Base fabric for airbag and production method of the same
Patent Information
- Application Number
- JP2024119354
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-10-13
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-10-13
AI Technical Summary
Existing airbag fabrics face challenges in maintaining consistent flame retardancy and combustion characteristics regardless of the coated surface, especially when exposed to outdoor environmental conditions, with increased combustion rates observed on the resin-coated surface during flammability evaluations.
A polyamide multifilament fabric with a silicone film layer on at least one side, controlled cyclopentanone content, and specific dimensional stability properties, along with precise manufacturing processes to ensure uniform flame retardancy and reduced combustion rates.
The airbag fabric maintains stable flame retardancy and reduced combustion rates on both coated and non-coated surfaces, even after exposure to harsh environmental conditions, ensuring consistent performance in airbags installed both inside and outside the vehicle cabin.
Abstract
Description
[Technical field]
[0001] The present invention relates to an airbag base fabric used in an airbag related to automobile safety. [Background technology]
[0002] As described in Patent Document 1 below, it is known that when a moving vehicle hits a pedestrian, the lower half of the pedestrian's body is swept away by the front of the vehicle body, causing a secondary collision with the upper surface of the hood at the front of the vehicle body, and there is also a need for protection against collisions with the highly rigid front pillars on both side edges of the windshield glass that rise from the upper surface of the hood. Therefore, as described in the following Patent Document 2, the pedestrian airbag device is folded and stored in a retainer case attached to a support member that is installed between left and right vehicle body members in the upper rear part of the engine compartment. Furthermore, the following Patent Document 3 discloses that an airbag, which has conventionally been used to protect occupants in the event of a vehicle collision, can also be used to protect pedestrians.
[0003] These airbags that are deployed outside the vehicle are required to have the specific durability required for being installed outside the vehicle in addition to the characteristics required for conventional airbags installed inside the vehicle, such as for the driver's seat and passenger seat. That is, they need to be able to withstand outdoor environmental conditions and working conditions for maintaining the performance of the vehicle, such as light, ultraviolet rays, heat, rain, snow, low temperatures, hot and cold water, oil and solvents, detergents, dust, etc. In particular, if the airbag is not stored in a sealed, sturdy container, or if the sealed container is damaged, the impact of these environmental factors becomes significant.
[0004] In response to this, for example, Patent Document 4 below discloses providing a covering material on the outer surface of the base fabric of the bag body.
[0005] In addition, in the following Patent Document 5, the coating amount is 20 g / m 2In order to obtain an airbag base fabric that is lightweight and can maintain air permeability and flame retardancy before and after heat resistance tests and moisture resistance tests, it is disclosed that the fabric is coated only with a specific water-soluble resin. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 7-108903 [Patent Document 2] JP 2018-172006 A [Patent Document 3] JP 2006-205805 A [Patent Document 4] JP 2004-115981 A [Patent Document 5] JP 2001-214371 A Summary of the Invention [Problem to be solved by the invention]
[0007] Due to the diversification of conditions under which airbags are used, such as inside and outside the vehicle, it is desirable for the airbag fabric to have excellent flame retardancy regardless of whether it is the front or back side that is used as the outer surface. Here, in the standard for flammability evaluation (FMVSS302), the sample is held horizontally and ignited with the surface exposed to the passenger compartment facing down. Therefore, the fabric side (opposite the resin-coated side), which is the outer surface of the airbag fabric, is usually evaluated with the resin-coated side facing down. When the resin-coated side is the outer surface of the airbag fabric, ignition is performed with the resin-coated side facing down, but ignition of the resin-coated side increases the burning rate. Furthermore, for airbags that are installed and deployed outside the passenger compartment, flame retardancy after exposure to outdoor environmental conditions is desirable.
[0008] Patent Document 4 does not fully consider the fire retardancy when the resin-coated surface is used as the outer surface of an airbag base fabric, nor the fire retardancy after exposure to outdoor environmental conditions. Patent Document 5 does not consider the flame retardancy of both the front and back surfaces of the airbag base fabric.
[0009] Therefore, the problem to be solved by the present invention is an airbag base fabric in which flammability is suppressed both in the case of ignition of the resin-coated surface and the case of ignition of the non-coated surface in the flammability evaluation defined by FMVSS302 after the environmental resistance test. The problem is to provide a base fabric. [Means for solving the problem]
[0010] The present invention relates to a base fabric for airbags made of a coated woven fabric, which has specific chemical properties and is thermally dimensionally stable, thereby making the combustion characteristics less susceptible to environmental influences. This has led to the creation of the present invention.
[0011] That is, the present invention is as follows. [1] An airbag fabric which is a polyamide multifilament woven fabric, The fabric has a layer of silicone membrane on at least one side thereof; The amount of silicone film is 10g / m 2 More than 100g / m 2 is as follows: The content of cyclopentanones is 0 ppm or more and 250 ppm or less based on the weight of the fabric, The larger of the shrinkage dimensional change rates in the warp and weft directions before and after heating at 105°C for 60 minutes is 0% or more and 1.4% or less, and An airbag fabric having a blade combing resistance of 350 N or more after 400 hours under an environment of 85°C and 95% relative humidity. [2] The airbag fabric according to [1], wherein the amount of oil component contained in the woven fabric is 0% by weight or more and 0.04% by weight or less. [3] The airbag fabric according to [1] or [2], containing phosphorus atoms in an amount of 10 ppm or more and 300 ppm or less based on the weight of the constituent yarns of the fabric. [4] The airbag fabric according to any one of [1] to [3] above, wherein the amount of carboxylic acid terminals at the molecular chain terminals of the polyamide exceeds the amount of amine terminals, the difference being 10 millimole equivalents / kg or more and 50 millimole equivalents / kg or less. [5] In a combustion test according to FMVSS302 after 400 hours at 80°C and 95% humidity, the following 1) or 2): 1) Self-extinguishing regardless of whether the fire is ignited from the front or back of the base fabric. 2) The airbag fabric according to any one of [1] to [4] above, wherein the burning rates on both sides of the fabric are 100 mm / min or less, and the ratio of the burning rates on both sides is 1.0 or more and 3.0 or less. [6] The following steps: A step of melt spinning a polyamide to obtain a polyamide multifilament yarn having a cyclopentanone content of 0 ppm or more and 800 ppm or less; A step of obtaining a woven fabric by weaving the obtained polyamide multifilament yarn; A refining process using an alkaline cleaning solution at a temperature of 35°C or higher; drying process, applying silicone to at least one surface of the fabric to form a layer of silicone membrane; and Vulcanization setting process, A method for producing a polyamide multifilament woven airbag fabric, comprising: [7] The method for producing an airbag fabric according to [6], wherein in the scouring step, rinsing with water is performed after the treatment bath of the alkaline cleaning solution or surfactant. [8] The method for producing an airbag fabric according to [6] or [7], wherein in the refining step, the warp tension of the fabric conveyance is 0.08 N / cm or more and 0.8 N / cm or less. [9] The method for producing an airbag fabric according to any one of [6] to [8], wherein in the vulcanization setting step, vulcanization setting is performed at a temperature of 160° C. or higher with a warp overfeed of 0.8% or more. Effect of the Invention
[0012] The airbag fabric of the present invention has a small difference in flammability evaluation between the coated side and the non-coated side, and is excellent in maintaining flame retardancy after environmental resistance testing. This fabric provides an airbag cushion that is particularly suitable for an airbag device that is installed outside the passenger compartment and is subject to severe environmental changes. [Brief description of the drawings]
[0013] [Figure 1] These are the structural formulas of compounds a) to d). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present invention will be described in detail. One embodiment of the present invention is an airbag fabric made of a polyamide multifilament woven fabric, The fabric has a layer of silicone membrane on at least one side thereof; The amount of silicone film is 10g / m 2 More than 100g / m 2 is as follows: The content of cyclopentanones is 0 ppm or more and 250 ppm or less based on the weight of the fabric, The larger of the shrinkage dimensional change rates in the warp and weft directions before and after heating at 105°C for 60 minutes is 0% or more and 1.4% or less, and This is an airbag fabric characterized by having a blade combing resistance of 350 N or more after 400 hours in an environment of 85°C and 95% relative humidity.
