Coated white paperboard

The coated white paperboard with controlled pigment coating layers and calcium carbonate content addresses cracking issues, providing a strong and crack-resistant coating for packaging applications.

JP2024149809AActive Publication Date: 2024-10-18NIPPON PAPER IND CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024137491
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-10-15
Filing Date
2024-08-19
Publication Date
2024-10-18
Estimated Expiration
2040-10-12

AI Technical Summary

Technical Problem

Coated white paperboard is prone to cracking during bending due to insufficient strength in the pigment coating layer, which affects its suitability for packaging applications.

Method used

The coated white paperboard features two or more pigment coating layers with controlled particle size distribution and specific calcium carbonate content, along with adhesives and optional kaolin, to enhance strength and density, reducing voids and improving adhesion.

Benefits of technology

The solution results in a dense and strong pigment coating layer that resists cracking, making it suitable for packaging boxes, particularly for gift items.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149809000001
    Figure 2024149809000001
Patent Text Reader

Abstract

To provide coated white paperboard bearable against fold-up load and strong against cracking in a pigment coated layer.SOLUTION: Coated white paperboard includes two or more pigment coated layers on a surface of base paper, where each of the pigment coated layers contains ground calcium carbonate as pigment in which a ratio (D75 / D25) of a particle diameter of 75 cumulative wt.% (D75) to a particle diameter of 25 cumulative wt.% (D25) is 3.3 or more and 4.0 or less, and a content ratio of the ground calcium carbonate in a top pigment coated layer coated outermost of all the pigment contained in the top pigment coated layer exceeds 5 wt.% and is 30 wt.% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coated white paperboard. In particular, the present invention relates to a coated white paperboard for use in both offset and gravure printing that is resistant to coating layer cracking. [Background technology]

[0002] Whiteboard is a thick paperboard with a multi-layered base paper structure, usually 2 to 9 layers, and recycled paper pulp is often used due to the increasing demand for environmental initiatives and cost reduction. For example, bleached pulp, deinked pulp, or bleached recycled paper pulp with high whiteness is used for the surface layer, while deinked pulp or non-deinked recycled paper pulp with lower whiteness and low cost is used for the middle and back layers. The ratio of recycled paper pulp is increasing year by year, and in low-grade whiteboard, recycled paper pulp is almost 100%. Under these circumstances, problems with the base paper caused by the increase in the recycled paper ratio include an increase in defects such as dust and black spots, and the occurrence of white unevenness. In order to remove foreign matter such as dust, measures have been taken to strengthen the deinking and dust removal processes, and the problem of dust has been greatly improved due to advances in deinking technology and dust removal equipment, but it is not yet possible to completely remove it. The more intensive the deinking and dust removal processes are, the worse the yield becomes and the more economically disadvantageous it becomes, so currently deinking and dust removal processes are not carried out beyond a certain level.

[0003] Coated whiteboard is a whiteboard with a pigment coating layer formed by coating a multi-layered base paper with a coating liquid mainly composed of pigments and adhesives, and is mainly used for packaging boxes for cosmetics, medicines, soaps, gifts, etc. After printing is applied to the surface of the coated whiteboard using various printing methods to appeal to the enclosed product, it is processed into paper containers by various post-processing. This coated whiteboard is classified into high-grade whiteboard, special whiteboard, and coated whiteboard based on the difference in the base paper composition and the coating layer formation state. High-grade whiteboard is a whiteboard with chemical pulp used in all layers and coated layers on both sides, while special whiteboard is a whiteboard with chemical pulp used in the front and back layers and recycled paper used in the inner layers, and coated layers on both sides or one side. These high-grade whiteboard and special whiteboard are called manilaboard. Coated white board is a white paperboard with a surface layer made of chemical pulp, a back layer and layers further inward made of recycled paper, and a coating layer on one side. Coated white paperboard is often processed into boxes after being printed and punched. When it is folded to be assembled into a box, the surface of the coated white paperboard is subjected to a stretching force. If the strength of the surface layer of the coated white paperboard cannot withstand this force, it will break and tear. This break is called "crease cracks" or "coating layer cracks", and in mild cases the surface layer will crack, but in severe cases large cracks will form including in the base paper. A coating layer crack is not only unsightly in appearance, but it also reduces the strength of the assembled box, which is a fatal defect as a packaging structure. As a countermeasure against such coating layer cracking, a technology related to a coated liner that contains 5% by weight or more of bleached softwood kraft pulp as pulp in the surface layer of the base paper, and a technology for setting the density, print surface roughness, and air permeability of the coated paperboard within specific ranges have been disclosed (see, for example, Patent Documents 1 and 2). However, these conventional technologies have not yet achieved sufficient results, and new technologies for preventing coating layer cracking are needed. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-249762 A [Patent Document 2] JP 2002-105895 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in consideration of the above-mentioned circumstances, and has as its object to provide a coated white paperboard that can withstand the load of folding and is resistant to cracking of the pigment coating layer. [Means for solving the problem]

[0006] As a result of extensive research into solving the above-mentioned problems, the inventors have found that a coated white paperboard having strength sufficient to withstand bending loads can be obtained by having all of the pigment coating layers contain heavy calcium carbonate as a pigment, with the ratio (D75 / D25) of the particle size distribution curve between the 75th cumulative weight % particle size (D75) and the 25th cumulative weight % particle size (D25) being 3.3 or more and 4.0 or less, and by setting the content of said heavy calcium carbonate in the outermost top pigment coating layer to more than 5% and not more than 30% by weight of the total pigment contained in said top pigment coating layer, and have thus completed the present invention.

