Manufacturing method of composite active material for lithium ion secondary battery
The method of pulverizing silicon raw material with an aqueous solvent and polymer coating in the production of silicon-based composite active materials for lithium ion secondary batteries addresses the inefficiencies of conventional methods by reducing process length and costs, ensuring structural stability during charging and discharging.
Patent Information
- Application Number
- JP2023071183
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional methods for manufacturing silicon-based composite active materials for lithium ion secondary batteries require a lengthy process and expensive alkoxide, increasing manufacturing costs.
A method involving pulverization of silicon raw material using an aqueous solvent, followed by polymer coating and precursor coating, which allows for the production of a composite active material with amorphous carbon having voids, where the silicon-based material is present, without the need for expensive alkoxide.
This method reduces the manufacturing process length and costs while maintaining the structural integrity of the composite active material, allowing it to accommodate volume changes during charging and discharging without collapsing.
Smart Images

Figure 2024157078000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a composite active material for a lithium ion secondary battery. [Background technology]
[0002] As a silicon-based negative electrode active material for lithium ion secondary batteries in which volume change during charging and discharging is suppressed, composite active materials have been investigated that are composed of a silicon-based material, such as metallic silicon or a silicon compound, and a carbon material, in which the silicon-based material is contained in the carbon material and has a structure in which there is a gap between the silicon-based material and the carbon material (Patent Document 1).
[0003] The composite active material disclosed in Patent Document 1 achieves such a structure by removing the polystyrene from polystyrene-coated silicon through firing; however, in order to coat the silicon with polystyrene, it was necessary to modify the surface of the silicon.
[0004] Therefore, in Patent Document 1, the silicon surface is modified by surface modification through hydrolysis of tetraethoxysilane (hereinafter also referred to as "TEOS") after crushing using alcohol such as methanol or ethanol or a hydrocarbon solvent such as hexane or toluene as a solvent. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication 2021 / 193662 [Patent Document 2] JP2015-195171A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the polystyrene coating in the manufacturing method disclosed in Patent Document 1 requires a pulverization step prior to the polystyrene coating and the use of an expensive alkoxide, which not only requires a long process length but also results in high manufacturing costs.
[0007] In view of the above circumstances, an object of the present disclosure is to provide a method for producing a composite active material for lithium-ion secondary batteries, which has a structure in which the length of production steps is shorter than in conventional methods for producing composite active materials, does not require expensive raw materials, and is made of a silicon-based material and a carbon material, the silicon-based material is contained in the carbon material, and the silicon-based material is present in voids between the silicon-based material and the carbon material. [Means for solving the problem]
[0008] In this disclosure, the relationship between the surface state of a silicon-based material and the manufacturing process in the manufacture of a composite active material made of a silicon-based material and a carbon material was examined. As a result, it was found that a silicon-based material having a surface state suitable for polymer coating can be obtained by carrying out a treatment that was previously considered unsuitable.
[0009] That is, the present invention is as described in the claims, and the gist of the present disclosure is as follows. [1] A method for producing a composite active material for a lithium ion secondary battery, comprising: a grinding step of grinding a silicon raw material consisting of at least one of metal silicon and a silicon compound using an aqueous solvent to obtain a ground silicon raw material; a polymer coating step of coating the ground silicon raw material with a polymer to obtain a polymer-coated silicon raw material; a precursor coating step of coating the polymer-coated silicon raw material with a carbon precursor to obtain a precursor-coated silicon raw material; and a calcination step of calcining the precursor-coated silicon raw material, the method comprising the steps of: [2] The method for producing a composite active material for a lithium ion secondary battery according to [1] above, wherein the aqueous solvent is distilled water. [3] The method for producing a composite active material for a lithium ion secondary battery according to the above [1] or [2], wherein the silicon raw material is metallic silicon. [4] The method for producing a composite active material for a lithium ion secondary battery according to [3] above, wherein the purity of the metallic silicon is 98 mass % or more. [5] The method for producing a composite active material for a lithium ion secondary battery according to any one of [1] to [4] above, wherein the pulverization method in the pulverization step is by using a bead mill. [6] The method for producing a composite active material for a lithium ion secondary battery according to any one of [1] to [5] above, wherein the silicon raw material has an average particle size (D50) of 0.01 μm or more and 5 μm or less. [7] The method for producing a composite active material for a lithium-ion secondary battery according to any one of the above [1] to [6], wherein the method for coating the polymer-coated silicon raw material with a carbon precursor in the precursor coating step is a method for polymerizing a monomer of the carbon precursor on the surface of the polymer-coated silicon raw material. [8] The method for producing a composite active material for a lithium-ion secondary battery according to the above item [7], wherein the method for polymerizing the carbon precursor monomer on the surface of the polymer-coated silicon raw material is a method for mixing the polymer-coated silicon raw material with a solution containing a solvent, the carbon precursor monomer, and a polymerization initiator. [9] The method for producing a composite active material for a lithium-ion secondary battery according to any one of the above [1] to [8], further comprising, after the precursor-coating step, a drying step of drying the precursor-coated silicon raw material, and a spheronizing step of shaping the precursor-coated silicon raw material of the drying step. Effect of the Invention
[0010] The present disclosure can provide a method for producing a composite active material for lithium ion secondary batteries that is made of a silicon-based material and a carbon material, has a structure in which the silicon-based material is contained in the carbon material and is present in voids between the silicon-based material and the carbon material, and that can reduce the process length and costs. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a schematic diagram showing a cross section of the present composite active material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] [Method of manufacturing composite active material for lithium-ion secondary batteries] Hereinafter, the present disclosure will be described with reference to an example of an embodiment.
