Manufacturing method for lithium ion secondary battery, and manufacturing supporting device

By estimating and controlling the liquid flow rate of electrode plates to maintain consistent ratios, the method addresses manufacturing variations, ensuring stable performance and reducing waste in lithium ion secondary batteries.

JP2024157450AActive Publication Date: 2024-11-07TOYOTA BATTERY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023071832
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-07
Estimated Expiration
2043-04-25

AI Technical Summary

Technical Problem

Manufacturing variations in positive and negative electrodes lead to inconsistent pore diameter ratios, affecting electrolyte flow characteristics and increasing internal resistance in lithium ion secondary batteries during high-rate charging and discharging.

Method used

A method to stabilize lithium ion secondary battery manufacturing by estimating the liquid flow rate of each manufacturing lot of positive and negative electrode plates, determining electrode pairs with a liquid flow ratio equal to or less than a predetermined threshold, and forming the electrode body from these pairs to maintain consistent electrolyte flow.

Benefits of technology

Stable production of lithium ion secondary batteries with desired performance is achieved by controlling manufacturing variations, reducing the amount of discarded electrode plates, and optimizing electrolyte flow characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157450000001_ABST
    Figure 2024157450000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method for a lithium ion secondary battery, by which a lithium ion secondary battery with desired performance can be manufactured stably, and a manufacturing supporting device for supporting the manufacture.SOLUTION: A manufacturing method for a lithium ion secondary battery includes the steps of: acquiring manufacturing data of each manufacturing lot about a plurality of manufacturing lots of a positive electrode plate and a plurality of manufacturing lots of a negative electrode plate; estimating the amount of liquid flow of each manufacturing lot from the acquired manufacturing data; extracting a pair of manufacturing lots of the positive electrode plate and the negative electrode plate to form an electrode body using the estimated amount of liquid flow of each manufacturing lot, in which the liquid flow ratio corresponding to a ratio of the amount of liquid flow of the manufacturing lot of the negative electrode plate to the amount of liquid flow of the manufacturing lot of the positive electrode plate is a predetermined threshold or less; and forming the electrode body from the extracted pair of manufacturing lots of the positive electrode plate and the negative electrode plate.SELECTED DRAWING: Figure 9
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a manufacturing method and manufacturing support device for a lithium ion secondary battery. [Background technology]

[0002] It is known that in lithium-ion secondary batteries, repeated high-rate charging and discharging at a large current causes a local increase in internal resistance. The increase in internal resistance is thought to occur through the following mechanism. First, the volume of the electrode body changes due to high-rate charging and discharging. This change in the volume of the electrode body causes a flow of electrolyte, such as the outflow of electrolyte from the electrode body and the re-inflow of electrolyte into the electrode body. This flow of electrolyte causes a bias in the salt concentration inside the electrode body, resulting in a local increase in internal resistance.

[0003] An increase in internal resistance leads to a decrease in battery performance. For this reason, various methods for suppressing the increase in internal resistance have been proposed. For example, Patent Document 1 discloses a lithium ion secondary battery that includes a negative electrode mixture layer, a positive electrode mixture layer facing the negative electrode mixture layer with a separator sandwiched therebetween, and an electrolyte, in which the negative electrode mixture layer contains 3% by mass to 7% by mass of hollow silica particles, the average particle diameter of the hollow silica particles is 50 nm to 110 nm, and the average pore diameter of the negative electrode mixture layer is 1.0 times to 1.83 times the average pore diameter of the positive electrode mixture layer.

[0004] The technology described in Patent Document 1 contains hollow silica in the negative electrode composite layer, thereby making the average pore size of the negative electrode closer to that of the positive electrode and reducing the difference in the permeation rate of the electrolyte between the positive and negative electrodes, thereby suppressing the increase in internal resistance that accompanies high-rate charging and discharging. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-66461 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the manufacturing process of the positive electrode and the negative electrode, manufacturing variations are unavoidable. Due to manufacturing variations, the ratio of the average pore diameter of the negative electrode to the average pore diameter of the positive electrode may vary. Therefore, in an electrode body manufactured from a positive electrode and a negative electrode that do not fall within the range of the target average pore diameter ratio, it may not be possible to suppress the increase in internal resistance accompanying high-rate charging and discharging.

[0007] In addition, the flow characteristics of the electrolyte affect many battery performances, and therefore other performances that are affected by the flow characteristics of the electrolyte must be similarly controlled.

[0008] An object of the present invention is to provide a manufacturing method for a lithium ion secondary battery that can stably manufacture lithium ion secondary batteries having desired performance, and a manufacturing support device for supporting the manufacturing method. [Means for solving the problem]

[0009] A method for manufacturing a lithium ion secondary battery according to a first aspect of the present disclosure includes the steps of acquiring manufacturing data for each of a plurality of production lots of positive plate production lots and a plurality of production lots of negative plate production lots, estimating a liquid flow volume for each production lot from the acquired manufacturing data, extracting pairs of the production lot of the positive plate production lot and the production lot of the negative plate production lot that form an electrode body using the estimated liquid flow volume for each production lot, where a liquid flow ratio, which is a ratio of the liquid flow volume of the production lot of the negative plate to the liquid flow volume of the production lot of the positive plate, is equal to or less than a predetermined threshold value, and forming the electrode body from the extracted pair of production lots of the positive plate production lot and the negative plate production lot.

