Lithium metal composite oxide, cathode active material for lithium secondary battery, cathode for lithium secondary battery, and lithium secondary battery

A lithium metal composite oxide with controlled composition and structure enhances lithium secondary battery cycle characteristics by improving lithium ion diffusion, leading to better battery performance.

JP2024153456AActive Publication Date: 2024-10-29SUMITOMO METAL MINING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023067359
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-29
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

Lithium secondary batteries require further improvements in cycle characteristics as their application fields expand.

Method used

A lithium metal composite oxide with a layered structure containing Co, element M1 (Si, Ca, or Na), and element M2 (Fe or Mg) is developed, with specific molar ratios and diffraction peak intensity ratios, along with controlled BET surface area, particle size distribution, and particle strength to enhance lithium ion diffusion.

Benefits of technology

The lithium metal composite oxide provides lithium secondary batteries with excellent cycle characteristics, maintaining high capacity retention over multiple charge-discharge cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153456000002
    Figure 2024153456000002
  • Figure 2024153456000003
    Figure 2024153456000003
  • Figure 2024153456000001
    Figure 2024153456000001
Patent Text Reader

Abstract

To provide a lithium metal composite oxide capable of producing a lithium secondary battery having excellent cycle properties.SOLUTION: Disclosed herein is a lithium metal composite oxide having a lamellar structure and satisfying the following (1) and (2). (1) The composite oxide includes Co, an element M1, and an element M2, with a molar ratio of the element M1 to the Co being 0.05 or over and 6 or under; the element M1 is at least one or more selected from the group consisting of Si, Ca, and Na, and the element M2 is at least one or more elements selected from the group consisting of Fe and Mg. (2) In an X-ray diffraction measurement using CuKα ray, two diffraction peaks exist in a range of 2θ=38.0±0.5°, and among the two diffraction peaks, when a diffraction peak on a low angle side is peak A and a diffraction peak on a high angle side is peak B, the following formula 0.50≤IA / IB≤0.75 is satisfied (IA is a peak area of the peak A, and IB is a peak area of the peak B).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lithium metal composite oxide, a positive electrode active material for a lithium secondary battery, a positive electrode for a lithium secondary battery, and a lithium secondary battery. [Background technology]

[0002] Lithium metal composite oxides are used as positive electrode active materials for lithium secondary batteries. The physical properties of lithium metal composite oxides affect the performance of lithium secondary batteries. For this reason, lithium metal composite oxides have been actively developed to improve the performance of lithium secondary batteries.

[0003] For example, Patent Document 1 discloses that a lithium metal composite oxide having a diffraction peak intensity ratio I(006) / I(102) of 0.44 or less between the (006) and (102) planes in the X-ray diffraction Miller indices hkl and satisfying other physical properties improves the charge / discharge capacity and rate characteristics of a lithium secondary battery. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP-A-2013-112531 Summary of the Invention [Problem to be solved by the invention]

[0005] As the range of applications for lithium secondary batteries expands, there is a demand for further improvements in their cycle characteristics.

[0006] An object of the present invention is to obtain a lithium metal composite oxide capable of providing a lithium secondary battery having excellent cycle characteristics.

[0007] A further object of the present invention is to provide a positive electrode active material for a lithium secondary battery, a positive electrode for a lithium secondary battery, and a lithium secondary battery, each containing the above-mentioned lithium metal composite oxide. [Means for solving the problem]

[0008] The present invention includes the following [1] to

[11] . [1] A lithium metal composite oxide having a layered structure and satisfying the following (1) and (2): (1) It contains Co, an element M1, and an element M2, and the molar ratio of the element M1 to the Co is 0.05 to 6. The element M1 is one or more elements selected from the group consisting of Si, Ca, and Na, and the element M2 is one or more elements selected from the group consisting of Fe and Mg. (2) In powder X-ray diffraction measurement using CuKα radiation, there are two diffraction peaks within the range of 2θ=38.0±0.5°, and when the diffraction peak on the lower angle side is designated as Peak A and the diffraction peak on the higher angle side is designated as Peak B, the following formula is satisfied. 0.50≦I A / I B ≦0.75 …Equation (I A is the peak area of ​​the peak A, and I B is the peak area of ​​the peak B. [2] The lithium metal composite oxide according to [1], wherein the total mass of Co, the element M1, and the element M2 contained in the lithium metal composite oxide is 12,000 ppm or less. [3] The lithium metal composite oxide according to [1] or [2], wherein the element M1 contains Ca and Si, and a molar ratio of the Si to the Ca is 8 or more. [4] The lithium metal composite oxide according to any one of [1] to [3], wherein the element M1 contains Na and Si, and the molar ratio of the Si to the Na is 0.5 or more. [5] BET specific surface area is 1.0m 2 / g or more 2.0m 2 The lithium metal composite oxide according to any one of [1] to [4], wherein the lithium metal composite oxide has a viscosity of 100% or less. [6]D 10 , D 50 and D. 90The lithium metal composite oxide according to any one of [1] to [5], which satisfies the following formula (I): 0.5≦(D 90 -D 10 ) / D 50 ≦1.5 … Formula (I) (D 10 is the 10% cumulative volume particle size of the lithium metal composite oxide, and D 50 is the 50% cumulative volume particle size of the lithium metal composite oxide, and D 90 is the 90% cumulative volume particle size of the lithium metal composite oxide. [7] The lithium metal composite oxide according to any one of [1] to [6], wherein the lithium metal composite oxide has an average particle strength of 20 MPa or more. [8] The lithium metal composite oxide according to any one of [1] to [7], wherein the standard deviation of particle strength of the lithium metal composite oxide is 40% or less. [9] A positive electrode active material for a lithium secondary battery, comprising the lithium metal composite oxide according to any one of [1] to [8].

[10] A positive electrode for a lithium secondary battery, comprising the positive electrode active material for a lithium secondary battery according to [9].

[11] A lithium secondary battery comprising the positive electrode for lithium secondary batteries according to

[10] . Effect of the Invention

[0009] According to the present invention, it is possible to obtain a lithium metal composite oxide capable of providing a lithium secondary battery having excellent cycle characteristics. Furthermore, it is possible to provide a positive electrode active material for a lithium secondary battery, a positive electrode for a lithium secondary battery, and a lithium secondary battery, each containing such a lithium metal composite oxide. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic diagram illustrating an example of a lithium secondary battery. [Diagram 2] FIG. 1 is a schematic diagram showing the overall configuration of an all-solid-state lithium secondary battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In this specification, Metal Composite Compound is hereinafter referred to as "MCC", Lithium Metal Composite Oxide is hereinafter referred to as "LiMO", and Cathode Active Material for Lithium Secondary Batteries is hereinafter referred to as "CAM". A lithium secondary battery is a battery in which an electrolyte (such as a non-aqueous electrolyte or a solid electrolyte) is placed between a positive electrode and a negative electrode, and charging and discharging are performed by lithium ions moving between the positive electrode and the negative electrode via the electrolyte.

[0012] "Ni" refers to nickel atoms, not nickel metal. Similarly, "Co" and "Li" refer to cobalt atoms, lithium atoms, etc.

[0013] For example, when a numerical range is described as "1-10 μm" or "1 to 10 μm," it means a range from 1 μm to 10 μm, including the lower limit of 1 μm and the upper limit of 10 μm.

[0014] [Method of measuring cycle maintenance rate] In this specification, "excellent cycle characteristics" means that the cycle retention rate measured as described below for a lithium secondary battery prepared by the method described below is 80% or more.

[0015] (Preparation of positive electrodes for lithium secondary batteries) LiMO is used as the CAM, and the CAM, conductive material (acetylene black), and binder (PVdF) are added and kneaded in a ratio of CAM:conductive material:binder = 92:5:3 (mass ratio) to prepare a paste-like positive electrode mixture. When preparing the positive electrode mixture, N-methyl-2-pyrrolidone is used as the organic solvent.

[0016] The obtained positive electrode mixture is applied to a 40 μm thick Al foil as a current collector and vacuum dried at 150 °C for 8 hours to obtain a positive electrode for a lithium secondary battery. The electrode area of ​​this positive electrode for a lithium secondary battery is 1.65 cm 2 Let us assume that.

[0017] (Production of lithium secondary batteries) The following operations are carried out in a glove box under an argon atmosphere. The above-mentioned positive electrode for lithium secondary battery is placed with the aluminum foil side facing down on the bottom cover of a part for coin-type battery R2032 (manufactured by Hosen Co., Ltd.), and a laminated film separator (thickness 16 μm) made of a heat-resistant porous layer laminated on a polyethylene porous film is placed on top of it. 300 μl of electrolyte is poured here. The electrolyte is a liquid in which LiPF6 is dissolved at a ratio of 1 mol / l in a mixture of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate in a ratio of 30:35:35 (volume ratio).

