Manufacturing method for mixture
Patent Information
- Application Number
- JP2023068774
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
【0007】 本開示の一態様によれば、グラスライニング機器の破損を防止することができる。
Smart Images

Figure 2024154754000001 
Figure 2024154754000002 
Figure 2024154754000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a mixture. [Background technology]
[0002] Glass-lined equipment can be damaged by static electricity generated during use. For example, Non-Patent Document 1 discloses a case of damage to a glass-lined mixing vessel caused by static electricity and measures against static electricity in glass-lined equipment. [Prior art documents] [Non-patent literature]
[0003] [Non-Patent Document 1] Masamitsu Sawada, "Static Electricity Damage to GL and Its Countermeasures," Kobelco Pantech Technical Report, Vol. 34, No. 3, pp. 22-27, 1990 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the effectiveness of conventional anti-static measures for glass-lined equipment in preventing damage is unclear. For example, the anti-static measures disclosed in Non-Patent Document 1 are only qualitative conditions, and the standards for preventing damage to glass-lined equipment are not clear.
[0005] One aspect of the present disclosure aims to prevent damage to glass-lined equipment. [Means for solving the problem]
[0006] A method for producing a mixture according to one embodiment of the present disclosure is a method for producing a mixture containing one or more solids and one or more liquids, in which A is the terminal settling velocity [m / s], B is the common logarithm of the solvent resistance [Ω·m], C is the power number, D is the floatation limit velocity ratio, and E is the specific surface area [m 2 / m 3], F is the common logarithm of the powder resistivity [Ω m], a = 26.54, b = 0.11, c = -1.71, d = -0.29, e = -0.50, f = 0.22, and the process includes a step of contacting a raw material mixture containing one or more types of solids and one or more types of liquids with a glass-lined equipment under the condition that a*A+b*B+c*C+d*D+e*E+f*F≦2.6. Effect of the Invention
[0007] According to one aspect of the present disclosure, damage to glass-lined equipment can be prevented. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. In this specification and the drawings, components having substantially the same functions are denoted by the same reference numerals, and redundant description will be omitted.
[0009] [Embodiment] One embodiment of the present invention is a method for producing a mixture containing a solid and a liquid by using glass-lined equipment. The glass-lined equipment is equipment that is glass-lined. Glass lining is a surface treatment method for forming a glass layer on a metal substrate such as steel. In the glass-lined equipment, the portion where the glass layer is formed is also called a glass-lined surface or the like.
[0010] Glass-lined equipment has, for example, corrosion resistance, inertness, heat resistance, etc., and is widely used in fields such as the chemical industry, pharmaceutical industry, food industry, electronics industry, etc. Examples of glass-lined equipment include reactors (or reaction kettles), stirring blades, stirring tanks, heat exchangers, dryers, evaporators, filters, etc.
[0011] Glass-lined equipment becomes electrically charged when the mixture is stirred, and when the charge is discharged, localized damage such as pinholes and peeling can occur on the glass-lined surface. If glass-lined equipment with a damaged glass-lined surface is continued to be used, corrosion will progress from the damaged area to the metal substrate, causing problems such as contamination of the contents due to metal elution and leakage of the contents outside the equipment. Therefore, if damage occurs to the glass-lined surface, it is necessary to stop using the glass-lined equipment and take measures such as repairing the damaged area and updating the equipment.
[0012] For example, Non-Patent Document 1 lists measures against static electricity in glass-lined equipment, such as using materials with low volume resistivity, avoiding strong stirring, and reducing the amount of contents. However, these measures against static electricity are qualitative conditions, and no clear criteria are given for preventing damage to the glass-lined surface of glass-lined equipment (hereinafter also referred to as "GL damage"). In addition, it is unclear to what extent these measures against static electricity can prevent GL damage.
[0013] The purpose of the method for producing a mixture in this embodiment is to prevent GL damage. In the method for producing a mixture in this embodiment, a mixture (hereinafter also referred to as a "target mixture") is produced under conditions in which the electrostatic parameters of the mixture (hereinafter also referred to as a "raw mixture") to be fed into the glass-lined equipment are within a specific range in order to prevent GL damage. According to this embodiment, the mixture is produced under conditions in which GL damage does not occur, so that GL damage can be prevented.
