Cushioning material and cushioning material manufacturing method
A cushioning material using cellulose fibers bound with thermoplastic starch and metal stearate maintains performance by preventing moisture absorption, addressing the issue of humidity-induced degradation in waste paper-based materials.
Patent Information
- Application Number
- JP2023073110
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Cushioning materials made from waste paper boards lose cushioning performance in high-humidity environments due to moisture absorption.
Incorporating cellulose fibers bound with a binding material comprising thermoplastic starch and metal stearate, which are mixed and molded to form a cushioning material.
The solution maintains cushioning performance by suppressing moisture absorption, ensuring stability and effectiveness in varying humidity conditions.
Smart Images

Figure 2024158151000001 
Figure 2024158151000002 
Figure 2024158151000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a cushioning material and a method for manufacturing the cushioning material. [Background technology]
[0002] Patent Document 1 proposes a waste paper board that can be used as a cushioning material, etc. This waste paper board is made from waste paper pulp fibers obtained by defibrating waste paper and thermoplastic resin fibers. Specifically, the waste paper pulp fibers and the thermoplastic resin fibers are mixed in a dry state, and a web is formed in a dry state from the fiber aggregate obtained by mixing. Then, this web is heated to a temperature equal to or higher than the melting point of the thermoplastic resin and pressure-molded, so that the waste paper pulp fibers are bonded together to produce the waste paper board. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 9-220709 Summary of the Invention [Problem to be solved by the invention]
[0004] However, cushioning materials made of waste paper boards as described above have the problem that when placed in a humid environment, such as during transportation, they absorb moisture from the air and soften, resulting in a decrease in cushioning performance. [Means for solving the problem]
[0005] The cushioning material includes cellulose fibers and a binder material that holds the cellulose fibers together, the binder material including thermoplastic starch and a metallic stearate.
[0006] The method for manufacturing the cushioning material includes a defibration process in which a raw material containing cellulose fibers is defibrated in a dry manner, a mixing process in which the cellulose fibers defibrated in the defibration process are mixed with a binding material in air to produce a mixture, and a molding process in which the mixture is heated to form the cushioning material, where the binding material contains thermoplastic starch and a metal stearate. [Brief description of the drawings]
[0007] [Figure 1] FIG. 2 is a diagram showing a schematic diagram of an example of a manufacturing apparatus capable of manufacturing a cushioning material. [Diagram 2] 4 is a flowchart showing a manufacturing process of the cushioning material. [Diagram 3] 4 is a graph showing an example of the relationship between stress applied to a cushioning material and distortion caused in the cushioning material. [Figure 4] 13 is a graph showing an example of the relationship between the damping coefficient and distortion. [Diagram 5] 1 is a graph showing the relationship between the blending ratio of the binder material and the stress at which the distortion is 0.2. [Figure 6] 1 is a graph showing the relationship between the blending ratio of a bonding material and the minimum cushioning coefficient. [Figure 7] 1 is a graph showing the relationship between the blending ratio of metal stearate and the stress at which the distortion is 0.2. [Figure 8] 1 is a graph showing the relationship between the blending ratio of metal stearate and the minimum cushioning coefficient. [Figure 9] 1 is a table showing the relationship between the blending ratio of metal stearate and water repellency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The cushioning material and the method for manufacturing the cushioning material according to the present embodiment will be described in detail below. The cushioning material and the method for manufacturing the cushioning material of the present embodiment are not limited to the contents described below, and various modifications are possible without departing from the spirit and scope of the present invention.
[0009] [1] Cushioning material First, the cushioning material will be described. The cushioning material of this embodiment includes a plurality of cellulose fibers and a binding material that bonds the cellulose fibers together.
[0010] [1-1] Cellulose fiber Cellulose fibers are abundant natural materials derived from plants, and the use of cellulose fibers as fibers can suitably address environmental issues and save buried resources. The use of cellulose fibers in cushioning materials is also preferable from the viewpoints of stable supply of cushioning materials, cost reduction, etc. Furthermore, among various fibers, cellulose fibers have particularly high theoretical strength, and are advantageous from the viewpoint of improving the strength of cushioning materials.
