Magnetic powder including metal oxide comprising m-type hexagonal ferrite as main phase, sintered body thereof, and high-frequency magnetic component

A magnetic powder with M-type hexagonal ferrite addresses the limitations of existing high-frequency components by providing high magnetic permeability, density, and low loss coefficient, enabling miniaturized and high-performance components.

JP2024152255APending Publication Date: 2024-10-25JAPAN METALS & CHEM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023066333
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing high-frequency magnetic components face limitations in magnetic permeability, density, and loss coefficient, particularly in the GHz band, making them unsuitable for high-frequency applications and requiring multiple ferrite materials for different frequency bands.

Method used

A magnetic powder with M-type hexagonal ferrite as the main phase, composed of specific metal elements in defined molar ratios, achieving high magnetic permeability, density, and low loss coefficient, suitable for GHz frequencies.

Benefits of technology

The solution provides a sintered body with enhanced magnetic permeability, density, and reduced loss coefficient, enabling miniaturization and improved performance of high-frequency components like antennas and EMI filters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152255000001
    Figure 2024152255000001
  • Figure 2024152255000002
    Figure 2024152255000002
Patent Text Reader

Abstract

To provide: magnetic powder including a metal oxide which has high magnetic permeability in hundreds of MHz to GHz band and high density, with which a sintered body having small loss coefficient can be obtained, and which comprises M-type hexagonal ferrite as a main phase; a sintered body of the magnetic powder; and a high-frequency magnetic component including the sintered body.SOLUTION: A high-frequency magnetic component is magnetic powder that includes a metal oxide comprising M-type hexagonal ferrite as a main phase, and includes MA, MB, MC and Fe as constituent metal elements. MA is at least one selected from the group consisting of Ba, Sr, Pb, Ca, Ce, and La, MB is at least one selected from the group consisting of Co, Zn, Ni, Mn, Mg, Cu, and Bi, and MC is at least one selected from the group consisting of Ti, Sn, Zr, and Ir. When a molar ratio of MA is 1.00, the molar ratio of MB is 0.50 or more and 2.00 or less, the molar ratio of MC is 0.50 or more and 1.50 or less, and the molar ratio of Fe is 4.00 or more and 10.80 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a magnetic powder containing a metal oxide having M-type hexagonal ferrite as a main phase, a sintered body thereof, and a high-frequency magnetic component. [Background technology]

[0002] Magnetic materials such as ferrite materials are widely used as materials for forming magnetic parts such as antennas, inductors, noise filters, radio wave absorbers, etc. In recent years, electronic devices such as wireless communication devices are increasingly using higher frequency bands, and materials for forming magnetic parts used in such devices are required to have higher magnetic permeability in the range from several hundred MHz to GHz.

[0003] Generally, as the frequency is increased, the magnetic permeability of ferrite remains constant up to a certain frequency, after which it increases as the frequency increases, reaching a maximum value at a certain point. After passing the maximum value, the magnetic permeability decreases almost inversely proportional to the frequency. The frequency at which the magnetic permeability reaches its maximum value is the limit frequency (resonant frequency) at which the magnetic material can be used practically, and is called the "Snake limit."

[0004] In this case, the product of the magnetic permeability of the ferrite and the frequency (resonant frequency) at which the magnetic permeability is at its maximum value is almost constant, and the higher the magnetic permeability, the lower the resonant frequency. This product of the magnetic permeability and the resonant frequency is called the "snake boundary", and ferrite materials have had to be used with the "snake boundary" as a given. Therefore, it has been necessary to use different ferrite materials depending on the frequency band to be used, and ferrite materials with high magnetic permeability could not be used at high frequencies.

[0005] For example, spinel ferrite, known as soft magnetic ferrite, has a low magnetic permeability in the MHz band due to the Snake limit. At the same time, the magnetic loss (μ'') starts to increase and the loss coefficient (tan δ) becomes large. For this reason, spinel ferrite is not suitable for high-frequency magnetic parts.

