Lithium-ion secondary battery, and manufacturing method lithium-ion secondary battery

The lithium-ion secondary battery employs core-shell structured active material particles with specific shell and buffer layers to address gas generation and resistance issues, ensuring stable Li ion concentrations and improved performance.

JP2024150335AInactive Publication Date: 2024-10-23KANEKA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023063704
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Lithium-ion secondary batteries face issues such as gas generation due to electrolyte decomposition, particularly in high-voltage environments, leading to increased resistance and reduced output, and existing coatings do not adequately address these issues.

Method used

A lithium-ion secondary battery design featuring core-shell structured active material particles with a phosphate ion-containing lithium compound shell film and a silicon-containing buffer section, which maintains distinct Li ion concentrations on the positive and negative electrodes, reducing direct contact with the electrolyte and suppressing gas generation.

Benefits of technology

The design effectively suppresses gas generation, enhances battery performance by maintaining stable Li ion concentrations, and improves safety and efficiency by reducing resistance and maintaining high energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150335000001_ABST
    Figure 2024150335000001_ABST
Patent Text Reader

Abstract

To provide a lithium-ion secondary battery with excellent characteristics capable of suppressing the generation of gas due to the decomposition of an electrolytic medium, and a manufacturing method thereof.SOLUTION: A positive electrode 10 and a negative electrode 11 include a current collector 20, 120 on which the active material layer is formed, and a coated active material particle 130 as a current collector with an active material layer, respectively. In the coated active material particles, the active material particles 30 are coated with a coating 35 containing Li ions. In the lithium-ion secondary battery, the positive electrode coating Li ion average concentration, which is the average concentration of Li ions in the coating of the positive electrode is different from the negative electrode coating Li ion average concentration, which is the average concentration of Li ions in the coating of the negative electrode.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lithium ion secondary battery and a method for manufacturing a lithium ion secondary battery. [Background technology]

[0002] Lithium-ion secondary batteries (LIBs) are required to have high energy density so that they can be used as on-board power sources for electric vehicles. In addition, as a temporary storage system for electricity from solar cells and fuel cells, in addition to increasing capacity through the electrical series connection of multiple cells to increase voltage and parallel connection to increase capacity, there is a demand for high capacity cells themselves.

[0003] LIBs are classified into non-aqueous charged liquid LIBs and all-solid-state LIBs based on the electrolytic medium they contain. The electrolytic medium for all-solid-state LIBs includes solid electrolytes and polymer electrolytes.

[0004] Non-aqueous charged liquid LIBs have problems with leakage and combustion, and the design has the disadvantage of being complicated to address these issues.

[0005] Polymer LIBs are LIBs that use a solid polymer electrolyte or a gel polymer containing a liquid electrolyte as the electrolytic medium. They have excellent stability and flexibility and can be made into a variety of forms, such as small size and thin film.

[0006] All-solid-state LIBs are known to be susceptible to "solid electrolyte oxidative degradation," in which the solid electrolyte is easily oxidized and degraded by repeated charging and discharging when in direct contact with the active material, in particular the positive electrode active material. From the perspective of extending the lifespan (for example, improving cycle characteristics), measures are needed to prevent the degradation of the solid electrolyte. Solid electrolytes can be broadly divided into bulk and thin-film types, with the bulk type being advantageous from the perspective of increasing capacity, as it can increase the absolute amount of active material.

[0007] For these reasons, a material has been proposed as an electrode material for bulk-type all-solid-state LIBs in which secondary particles of a high conductivity active material (1 x 10-4 S / cm or more) are coated with a low conductivity first ion-conducting layer (1 x 10-6 S / cm or more) and the gaps between the primary particles that make up the secondary particles are filled, thereby allowing all primary particles to directly contribute to charging and discharging, and in which the secondary particles coated with the first ion-conducting layer are layered and coated with a medium conductivity second ion-conducting layer (1 x 10-5 S / cm or more) that is a different material from the first ion-conducting layer, thereby preventing the fracture of the secondary particles due to repeated charging and discharging ("active material secondary particle fracture").

[0008] Meanwhile, lithium nickel manganese oxide (hereinafter, also referred to as LNMO) has been conventionally known as a positive electrode active material for LIBs (for example, Patent Document 1).

[0009] The operating voltage of LNMO is 4.7 V based on the deposition potential of Li metal, which is higher than that of conventional Li insertion materials used as positive electrode active materials (for example, lithium cobalt oxide has a deposition potential of 4 V), and it is expected to contribute to achieving high energy density.

[0010] In LIBs, the crystal structure of the active material changes when Li ions are inserted and removed, causing distortion, which can lead to instability (structural change, distortion, instability). As a result, the positive electrode active material undergoes dissolution of the transition metal ions that make up the crystal structure (transition metal dissolution), In the vicinity of the positive electrode, the bond with the transition metal is broken, resulting in "oxygen elimination", which generates oxygen gas, or reacts with the electrolytic medium to generate carbon dioxide gas, resulting in "gas generation". Even near the negative electrode, there is a problem of "reduced hydrogen gas generation" in which the electrolytic medium is reduced and hydrogen gas is generated. There is a demand to "suppress gas generation."

[0011] For example, in an LNMO positive electrode nonaqueous electrolyte LIB, which uses a nonaqueous electrolyte as the electrolytic medium and LNMO (described below) as the positive electrode active material, the operating voltage is high and the reaction proceeds in an oxidizing atmosphere near the positive electrode, resulting in the problem of significant "gas generation."

[0012] From the viewpoint of suppressing "oxygen desorption," it is conceivable to coat the positive electrode active material with a polyanion material such as LiFePO4 (LFP). This suppresses "oxygen desorption" as a result of "strengthening the polyanion transition metal-oxygen bond" which strengthens the bond between the transition metal in the material and oxygen. However, this gives rise to a new problem of "high polyanion resistance," which is an increase in resistance resulting from the low electrical conductivity of the polyanion.

[0013] In addition, the use of a positive electrode active material made of lithium transition metal composite oxide with a high nickel concentration results in a high-energy density LIB; however, it has been reported that output is reduced due to the inhibition of Li-ion conductivity by inactive NiO, which is generated by "oxygen desorption" due to charge-discharge cycles, etc., resulting in "inactive NiO conductivity inhibition." [Prior art documents] [Patent documents]

[0014] [Patent Document 1] Patent Publication No. 2021-051987 Summary of the Invention [Problem to be solved by the invention]

[0015] Regarding the output reduction caused by "inactive NiO conductivity inhibition," when the active material surface is coated with a carbon-supported Li-based polyanion to reduce the direct contact area with the electrolyte and suppress the generation of inactive NiO, especially when LMP is used as the Li-based polyanion, Mn 3+ Mn in PO4 3+It has been reported that the "mobile charge trap" caused by polaron holes due to the Jahn-Teller effect at the interface and the "interface mismatch" between MnPO4 and LMP cause the charge transfer potential barrier to rise, resulting in the high resistance at the interface leading to overvoltage application and, as a result, hastening the deterioration. As a countermeasure, a composite has been reported in which the surface of the first positive electrode active material of Ni-containing Li transition metal composite oxide is coated with a second positive electrode active material of an olivine type with surface carbon support and a coating layer containing CNT, but the ionic conductivity of the carbon-coated Li-based polyanion is considered to be insufficient as a distribution path for Li ions from the first positive electrode active material to the electrolytic medium.

[0016] Incidentally, polyanion materials not only have the above-mentioned "polyanion transition metal oxygen bond strengthening" effect, but also have a strong crystal structure that makes them less likely to release oxygen even at high temperatures and high voltages, making them a positive electrode active material. Polyanion-based positive electrode materials have the effect of "strongly crystalline low oxygen releasing polyanion", and for example, olivine-type Fe (LFP) and olivine-type Mn (LMP), which has a similar crystal structure, are being considered. LFP has a low energy density at low operating voltages, and LiMnPO4 has an operating voltage of 4.1V and a theoretical capacity of 160mAh / g, and is expected to have a higher energy density than the LiCoO2 currently commonly used LIB positive electrode. However, it has been reported that the material itself has a high resistance, known as "high resistance of LMP", resulting in a low output density.

[0017] Therefore, an object of the present invention is to provide a lithium ion secondary battery that can suppress the generation of gas due to decomposition of the electrolytic medium and has excellent characteristics. [Means for solving the problem]

[0018] One aspect of the present invention for solving the above problem is to A lithium ion secondary battery in which an electrode stack having a positive electrode and a negative electrode facing each other with an electrolytic medium sandwiched therebetween is enclosed in an exterior body, the positive electrode and the negative electrode each include a current collector on which an active material layer containing coated active material particles is formed, as a current collector with an active material layer; The coated active material particles are formed by coating the active material particles with a coating film containing Li ions, The positive electrode coating Li ion average concentration, which is the average concentration of the Li ions in the positive electrode coating, which is the coating of the positive electrode, is The negative electrode coating average Li-ion concentration is different from the average Li-ion concentration of the negative electrode coating, which is the coating of the negative electrode.

[0019] According to this aspect, it is possible to suppress the generation of gas due to decomposition of the electrolytic medium, and a lithium ion secondary battery having excellent characteristics is obtained.