[0013] The present embodiment is a method for producing a composite active material for lithium ion secondary batteries, which includes a grinding step of grinding a silicon raw material consisting of at least one of metal silicon and a silicon compound using an aqueous solvent to obtain a ground silicon raw material, a polymer coating step of coating the ground silicon raw material with a polymer to obtain a polymer-coated silicon raw material, a precursor coating step of coating the polymer-coated silicon raw material with a carbon precursor to obtain a precursor-coated silicon raw material, and a firing step of firing the precursor-coated silicon raw material. This allows the production of a composite active material for lithium ion secondary batteries (hereinafter referred to as "the composite active material") that contains a silicon-based material and amorphous carbon, has voids, and is present in the voids, more simply and with fewer steps than conventional production methods.
[0014] The composite active material contains a silicon-based material and amorphous carbon, the amorphous carbon having voids, and the silicon-based material existing in the voids.
[0015] In this embodiment, the silicon-based material is at least one of metallic silicon and a silicon compound, and is preferably metallic silicon. Note that metallic silicon is zero-valent silicon (silicon element).
[0016] The silicon-based material may have the same average particle size (D50) as the pulverized silicon raw material described later. The purity of the metal silicon is not particularly limited, and may be, for example, 98 mass% or more, preferably 2N (99%) or more, and more preferably 4N (99.99%) or more. Although a high purity is preferable, it is sufficient if it is 6N (99.9999%) or less.
[0017] A silicon compound is a compound composed of silicon (Si) and one or more elements other than silicon, and an example of such a compound is silica (SiO2).
[0018] In this embodiment, amorphous carbon refers to carbon having an X-ray diffraction peak half-width of the (002) plane of 3° or more.
[0019] The content of the silicon-based material in the present composite active material is, as the content of silicon relative to the total mass of the silicon-based material and amorphous carbon, 5% by mass or more or 15% by mass or more, and can be 80% by mass or less or 50% by mass or less, and is preferably 5% by mass or more and 80% by mass or less, or 15% by mass or more and 50% by mass or less.
[0020] In this composite active material, the silicon-based material is present in the voids. FIG. 1 shows a schematic diagram of a cross section of this composite active material. In FIG. 1, the composite active material (100) is composed of a silicon-based material (10) and amorphous carbon (11), and the silicon-based material (10) is present in the voids (12) of the amorphous carbon (11). With this structure, even if the silicon-based material expands upon charging, the volume change is limited to within the voids. Therefore, the expansion and contraction of the composite active material itself upon charging and discharging is suppressed, making it less likely to collapse.
[0021] (Water grinding process) This embodiment has a grinding step (hereinafter also referred to as "water grinding step") in which a silicon raw material consisting of at least one of metal silicon and silicon compound is ground using an aqueous solvent to obtain ground silicon raw material. This results in a ground silicon raw material with a hydrophilized surface. Conventionally, it has been considered that the use of an aqueous solvent for grinding silicon raw material is not suitable because the silicon raw material is excessively oxidized (Patent Document 2). Therefore, after grinding with a non-aqueous solvent, it was necessary to hydrophilize the surface by a hydrolysis reaction of an alkoxide such as TEOS. In contrast, in this embodiment, it is considered that the surface of the silicon raw material is modified by using an aqueous solvent as a solvent for grinding, that is, by grinding the silicon raw material in the state of an aqueous slurry. This allows the surface modification and grinding to be performed in a single step, and the present composite active material can be manufactured more simply and with fewer steps than conventional manufacturing methods. Furthermore, this allows the surface modification of the silicon raw material without the necessity of expensive alkoxides.