[0015] The yarns constituting the airbag fabric are long fibers made of polyamide multifilaments. Polyamide fibers have a high melting point and a large heat capacity, so they have excellent resistance to bursting due to melting when the airbag is deployed with explosives. Furthermore, they have excellent adhesion to coating films due to the presence of amide groups and amino or carboxyl groups at the polymer end groups. Examples of polyamides include polyamide 6, polyamide 6·6, polyamide 11, polyamide 12, polyamide 6·10, polyamide 6·12, polyamide 4·6, and fibers made of their copolymers and mixtures. Among them, polyamide 6·6 fibers made mainly of polyhexamethylene adipamide are preferred. Polyhexamethylene adipamide refers to a polyamide made of 100% hexamethylene diamine and adipic acid with a melting point of 250°C or higher. The polyamide 6·6 fiber of the present invention may include fibers made of a polymer obtained by copolymerizing or blending polyhexamethylene adipamide with polyamide 6, polyamide 6·I, polyamide 6·10, polyamide 6·T, etc., so long as the melting point is not less than 250°C.
[0016] <Multifilament> The fineness of the yarn constituting the base fabric is preferably 150 dtex or more and 750 dtex or less. If it is 150 dtex or more, it has excellent mechanical properties when woven into a material-use fabric. If it is 750 dtex or less, when weaving at high speed of 800 rpm or more with a shuttleless loom, the conveying weight is not too heavy when inserting the weft yarn and there is no problem in productivity. It is more preferably 220 dtex or more, more preferably 550 dtex or less, and even more preferably 450 dtex or less. In this embodiment, the yarn constituting the base fabric is a multifilament consisting of a bundle of single yarns, and the single yarn preferably has a fineness of 1 dtex or more and 7 dtex or less. If the single yarn fineness is 1 dtex or more, there is little deterioration of mechanical properties during processing from the weaving yarn to the base fabric, and if it is 7 dtex or less, there is good microscopic adhesion with the coating film, which is preferable for suppressing the burning rate and stabilizing the behavior. Furthermore, the base fabric has good flexibility and is easy to store when made into an airbag. The cross-sectional shape of the single yarn may be round or irregular.
[0017] The degree of filling of the base fabric can be expressed by the cover factor, which is the degree of filling within a plane. The cover factor is calculated from the fineness and weave density of the constituent yarns of the base fabric. The cover factor CF is calculated by adding up the warp direction (w) and weft direction (f) based on the fineness d (dtex) of the constituent yarns and the weave density D (threads / 2.54 cm). CF=(√(dw)×Dw)+(√(df)×Df) In this embodiment, the cover factor is preferably 1,800 or more and 2,500 or less. If the cover factor is 1,800 or more and is large, the mechanical properties of the base fabric are good due to the weaving density effect, which is preferable. The cover factor is more preferably 2,000 or more. The smaller the cover factor is and is 2,500 or less, the less the constituting yarns are mixed together and the better the flexibility of the base fabric is. This is preferable because it has excellent storage properties as an airbag. The cover factor is more preferably 2,300 or less.
[0018] The airbag fabric of this embodiment has a silicone film layer on at least one side of the woven fabric. The silicone film may be a coating film or a laminated film. The amount of the silicone film is 10 g / m 2 More than 100g / m 2 The amount of silicone film is 10g / m 2 If it is equal to or more than this, it contributes to the airtightness of the airbag and further contributes to the suppression of combustion. More preferably, it is 15 g / m 2 The silicone amount is 100g / m 2 If the amount of the silicone film is less than 70 g / m, the base fabric is lightweight and easy to store. 2 More preferably 40 g / m or less 2 The following is the result.
[0019] The airbag fabric of this embodiment has a cyclopentanone content of 250 ppm or less based on the weight of the constituent yarn. Cyclopentanones refer to the compounds a) Cyclopentanon, b) Cyclopenten-1-one, c) 1,1'-Bicyclopentyl-2-one, and d) Cyclopentanone, 2-cyclopentylidene shown in FIG. 1, and the content of cyclopentanones is the total content of these compounds. If the amount of cyclopentanones is 250 ppm or less, the adhesion of the silicone layer is good and the increase in the burning rate after the moist heat environment is small. More preferably, the amount of cyclopentanones is 150 ppm or less, and most preferably, 50 ppm or less. The lower limit of the amount of cyclopentanones is preferably 0 ppm or more, and more preferably 10 ppm or more. Cyclopentanones inhibit the adhesion between polyamide and silicone, and weaken the adhesion especially after the moist heat environment. Cyclopentanone is derived from polyamide. Polyamide undergoes thermal degradation at its melting temperature, producing cyclopentanone. Any cyclopentanone that was not completely removed during the process from polyamide weaving to processing into base fabric remains in the base fabric. The cyclopentanone content can be analyzed by gas chromatography, but since cyclopentanone is partially dimerized, including during the analysis process, it is quantified as cyclopentanones. The amount of cyclopentanone content varies depending on the cyclopentanone content of the polyamide raw yarn used for weaving and the processing conditions when processing it into base fabric. In order to make the content of cyclopentanones in the woven fabric of the base fabric 250 ppm or less based on the weight of the constituent yarns, it is preferable to use an alkaline washing solution at a temperature of 35°C or higher in the scouring step after weaving. More preferably, it is used at a temperature of 60°C or higher. Furthermore, the content of cyclopentanones can be reduced by rinsing with neutral water after the alkaline washing solution. Moreover, the base fabric is relaxed in this scouring step, which promotes the penetration of the washing solution between the constituent yarns of the base fabric, thereby reducing the content of cyclopentanones.
[0020] The airbag fabric of this embodiment has a larger shrinkage dimensional change rate of 1.4% or less among the shrinkage dimensional change rates in the warp and weft directions at 105°C for 60 minutes. The thermal dimensional stability is low at 1.4% or less, and the smaller the value, the smaller the increase in burning rate after a humid and hot environment. The thermal dimensional stability is more preferably 1.0% or less, and even more preferably 0.8% or less. The thermal dimensional stability of the fabric changes due to the influence of heat setting at the final stage of fabric processing. Usually, the dimensional change is large in the warp direction and relatively small and stable in the weft direction, being 0.1% or less. In order to suppress the burning rate of the airbag base fabric, it is necessary to suppress the supply of combustion gas to the burning flame. The combustion gas is mainly composed of decomposition gas of polyamide, but when the base fabric is installed with the silicone layer facing up in the horizontal burning method, the supply of combustion gas to the burning flame on the top surface of the base fabric is suppressed by the flame-retardant silicone layer, which suppresses the gas migration to the top surface, and the burning rate is suppressed. On the other hand, when the base fabric is installed with the silicone layer facing down in the horizontal burning method, the supply of combustion gas to the burning flame on the top surface of the base fabric is not blocked, and the burning rate is high. In particular, after the moist heat environment, the silicone layer peels off and cracks due to the decrease in adhesion and the dimensional change (shrinkage) of the base fabric, and the silicone layer does not block the burning gas, so the burning rate increases further. Therefore, the low content of cyclopentanones and good dimensional stability can suppress the increase in the burning rate after the moist heat environment. In order to set the larger shrinkage dimensional change rate of 0 to 1.4% in the warp and weft directions before and after heating at 105°C for 60 minutes, it is preferable that the overfeed in the warp direction is 0.8% or more at a temperature of 160°C or higher in the vulcanization setting process after silicone application. More preferably, it is an overfeed process of 1.0% or more. An overfeed process of 8.0% or less is preferable because it allows stable processing.
