Composition, magnetic particles-containing membrane, and electronic component
A magnetic particle composition with specific metal atoms and rheology control enhances isotropy and stability, addressing the challenges of existing films in achieving both properties.
Patent Information
- Application Number
- JP2024119371
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-06-09
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-06-08
AI Technical Summary
Existing magnetic particle-containing films face challenges in achieving both magnetic isotropy and long-term stability, particularly when using a high proportion of flat soft magnetic particles.
A composition comprising magnetic particles with an aspect ratio less than 8, containing metal atoms like Ni or Co, and a rheology control agent, with specific atom content and particle size, to enhance isotropy and stability.
The composition forms a magnetic particle-containing film with excellent magnetic isotropy and improved stability over time, suitable for use in electronic components.
Smart Images

Figure 2024149513000001 
Figure 2024149513000002 
Figure 2024149513000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition, a magnetic particle-containing film, and an electronic component. [Background technology]
[0002] As electronic devices become more compact and powerful, the integration of electronic circuits is increasing. Coating-type compositions containing magnetic particles are one of the materials that can improve integration. By using such compositions, magnetic bodies can be mounted in any shape, making it easier to realize smaller electronic devices with higher performance than the conventional method of placing individual pieces of magnetic bodies on a chip.
[0003] For example, Patent Document 1 discloses "a soft magnetic resin composition characterized by containing flat soft magnetic particles, a resin component, and a rheology control agent." [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-082554 A Summary of the Invention [Problem to be solved by the invention]
[0005] Meanwhile, the composition is required to have good stability over time. Furthermore, there are cases where a magnetic film is required to have isotropic magnetism. The present inventors have studied the composition (soft magnetic resin composition) described in Patent Document 1 and have confirmed that the use of a large amount of flat soft magnetic particles improves the temporal stability of the composition to a certain degree. However, it has also been confirmed that the use of a large amount of flat soft magnetic particles makes it difficult for the magnetism of a film formed from the composition to become isotropic.
[0006] Therefore, an object of the present invention is to provide a composition capable of forming a magnetic particle-containing film having excellent magnetic isotropy and excellent stability over time. Another object of the present invention is to provide a magnetic particle-containing film related to the composition, and an electronic component including the magnetic particle-containing film. [Means for solving the problem]
[0007] As a result of intensive research by the present inventors to solve the above problems, they have found that the above problems can be solved by the following configuration.
[0008] [1] A composition comprising magnetic particles and a rheology control agent, the content of the magnetic particles having an aspect ratio of less than 8 is 25% by mass or more based on the total mass of the magnetic particles; The magnetic particles contain metal atoms, The metal atom contains one or more specific atoms selected from the group consisting of Ni atoms and Co atoms, A composition, wherein the content of the specific atom is 50 mass % or more based on the total mass of the metal atoms. [2] The composition according to [1], wherein the specific atom is the Ni atom. [3] The composition according to [1] or [2], wherein the content of the specific atom is 70 mass% or more based on the total mass of the metal atoms. [4] The composition according to any one of [1] to [3], wherein the magnetic particles have a particle size of 5 μm or more. [5] The composition according to any one of [1] to [4], wherein the rheology control agent is an organic rheology control agent. [6] The composition according to any one of [1] to [5], wherein the rheology control agent is at least one selected from the group consisting of polycarboxylic acids, polycarboxylic anhydrides, and amide waxes. [7] The composition according to any one of [1] to [6], further comprising an epoxy curable compound as a polymerizable compound. [8] A magnetic particle-containing film formed using the composition according to any one of [1] to [7]. [9] An electronic component comprising the magnetic particle-containing film according to [8].
[10] The electronic component according to [9], which is used as an inductor.
[11] The electronic component according to [9], which is used as an antenna. Effect of the Invention
[0009] According to the present invention, it is possible to provide a composition capable of forming a magnetic particle-containing film having excellent magnetic isotropy and excellent stability over time. The present invention also provides a magnetic particle-containing film relating to the composition, and an electronic component including the magnetic particle-containing film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below. The following description of the components may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment. In the present specification, the notation of groups (atomic groups) that does not indicate whether they are substituted or unsubstituted includes both unsubstituted and substituted groups, unless it is contrary to the spirit of the present invention. For example, an "alkyl group" includes not only an alkyl group that does not have a substituent (unsubstituted alkyl group), but also an alkyl group that has a substituent (substituted alkyl group). In addition, an "organic group" in the present specification refers to a group that contains at least one carbon atom.
[0011] In this specification, "actinic rays" or "radiation" refers to, for example, the bright line spectrum of a mercury lamp, far ultraviolet light represented by an excimer laser, extreme ultraviolet light (EUV light: extreme ultraviolet), X-rays, and electron beams (EB), etc. In this specification, "light" refers to actinic rays or radiation. In this specification, unless otherwise specified, "exposure" includes not only exposure to the emission spectrum of a mercury lamp, far ultraviolet light represented by an excimer laser, extreme ultraviolet light, X-rays, EUV light, and the like, but also drawing with particle beams such as electron beams and ion beams.
[0012] In this specification, the symbol "to" is used to mean that the numerical values before and after it are included as the lower limit and upper limit.
[0013] In this specification, (meth)acrylate refers to acrylate and methacrylate, (meth)acrylic refers to acrylic and methacrylic, and (meth)acryloyl refers to acryloyl and methacryloyl.
[0014] In this specification, the "solid content" of a composition means the components that form a magnetic particle-containing film, and when the composition contains a solvent (organic solvent, water, etc.), it means all components excluding the solvent. In addition, liquid components are also considered to be solid contents if they form a magnetic particle-containing film.
[0015] In this specification, the weight average molecular weight (Mw) is a value calculated as polystyrene by the GPC (Gel Permeation Chromatography) method. In this specification, the GPC method is based on a method using HLC-8020GPC (manufactured by Tosoh Corporation), TSKgel SuperHZM-H, TSKgel SuperHZ4000, and TSKgel SuperHZ2000 (manufactured by Tosoh Corporation, 4.6 mm ID x 15 cm) as columns, and THF (tetrahydrofuran) as an eluent.
[0016] In addition, in this specification, unless otherwise specified, each component may be used alone or in combination of two or more substances corresponding to each component. Here, when two or more substances are used in combination for each component, the content of the component refers to the total content of the substances used in combination, unless otherwise specified.
[0017] [Composition] The composition of the present invention is a composition containing magnetic particles and a rheology control agent, the content of the magnetic particles having an aspect ratio of less than 8 is 25% by mass or more based on the total mass of the magnetic particles; The magnetic particles contain metal atoms, The metal atom contains one or more specific atoms selected from the group consisting of Ni atoms and Co atoms, The content of the specific atom is 50 mass % or more based on the total mass of the metal atoms. Although the details of why the problem of the present invention can be solved by having such a composition are not clear, it is generally presumed as follows.
[0018] When a predetermined amount or more of magnetic particles having an aspect ratio of less than 8 are contained, the magnetic particles are arranged isotropically in the magnetic particle-containing film, and the isotropy of magnetism in the magnetic particle-containing film can be improved. On the other hand, magnetic particles having an aspect ratio of less than 8 tend to settle in the composition compared to magnetic particles having an aspect ratio of 8 or more, and a large content of magnetic particles having an aspect ratio of less than 8 tends to adversely affect stability over time. In order to improve such problems, a rheology control agent may be applied to the composition, but the improvement in stability over time was insufficient only by applying the rheology control agent. Therefore, in the composition of the present invention, in addition to containing magnetic particles and a rheology control agent, it is also specified that the magnetic particles contain a predetermined amount or more of one or more specific atoms selected from the group consisting of Ni atoms and Co atoms. Since specific atoms are less likely to be ionized than atoms such as iron, the magnetic particles having the above-mentioned characteristics can achieve a moderate interaction with the rheology control agent without excessive interaction. Therefore, the rheology control agent that interacts with the magnetic particles can fully function as a rheology control agent, with a portion of the agent interacting with the magnetic particles while the other portion easily becomes incorporated into a network of the rheology control agents or forms an appropriate steric hindrance structure. As a result, it is believed that the rheology control agent has a better than usual effect of suppressing the sedimentation of the magnetic particles, and the stability over time has been sufficiently improved. In addition, since the magnetic particle-containing film is mounted in the coating process of the composition, it is exposed to more processes during the manufacturing process of the electronic circuit compared to the magnetic body mounted in the form of individual pieces in the latter half of the process. Therefore, it is preferable that the magnetic particle-containing film has various durability. In particular, it is preferable that the magnetic particle-containing film has good chemical resistance against chemicals such as acids, considering that the magnetic particle-containing film contains metal atoms. It has been found that the chemical resistance of the magnetic particle-containing film formed can be good by using the composition of the present invention. It is believed that this is because the standard redox potential of a specific atom in the magnetic particles contained in the composition is in an appropriate range. Hereinafter, the effect of the present invention is said to be superior when at least one of the stability over time of the composition, the magnetic isotropy of the magnetic particle-containing film formed, and the chemical resistance of the magnetic particle-containing film formed is superior.
[0019] [Magnetic particles] The composition contains magnetic particles. The magnetic particles contain metal atoms. As used herein, the metal atoms also include metalloid atoms such as boron, silicon, germanium, arsenic, antimony, and tellurium. The metal atoms may be contained in the magnetic particles as an alloy containing the metal element (preferably a magnetic alloy), a metal oxide (preferably a magnetic oxide), a metal nitride (preferably a magnetic oxide), or a metal carbide (preferably a magnetic carbide). The content of metal atoms relative to the total mass of the magnetic particles is preferably from 50 to 100 mass %, more preferably from 75 to 100 mass %, and even more preferably from 95 to 100 mass %.
[0020] The magnetic particles contain, as metal atoms, one or more specific atoms selected from the group consisting of Ni atoms and Co atoms. The specific atom may be a Ni atom, a Co atom, or both Ni and Co atoms. In view of the superior effect of the present invention, the specific atom is preferably a Ni atom. The content of the specific atom is 50% by mass or more, preferably 60% by mass or more, and more preferably 70% by mass or more, based on the total mass of the metal atoms in the magnetic particles. There is no upper limit to the content, and it is 100% by mass or less, preferably 98% by mass or less, and more preferably 95% by mass or less. When the magnetic particles contain Ni atoms, the content thereof is preferably 50 to 100 mass %, more preferably 60 to 95 mass %, and even more preferably 70 to 90 mass %, based on the total mass of metal atoms. When the magnetic particles contain Co atoms, the content thereof is preferably 40 to 100 mass %, more preferably 50 to 95 mass %, further preferably 60 to 90 mass %, and particularly preferably 70 to 90 mass %, based on the total mass of metal atoms.
[0021] The magnetic particles may contain both of the specific atoms, or may substantially contain only one of them. When the magnetic particles substantially contain only one of the specific atoms, the content of one of the Ni atoms and the Co atoms relative to the total mass of the specific atoms is, for example, 98 to 100 mass%, preferably 99 to 100 mass%, and more preferably 99.5 to 100 mass%. When the magnetic particles contain both of the specific atoms, the content of Ni atoms may be greater, the content of Co atoms may be greater, or the content of both may be the same. When the magnetic particles contain both specific atoms, the content of one of the specific atoms (Ni atoms or Co atoms) is, for example, 50 mass % or more and less than 98 mass % relative to the total mass of the specific atoms (the combined content of Ni atoms and Co atoms).
[0022] Examples of materials other than the specific atoms that make up the magnetic particles include Fe, Mo, Al, Si, S, Sc, Ti, V, Cu, Y, Mo, Rh, Pd, Ag, Sn, Sb, Te, Ba, Ta, W, Re, Au, Bi, La, Ce, Pr, Nd, P, Zn, Sr, Zr, Mn, Cr, Nb, Pb, Ca, B, C, and N. In addition to the specific atoms constituting the magnetic particles, the magnetic particles preferably contain metal atoms, and more preferably contain one or more types selected from the group consisting of Fe, Si, Cr, B and Mo. In the magnetic particles, the content of metal atoms other than the specific atoms is preferably 0 to 50 mass %, more preferably 5 to 40 mass %, and even more preferably 10 to 30 mass %, based on the total mass of metal atoms. The content of Fe (Fe atoms) in the magnetic particles is preferably 0 to 50 mass %, more preferably 0 to 35 mass %, and even more preferably 0 to 25 mass %, relative to the total mass of metal atoms. In the magnetic particles, the content of Si (Si atoms) is preferably 0 to 20 mass %, more preferably 0 to 15 mass %, and even more preferably 0 to 8 mass %, relative to the total mass of metal atoms. In the magnetic particles, the content of Cr (Cr atoms) is preferably 0 to 20 mass %, more preferably 0 to 15 mass %, and even more preferably 0 to 8 mass %, relative to the total mass of metal atoms. In the magnetic particles, the content of B (B atoms) is preferably from 0 to 15 mass %, more preferably from 0 to 8 mass %, and even more preferably from 0 to 5 mass %, relative to the total mass of metal atoms. The content of Mo (Mo atoms) in the magnetic particles is preferably from 0 to 50 mass %, more preferably from 0 to 35 mass %, and even more preferably from 0 to 25 mass %, relative to the total mass of metal atoms.
[0023] Specific examples of the magnetic particles include Fe-Co alloys (preferably permendur), Fe-Ni alloys (e.g. permalloy), Ni-Mo alloys (preferably supermalloy), Fe-Ni-Cu-Cr alloys (preferably mu-metal), Fe-Ni-Co alloys, Fe-Co-Si-B alloys, Co-based amorphous alloys, and Ni-Zn ferrites. The alloys may be amorphous. Among them, the magnetic particles are preferably made of permalloy, since the effect of the present invention is more excellent. Examples of permalloy include supermalloy and mu-metal, with supermalloy being preferred. Here, permalloy refers to, for example, a ferromagnetic alloy mainly composed of Fe and Ni. The permalloy may be an alloy containing one or more of Cr, Cu, and Mo in addition to Fe and Ni. Supermalloy refers to, for example, a ferromagnetic alloy mainly composed of Fe, Ni, and Mo, and is a type of permalloy. Mu-metal refers to, for example, a ferromagnetic alloy mainly composed of Fe, Ni, Cu, and Cr, and is a type of permalloy.
[0024] The composition of the magnetic particles is confirmed by high-frequency inductively coupled plasma (ICP) emission spectrometry. Specifically, a pressure-resistant container containing 12 mg of sample particles and 10 mL of 4 mol / L (liter; the same applies below) hydrochloric acid solution is kept in an oven set at a temperature of 120°C for 12 hours to obtain a solution. Next, 30 mL of pure water is added to the obtained solution, and then it is filtered using a 0.1 μm membrane filter. The elemental analysis of the filtrate thus obtained is performed using a high-frequency inductively coupled plasma (ICP) optical emission spectrometer. The content of each metal atom is calculated based on the results of the elemental analysis. The composition is confirmed based on the obtained content. As a measuring device, for example, a high-frequency inductively coupled plasma (ICP) optical emission spectrometer (model: ICPS-8100) manufactured by Shimadzu Corporation can be suitably used, although the measuring device is not limited to this.
[0025] The magnetic particles may have a surface layer on the surface thereof, and by having the surface layer on the magnetic particles in this way, it is possible to impart a function to the magnetic particles according to the material of the surface layer. The surface layer may be an inorganic layer or an organic layer.
[0026] As the compound for forming the inorganic layer, metal oxides, metal nitrides, metal carbides, metal phosphate compounds, metal borate compounds, or silicate compounds (e.g., silicate esters such as tetraethyl orthosilicate, and silicates such as sodium silicate) are preferred, since they can form a surface layer excellent in at least one of insulation, gas barrier properties, and chemical stability. Specific examples of elements contained in these compounds include Fe, Al, Ca, Mn, Zn, Mg, V, Cr, Y, Ba, Sr, Ge, Zr, Ti, Si, and rare earth elements. Materials constituting the inorganic layer obtained using the compound for forming an inorganic layer include silicon oxide, germanium oxide, titanium oxide, aluminum oxide, zirconium oxide, and magnesium oxide, and the inorganic layer may be a layer containing two or more of these.
[0027] Examples of the organic layer-forming compound include acrylic monomers. Specific examples of the acrylic monomer include the compounds described in paragraphs 0022 to 0023 of JP-A-2019-67960. Examples of materials constituting the organic layer obtained by using the organic layer-forming compound include acrylic resins.
[0028] The thickness of the surface layer is not particularly limited, but is preferably from 3 to 1000 nm in order to better exhibit the function of the surface layer.
[0029] The particle size of the magnetic particles is preferably 0.1 μm or more, more preferably 1 μm or more, and even more preferably 5 μm or more. In particular, when the particle size is 5 μm or more, the chemical resistance of the magnetic particle-containing film obtained from the composition is more likely to be excellent (particularly when the magnetic particles contain Ni atoms as the specific atom with the highest content of Ni atoms, or when the magnetic particles contain essentially only Ni atoms as the specific atom). Furthermore, when the particle size is 20 μm or more, the chemical resistance of the magnetic particle-containing film obtained from the composition is more likely to be excellent (particularly when the magnetic particles contain Co atoms as the specific atom with the highest content of Co atoms, or when the magnetic particles contain essentially only Co atoms as the specific atom). The particle size of the magnetic particles is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 30 μm or more. In this specification, the particle size of the magnetic particles means the average primary particle size of the particles. The particle diameter of the primary particles of the magnetic particles is measured by photographing the magnetic particles with a transmission electron microscope at a magnification of 100,000 times, printing the photograph on photographic paper to a total magnification of 500,000 times, tracing the outline of the particle (primary particle) with a digitizer, and calculating the diameter of a circle with the same area as the traced area (circular area diameter). Here, primary particles refer to independent particles without aggregation. Photographing using a transmission electron microscope is performed by a direct method using a transmission electron microscope with an acceleration voltage of 300 kV. Observation and measurement using a transmission electron microscope can be performed, for example, using a Hitachi transmission electron microscope H-9000 model and Carl Zeiss image analysis software KS-400.
[0030] The aspect ratio of the magnetic particles is preferably 1-8, more preferably 1 or more and less than 8, further preferably 1-5, and particularly preferably 1-3. When the composition contains one type of magnetic particle, the aspect ratio of the magnetic particle is 1 or more and less than 8. When the composition contains two or more types of the magnetic particles, at least one of them has an aspect ratio of less than 8 (preferably 1 to 5, more preferably 1 to 3). The content of the magnetic particles having an aspect ratio of less than 8 (preferably 1 to 5, more preferably 1 to 3) is at least 25% by mass, preferably 50% by mass or more, more preferably 75% by mass or more, and even more preferably 90% by mass or more, based on the total mass of the magnetic particles. There is no upper limit to the content, and it is, for example, 100% by mass or less. In this specification, the aspect ratio of a particle is calculated as follows: the particle for which the aspect ratio is to be calculated is observed under a transmission electron microscope (TEM), and 200 particles are randomly selected from the observation, and the longest width A of the particle is divided by the shortest width B (A / B) of each particle. The average of the 200 "A / B" values calculated is regarded as the aspect ratio of the particle.
[0031] The composition may contain only one type of the magnetic particles or may contain two or more types. One or more of the magnetic particles may be plate-like, elliptical, spherical, or irregular, so long as the magnetic particles in the composition as a whole satisfy the aspect ratio requirement described above.