[0022] The silicon raw material to be subjected to the water grinding step may be at least one of metal silicon and silicon compounds similar to the above-mentioned silicon-based materials, except that the average particle size (D50) is 0.01 μm or more and 5 μm or less, and is preferably metal silicon. The average particle size (D50) of the silicon material may be 0.01 μm or more, 0.1 μm or more, or 1 μm or less, and may be 5 μm or less, 4 μm or less, or 3 μm or less, and is preferably 0.01 μm or more and 5 μm or less, 0.1 μm or more and 4 μm or less, or 1 μm or more and 3 μm or less.
[0023] In this embodiment, the average particle size (D50) is a particle size corresponding to a cumulative 50% volume diameter (median diameter) in a volume particle size distribution curve measured using a general laser diffraction / scattering type particle size distribution measuring device (e.g., SALD7100, manufactured by Shimadzu Corporation) under the following conditions:
[0024] Light source: Semiconductor laser Measurement cell: Batch cell Solvent: Ethanol Refractive index: 3.20
[0025] The "aqueous solvent" used in the water grinding step may be any solvent in which the proportion of water (HO) in the solvent composition is greater than that of the organic solvent. Specifically, the solvent may be one or more selected from the group consisting of distilled water, deionized water, and pure water, and distilled water is preferred.
[0026] In the water grinding step, the silicon raw material is ground using an aqueous solvent, that is, a slurry consisting of the silicon raw material and an aqueous solvent (hereinafter also referred to as "silicon raw material slurry") is ground. Therefore, the grinding in the grinding step is so-called wet grinding, and it is preferable that the wet grinding is carried out using a grinding medium such as grinding beads.
[0027] The material of the grinding medium in the wet grinding is not particularly limited as long as it can grind the silicon raw material, and examples thereof include one or more selected from the group consisting of zirconia, alumina, tungsten oxide and stainless steel, and preferably zirconia.
[0028] The concentration of the silicon raw material in the silicon raw material slurry, expressed as the mass ratio of the silicon raw material to the mass of the silicon raw material slurry, is, for example, 0.01 mass% or more or 1 mass% or more, and 50 mass% or less or 30 mass% or less, and is preferably 0.01 mass% or more and 50 mass% or less, or 1 mass% or more and 30 mass% or less.
[0029] In the water grinding step, the ground silicon raw material is ground so that its average particle size (D50) is 0.005 μm or more and less than 5 μm, more preferably 0.01 μm or more and 1 μm or less, and even more preferably 0.05 μm or more and 0.6 μm or less. Such a particle size makes it difficult for the charge capacity and the initial charge / discharge efficiency to decrease due to surface oxidation during charging and discharging, and also makes it difficult for the composite active material particles to crack due to volume change caused by insertion of lithium ions during charging and discharging.
[0030] The wet grinding time is not particularly limited as long as the ground silicon raw material of the desired particle size is obtained, and the longer the grinding time, the smaller the average particle size (D50) tends to be until equilibrium is reached. The wet grinding time may be appropriately adjusted depending on the amount of silicon raw material slurry to be treated and the grinding method, and may be, for example, 6 hours or more and 30 hours or less.
[0031] The method of wet grinding is not particularly limited as long as it can grind the silicon raw material to a desired particle size, and examples thereof include one or more selected from the group consisting of a ball mill, a bead mill, a roll mill, a colloid mill, and a high-pressure wet opposed collision type disperser, and a bead mill is preferred.
[0032] After the treatment in the water grinding step, the mixture may be stirred at a temperature of 40°C or higher and 100°C or lower.
[0033] (Polymer coating process) The manufacturing method of this embodiment includes a polymer coating step of coating a pulverized silicon raw material with a polymer to obtain a polymer-coated silicon raw material. The polymer coating step produces a pulverized silicon raw material having a polymer on at least a part, preferably the entire, surface of the pulverized silicon raw material ("polymer-coated silicon raw material"). The firing step described below causes the coated polymer to pyrolyze, resulting in a composite active material having a structure with voids.
[0034] A preferred coating method in the polymer coating step is to mix the pulverized silicon raw material with a solution containing a solvent, a monomer and a polymerization initiator (hereinafter, also referred to as a "coating solution").
[0035] The solvent may be any solvent that does not inhibit the polymerization reaction of the monomer, and examples thereof include one or more selected from the group consisting of water, ethanol, methanol, isopropyl alcohol, propanol, and toluene, and preferably one or more selected from the group consisting of water, ethanol, and methanol.
[0036] The polymer coated on the pulverized silicon raw material may be any polymer that is thermally decomposed by the firing step described below, and examples thereof include one or more selected from the group consisting of polystyrene, polymethyl methacrylate, polymethyl acrylate, and polyacrylonitrile, with polystyrene being preferred.
