 230, and the negative electrode 240 are stacked in this order, and the separator 230 is disposed between the positive electrode 220 and the negative electrode 240.

[0053] In this embodiment, the details of the storage cell 112 will be described using as an example a case where the storage cell 112 does not substantially contain an electrolytic solution or a gel electrolyte. Also, in this embodiment, the details of the storage cell 112 will be described using as an example a case where the positive electrode current collector 222 has (i) a conductive layer containing a conductive material and (ii) a support layer that supports the conductive layer.

[0054] In this embodiment, by assembling the positive electrode case 212 and the negative electrode case 214, a space is formed inside the positive electrode case 212 and the negative electrode case 214. A metal spring 218, a positive electrode 220, a separator 230, and a negative electrode 240 are accommodated inside the space formed by the positive electrode case 212 and the negative electrode case 214. The positive electrode 220, the separator 230, and the negative electrode 240 are fixed inside the positive electrode case 212 and the negative electrode case 214 by the repulsive force of the metal spring 218.

[0055] The positive electrode case 212 and the negative electrode case 214 are made of, for example, a conductive material having a disk-like thin plate shape. In this embodiment, the sealant 216 seals a gap formed between the positive electrode case 212 and the negative electrode case 214. The sealant 216 includes an insulating material. The sealant 216 insulates the positive electrode case 212 and the negative electrode case 214.

[0056] (positive electrode) In this embodiment, the positive electrode current collector 222 holds the positive electrode active material layer 224. In this embodiment, the positive electrode current collector 222 has an electrical resistance of 0.01 mΩ to 1 Ω. This suppresses the fluctuation in voltage measured by applying a current to the conductive layer under specific measurement conditions before and after pressure is applied to the conductive layer (details of the conductive layer will be described later) of the positive electrode current collector 222 during the manufacture of the positive electrode current collector 222 to, for example, less than 100 mV. The positive electrode current collector 222 may have an electrical resistance of 0.01 mΩ to 333 mΩ, or may have an electrical resistance of 0.01 mΩ to 100 mΩ.

[0057] The density of the positive electrode current collector 222 is, for example, 1.1 to 2.0 g / cm 3As a result, for example, the main component of the active material contained in the positive electrode active material layer 224 is anthraquinone (density: 1.3 g / cm 3 ), anthracene (density: 1.25g / cm 3 ) and / or naphthalene (density: 1.14 g / cm 3 ), the mass of the positive electrode 220 including the positive electrode current collector 222 and the positive electrode active material layer 224 becomes very light, and the mass energy density of the power storage cell 112 becomes large.

[0058] In this embodiment, at least a portion of the positive electrode current collector 222 is made of a material having a lower density than metal. At least a portion of the positive electrode current collector 222 may be made of a material having a lower density than aluminum. For example, at least a portion of the positive electrode current collector 222 is made of resin. This can reduce the weight of the power storage cell 112.

[0059] In particular, when a separator 230 containing a solid electrolyte as a main component is used, the mass of the separator 230 may become relatively large depending on the type of solid electrolyte. Even in such a case, an increase in the overall mass of the power storage cell 112 is suppressed by forming at least a portion of the positive electrode current collector 222 from a resin. As a result, the capacity per mass of the power storage cell 112 and the energy density of the power storage cell 112 are improved.

[0060] For example, the positive electrode current collector 222 includes a conductive layer containing a conductive material and a support layer that supports the conductive layer. The conductive layer and the support layer will be described in detail later.

[0061] Examples of the shape of the positive electrode collector 222 include a foil shape (which may also be called a plate shape, film shape, sheet shape, etc.), a mesh shape, and a plate shape with holes. The mesh shape and the plate shape with holes may be examples of the foil shape. The thickness of the positive electrode collector 222 is not particularly limited, but is preferably 1 to 200 μm. The thickness of the positive electrode collector 222 may be 6 to 20 μm, or 4 to 10 μm.

[0062] In this embodiment, the positive electrode active material layer 224 is formed on at least one surface of the positive electrode current collector 222. The thickness of the positive electrode active material layer 224 per surface of the positive electrode current collector 222 may be 1 to 100 μm, or may be 5 to 50 μm.

[0063] The positive electrode active material layer 224 includes, for example, a positive electrode active material and a binding material (sometimes referred to as a binder). The positive electrode active material layer 224 may further include at least one of a conductive material and an ion conductive material. The positive electrode active material layer 224 may include a positive electrode active material and an ion conductive material. This can suppress disconnection of the ion conductive path and / or the electron conductive path formed inside the positive electrode active material layer 224.

[0064] In one embodiment, the positive electrode active material layer 224 is formed by applying a slurry containing a material constituting the positive electrode active material layer 224 and a solvent onto at least one surface of the positive electrode current collector 222, and drying the slurry. Examples of the above-mentioned solvent include various solvent substances or mixtures thereof. The type of the above-mentioned solvent substance is not particularly limited, but examples of the above-mentioned solvent substance include N-methylpyrrolidone (NMP) and water.

[0065] In another embodiment, the positive electrode active material layer 224 is formed by mixing the materials constituting the positive electrode active material layer 224, forming the mixture into a sheet, and pressing the sheet-like mixture onto at least one surface of the positive electrode current collector 222. When an organic compound is used as the positive electrode active material, the positive electrode current collector 222 and the positive electrode active material layer 224 may be pressed together so that excessive pressure is not applied to the positive electrode active material layer 224 in the above-mentioned pressing step.

[0066] For example, when a coater is used to coat the precursor material of the positive electrode active material layer 224 on the positive electrode current collector 222, the pressure applied to the precursor material of the positive electrode active material layer 224 is adjusted. For example, the coating gap by the coater is set to 180 μm or more. The coating gap may be set to 200 μm or more. This prevents the ion conduction path and / or electron conduction path in the positive electrode active material layer 224 from being broken.

[0067] (Cathode active material) As the positive electrode active material contained in the positive electrode active material layer 224, for example, various materials capable of absorbing and releasing carrier ions of the power storage cell 112 are used. The positive electrode active material may be an inorganic compound or an organic compound. These positive electrode active materials may be used alone, or two or more types of positive electrode active materials may be used in combination.

[0068] As described above, the positive electrode 220 includes the positive electrode current collector 222 and the positive electrode active material layer 224. The mass of the positive electrode active material layer 224 may be 80% or more of the total mass of the positive electrode 220. The mass of the positive electrode active material may be 80% or more of the total mass of the positive electrode active material layer 224.

[0069] Examples of inorganic compounds used as the positive electrode active material (sometimes referred to as inorganic positive electrode active materials) include metal oxides, metal silicates, metal phosphates, metal borates, etc. Examples of the metals include transition metals such as V, Mn, Ni, and Co.

[0070] As the organic compound used as the positive electrode active material (sometimes referred to as an organic positive electrode active material), various redox active compounds are used as the organic positive electrode active material. Examples of the organic positive electrode active material include conjugated polymers, disulfides, quinones, localized radicals, and non-localized radicals.

[0071] The organic positive electrode active material may be an organic compound having a relatively small molecular weight and having the ability to donate and accept multiple electrons. When the organic compound is a low molecular weight compound, the molecular weight of the organic compound is, for example, 500 or less. When the organic compound is a polymer or oligomer, the molecular weight of the organic compound is, for example, 5000 or less.

[0072] (Materials other than positive electrode active material) The binder material contained in the positive electrode active material layer 224 binds the materials constituting the positive electrode active material layer 224 and maintains the electrode shape of the positive electrode 220. As the binder material, for example, various polymer materials are used. Examples of the polymer materials include carboxymethyl cellulose, styrene-butadiene rubber, polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyacrylic acid, polyethylene oxide (PEO), poly(3,4-ethylenedioxythiophene) (PEDOT), and derivatives thereof.

[0073] When an organic positive electrode active material is used as the positive electrode active material, the binder material may be a material that dissolves in a solvent in which the solubility of the organic positive electrode active material is greater than a predetermined value. The solubility of the binder material in the above-mentioned solvent may be equal to or greater than the solubility of the organic positive electrode active material in the above-mentioned solvent. This facilitates the disassembly process of the storage cell 112, for example, when the constituent materials of the storage cell 112 are reused.

[0074] The conductive material contained in the positive electrode active material layer 224 improves the conductivity of the positive electrode active material layer 224. This reduces the resistance of the positive electrode 220. The conductive material is not particularly limited as long as it is a material having electronic conductivity. Examples of the conductive material include carbon-based materials, metal-based materials, and conductive polymer materials. These conductive materials may be used alone, or two or more conductive assistants may be used in combination.

[0075] Examples of carbon-based materials include graphite, carbon black (e.g., acetylene black, ketjen black, etc.), coke, amorphous carbon, carbon fiber, carbon nanotube, graphene, etc. Examples of metal-based materials include aluminum, gold, silver, copper, iron, platinum, chromium, tin, indium, titanium, nickel, etc. Examples of conductive polymer materials include polyphenylene derivatives, etc.

[0076] When an organic positive electrode active material is used as the positive electrode active material, the conductive material may be a material that dissolves in a solvent in which the solubility of the organic positive electrode active material is greater than a predetermined value. The solubility of the conductive material in the above-mentioned solvent may be equal to or greater than the solubility of the organic positive electrode active material in the above-mentioned solvent. This facilitates the disassembly process of the storage cell 112, for example, when the constituent materials of the storage cell 112 are reused.

[0077] The conductive material contained in the positive electrode active material layer 224 improves the conductivity of carrier ions in the positive electrode active material layer 224. For example, various solid electrolytes are used as the conductive material. Examples of the solid electrolyte include sulfide-based solid electrolytes, oxide-based solid electrolytes, and polymer solid electrolytes. A polymer solid electrolyte may be used as the conductive material. Examples of the polymer solid electrolyte include polyethylene oxide (PEO), poly(3,4-ethylenedioxythiophene) (PEDOT), and at least one compound selected from derivatives thereof.

[0078] As described below, in this embodiment, the separator 230 includes a polymer solid electrolyte. The type of polymer solid electrolyte used as the conductive material may be the same as or different from the type of polymer solid electrolyte included in the separator 230.

[0079] When an organic positive electrode active material is used as the positive electrode active material, the conductive material may be a material that dissolves in a solvent in which the solubility of the organic positive electrode active material is greater than a predetermined value. The solubility of the conductive material in the above-mentioned solvent may be equal to or greater than the solubility of the organic positive electrode active material in the above-mentioned solvent. This facilitates the disassembly process of the storage cell 112, for example, when the constituent materials of the storage cell 112 are reused.

[0080] (Separator) In this embodiment, the separator 230 is disposed between the positive electrode 220 and the negative electrode 240 to separate the positive electrode 220 and the negative electrode 240. The separator 230 also ensures the conductivity of carrier ions between the positive electrode 220 and the negative electrode 240. The thickness of the separator 230 is not particularly limited, but is preferably 10 to 50 μm.

[0081] In this embodiment, the separator 230 includes a layered (sometimes referred to as a plate-like, film-like, sheet-like, etc.) solid electrolyte (sometimes referred to as a solid electrolyte layer). As a result, the solid electrolyte layer functions as a separator for the power storage cell 112.

[0082] In one embodiment, a solid electrolyte layer is used as the separator 230. The solid electrolyte layer may be composed of a single solid electrolyte layer or may be composed of multiple solid electrolyte layers. In another embodiment, a laminate of one or multiple solid electrolyte layers and another layer containing a material other than the solid electrolyte is used as the separator 230. The other layer may have ion conductivity. An example of the other layer is a composite material including a resin having multiple through holes formed therein and an ion conductive material filled in the through holes.

[0083] This makes it possible to produce a secondary battery that does not contain an electrolytic solution or a gel electrolyte. As a result, even if the positive electrode active material layer 224 and / or the negative electrode active material layer 244 contain an organic active material as the main active material, it is possible to suppress a decrease in battery life caused by the organic active material dissolving in the solvent of the electrolytic solution or the gel electrolyte.

[0084] The separator 230 is not limited to the above embodiment. For example, a porous material in which a solid electrolyte is disposed inside the pores is used as the separator 230. The separator 230 may be produced by immersing an appropriate support material or holding material in a gel electrolyte or an electrolytic solution, allowing the gel electrolyte or electrolytic solution to infiltrate the inside of the support material or the holding material, and then solidifying the electrolyte disposed inside the support material or the holding material. For example, the support material or holding material containing the gel electrolyte or electrolytic solution is dried, whereby the electrolyte disposed inside the support material or the holding material is solidified.

[0085] Examples of the solvent for the electrolytic solution or gel electrolyte include ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), butylene carbonate (BC), fluoroethylene carbonate (FEC), γ-butyrolactone, sulfolane, acetonitrile, 1,2-dimethoxymethane, 1,3-dimethoxypropane, diethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, and mixtures thereof. In particular, ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC) are widely used as the solvent for the electrolytic solution or gel electrolyte.

[0086] (solid electrolyte layer) In this embodiment, the separator 230 includes a solid electrolyte layer containing a polymer solid electrolyte as a main constituent material. The solid electrolyte layer contains, for example, 80 mass % or more of a true polymer solid electrolyte. When the separator 230 contains a polymer solid electrolyte as a main constituent material, the separator 230 can be bonded to the positive electrode 220 and / or the negative electrode 240 without a high-pressure pressing process.

[0087] The solid electrolyte layer is produced, for example, by applying a slurry containing a material constituting the solid electrolyte layer and a solvent onto a smooth support plate and drying the slurry. Examples of the solvent include various solvents or mixtures thereof. The type of the solvent is not particularly limited, but examples of the solvent include N-methylpyrrolidone (NMP), water, and methanol.

[0088] Examples of the polymer solid electrolyte constituting the solid electrolyte layer include polyethylene oxide (PEO), poly(3,4-ethylenedioxythiophene) (PEDOT), and at least one compound selected from derivatives thereof. The solid electrolyte layer may be substantially composed of a single polymer solid electrolyte, or may contain two or more types of polymer solid electrolytes.

[0089] (Negative electrode) In this embodiment, the negative electrode current collector 242 holds the negative electrode active material layer 244. Examples of the material of the negative electrode current collector 242 include copper, aluminum, stainless steel, nickel, titanium, and alloys thereof.

[0090] The negative electrode current collector 242 may include a conductive resin. The negative electrode current collector 242 may be a conductive resin. In one embodiment, the conductive resin includes a conductive polymer. In another embodiment, the conductive resin may be a polymer including a conductive filler.

[0091] The negative electrode current collector 242 may have a similar configuration to the positive electrode current collector 222. For example, the negative electrode current collector 242 includes a conductive layer containing a conductive material and a support layer that supports the conductive layer. The support layer is made of a material having a lower density than metal. The support layer may be made of a material having a lower density than aluminum. For example, the support layer is made of resin. This can reduce the weight of the power storage cell 112.

[0092] When a carrier metal is used as the negative electrode active material, the carrier metal may also serve as a current collector. For example, when the carrier metal of the power storage cell 112 is lithium and the negative electrode active material is lithium metal, the lithium metal is used as a current collector. In this case, the power storage cell 112 does not need to include the negative electrode current collector 242.

[0093] Examples of the shape of the negative electrode current collector 242 include a foil shape (sometimes referred to as a plate shape, a film shape, etc.), a mesh shape, and a plate shape with holes. The mesh shape and the plate shape with holes may be examples of the foil shape. The thickness of the negative electrode current collector 242 is not particularly limited, but may be 1 to 200 μm. The thickness of the negative electrode current collector 242 may be 4 to 20 μm, or 6 to 10 μm.

[0094] In this embodiment, the negative electrode active material layer 244 is formed on at least one surface of the negative electrode current collector 242. The thickness of the negative electrode active material layer 244 per surface of the negative electrode current collector 242 may be 0 to 200 μm, or 1 to 100 μm.

[0095] The negative electrode active material layer 244 includes, for example, a negative electrode active material and a binding material (sometimes referred to as a binder). The negative electrode active material layer 244 may further include at least one of a conductive material and an ion conductive material. The negative electrode active material layer 244 may include a negative electrode active material and an ion conductive material. This can suppress disconnection of the ion conductive path and / or the electron conductive path formed inside the negative electrode active material layer 244.

[0096] In one embodiment, the negative electrode active material layer 244 is produced by applying a slurry containing the material constituting the negative electrode active material layer 244 and an organic solvent onto at least one surface of the negative electrode current collector 242, and drying the slurry. Examples of the above-mentioned solvent include various solvent substances or mixtures thereof. The type of the above-mentioned solvent substance is not particularly limited, but examples of the above-mentioned solvent substance include N-methylpyrrolidone (NMP) and water.

