Ink set for inkjet textile printing, image forming method and image formed object
The inkjet textile printing ink set with a block copolymer having hydrophilic blocks at both ends addresses adhesion and stability issues, enhancing ejection stability and fastness of printed images on fabrics.
Patent Information
- Application Number
- JP2023069162
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-04-20
AI Technical Summary
Existing inkjet textile printing technologies face issues with pigment adhesion to fabrics, leading to inadequate washing fastness and abrasion resistance, as well as ejection stability during printing, due to the use of pigment dispersants with hydrophilic sites only at one end of the molecule.
An inkjet textile printing ink set comprising an ink and a pretreatment liquid, where the ink contains a block copolymer with two hydrophilic blocks at both ends and a hydrophobic block in between, interacting with a flocculant, and an aqueous solvent, to enhance adhesion and stability.
The solution results in improved ejection stability and high washing and abrasion fastness of printed images on fabrics, with the block copolymer providing strong bonding at multiple points and preventing fabric hardening.
Smart Images

Figure 2024154928000001 
Figure 2024154928000002 
Figure 2024154928000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an ink set for ink-jet textile printing, an image forming method, and an image formed product. [Background technology]
[0002] In recent years, ink-jet printing, in which an image is formed on a fabric by an ink-jet system, has become widely used as a textile printing method because it allows dyeing in a short time and has high production efficiency.
[0003] Known pigment-based inks used in inkjet textile printing include inks containing a pigment and a pigment dispersant and inks containing a self-dispersing pigment. From the viewpoint of making it easier to aggregate the pigment contained in the pigment-based ink, suppressing bleeding of the pigment-based ink, and improving fixability, it has been considered to perform a pretreatment for applying an aggregating agent for aggregating the pigment dispersion to the fabric.
[0004] For example, Patent Document 1 discloses a method of forming an image by applying a pretreatment liquid to a fabric to perform pretreatment, and then applying an inkjet ink. The pretreatment liquid contains a thermoplastic resin, a cationic surfactant, and water; the ink contains a pigment, an anionic dispersant, a water-soluble organic solvent, and water. In the examples, a styrene-acrylic acid copolymer (random copolymer) is used as the pigment dispersant.
[0005] As a pigment-based ink set used for forming images on plain paper other than fabrics, Patent Document 2 discloses an ink set containing an ink containing carbon black and a dispersion resin, and a reaction liquid containing a reactive substance. In the examples, a terblock copolymer containing a hydrophobic block segment A, a nonionic hydrophilic block segment B, and an ionic hydrophilic block segment C in this order is used as the dispersion resin.
[0006] Patent Document 3 discloses an ink set having an ink containing carbon black dispersed with a polymer dispersant and a reaction liquid containing an inorganic salt and a polyamine that reacts with the ink. As the polymer dispersant, a block copolymer containing an A block composed of 2 to 8 units of methacrylic acid or a salt thereof and a B block containing at least 2 units of methacrylic acid or a salt thereof and at least 16 units of benzyl methacrylate is used.
[0007] In all of these documents, the carbon black dispersion contained in the ink is agglomerated by a reactive substance (agglomerating agent) contained in the reaction liquid, thereby improving the fixability of the pigment and the image density. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2008-231617 A [Patent Document 2] JP 2009-298842 A [Patent Document 3] JP 2010-513672 A Summary of the Invention [Problem to be solved by the invention]
[0009] In the above Patent Documents 2 and 3, the reaction between the hydrophilic portion of the pigment dispersant and the flocculant is utilized to aggregate the pigment. The pigment dispersants used in these documents all have a block containing a hydrophilic portion at only one end of the molecule. However, when a pigment-based ink using such a pigment dispersant is applied to a fabric, there are problems in that the adhesion of the ink coating to the fabric is insufficient or the fabric is likely to harden, which tends to reduce the abrasion resistance (washing fastness) and friction fastness of the image-formed product when washed. In addition, there is a problem in that the pigment is likely to aggregate due to the interaction between the pigment dispersants, and the ejection stability when ejected by the inkjet method is also likely to be impaired.
[0010] The present invention has been made in view of the above circumstances, and has an object to provide an ink set for ink-jet textile printing, which is capable of forming an image having good ejection stability while having high fastness to washing and friction, and an image formed therefrom. [Means for solving the problem]
[0011] The above problem can be solved by the following configuration.
[0012] [1] An ink set for inkjet textile printing comprising an ink and a pretreatment liquid, the pretreatment liquid comprising a flocculant, the ink comprising a pigment, a block copolymer, and an aqueous solvent, the block copolymer comprising two hydrophilic blocks A arranged at both ends of the block copolymer molecule and interacting or reacting with the flocculant, and a hydrophobic block B arranged between the two hydrophilic blocks. [2] The ink set for ink-jet textile printing according to [1], wherein the block copolymer is an ABA type block copolymer consisting of the two hydrophilic blocks A and one hydrophobic block B. [3] The ink set for ink-jet textile printing according to [1] or [2], wherein the two hydrophilic blocks A have the same monomer composition. [4] The ink set for ink-jet textile printing according to any one of [1] to [3], wherein the hydrophilic block A contains a structural unit derived from a hydrophilic monomer which is a vinyl-based monomer containing a hydrophilic functional group selected from the group consisting of a hydroxyl group, a carboxyl group, and a sulfonic acid group, and a content of the structural unit derived from the hydrophilic monomer in the hydrophilic block A is higher than that in the hydrophobic block B. [5] The ink set for ink-jet printing according to [4], wherein the hydrophobic block B contains a structural unit derived from a hydrophobic monomer selected from the group consisting of vinyl monomers containing an aromatic ring group or an alicyclic hydrocarbon group, and the content of the structural unit derived from the hydrophilic monomer in the hydrophobic block B is lower than that in the hydrophilic block A. [6] The ink set for ink-jet textile printing according to any one of [1] to [5], wherein the flocculating agent contains a polyvalent metal salt, an organic acid, or a compound having a cationic group. [7] A method for forming an image, comprising the step of applying an ink by an inkjet method onto a fabric having a flocculant adhered thereto, the ink comprising a pigment, a block copolymer, and an aqueous solvent, the block copolymer comprising two hydrophilic blocks A arranged at both ends of the molecule and interacting or reacting with the flocculant, and a hydrophobic block B arranged between the two hydrophilic blocks. [8] An image-formed product comprising: a fabric having a flocculant attached thereto; and an image layer disposed on the fabric, the image layer including a pigment and a block copolymer that interacts or reacts with the flocculant, the block copolymer including two hydrophilic blocks A that are disposed at both ends of the molecule and interact or react with the flocculant, and a hydrophobic block B disposed between the two hydrophilic blocks. Effect of the Invention
[0013] According to the present invention, it is possible to provide an ink set for ink-jet textile printing, which is capable of forming an image having good jetting stability and high fastness to washing and abrasion, and an image-formed product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] 1. Ink set 1-1.Ink The ink according to this embodiment contains a pigment, a block copolymer, and a water-based solvent.