[0037] The monomer may be any monomer that serves as a precursor of the polymer, and examples thereof include one or more selected from the group consisting of styrene, methyl methacrylate, methyl acrylate, and acrylonitrile, with styrene being preferred.
[0038] The polymerization initiator may be any one that dissolves in a solvent and generates radicals capable of initiating polymerization of a monomer, and examples thereof include one or more selected from the group consisting of azobisisobutyronitrile, potassium persulfate, and ammonium persulfate.
[0039] In order to improve the dispersibility of the pulverized silicon raw material, the coating solution may contain a dispersant, such as one or more selected from the group consisting of polyacrylic acid dispersants, styrene sulfonic acid dispersants, and polyvinylpyrrolidone, with styrene sulfonic acid dispersants being preferred.
[0040] The processing conditions in the polymer coating step are arbitrary as long as the polymer can be coated on at least a portion of the surface of the pulverized silicon raw material by polymerization of the monomer. For example, the polymerization temperature may be 20°C or higher or 50°C or higher, and 100°C or lower or 80°C or lower, and is preferably 20°C or higher and 100°C or lower, or 50°C or higher and 80°C or lower.
[0041] The polymer-coated silicon raw material obtained by the polymer coating step may have at least a portion of the surface of the pulverized silicon raw material coated with a polymer, and it is preferable that the entire surface of the pulverized silicon raw material is coated with a polymer.
[0042] (Precursor coating process) The manufacturing method of this embodiment includes a precursor coating step of coating a polymer-coated silicon raw material with a carbon precursor to obtain a precursor-coated silicon raw material. The precursor coating step produces a polymer-coated silicon raw material having a carbon precursor on at least a part, preferably the entire, surface of the raw material (the "precursor-coated silicon raw material"). The carbon precursor is converted to amorphous carbon by the firing step described below, and the composite active material is obtained.
[0043] Preferred methods for coating a polymer-coated silicon raw material with a carbon precursor include at least one of a method of polymerizing a monomer of a carbon precursor on the surface of the polymer-coated silicon raw material (hereinafter also referred to as a "polymerization coating method") and a method of mixing a polymer-coated silicon raw material with a carbon precursor (hereinafter also referred to as a "mixed coating method"), with the polymerization coating method being preferred.
[0044] The carbon precursor may be any polymeric compound that becomes amorphous carbon through a firing step described below, and examples of the carbon precursor include one or more selected from the group consisting of polyaniline, polypyrrole, polyacrylonitrile, polyvinyl alcohol, and phenol resin. Since denser amorphous carbon is more likely to be obtained, the carbon precursor is preferably polyacrylonitrile.
[0045] The monomer of the carbon precursor to be subjected to the polymerization coating method may be any monomer that becomes a carbon precursor on the surface of the polymer-coated silicon-based material by polymerization or coating, and may be, for example, one or more selected from the group consisting of aniline, pyrrole, acrylonitrile, vinyl alcohol, and phenol. The monomer of the carbon precursor is preferably acrylonitrile, since this makes it easier to obtain denser amorphous carbon.
[0046] The method of coating the carbon precursor in the polymerization coating method may be any method in which the monomer of the carbon precursor is polymerized on the surface of the polymer-coated silicon raw material, and is preferably a method of mixing the polymer-coated silicon raw material with a solution containing a solvent, a monomer of the carbon precursor, and a polymerization initiator (hereinafter also referred to as a "precursor coating solution"). In order to improve the dispersibility of the polymer-coated silicon raw material, the precursor coating solution may contain a dispersant. Also, the solvent, polymerization initiator, and dispersant of the polymer coating process can be used.
[0047] In the mixed coating method, the polymer-coated silicon raw material and the carbon precursor are mixed. In the mixed coating method, the method of mixing the polymer-coated silicon raw material and the carbon precursor may be any method that allows the two to be mixed uniformly, and includes at least one of dry mixing and wet mixing, and wet mixing is preferred.
[0048] The dry mixing may be performed by mixing the polymer-coated silicon raw material and the carbon precursor. For example, mixing may be performed using at least one of a mortar mixer, a ball mill, and a bead mill, with mixing using a ball mill being preferred.
[0049] The wet mixing may be performed by mixing the polymer-coated silicon raw material, the carbon precursor, and the solvent (hereinafter, also referred to as a "precursor mixed solution"). For example, mixing may be performed using at least one of a magnetic stirrer, a three-one motor, and a homomixer, and mixing using a three-one motor is preferred.
