Filler for separator hole, method for manufacturing concrete structure, concrete structure, coating material for separator, and separator
The ion-releasing compound and resin-based materials for concrete structures address the issue of long-term waterproofness and rust prevention by forming densifying salts, effectively preventing water leakage and maintaining structural integrity.
Patent Information
- Application Number
- JP2023070839
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-06
AI Technical Summary
Conventional protective equipment for concrete structures with separator holes fails to maintain long-term waterproofness and rust prevention due to interfacial delamination and external stress, leading to cracks and water infiltration.
A filling material and coating material for separator holes and separators in concrete structures, comprising an ion-releasing compound and resin, which generates poorly water-soluble salts to densify and protect the area, preventing water leakage and rust.
The materials improve waterproofness and rust prevention, maintaining concrete structures in a stable state for a long period by forming a layer of poorly water-soluble salts that block water intrusion routes and enhance structural durability.
Smart Images

Figure 2024156406000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a separator hole filler that can be used in separator holes in concrete structures. The present invention also relates to a method for manufacturing a concrete structure using the separator hole filler, and a concrete structure using the separator hole filler. The present invention also relates to a separator coating material that can be used for separators. The present invention also relates to a separator and a concrete structure using the separator coating material. [Background technology]
[0002] When pouring concrete at a construction site, a method is known in which separators (e.g., B-type separators and BC-type separators) and separator cones are used to maintain the distance between concrete forms. In such a method, after the poured concrete has sufficiently hardened, the concrete forms and separator cones are removed, and holes (separator holes) are formed on the concrete wall where the separator cones were removed. Even after the concrete forms and separator cones are removed, the separators remain inside the concrete without being removed, and the ends of the separators are exposed from the separator holes.
[0003] If the separator holes and separator ends are left untreated, rainwater and moisture adhering to the concrete may seep into the concrete through the separator, gradually reducing the strength of the concrete structure. Also, if the separator is made of metal, the exposed separator ends may rust and expand, causing cracks in the concrete structure. As a result, moisture may seep into the concrete through the cracks, accelerating the change in the condition of the concrete structure.
[0004] Specialized protective equipment is sometimes used to improve the waterproofing of concrete structures.
[0005] The following Patent Document 1 discloses a concrete form separator protector that is composed of a large diameter part having an anti-rust effect and a small diameter part that has a smaller diameter than the large diameter part, extends from one end of the large diameter part with a step, and has an anti-rust effect. Patent Document 1 describes that in the concrete form separator protector, the female thread part of the large diameter part is screwed into the male thread part of the concrete form separator to cover the end part of the concrete form separator and prevent rust from occurring. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2011-127329 A Summary of the Invention [Problem to be solved by the invention]
[0007] When the separator hole or the end of the separator is protected using a protective device such as that described in Patent Document 1, the separator hole and the end of the separator can be protected and water leakage can be prevented (waterproofness can be improved) for a certain period of time after the protective device is installed.
[0008] However, in conventional protective equipment, after a long period of time (for example, after 20 to 50 years have passed since installation), interfacial peeling may occur at the interface between the protective equipment and the concrete structure due to deterioration of the protective equipment, etc. In addition, interfacial peeling may also occur at the interface between the protective equipment and the concrete structure due to external stress such as an earthquake. For this reason, in conventional protective equipment, if new cracks or fine gaps occur in the separator hole or the separator end and the surrounding concrete structure due to external stress or changes in environmental conditions after installation, rust may occur at the separator end, water leakage may occur, and repairs may be required.
[0009] Conventionally, there is no known method for protecting or strengthening the separator holes and separators of a concrete structure and their surroundings in a self-healing manner for a long period of time.
[0010] The object of the present invention is to provide a separator hole filler that can improve the waterproofing of the separator hole and its surroundings and maintain the concrete structure in a stable state for a long period of time. Another object of the present invention is to provide a method for manufacturing a concrete structure using the separator hole filler and a concrete structure using the separator hole filler.
[0011] Another object of the present invention is to provide a coating material for a separator that can improve the rust prevention of the separator, improve the waterproofing of the separator and its surroundings, and maintain the concrete structure in a stable state for a long period of time. Another object of the present invention is to provide a separator and a concrete structure using the above-mentioned coating material for a separator. [Means for solving the problem]
[0012] This specification discloses the following separator hole filler, method for manufacturing a concrete structure, concrete structure, separator coating material, and separator.
[0013] Item 1. A filler for a separator hole in a concrete structure, comprising an ion-releasing compound capable of releasing cations or anions, and a resin, cement milk, or mortar, wherein the ion-releasing compound is capable of generating a poorly water-soluble salt.
[0014] Item 2. The separator hole filler according to Item 1, wherein the poorly water-soluble salt is calcium carbonate, barium carbonate, calcium phosphate, or iron hydroxide.
[0015] Item 3. The separator hole filler according to item 1 or 2, wherein the ion-releasing compound includes a compound capable of releasing cations, and the compound capable of releasing cations is calcium silicate, tricalcium silicate, dicalcium silicate, calcium aluminate, calcium aluminoferrite, calcium hydroxide, calcium oxide, calcium acetate, calcium lactate, barium lactate, calcium sulfate, calcium chloride, calcium nitrate, or calcium hydrogen carbonate.
[0016] Item 4. The ion-releasing compound includes a compound capable of releasing anions, and the compound capable of releasing anions is sodium hydrogen phosphate, potassium carbonate, potassium hydrogen carbonate, ammonium carbonate, ammonium hydrogen carbonate, sodium carbonate, sodium hydrogen carbonate, or calcium hydrogen carbonate. The separator hole filler according to any one of Items 1 to 3.
[0017] Item 5. The separator hole filler according to any one of Items 1 to 4, wherein the resin comprises an epoxy resin or a modified silicone resin.
[0018] Item 6. The separator hole filler according to any one of Items 1 to 5, having a viscosity of 2000 mPa·s or more and 50000 mPa·s or less at 23° C. and 20 rpm.
[0019] Item 7. The separator hole filler according to any one of items 1 to 6, wherein the ratio of the viscosity at 23° C. and 2 rpm to the viscosity at 23° C. and 20 rpm is 3.0 or more and 8.0 or less.
[0020] Item 8. A method for producing a concrete structure, comprising the steps of obtaining a concrete structure body having a separator hole using a separator and a separator cone, and filling the separator hole of the concrete structure body with the separator hole filler according to any one of items 1 to 7.
[0021] Item 9. A concrete structure comprising a concrete structure body having a separator hole and a filler filled in the separator hole of the concrete structure body, wherein the filler is formed by the separator hole filler according to any one of items 1 to 7. A concrete structure.
[0022] Item 10. A coating material for a separator in a concrete structure, comprising an ion-releasing compound capable of releasing cations or anions, and a resin, cement milk, or mortar, wherein the ion-releasing compound is capable of generating a poorly water-soluble salt. A coating material for a separator.
[0023] Item 11. The separator coating material according to Item 10, wherein the resin comprises an epoxy resin, a vinyl ester resin, an unsaturated polyester resin, or a polyolefin resin.
[0024] Item 12. A separator comprising a separator body and a coating material disposed on a surface of the separator body, the coating material being formed from the separator coating material according to item 10 or 11.
[0025] Item 13. A concrete structure comprising a concrete structure body and a separator disposed inside the concrete structure body, the separator comprising a separator body and a coating material disposed on a surface of the separator body, the coating material being formed by the separator coating material according to any one of items 10 to 12. Effect of the Invention
[0026] The separator hole filler according to the present invention is a filler used in separator holes in concrete structures, and contains an ion-releasing compound capable of releasing cations or anions, and a resin, cement milk, or mortar, and the ion-releasing compound is capable of generating poorly water-soluble salts. The separator hole filler according to the present invention has the above-mentioned configuration, and therefore can increase the waterproofing of the separator hole and its surroundings, and can maintain the concrete structure in a stable state for a long period of time.
[0027] The separator coating material according to the present invention is a coating material used for separators in concrete structures, and includes an ion-releasing compound capable of releasing cations or anions, and a resin, cement milk, or mortar, and the ion-releasing compound is capable of generating a poorly water-soluble salt. Since the separator coating material according to the present invention has the above-mentioned configuration, it is possible to improve the rust prevention of the separator, improve the waterproofing of the separator and its surroundings, and maintain the concrete structure in a stable state for a long period of time. [Brief description of the drawings]
[0028] [Figure 1] FIG. 1 is a cross-sectional view of a concrete structure using a separator hole filler according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of a concrete structure using a separator coating material according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] The present invention will be described in detail below.
[0030] (Separator hole filler) The separator hole filler according to the present invention is used in separator holes in concrete structures. The separator hole filler according to the present invention is used by filling separator holes in concrete structures. The separator hole filler according to the present invention includes an ion-releasing compound capable of releasing cations or anions (hereinafter, sometimes referred to as "ion-releasing compound"), and a resin, cement milk, or mortar. In the separator hole filler according to the present invention, the ion-releasing compound is capable of generating poorly water-soluble salts. The separator hole filler according to the present invention is a separator hole filler for generating poorly water-soluble salts.
[0031] Since the separator hole filler according to the present invention has the above-mentioned configuration, it is possible to improve the waterproofing of the separator hole and its surroundings and to maintain the concrete structure in a stable state for a long time. More specifically, when the separator hole filler is placed in the filling target portion (separator hole), the ion-releasing compound in the separator hole filler releases ions, generating a poorly water-soluble salt. This makes the filled portion (separator hole) and its surroundings dense, effectively preventing water leakage (improving waterproofing), and maintaining the concrete structure in a stable state for a long time (improving durability). In addition, when the end of the separator is exposed from the separator hole, the separator hole filler according to the present invention densifies the end of the separator and its surroundings, improving the rust prevention of the end of the separator, and as a result, it is possible to effectively prevent water leakage (improving waterproofing), and maintain the concrete structure in a stable state for a long time (improving durability). The present invention contributes to preventive maintenance of concrete structures. The present invention particularly contributes to preventive maintenance of newly constructed concrete structures.
