Method for regenerating cesium iodide and cesium iodide regeneration product
By leveraging solubility differences in water, the method selectively recovers cesium iodide from a mixture with thallium iodide, producing a high-purity cesium iodide product through controlled dissolution, precipitation, and drying processes.
Patent Information
- Application Number
- JP2023064129
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-24
AI Technical Summary
Existing methods for recovering cesium iodide from a mixture with thallium iodide lack selectivity, necessitating improvements for efficient separation and purification.
Utilizing water as a solvent to exploit the difference in solubility of cesium iodide and thallium iodide, the method involves dissolving the mixture, precipitating thallium iodide, and then drying to obtain highly pure cesium iodide through controlled temperature and concentration adjustments.
Achieves selective recovery of cesium iodide with low thallium iodide content, resulting in a high-purity cesium iodide product suitable for recycling and improved product performance.
Smart Images

Figure 2024151021000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for regenerating cesium iodide and a regenerated cesium iodide product. [Background technology]
[0002] Various methods for recovering inorganic iodides have been developed so far. One such technique is disclosed in Patent Document 1. Patent Document 1 describes that an organic solvent is added to an aqueous solution of mixed inorganic salts of reaction waste containing inorganic iodides, and the organic solvent layer separated into two layers (aqueous two-layer extraction) is separated and the organic solvent is concentrated, thereby isolating an aqueous solution or crystals of inorganic iodides dissolved in the organic solvent (paragraph 0012 of Patent Document 1, etc.). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2005-314158 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, as a result of investigations by the present inventors, it was found that the method for recovering inorganic iodides described in Patent Document 1 above has room for improvement in terms of selectively recovering cesium iodide from a mixture of cesium iodide and thallium iodide. [Means for solving the problem]
[0005] After further investigation, the inventors found that by selecting water as an appropriate solvent and utilizing the difference in solubility in water between cesium iodide and thallium iodide, thallium iodide can be selectively removed from an aqueous solution containing both of them outside the aqueous system, thereby making it possible to selectively recover (purify) cesium iodide in an aqueous system, and thus completed the present invention.
[0006] According to one aspect of the present invention, there is provided the following cesium iodide regenerating method and cesium iodide regenerated product. 1. A method for regenerating cesium iodide, comprising a purification step of selectively removing at least a portion of the thallium iodide using an aqueous solution containing cesium iodide and thallium iodide, thereby obtaining a regenerated cesium iodide product by leaving at least a portion of the cesium iodide in the aqueous solution. 2. A method for regenerating cesium iodide according to claim 1, comprising the steps of: The method for regenerating cesium iodide, wherein the purification step includes a dissolution step of adding an aqueous solvent to a mixture containing cesium iodide and thallium iodide, and preparing the aqueous solution in which the cesium iodide and the thallium iodide are dissolved in the aqueous solvent. 3. A method for regenerating cesium iodide according to 1. or 2., comprising the steps of: The method for regenerating cesium iodide, wherein the purification step includes a filtration step of removing the thallium iodide precipitated in the aqueous solution by solid-liquid separation. 4. A method for regenerating cesium iodide according to claim 3, comprising the steps of: The method for regenerating cesium iodide, wherein the purification step includes a drying step of removing water from the aqueous solution in which at least a portion of the cesium iodide is dissolved after the filtration step. 5. A method for regenerating cesium iodide according to any one of 1. to 4., comprising the steps of: A method for regenerating cesium iodide, comprising a recovery step of recovering a solid or liquid mixture containing cesium iodide and thallium iodide from a product produced using raw materials containing cesium iodide and thallium iodide or waste generated from a production device thereof. 6. A method for regenerating cesium iodide according to any one of 1. to 5., comprising the steps of: A method for regenerating cesium iodide, comprising the step of purifying the thallium iodide removed in the purification step. 7. A method for regenerating cesium iodide according to any one of 1. to 6., comprising the steps of: The method for regenerating cesium iodide, wherein the temperature of the aqueous solution when at least a portion of the thallium iodide is selectively removed during the purification step is 5°C or higher and 50°C or lower. 8. A cesium iodide regenerator comprising cesium iodide and thallium iodide, A cesium iodide regenerator, wherein the content of thallium iodide is 50 ppm or less by mass relative to the cesium iodide. 9. The cesium iodide regenerator according to claim 8, A cesium iodide regenerator having a content of thallium iodide of 30 ppm or less by mass relative to the cesium iodide. 10. The cesium iodide regenerator according to 8. or 9., Cesium iodide regenerator with a moisture content of 800 ppm or less as measured by a Karl Fischer moisture meter. 11. A cesium iodide regenerator according to any one of 8. to 10., Cesium iodide reclaimed material with a content of metal impurities other than I, Cs, and Tl of 1000 ppm or less as measured by IPC optical emission spectrometry. 12. The cesium iodide regenerator according to claim 11, A cesium iodide regenerator, wherein the metal impurities include one or more selected from the group consisting of Fe, Li, Na, K, Rb, Mg, Ca, Sr, Ba, Al, Cr, Mn, Ni, Cu, Zn, Ag, Si, and P. Effect of the Invention
[0007] According to the present invention, there are provided a method for regenerating cesium iodide which has excellent selectivity for cesium iodide relative to thallium iodide, and a regenerated cesium iodide product. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a flow diagram showing an example of a cesium iodide regeneration process according to the present embodiment. [Diagram 2]FIG. 1 is a diagram illustrating an example of the configuration of a cesium iodide regeneration system according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given similar reference numerals and their explanations will be omitted as appropriate. Also, the drawings are schematic diagrams and do not correspond to the actual dimensional ratios.