[0097] In another embodiment, the negative electrode active material layer 244 is formed by mixing materials constituting the negative electrode active material layer 244, forming the mixture into a sheet, and pressing the sheet-like mixture onto at least one surface of the negative electrode current collector 242. When an organic compound is used as the negative electrode active material, the negative electrode current collector 242 and the negative electrode active material layer 244 may be pressed together so that excessive pressure is not applied to the negative electrode active material layer 244 in the above-mentioned pressing step.

[0098] For example, when the precursor material of the negative electrode active material layer 244 is applied onto the negative electrode current collector 242 using a coater, the pressure applied to the precursor material of the negative electrode active material layer 244 is adjusted. For example, the coating gap by the coater is set to 180 μm or more. The coating gap may be set to 200 μm or more. This suppresses disconnection of the ion conductive path and / or the electron conductive path in the negative electrode active material layer 244.

[0099] (Negative electrode active material) As the negative electrode active material contained in the negative electrode active material layer 244, for example, various materials capable of absorbing and releasing carrier ions of the power storage cell 112 are used. The negative electrode active material may be an inorganic compound or an organic compound. These negative electrode active materials may be used alone, or two or more types of negative electrode active materials may be combined. For example, a metal foil capable of releasing carrier ions of the power storage cell 112 is used as the negative electrode active material layer 244. This improves the mass energy density of the power storage cell 112.

[0100] In one embodiment, the negative electrode current collector 242 includes a conductive layer containing a conductive material and a support layer supporting the conductive layer, similar to the positive electrode current collector 222. In this case, the mass of the negative electrode active material layer 244 may be 80% or more of the total mass of the negative electrode 240. The mass of the negative electrode active material may be 80% or more of the total mass of the negative electrode active material layer 244. In another embodiment, a metal capable of releasing carrier ions of the power storage cell 112 (e.g., Li metal) is used as the negative electrode active material. In this case, the negative electrode active material contained in the negative electrode active material layer 244 is almost entirely composed of the metal. In addition, when the negative electrode active material layer 244 is the above-mentioned metal in a foil shape, the negative electrode 240 does not need to include the negative electrode current collector 242.

[0101] Examples of inorganic compounds used as the negative electrode active material (sometimes referred to as inorganic negative electrode active materials) include (i) carrier metals and alloys containing the carrier metals, (ii) tin, silicon and alloys containing the carrier metals, (iii) silicon oxides, and (iv) titanium oxides. For example, when the power storage cell 112 is a lithium secondary battery, metallic lithium, lithium titanium oxide (LTO), and the like are used as the negative electrode active material. When a material not containing a carrier metal is used as the negative electrode active material, the material may be pre-doped with the carrier metal.

[0102] As the organic compound used as the negative electrode active material (sometimes referred to as an organic negative electrode active material), various redox active compounds are used as the organic positive electrode active material. Examples of the organic positive electrode active material include conjugated polymers, disulfides, quinones, localized radicals, and delocalized radicals.

[0103] The organic positive electrode active material may be an organic compound having a relatively small molecular weight and having the ability to donate and accept multiple electrons. When the organic compound is a low molecular weight compound, the molecular weight of the organic compound is, for example, 500 or less. When the organic compound is a polymer or oligomer, the molecular weight of the organic compound is, for example, 5000 or less.

[0104] As described above, the negative electrode active material layer 244 may include a foil-shaped carrier metal. For example, the negative electrode active material layer 244 includes a lithium metal foil. This provides the carrier metal to the power storage cell 112. The thickness of the metal foil may be 1 to 200 μm, 10 to 100 μm, or 20 to 50 μm. The thickness and / or mass of the metal foil may be determined depending on the content of the positive electrode active material in the positive electrode active material layer 224.

[0105] (Materials other than negative electrode active material) The binder material contained in the negative electrode active material layer 244 binds the materials constituting the negative electrode active material layer 244 and maintains the electrode shape of the negative electrode 240. As the binder material, for example, various polymer materials are used. Examples of the polymer materials include carboxymethyl cellulose, styrene-butadiene rubber, polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyacrylic acid, polyethylene oxide (PEO), poly(3,4-ethylenedioxythiophene) (PEDOT), and derivatives thereof.

[0106] When an organic negative electrode active material is used as the negative electrode active material, the binder material may be a material that dissolves in a solvent in which the solubility of the organic negative electrode active material is greater than a predetermined value. The solubility of the binder material in the above-mentioned solvent may be equal to or greater than the solubility of the organic negative electrode active material in the above-mentioned solvent. This facilitates the disassembly process of the storage cell 112, for example, when the constituent materials of the storage cell 112 are reused.

[0107] The conductive material contained in the negative electrode active material layer 244 improves the conductivity of the negative electrode active material layer 244. This reduces the resistance of the negative electrode 240. The conductive material is not particularly limited as long as it is a material having electronic conductivity. Examples of the conductive material include carbon-based materials, metal-based materials, and conductive polymer materials. These conductive materials may be used alone, or two or more conductive assistants may be combined.

[0108] Examples of carbon-based materials include graphite, carbon black (e.g., acetylene black, ketjen black, etc.), coke, amorphous carbon, carbon fiber, carbon nanotube, graphene, etc. Examples of metal-based materials include aluminum, gold, silver, copper, iron, platinum, chromium, tin, indium, titanium, nickel, etc. Examples of conductive polymer materials include polyphenylene derivatives, etc.

[0109] When an organic negative electrode active material is used as the negative electrode active material, the conductive material may be a material that dissolves in a solvent in which the solubility of the organic negative electrode active material is greater than a predetermined value. The solubility of the binder material in the above-mentioned solvent may be equal to or greater than the solubility of the organic negative electrode active material in the above-mentioned solvent. This facilitates the disassembly process of the storage cell 112, for example, when the constituent materials of the storage cell 112 are reused.

[0110] The conductive material contained in the negative electrode active material layer 244 improves the conductivity of carrier ions in the negative electrode active material layer 244. For example, various solid electrolytes are used as the conductive material. Examples of the solid electrolyte include sulfide-based solid electrolytes, oxide-based solid electrolytes, and polymer solid electrolytes. A polymer solid electrolyte may be used as the conductive material. Examples of the polymer solid electrolyte include at least one compound selected from polyethylene oxide (PEO), poly(3,4-ethylenedioxythiophene) (PEDOT), and derivatives thereof.

[0111] As described above, in this embodiment, the separator 230 includes a polymer solid electrolyte. The type of polymer solid electrolyte used as the conductive material may be the same as or different from the type of polymer solid electrolyte included in the separator 230.

[0112] When an organic negative electrode active material is used as the negative electrode active material, the conductive material may be a material that dissolves in a solvent in which the solubility of the organic negative electrode active material is greater than a predetermined value. The solubility of the conductive material in the above-mentioned solvent may be equal to or greater than the solubility of the organic negative electrode active material in the above-mentioned solvent. This facilitates the disassembly process of the storage cell 112, for example, when the constituent materials of the storage cell 112 are reused.

[0113] The positive electrode case 212 may be an example of a housing. The negative electrode case 214 may be an example of a housing. The positive electrode 220 may be an example of an electrode. The positive electrode current collector 222 may be an example of a current collector. The positive electrode active material layer 224 may be an example of an active material layer. The negative electrode 240 may be an example of an electrode. The negative electrode current collector 242 may be an example of a current collector. The negative electrode active material layer 244 may be an example of an active material layer. The organic active material may be an example of an organic compound. The organic positive electrode active material may be an example of an organic compound. The organic negative electrode active material may be an example of an organic compound.

[0114] (An example of another embodiment) In this embodiment, the details of the storage cell 112 are described by taking the case where the storage cell 112 is a coin-type secondary battery as an example. However, the type, structure, and the like of the storage cell 112 are not limited to this embodiment. In another embodiment, the storage cell 112 may be a cylindrical battery including a wound electrode body in which a positive electrode, a separator, and a negative electrode are wound in a spiral shape. In yet another embodiment, the storage cell 112 may be a laminated battery in which a laminated electrode body in which positive electrodes and negative electrodes are alternately stacked with a separator sandwiched therebetween is sealed with a laminate. In yet another embodiment, the structure 260 includes a plurality of stacked positive electrodes 220, and the positive electrode current collectors 222 of the stacked positive electrodes 220 may be integrated in a portion of the stacked positive electrodes 220. The structure 260 includes a plurality of stacked negative electrodes 240, and the negative electrode current collectors 242 of the stacked negative electrodes 240 may be integrated in a portion of the stacked negative electrodes 240. In this case, the structure 260 may be an example of a laminate or electrode structure.

[0115] In this embodiment, the details of the storage cell 112 have been described by taking as an example a case in which the negative electrode 240 has the negative electrode current collector 242 and the negative electrode active material layer 244. However, the negative electrode of the storage cell 112 is not limited to this embodiment. In other embodiments, a foil-shaped carrier metal functions as the negative electrode current collector 242 and the negative electrode active material layer 244. For example, when the storage cell 112 is a lithium metal secondary battery, metallic lithium can be used as the negative electrode.

[0116] Fig. 3 is a schematic diagram of another example of the storage cell 112. The storage cell 112 described in relation to Fig. 3 differs from the storage cell 112 described in relation to Fig. 2 in that a liquid or gel electrolyte 350 is accommodated in addition to the metal spring 218, the positive electrode 220, the separator 230, and the negative electrode 240 inside the space formed by the positive electrode case 212 and the negative electrode case 214, and that a material other than a solid electrolyte may be used as the separator 230. The storage cell 112 described in relation to Fig. 3 may have a similar configuration to the storage cell 112 described in relation to Fig. 2, except for the above differences.

[0117] A known electrolytic solution or gel electrolyte may be used as the liquid or gel electrolyte 350. A known separator may be used as the separator 230.

[0118] The positive electrode current collector 222 will be described in detail with reference to Figs. 4, 5, and 6. As described above, the negative electrode current collector 242 may have a similar configuration to the positive electrode current collector 222. Fig. 4 shows a schematic cross-sectional view of a current collector 400, which is an example of the positive electrode current collector 222. Fig. 5 shows a schematic cross-sectional view of a current collector 500, which is an example of the positive electrode current collector 222. Fig. 6 shows a schematic cross-sectional view of a current collector 600, which is an example of the positive electrode current collector 222.

[0119] 4, the current collector 400 includes a support layer 420, a conductive layer 442, and a conductive layer 444. In this embodiment, the support layer 420 has a first plane 422, a second plane 424, and a side surface 426. In this embodiment, the conductive layer 442 is disposed on the first plane 422 of the support layer 420. The conductive layer 444 is disposed on the second plane 424 of the support layer 420.

[0120] In this embodiment, the support layer 420 supports the conductive layer 442 and the conductive layer 444. This suppresses damage to the conductive layer 442 and the conductive layer 444. The density of the support layer 420 is lower than the density of the conductive layer 442 or the conductive layer 444. For example, the support layer 420 is made of a material having a lower density than the density of the conductive layer 442 or the conductive layer 444. The support layer 420 may be a sheet-shaped resin material.

[0121] The resin material may be a thermoplastic resin or a thermosetting resin. The support layer 420 may be made of a single type of resin material or may contain multiple types of resin materials. As described above, when a part of the stacked multiple current collectors 400 is welded, it is preferable that the resin material mainly contains a thermoplastic resin or is substantially made of a thermoplastic resin. As a result, for example, the support layer is heated before welding, thereby improving the fluidity of the support layer. Furthermore, when the support layer 420 mainly contains a thermoplastic resin or is substantially made of a thermoplastic resin, the multiple current collectors 400 are firmly welded together compared to when the support layer 420 mainly contains a thermosetting resin or is substantially made of a thermosetting resin. As a result, a stack having excellent strength at the welded parts and small electrical resistance at the welded parts can be produced.

[0122] The thermoplastic resin may be a resin having at least one property selected from the group consisting of (i) a thermal conductivity of 0.6 W / mK or less at 20° C., (ii) a specific heat of 2500 J / kg·° C. or less at 20° C., (iii) a thermal shrinkage rate of 1% or less at 20° C., (iv) a melting point of 300° C. or less, and (v) a density of 1.9 gcm3 or less at 20° C. This makes it easier to form the above-mentioned uneven regions in conductive layer 442 and conductive layer 444 when parts of the stacked current collectors 400 are integrated by welding.

[0123] Examples of thermoplastic resins include polyethylene (PE), polyethylene terephthalate (PET), polyacrylonitrile (PAN), polypropylene (PP), polyphenylene sulfide (PPS), etc. Examples of polyethylene include high-density polyethylene and low-density polyethylene, etc. Examples of polypropylene include biaxially oriented polypropylene (OPP) and non-oriented polypropylene (CCP), etc.

[0124] Support layer 420 may be substantially made of one or more types of resin material selected from the group consisting of PET, PP, and PE. This makes it easier for the above-mentioned uneven areas to be formed in conductive layer 442 and conductive layer 444 when a part of a plurality of stacked current collectors 400 is welded, compared with a case in which support layer 420 is substantially made of polyimide (sometimes referred to as PI). As a result, breakage of conductive layer 442 and / or conductive layer 444 during welding is suppressed.

[0125] The conductivity of support layer 420 is not particularly limited, but the conductivity of support layer 420 may be smaller than the conductivity of conductive layer 442 or conductive layer 444. The thickness of support layer 420 is not particularly limited, but the thickness of support layer 420 may be larger than the thickness of conductive layer 442 or conductive layer 444. When the thickness of support layer 420 is large, the mass of support layer 420 also becomes large. Therefore, when support layer 420 is a sheet-shaped resin material, the thickness of the resin material may be 10 μm or less, preferably 7 μm or less, and more preferably 5 μm or less.

[0126] The thickness of the resin material is preferably 1 μm or more and 10 μm or less at 20° C. The thickness of the resin material may be 1 μm or more and 7 μm or less at 20° C., or may be 1 μm or more and 5 μm or less at 20° C.

[0127] In this embodiment, the conductive layer 442 and the conductive layer 444 include a conductive material having a resistivity of 8.0×10 -8 The conductive material may be a material having a resistance of 0.1 to 1.0 kPa (Ω·m) or more. The conductive material may be a metal. Examples of the metal include aluminum, stainless steel, nickel, and alloys thereof. Examples of stainless steel include SUS-430 and SUS-304. The conductive material may be aluminum.

[0128] The thickness of the conductive layer 442 and / or the conductive layer 444 (shown as the length in the vertical direction in the drawing) may be 0.05 μm to 7 μm. The thickness of the conductive layer 442 and / or the conductive layer 444 may be 0.05 μm to 5 μm, 0.1 μm to 3 μm, 0.1 μm to 2 μm, or 0.5 μm to 1 μm. The thickness of the conductive layer 442 and / or the conductive layer 444 may be 0.05 μm to 4 μm, 0.05 μm to 3 μm, 0.05 μm to 2 μm, or 0.05 μm to 1 μm. The thickness of the conductive layer 442 and / or the conductive layer 444 is preferably 0.1 μm to 5 μm, and more preferably 0.1 μm to 1 μm. Even relatively thin commercially available aluminum foils have a thickness of 6 to 10 μm, so by providing current collector 400 with conductive layer 442 and / or conductive layer 444 having a thickness of 5 μm or less, the energy density per unit mass of the storage cell [Wh / kg-storage cell] is improved compared to when commercially available aluminum foils are used as conductive layer 442 and / or conductive layer 444.

[0129] At least one of the conductive layer 442 and / or the conductive layer 444 may be an aluminum layer or foil having the above-mentioned thickness. The aluminum layer or foil may be disposed on the surface of the support layer 420 by pasting, or may be formed on the surface of the support layer 420 by a vapor deposition method, a deposition method, or the like.

[0130] When the conductive layer 442 and / or the conductive layer 444 has a thickness of 7 μm or less, the mass energy density of the storage cell 112 is improved. When the conductive layer 442 and / or the conductive layer 444 has a thickness of 5 μm or less, the mass energy density of the storage cell 112 is further improved. When the conductive layer 442 and / or the conductive layer 444 has a thickness of 1 μm or less, the mass energy density of the storage cell 112 is significantly improved. In general, when the thickness of the conductive layer is 0.1 μm or less or less than 0.1 μm, the conductive layer 442 and / or the conductive layer 444 is easily damaged. However, the conductive layer 442 and the conductive layer 444 according to this embodiment are supported by the support layer 420. Therefore, even when the thickness of the conductive layer 442 and / or the conductive layer 444 is about 0.05 to 0.1 μm, damage to the conductive layer 442 and / or the conductive layer 444 can be suppressed.