[0020] Preferably, the coating is, from the active material particle side, The active material particles constitute a core, and a continuous shell film constitutes a shell. The shell film of a core-shell particle having a core-shell structure, and The outer surface of the core-shell particle A buffer portion formed over the entire outer surface of the shell membrane, The entire surface may include a non-forming region, and the formed region may include It consists of a buffer part, The positive electrode shell film Li ion average concentration, which is the average concentration of the Li ions in the positive electrode shell film, which is the shell film of the positive electrode, This is different from the negative electrode shell film Li ion average concentration, which is the average concentration of the Li ions in the negative electrode shell film, which is the shell film of the negative electrode.

[0021] Preferably, the positive electrode buffer Li ion average concentration, which is the average concentration of the Li ions in the positive electrode buffer, which is the buffer of the positive electrode, is The negative electrode buffer Li-ion average concentration is different from the negative electrode buffer average Li-ion concentration, which is the average concentration of the Li ions in the negative electrode buffer portion, which is the buffer portion of the negative electrode.

[0022] Preferably, the number-average ratio of the non-forming region / the entire region of the active material particles is 0.001 or more and 0.3 or less.

[0023] Preferably, the shell film is a phosphate ion-containing lithium compound containing one or more metals selected from the group consisting of Fe, Mn, Si, and Al.

[0024] Preferably, the active material particles of the negative electrode contain lithium titanate, resulting in a highly safe LIB.

[0025] Preferably, the active material particles of the positive electrode contain lithium nickel manganese oxide, resulting in a higher power LIB.

[0026] One aspect of the present invention for solving the above problem is to The method for producing the lithium ion secondary battery described above includes the steps of: On the current collector, a positive electrode active material layer including positive electrode active material particles formed on the positive electrode active material layer-attached current collector A; and A negative electrode active material layer containing negative electrode active material particles is formed to obtain a current collector A with a negative electrode active material layer. A manufacturing process for a current collector A with an active material layer; At least one pair of the positive electrode current collector A and the negative electrode current collector A is disposed opposite to each other, An electrode laminate A manufacturing process for manufacturing an electrode laminate A; The electrode laminate A is immersed in an electrolyte solution B under conditions B. As a buffer section B which is a part of the buffer section, A current collector B with a positive electrode active material layer including a positive electrode buffer portion B, and A current collector B having a negative electrode active material layer including a negative electrode buffer portion B is formed, An electrode laminate B manufacturing process for manufacturing an electrode laminate B including a buffer portion B; The electrode laminate B is immersed in an electrolyte solution C under conditions C. As a buffer section C which is a part of the buffer section, A current collector C with a positive electrode active material layer including a positive electrode buffer portion C, and A current collector C having a negative electrode active material layer including a negative electrode buffer portion C is formed. An electrode laminate C manufacturing process for manufacturing an electrode laminate C including a buffer portion C, Regarding the positive electrode buffer part and the negative electrode buffer part, which are the buffer parts of the positive electrode and the negative electrode, The thickness of the positive electrode buffer part B in the positive electrode buffer part: the thickness of the negative electrode buffer part B in the negative electrode buffer part, and The thickness of the positive electrode buffer part C in the positive electrode buffer part: the thickness of the negative electrode buffer part C in the negative electrode buffer part, The thickness of the buffer portion formed under each condition for the positive electrode and the negative electrode is Between the conditions, the positive electrode and the negative electrode are formed thicker on one side and thinner on the other side, The present invention relates to a method for producing an electrode laminate for a lithium ion secondary battery, in which the ratio is less than 10:5, or less than 5:10.

[0027] According to this aspect, one of the electrode stack B manufacturing process and the electrode stack C manufacturing process is a manufacturing method in which the positive electrode buffer part is mainly formed and the other is a manufacturing method in which the negative electrode buffer part is mainly formed. Therefore, buffer parts suitable for each can be formed, and it is possible to suppress the generation of gas due to decomposition of the electrolytic medium and to manufacture a lithium ion secondary battery with excellent characteristics. Effect of the Invention

[0028] The lithium ion secondary battery of the present invention is inhibited from generating gas due to decomposition of the electrolytic medium, and has excellent characteristics.

[0029] According to the method for producing a lithium ion secondary battery of the present invention, the generation of gas due to decomposition of the electrolytic medium is suppressed, and a lithium ion secondary battery with excellent characteristics can be produced. [Brief description of the drawings]

[0030] [Figure 1] FIG. 1 is an explanatory diagram conceptually illustrating a lithium ion secondary battery according to a first embodiment of the present invention, where (a) is a perspective view of the lithium ion secondary battery, (b) is a cross-sectional view taken along line AA in (a), and (c) is a cross-sectional view taken along line BB in (a). [Diagram 2] FIG. 2 is an explanatory diagram of the electrode parts of the positive electrode part and the negative electrode part in FIG. 1, where (a) is a cross-sectional view of the electrode parts and (b) is a cross-sectional view of coated active material particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] Hereinafter, an embodiment of the present invention will be described in detail.

[0032] (Lithium-ion secondary battery (LIB) 1) A lithium ion secondary battery (also simply referred to as a LIB) 1 of a first embodiment of the present invention has a battery assembly 2 in which an electrode stack 5 is housed in an outer casing 3, as shown in FIG. 1, and the outer casing 3 of the battery assembly 2 is filled with an electrolytic medium 6 and sealed.

[0033] The lithium ion secondary battery 1 may be a nonaqueous electrolyte LIB in which the electrolytic medium 6 is a nonaqueous electrolyte solution, an all-solid-state LIB in which the electrolytic medium 6 is a solid electrolyte, or a polymer LIB in which the electrolytic medium 6 is a polymer electrolyte, and is preferably a nonaqueous electrolyte LIB.

[0034] In the following description, the lithium ion secondary battery 1 is a non-aqueous electrolyte LIB. <Exterior body 3> The exterior body 3 can be appropriately selected so long as it is chemically stable to the electrolytic medium (electrolytic solution) 6, particularly stable to the nonaqueous electrolytic solution 6, and has sufficient water vapor barrier properties, and the electrode laminate 5 can ultimately form an airtight internal space that contains the electrolytic medium 6.

[0035] Materials and forms used for the exterior body 3 include cans primarily made of aluminum, iron, or stainless steel, and laminate films containing laminate resin. For exterior bodies 3 using laminate resin, in the case of non-aqueous electrolyte secondary batteries, laminate films such as aluminum, silica-coated polypropylene, and polyethylene can also be used; however, from the standpoint of versatility, cost, and the like, it is preferable to use aluminum laminate films. A preferred exterior body 3 is one formed by adhesively bonding two sheets of metal laminate films. <Electrode laminate 5> As shown in FIG. 1, the electrode laminate 5 has a positive electrode part 10, a negative electrode part 11, a separator 12, a positive electrode extraction member 13, and a negative electrode extraction member 14. (Positive electrode part 10, negative electrode part 11) The positive electrode part 10 and the negative electrode part 11 are formed by laminating a positive electrode active material layer 21 and a negative electrode active material layer 121 on at least one of the main surfaces of a positive electrode current collector 20 and a negative electrode current collector 120, as shown in FIG. 1(b), and are intercalation electrodes into which Li ions can be inserted and extracted.

[0036] In the positive electrode part 10 and the negative electrode part 11 of this embodiment, a positive electrode active material layer 21 and a negative electrode active material layer 121 are laminated on both main surfaces of a positive electrode current collector 20 and a negative electrode current collector 120, as shown in FIG. 2(a). (Positive electrode current collector 20, negative electrode current collector 120) The positive electrode current collector 20 and the negative electrode current collector 120 are plate-like or film-like bodies having electrical conductivity, and are not particularly limited as long as they are electrically conductive. For example, aluminum or an aluminum alloy can be used. However, since these are stable in the positive electrode reaction atmosphere and the negative electrode reaction atmosphere, aluminum or an aluminum alloy is preferable, and high-purity aluminum represented by JIS standards 1030, 1050, 1085, 1N90, 1N99, etc. is more preferable, and a coating in which a metal surface is coated with a metal that does not react at the positive electrode potential can be used. (Active material layer 2 (positive electrode active material layer 21, negative electrode active material layer 121)) The active material layer 2 (positive electrode active material layer 21, negative electrode active material layer 121) is configured to contain particles 30 of a Li-ion conductive active material, and is also configured to contain a binder 70, a conductive network 80, and a permeable pore network 81. The active material layer 2 is formed on the current collector 20, 120, and preferably includes an SEI structure. As shown in the enlarged view of FIG. 2( a ), the active material layer 2 is preferably a sea-island film having a sea-island structure, and has a cross-sectional shape including sea-like portions 60 and island-like portions 61, which is a so-called bulk film.

[0037] In the positive electrode active material layer 2, the coated active material particles 30 account for a large proportion by weight, but in terms of volume, the binder 70 and conductive network 80 account for a proportion that can be confirmed even with an electron microscope. (Coated active material particles 30) 2(b), the coated active material particle 30 includes an active material particle 40 and a core-shell particle 36 having a core-shell structure with a negative electrode active material layer 121 as a core and a shell film 41 as a shell. That is, in the core-shell particle 36, the shell film 41 covers the outer surface of the positive electrode active material particle 40.