[0021] The airbag fabric of this embodiment preferably has a blade combing resistance of 350N or more after a humid heat environment (400 hours under an environment of 85°C and 95% relative humidity). More preferably, it is 420N or more, and even more preferably, it is 470N or more. The blade combing resistance is the resistance of the constituent yarns of the fabric to slippage, and is a combination of the binding force of the constituent yarns of the fabric structure and the resistance of silicone adhesion. The higher the blade combing resistance is, at 350N or more, the better the adhesion of the silicone layer. This high blade combing resistance is one factor in suppressing the burning rate. On the other hand, if the blade combing resistance is 800N or less, the tear resistance is sufficiently high.
[0022] In the airbag fabric of this embodiment, the amount of oil agent contained in the woven fabric is preferably 0.04% by weight or less. The smaller the amount of oil agent, 0.04% by weight or less, the more sufficient the deoiling process in the scouring process is. The amount of oil agent contained in the woven fabric is more preferably 0.02% by weight or less. The small amount of oil agent provides good adhesion between the polyamide fiber and the silicone layer, and the reduced content of cyclopentanone contributes to improving adhesion and avoiding adhesion damage after a humid and hot environment. The weaving raw yarn contains about 1% processing oil, which can be removed by scouring after weaving. On the other hand, the amount of oil agent is preferably 0.005% by weight or more. The tear resistance is sufficiently high.
[0023] In the airbag fabric of this embodiment, the content of phosphorus atoms is preferably 10 ppm or more and 300 ppm or less based on the weight of the constituent yarn. The higher the content of phosphorus atoms, the more the combustion gas generation is suppressed, and the greater the combustion suppression effect. The content of phosphorus atoms is more preferably 30 ppm or more, and even more preferably 40 ppm or more. On the other hand, since phosphorus atoms may act as a catalyst poison for silicone crosslinking, there is an upper limit to the content. The content of phosphorus atoms is more preferably 200 ppm or less, and even more preferably 150 ppm or less. The phosphorus atom is derived from the catalyst used in the production of polyamide resin.As the catalyst, phosphoric acid compounds such as phosphoric acid, pyrophosphoric acid, polyphosphoric acid, phosphinic acid compounds such as dimethylphosphinic acid, phenylmethylphosphinic acid, hypophosphorous acid, sodium hypophosphite, ethyl hypophosphite, phosphonic acid compounds such as phenylphosphonous acid, sodium phenylphosphonite, ethyl phenylphosphonite, phosphonic acid compounds such as phenylphosphonic acid, ethylphosphonic acid, sodium phenylphosphonite, diethyl phenylphosphonite, sodium ethylphosphonite, phosphorous acid compounds such as phosphorous acid, sodium hydrogen phosphite, sodium phosphite, triethyl phosphite, triphenyl phosphite, pyrophosphorous acid, etc. can be added. The polyamide preferably contains phenylphosphonic acid or a metal salt thereof as a phosphorus component in an amount of 10 ppm to 300 ppm by weight of the polymer. Phenylphosphonic acid and the like are generally used as polymerization catalysts.
[0024] To obtain polyamide 6·6 containing phenylphosphonic acid or its metal salt, either phenylphosphonic acid or its metal salt may be added during solution polymerization, or phenylphosphinic acid or its metal salt may be added, since these will be oxidized to phenylphosphonic acid, etc. during the process. Either additive may be used. Additives may be introduced during the polymerization process. Examples of additives include antioxidants and heat stabilizers (hindered phenol compounds, hydroquinone compounds, thiazole compounds, phosphorus compounds such as phenylphosphonic acid, imidazole compounds such as 2-mercaptobenzimidazole, and their substitutes, copper halides, copper acetate and halogens, etc.), weathering agents (resorcinol, salicylate, benzotriazole, benzophenone, hindered amine, etc.), pigments (cadmium sulfide, phthalocyanine, carbon black, etc.), gloss improvers (titanium oxide, calcium carbonate, etc.), dyes (nigrosine, aniline black, etc.), crystal nucleating agents (talc, silica, kaolin, clay, etc.), plasticizers (p-oxybenzoyl chloride, etc.), and the like. The composition may contain small amounts of: antistatic agents (alkyl sulfate-type anionic antistatic agents, quaternary ammonium salt-type cationic antistatic agents, nonionic antistatic agents such as polyoxyethylene sorbitan monostearate, betaine-type amphoteric antistatic agents, etc.); flame retardants (melamine cyanurate, hydroxides such as magnesium hydroxide and aluminum hydroxide, ammonium polyphosphate, brominated polystyrene, brominated polyphenylene oxide, brominated polycarbonate, brominated epoxy resin, or combinations of these brominated flame retardants with antimony trioxide, etc.); light stabilizers such as manganese acetate; and antifoaming agents.
[0025] In the polymerization of polyamide, in order to suppress the production of cyclopentanones and to ensure that the polymerization reaction proceeds uniformly in a short period of time, it is important to increase the degree of polymerization by balancing the concentrations of amino terminal groups and carbo terminal groups. In order to obtain fibers with high physical properties, a high degree of polymerization is preferable. In the polyamide having a high degree of polymerization, the sum of the amount of amino end groups and the amount of carbo end groups is preferably 150 millimole equivalents / kg polymer or less, more preferably 130 millimole equivalents / kg polymer or less, and even more preferably 110 millimole equivalents / kg polymer or less. On the other hand, in order to obtain uniform fibers, the sum of the amount of amino end groups and the amount of carbo end groups is preferably 50 millimole equivalents / kg polymer or more, more preferably 70 millimole equivalents / kg polymer or more, and even more preferably 90 millimole equivalents / kg polymer or more. In addition, in this embodiment, the carboxyl end group concentration of the polyamide is excessive relative to the amino end group concentration, and the difference in the end group concentration is preferably 5 millimole equivalents / kg polymer or more and 80 millimole equivalents / kg polymer or less, more preferably 10 millimole equivalents / kg polymer or more and 60 millimole equivalents / kg polymer or less, and even more preferably 20 millimole equivalents / kg polymer or more and 50 millimole equivalents / kg polymer or less. When the carboxyl end group concentration is high and the concentration difference is large at 5 millimole equivalents / kg polymer or more, the hydrogen ion concentration is high in the polyamide internal environment, the catalytic toxicity of the phosphorus compound is suppressed, the adhesion between the polyamide and silicone is good, and the adhesion has good wet heat resistance. If the concentration difference of the excess carboxyl end group concentration is 80 millimole equivalents / kg polymer or less, the degree of polymerization is high, and it is easy to obtain a fiber with high strength during drawing. In addition, when the carboxyl end group concentration is higher, the generation of tertiary amine during melting is suppressed, the spinning operability is good, and a woven yarn with good fluff quality is obtained.
[0026] Another embodiment of the present invention is a method for producing a method for manufacturing a semiconductor device comprising the steps of: A step of melt spinning a polyamide to obtain a polyamide multifilament yarn having a cyclopentanone content of 0 ppm or more and 800 ppm or less; A step of obtaining a woven fabric by weaving the obtained polyamide multifilament yarn; A refining process using an alkaline cleaning solution at a temperature of 35°C or higher; drying process, applying silicone to at least one surface of the fabric to form a layer of silicone membrane; and Vulcanization setting process, The present invention relates to a method for producing a polyamide multifilament woven airbag fabric, comprising the steps of: The content of cyclopentanones in the polyamide resin before melt spinning is preferably 0 ppm or more and 1,000 ppm or less, more preferably 800 ppm or less, and even more preferably 80 ppm or less.