[0015] 1-1-1.Pigments The pigment contained in the ink is not particularly limited, but is preferably an organic pigment or an inorganic pigment having the following numbers as described in the Color Index.
[0016] Examples of orange pigments include Pigment Orange 31 and 43.
[0017] Examples of red or magenta pigments include Pigment Red 3, 5, 19, 22, 31, 38, 43, 48:1, 48:2, 48:3, 48:4, 48:5, 49:1, 53:1, 57:1, 57:2, 58:4, 63:1, 81, 81:1, 81:2, 81:3, 81:4, 88, 104, 108, 112, 122, 123, 144, 146, 149, 166, 168, 169, 170, 177, 178, 179, 184, 185, 208, 216, 226, 257, Pigment Violet 3, 19, 23, 29, 30, 37, 50, 88, Pigment Orange 13, 16, 20, 36.
[0018] Examples of blue or cyan pigments include Pigment Blue 1, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 17-1, 22, 27, 28, 29, 36, 60.
[0019] Examples of green or yellow pigments include Pigment Green 7, 26, 36, and 50. Examples of yellow pigments include Pigment Yellow 1, 3, 12, 13, 14, 15, 17, 34, 35, 37, 55, 74, 81, 83, 93, 94, 95, 97, 108, 109, 110, 128, 137, 138, 139, 151, 153, 154, 155, 157, 166, 167, 168, 180, 185, 193, and 213.
[0020] Examples of black pigments include Pigment Black 7, 28, and 26.
[0021] Commercially available examples of pigments include: Chromofine Yellow 2080, 5900, 5930, AF-1300, 2700L, Chromofine Orange 3700L, 6730, Chromofine Scarlet 6750, Chromofine Magenta 6880, 6886, 6891N, 6790, 6887, Chromofine Violet RE, Chromofine Red 6820, 6830, Chromofine Blue HS-3, 5187, 5108, 5197, 5085N, SR-5020, 5026, 5050, 4920, 4927, 4937, 4824, 4933GN-EP, 4940, 4973, 5205, 5208, 5214, 5221, 5000P , Chrome Fine Green 2GN, 2GO, 2G-550D, 5310, 5370, 6830, Chrome Fine Black A-1103, Seika Fast Yellow 10GH, A-3, 2035, 2054, 2200, 2270, 2300, 2400(B), 2500, 2600, ZAY-260, 2700(B), 2770 , Seika Fast Red 8040, C405(F), CA120, LR-116, 1531B, 8060R, 1547, ZAW-262, 1537B, GY, 4R-4016, 3820, 3891, ZA-215, Seika Fast Carmine 6B1476T-7, 1483LT, 3840, 3870, Seika Fast Bordeaux 10B-430, Seika Light Rose R40, Seika Light Violet B800, 7805, Seika Fast Maroon 460N, Seika Fast Orange 900, 2900, Seika Light Blue C718, A612, Cyanine Blue 4933M, 4933GN-EP, 4940, 4973 (Dainichi Seika Chemicals); KET Yellow 401, 402, 403, 404, 405, 406, 416, 424, KET Orange 501, KET Red 301, 302, 303, 304, 305, 306, 307, 308, 309, 310, 336, 337, 338, 346, KET Blue 101, 102, 103, 104, 105, 106, 111, 118, 124, KET Green 201 (manufactured by Dainippon Ink & Chemicals);Colortex Yellow 301, 314, 315, 316, P-624, 314, U10GN, U3GN, UNN, UA-414, U263, Finecol Yellow T-13, T-05, Pigment Yellow1705, Colortex Orange 202, Colortex Red101, 103, 115, 116, D3B, P-625, 102, H-1024, 105C, UFN, UCN, UBN, U3BN, URN, UGN, UG276, U456, U457, 105C, USN, Colortex Maroon601, Colortex BrownB610N, Colortex Violet600, Pigment Red 122, Colortex Blue516, 517, 518, 519, A818, P-908, 510, Colortex Green 402, 403, Colortex Black 702, U905 (Sanyo Pigment); Lionol Yellow 1405G, Lionol Blue FG7330, FG7350, FG7400G, FG7405G, ES, ESP-S (Toyo Ink Co., Ltd.); Toner Magenta E02, Permanent Rubin F6B, Toner Yellow HG, Permanent Yellow GG-02, Hostapearm Blue B2G (Hoechst Industry); Novoperm P-HG, Hostaperm Pink E, Hostaperm Blue B2G (manufactured by Clariant); Carbon black #2600, #2400, #2350, #2200, #1000, #990, #980, #970, #960, #950, #850, MCF88, #750, #650, MA600, MA7, MA8, MA11, MA100, MA100R, MA77, #52, #50, #47, #45, #45L, #40, #33, #32, #30, #25, #20, #10, #5, #44, CF9 (manufactured by Mitsubishi Chemical).
[0022] From the viewpoint of improving dispersibility in the ink, the pigment is preferably further dispersed with a pigment dispersant, which will be described later.
[0023] The pigment may also be a self-dispersing pigment. A self-dispersing pigment is a pigment particle whose surface is modified with a group having a hydrophilic group, and has a pigment particle and a group having hydrophilicity bonded to its surface. Examples of the hydrophilic group include a carboxy group, a sulfonic acid group, and a phosphorus-containing group. Examples of the phosphorus-containing group include a phosphoric acid group, a phosphonic acid group, a phosphinic acid group, a phosphite group, and a phosphate group.
[0024] Commercially available examples of self-dispersing pigments include Cabot's Cab-0-Jet® 200K, 250C, 260M, and 270V (sulfonic acid group-containing self-dispersing pigments), Cab-0-Jet® 300K (carboxylic acid group-containing self-dispersing pigments), and Cab-0-Jet® 400K, 450C, 465M, 470V, and 480V (phosphate group-containing self-dispersing pigments).
[0025] The pigment content is not particularly limited, but from the viewpoint of easily adjusting the viscosity of the ink to the range described below and forming a higher density image, it is preferably 0.3 to 12% by mass relative to the ink. If the pigment content is 0.3% by mass or more, the color of the obtained image tends to be vivid, and if it is 5% by mass or less, the viscosity of the ink does not become too high, so that the ejection stability is not easily impaired. From the same viewpoint, it is more preferable that the pigment content is 0.5 to 8% by mass relative to the ink.
[0026] 1-1-2.Block copolymer The block copolymer may be included as a pigment dispersant or as a fixing resin. In the present embodiment, the block copolymer is included as a pigment dispersant.
[0027] Conventionally, pigment dispersants that have been used are either random copolymers that randomly contain sites that interact or react with the flocculant, or AB-type block copolymers that have a block (usually a hydrophilic block A) that contains many sites that interact or react with the flocculant at only one end of the molecule. A random copolymer does not have a block containing many sites that interact or react with a flocculant, and therefore does not easily interact or react with the flocculant. Although an AB-type block copolymer has a block containing many sites that interact or react with a flocculant, the block is located only at one end of the molecule, and therefore there are few bonding points that can bond with the fabric. Therefore, it is difficult to obtain adhesion of the copolymer to the fabric, and the washing fastness and friction fastness are also low. In addition, since the copolymer can be continuously (film-like) bonded to the fabric at one bonding point, the fabric also tends to become hard.