[0032] The content of the magnetic particles is preferably from 30 to 99% by mass, more preferably from 35 to 97% by mass, and even more preferably from 40 to 95% by mass, based on the total mass of the composition. The content of the magnetic particles is preferably from 50 to 99% by mass, more preferably from 60 to 97% by mass, and even more preferably from 70 to 95% by mass, based on the total solid content of the composition.
[0033] <> The composition of the present invention is a composition formed using a magnetic particle raw material containing at least magnetic particles X having an aspect ratio of less than 8 and a rheology control agent, and the content of magnetic particles X is preferably 25 mass % or more relative to the total mass of the magnetic particles in the composition (in other words, the total mass of the magnetic particle raw material in the composition).
[0034] The magnetic particles X contain metal atoms, The metal atom contains one or more specific atoms selected from the group consisting of Ni atoms and Co atoms, and further contains The content of the specific atom is preferably 50 mass % or more based on the total mass of the metal atoms.
[0035] Here, the metal atom contained in the magnetic particle X has the same meaning as the metal atom explained in the upper section of [Magnetic Particle], and the preferred embodiments thereof are also the same. The content of metal atoms relative to the total mass of the magnetic particles X is preferably from 50 to 100 mass %, more preferably from 75 to 100 mass %, and even more preferably from 95 to 100 mass %.
[0036] Moreover, the specific atom contained in the magnetic particle X has the same meaning as the specific atom explained in the upper section of [Magnetic Particle], and the preferred embodiments thereof are also the same. The content of the specific atom is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, based on the total mass of metal atoms in the magnetic particles X. There is no upper limit to the content, and it is 100% by mass or less, preferably 98% by mass or less, and more preferably 95% by mass or less. When the magnetic particles X contain Ni atoms, the content thereof is preferably 50 to 100 mass % relative to the total mass of metal atoms in the magnetic particles X, more preferably 60 to 95 mass %, and even more preferably 70 to 90 mass %. When the magnetic particles X contain Co atoms, the content thereof relative to the total mass of metal atoms in the magnetic particles X is preferably 40 to 100 mass %, more preferably 50 to 95 mass %, further preferably 60 to 90 mass %, and particularly preferably 70 to 90 mass %. The magnetic particles X may contain both specific atoms, or may substantially contain only one of them. When the magnetic particles X substantially contain only one specific atom, the content of one of Ni atoms and Co atoms relative to the total mass of the specific atoms is, for example, 98 to 100 mass%, preferably 99 to 100 mass%, and more preferably 99.5 to 100 mass%. When the magnetic particles X contain both specific atoms, the content of Ni atoms may be greater, the content of Co atoms may be greater, or the content of both may be the same. When the magnetic particle X contains both specific atoms, the content of one of the specific atoms (Ni atoms or Co atoms) is, for example, 50 mass % or more and less than 98 mass % with respect to the total mass of the specific atoms (the total content of Ni atoms and Co atoms).
[0037] Moreover, the materials other than the specific atoms constituting the magnetic particles X are the same as the materials explained in the upper section of [Magnetic Particles], and the preferred embodiments thereof are also the same. The magnetic particles X preferably contain metal atoms in addition to the specific atoms, and more preferably contain one or more types selected from the group consisting of Fe, Si, Cr, B, and Mo. The content of metal atoms other than the specific atoms in the magnetic particles X is preferably 0 to 50 mass %, more preferably 5 to 40 mass %, and even more preferably 10 to 30 mass %, based on the total mass of metal atoms in the magnetic particles X. The content of Fe (Fe atoms) in the magnetic particles X is preferably 0 to 50 mass % relative to the total mass of metal atoms in the magnetic particles X, more preferably 0 to 35 mass %, and even more preferably 0 to 25 mass %. The content of Si (Si atoms) in the magnetic particles X is preferably 0 to 20 mass % relative to the total mass of metal atoms in the magnetic particles X, more preferably 0 to 15 mass %, and even more preferably 0 to 8 mass %. The content of Cr (Cr atoms) in the magnetic particles X is preferably 0 to 20 mass % relative to the total mass of metal atoms in the magnetic particles X, more preferably 0 to 15 mass %, and even more preferably 0 to 8 mass %. The content of B (B atoms) in the magnetic particles X is preferably 0 to 15 mass % relative to the total mass of metal atoms in the magnetic particles X, more preferably 0 to 8 mass %, and even more preferably 0 to 5 mass %. The content of Mo (Mo atoms) in the magnetic particles X is preferably 0 to 50 mass % relative to the total mass of metal atoms in the magnetic particles X, more preferably 0 to 35 mass %, and even more preferably 0 to 25 mass %.
[0038] Specific examples of the magnetic particles X are the same as those described in the upper section of [Magnetic Particles]. Among them, the magnetic particles X are preferably permalloys, since the effect of the present invention is more excellent. Examples of permalloys include supermalloys and mu-metals, and supermalloys are preferred.
[0039] Furthermore, the method for confirming the composition of magnetic particles X and the particle size of the magnetic particles are the same as those described in the upper section under [Magnetic Particles], and the preferred embodiments are also the same. A surface layer may be provided on the surface of the magnetic particle X. The surface layer of the magnetic particle X is the same as the surface layer of the magnetic particle described in the upper section [Magnetic Particles], and the preferred embodiments are also the same.
[0040] The aspect ratio of the magnetic particles X is preferably 1-8, more preferably 1 or more and less than 8, further preferably 1-5, and particularly preferably 1-3. The content of magnetic particles X having an aspect ratio of less than 8 (preferably 1 to 5, more preferably 1 to 3) is at least 25% by mass, preferably 50% by mass or more, more preferably 75% by mass or more, and even more preferably 90% by mass or more, based on the total mass of magnetic particles in the composition (in other words, the total mass of magnetic particle raw materials in the composition). There is no upper limit to the content, and it is, for example, 100% by mass or less. The aspect ratio is defined as described above.
[0041] As the above-mentioned magnetic particle raw material, it is sufficient to use at least magnetic particles X having an aspect ratio of less than 8, and magnetic particles Y having an aspect ratio of 8 or more may also be used in combination. As the magnetic particles X, only one type may be used, or two or more types may be used.
[0042] The magnetic particles X may be any of plate-like, elliptical, spherical, and amorphous. In preparing the composition, the total content of the magnetic particles (in other words, the total content of the magnetic particle raw materials in the composition) is preferably 30 to 99 mass %, more preferably 35 to 97 mass %, and even more preferably 40 to 95 mass %, based on the total mass of the composition. Also, the total content of the magnetic particles (in other words, the total content of the magnetic particle raw materials in the composition) is preferably 50 to 99 mass %, more preferably 60 to 97 mass %, and even more preferably 70 to 95 mass %, based on the total solid content of the composition.
[0043] [Rheology control agent] The composition contains a rheology control agent. The rheology control agent is a component that imparts thixotropic properties to the composition, ie, high viscosity when the shear stress (shear rate) is low and low viscosity when the shear stress (shear rate) is high. The content of the rheology control agent is preferably from 0.1 to 35 mass %, more preferably from 0.5 to 30 mass %, and even more preferably from 1 to 27 mass %, based on the total mass of the composition. The content of the rheology control agent is preferably from 0.1 to 35 mass %, more preferably from 0.5 to 30 mass %, and even more preferably from 1 to 27 mass %, based on the total solid content of the composition.
[0044] The rheology control agent may be an organic rheology control agent or an inorganic rheology control agent, with the organic rheology control agent being preferred.
[0045] <Organic rheology control agent> The content of the organic rheology control agent is preferably from 0.1 to 35 mass %, more preferably from 0.5 to 30 mass %, and even more preferably from 1 to 25 mass %, based on the total mass of the composition. The content of the organic rheology control agent is preferably from 0.1 to 35 mass %, more preferably from 0.5 to 30 mass %, and even more preferably from 1 to 25 mass %, based on the total solid content of the composition. The organic rheology control agents may be used alone or in combination of two or more kinds.
[0046] Examples of the organic rheology control agent include compounds having one or more (preferably two or more) adsorptive groups and further having a steric repulsive structural group. The adsorptive groups interact with the surface of the magnetic particles to cause the organic rheology control agent to be adsorbed to the surface of the magnetic particles. Examples of the adsorptive group include an acid group, a basic group, and an amide group. Examples of the acid group include a carboxy group, a phosphate group, a sulfo group, a phenolic hydroxyl group, and an acid anhydride group thereof (such as an acid anhydride group of a carboxy group), and the carboxy group is preferred in terms of achieving better effects of the present invention. Examples of basic groups include amino groups (groups in which one hydrogen atom has been removed from ammonia, primary amines, or secondary amines) and imino groups. Among these, the adsorptive group is preferably a carboxy group or an amide group, and more preferably a carboxy group. The steric repulsive structural group has a three-dimensionally bulky structure, and thus introduces steric hindrance to the magnetic particles to which the organic rheology control agent is adsorbed, thereby maintaining an appropriate space between the magnetic particles. As the steric repulsive structural group, for example, a chain group is preferable, a long-chain fatty acid group is more preferable, and a long-chain alkyl group is even more preferable. The organic rheology control agent also preferably has a hydrogen bonding unit. The hydrogen-bonding unit is a partial structure that functions to construct a hydrogen-bonding network between organic rheology control agents, and between an organic rheology control agent and another component. The organic rheology control agent that contributes to the formation of the network may or may not be adsorbed to the surface of the magnetic particle. The hydrogen-bonding unit may be the same as or different from the above-mentioned adsorptive group. When the hydrogen-bonding unit is the same as the above-mentioned adsorptive group, a part of the adsorptive group binds to the surface of the magnetic particle, and another part functions as the hydrogen-bonding unit. The hydrogen-bonding unit is preferably a carboxy group or an amide group. The carboxy group as the hydrogen-bonding unit is preferred because it is easily incorporated in the curing reaction when producing a magnetic particle-containing film, and the amide group is preferred because the composition has better stability over time.
[0047] When the organic rheology control agent is a resin, the organic rheology control agent may have a repeating unit containing a graft chain described below, or may not substantially have such a repeating unit. When the organic rheology control agent is a resin and does not substantially have a repeating unit containing a graft chain described below, the content of the repeating unit containing a graft chain described below relative to the total mass of the organic rheology control agent is preferably less than 2% by mass, more preferably 1% by mass or less, and even more preferably less than 0.1% by mass. The lower limit is 0% by mass or more.
[0048] The organic rheology control agent is preferably one or more selected from the group consisting of polycarboxylic acids (compounds having two or more carboxy groups), polycarboxylic anhydrides (compounds having two or more acid anhydride groups consisting of carboxy groups), and amide waxes. These may be resins or materials other than resins. These may also correspond to an aggregation control agent and / or an aggregation dispersant, which will be described later.
[0049] Examples of organic rheology control agents include modified urea, urea modified polyamide, fatty acid amide, polyurethane, polyamide amide, polymeric urea derivatives, and salts thereof (such as carboxylates). The modified urea is a reaction product of an isocyanate monomer or its adduct with an organic amine. The modified urea is modified with polyoxyalkylene polyol (polyoxyethylene polyol, polyoxypropylene polyol, etc.) and / or alkyd chain, etc. The urea modified polyamide is, for example, a compound containing a urea bond and a compound having a medium polarity group or a low polarity group introduced at the end of the compound. Examples of the medium polarity group or low polarity group include polyoxyalkylene polyol (polyoxyethylene polyol, polyoxypropylene polyol, etc.) and an alkyd chain. The fatty acid amide is a compound having a long chain fatty acid group and an amide group in the molecule. These may be resins or non-resins. These may also correspond to an aggregation control agent and / or an aggregation dispersant, which will be described later.
[0050] The molecular weight of the organic rheology control agent (weight average molecular weight when the agent has a molecular weight distribution) is preferably in the range of 200 to 50,000. When the organic rheology control agent has an acid value, the acid value is preferably from 5 to 400 mgKOH / g. When the organic rheology control agent has an amine acid value, the amine value is preferably from 5 to 300 mgKOH / g.
[0051] (Aggregation control agent) Organic rheology control agents also include aggregation control agents, which may be resins or other substances. The aggregation control agent has the function of binding to relatively dense aggregates such as magnetic particles, and further dispersing other optional components (e.g., polymerizable compounds, etc.) in the composition to create bulky aggregates. When the composition contains an aggregation control agent, the magnetic particles in the composition are prevented from forming a hard cake, and bulkier aggregates are formed, which can improve redispersibility.
[0052] The aggregation control agent may, for example, be a cellulose derivative. Examples of the cellulose derivatives include carboxymethyl cellulose, methyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxypropyl ethyl cellulose, and salts thereof.
[0053] When the composition contains an aggregation control agent, the content of the aggregation control agent is preferably 0.1 to 20 mass %, preferably 0.3 to 15 mass %, and more preferably 0.5 to 10 mass %, based on the total mass of the composition. The content of the aggregation control agent is preferably from 0.1 to 20 mass %, more preferably from 0.3 to 15 mass %, and further preferably from 0.5 to 10 mass %, based on the total solid content of the composition.
[0054] (Aggregation and dispersant) The organic rheology control agent also includes a flocculating dispersant. The flocculating dispersant may be a resin or may be something other than a resin. The flocculating dispersant has a function of adsorbing to the surface of the magnetic particles, separating the magnetic particles from each other, while maintaining the distance between the magnetic particles at a certain level or more through the interaction between the dispersants, thereby preventing the magnetic particles from flocculating directly with each other. As a result, the flocculation of the magnetic particles is suppressed, and even if floccules are formed, the floccules have a relatively low density. Furthermore, other components (e.g., polymerizable compounds, etc.) optionally contained in the composition can be dispersed in the composition to form bulky floccules, which can improve redispersibility.
[0055] As the flocculating dispersant, an alkylol ammonium salt of a polybasic acid is preferred. The polybasic acid may have two or more acid groups, and examples thereof include acidic polymers containing repeating units having an acid group (e.g., polyacrylic acid, polymethacrylic acid, polyvinylsulfonic acid, polyphosphoric acid, etc.). Other examples of polybasic acids include polymers obtained by polymerizing unsaturated fatty acids such as crotonic acid. Alkylolammonium salts of polybasic acids can be obtained by reacting these polybasic acids with alkylolammonium. The salts obtained by such reactions usually contain the following partial structure: -C(=O)-N(-R 1 )(-R 2 -OH) Here, R 1 is an alkyl group, R 2 is an alkylene group. The alkylol ammonium salt of a polybasic acid is preferably a polymer containing a plurality of the above partial structures. When the alkylol ammonium salt of a polybasic acid is a polymer, the weight average molecular weight is preferably 1,000 to 100,000, more preferably 5,000 to 20,000. The polymer of the alkylol ammonium salt of a polybasic acid is bonded to the surface of the magnetic particles and is also hydrogen bonded to other flocculating dispersant molecules, so that the main chain structure of the polymer can penetrate between the magnetic particles and separate the magnetic particles from each other.
[0056] One of the preferred embodiments of the flocculating dispersant is amide wax, which is a dehydration condensation product of at least any acid selected from (a) saturated aliphatic monocarboxylic acids and hydroxyl group-containing aliphatic monocarboxylic acids, and (b) polybasic acids, and (c) at least any amine selected from diamines and tetraamines. The above (a) to (c) are preferably used in such a manner that the molar ratio of (a):(b):(c)=1-3:0-5:1-6.
[0057] The saturated aliphatic monocarboxylic acids preferably have a carbon number of 12 to 22. Specific examples include lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, nonadecanoic acid, arachidic acid, and behenic acid. The hydroxyl group-containing aliphatic monocarboxylic acids preferably have a carbon number of 12 to 22. Specific examples include 12-hydroxystearic acid and dihydroxystearic acid. These saturated aliphatic monocarboxylic acids and hydroxyl group-containing aliphatic monocarboxylic acids may be used alone or in combination.
[0058] The polybasic acids are preferably dibasic or higher carboxylic acids having 2 to 12 carbon atoms, and more preferably dicarboxylic acids. Examples of such dicarboxylic acids include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,10-decanedicarboxylic acid, and 1,12-dodecanedicarboxylic acid, aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, and terephthalic acid, and alicyclic dicarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, and cyclohexylsuccinic acid. These polybasic acids may be used alone or in combination.
[0059] The diamines preferably have a carbon number of 2 to 14. Specific examples include ethylenediamine, 1,3-propanediamine, 1,4-butanediamine, hexamethylenediamine, metaxylenediamine, tolylenediamine, paraxylenediamine, phenylenediamine, isophoronediamine, 1,10-decanediamine, 1,12-dodecanediamine, 4,4-diaminodicyclohexylmethane, and 4,4-diaminodiphenylmethane. The tetraamines preferably have a carbon number of 2 to 14. Specific examples include butane-1,1,4,4-tetraamine and pyrimidine-2,4,5,6-tetraamine. These diamines and tetraamines may be used alone or in combination.
[0060] The amount of diamines and tetraamines is adjusted according to the number of moles of saturated aliphatic monocarboxylic acid or hydroxyl group-containing aliphatic monocarboxylic acid and the number of moles of polybasic acids so that the total number of carboxyl groups and the total number of amino groups are equivalent. For example, when there are n moles (n=0-5) of aliphatic dicarboxylic acid, which is a polybasic acid, for 2 moles of aliphatic monocarboxylic acid, and the number of moles of diamines is (n+1), the acid and amine are equivalent.
[0061] The amide wax may be obtained as a mixture of a plurality of compounds having different molecular weights. The amide wax is preferably a compound represented by the following chemical formula (I). The amide wax may be a single compound or a mixture. AC-(BC) m -A···(I) In formula (I), A is a dehydroxylated residue of a saturated aliphatic monocarboxylic acid and / or a hydroxyl group-containing saturated aliphatic monocarboxylic acid, B is a dehydroxylated residue of a polybasic acid, C is a dehydrogenated residue of a diamine and / or a tetraamine, and m is 0≦m≦5.
[0062] One preferred embodiment of the aggregation dispersant is a compound represented by the following formula (II).
[0063] [ka]
[0064] In formula (II), R 1 represents a monovalent linear aliphatic hydrocarbon group having 10 to 25 carbon atoms, R 2 and R 3 each independently represents a divalent aliphatic hydrocarbon group having 2, 4, 6, or 8 carbon atoms, a divalent alicyclic hydrocarbon group having 6 carbon atoms, or a divalent aromatic hydrocarbon group; R 4 represents a divalent aliphatic hydrocarbon group having 1 to 8 carbon atoms, R 5 and R 6 each independently represents a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or a hydroxyalkyl ether group. In formula (II), L 1 ~L 3 each independently represents an amide bond, L 1 and L 3 If -CONH-, then L 2 is -NHCO-, and L 1 and L 3 When is -NHCO-, L 2 is -CONH-.
[0065] R 1 is a monovalent linear aliphatic hydrocarbon group having 10 to 25 carbon atoms, and examples thereof include linear alkyl groups such as a decyl group, a lauryl group, a myristyl group, a pentadecyl group, a stearyl group, a palmityl group, a nonadecyl group, an eicosyl group, and a behenyl group; linear alkenyl groups such as a decenyl group, a pentadecenyl group, an oleyl group, and an eicosenyl group; and linear alkynyl groups such as a pentadecynyl group, an octadecynyl group, and a nonadecynyl group. Among them, R 1 is preferably a monovalent linear aliphatic hydrocarbon group having 14 to 25 carbon atoms, more preferably a monovalent linear aliphatic hydrocarbon group having 18 to 21 carbon atoms. The linear aliphatic hydrocarbon group is preferably an alkyl group.