[0010] The outline of the cesium iodide regeneration method of this embodiment will be described.
[0011] The method for regenerating cesium iodide of the present embodiment includes a purification step of selectively removing at least a portion of the thallium iodide using an aqueous solution containing cesium iodide and thallium iodide, thereby obtaining a regenerated cesium iodide product by leaving at least a portion of the cesium iodide in the aqueous solution.
[0012] According to the findings of the present inventors, the difference in the water solubility of each element, that is, cesium iodide is easily soluble in water and thallium iodide is slightly soluble in water, may have a similar tendency in an aqueous solution of a mixture of these elements, and it has been found that one of them can be selectively recovered from the aqueous solution. Specifically, it has been found that by precipitating slightly water-soluble thallium iodide in an aqueous solution and removing it, it is possible to selectively leave (recover) the water-soluble cesium iodide in the aqueous solution.
[0013] Further investigation by the present inventors has led to the discovery that the solubility of thallium iodide in the aqueous solution of the mixture can be adjusted by the liquid temperature, the cesium iodide concentration in the aqueous solution, etc. Based on this discovery, it is possible to further increase the selectivity of cesium iodide relative to thallium iodide by controlling the process conditions so that the solubility of thallium iodide is reduced.
[0014] According to the cesium iodide regeneration method of this embodiment, it is possible to selectively recover (recycle) cesium iodide from products (such as scintillators) that use thallium-activated cesium iodide or waste from the manufacturing process thereof.
[0015] The configuration of the cesium iodide regeneration method of this embodiment will be described in detail below.
[0016] Fig. 1 is a flow diagram showing an example of a cesium iodide regeneration process. Fig. 2 is a schematic diagram showing an example of the configuration of a cesium iodide regeneration system.
[0017] In the method for regenerating cesium iodide, an example of a purification process for obtaining a regenerated cesium iodide product includes a dissolving process, a filtering process, and a drying process, as shown in FIG.
[0018] The purification steps described above can be carried out using the system 100 shown in FIG. The cesium iodide regeneration system (hereinafter referred to as system 100) in FIG. 2 includes a dissolution tank 10, a filtration device 20, a storage tank 30, and a drying device 40.
[0019] In the dissolving step of FIG. 1, an aqueous solution in which cesium iodide and thallium iodide are dissolved in the aqueous solvent 2 is prepared by adding an aqueous solvent 2 to a mixture 1 containing cesium iodide and thallium iodide.
[0020] 2, the mixture 1 and the aqueous solvent 2 are each supplied via a line (piping) to a dissolution tank 10. In the dissolution tank 10, cesium iodide and thallium iodide are dissolved in the aqueous solvent 2. The dissolution tank 10 may be equipped with a stirrer that stirs the aqueous solution containing the mixture 1 and the water solvent 2 at an appropriate rotation speed.
[0021] Mixture 1 is derived from waste materials containing cesium iodide and thallium iodide, from which cesium iodide is regenerated. Mixture 1 can be in either a solid or liquid form. The method for regenerating cesium iodide may include a recovery step of recovering a solid mixture 1 or a liquid mixture 1 containing cesium iodide and thallium iodide from the waste prior to the dissolving step.