[0028] In contrast, the above block copolymers such as ABA type contain blocks at both ends of the molecule that contain many sites that interact or react with the flocculant. Since the blocks are present at at least two locations at both ends of the molecule, there are many bonding points that can be bonded to the fabric, and the bond with the fabric is likely to be strong. This improves adhesion to the fabric, and the washing fastness and friction fastness are likely to be high. In addition, since the above copolymer can be intermittently bonded to the fabric at multiple bonding points, the fabric is less likely to become hard than if it were continuously bonded at one bonding point. The block containing many sites that interact or react with the flocculant is a hydrophilic block.
[0029] That is, the block copolymer used in this embodiment contains two hydrophilic blocks A arranged at both ends of the molecule and a hydrophobic block B arranged therebetween.
[0030] The "hydrophilic block A" is a block that enhances the affinity with the aqueous solvent contained in the ink and contains a site that interacts or reacts with the coagulant attached to the fabric, and refers to a block that has a higher affinity with water among the blocks constituting the copolymer. The number of hydrophilic blocks is preferably two.
[0031] The hydrophilic block A contains a structural unit derived from a monomer having a hydrophilic functional group (hereinafter referred to as a "hydrophilic monomer") Examples of the hydrophilic functional group include a hydroxyl group, a carboxyl group, and a sulfonic acid group.
[0032] Examples of the hydrophilic monomer constituting the hydrophilic block A include vinyl monomers containing a hydrophilic functional group, and examples thereof include monomers containing a carboxyl group or an acid anhydride group, such as unsaturated polycarboxylic acids such as (meth)acrylic acid and maleic acid, and maleic anhydride, monomers containing a sulfonic acid group, such as styrenesulfonic acid and 4-(methacryloyloxy)butylsulfonic acid, and ethylene oxide-modified (meth)acrylic acid ester monomers, such as ethylene oxide-modified (meth)acrylic acid alkyl esters. Of these, the hydrophilic monomer is preferably (meth)acrylic acid, from the viewpoint of imparting appropriate water solubility to the hydrophilic block A.
[0033] The content of the constitutional units derived from hydrophilic monomers in the hydrophilic block A may be greater than the content of the constitutional units derived from hydrophilic monomers in the hydrophobic block B. Specifically, the content of the constitutional units derived from hydrophilic monomers in the hydrophilic block A is preferably 5% by mass or more relative to 100% by mass of the hydrophilic block A. When the content of the constitutional units derived from hydrophilic monomers is 5% by mass or more, not only is the dispersibility in aqueous solvents more likely to be improved, but the copolymer also more likely to interact or react with the flocculant, making it easier to improve the adhesion to the fabric. From the same viewpoint, the content is more preferably 10 to 40% by mass.
[0034] The hydrophilic block A may further contain a structural unit derived from a monomer other than the hydrophilic monomer. Examples of the other monomer include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate and tert-butyl (meth)acrylate. Among these, C2 or higher alkyl esters such as butyl (meth)acrylate are preferred. This is because the Tg of the block copolymer is low and the fabric is less likely to become hard. However, the other monomers do not include hydrophobic monomers described later.
[0035] The "hydrophobic block B" is a portion that is adsorbed to the pigment, and is a block that has a smaller affinity for the aqueous solvent contained in the ink among the blocks that constitute the copolymer. The number of hydrophobic blocks B is preferably one.
[0036] The hydrophobic block B contains a structural unit derived from a monomer having a hydrophobic functional group (hereinafter referred to as a "hydrophobic monomer"). Examples of the monomer having a hydrophobic functional group include vinyl monomers having an aromatic ring group or an alicyclic hydrocarbon group.
[0037] Examples of vinyl monomers having an aromatic ring group include (meth)acrylates having an aromatic ring group, such as benzyl (meth)acrylate, phenyl (meth)acrylate, and phenoxyethyl (meth)acrylate; and aromatic vinyl monomers such as styrene, α-methylstyrene, 4-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methoxystyrene, 2-hydroxymethylstyrene, and 1-vinylnaphthalene, among which vinyl monomers having an aromatic ring group having 6 to 15 carbon atoms are preferred.
[0038] Examples of vinyl monomers having an alicyclic alkyl group include (meth)acrylates having an alicyclic alkyl group such as cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, cyclododecyl (meth)acrylate, bornyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate, and vinyl monomers having an alicyclic alkyl group having 6 to 15 carbon atoms are preferred.
[0039] Of these, from the viewpoint of improving the adsorption to the pigment, the hydrophobic monomer is preferably a vinyl monomer having an aromatic ring group having 6 to 15 carbon atoms, such as styrene.
[0040] The content of the structural units derived from hydrophobic monomers in the hydrophobic block B is preferably 80% by mass or more relative to the hydrophobic block B. When the content is 80% by mass or more, the adsorption to the pigment is more likely to be enhanced. From the same viewpoint, the content is more preferably more than 90% by mass, and further preferably 95% by mass or more.
[0041] The hydrophobic block B may further contain a structural unit derived from a monomer other than the hydrophobic monomer. Examples of the other monomer include the above-mentioned other monomers and the above-mentioned hydrophilic monomers. However, when the hydrophobic block B contains a structural unit derived from a hydrophilic monomer, the content ratio of the structural unit derived from the hydrophilic monomer in the hydrophobic block B is lower than that in the hydrophilic block A. Specifically, the content of the structural unit derived from the hydrophilic monomer is preferably 20% by mass or less, more preferably less than 10% by mass, and even more preferably 5% by mass or less, relative to the hydrophobic block B. In other words, of the two hydrophilic blocks A and B, the hydrophobic block B has the lowest content of the structural unit derived from the hydrophilic monomer (molar number of hydrophilic functional groups).
[0042] The content of the hydrophobic block B in the ABA block copolymer is preferably 20% by mass or more and 80% by mass or less, and more preferably 20% by mass or more and 50% by mass or less, based on the total mass of the block copolymer. When the content is 20% by mass or more, the content of the hydrophilic block A is small (or the molecular weight is small), so that crosslinking aggregation is more easily suppressed, and when the content is 80% by mass or less, the content of the hydrophilic block A is large (or the molecular weight is large), so that affinity to aqueous solvents is more easily increased.
[0043] When the hydrophilic block is A and the hydrophobic block is B, examples of the structure of the block copolymer include ABA type, ABABA type, etc. Among them, the block copolymer is preferably an ABA type block copolymer consisting of two hydrophilic blocks A arranged at both ends of the molecule and a hydrophobic block B arranged between them.
[0044] The types and compositional ratios of monomers in the multiple blocks A contained in the block copolymer may be the same as or different from each other. When the block copolymer contains multiple blocks B, the types and compositional ratios of monomers in the multiple blocks B may be the same as or different from each other. In particular, it is preferable that the two hydrophilic blocks A have the same monomer composition.