[0131] 5, current collector 500 differs from current collector 400 described in relation to Fig. 4 in that a plurality of through holes 522 are formed in support layer 420. Current collector 500 may have a similar configuration to current collector 400, except for the above difference.

[0132] When a simple metal foil is used as a current collector, when an attempt is made to form a through hole in the current collector, the metal foil may bend, making it difficult to form a through hole. Therefore, it is difficult to form a through hole in the current collector, particularly when an active material layer is formed on both sides of the metal foil. In contrast, according to this embodiment, the conductive layer is supported by a support layer such as a resin sheet, so that the current collector is relatively unlikely to bend even when a through hole is formed in the current collector.

[0133] According to the present embodiment, a part of the plurality of through holes 522 is filled with a conductive material 546. The conductive material 546 electrically connects the conductive layer 442 and the conductive layer 444.

[0134] The circle-equivalent diameter (sometimes referred to as the circle-equivalent diameter) of each of the plurality of through holes 522 may be 15 μm to 150 μm. The interval between two adjacent through holes 522 may be 30 μm to 250 μm.

[0135] If the circle equivalent diameter of the through hole 522 is smaller than 15 μm, when forming a conductive layer (sometimes referred to as an internal conductive layer) for electrically connecting the conductive layer 442 and the conductive layer 444 on the inner wall surface of the through hole 522, it may be relatively difficult to form an internal conductive layer having a sufficient thickness, or the effort required to form an internal conductive layer having a sufficient thickness may increase. If the thickness of the internal conductive layer is insufficient, the electrical resistance of the internal conductive layer may increase. On the other hand, if the circle equivalent diameter of the through hole 522 is larger than 150 μm, the area of ​​the support layer 420 supporting the conductive layer 442 and the conductive layer 444 becomes smaller. As a result, the total amount of the conductive layer 442 and the conductive layer 444 included in the current collector 500 also becomes smaller, and the electrical resistance of the conductive layer 442 and the conductive layer 444 may become larger. In addition, if the circle equivalent diameter of the through hole 522 is larger than 150 μm, the strength of the current collector 500 may be insufficient.

[0136] The circle-equivalent diameter (sometimes referred to as circle-equivalent diameter) of each of the plurality of through holes 522 may be 15 μm to 150 μm, 15 μm to 50 μm, or 15 to 35 μm. The circle-equivalent diameter of the through holes 522 that are not filled with the conductive material 546 may be 15 μm to 50 μm, or 15 to 35 μm. The circle-equivalent diameter of the through holes 522 that are filled with the conductive material 546 is not particularly limited. This can realize the weight reduction of the current collector 500 while suppressing breakage of the conductive layers 442 and 444.

[0137] The ratio of the sum of the areas of the through holes 522 on one surface of the current collector 500 to the outer area of ​​the one surface of the current collector 500 may be 30% or more. The ratio of the sum of the areas of the through holes 522 not filled with the conductive material 546 on one surface of the current collector 500 to the outer area of ​​the one surface of the current collector 500 may be 30% or more. This can realize the weight reduction of the current collector 500 while suppressing breakage of the conductive layers 442 and 444.

[0138] 6, current collector 600 differs from current collector 500 described in relation to FIG. 5 in that a plurality of through holes 620 are formed penetrating support layer 420, conductive layer 442, and conductive layer 444. Current collector 500 may have the same configuration as current collector 500, except for the above differences. For example, through hole 620 has the same configuration as through hole 522, except for the fact that through hole 620 penetrates conductive layer 442 and conductive layer 444.

[0139] In this embodiment, a conductive layer 642 is formed on the surfaces of at least some of the inner walls 622 of the multiple through holes 620. The conductive layer 642 may electrically connect the conductive layer 442 and the conductive layer 444.

[0140] In this embodiment, the conductive layer 642 includes a conductive material. The conductive material may be a metal. Examples of the metal include aluminum, stainless steel, nickel, and alloys thereof. Examples of the stainless steel include SUS-430 and SUS-304. The conductive material may be aluminum.

[0141] The conductive layer 642 may have multiple layers with different main components. The conductive layer 642 may have three or more layers with different main components. The conductive layer 642 includes, for example, an auxiliary layer, a target layer, and a protective layer. For example, a first layer mainly made of nickel is formed on the surface of the inner wall portion 622 of the through hole 620, a second layer mainly made of copper is formed on the first layer, and a chromate coating is formed on the second layer. The thickness of the first layer may be about 0.1 μm, the thickness of the second layer may be about 1 μm, and the thickness of the chromate coating may be about 0.3 μm.

[0142] Current collector 400 may be an example of a sheet material. Current collector 400 may be an example of a first sheet material or a second sheet material. Support layer 420 may be an example of a support layer. Conductive layer 442 may be an example of one of a first metal layer and a second metal layer. Conductive layer 444 may be an example of the other of the first metal layer and the second metal layer.

[0143] Current collector 500 may be an example of a sheet material. Current collector 500 may be an example of a first sheet material or a second sheet material. Conductive material 546 may be an example of a conductive member.

[0144] The current collector 600 may be an example of a sheet material. The current collector 600 may be an example of a first sheet material or a second sheet material. The inner wall portion 622 may be an example of an inner wall of a through hole. The conductive layer 642 may be an example of a conductive member.

[0145] (An example of another embodiment) In the present embodiment, details of current collector 400, current collector 500, and current collector 600 have been described taking as an example a case where support layer 420 mainly contains a thermoplastic resin or is substantially made of a thermoplastic resin when a portion of a plurality of stacked current collectors is welded. However, current collector 400, current collector 500, and current collector 600 are not limited to this embodiment.

[0146] In another embodiment, when the conductive layer 442 and the conductive layer 444 arranged on both sides of the support layer 420 are electrically connected, the support layer 420 may mainly include a thermosetting resin, or may be substantially composed of a thermosetting resin. In particular, according to the current collector 500, the conductive material 546 is filled inside at least a part of the through holes 522. Similarly, according to the current collector 600, the conductive layer 642 is formed inside at least a part of the through holes 620. Therefore, even if the conductive layer 442 and the conductive layer 444 included in a single current collector are not close to each other or do not contact each other, a part of the stacked multiple current collectors can be integrated by welding. In addition, the fluidity of the support layer is reduced by heating the support layer before welding. This suppresses the support layer from being pushed out to the periphery of the welding point, and as a result, the volume expansion around the welding point can be suppressed.

[0147] In this embodiment, the current collector 400 has been described in detail with reference to Fig. 4, taking as an example a case where no through-holes are formed in the support layer 420. Also, the current collectors 500 and 600 have been described in detail with reference to Figs. 5 and 6, taking as an example a case where the circle equivalent diameter of the through-holes 522 or the through-holes 620 is 15 µm to 150 µm. However, the current collectors 400, 500, and 600 are not limited to this embodiment.

[0148] In another embodiment, the current collector 400, the current collector 500, and / or the current collector 600 may have one or more through holes with a circle equivalent diameter of 30 μm to 5 mm that penetrate the current collector. The through hole with a circle equivalent diameter of 30 μm to 5 mm is arranged, for example, at the center of gravity of the welded portion or in the vicinity of the center of gravity (sometimes referred to as the approximate center). This reduces the volume of the resin material extruded from the welded portion. As a result, breakage of the conductive layer 442 and the conductive layer 444 is further suppressed. A conductive layer that electrically connects the conductive layer 442 and the conductive layer 444 may be formed on the inner wall of the through hole. This can facilitate welding of a plurality of sheet materials.

[0149] In another embodiment of the current collector 500, a through hole having an equivalent circle diameter of 30 μm to 5 mm may be formed instead of the through hole 522 or together with the through hole 522. The equivalent circle diameter of the through hole may be larger than that of the through hole 522. In another embodiment of the current collector 600, a through hole having an equivalent circle diameter of 30 μm to 5 mm may be formed instead of the through hole 620 or together with the through hole 620. The equivalent circle diameter of the through hole may be larger than that of the through hole 620.

[0150] In this embodiment, the details of the current collector 500 and the current collector 600 have been described by taking as an example a case in which the conductive layer 442 and the conductive layer 444 are electrically connected by the conductive material 546 or the conductive layer 642 arranged inside the through-holes formed in the support layer 420. However, the current collector 400, the current collector 500, and the current collector 600 are not limited to this embodiment. In other embodiments, the conductive layer 442 and the conductive layer 444 may be electrically connected by a conductive member arranged on at least a part of the side surface of the support layer 420.

[0151] A laminated structure 760, which is another example of an electrode structure, will be described in detail with reference to Fig. 7 and Fig. 8. Fig. 7 shows an example of a cross section of the laminated structure 760. Fig. 8 shows an example of an electrical connection relationship between electrodes of the laminated structure 760.

[0152] In the embodiment described in relation to FIG. 2, the structure 260 is an example in which the positive electrode 220, the separator 230, and the negative electrode 240 are laminated in this order, and details of the structure (which may be referred to as an electrode structure) constituting a part of the battery are described. However, the electrode structure is not limited to the structure 260. The laminated structure 760 differs from the structure 260 in that the laminated structure 760 includes a plurality of positive electrodes 220, a plurality of separators 230, and a plurality of negative electrodes 240. The laminated structure 760 may have the same configuration as the structure 260, except for the above differences.

[0153] 7, in this embodiment, the laminated structure 760 includes one or more positive electrodes 220, one or more negative electrodes 240, and one or more separators 230 disposed between each of the one or more positive electrodes 220 and each of the one or more negative electrodes 240. As shown in FIG. 7, the laminated structure 760 includes a plurality of positive electrodes 220, a plurality of negative electrodes 240, and a plurality of separators 230 disposed between each of the plurality of positive electrodes 220 and each of the plurality of negative electrodes 240.

[0154] Each of the multiple positive electrodes 220, except for the positive electrode 220 arranged on the outermost side of the laminated structure 760, has a positive electrode active material layer 224 arranged on both sides of the positive electrode current collector 222. The positive electrode 220 arranged on the outermost side of the laminated structure 760 has a positive electrode active material layer 224 arranged on one side of the positive electrode current collector 222.

[0155] Each of the multiple negative electrodes 240, except for the negative electrode 240 arranged on the outermost side of the laminated structure 760, has a negative electrode active material layer 244 arranged on both sides of the negative electrode current collector 242. The negative electrode 240 arranged on the outermost side of the laminated structure 760 has a negative electrode active material layer 244 arranged on one side of the negative electrode current collector 242.

[0156] In this embodiment, the positive electrode active material layer 224 is disposed on a part of the positive electrode current collector 222. For example, in the vicinity of at least one end of the positive electrode current collector 222, the positive electrode active material layer 224 is not formed on at least one surface of the positive electrode current collector 222. The multiple positive electrodes 220 are stacked, for example, such that the end on the side where the positive electrode active material layer 224 is not formed faces substantially the same direction.

[0157] In this embodiment, the negative electrode active material layer 244 is disposed on a part of the negative electrode current collector 242. For example, in the vicinity of at least one end of the negative electrode current collector 242, the negative electrode active material layer 244 is not formed on at least one surface of the negative electrode current collector 242. The multiple negative electrodes 240 are stacked such that, for example, the end portions on the side where the negative electrode active material layer 244 is not formed face substantially in the same direction.

[0158] 8, the laminated structure 760 includes a positive electrode connection portion 820 that electrically connects each of the multiple positive electrodes 220. According to this embodiment, the positive electrode connection portion 820 has a lead 822 and a sub-lead 824 that sandwich and support a portion of the multiple positive electrodes 220. This improves the strength of the connection points of the multiple positive electrodes 220.

[0159] In this embodiment, the lead 822 and the sub-lead 824 sandwich and support the end portion and / or the vicinity of the end portion of each of the positive electrode current collectors 222 of the multiple positive electrodes 220. As described above, the positive electrode active material layer 224 is not formed in the vicinity of at least one end portion of each of the multiple positive electrodes 220. The lead 822 and the sub-lead 824 are arranged to sandwich the stacked positive electrode current collectors 222. Note that in other embodiments, the sub-lead 824 may not be used.

[0160] In the positive electrode connection portion 820, the multiple positive electrodes 220 may be physically connected by welding. For example, the multiple stacked positive electrode collectors 222 are physically connected by welding, so that the ends and / or the vicinity of the ends of the multiple positive electrode collectors 222 are integrated. As a result, the multiple positive electrodes 220 are physically connected. At the ends and / or the vicinity of the ends of the multiple positive electrode collectors 222, the multiple positive electrode collectors 222 may be integrated with the lead 822 and / or the sub-lead 824. For example, when the lead 822 and the sub-lead 824 contain metal, the multiple conductive layers 442 and the multiple conductive layers 444 included in each of the multiple positive electrode collectors 222 are integrated with the lead 822 and the sub-lead 824 in the above welding process. Examples of the welding method include ultrasonic welding, resistance welding, and laser welding.

[0161] In this embodiment, the details of the laminated structure 760 will be described taking as an example a case in which the positive electrode current collectors 222 of the multiple positive electrodes 220 are physically bonded by welding a region (which may be referred to as a welding region) located near an end of each of the positive electrode current collectors 222 of the multiple positive electrodes 220. Note that in other embodiments, the welding region may be disposed so as to include the end of each of the positive electrode current collectors 222 of the multiple positive electrodes 220.

[0162] For example, as described in relation to FIG. 4, FIG. 5, or FIG. 6, each of the multiple positive electrode current collectors 222 has a support layer 420 and a conductive layer 442 and a conductive layer 444 formed on both sides of the support layer 420. The conductive layer 442 and the conductive layer 444 are electrically connected by, for example, a conductive material 546 and / or a conductive layer 642. The composition or material of the support layer 420 of each of the multiple positive electrode current collectors 222 may be the same or different. The composition or material of the support layer 420 of one positive electrode current collector 222 may be the same or different from the composition or material of the support layer 420 of another positive electrode current collector 222.

[0163] In this embodiment, the welding region is, for example, near the ends of the multiple positive electrode current collectors 222, and is disposed in at least a part of the region sandwiched between the lead 822 and the sub-lead 824. The planar dimensions of the sub-lead 824 may be larger than the planar dimensions of the welding region. The planar dimensions of the lead 822 may be larger than the planar dimensions of the sub-lead 824.

[0164] The lead 822 is made of, for example, a plate-like conductive material. The lead 822 may contain a metal or may be substantially made of a metal. The thickness of the lead 822 may be 1 to 300 μm, preferably 5 to 200 μm, and more preferably 10 to 50 μm.

[0165] The material of the sub-lead 824 is not particularly limited. The sub-lead 824 may contain a metal or may be substantially made of a metal. The sub-lead 824 is made of at least one selected from the group consisting of aluminum, nickel, stainless steel, copper, and alloys thereof, for example. The sub-lead 824 may be made of a resin material such as polypropylene or polyimide. The thickness of the sub-lead 824 may be 1 to 300 μm, preferably 5 to 200 μm, and more preferably 10 to 50 μm.

[0166] Similarly, the laminated structure 760 includes a negative electrode connecting portion 840 that electrically connects each of the multiple negative electrodes 240. According to the present embodiment, the negative electrode connecting portion 840 has a lead 842 and a sub-lead 844 that sandwich and support a portion of the multiple negative electrodes 240. This improves the strength of the connection points of the multiple negative electrodes 240.

[0167] In this embodiment, the lead 842 and the sub-lead 844 sandwich and support the end and / or the vicinity of the end of each of the negative electrode current collectors 242 of the multiple negative electrodes 240. As described above, the negative electrode active material layer 244 is not formed in the vicinity of at least one end of each of the multiple negative electrodes 240. The lead 842 and the sub-lead 844 are arranged to sandwich the stacked multiple negative electrode current collectors 242. Note that in other embodiments, the sub-lead 844 may not be used.

[0168] In the negative electrode connection portion 840, the negative electrodes 240 may be physically connected by welding. For example, the stacked negative electrode current collectors 242 are physically connected by welding, so that the ends and / or the vicinity of the ends of the negative electrode current collectors 242 are integrated. As a result, the negative electrodes 240 are physically connected. The negative electrode current collectors 242 may be integrated with the lead 842 and / or the sub-lead 844 at the ends and / or the vicinity of the ends of the negative electrode current collectors 242. For example, when the lead 842 and the sub-lead 844 contain metal, the conductive layers 442 and the conductive layers 444 included in each of the negative electrode current collectors 242 are integrated with the lead 842 and the sub-lead 844 in the above welding process. Examples of the welding method include ultrasonic welding, resistance welding, and laser welding.