[0010] A manufacturing support device according to a second aspect of the present disclosure is a manufacturing support device that supports the manufacture of lithium-ion secondary batteries, and includes an acquisition unit that acquires manufacturing data for multiple production lots of positive electrode plates and multiple production lots of negative electrode plates, an estimation unit that estimates a liquid flow volume for each production lot from the manufacturing data acquired by the acquisition unit, an extraction unit that uses the liquid flow volumes for each production lot estimated by the estimation unit to extract, as combination candidates, a set of pairs of the production lot of the positive electrode plates and the production lot of the negative electrode plates that form an electrode body, where a liquid flow ratio, which is the ratio of the liquid flow volume of the production lot of the negative electrode plates to the liquid flow volume of the production lot of the positive electrode plates, is equal to or less than a predetermined threshold, and an output unit that outputs the combination candidates extracted by the extraction unit. Effect of the Invention

[0011] According to the present invention, lithium ion secondary batteries with desired performance can be stably manufactured. [Brief description of the drawings]

[0012] [Figure 1] 1 is a perspective view showing an example of a configuration of a lithium-ion secondary battery according to an embodiment of the present invention. [Diagram 2] 1 is a schematic diagram showing an example of the configuration of an electrode body according to an embodiment of the present invention. [Diagram 3] 2 is a flowchart showing an example of a flow of a method for manufacturing a lithium-ion secondary battery according to an embodiment of the present invention. [Figure 4] 1(A) and 1(B) are schematic diagrams illustrating an example of a method for measuring the liquid flow rate. [Diagram 5] 1 is a graph showing the correlation between estimated and measured liquid flow rates. [Figure 6] 1 is a graph showing the relationship between the liquid flow ratio and the high-rate resistance change rate. [Figure 7] 1A to 1C are schematic diagrams illustrating effects achieved by an embodiment of the present invention. [Figure 8] 2 is a block diagram showing an example of an electrical configuration of a manufacturing support device; [Figure 9]4 is a functional block diagram showing an example of a functional configuration of a control unit of the manufacturing support device. FIG. [Figure 10] 10 is a flowchart showing an example of a process flow of a manufacturing support program. [Figure 11] 13 is a flowchart showing an example of the flow of a liquid flow rate calculation process. [Figure 12] FIG. 13 is a schematic diagram showing an example of a display screen of a combination result. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] An embodiment of the present invention will now be described in detail with reference to the drawings.

[0014] <Structure of lithium-ion secondary battery> First, the configuration of the lithium ion secondary battery will be described. Fig. 1 is a perspective view showing an example of the configuration of a lithium-ion secondary battery according to an embodiment of the present invention. As shown in Fig. 1, the lithium-ion secondary battery 10 is configured as a flat rectangular cell battery. The lithium-ion secondary battery 10 includes a rectangular battery case 20 that is open on the upper side, and a lid body 30. The lid body 30 is joined to the battery case 20 by welding or the like. The battery case 20 and the lid body 30 are made of aluminum, an aluminum alloy, or the like.

[0015] A wound electrode assembly 40 and an electrolyte 22 are housed inside the battery case 20. As shown in Fig. 2, the electrode assembly 40 is an electrode plate group composed of a positive electrode plate 42, a negative electrode plate 44, and a separator 46. Each of the positive electrode plate 42, the negative electrode plate 44, and the separator 46 is a long sheet member. The positive electrode plate 42 and the negative electrode plate 44 may be collectively referred to as electrode plates.

[0016] The positive electrode plate 42 includes a positive electrode current collector 42A and a positive electrode active material layer 42B formed on one or both sides of the positive electrode current collector 42A except for the ends. The negative electrode plate 44 includes a negative electrode current collector 44A and a negative electrode active material layer 44B formed on one or both sides of the negative electrode current collector 44A except for the ends. The materials of the electrolyte 22, the positive electrode plate 42, the negative electrode plate 44, and the separator 46 will be described later.

[0017] The positive electrode plate 42 and the negative electrode plate 44 are stacked with a separator 46 interposed therebetween, and wound along the longitudinal direction of each plate. A positive electrode current collector 42A (i.e., a portion where the positive electrode active material layer 42B is not formed) is exposed at one end of the electrode body 40 in the winding axis direction perpendicular to the winding direction. A negative electrode current collector 44A (i.e., a portion where the negative electrode active material layer 44B is not formed) is exposed at the other end of the electrode body 40 in the winding axis direction.

[0018] The lid 30 is provided with a positive terminal 32P and a negative terminal 32N used for charging and discharging power. The positive terminal 32P is joined to a positive current collector 38P, which is joined to a positive current collector 42A of a positive plate 42. The negative terminal 32N is joined to a negative current collector 38N, which is joined to a negative current collector 44A of a negative plate 44. The lid 30 is also provided with a safety valve 34 that opens when the internal pressure of the battery exceeds a predetermined pressure, and a liquid injection port 36 for injecting an electrolyte. The positive terminal 32P, the negative terminal 32N, the positive current collector 38P, and the negative current collector 38N are made of aluminum, aluminum alloy, or the like.

[0019] The positive electrode current collector 42A of the positive electrode plate 42 is, for example, an aluminum foil. The positive electrode active material layer 42B includes, for example, a positive electrode active material, a conductive material, and a binder. The positive electrode active material is, for example, lithium cobalt oxide (LiCoO 2 ), lithium manganate (LiMn 2 O 4 ), lithium nickel oxide (LiNiO 2As the conductive material, for example, acetylene black (AB) can be used. As the binder, for example, polyvinylidene fluoride (PVDF) can be used.

[0020] The negative electrode current collector 44A of the negative electrode plate 44 is, for example, a copper foil. The negative electrode active material layer 44B includes, for example, a negative electrode active material, a binder, and a thickener. The negative electrode active material may be, for example, a powdered carbon material made of graphite. The binder may be, for example, styrene butadiene rubber (SBR). The thickener may be, for example, sodium carboxymethyl cellulose (CMC).