[0018] Next, metallic lithium is used as the negative electrode, placed on the top of the separator, and the top lid is placed over the gasket and crimped with a crimping machine to produce a lithium secondary battery (coin-type half cell R2032). The assembled lithium secondary battery is allowed to stand at room temperature for 12 hours to allow the separator and the positive electrode mixture layer to be sufficiently impregnated with the electrolyte.

[0019] At a test temperature of 25°C, the charging and discharging currents are set to 0.2 CA, and constant current and constant voltage charging and constant current discharging are performed, respectively. The maximum charging voltage is 4.3 V, and the minimum discharging voltage is 2.5 V.

[0020] Next, constant current / constant voltage charging and constant current discharging were repeated under the following conditions at a test temperature of 25° C. The charge / discharge cycle was repeated 50 times. Charging: Current setting value 1CA, maximum voltage 4.3V, constant voltage constant current charging Discharge: Battery setting value 1CA, minimum voltage 2.5V, constant current discharge

[0021] The cycle retention rate is calculated from the discharge capacity at the 1st cycle and the discharge capacity at the 50th cycle using the following formula. The higher the cycle retention rate, the more the battery capacity loss after repeated charging and discharging is suppressed, indicating superior cycle characteristics. Cycle retention rate (%) = 50th cycle discharge capacity (mAh / g) / 1st cycle discharge capacity (mAh / g) × 100

[0022] <Lithium metal composite oxide> The crystal structure of LiMO in this embodiment is a layered structure, and is more preferably a hexagonal crystal structure or a monoclinic crystal structure.

[0023] The hexagonal crystal structure is P3, P31, P32, R3, P-3, R-3, P312, P321, P3112, P3121, P3212, P3221, R32, P3m1, P 31m, P3c1, P31c, R3m, R3c, P-31m, P-31c, P-3m1, P-3c1, R-3m, R-3c, P6, P61, P65, P62, P64, P63 , P-6, P6 / m, P63 / m, P622, P6122, P6522, P6222, P6422, P6322, P6mm, P6cc, P63cm, P63mc, P-6m2, P-6c2, P-62m, P-62c, P6 / mmm, P6 / mcc, P63 / mcm, and P63 / mmc.

[0024] In addition, the monoclinic crystal structure belongs to any one space group selected from the group consisting of P2, P21, C2, Pm, Pc, Cm, Cc, P2 / m, P21 / m, C2 / m, P2 / c, P21 / c, and C2 / c.

[0025] From the viewpoint of obtaining a lithium secondary battery having excellent cycle characteristics, the crystal structure is more preferably a hexagonal crystal structure belonging to the space group R-3m, or a monoclinic crystal structure belonging to the space group C2 / m.

[0026] [How to confirm the crystal structure] The crystal structure of LiMO can be confirmed by observation using a powder X-ray diffraction measuring device (for example, Ultima IV manufactured by Rigaku Corporation).

[0027] Furthermore, the LiMO satisfies the following (1) and (2).

[0028] (1) LiMO contains Co, an element M1, and an element M2. The element M1 is one or more elements selected from the group consisting of Si, Ca, and Na, and the element M2 is one or more elements selected from the group consisting of Fe and Mg. In LiMO, the molar ratio of element M1 to Co, i.e., M1 / Co, is 0.05-6.

[0029] M1 / Co is preferably 0.06 or more, more preferably more than 0.07. Also, M1 / Co is preferably 5.5 or less, more preferably 5.0 or less, and even more preferably 4.5 or less. M1 / Co is preferably 0.05-5.5, more preferably 0.06-5.0, even more preferably 0.06-4.5, and particularly preferably more than 0.07 and 4.5 or less.

[0030] It is known that when a lithium secondary battery is in operation, lithium ions diffuse between the layers inside the LiMO crystal and move to the electrolyte interface. The more smoothly lithium ions can diffuse inside the LiMO crystal, the less likely the cycle characteristics will deteriorate, and a lithium secondary battery with a longer life will be obtained. In other words, if the crystal structure of LiMO can be controlled to one that allows lithium ions to diffuse more easily, it will be easier to improve the cycle characteristics of lithium secondary batteries.

[0031] One of the means for controlling the crystal structure of LiMO is to control the degree of sintering of the fired product obtained after the firing process. Specifically, by controlling the degree of sintering in the process of mixing and firing MCC containing Co and element M1 with a lithium compound, the degree of development of the layered structure of LiMO can be controlled.

[0032] The inventors have found that the use of LiMO in which the composition ratio of Co to element M1 satisfies the above (1) improves the cycle characteristics of a lithium secondary battery. This is presumably because a layered structure that allows lithium ions to diffuse smoothly is easily formed.

[0033] The total mass of Co, element M1, and element M2 contained in LiMO is preferably 12000 ppm or less, more preferably 10000 ppm or less, further preferably 8000 ppm or less, and particularly preferably 6100 ppm or less. The lower limit of the total mass of Co, element M1, and element M2 contained in LiMO is preferably 10 ppm or more, more preferably 50 ppm or more, further preferably 100 ppm or more, and particularly preferably 580 ppm or more.

[0034] From the viewpoint of environmental regulations and stable mass production, it is preferable that the content of the rare metal Co is small. Furthermore, element M1 acts on the site where Li is accommodated and contributes to the diffusion of lithium ions, and element M2 acts on the main metal elements (e.g., Ni and Mn) that constitute LiMO and contributes to the development of a layered structure. The presence of an excessive amount of element M1 hinders the diffusion of lithium ions, whereas the presence of an excessive amount of element M2 hinders the development of a layered structure. Therefore, from the viewpoint of stable supply of lithium secondary batteries in addition to cycle characteristics, the total amount of Co, element M1, and element M2 contained in LiMO is preferably equal to or less than the above upper limit.

[0035] The total mass of Co, element M1, and element M2 contained in LiMO is, for example, 10-12000 ppm, 50-10000 ppm, 100-8000 ppm, or 580-6100 ppm. Note that these values ​​are based on 100% by mass of the total amount of metal elements contained in LiMO.

[0036] The element M1 may be one or more selected from the group consisting of Si, Ca, and Na, and when two or more elements are included, the combination is not particularly limited. Moreover, the element M1 may include all of Si, Ca, and Na.

[0037] When the element M1 contains Ca and Si, the molar ratio of Si to Ca is preferably 8 or more, more preferably 8.5 or more, and even more preferably 9 or more. The molar ratio of Si to Ca is preferably 100 or less, more preferably 90 or less, further preferably 85 or less, and particularly preferably 80 or less.

[0038] The molar ratio of Si to Ca is preferably 8 to 100, more preferably 8.5 to 90, further preferably 9 to 85, and particularly preferably 8 to 80. When the molar ratio of Si to Ca is within the above range, the cycle characteristics can be improved.

[0039] When the element M1 contains Na and Si, the molar ratio of Si to Na is preferably 0.5 or more, more preferably 0.6 or more, and even more preferably 0.7 or more. The molar ratio of Si to Na is preferably 10 or less, more preferably 9 or less, and even more preferably 8 or less.

[0040] The molar ratio of Si to Na is preferably 0.5 to 10, more preferably 0.6 to 9, and further preferably 0.7 to 8. When the molar ratio of Si to Na is within the above range, the cycle characteristics can be improved.

[0041] LiMO contains Li in addition to Co, an element M1, and an element M2. Also, LiMO preferably further contains Ni and one or more elements M0 selected from the group consisting of Mn and Al.

[0042] (composition formula) In order to further improve cycle characteristics, the LiMO is preferably represented by the following composition formula (A). Li x Ni y Coz M0 s M1 t M2 u O2···(A) (In formula (A), 0.80 ≦ x ≦ 1.20, 0.70 ≦ y ≦ 0.98, 0 ≦ s < 0.30, 0 < z + t + u ≦ 0.02, and y + z + s + t + u = 1, M0 is the element M0, M1 is the element M1, and M2 is the element M2.)