[0045] The weight average molecular weight of the block copolymer is preferably 5000 to 70000, and more preferably 7000 to 30000. The larger the weight average molecular weight, the easier it is to increase the dispersibility of the pigment in an aqueous solvent, and the smaller the weight average molecular weight, the easier it is to suppress crosslinking and aggregation between pigment dispersions. The weight average molecular weight of the block copolymer can be measured in polystyrene equivalent terms by gel permeation chromatography.
[0046] The molecular weight distribution (PDI) (weight average molecular weight (Mw) of the block copolymer) / (number average molecular weight (Mn) of the block copolymer) is preferably 2.0 or less, more preferably 1.8 or less. The lower the PDI, the narrower and more uniform the molecular weight distribution is, and therefore the better the dispersibility is.
[0047] The acid value of the block copolymer is, for example, preferably 40 to 400 mgKOH / g, more preferably 40 to 300 mgKOH / g, and even more preferably 40 to 190 mgKOH / g. When the acid value is 40 mgKOH / g or more, the hydrophilicity of the pigment dispersant is increased, and the dispersibility of the pigment can be further improved. When the acid value is 400 mgKOH / g or less, the hydrophilicity of the pigment dispersant is further prevented from being excessively increased, and the water resistance of the resulting image-formed product can be further improved. The acid value can be measured according to the measurement method of JIS K0070:1992.
[0048] The content of the block copolymer is preferably 10 to 50% by mass, more preferably 20 to 40% by mass, based on the pigment. When the content is 10% by mass or more, the dispersibility of the pigment in the pigment dispersion can be further improved. When the content of the pigment dispersant is 50% by mass or less, an increase in the viscosity of the pigment dispersion caused by an excessive amount of the pigment dispersant can be further suppressed.
[0049] The method for synthesizing the block copolymer is not particularly limited, but for example, the block copolymer can be obtained by sequentially polymerizing vinyl monomers constituting the blocks by a living radical polymerization method.
[0050] 1-1-3. Water-based solvents The aqueous solvent preferably contains water and further contains a water-soluble organic solvent.
[0051] The content of water is, for example, 20 to 70% by mass, and preferably 30 to 60% by mass, based on the ink.
[0052] The water-soluble organic solvent is not particularly limited as long as it is compatible with water, but from the viewpoint of making it easier for the ink to penetrate into the interior of the fabric and making it difficult for the ink ejection stability to be impaired in the inkjet method, it is preferable that the ink does not easily thicken due to drying. Therefore, it is preferable that the ink contains a high-boiling point solvent having a boiling point of 200° C. or more.
[0053] The high-boiling solvent having a boiling point of 200° C. or higher may be any water-soluble organic solvent having a boiling point of 200° C. or higher, and is preferably a polyol or a polyalkylene oxide.
[0054] Examples of polyols having a boiling point of 200°C or higher include dihydric alcohols such as 1,3-butanediol (boiling point 208°C), 1,6-hexanediol (boiling point 223°C), and polypropylene glycol; and trihydric or higher alcohols such as glycerin (boiling point 290°C) and trimethylolpropane (boiling point 295°C).
[0055] Examples of polyalkylene oxides having a boiling point of 200° C. or higher include ethers of dihydric alcohols such as diethylene glycol monoethyl ether (boiling point 202° C.), triethylene glycol monomethyl ether (boiling point 245° C.), tetraethylene glycol monomethyl ether (boiling point 305° C.), tripropylene glycol monoethyl ether (boiling point 256° C.) and polypropylene glycol, and ethers of trihydric or higher alcohols such as glycerin (boiling point 290° C.) and hexanetriol.
[0056] The solvent may further include other solvents in addition to the high boiling point solvent. Examples of the other solvents include polyhydric alcohols having a boiling point of less than 200° C. (e.g., ethylene glycol, propylene glycol, hexanetriol, etc.); polyhydric alcohol ethers having a boiling point of less than 200° C. (e.g., ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol dimethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether); monohydric alcohols (e.g., methanol, ethanol, propanol, pentanol, hexanol, cyclohexanol, butyl ether ... alcohol); amines (e.g., ethanolamine, N-ethyldiethanolamine, morpholine, N-ethylmorpholine, ethylenediamine, diethylenediamine, triethylenetetramine); amides (e.g., formamide, N,N-dimethylformamide, N,N-dimethylacetamide); heterocycles (e.g., 2-pyrrolidone, N-methyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, 2-oxazolidone, 1,3-dimethyl-2-imidazolidine), sulfoxides (e.g., dimethyl sulfoxide); and sulfones (e.g., sulfolane).
[0057] The content of the water-soluble organic solvent is, for example, 20 to 70% by mass, and preferably 30 to 60% by mass, relative to the ink.
[0058] 1-1-4.Other ingredients The ink may further contain other components in addition to those described above, if necessary. Examples of the other components include additives such as a water-dispersible resin and a neutralizing agent.
[0059] (Water dispersible resin) The water-dispersible resin can have a function of fixing the pigment, etc. to the fabric. The water-dispersible resin can be contained in the ink as resin particles.
[0060] Examples of the water-dispersible resin include urethane resin, butadiene resin, (meth)acrylic resin, and polystyrene. Examples of the butadiene resin include styrene-butadiene copolymer and acrylonitrile-butadiene copolymer. Examples of the (meth)acrylic resin include (meth)acrylic acid ester copolymer, styrene-(meth)acrylic copolymer, silicone-(meth)acrylic copolymer, and acrylic modified fluororesin. Among them, urethane resin, (meth)acrylic acid ester copolymer as the (meth)acrylic resin, and styrene-(meth)acrylic copolymer are preferable. It is presumed that these are bound to the block copolymer by intermolecular hydrogen bonds, and thus the adhesion of the pigment to the fabric is more easily improved, and the friction fastness is more easily improved.
[0061] Examples of styrene-(meth)acrylic copolymers include styrene-(meth)acrylic acid copolymers and styrene-(meth)acrylic acid-(meth)acrylic acid ester copolymers. Examples of (meth)acrylic acid esters include benzyl (meth)acrylate, cyclohexyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-ethylhexyl carbitol (meth)acrylate, phenol EO modified (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate.
[0062] The urethane resin is a polymer obtained by reacting a polyol with a polyisocyanate. Examples of the polyol include polypropylene glycol, polyethylene glycol, polytetramethylene glycol, poly(ethylene adipate), poly(diethylene adipate), poly(propylene adipate), poly(tetramethylene adipate), poly(hexamethylene adipate), poly-ε-caprolactone, poly(hexamethylene carbonate), and silicone polyol. Examples of the isocyanate include tolylene diisocyanate, 4,4-diphenylmethane diisocyanate, xylylene diisocyanate, naphthalene diisocyanate, hexamethylene diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated 4,4-diphenylmethane diisocyanate, isophorone diisocyanate, and tetramethylxylylene diisocyanate.