[0006] On the other hand, among ferrite materials, hexagonal ferrite has magnetic anisotropy and can overcome the "Snake's limit". In other words, it can maintain high magnetic permeability up to high frequencies. For this reason, hexagonal ferrite is a magnetic material suitable for high-frequency magnetic parts.

[0007] Among hexagonal ferrites, Z-type hexagonal ferrite is known to have high magnetic permeability. However, the magnetic permeability of Z-type hexagonal ferrite starts to decrease at several hundred MHz. Therefore, it is not suitable for use at high frequencies from several hundred MHz to the GHz range.

[0008] For example, Patent Document 1 describes a soft magnetic composition that is a metal oxide containing specific metal elements in a specific composition and has W-type hexagonal ferrite as a main phase. The soft magnetic composition of Patent Document 1 is described as a hexagonal ferrite material that has high resistivity and high magnetic permeability in the GHz band. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. 2020 / 162295 Summary of the Invention [Problem to be solved by the invention]

[0010] The soft magnetic composition having W-type hexagonal ferrite as the main phase described in Patent Document 1 has a maximum magnetic permeability of 2.82 at 1 GHz (No. 43 in Table 4). However, this is still not satisfactory as a magnetic permeability for high-frequency magnetic parts, and higher values ​​are desired.

[0011] Generally, when high-frequency magnetic parts are used in mobile communications, they are required to have strength as a physical property since they may be subjected to shocks such as being dropped, etc. Furthermore, since the ferrite that constitutes high-frequency magnetic parts is usually a sintered body, it is required to have a high density in order to satisfy the required strength.

[0012] However, Patent Document 1 does not disclose the density of the soft magnetic composition containing W-type hexagonal ferrite as a main phase.

[0013] Furthermore, when a high-frequency magnetic part is used as an antenna, for example, it is desirable that the loss factor (tan δ) be small in order to suppress a decrease in sensitivity.

[0014] The present invention has been made to solve the above problems, and aims to provide a magnetic powder containing a metal oxide having M-type hexagonal ferrite as a main phase, which can produce a sintered body having high magnetic permeability in the hundreds of MHz to GHz band, high density, and a small loss factor, a sintered body thereof, and a high-frequency magnetic component using the same. [Means for solving the problem]

[0015] The inventors have found that, for example, BaFe 12 O 19 M-type hexagonal ferrite such as those described above has high saturation magnetization and large uniaxial anisotropy in the C-axis direction, and therefore it has been noted that it retains relatively high magnetic permeability up to a high frequency band of 50 GHz.

[0016] In addition, M-type hexagonal ferrite, which has been soft-magnetically modified by element substitution, is called BaCo x Ti x Fe 12-2x O 19 is a Co in a hexagonal crystal lattice. 2+ The inventors have focused on the fact that the inclusion of α reduces the uniaxial anisotropy in the C-axis direction, thereby increasing the magnetic permeability.

[0017] In order to solve the above problems, the present inventors have conducted further studies based on the above. As a result, in a metal oxide having M-type hexagonal ferrite as a main phase, Fe is reduced from the theoretical composition, and Fe 2+ They found that by suppressing the generation of , the metal oxide has high magnetic permeability in the hundreds of MHz to GHz range, high density, and low loss factor.