[0169] According to the present embodiment, the laminated structure 760 will be described in detail by taking as an example a case in which the negative electrode current collectors 242 of the multiple negative electrodes 240 are physically bonded to each other by welding a region (which may be referred to as a welding region) located near an end of each of the negative electrode current collectors 242 of the multiple negative electrodes 240. Note that in other embodiments, the welding region may be disposed so as to include an end of each of the negative electrode current collectors 242 of the multiple negative electrodes 240.

[0170] For example, as described in relation to FIG. 4, FIG. 5, or FIG. 6, each of the multiple negative electrode current collectors 242 has a support layer 420 and a conductive layer 442 and a conductive layer 444 formed on both sides of the support layer 420. The conductive layer 442 and the conductive layer 444 are electrically connected by, for example, a conductive material 546 and / or a conductive layer 642. The composition or material of the support layer 420 of each of the multiple negative electrode current collectors 242 may be the same or different. The composition or material of the support layer 420 of one negative electrode current collector 242 may be the same or different from the composition or material of the support layer 420 of another negative electrode current collector 242.

[0171] In this embodiment, the welding region is, for example, near the ends of the multiple negative electrode current collectors 242, and is disposed in at least a part of the region sandwiched between the lead 842 and the sub-lead 844. The planar dimensions of the sub-lead 844 may be larger than the planar dimensions of the welding region. The planar dimensions of the lead 842 may be larger than the planar dimensions of the sub-lead 844.

[0172] The lead 842 is made of, for example, a plate-shaped conductive material. The lead 842 may contain a metal or may be substantially made of a metal. The thickness of the lead 842 may be 1 to 300 μm, preferably 5 to 200 μm, and more preferably 10 to 50 μm.

[0173] The material of the sub-lead 844 is not particularly limited. The sub-lead 844 may contain a metal or may be substantially made of a metal. The sub-lead 844 is made of at least one selected from the group consisting of aluminum, nickel, stainless steel, copper, and alloys thereof, for example. The sub-lead 844 may be made of a resin material such as polypropylene or polyimide. The thickness of the sub-lead 844 may be 1 to 300 μm, preferably 5 to 200 μm, and more preferably 10 to 50 μm.

[0174] The lead 822 may be an example of one of the first support member and the second support member. The sub-lead 824 may be an example of the other of the first support member and the second support member. The lead 842 may be an example of one of the first support member and the second support member. The sub-lead 844 may be an example of the other of the first support member and the second support member. The laminated structure 760 may be an example of an electrode structure. The multiple positive electrode current collectors 222 included in the laminated structure 760 may be an example of multiple stacked sheet materials. The multiple negative electrode current collectors 242 included in the laminated structure 760 may be an example of multiple stacked sheet materials.

[0175] Of the multiple positive electrode current collectors 222 stacked in the positive electrode connection portion 820, the positive electrode current collector 222 in contact with the lead 822 may be an example of one of the first sheet material and the second sheet material. Of the multiple positive electrode current collectors 222 stacked in the positive electrode connection portion 820, the positive electrode current collector 222 in contact with the sub-lead 824 may be an example of the other of the first sheet material and the second sheet material.

[0176] Of the multiple negative electrode current collectors 242 stacked in the negative electrode connection portion 840, the negative electrode current collector 242 in contact with the lead 842 may be an example of one of the first sheet material and the second sheet material. Of the multiple negative electrode current collectors 242 stacked in the negative electrode connection portion 840, the negative electrode current collector 242 in contact with the sub-lead 844 may be an example of the other of the first sheet material and the second sheet material.

[0177] The multiple positive electrodes 220 included in the laminate structure 760 may be an example of a first electrode and a second electrode, and the multiple negative electrodes 240 included in the laminate structure 760 may be an example of a third electrode and a fourth electrode. The multiple positive electrodes 220 included in the laminate structure 760 may be an example of a third electrode and a fourth electrode, and the multiple negative electrodes 240 included in the laminate structure 760 may be an example of a first electrode and a second electrode. Each of the multiple separators 230 included in the laminate structure 760 may be an example of a first separator, a second separator, or a third separator.

[0178] (An example of another embodiment) In the present embodiment, the details of the laminated structure 760 have been described by taking as an example a case in which the laminated structure 760 includes the positive electrode connecting portion 820 and the negative electrode connecting portion 840. However, the laminated structure 760 is not limited to this embodiment. In other embodiments, the laminated structure 760 may include at least one of the positive electrode connecting portion 820 and the negative electrode connecting portion 840.

[0179] In the present embodiment, the positive electrode connecting portion 820 has been described in detail by taking as an example a case in which the multiple positive electrode current collectors 222 are supported by the lead 822 and the sub-lead 824 in the positive electrode connecting portion 820. However, the positive electrode connecting portion 820 is not limited to this embodiment. In other embodiments, the positive electrode connecting portion 820 may not include the sub-lead 824. In this case, the multiple positive electrode current collectors 222 are supported by the lead 822.

[0180] In the present embodiment, the negative electrode connecting portion 840 has been described in detail by taking as an example a case in which the multiple negative electrode current collectors 242 are supported by the lead 842 and the sub-lead 844 in the negative electrode connecting portion 840. However, the negative electrode connecting portion 840 is not limited to this embodiment. In other embodiments, the negative electrode connecting portion 840 may not include the sub-lead 844. In this case, the multiple negative electrode current collectors 242 are supported by the lead 842.

[0181] FIG. 9 shows an example of a method for manufacturing the storage cell 112. In this embodiment, a method for producing the storage cell 112 including the stacked structure 760 is described. According to this embodiment, first, in step 912 (step may be abbreviated as S), a plurality of positive electrodes 220 and a plurality of negative electrodes 240 are prepared. Details of the method for preparing the positive electrodes 220 or the negative electrodes 240 will be described later. Also, in S914, a plurality of separators 230 are prepared. Next, in S920, the positive electrodes 220, the separators 230, and the negative electrodes 240 are stacked in this order. In this way, the stacked structure 760 is produced.

[0182] Next, in S932, the multiple positive electrodes 220 of the laminated structure 760 are electrically connected. Also, in S934, the multiple negative electrodes 240 of the laminated structure 760 are electrically connected. Thereafter, in S940, the laminated structure 760 is housed inside the positive electrode case 212 and the negative electrode case 214, and the energy storage cell 112 is assembled.

[0183] The positive electrodes 220 prepared in S912 may be an example of a first electrode and a second electrode, and the negative electrodes 240 prepared in S912 may be an example of a third electrode and a fourth electrode. The positive electrodes 220 prepared in S912 may be an example of a third electrode and a fourth electrode, and the negative electrodes 240 prepared in S912 may be an example of a first electrode and a second electrode. Each of the separators 230 prepared in S914 may be an example of a first separator, a second separator, or a third separator. The laminated structure 760 may be an example of an electrode structure in which a first electrode, a first separator, a third electrode, a second separator, a second electrode, a third separator, and a fourth negative electrode are laminated in this order.

[0184] 10 is a schematic diagram showing an example of a method for manufacturing the positive electrode 220. According to this embodiment, first, in S1010, a positive electrode current collector 222 is prepared. Next, in S1022, a positive electrode slurry containing a positive electrode active material and a solvent is prepared. Next, in S1024, the positive electrode slurry is applied to the surface of the positive electrode current collector 222. The positive electrode slurry is then dried. As a result, a positive electrode active material layer 224 is formed on the surface of the positive electrode current collector 222.

[0185] Next, in S1030, the positive electrode active material layer 224 and the positive electrode current collector 222 are fixed to each other. More specifically, pressure is applied to the stacked positive electrode active material layer 224 and the positive electrode current collector 222 to fix the positive electrode active material layer 224 and the positive electrode current collector 222 to each other.

[0186] In one embodiment, the pressure in the fixing step is set or adjusted so that (i) the rate of change in the electrical resistance (resistivity) of the current collector before and after pressure is applied to the active material layer and the current collector is within 50%, or (ii) the absolute value of the difference in the electrical resistance (resistivity) of the current collector before and after pressure is applied to the active material layer and the current collector is 1 [Ω] or less. The pressure in the fixing step may be set or adjusted so that the absolute value of the difference is less than 1 [Ω]. The pressure in the fixing step is preferably set or adjusted so that the absolute value of the difference is 500 m [Ω] or less, and more preferably set or adjusted so that the absolute value of the difference is 100 m [Ω] or less. This suppresses breakage of the conductive layer of the current collector. The electrical resistance of the current collector can be measured, for example, by a four-terminal four-probe method using a low resistivity meter (Loresta-GX MCP-T700, manufactured by Nitto Seiko Analytech Co., Ltd.).

[0187] In another embodiment, the pressure in the fixing step is set or adjusted so that (i) the value of the second voltage measured by applying a current to the conductive layer of the current collector after the pressure is applied minus (ii) the value of the first voltage measured by applying a current to the conductive layer of the current collector before the pressure is applied is less than 100 mV. This suppresses breakage of the conductive layer of the current collector. The first and second voltages are measured, for example, by a low resistivity meter having a function of measuring and outputting voltage values. The first and second voltages can be measured, for example, by a four-terminal four-probe method using a low resistivity meter (Loresta-GX MCP-T700, manufactured by Nitto Seiko Analytech Co., Ltd.).

[0188] (Procedure for physically connecting multiple electrodes) An example of a procedure for physically bonding multiple electrodes will be described with reference to Figures 11, 12, 13, and 14. For example, as described in relation to Figures 8 and 9, according to one embodiment of the laminated structure 760, multiple positive electrodes 220 are physically bonded by welding at the positive electrode connection portion 820. For example, the positive electrode current collectors 222 of the multiple positive electrodes 220 are physically bonded by welding. According to one embodiment of the laminated structure 760, multiple negative electrodes 240 are physically bonded by welding at the negative electrode connection portion 840. For example, the negative electrode current collectors 242 of the multiple negative electrodes 240 are physically bonded by welding.

[0189] In this embodiment, in order to facilitate understanding of the procedure for physically connecting a plurality of electrodes, the procedure for physically connecting a plurality of electrodes will be described in detail by taking as an example a case in which parts of two positive electrodes 220 are connected by welding using a welding device 1120. Note that the number of electrodes connected by welding is not limited to two. In other embodiments, three or more electrodes may be connected by welding.

[0190] In addition, in this embodiment, for the purpose of facilitating understanding of the procedure for physically bonding multiple electrodes, the procedure for physically bonding multiple electrodes is described in detail using as an example a case where one positive electrode 220 includes a current collector 1102 and a positive electrode active material layer 224 arranged on at least one surface of the current collector 1102, and the other positive electrode 220 includes a current collector 1104 and a positive electrode active material layer 224 arranged on at least one surface of the current collector 1104. In this embodiment, the procedure for physically bonding multiple electrodes is described in detail using as an example a case where the positive electrode active material layer 224 is not formed in the vicinity of the ends of the current collector 1102 and the current collector 1104.

[0191] Fig. 11 shows an example of a system configuration of a welding device 1120 together with an example of ends and / or vicinity of the current collector 1102 and the current collector 1104. An example of a welding procedure using the welding device 1120 will be described with reference to Fig. 11. More specifically, an example of a procedure will be described with reference to Fig. 11 in which the welding device 1120 presses the ends and vicinity of the ends of the current collector 1102 and the current collector 1104 while welding a part of the vicinity of the ends of the current collector 1102 and the current collector 1104 to produce a positive electrode connection part 820.

[0192] (Welding target) In this embodiment, the current collector 1102 and the current collector 1104 to be subjected to the welding process have the same configuration as the current collector 600 described in relation to FIG. 6. As described in relation to FIG. 6, the current collector 600 has a support layer 420, and a conductive layer 442 and a conductive layer 444 formed on both sides of the support layer 420. The current collector 600 has a plurality of through holes 620 penetrating the support layer 420, the conductive layer 442, and the conductive layer 444. The shape of the through holes 620 is not particularly limited. A conductive layer 642 that electrically connects the conductive layer 442 and the conductive layer 444 is formed on the surface of at least a part of the inner wall portion 622 of the plurality of through holes 620.

[0193] In this embodiment, the support layer 420 of the current collector 1102 and the current collector 1104 includes a thermoplastic resin material (sometimes referred to as a thermoplastic resin). In this embodiment, the support layer 420 of the current collector 1102 and the current collector 1104 may be a resin layer substantially made of a thermoplastic resin material. The support layer 420 of the current collector 1102 and the current collector 1104 may be an insulating layer substantially made of a thermoplastic resin material.

[0194] According to this embodiment, when energy is applied to support layer 420 of current collector 1102 and current collector 1104, the temperature of support layer 420 increases and the resin material contained in support layer 420 softens. When pressure is applied to current collector 1102 and current collector 1104 in a state in which the resin material contained in support layer 420 is softened, the resin material may move inside support layer 420. The above energy may be any energy capable of increasing the temperature of support layer 420 and / or the resin material contained in support layer 420, and the type of energy is not particularly limited. The above energy may be thermal energy.

[0195] The thermoplastic resin material may be a resin material having a thermal shrinkage rate of 1% or less at 25° C. Examples of the thermoplastic resin material include PE, PET, PAN, PP, and PPS.

[0196] The thickness of the support layer 420 of the current collector 1102 and the current collector 1104 may be 0.5 μm to 20 μm. The thickness of the support layer 420 is preferably 1 μm to 10 μm, and more preferably 2 μm to 8 μm.

[0197] In this embodiment, the conductive layer 442 and the conductive layer 444 of the current collector 1102 and the current collector 1104, respectively, contain a metal material. The conductive layer 442 and the conductive layer 444 of the current collector 1102 and the current collector 1104, respectively, may be a metal layer substantially made of a metal material. The metal layer substantially made of a metal material contains, for example, inevitable impurities. The metal material contained in the conductive layer 442 and the conductive layer 444 may be a simple metal or an alloy.

[0198] The thickness of the conductive layer 442 and the conductive layer 444 of the current collector 1102 and the current collector 1104 may be 0.1 μm to 10 μm. The thickness of the conductive layer 442 and the conductive layer 444 is preferably 0.1 μm to 5 μm, and more preferably 0.1 μm to 1 μm.

[0199] In this embodiment, the conductive layers 442 and 444 of the current collectors 1102 and 1104 are electrically connected to each other. Thus, a welding current applied to the conductive layer 442 of the current collector 1102 by the welding device 1120 flows through the conductive layer 442 of the current collector 1102, the conductive layer 442 of the current collector 1104, and the conductive layer 444 of the current collector 1104.

[0200] Conductive layer 442 and conductive layer 444 may be electrically connected in any manner. In one embodiment, a conductive member that electrically connects conductive layer 442 and conductive layer 444 is disposed on side surface 426 of support layer 420. In another embodiment, a conductive member that electrically connects conductive layer 442 and conductive layer 444 is disposed inside support layer 420.

[0201] In this embodiment, a portion of the current collector 1102 has a plurality of through holes 620 formed therein, penetrating the support layer 420, the conductive layer 442, and the conductive layer 444 of the current collector 1102. At least a portion of the plurality of through holes 620 is disposed in the above-described welding region (represented as Rw in FIG. 11). This reduces the amount of resin material present in the welding region of the support layer 420 compared to a case in which no through holes, grooves, or recesses are formed in the welding region of the support layer 420. As a result, the amount of resin material displaced by the welding of the conductive layers 442 and 444 is reduced, and volume expansion around the welding region due to welding is suppressed.

[0202] According to this embodiment, through holes 620 are also formed in the conductive layers 442 and 444. As a result, a part of the resin material pushed aside as the conductive layers 442 and 444 are welded together can flow into the through holes 620 in the conductive layers 442 and 444. As a result, volume expansion around the welded region caused by welding is suppressed. In this case, the resin material remains in the welded region after welding.

[0203] At least some of the through holes 620 may be arranged in a region adjacent to the welded region (sometimes referred to as an adjacent region). As described above, as the conductive layer 442 and the conductive layer 444 are welded, a part of the resin material that was present in the welded region before welding is pushed aside and moves toward the adjacent region. According to this embodiment, since the through holes 620 are formed in the adjacent region, the resin material pushed aside as the conductive layer 442 and the conductive layer 444 are welded can flow into the through holes 620 arranged in the adjacent region. As a result, volume expansion around the welded region due to welding is suppressed.

[0204] At least some of the through holes 620 may be disposed in the welded region and in a region adjacent to the welded region. This further suppresses volume expansion around the welded region due to welding. Details of the through holes 620 will be described later.