[0032] In the separator hole filler according to the present invention, when the separator hole filler comes into contact with moisture or the like attached to the concrete structure at the filled portion (separator hole), the ion-releasing compound in the separator hole filler releases ions, thereby generating a poorly water-soluble salt at the contact surface between the moisture or the like and the separator hole filler. That is, the separator hole filler according to the present invention can generate a layer of poorly water-soluble salt on the surface of the separator hole filler. When a water intrusion path occurs near the interface of the separator hole filler due to cracks or the like, the poorly water-soluble salt generated blocks the water intrusion path, and the strength of the filled portion (separator hole) and its surroundings is further increased. The poorly water-soluble salt is usually generated over several months to several years. In addition, the generated poorly water-soluble salt effectively suppresses further contact between the separator hole filler and moisture, and can effectively suppress deterioration of the concrete structure. The separator hole filler according to the present invention can preserve concrete structures for various applications.
[0033] The concrete structure is not particularly limited. Examples of the concrete structure include buildings, underground tunnels, undersea tunnels, and mountain tunnels. The concrete structure may be an underground structure.
[0034] The shape of the separator hole to be filled with the separator hole filler is not particularly limited. The shape of the separator hole (the shape of the separator cone) can be appropriately selected depending on the application of the concrete structure. The shape of the separator hole (the shape of the separator cone) may be a truncated cone, a cylindrical shape, a square prism, or a hemisphere. In the separator hole, the end of the separator may or may not be exposed.
[0035] The size of the separator holes (the size of the separator cone) into which the separator hole filler is filled is not particularly limited.
[0036] The viscosity of the separator hole filler at 23°C and 20 rpm is preferably 2000 mPa·s or more, more preferably 3000 mPa·s or more, even more preferably 5000 mPa·s or more, and preferably 50000 mPa·s or less, more preferably 45000 mPa·s or less, and even more preferably 40000 mPa·s or less. When the viscosity at 23°C and 20 rpm is equal to or more than the lower limit and equal to or less than the upper limit, the separator hole filler can be easily filled (injected) into the separator hole, and workability can be improved. The viscosity at 23°C and 20 rpm can be appropriately adjusted depending on the type and amount of the blended components.
[0037] The viscosity at 23° C. and 20 rpm can be measured, for example, using a Brookfield viscometer ("VISCOSTAR" manufactured by FUNGILAB) under conditions of 23° C. and 20 rpm.
[0038] The viscosity of the separator hole filler at 23°C and 2 rpm is preferably 6000 mPa·s or more, more preferably 8000 mPa·s or more, even more preferably 10000 mPa·s or more, and preferably 400000 mPa·s or less, more preferably 350000 mPa·s or less, and even more preferably 300000 mPa·s or less. When the viscosity at 23°C and 2 rpm is equal to or more than the lower limit and equal to or less than the upper limit, the application can be performed satisfactorily. The viscosity at 23°C and 2 rpm can be appropriately adjusted by the type and amount of the blended components.
[0039] The viscosity at 23° C. and 2 rpm can be measured, for example, using a Brookfield viscometer ("VISCOSTAR" manufactured by FUNGILAB) under conditions of 23° C. and 2 rpm.
[0040] In the above separator hole filler, the ratio of the viscosity at 23°C and 2 rpm to the viscosity at 23°C and 20 rpm (viscosity at 23°C and 2 rpm / viscosity at 23°C and 20 rpm) is preferably 3.0 or more, more preferably 3.5 or more, and even more preferably 4.0 or more. In the above separator hole filler, the ratio (viscosity at 23°C and 2 rpm / viscosity at 23°C and 20 rpm) is preferably 8.0 or less, more preferably 7.5 or less, and even more preferably 7.0 or less. When the ratio (viscosity at 23°C and 2 rpm / viscosity at 23°C and 20 rpm) is equal to or greater than the lower limit and equal to or less than the upper limit, the separator hole filler can be easily filled (injected) into the separator hole, and workability can be improved.
[0041] (Separator coating material) The separator coating material according to the present invention is used for separators in concrete structures. The separator coating material according to the present invention includes an ion-releasing compound capable of releasing cations or anions (hereinafter, may be referred to as "ion-releasing compound"), and a resin, cement milk, or mortar. In the separator coating material according to the present invention, the ion-releasing compound is capable of generating a poorly water-soluble salt. The separator coating material according to the present invention is a separator coating material for generating a poorly water-soluble salt.
[0042] The separator coating material according to the present invention has the above-mentioned configuration, and therefore can improve the rust prevention of the separator, improve the waterproofing of the separator and its surroundings, and maintain the concrete structure in a stable state for a long time. More specifically, when the separator coating material is placed on the surface of the separator, the ion-releasing compound in the separator coating material releases ions, generating poorly water-soluble salts and forming concretions. This makes the coated area (surface of the separator) and its surroundings dense, improving the rust prevention of the separator, effectively preventing water leakage from the separator and its surroundings (improving waterproofing), and maintaining the concrete structure in a stable state for a long time (improving durability). The present invention contributes to preventive maintenance of concrete structures. In particular, the present invention contributes to preventive maintenance of newly constructed concrete structures.
[0043] When the separator coating material according to the present invention comes into contact with moisture or the like attached to a concrete structure at the coated portion (surface of the separator), the ion-releasing compound in the separator coating material releases ions, thereby generating a poorly water-soluble salt at the contact surface between the moisture or the like and the separator coating material. That is, the separator coating material according to the present invention can generate a layer of poorly water-soluble salt on the surface of the separator by the separator coating material. The generated poorly water-soluble salt further increases the strength of the coated portion (surface of the separator) and its surroundings. The poorly water-soluble salt is usually thought to be generated over several months to several years. In addition, the generated poorly water-soluble salt effectively prevents further contact between the separator coating material and moisture, and effectively prevents deterioration of the separator coating material and deterioration of the concrete structure. When the resin in the separator coating material contains a curable resin, the poorly water-soluble salt produced can effectively suppress deterioration of the separator coating material after the curing reaction of the curable resin, and can effectively suppress deterioration of the cured product of the separator coating material. When the resin in the separator coating material contains a thermoplastic resin, the poorly water-soluble salt produced can effectively suppress deterioration of the separator coating material after molding, and can effectively suppress deterioration of the molded product of the separator coating material.
[0044] The separator coating material can be used whether the separator is in a dry state or a wet state. The separator coating material can also be used when water is flowing out from the end of the separator. Therefore, the separator coating material according to the present invention can preserve concrete structures for various applications.
[0045] The concrete structure is not particularly limited. Examples of the concrete structure include buildings, underground tunnels, undersea tunnels, and mountain tunnels. The concrete structure may be an underground structure.
[0046] The separator coating material is used to coat the separator. The separator coating material may be used on the outer periphery of the separator, or on the end portion. The separator coating material may be used on only a part of the surface of the separator, or on the entire surface of the separator. From the viewpoint of more effectively exerting the effects of the present invention, the separator coating material is preferably used on the outer periphery of the separator, and more preferably used on the entire surface of the separator. From the viewpoint of more effectively exerting the effects of the present invention, the separator coating material is more preferably used to coat the entire surface of the separator.
[0047] The above-mentioned separator coating material may be used on a separator (such as an end of a separator) exposed from a concrete structure having a separator hole, or on a separator (such as an end of a separator) exposed from a concrete structure not having a separator hole.
[0048] The separator coating material may be applied by coating or spraying.
[0049] The separator coating material may be applied before pouring concrete, or after pouring concrete. The separator coating material may be applied to the outer periphery of the separator before pouring concrete, or to the end of the separator before pouring concrete, or to the entire surface of the separator before pouring concrete. The separator coating material may be applied to the end of the separator after pouring concrete. The separator coating material may be applied to the exposed end of the separator after pouring concrete.
[0050] The material of the separator using the separator coating material is not particularly limited. The separator may be made of metal.
[0051] The shape of the end of the separator is not particularly limited, and may be a cylindrical shape, a polygonal prism shape, or a male screw shape.
[0052] The coating thickness of the separator coating material and the thickness of the coating material disposed on the surface of the separator are preferably 10 μm or more, more preferably 50 μm or more, and even more preferably 100 μm or more, and preferably 10000 μm or less, more preferably 5000 μm or less, and even more preferably 3000 μm or less. When the coating thickness of the separator coating material and the thickness of the coating material disposed on the surface of the separator are not less than the above lower limit, the effects of the present invention can be more effectively exhibited. When the coating thickness of the separator coating material and the thickness of the coating material disposed on the surface of the separator are not more than the above upper limit, the coating can be applied satisfactorily.
[0053] (Other details of separator hole filler and separator coating material) In the separator hole filling material and the separator coating material, the solubility of the poorly water-soluble salt in water at 20° C. is preferably 1.0×10 -3 mol / L or less, more preferably 8.0×10 -4 mol / L or less, more preferably 5.0×10 -4 mol / L or less, particularly preferably 2.0×10 -4 mol / L or less. When the solubility of the poorly water-soluble salt in water at 20°C is equal to or less than the upper limit, the effects of the present invention can be more effectively exhibited. There is no particular limitation on the lower limit of the solubility of the poorly water-soluble salt in water at 20°C. The solubility of the poorly water-soluble salt in water at 20°C is 1.0 x 10 -10 mol / L or more, and may be 1.0×10 -9 It may be mol / L or more.
[0054] The solubility of the above poorly water-soluble salt in water at 20°C can be measured by the following method. 10 g of the poorly water-soluble salt is added to 100 g of pure water, and the mixture is stirred at 20°C for 10 minutes. Then, 10 g of the solution is placed in an evaporating dish, and the water is completely removed at 100°C. The solubility of the above poorly water-soluble salt in water at 20°C is calculated from the weight of the poorly water-soluble salt remaining on the evaporating dish.
[0055] Hereinafter, details of each component used in the separator hole filling material and separator coating material according to the present invention will be described.
[0056] The separator hole filling material and the separator coating material include an ion releasing compound and a resin, cement milk, or mortar.
[0057] The separator hole filler may contain a resin, may contain cement milk, or may contain mortar. The separator hole filler preferably contains a resin, preferably contains cement milk, and preferably contains mortar.