[0022] Examples of waste materials include scrap products manufactured using raw materials containing cesium iodide and thallium iodide, such as products that use thallium-activated cesium iodide (scintillators, flat panel detectors, non-flat panel scintillators, etc.), waste materials discharged during the manufacturing process, and waste materials generated when cleaning equipment used in manufacturing (distillation equipment, etc.).
[0023] In order to recover the mixture 1 from the manufacturing equipment, for example, when cleaning an apparatus such as a distillation apparatus, a method of removing the deposits attached to the apparatus with a spatula or a method of removing such deposits with washing water can be used. In this case, the mixture 1 can be solid deposits or washing water containing deposits. Waste liquid such as washing water containing deposits may be subjected to a known pretreatment such as filtering before being used as the mixture 1. That is, the liquid mixture 1 obtained in the recovery step may be used as an aqueous solution as it is, or may be used after being pretreated, and if necessary, a water solvent may be added after the pretreatment.
[0024] The aqueous solvent 2 is not particularly limited as long as it contains water, but may contain water (H20) as the main component (50% by mass of the total amount). The water content in the aqueous solvent 2 may be, for example, 80% by mass or more, or 90% by mass or more. Examples of the aqueous solvent 2 include distilled water and ion-exchanged water. The aqueous solvent 2 is permissible to contain trace amounts of impurities such as metal or nonmetal ions or compounds, as long as the effects of the present invention are not impaired. Similarly, the aqueous solvent 2 may contain solvents other than water, such as water-soluble alcohols such as methanol, ethanol, 1-propanol, and 2-propanol, water-soluble ketones such as acetone, acetaldehyde, and acetic acid, aldehydes, and carboxylic acids.
[0025] In the dissolution tank 10 of FIG. 2, at least a portion of thallium iodide is precipitated in an aqueous solution containing cesium iodide and thallium iodide.
[0026] According to the findings of the present inventors, when comparing the TI solubility in an aqueous solution of thallium iodide alone with the TI solubility in an aqueous solution saturated with cesium iodide, it has been found that the solubility of thallium iodide (TI solubility) in an aqueous solution saturated with cesium iodide is smaller at approximately 20 to 45°C (particularly approximately 25 to 40°C).
[0027] Based on these findings, the relationship between the cesium iodide concentration and the liquid temperature was further investigated for the TI solubility in the cesium iodide aqueous solution. As a result, it was found that the TI solubility is smaller when the CsI concentration (mass%) in the cesium iodide aqueous solution is about 15 to 45 mass%, more preferably about 20 to 40 mass%, than when the CsI concentration is other than 15 to 45 mass%. It was also found that in the case of an aqueous cesium iodide solution having a CsI concentration of about 15 to 45% by mass, the TI solubility is smaller when the liquid temperature is about 5 to 50°C, preferably about 10 to 40°C, and more preferably about 10 to 30°C, compared to other liquid temperatures. On the other hand, when the residual concentration of thallium iodide in cesium iodide when the aqueous solution was dried was examined, it was found that the residual concentration of thallium iodide could be reduced more effectively when the cesium iodide aqueous solution had a CsI concentration of approximately 20 to 40 mass% and a liquid temperature of approximately 5 to 25°C than under other conditions.
[0028] It is possible to determine an appropriate range for the cesium iodide concentration in the aqueous solution and the liquid temperature of the aqueous solution, taking into consideration the balance between the amount of thallium iodide removed from the aqueous solution and the amount of thallium iodide remaining after the aqueous solution is dried. This makes it possible to selectively precipitate at least a portion of the thallium iodide in an aqueous solution containing cesium iodide and thallium iodide, while leaving the cesium iodide dissolved.
[0029] In the purification step, the cesium iodide concentration in the aqueous solution before the subsequent solid-liquid separation can be preferably 20 to 45 mass%, more preferably 30 to 40 mass%, and / or the liquid temperature of the aqueous solution before the subsequent solid-liquid separation can be preferably 5 to 25°C, more preferably 10 to 20°C.
[0030] The dissolution tank 10 may also be equipped with a temperature sensor or a temperature regulator such as a heater or a cooler in order to adjust the temperature of the aqueous solution. In order to adjust the cesium iodide concentration in the aqueous solution, cesium iodide or a mixture containing cesium iodide may be supplied to the dissolution tank 10 through a separate line.