[0043] x is preferably 0.81 or more, more preferably 0.82 or more. x is preferably 1.19 or less, more preferably 1.18 or less. The range of x is preferably 0.81 ≦ x ≦ 1.19, more preferably 0.82 ≦ x ≦ 1.18. y is preferably 0.71 or more, more preferably 0.72 or more, still more preferably 0.80 or more. y is preferably 0.95 or less, more preferably 0.94 or less, still more preferably 0.93 or less. The range of y is preferably 0.71 ≦ y ≦ 0.95, more preferably 0.72 ≦ y ≦ 0.94, still more preferably 0.80 ≦ y ≦ 0.93. When LiMO contains the element M0, s is preferably 0.28 or less, more preferably 0.20 or less, still more preferably 0.10 or less, particularly preferably 0.09 or less. The range of s is preferably 0 < s ≦ 0.28, more preferably 0 < s ≦ 0.20, still more preferably 0 < s ≦ 0.1, particularly preferably 0 < s ≦ 0.09. z + t + u is preferably 0.015 or less. z + t + u is preferably 0.0003 or more, more preferably 0.0005 or more. z + t + u is preferably 0.0003 ≦ z + t + u ≦ 0.02, more preferably 0.0005 ≦ z + t + u ≦ 0.015.

[0044] [Composition Analysis] For the composition analysis of LiMO, after dissolving the powder of LiMO in hydrochloric acid, it is measured using an ICP emission spectroscopic analyzer. As the ICP emission spectroscopic analyzer, for example, Optima 7300 manufactured by PerkinElmer, Inc. can be used.

[0045] (2) In X-ray diffraction measurement using CuKα radiation, the LiMO has two diffraction peaks within the range of 2θ=38.0±0.5°. When the lower angle peak is designated as peak A and the higher angle peak is designated as peak B, LiMO satisfies the following formula: 0.50≦I A / I B ≦0.75 …Equation (I A is the peak area of ​​peak A, and I B is the peak area of ​​peak B.)

[0046] I A / I B is preferably 0.52 or more, and more preferably 0.53 or more. A / I B is more preferably 0.74 or less, and further preferably 0.73 or less. I A / I B More preferably, it satisfies the following formula (B) or (C). 0.52≦I A / I B ≦0.74 …Formula (B) 0.53≦I A / I B ≦0.73 …Formula (C)

[0047] Distortion in the crystal structure tends to hinder the smooth diffusion of lithium ions, so eliminating the distortion in the crystal structure further improves cycle characteristics. In addition, if the crystal faces through which lithium ions easily enter and exit are exposed to the electrolyte, the cycle characteristics are less likely to deteriorate. Through research by the present inventors, it was found that the use of LiMO that satisfies the above condition (2) in addition to the above condition (1) improves the cycle characteristics of a lithium secondary battery. This is presumably because the distortion of the crystal structure of LiMO is eliminated, and the crystal plane through which lithium ions can easily enter and exit is exposed to the electrolyte.

[0048] [I A / I B How to get it The powder X-ray diffraction measurement of LiMO is carried out using a powder X-ray diffractometer, such as LINT2000 manufactured by Rigaku Corporation. Specifically, LiMO powder is loaded onto a dedicated substrate, and a powder X-ray diffraction pattern is obtained by measuring using a Cu-Kα source under conditions of a diffraction angle 2θ = 10° to 90°, a sampling width of 0.02°, and a scan speed of 4° / min. Using the integrated powder X-ray analysis software, two diffraction peaks within the range of 2θ = 38.0 ± 0.5° are identified from the obtained powder X-ray diffraction pattern. The two peaks selected at this time are the peak with the maximum peak intensity and the peak with the second maximum peak intensity. Of the two peaks identified, the diffraction peak on the low angle side is designated as Peak A, and the diffraction peak on the high angle side is designated as Peak B.

[0049] Next, the peak area of ​​peak A, I A and the peak area of ​​peak B, I B Request. Specifically, the peak area is calculated within the range enclosed by the peak curve from the peak start to the peak end of the peak and the baseline. In this specification, the peak start refers to the rising point of a peak after peak separation, and means the point of contact between the peak and the baseline. In this specification, the term "peak end" refers to the point where a peak ends after peak separation, and means the point of contact between the peak and the baseline.

[0050] Peak areas can be calculated automatically using integrated powder X-ray analysis software. As the integrated powder X-ray analysis software, for example, JADE manufactured by Materials Data Corporation can be used.

[0051] The BET specific surface area of ​​LiMO is 1.0m 2 / g or more is preferable, and 1.1m 2 / g or more is more preferable, and 1.2m 2 / g or more is more preferable. The BET specific surface area is 2.0 m 2 / g or less is preferable, and 1.8m 2 / g or less is more preferable, and 1.7m 2 / g or less is more preferable. The BET specific surface area is 1.0-2.0 m 2 / g is preferred, 1.1-1.8m 2 / g is more preferable, 1.2-1.7m 2 / g is more preferred. When LiMO having a BET specific surface area equal to or greater than the lower limit is used, the reaction interface of LiMO increases, making it easier for lithium ions to enter and exit, and the cycle characteristics are less likely to deteriorate. When LiMO having a BET specific surface area of ​​less than the upper limit is used, the contact area between LiMO and the electrolyte is less likely to increase, and the coating caused by the decomposition of the electrolyte is less likely to form. If the amount of such a coating is small, the lithium ion conductivity is less likely to be inhibited, and therefore the cycle characteristics are less likely to deteriorate.

[0052] [Measurement of BET specific surface area] The BET specific surface area of ​​LiMO can be measured by a BET specific surface area measuring device. For example, Macsorb (registered trademark) manufactured by Mountec Co., Ltd. can be used as the BET specific surface area measuring device. When measuring powdered LiMO, it is preferable to dry it in a nitrogen atmosphere at 105°C for 30 minutes as a pretreatment.

[0053] LiMO's D 10 , D 50 and D. 90 It is preferable that the following formula (I) is satisfied. 0.5≦(D 90 -D 10 ) / D 50 ≦1.5 … Formula (I) (D 10 is the 10% cumulative volumetric particle size of LiMO, and D 50 is the 50% cumulative volumetric particle size of LiMO, and D 90 is the 90% cumulative volumetric particle size of LiMO.)

[0054] LiMO that satisfies the above condition (I) is ideally packed in a crucible or sheath, and sintering is easily promoted, facilitating crystal growth, which in turn improves cycle characteristics.

[0055] (D 90 -D 10 ) / D 50 is preferably 0.6 or more, and more preferably 0.8 or more. 90 -D 10 ) / D 50 is more preferably 1.4 or less. (D 90 -D 10 ) / D 50 is preferably 0.6 to 1.5, more preferably 0.6 to 1.4, and even more preferably 0.8 to 1.4.

[0056] D 50 is preferably 8 μm or more, and more preferably 10 μm or more. 50 is preferably 25 μm or less, more preferably 20 μm or less. 50 is preferably 8-25 μm, more preferably 10-20 μm. 50 In LiMO having the above range, when LiMO is mixed with a conductive material and a binder in a layer, the particles in the LiMO are ideally packed together. As a result, lithium ions can move efficiently in the electrode mixture layer during operation of the lithium secondary battery, and the cycle characteristics are likely to be improved.

[0057] [D 10 , D 90 and D. 50 Measurement of The above LiMO D 10 (μm), D 50 (μm) and D 90 (μm) can be measured by the following dry method.

[0058] Specifically, first, 2 g of LiMO is used to measure the dry particle size distribution using a laser diffraction particle size distribution analyzer, and a cumulative particle size distribution curve based on volume is obtained. In the cumulative particle size distribution curve obtained, the particle size values ​​at 10%, 50%, and 90% accumulation from the fine particle side are respectively D 10, D 50 , D 90 It is. As the laser diffraction particle size distribution analyzer, for example, MS2000 manufactured by Malvern Instruments can be used.

[0059] The average particle strength of LiMO is preferably 20 MPa or more, more preferably 21 MPa or more, and even more preferably 25 MPa or more. The average particle strength of LiMO is preferably 60 MPa or less, more preferably 55 MPa or less, and even more preferably 50 MPa or less. The upper limit value and the lower limit value of the average particle strength may be combined arbitrarily. The average particle strength is preferably from 20 to 60 MPa, more preferably from 21 to 55 MPa, and even more preferably from 25 to 50 MPa.

[0060] When LiMO having an average particle strength in the above range is used as the CAM, the CAM particles are less likely to crack during battery operation, which means that cracks that could cause resistance are less likely to occur and the cycle characteristics are less likely to deteriorate.

[0061] [Method of measuring average particle strength] The average particle strength of LiMO is measured in the following manner. First, the above [D 10 , D 90 and D. 50 D measured by the method described in "Measurement of 50 Select at least three or more LiMO particles with a size of about ±2 μm. When selecting, avoid particles with extremely irregular shapes. Specifically, select particles with a ratio of the short diameter to the long diameter (short diameter / long diameter) of 0.7 to 1.3.

[0062] Here, "major axis" means the longest diameter of the particle. "Minor axis" means the shortest diameter of the particle. Next, a test pressure (load) is applied to one of the LiMO particles selected above, and the displacement of the LiMO particle is measured.