[0018] That is, the present invention includes the following aspects. [1] A magnetic powder containing a metal oxide having M-type hexagonal ferrite as a main phase, The constituent metal elements include MA, MB, MC, and Fe, MA is at least one selected from the group consisting of Ba, Sr, Pb, Ca, Ce, and La; MB is at least one selected from the group consisting of Co, Zn, Ni, Mn, Mg, Cu, and Bi; M is at least one selected from the group consisting of Ti, Sn, Zr, and Ir; When the molar ratio of MA to the constituent metal elements is 1.00, the molar ratio of MB to the constituent metal elements is 0.50 or more and 2.00 or less, the molar ratio of MC to the constituent metal elements is 0.50 or more and 1.50 or less, and the molar ratio of Fe to the constituent metal elements is 4.00 or more and 10.80 or less, The molar ratios of MB, MC, and Fe in the constituent metal elements satisfy the following formula (1): magnetic powder. 6.70≦MB+MC+Fe≦11.80 (1) [2] A sintered body of the magnetic powder according to aspect [1], A sintered body whose main phase is M-type hexagonal ferrite, and whose magnetic permeability is 2.5 or more in the range of 500 MHz to 1 GHz. [3] A sintered body of the magnetic powder according to aspect [1], Density is 4.6×10 3 kg / m 3 The above is a sintered body having M-type hexagonal ferrite as a main phase. [4] A high-frequency magnetic component including a sintered body mainly composed of an M-type hexagonal ferrite described in Embodiment [2] or [3].

Advantages of the Invention

[0019] According to the magnetic powder containing a metal oxide mainly composed of the M-type hexagonal ferrite of the present invention, a sintered body of a metal oxide having a high magnetic permeability in the range of several hundred MHz to GHz band, being of high density and having a low loss coefficient can be obtained, and a high-frequency magnetic component using the same can be obtained. The sintered body of the present invention and the high-frequency magnetic component using the same can be used as electronic components such as an inductor, an antenna, an EMI filter, and a radio wave absorber, thereby enabling miniaturization and high performance improvement thereof.

Modes for Carrying Out the Invention

[0020] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments. Further, constituent elements in the following embodiments include those that can be easily assumed by those skilled in the art, substantially identical ones, and those within a so-called equivalent range.

[0021] <Magnetic powder containing a metal oxide mainly composed of an M-type hexagonal ferrite> The magnetic powder containing a metal oxide mainly composed of the M-type hexagonal ferrite of the present disclosure contains, as constituent metal elements, MA, MB, MC, and Fe, MA is at least one selected from the group consisting of Ba, Sr, Pb, Ca, Ce, and La, MB is at least one selected from the group consisting of Co, Zn, Ni, Mn, Mg, Cu, and Bi, MC is at least one selected from the group consisting of Ti, Sn, Zr, and Ir, When the molar ratio of MA to the constituent metal elements is 1.00, the molar ratio of MB to the constituent metal elements is 0.50 or more and 2.00 or less, the molar ratio of MC to the constituent metal elements is 0.50 or more and 1.50 or less, the molar ratio of Fe to the constituent metal elements is 4.00 or more and 10.80 or less, and the molar ratios of MB, MC, and Fe to the constituent metal elements satisfy the following formula (1). 6.70≦MB+MC+Fe≦11.80 (1)

[0022] The magnetic powder containing a metal oxide having M-type hexagonal ferrite as a main phase according to the present disclosure has diffraction intensity peaks in the ranges of 31.9°≦2θ≦32.5° and 33.8°≦2θ≦34.5° in X-ray diffraction measurement using Cu-Kα radiation. These diffraction intensity peaks are derived from M-type hexagonal ferrite.

[0023] The magnetic powder of the present disclosure may have a content of M-type hexagonal ferrite of substantially 100% by mass, and may contain other phases as subphases and other components in addition to M-type hexagonal ferrite. Examples of other components include by-products other than M-type hexagonal ferrite that are generated during the manufacturing process of the magnetic powder.

[0024] Examples of the different phases that become subphases include other ferrites such as Y-type hexagonal ferrite, W-type hexagonal ferrite, Z-type hexagonal ferrite, and spinel ferrite, as well as oxides having a perovskite structure that are mainly composed of metal elements that become the constituent metal elements MA and MC and contain Fe as an optional component. It is preferable that the magnetic powder of the present disclosure contains a subphase and other components in addition to M-type hexagonal ferrite, in that a sintered body with high electrical resistance can be obtained.