[0058] The separator coating material may contain a resin, may contain cement milk, or may contain mortar. The separator coating material preferably contains a resin.
[0059] <Resin> The resin may be a thermoplastic resin, a curable resin, etc. The resin may be used alone or in combination of two or more kinds.
[0060] Examples of the thermoplastic resin include fluororesin, polyolefin resin, polyvinyl chloride resin, polyamide resin, polycarbonate resin, polystyrene resin, polyester resin, acrylonitrile-butadiene-styrene resin (ABS resin), polyethylene terephthalate (PET), and polymethyl methacrylate (PMMA).
[0061] Examples of the polyolefin resin include polyethylene, polypropylene, ethylene-propylene copolymer (EPDM), isobutylene-isoprene copolymer, polystyrene, polybutene, polyisobutylene, polybutadiene, acrylonitrile-butadiene copolymer, ethylene-vinyl acetate copolymer, and ethylene-α-olefin copolymer.
[0062] Examples of the curable resin include modified silicone resin, silicone resin, epoxy resin, acrylic resin, unsaturated polyester resin, polyurea resin, urethane resin, phenol resin, vinyl ester resin, naphthoxazine resin, etc. The curable resin may be used alone or in combination of two or more kinds.
[0063] The curable resin may be a one-component curable resin or a two-component curable resin. Examples of the one-component curable resin include a thermosetting resin, a photocurable resin, and a moisture curable resin. The two-component curable resin is used in combination with a curing agent. From the viewpoint of improving workability on site, the curable resin preferably contains a moisture curable resin, and is preferably a moisture curable resin. The curable resin may be used in combination with a curing agent, or may not be used in combination with a curing agent.
[0064] From the viewpoint of increasing elasticity, the curable resin preferably contains a modified silicone resin, and is preferably a modified silicone resin.
[0065] From the viewpoint of improving workability on site, the modified silicone resin is preferably a moisture-curable modified silicone resin. The moisture-curable modified silicone resin has a hydrolyzable silicon group. The modified silicone resin having the hydrolyzable silicon group has a polyether polymer, a polyolefin polymer, or an acrylic polymer as a main chain (a portion excluding the hydrolyzable silicon group). Therefore, examples of monomers that are materials for the main chain include alkylene oxide monomers, olefin monomers, and acrylic monomers. The polymer may be a homopolymer or a copolymer. When the polymer is a copolymer, examples of monomers used include alkylene oxide monomers, olefin monomer components, acrylic monomers, and vinyl monomers. Only one type of modified silicone resin may be used, or two or more types may be used in combination.
[0066] Examples of the alkylene oxide monomer include ethylene oxide, propylene oxide, butylene oxide, etc. From the viewpoint of improving the elongation and viscous handleability after curing, the alkylene oxide monomer is preferably polypropylene oxide obtained by polymerizing propylene oxide.
[0067] The olefin monomer includes isobutylene and the like.
[0068] Examples of the acrylic monomer include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isomyristyl (meth)acrylate, stearyl (meth)acrylate, and isobornyl (meth)acrylate. acrylate, benzyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, hexanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tetrahydrofurfuryl di(meth)acrylate, hexanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, Dimethylolpropane tri(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, epoxy acrylate, polyester acrylate, urethane acrylate, 2-hydroxyethyl(meth)acrylate, 3-hydroxypropyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, 4-hydroxybutyl(meth)acrylate ) acrylate, 2-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 3-hydroxy-3-methylbutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, pentaerythritol tri(meth)acrylate, 2-[(meth)acryloyloxy]ethyl 2-hydroxyethyl phthalate, 2-[(meth)acryloyloxy]ethyl 2-hydroxypropyl phthalate, and the like.When the acrylic polymer is one in which another vinyl monomer component has been copolymerized, a hydrolyzable silicon group can be introduced by copolymerizing a vinyl monomer component having a hydrolyzable silicon group.
[0069] From the standpoint of improving weather resistance, the main chain in the modified silicone resin preferably has a structural unit derived from an acrylic monomer.
[0070] From the standpoint of improving weather resistance, the content of structural units derived from acrylic monomers in 100% by weight of the main chain in the modified silicone resin is preferably 5% by weight or more, and preferably 20% by weight or less.
[0071] The hydrolyzable silicon group is not particularly limited, but examples thereof include a halogenated silyl group, an alkenyloxysilyl group, an acyloxysilyl group, an aminosilyl group, an aminooxysilyl group, an oximesilyl group, an amidosilyl group, and an alkoxysilyl group.
[0072] The number of hydrolyzable groups bonded to a silicon atom in the hydrolyzable silicon group is preferably 1 or more, and preferably 3 or less. The hydrolyzable group bonded to one silicon atom may be one type or two or more types. The hydrolyzable group and the non-hydrolyzable group may be bonded to one silicon atom. The hydrolyzable silicon group is preferably a monoalkoxysilyl group, a dialkoxysilyl group, or a trialkoxysilyl group, because of its excellent stability and easy handling.
[0073] When the curable resin contains the modified silicone resin, the curable resin preferably contains a silanol condensation catalyst. The curable resin preferably contains the modified silicone resin and a silanol condensation catalyst. By using the silanol condensation catalyst, the modified silicone resin can be cured in a short time. The silanol condensation catalyst may be used alone or in combination of two or more.
[0074] Examples of the silanol condensation catalyst include tin catalysts such as monoalkyltin esters and dialkyltin esters, poly(dialkylstannoxane) disilicate resins, and organic titanates.
[0075] Examples of the monoalkyltin ester include butyltin tris(2-ethylhexanoate), etc. Examples of the dialkyltin ester include dibutyltin acetate, dibutyltin dilaurate, dibutyltin dioctoate, dibutyltin dioleate, dibutyltin dimethoxide, dibutyltin diphenoxide, dibutyltin diacetylacetonate, dibutyltin acetoacetate, and stannous octoate, etc.
[0076] Examples of the organic titanate include titanium alkoxides such as tetrabutyl titanate, tetraisopropyl titanate, tetramethyl titanate, and tetra(2-ethylhexyl titanate)triethanolamine titanate; and titanium chelates such as titanium tetraacetylacetonate, titanium ethylacetoacetate, and octylene glycolate.
[0077] The content of the silicone condensation catalyst is preferably 0.1 parts by weight or more, more preferably 1 part by weight or more, preferably 10 parts by weight or less, more preferably 5 parts by weight or less, based on 100 parts by weight of the modified silicone resin.When the content of the silicone condensation catalyst is above the lower limit, the material of the resin layer containing the modified silicone resin can be cured in a short time, and the resin layer can be obtained well in a short time.When the content of the silicone condensation catalyst is below the upper limit, the adhesive strength of the resin layer can be increased.
[0078] The silicone resin may be an organopolysiloxane having two or more alkenyl groups bonded to silicon atoms. The main chain of the organopolysiloxane is generally a diorganosiloxane polymer, but may have a partially branched structure or a cyclic structure. The alkenyl group of the organopolysiloxane may be a vinyl group, a 1-propenyl group, a 2-propenyl group, an isopropenyl group, a butenyl group, a 1-methyl-2-propenyl group, a petenyl group, a hexenyl group, an octenyl group, and a cyclohexenyl group.
[0079] The curing agent (crosslinking agent) for the silicone resin may be, for example, an organohydrogenpolysiloxane having two or more SiH groups. Examples of the organohydrogenpolysiloxane include phenylmethylhydrogenpolysiloxane, 1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethylcyclotetrasiloxane, methylhydrogenpolysiloxane blocked at both ends with trimethylsiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymer blocked at both ends with trimethylsiloxy groups, dimethylpolysiloxane blocked at both ends with dimethylhydrogensiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymer blocked at both ends with dimethylhydrogensiloxane, methylhydrogensiloxane-diphenylsiloxane copolymer blocked at both ends with trimethylsiloxy groups, and methylhydrogensiloxane-diphenylsiloxane-dimethylsiloxane copolymer blocked at both ends with trimethylsiloxy groups.
[0080] Examples of the epoxy resin include bisphenol-type epoxy resins such as bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, bisphenol S-type epoxy resins, and hydrogenated products thereof; glycidyl ether-type epoxy resins such as polypropylene glycol diglycidyl ether-type epoxy resins; ester-type epoxy resins such as phthalic acid diglycidyl ester-type epoxy resins; novolac-type epoxy resins such as phenol novolac-type epoxy resins, bisphenol A novolac-type epoxy resins, cresol novolac-type epoxy resins, and hydrogenated products thereof; trisphenol-type multifunctional epoxy resins such as triphenol methane-type epoxy resins; triglycidyl isopropyl ether-type epoxy resins; Examples of the epoxy resins include nitrogen-containing ring-type polyfunctional epoxy resins such as cyanurate-type epoxy resins, tetraglycidyldiaminodiphenylmethane-type epoxy resins, tetraglycidylmeta-xylylenediamine-type epoxy resins, and hydantoin-type epoxy resins; condensed-ring type epoxy resins such as naphthalene-type epoxy resins; biphenyl-type epoxy resins; dicyclopentadiene-type epoxy resins; ether ester-type epoxy resins; epoxy resins having an alicyclic structure such as 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate; urethane-type epoxy resins; and rubber-modified epoxy resins having a rubber skeleton such as polybutadiene and acrylonitrile butadiene rubber (NBR).
[0081] In the case where the curable resin contains the epoxy resin, the curable resin preferably contains a curing agent for the epoxy resin (epoxy curing agent). That is, the curable component preferably contains the epoxy resin and the epoxy curing agent.
[0082] Examples of the epoxy resin curing agent (epoxy curing agent) include amine compounds, imidazole compounds, amide compounds, and cyano compounds. Examples of the amine compounds include ethylenediamine, propylenediamine, diethylenetriamine, triethylenetetramine, their amine adducts, metaphenylenediamine, diaminodiphenylmethane, and diaminodiphenylsulfone. Examples of the imidazole compounds include methylimidazole, 2-ethyl-4-methylimidazole, 1-isobutyl-2-methylimidazole, 1-benzyl-2-methylimidazole, 2-ethyl-4-methylimidazole, ethylimidazole, isopropylimidazole, 2,4-dimethylimidazole, phenylimidazole, undecylimidazole, heptadecylimidazole, 2-phenyl-4-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. The amide compound may be polyamide, etc. The cyano compound may be dicyandiamide, etc.