[0007] Specifically, the present invention relates to the following items. 1. A coated white paperboard having two or more pigment coating layers on the surface of the base paper, each of the pigment coating layers contains ground calcium carbonate as a pigment, the ratio (D75 / D25) of the particle size distribution curve between the 75th cumulative weight % particle size (D75) and the 25th cumulative weight % particle size (D25) being 3.3 or more and 4.0 or less; A coated white paperboard, characterized in that the content of the ground calcium carbonate in the outermost topcoat pigment coating layer is more than 5% by weight and not more than 30% by weight of all pigments contained in the topcoat pigment coating layer. 2. The coated white paperboard described in 1., characterized in that the content of the heavy calcium carbonate in the topcoat pigment coating layer is 18% by weight or more and 23% by weight or less of the total pigment contained in the topcoat pigment coating layer. 3. A coated white paperboard according to 1. or 2., characterized in that the topcoat pigment coating layer contains calcium carbonate including the heavy calcium carbonate, and the content of calcium carbonate in the topcoat pigment coating layer is in the range of 15% by weight or more and 50% by weight or less of the total pigment contained in the topcoat pigment coating layer. 4. The coated white paperboard described in 3., characterized in that the content of calcium carbonate in the topcoat pigment coating layer is in the range of 19% by weight or more and less than 40% by weight of the total pigment contained in the topcoat pigment coating layer. 5. A coated white paperboard according to any one of 1. to 4., characterized in that the undercoat pigment coating layer, which is closer to the base paper than the topcoat pigment coating layer, contains kaolin as a pigment in an amount of 5% by weight or more and 25% by weight or less of the total pigment contained in the undercoat pigment coating layer. 6. The coated white paperboard according to 5., wherein the undercoat pigment coating layer contains delaminated kaolin having an average aspect ratio of 30 or more and 60 or less as the kaolin. 7. A coated white paperboard according to any one of 1. to 6., characterized in that the content of the heavy calcium carbonate in the undercoat pigment coating layer, which is closer to the base paper than the topcoat pigment coating layer, is 60% by weight or more of the total pigment contained in the undercoat pigment coating layer. 8. A coated white paperboard according to any one of 1. to 7., characterized in that the topcoat pigment coating layer contains kaolin as a pigment in an amount of 5% by weight or more and 80% by weight or less of the total pigments contained in the topcoat pigment coating layer. 9. A coated white paperboard described in any one of 1. to 8., characterized in that the topcoat pigment coating layer contains a styrene-butadiene-based latex having a single glass transition temperature of 0°C or higher and 30°C or lower as an adhesive. 10. A coated white paperboard described in any one of 1. to 9., characterized in that the undercoat pigment coating layer, which is closer to the base paper than the topcoat pigment coating layer, contains a styrene-butadiene-based latex having a single glass transition temperature of -50°C or higher and lower than 0°C as an adhesive. 11. A coated white paperboard described in any one of 1. to 10., characterized in that each of the pigment coating layers contains a pigment and an adhesive in a range of 5 parts by weight to 30 parts by weight of the adhesive per 100 parts by weight of the pigment. 12. The coating amount of the topcoat pigment coating layer is 3 to 15 g / m2 in total per side in dry weight. 2 12. The coated white paperboard according to any one of 1. to 11., 13. The coating weight of the undercoat pigment coating layer, which is closer to the base paper than the topcoat pigment coating layer, is 5 to 30 g / m2 in total per side in dry weight. 2 13. The coated white paperboard according to any one of 1. to 12., 14. The coated white paperboard according to any one of 1. to 13., characterized in that the base paper has at least three pulp layers. Effect of the Invention

[0008] According to the present invention, since each of the two or more pigment coating layers contains heavy calcium carbonate with a relatively wide particle size distribution, the voids in the pigment coating layer are reduced, resulting in a dense, strong pigment coating layer, and it is possible to provide a coated white paperboard that is resistant to cracking of the pigment coating layer and is suitable for use in packaging boxes for gifts, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The coated white paperboard of the present invention will be described in detail below. <About the pigment coating layer> The coated white paperboard of the present invention has two or more pigment coating layers containing a pigment containing heavy calcium carbonate and an adhesive on the surface of a base paper. In the pigment coating layers of the present invention, the outermost coating layer is also called the topcoat pigment coating layer, and the coating liquid that forms the topcoat pigment coating layer is also called the topcoat pigment coating liquid. In addition, the layer that is closer to the base paper than the outermost coating layer is also called the undercoat pigment coating layer, and the coating liquid that forms the undercoat pigment coating layer is also called the undercoat pigment coating liquid.