[0021] The electrolyte 22 is a solution in which a supporting salt is contained in a non-aqueous solvent. As the non-aqueous solvent, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), etc. can be used. As the supporting salt, LiPF 6 , LiBF 4 , LiClO 4 , LiAsF 6 , LiCF 3 SO 3 , LiC 4 F 9 SO 3 , LiN(CF 3 SO 2 ) 2 , LiC(CF 3 SO 2 ) 3 Lithium salts such as LiI can be used.

[0022] The separator 46 is a porous insulating film that insulates the positive electrode plate 42 from the negative electrode plate 44 and allows the electrolyte 22 to pass through. As the separator 46, a porous polyolefin film such as a porous polyethylene film or a porous polypropylene film can be used.

[0023] <Method of manufacturing lithium-ion secondary battery> Next, a method for producing a lithium ion secondary battery will be described. FIG. 3 is a flowchart showing an example of the flow of the method for producing a lithium ion secondary battery according to an embodiment of the present invention.

[0024] As shown in Fig. 3, first, the positive electrode material and the negative electrode material are prepared (S10). Next, a kneading step is performed (S12). In the kneading step, the active material, the conductive material, the binder, etc. are mixed for each of the positive electrode material and the negative electrode material to prepare a positive electrode paste and a negative electrode paste. Such a mixture is also called a "composite material."

[0025] Next, a coating step is performed (S14). In the coating step, a positive electrode paste is applied to one or both sides of a positive electrode current collector 42A made of aluminum foil and dried to form a positive electrode active material layer 42B. This results in a positive electrode plate 42. Similarly, a negative electrode paste is applied to one or both sides of a negative electrode current collector 44A made of copper foil and dried to form a negative electrode active material layer 44B. This results in a negative electrode plate 44.

[0026] Next, a pressing step is performed (S16). In the pressing step, the positive electrode plate 42 and the negative electrode plate 44 are pressed to adjust them to a predetermined thickness. After this, the positive electrode plate 42 and the negative electrode plate 44 are cut to a predetermined size.

[0027] Next, an electrode pair determination step is performed (S18). Through steps S10 to S16, multiple production lots of positive electrode plates 42 and multiple production lots of negative electrode plates 44 are obtained. In the electrode pair determination step, multiple production lots of positive electrode plates 42 and multiple production lots of negative electrode plates 44 are paired in pairs to form an electrode body, and multiple pairs of combinations of production lots of positive electrode plates 42 and production lots of negative electrode plates 44 are determined.

[0028] Next, an electrode body forming step is performed (S20). In the electrode body forming step, positive electrode plates 42 and negative electrode plates 44, which have been cut to a predetermined size, are alternately stacked with separators 46 interposed therebetween to form the electrode body 40. The positive electrode plates 42, negative electrode plates 44, and separators 46 are pressed against each other and shaped into a desired shape.

[0029] Next, a cell assembly process is performed (S22). In the cell assembly process, a battery cell is assembled as follows. The positive current collector 38P is welded to the positive current collector 42A of the electrode body 40, and the negative current collector 38N is welded to the negative current collector 44A. The electrode body 40 to which the positive current collector 38P and the negative current collector 38N are attached is housed in the battery case 20. The battery case 20 and the lid 30 are joined by welding. At this stage, the liquid injection port 36 of the lid 30 is still open.

[0030] Next, a cell drying step is performed (S24). In the cell drying step, moisture is removed from the electrode body 40 by heating. Next, an electrolyte injection / hermetically sealing step is performed (S26). In this step, the electrolyte 22 is filled into the battery case 20, and then the injection port 36 is hermetically sealed. In this way, a lithium ion secondary battery 10 is obtained.

[0031] Next, an activation process is performed (S28). In the activation process, the lithium ion secondary battery 10 is initially charged, and then a high-temperature aging process is performed in which the battery is stored at a high temperature for a certain period of time. Finally, an inspection process is performed (S30). In the inspection process, various inspections are performed on the lithium ion secondary battery 10, and the manufacturing process is completed.

[0032] <Electrode pair determination> In this embodiment, the liquid flow rate of each production lot of the positive electrode plate 42 and the negative electrode plate 44 is estimated, and a combination of the production lot of the positive electrode plate 42 and the production lot of the negative electrode plate 44 (i.e., an electrode pair) is determined so that the ratio of the estimated liquid flow rates is equal to or less than a predetermined threshold value. The liquid flow rate of each production lot is estimated from various production data obtained in the production process, so that the production variation is reflected in the liquid flow rate. Then, by determining the electrode pair so that the ratio of the liquid flow rates is equal to or less than a threshold value, it becomes possible to stably produce lithium ion secondary batteries with desired performance regardless of the production variation. A method for determining an electrode pair will be specifically described below.

[0033] (Liquid flow rate) The liquid flow rate is an index that indicates the amount of electrolyte flow, including the outflow of electrolyte from the electrode body and the inflow of electrolyte into the electrode body. The actual value of the liquid flow rate can be measured, for example, as follows. First, as shown in FIG. 4(A), an electrode plate (here, the positive electrode plate 42) and a separator 46 are wound around a cylindrical winding core 52 to prepare a measurement sample 50. The open end of the winding core 52 is blocked with a rubber plug 56. Next, as shown in FIG. 4(B), the measurement sample 50 is housed in a measurement case 54. An O-ring 58 is used to prevent electrolyte from leaking from the gap between the measurement sample 50 and the measurement case 54.

[0034] Next, the electrolyte is injected into the measurement case 54, and the measurement sample 50 is impregnated with the electrolyte. After the impregnation, a predetermined pressure is applied, and the amount of electrolyte flowing out of the measurement sample 50 per unit time is measured. The pressure value is changed in various ways, and the amount of electrolyte flowing out per unit time is measured. Then, a straight line that represents the amount of electrolyte flowing out per unit time against the pressure is obtained, and the slope of this straight line is defined as the "liquid flow amount." The unit of the liquid flow amount obtained by this method is, for example, "g / kPa."