[0025] The content of M-type hexagonal ferrite in the magnetic powder of the present disclosure is preferably 75% by mass or more from the viewpoint of improving magnetic permeability. The content of M-type hexagonal ferrite in the magnetic powder of the present disclosure is preferably less than 75% by mass from the viewpoint of loss factor. The lower limit of the content of M-type hexagonal ferrite may be, for example, 50% by mass or more, as long as the crystal structure of M-type hexagonal ferrite can be maintained. Here, the content of M-type hexagonal ferrite in the magnetic powder is calculated from the measurement results by X-ray diffraction measurement using Cu-Kα radiation on the magnetic powder and the reference intensity ratio method (RIR method).

[0026] In the magnetic powder containing a metal oxide having M-type hexagonal ferrite as the main phase of the present disclosure, since the hexagonal ferrite is M-type, it is easier to make it into a single phase compared to other types of hexagonal ferrite, and it is possible to stably produce it while controlling the ratio of M-type hexagonal ferrite to the subphase.

[0027] The M-type hexagonal ferrite contained in the magnetic powder of the present disclosure has a reduced amount of Fe compared to the theoretical composition. 3+ Co 2+ MB and Ti etc. 4+ The theoretical composition when MC is replaced with MAFe 12-x-y MB x MC y O 19 In comparison with the above, the amount of elements located at the Fe site is reduced, which may result in the formation of subphases.

[0028] The M-type hexagonal ferrite contained in the magnetic powder of the present disclosure has Fe reduced from the theoretical composition, so that Fe 2+It is presumed that the generation of is suppressed and the resistivity is improved. In addition, by subtracting Fe from the theoretical composition, lattice defects are generated at the location of the crystal lattice where Fe is coordinated, and therefore the Fe ions are positioned apart from each other, suppressing the hopping conduction caused by the valence fluctuation of the Fe ions, which is also presumed to contribute to the improvement of the resistivity. By improving the resistivity, the sintered body obtained from the magnetic powder of the present disclosure has reduced eddy current loss. Therefore, it is presumed that the magnetic flux generated in a direction that cancels the magnetic flux caused by the generation of eddy currents can be reduced, improving the magnetic permeability.

[0029] In addition, the M-type hexagonal ferrite contained in the magnetic powder of the present disclosure has a reduced Fe content compared to the theoretical composition, and depending on the degree of reduction, 2+ MB and Ti etc. 4+ It is presumed that the coordination site of MC in the M-type crystal structure changes. The change in the coordination site leads to a change in the anisotropy field H A It is presumed that the coercive force and saturation magnetization have been adjusted, improving the magnetic permeability.

[0030] Furthermore, the magnetic powder of the present disclosure may contain an oxide containing MA and MC that is generated as a subphase by reducing Fe from the theoretical composition of M-type hexagonal ferrite. This oxide may further contain Fe. The oxide preferably has a perovskite structure. By including an oxide having a perovskite structure as a subphase, the resistivity of the sintered body obtained from the magnetic powder of the present disclosure can be improved.

[0031] Among the constituent metal elements constituting the magnetic powder containing the metal oxide having the M-type hexagonal ferrite as the main phase of the present disclosure, MA is at least one selected from the group consisting of Ba, Sr, Pb, Ca, Ce, and La. Among the constituent metal elements, MA is preferably at least one selected from the group consisting of Ba and Sr. If MA is at least one selected from the group consisting of Ba and Sr, high saturation magnetization can be obtained.

[0032] Among the constituent metal elements constituting the magnetic powder containing a metal oxide having M-type hexagonal ferrite as a main phase according to the present disclosure, MB is at least one selected from the group consisting of Co, Zn, Ni, Mn, Mg, Cu, and Bi. Among the constituent metal elements, MB is preferably at least one selected from the group consisting of Co and Zn. If MB is at least one selected from the group consisting of Co and Zn, the coercive force can be reduced and soft magnetism can be achieved. Furthermore, when the M-type hexagonal ferrite is Co, 2+ When ions are contained, the uniaxial magnetic anisotropy in the C-axis direction of the M-type crystal structure is relaxed, which is preferable since a higher magnetic permeability can be obtained in the high frequency band.