[0050] The solvent used in the wet mixing is not particularly limited, but may be, for example, one or more selected from the group consisting of water, ethanol, and methanol, and is preferably one or more selected from the group consisting of water and ethanol.
[0051] (drying process) The manufacturing method of this embodiment may include a step of drying the precursor-coated silicon feedstock (hereinafter, also referred to as a "drying step"). The drying step tends to improve the moldability of the precursor-coated silicon feedstock.
[0052] The drying method may be at least one selected from the group consisting of centrifugation, standing, heating and reduced pressure, and is preferably heating. For example, a heating method may be a method of drying by heating using a spray dryer.
[0053] The heating temperature may be any temperature at which the solvent and physically adsorbed water can be removed, and may be 30°C or more or 100°C or more, and 300°C or less or 250°C or less, and is preferably 30°C or more and 300°C or less, or 100°C or more and 250°C or less.
[0054] The heating atmosphere is not particularly limited as long as it does not affect the precursor-coated silicon raw material, and is preferably, for example, one or more atmospheres selected from the group consisting of air, nitrogen, argon, and helium.
[0055] The drying atmosphere may be a flow atmosphere.
[0056] (Spheronization process) The manufacturing method of this embodiment may include a step of forming the precursor-coated silicon feedstock (hereinafter, also referred to as a "spheroidizing step"). The precursor-coated silicon feedstock can be formed into any shape by the spheroidizing step.
[0057] The shape of the precursor-coated silicon raw material after molding is not particularly limited as long as it allows the production of a lithium ion secondary battery, and from the viewpoint of the powder packing density, at least one of a sphere and an approximately sphere is preferable. Note that the approximately sphere does not necessarily have to be an ideal sphere (a perfect sphere), and examples thereof include an elliptical sphere, a sphere with a chipped part, a distorted sphere, and a sphere with an uneven surface.
[0058] The spheronization step may be any step that can mold the precursor-coated silicon raw material into any shape, and may involve the use of impact force, for example, a method that uses impact force generated by the rotation of a rotor.
[0059] The rotation speed of the rotor is 40 m / s or more, or 60 m / s or more, and can be 120 m / s or less, or 100 m / s or less, and is preferably 40 m / s or more and 120 m / s or less, or 60 m / s or more and 100 m / s or less.
[0060] The treatment time may be any time required for the precursor-coated silicon raw material to assume the desired shape, and may be set appropriately depending on the amount of precursor-coated silicon raw material to be subjected to treatment and the treatment method. For example, the treatment time may be 1 minute or more, or 2 minutes or more, and 20 minutes or less, or 10 minutes or less, and is preferably 1 minute or more and 20 minutes or less, or 2 minutes or more and 10 minutes or less.
[0061] (Firing process) The manufacturing method of this embodiment includes a step of calcining the precursor-coated silicon raw material (hereinafter, also referred to as the "calcination step"). As a result, the polymer present on the surface of the pulverized silicon raw material is thermally decomposed to form voids, and at the same time, the carbon precursor is carbonized to become amorphous carbon, thereby obtaining the present composite active material.
[0062] The firing temperature is 300° C. or more or 600° C. or more, and may be 1500° C. or less or 1100° C. or less, and is preferably 300° C. or more and 1100° C. or less, or 600° C. or more and 1100° C. or less. By setting the firing temperature in this range, the polymer on the surface of the pulverized silicon raw material is more easily removed.
[0063] The rate of temperature rise to the firing temperature is 1° C. / min or more, or 3° C. / min or more, and can be 100° C. / min or less, or 50° C. / min or less, and is preferably 1° C. / min or more and 100° C. / min or less, or 3° C. / min or more and 50° C. / min or less.
[0064] The firing atmosphere is not particularly limited as long as it is an oxygen-free atmosphere, and is, for example, one or more selected from the group consisting of nitrogen, argon, and helium, with nitrogen being more preferred.
[0065] The firing atmosphere may be a flow atmosphere.
[0066] [Composite active materials for lithium-ion secondary batteries] The composite active material for lithium ion secondary batteries obtained by this embodiment (the present composite active material) can be used as an electrode active material for lithium ion secondary batteries, preferably as a negative electrode active material, and can also be used in a negative electrode comprising the present composite active material and in a lithium ion secondary battery comprising the composite active material.
[0067] When the present composite active material is used in a negative electrode or a lithium ion secondary battery, the negative electrode and the lithium secondary battery may be produced by any method except for using the composite active material as a negative electrode active material.