[0063] The Tg of the water-dispersible resin is not particularly limited, but is preferably low from the viewpoint of preventing the fabric from becoming hard even after image formation and making it easier to maintain the texture. The Tg of the water-dispersible resin may be, for example, −30 to 100° C., and preferably −10 to 50° C.
[0064] The acid value of the water-dispersible resin is not particularly limited, but from the viewpoint of improving the dispersion stability, it is preferably 44 mgKOH / g or more, more preferably 60 mgKOH / g or more. The upper limit of the acid value can be, for example, 110 mgKOH / g. The acid value can be measured by the same method as above.
[0065] The average particle size of the water-dispersible resin is not particularly limited, but from the viewpoint of preventing clogging of the nozzles of the inkjet head, it is preferably 300 nm or less, and more preferably 130 nm or less. The average particle size of the water-dispersible resin can be measured by a laser diffraction / scattering type particle size distribution measurement.
[0066] The content of the water-dispersible resin is preferably 1 to 15% by mass relative to the ink. When the content of the water-dispersible resin is 1% by mass or more, the viscosity of the ink is easily increased appropriately, and not only the ejection stability can be improved, but also the adhesion to the fabric and the abrasion resistance of the obtained image can be easily increased. When the content of the water-dispersible resin is 15% by mass or less, the viscosity of the ink does not become too high, and nozzle clogging and the like are unlikely to occur. From the same viewpoint, the content of the water-dispersible resin is more preferably 2 to 10% by mass relative to the ink.
[0067] (Additives) Examples of the additives include neutralizing agents, surfactants, preservatives, antifungal agents, pH adjusters, and the like.
[0068] In this embodiment, when the block copolymer has an anionic group such as a carboxyl group or a sulfonic acid group, the ink may further contain a neutralizing agent. The neutralizing agent may be a known basic compound, such as sodium hydroxide, potassium hydroxide, ammonia, or triethylamine. When the pigment dispersion contains a neutralizing agent, the anionic group is appropriately promoted to dissociate in the pigment dispersion, and dispersibility can be further improved.
[0069] The content of the neutralizing agent is not particularly limited, but it is set so that the neutralization rate is 30% or more and 100% or less. The neutralization rate can be calculated by the following formula (1).
[0070] Neutralization rate (%) = (mass of basic compound [g] / (equivalent of basic compound [g / mol] × (valence of basic compound)) ÷ ((acid value of pigment dispersant [mgKOH / g] × mass of pigment dispersant [g]) / (56[g / mol]×1000)) (1)
[0071] The surfactant can reduce the surface tension of the ink and increase the wettability of the ink to the fabric. The type of the surfactant is not particularly limited, and can be, for example, an acetylene glycol surfactant, a silicone surfactant, a fluorine surfactant, or the like.
[0072] Examples of preservatives or antifungal agents include aromatic halogen compounds (eg, Preventol CMK), methylene dithiocyanate, halogen-containing nitrogen-sulfur compounds, 1,2-benzisothiazolin-3-one (eg, PROXEL GXL), and the like.
[0073] Examples of pH adjusters include citric acid, sodium citrate, hydrochloric acid, sodium hydroxide, and the like.
[0074] 1-2. Pretreatment solution The pretreatment liquid contains a flocculant.
[0075] 1-2-1. Flocculant The type of aggregating agent may be any agent that can aggregate the pigments contained in the ink, etc. Aggregation may be achieved by utilizing a change in pH or by utilizing an electrical effect.
[0076] Examples of flocculants that cause flocculation by changing the pH include organic acids, such as carboxylic acids having 6 or less carbon atoms, saturated fatty acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, and hexanoic acid, and hydroxy acids such as lactic acid, malic acid, and citric acid.
[0077] Examples of the flocculant that causes flocculation by electrical action include compounds having a cationic group and polyvalent metal salts. These flocculants can interact or react with the anionic block copolymer that is the pigment dispersant contained in the ink.
[0078] Examples of the cationic group in the compound having a cationic group include a secondary amino group, a tertiary amino group, a quaternary ammonium base, etc. Examples of the compound having a cationic group include a cationic resin and a cationic surfactant, and preferably a cationic resin.
[0079] Examples of cationic resins include cationic urethane resins, cationic olefin resins, and cationic alkylamine resins. Examples of commercially available products include MPT-60 (manufactured by Mitsubishi Pencil Co., Ltd.), Unisense KHE100L (manufactured by Senka Co., Ltd.), and MZ477 (urethane resin, manufactured by Takamatsu Oil Co., Ltd.). Among them, cationic alkylamine resins MPT-60 and Unisense KHE100L (manufactured by Senka Co., Ltd.) are preferred from the viewpoint of more easily generating an interaction or reaction with the block copolymer.
[0080] Polyvalent metal salts can be water-soluble compounds having a divalent or higher polyvalent metal ion and an anion associated with it. Examples of polyvalent metal ions include Ca 2+ , Cu 2+ , Ni 2+ , Mg 2+ , Zn 2+ , B.A. 2+ Divalent metal ions such as Al 3+ , Fe 3+ , Cr 3+ Examples of anions include trivalent metal ions such as Cl. - , I - , Br - , SO4 2- , ClO3 - , NO3 - , and H.C.O.O. - , CH3COO - Examples of such polyvalent metal salts include zinc acetate dihydrate, magnesium nitrate, calcium chloride, magnesium chloride, aluminum chloride, magnesium sulfate, and metal salts of organic acids such as calcium salts, magnesium salts, nickel salts, and aluminum salts, such as acetic acid. Among these, calcium salts and magnesium salts are preferred, and calcium nitrate and calcium chloride are preferred.
[0081] Among these, compounds having a cationic group or organic acids are preferred, and compounds having a cationic group are more preferred.
[0082] The content of the flocculant in the pretreatment liquid is not particularly limited, but is preferably 0.1 to 15% by mass, and more preferably 0.5 to 8% by mass, based on the pretreatment liquid.
[0083] 1-2-2.Other ingredients If necessary, the pretreatment liquid may further contain additives such as a solvent, a pH adjuster, a preservative, etc. The solvent, pH adjuster, and preservative may be the same as those used in the ink.
[0084] 2. Image forming method The image-formed product according to one embodiment of the present invention can be produced by applying the ink by an inkjet method onto a fabric having a flocculant attached thereto. The fabric having a flocculant attached thereto can be obtained by applying a pretreatment liquid containing the flocculant to the fabric. The ink set described above can be used as the ink and the pretreatment liquid.
[0085] That is, the image forming method according to this embodiment includes a step of 1) pretreating a fabric to obtain a fabric having a flocculant attached thereto, and 2) applying ink onto the fabric by an inkjet method.
[0086] 2-1. Step of applying pretreatment liquid In this step, the fabric is pretreated to obtain a fabric having a flocculant attached thereto.