[0033] Among the constituent metal elements constituting the magnetic powder containing a metal oxide having M-type hexagonal ferrite as a main phase according to the present disclosure, M is at least one selected from the group consisting of Ti, Sn, Zr, and Ir. Among the constituent metal elements, M is preferably at least one selected from the group consisting of Ti and Sn. Furthermore, when the M-type hexagonal ferrite contains Ti, the density is 4.6×10 3 kg / m 3 This is preferable in that the above-mentioned M-type hexagonal ferrite sintered body can be obtained.

[0034] In the magnetic powder containing the metal oxide having M-type hexagonal ferrite as the main phase of the present disclosure, the molar ratio of MB to the constituent metal elements is 0.50 to 2.00, and the molar ratio of MC to the constituent metal elements is 0.50 to 1.50, when the molar ratio of MA to the constituent metal elements is 1.00. If the molar ratio of MB and the molar ratio of MC are within the above ranges, the coercive force can be reduced while maintaining high saturation magnetization, which can contribute to high magnetic permeability in the GHz band.

[0035] The molar ratio of Fe in the constituent metal elements constituting the magnetic powder containing the metal oxide having the M-type hexagonal ferrite as the main phase of the present disclosure is 4.00 or more and 10.80 or less, when the molar ratio of MA in the constituent metal elements is 1.00. If the molar ratio of Fe is within the above range, M-type hexagonal ferrite that contributes to high magnetic permeability in the GHz band can be sufficiently generated. From the viewpoint of high magnetic permeability, the molar ratio of Fe in the constituent metal elements is preferably 7.80 or more and 9.10 or less, and from the viewpoint of low magnetic loss, it is preferably 4.00 or more and 7.80 or less, and particularly preferably 4.00 or more and 5.50 or less.

[0036] In the magnetic powder containing a metal oxide having M-type hexagonal ferrite as a main phase according to the present disclosure, when the molar ratio of MA among the constituent metal elements constituting the magnetic powder is taken as 1.00, the molar ratios of MB, MC, and Fe among the constituent metal elements satisfy the following formula (1): By having the molar ratios of MB, MC, and Fe satisfy the following formula (1), it is possible to reduce the coercive force while maintaining high saturation magnetization, which can contribute to high magnetic permeability in the GHz band. 6.70≦MB+MC+Fe≦11.80 (1)

[0037] The composition of the magnetic powder of the present disclosure is determined by determining the molar concentration of each element contained in the magnetic powder through composition analysis using inductively coupled plasma atomic emission spectroscopy (ICP-AES), and then determining the ratio of Fe, MB, and MC when the sum of the molar concentrations of the above MA in the constituent metal elements is taken as 1.00.

[0038] [Method for producing magnetic powder containing metal oxide with M-type hexagonal ferrite as the main phase] The magnetic powder containing a metal oxide having M-type hexagonal ferrite as a main phase according to the present disclosure can be obtained by a conventional solid-phase reaction method. For example, raw materials are weighed and wet-mixed to obtain a target composition, and the resulting mixed powder is dried and then fired at 1200°C for 2 hours in air, thereby obtaining the magnetic powder containing a metal oxide having M-type hexagonal ferrite as a main phase according to the present disclosure.

[0039] <Sintered body mainly composed of M-type hexagonal ferrite> The sintered body mainly composed of M-type hexagonal ferrite of the present disclosure is a sintered body of magnetic powder containing the above-described metal oxide mainly composed of M-type hexagonal ferrite of the present disclosure. Specifically, for example, it is manufactured by molding the above-described magnetic powder of the present disclosure into a predetermined shape and firing it. Before molding, SiO2 and / or CaCO3 may be added as additives, or the magnetic powder may be pulverized into fine powder by wet pulverization and dried.