[0031] The purification step in FIG. 1 includes a filtration step of removing at least a portion of the thallium iodide precipitated in the aqueous solution by solid-liquid separation. As a method for separating thallium iodide into solid and liquid, known means such as filtration and crystallization are used.
[0032] The system 100 of FIG. The aqueous solution is supplied from the dissolution tank 10 through a line to the filtration device 20. The supplied aqueous solution is passed through a filtration layer in the filtration device 20, and the passed filtrate is collected in a storage tank 30. Meanwhile, thallium iodide precipitated in the aqueous solution remains in the filtration tank. As a result, the precipitated thallium iodide is removed, and the aqueous solution in which cesium iodide is dissolved can be recovered.
[0033] If necessary, hydrazine may be added to the filtrate recovered in the storage tank 30. This makes it possible to make the color of the filtrate transparent. In this case, the filtrate recovered in the storage tank 30 may be circulated back to the storage tank 30 in order to promote the reaction with hydrazine.
[0034] 1 includes a drying step for removing water from the aqueous solution in which at least a portion of the cesium iodide is dissolved, after the filtration step. A known method is used to remove water.
[0035] In the system 100 of Fig. 2, the aqueous solution collected in the storage tank 30 is supplied to the drying device 40 via a line. In the drying device 40, the aqueous solvent (e.g., water) in the aqueous solution is removed. This allows a dried regenerated cesium iodide product (purified product) to be collected.
[0036] A known drying device can be used as the drying device 40, for example, a continuous spray fluidized granulation dryer, etc. The drying speed and drying temperature of the drying device 40 can be set to known conditions.
[0037] The regeneration method may include a step of purifying the thallium iodide removed in the purification step of FIG. In the filtration step of FIG. 1, the residue 3 containing thallium iodide removed by the filtration device 20 may be purified based on another regeneration process. As an example of purification, the residue 3 can be dried by a known method to recover a regenerated thallium iodide product (purified product) containing thallium iodide.
[0038] The cesium iodide regenerated product obtained by the regeneration method of this embodiment will be described in detail below.
[0039] The cesium iodide regenerated material contains cesium iodide as a main component, and does not contain thallium iodide, or if it does contain thallium iodide, the content of thallium iodide is 50 ppm or less, more preferably 30 ppm or less, and even more preferably 10 ppm or less, calculated by mass relative to the cesium iodide. The content of cesium iodide in the cesium iodide regenerated product is, for example, 98 mass % or more, preferably 99 mass % or more, and more preferably 99.99 mass % or more.
[0040] In another embodiment, the cesium iodide reclaimed product may contain trace amounts of other components other than cesium iodide and thallium iodide, as long as the components are permitted by the product or manufacturing process in which the product is used. Examples of other components include metal impurities.
[0041] The metal impurities may include, for example, one or more selected from the group consisting of Fe, Li, Na, K, Rb, Mg, Ca, Sr, Ba, Al, Cr, Mn, Ni, Cu, Zn, Ag, Si, and P.
[0042] The content of metal impurities other than I, Cs, and Tl in the cesium iodide regenerated material may be, for example, 1000 ppm or less, which can improve the performance of products in which cesium iodide is reused, such as scintillators manufactured using the cesium iodide regenerated material. When reusing, a predetermined amount of thallium iodide may be added to the regenerated cesium iodide.
[0043] The cesium iodide regenerant is a solid at room temperature, and its shape is not particularly limited, but it may be in the form of powder or granules.
[0044] The moisture content of the cesium iodide regenerated product measured by a Karl Fischer moisture meter is, for example, 800 ppm or less, preferably 500 ppm or less, and more preferably 100 ppm or less, which can improve prevention of caking.
[0045] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES
[0046] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.
[0047] <Cesium iodide purification> Example 1 200 g of cesium iodide scrap was dissolved in 400 g of water, and the solution was filtered while maintaining the liquid temperature at 18° C. The filtrate was dried at 110° C. to obtain a purified cesium iodide product. The cesium iodide yield in Example 1 was 92% by weight. The amount of thallium remaining in the refined product in Example 1 was 12 ppm by weight.
[0048] Example 2 200 g of cesium iodide scrap was dissolved in 1130 g of water, and the solution was filtered while maintaining the liquid temperature at 23° C. The filtrate was dried at 110° C. to obtain a purified cesium iodide product. The cesium iodide yield in Example 2 was 92% by weight. The amount of thallium remaining in the refined product in Example 2 was 13 ppm by weight.