[0035] (Estimated liquid flow rate) In this embodiment, an estimated value of the liquid flow rate is obtained. Hereinafter, the actual measured value of the liquid flow rate is referred to as "liquid flow rate (actual measured value)", and the estimated value of the liquid flow rate is referred to as "liquid flow rate (estimated value)". The liquid flow rate (estimated value) is calculated using an estimation formula prepared for each of the positive electrode and the negative electrode. The estimation formula is a multiple regression formula with the liquid flow rate (estimated value) as the objective variable and each item of the manufacturing data obtained in the manufacturing process as the explanatory variables. The manufacturing data obtained in the manufacturing process includes data representing the manufacturing conditions and physical property data.

[0036] The manufacturing data used in the estimation formula for the negative electrode can include the average particle size (D50) of the negative electrode active material, the coating surface of the negative electrode paste, the weight per unit area, the thickness after pressing, etc. The manufacturing data used in the estimation formula for the positive electrode can include the particle shape and specific surface area of ​​the positive electrode active material, the coating surface of the positive electrode paste, the weight per unit area, the composite density after pressing, etc. Other manufacturing data can include the mixing ratio of each material in the composite, the viscosity of the paste, etc.

[0037] For multiple samples, the liquid flow rate (actual measured value) and manufacturing data are obtained, and a multiple regression equation is fitted using these data to determine the constants and partial regression coefficients of the multiple regression equation. The partial regression coefficients represent the sensitivity to each explanatory variable. In general, fitting a multiple regression equation requires approximately 10 times the number of samples as the number of explanatory variables. The multiple regression equation with the constants and partial regression coefficients determined by fitting is used as an estimated equation. The liquid flow rate (estimated value) is calculated by substituting the manufacturing data into this estimated equation.

[0038] In addition, the validity of the estimation formula may be verified by determining the correlation between the liquid flow rate (estimated value) and the liquid flow rate (actual value). As shown in FIG. 5, the correlation is calculated using the coefficient of determination R, which is the square of the multiple correlation coefficient R between the liquid flow rate (estimated value) and the liquid flow rate (actual value). 2 It can be expressed as the coefficient of determination R 2 The closer to 1, the higher the correlation. 2 If the correlation is 0.5 or more, it can be said that there is sufficient correlation, and the estimation formula is judged to be valid. From the viewpoint of the reliability of the liquid flow rate (estimated value), the coefficient of determination R 2 is preferably 0.7 or more. 2 If is less than 0.5, it is preferable to reset the estimation equation by increasing the number of samples and redoing the fitting, reviewing the explanatory variables, etc.

[0039] (Liquid flow ratio and threshold judgment) The liquid flow ratio is the ratio of the liquid flow rate (estimated value) of the negative electrode plate 44 to the liquid flow rate (estimated value) of the positive electrode plate 42. Conventionally, it has been considered preferable to make the liquid flow rate of the positive electrode plate 42 and the liquid flow rate of the negative electrode plate 44 equal. However, in reality, it is common to design the liquid flow rate of the negative electrode plate 44 to be greater than the liquid flow rate of the positive electrode plate 42. For this reason, in reality, the liquid flow ratio is greater than 1.

[0040] In this embodiment, the upper threshold value of the liquid flow ratio is flexibly set based on the range that is acceptable in terms of performance. For example, the upper threshold value of the liquid flow ratio is determined taking into consideration the degree of increase in internal resistance accompanying high-rate charging and discharging (i.e., "high-rate resistance change rate"). For example, as shown in FIG. 6, the value of the liquid flow ratio corresponding to the allowable upper limit of the high-rate resistance change rate is set as the upper threshold value using the correspondence relationship between the actual values ​​of the liquid flow ratio and the actual values ​​of the high-rate resistance change rate (the straight line represented by the dotted line in FIG. 6).

[0041] For example, as shown by the solid line, if the allowable upper limit of the high-rate resistance change rate is a, the threshold of the liquid flow ratio is 2.00. Also, as shown by the dotted line, if the allowable upper limit of the high-rate resistance change rate is b, the threshold of the liquid flow ratio is 2.65. Then, the electrode pair is determined so that the ratio of the liquid flow rate (estimated value) of the negative electrode plate 44 to the liquid flow rate (estimated value) of the positive electrode plate 42 is equal to or less than the threshold. The threshold of the liquid flow ratio is preferably in the range of 1.5 to 3.0, and more preferably in the range of 2.0 to 2.5.

[0042] 7, a production lot of positive electrode plates 42 having a large liquid flow rate is paired with a production lot of negative electrode plates 44 having a similarly large liquid flow rate. A production lot of positive electrode plates 42 having a medium liquid flow rate is paired with a production lot of negative electrode plates 44 having a similarly medium liquid flow rate. A production lot of positive electrode plates 42 having a small liquid flow rate is paired with a production lot of negative electrode plates 44 having a small liquid flow rate. In this way, in this embodiment, the liquid flow ratio can be made approximately constant regardless of production variations, and lithium ion secondary batteries with desired performance can be stably produced.

[0043] Furthermore, for example, when manufacturing each electrode plate so that the liquid flow rate is a target value, there is a possibility that an electrode plate that does not meet the standard will be generated due to manufacturing variations. Conventionally, the non-standard electrode plate would be discarded. In contrast, in this embodiment, even if the non-standard electrode plate is capable of forming an electrode pair, it can be used to form the electrode body 40. In this way, in this embodiment, the amount of discarded electrode plates can be reduced.