[0040] [Magnetic permeability] The sintered body mainly composed of M-type hexagonal ferrite of the present disclosure may have a magnetic permeability (μ') in the range of 500 MHz or more and 1 GHz or less of 2.5 or more. If the magnetic permeability in the range of 500 MHz or more and 1 GHz or less is 2.5 or more, the sintered body mainly composed of M-type hexagonal ferrite of the present disclosure can be sufficiently miniaturized when used as a high-frequency magnetic component, for example, as an antenna.

[0041] When the magnetic permeability is μ' and the dielectric constant is ε', the wavelength λ of the electromagnetic wave passing through the magnetic material has the relationship shown in the following formula. Therefore, if at least one of the magnetic permeability μ' and the dielectric constant ε' is increased, the wavelength λ becomes smaller. Therefore, according to the sintered body mainly composed of M-type hexagonal ferrite of the present disclosure having a large magnetic permeability, high-frequency magnetic components such as antennas can be miniaturized. λ ∝ 1 / √(μ' × ε')

[0042] [Loss factor] The sintered body mainly composed of M-type hexagonal ferrite of the present disclosure preferably maintains a loss factor (tanδ) in the range of 500 MHz or more and 1 GHz or less of 1.0 or less. By maintaining the loss factor (tanδ) at 1.0 or less, the sintered body of the present disclosure can be sufficiently used as a magnetic component. As a method of lowering the loss factor (tanδ), for example, while maintaining a high saturation magnetization, increasing the value of z to control the anisotropic magnetic field H A can be mentioned. Also, improving the specific resistance can be mentioned.

[0043] The loss factor (tan δ) in the range of 500 MHz to 1 GHz of the sintered body having M-type hexagonal ferrite as a main phase of the present disclosure is preferably 0.5 or less, more preferably 0.2 or less, even more preferably 0.10 or less, and most preferably 0.05 or less.

[0044] [density] The sintered body of the present disclosure having M-type hexagonal ferrite as the main phase has a density of 4.6 × 10 3 kg / m 3 The density is 4.6×10 3 kg / m 3 If the above is the case, a high-strength high-frequency magnetic component can be provided, which can be suitably used, for example, in mobile communications where shocks are likely to occur.

[0045] The density of the sintered body having M-type hexagonal ferrite as the main phase of the present disclosure is 4.6 × 10 3 kg / m 3 As a method for achieving the above, for example, TiO2 is used as a raw material for the magnetic powder containing a metal oxide having M-type hexagonal ferrite as a main phase according to the present disclosure, and Ti is included as MC in the constituent metal elements.

[0046] [Coercive force] The sintered body having the M-type hexagonal ferrite as the main phase of the present disclosure may have a coercive force of 100 kA / m or less. The sintered body having the M-type hexagonal ferrite as the main phase of the present disclosure has an anisotropic magnetic field H A By controlling the coercive force to be 100 kA / m or less, the sintered body of the present disclosure having M-type hexagonal ferrite as a main phase can be made magnetically soft.

[0047] <High-frequency magnetic components> The high-frequency magnetic part of the present disclosure includes a sintered body having the above-mentioned M-type hexagonal ferrite as a main phase. As long as it includes the sintered body having the M-type hexagonal ferrite as a main phase of the present disclosure, it is not particularly limited, but examples thereof include inductors, EMI filters used for noise suppression, and radio wave absorbers used in wireless communication devices, and can be used as electronic components of electronic devices or wireless communication devices. The high-frequency magnetic part of the present disclosure may also be an antenna using an M-type hexagonal ferrite sintered body with a particularly low loss factor. EXAMPLES

[0048] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these.