[0068] The negative electrode may be an electrode consisting of a negative electrode mixture containing at least the composite active material, a conductive material, and a binder, and a current collector. The conductive material, binder, and current collector may be any material that can be used in a negative electrode for a lithium ion secondary battery, and examples of the conductive material include one or more selected from the group consisting of conductive carbon black, carbon nanofiber, and carbon nanotube, the binder includes one or more selected from the group consisting of polyvinylidene fluoride, styrene butadiene rubber (SBR), carboxymethyl cellulose, and polyacrylic acid, and the current collector includes one or more selected from the group consisting of nickel foil, aluminum foil, stainless steel foil, and copper foil.
[0069] The lithium ion secondary battery may include at least a positive electrode, a negative electrode, an electrolyte, and a separator. The positive electrode, the electrolyte, and the separator may be any material that can be used in a lithium ion secondary battery. For example, the positive electrode may be LiCoO2, LiNiO2, LiNi 1-y Co y O2, LiNi 1-x-y Co x Al yExamples of the positive electrode active material include an electrode having one or more selected from the group consisting of O2, LiMnO2, LiMn2O4, and LiFeO2 as a positive electrode active material; an electrolyte solution containing one or more selected from the group consisting of ethylene carbonate, propylene carbonate, dimethyl carbonate, and diethyl carbonate as a solvent and one or more selected from the group consisting of LiPF6, LiBF4, LiClO4, and LiCF3SO3 as an electrolyte salt; and a separator made of at least one of polyethylene and polypropylene as a separator. EXAMPLES
[0070] The present disclosure will be described below with reference to examples. However, the present disclosure is not limited to the following examples.
[0071] (Production of lithium-ion secondary batteries) A negative electrode mixture obtained by mixing 92.5 mass % of the composite active material, 0.5 mass % of acetylene black (conductive material), and 7.0 mass % of polycarboxylic acid (binder) was mixed with pure water to obtain a negative electrode mixture slurry.
[0072] The obtained negative electrode mixture slurry was applied onto a copper foil of 150 mm in length and 150 mm in width, and after vacuum drying, it was punched out into a circle of 14 mm in diameter. The copper foil carrying the negative electrode mixture was fed at a speed of 1 m / min and a pressure of 4.0 t / cm 2 After roll pressing under the conditions above, the mixture was dried in a vacuum to obtain a negative electrode for a lithium ion secondary battery.
[0073] Lithium ion secondary batteries for initial evaluation and cycle evaluation were fabricated, each of which contained the obtained negative electrode and had the following configuration.
[0074] <Lithium-ion secondary battery for initial evaluation> Counter electrode: metallic lithium Separator: Polypropylene separator Electrolyte: Solvent Ethylene carbonate:Diethyl carbonate:Fluoroethylene carbonate =1:1:0.04 (volume ratio) Electrolyte: 1.2mol / L lithium hexafluorophosphate Battery type: Screw cell <Lithium-ion secondary battery for cycle evaluation> Counter electrode: metallic lithium Separator: Polypropylene separator Electrolyte: Solvent Ethylene carbonate:Diethyl carbonate:Fluoroethylene carbonate =1:1:0.04 (volume ratio) Electrolyte: 1.2mol / L lithium hexafluorophosphate Battery type: CR2032 coin cell
[0075] (electrode density) The electrode density was calculated based on the following formula (1).
[0076] Electrode density (g / cm 3 ) = {(Mass of negative electrode) - (Mass of copper foil)} / [{(Thickness of negative electrode) - (Thickness of copper foil)} × (area of a circle with a diameter of 14 mm)] (1) The mass and thickness of the copper foil were measured before application of the negative electrode mixture slurry, and the mass and thickness of the negative electrode were measured after roll pressing and vacuum drying.
[0077] (Initial Characterization) The lithium ion secondary battery for initial evaluation was used and charged at a constant current and constant voltage of 0.1 C to 0.005 V in a thermostatic chamber at 25° C., and then charged at a constant voltage of 0.005 V to 0.05 C. The charge capacity at this time was taken as the initial charge capacity.
[0078] In addition, "C" indicates the C rate, and 1.0C is the current value that discharges the theoretical capacity calculated from the following formula (2) in one hour.
[0079] Theoretical capacity (mAh / g) = (theoretical capacity of silicon (4200mAh / g) × silicon content in the composite active material (%)) + (theoretical capacity of carbon (372mAh / g) × carbon content in the composite active material (%)) (2)
[0080] In addition, the thickness of the negative electrode was measured before and after charging, and the initial electrode expansion rate (%) was calculated using the following formula (3).