[0010] (About ground calcium carbonate) All of the pigment coating layers of the present invention contain heavy calcium carbonate as a pigment, in which the ratio (D75 / D25) of the particle size of 75 cumulative weight % (D75 (μm)) to the particle size of 25 cumulative weight % (D25 (μm)) measured by X-ray sedimentation particle size distribution measurement method (X-ray gravity sedimentation method) is in the range of 3.3 or more and 4.0 or less. In the present invention, the lower limit of D75 / D25 is preferably more than 3.3, more preferably 3.4 or more, and particularly preferably 3.5 or more. The smaller the D75 / D25 value, the narrower the particle size distribution, i.e., the sharper the peak of the particle size distribution of the heavy calcium carbonate. Therefore, the heavy calcium carbonate used in the pigment coating layer of the present invention has a relatively broad particle size distribution. In the present invention, the particle size distribution of the heavy calcium carbonate is made relatively broad and not uniform in particle size, thereby reducing the voids in the pigment coating layer and making it possible to obtain a pigment coating layer with high density and strength. Furthermore, by reducing the voids in the pigment coating layer, the pigments can be bonded with a small amount of binder, making it possible to obtain a pigment coating layer with good adhesion efficiency. The particle size distribution measurement by the X-ray transmission sedimentation particle size distribution measurement method employs a liquid-phase sedimentation method, and measures the particle size based on Stokes' law. In addition, X-rays are irradiated onto the suspension during settling, and the particle size distribution is measured from the amount of X-ray transmission according to the Beer-Lambert law. In the present invention, values ​​measured by an X-ray transmission sedimentation particle size distribution measurement device (Sedigraph 5100 manufactured by Micromeritics) are used.

[0011] The topcoat pigment coating layer, which is the outermost layer of the pigment coating layers of the present invention, contains the above-mentioned heavy calcium carbonate in a range of more than 5% by weight and not more than 30% by weight of the total pigment contained in the topcoat pigment coating layer. If the content is within this range, the effect of suppressing coating layer cracking can be remarkable. If the content is 5% by weight or less, the amount blended is too small to obtain a sufficient effect of suppressing coating layer cracking, and if the content is more than 30% by weight, the gaps between the white pigment particles are reduced, reducing the light scattering properties of the pigment coating layer, which may result in poor opacity. The ground calcium carbonate is contained in an amount of preferably 10% by weight or more, more preferably 15% by weight or more, and particularly preferably 18% by weight or more of the total pigment contained in the topcoat pigment coating layer, and preferably 28% by weight or less, more preferably 25% by weight or less, and particularly preferably 23% by weight or less. In addition, in the pigment coating layer of the present invention, the undercoat pigment coating layer close to the base paper preferably contains the above-mentioned heavy calcium carbonate in an amount of 60% by weight or more of the total pigment contained in the undercoat pigment coating layer in order to obtain the effect of suppressing coating layer cracking, more preferably 70% by weight or more, and particularly preferably 80% by weight or more.

[0012] The undercoat pigment coating layer of the present invention may further contain kaolin as a pigment. The content of kaolin in the undercoat pigment coating layer is preferably in the range of 0% by weight to 30% by weight, more preferably in the range of 5% by weight to 25% by weight. When the undercoat pigment coating layer contains kaolin, delaminated kaolin is preferred. Delaminated kaolin is obtained by peeling off ordinary kaolin, which is a laminate of hexagonal plate-shaped crystals, into a single layer. Since it has a relatively large particle size and a high aspect ratio, when it is added to the coating layer, the coverage of the base paper is improved and the smoothness is improved. Among them, delaminated kaolin with an average aspect ratio of 30 to 60 is preferred. Delaminated kaolin with an average aspect ratio of 30 to 60 improves white unevenness and further improves water retention. It is presumed that this is because the flat pigment fills the gaps between the pigments, suppressing dehydration and improving water retention. On the other hand, flat pigments such as delaminated kaolin with a high aspect ratio have a main surface with acidic groups, so they have poor affinity with adhesives containing many acidic groups such as latex, resulting in low adhesion efficiency. Therefore, the content of delaminated kaolin in the pigment coating layer is preferably 30% by weight or less, more preferably 25% by weight or less. In order to obtain high hiding power, smoothness, and high slipperiness during box processing, the top-coat pigment coating layer of the present invention preferably further contains kaolin as a pigment, the content of which is preferably in the range of 5% by weight to 80% by weight, more preferably 30% by weight to 80% by weight, of the total pigments contained in the top-coat pigment coating layer.