[0027] The resin composition constituting the polyamide fiber is useful for a polymerization reaction apparatus for producing the same in a process of heating at a relatively low temperature and removing moisture under high pressure, and a process of promoting a polycondensation reaction at a high temperature. The reaction apparatus may be a single tank or a continuous two-tank apparatus. The polyamide resin composition is discharged from the polymerization reaction apparatus in a strand shape, cooled / cut once, pelletized, and then dried to remove moisture, thereby obtaining pellets suitable for fiber use. In the method for producing a resin composition for polyamide fiber, the polyamide resin composition is polymerized in a liquid phase, and then solid-phase polymerization can be performed to further increase the degree of polymerization. The solid-phase polymerization method performed at or below the melting temperature can also suppress the thermal degradation of the polymer itself, and is a preferred method for preventing the increase of cyclopentanones in the polymer. Polyamide resins may contain, for example, antioxidants and heat stabilizers (hindered phenol compounds, hydroquinone compounds, thiazole compounds, phosphorus compounds such as phenylphosphonic acid, imidazole compounds such as 2-mercaptobenzimidazole, and their substitutes, copper halides, iodine compounds, etc.), weathering agents (resorcinol, salicylate, benzotriazole, benzophenone, hindered amine, etc.), pigments (cadmium sulfide, phthalocyanine, carbon black, etc.), gloss improvers (titanium oxide, calcium carbonate, etc.), dyes (nigrosine, aniline black, etc.), crystal nucleating agents (talc, silica, kaolin, crystallographic, etc.), and the like. The resin composition may contain small amounts of additives such as butyl ether, butyl ether, butyl ether, etc.), plasticizers (octyl p-oxybenzoate, N-butylbenzenesulfonamide, etc.), antistatic agents (anionic antistatic agents of alkyl sulfate type, cationic antistatic agents of quaternary ammonium salt type, nonionic antistatic agents such as polyoxyethylene sorbitan monostearate, betaine amphoteric antistatic agents, etc.), and flame retardants (hydroxides such as melamine cyanurate, magnesium hydroxide, and aluminum hydroxide, ammonium polyphosphate, brominated polystyrene, brominated polyphenylene oxide, brominated polycarbonate, brominated epoxy resin, or combinations of these brominated flame retardants with antimony trioxide, etc.).
[0028] The spinning temperature in melt spinning is preferably 290° C. or higher and 310° C. or lower. Setting the spinning temperature to 310° C. or lower is preferable because thermal decomposition of the polyamide can be suppressed, more preferably 300° C. or lower, and even more preferably 295° C. or lower. On the other hand, a spinning temperature of 290° C. or higher is preferable because the polyamide exhibits sufficient melt fluidity, the discharge amount between the discharge holes is uniform, and high-magnification drawing is possible. The shorter the residence time in the melt spinning process (the time from when the polyamide resin is melted until it is discharged from the spinneret), the better. The residence time is preferably 30 minutes or less, more preferably 15 minutes or less, and even more preferably 0.5 minutes to 7 minutes. A short residence time is preferable because cyclopentanones in the polymer increase at the melting temperature. In the melt spinning process, a single-screw or twin-screw extruder is preferably used in the melting section, since the polyamide resin can be guided to the polymer pipe, gear pump, and spinning pack while being subjected to an appropriate pressure by the extruder, and therefore abnormal retention does not occur in these flow paths, and an increase in cyclopentanones due to thermal decomposition of the polyamide can be suppressed, which is preferable. In addition, it is preferable to filter the polyamide resin using a metal fiber nonwoven fabric filter, sand, or the like before it is discharged from the spinneret, since this stabilizes the spinning operation. The shape of the spinneret holes may be selected according to the cross-sectional shape of the single fibers constituting the filaments to be produced. The yarn spun from the spinneret is solidified with cooling air, a process oil is applied, and the yarn is taken up, stretched, and heat-treated to obtain the polyamide fiber used in the present invention.
[0029] It is important that the amount of cyclopentanones in the polymer is small by the above-mentioned appropriate manufacturing method for polyamide fibers. The amount of cyclopentanones in the airbag fabric can be reduced by reducing the amount of cyclopentanones in the polyamide fibers used for weaving. The amount of cyclopentanones in the polyamide fibers is preferably 800 ppm or less, more preferably 600 ppm or less, even more preferably 400 ppm or less, and particularly preferably 80 ppm or less. The polyamide fiber filaments preferably have a strength of 7 cN / dtex. A strength of 7 cN / dtex or more is preferable because fluff is unlikely to occur even if the weaving tension is increased in the weaving process, and a high-density woven fabric can be obtained with good passability through the manufacturing process, and is more preferably 7.5 cN / dtex or more, even more preferably 8 cN / dtex or more, even more preferably 9.0 cN / dtex or more, and most preferably 9.5 cN / dtex or more. The tensile strength of the polyamide fiber filaments is substantially 10.5 cN / dtex or less, taking into consideration other characteristics and production costs, etc. The oil agent adhesion rate of the polyamide fiber is preferably 0.6 to 1.5 wt%. If the oil agent adhesion rate is 1.5 wt% or less, the weft yarn hardly has difficulty in flying due to stickiness (tackiness), and the weft yarn transport medium, air or water, does not lose its weft yarn transport force due to the single yarn bundle being too good compared to the single yarn bundle due to entanglement, resulting in a reduction in apparent cross-sectional area, and weaving stability is good. On the other hand, if the oil agent adhesion rate is 0.6 wt% or more, the weft yarn is smoothly supplied due to an appropriate friction reduction effect, resulting in excellent productivity without weaving stoppage.
[0030] In weaving, a water jet loom, an air jet loom, a rapier loom, or the like can be used as the loom. The airbag base fabric is a high-density woven fabric, and it is preferable to increase the warp tension in the warping and weaving processes to manufacture it with good process passability. A high-density woven fabric is formed by setting the warp tension high in weaving and creating effective beating conditions. In particular, a bent shape in which the warp threads are sufficiently interlocked is created, and the warp crimp is large.
[0031] The fabric woven in this manner can be subjected to a scouring process to wash off the process oil from the polyamide fibers, and at the same time, the content of cyclopentanones in the fibers can be reduced. The refining process can be performed using hot water or hot compressed water, and the treatment process can be a single-stage or a multi-stage process of two or more stages. It is also preferable to perform refining by applying a conventionally known refining agent. A combination of a nonionic surfactant and soda ash or a combination of a higher alcohol sulfate and soda ash is used. In particular, refining with an alkaline agent such as soda ash is effective in removing the process oil from the fiber surface and reducing the amount of cyclopentanone in the fiber. The temperature in the scouring process is preferably 35°C or higher, and more preferably in the range of 60°C to 98°C. The higher the temperature in the scouring process, the more the content of cyclopentanones in the fiber can be reduced. In the scouring process, it is preferable to perform a water washing treatment (water rinsing) after scouring with a scouring agent. In order to increase the hydrogen ion concentration inside the polyamide fiber, it is preferable to perform a multi-stage water washing process or to extend the residence time. By increasing the hydrogen ion concentration inside the polyamide fiber, the catalytic toxicity of the silicone addition reaction of phosphorus compounds can be suppressed, and the inhibition of adhesion between silicone and textile can be avoided. The scouring step may be carried out continuously after the weaving step, or may be carried out as a separate step after weaving. In addition, either a batch method or a continuous method may be adopted, but it is preferable to carry out the treatment continuously while feeding and discharging the base fabric to and from the treatment zone, because this is excellent in productivity. The scouring process can facilitate the removal of cyclopentanone by loosening the fabric structure. Regarding gripping of the fabric in the scouring bath, it is preferable to convey the fabric without gripping it in the width direction, and in the warp direction, the conveying tension is preferably 0.8 N / cm or less, more preferably 0.5 N / cm or less. In order to prevent the woven fabric from sagging during transportation and to avoid the occurrence of wrinkles, it is preferable to set the warp tension to 0.08 N / cm or more. During transport, the tension load can be controlled by providing a dancer roll or the like to control the tension. In the scouring process, the fabric shrinks depending on the bath temperature and the thermal shrinkage characteristics of the constituent fibers, but controlling the warp tension to a low level while shrinkage occurs and allowing the fabric to shrink in the width direction contributes to removing cyclopentanone.