[0063] For the measurements, a micro-compression tester MCT-510 manufactured by Shimadzu Corporation is used. The three or more particles selected above are placed in the device, and the test pressure is gradually increased. The pressure value at which the displacement becomes maximum while the test pressure remains almost constant is defined as the test force (P) (unit: MPa). From the obtained test force (P), the crushing strength (St) (unit: MPa) is calculated using the following formula (X) (see Journal of the Mining Industry of Japan, Vol. 81, (1965)). This operation is carried out a total of seven times, and the average value of the five times excluding the maximum and minimum values ​​of the crushing strength is calculated as the average particle strength. In the following formula (X), d is the secondary particle diameter (unit: μm) of the particles in LiMO. St=2.8×P / (π×d×d) Formula (X)

[0064] The standard deviation of the particle strength of LiMO is preferably 40% or less, more preferably 30% or less, and even more preferably 25% or less. The standard deviation is preferably 3% or more, more preferably 5% or more, and even more preferably 10% or more. The standard deviation is preferably 3-40%, more preferably 5-30%, and even more preferably 10-25%. When an electrode mixture layer is produced using LiMO having the standard deviation in the above range, the particle strength in the electrode mixture layer varies little and the layer is homogeneous. As a result, the LiMO particles are less likely to crack during operation of the lithium secondary battery, and the cycle characteristics are less likely to deteriorate.

[0065] [Method of measuring standard deviation of particle strength] The standard deviation of particle intensity is calculated using the particle intensity and average particle intensity values ​​obtained by the above [Method of measuring average particle intensity]. Specifically, the squares of the differences between the particle intensity and the average particle intensity values ​​of each data are summed up, and the positive square root of the sum obtained is divided by the total number of data, and the standard deviation of particle intensity is calculated.

[0066] <LiMO manufacturing method> The method for producing LiMO includes a step of obtaining MCC and a step of obtaining LiMO. The steps of obtaining MCC and LiMO will be described below in that order.

[0067] [Process for obtaining MCC] MCC contains Co, element M1, and element M2. "MCC contains Co, element M1, and element M2" includes an embodiment in which Co, element M1, and element M2 are present in the crystal of MCC, and an embodiment in which Co, element M1, and element M2 are present around MCC. MCC preferably further contains Ni and the above-mentioned element M0. Examples of MCC include metal composite hydroxides, metal composite oxides, and mixtures of metal composite hydroxides and metal composite oxides that contain the above elements.

[0068] MCC can be produced by a commonly known batch co-precipitation method or a continuous co-precipitation method. The production method will be described in detail below using MCC containing Ni, element M0, Co, element M1, and element M2 as an example.

[0069] First, a nickel salt solution, a metal salt solution of element M0, a cobalt salt solution, a metal salt solution of element M1, a metal salt solution of element M2, and a complexing agent are reacted by a coprecipitation method, particularly a continuous coprecipitation method described in JP-A-2002-201028, to produce a metal composite hydroxide.

[0070] The nickel salt that is the solute of the nickel salt solution is not particularly limited, but for example, one or more of nickel sulfate, nickel nitrate, nickel chloride, and nickel acetate can be used.

[0071] As the metal salt of element M0, which is the solute of the metal salt solution of element M0, for example, one or more of manganese sulfate, manganese nitrate, manganese chloride, manganese acetate, aluminum sulfate, and sodium aluminate can be used.

[0072] The nickel salt solution and the metal salt solution of element M0 are used in a ratio corresponding to the desired composition ratio of LiMO (for example, composition formula (A)).

[0073] The nickel salt solution and the metal salt solution of element M0 are fed into a reaction vessel and mixed to obtain a raw material liquid.

[0074] Next, the cobalt salt solution, the metal salt solution of element M1, and the metal salt solution of element M2 are added to the raw material liquid in the reaction vessel to obtain a mixed raw material liquid.

[0075] As the cobalt salt that is the solute of the cobalt salt solution, for example, one or more of cobalt sulfate, cobalt nitrate, cobalt chloride, and cobalt acetate can be used.

[0076] As the metal salt of element M1, which is the solute of the metal salt solution of element M1, when it is Ca, one or more of calcium sulfate, calcium nitrate, calcium chloride, calcium acetate, calcium carbonate, calcium oxide, and calcium hydroxide can be used; when it is Si, one or more of silicon dioxide, sodium silicate, and aluminum silicate can be used; and when it is Na, one or more of sodium sulfate, sodium nitrate, sodium chloride, sodium acetate, sodium carbonate, sodium oxide, sodium hydroxide, and sodium silicate can be used.

[0077] As the metal salt of element M2, which is the solute of the metal salt solution of element M2, when element M2 is Fe, one or more of iron sulfate (II), iron sulfate (III), iron nitrate (II), iron nitrate (III), iron chloride (II), iron chloride (III), iron acetate (II), iron oxide (II), iron oxide (III), iron hydroxide (II), and iron hydroxide (III) can be used; when element M2 is Mg, one or more of magnesium sulfate, magnesium nitrate, magnesium chloride, magnesium acetate, magnesium carbonate, calcium oxide, and magnesium hydroxide can be used.

[0078] The cobalt salt solution, the metal salt solution of element M1, and the metal salt solution of element M2 are added in a ratio that satisfies the above-mentioned (1), thereby obtaining LiMO that satisfies the above-mentioned (1).

[0079] The amounts of the cobalt salt solution, the metal salt solution of element M1, and the metal salt solution of element M2 added are preferably such that the total amount of Co, element M1, and element M2 contained in the desired LiMO is 12,000 ppm or less.

[0080] The solvent for the nickel salt solution, the metal salt solution of the element M0, the cobalt salt solution, the metal salt solution of the element M1, and the metal salt solution of the element M2 is, for example, water.

[0081] The complexing agent is a compound capable of forming a complex with Ni and ions of element M0 in an aqueous solution, for example, ammonium ion donors, hydrazine, ethylenediaminetetraacetic acid, nitrilotriacetic acid, uracildiacetic acid, and glycine.

[0082] Examples of the ammonium ion donor include ammonium salts such as ammonium hydroxide, ammonium sulfate, ammonium chloride, ammonium carbonate, and ammonium fluoride.

[0083] A complexing agent may not be included. When a complexing agent is included, the amount of the complexing agent included in the mixed raw material liquid and the mixed liquid containing the complexing agent is, for example, a molar ratio of more than 0 and not more than 2 to the total number of moles of the metal salts included in the mixed liquid.

[0084] In the coprecipitation method, in order to adjust the pH value of the mixture, an alkaline aqueous solution is added to the mixture before the pH of the mixture becomes neutral from alkaline. The alkaline aqueous solution can be an aqueous solution of sodium hydroxide or potassium hydroxide.

[0085] In this specification, the pH value is defined as the value measured when the temperature of the mixed liquid is 40° C. If the temperature of the mixed liquid sampled from the reaction tank is not 40° C., the mixed liquid is heated or cooled to 40° C. before measuring the pH.

[0086] During the reaction, the temperature of the reaction vessel is controlled within the range of, for example, 20 to 80°C, preferably 30 to 70°C.

[0087] During the reaction, the pH value in the reaction tank is controlled within the range of, for example, 9 to 13, and preferably 11 to 13.

[0088] The materials in the reaction vessel are mixed by suitable stirring. As a reaction vessel used in the continuous coprecipitation method, an overflow type reaction vessel can be used in order to separate the formed reaction precipitate.

[0089] Here, for example, an inert gas such as nitrogen, argon or carbon dioxide, an oxidizing gas such as air or oxygen, or a mixture of these gases may be supplied into the reaction vessel.

[0090] In order to control the inside of the reaction vessel to a desired atmosphere, a specific gas may be passed through the reaction vessel or the reaction liquid may be directly bubbled into the reaction vessel.

[0091] After the above reaction, the resulting reaction precipitate is washed with water and dried as necessary to obtain a metal composite hydroxide. If necessary, the reaction precipitate may be washed with weak acid water or an alkaline solution containing sodium hydroxide or potassium hydroxide.

[0092] When producing a metal composite oxide as MCC, the metal composite oxide is obtained by oxidizing a metal composite hydroxide.

[0093] In this case, the oxidation time, from the start of the temperature rise to the end of the temperature holding after the temperature has been reached, is preferably 2 to 10 hours in total. The oxidation temperature is preferably 500 to 800°C.

[0094] During the oxidation, various gases, for example, inert gases such as nitrogen, argon, carbon dioxide, etc., oxidizing gases such as air, oxygen, etc., or mixtures thereof, may be supplied into the reaction vessel.