[0049] <Example 1> [Preparation of magnetic powder (calcined powder) containing metal oxides with M-type hexagonal ferrite as the main phase] Fe2O3, BaCO3, SrCO3, Co3O4, ZnO, H3BO3, SnO2, or TiO2 were weighed out so that the constituent metal elements of the magnetic powder containing a metal oxide with M-type hexagonal ferrite as the main phase were in the ratio shown in Table 1, and mixed in an attritor for 1 hour using water as a medium to obtain a mixed powder. The obtained mixed powder was dried and then calcined in air at 1200°C for 2 hours to obtain a magnetic powder (calcined powder) containing a metal oxide with M-type hexagonal ferrite as the main phase.

[0050] [Preparation of sintered bodies with M-type hexagonal ferrite as the main phase] The obtained magnetic powder (calcined powder) containing metal oxides with M-type hexagonal ferrite as the main phase was added with appropriate amounts of SiO2 and CaCO3, and ground in a planetary ball mill using water as a medium for 2 hours to produce ground powder. The ground powder was added with 1% binder (PVA) and granulated. The granulated powder was compression molded into ring and disk shapes, and the obtained molded bodies were fired in air at 1100°C for 8 hours to obtain ring-shaped sintered bodies with an outer diameter of 1.7 mm, an inner diameter of 1.0 mm, and a height of 0.5 mm, and disk-shaped sintered bodies with a diameter of 34 mm and a thickness of 1.8 mm, as sintered bodies with M-type hexagonal ferrite as the main phase.

[0051] <Examples 2 to 27 and Comparative Examples 1 to 5> [Preparation of magnetic powder (calcined powder) containing metal oxides with M-type hexagonal ferrite as the main phase] Fe2O3, BaCO3, SrCO3, Co3O4, ZnO, H3BO3, SnO2, or TiO2 was weighed out so that the constituent metal elements of the magnetic powder containing a metal oxide having M-type hexagonal ferrite as the main phase were in the ratio shown in Table 1, and a magnetic powder (calcined powder) containing a metal oxide having M-type hexagonal ferrite as the main phase was obtained in the same manner as in Example 1.

[0052] [Preparation of sintered bodies with M-type hexagonal ferrite as the main phase] A ring-shaped M-type hexagonal ferrite sintered body and a disk-shaped M-type hexagonal ferrite sintered body were obtained in the same manner as in Example 1, except that the sintering was performed in air at 1200° C. for 2 hours.

[0053] <Example 28> Fe2O3, BaCO3, Co3O4, ZnO, and TiO2 were weighed out so that the constituent metal elements of the magnetic powder containing a metal oxide having M-type hexagonal ferrite as the main phase were in the ratios shown in Table 1, and a magnetic powder (calcined powder) containing a metal oxide having M-type hexagonal ferrite as the main phase was produced in the same manner as in Example 1. Next, a ring-shaped M-type hexagonal ferrite sintered body and a disk-shaped M-type hexagonal ferrite sintered body were obtained in the same manner as in Example 2, except that SiO2 and CaCO3 were not added.

[0054] [Table 1]

[0055] [measurement] The following measurements were carried out on the obtained ring-shaped sintered body having M-type hexagonal ferrite as the main phase. The measurement results are shown in Table 2. In Table 2, "-" indicates that the measurement was not carried out.

[0056] (density) For the ring-shaped sintered body having M-type hexagonal ferrite as the main phase, the volume was measured using a vernier caliper and a micrometer, and the mass was then measured using an electronic balance. The density was calculated by dividing the mass by the volume.

[0057] (Magnetic permeability (μ'), loss coefficient (tanδ)) The magnetic permeability (μ') and loss factor (tanδ) at 25℃ were measured for the sintered body with ring-shaped M-type hexagonal ferrite as the main phase using an impedance analyzer (Agilent E4991A). Table 2 shows the results for frequencies from 500MHz to 1GHz.

[0058] (specific resistance) The resistivity (volume resistivity) of the sintered body consisting of disk-shaped M-type hexagonal ferrite as the main phase was measured using a resistivity meter (model: Analytech Hiresta-UX MCP-HT800, Mitsubishi Chemical Corporation).