[0087] Specifically, the fabric is brought into contact with a pretreatment liquid containing a flocculant to obtain a fabric to which the flocculant is attached. The method for bringing the fabric into contact with the pretreatment liquid is not particularly limited, and may be, for example, a pad method, a coating method, a spray method, an inkjet method, or the like.
[0088] The fabric that has been contacted with the pretreatment liquid may be heated and dried using hot air, a hot plate, or a heat roller.
[0089] The amount of the pretreatment liquid to be applied is not particularly limited, and can be adjusted depending on the type of fabric, the amount of ink to be applied, and the like.
[0090] 2-2. Ink application process Next, the ink is applied by an inkjet method onto the fabric to which the coagulant has been attached.
[0091] The type of fiber contained in the fabric is not particularly limited, and examples thereof include natural fibers such as cotton (cellulose fiber), hemp, wool, and silk; chemical fibers such as rayon, vinylon, nylon, acrylic, polyurethane, polyester, and acetate, and blended fibers thereof. Of these, cotton fabric is preferred. The fabric may be any form of woven fabric, nonwoven fabric, knitted fabric, etc., made from these fibers. The fabric may also be a blended woven fabric or blended nonwoven fabric of two or more types of fibers.
[0092] In this embodiment, the ink contains the block copolymer as a pigment dispersant. The block copolymer has hydrophilic blocks at both ends of the molecule, and is therefore less likely to cause cross-linking aggregation with other pigment dispersants than conventional AB-type block copolymers that have a hydrophilic block at only one end of the molecule. This makes it easier to suppress aggregation of the pigment dispersion, and high ejection stability can be obtained.
[0093] 2-3. Other processes The image forming method may further include other steps as necessary. For example, a step of applying a post-treatment liquid (also called an overcoat liquid) onto the ink applied to the fabric may be further carried out.
[0094] The method for applying the post-treatment liquid is not particularly limited, and may be, for example, a spray method or an ink-jet method. Thereafter, the fabric to which the post-treatment liquid has been applied may be dried.
[0095] 3. Image formation The resulting image-formed product has the fabric to which the coagulant is attached and an image layer.
[0096] The flocculant is preferably disposed on the surface of the fabric. The image layer is preferably disposed on the surface of the fabric on which the flocculant is disposed. The image layer contains a pigment and the block copolymer, and may further contain the water-dispersible resin and the like as necessary.
[0097] The block copolymer can bond to the fabric at multiple bonding points, including two at both ends of the molecule, and therefore can adhere the pigment to the fabric better than conventional AB block copolymers that bond to the fabric at only one end of the molecule. As a result, the image formed has high washing fastness and friction fastness. In addition, since the block copolymer is bonded to the fabric at multiple points, the fabric is less likely to become hard than conventional AB block copolymers that bond to the fabric at only one point.
[0098] In the above embodiment, the block copolymer is used as a dispersant for dispersing the pigment, but the present invention is not limited to this and may be used as a water-dispersible resin (fixing resin). EXAMPLES
[0099] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these.
[0100] 1. Ink Preparation 1-1. Preparation of block copolymers <Preparation of Block Copolymer P-1> In a flask equipped with an argon gas inlet tube and a stirring blade, 138.8 g of n-butyl methacrylate (hereinafter referred to as "BMA"), 73.5 g of methyl methacrylate (hereinafter referred to as "MMA"), 59.6 g of methacrylic acid (hereinafter referred to as "MAA"), 23.3 g of ethyl-2-methyl-2-n-butyltellanyl-propionate (hereinafter referred to as "BTEE"), 14.3 g of dibutyl ditelluride (hereinafter referred to as "DBDT"), 2.6 g of 2,2'-azobisisobutyronitrile (hereinafter referred to as "AIBN"), 166.1 g of methyl ethyl ketone, and 166.1 g of acetonitrile were charged and reacted at 60°C for 18 hours. As a result, a prepolymer (hydrophilic block A1, Mw: 6920) was obtained.
[0101] A mixed solution of 233 g of benzyl methacrylate (hereinafter referred to as "BzMA"), 23.3 g of MAA, 2.6 g of AIBN, 98.0 g of methyl ethyl ketone, and 98.0 g of acetonitrile, which had been previously argon-substituted, was added to the above reaction solution, and the mixture was reacted at 60° C. for 9 hours. As a result, a prepolymer (Mw: 9910) containing a hydrophilic block A and a hydrophobic block B was obtained.
[0102] A mixed solution of 138.8 g of BMA, 73.5 g of MMA, 59.6 g of MAA, 1.3 g of AIBN, 61.1 g of methyl ethyl ketone, and 388.5 g of acetonitrile, which had been previously purged with argon, was added to the above reaction solution, and the mixture was reacted at 60° C. for 23 hours. As a result, a polymer (Mw: 13,800) containing hydrophilic block A1, hydrophobic block B, and hydrophilic block A2 was obtained.
[0103] After the reaction was completed, 3.6 kg of methyl ethyl ketone was added to the reaction solution, which was then poured into 21 L of heptane under stirring. The precipitated polymer was filtered by suction and dried to obtain a block copolymer P-1.
[0104] <Preparation of Block Copolymer P-2> A flask equipped with an argon gas inlet tube and a stirring blade was charged with 4.16 g of BMA, 2.20 g of MMA, 1.79 g of MAA, 0.70 g of BTEE, 0.43 g of DBDT, 0.08 g of AIBN, 6.20 g of methyl ethyl ketone, and 6.28 g of acetonitrile, and reacted at 60° C. for 13 hours. As a result, a prepolymer (hydrophilic block A1, Mw: 5790) was obtained.
[0105] A mixed solution of 7.00 g of cyclohexyl methacrylate (hereinafter referred to as "CHMA"), 0.70 g of MAA, 0.8 g of AIBN, 2.94 g of methyl ethyl ketone, and 2.94 g of acetonitrile, which had been previously argon-substituted, was added to the above reaction solution, and the mixture was reacted at 60° C. for 10 hours. As a result, a prepolymer (Mw: 9180) containing a hydrophilic block A1 and a hydrophobic block B was obtained.
[0106] A mixed solution of 4.16 g of BMA, 2.20 g of MMA, 1.79 g of MAA, 0.08 g of AIBN, 1.84 g of methyl ethyl ketone, and 11.66 g of acetonitrile, which had been previously purged with argon, was added to the above reaction solution, and the mixture was reacted at 60° C. for 24 hours. As a result, a polymer (Mw: 13,300) containing hydrophilic block A1, hydrophobic block B, and hydrophilic block A2 was obtained.
[0107] After the reaction was completed, 108 g of methyl ethyl ketone was added to the reaction solution, which was then poured into 0.63 L of heptane under stirring. The precipitated polymer was filtered by suction and dried to obtain a block copolymer P-2.
[0108] <Preparation of Block Copolymer P-3> Block copolymer P-3 was prepared in the same manner as block copolymer P-1, except that the monomer composition of hydrophilic block A2 was changed as shown in Table 1.