[0066] R 2 and R 3Examples of the divalent aliphatic hydrocarbon group having 2, 4, 6 or 8 carbon atoms include an ethylene group, an n-butylene group, an n-hexylene group, and an n-octylene group. R 2 and R 3 Examples of the divalent alicyclic hydrocarbon group having 6 carbon atoms include a 1,4-cyclohexylene group, a 1,3-cyclohexylene group, and a 1,2-cyclohexylene group. R 2 and R 3 Examples of the divalent aromatic hydrocarbon group in include arylene groups having 6 to 10 carbon atoms, such as a 1,4-phenylene group, a 1,3-phenylene group, and a 1,2-phenylene group.
[0067] Among them, R 2 and R 3 is preferably a divalent aliphatic hydrocarbon group having 2, 4, 6 or 8 carbon atoms, more preferably a divalent aliphatic hydrocarbon group having 2, 4 or 6 carbon atoms, still more preferably a divalent aliphatic hydrocarbon group having 2 or 4 carbon atoms, and still more preferably a divalent aliphatic hydrocarbon group having 2 carbon atoms. The divalent aliphatic hydrocarbon group is preferably a linear alkylene group.
[0068] R 4 represents a divalent aliphatic hydrocarbon group having 1 to 8 carbon atoms, and among these, a linear or branched alkylene group is preferred, and a linear alkylene group is more preferred, in that they have an excellent thickening effect. Also, R 4 The divalent aliphatic hydrocarbon group in has 1 to 8 carbon atoms, and from the viewpoint of excellent thickening effect, it is preferably 1 to 7, more preferably 3 to 7, further preferably 3 to 6, and particularly preferably 3 to 5. Therefore, R 4 is preferably a linear or branched alkylene group having 1 to 8 carbon atoms, more preferably a linear alkylene group having 1 to 7 carbon atoms, still more preferably a linear alkylene group having 3 to 7 carbon atoms, particularly preferably a linear alkylene group having 3 to 6 carbon atoms, and most preferably a linear alkylene group having 3 to 5 carbon atoms.
[0069] R5 and R 6 Examples of the monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms include linear or branched alkyl groups having 1 to 3 carbon atoms, such as a methyl group, an ethyl group, a propyl group, and an isopropyl group; linear or branched alkenyl groups having 2 to 3 carbon atoms, such as a vinyl group, a 1-methylvinyl group, and a 2-propenyl group; and linear or branched alkynyl groups having 2 to 3 carbon atoms, such as an ethynyl group and a propynyl group.
[0070] R 5 and R 6 Examples of the hydroxyalkyl ether group in the formula (I) include mono- or di(hydroxy)C groups such as a 2-hydroxyethoxy group, a 2-hydroxypropoxy group, and a 2,3-dihydroxypropoxy group. 1-3 Examples of such groups include alkyl ether groups.
[0071] Among them, R 5 and R 6 are each independently preferably a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms, more preferably a linear or branched alkyl group having 1 to 3 carbon atoms, still more preferably a linear alkyl group having 1 to 3 carbon atoms, and particularly preferably a methyl group.
[0072] As the compound represented by formula (II), the compounds represented by the following formulae (II-1) to (II-9) are preferred.
[0073] [ka]
[0074] Examples of the flocculating dispersant include ANTI-TERRA-203, 204, 206, and 250 (all trade names, manufactured by BYK); ANTI-TERRA-U (trade name, manufactured by BYK); DISPER BYK-102, 180, and 191 (all trade names, manufactured by BYK); BYK-P105 (trade name, manufactured by BYK); TEGO Disper 630 and 700 (all trade names, manufactured by Evonik Degussa Japan); TALENE VA-705B (trade name, manufactured by Kyoeisha Chemical Co., Ltd.); and FLOWNON RCM-300TL and RCM-230AF (trade names, manufactured by Kyoeisha Chemical Co., Ltd., Amide Wax).
[0075] When the composition contains an aggregating dispersant, the content of the aggregating dispersant is preferably from 0.1 to 35 mass %, more preferably from 0.3 to 30 mass %, and further preferably from 0.5 to 27 mass %, based on the total mass of the composition. The content of the aggregation dispersant is preferably from 0.1 to 35 mass %, more preferably from 0.3 to 30 mass %, and further preferably from 0.5 to 27 mass %, based on the total solid content of the composition.
[0076] <Inorganic rheology control agent> Inorganic rheology control agents include, for example, bentonite, silica, calcium carbonate, and smectite.
[0077] [Other resins] The composition also preferably contains other resins. The above-mentioned "other resins" refer to resins that do not fall under the category of rheology control agents which are resins. The other resins preferably have a weight average molecular weight of more than 2,000.
[0078] Other resins include (meth)acrylic resins, epoxy resins, enethiol resins, polycarbonate resins, polyether resins, polyarylate resins, polysulfone resins, polyethersulfone resins, polyphenylene resins, polyarylene ether phosphine oxide resins, polyimide resins, polyamideimide resins, polyolefin resins, cyclic olefin resins, polyester resins, styrene resins, and phenoxy resins. One of these resins may be used alone, or two or more may be mixed and used. As the cyclic olefin resin, norbornene resins are preferred from the viewpoint of improving heat resistance. Commercially available norbornene resins include, for example, the ARTON series (e.g., ARTON F4520) manufactured by JSR Corporation. Examples of epoxy resins include epoxy resins which are glycidyl ethers of phenolic compounds, epoxy resins which are glycidyl ethers of various novolac resins, alicyclic epoxy resins, aliphatic epoxy resins, heterocyclic epoxy resins, glycidyl ester epoxy resins, glycidylamine epoxy resins, epoxy resins obtained by glycidylating halogenated phenols, condensates of silicon compounds having epoxy groups and other silicon compounds, copolymers of polymerizable unsaturated compounds having epoxy groups and other polymerizable unsaturated compounds, etc. Also, examples of epoxy resins that can be used include Marproof G-0150M, G-0105SA, G-0130SP, G-0250SP, G-1005S, G-1005SA, G-1010S, G-2050M, G-01100, and G-01758 (manufactured by NOF Corp., epoxy group-containing polymers). In addition, the other resins may be those described in the examples of WO 2016 / 088645. In addition, when the other resins have an ethylenically unsaturated group, particularly a (meth)acryloyl group, in a side chain, it is also preferable that the main chain and the ethylenically unsaturated group are bonded via a divalent linking group having an alicyclic structure.
[0079] One of the preferred embodiments of the other resins is a resin having a polymerizable group such as an unsaturated double bond (e.g., an ethylenically unsaturated double bond), an epoxy group, or an oxetanyl group. When the polymerizable group reacts during the formation of the magnetic particle-containing film, a magnetic particle-containing film having excellent mechanical strength is obtained. Examples of such other resins include polymers having epoxy groups in their side chains, and polymerizable monomers or oligomers having two or more epoxy groups in their molecules. Specific examples of such resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, and aliphatic epoxy resins. These other resins may be commercially available products or may be obtained by introducing an epoxy group into the side chain of a polymer. For commercially available products, see, for example, paragraph 0191 of JP 2012-155288 A, the contents of which are incorporated herein by reference. Other examples include ADEKA RESIN EP-4000S, EP-4003S, EP-4010S, and EP-4011S (all manufactured by ADEKA Corporation), NC-2000, NC-3000, NC-7300, XD-1000, EPPN-501, and EPPN-502 (all manufactured by ADEKA Corporation), and JER1031S. Furthermore, commercially available products of phenol novolac type epoxy resins include JER-157S65, JER-152, JER-154, and JER-157S70 (all manufactured by Mitsubishi Chemical Corporation). Specific examples of polymers having oxetanyl groups in their side chains and polymerizable monomers or oligomers having two or more oxetanyl groups in the molecule include Aron Oxetane OXT-121, OXT-221, OX-SQ, and PNOX (all manufactured by Toagosei Co., Ltd.). When synthesizing other resins having epoxy groups by introducing epoxy groups into the polymer side chains, the introduction reaction can be carried out by reacting for a predetermined time at a reaction temperature of 50 to 150°C in an organic solvent using, for example, a tertiary amine such as triethylamine or benzylmethylamine, a quaternary ammonium salt such as dodecyltrimethylammonium chloride, tetramethylammonium chloride or tetraethylammonium chloride, pyridine, triphenylphosphine, or the like as a catalyst. The amount of the alicyclic epoxy unsaturated compound introduced can be controlled so that the acid value of the resulting polymer is in the range of 5 to 200 KOH mg / g. The weight average molecular weight can be in the range of 500 to 5,000,000, preferably 1,000 to 500,000. Instead of the alicyclic epoxy unsaturated compound, compounds having a glycidyl group as an epoxy group such as glycidyl (meth)acrylate and allyl glycidyl ether can also be used. For such compounds, see, for example, paragraph 0045 of JP-A-2009-265518, the contents of which are incorporated herein by reference.
[0080] One of the preferred embodiments of the other resin is a resin having an acid group, a basic group, or an amide group. The other resin having an acid group, a basic group, or an amide group is preferred because it easily functions as a dispersant for dispersing magnetic particles and provides a superior effect of the present invention. Examples of the acid group include a carboxy group, a phosphate group, a sulfo group, and a phenolic hydroxyl group. The carboxy group is preferred in terms of obtaining superior effects of the present invention. Examples of the basic group include an amino group (a group in which one hydrogen atom has been removed from ammonia, a primary amine, or a secondary amine) and an imino group. In particular, in terms of obtaining superior effects of the present invention, it is preferable that the other resin has a carboxy group or an amide group.
[0081] When the other resin has an acid group, the acid value of the other resin is preferably from 10 to 500 mgKOH / g, particularly preferably from 30 to 400 mgKOH / g, in terms of better effects of the present invention.
[0082] As the other resin, it is preferable to use another resin having a solubility in the solvent of 10 g / L or more, and it is more preferable to use another resin having a solubility in the solvent of 20 g / L or more, since this improves the dispersibility of the other resin in the composition and makes the effects of the present invention more excellent. The upper limit of the solubility of the other resin in the solvent is preferably 2000 g / L or less, particularly preferably 1000 g / L or less. The solubility of a resin in a solvent means the amount (g) of the resin that can be dissolved in 1 L of the solvent at 25°C.
[0083] The content of the other resins is preferably 0.1 to 30 mass%, more preferably 1 to 20 mass%, even more preferably 2 to 15 mass%, and particularly preferably 2.5 to 10 mass%, relative to the total mass of the composition, in terms of better effects of the present invention. The content of the other resins is preferably from 0.1 to 30 mass %, more preferably from 1 to 20 mass %, further preferably from 2 to 15 mass %, particularly preferably from 2.5 to 10 mass %, based on the total solid content of the composition.
[0084] <Resin having a repeating unit containing a graft chain (Resin A)> Examples of other resins include a resin having a repeating unit containing a graft chain (hereinafter, also referred to as "resin A"). Resin A can enhance the effect of improving the stability over time of the composition by supporting the effect of the rheology control agent.
[0085] When the composition contains resin A, the content of resin A is preferably 0.1 to 30 mass%, more preferably 0.5 to 20 mass%, and even more preferably 1 to 10 mass%, relative to the total mass of the composition, in terms of better effects of the present invention. The content of the resin A is preferably from 0.1 to 30 mass %, more preferably from 0.5 to 20 mass %, and further preferably from 1 to 10 mass %, based on the total solid content of the composition. When resin A is used, the mass ratio of the content of the rheology control agent to the content of resin A (rheology control agent / resin A) is preferably 10 / 90 to 90 / 10, more preferably 30 / 70 to 80 / 20, and even more preferably 50 / 50 to 70 / 30.
[0086] (Repeating unit including graft chain) In a repeating unit containing a graft chain, as the graft chain becomes longer, the steric repulsion effect increases, and the dispersibility of the magnetic particles improves. On the other hand, if the graft chain is too long, the adsorptive force to the magnetic particles decreases, and the dispersibility of the magnetic particles tends to decrease. For this reason, the graft chain preferably has an atomic number excluding hydrogen atoms of 40 to 10,000, more preferably an atomic number excluding hydrogen atoms of 50 to 2,000, and even more preferably an atomic number excluding hydrogen atoms of 60 to 500. Here, the graft chain refers to a chain extending from the root of the main chain (an atom attached to the main chain in a group branching from the main chain) to the end of the group branching from the main chain.
[0087] In addition, the graft chain preferably contains a polymer structure. Examples of such polymer structures include a poly(meth)acrylate structure (e.g., a poly(meth)acrylic structure), a polyester structure, a polyurethane structure, a polyurea structure, a polyamide structure, and a polyether structure. In order to improve the interaction between the graft chain and the solvent and thereby enhance the dispersibility of the magnetic particles, the graft chain is preferably a graft chain containing at least one structure selected from the group consisting of a polyester structure, a polyether structure, and a poly(meth)acrylate structure, and more preferably a graft chain containing at least one of a polyester structure and a polyether structure.
[0088] Resin A may be a resin obtained by using a macromonomer containing a graft chain (a monomer having a polymer structure and bonding to a main chain to form a graft chain). The macromonomer containing a graft chain (a monomer having a polymer structure and bonding to a main chain to form a graft chain) is not particularly limited, but a macromonomer containing a reactive double bond group can be preferably used.
[0089] Commercially available macromonomers corresponding to the repeating units containing the graft chain and suitable for use in the synthesis of resin A include AA-6, AA-10, AB-6, AS-6, AN-6, AW-6, AA-714, AY-707, AY-714, AK-5, AK-30, and AK-32 (all trade names, manufactured by Toagosei Co., Ltd.), as well as Blenmer PP-100, Blenmer PP-500, Blenmer PP-800, Blenmer PP-1000, Blenmer 55-PET-800, Blenmer PME-4000, Blenmer PSE-400, Blenmer PSE-1300, and Blenmer 43PAPE-600B (all trade names, manufactured by NOF Corp.). Among these, AA-6, AA-10, AB-6, AS-6, AN-6, or Blenmer PME-4000 are preferred.
[0090] Resin A preferably contains at least one structure selected from the group consisting of polymethyl acrylate, polymethyl methacrylate, and cyclic or linear polyester, more preferably contains at least one structure selected from the group consisting of polymethyl acrylate, polymethyl methacrylate, and linear polyester, and further preferably contains at least one structure selected from the group consisting of polymethyl acrylate structure, polymethyl methacrylate structure, polycaprolactone structure, and polyvalerolactone structure. Resin A may contain one of the above structures alone, or may contain a plurality of these structures. Here, the polycaprolactone structure refers to a structure containing a ring-opened ε-caprolactone structure as a repeating unit, and the polyvalerolactone structure refers to a structure containing a ring-opened δ-valerolactone structure as a repeating unit.
[0091] When resin A contains repeating units in which j and k are 5 in formula (1) described below and formula (2) described below, the above-mentioned polycaprolactone structure can be introduced into resin A. Furthermore, when resin A contains repeating units in which j and k are 4 in formula (1) described below and formula (2) described below, the above-mentioned polyvalerolactone structure can be introduced into the resin. In addition, the resin A is X in the formula (4) described below. 5 is a hydrogen atom, and R 4 When the resin A contains a repeating unit in which is a methyl group, the above-mentioned polymethyl acrylate structure can be introduced into the resin A. In addition, the resin A is X in the formula (4) described below. 5 is a methyl group, and R 4 When the resin A contains a repeating unit in which is a methyl group, the above-mentioned polymethyl methacrylate structure can be introduced into the resin A.
[0092] Resin A preferably contains, as a repeating unit including a graft chain, a repeating unit represented by any one of the following formulae (1) to (4), and more preferably contains a repeating unit represented by any one of the following formulae (1A), (2A), (3A), (3B), and (4).
[0093] [ka]
[0094] In formulas (1) to (4), W 1 , W 2 , W 3 , and W 4 Each independently represents an oxygen atom or NH. 1 , W 2 , W 3 , and W 4 is preferably an oxygen atom. In formulas (1) to (4), X 1 , X 2 , X 3 , X 4 , and X 5Each of X independently represents a hydrogen atom or a monovalent organic group. 1 , X 2 , X 3 , X 4 , and X 5 From the viewpoint of synthesis constraints, each of the is preferably a hydrogen atom or an alkyl group having 1 to 12 carbon atoms (number of carbon atoms), more preferably a hydrogen atom or a methyl group, and further preferably a methyl group.
[0095] In formulas (1) to (4), Y 1 , Y 2 , Y 3 , and Y 4 Each of Y independently represents a divalent linking group, and the linking group is not particularly limited in structure. 1 , Y 2 , Y 3 , and Y 4 Specific examples of the divalent linking group represented by the formula include the following linking groups (Y-1) to (Y-21). In the structures shown below, A and B respectively represent the bonding sites with the left and right terminal groups in formulas (1) to (4). Among the structures shown below, (Y-2) or (Y-13) is more preferred from the viewpoint of ease of synthesis.
[0096] [ka]
[0097] In formulas (1) to (4), Z 1 , Z 2 , Z 3 , and Z 4 Each of Z independently represents a hydrogen atom or a monovalent substituent. The structure of the above-mentioned substituent is not particularly limited, but specific examples thereof include an alkyl group, a hydroxyl group, an alkoxy group, an aryloxy group, a heteroaryloxy group, an alkylthioether group, an arylthioether group, a heteroarylthioether group, and an amino group. Among these, Z 1 , Z 2 , Z 3 , and Z 4As the group represented by the formula (I), a group having a steric repulsion effect is preferable, particularly from the viewpoint of improving dispersibility, and each independently an alkyl group or alkoxy group having 5 to 24 carbon atoms is more preferable, and among these, each independently a branched alkyl group having 5 to 24 carbon atoms, a cyclic alkyl group having 5 to 24 carbon atoms, or an alkoxy group having 5 to 24 carbon atoms is even more preferable. The alkyl group contained in the alkoxy group may be linear, branched, or cyclic. Also, Z 1 , Z 2 , Z 3 , and Z 4 The substituent represented by the formula (I) is preferably a group containing a curable group such as a (meth)acryloyl group, an epoxy group, and / or an oxetanyl group. Examples of the group containing a curable group include "-O-alkylene group-(-O-alkylene group-) AL -(meth)acryloyloxy group". AL represents an integer of 0 to 5, preferably 1. The above alkylene groups each independently preferably have 1 to 10 carbon atoms. When the above alkylene group has a substituent, the substituent is preferably a hydroxyl group. The above-mentioned substituent may be a group containing an onium structure. The onium structure-containing group is a group having an anion moiety and a cation moiety. The anion moiety is, for example, an oxygen anion (-O - ) containing partial structures. Among them, oxygen anions (-O - ) is preferably directly bonded to the end of the repeating structure to which n, m, p, or q is added in the repeating units represented by formula (1) to (4), and is preferably bonded to the end of the repeating structure to which n is added in the repeating unit represented by formula (1) (i.e., -(-OC j H 2j -CO-) n It is more preferable that the aryl group is directly bonded to the aryl group (the right end in -). The cation of the cationic moiety of the group containing an onium structure can be, for example, an ammonium cation. When the cationic moiety is an ammonium cation, the cationic moiety is a cationic nitrogen atom (>N + It is a partial structure containing a cationic nitrogen atom (>N+ <) is preferably bonded to four substituents (preferably organic groups), of which 1 to 4 are preferably alkyl groups having 1 to 15 carbon atoms. It is also preferable that one or more (preferably one) of the four substituents is a group containing a curable group such as a (meth)acryloyl group, an epoxy group, and / or an oxetanyl group. Examples of the group containing a curable group that the substituent may be include the above-mentioned "-O-alkylene group-(-O-alkylene group-)" as mentioned above. AL -(meth)acryloyloxy group.