[0083] The epoxy curing agent may be a latent curing agent such as ketimine, in which the active amine is blocked and which is activated under a certain condition such as moisture, etc. For example, ketimine is stable in the absence of moisture, but generally becomes a primary amine in the presence of moisture and reacts with the epoxy resin. Examples of the latent curing agent include 2,5,8-triaza-1,8-nonadiene, 2,10-dimethyl-3,6,9-triaza-2,9-undecadiene, 2,10-diphenyl-3,6,9-triaza-2,9-undecadiene, 3,11-dimethyl-4,7,10-triaza-3,10-tridecadiene, 3,11-diethyl-4,7,10-triaza-3,10-tridecadiene, 2,4,12,14-tetramethyl-5,8,11-triaza-4,11-pentadecadiene, 2,4,20,22-tetramethyl-5,12,19-triaza-4,19-trieicosadiene, and 2,4,15,17-tetramethyl-5,8,11,14-tetraaza-4,14-octadecadiene.
[0084] A cured epoxy resin can be obtained by reacting the epoxy resin with the epoxy curing agent.
[0085] From the viewpoint of exerting the effects of the present invention more effectively, the epoxy resin preferably contains an epoxy resin having an aromatic skeleton, and is more preferably a bisphenol A type epoxy resin or a bisphenol F type epoxy resin.
[0086] In order to more effectively exert the effects of the present invention, the epoxy curing agent is preferably an amine-based curing agent (amine compound).
[0087] A urethane resin can be obtained by curing a polyol compound with an isocyanate compound. Examples of the polyol compound include bisphenol A, bisphenol F, phenol novolac, cresol novolac, cyclohexanediol, methylcyclohexanediol, isophoronediol, dicyclohexylmethanediol, dimethyldicyclohexylmethanediol, ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, polyester polyol, polyether polyol, a polymer obtained by dehydration condensation of a polybasic acid and a polyhydric alcohol, and a polymer obtained by ring-opening polymerization of lactone such as ε-caprolactone or α-methyl-ε-caprolactone.
[0088] The isocyanate compound may be a polyisocyanate compound. The polyisocyanate compound may be an aromatic polyisocyanate, an alicyclic polyisocyanate, or an aliphatic polyisocyanate. The aromatic polyisocyanate may be phenylene diisocyanate, toluene diisocyanate, tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, dimethyldiphenylethane diisocyanate, triphenylmethane triisocyanate, naphthalene diisocyanate, or polymethylene polyphenyl polyisocyanate. The alicyclic polyisocyanate may be cyclohexylene diisocyanate, methylcyclohexylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, or dimethyldicyclohexylmethane diisocyanate. Examples of the aliphatic polyisocyanate include methylene diisocyanate, ethylene diisocyanate, propylene diisocyanate, tetramethylene diisocyanate, and hexamethylene diisocyanate.
[0089] From the viewpoint of exerting the effects of the present invention more effectively, the polyol compound is preferably a polyester polyol or a polyether polyol. From the viewpoint of exerting the effects of the present invention more effectively, the curing agent (isocyanate compound) of the polyol compound is preferably diphenylmethane diisocyanate or toluene diisocyanate.
[0090] The mixing ratio of the polyol compound and the polyisocyanate compound can be appropriately changed depending on the combination of the types of the polyol compound and the polyisocyanate compound. The mixing amount of the polyisocyanate compound is preferably an amount such that the amount of hydroxyl groups of the polyol compound is equal to the amount of isocyanate groups (NCO amount) of the polyisocyanate compound.
[0091] Examples of the phenol resin include novolac type phenol, biphenol type phenol, naphthalene type phenol, dicyclopentadiene type phenol, aralkyl type phenol, and dicyclopentadiene type phenol.
[0092] The hardener for the phenol resin includes hexamethylenetetramine, paraformaldehyde, and the like.
[0093] Examples of the vinyl ester resin include a reaction product of an epoxy resin and an unsaturated monobasic acid. Examples of the epoxy resin include aliphatic glycidyl ethers such as bisphenol A diglycidyl ether and its high molecular weight homologues, novolac-type polyglycidyl ether and its high molecular weight homologues, and 1,6-hexanediol diglycidyl ether. Examples of the unsaturated monobasic acid include acrylic acid and methacrylic acid. Examples of the reaction product of the epoxy resin with the acrylic acid and the methacrylic acid include epoxy (meth)acrylate.
[0094] Examples of the curing agent for the vinyl ester resin include organic peroxides, such as ketone peroxides, perbenzoates, hydroperoxides, diacyl peroxides, peroxyketals, hydroperoxides, diallyl peroxides, peroxyesters, and peroxydicarbonates.
[0095] When the curable resin contains the vinyl ester resin, the curable component may contain a radical polymerizable unsaturated monomer. Examples of the radical polymerizable unsaturated monomer include styrene monomer, α-, o-, m-, p-alkyl, nitro, cyano, amide, and ester derivatives of styrene, chlorostyrene, vinyltoluene, and divinylbenzene, and other styrene-based monomers, butadiene, 2,3-dimethylbutadiene, isoprene, and chloroprene, and other dienes; ethyl (meth)acrylate, methyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, dodecyl (meth)acrylate, and (meth)acrylate. (meth)acrylic acid esters such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, tetrahydrofuryl (meth)acrylate, acetoacetoxyethyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, and phenoxyethyl (meth)acrylate; (meth)acrylic acid amides such as (meth)acrylic acid amide and (meth)acrylic acid N,N-dimethylamide; vinyl resins such as (meth)acrylic acid anilide; unsaturated dicarboxylic acid diesters such as diethyl citraconic acid; monomaleimide resins such as N-phenylmaleimide; and N-(meth)acryloylphthalimide.
[0096] In the above separator hole filler, from the viewpoint of filling the separator hole well with the above separator hole filler, the above resin preferably contains a curable resin, and more preferably contains an epoxy resin or a modified silicone resin.
[0097] In the above separator coating material, from the viewpoint of improving the handleability of the separator immediately after coating with the coating material, the resin preferably includes a thermoplastic resin, and more preferably includes a polyolefin resin. In the above separator coating material, from the viewpoint of coating the separator well with the separator coating material, the resin preferably includes a curable resin, and more preferably includes an epoxy resin, a vinyl ester resin, or an unsaturated polyester resin. In the above separator coating material, the resin preferably includes an epoxy resin, a vinyl ester resin, an unsaturated polyester resin, or a polyolefin resin.
[0098] In 100% by weight of the separator hole filler, the content of the resin is preferably 30% by weight or more, more preferably 50% by weight or more, even more preferably 55% by weight or more, particularly preferably 60% by weight or more, and preferably 97% by weight or less, more preferably 95% by weight or less, even more preferably 90% by weight or less, particularly preferably 80% by weight or less. When the content of the resin is equal to or more than the lower limit and equal to or less than the upper limit, cations or anions are released more effectively, and poorly water-soluble salts are produced well. As a result, the separator hole and its surroundings are further densified, and the concrete structure can be maintained in a stable state for a longer period of time.
[0099] In 100% by weight of the separator hole filler, the content of the curable resin is preferably 30% by weight or more, more preferably 50% by weight or more, even more preferably 55% by weight or more, particularly preferably 60% by weight or more, and preferably 97% by weight or less, more preferably 95% by weight or less, even more preferably 90% by weight or less, particularly preferably 80% by weight or less. When the content of the curable resin is above the lower limit and below the upper limit, cations or anions are released more effectively, and poorly water-soluble salts are produced well. As a result, the separator hole and its surroundings are further densified, and the concrete structure can be maintained in a stable state for a longer period of time.
[0100] In 100% by weight of the separator hole filler, the content of the epoxy resin is preferably 35% by weight or more, more preferably 50% by weight or more, even more preferably 55% by weight or more, particularly preferably 60% by weight or more, and preferably 95% by weight or less, more preferably 90% by weight or less, even more preferably 85% by weight or less, particularly preferably 80% by weight or less. When the content of the epoxy resin is equal to or more than the lower limit and equal to or less than the upper limit, cations or anions are released more effectively, and poorly water-soluble salts are produced well. As a result, the separator hole and its surroundings are further densified, and the concrete structure can be maintained in a stable state for a longer period of time.
[0101] In 100% by weight of the separator hole filler, the content of the modified silicone resin is preferably 35% by weight or more, more preferably 50% by weight or more, even more preferably 55% by weight or more, particularly preferably 60% by weight or more, and preferably 97% by weight or less, more preferably 95% by weight or less, even more preferably 90% by weight or less, particularly preferably 80% by weight or less. When the content of the modified silicone resin is above the lower limit and below the upper limit, cations or anions are released more effectively, and poorly water-soluble salts are produced well. As a result, the separator hole and its surroundings are further densified, and the concrete structure can be maintained in a stable state for a longer period of time.
[0102] In 100% by weight of the separator coating material, the content of the resin is preferably 30% by weight or more, more preferably 50% by weight or more, even more preferably 55% by weight or more, particularly preferably 60% by weight or more, and is preferably 97% by weight or less, more preferably 95% by weight or less, even more preferably 90% by weight or less, particularly preferably 80% by weight or less. When the content of the resin is equal to or more than the lower limit and equal to or less than the upper limit, cations or anions are released more effectively, and poorly water-soluble salts are produced well. As a result, the separator and its surroundings are further densified, and the concrete structure can be maintained in a stable state for a longer period of time.
[0103] In 100% by weight of the separator coating material, the content of the curable resin is preferably 30% by weight or more, more preferably 50% by weight or more, even more preferably 55% by weight or more, particularly preferably 60% by weight or more, and is preferably 97% by weight or less, more preferably 95% by weight or less, even more preferably 90% by weight or less, particularly preferably 80% by weight or less. When the content of the curable resin is equal to or more than the lower limit and equal to or less than the upper limit, cations or anions are released more effectively, and poorly water-soluble salts are produced well. As a result, the separator and its surroundings are further densified, and the concrete structure can be maintained in a stable state for a longer period of time.