[0059] (Saturation magnetization, coercive force) For the crushed powder of the sintered body having ring-shaped M-type hexagonal ferrite as the main phase, the saturation magnetization and coercivity were measured by magnetization curve at 25°C and a maximum magnetic field of 16 kOe using a vibration sample magnetometer (model: VSM-P7, Toei Kogyo Co., Ltd.).

[0060] [Table 2]

[0061] All of the sintered bodies having M-type hexagonal ferrite as the main phase in Examples 1 to 28 within the scope of the present invention had a magnetic permeability of 2.5 or more at 500 MHz, 800 MHz, and 1 GHz, and a density of 4.6 × 10 3 kg / m 3or more. On the other hand, Comparative Example 1, in which MC was Ti and y was 2.00, had a high density but a magnetic permeability of less than 2.5 at 1 GHz. Comparative Example 2, which contained neither MB nor MC, and Comparative Examples 4 and 5, in which MB was boron (B), did not reach a magnetic permeability of 2.5 at any frequency. Comparative Example 3, in which Fe was not reduced from the theoretical composition, had a magnetic permeability of 2.5 or more in the range of 500 MHz to 1 GHz and a density of 4.6×10 3 kg / m 3 The results were as above, but the loss factor (tan δ) was large.

[0062] Comparing Example 26 and Example 28, Example 28, which did not contain SiO2 and CaCO3, showed a slight increase in permeability due to an increase in the amount of domain walls accompanying an increase in the crystal grain size, but the permeability at 1 GHz was almost the same. However, the sintered density of Example 26 was significantly higher than that of Example 28. This shows that the density of a sintered body having M-type hexagonal ferrite as the main phase to which SiO2 and CaCO3 are added as additives is significantly increased. [Industrial Applicability]

[0063] According to the magnetic powder containing a metal oxide having M-type hexagonal ferrite as a main phase of the present invention, a sintered body suitable for use in high frequency bands from several hundred MHz to the GHz band can be obtained. Therefore, the magnetic powder containing a metal oxide having M-type hexagonal ferrite as a main phase of the present invention and the sintered body thereof can be suitably used for high frequency magnetic parts such as inductors, EMI filters, and radio wave absorbers. In addition, according to a preferred embodiment of the present invention, a sintered body having a particularly low loss factor can be obtained, so that it can be suitably used for magnetic parts such as antennas.

Claims

1. A magnetic powder containing a metal oxide having M-type hexagonal ferrite as a main phase, Constituent metal elements include MA, MB, MC, and Fe, MA is at least one selected from the group consisting of Ba, Sr, Pb, Ca, Ce, and La; MB is at least one selected from the group consisting of Co, Zn, Ni, Mn, Mg, Cu, and Bi; M is at least one selected from the group consisting of Ti, Sn, Zr, and Ir; When the molar ratio of MA to the constituent metal elements is 1.00, the molar ratio of MB to the constituent metal elements is 0.50 or more and 2.00 or less, the molar ratio of MC to the constituent metal elements is 0.50 or more and 1.50 or less, and the molar ratio of Fe to the constituent metal elements is 4.00 or more and 10.80 or less, The molar ratios of MB, MC, and Fe in the constituent metal elements satisfy the following formula (1): magnetic powder. 6.70≦MB+MC+Fe≦11.80 (1)

2. A sintered body of the magnetic powder according to claim 1, A sintered body having M-type hexagonal ferrite as a main phase, the sintered body having a magnetic permeability of 2.5 or more in the range of 500 MHz to 1 GHz.

3. A sintered body of the magnetic powder according to claim 1, Density is 4.6 x 10 3 kg / m 3 The above is a sintered body having M-type hexagonal ferrite as a main phase.

4. A high-frequency magnetic part comprising a sintered body having the M-type hexagonal ferrite as defined in claim 2 or 3 as a main phase.

Citation Information

Patent Citations

  • Soft magnetic composition, sintered compact, composite, paste, coil component, and antenna