[0013] The pigment coating layer of the present invention may further contain conventionally known pigments in addition to the above.Specific examples of the pigments include inorganic fillers such as clay, calcined clay, diatomaceous earth, talc, calcined kaolin, light calcium carbonate, magnesium carbonate, barium carbonate, titanium dioxide, zinc oxide, silicon oxide, amorphous silica, calcium sulfite, gypsum, white carbon, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, zinc hydroxide, papermaking sludge, and recycled inorganic particles from deinking floss, and organic fillers such as urea-formaldehyde resin, polystyrene resin, vinyl chloride resin, melamine resin, phenol resin, and plastic hollow microparticles. In particular, in order to obtain hiding power while maintaining high whiteness, it is preferable to contain light calcium carbonate in one of the pigment coating layers, and it is more preferable to contain it in the topcoat pigment coating layer, which is particularly preferable for hiding power and high whiteness. When the topcoat pigment coating layer contains light calcium carbonate, the lower limit of the proportion of light calcium carbonate and heavy calcium carbonate relative to the total pigment contained in the topcoat pigment coating layer is preferably 15% by weight or more, more preferably 18% by weight or more, and particularly preferably 19% by weight or more, and the upper limit is preferably 50% by weight or less, more preferably 45% by weight or less, particularly preferably less than 40% by weight, and most preferably 35% by weight or less.

[0014] The adhesive (binder) contained in the pigment coating liquid in the present invention is not particularly limited, and adhesives conventionally used in coated paper can be used.Specific examples include various copolymers or latexes such as styrene-butadiene, styrene-acrylic, ethylene-vinyl acetate, butadiene-methyl methacrylate, acrylic acid-methyl methacrylate, vinyl acetate-butyl acrylate, styrene-maleic anhydride, and ethylene-maleic anhydride, polyvinyl alcohols such as fully saponified polyvinyl alcohol, partially saponified polyvinyl alcohol, acetoacetylated polyvinyl alcohol, and carboxy-modified polyvinyl alcohol, proteins such as casein, soybean protein, and synthetic protein, oxidized starch, cationic starch, urea phosphate esterified starch, etherified starch such as hydroxyethyl etherified starch, starches such as dextrin, cellulose derivatives such as carboxymethyl cellulose, hydroxyethyl cellulose, hydroxymethyl cellulose, and nanocellulose, and one or more of these adhesives can be appropriately selected and used. Among them, the adhesive used in the pigment coating liquid of the present invention preferably contains latex and starch. The latex used is preferably a styrene-butadiene-based latex (hereinafter sometimes referred to as "SBR") having a single glass transition temperature (hereinafter sometimes referred to as "Tg"). In the present invention, the undercoat pigment coating layer preferably contains an SBR having a low Tg, and the topcoat pigment coating layer preferably contains an SBR having a high Tg. Specifically, the Tg of the SBR used in the undercoat pigment coating layer is preferably -50°C or more and less than 0°C, and the Tg of the SBR used in the topcoat pigment coating layer is preferably 0°C or more and 30°C or less. Since SBR is generally softer when its Tg is lower, by using SBR having the above-mentioned Tg in each pigment coating layer, it is possible to impart cushioning properties to the undercoat pigment coating layer and strength to the topcoat pigment coating layer. Furthermore, the use of starch in the pigment coating liquid can increase the water retention of the pigment coating liquid. When a pigment coating liquid with high water retention is used, the penetration of the adhesive components into the paper during coating is suppressed, and a large amount of adhesive can be retained in the pigment coating layer, so that the effectiveness of the adhesive components in the pigment coating layer is highly expressed, resulting in a pigment coating layer with excellent pigment coating layer strength, surface strength, and cushioning properties.

[0015] The blending ratio of the pigment and adhesive in the pigment coating liquid forming each pigment coating layer of the present invention is appropriately adjusted within a range in which a desired pigment coating liquid can be obtained. Usually, the adhesive is preferably contained in a range of 5 parts by weight to 30 parts by weight, more preferably 8 parts by weight to 20 parts by weight, per 100 parts by weight of pigment, in terms of solid content ratio. If it is less than 5 parts by weight, the strength of the pigment coating layer is weakened, and problems such as the generation of paper powder and poor printing strength are likely to occur. If it is more than 30 parts by weight, the gaps between the white pigment particles in the coating layer are reduced, and although the adhesion efficiency is increased, the light scattering property of the pigment coating layer is reduced, and problems such as poor opacity and high costs are likely to occur.

[0016] In addition to the pigment and adhesive, the pigment coating liquid that forms the pigment coating layer of the present invention may contain, as necessary, various auxiliary agents that are typically blended into pigment coating liquids for coated paper, such as dispersants, viscosity improvers, water retention agents, defoamers, water resistance agents, fluorescent dyes, coloring dyes, surfactants, pH adjusters, cationic resins, anionic resins, ultraviolet absorbers, and metal salts. The solids concentration of the pigment coating liquid is preferably 58% by weight or more, and more preferably 62% by weight or more. If the solids content is lower than 58% by weight, the water retention decreases, and the quality of the coated white paperboard may decrease due to excessive penetration of the pigment coating liquid into the base paper. On the other hand, there is no particular upper limit to the solids concentration, but taking into consideration the liquid transportability, etc., it is preferably 75% by weight or less, and more preferably 70% by weight or less.