[0044] The above-mentioned electrode pair determination process is performed using a manufacturing support device including a computer. Therefore, the configuration of the manufacturing support device and a manufacturing support program for executing the manufacturing support process in the manufacturing support device will be described below.

[0045] <Manufacturing support equipment> First, the electrical configuration of the manufacturing support device will be described. Fig. 8 is a block diagram showing an example of the electrical configuration of a manufacturing support device 60. As shown in Fig. 8, the manufacturing support device 60 includes a control unit 62, a display unit 76, an input unit 78, a communication unit 80, and a storage unit 82. The control unit 62 is an information processing device such as a computer, and controls the entire device and performs various calculations.

[0046] The control unit 62 includes a CPU (Central Processing Unit) 64, a ROM (Read Only Memory) 66, a RAM (Random Access Memory) 68, a non-volatile memory 70, and an input / output unit (I / O) 72. The CPU 64, the ROM 66, the RAM 68, the memory 70, and the I / O 72 are each connected to one another via a bus 74. The CPU 64 reads a program stored in the storage device and executes the program using the RAM 68 as a work area.

[0047] Each of the display unit 76, the input unit 78, the communication unit 80, and the memory unit 82 is connected to the I / O 72. The display unit 76 is a display device such as a display. The input unit 78 is an input device such as a keyboard, a mouse, or a touch input device. The communication unit 80 is a communication interface (I / F) for connecting to a communication line. The memory unit 82 is an external storage device such as a hard disk. In this embodiment, a "manufacturing support program" to be described later and various data are stored in the memory unit 82. The various data stored in the memory unit 82 include an estimation formula for the liquid flow volume, a threshold value for the liquid flow ratio, and the like.

[0048] Next, the functional configuration of the control unit 62 will be described. 9 is a functional block diagram showing an example of the functional configuration of the control unit 62 of the manufacturing support device 60. As shown in FIG. 9, the control unit 62 includes an acquisition unit 90 that acquires manufacturing data for each of a plurality of manufacturing lots of positive electrode plates and a plurality of manufacturing lots of negative electrode plates, an estimation unit 92 that estimates the liquid flow amount of each manufacturing lot from the manufacturing data acquired by the acquisition unit 90, an extraction unit 94 that extracts pairs of manufacturing lots of positive electrode plates and negative electrode plates forming an electrode body, in which the liquid flow ratio, which is the ratio of the liquid flow amount of the manufacturing lot of the negative electrode plates to the liquid flow amount of the manufacturing lot of the positive electrode plates, is equal to or less than a predetermined threshold value, using the liquid flow amount of each manufacturing lot estimated by the estimation unit 92, and an output unit 96 that outputs pairs in which the liquid flow ratio extracted by the extraction unit 94 is equal to or less than a predetermined threshold value. Each of these functional units is realized by the CPU 64 of the control unit 62 executing a "manufacturing support program" described later.

[0049] <Manufacturing Support Program> Next, a "manufacturing support program" for executing the manufacturing support process will be described. 10 is a flowchart showing an example of the processing flow of the manufacturing support program. The "manufacturing support program" is executed by the CPU 64 of the control unit 62. The "manufacturing support program" is started when manufacturing data is input by operating the input unit 78 and an instruction to extract combination candidates is given via a reception screen (not shown) displayed on the display unit 76.

[0050] In the flowchart, reference numerals are omitted other than those for the components of the manufacturing support device 60. Furthermore, the manufacturing lot of the positive electrode plates 42 is abbreviated as "positive electrode lot", and the manufacturing lot of the negative electrode plates 44 is abbreviated as "negative electrode lot".

[0051] First, in step S100, the CPU 64 acquires manufacturing data. The manufacturing data for all samples of the positive electrode lot and the negative electrode lot is acquired and temporarily stored in the RAM 68. Next, in step S102, the CPU 64 executes a "liquid flow rate estimation process."

[0052] Here, the "liquid flow volume estimation process" will be described with reference to FIG. First, in step S200, the CPU 64 selects one sample. Next, in step S202, the CPU 64 determines whether the selected sample is a positive electrode lot. If the selected sample is a positive electrode lot, the process proceeds to step S204. Next, in step S204, the CPU 64 reads out an estimation equation for the positive electrode from the storage unit 82. On the other hand, if the selected sample is a negative electrode lot, the process proceeds to step S206. Next, in step S206, the CPU 64 reads out an estimation equation for the negative electrode from the storage unit 82.

[0053] Next, in step S208, the CPU 64 acquires manufacturing data of the selected sample. Next, in step S210, the CPU 64 calculates the liquid flow rate (estimated value) of the sample using the manufacturing data of the sample and the estimation formula. Next, in step S212, the CPU 64 determines whether or not there is a next sample. If there is a next sample, the process returns to step S200. On the other hand, if there is no next sample, the routine ends. That is, the processes from step S200 to step S212 are repeated until the liquid flow rates (estimated values) are calculated for all samples.

[0054] Returning to the description of FIG. 10, next, in step S104, the CPU 64 calculates the liquid flow ratio of all electrode pairs of positive electrode lots and negative electrode lots. Next, in step S106, the CPU 64 acquires all combinations of positive electrode lots and negative electrode lots. Next, in step S108, the CPU 64 excludes combinations including electrode pairs whose liquid flow ratios are greater than a threshold value. Next, in step S110, the CPU 64 displays the remaining combinations of positive electrode lots and negative electrode lots on the display unit 76 as combination candidates.

[0055] Here, steps S104 to S110 will be described using a specific example. Here, an example will be described in which combinations of positive electrode lots A, B, and C and negative electrode lots D, E, and F are obtained. In this case, there are nine electrode pairs in total: (A, D), (A, E), (A, F), (B, D), (B, E), (B, F), (C, D), (C, E), and (C, F). The liquid flow ratio is calculated for each electrode pair.