[0095] The MCC may be classified as appropriate.

[0096] [Process for obtaining LiMO] The process for obtaining LiMO includes a mixing step of mixing MCC with a lithium compound, and a firing step of firing the resulting mixture.

[0097] ·Mixing process The MCC and the lithium compound are mixed. The lithium compound may be at least one of lithium carbonate, lithium nitrate, lithium acetate, lithium hydroxide, lithium hydroxide hydrate, lithium oxide, lithium chloride, and lithium fluoride. Of these, lithium hydroxide, lithium hydroxide hydrate, and lithium carbonate or a mixture thereof is preferred.

[0098] The lithium compound and MCC are mixed in consideration of the composition ratio of the final target product to obtain a mixture of the lithium compound and MCC. The amount (molar ratio) of Li relative to the total amount of metal elements contained in MCC is preferably 0.90 to 1.10, more preferably 0.91 to 1.10, and even more preferably 0.92 to 1.10.

[0099] · Firing process By firing the mixture of MCC and a lithium compound, crystals grow and LiMO is obtained. For firing, dry air, an oxygen atmosphere, or the like is used depending on the desired composition. In this embodiment, firing in an oxygen atmosphere is preferred.

[0100] The firing process may involve only one firing step, or may involve multiple firing steps. In the case of multiple firing steps, the firing step at the highest temperature is referred to as the main firing. Prior to the main firing, a preliminary firing step at a temperature lower than the main firing step may be performed. In addition, after the main firing step, a post-firing step at a temperature lower than the main firing step may be performed.

[0101] In this embodiment, it is preferable to first calcinate the mixture of MCC and the lithium compound, and then calcinate the mixture, and it is also preferable that both the calcination and the calcination are performed in an oxygen atmosphere.

[0102] The calcination temperature during the calcination is preferably 600 to 900° C., more preferably 610 to 850° C., and even more preferably 620° C. or more and less than 700° C. When the calcination temperature is equal to or more than the lower limit, LiMO having a strong crystal structure can be obtained. On the other hand, when the calcination temperature is equal to or less than the upper limit, the volatilization of lithium ions on the surface of LiMO particles can be reduced.

[0103] The firing temperature during the main firing is preferably 600 to 900° C., more preferably 650 to 850° C., and even more preferably 700 to 820° C. When the firing temperature is equal to or higher than the lower limit, LiMO having a strong crystal structure can be obtained. On the other hand, when the firing temperature is equal to or lower than the upper limit, volatilization of lithium ions on the surface of LiMO particles can be reduced.

[0104] The firing temperature in this specification refers to the maximum temperature maintained in the atmosphere of the firing furnace during firing. When firing is performed multiple times, the firing temperature refers to the maximum temperature at the stage where firing is performed at the highest temperature. The firing furnace used for firing may be, for example, a continuous static firing furnace or a fluidized firing furnace. Examples of the continuous static firing furnace include a tunnel furnace or a roller hearth kiln. Examples of the fluidized firing furnace include a rotary kiln.

[0105] The retention time during the pre-firing and main firing is preferably 1 to 50 hours, more preferably 2 to 20 hours. When the retention time is equal to or less than the upper limit, the volatilization of lithium ions is suppressed, and the deterioration of battery performance is suppressed. When the retention time is equal to or more than the lower limit, the development of crystals is promoted, and the deterioration of battery performance is suppressed. By adjusting the conditions in the calcination step, the BET specific surface area, average particle strength, or standard deviation of particle strength of the resulting LiMO can be adjusted to fall within the above-mentioned ranges.

[0106] ·Crushing process The fired product obtained after the firing step is pulverized using a stone mill grinder (e.g., Masscolloider (registered trademark)). The mass colloider may be, for example, MKCA6-5J manufactured by Masuko Sangyo Co., Ltd. In the crushing step, a stone mill grinder is used to crush the material under conditions of, for example, a rotation speed of 800 to 1500 rpm and a gap of 10 to 1000 μm.

[0107] By crushing the fired material using a stone mill, LiMO that satisfies the above (2) can be obtained.

[0108] [Optional process] Cleaning process It is preferable to wash the crushed material obtained in the above crushing step with a washing liquid such as pure water or an alkaline washing liquid. Examples of the alkaline cleaning liquid include an aqueous solution of one or more anhydrides selected from the group consisting of lithium hydroxide, sodium hydroxide, potassium hydroxide, lithium carbonate, sodium carbonate, potassium carbonate, and ammonium carbonate, an aqueous solution of a hydrate of the anhydrides, and ammonia.

[0109] The temperature of the cleaning solution is preferably not higher than 20° C., more preferably not higher than 15° C., and even more preferably not higher than 10° C. By controlling the temperature of the cleaning solution to be equal to or lower than the upper limit value and at a temperature at which the cleaning solution does not freeze, it is possible to suppress excessive elution of lithium ions from the crystal structure of the crushed material into the cleaning solution during cleaning.

[0110] It is preferable to wash the crushed material with a washing liquid having a mass of at least twice the mass of the crushed material. In addition, if washing is performed in a batch system, it is preferable to perform washing two or more times. After washing with a solution other than water, it is preferable to further wash with water to prevent compounds derived from the solution from remaining in the crushed material.

[0111] ·Drying process After the washing step, the washed crushed material may be dried. In this case, the drying temperature is preferably 80 to 250° C., and more preferably 90 to 230° C. The drying time is preferably 0.5 to 24 hours, and more preferably 1 to 10 hours. The drying pressure may be normal pressure or reduced pressure.

[0112] By the above steps, the above LiMO is obtained.

[0113] <cam> The CAM of this embodiment contains LiMO produced by the method described above.

[0114] <Lithium secondary battery> A positive electrode for a lithium secondary battery suitable for use with the CAM containing LiMO according to the present embodiment will be described. Hereinafter, the positive electrode for a lithium secondary battery may be referred to as a positive electrode. Furthermore, a lithium secondary battery suitable for use as a positive electrode will be described.

[0115] An example of a suitable lithium secondary battery for use with the CAM of this embodiment has a positive electrode, a negative electrode, a separator sandwiched between the positive electrode and the negative electrode, and an electrolyte solution disposed between the positive electrode and the negative electrode.

[0116] 1 is a schematic diagram showing an example of a lithium secondary battery. For example, a cylindrical lithium secondary battery 10 is manufactured as follows.

[0117] First, as shown in the partially enlarged view of FIG. 1 , a pair of strip-shaped separators 1, a strip-shaped positive electrode 2 having a positive electrode lead 21 at one end, and a strip-shaped negative electrode 3 having a negative electrode lead 31 at one end are laminated in the order of separator 1, positive electrode 2, separator 1, and negative electrode 3, and then wound to form an electrode group 4.

[0118] The positive electrode 2, for example, has a positive electrode active material layer 2a containing CAM, and a positive electrode current collector 2b on one surface of which the positive electrode active material layer 2a is formed. Such a positive electrode 2 can be manufactured by first preparing a positive electrode mixture containing CAM, a conductive material, and a binder, and supporting the positive electrode mixture on one surface of the positive electrode current collector 2b to form the positive electrode active material layer 2a.

[0119] Examples of the negative electrode 3 include an electrode in which a negative electrode mixture containing a negative electrode active material (not shown) is supported on a negative electrode current collector, and an electrode made of only the negative electrode active material. The negative electrode 3 can be manufactured in a manner similar to that for the positive electrode 2.

[0120] Next, the electrode group 4 and an insulator (not shown) are housed in the battery can 5, the bottom of the can is sealed, the electrode group 4 is impregnated with an electrolyte solution 6, and the electrolyte is disposed between the positive electrode 2 and the negative electrode 3. Furthermore, the upper part of the battery can 5 is sealed with a top insulator 7 and a sealing body 8, whereby a lithium secondary battery 10 can be manufactured.

[0121] The shape of the electrode group 4 can be, for example, a columnar shape such that the cross-sectional shape when the electrode group 4 is cut perpendicular to the winding axis is a circle, an ellipse, a rectangle, or a rectangle with rounded corners.

[0122] The shape of a lithium secondary battery having such an electrode group 4 can be any shape defined by IEC60086, which is a standard for batteries defined by the International Electrotechnical Commission (IEC), or JIS C 8500. For example, cylindrical or rectangular shapes can be used.

[0123] Furthermore, the lithium secondary battery is not limited to the above-mentioned wound type configuration, and may be a laminated type configuration in which a laminated structure of a positive electrode, a separator, a negative electrode, and a separator is repeatedly stacked. Examples of the laminated type lithium secondary battery include a so-called coin type battery, a button type battery, and a paper type (or sheet type) battery.