[0098] In the formulas (1) to (4), n, m, p, and q each independently represent an integer of 1 to 500. In the formulae (1) and (2), j and k each independently represent an integer of 2 to 8. In the formulae (1) and (2), j and k each preferably represent an integer of 4 to 6, and more preferably 5. In addition, in formulas (1) and (2), n and m are, for example, integers of 2 or more, preferably integers of 6 or more, more preferably integers of 10 or more, and further preferably integers of 20 or more. In addition, when resin A contains a polycaprolactone structure and a polyvalerolactone structure, the sum of the repeat number of the polycaprolactone structure and the repeat number of the polyvalerolactone structure is preferably an integer of 10 or more, and more preferably an integer of 20 or more.
[0099] In formula (3), R 3 represents a branched or linear alkylene group, preferably an alkylene group having 1 to 10 carbon atoms, more preferably an alkylene group having 2 or 3 carbon atoms. 3 may be the same or different from each other. In formula (4), R 4 R represents a hydrogen atom or a monovalent organic group, and the structure of this monovalent substituent is not particularly limited. 4 R is preferably a hydrogen atom, an alkyl group, an aryl group, or a heteroaryl group, and more preferably a hydrogen atom or an alkyl group. 4When is an alkyl group, the alkyl group is preferably a linear alkyl group having 1 to 20 carbon atoms, a branched alkyl group having 3 to 20 carbon atoms, or a cyclic alkyl group having 5 to 20 carbon atoms, more preferably a linear alkyl group having 1 to 20 carbon atoms, and further preferably a linear alkyl group having 1 to 6 carbon atoms. In formula (4), when q is 2 to 500, a plurality of X present in the graft chain 5 and R 4 may be the same or different from each other.
[0100] Resin A may contain repeating units having two or more different structures, including a graft chain. That is, the molecule of resin A may contain repeating units represented by formulas (1) to (4) having structures different from one another, and when n, m, p, and q in formulas (1) to (4) each represent an integer of 2 or more, in formulas (1) and (2), j and k may have structures different from one another in the side chain, and in formulas (3) and (4), R present in a plurality of units in the molecule may be present. 3 , R 4 , and X 5 may be the same or different from each other.
[0101] The repeating unit represented by formula (1) is more preferably a repeating unit represented by the following formula (1A). The repeating unit represented by formula (2) is more preferably a repeating unit represented by the following formula (2A).
[0102] [ka]
[0103] In formula (1A), X 1 , Y 1 , Z 1 , and n is X in formula (1). 1 , Y 1 , Z 1 In formula (2A), X has the same meaning as n, and the preferred range is also the same. 2 , Y 2 , Z 2, and m is X in formula (2). 2 , Y 2 , Z 2 , and m have the same meaning and preferred range.
[0104] The repeating unit represented by formula (3) is more preferably a repeating unit represented by the following formula (3A) or (3B).
[0105] [ka]
[0106] In formula (3A) or (3B), X 3 , Y 3 , Z 3 , and p is X in formula (3). 3 , Y 3 , Z 3 , and p have the same meanings and preferred ranges.
[0107] Resin A more preferably contains a repeating unit represented by formula (1A) as a repeating unit including a graft chain.
[0108] Resin A also preferably contains a repeating unit containing a polyalkyleneimine structure and a polyester structure. The repeating unit containing a polyalkyleneimine structure and a polyester structure preferably contains a polyalkyleneimine structure in the main chain and a polyester structure as a graft chain.
[0109] The polyalkyleneimine structure is a polymerized structure containing two or more identical or different alkyleneimine chains. Specific examples of the alkyleneimine chain include those represented by the following formula (4A) and formula (4B).
[0110] [ka]
[0111] In formula (4A), R X1 and R X2 each independently represents a hydrogen atom or an alkyl group. 1 represents an integer greater than or equal to 2. 1 represents a bonding position to a polyester chain, an adjacent alkyleneimine chain, or a hydrogen atom or a substituent.
[0112] [ka]
[0113] In formula (4B), R X3 and R X4 each independently represents a hydrogen atom or an alkyl group. 2 represents an integer of 2 or more. The alkyleneimine chain represented by formula (4B) is a polyester chain having an anionic group and a N + The anionic groups contained in the polyester chain form salt bridges, resulting in bonding.
[0114] * in formula (4A) and formula (4B), and * in formula (4B) 2 each independently represents a position at which the group is bonded to an adjacent alkyleneimine chain, or a hydrogen atom or a substituent. In the formula (4A) and the formula (4B), it is particularly preferable that the * represents the position at which the alkyleneimine chain is bonded to the adjacent alkyleneimine chain.
[0115] R in formula (4A) X1 and R X2 and R in formula (4B) X3 and R X4 each independently represents a hydrogen atom or an alkyl group. The alkyl group preferably has 1 to 6 carbon atoms, and more preferably has 1 to 3 carbon atoms. In formula (4A), R X1 and R X2 are preferably all hydrogen atoms. In formula (4B), R X3 and R X4are preferably all hydrogen atoms.
[0116] a in formula (4A) 1 and a in formula (4B) 2 is not particularly limited as long as it is an integer of 2 or more. The upper limit is preferably 10 or less, more preferably 6 or less, even more preferably 4 or less, still more preferably 2 or 3, and particularly preferably 2.
[0117] In formula (4A) and formula (4B), * represents the bonding position to the adjacent alkyleneimine chain, or to a hydrogen atom or a substituent. Examples of the substituent include an alkyl group (for example, an alkyl group having 1 to 6 carbon atoms), etc. Furthermore, a polyester chain may be bonded as the substituent.
[0118] The alkyleneimine chain represented by formula (4A) is the same as that described above. 1 Specifically, it is preferable that the carbonyl carbon in the polyester chain is linked to the polyester chain at the position of 1 It is preferred that the bond is at the position The polyester chain may be represented by the following formula (5A).
[0119] [ka]
[0120] When the alkyleneimine chain is an alkyleneimine chain represented by formula (4B), the polyester chain is anionic (preferably an oxygen anion O - ), and the anionic group and the N in formula (4B) + It is preferred that these form a salt bridge. An example of such a polyester chain is a polyester chain represented by the following formula (5B).
[0121] [ka]
[0122] L in formula (5A) X1 and L in formula (5B) X2 each independently represents a divalent linking group. The divalent linking group is preferably an alkylene group having 3 to 30 carbon atoms.
[0123] b in formula (5A) 11 and b in formula (5B) 21 each independently represents an integer of 2 or more, preferably an integer of 6 or more, and the upper limit thereof is, for example, 200 or less.
[0124] b in formula (5A) 12 and b in formula (5B) 22 each independently represents 0 or 1.
[0125] X in formula (5A) A and X in formula (5B) B each independently represents a hydrogen atom or a substituent. Examples of the substituent include an alkyl group, an alkoxy group, a polyalkyleneoxyalkyl group, and an aryl group.
[0126] The number of carbon atoms in the alkyl group (which may be linear, branched, or cyclic) and the alkyl group contained in the alkoxy group (which may be linear, branched, or cyclic) can be 1 to 30, and preferably 1 to 10. The alkyl group may further have a substituent, and examples of the substituent include a hydroxyl group and a halogen atom (examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom).
[0127] Polyalkyleneoxyalkyl groups are R X6 (OR X7 ) p (O) q R is a substituent represented by the formula: X6 represents an alkyl group, R X7 represents an alkylene group, p represents an integer of 2 or more, and q represents 0 or 1. RX6 The alkyl group represented by X A In addition, R X7 The alkylene group represented by the formula: X A Examples of the alkyl group include those obtained by removing one hydrogen atom from the alkyl group represented by the following formula: p is an integer of 2 or more, and its upper limit is, for example, 10 or less, and preferably 5 or less.
[0128] The aryl group may be, for example, an aryl group having 6 to 24 carbon atoms (which may be either monocyclic or polycyclic). The aryl group may further have a substituent, and examples of the substituent include an alkyl group, a halogen atom, and a cyano group.
[0129] The polyester chain is preferably a structure obtained by ring-opening a lactone such as ε-caprolactone, δ-caprolactone, β-propiolactone, γ-butyrolactone, δ-valerolactone, γ-valerolactone, enantholactone, β-butyrolactone, γ-hexanolactone, γ-octanolactone, δ-hexalanolactone, δ-octanolactone, δ-dodecanolactone, α-methyl-γ-butyrolactone, or lactide (which may be either L- or D-form), and more preferably a structure obtained by ring-opening ε-caprolactone or δ-valerolactone.
[0130] The repeating unit containing the polyalkyleneimine structure and the polyester structure can be synthesized according to the synthesis method described in Japanese Patent No. 5,923,557.
[0131] In the resin A, the content of the repeating unit containing a graft chain is, in mass terms, for example, 2 to 100 mass%, preferably 2 to 95 mass%, more preferably 2 to 90 mass%, and still more preferably 5 to 30 mass%, relative to the total mass of the resin A. When the repeating unit containing a graft chain is contained within this range, the effects of the present invention are more excellent.
[0132] (hydrophobic repeating unit) Resin A may also contain a hydrophobic repeating unit different from the repeating unit containing a graft chain (i.e., not corresponding to the repeating unit containing a graft chain). However, in this specification, a hydrophobic repeating unit is a repeating unit that does not have an acid group (e.g., a carboxylic acid group, a sulfonic acid group, a phosphoric acid group, a phenolic hydroxyl group, etc.).
[0133] The hydrophobic repeating unit is preferably a repeating unit derived from (corresponding to) a compound (monomer) having a ClogP value of 1.2 or more, and more preferably a repeating unit derived from a compound having a ClogP value of 1.2 to 8. This makes it possible to more reliably exhibit the effects of the present invention.
[0134] The ClogP value is a value calculated by the program "CLOGP" available from Daylight Chemical Information System, Inc. This program provides a "calculated logP" value calculated by the fragment approach of Hansch and Leo (see the literature below). The fragment approach is based on the chemical structure of a compound, and divides the chemical structure into partial structures (fragments), and estimates the logP value of the compound by summing up the logP contributions assigned to the fragments. Details are described in the literature below. In this specification, the ClogP value calculated by the program CLOGP v4.82 is used. AJ Leo, Comprehensive Medicinal Chemistry, Vol.4, C. Hansch, PG Sammnens, JB Taylor and CA Ramsden, Eds., p.295, Pergamon Press, 1990 C. Hansch & AJ Leo. SUbstituent Constants For Correlation Analysis in Chemistry and Biology. John Wiley & Sons. AJ Leo. Calculating logPoct from structure. Chem. Rev., 93, 1281-1306, 1993.
[0135] logP stands for the common logarithm of the partition coefficient P, and is a physical property that quantitatively represents how an organic compound is distributed in equilibrium in a two-phase system of oil (generally 1-octanol) and water, and is expressed by the following formula. logP = log(Coil / Cwater) In the formula, Coil represents the molar concentration of the compound in the oil phase, and Cwater represents the molar concentration of the compound in the water phase. As the logP value increases toward the positive side, around 0, the oil solubility increases, and as the absolute value increases toward the negative side, the water solubility increases. It has a negative correlation with the water solubility of organic compounds, and is widely used as a parameter to estimate the hydrophilicity or hydrophobicity of organic compounds.
[0136] Resin A preferably contains, as a hydrophobic repeating unit, one or more repeating units selected from repeating units derived from monomers represented by the following formulas (i) to (iii).
[0137] [ka]
[0138] In the above formulas (i) to (iii), R 1 , R 2 , and R3 each independently represents a hydrogen atom, a halogen atom (for example, a fluorine atom, a chlorine atom, a bromine atom, etc.), or an alkyl group having 1 to 6 carbon atoms (for example, a methyl group, an ethyl group, a propyl group, etc.). R 1 , R 2 , and R 3 R is preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and more preferably a hydrogen atom or a methyl group. 2 and R 3 is more preferably a hydrogen atom. X represents an oxygen atom (-O-) or an imino group (-NH-), and is preferably an oxygen atom.
[0139] L is a single bond or a divalent linking group. Examples of the divalent linking group include a divalent aliphatic group (e.g., an alkylene group, a substituted alkylene group, an alkenylene group, a substituted alkenylene group, an alkynylene group, and a substituted alkynylene group), a divalent aromatic group (e.g., an arylene group, and a substituted arylene group), a divalent heterocyclic group, an oxygen atom (-O-), a sulfur atom (-S-), an imino group (-NH-), and a substituted imino group (-NR 31 -, where R 31 is an aliphatic group, an aromatic group, or a heterocyclic group), a carbonyl group (-CO-), and combinations thereof.
[0140] The divalent aliphatic group may have a cyclic structure or a branched structure. The number of carbon atoms in the aliphatic group is preferably 1 to 20, more preferably 1 to 15, and even more preferably 1 to 10. The aliphatic group may be an unsaturated aliphatic group or a saturated aliphatic group, but a saturated aliphatic group is preferred. The aliphatic group may have a substituent. Examples of the substituent include a halogen atom, an aromatic group, and a heterocyclic group.
[0141] The number of carbon atoms in the divalent aromatic group is preferably 6 to 20, more preferably 6 to 15, and further preferably 6 to 10. The aromatic group may have a substituent. Examples of the substituent include a halogen atom, an aliphatic group, an aromatic group, and a heterocyclic group.
[0142] The divalent heterocyclic group preferably contains a 5-membered or 6-membered ring as a heterocycle. The heterocycle may be condensed with another heterocycle, an aliphatic ring, or an aromatic ring. The heterocyclic group may have a substituent. Examples of the substituent include a halogen atom, a hydroxyl group, an oxo group (=O), a thioxo group (=S), an imino group (=NH), a substituted imino group (=NR 32 , where R 32 is an aliphatic group, an aromatic group, or a heterocyclic group), an aliphatic group, an aromatic group, and a heterocyclic group.
[0143] L is preferably a single bond, an alkylene group, or a divalent linking group containing an oxyalkylene structure. The oxyalkylene structure is more preferably an oxyethylene structure or an oxypropylene structure. L may also contain a polyoxyalkylene structure containing two or more repeated oxyalkylene structures. The polyoxyalkylene structure is preferably a polyoxyethylene structure or a polyoxypropylene structure. The polyoxyethylene structure is represented by -(OCH2CH2)n-, where n is preferably an integer of 2 or more, more preferably an integer of 2 to 10.
[0144] Z includes an aliphatic group (e.g., an alkyl group, a substituted alkyl group, an unsaturated alkyl group, a substituted unsaturated alkyl group), an aromatic group (e.g., an aryl group, a substituted aryl group, an arylene group, a substituted arylene group), a heterocyclic group, and combinations thereof. These groups include an oxygen atom (-O-), a sulfur atom (-S-), an imino group (-NH-), a substituted imino group (-NR 31 -, where R 31 may contain an aliphatic group, an aromatic group, or a heterocyclic group), or a carbonyl group (-CO-).
[0145] The aliphatic group may have a cyclic structure or a branched structure. The number of carbon atoms in the aliphatic group is preferably 1 to 20, more preferably 1 to 15, and even more preferably 1 to 10. The aliphatic group further includes a ring assembly hydrocarbon group and a bridged cyclic hydrocarbon group. Examples of the ring assembly hydrocarbon group include a bicyclohexyl group, a perhydronaphthalenyl group, a biphenyl group, and a 4-cyclohexylphenyl group. Examples of the bridged cyclic hydrocarbon ring include bicyclic hydrocarbon rings such as pinane, bornane, norpinane, norbornane, and bicyclooctane rings (such as bicyclo[2.2.2]octane ring and bicyclo[3.2.1]octane ring), homobredane, adamantane, and tricyclo[5.2.1.0]octane ring. 2,6 ]decane and tricyclo[4.3.1.1 2,5 ]undecane ring and other tricyclic hydrocarbon rings, as well as tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodecane, and tetracyclic hydrocarbon rings such as perhydro-1,4-methano-5,8-methanonaphthalene ring. The bridged cyclic hydrocarbon ring also includes condensed rings in which multiple 5- to 8-membered cycloalkane rings are condensed, such as perhydronaphthalene (decalin), perhydroanthracene, perhydrophenanthrene, perhydroacenaphthene, perhydrofluorene, perhydroindene, and perhydrophenalene rings. The aliphatic group is preferably a saturated aliphatic group rather than an unsaturated aliphatic group. The aliphatic group may have a substituent. Examples of the substituent include a halogen atom, an aromatic group, and a heterocyclic group. However, the aliphatic group does not have an acid group as a substituent.
[0146] The number of carbon atoms in the aromatic group is preferably 6 to 20, more preferably 6 to 15, and further preferably 6 to 10. The aromatic group may have a substituent. Examples of the substituent include a halogen atom, an aliphatic group, an aromatic group, and a heterocyclic group. However, the aromatic group does not have an acid group as a substituent.
[0147] The heterocyclic group preferably contains a 5- or 6-membered ring as a heterocycle. The heterocycle may be condensed with another heterocycle, an aliphatic ring, or an aromatic ring. The heterocyclic group may have a substituent. Examples of the substituent include a halogen atom, a hydroxyl group, an oxo group (=O), a thioxo group (=S), an imino group (=NH), a substituted imino group (=NR 32 , where R 32 is an aliphatic group, an aromatic group, or a heterocyclic group), an aliphatic group, an aromatic group, and a heterocyclic group, provided that the heterocyclic group does not have an acid group as a substituent.
[0148] In the above formula (iii), R 4 , R 5 , and R 6 R each independently represents a hydrogen atom, a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, etc.), an alkyl group having 1 to 6 carbon atoms (e.g., a methyl group, an ethyl group, a propyl group, etc.), Z, or LZ, where L and Z are the same as the groups defined above. 4 , R 5 , and R 6 is preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and more preferably a hydrogen atom.
[0149] As the monomer represented by the above formula (i), R 1 , R 2 , and R 3 is a hydrogen atom or a methyl group, L is a single bond or a divalent linking group containing an alkylene group or an oxyalkylene structure, X is an oxygen atom or an imino group, and Z is an aliphatic group, a heterocyclic group, or an aromatic group. In addition, as the monomer represented by the above formula (ii), R 1 is a hydrogen atom or a methyl group, L is an alkylene group, and Z is an aliphatic group, a heterocyclic group, or an aromatic group. 4 , R 5 , and R 6 is a hydrogen atom or a methyl group, and Z is an aliphatic group, a heterocyclic group, or an aromatic group.
[0150] Representative examples of the compounds represented by formulas (i) to (iii) include radically polymerizable compounds selected from acrylic acid esters, methacrylic acid esters, styrenes, and the like. Representative examples of the compounds represented by formulas (i) to (iii) can be found in the compounds described in paragraphs 0089 to 0093 of JP-A No. 2013-249417, the contents of which are incorporated herein by reference.