[0104] In 100% by weight of the separator coating material, the content of the epoxy resin is preferably 35% by weight or more, more preferably 50% by weight or more, even more preferably 55% by weight or more, particularly preferably 60% by weight or more, and is preferably 95% by weight or less, more preferably 90% by weight or less, and even more preferably 85% by weight or less. When the content of the epoxy resin is equal to or more than the lower limit and equal to or less than the upper limit, cations or anions are released more effectively, and poorly water-soluble salts are produced well. As a result, the separator and its surroundings are further densified, and the concrete structure can be maintained in a stable state for a longer period of time.
[0105] In 100% by weight of the separator coating material, the content of the vinyl ester resin is preferably 35% by weight or more, more preferably 50% by weight or more, even more preferably 55% by weight or more, particularly preferably 60% by weight or more, and is preferably 97% by weight or less, more preferably 95% by weight or less, and even more preferably 90% by weight or less. When the content of the vinyl ester resin is equal to or more than the lower limit and equal to or less than the upper limit, cations or anions are released more effectively, and poorly water-soluble salts are produced well. As a result, the separator and its surroundings are further densified, and the concrete structure can be maintained in a stable state for a longer period of time.
[0106] In 100% by weight of the separator coating material, the content of the unsaturated polyester resin is preferably 35% by weight or more, more preferably 50% by weight or more, even more preferably 55% by weight or more, particularly preferably 60% by weight or more, and is preferably 97% by weight or less, more preferably 95% by weight or less, and even more preferably 90% by weight or less. When the content of the unsaturated polyester resin is equal to or more than the lower limit and equal to or less than the upper limit, cations or anions are released more effectively, and poorly water-soluble salts are produced well. As a result, the separator and its surroundings are further densified, and the concrete structure can be maintained in a stable state for a longer period of time.
[0107] In 100% by weight of the separator coating material, the content of the polyolefin resin is preferably 35% by weight or more, more preferably 50% by weight or more, even more preferably 55% by weight or more, particularly preferably 60% by weight or more, and is preferably 97% by weight or less, more preferably 95% by weight or less, and even more preferably 90% by weight or less. When the content of the polyolefin resin is equal to or more than the lower limit and equal to or less than the upper limit, cations or anions are released more effectively, and poorly water-soluble salts are produced well. As a result, the separator and its surroundings are further densified, and the concrete structure can be maintained in a stable state for a longer period of time.
[0108] <Cement milk and mortar> In this specification, "cement milk" refers to a mixture of cement and water (mixing water). In this specification, "cement milk" does not include fine aggregate and coarse aggregate. In this specification, "mortar" refers to a mixture of cement, fine aggregate, and water (mixing water). In this specification, "mortar" does not include coarse aggregate. In this specification, "concrete" refers to a mixture of cement, fine aggregate, coarse aggregate, and water (mixing water). In this specification, "cement" refers to a powder whose main raw materials are limestone, clay, silica stone, and iron oxide raw materials, etc., and which can harden by a chemical reaction with water.
[0109] The cement contained in the cement milk and the mortar is not particularly limited. Examples of the cement contained in the cement milk and the mortar include Portland cement, blast furnace cement, silica cement, and fly ash cement. The Portland cement may be ordinary Portland cement or special Portland cement (high early strength Portland cement).
[0110] Examples of the fine aggregate include artificial aggregate and natural aggregate. Examples of the artificial aggregate include blast furnace slag and fly ash. Examples of the natural aggregate include sand. From the viewpoint of reducing material costs, it is preferable that the fine aggregate is sand.
[0111] The average particle size of the fine aggregate is preferably 0.01 mm or more, more preferably 0.1 mm or more, and is preferably 5 mm or less, more preferably 4 mm or less. When the average particle size of the fine aggregate is equal to or more than the lower limit, the strength of the concrete structure can be increased. When the average particle size of the fine aggregate is equal to or less than the upper limit, the fine aggregate can be prevented from settling, and the viscosity of the mortar can be improved. The average particle size of the fine aggregate is preferably a number average particle size.
[0112] From the viewpoint of exerting the effects of the present invention more effectively, the cement content in 100% by weight of the cement milk is preferably 10% by weight or more, more preferably 20% by weight or more, even more preferably 30% by weight or more, and preferably 90% by weight or less, more preferably 80% by weight or less, even more preferably 70% by weight or less.
[0113] In the above cement milk, the content of water (mixing water) relative to 100 parts by weight of cement is preferably 11 parts by weight or more, more preferably 25 parts by weight or more, even more preferably 35 parts by weight or more, and preferably 125 parts by weight or less, more preferably 100 parts by weight or less, even more preferably 66 parts by weight or less. When the content of the water (mixing water) is equal to or more than the above lower limit, the cement and the water (mixing water) can be reacted well, and the strength of the concrete structure can be increased. When the content of the water (mixing water) is equal to or less than the above upper limit, the cement and the water (mixing water) can be mixed uniformly, and the strength of the concrete structure can be increased.
[0114] From the viewpoint of exerting the effects of the present invention more effectively, the cement content in 100% by weight of the mortar is preferably 10% by weight or more, more preferably 15% by weight or more, even more preferably 20% by weight or more, and is preferably 60% by weight or less, more preferably 50% by weight or less, even more preferably 40% by weight or less.
[0115] From the viewpoint of exerting the effects of the present invention more effectively, the content of fine aggregate in 100% by weight of the above mortar is preferably 10% by weight or more, more preferably 15% by weight or more, even more preferably 20% by weight or more, and is preferably 90% by weight or less, more preferably 85% by weight or less, even more preferably 80% by weight or less.
[0116] From the viewpoint of exerting the effects of the present invention more effectively, in the above mortar, the content of fine aggregate per 100 parts by weight of cement is preferably 11 parts by weight or more, more preferably 25 parts by weight or more, even more preferably 40 parts by weight or more, and is preferably 900 parts by weight or less, more preferably 400 parts by weight or less, even more preferably 300 parts by weight or less.
[0117] In the above mortar, the content of water (mixing water) relative to 100 parts by weight of cement is preferably 20 parts by weight or more, more preferably 30 parts by weight or more, and even more preferably 40 parts by weight or more, and is preferably 200 parts by weight or less, more preferably 100 parts by weight or less, and even more preferably 60 parts by weight or less. When the content of the water (mixing water) is equal to or more than the lower limit, the cement and the water (mixing water) can be reacted well, and the strength of the concrete structure can be increased. When the content of the water (mixing water) is equal to or less than the upper limit, the cement and the water (mixing water) can be mixed uniformly, and the strength of the concrete structure can be increased.
[0118] In 100% by weight of the separator hole filler, the content of the cement milk or the mortar is preferably 80% by weight or more, more preferably 90% by weight or more, even more preferably 94% by weight or more, and preferably 99.9% by weight or less, more preferably 99.5% by weight or less, even more preferably 99% by weight or less. When the content of the cement milk or the mortar is equal to or more than the lower limit and equal to or less than the upper limit, the effect of the present invention can be more effectively exhibited.
[0119] <Ion-releasing compound> The separator hole filling material and the separator coating material contain an ion-releasing compound capable of releasing cations or anions. The ion-releasing compound is capable of generating a poorly water-soluble salt.
[0120] The ion-releasing compound may be a compound capable of releasing a cation, may be a compound capable of releasing an anion, may be a compound capable of releasing both a cation and an anion, or may be a mixture of a compound capable of releasing a cation and a compound capable of releasing an anion. The ion-releasing compound may contain a compound capable of releasing a cation, may contain a compound capable of releasing an anion, or may contain a compound capable of releasing a cation and a compound capable of releasing an anion. The ion-releasing compound may be used alone or in combination of two or more.
[0121] It is preferable that the ion-releasing compound generates a poorly water-soluble salt by contact with moisture or the like attached to the concrete structure. It is preferable that the ion-releasing compound releases cations or anions due to water or moisture that reaches the location where the separator hole filling material and the separator coating material are arranged. Specifically, when the ion-releasing compound is a compound capable of releasing cations, it is preferable that the cations released from the ion-releasing compound and the anions dissolved in moisture or the like react chemically to form a poorly water-soluble salt. When the ion-releasing compound is a compound capable of releasing anions, it is preferable that the anions released from the ion-releasing compound and the cations dissolved in moisture or the like react chemically to form a poorly water-soluble salt. In addition, when the ion-releasing compound is a compound capable of releasing both cations and anions, or a mixture of a compound capable of releasing cations and a compound capable of releasing anions, it is preferable that the cations and anions released from the ion-releasing compound move to a medium through moisture or the like, and form a poorly water-soluble salt at the point where they meet.
[0122] The ion-releasing compound may be an inorganic salt, an ion-exchange resin, or an ion complex.
[0123] Examples of the ion-releasing compound include calcium silicate, tricalcium silicate, dicalcium silicate, calcium aluminate, calcium aluminoferrite, calcium hydroxide, calcium oxide, calcium acetate, calcium lactate, barium lactate, calcium sulfate, calcium chloride, calcium nitrate, calcium hydrogen carbonate, sodium hydrogen phosphate, potassium carbonate, potassium hydrogen carbonate, ammonium carbonate, ammonium hydrogen carbonate, sodium carbonate, and sodium hydrogen carbonate. The ion-releasing compound is preferably one of these ion-releasing compounds. These ion-releasing compounds can produce poorly water-soluble salts more effectively.
[0124] Examples of the compound capable of releasing the cations include calcium silicate, tricalcium silicate, dicalcium silicate, calcium aluminate, calcium aluminoferrite, calcium hydroxide, calcium oxide, calcium acetate, calcium lactate, barium lactate, calcium sulfate, calcium chloride, calcium nitrate, calcium hydrogen carbonate, etc. Only one type of the compound capable of releasing the cations may be used, or two or more types may be used in combination.