[0205] In this embodiment, a conductive layer 642 that electrically connects the conductive layer 442 and the conductive layer 444 is disposed on the surface of at least some of the inner wall portions 622 of the multiple through holes 620. The material constituting the conductive layer 642 may be a substance having conductivity, and the type and structure of the material are not particularly limited. The conductive layer 642 may include a metal material. The conductive layer 642 may be a metal layer substantially made of a metal material. The metal layer substantially made of a metal material includes, for example, inevitable impurities.

[0206] The metal material contained in the conductive layer 642 may be a single metal or an alloy. The metal material contained in the conductive layer 642 may be the same as or different from the metal material contained in at least one of the conductive layers 442 and 444. Examples of the metal material include copper, nickel, aluminum, stainless steel, and alloys thereof. Examples of stainless steel include SUS304 and SUS430.

[0207] The conductive layer 642 may include a plurality of layers. Each of the plurality of layers may be made of a material different from the others. For example, the conductive layer 642 may include a layer (sometimes referred to as a target layer) for electrically connecting the conductive layer 442 and the conductive layer 444, and an auxiliary layer disposed between the inner wall portion 622 of the through hole 620 and the target layer. The auxiliary layer is formed to assist the conductivity of the target layer and to improve the adhesion between the through hole 620 and the target layer. A protective layer for protecting the target layer may be formed on the surface of the target layer. Examples of the protective layer include a chromate coating and a zinc coating.

[0208] The conductive layer 642 may include an auxiliary layer, a target layer, and a protective layer. For example, a first layer mainly made of nickel is formed on the surface of the inner wall portion 622 of the through hole 620, a second layer mainly made of copper is formed on the first layer, and a chromate coating is formed on the second layer. The thickness of the first layer may be about 0.1 μm, the thickness of the second layer may be about 1 μm, and the thickness of the chromate coating may be about 0.3 μm.

[0209] As described above, the thickness of the conductive layer 642 of the current collector 1102 and the current collector 1104 may be more than 0 μm and not more than 5 μm. The thickness of the conductive layer 642 is preferably 0.1 μm to 3 μm, and more preferably 0.1 μm to 1 μm.

[0210] The conductive layer 642 is formed by a known method. For example, the conductive layer 642 is formed by electroless plating, vapor deposition, or sputtering. The conductive layer 642 may be formed by various secondary growth methods, or may be formed by attaching a metal foil to the surface of the inner wall portion 622 of the through hole 620.

[0211] Similarly, a portion of the current collector 1104 has a plurality of through holes 620 formed therein, penetrating the support layer 420, the conductive layer 442, and the conductive layer 444 of the current collector 1104. A conductive layer 642 is disposed on the surface of an inner wall portion 622 of at least a portion of the plurality of through holes 620, electrically connecting the conductive layer 442 and the conductive layer 444. The conductive layer 642 of the current collector 1104 may have similar features to those described in relation to the conductive layer 642 of the current collector 1102.

[0212] (Support member) As described above, the conductive layers 442 and 444 according to this embodiment are formed of thin metal films, and therefore have a relatively low strength. Therefore, according to this embodiment, the current collector 1102 and the current collector 1104 are supported by the lead 822 and the sub-lead 824 described in relation to Fig. 8. In this embodiment, the lead 822 and the sub-lead 824 are arranged to sandwich the stacked current collector 1102 and the current collector 1104. This prevents the thin metal films from breaking during welding.

[0213] As described above, a conductive material is used as the lead 822. The lead 822 may include a metal or may be substantially composed of a metal. On the other hand, a conductive or non-conductive material is used as the sub-lead 824. The sub-lead 824 may include a metal or may be substantially composed of a metal.

[0214] Before the current collector 1102 and the current collector 1104 are welded, a through hole penetrating the lead 822 and the sub-lead 824 and the laminated current collector 1102 and the current collector 1104 may be formed. In addition, a conductive layer may be formed on the inner wall of the through hole to electrically connect the lead 822, the sub-lead 824, the conductive layer 442 and the conductive layer 444 of the current collector 1102, and the conductive layer 442 and the conductive layer 444 of the current collector 1104. The circle equivalent diameter of the through hole may be 30 μm to 5 mm. The circle equivalent diameter of the through hole may be larger than the circle equivalent diameter of the through hole 620 formed in the current collector 1102 and the current collector 1104.

[0215] (Welding equipment) In this embodiment, the welding device 1120 includes a pair of welding heads 1130, a heating power supply 1140, a welding power supply 1150, and a controller 1160. In this embodiment, the welding device 1120 includes a pair of heating power supplies 1140 that supply power to each of the pair of welding heads 1130. In this embodiment, the welding head 1130 includes a position adjustment unit 1132, a heating unit 1134, and a welding unit 1136.

[0216] In this embodiment, the welding head 1130 applies energy to the welding target. For example, the welding head 1130 heats the welding target. The welding head 1130 presses the welding target. In this way, the welding head 1130 can apply pressure to the welding target.

[0217] In this embodiment, the position adjustment unit 1132 adjusts the position of the welding head 1130. For example, the position adjustment unit 1132 moves the welding head 1130 to a welding area of ​​the welding target. For example, the position adjustment unit 1132 presses the welding head 1130 against the welding area of ​​the welding target. This causes the welding head 1130 to press the welding area of ​​the welding target. As a result, pressure is applied to the welding area of ​​the welding target.

[0218] In this embodiment, the heating unit 1134 applies energy to the softened region of the welding target. This heats the softened region of the welding target. In this embodiment, the welding unit 1136 applies a current and / or a voltage to the welding region of the welding target. This welds the welding region of the welding target.

[0219] In this embodiment, a heating power supply 1140 supplies power to the heating section 1134. In this embodiment, a welding power supply 1150 supplies power to the position adjustment section 1132 and the welding section 1136. In this embodiment, a controller 1160 controls the operation of each section of the welding device 1120.

[0220] (Welding Procedure) Next, an example of a procedure for welding a portion of the current collector 1102 and the current collector 1104 using the welding device 1120 will be described. According to this embodiment, first, the current collector 1102 and the current collector 1104 to be welded are prepared. In one embodiment, the current collector 1102 and the current collector 1104 having the structure described above are fabricated. In another embodiment, the current collector 1102 and the current collector 1104 having the structure described above are purchased.

[0221] Next, the current collector 1102 and the current collector 1104 are welded to produce a laminate in which parts of the current collector 1102 and the current collector 1104 are joined together. More specifically, first, the current collector 1102 and the current collector 1104 are laminated. For example, the current collector 1102 and the current collector 1104 are laminated such that the second flat surface 424 side of the current collector 1102 and the first flat surface 422 side of the current collector 1104 are in contact with each other.

[0222] In one embodiment, the through holes 620 of the current collector 1102 are aligned with the through holes 620 of the current collector 1104. In other embodiments, alignment of the through holes 620 of the current collector 1102 with the through holes 620 of the current collector 1104 is not performed.

[0223] Next, the current collector 1102 and the current collector 1104 are reinforced using the lead 822 and the sub-lead 824. For example, the current collector 1102 and the current collector 1104, and the lead 822 and the sub-lead 824 are placed at the working position of the welding device 1120 so that the lead 822 and the sub-lead 824 sandwich the welding area of ​​the current collector 1102 and the current collector 1104 or the area surrounding the welding area.

[0224] Next, a welding region is determined for the current collector 1102 and the current collector 1104. Also, a region that includes the welding region of the stacked current collector 1102 and the current collector 1104 and is to be subjected to heat treatment (for example, a softened region represented as Rs in FIG. 11) is determined.

[0225] For example, a user of the welding device 1120 operates the welding device 1120 to input the positions of the welding area and the softened area into the welding device 1120. The controller 1160 of the welding device 1120 controls the position adjustment unit 1132 to move the welding head 1130 to an arbitrary position (e.g., the welding area) of the softened areas of the current collector 1102 and the current collector 1104. The controller 1160 of the welding device 1120 controls the position adjustment unit 1132 to bring the welding head 1130 into contact with the softened areas of the current collector 1102 and the current collector 1104.

[0226] Next, energy is applied to a region (sometimes referred to as a softened region) including the welded region of the stacked current collectors 1102 and 1104 to soften the resin material in the softened region. For example, the controller 1160 of the welding device 1120 controls the heating power source 1140 to supply power from the heating power source 1140 to the heating unit 1134. This causes the heating unit 1134 to increase the temperature of the welding head 1130. As a result, thermal energy is applied from the welding head 1130 to the softened regions of the current collectors 1102 and 1104.

[0227] As described above, in this embodiment, the support layer 420 of the current collector 1102 and the current collector 1104 includes a thermoplastic resin. When thermal energy is applied to the softening regions of the current collector 1102 and the current collector 1104, the thermoplastic resin disposed in the softening regions softens.

[0228] Next, a welding area disposed on at least a portion of the softened area is pressed. For example, the controller 1160 of the welding device 1120 controls the position adjustment unit 1132 to press the welding head 1130 against the welding area.

[0229] For example, the controller 1160 controls the position adjustment unit 1132 to bring the conductive layers 442 and 444 of the current collectors 1102 and 1104 close to each other to a distance that allows welding. At this time, pressure is also applied to the thermoplastic resin disposed between the conductive layers 442 and 444. According to this embodiment, the thermoplastic resin is softened and has appropriate fluidity. Therefore, when an appropriate pressure is applied to the thermoplastic resin, the thermoplastic resin moves toward the inside of the through-holes 620 formed in the conductive layers 442 and 444 in the welding area and / or toward the outside of the welding area.

[0230] The controller 1160 of the welding device 1120 may control the position adjustment unit 1132 to apply pressure to the stacked current collectors 1102 and 1104 so that the softened resin material flows into at least some of the through-holes 620 arranged in the softened region and / or the welded region. This significantly suppresses volume expansion around the welded region due to welding.

[0231] The controller 1160 may control the position adjustment unit 1132 to apply pressure to the stacked current collectors 1102 and 1104 so that the softened resin material breaks the conductive layer 642 arranged on the surface of the inner wall portion 622 of at least a part of the through-hole 620 arranged in the softened region and / or the welded region, and flows into the inside of the through-hole 620. This significantly suppresses volume expansion around the welded region due to welding.

[0232] The controller 1160 of the welding device 1120 may control the position adjustment unit 1132 to apply pressure to the stacked current collectors 1102 and 1104 so that a region where each metal layer has a bellows-like or wrinkled shape (sometimes referred to as an uneven region) is formed in a part of the conductive layer 442 and the conductive layer 444 of the current collector 1102. This suppresses breakage of the conductive layer 442 and the conductive layer 444 due to welding.

[0233] The controller 1160 of the welding device 1120 may control the position adjustment unit 1132 to apply pressure to the stacked current collectors 1102 and 1104 so that a region where each metal layer has a bellows-like or wrinkled shape (sometimes referred to as an uneven region) is formed in a part of the conductive layer 442 and the conductive layer 444 of the current collector 1104. This suppresses breakage of the conductive layer 442 and the conductive layer 444 due to welding.

[0234] Next, a current and / or a voltage is applied to the pressed welding area. This welds the conductive layers 442 and 444 of the current collectors 1102 and 1104, respectively. Also, for example, the conductive layer 444 of the current collector 1102 and the conductive layer 442 of the current collector 1104 are welded together. As a result, a laminate is produced in which the conductive layers 442 and 444 of the current collectors 1102 and 1104 are partially integrated together.

[0235] For example, controller 1160 of welding device 1120 controls welding power supply 1150 to supply power from welding power supply 1150 to welding portion 1136. As a result, a current and / or a voltage is applied to the pressed welding area, and a welding current flows through conductive layer 442 and conductive layer 444 of current collector 1102 and current collector 1104, respectively. At this time, controller 1160 of welding device 1120 may control position adjustment unit 1132 and welding power supply 1150 to apply a current and / or a voltage to the welding area while further pressing the welding area.

[0236] According to the present embodiment, in each of current collector 1102 and current collector 1104, conductive layer 442 and conductive layer 444 are electrically connected by conductive layer 642. This allows a welding current to flow through conductive layer 442 and conductive layer 444 of current collector 1102 and conductive layer 442 and conductive layer 444 of current collector 1104. As a result, the four conductive layers are integrated together in at least a portion of the welded region.

[0237] This produces a laminate in which the conductive layer 442 and the conductive layer 444 of the current collector 1102 and the conductive layer 442 and the conductive layer 444 of the current collector 1104 are integrated near one end of the current collector 1102 and the current collector 1104. Thermoplastic resin may be present in a region where part of the conductive layer 442 and the conductive layer 444 are integrated (sometimes referred to as an integrated region). Voids may be present in the integrated region. This produces a laminate in which at least one of the thermoplastic resin and the voids is dispersed inside the integrated metal.

[0238] In the integrated region, the conductive layer 442 and the conductive layer 444 may have a different shape than before welding. Similarly, the thermoplastic resin contained in the support layer 420 may have a different shape than before welding. A portion of the integrated region may include the conductive layer 442, the conductive layer 444, and / or the support layer 420 that maintains a shape substantially similar to that before welding.

[0239] When the lead 822 is made of metal, a laminate may be produced in which the lead 822, the conductive layer 442 and the conductive layer 444 of the current collector 1102, and the conductive layer 442 and the conductive layer 444 of the current collector 1104 are integrated. In this case, the integrated region refers to a region in which the lead 822, the conductive layer 442, and the conductive layer 444 are partially integrated. Similarly, when the lead 822 and the sub-lead 824 are made of metal, a laminate may be produced in which the lead 822, the conductive layer 442 and the conductive layer 444 of the current collector 1102, the conductive layer 442 and the conductive layer 444 of the current collector 1104, and the sub-lead 824 are integrated. In this case, the integrated region refers to a region in which the lead 822, the conductive layer 442, the conductive layer 444, and the sub-lead 824 are partially integrated.

[0240] As described above, a plurality of through holes 620 are formed in the welding region of the current collector 1102. Similarly, a plurality of through holes 620 are formed in the welding region of the current collector 1104. During welding, some of the plurality of through holes 620 are filled with metal contained in the conductive layer 442, the conductive layer 444, and / or the conductive layer 642. As a result, some of the plurality of through holes 620 disappear, or the volume of some of the voids in the plurality of through holes 620 decreases. Similarly, during welding, some of the plurality of through holes 620 are filled with thermoplastic resin contained in the support layer 420. As a result, some of the plurality of through holes 620 disappear, or the volume of some of the voids in the plurality of through holes 620 decreases. As a result, depending on the conditions and / or circumstances during welding, thermoplastic resin and / or voids may remain in the integrated region.

[0241] The integrated region may not include a thermoplastic resin, and may not include a void. For example, by adjusting the degree of pressure during welding and / or the magnitude of the welding current, a laminate that does not include a thermoplastic resin and / or a void in the integrated region can be produced.

[0242] (Resin content in integrated area) The ratio of the volume of the resin present in the integrated region to the volume of the metal present in the integrated region (sometimes referred to as the resin content in the integrated region) may be 0% or may be 0.1 to 50%. The resin content is preferably 0.1 to 50%, more preferably 1 to 30%, and even more preferably 5 to 20%.

[0243] When the lead 822 and / or the sub-lead 824 are made of a metal, and a laminate is produced in which the lead 822 and / or the sub-lead 824, the conductive layer 442 and the conductive layer 444 of the current collector 1102, and the conductive layer 442 and the conductive layer 444 of the current collector 1104 are integrated, the resin content in the integrated region can be derived as the ratio of the volume of the resin present in the integrated region to the volume of the metal originating from the conductive layer 442 and the conductive layer 444 present in the integrated region. The volume of the metal originating from the conductive layer 442, the conductive layer 444, and / or the conductive layer 642 may be the volume of the same type of metal as the component that mainly constitutes the conductive layer 442, the conductive layer 444, and / or the conductive layer 642 (sometimes referred to as the main component).

[0244] For example, when the main component of the lead 822 and / or the sub-lead 824 is different from the main components of the conductive layer 442 and the conductive layer 444 of the current collector 1102 and the main components of the conductive layer 442 and the conductive layer 444 of the current collector 1104, the boundary between the metal originating from the lead 822 and / or the sub-lead 824 and the metal originating from the conductive layer 442 and / or the conductive layer 444 is determined, for example, by observing a cross section obtained by cutting the integrated region along a plane approximately parallel to the stacking direction of the integrated multiple current collectors (the vertical direction in FIG. 11) using a scanning electron microscope (SEM). The same is true when the main component of the lead 822 and / or the sub-lead 824 is different from the main components of the conductive layer 442, the conductive layer 444, and the conductive layer 642 of the current collector 1102 and the main components of the conductive layer 442, the conductive layer 444, and the conductive layer 642 of the current collector 1104.