[0151] In the resin A, the content of the hydrophobic repeating unit is preferably from 10 to 90 mass %, and more preferably from 20 to 80 mass %, based on the total mass of the resin A, in terms of mass.
[0152] (Functional group capable of forming an interaction with magnetic particles) Resin A may have a functional group capable of forming an interaction with the magnetic particles. It is preferable that resin A further contains a repeating unit containing a functional group capable of forming an interaction with the magnetic particles. Examples of functional groups capable of forming interactions with magnetic particles include acid groups, basic groups, coordinating groups, and reactive functional groups. When resin A contains an acid group, a basic group, a coordinating group, or a reactive functional group, it preferably contains a repeating unit containing an acid group, a repeating unit containing a basic group, a repeating unit containing a coordinating group, or a repeating unit having a reactive functional group, respectively.
[0153] The repeating unit containing an acid group may be the same as or different from the repeating unit containing the graft chain described above, but the repeating unit containing an acid group is a repeating unit different from the hydrophobic repeating unit described above (i.e., it does not correspond to the hydrophobic repeating unit described above).
[0154] Examples of the acid group, which is a functional group capable of forming an interaction with the magnetic particles, include a carboxylic acid group, a sulfonic acid group, a phosphoric acid group, and a phenolic hydroxyl group, and at least one of the carboxylic acid group, the sulfonic acid group, and the phosphoric acid group is preferred, and the carboxylic acid group is more preferred. The carboxylic acid group has a good adsorption force to the magnetic particles and is highly dispersible. That is, it is preferable that resin A further contains a repeating unit containing at least one of a carboxylic acid group, a sulfonic acid group, and a phosphoric acid group.
[0155] Resin A may have one or more types of repeating units containing an acid group. When the resin A contains a repeating unit containing an acid group, the content thereof is preferably from 5 to 80 mass %, and more preferably from 10 to 60 mass %, based on the total mass of the resin A, in mass terms.
[0156] Examples of basic groups that are functional groups capable of forming interactions with magnetic particles include primary amino groups, secondary amino groups, tertiary amino groups, heterocycles containing N atoms, and amide groups, and a preferred basic group is a tertiary amino group because of its good adsorption to magnetic particles and high dispersibility. Resin A may contain one or more of these basic groups. When the resin A contains a repeating unit containing a basic group, the content thereof is preferably from 0.01 to 50 mass %, and more preferably from 0.01 to 30 mass %, based on the total mass of the resin A, in mass conversion.
[0157] Examples of the coordinating group, which is a functional group capable of forming an interaction with the magnetic particles, and the reactive functional group include an acetylacetoxy group, a trialkoxysilyl group, an isocyanate group, an acid anhydride, and an acid chloride. A preferred functional group is an acetylacetoxy group, which has good adsorption power to the magnetic particles and high dispersibility of the magnetic particles. Resin A may have one or more of these groups. When resin A contains a repeating unit containing a coordinating group or a repeating unit containing a reactive functional group, the content of these units, calculated on a mass basis, is preferably 10 to 80 mass % and more preferably 20 to 60 mass % based on the total mass of resin A.
[0158] When the resin A contains functional groups capable of forming interactions with magnetic particles other than the graft chains, it is sufficient that the resin A contains functional groups capable of forming interactions with the various magnetic particles, and there are no particular limitations on how these functional groups are introduced. For example, it is preferable that the resin contained in the composition contains one or more repeating units selected from repeating units derived from monomers represented by the following formulas (iv) to (vi).
[0159] [ka]
[0160] In formulas (iv) to (vi), R 11 , R 12 , and R 13 each independently represents a hydrogen atom, a halogen atom (for example, a fluorine atom, a chlorine atom, a bromine atom, etc.), or an alkyl group having 1 to 6 carbon atoms (for example, a methyl group, an ethyl group, a propyl group, etc.). In formulas (iv) to (vi), R 11 , R 12 , and R 13 In general formula (iv), R is preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and more preferably a hydrogen atom or a methyl group. 12 and R 13 is more preferably a hydrogen atom.
[0161] X1 in formula (iv) represents an oxygen atom (-O-) or an imino group (-NH-), and is preferably an oxygen atom. In addition, Y in the formula (v) represents a methine group or a nitrogen atom.
[0162] Furthermore, L1 in formulas (iv) to (v) represents a single bond or a divalent linking group. The definition of the divalent linking group is the same as the definition of the divalent linking group represented by L in formula (i) above.
[0163] L1 is preferably a single bond, an alkylene group, or a divalent linking group containing an oxyalkylene structure. The oxyalkylene structure is more preferably an oxyethylene structure or an oxypropylene structure. L1 may also contain a polyoxyalkylene structure containing two or more repeated oxyalkylene structures. The polyoxyalkylene structure is preferably a polyoxyethylene structure or a polyoxypropylene structure. The polyoxyethylene structure is represented by -(OCH2CH2)n-, where n is preferably an integer of 2 or more, more preferably an integer of 2 to 10.
[0164] In the formulae (iv) to (vi), Z1 represents a functional group capable of forming an interaction with the magnetic particles other than the graft chain, and is preferably a carboxylic acid group or a tertiary amino group, more preferably a carboxylic acid group.
[0165] In formula (vi), R 14 , R 15 , and R 16 R each independently represents a hydrogen atom, a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, etc.), an alkyl group having 1 to 6 carbon atoms (e.g., a methyl group, an ethyl group, a propyl group, etc.), -Z1, or L1-Z1. Here, L1 and Z1 have the same meanings as L1 and Z1 above, and preferred examples are also the same. R 14 , R 15 , and R 16 is preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and more preferably a hydrogen atom.
[0166] As the monomer represented by formula (iv), R 11 , R 12 , and R 13are each independently a hydrogen atom or a methyl group, L1 is an alkylene group or a divalent linking group containing an oxyalkylene structure, X1 is an oxygen atom or an imino group, and Z1 is a carboxylic acid group. In addition, as the monomer represented by formula (v), R 11 is a hydrogen atom or a methyl group, L1 is an alkylene group, Z1 is a carboxylic acid group, and Y is a methine group. Further, as the monomer represented by formula (vi), R 14 , R 15 , and R 16 are each independently a hydrogen atom or a methyl group, and Z1 is a carboxylic acid group.
[0167] Representative examples of the monomers (compounds) represented by formulas (iv) to (vi) are shown below. Examples of the monomer include methacrylic acid, crotonic acid, isocrotonic acid, a reaction product of a compound containing an addition polymerizable double bond and a hydroxyl group in the molecule (e.g., 2-hydroxyethyl methacrylate) with succinic anhydride, a reaction product of a compound containing an addition polymerizable double bond and a hydroxyl group in the molecule with phthalic anhydride, a reaction product of a compound containing an addition polymerizable double bond and a hydroxyl group in the molecule with tetrahydroxyphthalic anhydride, a reaction product of a compound containing an addition polymerizable double bond and a hydroxyl group in the molecule with trimellitic anhydride, a reaction product of a compound containing an addition polymerizable double bond and a hydroxyl group in the molecule with pyromellitic anhydride, acrylic acid, acrylic acid dimer, acrylic acid oligomer, maleic acid, itaconic acid, fumaric acid, 4-vinylbenzoic acid, vinylphenol, and 4-hydroxyphenylmethacrylamide.
[0168] The content of the repeating unit containing a functional group capable of forming an interaction with the magnetic particles is, in terms of the interaction with the magnetic particles, stability over time, and permeability into the developer, preferably 0.05 to 90 mass %, more preferably 1.0 to 80 mass %, and even more preferably 10 to 70 mass %, relative to the total mass of resin A.
[0169] (ethylenically unsaturated group) Resin A may contain an ethylenically unsaturated group. The ethylenically unsaturated group is not particularly limited, but examples thereof include a (meth)acryloyl group, a vinyl group, and a styryl group, with a (meth)acryloyl group being preferred. Resin A preferably contains a repeating unit containing an ethylenically unsaturated group in the side chain, and more preferably contains a repeating unit containing an ethylenically unsaturated group in the side chain and derived from a (meth)acrylate (hereinafter also referred to as a "(meth)acrylic repeating unit containing an ethylenically unsaturated group in the side chain"). The (meth)acrylic repeating unit containing an ethylenically unsaturated group in the side chain can be obtained, for example, by adding an ethylenically unsaturated compound containing a glycidyl group or an alicyclic epoxy group to the carboxylic acid group in the resin A containing a (meth)acrylic repeating unit containing a carboxylic acid group. By reacting the ethylenically unsaturated group (glycidyl group or alicyclic epoxy group) introduced in this way, a (meth)acrylic repeating unit containing an ethylenically unsaturated group in the side chain can be obtained.
[0170] When the resin A contains a repeating unit containing an ethylenically unsaturated group, the content thereof is preferably from 30 to 70 mass %, and more preferably from 40 to 60 mass %, based on the total mass of the resin A in mass terms.
[0171] (Other curing groups) Resin A may contain other curable groups in addition to the ethylenically unsaturated group. Other curable groups include, for example, epoxy groups and oxetanyl groups. Resin A preferably contains a repeating unit containing another curable group in the side chain, and more preferably contains a repeating unit containing another curable group in the side chain and derived from a (meth)acrylate (hereinafter also referred to as a "(meth)acrylic repeating unit containing another curable group in the side chain"). An example of a (meth)acrylic repeating unit containing another curable group in the side chain is glycidyl (meth)acrylate.
[0172] When the resin A contains a repeating unit containing another curable group, the content thereof is preferably from 5 to 50 mass %, and more preferably from 10 to 30 mass %, based on the total mass of the resin A, in mass conversion.
[0173] (Other repeating units) Furthermore, for the purpose of improving various properties such as film-forming ability, resin A may further contain other repeating units having various functions different from the repeating units described above, as long as the effects of the present invention are not impaired. Examples of such other repeating units include repeating units derived from radically polymerizable compounds selected from acrylonitriles and methacrylonitriles. Resin A may use one or more of these other repeating units, and the content thereof, calculated on a mass basis, is preferably from 0 to 80 mass %, more preferably from 10 to 60 mass %, based on the total mass of resin A.
[0174] (Physical properties of resin A) The acid value of resin A is not particularly limited, but is, for example, preferably 0 to 400 mgKOH / g, more preferably 10 to 350 mgKOH / g, further preferably 30 to 300 mgKOH / g, and particularly preferably in the range of 50 to 200 mgKOH / g. If the acid value of resin A is 50 mgKOH / g or more, the sedimentation stability of the magnetic particles can be further improved.
[0175] In this specification, the acid value can be calculated, for example, from the average content of acid groups in a compound. Furthermore, a resin having a desired acid value can be obtained by changing the content of repeating units containing an acid group in the resin.
[0176] The weight average molecular weight of the resin A is not particularly limited, but is preferably, for example, 3,000 or more, more preferably 4,000 or more, even more preferably 5,000 or more, and particularly preferably 6,000 or more. The upper limit is, for example, preferably 300,000 or less, more preferably 200,000 or less, even more preferably 100,000 or less, and particularly preferably 50,000 or less. Resin A can be synthesized based on a known method.
[0177] As specific examples of Resin A, reference can be made to the polymer compounds described in paragraphs 0127 to 0129 of JP-A No. 2013-249417, the contents of which are incorporated herein by reference.
[0178] Furthermore, as the resin A, the graft copolymers described in paragraphs 0037 to 0115 of JP 2010-106268 A (corresponding paragraphs 0075 to 0133 of US 2011 / 0124824) can also be used, the contents of which are incorporated herein by reference.
[0179] <Alkali-soluble resin> The other resin may include an alkali-soluble resin. In this specification, the alkali-soluble resin refers to a resin that contains a group that promotes alkali solubility (alkali-soluble group, for example an acid group such as a carboxylic acid group), and refers to a resin different from the resin A described above.
[0180] Examples of the alkali-soluble resin include resins containing at least one alkali-soluble group in the molecule, such as polyhydroxystyrene resins, polysiloxane resins, (meth)acrylic resins, (meth)acrylamide resins, (meth)acrylic / (meth)acrylamide copolymers, epoxy resins, and polyimide resins.
[0181] Specific examples of alkali-soluble resins include copolymers of unsaturated carboxylic acids and ethylenically unsaturated compounds. The unsaturated carboxylic acid is not particularly limited, but examples thereof include monocarboxylic acids such as (meth)acrylic acid, crotonic acid, and vinylacetic acid; dicarboxylic acids such as itaconic acid, maleic acid, and fumaric acid, or acid anhydrides thereof; and polycarboxylic acid monoesters such as mono(2-(meth)acryloyloxyethyl)phthalate.
[0182] Examples of the copolymerizable ethylenically unsaturated compound include methyl (meth)acrylate, etc. Compounds described in paragraph 0027 of JP 2010-97210 A and paragraphs 0036-0037 of JP 2015-68893 A can also be used, and the contents of the above are incorporated herein by reference.
[0183] In addition, a copolymerizable ethylenically unsaturated compound having an ethylenically unsaturated group in a side chain may be used in combination. In other words, the alkali-soluble resin may contain a repeating unit having an ethylenically unsaturated group in a side chain. The ethylenically unsaturated group contained in the side chain is preferably a (meth)acrylic acid group. A repeating unit containing an ethylenically unsaturated group in a side chain can be obtained, for example, by subjecting a carboxylic acid group of a (meth)acrylic repeating unit containing a carboxylic acid group to an addition reaction with an ethylenically unsaturated compound containing a glycidyl group or an alicyclic epoxy group.
[0184] The alkali-soluble resin is also preferably an alkali-soluble resin containing a curable group. Examples of the curable group include, but are not limited to, ethylenically unsaturated groups (e.g., (meth)acryloyl groups, vinyl groups, styryl groups, etc.) and cyclic ether groups (e.g., epoxy groups, oxetanyl groups, etc.). Among these, the curable group is preferably an ethylenically unsaturated group, and more preferably a (meth)acryloyl group, in terms of the ability to control polymerization by radical reaction. The alkali-soluble resin containing a curable group is preferably an alkali-soluble resin having a curable group in a side chain, etc. Examples of the alkali-soluble resin containing a curable group include Dianaru NR series (manufactured by Mitsubishi Rayon Co., Ltd.), Photomer 6173 (COOH-containing polyurethane acrylic oligomer, manufactured by Diamond Shamrock Co., Ltd.), Viscoat R-264, KS Resist 106 (all manufactured by Osaka Organic Chemical Industry Co., Ltd.), Cyclomer P series (e.g., ACA230AA), Plaxel CF200 series (all manufactured by Daicel Corporation), Ebecryl 3800 (manufactured by Daicel-Allnex Corporation), and Acricur RD-F8 (manufactured by Nippon Shokubai Co., Ltd.).
[0185] Examples of the alkali-soluble resin include radical polymers having a carboxylic acid group in the side chain described in JP-A-59-44615, JP-B-54-34327, JP-B-58-12577, JP-B-54-25957, JP-A-54-92723, JP-A-59-53836, and JP-A-59-71048; Examples of binder resins that can be used include acetal-modified polyvinyl alcohol-based binder resins containing an alkali-soluble group as described in JP 1-318463 A; polyvinylpyrrolidone; polyethylene oxide; alcohol-soluble nylon, and polyethers which are reaction products of 2,2-bis-(4-hydroxyphenyl)-propane and epichlorohydrin; and polyimide resins as described in WO 2008 / 123097 A.
[0186] As the alkali-soluble resin, for example, the compounds described in paragraphs 0225 to 0245 of JP-A-2016-75845 can also be used, the contents of which are incorporated herein by reference.
[0187] As the alkali-soluble resin, a polyimide precursor can also be used. The polyimide precursor refers to a resin obtained by subjecting a compound containing an acid anhydride group and a diamine compound to an addition polymerization reaction at 40 to 100°C. Specific examples of the polyimide precursor include compounds described in paragraphs 0011 to 0031 of JP 2008-106250 A, compounds described in paragraphs 0022 to 0039 of JP 2016-122101 A, compounds described in paragraphs 0061 to 0092 of JP 2016-68401 A, resins described in paragraph 0050 of JP 2014-137523 A, resins described in paragraph 0058 of JP 2015-187676 A, and resins described in paragraphs 0012 to 0013 of JP 2014-106326 A, the contents of which are incorporated herein by reference.
[0188] As the alkali-soluble resin, a copolymer of benzyl (meth)acrylate / (meth)acrylic acid / if necessary, other addition-polymerizable vinyl monomers and a copolymer of allyl (meth)acrylate / (meth)acrylic acid / if necessary, other addition-polymerizable vinyl monomers are preferred, as they have an excellent balance of film strength, sensitivity, and developability. The other addition-polymerizable vinyl monomers may be used alone or in combination of two or more kinds. The copolymer preferably contains a curable group, and more preferably contains an ethylenically unsaturated group such as a (meth)acryloyl group, in order to provide a cured film with better moisture resistance. For example, a curable group may be introduced into the copolymer by using a monomer having a curable group as the other addition polymerizable vinyl monomer. Also, a curable group (preferably an ethylenically unsaturated group such as a (meth)acryloyl group) may be introduced into a part or all of one or more of the units derived from (meth)acrylic acid and / or the other addition polymerizable vinyl monomer in the copolymer. Examples of the other addition-polymerizable vinyl monomers include methyl (meth)acrylate, styrene-based monomers (such as hydroxystyrene), and ether dimers. Examples of the ether dimer include a compound represented by the following general formula (ED1) and a compound represented by the following general formula (ED2).
[0189] [ka]
[0190] In general formula (ED1), R 1 and R 2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms.
[0191] [ka]
[0192] In the general formula (ED2), R represents a hydrogen atom or an organic group having a carbon number of 1 to 30. Specific examples of the general formula (ED2) can be found in JP-A-2010-168539.
[0193] For specific examples of the ether dimer, see, for example, paragraph 0317 of JP 2013-29760 A, the contents of which are incorporated herein by reference. The ether dimer may be one type only, or two or more types.
[0194] The acid value of the alkali-soluble resin is not particularly limited, but in general, it is preferably from 30 to 500 mgKOH / g, and more preferably from 50 to 200 mgKOH / g or more.
[0195] When the composition contains an alkali-soluble resin, the content of the alkali-soluble resin is preferably 0.1 to 40 mass %, more preferably 0.5 to 30 mass %, and further preferably 1 to 20 mass %, based on the total mass of the composition. When the composition contains an alkali-soluble resin, the content of the alkali-soluble resin is preferably 0.1 to 40 mass %, more preferably 0.5 to 30 mass %, and further preferably 1 to 20 mass %, based on the total solid content of the composition.
[0196] [Polymerizable compound] The composition of the present invention may contain a polymerizable compound as a component different from the above-mentioned components.
[0197] The content of the polymerizable compound is preferably from 1 to 35 mass %, more preferably from 1 to 30 mass %, and further preferably from 3 to 27 mass %, based on the total mass of the composition. The content of the polymerizable compound is preferably from 1 to 35 mass %, more preferably from 1 to 30 mass %, and further preferably from 3 to 27 mass %, based on the total solid content of the composition. The molecular weight (or weight average molecular weight) of the polymerizable compound is not particularly limited, but is preferably 2000 or less.