[0125] The compound capable of releasing the cations is preferably calcium silicate, tricalcium silicate, dicalcium silicate, calcium aluminate, calcium aluminoferrite, calcium hydroxide, calcium oxide, calcium acetate, calcium lactate, barium lactate, calcium sulfate, calcium chloride, calcium nitrate, or calcium hydrogen carbonate. When the compound capable of releasing the cations is the above-mentioned preferred compound, the effect of the present invention can be more effectively exhibited. From the viewpoint of more effectively exhibiting the effect of the present invention, the compound capable of releasing the cations is more preferably calcium oxide, calcium chloride, calcium nitrate, calcium acetate, calcium lactate, or barium lactate, and more preferably calcium lactate. From the viewpoint of more effectively exhibiting the effect of the present invention, the compound capable of releasing the cations is preferably a compound capable of releasing calcium ions, and more preferably an organic acid calcium salt. Examples of the organic acid calcium salt include calcium acetate and calcium lactate.
[0126] Examples of the compound capable of releasing the anion include sodium hydrogen phosphate, potassium carbonate, potassium hydrogen carbonate, ammonium carbonate, ammonium hydrogen carbonate, sodium carbonate, sodium hydrogen carbonate, calcium hydrogen carbonate, etc. The compound capable of releasing the anion may be used alone or in combination of two or more kinds.
[0127] From the viewpoint of exerting the effects of the present invention more effectively, the compound capable of releasing the anion is preferably sodium hydrogen phosphate, potassium carbonate, potassium hydrogen carbonate, ammonium carbonate, ammonium hydrogen carbonate, sodium carbonate, sodium hydrogen carbonate, or calcium hydrogen carbonate. From the viewpoint of exerting the effects of the present invention more effectively, the compound capable of releasing the anion is more preferably sodium hydrogen phosphate, sodium carbonate, or sodium hydrogen carbonate, and even more preferably sodium hydrogen carbonate. From the viewpoint of exerting the effects of the present invention more effectively, the compound capable of releasing the anion is preferably a compound capable of releasing hydrogen carbonate ion (bicarbonate ion) or carbonate ion.
[0128] An example of the compound capable of releasing both cations and anions is calcium hydrogen carbonate.
[0129] From the viewpoint of producing poorly water-soluble salts more satisfactorily, the separator hole filler and the separator coating material are preferably a mixture of a compound capable of releasing cations and a compound capable of releasing anions, and more preferably a mixture of a compound capable of releasing calcium ions and a compound capable of releasing bicarbonate ions or carbonate ions. From the viewpoint of producing poorly water-soluble salts more satisfactorily, the separator hole filler and the separator coating material preferably contain a compound capable of releasing cations and a compound capable of releasing anions, and more preferably contain a compound capable of releasing calcium ions and a compound capable of releasing bicarbonate ions or carbonate ions.
[0130] Examples of the poorly water-soluble salt include the following compounds: Calcium carbonate (specific gravity: 2.71, solubility in water at 20°C: 1.5 x 10 -4 mol / L). Barium carbonate (specific gravity: 4.29, solubility in water at 20°C: 1.25 x 10 -4 mol / L). Calcium phosphate (specific gravity: 3.14, solubility in water at 20°C: 6.5×10 -5mol / L). Iron hydroxide (specific gravity: 3.40, solubility in water at 20°C: 5.0 x 10 -6 (mol / L).
[0131] From the viewpoint of exerting the effects of the present invention more effectively, the poorly water-soluble salt is preferably calcium carbonate, barium carbonate, calcium phosphate, or iron hydroxide. From the viewpoint of exerting the effects of the present invention more effectively, the ion-releasing compound is preferably capable of generating calcium carbonate, barium carbonate, calcium phosphate, or iron hydroxide as the poorly water-soluble salt. From the viewpoint of exerting the effects of the present invention more effectively, the poorly water-soluble salt is preferably calcium carbonate. From the viewpoint of exerting the effects of the present invention more effectively, the ion-releasing compound is preferably capable of generating calcium carbonate as the poorly water-soluble salt.
[0132] The ion-releasing compound may be particulate. The ion-releasing compound may be spherical, may be a shape other than spherical, or may be flat. The ion-releasing compound is preferably spherical.
[0133] The particle size of the ion-releasing compound is preferably 1.0 μm or more, more preferably 5.0 μm or more, even more preferably 10 μm or more, and preferably 1000 μm or less, more preferably 500 μm or less, even more preferably 150 μm or less, and particularly preferably 100 μm or less. When the particle size of the ion-releasing compound is the above-mentioned lower limit or more, the ion-releasing compound is well coated with the coating material (A) described later, and the dispersibility of the ion-releasing compound in the separator hole filler and the separator coating material can be improved. In addition, when the particle size of the ion-releasing compound is the above-mentioned lower limit or more, the viscosity when the separator hole filler is filled into the separator hole can be improved, and the viscosity when the separator is coated using the separator coating material can be improved, and the arrangement of the separator hole filler and the separator coating material can be improved. When the particle size of the ion-releasing compound is equal to or less than the upper limit, the dispersibility of the ion-releasing compound in the separator hole filling material and the separator coating material can be improved.
[0134] The particle size of the ion-releasing compound is preferably an average particle size. The average particle size indicates a number average particle size. The average particle size of the ion-releasing compound is determined by observing 50 arbitrary ion-releasing compounds with an electron microscope or an optical microscope and calculating the average value.
[0135] In the separator hole filler and the separator coating material, the surface of the ion-releasing compound may be coated with a coating material (in this specification, the coating material for coating the ion-releasing compound may be referred to as "coating material (A)"). The ion-releasing compound may be an inclusion of a microcapsule. When the ion-releasing compound is an inorganic salt, the surface of the ion-releasing compound is preferably coated with a coating material (A) in the separator hole filler and the separator coating material. When the ion-releasing compound is an inorganic salt, the separator hole filler and the separator coating material preferably contain a microcapsule containing the ion-releasing compound as an inclusion. When the surface of the ion-releasing compound is coated with a coating material (A) or the ion-releasing compound is an inclusion of a microcapsule, the time and amount of cations or anions released from the ion-releasing compound can be controlled.
[0136] The ion-releasing compound coated with the coating material (A) is preferably capable of releasing cations or anions when moisture such as water or humidity comes into contact with the separator hole filler and the separator coating material and the moisture diffuses and penetrates into the coating material (A). The ion-releasing compound coated with the coating material (A) may be capable of releasing cations or anions from voids in the coating material (A). The ion-releasing compound coated with the coating material (A) may be capable of diffusing into the coating material (A) and releasing cations or anions. In these cases, the timing and amount of cations or anions released from the ion-releasing compound can be controlled even better.
[0137] The microcapsules are preferably capable of releasing the ion-releasing compound. The membrane constituting the microcapsules is preferably disintegrated when the microcapsules come into contact with water or moisture such as humidity. In this case, the timing and amount of cations or anions released from the ion-releasing compound can be more effectively controlled.
[0138] The material of the membrane constituting the microcapsules and the material of the coating material (A) for coating the surface of the ion-releasing compound can be appropriately selected depending on the type of the ion-releasing compound. The material of the membrane constituting the microcapsules and the material of the coating material (A) for coating the surface of the ion-releasing compound preferably contain a coupling agent or a resin. In this case, the dispersibility of the ion-releasing compound in the separator hole filler and the separator coating material can be improved, and the timing and amount of the release of cations or anions can be well controlled. In addition, the thickness of the membrane constituting the microcapsules can be made uniform, and the surface of the ion-releasing compound can be uniformly coated with the coating material (A).
[0139] The coupling agent includes a silane coupling agent, a titanium coupling agent, and the like.
[0140] The resin may be a water-soluble resin, a thermoplastic resin, a curable resin, etc. The resin may be used alone or in combination of two or more. The resin contained in the separator hole filling material and the separator coating material may be the same as or different from the resin contained in the coating material (A).
[0141] Examples of the water-soluble resin include polyvinyl alcohol, polylactic acid resin (PLA resin), poly(meth)acrylic acid, poly(meth)acrylamide, polyvinylpyrrolidone, polyethylene oxide, and methylcellulose.
[0142] Examples of the thermoplastic resin and the curable resin include the above-mentioned thermoplastic resin and curable resin.
[0143] From the viewpoint of better controlling the timing and amount of cations or anions released from the ion-releasing compound, the resin contained in the material of the coating material (A) preferably contains a thermoplastic resin, more preferably contains a polyolefin resin or an ethylene-vinyl acetate copolymer, and particularly preferably is an ethylene-vinyl acetate copolymer.
[0144] The thickness of the membrane constituting the microcapsules and the thickness of the coating layer of the coating material (A) are not particularly limited. From the viewpoint of better controlling the timing and amount of release of cations or anions from the ion-releasing compound, the thickness of the membrane constituting the microcapsules and the thickness of the coating layer of the coating material (A) are preferably 1 μm or more, more preferably 5 μm or more, and preferably 1000 μm or less, more preferably 200 μm or less.
[0145] In 100% by weight of the separator hole filler, the content of the ion-releasing compound is preferably 3% by weight or more, more preferably 5% by weight or more, even more preferably 10% by weight or more, particularly preferably 20% by weight or more, and preferably 70% by weight or less, more preferably 50% by weight or less, even more preferably 45% by weight or less, particularly preferably 40% by weight or less. When the content of the ion-releasing compound is above the lower limit and below the upper limit, cations or anions are released more effectively, and poorly water-soluble salts are produced well. As a result, the separator hole and its surroundings are further densified, and the concrete structure can be maintained in a stable state for a longer period of time. When the content of the ion-releasing compound is below the upper limit, the appearance of the concrete structure after filling with the separator hole filler can be improved, and the strength of the separator hole and its surroundings can be increased.
[0146] In the separator hole filler, the content of the ion-releasing compound is preferably 3 parts by weight or more, more preferably 5 parts by weight or more, even more preferably 10 parts by weight or more, particularly preferably 20 parts by weight or more, and preferably 200 parts by weight or less, more preferably 100 parts by weight or less, and even more preferably 70 parts by weight or less, relative to 100 parts by weight of the resin. When the content of the ion-releasing compound is above the lower limit and below the upper limit, the cations or anions are released more effectively, and the poorly water-soluble salt is well generated. As a result, the separator hole and its surroundings are further densified, and the concrete structure can be maintained in a stable state for a longer period of time. When the content of the ion-releasing compound is below the upper limit, the viscosity of the separator hole filler when filling the separator hole can be improved, and the arrangement of the separator hole filler can be improved.