[0038] The coated active material particle 30 of this embodiment further includes a buffer portion 42 on a part or all of the outer surface of the shell film 41. That is, the coated active material particle 30 of this embodiment has a coating 35 covering the surface of the positive electrode active material particle 40, and the coating 35 is a multilayer film of the shell film 41 and the buffer portion 42.

[0039] From the viewpoint of achieving a higher performance LIB, it is preferable that the positive electrode shell film Li ion concentration, which is the concentration of Li ions contained in the shell film 41 of the positive electrode active material particle 130, is different from the negative electrode shell film Li ion concentration, which is the concentration of Li ions contained in the shell film 41 of the negative electrode active material particle 130, and it is more preferable to design and manufacture them separately for LIBs that require high-speed charging and LIBs that require high-speed discharging, and these concentrations are average concentrations in the film. Furthermore, in the multilayer film of the shell film 41 / buffer section 42 described above, the buffer section 42 contains oxides and / or organic matter that do not contain Li ions and is composed of Li ions as a whole, so by making the positive electrode multilayer film Li ion concentration and the negative electrode multilayer film Li ion concentration different, it is possible to achieve a higher performance LIB, and it is preferable, and more preferable, to design and manufacture them separately for LIBs that require high-speed charging and LIBs that require high-speed discharging. (active material particles 40, 140) The active material particles 40, 140 are lithium transition metal composite oxide particles, and are capable of inserting and desorbing lithium ions.

[0040] The particle size is not particularly limited, but the median diameter d50 is preferably 5 μm or more, more preferably 10 μm or more, still more preferably 20 μm or more, preferably 100 μm or less, more preferably 80 μm or less, still more preferably 50 μm or less, and particularly preferably 30 μm or less.

[0041] <Positive electrode active material particles 40> The positive electrode active material particles 40 preferably have an average potential of lithium desorption and insertion of 4.5 V or more and 5.0 V or less with respect to the deposition potential of lithium metal (vs. Li + / Li, also denoted as). That is, the positive electrode active material particles 40 preferably have an operating potential based on lithium metal of 4.5 V or more and 5.0 V or less when alone.

[0042] The potential of the lithium ion insertion / desorption reaction (hereinafter also referred to as voltage) (vs. Li + / Li) can be determined, for example, by measuring the charge-discharge characteristics of a working electrode using the positive electrode active material particles 40 and a lithium metal counter electrode, and reading the voltage values at the start and end of the plateau. When there are two or more plateaus, it is sufficient that the plateau with the lowest voltage value is 4.5 V (vs. Li + / Li) or more, and it is sufficient that the plateau with the highest voltage value is 5.0 V (vs. Li + / Li) or less.

[0043] The positive electrode active material particles 40 are not particularly limited, but spinel-type lithium manganese-based oxides represented by the following formula (1) are preferred.

[0044] Li 1+x M y Mn 2-x-y O4 ···(1) In the above formula (1), x and y each satisfy 0 ≦ x ≦ 0.2 and 0 < y ≦ 0.8, M is at least one selected from the group consisting of Al, Mg, Zn, Ni, Co, Fe, Ti, Cu, and Cr, and attention should also be paid to the "influence of promoting reduction decomposition of acetonitrile-eluted metal ion negative electrode deposition SEI damage" described later.

[0045] Among the above formula (1), lithium nickel manganese oxide (LNMO) in which M is Ni is preferable, but measures against the above-mentioned "diffusion inhibition of oxygen desorption inactive NiO" are required. (Negative electrode active material particles 140) It is preferable to use lithium titanate for the negative electrode active material particles 140, since lithium deposition is less likely to occur and safety is improved.

[0046] Among lithium titanate, the negative electrode active material particles 140 are particularly preferably lithium titanate having a spinel structure, since the expansion and contraction of the active material during the lithium ion insertion and desorption reaction is small.

[0047] Lithium titanate may contain trace amounts of elements other than lithium and titanium, such as Nb. (Shell Membrane 41) The shell film 41 is a film having a continuous layer structure that densely covers the surface shape of the active material particle 30, and is a coating composed of a Li-ion conductive compound containing phosphorus as an element, and is preferably composed of an intercalation material that functions as a positive electrode active material by itself.

[0048] Shell film 41 contains a phosphate ion-containing Li compound that further contains one or more metals selected from the group consisting of Fe, Mn, Si, and Al.

[0049] Such phosphate ion-containing Li compounds are preferably lithium phosphate compounds such as lithium manganese phosphate (hereinafter also referred to as LMP) and Li iron phosphate (hereinafter also referred to as LFP) having an olivine type crystal structure, lithium titanium aluminum phosphate (hereinafter also referred to as LATP) having a NASICON type crystal structure, and lithium phosphate (hereinafter also referred to as LP), and lithium transition metal phosphates such as LMP, LFP, and LATP are preferred.

[0050] As for LP, Li3PO 4-a-b X aY b (X is one selected from the group consisting of N, S, B, and Si, and Y is any halogen atom), which suppresses the consumption of Li present in the LIB and results in a high-capacity, low-resistance LIB. It has been reported that the compound has a structure in which some of the oxygen atoms are replaced by X and Y, and since the introduction of X improves the Li conductivity but reduces the electrical insulation, the introduction of an appropriate amount of Y ensures electrical insulation.

[0051] Among these, the shell film 41 is preferably a phosphate ion-containing lithium compound film containing manganese (Mn) element, and is more preferably an LMP having the characteristics of the "strongly crystalline low oxygen releasing polyanion" described above.

[0052] From the viewpoint of fully exerting the effects of the "strongly crystalline, low-oxygen releasing polyanion" and the effect as an "insertion destruction prevention" layer while suppressing the adverse effects of "high LMP resistance," "mobile charge traps," "elevated charge transfer potential barrier," and "interface mismatch," it is preferable that the shell film 41 has different metal components and / or compositions on both sides and has an LFP / LMP two-layer structure from the center of the active material particle 30 to the outside, more preferably, the shell film 41 has a constituent transition metal that is gradually changed from Fe to Mn, and even more preferably, the composition and / or ratio of the metal components of the "Li-based polyanion" is changed, including the buffer section 42 described later.

[0053] The thickness of shell film 41 is thinner than the particle diameter of the lithium ion conductive oxide, and is preferably 5 nm or more and 20 nm or less, and more preferably 5 nm or more and 15 nm or less.

[0054] Within this range, the amount of gas generated can be suppressed while suppressing the resistance loss in shell film 41.

[0055] The shell film 41 covers at least a portion of the surface of the positive electrode active material particle 40, more preferably covers 95% or more, and preferably covers the surface completely.

[0056] Shell film 41 is preferably amorphous from the viewpoint of “replenishment of consumed Li” for replenishing Li ions of positive electrode active material particles 40 consumed by the SEI structure of buffer section 42 described later. (Buffer part 42) The buffer portion 42 is a silicon-containing compound film that contains lithium element and further contains silicon element.

[0057] The buffer section 42 has a solid electrolyte interface (hereinafter also referred to as SEI) structure generated by an electrochemical reaction between the core-shell particles 36 and the interface electrolyte, and is preferably a siloxane-modified coating layer containing silicon element.

[0058] The buffer section 42 is a selectively permeable membrane that passes only lithium ions but not electrons, and is an “insertion / destruction prevention” layer that prevents organic solvent molecules with a large molecular weight that move together with Li ions in the electrolytic medium 6 from being inserted into the core-shell particles 36, particularly into the Li ion insertion / desorption sites of the active material particles 30, thereby preventing the structure from being destroyed.

[0059] The buffer portion 42 preferably includes a modified region that is inseparably integrated with the SEI structure at the surface near the interface with the core-shell particle 36, particularly at the contact portion with the permeable pore network 81.

[0060] In addition to lithium and silicon elements, the buffer portion 42 may contain a metal oxide and / or a metal phosphate.

[0061] Furthermore, it is preferable that the multilayer film of shell film 41 / buffer section 42 has different metal components and / or compositions on both sides and different concentrations of phosphate ions, from the viewpoint of fully exerting the effects of "strongly crystalline, low-oxygen-releasing polyanion" and "replenishment of consumed Li" while suppressing the adverse effects of high resistance due to Li-based polyanion coating, and it is preferable to decrease the concentration of phosphate ions and increase the concentration of oxides from the center to the outside of active material particle 30, and when shell film 41 contains LMP, it is more preferable to gradually change the composition and / or concentration in order to suppress "mobile charge traps" and "rise in charge transfer potential barrier", and to suppress "interface mismatch".

[0062] The buffer portion 42 covers at least a portion of the surface of the core-shell particle 36, more preferably covers 95% or more, and preferably covers the surface completely. (Binder 70) The binder 70 is not particularly limited, but may be, for example, at least one selected from the group consisting of polyethylene glycol (PEG), polyethylene oxide (PEO), polyacrylonitrile (PAN), polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), styrene-butadiene rubber, polyimide, and derivatives thereof.

[0063] The binder 70 may include dispersants, thickeners, and conductive aids that are soluble in the binder material.