[0124] For the positive electrode, separator, negative electrode, and electrolyte constituting the lithium secondary battery, for example, the configurations, materials, and manufacturing methods described in

[0113] to

[0140] of WO2022 / 113904A1 can be used.

[0125] <All-solid-state lithium secondary battery> The CAM of this embodiment can be used as a CAM for an all-solid-state lithium secondary battery.

[0126] Fig. 2 is a schematic diagram showing an example of an all-solid-state lithium secondary battery. The all-solid-state lithium secondary battery 1000 shown in Fig. 2 has a laminate 100 having a positive electrode 110, a negative electrode 120, and a solid electrolyte layer 130, and an exterior body 200 that houses the laminate 100. The all-solid-state lithium secondary battery 1000 may also have a bipolar structure in which a CAM and a negative electrode active material are arranged on both sides of a current collector. A specific example of the bipolar structure is the structure described in JP-A-2004-95400.

[0127] The positive electrode 110 has a positive electrode active material layer 111 and a positive electrode current collector 112. The positive electrode active material layer 111 contains the above-mentioned CAM and a solid electrolyte. The positive electrode active material layer 111 may also contain a conductive material and a binder.

[0128] The negative electrode 120 has a negative electrode active material layer 121 and a negative electrode current collector 122. The negative electrode active material layer 121 contains a negative electrode active material. The negative electrode active material layer 121 may also contain a solid electrolyte and a conductive material.

[0129] The laminate 100 may have an external terminal 113 connected to the positive electrode current collector 112 and an external terminal 123 connected to the negative electrode current collector 122. In addition, the all-solid-state lithium secondary battery 1000 may have a separator between the positive electrode 110 and the negative electrode 120.

[0130] The all-solid-state lithium secondary battery 1000 further includes an insulator (not shown) that insulates the laminate 100 from the exterior body 200 , and a sealing body (not shown) that seals the opening 200 a of the exterior body 200 .

[0131] A container molded from a highly corrosion-resistant metal material such as aluminum, stainless steel, or nickel-plated steel can be used as the exterior body 200. Also, a container formed into a bag shape from a laminate film having at least one surface treated to be corrosion-resistant can be used as the exterior body 200.

[0132] Examples of the shape of the all-solid-state lithium secondary battery 1000 include a coin type, a button type, a paper type (or a sheet type), a cylindrical type, a square type, and a laminate type (pouch type).

[0133] The all-solid-state lithium secondary battery 1000 is illustrated as having one laminate 100 as an example, but the present embodiment is not limited to this. The all-solid-state lithium secondary battery 1000 may have a configuration in which the laminate 100 is used as a unit cell, and a plurality of unit cells (laminated bodies 100) are sealed inside an exterior body 200.

[0134] For the all-solid-state lithium secondary battery, for example, the configuration, materials, and manufacturing method described in

[0151] to

[0181] of WO2022 / 113904A1 can be used.

[0135] In the lithium secondary battery having the above-mentioned configuration, since the CAM is used, it is possible to provide a lithium secondary battery having excellent cycle characteristics.

[0136] Furthermore, since the positive electrode having the above-mentioned configuration has the CAM having the above-mentioned configuration, the cycle characteristics of the lithium secondary battery are excellent.

[0137] Furthermore, the lithium secondary battery having the above-mentioned structure has excellent cycle characteristics because it has the above-mentioned positive electrode.

[0138] Although the preferred embodiment of the present invention has been described above with reference to the accompanying drawings, the present invention is not limited to the above embodiment. The shapes and combinations of the components shown in the above embodiment are merely examples, and various modifications can be made based on design requirements, etc., without departing from the spirit of the present invention.

[0139] The present invention includes the following aspects.

[21] LiMO having a layered structure and satisfying the above (1) and formula (C).

[22] The LiMO according to

[21] , wherein the total mass of Co, the element M1, and the element M2 contained in the LiMO is 8000 ppm or less.

[23] The LiMO according to

[21] or

[22] , wherein the element M1 contains Ca and Si, and the molar ratio of the Si to the Ca is 8-80.

[24] The LiMO according to any one of

[21] to

[23] , wherein the element M1 contains Na and Si, and the molar ratio of the Si to the Na is 0.5 to 10.

[25] BET specific surface area is 1.1-1.8m 2 / g. The LiMO according to any one of

[21] to

[24] .

[26] D 10 , D 50 and D. 90 The lithium metal composite oxide according to any one of

[21] to

[25] , wherein the above formula (I) is satisfied.

[27] The LiMO according to any one of

[21] to

[26] , wherein the LiMO has an average particle strength of 20 MPa or more.

[28] The LiMO according to any one of

[21] to

[27] , wherein the standard deviation of particle intensity of the LiMO is 40% or less.

[29] LiMO according to any one of

[21] to

[28] , represented by the above composition formula (A).

[30] The LiMO according to any one of

[21] to

[29] , wherein the LiMO has an average particle strength of 21-55 MPa.

[31] The LiMO according to any one of

[21] to

[30] , wherein the standard deviation of particle intensity of the LiMO is 10-25%.

[32] The LiMO according to any one of

[21] to

[31] , wherein the total mass of the Co, the element M1 and the element M2 contained in the LiMO is 580 to 6100 ppm.

[33] The LiMO according to any one of

[21] to

[32] , wherein the LiMO has an average particle strength of 25-50 MPa.

[34] BET specific surface area is 1.2-1.7m 2 / g. The LiMO according to any one of

[21] to

[33] .

[35] (D 90 -D 10 ) / D 50 The LiMO according to any one of

[21] to

[34] , wherein the LiMO has a molecular weight of 0.8 to 1.4.

[36] D 50 The LiMO according to any one of

[21] to

[35] , wherein the LiMO has a diameter of 8-25 μm.

[37] The LiMO according to any one of

[21] to

[36] , wherein a molar ratio of the element M1 to the Co is greater than 0.07 and is not greater than 4.5.

[38] A CAM containing LiMO according to any one of

[21] to

[37] .

[39] A positive electrode for a lithium secondary battery comprising the CAM according to

[38] .

[40] A lithium secondary battery comprising the positive electrode for lithium secondary batteries according to

[39] . EXAMPLES

[0140] Next, the present invention will be described in more detail with reference to examples.

[0141] <Measurement of various parameters> The measurement of various parameters of LiMO produced by the method described below is carried out according to the above-mentioned [Method of confirming crystal structure], [Composition analysis], and [I A / I B [Method of obtaining BET specific surface area], [D 10 , D 90 and D. 50 [Method of measuring the average particle strength], and [Method of measuring the standard deviation of particle strength].

[0142] <Method of measuring cycle maintenance rate> The cycle retention rate of the lithium secondary battery prepared by the above method was measured according to the method described in the above [Method for measuring cycle retention rate].

[0143] <Example 1> Water was placed in a reaction vessel equipped with a stirrer and an overflow pipe, and then an aqueous sodium hydroxide solution was added and the liquid temperature (reaction temperature) was maintained at 50°C. A raw material liquid 1 was prepared by mixing an aqueous solution of nickel sulfate, an aqueous solution of manganese sulfate, and an aqueous solution of aluminum sulfate in such a ratio that the atomic ratio of Ni, Mn, and Al was 93:1:6.

[0144] Next, a 0.1 wt% aqueous calcium hydroxide solution, a 0.1 wt% aqueous magnesium sulfate solution, a 0.1 wt% aqueous sodium silicate solution, a 0.1 wt% aqueous iron chloride solution, and a 0.1 wt% aqueous cobalt sulfate solution were added to raw material liquid 1 in such proportions that (Si+Na+Ca) / Co=4.29, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=1680 ppm, Si / Na=6.61, and Si / Ca=69.18, thereby obtaining a mixed raw material liquid 1.

[0145] Next, in the reaction vessel, an aqueous solution of ammonium sulfate was continuously added as a complexing agent to the mixed raw material liquid 1 under stirring. An aqueous solution of sodium hydroxide was added dropwise at appropriate times under the condition that the pH of the mixed liquid in the reaction vessel became 12.1 (when the liquid temperature was 40°C), to obtain a metal composite hydroxide 1.

[0146] The obtained metal composite hydroxide 1 was washed and then dried at 105° C. for 20 hours to obtain a metal composite hydroxide MCC1.

[0147] MCC1 and lithium hydroxide monohydrate powder were weighed and mixed in a ratio of Li / (Ni+Mn+Al)=1.03 to obtain mixture 1. Thereafter, the mixture 1 was pre-fired in an oxygen atmosphere at 650° C. for 5 hours. Next, the mixture was subjected to main calcination in an oxygen atmosphere at 750° C. for 5 hours to obtain calcined product 1.