[0014] The mixture in this embodiment may be, for example, a slurry. The slurry in this embodiment may be, for example, a highly charged slurry having high electrostatic chargeability. An example of a highly charged slurry is a slurry that, when charged into a glass-lined device and stirred, produces a potential difference of 0.1 kV or more between the ground surface and the glass surface inside the device. An example of a highly charged slurry is a slurry that uses heptane or hexane as a solvent.
[0015] <Charge parameters> The charging parameters are a group of parameters that affect the charged state of the glass-lined equipment when a mixture is produced using the glass-lined equipment. The charging parameters are a group of parameters including charging factors that charge the glass-lined equipment and static electricity removal factors that remove static electricity from the glass-lined equipment. The charging factors and static electricity removal factors include factors related to the physical properties of the mixture, factors related to the stirring conditions for the mixture, and factors related to both.
[0016] In this embodiment, the following charging parameters (1) to (6) are used. Note that the following explanation is an example of candidate parameters when the glass-lined equipment is a glass-lined reactor and the mixture is a slurry.
[0017] (1) Powder resistance [Ω·m]: Powder resistance is the volume resistivity of a solid. Volume resistivity is also called electrical conductivity. Powder resistance may be converted into a logarithmic value for use.
[0018] (1) Powder resistance can be measured by filling a sample into a powder sample container and measuring the value one minute after voltage application. The measurement should be carried out 3 to 10 times by replacing the sample, and the average of the three stable results should be used as the measured powder resistance.
[0019] (1) Powder resistance is 1.5 x 10 5 [Ω m] or more 6.0×10 18 (1) The powder resistivity is preferably 1.5×10 7 [Ω m] or more 6.0×10 16 (1) The powder resistivity is 1.4×10 9 [Ω m] or more 3.7×10 14 It is more preferable that the resistance be 0.1 to 1.0 Ω·m or less.
[0020] (2) Solvent resistance [Ω·m]: Solvent resistance is the volume resistivity of a liquid. Solvent resistance may be converted to a logarithmic value for use, as with powder resistance.
[0021] When the mixture is a slurry using multiple solvents, (2) the solvent resistance can be calculated using equation (1).
[0022]
number
[0023] where k is the solvent resistance of the slurry, ki (i = 1, 2, ···) is the solvent resistance of pure component i, and xi is the composition of component i in the liquid phase of the slurry.
[0024] The solvent resistance of each component may be measured, for example, by filling a sample into a liquid sample container and measuring the value one minute after voltage application. The measurement should be carried out 3 to 10 times by replacing the sample, and the average of the three stable results should be used as the measured value of the solvent resistance.
[0025] (2) Solvent resistance is 10[Ω·m] or more, 1.7×10 15 (2) The solvent resistance is preferably 1.0×10 2 [Ω m] or more 1.7×10 14 (2) The solvent resistance is preferably 1.0×10 3 [Ω m] or more 3.3×10 13 It is more preferable that the resistance be 0.1 to 1.0 Ω·m or less.
[0026] (3) Power number: The power number is determined by the shape of the stirring blade and the type and number of baffle plates. The power number is a value specific to the glass-lined reactor.
[0027] (3) The power number is preferably 0.2 or greater and 4.8 or less. (3) The power number is more preferably 0.3 or greater and 2.9 or less. (3) The power number is even more preferably 0.4 or greater and 1.0 or less.
[0028] (4) Terminal settling velocity [m / s]: Terminal settling velocity is the velocity that a solid of D50 reaches when it falls through a liquid used for a slurry in an unstirred state.
[0029] Note that D50 is the particle diameter at the point where the integrated value is 50% (also called the "median diameter"). The particle diameter used is that of the solid particles in the dry state (also called "dry cake" or "D / C").
[0030] (4) The terminal settling velocity can be calculated by applying the formula for obtaining the terminal settling velocity applicable to each region determined according to the value of the particle Reynolds number (Re number). The Re number can be calculated using Equation (2).