[0017] <About the base paper> The base paper in the coated white paperboard of the present invention is preferably a multi-layered paper having two or more pulp layers (paper layers). The number of layers of the base paper is preferably three or more, and more preferably five or more. The outermost paper layers of the base paper are called the front layer and back layer, and the inner layer sandwiched between the front layer and back layer is called the middle layer. The second layer in contact with the front layer toward the middle layer is called the lower surface layer. The middle layer may be one layer or two or more layers. The layers of the base paper of the present invention may be called the first layer, second layer, third layer, etc., counting from the side where the pigment coating layer is provided. The base paper of the present invention can be any paper generally used for coated white paperboard, but it is preferable that recycled paper pulp is blended in at least one layer of the multi-layered base paper. Using a base paper containing a large amount of recycled paper pulp is advantageous in terms of cost and also reduces the environmental load. The recycled paper pulp may be deinked pulp (DIP) or non-deinked pulp, and the raw material for the recycled paper pulp may be selected recycled paper such as fine paper, medium-quality paper, low-quality paper, newspaper, flyers, magazines, etc., or unselected recycled paper in which these are mixed. Pulps other than the recycled paper pulp are not particularly limited, and chemical pulps such as kraft pulp and sulfite pulp made from broadleaf or softwood trees; mechanical pulps such as thermomechanical pulp and pressurized groundwood pulp; and semi-chemical pulps such as chemical thermomechanical pulp can be used. The pulp used may be a mixture of these various pulps, or the same pulp may be used. Also, one or more paper layers containing different pulps may be laminated. The base paper of the present invention may, for example, use a pulp with low whiteness in the middle layer and a pulp with higher whiteness in the front and back layers, or may use the same pulp in all layers. In the present invention, when the number of layers of the base paper is three or more, the front and back layers preferably contain 30% by weight or more, and more preferably 50% by weight or more, of hardwood bleached kraft pulp (hereinafter sometimes referred to as "LBKP"), which has high whiteness and little impurities, relative to 100% by weight of the pulp of the front or back layer. The middle layer preferably contains 10% by weight or more, and more preferably 30% by weight or more, of waste paper pulp, which has low whiteness and relatively high impurities, relative to 100% by weight of the pulp of the middle layer.

[0018] The base paper in the present invention is usually internally added with a filler. The filler is not particularly limited, but may be, for example, inorganic fillers such as clay, calcined clay, diatomaceous earth, talc, kaolin, calcined kaolin, delaminated kaolin, heavy calcium carbonate, light calcium carbonate, magnesium carbonate, barium carbonate, titanium dioxide, zinc oxide, silicon oxide, amorphous silica, calcium sulfite, gypsum, white carbon, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, zinc hydroxide, papermaking sludge, and inorganic particles recycled from deinking floss, organic fillers such as urea-formaldehyde resin, polystyrene resin, vinyl chloride resin, melamine resin, phenolic resin, and plastic micro hollow particles, and further fillers contained in waste paper, broken paper, etc., may be used alone or in combination of two or more kinds. In blending the filler into the base paper, in order to cover up dust and color unevenness present in the middle layer, it is preferable to blend the above fillers in the back layer in an amount of 2% by weight or more relative to 100% by weight of the pulp in the back layer. There are no particular restrictions on the amount of filler contained in the surface and middle layers, but as the filler content increases, the interlaminar strength of the base paper decreases, so it is necessary to adjust the amount appropriately according to the desired quality.

[0019] The method for making the base paper in the present invention is not particularly limited, and may be carried out using a Fourdrinier papermaking machine including a top wire, an on-top former, a gap former, a cylinder papermaking machine, a board papermaking machine using a combination of a Fourdrinier papermaking machine and a cylinder papermaking machine, a Yankee dryer machine, or a hybrid papermaking machine combining these. The pH during papermaking may be acidic, neutral, or alkaline. In the case of a multi-layered base paper, the pH during papermaking may be the same for each layer or may be different for each layer. The papermaking speed is not particularly limited. The basis weight of the base paper in the coated white paperboard of the present invention is usually 150 to 650 g / m 2 That's about it. When producing a coated white paperboard according to the present invention, the base paper may be previously smoothed with an online soft calender, online chilled calender or the like before the pigment coating layer is formed.

[0020] In the present invention, the method for drying the base paper is not limited. For example, various methods such as a steam heating cylinder, a heated hot air dryer, a gas heater dryer, an electric heater dryer, and an infrared heater dryer can be used alone or in combination.

[0021] In the present invention, a base paper having low smoothness may be used, but a base paper having high smoothness may be used as long as the accumulation of the coating liquid, called puddling, during the formation of the pigment coating layer does not occur. In order to increase the smoothness of the base paper, as described above, a treatment such as precalendering may be performed before the formation of the pigment coating layer. Furthermore, as a means for improving the smoothness of the base paper, a clear coating liquid mainly composed of starch or a pigment coating liquid containing a pigment can be pre-coated on the base paper before the formation of the pigment coating layer. This pre-coated base paper may be used for the formation of the pigment coating layer without undergoing a drying process, i.e., while the coating liquid on the base paper is wet. In this way, there are no restrictions on the state of the base paper after pre-coating before being used for the formation of the pigment coating layer.