[0147] In the separator hole filler, the content of the ion-releasing compound is preferably 3 parts by weight or more, more preferably 5 parts by weight or more, and even more preferably 10 parts by weight or more, and is preferably 200 parts by weight or less, more preferably 100 parts by weight or less, and even more preferably 70 parts by weight or less, relative to 100 parts by weight of the cement milk or the mortar. When the content of the ion-releasing compound is above the lower limit and below the upper limit, the cations or anions are more effectively released, and the poorly water-soluble salt is well generated. As a result, the separator hole and its surroundings are more dense, and the concrete structure can be maintained in a stable state for a longer period of time. When the content of the ion-releasing compound is below the upper limit, the viscosity of the separator hole filler when filling the separator hole can be improved, and the placement of the separator hole filler can be improved.
[0148] In 100% by weight of the separator hole filler, the total content of the ion-releasing compound and the coating material (A) is preferably 3% by weight or more, more preferably 5% by weight or more, and preferably 70% by weight or less, more preferably 50% by weight or less. When the total content of the ion-releasing compound and the coating material (A) is equal to or more than the lower limit and equal to or less than the upper limit, the cations or anions are more effectively released, and the poorly water-soluble salts are well generated. As a result, the separator hole and its surroundings are more dense, and the concrete structure can be maintained in a stable state for a longer period of time. When the total content of the ion-releasing compound and the coating material (A) is equal to or less than the upper limit, the viscosity of the separator hole filler when filling the separator hole can be improved, and the arrangement of the separator hole filler can be improved.
[0149] In 100% by weight of the separator coating material, the content of the ion-releasing compound is preferably 3% by weight or more, more preferably 5% by weight or more, even more preferably 10% by weight or more, and particularly preferably 20% by weight or more. In 100% by weight of the separator coating material, the content of the ion-releasing compound is preferably 70% by weight or less, more preferably 50% by weight or less, even more preferably 45% by weight or less, and particularly preferably 40% by weight or less. When the content of the ion-releasing compound is equal to or more than the lower limit and equal to or less than the upper limit, the cations or anions are more effectively released, and the poorly water-soluble salt is well produced. As a result, the separator and its surroundings are more dense, and the concrete structure can be maintained in a stable state for a longer period of time. When the content of the ion-releasing compound is equal to or less than the upper limit, the strength of the separator and its surroundings can be increased.
[0150] In the separator coating material, the content of the ion-releasing compound is preferably 3 parts by weight or more, more preferably 5 parts by weight or more, even more preferably 10 parts by weight or more, particularly preferably 20 parts by weight or more, and preferably 200 parts by weight or less, more preferably 100 parts by weight or less, and even more preferably 70 parts by weight or less, relative to 100 parts by weight of the resin. When the content of the ion-releasing compound is equal to or more than the lower limit and equal to or less than the upper limit, the cations or anions are more effectively released, and the poorly water-soluble salt is well produced. As a result, the sealed area and its surroundings are more dense, and the concrete structure can be maintained in a stable state for a longer period of time. When the content of the ion-releasing compound is equal to or less than the upper limit, the viscosity when coating the separator with the separator coating material is improved, and the placement of the separator coating material can be improved.
[0151] In 100% by weight of the separator coating material, the total content of the ion-releasing compound and the coating material (A) is preferably 3% by weight or more, more preferably 5% by weight or more, and preferably 70% by weight or less, more preferably 50% by weight or less. When the total content of the ion-releasing compound and the coating material (A) is equal to or more than the lower limit and equal to or less than the upper limit, cations or anions are released more effectively, and poorly water-soluble salts are produced well. As a result, the separator holes and their surroundings are further densified, and the structure can be maintained in a stable state for a longer period of time. When the total content of the ion-releasing compound and the coating material (A) is equal to or less than the upper limit, the viscosity when coating the separator with the separator coating material is improved, and the placement of the separator coating material can be improved.
[0152] <Other ingredients> The separator hole filler and the separator coating material may contain other components, as necessary, in addition to the ion-releasing compound, the resin, the cement milk, the mortar, and the coating material (A), such as a reaction catalyst, a reaction accelerator, a crosslinking agent, a water absorbent, a foam stabilizer, an antioxidant, and a colorant.
[0153] (Separator) The separator according to the present invention includes a separator body and a coating material disposed on a surface of the separator body. In the separator according to the present invention, the coating material is formed from the above-mentioned separator coating material.
[0154] Since the separator according to the present invention has the above-mentioned configuration, it is possible to improve the rust resistance of the separator, improve the waterproofing of the separator and its surroundings, and maintain the concrete structure in a stable state for a long period of time.
[0155] In the separator, the coating material is preferably disposed on the surface of at least the end portions of the separator body, and is preferably disposed on the entire surface of the separator body.
[0156] The coating material may be the separator coating material itself. The coating material may be formed by hardening a resin (curable resin), cement milk, or mortar in the separator coating material. The coating material may be a hardened product of the separator coating material.
[0157] In the separator, the ion-releasing compound in the coating material (in the separator coating material or in the cured product of the separator coating material) is preferably dispersed in the resin (or in the cement milk or in the mortar) or in the cured product of the resin (or the cement milk or the mortar).
[0158] (Concrete structure and manufacturing method of concrete structure) A concrete structure can be obtained by using the separator hole filling material or separator coating material according to the present invention.
[0159] The above concrete structure (first concrete structure) comprises a concrete structure main body having a separator hole, and a filler filled in the separator hole of the concrete structure main body. In the above concrete structure (first concrete structure), the filler is formed from the above-mentioned separator hole filler. In the above concrete structure (first concrete structure), the filled area (separator hole) and its surroundings can be densified, and a stable state can be maintained for a long period of time. The above first concrete structure may comprise a separator of a second concrete structure described later.
[0160] The filler may be the separator hole filler itself. The filler may be formed by hardening the resin (curable resin), cement milk, or mortar in the separator hole filler. The filler may be a hardened product of the separator hole filler. The filler may be formed by extrusion molding or injection molding the separator hole filler. The filler may be a molded product of the separator hole filler.
[0161] It is preferable that the ion-releasing compound in the filler (in the filler for the separator holes, in the hardened product of the filler for the separator holes, or in the molded body of the filler for the separator holes) is dispersed in the resin (or in the cement milk or in the mortar) or in the hardened product of the resin (or the cement milk or the mortar).
[0162] The concrete structure (second concrete structure) comprises a concrete structure main body and a separator disposed inside the concrete structure main body. The separator comprises a separator main body and a coating material disposed on the surface of the separator main body. The coating material is formed from the separator coating material. In the concrete structure (second concrete structure), the coated area (on the surface of the separator main body) and its surroundings can be densified, and a stable state can be maintained for a long period of time. The second concrete structure may comprise the filler material of the first concrete structure described above.
[0163] In the concrete structure (second concrete structure), the coating material is preferably disposed on the surface of at least the end of the separator body, and is preferably disposed on the entire surface of the separator body. The concrete structure (second concrete structure) is preferably provided with the coating material on at least the end of the separator. The concrete structure (second concrete structure) is preferably provided with the coating material on the entire surface of the separator.
[0164] The coating material may be the separator coating material itself. The coating material may be formed by hardening a resin (curable resin), cement milk, or mortar in the separator coating material. The coating material may be a hardened product of the separator coating material.
[0165] The ion-releasing compound in the coating material (in the separator coating material or in the cured product of the separator coating material) is preferably dispersed in the resin (or in the cement milk or in the mortar) or in the cured product of the resin (or the cement milk or the mortar).
[0166] FIG. 1 is a cross-sectional view of a concrete structure (first concrete structure) using a separator hole filler according to one embodiment of the present invention.
[0167] The concrete structure 1 includes a filler 11, a separator 12, and a concrete structure body 13. The concrete structure body 13 has a separator hole 13a. The filler 11 is filled in the separator hole 13a of the concrete structure body 13. The separator 12 is disposed inside the concrete structure body 13.
[0168] In the concrete structure 1, the filler 11 is formed of a separator hole filler. The filler may be the separator hole filler itself, or may be a hardened product (protective cap) of the separator hole filler.
[0169] FIG. 2 is a cross-sectional view of a concrete structure using a separator coating material according to one embodiment of the present invention.
[0170] The concrete structure 1A includes a separator 12A and a concrete structure main body 13A. The concrete structure main body 13A has a separator hole 13Aa.
[0171] The separator 12A includes a separator body 12Aa and a coating material 12Ab. The coating material 12Ab is disposed on the surface of the separator body 12Aa. The coating material 12Ab is disposed on the surface (outer periphery and end portion) of the separator body 12Aa. The coating material 12Ab is disposed over the entire surface of the separator body 12Aa. In the concrete structure 1A, the coating material 12Ab is formed from a separator coating material. The coating material may be the separator coating material itself, or may be a hardened product of the separator coating material.
[0172] The manufacturing method of the above concrete structure (first concrete structure) preferably comprises the steps of (1A) obtaining a concrete structure main body having a separator hole using a separator and a separator cone, and (2A) filling the separator hole of the above concrete structure main body with the above separator hole filler. The manufacturing method of the above concrete structure (first concrete structure) preferably comprises the step of (3A) hardening the resin (or the cement milk or the mortar) in the separator hole filler. Note that the step (3A) may or may not be performed.
[0173] The manufacturing method of the concrete structure (first concrete structure) may include the following steps: (1A) a step of obtaining a concrete structure main body having a separator hole using a separator and a separator cone, (2B) a molding step of forming a filler (protective cap) by extrusion molding or injection molding the separator hole filler, and (3B) a placement step of placing the filler (protective cap) in the separator hole of the concrete structure main body.
[0174] The method of filling the separator hole filler into the filling target portion (separator hole) is not particularly limited. Examples of the method of filling the separator hole filler into the filling target portion (separator hole) include a method of embedding with a spatula and a method of filling (injecting) with a gun. The injection amount of the separator hole filler can be appropriately changed depending on the size of the filling target portion (separator hole), etc.