[0056] And there are six possible combinations of positive electrode lots and negative electrode lots: Combination 1: [(A,D), (B,E), (C,F)] Combination 2: [(A,D), (B,F), (C,E)] Combination 3: [(A,E), (B,D), (C,F)] Combination 4: [(A,E), (B,F), (C,D)] Combination 5: [(A,F), (B,D), (C,E)] Combination 6: [(A,F), (B,E), (C,D)]

[0057] For example, when the liquid flow ratio of the electrode pair of positive electrode lot B and negative electrode lot F is greater than the threshold value, combination 2 and combination 4 including the electrode pair (B, F) are excluded. As a result, combination 1, combination 3, combination 5, and combination 6 are displayed on display unit 76 as combination candidates.

[0058] 12 is a schematic diagram showing an example of a display screen of the combination result. The display screen 100 of the combination result shows candidate combinations 102. 1 ~102 NFor example, combination 102 is displayed. 1 ~102 N For each of the combinations, an identification number for identifying each combination, the electrode pairs included, the liquid flow ratio of the electrode pairs, etc. may be displayed. Alternatively, instead of or in addition to the liquid flow ratio, the corresponding high-rate resistance change rate may be displayed.

[0059] The display screen 100 may also include an output button 104 for instructing printing or downloading of data, and a rearrangement instruction button 106 for instructing rearrangement of data. The rearrangement of data may be performed based on representative values ​​(standard deviation, average value, maximum value, minimum value) of the liquid flow ratio. An example of rearranging data based on the standard deviation of the liquid flow ratio will be described below.

[0060] Returning to the explanation of FIG. 10, next, in step S112, the CPU 64 determines whether or not rearrangement has been instructed via the input unit 78 and the display unit 76. If rearrangement has been instructed, the process proceeds to step S114. On the other hand, if rearrangement has not been instructed, the routine ends. Next, in step S114, the CPU 64 calculates the standard deviation of the liquid flow ratio for the remaining combinations of positive electrode lots and negative electrode lots. Next, in step S116, the CPU 64 rearranges the remaining combinations of positive electrode lots and negative electrode lots in ascending order of standard deviation, displays them on the display unit 76, and ends the routine.

[0061] As described above, according to this embodiment, the liquid flow rates (estimated values) of the positive electrode lot and the negative electrode lot are estimated from various production data obtained in the production process, so that production variations can be reflected in the liquid flow rates (estimated values). Furthermore, since the electrode pair is determined so that the liquid flow ratio is equal to or less than a threshold value, the liquid flow ratio can be made substantially constant regardless of production variations, and lithium ion secondary batteries with desired performance can be stably produced.

[0062] In this embodiment, even if the electrode plate has a large or small amount of liquid flow, it can be used to form an electrode body as long as it is possible to form an electrode pair. Also, it is possible to use a sample with which an electrode pair could not be formed in the next calculation. Furthermore, since the upper limit threshold is flexibly set based on the range that is acceptable in terms of performance for the liquid flow ratio, it is possible to relax the manufacturing conditions for each electrode plate and also to relax the requirements for determining an electrode pair, compared to the case where the liquid flow rate of the positive electrode lot and the liquid flow rate of the negative electrode lot are made to match. As a result, the amount of electrode plates to be discarded can be reduced.

[0063] Moreover, according to this embodiment, the estimation of the liquid flow rate, the calculation of the liquid flow ratio, and the extraction and output of combination candidates of the positive electrode lot and the negative electrode lot can all be performed by a computer. Moreover, the manufacturing data is a value obtained in the manufacturing process, and there is no need to measure it anew. Therefore, compared to the case where the actual value of the liquid flow rate is measured and the user determines the combination of the positive electrode lot and the negative electrode lot by trial and error, the user's effort can be reduced. Also, an increase in the number of samples can be easily accommodated.

[0064] <Modification> The manufacturing method of the lithium ion secondary battery and the configuration of the manufacturing support device described in the above embodiment are merely examples, and it goes without saying that the configuration may be changed without departing from the spirit of the present invention.

[0065] The manufacturing method and manufacturing support device for a lithium ion secondary battery disclosed herein can be applied regardless of the configuration of the lithium ion secondary battery. For example, in the above embodiment, a wound type electrode body is exemplified, but the form of the electrode body is not limited to the wound type. For example, the electrode body may be a laminated type electrode body. In addition, in the above embodiment, a flat prismatic lithium ion secondary battery is exemplified, but the shape of the lithium ion secondary battery is not limited to the flat prismatic type. For example, the lithium ion secondary battery may be cylindrical.

[0066] In the above embodiment, the value of the electrolyte flow ratio corresponding to the allowable upper limit of the high-rate resistance change rate is set as the upper limit threshold of the electrolyte flow ratio, but the desired performance is not limited to the performance of suppressing the increase in internal resistance accompanying high-rate charging and discharging. For example, the electrolyte flow ratio threshold may be set in relation to other performances (battery resistance and output) that are affected by the electrolyte flow characteristics. The electrolyte flow ratio threshold may also be set in relation to multiple performances.

[0067] In the above embodiment, an example was described in which a combination of a positive electrode lot and a negative electrode lot that does not include an electrode pair whose liquid flow ratio is greater than a threshold value is extracted and displayed as a combination candidate, but the method of extraction and display is not limited to this. For example, an electrode pair whose liquid flow ratio is equal to or less than a threshold value may be extracted and displayed. In addition, in order to reduce the amount of calculation, the calculation may be terminated and the result may be output when even one combination that does not include an electrode pair whose liquid flow ratio is greater than a threshold value is found. In addition, a combination in which the number of pairs whose liquid flow ratio is greater than a predetermined threshold value is equal to or less than a predetermined number may be extracted and displayed as a combination candidate.