[0022] The pigment coating layer of the present invention is formed by coating the surface of the base paper with a pigment coating liquid prepared by mixing necessary ingredients such as a pigment containing heavy calcium carbonate and an adhesive with water using a conventional mixing means such as a mixer. <About the coating method> There is no particular limitation on the coating method for forming the pigment coating layer of the present invention, and various common coating devices such as a blade coater, a rod coater, an air knife coater, a roll coater, and a curtain coater can be used. Among these, the coating method using a blade coater or a rod coater is suitable as the coating method of the present invention because it can increase the density of the pigment coating layer and obtain a pigment coating layer that is less likely to crack. A rod coater is also called a bar coater or a bar blade coater.

[0023] In the present invention, the coating amount of the pigment coating layer is 8 to 50 g / m2 in total for each layer on one side in terms of dry weight. 2 is preferred, and 45 g / m 2It is more preferable that the thickness is 10 to 40 g / m or less. 2 More preferably, 11 to 35 g / m 2 The total coating weight of each layer is particularly preferably 8 g / m 2 If the coating weight is less than 50 g / m, the pigment coating layer will be too thin and the whiteness and whiteness unevenness of the coated white board may not be improved sufficiently. 2 If the temperature exceeds this range, the drying property in the drying process may decrease, resulting in a decrease in runnability, and binder migration may cause printing unevenness. In the present invention, the coating weight of the undercoat pigment coating layer and the coating weight of the topcoat pigment coating layer are not particularly limited, but in order to achieve both hiding power and whiteness, the undercoat pigment coating layer should be 5 to 30 g / m2 in total per side in terms of dry weight. 2 , topcoat pigment coating layer is 3~15g / m 2 The coating weight of the undercoat pigment coating layer and the topcoat pigment coating layer is preferably in the range of 5 g / m 2 , 3g / m 2 If the coating weight is less than this, the effect of improving the brightness and whiteness unevenness of the coated white board may not be sufficient. On the other hand, if the coating weight is too high, the drying process will be slowed down, and runnability will decrease, and the pigment coating layer will tend to be easily cracked.

[0024] The coated white paperboard of the present invention is manufactured by providing a pigment coating layer on a base paper and then undergoing a normal drying process, but may be smoothed by a surface treatment process or the like, if necessary. In a preferred embodiment, the moisture content of the coated white paperboard after manufacture is adjusted to about 3 to 10% by weight, more preferably about 4 to 8% by weight. For the smoothing process, normal smoothing treatment devices such as a supercalender, gloss calender, soft calender, thermal calender, shoe calender, etc. can be used. The smoothing treatment device is used on-machine or off-machine as appropriate, and the type of the pressure device, the number of pressure nips, heating, etc. are also adjusted as appropriate. In a preferred embodiment of the present invention, the smoothness is adjusted so that the PPS roughness of the coated white paperboard after production is 0.5 μm or more and 1.6 μm or less under a clamp pressure of 2000 kPa. The PPS roughness is preferably 0.8 μm or more. If the PPS roughness is less than 0.5 μm, the pigment coating layer becomes significantly densified during the smoothing process, the opacity of the pigment coating layer decreases, and the effect of hiding dust and color unevenness of the base paper tends to decrease. On the other hand, if the PPS roughness exceeds 1.6 μm, the smoothness is low and the feeling of the blank paper surface and the feeling of the printed surface tend to decrease.

[0025] In the present invention, a clear coating layer may be provided on the surface of the back layer in order to impart stiffness and suppress curling. The clear coating liquid for forming the clear coating layer on the surface of the back layer may contain, as necessary, various auxiliaries that are conventionally known and used, such as binders, dispersants, viscosity improvers, water retention agents, defoamers, water resistance agents, surfactants, pH adjusters, cationic resins, anionic resins, ultraviolet absorbers, and metal salts, which are typically blended into coating liquids. EXAMPLES

[0026] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In each example and comparative example, "parts" means "parts by weight" and "%" means "% by weight" unless otherwise specified.

[0027] [Example 1] <Base paper> Using 100% LBKP pulp, the basis weight is 33g / m 2 The surface layer (first layer) is made of 100% deinked recycled paper pulp with a basis weight of 36g / m 2 The second layer is made of 100% undeinked magazine waste paper pulp, weighing 45g / m 2 The middle layer and back layer (3rd to 7th layers) are made separately, laminated, pressed, and dried to form a paper with a basis weight of 294g / m2 and 7 layers. 2 The pulp slurry for each layer contained 0.6% by weight of strength agent and 1.5% by weight of aluminum sulfate per 100% by weight of pulp.