[0148] The obtained fired product 1 was pulverized by a mass colloider to obtain a pulverized product 1. The operating conditions and the equipment used for the mass colloider were as follows. (Mascolloider operating conditions) Equipment used: Masuko Sangyo MKCA6-5J Rotational speed: 1200 rpm Spacing: 100μm

[0149] The crushed material 1 was mixed with pure water whose liquid temperature had been adjusted to 5° C. in a ratio such that the mass ratio of the crushed material 1 to the total amount was 0.5 to prepare a slurry, which was then stirred for 20 minutes. After that, it was dehydrated and dried at 210℃ for 10 hours under nitrogen atmosphere to obtain LiMO-1 with a layered structure. In the composition formula (A), LiMO-1 had x=0.99, y=0.93, s=0.064, z+t+u=0.005, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg. Composition of LiMO-1, I A / I B , BET specific surface area, D 50 , (D 90 -D 10 ) / D 50 The average particle strength, the standard deviation of the particle strength, and the cycle retention rate are shown in Table 1. The same is true for the following Examples and Comparative Examples.

[0150] <Example 2> Water was placed in a reaction vessel equipped with a stirrer and an overflow pipe, and then an aqueous sodium hydroxide solution was added and the liquid temperature (reaction temperature) was maintained at 50°C. A raw material liquid 2 was prepared by mixing an aqueous solution of nickel sulfate, an aqueous solution of manganese sulfate, and an aqueous solution of aluminum sulfate in such a ratio that the atomic ratio of Ni, Mn, and Al was 93:3.5:3.5.

[0151] Next, a 0.1 wt% aqueous calcium hydroxide solution, a 0.1 wt% aqueous magnesium sulfate solution, a 0.1 wt% aqueous sodium silicate solution, a 0.1 wt% aqueous iron chloride solution, and a 0.1 wt% aqueous cobalt sulfate solution were added to raw material liquid 2 in ratios such that (Si+Na+Ca) / Co=0.65, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=758 ppm, Si / Na=1.80, and Si / Ca=15.69, to obtain a mixed raw material liquid 2.

[0152] LiMO-2 having a layered structure was obtained in the same manner as in Example 1, except that the mixed raw material liquid 2 was used and the temperature during main firing was set to 770° C. In the composition formula (A) of LiMO-2, x = 0.95, y = 0.93, s = 0.066, z + t + u = 0.0017, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0153] <Example 3> To the above-mentioned raw material liquid 2, a calcium hydroxide aqueous solution having a concentration of 0.1 wt%, a magnesium sulfate aqueous solution having a concentration of 0.1 wt%, a sodium silicate aqueous solution having a concentration of 0.1 wt%, an iron chloride aqueous solution having a concentration of 0.1 wt%, and a cobalt sulfate aqueous solution having a concentration of 0.1 wt% were added in such proportions that the following values ​​were obtained: (Si+Na+Ca) / Co=0.07, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=6197 ppm, Si / Na=0.92, and Si / Ca=12.84, to obtain a mixed raw material liquid 3.

[0154] Next, in the reaction vessel, an aqueous solution of ammonium sulfate was continuously added as a complexing agent to the mixed raw material liquid 3 under stirring. An aqueous solution of sodium hydroxide was added dropwise at appropriate times under the condition that the pH of the mixed liquid in the reaction vessel became 12.1 (when the liquid temperature was 40° C.), to obtain a metal composite hydroxide 3.

[0155] The obtained metal composite hydroxide 3 was washed and then dried at 105° C. for 20 hours to obtain a metal composite hydroxide MCC3.

[0156] MCC3 and lithium hydroxide monohydrate powder were weighed and mixed in a ratio of Li / (Ni+Co+Mn)=1.05 to obtain mixture 3. LiMO-3 having a layered structure was obtained in the same manner as in Example 1, except that Mixture 3 was used. In the composition formula (A) of LiMO-3, x = 0.98, y = 0.92, s = 0.073, z + t + u = 0.011, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0157] <Example 4> To the above-mentioned raw material liquid 2, a calcium hydroxide aqueous solution having a concentration of 0.1 wt%, a magnesium sulfate aqueous solution having a concentration of 0.1 wt%, a sodium silicate aqueous solution having a concentration of 0.1 wt%, an iron chloride aqueous solution having a concentration of 0.1 wt%, and a cobalt sulfate aqueous solution having a concentration of 0.1 wt% were added in such proportions that the following values ​​were obtained: (Si+Na+Ca) / Co=0.73, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=588 ppm, Si / Na=0.95, and Si / Ca=9.98, to obtain a mixed raw material liquid 4.

[0158] LiMO-4 having a layered structure was obtained in the same manner as in Example 1, except that the mixed raw material liquid 4 was used. In the composition formula (A) of LiMO-4, x = 0.99, y = 0.94, s = 0.064, z + t + u = 0.0013, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0159] <Example 5> To the above-mentioned raw material liquid 2, a calcium hydroxide aqueous solution having a concentration of 0.1 wt%, a magnesium sulfate aqueous solution having a concentration of 0.1 wt%, a sodium silicate aqueous solution having a concentration of 0.1 wt%, an iron chloride aqueous solution having a concentration of 0.1 wt%, and a cobalt sulfate aqueous solution having a concentration of 0.1 wt% were added in such proportions that the following values ​​were obtained: (Si+Na+Ca) / Co=0.67, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=570 ppm, Si / Na=1.64, and Si / Ca=11.41, to obtain a mixed raw material liquid 5.

[0160] LiMO-5 having a layered structure was obtained in the same manner as in Example 1, except that mixed raw material liquid 5 was used. In the composition formula (A) of LiMO-5, x = 1.00, y = 0.93, s = 0.066, z + t + u = 0.0013, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0161] <Comparative Example 1> To the above-mentioned raw material liquid 2, a calcium hydroxide aqueous solution having a concentration of 0.1 wt%, a magnesium sulfate aqueous solution having a concentration of 0.1 wt%, a sodium silicate aqueous solution having a concentration of 0.1 wt%, an iron chloride aqueous solution having a concentration of 0.1 wt%, and a cobalt sulfate aqueous solution having a concentration of 0.1 wt% were added in such proportions that the following values ​​were obtained: (Si+Na+Ca) / Co=8.34, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=3758 ppm, Si / Na=1.80, and Si / Ca=0.05, to obtain a mixed raw material liquid 6.

[0162] Next, in the reaction vessel, an aqueous solution of ammonium sulfate was continuously added as a complexing agent to the mixed raw material liquid 6 under stirring. An aqueous solution of sodium hydroxide was added dropwise at appropriate times under the condition that the pH of the mixed liquid in the reaction vessel became 12.1 (when the liquid temperature was 40° C.), to obtain a metal composite hydroxide 6.

[0163] The obtained metal composite hydroxide 6 was washed and then dried at 105° C. for 20 hours to obtain a metal composite hydroxide MCC6.

[0164] MCC6 and lithium hydroxide monohydrate powder were weighed and mixed in a ratio of Li / ((Ni+Mn+Al)=1.15 to obtain mixture 6. Thereafter, the mixture 6 was pre-fired in an oxygen atmosphere at 650° C. for 5 hours. Then, the mixture was subjected to main calcination in an oxygen atmosphere at 770° C. for 5 hours to obtain calcined product 6.

[0165] LiMO-6 having a layered structure was obtained in the same manner as in Example 1, except that the fired product 6 was used. In the composition formula (A) of LiMO-6, x = 1.02, y = 0.93, s = 0.055, z + t + u = 0.0091, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0166] <Comparative Example 2> To the above-mentioned raw material liquid 2, a calcium hydroxide aqueous solution having a concentration of 0.1 wt%, a magnesium sulfate aqueous solution having a concentration of 0.1 wt%, a sodium silicate aqueous solution having a concentration of 0.1 wt%, an iron chloride aqueous solution having a concentration of 0.1 wt%, and a cobalt sulfate aqueous solution having a concentration of 0.1 wt% were added in such proportions that the following values ​​were obtained: (Si+Na+Ca) / Co=0.03, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=13196 ppm, Si / Na=13.09, and Si / Ca=22.82, thereby obtaining a mixed raw material liquid 7.