[0109] <Preparation of Block Copolymer P-4> With reference to Synthesis Example 1 of JP-A-2009-299842, the following BAA-type block copolymer P-4 was prepared. [ka]
[0110] <Preparation of Block Copolymer P-5> A block copolymer P-5 was prepared with reference to the description of Dispersion 1 in JP-A-2010-513672.
[0111] <Preparation of Block Copolymer P-6> Into a flask equipped with an argon gas inlet tube and a stirring blade were placed 1165.0 g of BzMA, 116.5 g of MAA, 116.5 g of BTEE, 43.0 g of DBDT, 6.4 g of AIBN, and 1282.0 g of methyl ethyl ketone, and the mixture was reacted at 60° C. for 24 hours.
[0112] To the above reaction solution, a mixed solution of 1388.0 g of BMA, 734.0 g of MMA, 596.0 g of MAA, 12.8 g of AIBN, 538.0 g of methyl ethyl ketone, 1677.0 g of acetonitrile, and 503.0 g of methanol, which had been previously purged with argon, was added, and the reaction was carried out at 60° C. for 28 hours.
[0113] After the reaction was completed, 18.7 kg of methyl ethyl ketone was added to the reaction solution, which was then poured into 107 L of heptane under stirring. The precipitated polymer was filtered by suction and dried to obtain a block copolymer.
[0114] <Preparation of random copolymer P-7> A random copolymer P-7 having the monomer composition shown in Table 1 was prepared by known radical polymerization.
[0115] Table 1 shows the compositions of the block copolymers P-1 to P-6 and the random copolymer P-7. [Table 1] BMA: Butyl methacrylate MMA: Methyl methacrylate MAA: Methacrylic acid BzMA: benzyl methacrylate
[0116] In Table 1, the acid value is a value measured according to the measurement method of JIS K0070: 1992. The molecular weight is a weight average molecular weight Mw, and is a value obtained by the GPC method in terms of polystyrene.
[0117] 1-2. Preparation of pigment dispersion <Preparation of Pigment Dispersions A-1 to A-7> 20.0 parts by mass of carbon black pigment was mixed with a block copolymer shown in Table 2 as a pigment dispersant, in which the amount added relative to the pigment was 30% by mass, 20 parts by mass of propylene glycol (PG), and 5 parts by mass of 1,2-hexanediol (1,2-HD), along with ion-exchanged water to obtain an aqueous pigment dispersion with a pigment concentration of 20.0%.
[0118] Dispersion treatment was performed using a horizontal media disperser (Labostar Mini LMZ015, zirconia bead diameter 0.3 mm, manufactured by Ashizawa Finetech Co., Ltd.) to prepare pigment dispersions A-1 to A-7 with a pigment concentration of 20.0%. The volume-based average particle size of the pigment particles was measured using a particle size distribution measuring device (Zeta Nanosizer 1000HS, manufactured by Malvern Instruments).
[0119] Table 2 shows the pigment dispersants used in the pigment dispersions A-1 to A-7. [Table 2]
[0120] 1-3. Preparation of ink <Preparation of Ink B-1> The following components were mixed to obtain ink B-1. Pigment dispersion A-1: 30 parts by weight Water-dispersible resin WBR-2000U (Acrylate, polyurethane resin particles, Tg: 45°C, manufactured by Taisei Fine Chemical Co., Ltd.): 10 parts by mass as solid content Glycerin: 10 parts by weight Propylene glycol: 20 parts by weight Proxel GXL(S) (preservative): 0.05 parts by weight Olfin E1010 (manufactured by Nissin Chemical Industry Co., Ltd., surfactant): 0.1 parts by mass Ion exchange water: remaining amount The amount of ion-exchanged water was adjusted so that the total amount of ink was 100 parts by mass.
[0121] <Preparation of Inks B-2 to B-10> Except for changing the types of pigment dispersion and water-dispersible resin as shown in Table 3, inks B-2 to B-10 were prepared in the same manner as ink B-1.
[0122] Table 3 shows the types of pigment dispersions and water-dispersible resins used in inks B-1 to B-10. [Table 3] WBR-2000U (Taisei Fine Chemical Co., Ltd. Acrylate, polyurethane resin particles, Tg: 45℃) J7600 (Joncryl 7600 manufactured by BASF Japan, (meth)acrylic resin particles, Tg: 35°C) J390 (BASF Japan Joncryl 390, styrene-acrylic acid copolymer, Tg: -5°C, acid value: 54mgKOH / g, average particle size: 0.09μm) The above block copolymer P-1
[0123] 2. Preparation of Pretreatment Solution 2-1. Preparation of pretreatment solution <Preparation of pretreatment solution PC-1> The following components were mixed to prepare pretreatment solution PC-1. Flocculant 1 (Unisense KHE100L): 4 parts by weight Glycerin: 10 parts by weight Propylene glycol: 20 parts by weight Proxel GXL(S) (preservative): 0.05 parts by weight Olfin E1010 (manufactured by Nissin Chemical Industry Co., Ltd., surfactant): 0.1 parts by mass Ion-exchanged water: 44.85 parts by weight
[0124] <Preparation of pretreatment solutions PC-2 to PC-3> Pretreatment solutions PC-2 to PC-3 were prepared in the same manner except that the type and content of the flocculant were changed as shown in Table 4 and the amount of ion-exchanged water was adjusted so that the total amount was 100 parts by mass.
[0125] Table 4 shows the compositions of pretreatment solutions PC-1 to PC-3. [Table 4] Unisense KHE100L: Poly(diallyldimethylammonium chloride)
[0126] 3. Image formation and evaluation 3-1.Image formation <Test 1> (1) Pretreatment A 100% cotton fabric (white) was prepared. Next, a pretreatment liquid of the type shown in Table 5 was applied to the surface of the fabric at a concentration of 10 g / m 2 After applying the ink by the inkjet method so as to obtain an application amount of 100° C., the ink was dried at 100° C. for 2 minutes.
[0127] (2) Applying ink Next, an inkjet printer having an inkjet head (Konica Minolta head KM1024iMAE) was prepared as an image forming apparatus. The inks shown in Table 5 were then sprayed from the nozzles of the inkjet head at a rate of 15 g / m 2 A solid image was formed on the pretreated fabric (ink application step).
[0128] Specifically, a solid image (total 200 mm x 200 mm) was formed at 540 dpi in the main scan direction and 720 dpi in the sub scan direction. dpi represents the number of ink droplets (dots) per 2.54 cm. The ejection frequency was 22.4 kHz.
[0129] (3) Drying and Fixation The ink-applied fabric was then dried in a belt-type dryer at 150°C for 3 minutes. As a result, an image-formed product was obtained.
[0130] <Tests 2-24> Image formation was carried out in the same manner as in Test 1, except that at least one of the type of pretreatment liquid and the type of ink was changed as shown in Table 5.
[0131] 3-2.Evaluation The resulting image-formed product was subjected to the following evaluations.