[0032] The woven fabric is preferably heat-set in a heat-setting process. The heat-setting temperature is preferably 110°C or higher and 160°C or lower, more preferably 130°C or higher and 150°C or lower, and the heat-setting time may be appropriately selected within the range of 0.1 minutes or higher and 30 minutes or lower. In the heat-setting process, the woven fabric is preferably dried under tension so that the shrinkage force of the woven fabric is maintained at a predetermined force. Heat-setting the woven fabric can stabilize the processability of the subsequent resin application process.
[0033] The fabric after the scouring step may be dried as necessary before the heat setting step. The drying temperature is preferably in the range of 80°C to 130°C, more preferably 100°C to 120°C. The treatment time is preferably selected appropriately from 0.1 minutes to 30 minutes. Drying may be performed with the fabric in a relaxed or tensioned state.
[0034] The airbag fabric of this embodiment is coated with silicone and then subjected to a finish heat setting process to form an airbag coat fabric. The silicone to be applied is preferably one that is excellent in flame retardancy, heat resistance, air barrier properties, and the like. The silicone is preferably an addition reaction type curable silicone rubber that can be applied without a solvent. The main component of silicone is alkenylorganopolysiloxane, which is the base polymer of the coating agent and contains at least two alkenyl groups bonded to silicon atoms. In general, it is preferable that the organopolysiloxane is substantially linear, and specifically, it is preferable that the molecular chain is mainly composed of repeated diorganosiloxane units and is linear diorganopolysiloxane in which both ends of the molecular chain are blocked with triorganosiloxy groups. Furthermore, the position of the alkenyl group bonded to the silicon atom of the main chain is not particularly limited, and the alkenyl group may be bonded to only one of the silicon atom at the molecular chain terminal portion and the silicon atom at the molecular chain non-terminal portion, or may be bonded to both of them. Examples of the organo group in the side chain include unsubstituted or substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms and no aliphatic unsaturated bonds. Among them, methyl group, phenyl group, or a combination of both of them is preferable. Examples of the alkenyl group include alkenyl groups having 2 to 8 carbon atoms. Examples include vinyl groups, allyl groups, 1-propenyl groups, isopropenyl groups, 1-butenyl groups, isobutenyl groups, and hexenyl groups. Of these, vinyl groups are preferred.
[0035] The organosilicon compound of the crosslinking component of silicone is at least one selected from the group consisting of organohydrogensilanes containing at least two hydrogen atoms bonded to silicon atoms, linear or branched organohydrogenpolysiloxanes containing at least two (particularly, two or three) diorganohydrogensilyl groups (i.e., hydrogen atoms bonded to silicon atoms at the molecular chain terminals), and hydrocarbon compounds containing at least two (particularly, two or three) diorganohydrogensilyl groups. Examples of the organic groups bonded to the silicon atoms include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, and hexyl groups; aryl groups such as phenyl, tolyl, and xylyl groups; and halogenated alkyl groups such as 3-chloropropyl and 3,3,3-trifluoropropyl groups. Examples of the diorganohydrogensilyl groups include dimethylhydrogensilyl groups. Specific examples include methylsilane ((CH3)SiH3), dimethylsilane ((CH3)2SiH2), ethylsilane ((C2H5)SiH3), diethylsilane ((C2H5)2SiH2), hexylsilane ((C6H 13 )SiH3), dihexylsilane ((C6H 13 )2SiH2), n-octylsilane ((n-C8H 17 )SiH3), di(n-octyl)silane ((n-C8H 17 )2SiH2), phenylsilane ((C6H5)SiH3), diphenylsilane ((C6H5)2SiH2), tris(dimethylhydrogensiloxy)methylsilane, tris(dimethylhydrogensiloxy)phenylsilane, tris(dimethylhydrogensilylethyl)methylsilane, tris(dimethylhydrogensilylethyl)phenylsilane, and 1,4-bis(dimethylhydrogensilyl)benzene.
[0036] The content of the crosslinking component is an amount such that the molar ratio of silicon-bonded hydrogen atoms in this component to the alkenyl groups in the entire coating agent is in the range of 0.01 to 5.0, preferably in the range of 0.1 to 2.0, and particularly preferably in the range of 0.1 to 1.0. In this case, the ratio of alkenyl groups in component (A) to the alkenyl groups present in the entire coating agent is preferably 90 mol % to 100 mol %, more preferably 95 to 100 mol %. The silicone reaction catalyst or component is a platinum group metal catalyst, and those known as hydrosilylation reaction catalysts can be used. For example, platinum group metals such as platinum (including platinum black), rhodium, and palladium; platinum chloride, chloroplatinic acid, and chloroplatinate salts such as H2PtCl4·nH2O, H2PtCl6·nH2O, NaHPtCl6·nH2O, KHPtCl6·nH2O, Na2PtCl6·nH2O, K2PtCl4·nH2O, PtCl4·nH2O, PtCl2, and Na2HPtCl4·nH2O (wherein n is an integer of 0 to 6, preferably 0 or 6); Examples of suitable catalysts include alcohol-modified chloroplatinic acid, complexes of chloroplatinic acid and olefins, platinum black, platinum group metals such as palladium supported on alumina, silica, carbon, and other carriers, complexes of platinum and triphenylphosphine, rhodium-olefin complexes, chlorotris(triphenylphosphine)rhodium (Wilkinson's catalyst), complexes of platinum chloride, chloroplatinic acid, or chloroplatinic acid salts with vinyl group-containing siloxanes, particularly vinyl group-containing cyclic siloxanes, and the like. Among these, platinum-based catalysts such as complexes of vinyl group-containing cyclic siloxanes, and complexes of platinum and triphenylphosphine are particularly preferred. In addition to the above, silicone may contain other components. For example, inorganic fillers for improving the properties of the cured resin include fine silica powder for reinforcing resin strength and calcium carbonate powder for enhancing resin toughness, curing reaction inhibitors include acetylene compounds such as 3,5-dimethyl-1-hexyne-3-ol and ene-yne compounds such as 3,5-dimethyl-3-hexene-1-yne, and adhesion improvers include silane coupling agents such as methyltrimethoxysilane.