[0081] Initial electrode expansion rate (%) = {(thickness of negative electrode after charging) - (thickness of copper foil)} / {(thickness of negative electrode before charging) - (thickness of copper foil)} x 100 (3)
[0082] The thickness of the copper foil was measured before applying the negative electrode mixture slurry, the thickness of the negative electrode before charging was measured after roll pressing and vacuum drying, and the thickness of the negative electrode before charging was measured after dismantling and recovering the lithium ion secondary battery for initial evaluation after charging.
[0083] (Cycle characteristic evaluation) A lithium-ion secondary battery for cycle evaluation was used, and in a thermostatic chamber at 25°C, it was charged at a constant current and constant voltage of 0.3 C to 0.01 V, then charged at a constant voltage of 0.01 V until the current value reached 0.03 C, and then discharged at a constant current of 0.5 C until the voltage reached 1.5 V, forming a charge-discharge cycle. The charge-discharge cycle was carried out 100 times, and the capacity retention rate (%) was calculated from the discharge capacity at the first cycle and the discharge capacity at the 100th cycle according to the following formula (4).
[0084] Capacity retention rate (%) = (discharge capacity at 100th cycle) / (1st cycle discharge capacity) × 100 (4)
[0085] Example 1 Preparation of silicon / amorphous carbon composite active material (Water grinding process) Metallic silicon (average particle size D50 = 3 μm) and distilled water were mixed so that the metallic silicon concentration was 17 mass%, and this was ground for 25 hours in a bead mill using zirconia beads with a diameter of 0.3 mm as a grinding medium. Distilled water was then added to produce a ground silicon slurry with a metallic silicon concentration of 11 mass%.
[0086] (Polymer coating process) 75.2 g of pulverized silicon slurry (8.3 g of metallic silicon) and 617 g of distilled water were mixed and substituted with nitrogen. The mixture was then heated to 35° C., 0.32 g of 3-methacryloxypropyltrimethoxysilane was added, and the mixture was stirred at 250 rpm in a nitrogen atmosphere at 35° C. for 1 hour.
[0087] After stirring, 53g of styrene monomer purified using an alumina column of a polymerization inhibitor treatment agent and 10mL of LiSS aqueous solution with a lithium p-styrenesulfonate concentration of 0.60% by mass were added, and the mixture was stirred in a nitrogen atmosphere at 35°C for 2 hours at a rotation speed of 250 rpm. Next, the mixture was heated to 62°C, and 35mL of ammonium persulfate (hereinafter also referred to as "APS") aqueous solution with a concentration of 0.56% by mass was added at a rate of 3.5mL / hr, and the mixture was stirred in a nitrogen atmosphere at 62°C for 15 hours at a rotation speed of 250 rpm. This resulted in a polystyrene-coated silicon slurry.
[0088] (Precursor coating process) 216 g of the polystyrene-coated silicon slurry (2.8 g as polystyrene-coated silicon) was mixed with 546 g of distilled water to obtain a slurry, which was then purged with nitrogen, heated to 35°C, 20 g of acrylonitrile monomer was added, and the mixture was stirred at 250 rpm for 30 minutes at 35°C in a nitrogen atmosphere.
[0089] After stirring, the temperature was raised to 62°C, and 10 mL of an aqueous APS solution with an APS concentration of 2.2% by mass was added. The mixture was then stirred for 10 hours at 62°C in a nitrogen atmosphere, and the precipitate recovered by centrifugation was redispersed in distilled water to obtain a polyacrylonitrile-coated silicon slurry.
[0090] (drying process) The polyacrylonitrile-coated silicon slurry was spray-dried using a three-fluid nozzle type spray dryer under the following conditions to obtain a polyacrylonitrile-coated silicon dry powder.
[0091] Drying temperature: 200℃ (inlet temperature) Slurry spray rate: 20g / min Dry atmosphere: Air circulating atmosphere Air flow rate: 100L / min
[0092] (Spheronizing process) The polyacrylonitrile-coated silicon dry powder was crushed and molded at the same time using a hybridization system (manufactured by Nara Machinery Co., Ltd.) at a peripheral speed of 100 m / s for 3 minutes to obtain a roughly spherical polyacrylonitrile-coated silicon powder.
[0093] (Firing process) The obtained substantially spherical polyacrylonitrile-coated silicon powder was packed into a quartz boat and fired in a tubular furnace under the following conditions.
[0094] Firing method: Normal pressure firing Firing atmosphere: Nitrogen flow atmosphere (gas linear velocity 38 cm / min) Holding temperature: 1100℃ Holding time: 1 hour Heating rate: 5℃ / min
[0095] In this way, a composite active material for a lithium ion secondary battery of this example was obtained.
[0096] Example 2 The crushed silicon slurry obtained in the same manner as in Example 1 was transferred to a round-bottom flask so that the amount of the slurry was 550 g, and the mixture was stirred at 80° C. for 10 hours at a rotation speed of 250 rpm to obtain a hot water-treated silicon slurry.