[0064] The amount of binder 70 is preferably 1 part by weight or more and 30 parts by weight or less per 100 parts by weight of core-shell particles 36, which can impart to the active material layer 2 the strength necessary to support the active material particles 30 and the core-shell particles 130 as an integral layer, and can also stably form a low-resistance conductive network 80, and can provide sufficient adhesive strength to the current collectors 20, 120.

[0065] Within this range, the positive electrode active material layer 21 can be formed in which the core-shell particles 36 are bonded with sufficient adhesive strength, and a stable low-resistance conductive network 80 can be configured. Furthermore, sufficient adhesive strength can be obtained with respect to the current collector 20. (Conductive network 80) The conductive network 80 is composed of a conductive material, preferably a conductive carbon material, and more preferably at least one selected from natural graphite, artificial graphite, vapor-grown carbon fiber, carbon nanotubes, acetylene black, ketjen black, and furnace black.

[0066] The amount of the conductive network 80 is preferably 1 part by weight or more and 30 parts by weight or less with respect to 100 parts by weight of the core-shell particles 36 .

[0067] Within this range, the conductivity of the positive electrode part 10 can be ensured while maintaining the adhesiveness to the binder 70. In addition, the adhesiveness to the current collector 20 can be sufficiently obtained while the electrical conductivity with the current collector 20 can be sufficiently obtained.

[0068] At least a portion of the conductive network 80 contacts the core-shell particles 36 and extends outward from the contact portion with the core-shell particles 36 . (Sea-like part 60) The sea-like portion 60 is composed of coated active material particles 30, a binder 70, and a conductive network 80, as shown in the enlarged view of FIG. 2(a).

[0069] The sea-like portion 60 is longer than the conductive paths between adjacent coated active material particles 30, 30, and has a chain-like conductive network 80 as its main skeleton, with the binder 70 supporting the state in which multiple coated active material particles 30 are in contact with this conductive network 80.

[0070] It is presumed that the potential uniformity in the active material layer 2 is achieved not by the conductive paths between the coated active material particles 130 but by the conductive network 80, which is like a long chain, mainly composed of the conductive assistant.

[0071] The reason why a structure is formed in which the binder 70 supports the state in which multiple coated active material particles 30 are in contact with such a conductive network 80 is that, when produced by the manufacturing method described below, in the slurry formed in the paste application process, the coated active material particles 30 with hydrophilic surfaces are arranged in a hydrophobic medium containing a conductive material, binder, and solvent, and then, by drying and removing the solvent, the particles are supported by the binder 70. (Island 61) The islands 61 are composed of a permeable pore network 81, as shown in FIG. 2(a).

[0072] The permeable pore network 81 has a plurality of pores which are interconnected to allow the electrolytic medium 6 to permeate therethrough.

[0073] Preferably, the permeating pore network 81 has some of its pores extending to and contacting the core-shell particles 36 .

[0074] The permeable pore network 81 has a non-liquid lithium ion conductor having an SEI structure disposed at least in the contact portion.

[0075] The lithium ion conductor preferably contains one or more metal elements selected from Mn, Fe, Al and Si.

[0076] From another perspective, the permeable pore network 81 is a cavity formed by the contours of the coated active material particles 30, the binder 70, and the conductive network 80, and is three-dimensionally continuous from the positive electrode collector 20 side (inside) to the outside.

[0077] On the surface of the positive electrode active material particle 40 or the shell film 41, the ratio of the total area of ​​the pores to the area of ​​the surface is preferably 0.1% to 30%, and more preferably 1% to 10%.

[0078] The permeable pore network 81 is in contact with the positive electrode active material particles 40 or the shell film 41, and at least a portion of the electrolytic medium 6 permeates therethrough during charging and discharging of the LIB1. It is preferable that an SEI structure-containing non-liquid Li ion conductor is formed in the contact portion of the permeable pore network 81, and such an SEI structure-containing non-liquid Li ion conductor preferably contains one or more metal elements selected from the group consisting of Mn, Si, Fe, and Al, and more preferably contains Mn and Si.

[0079] <Conductive materials> The conductive material constituting the conductive network 80 of the present invention is preferably a conductive carbon material, and is preferably at least one selected from natural graphite, artificial graphite, vapor-grown carbon fiber, carbon nanotubes, acetylene black, ketjen black, and furnace black.

[0080] The amount of the conductive material contained in the active material layer 2 is preferably 1 part by weight or more and 30 parts by weight or less per 100 parts by weight of the (coated) active material particles 30, 130 and coated active material precursor particles 36, and while ensuring the conductivity of the positive electrode portion 10 and the negative electrode portion 11, preferably the conductivity of the conductive network 80 of the present invention is sufficiently ensured, adhesion to the binder 70 is maintained, and sufficient adhesion to the current collectors 20, 120 is obtained while ensuring sufficient conductivity with the current collectors 20, 120. <Electrolytic medium 6> The electrolytic medium 6 is an electrolytic solution or a solid electrolyte, and in this embodiment is a non-aqueous electrolytic solution.

[0081] The electrolytic medium 6 is not particularly limited, but may be a non-aqueous electrolyte solution in which a solute is dissolved in a non-aqueous solvent, or a gel electrolyte in which a polymer is impregnated with a non-aqueous electrolyte solution in which a solute is dissolved in a non-aqueous solvent.

[0082] The electrolytic medium 6 is not particularly limited, but may be a nonaqueous electrolyte, a polymer electrolyte, or a solid electrolyte. From the viewpoint of effectively achieving the effects of the present invention, it is preferable that the electrolytic medium 6 be a nonaqueous electrolyte having a solute dissolved in a nonaqueous solvent, or a polymer electrolyte having a polymer impregnated with a nonaqueous electrolyte having a solute dissolved in a nonaqueous solvent, and more preferably a nonaqueous electrolyte.

[0083] (Electrolytic medium 6) The electrolytic medium 6 may be previously contained in the positive electrode part 10 and the negative electrode part 11, and preferably in the separator 12 present in the electrolytic medium 6, or may be added after wrapping or laminating the separator 12 disposed between the positive electrode part 10 side and the negative electrode part 11 side.

[0084] The non-aqueous electrolyte is a liquid in which a Li salt is dissolved in a non-aqueous solvent, and various additives described below are added as necessary. In addition, other additives can be added for the purpose of improving charge / discharge cycle characteristics, high-temperature storage properties, safety, etc.

[0085] Polymers for polymer electrolytes include PEG, PEO, PAn, PVDF, fluoropolymers, and polymers obtained by grafting (meth)acrylic polymers onto these, and the like, and those having a weight average molecular weight of 5,000 to 20,000 are used.

[0086] As the solid electrolyte, any electrolyte having high ionic conductivity can be used. A ceramic electrolyte containing Li is preferable. For example, Li 10 GeP2S12, Li7P3S13, 70Li2S-30P2S5, La 0.1 Li 0.34 TiO 2.94 , Li 1.1 Al 0.7 Ti 1.5 (PO4)3, etc., and the preferred conductivity is 1×10 -4 S / cm or more, more preferably 1×10 -3S / cm or more, and a preferable thickness is 5 μm or more and 200 μm or less. If it is less than 5 μm, the mechanical strength of the solid electrolyte layer is insufficient and it is prone to short circuits, and a thickness of 10 μm or more and 100 μm or less is more preferable.

[0087] <Non-aqueous solvent> The non-aqueous solvent preferably contains a cyclic aprotic solvent and / or a chain aprotic solvent.

[0088] Examples of cyclic aprotic solvents include cyclic carbonates, cyclic esters, cyclic sulfones, and cyclic ethers. From the viewpoint of forming a high-quality SEI, a cyclic carbonate-based compound containing an unsaturated bond or a halogen atom may be used.

[0089] As the chain aprotic solvent, a solvent generally used as a solvent for a nonaqueous electrolyte, such as a chain carbonate, a chain carboxylate, a chain ether, or acetonitrile, may be used. From the viewpoint of forming a high-quality SEI, a chain carbonate-based compound containing an unsaturated bond or a halogen atom may be used.

[0090] More specifically, examples of aprotic solvents that can be used include dimethyl carbonate, methyl ethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, γ-butyrolactone, 1,2-dimethoxyethane, sulfolane, dioxolane, and methyl propionate.

[0091] These solvents may be used alone or in combination of two or more. However, it is preferable to use a mixture of two or more solvents in view of the ease of dissolving the solute described below and the high conductivity of Li ions.

[0092] When two or more types of aprotic solvents are mixed, it is preferable to mix one or more types of chain carbonates exemplified by dimethyl carbonate, methyl ethyl carbonate, diethyl carbonate, dipropyl carbonate, and methyl propyl carbonate with one or more types of cyclic compounds exemplified by ethylene carbonate, propylene carbonate, butylene carbonate, and γ-butyrolactone, because these have high stability at high temperatures and high Li conductivity at low temperatures.

[0093] A mixture of one or more chain carbonates exemplified by dimethyl carbonate, methyl ethyl carbonate, and diethyl carbonate and one or more cyclic carbonates exemplified by ethylene carbonate, propylene carbonate, and butylene carbonate is particularly preferred.