[0049] Comparative Example 1 200g of cesium iodide scrap was dissolved in 173g of water, and the liquid temperature was lowered to 3°C to precipitate crystals. The solution containing the crystals was filtered using filter paper, and the crystals (residue) were dried at 110°C to obtain purified cesium iodide. The cesium iodide yield in Comparative Example 1 was 55% by weight. The amount of thallium remaining in the refined product in Comparative Example 1 was 1.3% by weight.
[0050] The cesium iodide purification methods of Examples 1 and 2 showed results of a higher yield and a smaller amount of thallium remaining compared to Comparative Example 1. Furthermore, Examples 1 and 2 are simpler methods than Comparative Example 1 in that they do not require the effort of recovering the residue remaining on the filter paper in the cesium iodide purification process. [Explanation of symbols]
[0051] 1 mixture 2 water 3 Residue 4. Cesium iodide regenerator 10 Dissolution tank 20 Filtration device 30 Storage Tank 40 Drying equipment 100 Cesium Iodide Regeneration System
Claims
1. A method for regenerating cesium iodide, comprising a purification step of selectively removing at least a portion of the thallium iodide using an aqueous solution containing cesium iodide and thallium iodide, thereby obtaining a regenerated cesium iodide product by leaving at least a portion of the cesium iodide in the aqueous solution.
2. 2. A method for regenerating cesium iodide according to claim 1, comprising the steps of: The method for regenerating cesium iodide, wherein the purification step includes a dissolution step of adding an aqueous solvent to a mixture containing cesium iodide and thallium iodide, and preparing the aqueous solution in which the cesium iodide and the thallium iodide are dissolved in the aqueous solvent.
3. A method for regenerating cesium iodide according to claim 1 or 2, comprising the steps of: The method for regenerating cesium iodide, wherein the purification step includes a filtration step of removing the thallium iodide precipitated in the aqueous solution by solid-liquid separation.
4. 4. A method for regenerating cesium iodide according to claim 3, comprising the steps of: The method for regenerating cesium iodide, wherein the purification step includes a drying step of removing water from the aqueous solution in which at least a portion of the cesium iodide is dissolved after the filtration step.
5. A method for regenerating cesium iodide according to claim 1 or 2, comprising the steps of: A method for regenerating cesium iodide, comprising a recovery step of recovering a solid or liquid mixture containing cesium iodide and thallium iodide from a product produced using raw materials containing cesium iodide and thallium iodide or waste generated from a production device thereof.
6. A method for regenerating cesium iodide according to claim 1 or 2, comprising the steps of: A method for regenerating cesium iodide, comprising the step of purifying the thallium iodide removed in the purification step.
7. A method for regenerating cesium iodide according to claim 1 or 2, comprising the steps of: The method for regenerating cesium iodide, wherein the temperature of the aqueous solution when at least a portion of the thallium iodide is selectively removed during the purification step is 5°C or higher and 50°C or lower.
8. A cesium iodide regenerator comprising cesium iodide and thallium iodide, A cesium iodide regenerator, wherein the content of thallium iodide is 50 ppm or less by mass relative to the cesium iodide.
9. 9. The cesium iodide regenerator according to claim 8, A cesium iodide regenerator, wherein the content of thallium iodide is 30 ppm or less by mass relative to the cesium iodide.
10. The cesium iodide regenerator according to claim 8 or 9, A cesium iodide regenerator having a moisture content of 800 ppm or less as measured by a Karl Fischer moisture meter.
11. The cesium iodide regenerator according to claim 8 or 9, A cesium iodide regenerator having a content of metal impurities other than I, Cs, and Tl of 1000 ppm or less as measured by IPC emission spectrometry.
12. 12. The cesium iodide regenerator of claim 11, The cesium iodide regenerator, wherein the metal impurities include one or more selected from the group consisting of Fe, Li, Na, K, Rb, Mg, Ca, Sr, Ba, Al, Cr, Mn, Ni, Cu, Zn, Ag, Si, and P.
Citation Information
Patent Citations
Method for recovering inorganic iodide
JP2005314158A
Cited By
Methods for recovering iodide scrap
JP2026113365A
Methods for recovering iodide scrap
JP7916485B2