[0167] LiMO-7 having a layered structure was obtained in the same manner as in Example 3, except that mixed raw material liquid 7 was used. In LiMO-7, in the composition formula (A), x = 1.02, y = 0.94, s = 0.034, z + t + u = 0.023, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0168] <Comparative Example 3> To the above-mentioned raw material liquid 2, a calcium hydroxide aqueous solution having a concentration of 0.1 wt%, a magnesium sulfate aqueous solution having a concentration of 0.1 wt%, a sodium silicate aqueous solution having a concentration of 0.1 wt%, an iron chloride aqueous solution having a concentration of 0.1 wt%, and a cobalt sulfate aqueous solution having a concentration of 0.1 wt% were added in such proportions that the following values ​​were obtained: (Si+Na+Ca) / Co=117.92, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=130 ppm, Si / Na=1.39, and Si / Ca=3.47, to obtain a mixed raw material liquid 8.

[0169] Next, in the reaction vessel, an aqueous solution of ammonium sulfate was continuously added as a complexing agent to the mixed raw material liquid 8 under stirring. An aqueous solution of sodium hydroxide was added dropwise at appropriate times under the condition that the pH of the mixed liquid in the reaction vessel became 12.1 (when the liquid temperature was 40° C.), thereby obtaining a metal composite hydroxide 8.

[0170] The obtained metal composite hydroxide 8 was washed and then dried at 105° C. for 20 hours to obtain a metal composite hydroxide MCC8.

[0171] MCC8 and lithium hydroxide monohydrate powder were weighed and mixed in a ratio of Li / (Ni+Mn+Al)=1.03 to obtain mixture 8. Thereafter, the mixture 8 was pre-fired in an oxygen atmosphere at 650° C. for 5 hours. Then, the mixture was subjected to main calcination in an oxygen atmosphere at 750° C. for 5 hours to obtain calcined product 8.

[0172] The obtained fired product 8 was crushed in a mortar to obtain a crushed product 8.

[0173] LiMO-8 having a layered structure was obtained in the same manner as in Example 1, except that the crushed material 8 was used. In the composition formula (A) of LiMO-8, x = 1.00, y = 0.94, s = 0.061, z + t + u = 0.0004, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0174] <Comparative Example 4> Water was placed in a reaction vessel equipped with a stirrer and an overflow pipe, and then an aqueous sodium hydroxide solution was added and the liquid temperature (reaction temperature) was maintained at 50°C. A nickel sulfate aqueous solution, a manganese sulfate aqueous solution, and an aluminum sulfate aqueous solution were mixed in such a ratio that the atomic ratio of Ni, Mn, and Al was 93:6:1, to prepare raw material liquid 4. To the above-mentioned raw material liquid 4, a calcium hydroxide aqueous solution having a concentration of 0.1 wt%, a magnesium sulfate aqueous solution having a concentration of 0.1 wt%, a sodium silicate aqueous solution having a concentration of 0.1 wt%, an iron chloride aqueous solution having a concentration of 0.1 wt%, and a cobalt sulfate aqueous solution having a concentration of 0.1 wt% were added in such proportions that the following values ​​were obtained: (Si+Na+Ca) / Co=1.23, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=925 ppm, Si / Na=0.35, and Si / Ca=12.84, to obtain a mixed raw material liquid 9.

[0175] Next, in the reaction vessel, an aqueous solution of ammonium sulfate was continuously added as a complexing agent to the mixed raw material liquid 9 under stirring. An aqueous solution of sodium hydroxide was added dropwise at appropriate times under the condition that the pH of the mixed liquid in the reaction vessel became 12.1 (when the liquid temperature was 40° C.), thereby obtaining a metal composite hydroxide 9.

[0176] The obtained metal composite hydroxide 9 was washed and then dried at 105° C. for 20 hours to obtain a metal composite hydroxide MCC9.

[0177] MCC9 and lithium hydroxide monohydrate powder were weighed and mixed in a ratio of Li / (Ni+Mn+Al)=1.05 to obtain mixture 9. LiMO-9 having a layered structure was obtained in the same manner as in Comparative Example 3, except that Mixture 9 was used and the temperature during main firing was set to 770° C. In LiMO-9, in the composition formula (A), x = 1.02, y = 0.93, s = 0.067, z + t + u = 0.0023, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0178] <Comparative Example 5> To the above-mentioned raw material liquid 2, a calcium hydroxide aqueous solution having a concentration of 0.1 wt%, a magnesium sulfate aqueous solution having a concentration of 0.1 wt%, a sodium silicate aqueous solution having a concentration of 0.1 wt%, an iron chloride aqueous solution having a concentration of 0.1 wt%, and a cobalt sulfate aqueous solution having a concentration of 0.1 wt% were added in such proportions that the following values ​​were obtained: (Si+Na+Ca) / Co=0.64, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=752 ppm, Si / Na=1.80, and Si / Ca=39.22, to obtain a mixed raw material liquid 10.

[0179] LiMO-10 having a layered structure was obtained in the same manner as in Comparative Example 3, except that the mixed raw material liquid 10 was used. In the composition formula (A) of LiMO-10, x = 0.98, y = 0.93, s = 0.064, z + t + u = 0.0016, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0180] [Table 1]

[0181] As shown in Table 1 above, in Examples 1 to 5 which satisfied the above (1) and (2), the cycle retention rates were all 80% or more, and the cycle characteristics were excellent.

[0182] On the other hand, in Comparative Examples 1 and 2 which did not satisfy the above (1), in Comparative Examples 4 and 5 which did not satisfy the above (2), and in Comparative Example 3 which did not satisfy the above (1) and (2), the cycle retention was less than 80%. [Explanation of symbols]

[0183] 1: separator, 2: positive electrode, 2a: positive electrode active material layer, 2b: positive electrode current collector layer, 3: negative electrode, 4: electrode group, 5: battery can, 6: electrolyte, 7: top insulator, 8: sealing body, 10: lithium secondary battery, 21: positive electrode lead, 31: negative electrode lead, 100: laminate, 110: positive electrode, 111: positive electrode active material layer, 112: positive electrode current collector, 113: external terminal, 120: negative electrode, 121: negative electrode active material layer, 122: negative electrode current collector, 123: external terminal, 130: solid electrolyte layer, 200: exterior body, 200a: opening, 1000: all-solid-state lithium secondary battery< / cam>

Claims

1. A lithium metal composite oxide having a layered structure and satisfying the following (1) and (2): (1) The alloy contains Co, an element M1, and an element M2, and the molar ratio of the element M1 to the Co is 0.05 or more and 6 or less. The element M1 is one or more elements selected from the group consisting of Si, Ca, and Na, and the element M2 is one or more elements selected from the group consisting of Fe and Mg. (2) In powder X-ray diffraction measurement using CuKα radiation, there are two diffraction peaks within the range of 2θ = 38.0 ± 0.5°, and when the diffraction peak on the lower angle side of the two diffraction peaks is designated as Peak A and the diffraction peak on the higher angle side is designated as Peak B, the following formula is satisfied. 0.50≦I A / I B ≦0.75...Formula (I A is the peak area of ​​the peak A, and I B is the peak area of ​​the peak B.

2. 2. The lithium metal composite oxide according to claim 1, wherein the total mass of said Co, said element M1 and said element M2 contained in said lithium metal composite oxide is 12000 ppm or less.

3. 3. The lithium metal composite oxide according to claim 1, wherein the element M1 contains Ca and Si, and a molar ratio of the Si to the Ca is 8 or more.

4. 3. The lithium metal composite oxide according to claim 1, wherein the element M1 contains Na and Si, and a molar ratio of the Si to the Na is 0.5 or more.

5. BET specific surface area is 1.0 m 2 / g or more 2.0m 2 The lithium metal composite oxide according to claim 1 or 2, wherein the Li-ion concentration is 0.1 to 0.5% by mass.

6. D 10 , D 50 and D. 90 The lithium metal composite oxide according to claim 1 or 2, which satisfies the following formula (I): 0.5≦(D 90 -D 10 ) / D 50 ≦1.5...Formula (I) (D 10 is the 10% cumulative volume particle size of the lithium metal composite oxide, and D 50 is the 50% cumulative volume particle size of the lithium metal composite oxide, and D 90 is the 90% cumulative volume particle size of the lithium metal composite oxide.

7. 3. The lithium metal composite oxide according to claim 1, wherein the lithium metal composite oxide has an average particle strength of 20 MPa or more.

8. 3. The lithium metal composite oxide according to claim 1, wherein the standard deviation of particle strength of the lithium metal composite oxide is 40% or less.

9. A positive electrode active material for a lithium secondary battery, comprising the lithium metal composite oxide according to claim 1 or 2.

10. A positive electrode for a lithium secondary battery, comprising the positive electrode active material for a lithium secondary battery according to claim 9.

11. A lithium secondary battery comprising the positive electrode for lithium secondary batteries according to claim 10.

Citation Information

Patent Citations

  • Lithium metal composite oxide and method for producing the same

    JP2013112531A