[0094] <Solute> The solute is not particularly limited, but for example, LiClO4, LiBF4, LiPF6, LiAsF6, LiCF3SO3, LiBOB (Lithium Bis(Oxalato)Borate), LiN(SO2CF3)2, etc. are preferred because they are easily dissolved in the solvent.

[0095] (Additives for non-aqueous electrolyte 6) Examples of additives to the non-aqueous electrolyte 6 include an electrode protector, a gas generation inhibitor, an SEI forming agent, an SEI formation promoter, an SEI characteristic improver, a stabilizer, a metal elution inhibitor, and a flame retardant.

[0096] (Silicon-containing compounds) Examples of the silicon-containing compound include siloxane compounds, silazane compounds, and silylamide compounds each containing one or more unsaturated groups. Preferred silicon-containing compounds include cyclic siloxanes having a vinyl group, such as 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane (4VC4S).

[0097] A siloxane-based compound containing one or more unsaturated groups contains a -Si-O-Si- bond (siloxane bond) and at least one carbon-carbon double bond. It is believed that the siloxane bond site can conduct Li ions and that this double bond can contribute to the formation of an SEI structure through cross-linking. (Separator 12) As shown in FIG. 1, the separator 12 is disposed between the positive electrode part 10 and the negative electrode part 11, and has a structure that is insulating and can contain the electrolytic medium 6.

[0098] Examples of the separator 12 include woven fabrics, nonwoven fabrics, and microporous membranes made of nylon, cellulose, polysulfone, polyethylene, polypropylene, polybutene, polyacrylonitrile, polyimide, polyamide, polyethylene terephthalate, and composites of two or more of these.

[0099] The separator 12 may contain various plasticizers, antioxidants, and flame retardants, and may be coated with metal oxides or the like.

[0100] (Positive electrode extraction member 13, negative electrode extraction member 14) The extraction members 13 and 14 are terminals that are connected to one or more positive electrode parts 10 and one or more negative electrode parts 11 and can be connected to an external load, and are provided across the inside and outside of the exterior body 3.

[0101] (Manufacturing method of Li-ion secondary battery 1) Next, a method for manufacturing the Li-ion secondary battery 1 of this embodiment will be described.

[0102] (All-solid-state LLIB manufacturing method) The method for producing an all-solid-state LIB involves applying a solid electrolyte slurry to both sides of the prepared positive electrode part 10 and negative electrode part 11 using a doctor blade method, volatilizing the solvent to form a solid electrolyte layer, and then heating and drying (e.g., in the air, at 150°C) the electrode laminate 5 in which the positive electrode part 10 and the negative electrode part 11 are stacked, preferably alternately, with the solid electrolyte layer between them, and then compression molding using a press to complete the basic structure of the all-solid-state LIB.

[0103] (Nonaqueous electrolyte LIB) The method for producing the Li-ion secondary battery 1 of this embodiment, which is a method for producing a non-aqueous electrolyte LIB, is mainly composed of a coated active material forming process, a paste-coated current collector firing process, an electrode laminate forming process, a battery assembly creating process, an interface electrolyte injection process, a voltage application process, an electrolytic medium injection process, and an aging process. <Coated active material formation process> The coated active material forming step is a step of forming the coated active material particles 30, 130.

[0104] The coated active material forming step is mainly composed of an active material particle preparing step, a shell film forming step, and a paste applying step. (Active material particle preparation process) The active material particle preparation step is a step of preparing the active material particles 40, 140. (Shell film formation process) The shell film forming step is a step of forming the shell film 41, which is a Li compound film containing phosphate ions, on the surface of the active material particles 40,140.

[0105] Specifically, in the shell film formation step, first, a phosphate ion-containing Li compound is pulverized by a pulverizing device such as a ball mill to form phosphate ion-containing Li compound particles (pulverizing step).

[0106] Subsequently, the mixture is pulverized in a pulverization step, and the phosphate ion-containing Li compound particles are dispersed in a dispersion solvent to form a fine particle fluid (fine particle fluid formation step).

[0107] The dispersion solvent used in this case is preferably one or more alcohol solutions, and more preferably ethanol from the viewpoints of volatility and safety.

[0108] The fine particle fluid formed at this time is a transparent sol in a sol state and has fluidity.

[0109] Next, at least one type of energy of shear force, compression force, collision force, and centrifugal force is applied to the positive electrode active material particles 30 and / or the phosphate ion-containing Li compound particles constituting the shell film 41, while a mechanical coating method is used to mechanically contact the active material particles 30 with the phosphate ion-containing Li compound particles in the microparticle fluid, thereby forming a shell film 41 on the surface of the positive electrode active material particles 30.

[0110] In this embodiment, the microparticle fluid is ground into active material particles 30 by a grinding device such as a grinding mill to form a ground product (ground product forming step).

[0111] At this time, the amount of the phosphate ion-containing Li compound particles put into the grinding device is preferably 0.5 wt % or more.

[0112] At this time, the amount of the phosphate ion-containing Li compound particles put into the grinding device is preferably 2.5 wt % or less, more preferably 1.6 wt % or less, and particularly preferably 1 wt % or less.

[0113] The treatment temperature in the milling device is preferably 5°C or higher and 100°C or lower, more preferably 8°C or higher and 80°C or lower, and even more preferably 10°C or higher and 50°C or lower.

[0114] The treatment time in the milling device is preferably from 5 to 90 minutes, and more preferably from 10 to 60 minutes.

[0115] The atmosphere in the milling apparatus at this time is preferably an inert gas atmosphere or an air atmosphere.

[0116] Next, the ground product is subjected to a heat treatment to remove the dispersion solvent from the ground product, thereby forming a shell film 41 (removal step).

[0117] The heat treatment temperature at this time is preferably 300° C. or higher, and more preferably 350° C. or higher.

[0118] If the heat treatment temperature is below 300° C., the adhesion between the active material particles 30 and the shell film 41 will be insufficient, and the shell film 41 may peel off during charging and discharging of the battery, which may lead to a decrease in the long-term reliability of the battery.

[0119] On the other hand, if the heat treatment temperature is too high, the crystal structure of shell film 41 may change, causing a decrease in Li-ion conductivity and preventing normal charging and discharging of the battery. Therefore, the heat treatment temperature is preferably 850°C or less, and more preferably 500°C or less from the viewpoint of suppressing crystallization of the amorphous portion of the partially formed shell film 41, which may be preferable.

[0120] The heat treatment time is preferably 30 minutes or more, more preferably 45 minutes or more, and is preferably 180 minutes or less, more preferably 150 minutes or less.

[0121] The above is an explanation of the shell film forming step for forming the shell film 41, which is a phosphate ion-containing Li compound film, on the surface of the active material particle 30. The shell film formation process of forming a shell film 41, which is a phosphate ion-containing Li compound film, on the surface of a positive electrode active material particle 40 and the shell film formation process of forming a shell film 41, which is a phosphate ion-containing Li compound film, on the surface of a negative electrode active material particle 140 are basically the same, except that the active material particles 30 to be coated are positive electrode active material particles 40 or negative electrode active material particles 140. (Paste application process) The paste application process is a process in which active material particles 40, 140 having shell film 41 formed thereon are mixed with a conductive assistant and a binder, and optionally a silicon-containing compound, dispersed in a solvent to form a paste-like slurry, and the slurry is applied to current collector 20, 120 to form a paste-coated current collector.

[0122] The solvent used in this step is not particularly limited as long as it can dissolve or disperse the active material particles 40, 140, the conductive assistant, and the binder, and examples of the solvent that can be used include N-methyl-2-pyrrolidone (NMP), dimethylformamide, dimethylacetamide, methyl ethyl ketone, methyl acetate, ethyl acetate, and tetrahydrofuran. A dispersant and a thickener may be added to these. <Paste-coated current collector firing process> The paste-coated current collector firing process is a process in which the paste-coated current collector is fired for a predetermined firing time at a predetermined firing temperature to form a work-in-progress positive electrode part containing positive electrode active material particles 40 and a work-in-progress negative electrode part containing negative electrode active material particles 140, respectively.

[0123] The firing temperature is not particularly limited as long as the paste-coated current collector is fired and the slurry is solidified at the temperature, but is preferably, for example, 80° C. or higher and 200° C. or lower. <Electrode laminate formation process> The electrode laminate formation step is a step of forming an in-progress electrode laminate by sandwiching a separator 12 between an in-progress positive electrode part and an in-progress negative electrode part. <Battery assembly manufacturing process> The battery assembly fabrication step is a step in which a part-time electrode laminate is placed inside the exterior body 3 to fabricate a part-time battery assembly. <Interfacial electrolyte injection process> The interface electrolyte injection process is a process in which, for example, using a vacuum packaging machine, the interior is reduced in pressure to 0.1 atmospheres or less while sealing the exterior body 3 containing the in-progress electrode laminate inside except for the injection port, and then the interface electrolyte is injected into the exterior body 3 of the in-progress battery assembly.

[0124] The interface electrolyte has Li-ion conductivity and can contain a silicon-containing compound that constitutes the active material layer 2. In that case, in addition to the electrolytic medium 6 described above, it contains the silicon-containing compound of the present invention. <Voltage application process> The voltage application step is a step of applying a voltage between the positive electrode extraction member 13 and the negative electrode extraction member 14 of the in-progress electrode laminate.