[0245] For example, when the main components of the lead 822 and / or sub-lead 824 and the conductive layer 442 and / or conductive layer 444 are the same or similar, it may be relatively difficult to determine the position of the boundary from an observation of a cross section of the integrated region. In this case, the position of the boundary may be estimated based on the position of the boundary between the lead 822 and / or sub-lead 824 and the conductive layer 442 and / or conductive layer 444 in an adjacent region where the metal originating from the lead 822 and / or sub-lead 824 and the metal originating from the conductive layer 442 and / or conductive layer 444 are not integrated.

[0246] The resin content may be 5 to 50%. The resin content is preferably 5 to 30%, and more preferably 5 to 20%. According to this embodiment, the through hole 620 is formed in the softened region and / or the welded region. Therefore, the resin content may be higher than when the through hole 620 is not formed in the softened region and / or the welded region. Furthermore, a relatively high resin content may suggest that the through hole 620 has been formed in the softened region and / or the welded region.

[0247] If the resin content exceeds 50%, the welding is insufficient and the durability of the welded portion decreases. Also, if the resin content exceeds 50%, the conductivity between the lead 822 and the sub-lead 824 decreases and the resistance increases. On the other hand, if the integrated region contains an appropriate amount of resin, the resin can contribute to ensuring the strength of the integrated region. Also, in this case, since the integrated region contains a sufficient amount of conductive material, the conductivity of the integrated region is ensured.

[0248] The ratio of the volume of the thermoplastic resin originating from the support layer 420 among the resins present in the integrated region to the volume of the metal originating from the conductive layer 442, the conductive layer 444, and / or the conductive layer 642 among the metals present in the integrated region may be 5 to 50%. The above ratio may be 10 to 50%, 10 to 40%, or 5 to 30%. As described above, for example, when the main component of the lead 822 and / or the sub-lead 824 is different from the main components of the conductive layer 442 and the conductive layer 444 of the current collector 1102 and the main components of the conductive layer 442 and the conductive layer 444 of the current collector 1104, the volume of the metal originating from the conductive layer 442, the conductive layer 444, and / or the conductive layer 642 among the metals present in the integrated region can be relatively easily determined by observation with a scanning electron microscope.

[0249] As described above, the resin content in the integrated region is determined, for example, by observing a cross section obtained by cutting the integrated region along a plane approximately parallel to the stacking direction (vertical direction in FIG. 11) of the integrated current collectors using a scanning electron microscope (SEM). The cross section (i.e., the observation surface of the SEM) may be a cross section obtained by cutting the integrated region along a plane approximately parallel to the stacking direction (vertical direction in FIG. 11) of the integrated current collectors and approximately perpendicular to the extension direction (horizontal direction in FIG. 11) of the integrated current collectors (a plane penetrating the paper surface approximately perpendicularly in FIG. 11).

[0250] The cross section may be a plane passing through the approximate center of the integrated region. The approximate center of the integrated region is determined, for example, by visually observing the surface of one side (e.g., first plane 422) of the integrated current collectors. The surface may be the surface on the first plane 422 side of the current collector arranged on the uppermost surface, or the surface on the second plane 424 side of the current collector arranged on the lowermost surface.

[0251] In the step of cutting the integrated region of the laminate to observe the cross section of the laminate using an SEM, the approximate position of the outer edge of the integrated region is determined, for example, by visually checking the weld marks. Note that the exact position of the outer edge of the integrated region is determined, for example, by observing the cross section with an SEM after the integrated region of the laminate is cut.

[0252] According to one embodiment, the magnification of the SEM image near the outer edge of the integrated region is appropriately adjusted, so that the region where the conductive layers are integrated and the region where the conductive layers are simply in contact but not integrated can be visually distinguished, and the position of the outer edge (sometimes referred to as the edge) of the integrated region can be determined.

[0253] According to another embodiment, the position of the outer edge of the integrated region is determined based on the length (sometimes referred to as thickness) of the stack in the stacking direction of the multiple current collectors. For example, the position where the thickness near the end of the integrated region is 1.1 times the average value of the thickness near the center of the integrated region is determined as the end of the integrated region. The thickness near the center of the integrated region is determined, for example, by averaging the thickness at three positions in an SEM image near the center of the integrated region. The measurement interval is appropriately set so as to obtain the above number of measured values.

[0254] When there are a plurality of positions having a thickness 1.1 times the average thickness of the integrated region, the end of the integrated region may be the position among the plurality of positions that is closest to the center of the integrated region. When a plurality of current collectors are welded using leads and sub-leads, the thickness of the integrated region may be the distance between the leads and the sub-leads.

[0255] The resin content in the integrated region is derived, for example, as a ratio of the area of ​​the thermoplastic resin in the SEM image to the area of ​​the metal in the SEM image. The resin content in the integrated region may be derived as an average value of the resin content values ​​obtained by observing a plurality of SEMs at different observation positions in a single cross section. For example, first, five resin contents corresponding to five SEM images are derived. Next, three measurement values ​​excluding the maximum and minimum measurement values ​​of the five resin content measurements are averaged. This determines the resin content in the integrated region. One of the plurality of SEM images may be an image of approximately the center of the integrated region.

[0256] (Porosity in the integrated area) The ratio of the volume of voids to the volume of metal in the integrated region (sometimes referred to as the porosity in the integrated region) may be 0 to 10%. The porosity in the integrated region is preferably 0 to 10%, more preferably 0.1 to 8%, and even more preferably 0.1 to 5%. The porosity in the integrated region may exceed 10%, but as the porosity increases, the strength and electrical conductivity of the integrated region decrease. Therefore, the porosity in the integrated region is preferably 10% or less.

[0257] According to this embodiment, the through-hole 620 is formed in the softened region and / or the welded region. Therefore, the above-mentioned porosity may be larger than when the through-hole 620 is not formed in the softened region and / or the welded region. Furthermore, a relatively large porosity may suggest that the through-hole 620 has been formed in the softened region and / or the welded region.

[0258] The porosity of the integrated region is determined, for example, by observing a cross section obtained by cutting the integrated region along a plane approximately parallel to the stacking direction of the integrated current collectors (the vertical direction in FIG. 11) using a scanning electron microscope (SEM). The porosity of the integrated region is determined, for example, by the same procedure as for the resin content in the integrated region.

[0259] As described above, the above-mentioned laminate constitutes a part of the laminate structure 760. As described in relation to Fig. 8, the laminate structure 760 has a structure in which the first positive electrode 220, the first separator 230, the first negative electrode 240, the second separator 230, the second positive electrode 220, the third separator 230, and the second negative electrode 240 are laminated in this order.

[0260] In this embodiment, the positive electrode connection part 820 including the stack of the current collector 1102 and the current collector 1104 is disposed near the end of the positive electrode 220 including the current collector 1102 and the positive electrode 220 including the current collector 1104. Therefore, according to this embodiment, the two positive electrodes 220 are integrated near these ends. This reduces the mass of the power storage cell 112 compared to a case where a tab is provided on each of the multiple current collectors and the tabs of the multiple current collectors are electrically connected by wiring. As a result, a power storage cell 112 with a high mass energy density is obtained.

[0261] In this embodiment, before the above-described softening treatment or pressing treatment of the thermoplastic resin is performed, the current collector 1102 and the current collector 1104 are reinforced using the lead 822 and the sub-lead 824. This prevents the conductive layer 442 and / or the conductive layer 444 from being broken due to the pressure applied during welding.

[0262] Current collector 1102 may be an example of a sheet material, a first sheet material, or a second sheet material. Current collector 1104 may be an example of a sheet material, a first sheet material, or a second sheet material.

[0263] An example of the plurality of through holes 620 arranged in the current collector 1102 will be described with reference to Fig. 12 and Fig. 13. Fig. 12 is an example of a top view of the current collector 1102. Fig. 13 is an example of a cross-sectional view of the current collector 1102. Note that the plurality of through holes 620 arranged in the current collector 1104 may have similar characteristics to the plurality of through holes 620 arranged in the current collector 1102.

[0264] 12, in this embodiment, the diameter d (e.g., a circle-equivalent diameter) of each of the plurality of through holes 620 may be 15 μm to 150 μm. If the diameter d is less than 15 μm, the thermoplastic resin is less likely to flow into the through holes 620. In addition, since the volume of the through holes 620 is small, the volume expansion rate of the welded laminate is large. On the other hand, if the diameter d exceeds 150 μm, the strength of the current collector 1102 is reduced, and the current collector 1102 is more likely to break during welding.

[0265] In this embodiment, the interval (sometimes referred to as the pitch) P between two adjacent through holes 620 may be 30 μm to 250 μm. If the pitch P is less than 30 μm, the strength of the current collector 1102 is reduced, and the current collector 1102 is more likely to break during welding. In addition, the resistance of the current collector 1102 is increased. On the other hand, if the pitch P exceeds 250 μm, the total amount of thermoplastic resin present in the welded region may also be relatively large. Therefore, the volume expansion rate of the welded laminate may be increased. In contrast, by forming an appropriate amount of through holes 620 in the welded region, the total amount of thermoplastic resin present in the welded region before welding is reduced. As a result, the volume expansion of the adjacent region due to welding may be suppressed.

[0266] The length TL of the current collector 1102 in the extension direction may be greater than the length HL of the region (sometimes referred to as the through hole band) in which the multiple through holes 620 are formed, or TL and HL may be approximately the same. The length TW of the current collector 1102 in a direction approximately perpendicular to the extension direction (sometimes referred to as the width direction) may be greater than the length HW of the through hole band in the width direction, or TW and HW may be approximately the same.

[0267] In this embodiment, the welded region is disposed within the through hole band. At least a portion of the softened region is disposed within the through hole band. For example, the adjacent region is disposed within the through hole band. The softened region may be disposed within the through hole band.

[0268] The size of the softened region Rs may be determined based on the size of the welded region Rw. For example, the size of the softened region Rs is determined so that the ratio of the area Ss of the softened region Rs on the first plane 422 or the second plane 424 of the support layer 420 to the area Sw of the welded region Rw on the first plane 422 or the second plane 424 of the support layer 420 is expressed by the following formula (1). As a result, the volume of the through hole 620 present inside the softened region Rs becomes equal to or larger than the volume of the thermoplastic resin present inside the welded region Rw. (Formula 1) Ss / Sw ≧(1-ε w +εout ) / ε out

[0269] In Equation 1, ε w represents the porosity of the multiple through holes in the welded region Rw. ε out represents the porosity of the multiple through holes in the softened region Rs other than the welded region Rw. ε w and ε out is the porosity at the softening temperature.

[0270] Porosity ε of multiple through holes in the welded region Rw w may be 10% or more at the softening temperature. w is preferably 20% or more, and more preferably 30% or more.

[0271] 13, a conductive layer 642 is formed inside the through hole 620. Therefore, a diameter dv of the space formed inside the through hole 620 is smaller than a diameter d of the through hole 620.

[0272] As described above, the thickness Hd of the conductive layer 642 may be 0 μm to 5 μm. The thickness Hd of the conductive layer 642 is preferably 0.1 μm to 3 μm, and more preferably 0.1 μm to 1 μm.

[0273] As described above, the thickness hr of the support layer 420 may be 0.5 μm to 20 μm. The thickness hr of the support layer 420 is preferably 1 μm to 10 μm, and more preferably 2 μm to 8 μm.

[0274] As described above, the thickness hm of the conductive layer 442 and the conductive layer 444 may be 0.1 μm to 10 μm. The thickness hm of the conductive layer 442 and the conductive layer 444 is preferably 0.1 μm to 5 μm, and more preferably 0.1 μm to 1 μm.

[0275] 14 shows an example of a procedure for producing a laminated structure 760 in which a portion of each of the positive electrode current collectors 222 of a plurality of positive electrodes 220 is integrated. As described in relation to FIG. 11, according to this embodiment, first, in S1410, a plurality of positive electrodes 220 are prepared. Next, in S1420, ends of the positive electrode current collectors 222 of the plurality of positive electrodes 220 are laminated. In S1430, the lead 822 and the sub-lead 824 are installed so as to sandwich the end of the laminated positive electrode current collector 222.

[0276] In S1440, energy is applied to the softened region of the stacked positive current collectors 222 to soften the thermoplastic resin contained in the support layer 420 of the positive current collector 222. In S1450, pressure is applied to the welding region of the stacked positive current collectors 222 to move the softened thermoplastic resin into the through-hole 620 of the positive current collector 222. In S1450, a welding current is applied to the welding region of the stacked positive current collectors 222 to weld the conductive layer 442 and the conductive layer 444 of the positive current collector 222.

[0277] The details of the positive electrode connection part 820 in which the above-mentioned uneven region is formed will be described with reference to Figs. 15, 16, 17, and 18. In this embodiment, in order to facilitate understanding of the above-mentioned uneven region, the details of the positive electrode connection part 820 will be described taking as an example a case in which the lead 822, the three positive electrode current collectors 222, and the sub-lead 824 are integrated by welding. In this embodiment, the lead 822 and the sub-lead 824 are arranged to sandwich the three stacked positive electrode current collectors 222. The negative electrode connection part 840 may have a similar configuration to the positive electrode connection part 820.

[0278] Fig. 15 shows an example of a top view of the positive electrode connection part 820 after welding. Fig. 15 shows an example of one of the two faces of the positive electrode connection part 820 on which the sub-lead 824 is arranged. Figs. 16 and 17 show an example of a cross section of the positive electrode connection part 820 after welding. Fig. 18 shows an example of a positive electrode current collector 222 including an uneven region 1600. In the figure, the xy plane shows a plane approximately perpendicular to the stacking direction of the positive electrode current collector 222 (the z direction in the figure).

[0279] 15, in this embodiment, the lead 822 and the sub-lead 824 are disposed near the ends of the three stacked positive electrode collectors 222 so as to sandwich the three positive electrode collectors 222. An integrated region 1520 is formed in the sub-lead 824.

[0280] 11, in the process for integrating by welding a part of a laminate including the lead 822, the sub-lead 824, and the three positive electrode current collectors 222, a welding region including the integrated region 1520 is pressed. The sub-lead 824 has a shape recessed from the outer edge of the sub-lead 824 toward the integrated region 1520.

[0281] In a region (sometimes referred to as a smooth region) sufficiently distant from integrated region 1520, the surface of positive current collector 222 has a sufficiently small flatness. The smooth region may be a region that is sufficiently distant from both ends of lead 822 and sub-lead 824, and in which the surface of positive current collector 222 has a sufficiently small flatness. For example, the flatness of positive current collector 222 in the smooth region is approximately equal to a value obtained by taking into consideration the flatness of the sheet or film used as support layer 420 and the manufacturing errors of conductive layer 442 and conductive layer 444.

[0282] On the other hand, in an adjacent region between the integrated region and the smooth region, the resin material extruded from the integrated region in the above-mentioned welding process forms the above-mentioned uneven region in the conductive layer 442 and the conductive layer 444 of the positive electrode current collector 222. The above-mentioned uneven region is formed outside the above-mentioned integrated region 1520. The uneven region is, for example, disposed adjacent to the integrated region.

[0283] The flatness of the conductive layer 442 in the uneven region is greater than the flatness of the conductive layer 442 in the smooth region. The ratio of the flatness of the conductive layer 442 in the smooth region to the flatness of the conductive layer 442 in the uneven region may be 0.5 to 0.9, 0.5 to 0.8, or 0.5 to 0.75. The ratio may be 0.7 to 0.8. This can suppress peeling between the lead 822 and the positive electrode current collector 222. Also, the above-mentioned variation can be suppressed.

[0284] Similarly, the flatness of the conductive layer 444 in the uneven region is greater than the flatness of the conductive layer 444 in the smooth region. The ratio of the flatness of the conductive layer 444 in the smooth region to the flatness of the conductive layer 444 in the uneven region may be 0.5 to 0.9, 0.5 to 0.8, or 0.5 to 0.75. The ratio may be 0.7 to 0.8. This can prevent the lead 822 from peeling off the positive electrode current collector 222. Also, the above-mentioned variations can be prevented.

[0285] In this embodiment, the dimensions of the sub-lead 824 are smaller than the dimensions of the lead 822. In this case, (i) the ratio of the flatness of the conductive layer 442 in the smooth region to the flatness of the conductive layer 442 in the uneven region may be 0.5 to 0.9, and (ii) the ratio of the flatness of the conductive layer 444 in the smooth region to the flatness of the conductive layer 444 in the uneven region may be 0.7 to 0.8.