[0037] The amount of silicone applied to the airbag base fabric is 10g / m 2 More than 100g / m 2 More preferably, it is 15 g / m or less. 2 More than 70g / m 2 More preferably, it is 20 g / m or less. 2 More than 40g / m 2 Less than or equal to 10g / m 2 The required airtightness can be obtained with an application amount of 100 g / m or more. 2 At the following application amounts, the coated fabric has flexibility, good packability, and reduces the overall weight of the bag. Methods of coating the surface of a fabric with silicone include immersing the fabric in a resin solution bath, then forming and homogenizing the excess resin using a mangle, vacuum, or even a coating knife, bar coating methods such as a comma coater, and spraying the resin using a spray device or forming device. Of these, from the viewpoint of applying a small amount of resin uniformly, the knife coating method of solvent-free silicone is preferred. In particular, when coating by air knife coating, it is preferable to coat with a contact pressure between the knife and the fabric in the range of 15 N / cm to 15 N / cm and a fabric tension in the range of 100 N / cm to 3000 N / cm. By using a high contact pressure with the knife, the coating thickness can be thinned and the coating amount can be controlled lightly and uniformly. The fabric tension in the coating process stretches the fabric in the warp direction and acts to accumulate thermal strain.
[0038] After the silicone coating, a vulcanization setting process (finishing heat setting process) is carried out in order to vulcanize and crosslink the silicone and to finally heat set the base fabric. Here, it is important to stabilize the warp strain caused by the warp tension in the coating process. For this reason, it is preferable to carry out the setting process with an overfeed of 0.8% or more in the feed direction of the fabric, i.e., the warp direction, and more preferably an overfeed process of 1.0% to 3.0%. The amount of overfeed can be determined according to the shrinkage rate of the weaving yarn and the heat treatment conditions of each process. By feeding in the overfeed, the warp strain is eliminated, making it possible to improve the thermal dimensional stability of the base fabric. The temperature for the final heat setting process is selected so as to contribute to the acceleration of silicone vulcanization and the improvement of the dimensional stability of the nylon fabric. The temperature for the final heat setting process is preferably 160°C or higher and 210°C or lower. More preferably, it is 170°C or higher and 200°C or lower. In the final heat setting process, an overfeed of 0.8% to 3.0% in the warp direction and a temperature of 160° C. to 210° C. are preferable for improving the thermal dimensional stability of the base fabric.
[0039] In the airbag fabric of this embodiment, in a combustion test of FMVSS302 after 400 hours at 80°C and 95%, it is preferable that the fabric is self-extinguishing in both warp and weft directions, or the burning speed is 100 mm / min or less, regardless of whether the fabric is ignited from the front or back. In other words, in a combustion test of FMVSS302 after 400 hours at 80°C and 95%, it is preferable that the airbag fabric is not ignited on the test piece within a specified time or is extinguished before the A-mark line, regardless of whether the fabric is ignited from the front or back, in both warp and weft directions, that is, it is preferable that the fabric is judged to be self-extinguishing, or the burning speed is 100 mm / min or less. Furthermore, it is preferable that the airbag fabric of this embodiment does not increase in flammability by moist heat treatment. That is, the airbag fabric has a burning rate increase of 40% or less, more preferably 30% or less, and even more preferably 20% or less, after moist heat treatment, relative to the burning rate before moist heat treatment, which is held at 80°C and 95% humidity for 400 hours. Silicone adheres well to nylon fabric and has thermal dimensional stability, which suppresses the increase in burning rate caused by moist heat treatment. If the increase in burning rate caused by moist heat treatment is suppressed, the airbag can maintain its flame retardancy even when installed in a vehicle under harsh conditions.
[0040] In the airbag fabric of this embodiment, in the evaluation of the burning rate after moist heat treatment in the FMVSS302 burning test, the burning rate ratio of the coated surface ignition (burned with the coated surface facing down) to the woven surface ignition (burned with the coated surface facing up) is 3.0 or less, more preferably 2.5 or less. The lower limit of the burning rate ratio is preferably 1.0 or more. Since the silicone adheres sufficiently to the polyamide fiber fabric and is thermally dimensionally stable, the difference in burning rate between the front and back of the coating does not increase under environmental conditions. In other words, even in the case of an airbag cushion in which the coated surface is exposed in an airbag mounted in a vehicle under harsh conditions, the flame retardancy can be maintained. As described above, the airbag fabric of this embodiment preferably has a blade combing resistance of 350N or more after humid heat environment (400 hours under an environment of 85°C and 95% relative humidity). More preferably, it is 420N or more, and even more preferably, it is 470N or more. The blade combing resistance is the resistance of the constituent yarns of the fabric to slippage, and is a combination of the binding force of the constituent yarns of the fabric structure and the resistance of silicone adhesion. The higher the blade combing resistance is, 350N or more, the better the adhesion of the silicone layer. This high blade combing resistance is one factor in suppressing the burning rate. On the other hand, if the blade combing resistance is 800N or less, the tear resistance is sufficiently high. EXAMPLES
[0041] The present invention will now be described in detail with reference to examples. Various evaluations in the examples were carried out according to the following methods.
[0042] (1) Amount of silicone applied to the base fabric A sample with an area (A) of 0.3 m square is taken from the base fabric, degreased with dichloromethane, and dried at 105°C. This is dissolved in 200 g of 90% formic acid at room temperature, and the insoluble matter is filtered out using a sintered glass filter (VIDTEC glass filter 17G-3, manufactured by Cosmospeed Co., Ltd.), thoroughly washed with formic acid and rinsed with water, the insoluble matter is dried at 105°C, and the mass is precisely weighed (M). Coating weight (g / m 2 ) was obtained by dividing the formic acid insoluble matter (M) by the area (A) of the fabric sample.
[0043] (2) Determination of cyclopentanones in polyamide resin, fiber, and fabric before melt spinning The polyamide resin, polyamide fiber, or base fabric was cut into pieces and prepared under standard conditions (20° C., relative humidity 65%, left for 24 hours or more). The analysis was performed using the HS-SPME-GC / MS method. Approximately 10 mg of the sample was precisely weighed, placed in a vial for headspace, and an SPME fiber assembly was attached. The SPME fiber assembly is a PDMS fiber coated with polydimethylsiloxane. The vial in which the sample was set was heated to 180°C for 5 minutes using a block heater, then removed and cooled at room temperature for 5 minutes. The SPME was removed and analyzed by GC / MS. A quantitative analysis was performed using a cyclopentanone standard, and the content of cyclopentanones was determined by adding up the four compounds a) cyclopentanone, b) Cyclopenten-1-one, c) 1,1'-Bicyclopentyl-2-one, and d) Cyclopentanone, 2-cyclopentylidene. In this case, when the sample was a polyamide fiber, the content (ppm) of cyclopentanone in the precisely weighed sample was obtained. When the sample was a base fabric, the weight of the base fabric was precisely weighed and converted into the fabric weight by subtracting the amount of silicone applied, and the cyclopentanone content (ppm) in the constituent fabric was determined. The GC / MS was manufactured by Agilent, GC: 7890B, MS: 5977B. The conditions were as follows: Column: DB-1MS (30m x 0.25mm, film thickness 0.25μm) Column temperature: 40℃ (3 min) → 20℃ / min → 300℃ Column flow rate: 1.0 ml / min Column flow rate: 1.0 mL / min Injection method: splitless Injection temperature: 250℃ Interface temperature: 280℃ Ion source temperature: 230℃ Ion source: EI method Scan range: 50-500m / z
[0044] (3) End group weight of the constituent yarns of the base fabric (base fabric 20 cm square) The constituent yarns were peeled off from the base fabric and samples of 5 to 10 g were taken. (3a) Amino end group concentration The fiber sample was peeled off from the base fabric and weighed precisely, then dissolved in a 90% aqueous phenol solution. After complete dissolution, the solution was titrated with a 0.05N aqueous hydrochloric acid solution until the pH of the solution reached 3. The amino end group concentration per kg of polymer was calculated from the titration amount. (3b) Carboxyl end group concentration The yarn sample was weighed out exactly as described above and dissolved in benzyl alcohol at 170°C. After complete dissolution, phenolphthalein indicator was added. Then, colorimetric titration was performed with 0.1N NaOH ethylene glycol solution. The carboxyl end group concentration per 1 kg of polymer was calculated from the titration amount. The difference in terminal groups of the constituent fabrics was determined by subtracting the amino terminal group concentration from the carboxyl terminal group concentration, and the sum of the carboxyl terminal group concentration and the amino terminal group concentration was determined as the sum of the terminal groups of the constituent fabrics.