[0125] The voltage application process causes the silicon-containing compound in the interface electrolyte to be laminated on the shell film 41 of the in-progress electrode laminate, forming an active material layer 2, and forming an electrode laminate 5 having a positive electrode portion 10 and a negative electrode portion 11.

[0126] In this step, the voltage applied between the positive electrode extraction member 13 and the negative electrode extraction member 14 is a voltage at which the silicon-containing compound in the interface electrolyte precipitates on the surface of the shell film 41, and is preferably 4.5 V or more and 5 V or less with respect to the lithium dissolution and deposition potential. <Electrolytic medium injection process> The electrolytic medium injection step is a step of discharging the interface electrolyte from inside the exterior body 3 as necessary and injecting the electrolytic medium 6 into the exterior body 3 of the battery assembly 2 . <Aging process> The aging process is a process for checking the initial deterioration of the battery assembly 2, and is made up of an initial charging operation process and a curing operation process.

[0127] The initial charging operation step is a step of applying a voltage between the positive electrode take-out member 13 and the negative electrode take-out member 14 of the electrode laminate 5 to charge it.

[0128] The curing step is a step of curing the exterior body 3 to seal the electrode laminate 5 and the electrolytic medium 6.

[0129] According to the Li-ion secondary battery 1 of this embodiment, the coating 41, 141 covering the active material particles 40, 140 contains a phosphate ion-containing Li compound, and preferably the shell film 41 contains one or more metals selected from the group consisting of Fe, Mn, Si, and Al, more preferably the shell film 41 uniformly covers the active material particles 40, 140, and even more preferably the active material layer 2 is present, so that the area of ​​contact between the active material particles 40, 140 and the non-aqueous electrolyte 5 is reduced, and gas generation due to decomposition of the electrolytic medium 6 can be suppressed.

[0130] According to the Li-ion secondary battery 1 of this embodiment, the active material layer 2 preferably has a conductive network 80 and a permeable pore network 81, which facilitates the exchange of charges and Li ions between the electrolytic medium 6 and the active material particles 40, 140, making it easier for electrode reactions to occur.

[0131] According to the Li-ion secondary battery 1 of this embodiment, the permeable pore network 81 preferably has a Li-ion conductor provided from the contact portion with the active material particles 40, 140 or the shell membrane 41 toward the pores, so that the exchange of charges and Li ions between the electrolytic medium 6 and the active material particles 40, 140 becomes smoother, making it easier for the electrode reaction to occur.

[0132] According to the Li-ion secondary battery 1 of this embodiment, the active material layer 2 has a silicon-containing compound film containing elemental silicon, so that the binding property of the active material layer 2 is improved and cracks and the like are less likely to occur.

[0133] According to Li-ion secondary battery 1 of the present embodiment, shell film 41 contains Li element, and the Li in shell film 41 can be used to replenish Li consumed for some reason, so that performance is less likely to deteriorate.

[0134] According to the Li-ion secondary battery 1 of this embodiment, the elution of Mn from the positive electrode active material particles 40 into the electrolytic medium 6 can be suppressed, and therefore the performance is less likely to deteriorate.

[0135] In the above-described embodiment, the active material layer 2 is formed by injecting the interface electrolyte in the interface electrolyte injection step and applying a voltage between the positive electrode extraction member 13 and the negative electrode extraction member 14 in the voltage application step, but the present invention is not limited to this.

[0136] For example, a silicon-containing compound containing elemental silicon may be added to the slurry in the paste application step, and active material layer 2 may be formed in the paste-applied current collector firing step.

[0137] Alternatively, after the paste-applied current collector firing step, a paste containing a silicon-containing compound may be applied to the in-progress positive electrode part and in-progress negative electrode part, and the active material layer 2 may be formed by solidifying the paste by heating, ultraviolet light, or the like.

[0138] After the electrode laminate formation step, the active material layer 2 may be formed by applying a paste containing a silicon-containing compound to the in-progress electrode laminate and solidifying it by heating, ultraviolet light, or the like.

[0139] In the above embodiment, the buffer section 42 is formed, but the present invention is not limited to this, and it is not necessary to form the buffer section 42. In this case, the battery assembly fabrication step, the interface electrolyte injection step, and the voltage application step are omitted, and the electrolytic medium injection step is performed after the battery assembly fabrication step.

[0140] In the above-described embodiments, each component may be freely substituted or added between the respective embodiments as long as it falls within the technical scope of the present invention. EXAMPLES

[0141] The present invention will be described in detail below with reference to examples. Note that the present invention is not limited to the following examples, and can be practiced with appropriate modifications within the scope of the present invention.

[0142] (Experimental Example 1) (i) Preparation of the positive electrode First, a certain amount of ethanol as a solvent was mixed with lithium manganese phosphate (hereinafter also referred to as LMP) powder with an olivine crystal structure, and the mixture was treated in a planetary ball mill for 3 hours using zirconia balls with a diameter of 0.5 mm. After the treatment, the zirconia balls were removed from the mixture using a sieve, and the mixture was dried at 120°C to remove the ethanol, obtaining LMP fine powder. Next, the LMP fine powder was mixed with ethanol to obtain a slurry with a solid content of 16.4 wt%, in which the LMP fine powder was dispersed in ethanol.

[0143] As the positive electrode active material, spinel-type lithium nickel manganese oxide (LiNi0.5Mn1.5O4, hereinafter also referred to as LNMO) with a median diameter of 5 μm was used.

[0144] 30 g of LNMO was put into a grinding mill (manufactured by Hosokawa Micron Corporation, product name: Nobilta), and while rotating with a clearance of 0.6 mm, rotor load power of 1.5 kW, and 2600 rpm, an ethanol dispersion slurry of LMP fine powder was added in two portions so that the amount of LMP fine powder added was 0.6 wt%. Then, the rotor rotation speed was kept in the range of 2600 rpm to 3000 rpm, and the mixture was treated at room temperature in an air atmosphere for 10 minutes to obtain LNMO with a surface coated with LMP. The obtained surface-coated LNMO was heat-treated at 350°C for 1 hour to obtain a positive electrode composite active material.

[0145] A mixture containing the obtained positive electrode composite active material, acetylene black as a conductive material, and polyvinylidene fluoride (PVdF) as a binder at solid concentrations of 90 parts by weight, 6 parts by weight, and 4 parts by weight, respectively, was dispersed in N-methyl-2-pyrrolidone (NMP) to prepare a slurry. Note that the binder was prepared by adjusting the solid concentration to 5% by weight in N-methyl-2-pyrrolidone (NMP) solution, and NMP was further added to adjust the viscosity to facilitate coating, which will be described later.

[0146] The slurry was applied to an aluminum foil having a thickness of 20 μm, and then dried in an oven at 120° C. This operation was performed on both sides of the aluminum foil, and then the aluminum foil was further vacuum-dried at 170° C. to prepare a positive electrode.

[0147] (ii) Preparation of the negative electrode Spinel-type lithium titanate (Li4Ti5O12, hereinafter also referred to as LTO) was used as the negative electrode active material. A mixture containing 100 parts by weight, 5 parts by weight, and 5 parts by weight of the LTO, acetylene black as a conductive assistant, and polyvinylidene fluoride (PVdF) as a binder, respectively, in solid content concentrations, was dispersed in N-methyl-2-pyrrolidone (NMP) to prepare a slurry. The binder was prepared as an NMP solution with a solid content concentration of 5 wt%, and NMP was further added to adjust the viscosity to facilitate coating, which will be described later.

[0148] The slurry was applied to an aluminum foil having a thickness of 20 μm, and then dried in an oven at 120° C. This operation was performed on both sides of the aluminum foil, and then the aluminum foil was further vacuum-dried at 170° C. to prepare a negative electrode.

[0149] (iii) Fabrication of lithium-ion secondary batteries A battery was fabricated using the positive and negative electrodes prepared in (i) and (ii) above and a 20 μm polypropylene separator according to the following procedure.

[0150] First, the positive and negative electrodes were dried under reduced pressure at 80°C for 12 hours. Next, 15 positive electrodes and 16 negative electrodes were stacked in the order of negative electrode / separator / positive electrode. The outermost layers of both were separators. Next, aluminum tabs were vibration welded to the positive and negative electrodes at both ends.

[0151] Two sheets of aluminum laminate film were prepared as exterior materials, and a depression to become a battery portion and a depression to become a gas collecting portion were formed by pressing, after which the electrode laminate was inserted.

[0152] The outer periphery, leaving a space for injecting the non-aqueous electrolyte, was heat-sealed at 180°C for 7 seconds, and LiPF6 was dissolved in a solvent prepared by mixing ethylene carbonate, propylene carbonate, and ethyl methyl carbonate in a volumetric ratio of ethylene carbonate / propylene carbonate / ethyl methyl carbonate = 15 / 15 / 70, at a ratio of 1 mol / L, and the non-aqueous electrolyte was then poured into the unsealed area, and the unsealed area was heat-sealed at 180°C for 7 seconds while reducing the pressure.