[0286] In the uneven region of the conductive layer 442, the conductive layer 442 has a bellows-like shape or a wrinkled shape. In the uneven region of the conductive layer 442, the conductive layer 442 includes a plurality of peaks and at least one valley that are arranged side by side along the in-plane direction of the conductive layer 442. As a result, wrinkles are formed on the surface of the conductive layer 442.

[0287] In a plane (xy plane in the drawing) approximately parallel to the stacking direction of the positive electrode current collector 222, the uneven region of the conductive layer 442 may extend in a single direction from the end of the integrated region 1520, or may extend in multiple directions. The shape of the uneven region in a plane approximately parallel to the stacking direction of the positive electrode current collector 222 may be approximately rectangular, approximately circular, or approximately fan-shaped. The shape of the uneven region in a plane approximately parallel to the stacking direction of the positive electrode current collector 222 may be approximately concentric circular, or approximately concentric polygonal.

[0288] In one embodiment, a bellows-like shape or a wrinkled shape may be formed in a part of the conductive layer 442 in a cross section obtained by cutting the conductive layer 442 at a first cut surface which is a plane including the approximate center 1522 of the integrated region 1520 and approximately parallel to the stacking direction (z direction in the figure) of the positive electrode current collector 222. In another embodiment, a bellows-like shape or a wrinkled shape may be formed in a part of the conductive layer 442 in both (i) a cross section obtained by cutting the conductive layer 442 at the first cut surface and (ii) a cross section obtained by cutting the conductive layer 442 at a second cut surface which is a plane including the approximate center 1522 of the integrated region 1520 and approximately parallel to the stacking direction (z direction in the figure) of the positive electrode current collector 222 and different from the first cut surface.

[0289] Similarly, in the uneven region of the conductive layer 444, the conductive layer 444 has a bellows-like shape or a wrinkled shape. The uneven region of the conductive layer 444 includes a plurality of peaks and at least one valley that are arranged side by side along the in-plane direction of the conductive layer 444. As a result, wrinkles are formed on the surface of the conductive layer 444.

[0290] In a plane (xy plane in the drawing) approximately parallel to the stacking direction of the positive electrode current collector 222, the uneven region of the conductive layer 444 may extend in a single direction from the end of the integrated region 1520, or may extend in multiple directions. The shape of the uneven region in a plane approximately parallel to the stacking direction of the positive electrode current collector 222 may be approximately rectangular, approximately circular, or approximately sector-shaped. The shape of the uneven region in a plane approximately parallel to the stacking direction of the positive electrode current collector 222 may be approximately concentric circular, or approximately concentric polygonal.

[0291] In one embodiment, a bellows-like shape or a wrinkled shape may be formed in a part of the conductive layer 444 in a cross section obtained by cutting the conductive layer 444 at a first cut surface which is a plane including the approximate center 1522 of the integrated region 1520 and approximately parallel to the stacking direction (z direction in the figure) of the positive electrode current collector 222. In another embodiment, a bellows-like shape or a wrinkled shape may be formed in a part of the conductive layer 444 in both (i) a cross section obtained by cutting the conductive layer 444 at the first cut surface and (ii) a cross section obtained by cutting the conductive layer 444 at a second cut surface which is a plane including the approximate center 1522 of the integrated region 1520 and approximately parallel to the stacking direction (z direction in the figure) of the positive electrode current collector 222 and different from the first cut surface.

[0292] The plurality of conductive layers 442 may include the above-described uneven regions, and the plurality of conductive layers 444 may include the above-described uneven regions. The shapes of the uneven regions formed in each of the plurality of conductive layers 442 may be substantially the same or substantially similar, or may be different. The shapes of the uneven regions formed in each of the plurality of conductive layers 444 may be substantially the same or substantially similar, or may be different.

[0293] It is preferable that 30% or more of the total number of conductive layers included in the laminate have the above-mentioned uneven region. 80% or more of the total number of conductive layers included in the laminate may have the above-mentioned uneven region. This significantly suppresses the above-mentioned variation in resistance between the conductive layers.

[0294] 16 and 17 show an example of a cross section taken along line AA of region 1540 enclosed by a dotted line in FIG. 15. As shown in FIG. 15, region 1540 includes a portion of the smooth region, an adjacent region, and a portion of the integrated region. Region 1540 includes an approximate center 1522 of integrated region 1520.

[0295] 16 and 17, in this embodiment, three conductive layers 442 included in three positive electrode current collectors 222 have an uneven region 1600. In addition, two conductive layers 444 included in three positive electrode current collectors 222 have an uneven region 1600. In this embodiment, the conductive layer 444 in contact with the lead 822 does not have an uneven region 1600. As shown in FIG. 16, in this embodiment, the uneven region 1600 of each conductive layer is formed in a part of an adjacent region 1620 of the stack.

[0296] As discussed above, the adjacent region 1620 of the laminate is disposed between the integrated region 1520 of the laminate and the smooth region 1640 of the laminate. The adjacent region 1620 of the laminate may be disposed adjacent the integrated region 1520 of the laminate. The adjacent region 1620 may include at least a portion of the softened region discussed above.

[0297] The position of the end of the integrated region 1520 is determined by the method described above. As described above, the smooth region 1640 is a region that is sufficiently distant from the end of the integrated region 1520 and has a sufficiently small flatness on the surface of the laminated positive electrode current collector 222. The smooth region 1640 may be a region whose shape is almost unchanged before and after the welding process.

[0298] Whether or not a particular region corresponds to the smooth region 1640 is determined, for example, by the following procedure. First, the thickness of the laminated positive electrode current collector 222 is measured at three positions (sometimes referred to as measurement positions) that are located outside the integrated region 1520 and arranged on a straight line passing through the approximate center 1522 of the integrated region 1520. The interval between the three measurement positions (sometimes referred to as the measurement interval) is preferably 0.1 mm or more, but the measurement interval can be appropriately set depending on the size of the sample.

[0299] When the absolute value of the difference between the maximum and minimum values ​​of the three measured values ​​is 5% or less of the average value of the three measured values, the particular region may be determined to be a smooth region 1640. In this case, the thickness Hs of the laminated positive electrode current collector 222 in the smooth region 1640 may be the average value of the above three measured values.

[0300] 17, in this embodiment, the maximum thickness Hmax of the stacked positive electrode current collectors 222 in the adjacent region 1620 of the laminate is greater than the thickness Hs of the stacked positive electrode current collectors 222 in the smooth region 1640. The value of Hmax may be 1.0 to 1.5 times the value of Hs, or 1.1 to 1.3 times the value of Hs. When the value of Hmax is within the above numerical range, application of excessive pressure to the weld point is suppressed. As a result, the strength of the weld is improved.

[0301] Fig. 18 shows a schematic example of a cross section of one of the three positive current collectors 222 shown in Fig. 16 and Fig. 17. As shown in Fig. 18, the conductive layer 442 of the positive current collector 222 includes an uneven region 1600. In this embodiment, the uneven region 1600 of the conductive layer 442 includes a plurality of peaks and valleys arranged side by side along the extension direction of the conductive layer 442 in the cross section (the x direction in the figure).

[0302] In this embodiment, the conductive layer 444 of the positive electrode current collector 222 also includes an uneven region 1600. In this embodiment, the uneven region 1600 of the conductive layer 444 includes a plurality of peaks and valleys arranged side by side along the extension direction of the conductive layer 444 in the cross section (the x-direction in the drawing).

[0303] In this embodiment, the maximum length Smax of adjacent peaks and valleys in the uneven region 1600 is greater than the thickness Hf of a single positive electrode current collector 222 in the smooth region 1640. The value of Smax may be 1.1 to 2 times the value of Hf, or may be 1.2 to 1.5 times the value of Hf.

[0304] In this embodiment, the maximum distance Fmax between two adjacent peaks may be 10 to 200 μm, or 20 to 70 μm. The value of Fmax may be 2 to 20 times the value of Hf, or 3 to 10 times the value of Hf.

[0305] The positive electrode current collector 222 has a thickness of at least 5 to 7 μm, for example. Therefore, by observing an SEM image, an X-ray CT image, or the like, it is possible to distinguish between an uneven region formed by welding and fine unevenness that is unavoidably formed during the manufacture of the conductive layer 442 and / or the conductive layer 444.

[0306] In this embodiment, the number N of peaks arranged in the uneven region 1600 may be 2 or more, or may be 3 or more. The number N of peaks is preferably 6 or more, and may be 10 or more. The greater the number of peaks, the greater the weld strength.

[0307] The conductive layer 442 in which the uneven region is formed may be an example of a first metal layer including an uneven region. The extension direction of the conductive layer 442 may be an example of an in-plane direction of a metal layer. The conductive layer 444 in which the uneven region is formed may be an example of a second metal layer including an uneven region. The extension direction of the conductive layer 444 may be an example of an in-plane direction of a metal layer. The peaks of the uneven region 1600 may be an example of peak portions. The valleys of the uneven region 1600 may be an example of valley portions.

[0308] Figure 19 illustrates a schematic example of an uneven region 1900. Another example of a cross section of one of the three positive current collectors 222 illustrated in Figures 16 and 17 is illustrated. As illustrated in Figure 19, the conductive layer 442 of the positive current collector 222 includes an uneven region 1900.

[0309] 16 to 18 in that uneven region 1900 of conductive layer 442 has a region that does not include a valley between two adjacent peaks. Also, uneven region 1900 of conductive layer 442 has a region that does not include a peak between two adjacent valleys. Also, uneven region 1900 of conductive layer 442 has a region that does not include a peak between two adjacent valleys.

[0310] Except for the above differences, uneven region 1900 of conductive layer 442 may have the same configuration as uneven region 1600 described with reference to Figures 16 to 18. For example, in this embodiment, uneven region 1900 of conductive layer 442 includes a plurality of peaks and valleys arranged side by side along the extension direction (x direction in the figure) of conductive layer 442 in the above cross section. In other words, uneven region 1900 includes a region where peaks, valleys, and peaks are arranged in this order.

[0311] Fig. 20 shows another example of a cross section of the positive electrode connecting part 820. The positive electrode connecting part 820 described with reference to Fig. 20 differs from the positive electrode connecting part 820 described with reference to Figs. 15 to 19 in that a composite region 2020 is disposed between the integrated region 1520 and the adjacent region 1620 or in a part of the adjacent region 1620. The positive electrode connecting part 820 described with reference to Figs. 15 to 19 may have a similar configuration to the positive electrode connecting part 820 described with reference to Figs. 15 to 19 except for the above differences.

[0312] In the composite region 2020 of the laminate, at least a portion of the conductive layer 442 and the conductive layer 444 maintains a foil-like shape and is integrated with the metal of the lead 822 and / or the sub-lead 824. For example, in the composite region 2020 of the laminate, the laminate has a solid 2022 between adjacent conductive layers 442 and 444 that is formed by melting and solidifying the metal of the lead 822 and / or the sub-lead 824 in the welding process.

[0313] Fig. 21 shows a schematic diagram of yet another example of a cross section of a positive electrode connecting portion 820. The positive electrode connecting portion 820 described with reference to Fig. 21 differs from the positive electrode connecting portion 820 described with reference to Figs. 15 to 20 in that the adjacent region 1620 is covered with a sub-lead 824 and that a composite region 2020 is provided. The positive electrode connecting portion 820 described with reference to Figs. 15 to 20 may have a similar configuration to the positive electrode connecting portion 820 described with reference to Figs. 15 to 20 except for the above differences. EXAMPLES

[0314] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples.

[0315] (Preparation of negative electrode current collector) (Production Example 1) Six negative electrode current collectors were prepared by the following procedure. First, a PET film (Toray Industries, Inc., Lumirror #19-F60, thickness 6 μm) was prepared as a support layer for the negative electrode current collector. Next, Ni layers with a thickness of about 0.1 μm were formed on both sides of the PET film by electroless plating. Next, copper layers with a thickness of 0.5 μm were formed on the Ni layers on each side of the PET film by electrolytic plating.

[0316] Next, a plurality of through holes were formed in a part of the PET film. This resulted in the formation of a through hole band. The cross-sectional shape of each through hole was circular, and the average diameter of each through hole was 30 μm. The pitch of the through holes was 80 μm.

[0317] Next, a copper layer was formed on the inner wall of the through hole by the same procedure as the copper layer on the PET film surface. The thickness of the copper layer was 0.5 μm. The average diameter of the space of the through hole after the copper layer was formed was 29 μm.

[0318] Thereafter, the PET film with the through-hole band and the copper layer in the through-hole was cut to prepare six current collectors. The PET film was cut so that each current collector had an L-shaped planar shape having a rectangular current collector portion of 38 mm x 50 mm and a rectangular tab portion of 10 mm x 5 mm. In each current collector, the PET film was cut so that the short side of the tab portion was in contact with one of the short sides of the current collector portion. In each current collector, the PET film was cut so that one of the other long sides of the tab portion and one of the long sides of the current collector portion were arranged on the same straight line.

[0319] As described in relation to FIG. 12, the PET film was cut so that the through-hole band formed in the PET film was included in the tab portion. As described above, the TL of the tab portion of each current collector was 10 mm, and the TW was 5 mm. A through-hole band was formed in the tab portion of each current collector, and the HL of each current collector was 2 mm, and the HW was 5 mm. The distance from the side of the tab portion that contacted the current collecting portion to the through-hole band was 6 mm. The distance from the side of the tab portion opposite to the side that contacted the current collecting portion to the through-hole band was 2 mm.

[0320] As a result, six negative electrode current collectors were obtained. The specifications of the negative electrodes are shown in Table 1.

[0321] (Production Example 2) Six negative electrode current collectors were produced in the same manner as in Production Example 1, except that a single through hole having a diameter of 500 μm was formed instead of a through hole band consisting of multiple through holes. Table 1 shows the specifications of the negative electrode.

[0322] (Production Example 3) Six negative electrode current collectors were produced in the same manner as in Production Example 1, except that a polyimide film (Kapton, manufactured by Toray DuPont, thickness 6 μm) was used as the support layer for the negative electrode current collector. Table 1 shows the specifications of the negative electrodes.

[0323] (Production Example 4) Six negative electrode current collectors were produced in the same manner as in Production Example 2, except that a polyimide film (Kapton, manufactured by Toray DuPont, thickness 6 μm) was used as the support layer for the negative electrode current collector. Table 1 shows the specifications of the negative electrodes.

[0324] (Production Example 5) First, a Cu foil (manufactured by AS ONE Corporation, model number 3-2349-01, thickness 10 μm) was prepared as a support layer for the negative electrode current collector. Next, the Cu foil was cut in the same manner as in Production Example 1 to prepare six current collectors. Table 1 shows the specifications of the negative electrode.

[0325] [Table 1]

[0326] Example 1 (Production of lithium-ion secondary batteries) First, six current collectors obtained in Production Example 1 were prepared as negative electrode current collectors. Five sheets of Al foil (manufactured by MTI Corporation, BCAF-15U180, dimensions 34 mm x 46 mm, thickness 15 μm) were prepared as positive electrode current collectors. The planar shape of the Al foil was an L-shape having a rectangular current collecting portion of 34 mm x 46 mm and a rectangular tab portion of 10 mm x 5 mm.

[0327] As the negative electrode active material, a 38 mm x 50 mm Li metal foil (Honjo Metals Co., Ltd., rolled lithium foil, thickness 20 μm) was prepared. As the positive electrode active material, NCM811 (Nichia Chemical Industries Co., Ltd.) was prepared. As the separator, 10 sheets of SW316F (Shenzhen Staryuan Materials Co., Ltd., thickness 10 μm) were prepared. The planar shape of the separator was a rectangle of 42 mm x 54 mm.

[0328] Next, NCM811, Denka Black (manufactured by Denka Co., Ltd.), and PVDF (#1100 manufactured by Kureha Trading Co., Ltd.) were added to N-methylpyrrolidone (Mitsubishi Chemical Co., Ltd.) to prepare a slurry of a positive electrode active material. The mass ratio of NCM811, Denka Black, and PVDF was 94:3:3. The above slurry was applied to the entire surface of the Al foil. The above slurry was applied to both sides of the Al foil. The slurry was then dried to obtain a positive electrode in which a positive electrode active material layer was formed on both sides of the Al foil. The thickness of the positive electrode active material layer after drying was 50 μm per side. As a result, five positive electrodes were obtained. The thickness of each positive electrode was 115 μm.

[0329] Next, the above Li metal foil was attached to both sides of the current collector obtained in Production Example 1. In this way, six negative electrodes were obtained.

[0330] Next, an electrolyte solution (LBG-00062, manufactured by Kishida Chemical Co., Ltd.) was prepared. In the electrolyte solution, the solvent was a mixed solvent of ethylene carbonate and ethyl methyl carbonate, and the volume ratio of ethylene carbonate to ethyl methyl carbonate was 1:3. In the electrolyte solution, LiPF 6 The concentration was 1 mol / L.