[0198] <Compound containing a group containing an ethylenically unsaturated bond> Examples of the polymerizable compound include compounds that contain a group containing an ethylenically unsaturated bond (hereinafter, also simply referred to as an "ethylenically unsaturated group"). That is, the composition of the present invention preferably contains a low molecular weight compound containing an ethylenically unsaturated group as a polymerizable compound. The polymerizable compound is preferably a compound containing one or more ethylenically unsaturated bonds, more preferably a compound containing two or more, even more preferably a compound containing three or more, and particularly preferably a compound containing five or more. The upper limit is, for example, 15 or less. Examples of the ethylenically unsaturated group include a vinyl group, a (meth)allyl group, and a (meth)acryloyl group.
[0199] As the polymerizable compound, for example, the compounds described in paragraph 0050 of JP-A-2008-260927 and paragraph 0040 of JP-A-2015-68893 can be used, the contents of which are incorporated herein by reference.
[0200] The polymerizable compound may be in any chemical form, such as a monomer, a prepolymer, an oligomer, a mixture thereof, or a polymer thereof. The polymerizable compound is preferably a 3- to 15-functional (meth)acrylate compound, and more preferably a 3- to 6-functional (meth)acrylate compound.
[0201] The polymerizable compound is also preferably a compound containing one or more ethylenically unsaturated groups and having a boiling point of 100° C. or higher under normal pressure. For example, the compounds described in paragraphs
[0227] of JP-A-2013-29760 and paragraphs
[0254] to
[0257] of JP-A-2008-292970 can be referred to, the contents of which are incorporated herein by reference.
[0202] The polymerizable compound is preferably dipentaerythritol triacrylate (commercially available product is KAYARAD D-330; manufactured by Nippon Kayaku Co., Ltd.), dipentaerythritol tetraacrylate (commercially available product is KAYARAD D-320; manufactured by Nippon Kayaku Co., Ltd.), dipentaerythritol penta(meth)acrylate (commercially available product is KAYARAD D-310; manufactured by Nippon Kayaku Co., Ltd.), dipentaerythritol hexa(meth)acrylate (commercially available products are KAYARAD DPHA; manufactured by Nippon Kayaku Co., Ltd., A-DPH-12E; manufactured by Shin-Nakamura Chemical Co., Ltd.), and a structure in which the (meth)acryloyl group of these is mediated by an ethylene glycol residue or a propylene glycol residue (for example, SR454, SR499, commercially available from Sartomer Co., Ltd.). Oligomer types of these can also be used. In addition, NK Ester A-TMMT (pentaerythritol tetraacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.), KAYARAD RP-1040, KAYARAD DPEA-12LT, KAYARAD DPHA LT, KAYARAD RP-3060, and KAYARAD DPEA-12 (all trade names, manufactured by Nippon Kayaku Co., Ltd.), etc. may also be used.
[0203] The polymerizable compound may have an acid group such as a carboxylic acid group, a sulfonic acid group, and a phosphoric acid group. The polymerizable compound containing an acid group is preferably an ester of an aliphatic polyhydroxy compound and an unsaturated carboxylic acid, more preferably the polymerizable compound in which an acid group is provided by reacting an unreacted hydroxyl group of an aliphatic polyhydroxy compound with a non-aromatic carboxylic anhydride, and more preferably the compound in which the aliphatic polyhydroxy compound is pentaerythritol and / or dipentaerythritol in the ester. Examples of commercially available products include Aronix TO-2349, M-305, M-510, and M-520 manufactured by Toagosei Co., Ltd.
[0204] The acid value of the polymerizable compound containing an acid group is preferably 0.1 to 40 mgKOH / g, more preferably 5 to 30 mgKOH / g. If the acid value of the polymerizable compound is 0.1 mgKOH / g or more, the development dissolution property is good, and if it is 40 mgKOH / g or less, it is advantageous in terms of production and / or handling. Furthermore, the photopolymerization performance is good and the curing property is excellent.
[0205] In a preferred embodiment, the polymerizable compound is a compound containing a caprolactone structure. The compound containing a caprolactone structure is not particularly limited as long as it contains a caprolactone structure in the molecule, and examples thereof include ε-caprolactone-modified polyfunctional (meth)acrylates obtained by esterifying a polyhydric alcohol such as trimethylolethane, ditrimethylolethane, trimethylolpropane, ditrimethylolpropane, pentaerythritol, dipentaerythritol, tripentaerythritol, glycerin, diglycerol, or trimethylolmelamine with (meth)acrylic acid and ε-caprolactone. Among these, a compound containing a caprolactone structure represented by the following formula (Z-1) is preferred.
[0206] [ka]
[0207] In formula (Z-1), all of the six R's are groups represented by the following formula (Z-2), or 1 to 5 of the six R's are groups represented by the following formula (Z-2), and the remainder are groups represented by the following formula (Z-3).
[0208] [ka]
[0209] In formula (Z-2), R 1 represents a hydrogen atom or a methyl group, m represents the number 1 or 2, and "*" represents a bond.
[0210] [ka]
[0211] In formula (Z-3), R 1 represents a hydrogen atom or a methyl group, and "*" represents a bond.
[0212] The above polymerizable compound containing a caprolactone structure is commercially available, for example, from Nippon Kayaku as the KAYARAD DPCA series, and is DPCA-20 (in the above formulas (Z-1) to (Z-3), m=1, the number of groups represented by formula (Z-2)=2, R 1 are all hydrogen atoms), DPCA-30 (same formula, m=1, the number of groups represented by formula (Z-2)=3, R 1 are all hydrogen atoms), DPCA-60 (same formula, m=1, the number of groups represented by formula (Z-2)=6, R 1 are all hydrogen atoms), and DPCA-120 (wherein m=2, the number of groups represented by formula (Z-2)=6, R 1 are all hydrogen atoms). In addition, a commercially available product of the polymerizable compound containing a caprolactone structure is M-350 (trade name) (trimethylolpropane triacrylate) manufactured by Toagosei Co., Ltd.
[0213] As the polymerizable compound, a compound represented by the following formula (Z-4) or (Z-5) can also be used.
[0214] [ka]
[0215] In formulas (Z-4) and (Z-5), E is -((CH2) y CH2O)- or ((CH2) y CH(CH3)O)-, y represents an integer of 0 to 10, and X represents a (meth)acryloyl group, a hydrogen atom, or a carboxylic acid group. In formula (Z-4), the total number of (meth)acryloyl groups is 3 or 4; m represents an integer of 0 to 10; the sum of the m's is an integer of 0 to 40. In formula (Z-5), the total number of (meth)acryloyl groups is 5 or 6; n represents an integer of 0 to 10; and the sum of the n's is an integer of 0 to 60.
[0216] In formula (Z-4), m is preferably an integer of 0 to 6, and more preferably an integer of 0 to 4. The sum of the m's is preferably an integer of 2 to 40, more preferably an integer of 2 to 16, and further preferably an integer of 4 to 8. In the formula (Z-5), n is preferably an integer of 0 to 6, and more preferably an integer of 0 to 4. The sum of each n is preferably an integer of 3 to 60, more preferably an integer of 3 to 24, and further preferably an integer of 6 to 12. In addition, -((CH2) y CH2O)- or ((CH2) y In the case of CH(CH3)O)-, the terminal on the oxygen atom side is preferably bonded to X.
[0217] The compound represented by formula (Z-4) or formula (Z-5) may be used alone or in combination of two or more. In particular, in formula (Z-5), the form in which all six Xs are acryloyl groups, and in formula (Z-5), the mixture of the compound in which all six Xs are acryloyl groups and the compound in which at least one of the six Xs is a hydrogen atom are preferred. With this configuration, the developability can be further improved.
[0218] The total content of the compound represented by formula (Z-4) or formula (Z-5) in the polymerizable compound is preferably 20% by mass or more, and more preferably 50% by mass or more. Among the compounds represented by formula (Z-4) or formula (Z-5), pentaerythritol derivatives and / or dipentaerythritol derivatives are more preferred.
[0219] The polymerizable compound may contain a cardo skeleton. As the above-mentioned polymerizable compound containing a cardo skeleton, the above-mentioned polymerizable compound containing a 9,9-bisarylfluorene skeleton is preferable. The above-mentioned polymerizable compound containing a cardo skeleton is not limited, but examples thereof include Oncoat EX series (manufactured by Nagase & Co., Ltd.) and OGSOL (manufactured by Osaka Gas Chemicals Co., Ltd.). The polymerizable compound is also preferably a compound containing an isocyanuric acid skeleton as a central core. An example of such a polymerizable compound is NK Ester A-9300 (manufactured by Shin-Nakamura Chemical Co., Ltd.). The content of the ethylenically unsaturated group in the polymerizable compound (meaning the value obtained by dividing the number of ethylenically unsaturated groups in the polymerizable compound by the molecular weight (g / mol) of the polymerizable compound) is preferably 5.0 mmol / g or more. The upper limit is not particularly limited, but is generally 20.0 mmol / g or less.
[0220] <Compound Having Epoxy Group and / or Oxetanyl Group> The polymerizable compound is also preferably a compound having an epoxy group and / or an oxetanyl group. The polymerizable compound preferably has one or more epoxy groups and / or oxetanyl groups, and more preferably has 2 to 10 epoxy groups and / or oxetanyl groups. Among them, the polymerizable compound is more preferably an epoxy-curable compound having an epoxy group (epoxy compound). In the above polymerizable compound, the epoxy group and / or oxetanyl group (preferably the epoxy group) may be condensed with a cyclic group (such as an alicyclic group). The cyclic group condensed with the epoxy group and / or oxetanyl group preferably has 5 to 15 carbon atoms. In the above cyclic group, the portion other than the condensed epoxy group and / or oxetanyl group may be a monocyclic or polycyclic ring. Only one epoxy group or oxetanyl group may be condensed with one cyclic group, or two or more epoxy groups and / or oxetanyl groups may be condensed with one cyclic group.
[0221] The polymerizable compound may, for example, be a monofunctional or polyfunctional glycidyl ether compound. The polymerizable compound may be, for example, a (poly)alkylene glycol diglycidyl ether.
[0222] The polymerizable compound may be a compound containing a caprolactone structure represented by the above formula (Z-1), in which the group represented by formula (Z-2) is changed to the following formula (Z-2E) and the group represented by formula (Z-3) is changed to the group represented by formula (Z-3E).
[0223] [ka]
[0224] In formula (Z-2E), m represents the number 1 or 2, X and Y each independently represent a hydrogen atom or a substituent (preferably an alkyl group, preferably having 1 to 3 carbon atoms), and "*" represents a bond. In formula (Z-3E), X and Y each independently represent a hydrogen atom or a substituent (preferably an alkyl group, preferably having 1 to 3 carbon atoms), and "*" represents a bond.
[0225] The polymerizable compound may be a compound represented by the above formula (Z-4) modified so that X represents a group represented by formula (Z-3E) or a hydrogen atom. In the formula (Z-4) modified in this way, the total number of groups represented by formula (Z-3E) is 2 to 4.
[0226] The polymerizable compound may be a compound represented by the above formula (Z-5) modified so that X represents a group represented by formula (Z-3E) or a hydrogen atom. In the formula (Z-5) modified in this way, the total number of groups represented by formula (Z-3E) is 2 to 6 (preferably 5 or 6).
[0227] The polymerizable compound may be a compound having a structure in which N (number of) cyclic groups condensed with an epoxy group and / or an oxetanyl group are bonded via a linking group. N is an integer of 2 or more, preferably an integer of 2 to 6, and more preferably 2. The total number of atoms other than hydrogen atoms in the linking group is preferably 1 to 20, and more preferably 2 to 6. When N is 2, examples of the linking group include an alkyleneoxycarbonyl group.
[0228] Commercially available polymerizable compounds include polyfunctional aliphatic glycidyl ether compounds such as Denacol EX-212L, EX-214L, EX-216L, EX-321L, and EX-850L (all manufactured by Nagase ChemteX Corp.). These are low-chlorine products, but not low-chlorine products such as EX-212, EX-214, EX-216, EX-321, EX-614, and EX-850 can also be used. In addition, a commercially available product such as Celloxide 2021P (manufactured by Daicel Corporation, a multifunctional epoxy monomer) can also be used.
[0229] The composition may contain, as the polymerizable compound, both a compound containing a group containing an ethylenically unsaturated bond and a compound having an epoxy group and / or an oxetanyl group. In this case, the mass ratio of their contents (the content of "compound containing a group containing an ethylenically unsaturated bond" / the content of "compound having an epoxy group and / or an oxetanyl group") is preferably 10 / 90 to 90 / 10, more preferably 20 / 80 to 80 / 20, and even more preferably 30 / 70 to 70 / 30.
[0230] [Curing Accelerator] The composition may contain a cure accelerator. In particular, when the composition contains a compound having an epoxy group and / or an oxetanyl group as the polymerizable compound, it is preferred that the composition contains a curing accelerator. Examples of the curing accelerator include triphenylphosphine, methyltributylphosphonium dimethylphosphate, tris-orthotolylphosphine, and boron trifluoride amine complex. Other examples include 2-methylimidazole (trade name: 2MZ), 2-undecylimidazole (trade name: C11-Z), 2-heptadecylimidazole (trade name: C17Z), 1,2-dimethylimidazole (trade name: 1.2DMZ), 2-ethyl-4-methylimidazole (trade name: 2E4MZ), 2-phenylimidazole (trade name: 2PZ), 2-phenyl-4-methylimidazole (trade name: 2P4MZ), 1-benzyl-2-methylimidazole (trade name: 1B2 ... 1-cyanoethyl-2-phenylimidazole (trade name; 1B2PZ), 1-cyanoethyl-2-methylimidazole (trade name; 2MZ-CN), 1-cyanoethyl-2-undecylimidazole (trade name; C11Z-CN), 1-cyanoethyl-2-phenylimidazolium trimellitate (trade name; 2PZCNS-PW), 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine (trade name; 2MZ-A), 2,4-diamino-6-[2'-undecylimidazolyl -(1')]-ethyl-s-triazine (trade name; C11Z-A), 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine (trade name; 2E4MZ-A), 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct (trade name; 2MA-OK), 2-phenyl-4,5-dihydroxymethylimidazole (trade name; 2PHZ-PW), 2-phenyl-4-methyl-5- ... Examples of imidazole-based curing accelerators include phenylimidazole (trade name: 2P4MHZ-PW), 1-cyanoethyl-2-phenylimidazole (trade name: 2PZ-CN), 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine (trade name: 2MZA-PW), and 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct (trade name: 2MAOK-PW) (all manufactured by Shikoku Chemical Industry Co., Ltd.).Further, examples of triarylphosphine-based curing accelerators include the compounds described in JP-A-2004-43405, paragraph 0052. Examples of phosphorus-based curing accelerators in which triphenylborane is added to triarylphosphine include the compounds described in JP-A-2014-5382, paragraph 0024. The content of the curing accelerator is preferably from 0.0002 to 3 mass %, more preferably from 0.002 to 2 mass %, and even more preferably from 0.02 to 1 mass %, based on the total mass of the composition. The content of the curing accelerator is preferably from 0.0002 to 3 mass %, more preferably from 0.002 to 2 mass %, and even more preferably from 0.02 to 1 mass %, based on the total solid content of the composition.
[0231] [Polymerization initiator] The composition may contain a polymerization initiator. The polymerization initiator is not particularly limited, and a known polymerization initiator can be used. Examples of the polymerization initiator include a photopolymerization initiator and a thermal polymerization initiator, and a photopolymerization initiator is preferable. In addition, the polymerization initiator is preferably a so-called radical polymerization initiator. When the composition contains a polymerization initiator, the content thereof is preferably from 0.5 to 15 mass %, more preferably from 1.0 to 10 mass %, and further preferably from 1.5 to 8.0 mass %, based on the total mass of the composition. When the composition contains a polymerization initiator, the content thereof is preferably from 0.5 to 15 mass %, more preferably from 1.0 to 10 mass %, and further preferably from 1.5 to 8.0 mass %, based on the total solid content of the composition.
[0232] <Thermal polymerization initiator> Examples of the thermal polymerization initiator include azo compounds such as 2,2'-azobisisobutyronitrile (AIBN), 3-carboxypropionitrile, azobismalenonitrile, and dimethyl-(2,2')-azobis(2-methylpropionate) [V-601], and organic peroxides such as benzoyl peroxide, lauroyl peroxide, and potassium persulfate. Specific examples of the polymerization initiator include those described on pages 65 to 148 of "Ultraviolet Curing System" by Kiyomi Kato (published by Sogo Gijutsu Center Co., Ltd. in 1989).
[0233] <Photopolymerization initiator> The photopolymerization initiator is not particularly limited as long as it can initiate polymerization of the polymerizable compound, and a known photopolymerization initiator can be used. For example, the photopolymerization initiator is preferably a photopolymerization initiator having photosensitivity to the ultraviolet region to the visible light region. In addition, it may be an activator that generates an active radical by reacting with a photoexcited sensitizer, or an initiator that initiates cationic polymerization according to the type of polymerizable compound. The photopolymerization initiator preferably contains at least one compound having a molar absorption coefficient of at least 50 within a range of 300 to 800 nm (more preferably 330 to 500 nm).
[0234] Examples of the photopolymerization initiator include halogenated hydrocarbon derivatives (e.g., compounds containing a triazine skeleton, compounds containing an oxadiazole skeleton, etc.), acylphosphine compounds such as acylphosphine oxides, hexaarylbiimidazoles, oxime compounds such as oxime derivatives, organic peroxides, thio compounds, ketone compounds, aromatic onium salts, aminoacetophenone compounds, and hydroxyacetophenones. Specific examples of photopolymerization initiators can be found in, for example, paragraphs
[0265] to
[0268] of JP-A-2013-29760, the contents of which are incorporated herein by reference.
[0235] More specifically, for example, the aminoacetophenone-based initiators described in JP-A-10-291969 and the acylphosphine-based initiators described in Japanese Patent No. 4225898 can also be used as the photopolymerization initiator. As the hydroxyacetophenone compound, for example, Omnirad-184, Omnirad-1173, Omnirad-500, Omnirad-2959, and Omnirad-127 (trade names, all manufactured by IGM Resins BV) can be used. As the aminoacetophenone compound, for example, commercially available products Omnirad-907, Omnirad-369, and Omnirad-379EG (trade names, all manufactured by IGM Resins BV) can be used. As the aminoacetophenone compound, compounds described in JP-A-2009-191179, which have an absorption wavelength matching a long-wavelength light source such as a wavelength of 365 nm or 405 nm, can also be used. As the acylphosphine compound, commercially available products Omnirad-819 and Omnirad-TPO (trade names, both manufactured by IGM Resins BV) can be used.