[0153] The obtained battery was charged at a constant current of 0.2 C until the battery voltage reached a cut-off voltage of 3.4 V, and then the charging was stopped. After that, the battery was left to stand in an environment of 60°C for 24 hours, and then discharged at a constant current of 0.2 C. When the battery voltage reached 2.5 V, the discharge was stopped. After the discharge was stopped, the gas accumulated in the gas collector was removed and the battery was resealed. A lithium-ion secondary battery for evaluation was produced by the above operations.

[0154] (Experimental Example 2) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 1 was carried out except that the coating amount of the LMP fine powder was adjusted to 0.9 wt %, and this was designated Experimental Example 2.

[0155] (Experimental Example 3) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 1 was carried out except that the coating amount of the LMP fine powder was adjusted to 1.5 wt %, and this was designated Experimental Example 3.

[0156] (Experimental Example 4) (i) In preparing the positive electrode, the same procedure as in Experimental Example 1 was repeated except that LiFePO4 (hereinafter also referred to as LFP) having an olivine type crystal structure was used instead of the LMP fine powder, and the coating amount of the LFP fine powder was adjusted to 1.2 wt %. This was designated Experimental Example 4.

[0157] (Experimental Example 5) (i) In producing the positive electrode, the same procedure as in Experimental Example 4 was carried out except that the coating amount of the LFP fine powder was adjusted to 2.4 wt %, and this was designated Experimental Example 5.

[0158] (Experimental Example 6) (i) In preparing the positive electrode, Li1.3Al0.3Ti1.7(PO4)3 (hereinafter also referred to as LATP) was used instead of LMP, and the coating amount of LATP fine powder was adjusted to 1.2 wt %, except that the procedure was the same as in Example 4. This was designated as Example 6.

[0159] The LATP fine powder was prepared by the following method.

[0160] As starting materials, Li2CO3, AlPO4, TiO2, NH4H2PO4, and ethanol as a solvent were mixed in a predetermined amount and treated with a planetary ball mill at 150G for 1 hour using zirconia balls with a diameter of 3 mm. After removing the zirconia balls from the treated mixture with a sieve, the mixture was dried at 120°C to remove the ethanol. After that, it was treated at 800°C for 2 hours to obtain LATP fine powder.

[0161] (Experimental Example 7) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 4 was carried out except that the coating amount of the LATP fine powder was adjusted to 2.4 wt %, and this was designated Experimental Example 7.

[0162] (Experimental Example 8) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 1 was conducted except that the surface-coated LNMO was heat-treated at 450° C. for 1 hour to obtain a positive electrode composite active material, which was designated Experimental Example 8.

[0163] (Experimental Example 9) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 1 was conducted except that the surface-coated LNMO was heat-treated at 800° C. for 1 hour to obtain a positive electrode composite active material, which was designated as Experimental Example 9.

[0164] (Experimental Example 10) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 2 was conducted except that the surface-coated LNMO was heat-treated at 450° C. for 1 hour to obtain a positive electrode composite active material, which was designated Experimental Example 10.

[0165] (Experimental Example 11) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 2 was conducted except that the surface-coated LNMO was heat-treated at 800° C. for 1 hour to obtain a positive electrode composite active material, which was designated Experimental Example 11.

[0166] (Experimental Example 12) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 1 was conducted except that the surface-coated LNMO was heat-treated at 350° C. for 2 hours to obtain a positive electrode composite active material, which was designated Experimental Example 12.

[0167] (Experimental Example 13) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 2 was conducted except that the surface-coated LNMO was heat-treated at 350° C. for 2 hours to obtain a positive electrode composite active material, which was designated Experimental Example 13.

[0168] (Experimental Example 14) (i) In the preparation of the positive electrode, the amount of LATP fine powder coated was adjusted to 1.2 wt %, and the surface-coated LNMO was heat-treated at 400° C. for 1 hour to obtain a positive electrode composite active material.

[0169] (ii) In the preparation of the negative electrode, following the preparation of the positive electrode (i), LTO was used as the active material of the negative electrode, and 30 g of LTO was put into a grinding mill, and while rotating with a clearance of 0.6 mm, a rotor load power of 1.5 kW, and 2600 rpm, an ethanol dispersion slurry of LMP fine powder was added in two portions so that the amount of LMP fine powder added was 2.4 wt%. Then, the rotor rotation speed was kept in the range of 2600 rpm to 3000 rpm, and the treatment was performed at room temperature in an air atmosphere for 10 minutes to obtain LTO whose surface was coated with LMP. The obtained surface-coated LTO was heat-treated at 350°C for 1 hour to obtain a negative electrode composite active material.

[0170] A mixture containing the obtained negative electrode composite active material, acetylene black as a conductive material, and polyvinylidene fluoride (PVdF) as a binder at solid concentrations of 90 parts by weight, 6 parts by weight, and 4 parts by weight, respectively, was dispersed in N-methyl-2-pyrrolidone (NMP) to prepare a slurry. Note that the binder was prepared by adjusting the solid concentration to 5% by weight in N-methyl-2-pyrrolidone (NMP) solution, and NMP was further added to adjust the viscosity to facilitate coating, which will be described later.

[0171] The slurry was applied to an aluminum foil having a thickness of 20 μm, and then dried in an oven at 120° C. This operation was performed on both sides of the aluminum foil, and then the aluminum foil was further vacuum-dried at 170° C. to prepare a negative electrode.

[0172] Other than the above, the same procedure as in Experimental Example 6 was repeated, and this was designated Experimental Example 14.

[0173] (Experimental Example 15) (ii) In the preparation of the negative electrode, the surface-coated LTO was heat-treated at 600° C. for 1 hour to obtain a negative electrode composite active material. The procedure was the same as in Experimental Example 14, except that this was used as Experimental Example 15.

[0174] (Experimental Example 16) (ii) In producing the negative electrode, the same procedure as in Experimental Example 14 was repeated except that LFP was used instead of LMP and the amount of LFP fine powder coated was adjusted to 2.4 wt %. This was designated Experimental Example 16.

[0175] (Experimental Example 17) (ii) In the preparation of the negative electrode, the same procedure as in Experimental Example 16 was conducted except that the surface-coated LTO was heat-treated at 600° C. for 1 hour to obtain a negative electrode composite active material, which was designated Experimental Example 17.

[0176] (Experimental Example 18) (i) In the preparation of the positive electrode, the same procedure as in Experimental Example 1 was conducted except that LNMO was used as it was without forming a coating, and this was designated Experimental Example 18.

[0177] That is, in Experimental Example 18, LNMO was used for the positive electrode, and LTO was used for the negative electrode.

[0178] (Gas generation rate measurement) The amount of gas generated from the lithium ion secondary battery before and after the cycle characteristics evaluation in each of Experimental Examples 1 to 18 was evaluated using the Archimedes method, that is, the buoyancy of the lithium ion secondary battery. The evaluation was performed as follows.

[0179] First, the weight of the lithium-ion secondary battery was measured using an electronic balance. Next, the weight in water was measured using a specific gravity meter (manufactured by Alpha Mirage, product number: MDS-3000), and the buoyancy was calculated by taking the difference between these weights. The volume of the lithium-ion secondary battery was calculated by dividing the buoyancy by the density of water (1.0 g / cm3). The amount of gas generated was calculated by comparing the volume after aging with the volume after the cycle characteristic evaluation described below.

[0180] (Evaluation of cycle characteristics of lithium-ion secondary batteries) The lithium ion secondary batteries prepared in each of Experimental Examples 1 to 18 were connected to a charge / discharge device (HJ1005SD8, manufactured by Hokuto Denko Corporation) and cycle operation was performed. In an environment of 60°C, constant current charging was performed at a current value equivalent to 1.0 C until the battery voltage reached the final voltage of 3.4 V, and charging was then stopped. Subsequently, constant current discharging was performed at a current value equivalent to 1.0 C, and discharging was stopped when the battery voltage reached 2.5 V. This constituted one cycle, and charging and discharging were repeated.

[0181] The stability of the cycle characteristics was evaluated as the capacity retention rate (%) of the 500th discharge capacity when the first discharge capacity was taken as 100.

[0182] (Rate characteristic evaluation) The lithium ion secondary batteries produced in each of Experimental Examples 1 to 18 were charged and discharged at 25° C. and 0.2 C, and then continuously charged and discharged at 2.0 C to evaluate the rate characteristics.

[0183] The end-of-charge voltage and the end-of-discharge voltage were set to 2.5 V and 3.4 V, respectively. The ratio of the discharge capacity at 2.0 C to the discharge capacity at 0.2 C was defined as the discharge rate characteristic.

[0184] First, the evaluation results of each of Experimental Examples 1 to 7 are shown in Table 1.

[0185] [Table 1] As shown in Table 1, in Experimental Examples 1 to 7 in which a coating was formed, the amount of gas generated after 100 cycles was suppressed to 10 cc / Ah or less in all cases.

[0186] This suggests that the formation of a coating film has the effect of suppressing gas generation (hereinafter also referred to as gas generation suppression effect).