[0097] The composite active material for a lithium ion secondary battery of this example was obtained in the same manner as in Example 1, except that the obtained hot water-treated silicon slurry was subjected to a polymer coating step.
[0098] Comparative Example 1 (Crushing process) Metallic silicon similar to that in Example 1 was dispersed in ethanol to adjust the metallic silicon concentration to 14 mass %, and then pulverized for 9 hours in a bead mill using zirconia beads with a diameter of 0.3 mm as the pulverizing medium to obtain pulverized silicon slurry.
[0099] (Surface modification process) 120g of pulverized silicon slurry (17.5g of metal silicon), 340g of ethanol, 39g of polycarboxylic acid dispersant, 1.0g of 10mol / L hydrochloric acid, and 140g of distilled water were added and stirred at 250rpm for 30 minutes. After stirring, 35g of TEOS was added, the mixture was heated to 70°C, and stirred at 250rpm for 12 hours to obtain a surface-modified silicon slurry.
[0100] The surface-modified silicon slurry was dispersed in ethanol and then ground for 8 hours in a ball mill using zirconia beads with a diameter of 1.0 mm as the grinding medium. Distilled water was then added to obtain a surface-modified silicon slurry with a surface-modified silicon concentration of 5.2% by mass.
[0101] A composite active material for a lithium ion secondary battery of this comparative example was obtained in the same manner as in Example 1, except that the surface-modified silicon slurry was subjected to the polymer coating step.
[0102] The evaluation results of the composite active materials for lithium ion secondary batteries obtained in the Examples and Comparative Examples are shown in the table below.
[0103] [Table 1]
[0104] As shown in Table 1, the first charge capacity, electrode density, first electrode expansion rate, and 100-cycle capacity retention rate of the examples and comparative examples were all comparable, and the obtained composite active materials for lithium ion secondary batteries all exhibited similar battery characteristics. This confirmed that the manufacturing method of this example allows pulverization and surface modification to be performed in a single step, and also allows the production of a composite active material for lithium secondary batteries without using an alkoxide.
Claims
1. A method for producing a composite active material for a lithium ion secondary battery, comprising: a grinding step of grinding a silicon raw material consisting of at least one of metal silicon and a silicon compound using an aqueous solvent to obtain a ground silicon raw material; a polymer coating step of coating the ground silicon raw material with a polymer to obtain a polymer-coated silicon raw material; a precursor coating step of coating the polymer-coated silicon raw material with a carbon precursor to obtain a precursor-coated silicon raw material; and a calcination step of calcining the precursor-coated silicon raw material, the method comprising the steps of:
2. The method for producing a composite active material for a lithium ion secondary battery according to claim 1 , wherein the aqueous solvent is distilled water.
3. The method for producing a composite active material for a lithium ion secondary battery according to claim 1 or 2, wherein the silicon raw material is metallic silicon.
4. The method for producing a composite active material for a lithium ion secondary battery according to claim 1 or 2, wherein the purity of the metallic silicon is 98 mass % or more.
5. The method for producing a composite active material for a lithium ion secondary battery according to claim 1 or 2, wherein the pulverization method in the pulverization step is a bead mill.
6. 3. The method for producing a composite active material for a lithium ion secondary battery according to claim 1, wherein the silicon raw material has an average particle size (D50) of 0.01 μm or more and 5 μm or less.
7. 3. The method for producing a composite active material for a lithium ion secondary battery according to claim 1, wherein the method for coating the polymer-coated silicon raw material with a carbon precursor in the precursor coating step is a method for polymerizing a monomer of the carbon precursor on a surface of the polymer-coated silicon raw material.
8. 3. The method for producing a composite active material for a lithium ion secondary battery according to claim 1, wherein the method for polymerizing the monomer of the carbon precursor on the surface of the polymer-coated silicon raw material is a method of mixing the polymer-coated silicon raw material with a solution containing a solvent, the monomer of the carbon precursor, and a polymerization initiator.
9. 3. The method for producing a composite active material for a lithium ion secondary battery according to claim 1, further comprising, after the precursor coating step, a drying step of drying the precursor-coated silicon raw material, and a spheronizing step of shaping the precursor-coated silicon raw material of the drying step.
Citation Information
Patent Citations
Negative electrode active material for lithium ion secondary battery and method of manufacturing the same
JP2015195171A
Composite active material for lithium secondary battery, electrode composition for lithium secondary battery, lithium secondary battery electrode, and method for manufacturing composite active material for lithium secondary battery
WO2021193662A1