[0236] As the photopolymerization initiator, an oxime ester-based polymerization initiator (oxime compound) is more preferable. In particular, an oxime compound is preferable because it has high sensitivity and high polymerization efficiency, and it is easy to design the content of the coloring material in the composition to be high. Specific examples of the oxime compound that can be used include the compounds described in JP-A-2001-233842, JP-A-2000-80068, and JP-A-2006-342166. Examples of the oxime compound include 3-benzoyloxyiminobutan-2-one, 3-acetoxyiminobutan-2-one, 3-propionyloxyiminobutan-2-one, 2-acetoxyiminopentan-3-one, 2-acetoxyimino-1-phenylpropan-1-one, 2-benzoyloxyimino-1-phenylpropan-1-one, 3-(4-toluenesulfonyloxy)iminobutan-2-one, and 2-ethoxycarbonyloxyimino-1-phenylpropan-1-one. Further examples include compounds described in J.C.S. Perkin II (1979) pp.1653-1660, J.C.S. Perkin II (1979) pp.156-162, Journal of Photopolymer Science and Technology (1995) pp.202-232, JP-A No. 2000-66385, JP-A No. 2000-80068, JP-T No. 2004-534797, and JP-A No. 2006-342166. Commercially available products include IRGACURE-OXE01 (manufactured by BASF), IRGACURE-OXE02 (manufactured by BASF), IRGACURE-OXE03 (manufactured by BASF), and IRGACURE-OXE04 (manufactured by BASF). In addition, TR-PBG-304 (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.), Adeka Arcles NCI-831, Adeka Arcles NCI-930 (manufactured by ADEKA), and N-1919 (carbazole oxime ester skeleton-containing photoinitiator (manufactured by ADEKA)) can also be used.
[0237] In addition, as oxime compounds other than those described above, the compound described in JP-T-2009-519904 A in which an oxime is linked to the N-position of the carbazole; the compound described in U.S. Pat. No. 7,626,957 A in which a heterosubstituent is introduced at the benzophenone moiety; the compounds described in JP-A-2010-15025 A and U.S. Patent Publication No. 2009-292039 in which a nitro group is introduced at the dye moiety; the ketoxime compounds described in WO-A-2009-131189; and the compound described in U.S. Pat. No. 7,556,910 in which a triazine skeleton and an oxime skeleton are contained in the same molecule; and the compound described in JP-A-2009-221114 A in which an absorption maximum is at 405 nm and which has good sensitivity to a g-line light source; etc. may be used. For example, see paragraphs 0274 to 0275 of JP 2013-29760 A, the contents of which are incorporated herein by reference. Specifically, the oxime compound is preferably a compound represented by the following formula (OX-1): The oxime compound may be an oxime compound in which the NO bond is an (E) form, an oxime compound in which the NO bond is an (Z) form, or a mixture of the (E) form and the (Z) form.
[0238] [ka]
[0239] In formula (OX-1), R and B each independently represent a monovalent substituent, A represents a divalent organic group, and Ar represents an aryl group. In formula (OX-1), the monovalent substituent represented by R is preferably a monovalent nonmetallic atomic group. Examples of the monovalent nonmetallic atomic group include an alkyl group, an aryl group, an acyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, a heterocyclic group, an alkylthiocarbonyl group, and an arylthiocarbonyl group. These groups may have one or more substituents. The aforementioned substituents may be further substituted with other substituents. Examples of the substituent include a halogen atom, an aryloxy group, an alkoxycarbonyl group, an aryloxycarbonyl group, an acyloxy group, an acyl group, an alkyl group, and an aryl group. In formula (OX-1), the monovalent substituent represented by B is preferably an aryl group, a heterocyclic group, an arylcarbonyl group, or a heterocyclic carbonyl group, and more preferably an aryl group or a heterocyclic group. These groups may have one or more substituents. Examples of the substituent include the above-mentioned substituents. In formula (OX-1), the divalent organic group represented by A is preferably an alkylene group, a cycloalkylene group, or an alkynylene group having 1 to 12 carbon atoms. These groups may have one or more substituents. Examples of the substituents include the above-mentioned substituents.
[0240] As the photopolymerization initiator, an oxime compound containing a fluorine atom can also be used. Specific examples of the oxime compound containing a fluorine atom include the compounds described in JP-A-2010-262028; compounds 24, 36 to 40 described in JP-T-2014-500852; and compound (C-3) described in JP-A-2013-164471. The contents of these compounds are incorporated herein by reference.
[0241] As the photopolymerization initiator, compounds represented by the following general formulas (1) to (4) can also be used.
[0242] [ka]
[0243] [ka]
[0244] In formula (1), R 1 and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms, an alicyclic hydrocarbon group having 4 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an arylalkyl group having 7 to 30 carbon atoms; R 1 and R 2 When R is a phenyl group, the phenyl groups may be bonded to each other to form a fluorene group, 3 and R 4 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 4 to 20 carbon atoms, and X represents a direct bond or a carbonyl group.
[0245] In formula (2), R 1 , R 2 , R 3 , and R 4 is R in formula (1). 1 , R 2 , R 3 , and R 4 is synonymous with R 5 -R 6, -OR 6 , -SR 6 , -COR 6 , -CONR 6 R 6 , -NR 6 COR 6 , -OCOR 6 , -COOR 6 , -SCOR 6 , -OCSR 6 , -COSR 6 , -CSOR 6 , -CN, a halogen atom, or a hydroxyl group; R 6 represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 4 to 20 carbon atoms; X represents a direct bond or a carbonyl group; and a represents an integer of 0 to 4.
[0246] In formula (3), R 1 represents an alkyl group having 1 to 20 carbon atoms, an alicyclic hydrocarbon group having 4 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an arylalkyl group having 7 to 30 carbon atoms; R 3 and R 4 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 4 to 20 carbon atoms, and X represents a direct bond or a carbonyl group.
[0247] In formula (4), R 1 , R 3 , and R 4 is R in Eq. (3). 1 , R 3 , and R 4 is synonymous with R 5 -R 6 , -OR 6 , -SR 6 , -COR 6 , -CONR 6 R 6 , -NR 6 COR 6 , -OCOR 6 , -COOR 6 , -SCOR 6 , -OCSR6 , -COSR 6 , -CSOR 6 , -CN, a halogen atom, or a hydroxyl group; R 6 represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 4 to 20 carbon atoms; X represents a direct bond or a carbonyl group; and a represents an integer of 0 to 4.
[0248] In the above formulas (1) and (2), R 1 and R 2 is preferably a methyl group, an ethyl group, an n-propyl group, an i-propyl group, a cyclohexyl group, or a phenyl group. 3 R is preferably a methyl group, an ethyl group, a phenyl group, a tolyl group, or a xylyl group. 4 R is preferably an alkyl group having 1 to 6 carbon atoms or a phenyl group. 5 is preferably a methyl group, an ethyl group, a phenyl group, a tolyl group, or a naphthyl group. X is preferably a direct bond. In addition, in the above formulas (3) and (4), R 1 is preferably a methyl group, an ethyl group, an n-propyl group, an i-propyl group, a cyclohexyl group, or a phenyl group. 3 R is preferably a methyl group, an ethyl group, a phenyl group, a tolyl group, or a xylyl group. 4 is preferably an alkyl group having 1 to 6 carbon atoms or a phenyl group. 5 is preferably a methyl group, an ethyl group, a phenyl group, a tolyl group, or a naphthyl group. X is preferably a direct bond. Specific examples of the compounds represented by formula (1) and formula (2) include the compounds described in paragraphs 0076 to 0079 of JP2014-137466A, the contents of which are incorporated herein by reference.
[0249] Specific examples of oxime compounds that can be preferably used in the above composition are shown below. Among the oxime compounds shown below, the oxime compound represented by the general formula (C-13) is more preferred. In addition, as the oxime compound, compounds described in Table 1 of International Publication No. 2015-036910 can also be used, the contents of which are incorporated herein by reference.
[0250] [ka]
[0251] [ka]
[0252] The oxime compound preferably has a maximum absorption wavelength in the wavelength region of 350 to 500 nm, more preferably has a maximum absorption wavelength in the wavelength region of 360 to 480 nm, and further preferably has high absorbance at wavelengths of 365 nm and 405 nm. The molar absorption coefficient of the oxime compound at 365 nm or 405 nm is preferably from 1,000 to 300,000, more preferably from 2,000 to 300,000, and even more preferably from 5,000 to 200,000, from the viewpoint of sensitivity. The molar absorption coefficient of a compound can be measured by a known method, but it is preferable to measure it, for example, using an ultraviolet-visible spectrophotometer (Varian Cary-5 spectrophotometer) using ethyl acetate at a concentration of 0.01 g / L. Two or more kinds of photopolymerization initiators may be used in combination, if necessary.
[0253] In addition, as the photopolymerization initiator, the compounds described in paragraph 0052 of JP-A-2008-260927, paragraphs 0033 to 0037 of JP-A-2010-97210, and paragraph 0044 of JP-A-2015-68893 can also be used, the contents of which are incorporated herein by reference.
[0254] [Polymerization inhibitor] The composition may contain a polymerization inhibitor. The polymerization inhibitor is not particularly limited, and known polymerization inhibitors can be used. Examples of the polymerization inhibitor include phenol-based polymerization inhibitors (e.g., p-methoxyphenol, 2,5-di-tert-butyl-4-methylphenol, 2,6-di-tert-butyl-4-methylphenol, 4,4'-thiobis(3-methyl-6-t-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), 4-methoxynaphthol, etc.); hydroquinone-based polymerization inhibitors (e.g., hydroquinone, 2,6-di-tert-butylhydroquinone, etc.); quinone, etc.); quinone-based polymerization inhibitors (e.g., benzoquinone, etc.); free radical-based polymerization inhibitors (e.g., 2,2,6,6-tetramethylpiperidine 1-oxyl free radical, 4-hydroxy-2,2,6,6-tetramethylpiperidine 1-oxyl free radical, etc.); nitrobenzene-based polymerization inhibitors (e.g., nitrobenzene, 4-nitrotoluene, etc.); and phenothiazine-based polymerization inhibitors (e.g., phenothiazine, 2-methoxyphenothiazine, etc.); and the like. Among these, phenol-based polymerization inhibitors or free radical-based polymerization inhibitors are preferred.
[0255] The effect of the polymerization inhibitor is remarkable when it is used together with a resin containing a curable group. The content of the polymerization inhibitor in the composition is not particularly limited, but is preferably from 0.0001 to 0.5 mass %, more preferably from 0.0001 to 0.2 mass %, and even more preferably from 0.0001 to 0.05 mass %, based on the total mass of the composition. The content of the polymerization inhibitor is preferably from 0.0001 to 0.5 mass %, more preferably from 0.0001 to 0.2 mass %, and even more preferably from 0.0001 to 0.05 mass %, based on the total solid content of the composition. In addition, the ratio of the content of the polymerization inhibitor to the content of the polymerizable compound (particularly, a compound containing a group having an ethylenically unsaturated bond) in the composition (content of the polymerization inhibitor / content of the polymerizable compound (mass ratio)) is preferably more than 0.0005, more preferably 0.0006 to 0.02, and even more preferably 0.0006 to 0.005.
[0256] [Surfactant] The composition may contain a surfactant. The surfactant contributes to improving the coatability of the composition. When the composition contains a surfactant, the content of the surfactant is preferably from 0.001 to 2.0 mass %, more preferably from 0.005 to 0.5 mass %, and even more preferably from 0.01 to 0.1 mass %, relative to the total mass of the composition. The content of the surfactant is preferably from 0.001 to 2.0 mass %, more preferably from 0.005 to 0.5 mass %, and even more preferably from 0.01 to 0.1 mass %, based on the total solid content of the composition.
[0257] Examples of the surfactant include a fluorine-based surfactant, a nonionic surfactant, a cationic surfactant, an anionic surfactant, and a silicone-based surfactant.
[0258] For example, if the composition contains a fluorine-based surfactant, the liquid properties (particularly, fluidity) of the composition are improved. That is, when a film is formed using a composition containing a fluorine-based surfactant, the interfacial tension between the surface to be coated and the coating liquid is reduced, improving the wettability to the surface to be coated, and improving the coatability to the surface to be coated. Therefore, even if a thin film of about several μm is formed with a small amount of liquid, it is effective in that a film of uniform thickness with little thickness unevenness can be more suitably formed.
[0259] The fluorine content in the fluorosurfactant is preferably 3 to 40 mass%, more preferably 5 to 30 mass%, and even more preferably 7 to 25 mass%. A fluorosurfactant having a fluorine content within this range is effective in terms of uniformity of the coating film thickness and / or liquid saving properties, and also has good solubility in the composition.
[0260] Examples of fluorine-based surfactants include Megafac F171, F172, F173, F176, F177, F141, F142, F143, F144, R30, F437, F475, F479, F482, F554, and F780 (all manufactured by DIC Corporation); Fluorad FC430, FC431, and FC171 (all manufactured by DIC Corporation). , manufactured by Sumitomo 3M Limited); Surflon S-382, Surflon SC-101, Surflon SC-103, Surflon SC-104, Surflon SC-105, Surflon SC1068, Surflon SC-381, Surflon SC-383, Surflon S393, and Surflon KH-40 (all manufactured by AGC); and PF636, PF656, PF6320, PF6520, and PF7002 (manufactured by OMNOVA). A block polymer can also be used as the fluorine-based surfactant, and specific examples include the compounds described in JP-A-2011-89090. An example of the silicone surfactant is KF6007 (manufactured by Shin-Etsu Chemical Co., Ltd.).
[0261] 〔solvent〕 The composition may contain a solvent. The solvent includes water and organic solvents, with organic solvents being preferred. From the viewpoint of coatability, the boiling point of the solvent is preferably from 100 to 400° C., more preferably from 150 to 300° C., and further preferably from 170 to 250° C. In this specification, the boiling point means the normal boiling point, unless otherwise specified.
[0262] Examples of the organic solvent include acetone, methyl ethyl ketone, cyclohexane, ethyl acetate, ethylene dichloride, tetrahydrofuran, toluene, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, acetylacetone, cyclohexanone, cyclopentanone, diacetone alcohol, ethylene glycol monomethyl ether acetate, ethylene glycol ethyl ether acetate, ethylene glycol monoisopropyl ether, and ethylene glycol monobutyl ether acetate. acetate, 1,4-butanediol diacetate, 3-methoxypropanol, methoxymethoxyethanol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, 3-methoxypropyl acetate, N,N-dimethylformamide, dimethylsulfoxide, γ-butyrolactone, ethyl acetate, butyl acetate, methyl lactate, N-methyl-2-pyrrolidone, and ethyl lactate, but are not limited thereto.
[0263] When the composition contains a solvent, the content thereof is preferably 1 to 60 mass %, more preferably 1 to 40 mass %, and even more preferably 1 to 25 mass %, relative to the total mass of the composition, in terms of better effects of the present invention. It is also preferable that the composition is substantially free of a solvent. The term "substantially free of a solvent" means that the content of the solvent is less than 1% by mass relative to the total mass of the composition, and for example, is preferably 0% by mass or more and less than 1% by mass, more preferably 0 to 0.5% by mass, and even more preferably 0 to 0.1% by mass. The solid content concentration of the composition is preferably from 20 to 100% by mass, more preferably from 40 to 100% by mass, and further preferably from 75 to 100% by mass.
[0264] [Other optional ingredients] The composition may further contain other optional components other than the above-mentioned components. For example, magnetic particles other than the above-mentioned magnetic particles, sensitizers, co-sensitizers, crosslinking agents (curing agents), curing accelerators, heat curing accelerators, plasticizers, diluents, oil sensitizers, and rubber components can be mentioned, and further, known additives such as adhesion promoters to the substrate surface and other auxiliaries (for example, defoamers, flame retardants, leveling agents, peeling accelerators, antioxidants, fragrances, surface tension adjusters, and chain transfer agents) may be added as necessary.
[0265] [Physical Properties of Composition] When the shear rate is 0.1 (1 / s), the viscosity of the composition at 23° C. is preferably 1 to 1,000,000 Pa·s, more preferably 10 to 50,000 Pa·s, and even more preferably 50 to 10,000 Pa·s, in view of superior sedimentation stability of the magnetic particles. When the shear rate is 1000 (1 / s), the viscosity of the composition at 23°C is preferably 100 Pa s or less, more preferably 50 Pa s or less, and even more preferably 10 Pa s or less, in terms of superior sedimentation stability of the magnetic particles. When the shear rate is 1000 (1 / s), the lower limit is preferably 0.001 Pa s or more. Here, the viscosity of the composition at 23°C can be obtained by measuring at 23°C using MCR-102 (manufactured by Anton Paar) while increasing the speed from 0.1 / s to 1000 / s.
[0266] [Method of producing the composition] The composition can be prepared by mixing the above-mentioned components by a known mixing method (for example, a mixing method using a stirrer, a homogenizer, a high-pressure emulsifier, a wet grinder, or a wet disperser). When preparing the composition of the present invention, each component may be mixed at once, or each component may be dissolved or dispersed in a solvent and then mixed successively. The order of addition and working conditions when mixing are not particularly limited. For example, when using multiple types of other resins, they may be mixed at once, or each type may be mixed in multiple batches.
[0267] [Magnetic particle-containing film] The magnetic particle-containing film of the present invention is formed using the above-mentioned composition of the present invention. The thickness of the magnetic particle-containing film is preferably from 1 to 10,000 μm, more preferably from 10 to 1,000 μm, and even more preferably from 15 to 800 μm, in terms of superior magnetic permeability. The magnetic particle-containing film is suitably used as an electronic component such as an antenna or inductor mounted on an electronic communication device or the like.
[0268] [Method for producing a magnetic particle-containing film] The magnetic particle-containing film of the present invention can be obtained, for example, by curing the above-mentioned composition. The method for producing the magnetic particle-containing film is not particularly limited, but preferably includes the following steps. ·Composition layer formation process ·Curing process
[0269] <Composition layer formation process> In the composition layer forming step, a composition layer (composition layer) is formed by applying the composition onto a substrate (support) etc. As the substrate, for example, a wiring board having an antenna part or an inductor part etc. can be used.
[0270] The composition can be applied to a substrate by a variety of coating methods, including slit coating, inkjet, spin coating, casting, roll coating, and screen printing. The thickness of the composition layer is preferably 1 to 10,000 μm, more preferably 10 to 1,000 μm, and even more preferably 15 to 800 μm. The composition layer applied to the substrate may be heated (prebaked), and the prebaking can be performed, for example, on a hot plate or in an oven at a temperature of 50 to 140° C. for 10 to 1,800 seconds. Prebaking is preferably performed when the composition contains a solvent.
[0271] <Curing process> The curing step is not particularly limited as long as it can cure the composition layer, and examples thereof include a heat treatment for heating the composition layer and an exposure treatment for irradiating the composition layer with actinic rays or radiation.
[0272] When the heat treatment is carried out, the heat treatment can be carried out continuously or batchwise using a heating means such as a hot plate, a convection oven (hot air circulation type dryer), or a high-frequency heater. The heating temperature in the heat treatment is preferably 120 to 260° C., more preferably 150 to 240° C. The heating time is not particularly limited, but is preferably 10 to 1800 seconds. The pre-baking in the composition layer forming step may also serve as the heat treatment in the curing step.
[0273] When exposure treatment is performed, the method of irradiating with actinic rays or radiation is not particularly limited, but it is preferable to irradiate through a photomask having openings in a pattern. The exposure is preferably carried out by irradiation with radiation. The radiation that can be used for exposure is preferably ultraviolet light such as g-rays, h-rays, or i-rays, and the light source is preferably a high-pressure mercury lamp. The irradiation intensity is 5 to 1500 mJ / cm. 2 is preferable, and 10 to 1000 mJ / cm 2 is more preferred. When the composition contains a thermal polymerization initiator, the composition layer may be heated in the exposure treatment. The heating temperature is not particularly limited, but is preferably 80 to 250° C. The heating time is not particularly limited, but is preferably 30 to 300 seconds. In addition, when the composition layer is heated in the exposure treatment, this may also serve as a post-heating step described later. In other words, when the composition layer is heated in the exposure treatment, the method for producing a magnetic particle-containing film does not need to include a post-heating step.