[0132] (Washing fastness) The washing fastness of the image-formed product was evaluated by comparing the color fading of a sample washed once in a household washing machine (washed with water) with a sample that had not been washed. The following evaluation criteria were used: It was evaluated based on. ◎: Almost no color fading after rinsing, no practical problems ○: Color fading after rinsing is slight and of a level that is completely problem-free for practical use. △: Color fades after rinsing, but is not a problem for practical use. ×: Discoloration after rinsing is significant and at a level that is problematic for practical use. If it was △ or higher, it was considered to be within the acceptable range.
[0133] (Friction resistance) A Gakushin type rub fastness tester (product name: AB-301, manufactured by Tester Sangyo Co., Ltd.) was used to impregnate a white cloth for JIS dye fastness testing (JIS L 0803:2011 compliant No. 3-1) with pure water under conditions of a load of 200.0 g and a speed of 10.0 cm / s, and the cloth was run back and forth 10.0 times over the ink-applied surface of the image-formed product. Thereafter, the dye transfer density onto a test white cloth was evaluated based on the following evaluation criteria. ◯: The dye transfer density is slight or almost nonexistent, and is at a level that is completely problem-free for practical use. △: There is some dye migration, but it is at a level that does not cause any problems in practical use. ×: The dye transfer density is significant and at a level that is problematic for practical use. If it was △ or higher, it was considered to be within the acceptable range.
[0134] (Discharge stability) The ejection stability and the presence or absence of nozzle clogging of the inks B-1 to B-10 used in image formation were evaluated by the following methods.
[0135] (1) Injection stability After continuous ejection for 10 minutes under image forming conditions, the ink was checked for missing or bent ink using an ejection inspection machine. The ejection stability was evaluated according to the following criteria. 5: No problems even with long periods of continuous use 4: No injection failures 3: Slight bending occurs, but no problems. 2: Missing ink occurs during printing 1: Injection failure occurs immediately or injection cannot be performed normally A score of 3 or higher was considered to be good.
[0136] (2) Nozzle clogging Maintenance of the nozzle surface was performed during image formation using a print test machine, and the state of nozzle missing after the maintenance was confirmed using a nozzle check chart. Nozzle clogging was then evaluated according to the following criteria. 5: No clogging even with long periods of continuous use 4: No clogging occurs 3: Even if clogging occurs, it can be fixed with maintenance 2: Many blockages occur that cannot be fixed through maintenance 1: Unable to eject normally A score of 3 or higher was considered good.
[0137] Table 5 shows the evaluation results of the image formations of Tests 1 to 24, and Table 6 shows the evaluation results of the ink ejection stability.
[0138] [Table 5]
[0139] [Table 6]
[0140] Image formation evaluation As shown in Table 5, the image-formed products obtained in Tests 7 to 10, 14 to 17, and 21 to 24 (comparison) were poor in both washing fastness and rubbing fastness, whereas the image-formed products obtained in Tests 1 to 6, 11 to 13, and 18 to 20 (present invention) were good in both washing fastness and rubbing fastness.
[0141] From these results, it is considered that ABA and ABC block copolymers, which have hydrophilic blocks at two locations in the polymer, have a higher and stronger bond with the fabric than AB block copolymers, which have a hydrophobic block at one end, because they have multiple sites that react with the flocculant. This is thought to improve adhesion to the fabric and improve wash fastness and friction fastness.
[0142] In particular, a comparison of Tests 1, 11, and 18 reveals that when a urethane resin is used as the water-dispersible resin, by combining it with a pretreatment liquid containing a cationic resin as a flocculant, the washing fastness is improved and the bonding strength with the fabric is further improved.
[0143] Regarding ejection performance evaluation Furthermore, as shown in Table 6, inks B-7 to B-10 used in tests 7 to 10, 14 to 17, and 21 to 24 (comparison) have poor ejection stability and nozzle clogging, whereas inks B-1 to B-6 used in tests 1 to 6, 11 to 13, and 18 to 20 (invention) have good ejection stability and nozzle clogging.
[0144] For these reasons, it is believed that ABA and ABC block copolymers, which have hydrophilic blocks at two locations in the polymer, are less likely to undergo cross-linking aggregation with other dispersants than AB block copolymers, which have a hydrophilic block at one end, making it easier to suppress the formation of aggregates in the pigment dispersion and improving the ejection stability. [Industrial Applicability]
[0145] According to the present invention, it is possible to provide an ink set for ink-jet textile printing that has good ejection stability and is capable of forming images that have high fastness to washing and abrasion.
Claims
1. An inkjet printing ink set comprising an ink and a pretreatment liquid, The pretreatment liquid contains a flocculant, The ink contains a pigment, a block copolymer, and a water-based solvent, The block copolymer includes two hydrophilic blocks A arranged at both ends of the molecule and interacting or reacting with the flocculant, and a hydrophobic block B arranged between the two hydrophilic blocks. Ink set for inkjet textile printing.
2. The block copolymer is an ABA type block copolymer consisting of the two hydrophilic blocks A and one hydrophobic block B. The ink set for ink-jet textile printing according to claim 1 .
3. The two hydrophilic blocks A have the same monomer composition. The ink set for ink-jet textile printing according to claim 1 or 2.
4. the hydrophilic block A includes a structural unit derived from a hydrophilic monomer that is a vinyl monomer containing a hydrophilic functional group selected from the group consisting of a hydroxyl group, a carboxyl group, and a sulfonic acid group, the content ratio of the structural unit derived from the hydrophilic monomer in the hydrophilic block A is higher than that in the hydrophobic block B; The ink set for ink-jet textile printing according to claim 1 .
5. the hydrophobic block B comprises a structural unit derived from a hydrophobic monomer selected from the group consisting of vinyl monomers containing an aromatic ring group or an alicyclic hydrocarbon group, the content ratio of the structural unit derived from the hydrophilic monomer in the hydrophobic block B is lower than that in the hydrophilic block A; The ink set for ink-jet textile printing according to claim 4.
6. The flocculant includes a polyvalent metal salt, an organic acid, or a compound having a cationic group. The ink set for ink-jet textile printing according to claim 1 .
7. The method includes a step of applying ink by an inkjet method onto the fabric to which the flocculant is attached, The ink contains a pigment, a block copolymer, and a water-based solvent, The block copolymer includes two hydrophilic blocks A arranged at both ends of the molecule and interacting or reacting with the flocculant, and a hydrophobic block B arranged between the two hydrophilic blocks. Image forming method.
8. A fabric having a flocculant attached thereto; an image layer disposed on the fabric; having the image layer comprises a pigment and a block copolymer that interacts or reacts with the flocculant; The block copolymer includes two hydrophilic blocks A arranged at both ends of the molecule and interacting or reacting with the flocculant, and a hydrophobic block B arranged between the two hydrophilic blocks. Image formation.
Citation Information
Patent Citations
Water-base pigment ink for ink jet printer
JP1992227668A
Textile printing method
JP2018009260A
Pigment dispersant and method for producing the same, pigment dispersion for inkjet ink and aqueous inkjet ink
JP2022073013A
Ink fluid set for printing on textiles
JP2022548985A
Method of producing printed article
JP2023005600A