[0045] (4) Determination of phosphorus content in base fabric The constituent yarns were peeled off from the base fabric and a sample of about 0.5 g was taken. The content of phosphorus atoms derived from phosphate groups in the constituent yarns was determined by inductively coupled plasma atomic emission spectrometry (ICP-AES) using the following equipment and conditions. (Measurement conditions) ICP-AES device: Thermo Fisher Scientific, iCAP6300Duo High frequency output: 1150W Plasma gas: 12L / min Auxiliary gas: 0.5L / min Nebulizer gas: 0.5L / min Photometry: Axial direction Measurement wavelength: 213nm Pretreatment method: The sample was wet decomposed with sulfuric acid, nitric acid, and hydrochloric acid to prepare the test solution.
[0046] (5) Amount of oil in the base fabric The measurement was performed by Soxhlet extraction in accordance with JISL1095 (2010) 9.30. Cyclohexane was used as the solvent. The moisture content of the base fabric sample was measured by the Karl Fischer titration method by moisture evaporation in JISK0068 (2001), and the bone dry weight was calculated from the precisely weighed weight of the base fabric sample. The weight of the fabric was then converted by subtracting the amount of silicone applied from the weight of the base fabric, and this was used as the sample weight of the constituent fabric. The amount of oil component in the constituent fabric (wt%) was calculated from the amount of oil component extracted by Soxhlet and the sample weight of the constituent fabric. To ensure the weighing accuracy of the extracted dried product, the base fabric sample was replaced with a new one and additional extraction was repeated if necessary.
[0047] (6) Shrinkage dimensional change rate of base fabric The base fabric is exposed to an environment with a temperature of 20°C and a relative humidity of 65% for at least 24 hours, and a 150mm square piece is taken along the warp and weft directions of the base fabric as a sample. Marked lines are drawn on the taken piece at precise intervals of 100mm in both the warp and weft directions. The sample piece is placed in a hot air oven at 105°C without tension for 60 minutes. After removing it and exposing it to an environment with a temperature of 20°C and a relative humidity of 65% for at least 24 hours, the distance between the marks is measured in both the warp and weft directions. The shrinkage change rate (%) of the mark distance compared to the original 100mm is calculated. This is repeated three times and the average is calculated. The value in the warp and weft directions that shows the largest shrinkage change rate is used as the shrinkage dimensional change rate.
[0048] (7) Burning rate of the base fabric, increase in burning rate after moist heat treatment, and burning rate ratio between the front and back (C / W ratio) FMVSS302 combustion test was conducted. The base fabric in a standard state and the base fabric returned to the standard state after being kept in an environment of 80°C and 95% relative humidity for 400 hours were fixed to a U-shaped frame and placed horizontally, with the coated side facing down, and the sample edge was ignited with a burner flame to evaluate the burning rate. Tests were performed in both warp and weft directions, and the increase in burning rate (%) before and after the moist heat treatment was evaluated. In addition, for a base fabric sample that had been kept in an environment of 80°C and 95% relative humidity for 400 hours and then returned to its standard condition, the sample was fixed to a U-shaped frame and placed horizontally. The burning rate was evaluated for each case: when the coated side was placed facing down and ignited from the end of the sample with a burner flame, and when the woven side was placed facing down and ignited from the end of the sample with a burner flame. The ratio of the burning rate with the coated side facing down (C rating) to the burning rate with the woven side facing down (W rating) was evaluated and is shown in the table below as the burning rate ratio between the front and back after moist heat treatment (C / W ratio).
[0049] (8) Increased breathability of the base fabric after wet heat treatment The air permeability (mm / s) was measured at a pressure of 50 kPa using a "High Pressure Air Permeability Tester" manufactured by Cosmo Instruments Co., Ltd. The base fabric samples were compared between a standard condition sample and a sample that had been kept in an environment of 80°C and 95% relative humidity for 400 hours and then brought to a standard condition, and the increase in air permeability (mm / s) after the moist heat treatment was measured.
[0050] (9) Combing resistance of the base fabric after wet heat treatment After keeping the fabric in an environment of 80°C and 95% relative humidity for 400 hours, the blade combing resistance of the base fabric was measured in the standard condition for five samples in each warp and weft directions according to ASTM-D6479(2015), and the values were averaged. The base fabric samples were kept in an environment of 80° C. and 95% relative humidity for 400 hours and then brought to standard conditions.
[0051] (10) Scrub evaluation of base fabric Coating adhesion was confirmed by a rubbing test. The test equipment was a scrub tester, and the test was conducted in accordance with ISO 5981. Tests were conducted on a base fabric in a standard state and a base fabric that had been kept in an environment of 80°C and 95% relative humidity for 400 hours and then returned to a standard state. Observations were made every 50 times out of 200 rubs, and the number of rubs at which peeling was observed was evaluated.
[0052] [Example 1] A non-end-blocked polyamide 6·6 polymer was polymerized using phenylphosphonic acid as a polymerization catalyst and copper iodide and potassium iodide as thermal stabilizers, and then the polymer was discharged as chips and further polymerized in the solid state. Polymer chips were melted at 300°C, extruded by melt spinning at 290°C for 180 seconds, and stretched after adding an aliphatic synthetic ester spinning oil to obtain polyamide 6·6 fiber 470dtex 136 filament. This fiber contained 140ppm phosphorus, 60ppm copper, and 1800ppm iodine. The difference between the carboxyl end group concentration and the amino end group concentration was 50 mmol equivalents / kg polymer. The fiber contained 500ppm of cyclopentanones. The boiling water shrinkage according to JISL1017(2002)8.14 was 7.5%. The fibers were warped without twist or sizing, and woven into a plain weave on a water jet loom using the same yarn as the weft. The fabric was scoured using an open soap type scourer. After soaking and retaining in an 80°C hot water bath containing 0.5 g / l of sodium alkylbenzene sulfonate and 0.5 g / l of soda ash for 1 minute, it was immersed in three layers of neutral 80°C hot water baths for 1 minute each. In order to stably transport the fabric during scour, the warp tension was controlled to 0.22 N / cm using a dancer roll. It was then dried with hot air at 110°C for 3 minutes. Furthermore, a solvent-free addition type silicone resin was applied at 20 g / m by air knife coating. 2 At this time, the tension of the base fabric in the warp direction was set to 580 N / m, and the knife blade thickness was selected so as to obtain the desired coating amount. Next, the fabric was heat treated at 190°C for 2 minutes using a pin tenter heat treatment machine with a warp overfeed shrinkage of 2.0% and a width extension of 0%, to obtain a coated fabric for airbags. The cover factor was 2145 based on the weave density and the constituent yarn fineness. The physical properties of the obtained base fabric are shown in Table 1 below. Dimensional stability was measured in the warp direction because the rate of change was large in that direction. The increase in burning rate due to moist heat treatment was suppressed. Furthermore, the burning rate with the coated side facing down was higher than that with the woven side facing down, but this level remained even after moist heat treatment.
[0053] [Examples 2 to 4] An airbag base fabric was obtained in the same manner as in Example 1, except that when the woven fabric was scoured in an open soap type scourer, the temperature of the hot water bath was set to the temperature shown in Table 1 below.