[0028] <Topcoat pigment coating liquid 1> A pigment slurry was prepared consisting of 60 parts by weight of fine kaolin (Kaofine, manufactured by Thiele), 20 parts by weight of heavy calcium carbonate (Carbital 97, manufactured by Imerys, D75 / D25=3.87), 15 parts by weight of spindle-shaped precipitated calcium carbonate (TP-221F, manufactured by Okutama Kogyo Co., Ltd., D75 / D25=2.5), and 5 parts by weight of titanium dioxide. To 100 parts by weight of the pigment, 14.5 parts by weight of styrene-butadiene copolymer latex A (ALB1443, manufactured by Asahi Kasei Co., Ltd., Tg=17°C) and 2 parts by weight of urea phosphate esterified starch were added as adhesives, and water was further added to obtain a topcoat pigment coating solution with a solids concentration of 60%. <Pigmented undercoat coating liquid 1> A pigment slurry consisting of 80 parts by weight of heavy calcium carbonate (Imerys, Carbital 90, D75 / D25 = 3.82) and 20 parts by weight of delaminated kaolin (Imerys, Contour 1500, average aspect ratio 60) was prepared, and then 12 parts by weight of styrene-butadiene copolymer latex B (Asahi Kasei, ALB1735: Tg = -8°C) and 3 parts by weight of urea phosphate ester starch were added per 100 parts by weight of pigment, and water was then added to obtain a primer pigment coating solution with a solids concentration of 60%.

[0029] <Coating> Apply the undercoat pigment coating solution 1 to the surface of the base paper using a rod coater so that the coating amount per side is 8 g / m2 (dry weight). 2 After coating so that the thickness was 12 g / m2 on each side, the top pigment coating layer 1 was applied by a blade coater without a drying step. 2 The coating was then applied and dried so that the surface was smoothed with a calendar to a basis weight of 314 g / m. 2 The resulting coated white paperboard 1 had a paper thickness of 375 μm.

[0030] [Example 2] Coated white paperboard 2 was produced in the same manner as in Example 1, except that the amount of heavy calcium carbonate in the "topcoat pigment coating liquid 1" was 25 parts by weight and the amount of light calcium carbonate was 20 parts by weight. The basis weight of the resulting coated white paperboard 2 was 314 g / m 2 The paper thickness was 387 μm.

[0031] [Example 3] Coated white paperboard 3 was produced in the same manner as in Example 1, except that the heavy calcium carbonate in the "topcoat pigment coating liquid 1" was changed to 15 parts by weight and the light calcium carbonate to 30 parts by weight. The basis weight of the obtained coated white paperboard 3 was 314 g / m 2 The paper thickness was 375 μm.

[0032] [Example 4] Coated white paperboard 4 was produced in the same manner as in Example 1, except that the amount of heavy calcium carbonate in the "topcoat pigment coating liquid 1" was 30 parts by weight and the amount of light calcium carbonate was 15 parts by weight. The basis weight of the resulting coated white paperboard 4 was 314 g / m 2 The paper thickness was 375 μm.

[0033] [Example 5] Coated white paperboard 5 was produced in the same manner as in Example 1, except that the amount of fine kaolin, heavy calcium carbonate, and light calcium carbonate in the "topcoat pigment coating liquid 1" was 86 parts by weight, 9 parts by weight, and 5 parts by weight, respectively. The basis weight of the resulting coated white paperboard 5 was 314 g / m 2 The paper thickness was 375 μm.

[0034] [Example 6] Coated white paperboard 6 was produced in the same manner as in Example 1, except that the amount of heavy calcium carbonate in the above "undercoat pigment coating liquid 1" was 70 parts by weight and the amount of kaolin was 30 parts by weight. The basis weight of the obtained coated white paperboard 6 was 314 g / m 2 The paper thickness was 375 μm.

[0035] [Comparative Example 1] Coated white paperboard a was produced in the same manner as in Example 1, except that the heavy calcium carbonate in the "topcoat pigment coating solution 1" (Imerys, Carbital 97, D75 / D25=3.87) was replaced with heavy calcium carbonate (Fimatec, FMT-OP, D75 / D25=3.0). The basis weight of the resulting coated white paperboard a was 314 g / m 2 The paper thickness was 386 μm.

[0036] [Comparative Example 2] Coated white paperboard b was produced in the same manner as in Example 1, except that the amount of heavy calcium carbonate (Imerys, Carbital 97, D75 / D25=3.87) in the "Topcoat Pigment Coating Solution 1" was 4 parts by weight, and heavy calcium carbonate (Fimatec, FMT-OP, D75 / D25=3.0) was 16 parts by weight. The basis weight of the resulting coated white paperboard b was 314 g / m 2 The paper thickness was 375 μm.