[0068] [Additional Notes] The following additional notes are provided in relation to the above-described embodiments. A first aspect of the present disclosure is a method for manufacturing a lithium ion secondary battery, including the steps of acquiring manufacturing data for each of a plurality of production lots of positive plate production lots and a plurality of production lots of negative plate production lots, estimating a liquid flow volume for each production lot from the acquired manufacturing data, extracting pairs of the production lots of the positive plate production lots and the negative plate production lots that form an electrode body using the estimated liquid flow volumes for each production lot, where a liquid flow ratio, which is the ratio of the liquid flow volume of the production lot of the negative plate production lot to the liquid flow volume of the production lot of the positive plate production lot, is equal to or less than a predetermined threshold value, and forming the electrode body from the extracted pairs of production lots of the positive plate production lots and the negative plate production lots. A second aspect of the present disclosure is the method for producing a lithium ion secondary battery according to the first aspect, wherein the predetermined threshold value is determined in advance based on battery performance. A third aspect of the present disclosure is the method for producing the lithium ion secondary battery of the second aspect, wherein the battery performance is a performance of suppressing an increase in internal resistance accompanying high-rate charging and discharging. A fourth aspect of the present disclosure is the method for producing a lithium ion secondary battery according to any one of the first to third aspects, wherein the predetermined threshold value of the liquid flow ratio is in the range of 1.5 to 3.0. A fifth aspect of the present disclosure is a method for producing a lithium ion secondary battery according to any one of the first to fourth aspects, wherein the estimating step estimates the liquid flow volume of each production lot from the production data using a multiple regression equation having the liquid flow volume as a response variable and the production data items as explanatory variables. A sixth aspect of the present disclosure is the method for producing a lithium ion secondary battery according to the fifth aspect, wherein the multiple regression equation is prepared for each of the positive electrode plate and the negative electrode plate. A seventh aspect of the present disclosure is the method for producing a lithium ion secondary battery according to Aspect 5 or Aspect 6, wherein the items of the production data serving as explanatory variables of the multiple regression equation for the negative electrode plate are one or more items selected from the group consisting of an average particle size of the negative electrode active material, a type of coating surface of the negative electrode paste, a basis weight of the negative electrode paste, a ratio of each material contained in the negative electrode paste, a viscosity of the negative electrode paste, and a thickness of the negative electrode plate after pressing. An eighth aspect of the present disclosure is a method for producing a lithium ion secondary battery according to any one of the fifth to seventh aspects, wherein the production data items serving as explanatory variables of the multiple regression equation for the positive electrode plate are one or more items selected from the group consisting of a particle shape of a positive electrode active material, a specific surface area of ​​particles of a positive electrode active material, a coating surface of a positive electrode paste, a basis weight of the positive electrode paste, a ratio of each material contained in the positive electrode paste, a viscosity of the positive electrode paste, and a composite density of the positive electrode plate after pressing. A ninth aspect of the present disclosure is the method for producing a lithium ion secondary battery according to any one of the fifth to eighth aspects, wherein the coefficient of determination of the multiple regression equation is 0.7 or more. A tenth aspect of the present disclosure is a manufacturing support device that supports the manufacture of lithium ion secondary batteries, the manufacturing support device comprising: an acquisition unit that acquires manufacturing data for multiple production lots of positive electrode plates and multiple production lots of negative electrode plates; an estimation unit that estimates a liquid flow volume for each production lot from the manufacturing data acquired by the acquisition unit; an extraction unit that uses the liquid flow volume for each production lot estimated by the estimation unit to extract pairs of the production lot of the positive electrode plates and the production lot of the negative electrode plates that form an electrode body, where a liquid flow ratio, which is the ratio of the liquid flow volume of the production lot of the negative electrode plates to the liquid flow volume of the production lot of the positive electrode plates, is equal to or less than a predetermined threshold; and an output unit that outputs pairs where the liquid flow ratio extracted by the extraction unit is equal to or less than a predetermined threshold. An eleventh aspect of the present disclosure is the manufacturing support device of aspect 10, wherein the extraction unit obtains, as combination candidates, a set of pairs of the production lots of the positive electrode plates and the production lots of the negative electrode plates, in which the number of pairs in which the liquid flow ratio is greater than a predetermined threshold value is equal to or less than a predetermined number, and the output unit outputs the combination candidates obtained by the extraction unit. A twelfth aspect of the present disclosure is the manufacturing support device of aspect 11, wherein the extraction unit calculates the liquid flow ratio for all pairs of the production lots of positive plates and the production lots of negative plates for multiple production lots of positive plates and multiple production lots of negative plates, obtains all combinations that are sets of pairs of the production lots of the positive plates and the production lots of the negative plates, excludes from all the combinations combinations in which the number of pairs in which the liquid flow ratio is greater than the predetermined threshold value exceeds a predetermined number, and sets the remaining combinations as the candidate combinations. A thirteenth aspect of the present disclosure is a manufacturing support device according to any one of aspects ten to twelve, wherein the estimation unit estimates the liquid flow volume of each manufacturing lot from the manufacturing data using a multiple regression equation stored in advance, the multiple regression equation having the liquid flow volume as a response variable and the manufacturing data items as explanatory variables. A fourteenth aspect of the present disclosure is the manufacturing support device of Aspect thirteen, wherein the multiple regression equation is stored in advance for each of the positive electrode plate and the negative electrode plate. A fifteenth aspect of the present disclosure is the manufacturing support device of any one of the tenth to fourteenth aspects, wherein the output unit displays the extraction result on a display unit. [Explanation of symbols]