[0031] [Number]
[0032] However, ρf is the solvent density [kg / m 3 , us is the terminal settling velocity, dp is the particle diameter of D50 [m], and μf is the solvent viscosity [Pa·s].
[0033] The terminal settling velocity us is calculated by Equation (2-1) in the Stokes region (Re < 2) and by Equation (2-2) in the Allen region (2 < Re < 500).
[0034] [Number]
[0035] However, ρs is the powder density [kg / m 3 , and g is the gravitational acceleration [kg / ·s 2 .
[0036] (4) The terminal settling velocity is preferably 2.0×10 -5 [m / s] or more and 8.4×10 -2 [m / s] or less.
[0037] (5) Suspension limit speed ratio: The suspension limit speed ratio is the ratio between the rotation speed [rpm] and the suspension limit speed [rpm]. If the suspension limit speed ratio is greater than 1, the solids can be uniformly stirred in the glass-lined reactor. On the other hand, if the suspension limit speed ratio is less than 1, the solids tend to accumulate in the lower part of the glass-lined reactor.
[0038] The rotation speed is the number of rotations per minute of the agitator in the glass-lined reactor. The floating limit speed is the rotation speed required to float the solid D50 that has settled to the bottom of the glass-lined reactor to the top of the glass-lined reactor.
[0039] The critical floating speed can be calculated using the stirring speed calculated by Zwietering's formula (3).
[0040]
number
[0041] where Nf is the limit velocity of buoyancy, φ is a coefficient determined by the impeller shape, D is the vessel diameter of the glass-lined reactor [m], d is the impeller span [m], t is a coefficient determined by the impeller shape, and Δρ is the density difference between the powder and the solvent [kg / m 3 ] and ρf is the solvent density [kg / m 3 ], and g is the gravitational acceleration [kg / m s 2 ], μf is the solvent viscosity [Pa s], dp is the D50 particle size [m], and X is the weight ratio of solid to liquid (solid concentration) [kg / kg].
[0042] (5) The maximum floating speed ratio is preferably greater than or equal to 0.96 and less than or equal to 5.38.
[0043] (6) Specific surface area [m 2 / m 3 ]: Specific surface area is the amount of slurry [m 3 ] Wetted area per unit volume [m 2 ].
[0044] The slurry liquid volume is the volume of the slurry in the glass-lined reactor. The slurry liquid volume is not the volume of only the liquid, but the sum of the liquid volume and the solid volume. The liquid contact area is the area where the glass-lined surface and the slurry come into contact when a specified volume of slurry is placed in a glass-lined reactor of a specified volume.
[0045] (6) The specific surface area is 1.8 [m 2 / m 3 ] or more than 6.3[m 2 / m 3 (6) The specific surface area is preferably 1.8 [m 2 / m 3 ] or more than 4.8[m 2 / m 3 (6) The specific surface area is preferably 1.8 [m 2 / m 3 ] or more than 4.2[m 2 / m 3 ] or less is even more preferable.
[0046] <Method of manufacturing the mixture> An example of a method for producing a mixture in this embodiment will be described. The method for producing a mixture in this embodiment is a method for producing a target mixture using glass-lined equipment. The production of the target mixture includes a step of contacting a raw material mixture with the glass-lined equipment. The step of contacting the raw material mixture with the glass-lined equipment includes, for example, putting the raw material mixture into a glass-lined reactor and stirring the raw material mixture under conditions where the charging parameters are in a specific range.
[0047] In the method for producing a mixture according to the present embodiment, the raw material mixture is brought into contact with a glass-lined device under conditions in which the electrification parameter falls within a specific range. The specific range is specifically expressed by formula (4).
[0048]
number
[0049] where A is the terminal settling velocity, B is the common logarithm of the solvent resistance, C is the power number, D is the floating limit velocity ratio, E is the specific surface area, F is the common logarithm of the powder resistance, and a, b, c, d, e, and f are predetermined constants. The constants a, b, c, d, e, and f are a = 26.54, b = 0.11, c = -1.71, d = -0.29, e = -0.50, and f = 0.22.