[0037] <Evaluation method for cracking of pigment coating layer> The pigment coating layers of the coated white paperboards 1 to 6 and a, b produced in Examples 1 to 6 and Comparative Examples 1 and 2 above were printed with 100% indigo solid ink using a sheet-fed printing press, and the printed surface was then creasing processed using a laboratory creaser. The creasing portion was then folded, and the pigment coating layer cracks at the folded portion were visually evaluated according to the following evaluation criteria. Only the evaluation results of "◎" and "◯" were judged to be practical coated white paperboards. The evaluation results are shown in Table 1 below. [Evaluation Criteria] ◎: No cracks in the pigment coating layer are observed ○: Almost no cracking of the pigment coating layer is observed △: Some cracking of the pigment coating layer is observed. ×: Significant cracking of the pigment coating layer is observed

[0038] [Table 1] [Industrial Applicability]

[0039] The coated white paperboard of the present invention has two or more pigment coating layers, each of which contains heavy calcium carbonate with a relatively wide particle size distribution, which suppresses voids in the pigment coating layer and results in a dense, strong pigment coating layer, making it ideal for use in packaging boxes for gifts, etc., and useful as it is resistant to cracking of the pigment coating layer.

Claims

1. A coated white paperboard having two or more pigment coating layers on the surface of a base paper, each of the pigment coating layers contains ground calcium carbonate as a pigment, the ratio (D75 / D25) of the particle size distribution curve of the 75th cumulative weight % particle size (D75) to the 25th cumulative weight % particle size (D25) being 3.3 or more and 4.0 or less; A coated white paperboard, characterized in that the content of said ground calcium carbonate in the outermost topcoat pigment coating layer is more than 5% by weight and not more than 30% by weight of all pigments contained in said topcoat pigment coating layer.

2. 2. The coated white paperboard according to claim 1, wherein the content of the ground calcium carbonate in the topcoat pigment coating layer is 18% by weight or more and 23% by weight or less of the total pigment contained in the topcoat pigment coating layer.

3. 3. The coated white paperboard according to claim 1 or 2, characterized in that the topcoat pigment coating layer contains calcium carbonate including the heavy calcium carbonate, and the content of calcium carbonate in the topcoat pigment coating layer is in the range of 15% by weight or more and 50% by weight or less of the total pigment contained in the topcoat pigment coating layer.

4. 4. The coated white paperboard according to claim 3, wherein the content of calcium carbonate in the topcoat pigment coating layer is in the range of 19% by weight or more and less than 40% by weight of the total pigment contained in the topcoat pigment coating layer.

5. A coated white paperboard according to any one of claims 1 to 4, characterized in that the undercoat pigment coating layer, which is closer to the base paper than the topcoat pigment coating layer, contains kaolin as a pigment in an amount of 5% by weight or more and 25% by weight or less of the total pigment contained in the undercoat pigment coating layer.

6. 6. The coated white paperboard according to claim 5, wherein the undercoat pigment coating layer contains delaminated kaolin having an average aspect ratio of 30 or more and 60 or less as the kaolin.

7. 7. The coated white paperboard according to claim 1, wherein the content of the ground calcium carbonate in the undercoat pigment coating layer, which is closer to the base paper than the topcoat pigment coating layer, is 60% by weight or more of the total pigment contained in the undercoat pigment coating layer.

8. The coated white paperboard according to any one of claims 1 to 7, characterized in that the topcoat pigment coating layer contains kaolin as a pigment in an amount of 5% by weight or more and 80% by weight or less of the total pigment contained in the topcoat pigment coating layer.

9. The coated white paperboard according to any one of claims 1 to 8, characterized in that the top-coat pigment coating layer contains a styrene-butadiene-based latex having a single glass transition temperature of 0°C or more and 30°C or less as an adhesive.

10. The coated white paperboard according to any one of claims 1 to 9, characterized in that the undercoat pigment coating layer, which is closer to the base paper than the topcoat pigment coating layer, contains a styrene-butadiene-based latex having a single glass transition temperature of -50°C or more and less than 0°C as an adhesive.

11. The coated white paperboard according to any one of claims 1 to 10, characterized in that each of the pigment coating layers contains a pigment and an adhesive in a range of 5 parts by weight to 30 parts by weight of the adhesive per 100 parts by weight of the pigment.

12. The coating amount of the topcoat pigment coating layer is 3 to 15 g / m2 in total per side in terms of dry weight. 2 The coated white paperboard according to any one of claims 1 to 11, characterized in that

13. The coating amount of the undercoat pigment coating layer, which is closer to the base paper than the topcoat pigment coating layer, is 5 to 30 g / m2 in total per side in terms of dry weight. 2 The coated white paperboard according to any one of claims 1 to 12, characterized in that

14. The coated white paperboard according to any one of claims 1 to 13, characterized in that the base paper has at least three pulp layers.

Citation Information

Patent Citations

  • Coated paper for offset rotary printing

    JP1998168795A

  • Coated white board applicable to sharable use in offset / gravure printing

    JP2002363887A

  • Coated white paperboard and method for producing the same

    JP2014208940A

  • Coating white paperboard for laser marking and method for producing the same

    JP2019056193A

  • Coated white board and manufacturing method thereof

    WO2012133092A1