[0069] 10 Lithium-ion secondary battery 20 Battery case 22 Electrolyte 30 Lid 32N negative terminal 32P positive terminal 34 Safety valve 36 Filling port 38N negative electrode current collector plate 38P positive current collector 40 Electrode body 42 Positive plate 42A positive electrode current collector 42B Positive electrode active material layer 44 Negative plate 44A negative electrode current collector 44B Negative electrode active material layer 46 Separator 50 measurement samples 52 Winding core 54 Measurement Case 56 Rubber stopper 58 O-ring 60 Manufacturing support equipment 62 Control section 64 CPU 66 ROM 68 RAM 70 Memory 72 Input / output section 74 Bus 76 Display section 78 Input section 80 Communications Department 82 Memory section 100 display screens 104 Output button 106 Instruction Button

Claims

1. Acquiring production data for each of a plurality of production lots of positive electrode plates and a plurality of production lots of negative electrode plates; estimating a liquid flow rate for each production lot from the acquired production data; extracting pairs of the production lot of the positive electrode plate and the production lot of the negative electrode plate that form an electrode body, the pairs having a liquid flow ratio, which is a ratio of the liquid flow rate of the production lot of the negative electrode plate to the liquid flow rate of the production lot of the positive electrode plate, that is equal to or less than a predetermined threshold value, using the estimated liquid flow rate of each production lot; forming the electrode assembly from an extracted pair of the positive electrode plate manufacturing lot and the negative electrode plate manufacturing lot; A method for producing a lithium ion secondary battery comprising the steps of:

2. The method for producing a lithium ion secondary battery according to claim 1 , wherein the predetermined threshold value is determined in advance based on battery performance.

3. The method for producing a lithium ion secondary battery according to claim 2 , wherein the battery performance is a performance of suppressing an increase in internal resistance accompanying high-rate charging and discharging.

4. 2. The method for producing a lithium ion secondary battery according to claim 1, wherein the predetermined threshold value of the liquid flow ratio is in a range of 1.5 to 3.

0.

5. 2. The method for producing a lithium ion secondary battery according to claim 1, wherein the estimating step estimates the liquid flow rate of each production lot from the production data using a multiple regression equation in which the liquid flow rate is a response variable and the items of the production data are explanatory variables.

6. The method for producing a lithium ion secondary battery according to claim 5 , wherein the multiple regression equation is prepared for each of the positive electrode plate and the negative electrode plate.

7. 6. The method for producing a lithium ion secondary battery according to claim 5, wherein the items of the production data serving as explanatory variables of the multiple regression equation for the negative electrode plate are one or more items selected from the group consisting of an average particle size of the negative electrode active material, a type of coating surface of the negative electrode paste, a basis weight of the negative electrode paste, a ratio of each material contained in the negative electrode paste, a viscosity of the negative electrode paste, and a thickness of the negative electrode plate after pressing.

8. 6. The method for producing a lithium ion secondary battery according to claim 5, wherein the items of the production data serving as explanatory variables of the multiple regression equation for the positive electrode plate are one or more items selected from the group consisting of a particle shape of the positive electrode active material, a specific surface area of ​​the particles of the positive electrode active material, a coating surface of the positive electrode paste, a basis weight of the positive electrode paste, a ratio of each material contained in the positive electrode paste, a viscosity of the positive electrode paste, and a composite density of the positive electrode plate after pressing.

9. The method for producing a lithium ion secondary battery according to claim 5 , wherein the coefficient of determination of the multiple regression equation is 0.7 or more.

10. A manufacturing support device for supporting the manufacturing of a lithium ion secondary battery, An acquisition unit that acquires manufacturing data for each of a plurality of manufacturing lots of positive electrode plates and a plurality of manufacturing lots of negative electrode plates; an estimation unit that estimates a liquid flow amount of each production lot from the production data acquired by the acquisition unit; an extraction unit that uses the liquid flow rate of each production lot estimated by the estimation unit to extract pairs of the production lot of the positive electrode plate and the production lot of the negative electrode plate that form an electrode body, the pairs having a liquid flow ratio, which is a ratio of the liquid flow rate of the production lot of the negative electrode plate to the liquid flow rate of the production lot of the positive electrode plate, that is equal to or less than a predetermined threshold value; an output unit that outputs pairs whose liquid flow ratios extracted by the extraction unit are equal to or less than a predetermined threshold; A manufacturing support device comprising:

11. The extraction unit obtains, as combination candidates, a set of pairs of the production lot of the positive electrode plate and the production lot of the negative electrode plate, in which the number of pairs in which the liquid flow ratio is greater than a predetermined threshold value is equal to or less than a predetermined number; The output unit outputs the combination candidates obtained by the extraction unit. The manufacturing support device according to claim 10.

12. The extraction unit is For multiple production lots of positive plates and multiple production lots of negative plates, Calculating the liquid flow ratio for all pairs of the production lots of the positive electrode plates and the negative electrode plates; determining all combinations that are sets of pairs of the manufacturing lots of the positive electrode plates and the manufacturing lots of the negative electrode plates; excluding a combination in which the number of pairs in which the liquid flow ratio is greater than the predetermined threshold value exceeds a predetermined number from all of the combinations; The remaining combinations are set as the combination candidates. The manufacturing support device according to claim 11.

13. 11. The manufacturing support device according to claim 10, wherein the estimation unit estimates the liquid flow volume of each production lot from the manufacturing data using a pre-stored multiple regression equation in which the liquid flow volume is a response variable and the items of the manufacturing data are explanatory variables.

14. The manufacturing support device according to claim 13 , wherein the multiple regression equation is stored in advance for each of the positive electrode plate and the negative electrode plate.

15. The manufacturing support device according to claim 10 , wherein the output unit causes a display unit to display the extraction result.

Citation Information

Patent Citations

  • Lithium ion secondary battery

    JP2016066461A