[0274] <Developing process> When an exposure treatment is performed in the curing step, a development step may be further included. The development step is a step of developing the composition layer after exposure to form a magnetic particle-containing film. By this step, the composition layer in the portion not irradiated with light in the exposure treatment is dissolved, and only the photocured portion remains, thereby obtaining a patterned magnetic particle-containing film. The type of developer used in the development step is not particularly limited, but an alkaline developer that does not damage circuits and the like is preferable. The development temperature is, for example, 20 to 30°C. The developing time is, for example, 20 to 90 seconds. In recent years, in order to remove residues more effectively, the developing time may be 120 to 180 seconds. Furthermore, in order to further improve the removability of residues, the process of shaking off the developing solution every 60 seconds and supplying new developing solution may be repeated several times.
[0275] The alkaline developer is preferably an alkaline aqueous solution prepared by dissolving an alkaline compound in water to a concentration of 0.001 to 10% by mass (preferably 0.01 to 5% by mass). Examples of alkaline compounds include sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, aqueous ammonia, ethylamine, diethylamine, dimethylethanolamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxyl, benzyltrimethylammonium hydroxide, choline, pyrrole, piperidine, and 1,8-diazabicyclo[5.4.0]-7-undecene (among these, organic alkalis are preferred). When an alkaline developer is used, a washing treatment with water is generally carried out after development.
[0276] <Post bake> When an exposure treatment is performed in the curing step, it is preferable to perform a heat treatment (post-baking) after the curing step. Post-baking is a heat treatment for completing the curing. When a development step is performed, it is preferable to perform post-baking after the development step. The heating temperature is preferably 240° C. or less, more preferably 220° C. or less. There is no particular lower limit, but in consideration of efficient and effective processing, it is preferably 50° C. or more, more preferably 100° C. or more. In addition, the heating time is not particularly limited, but is preferably 10 to 1800 seconds. The post-baking can be carried out continuously or batchwise using a heating means such as a hot plate, a convection oven (hot air circulation dryer), or a high-frequency heater.
[0277] The post-baking is preferably carried out in an atmosphere with a low oxygen concentration. The oxygen concentration is preferably 19% by volume or less, more preferably 15% by volume or less, even more preferably 10% by volume or less, particularly preferably 7% by volume or less, and most preferably 3% by volume or less. There is no particular lower limit, but a concentration of 10 ppm by volume or more is practical.
[0278] Moreover, instead of the post-baking by heating, the curing may be completed by UV (ultraviolet) irradiation. In this case, the composition preferably further contains a UV curing agent. The UV curing agent is preferably a UV curing agent that can be cured at a wavelength shorter than 365 nm, which is the exposure wavelength of a polymerization initiator added for a lithography process using normal i-line exposure. An example of the UV curing agent is Chiba Ilgacure 2959 (trade name). In the case of performing UV irradiation, it is preferable that the composition layer is a material that cures at a wavelength of 340 nm or less. There is no particular lower limit of the wavelength, but it is generally 220 nm or more. The exposure dose of UV irradiation is preferably 100 to 5000 mJ, more preferably 300 to 4000 mJ, and even more preferably 800 to 3500 mJ. It is preferable to perform this UV curing process after the exposure treatment in order to perform low-temperature curing more effectively. It is preferable to use an ozone-free mercury lamp as the exposure light source.
[0279] [Electronic components] The electronic component of the present invention includes the above-mentioned magnetic particle-containing film of the present invention. That is, the electronic component of the present invention may include the above-mentioned magnetic particle-containing film as a part of the component. Examples of the electronic component include an inductor and an antenna. The electronic component may have a known structure. EXAMPLES
[0280] The present invention will be described in more detail below based on examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the following examples. In the following description, unless otherwise specified, "%" means "% by mass" and "parts" means "parts by mass".
[0281] [Various components used in the preparation of the composition] In preparing the composition, the components shown in Table 1 were prepared. The outline of each component shown in Table 1 is shown below.
[0282] [Magnetic particles] P-1: 80%Ni-4Mo PF-5F (Epson Atomics), particle size (average primary particle size): 4 μm, Ni content: 80%, aspect ratio: 1-2 P-2: 80%Ni-4Mo PF-15F (Epson Atomics), particle size: 8μm, Ni content: 80%, aspect ratio: 1-2 P-3: 80%Ni-4Mo WA13 (Epson Atomics), particle size: 12.5μm, Ni content: 80%, aspect ratio: 1-2 P-4: Particles produced by mechanochemical treatment of 80%Ni-4Mo WA13, particle size: 12.5μm, Ni content: 80%, aspect ratio: 3~4 P-5: Particles produced by mechanochemical treatment of 80%Ni-4Mo WA13, particle size: 12.5μm, Ni content: 80%, aspect ratio: 5~6 P-6: Particles produced by mechanochemical treatment of 80%Ni-4Mo WA13, particle size: 12.5μm, Ni content: 80%, aspect ratio: 7 or more but less than 8 P-7; KUAMET-CT5-25um (Epson Atomics), particle size: 15μm, Co content: 81%, aspect ratio: 1-2 P-8: KUAMET-CT5-38um (Epson Atomics), particle size: 20μm, Co content: 81%, aspect ratio: 1-2 P-9; KUAMET-CT5-53um (Epson Atomics), particle size: 25μm, Co content: 81%, aspect ratio: 1-2 P-10: Particles produced by water atomization containing Co: 70%, Fe: 15%, Si: 9%, Cr: 4%, B: 2%. Particle size: 15 μm, Co content: 70%, aspect ratio: 1-2 P-11: Particles produced by water atomization containing Co: 60%, Fe: 25%, Si: 9%, Cr: 4%, B: 2%. Particle size: 15 μm, Co content: 60%, aspect ratio: 1-2 P-12: Particles produced by water atomization containing Co: 50%, Fe: 35%, Si: 9%, Cr: 4%, B: 2%. Particle size: 15 μm, Co content: 50%, aspect ratio: 1-2 P-13: Particles produced by water atomization containing Co: 90%, Si: 4%, Cr: 4%, B: 2%. Particle size: 15 μm, Co content: 90%, aspect ratio: 1-2 P-14: Particles produced by water atomization containing Ni: 80%, Fe: 19%, Mo: 1%. Particle size: 12.5 μm, Ni content: 80%, aspect ratio: 1-2 P-15: Particles produced by water atomization containing Ni: 80%, Fe: 10%, Mo: 10%. Particle size: 12.5 μm, Ni content: 80%, aspect ratio: 1-2 P-16: Particles produced by water atomization containing Ni: 80%, Mo: 15%, Fe: 5%. Particle size: 12.5 μm, Ni content: 80%, aspect ratio: 1-2 P-17: Particles produced by water atomization containing Co: 40%, Fe: 45%, Si: 9%, Cr: 4%, B: 2%. Particle size: 15 μm, Co content: 40%, aspect ratio: 1-2 P-18: Particles produced by mechanochemical treatment of 80%Ni-4Mo WA13, particle size: 12.5μm, Ni content: 80%, aspect ratio: 8~9 P-19: Particles produced by water atomization containing Ni: 40%, Fe: 55%, Mo: 5%. Particle size: 12.5 μm, Ni content: 40%, aspect ratio: 1-2 P-20; AW2-08 PF-3F (Epson Atomics), particle size: 3 μm, Ni, Co content: 0%, aspect ratio: 1-2 All of the magnetic particles were composed substantially of metal atoms only. The particle size (average primary particle size) of the magnetic particles was measured by the method described in the specification. Among the above magnetic particles, P-1 to P-16 also correspond to the "magnetic particles X having an aspect ratio of less than 8" already described in the upper part.
[0283] [Rheology control agents or other resins] D-1: Product name "BYK-P105" (manufactured by BYK), low molecular weight unsaturated carboxylic acid polymer, acid value 365mgKOH / g, solid content 100% D-2: Product name: "ANTI-TERRA-204" (manufactured by BYK), solution of polycarboxylate of polyaminoamide, amine value 37mgKOH / g, acid value 41mgKOH / g, solid content 52% D-3: Product name: "Taren VA-705B" (Kyoeisha Chemical Co., Ltd.), higher fatty acid amide, solid content 100% D-4: Product name: "FLOWNON RCM-230AF" (Kyoeisha Chemical Co., Ltd.), higher fatty acid amide, solid content 10% D-5: The following compound (weight average molecular weight 10,000, amine value 50 mgKOH / g, acid value 50 mgKOH / g, solid content concentration 30%) D-6: The following compound (weight average molecular weight 25,000, acid value 100 mgKOH / g), solid content concentration 30% D-7: The following compound (weight average molecular weight 10,000, acid value 40 mgKOH / g), solid content concentration 30% D-1 and D-3 are the rheology control agents themselves, and D-2 and D-4 are solutions containing the rheology control agents (solid content). D-5 to D-7 are solutions containing other resins (solid content) that do not fall under the category of rheology control agents. In the following compounds shown for D-5 to D-7, the numbers attached to each repeating unit indicate the mass ratio.
[0284] [ka]
[0285] [ka]
[0286] [ka]
[0287] [Polymerizable compound] M-1: Celloxide 2021P (manufactured by Daicel Chemical Industries), 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate M-2: Denacol EX-411 (Nagase Chemtex), pentaerythritol polyglycidyl ether M-3: KAYARAD RP-1040 (manufactured by Nippon Kayaku), the following compound M-4: A-TMMT (manufactured by Toagosei), pentaerythritol tetraacrylate
[0288] [ka]
[0289] [Additives (curing accelerators or polymerization initiators)] A-1: Triphenylphosphine (Tokyo Chemical Industry Co., Ltd.), hardening accelerator A-2: Hishicoline PX-4MP (manufactured by Nippon Chemical Industry Co., Ltd.), methyl tributyl phosphonium dimethyl phosphate, hardening accelerator A-3: IRGACURE-OXE03 (BASF), photopolymerization initiator A-4: Omnirad-369 (IGM Resins BV), photopolymerization initiator
[0290] [Surfactant] Sur-1: MEGAFAC F-781F (DIC), a fluorosurfactant Sur-2; KF6001 (Shin-Etsu Chemical Co., Ltd.), silicone surfactant
[0291] 〔solvent〕 · S-1; Propylene glycol monomethyl ether acetate (PGMEA) S-2: 1,4-butanediol diacetate (1,4-BDDA)
[0292] [Preparation of compositions of examples and comparative examples] The components other than the solvent shown in Table 1 were mixed in the composition ratio (mass basis) shown in Table 1 and placed in a sealed container made of PTFE (polytetrafluoroethylene). Next, a solvent was added to the composition ratio (mass basis) shown in Table 1, and the container was sealed. The mixture was dispersed at 50 G for 2 hours using a RAM (low frequency resonant acoustic mixer) manufactured by Resodyn, to prepare the compositions of each of the examples and comparative examples.
[0293] [Evaluation test] [Sedimentation stability] 3 mL of the composition obtained as described above was placed in a glass sample bottle (cylindrical, diameter 23 mm×height 35 mm), sealed, and then allowed to stand at 25° C. for 30 days. Thereafter, the composition in the sample bottle was visually observed, and the distance d1 from the gas-liquid interface to the interface between the transparent region and the opaque region, and the distance d2 from the gas-liquid interface to the bottom of the sample bottle were measured. Subsequently, the same sample bottle was stirred at 3300 r / min for 30 seconds using a shaker Se-08 manufactured by Taitec Co., Ltd., and then allowed to stand at 25°C for 12 hours. Thereafter, the composition was visually observed, and the distance d´1 from the gas-liquid interface to the interface between the transparent region and the opaque region, and the distance d´2 from the gas-liquid interface to the bottom of the sample bottle were measured. The sedimentation stability was evaluated based on the following criteria using the distance d1 and the distance d2, and the distance d´1 and the distance d´2. If the following criteria were "2" or more, it was judged that the sedimentation stability was excellent. The results are shown in Table 1. 3: 0 ≤ d1 / d2 ≤ 0.1, and 0 ≤ d´1 / d´2 ≤ 0.1 2: 0.1 < d1 / d2 ≤ 0.3, and 0 ≤ d´1 / d´2 ≤ 0.1 1: 0.3 < d1 / d2, or 0.1 ≤ d´1 / d´2
[0294] 〔Magnetic Isotropy of Magnetic Particle-Containing Film〕 Each composition was applied onto a Si wafer (film thickness: 100 μm) using an applicator to form a composition layer such that the film thickness of the magnetic particle-containing film after film formation was 100 μm. Thereafter, when the applied composition was a composition not containing a photoinitiator, the composition layer was heated at 100°C for 10 minutes and then further heated at 230°C for 10 minutes to obtain a magnetic particle-containing film. When the applied composition was a composition containing a photoinitiator, exposure treatment was performed under the condition of 1000 mJ / cm 2 using a proximity exposure machine, and then further heated at 230°C for 10 minutes to obtain a magnetic particle-containing film. Hereinafter, the Si wafer with the magnetic particle-containing film is also simply referred to as a substrate. One obtained substrate was cut into 1 cm × 2.8 cm, and a substrate A cut such that the long axis came in the coating direction of the applicator and a substrate B cut such that the short axis direction came were obtained. Thereafter, using PER-01 (a high-frequency magnetic permeability measuring device manufactured by Keycom Co., Ltd.), the magnetic permeability at 100 MHz was measured, and the specific magnetic permeability μ´A and μ´B of the magnetic particle-containing film on each substrate were obtained, and the value of "μ´A / μ´B" was determined. It should be noted that μ′A is the magnetic permeability measured using substrate A, and μ′B is the magnetic permeability measured using substrate B. The same procedure was repeated another nine times, and ten substrates and magnetic permeability measurements were performed for each composition. The number n (n is an integer from 0 to 10) of substrates for which 0.9<μ´A / μ´B<1.1 was evaluated according to the following criteria. If the following criteria was scored as "2", the magnetic particle-containing film was judged to have excellent magnetic isotropy. The results are shown in Table 1. 2:n≦3 1:3 <n
[0295] [Chemical resistance of magnetic particle-containing film] Each composition was applied onto a Si wafer (film thickness: 100 μm) using an applicator so that the thickness of the magnetic particle-containing film after film formation was 100 μm, forming a composition layer. If the applied composition did not contain a photopolymerization initiator, the composition layer was heated at 100° C. for 10 minutes, and then further heated at 230° C. for 10 minutes to obtain a magnetic particle-containing film. If the applied composition contained a photopolymerization initiator, the composition was exposed to 1000 mJ / cm 2 using a proximity exposure machine. 2 The film was then heated at 230° C. for 10 minutes to obtain a magnetic particle-containing film. Hereinafter, the Si wafer with the magnetic particle-containing film will also be simply referred to as the substrate. The obtained magnetic particle-containing film was cut together with the substrate into a piece of 1 cm x 2.8 cm, and the magnetic permeability was then measured at 100 MHz using PER-01 to obtain the relative magnetic permeability μ'X of the magnetic particle-containing film on the substrate. Thereafter, the same substrate was immersed in a 10% aqueous hydrochloric acid solution at 25° C. for 30 minutes, and the relative permeability μ′Y of the magnetic particle-containing film was similarly measured. The rate of change Δμ' before and after immersion in a 10% hydrochloric acid aqueous solution was calculated using the following formula and evaluated according to the following criteria. If the result of the following criteria was "2" or more, the magnetic particle-containing film was judged to have excellent chemical resistance. The results are shown in Table 1. Formula: Δμ´(%)=|μ´Y-μ´X| / μ´X×100 3:Δμ´<5% 2:5%≦Δμ´<10% 1:10%≦Δμ´
[0296] [result] The following table shows the formulation of each composition and the results of the evaluation tests carried out on each composition. The value shown in the "Amount" column in the table indicates the mass ratio (mass %) of that component to the total mass of the composition.
[0297] [Table 1]
[0298] [Table 2]
[0299] As shown in Table 1, it was confirmed that the composition of the present invention has good stability over time, and that a magnetic particle-containing film with excellent magnetic isotropy can be formed by using the composition of the present invention. It was also confirmed that the composition has good chemical resistance.
[0300] It was confirmed that when the magnetic particles contain Ni atoms as specific atoms and the particle size of the magnetic particles is 5 μm or more, the effects of the present invention are superior (see comparison of the results of Examples 1 to 3, etc.).
[0301] It was confirmed that when the magnetic particles contain Co atoms as specific atoms and the particle size of the magnetic particles is 20 μm or more, the effects of the present invention are superior (see comparison of the results of Examples 7 to 9, etc.).
[0302] It has been confirmed that in order to obtain a more excellent effect of the present invention, the content of the specific atom is preferably 70 mass% or more, and more preferably 85 mass% or more, of the total mass of the metal atoms (see comparison of the results of Examples 7, and 10 to 13, etc.).
[0303] It was confirmed that the effects of the present invention are better when the magnetic particles contain Ni atoms as specific atoms (see comparison of the results of Examples 3 and 7. As a general trend for the examples, the effects of the present invention are better when the particle size of the magnetic particles is larger. On the other hand, Example 3, which used P-3, a magnetic particle with a smaller particle size containing Ni atoms, achieved a better effect of the present invention than Example 7, which used P-7, a magnetic particle with a larger particle size containing Co atoms).
[0304] It was confirmed that the effects of the present invention were more excellent when the solid content concentration of the composition was 75 mass % or more (see comparison of the results of Examples 25, and 53 to 60, etc.).
[0305] It was confirmed that the effects of the present invention are more excellent when the composition contains an epoxy compound (epoxy curable compound) as a polymerizable compound (see comparison of the results of Examples 37 to 43, etc.).
Claims
1. A composition comprising magnetic particles and a rheology control agent, the content of the magnetic particles having an aspect ratio of less than 8 is 25% by mass or more based on the total mass of the magnetic particles; The magnetic particles contain metal atoms, The metal atom contains one or more specific atoms selected from the group consisting of Ni atoms and Co atoms, A composition, wherein the content of the specific atom is 50 mass% or more based on the total mass of the metal atoms.
2. The composition according to claim 1 , wherein the specific atom is the Ni atom.
3. The composition according to claim 1 or 2, wherein the content of the specific atom is 70 mass% or more based on the total mass of the metal atoms.
4. The composition according to any one of claims 1 to 3, wherein the magnetic particles have a particle size of 5 µm or more.
5. The composition according to any one of claims 1 to 4, wherein the rheology control agent is an organic rheology control agent.
6. The composition according to any one of claims 1 to 5, wherein the rheology control agent is at least one selected from the group consisting of polycarboxylic acids, polycarboxylic anhydrides, and amide waxes.
7. The composition according to any one of claims 1 to 6, further comprising an epoxy curable compound as a polymerizable compound.
8. A magnetic particle-containing film formed using the composition according to any one of claims 1 to 7.
9. An electronic component comprising the magnetic particle-containing film according to claim 8 .
10. 10. The electronic component according to claim 9, which is used as an inductor.
11. The electronic component according to claim 9, which is used as an antenna.
Citation Information
Patent Citations
Magnetic composite and magnetic composite material
JP2004111756A
Method of producing composite magnetic body and composite magnetic body
JP2014029936A
Soft magnetic resin composition and soft magnetic film
JP2016006852A
Near field noise suppression sheet
JP2017208415A
Magnetic paste
JP2020087939A