[0054] [Comparative Example 1] An airbag base fabric was obtained in the same manner as in Example 1, except that when the woven fabric was refined in an open soap type scouring machine, it was immersed in three layers of neutral 80 ° C. hot water baths successively for 1 minute each and then dried at 110 ° C. for 3 minutes. The increase in burning rate due to moist heat treatment is large. Furthermore, the burning rate with the coated side facing down is higher than the burning rate with the woven side facing down, and the difference is large after moist heat treatment.
[0055] [Examples 5 to 7, Comparative Example 2] In the vulcanization setting process using a pin tenter heat treatment machine after knife coating, the overfeed shrinkage in the warp direction was set to the value shown in Table 1 or 2 below. In the same manner as in Example 1, an airbag fabric was obtained. The increase in burning rate due to the moist heat treatment is large in Comparative Example 2. Furthermore, the burning rate with the coated side facing down is higher than the burning rate with the woven side facing down, and the difference is large after the moist heat treatment.
[0056] [Example 8] An airbag base fabric was obtained in the same manner as in Example 1, except that when the grey fabric was scoured in an open soap type scourer, it was immersed and retained for 1 minute in a 60°C warm water bath containing 0.5 g / l sodium alkylbenzene sulfonate and 0.5 g / l soda ash, and then immersed in three layers of neutral 60°C warm water baths for 1 minute each, and then dried at 110°C for 3 minutes. After the knife coating, a pin tenter heat treatment machine was used to obtain a coated airbag fabric by treating the fabric at 190°C for 2 minutes with a warp overfeed shrinkage of 1.5% and a width extension of 0%, in the same manner as in Example 1. An airbag fabric was obtained.
[0057] [Comparative Example 3] An airbag fabric was obtained in the same manner as in Example 8, except that in the vulcanization setting step using a pin tenter heat treatment machine after knife coating, the warp overfeed shrinkage was set to 0.5%. The burning rate is often increased by moist heat treatment.
[0058] [Comparative Example 4] When the green fabric was scoured with an open soap type scourer, it was immersed and retained in a 30°C warm water bath containing 0.5g / l of sodium alkylbenzene sulfonate and 0.5g / l of soda ash for 1 minute, then immersed in a neutral 30°C warm water bath for 1 minute, and then dried at 110°C for 3 minutes. In addition, in the vulcanization setting process using a pin tenter heat treatment machine after knife coating, the overfeed shrinkage of the warp was set to 1.0%. Except for these, the airbag base fabric was obtained in the same manner as in Example 1.
[0059] [Example 9] Polyamide 6·6 polymer was polymerized without end-capping using hypophosphorous acid as a polymerization catalyst and copper iodide and potassium iodide as thermal stabilizers, and then chipped and further polymerized in the solid state. The polymer chips were extruded, coated with an aliphatic synthetic ester spinning oil, and stretched to obtain 470 dtex 136 polyamide 6·6 fiber filaments. This fiber contained 10 ppm phosphorus, 60 ppm copper, and 1800 ppm iodine. The difference between the carboxyl end group concentration and the amino end group concentration was 50 millimole equivalents / kg polymer. The fiber contained 400 ppm cyclopentanones. This fiber was used to obtain an airbag fabric in the same manner as in Example 1. The increase in burning rate due to moist heat treatment was suppressed. Furthermore, the burning rate with the coated side facing down was higher than the burning rate with the woven side facing down, but this level was maintained even after moist heat treatment.
[0060] [Comparative Example 5] When refining the green fabric with an open soap type refining machine, no alkaline cleaning solution was used, and the fabric was immersed in three layers of neutral 80°C hot water baths for 1 minute each, and then dried at 110°C for 3 minutes. An airbag base fabric was obtained in the same manner as in Example 10. The increase in combustion rate due to moist heat treatment is large.
[0061] [Example 10] In Example 9, when polymerizing polyamide 6·6 polymer, hexamethylenediamine was added to the equimolar monomer salt so that the difference between the carboxyl end group concentration and the amino end group concentration was small. The polymer chips were discharged, and after applying an aliphatic synthetic ester spinning oil, they were stretched to obtain polyamide 6·6 fiber 470 dtex 136 filament. This fiber contained 10 ppm phosphorus, 60 ppm copper, and 1800 ppm iodine. The difference between the carboxyl end group concentration and the amino end group concentration was 5 millimole equivalents / kg polymer. The cyclopentanones in the fiber were 400 ppm. The fiber was used to obtain an airbag base fabric in the same manner as in Example 1.
[0062] [Example 11] An airbag fabric was obtained in the same manner as in Example 1, except that when the woven fabric was refined with an open soap type scouring machine, the tension of the woven fabric transport was set to 1.5 N / cm.
[0063] [Example 12] An airbag base fabric was obtained in the same manner as in Example 1, except that when the woven fabric was scoured in an open soap type scourer, it was immersed and retained in an 80°C warm water bath containing 0.5 g / L of sodium alkylbenzene sulfonate and 0.5 g / L of soda ash for 1 minute, and then was continued to the hot air drying process without being immersed in a neutral 80°C warm water bath.
[0064] The conditions, physical property results, etc. of the above-mentioned Examples 1 to 12 and Comparative Examples 1 to 5 are shown in Tables 1 and 2 below. [Table 1]
[0065] [Table 2] [Industrial Applicability]
[0066] The airbag fabric of the present invention has stabilized flame retardancy under environmental conditions, and the difference in flame retardancy between the front and back sides of the coated fabric is maintained small. Therefore, the fabric can be used as an airbag cushion without distinguishing between the front and back sides of the coated fabric. It is also possible to design an airbag cushion in which the coated surface is exposed and the inner surface of the airbag cushion is protected from environmental conditions by covering it with a coating film. The flame retardancy under more severe environmental conditions is stabilized, and the fabric can be suitably used for airbags installed outside the passenger compartment.
Claims
1. An airbag fabric which is a polyamide multifilament woven fabric, The fabric has a layer of silicone membrane on at least one side thereof; The amount of the silicone film is 10 g / m 2 More than 100g / m 2 is as follows: The content of cyclopentanones is 0 ppm or more and 250 ppm or less based on the weight of the fabric, The larger of the shrinkage dimensional change rates in the warp and weft directions before and after heating at 105° C. for 60 minutes is 0% or more and 1.4% or less, and An airbag base fabric, characterized in that the increase in burning rate of the base fabric when kept in a standard state after being kept in an environment of 85°C and 95% relative humidity for 400 hours is 40% or less.
2. The airbag fabric according to claim 1, wherein the amount of an oil agent contained in the woven fabric is 0% by weight or more and 0.04% by weight or less.
3. The airbag fabric according to claim 1 or 2, containing phosphorus atoms in an amount of 10 ppm or more and 300 ppm or less based on the weight of the constituent yarns of the fabric.
4. The airbag fabric according to any one of claims 1 to 3, wherein the amount of carboxylic acid terminals exceeds the amount of amine terminals at the molecular chain ends of the polyamide, the difference being 10 millimole equivalents / kg or more and 50 millimole equivalents / kg or less.
5. In a combustion test of FMVSS302 after 400 hours under an environment of 80°C and 95%, the following 1) or 2): 1) It will self-extinguish regardless of whether the fire is ignited from the front or back of the base fabric. 2) The burning speeds on both sides are 100 mm / min or less, and the ratio of the burning speeds on both sides is 1.0 or more and 3.0 or less. The airbag fabric according to any one of claims 1 to 4, wherein
6. An airbag base fabric described in any one of claims 1 to 5, having a blade combing resistance of 350 N or more after 400 hours under an environment of 85°C and 95% relative humidity.
7. An airbag cushion comprising an airbag base fabric according to any one of claims 1 to 6.
8. An airbag comprising an airbag base fabric according to any one of claims 1 to 6.