[0175] The manufacturing method of the above concrete structure (second concrete structure) preferably comprises the following steps: (1C) a step of using a separator body to obtain a concrete structure with an exposed end of the separator body; (2C) a step of using the above-mentioned separator coating material to place the separator coating material on the end (on the surface) of the separator body of the concrete structure with the exposed end of the separator body; and (3C) a step of hardening the resin (or the cement milk or the mortar) in the separator coating material. Note that step (3C) may or may not be performed.
[0176] It is also preferable that the manufacturing method of the above concrete structure (second concrete structure) comprises the following steps: (1D) a step of arranging a separator coating material on the surface of the separator body; (2D) a step of hardening the resin (or the cement milk or the mortar) in the separator coating material; and (3D) a step of using a concrete structure body and the separator to obtain a concrete structure in which the separator is arranged inside the concrete structure body. Note that step (2D) may or may not be performed.
[0177] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0178] The following materials were prepared:
[0179] (resin) Curable resin A (two-component curing epoxy resin, "Infraguard CRJ" manufactured by Sekisui Chemical Co., Ltd., 50% by weight of base material: 50% by weight of curing agent) Curable resin B (one-liquid modified silicone resin, Konishi's "Bond modified silicone caulk") Thermoplastic resin (ethylene-vinyl acetate copolymer, Tosoh Corporation's "EVA Ultrathene #636")
[0180] (mortar) Cement (Pacific Cement Corporation "ordinary Portland cement") 100 parts by weight Fine aggregate (silica sand No. 6) 300 parts by weight 60 parts by weight of water for kneading
[0181] (Ion-releasing compound) Compounds capable of releasing cations: Calcium acetate (Fujifilm Wako Pure Chemical Industries, average particle size 10 μm) Calcium formate (Asahi Chemical Industry Co., Ltd., powder) Calcium lactate (Nacalai Tesque, average particle size 50 μm) Barium lactate (Fujifilm Wako Pure Chemical Industries, powder) Compounds capable of releasing anions: Sodium bicarbonate (Fujifilm Wako Pure Chemical Industries, average particle size 107 μm) Sodium carbonate (manufactured by Fujifilm Wako Pure Chemical Industries, average particle size 100 μm) Sodium hydrogen phosphate (Fujifilm Wako Pure Chemical Industries, powder) Sodium silicate (Nacalai Tesque's "Sodium orthosilicate (Na4SiO4)")
[0182] Preparation of filler for separator holes: Example 1 A separator hole filler was obtained by mixing 100 parts by weight of curable resin A, 30 parts by weight of calcium acetate, and 30 parts by weight of sodium hydrogen carbonate.
[0183] (Examples 2 to 4 and Comparative Example 1) A separator hole filler was obtained in the same manner as in Example 1, except that the types and contents of the blended components of the separator hole filler were changed as shown in Tables 1 and 3.
[0184] Example 5 1.5 parts by weight of calcium formate, 1.5 parts by weight of sodium carbonate, and 3 parts by weight of hardening resin A were mixed, and the mixture was coated to a thickness of 1 mm, and then hardened to obtain a plate-shaped hardened product. This plate-shaped hardened product was freeze-pulverized to obtain a powder with an average particle size of 50 μm. 6 parts by weight of the obtained powder was mixed with 100 parts by weight of mortar to obtain a separator hole filler.
[0185] Preparation of specimen 1: A separator (Kondotec's "B-type separator") and a separator cone (Kondotec's "plastic cone") were placed between the concrete forms, and concrete was poured. The concrete was left to harden for 28 days, and then the concrete form and separator cone were removed to form a separator hole. Thereafter, the separator hole fillers obtained in Examples 1 to 5 and Comparative Example 1 were filled, and the separator hole fillers were left to harden for 28 days. A crack was then made in the bottom of the separator hole, and test specimen 1 was obtained.
[0186] Preparation of separator coating material: Example 6 A separator coating material was obtained by mixing 100 parts by weight of the curable resin A and 50 parts by weight of sodium hydrogen carbonate.
[0187] (Example 7 and Comparative Example 2) Separator coating materials were obtained in the same manner as in Example 6, except that the types and amounts of the components in the separator coating material were changed as shown in Tables 2 and 3.
[0188] Example 8 100 parts by weight of a thermoplastic resin, 25 parts by weight of calcium formate, and 50 parts by weight of sodium carbonate were melt-mixed in an extruder, extruded, and pelletized to obtain a pellet-shaped separator coating material.
[0189] Example 9 A pellet-shaped separator coating material was obtained in the same manner as in Example 8, except that 100 parts by weight of a thermoplastic resin, 50 parts by weight of calcium lactate, and 50 parts by weight of sodium carbonate were used.
[0190] Preparation of specimen 2: The separator coating materials obtained in Examples 6 to 7 and Comparative Example 2 were applied to a thickness of 0.3 mm on the surface of the central portion of a separator body ("B-type separator" manufactured by Kondotec Co., Ltd.) when the separator body was divided into three equal parts in the longitudinal direction. The separator with the separator coating material applied thereto was placed between concrete forms, and concrete was poured. The concrete was left to stand for 28 days to harden, and then the concrete forms were removed. Then, cracks were made in the concrete around the separator to obtain Test Specimen 2. Test Specimen 2 was obtained in the same manner as in Examples 6 to 7 and Comparative Example 2, except that the separator coating materials obtained in Examples 8 to 9 were melt-applied using a hot melt gun.
[0191] (evaluation) (1) Viscosity The viscosity of the obtained separator hole filling material at 23° C. and 20 rpm and at 23° C. and 2 rpm were measured by the above-mentioned method. In addition, the ratio (viscosity at 23° C. and 2 rpm / viscosity at 23° C. and 20 rpm) was calculated.
[0192] (2) Waterproof The obtained specimens 1 and 2 were immersed in a water tank for one month so that the cracked areas were in contact with the water. The cracks and the surrounding surfaces of specimens 1 and 2 were visually observed in detail to see whether particles had precipitated. The specimens on which particles had precipitated were observed using a scanning electron microscope, and the solubility of the particles in water at 20°C was measured using the method described above.
[0193] [Waterproofing criteria] ○: Poorly water-soluble salt is formed ×: No poorly water-soluble salt was produced
[0194] In Examples 1, 2, 5, 6, 8, and 9, calcium carbonate (solubility in water at 20° C.: 1.5×10 -4 In Example 3, calcium phosphate (solubility in water at 20° C.: 6.5×10 -5 In Example 4, calcium silicate (solubility in water at 20° C.: 5.8×10 mol / L) was produced as a poorly water-soluble salt. -4 In Example 7, barium carbonate (solubility in water at 20° C.: 1.25×10 -4 mol / L) was produced.
[0195] The compositions of the separator hole filler and separator coating material, as well as the results, are shown in Tables 1 to 3 below.
[0196] [Table 1]
[0197] [Table 2]
[0198] [Table 3] [Explanation of symbols]
[0199] 1,1A…Concrete structure 11...Filling material 12,12A…Separator 12Aa…Separator body 12Ab…Coating material 13, 13A…Concrete structure body 13a, 13Aa…Separator hole
Claims
1. It is a filler used for separator holes in concrete structures. The present invention includes an ion-releasing compound capable of releasing cations or anions, and a resin, cement milk, or mortar, The ion-releasing compound is capable of generating a poorly water-soluble salt, and the separator hole filler.
2. The separator hole filler according to claim 1 , wherein the poorly water-soluble salt is calcium carbonate, barium carbonate, calcium phosphate, or iron hydroxide.
3. the ion-releasing compound comprises a compound capable of releasing a cation, The filler for a separator hole according to claim 1 or 2, wherein the compound capable of releasing cations is calcium silicate, tricalcium silicate, dicalcium silicate, calcium aluminate, calcium aluminoferrite, calcium hydroxide, calcium oxide, calcium acetate, calcium lactate, barium lactate, calcium sulfate, calcium chloride, calcium nitrate, or calcium bicarbonate.
4. the ion-releasing compound comprises a compound capable of releasing anions, 3. The separator hole filler according to claim 1 or 2, wherein the compound capable of releasing anions is sodium hydrogen phosphate, potassium carbonate, potassium bicarbonate, ammonium carbonate, ammonium bicarbonate, sodium carbonate, sodium bicarbonate, or calcium bicarbonate.
5. The separator hole filler according to claim 1 or 2, wherein the resin comprises an epoxy resin or a modified silicone resin.
6. 3. The separator hole filler according to claim 1, having a viscosity of 2,000 mPa·s or more and 50,000 mPa·s or less at 23° C. and 20 rpm.
7. 3. The separator hole filler according to claim 1 or 2, wherein the ratio of the viscosity at 23° C. and 2 rpm to the viscosity at 23° C. and 20 rpm is 3.0 or more and 8.0 or less.
8. Obtaining a concrete structure body having a separator hole using a separator and a separator cone; and filling the separator hole filler according to claim 1 or 2 into the separator hole of the concrete structure body.
9. A concrete structure body having a separator hole; A filler material is filled in the separator hole of the concrete structure body, A concrete structure, wherein the filler is formed from the separator hole filler according to claim 1 or 2.
10. A coating material used for separators in concrete structures, The present invention includes an ion-releasing compound capable of releasing cations or anions, and a resin, cement milk, or mortar, The separator coating material, wherein the ion-releasing compound is capable of generating a poorly water-soluble salt.
11. The separator coating material according to claim 10, wherein the resin comprises an epoxy resin, a vinyl ester resin, an unsaturated polyester resin, or a polyolefin resin.
12. A separator body; a coating material disposed on a surface of the separator body; A separator, wherein the coating material is formed from the coating material for a separator according to claim 10 or 11.
13. A concrete structure body and a separator disposed inside the concrete structure body, the separator comprises a separator body and a coating material disposed on a surface of the separator body; A concrete structure, wherein the coating material is formed from the coating material for a separator according to claim 10 or 11.
Citation Information
Patent Citations
Concrete form separator protector and construction method thereof
JP2011127329A