[0331] Next, a battery structure was produced by stacking the negative electrode, separator, positive electrode, separator, negative electrode, separator, positive electrode, separator, negative electrode, separator, positive electrode, separator, negative electrode, separator, positive electrode, separator, negative electrode, separator, positive electrode, separator, negative electrode in this order. A Cu plate (manufactured by Nets Corporation, thickness 100 μm) coated with a 0.1 μm thick Ni layer was cut to produce a lead for the negative electrode. The planar shape of the lead was a rectangle of 40 mm × 15 mm. A Cu plate (manufactured by Nets Corporation, thickness 30 μm) coated with a 0.1 μm thick Ni layer was cut to produce a sub-lead for the negative electrode. The planar shape of the sub-lead was a square of 15 mm × 15 mm. Similarly, an Al plate (manufactured by Nets Corporation, thickness 100 μm) was cut to produce a lead for the positive electrode. The planar shape of the lead was a rectangle of 40 mm x 15 mm.

[0332] Next, the five stacked positive electrode tabs were integrated. Specifically, the five positive electrode tabs were first stacked, and then the positive electrode lead was placed on the topmost tab. This produced a laminate to be welded in the welding process on the positive electrode side. As described above, the positive electrode current collector was an Al foil, and the positive electrode lead was an Al plate.

[0333] The five Al foils and one Al plate were welded together using a lithium-ion battery laminated foil welding device (manufactured by Nag Systems Co., Ltd.) equipped with a welding head with a nugget diameter of 4 mm. This resulted in the five positive electrode tabs being integrated together.

[0334] Next, the six stacked negative electrode tabs were integrated. Specifically, the six negative electrode tabs were first stacked, and then the six stacked tabs were sandwiched between the negative electrode lead and the sub-lead. This produced a stack that was to be welded in the welding process on the negative electrode side.

[0335] A 4 mm x 4 mm area on the inside of the sub-lead was set as the softened area. The position of the softened area was set so that the approximate center of the softened area coincided with the approximate center of the tab portion. A 2 mm x 2 mm area on the inside of the sub-lead was set as the welded area. The position of the welded area was set so that the approximate center of the welded area coincided with the approximate center of the softened area.

[0336] The above welding objects (i.e., the sub-lead, the six tab portions, and the laminate of the leads) were placed in the working area of ​​a welding device. A lithium-ion battery laminate foil welding device (manufactured by Nag System Co., Ltd.) equipped with a welding head with a nugget diameter of 4 mm was used as the welding device.

[0337] First, the softened region of the sub-lead was pressed using the welding head of the welding device, and a pressure of 1.8 kN was applied to the softened region of the sub-lead. Next, power was supplied to the heating section of the welding device to heat the softened region. The power supply conditions during heating were a current of 1.5 kA, a voltage of 3 V, and an application time of 10 ms. After the power supply to the heating section was stopped, power was supplied to the welding section of the welding device to weld the welded region. The length of the period from when the power supply to the heating section was stopped to when the power supply to the welding section was started was set to 1 ms. The power supply conditions during welding were a current of 2.5 kA, a voltage of 3.5 V, and an application time of 20 ms. In this way, an electrode structure was produced.

[0338] Next, a compression test was performed on the welded portion of the negative electrode using a heater plate press (PCH-100-DAH, manufactured by LabNect Co., Ltd.) having a plate of 80 mm square. The compression test was performed at room temperature. A pressure of 506.625 kPa was applied to the entire sub-lead. The pressure was applied for 20 seconds.

[0339] Next, the electrode structure after the compression test and the above-mentioned electrolyte were placed inside an aluminum laminate packaging material, and the laminate packaging material was then sealed. This produced a test battery. The specifications of the test battery are shown in Table 2.

[0340] Example 2 A test battery was produced in the same manner as in Example 1, except that a tensile test was conducted on the welded portion of the negative electrode instead of a compression test on the welded portion. The specifications of the test battery are shown in Table 2.

[0341] The tensile test was carried out using a tensile compression tester (Force Tester MCT-2150W, manufactured by A&D Co., Ltd.) according to the following procedure. First, the lead was set on one side of the sample jig of the tensile compression tester, and the base of the tab portion was set on the other side of the sample jig. Next, the tensile compression tester was used to perform a tensile test at 5 N / mm 2 The base of the lead and tab were pulled with a force of 1000 MPa. The tensile strength was gradually increased, and the tensile test was terminated when the displacement reached 5% strain from before the test.

[0342] Example 3 A test battery was produced in the same manner as in Example 1, except that the current collector obtained in Production Example 2 was used as the negative electrode current collector. The specifications of the test battery are shown in Table 2.

[0343] Example 4 A test battery was produced in the same manner as in Example 2, except that the current collector obtained in Production Example 2 was used as the negative electrode current collector. The specifications of the test battery are shown in Table 2.

[0344] Comparative Example 1 A test battery was produced in the same manner as in Example 1, except that the current collector obtained in Production Example 3 was used as the negative electrode current collector. The specifications of the test battery are shown in Table 2.

[0345] Comparative Example 2 A test battery was produced in the same manner as in Example 2, except that the current collector obtained in Production Example 3 was used as the negative electrode current collector. The specifications of the test battery are shown in Table 2.

[0346] Comparative Example 3 A test battery was produced in the same manner as in Example 1, except that the current collector obtained in Production Example 4 was used as the negative electrode current collector. The specifications of the test battery are shown in Table 2.

[0347] Comparative Example 4 A test battery was produced in the same manner as in Example 2, except that the current collector obtained in Production Example 4 was used as the negative electrode current collector. The specifications of the test battery are shown in Table 2.

[0348] (Reference example 1) A test battery was produced in the same manner as in Example 1, except that the current collector obtained in Production Example 5 was used as the negative electrode current collector. The specifications of the test battery are shown in Table 2.

[0349] (Reference example 2) A test battery was produced in the same manner as in Example 2, except that the current collector obtained in Production Example 5 was used as the negative electrode current collector. The specifications of the test battery are shown in Table 2.

[0350] (Reference example 3) A test battery was produced in the same manner as in Example 1, except that the current collector obtained in Production Example 5 was used as the negative electrode current collector and that the compression test of the welded portion was not performed. The specifications of the test battery are shown in Table 2. The test battery of Reference Example 3 was used as a reference for the cycle test described later.

[0351] [Table 2]

[0352] (evaluation) (Cycle performance) The test batteries prepared in each of Examples 1 to 4, Comparative Examples 1 to 4, and Reference Examples 1 to 3 were used to evaluate the cycle characteristics of each test battery under conditions of 4.2 V to 2.4 V. Specifically, charging and discharging at a constant current were repeated 100 cycles, and the charge capacity, discharge capacity, and voltage values ​​during charging and discharging were recorded. The charge time per cycle was 10 hours, and the discharge time per cycle was 2 hours. The charging conditions were a temperature of 25° C. and a current density of 1.53 mA / cm. 2 The discharge conditions were a temperature of 25°C and a current density of 7.67mA / cm.2 and the current value was 120 mA.

[0353] The results of the cycle tests for each test battery are shown in Table 2. In Table 2, ◎ indicates that the capacity retention rate after 100 cycles of the test battery of Reference Example 3 is set as a reference value, and the test battery has a performance of 90% or more of the reference value. ◯ indicates that the test battery has a performance of 80% or more and less than 90% of the above reference value. △ indicates that the test battery has a performance of 70% or more and less than 80% of the above reference value. × indicates that the test battery has a performance of less than 70% of the above reference value.

[0354] (Observation of the negative electrode welding points) The welded portions of the negative electrodes of the test batteries fabricated in each of Examples 1 to 4, Comparative Examples 1 to 4, and Reference Examples 1 to 3 were observed to confirm the presence or absence of the above-described uneven regions. The results are shown in Table 2.

[0355] The presence or absence of unevenness was confirmed according to the following procedure. First, a sample including the welded region of the negative electrode was cut out from the negative electrode of each test battery. The size of each sample was 50 mm x 50 mm, and the welded region was located approximately in the center of each sample.

[0356] Next, X-CT observation was performed on the samples of each Example and Comparative Example. For the X-CT observation, an X-ray microscope (SKYSCAN 1272 CMOS EDITION) manufactured by BRUKER was used. The above-mentioned bellows shape was observed in all Examples. On the other hand, the above-mentioned bellows shape was not observed in the samples of each Comparative Example. Therefore, SEM observation was performed on the samples of each Comparative Example. First, the samples of each Comparative Example were cut using a cross-section polisher (manufactured by JEOL Ltd., product number IB-09020CP). Each sample was cut so that the cut surface included approximately the center of the welded region. Next, the cut surface was observed by SEM.

[0357] FIG. 22 shows the X-CT observation result of the welded portion of the negative electrode produced in Example 2. FIG. 22 is an X-CT image when the sample is observed from the lead side and the depth of the observation surface is appropriately adjusted. Specifically, the image is taken by observing the sample at an angle with the lead side as the front so that the lead is not reflected except for the welded portion. The approximately circular area near the center of FIG. 22 is the welded area. As shown in FIG. 22, according to this example, it can be seen that a plurality of wrinkles having an approximately circular or approximately polygonal shape are arranged in a concentric circle shape or a concentric polygon shape. For example, in the observation area 2200, a plurality of wrinkles are formed adjacent to the welded area.

[0358] Fig. 23 shows the results of X-CT observation of the cross section of the observation region 2200 shown in Fig. 22. As shown in Fig. 23, according to this embodiment, it can be seen that a plurality of wrinkles or bellows shapes are formed not only inside the observation region 2300 sandwiched between the lead and the sub-lead, but also outside the observation region 2300. Specifically, at least three peaks are observed outside the observation region 2300.

[0359] Fig. 24 shows the X-CT observation result of the observation region 2300 shown in Fig. 23. As shown in Fig. 23, according to this embodiment, it can be seen that many wrinkles or bellows shapes are formed even inside the observation region 2300 sandwiched between the lead and the sub-lead.

[0360] Fig. 25 shows an SEM image of the welded portion of the negative electrode produced in Comparative Example 1. Fig. 25 shows a cross section of an adjacent region adjacent to the welded region. As shown in Fig. 25, according to this Comparative Example, the copper layers formed on both sides of the negative electrode current collector are broken by the resin material extruded from the welded region.

[0361] Although the present invention has been described above using the embodiments, the technical scope of the present invention is not limited to the scope described in the above embodiments. It is clear to those skilled in the art that various modifications and improvements can be made to the above embodiments. It is clear from the description of the claims that such modifications and improvements can also be included in the technical scope of the present invention.

[0362] It should be noted that the order of execution of each process, such as operations, procedures, steps, and stages, in the devices, systems, programs, and methods shown in the claims, specifications, and drawings is not specifically stated as "before" or "prior to," and that the process may be performed in any order unless the output of a previous process is used in a later process. Even if the operational flow in the claims, specifications, and drawings is described using "first," "next," and the like for convenience, this does not mean that the process must be performed in this order. [Explanation of symbols]

[0363] 100 aircraft, 110 storage battery, 112 storage cell, 120 power control circuit, 130 motor, 140 propeller, 150 sensor, 160 control device, 212 positive electrode case, 214 negative electrode case, 216 sealant, 218 metal spring, 220 positive electrode, 222 positive electrode current collector, 224 positive electrode active material layer, 230 separator, 240 negative electrode, 242 negative electrode current collector, 244 negative electrode active material layer, 260 structure, 350 electrolyte, 400 current collector, 420 support layer, 422 first plane, 424 second plane, 426 side, 442 conductive layer, 444 conductive layer, 500 current collector, 522 through hole, 546 conductive material, 600 current collector, 620 Through hole, 622 inner wall portion, 642 conductive layer, 760 laminated structure, 820 positive electrode connection portion, 822 lead, 824 sub-lead, 840 negative electrode connection portion, 842 lead, 844 sub-lead, 1102 current collector, 1104 current collector, 1120 welding device, 1130 welding head, 1132 position adjustment portion, 1134 heating portion, 1136 welding portion, 1140 heating power source, 1150 welding power source, 1160 controller, 1520 integrated region, 1522 approximately center, 1540 region, 1600 uneven region, 1620 adjacent region, 1640 smooth region, 1900 uneven region, 2020 composite region, 2022 solid, 2200 observation region, 2300 observation region

Claims

1. A plurality of sheets of material stacked together; Each of the plurality of sheet materials comprises: A support layer including a thermoplastic resin material; a first metal layer and a second metal layer formed on both sides of the support layer; having In some of the plurality of sheet materials, the plurality of first metal layers and the plurality of second metal layers included in the plurality of sheet materials are integrated together, Each of the first metal layers and the second metal layers includes a concave-convex region in which each metal layer has a bellows-like or wrinkled shape. Laminate.

2. In the uneven region, the first metal layers and the second metal layers are not integrated together; Each metal layer includes a plurality of peaks and at least one valley arranged side by side along an in-plane direction of each metal layer. The laminate according to claim 1 .

3. The uneven region is disposed adjacent to an integrated region, which is a region where the plurality of first metal layers and the plurality of second metal layers are integrated. The laminate according to claim 1 .

4. a ratio of a volume of a resin contained in an integrated region to a volume of a metal contained in the integrated region, which is a region where the plurality of first metal layers and the plurality of second metal layers are integrated, is 5 to 50%; The laminate according to claim 1 .

5. a ratio of a volume of voids included in an integrated region, which is a region where the plurality of first metal layers and the plurality of second metal layers are integrated, to a volume of metal included in the integrated region is 10% or less; The laminate according to claim 1 .

6. The plurality of sheets of material include a first sheet material disposed on an outermost side of one side of the plurality of sheet materials; a second sheet material disposed on the outermost side of the other side of the plurality of sheet materials; having The laminate comprises: a first support member supporting the first sheet material; a second support member supporting the second sheet material; Further equipped with the first support member and the second support member include a metal; the first support member, the second support member, the first metal layers, and the second metal layers are integrated in the portion of the plurality of sheet materials; The laminate according to claim 1 .

7. Each of the plurality of sheet materials has a region in which a plurality of through holes are formed penetrating each sheet material, in the vicinity of an integrated region where the plurality of first metal layers and the plurality of second metal layers are integrated. The laminate according to claim 1 .

8. a conductive member electrically connecting the first metal layer and the second metal layer disposed on each of the plurality of sheet materials; The laminate according to claim 1 .

9. A first electrode and a second electrode; A third electrode; A first separator and a second separator; Equipped with the first electrode, the first separator, the third electrode, the second separator, and the second electrode are laminated in this order; Each of the first electrode and the second electrode is A current collector; an active material layer disposed on at least one surface of the current collector; having The current collector is A support layer including a thermoplastic resin material; a first metal layer and a second metal layer formed on both sides of the support layer; Including, the first metal layer and the second metal layer of the first electrode, and the first metal layer and the second metal layer of the second electrode are integrated in the vicinity of ends of the first electrode and the second electrode, The first metal layer and the second metal layer of the first electrode, and the first metal layer and the second metal layer of the second electrode each include an uneven region having a bellows-like shape or a wrinkled shape. Electrode structure.

10. A fourth electrode; and A third separator; and Further equipped with the first electrode, the first separator, the third electrode, the second separator, the second electrode, the third separator, and the fourth electrode are laminated in this order, Each of the first electrode, the second electrode, the third electrode, and the fourth electrode is The current collector; The active material layer; having the first metal layer and the second metal layer of the third electrode, and the first metal layer and the second metal layer of the fourth electrode are integrated in the vicinity of ends of the third electrode and the fourth electrode, The first metal layer and the second metal layer of the third electrode, and the first metal layer and the second metal layer of the fourth electrode each include an uneven region having a bellows-like shape or a wrinkled shape. The electrode structure of claim 9.

11. The electrode structure according to claim 9 ; A housing that houses the electrode structure; Equipped with a battery.

12. A battery according to claim 11; a thrust generating device that generates thrust by utilizing the electric energy stored in the battery; An aircraft equipped with

Citation Information

Patent Citations

  • Nonaqueous secondary battery

    JP2012155974A

  • Nonaqueous secondary battery, and method of manufacturing the same

    JP2013008564A

  • Manufacturing method, program, manufacturing system, laminated current collector, and battery

    JP2021097020A

  • Battery structure, battery, manufacturing method, program, and manufacturing apparatus

    JP2022131562A

  • Manufacturing method, program, manufacturing system, laminated collector, battery, moving body, and flight body

    JP2023000600A