[0187] As shown in Table 1, in Experimental Examples 1 to 3 in which LMP was used as the coating, the rate characteristics were improved compared to Experimental Examples 4 and 5 in which LFP was used as the coating and Experimental Examples 6 and 7 in which LATP was used.

[0188] In Experimental Examples 4 and 5, where LFP was used as the coating, and Experimental Examples 6 and 7, where LATP was used, as the amount of LATP added increased, the initial capacity decreased, the 2C value also decreased, and the amount of gas generated decreased. On the other hand, in Experimental Examples 1 to 3, where LMP was used as the coating, as the amount of LMP added increased, the initial capacity increased, the 2C value remained almost constant, and the amount of gas generated increased.

[0189] This suggests that when LMP is used as the coating, the capacity is maintained even if a small amount of coating is added, and the effect of suppressing gas generation is high.

[0190] Next, the evaluation results of each of Experimental Examples 1, 2, and 8 to 11 are shown in Table 2.

[0191] [Table 2] In each of Experimental Examples 1, 2, and 8 to 11, as shown in Table 2, the amount of gas generated after 100 cycles was kept below 10 cc / Ah. Although there was concern that cracks might occur as the treatment temperature increased, no clear increase in the amount of gas generated was observed even when heat treatment was performed at 800 degrees.

[0192] Furthermore, when comparing Experimental Examples 1, 8, and 9 in which the amount added was 0.6 wt%, the initial capacity and 2C value increased as the treatment temperature increased.

[0193] Similarly, when comparing Experimental Examples 2, 10, and 11 in which the amount added was 0.9 wt%, the initial capacity and 2C value increased as the treatment temperature increased.

[0194] These results suggest that increasing the treatment temperature increases the initial capacity and 2C value while suppressing gas generation.

[0195] Next, the evaluation results of each of Experimental Examples 1, 2, 12, and 13 are shown in Table 3.

[0196] [Table 3] As shown in Table 3, in each of Experimental Examples 1, 2, 12, and 13, the amount of gas generated after 100 cycles was suppressed to 10 cc / Ah or less.

[0197] In Experimental Examples 1 and 12, in which the amount of coating added was 0.6 wt %, there was almost no change in the amount of gas generated after 100 cycles and after 300 cycles with an increase in treatment time.

[0198] In Experimental Examples 1 and 12, in which the coating amount was 0.6 wt%, the amount of gas generated after 300 cycles was smaller than in Experimental Examples 2 and 13, in which the coating amount was 0.9 wt%.

[0199] In addition, in Experimental Examples 1, 2, 12, and 13, the initial capacity and the 2C value increased with an increase in the treatment time.

[0200] These results suggest that extending the treatment time improves the uniformity of the coating and the gas suppression effect. It also suggests that extending the treatment time restores the initial capacity, and that the effect of the coating is enhanced by adding a small amount of the compound and coating thinly.

[0201] Next, the evaluation results of each of Experimental Examples 14 to 18 are shown in Table 4.

[0202] [Table 4] In each of Experimental Examples 14 to 17 in which a coating was formed, the rate characteristics were almost the same as in Experimental Example 18 in which a coating was not formed, but the amount of gas generated after 500 cycles was reduced to 35 cc / Ah or less, and the capacity retention rate was also improved.

[0203] This suggests that the gas generation suppression effect can be obtained by forming a coating on the negative electrode as well.

[0204] Moreover, when comparing Experimental Examples 14 and 15, the rate characteristics improved as the treatment temperature increased. Similarly, when comparing Experimental Examples 16 and 17, the rate characteristics improved as the treatment temperature increased.

[0205] This suggests that the rate characteristics can be improved by increasing the treatment temperature.

[0206] In Experimental Examples 14 and 15, in which LMP was coated, the amount of gas generated was reduced and the rate characteristics were improved compared to Experimental Examples 16 and 17, in which LFP was coated.

[0207] From the above, it was found that the amount of gas generation can be suppressed by coating the surface of the active material particles with a film containing a lithium compound containing phosphate ions.

[0208] In particular, it was found that by coating the surface of the active material particles with LMP, the amount of gas generation could be suppressed and the rate characteristics were improved. [Explanation of symbols]

[0209] 1 Li-ion secondary battery 2 Active material layer 21 Positive electrode active material layer 3 Exterior body 5 Electrode laminate 6 Electrolytic medium (electrolyte) 10 Positive electrode 11 Negative electrode 12 Separator 13 Positive electrode removal member 14 Negative electrode removal member 20 Positive electrode current collector 120 Negative electrode current collector 30 Active material particles 130 Coated active material particles (coated active material particles for Li-ion secondary batteries) 35 Coating 36 Core-shell particles 40 Positive electrode active material particles 140 Negative electrode active material particles 41 Shell Membrane 42 Buffer section 60 Marine part 61 Island 70 Binder 80 Conductive Network 81 Permeable Pore Network

Claims

1. A lithium ion secondary battery in which an electrode stack having a positive electrode and a negative electrode facing each other with an electrolytic medium sandwiched therebetween is enclosed in an exterior body, the positive electrode and the negative electrode each include a current collector on which an active material layer containing coated active material particles is formed, as a current collector with an active material layer; The coated active material particles are formed by coating the active material particles with a coating film containing Li ions, The positive electrode coating Li ion average concentration, which is the average concentration of the Li ions in the positive electrode coating, which is the coating of the positive electrode, is a negative electrode coating average Li ion concentration, which is an average concentration of Li ions in the negative electrode coating, which is the coating of the negative electrode, is different from an average negative electrode coating Li ion concentration.

2. The coating is, from the active material particle side, The active material particles constitute a core, and a continuous shell film constitutes a shell. The shell film of a core-shell particle having a core-shell structure, and The outer surface of the core-shell particle A buffer portion formed over the entire outer surface of the shell membrane, The entire surface may include a non-forming region, and the formed region may include It consists of a buffer section, The positive electrode shell film Li ion average concentration, which is the average concentration of the Li ions in the positive electrode shell film, which is the shell film of the positive electrode, The lithium ion secondary battery according to claim 1 , wherein the negative electrode shell film Li ion average concentration is different from the average concentration of the Li ions in the negative electrode shell film, which is the shell film of the negative electrode.

3. The positive electrode buffer Li ion average concentration, which is the average concentration of the Li ions in the positive electrode buffer, which is the buffer of the positive electrode, is The lithium ion secondary battery according to claim 2 , wherein the average Li ion concentration of the negative electrode buffer portion, which is the buffer portion of the negative electrode, is different from the average Li ion concentration of the negative electrode buffer portion.

4. 4. The lithium ion secondary battery according to claim 2, wherein the ratio of the non-forming region / the entire region, averaged over the number of the active material particles, is 0.001 or more and 0.3 or less.

5. The lithium ion secondary battery according to any one of claims 2 to 4, The shell film is a phosphate ion-containing lithium compound containing one or more metals selected from the group consisting of Fe, Mn, Si, and Al.

6. The lithium ion secondary battery according to any one of claims 1 to 4, The active material particles of the negative electrode include lithium titanate.

7. The lithium ion secondary battery according to any one of claims 1 to 4, The active material particles of the positive electrode include lithium nickel manganese oxide.

8. A method for producing a lithium ion secondary battery according to any one of claims 2 to 7, comprising the steps of: On the current collector, a positive electrode active material layer including positive electrode active material particles formed on the positive electrode active material layer-attached current collector A; and A negative electrode active material layer containing negative electrode active material particles is formed to obtain a current collector A with a negative electrode active material layer. A process for producing a current collector A with an active material layer; At least one pair of the positive electrode current collector A and the negative electrode current collector A is disposed opposite to each other, An electrode laminate A manufacturing process for manufacturing an electrode laminate A; The electrode laminate A is immersed in an electrolyte solution B under conditions B. As a buffer section B which is a part of the buffer section, A current collector B with a positive electrode active material layer including a positive electrode buffer portion B, and A current collector B with a negative electrode active material layer including a negative electrode buffer portion B is formed, An electrode stack B manufacturing process for manufacturing an electrode stack B including a buffer portion B; The electrode laminate B is immersed in an electrolytic solution C under conditions C. As a buffer portion C which is a part of the buffer portion, A current collector C with a positive electrode active material layer including a positive electrode buffer portion C, and A current collector C having a negative electrode active material layer including a negative electrode buffer portion C is formed, An electrode stack C manufacturing process for manufacturing an electrode stack C including a buffer portion C, Regarding the positive electrode buffer part and the negative electrode buffer part, which are the buffer parts of the positive electrode and the negative electrode, The thickness of the positive electrode buffer part B in the positive electrode buffer part: the thickness of the negative electrode buffer part B in the negative electrode buffer part, and The thickness of the positive electrode buffer part C in the positive electrode buffer part: the thickness of the negative electrode buffer part C in the negative electrode buffer part, The thickness of the buffer portion formed under each condition for the positive electrode and the negative electrode is Between the conditions, the positive electrode and the negative electrode are formed thicker on one side and thinner on the other side, The method for producing an electrode laminate for a lithium ion secondary battery, wherein the ratio is less than 10:5 or less than 5:10.

Citation Information

Patent Citations

  • Electrode group, nonaqueous electrolyte secondary battery, battery pack and vehicle

    JP2021051987A