[0050] <Verification results> The results of verifying the presence or absence of GL damage according to this embodiment will be described with reference to Table 1. Table 1 is a table showing an example of the verification results.
[0051] [Table 1]
[0052] In verifying the presence or absence of GL damage, performance data including many charging parameters and the presence or absence of GL damage was collected, and an evaluation value Y was calculated under the conditions of each performance data. Below, the conditions under which there was no GL damage are described as examples, and the conditions under which there was GL damage are described as comparative examples.
[0053] As shown in Table 1, in Comparative Examples 1 and 2, the evaluation values Y were 4.0 and 2.4, respectively, which were outside the range of -3.8 to 2.6. In Examples 1 to 3, the evaluation values Y were 1.7, -0.018, and -2.6, respectively, which were within the range of -3.8 to 2.6.
[0054] As described above, in all of the examples in which there was no GL damage, the evaluation value Y was within the specific range. On the other hand, in all of the comparative examples in which there was GL damage, the evaluation value Y was outside the specific range. This verification showed that according to the method for producing a mixture in this embodiment, it is possible to produce a mixture without causing GL damage.
[0055] <Effects of the embodiment> In the method for producing a mixture in this embodiment, the raw material mixture is brought into contact with glass-lined equipment under conditions where the weighted sum of a plurality of electrification parameters is within a specific range. Analysis of past records of GL damage has revealed that GL damage due to the mixture does not occur when the weighted sum of predetermined electrification parameters is within a specific range. Therefore, according to this embodiment, GL damage of glass-lined equipment can be prevented.
[0056] The charging parameters in this embodiment are terminal settling velocity, solvent resistance, power number, floating limit velocity ratio, specific surface area, and powder resistance. These charging parameters are factors that change the charging state of the glass-lined equipment when the mixture is brought into contact with the glass-lined equipment. It is known that one cause of GL damage is static electricity generated by stirring the mixture. Therefore, according to this embodiment, GL damage of the glass-lined equipment due to static electricity can be accurately prevented.
[0057] The mixture in this embodiment includes one or more solids and one or more liquids. The mixture including one or more solids and one or more liquids may be a slurry. The slurry may be a highly charged slurry. Therefore, according to this embodiment, damage to the GL of the glass-lined equipment when producing the slurry can be prevented.
[0058] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to these embodiments, and various modifications and changes are possible within the scope of the gist of the present invention described in the claims.
Claims
1. 1. A method for producing a mixture comprising producing a mixture comprising one or more solids and one or more liquids, comprising the steps of: A is the terminal settling velocity [m / s], B is the common logarithm of the solvent resistance [Ω·m], C is the power number, D is the maximum floating speed ratio, E is the specific surface area [m 2 / m 3 ], F is the common logarithm of the powder resistance [Ω m], a = 26.54, b = 0.11, c = -1.71, d = -0.29, e = -0.50, f = 0.22, The method includes contacting a raw material mixture containing one or more solids and one or more liquids with a glass-lined equipment under the condition that a*A+b*B+c*C+d*D+e*E+f*F≦2.6; Method for producing the mixture.
2. The contacting step contacts the raw material mixture with the glass-lined equipment under a condition of -3.8≦a*A+b*B+c*C+d*D+e*E+f*F≦2.
6. A method for producing the mixture of claim 1.
3. A is 2.0 x 10 -5 Above 8.4 x 10 -2 is as follows: B is 10 or more, 1.7 x 10 15 is as follows: C is equal to or greater than 0.2 and equal to or less than 4.8; D is equal to or greater than 0.96 and equal to or less than 5.38; E is equal to or greater than 1.8 and equal to or less than 6.3; F is 1.5 x 10 5 Above 6.0 x 10 18 Below is the A method for producing the mixture of claim 1.
4. The mixture is a slurry. A method for producing the mixture according to any one of claims 1 to 3.
5. The slurry is a highly charged slurry. A method for producing the mixture according to claim 4.