[0011] Cellulosic fibers are generally composed mainly of cellulose, but may contain components other than cellulose, such as hemicellulose and lignin.
[0012] The cellulose content in the cellulose fibers is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 80% by mass or more.
[0013] The cellulose fibers to be used may be those that have been subjected to a treatment such as bleaching, etc. The cellulose fibers to be used may be those that have been subjected to a treatment such as ultraviolet irradiation treatment, ozone treatment, plasma treatment, etc.
[0014] The cellulose fibers may be natural cellulose fibers such as animal cellulose fibers and plant cellulose fibers, or chemical cellulose fibers such as organic cellulose fibers, inorganic cellulose fibers, and organic-inorganic composite cellulose fibers. More specifically, the cellulose fibers may be cellulose fibers made of cellulose, cotton, hemp, kenaf, flax, ramie, jute, Manila hemp, sisal, coniferous trees, broadleaf trees, etc., which may be used alone or in appropriate mixtures, or may be used as regenerated cellulose fibers that have been purified, etc. The cellulose fibers may also be subjected to various surface treatments.
[0015] The average length of the cellulose fibers is not particularly limited, but the length-length weighted average cellulose fiber length is preferably 10 μm or more and 50 mm or less, more preferably 20 μm or more and 5.0 mm or less, and even more preferably 30 μm or more and 3.0 mm or less.
[0016] This can improve the shape stability, strength, etc. of the cushioning material, and can also improve the cushioning performance of the cushioning material.
[0017] The cellulose fibers contained in the cushioning material of this embodiment, when treated as individual cellulose fibers, preferably have an average thickness of 1.0 μm or more and 1000 μm or less, and more preferably 2.0 μm or more and 100.0 μm or less.
[0018] This can improve the stability of the shape of the cushioning material, the strength, etc. Also, the cushioning performance of the cushioning material can be improved. Also, the occurrence of undesired irregularities on the surface of the cushioning material can be more effectively prevented.
[0019] In addition, when the cross section of a cellulose fiber is not circular, the diameter of a circle having an area equal to the area of the cross section is regarded as the thickness of the cellulose fiber.
[0020] The average aspect ratio of cellulose fibers, that is, the average length to the average thickness, is not particularly limited, but is preferably 10 or more and 1,000 or less, and more preferably 15 or more and 500 or less.
[0021] This can improve the stability of the shape of the cushioning material, the strength, etc. Also, the cushioning performance of the cushioning material can be improved. Also, the occurrence of undesired irregularities on the surface of the cushioning material can be more effectively prevented.
[0022] In this specification, the term "cellulose fiber" may refer to a single cellulose fiber or an aggregate of multiple cellulose fibers. The cellulose fiber may be cellulose fiber that has been untangled into fibers by subjecting a material to defibration treatment, i.e., a defibrated material. Examples of the material to be defibrated include pulp sheets, paper, waste paper, tissue paper, kitchen paper, cleaners, filters, liquid absorbents, sound absorbers, cushioning materials, mats, cardboard, and other materials in which cellulose fibers are entangled or bound together.
[0023] [1-2] Bonding material The binder material of this embodiment includes thermoplastic starch and a metallic stearate. According to this configuration, the hydrophobicity of the metal stearate makes it possible to suppress a decrease in the cushioning performance caused by moisture absorption of the cushioning material.
[0024] The binding material may have a function other than that of binding the cellulose fibers together. For example, the binding material may have a function of suppressing components other than the cellulose fibers, such as a colorant described below, from falling off from the cushioning material.
[0025] The ratio of the mass of the binding material to the total mass of the cellulose fibers and the binding material is preferably 20% by mass or more and 50% by mass or less. According to this configuration, a cushioning material having good cushioning performance can be obtained. The total mass of the cellulose fiber and the binding material corresponds to the mass of the cushioning material minus the mass of other components described later.
[0026] Thermoplastic starch is a mixture of starch and a plasticizer such as dextrin. Starch is a polymeric material formed by the polymerization of multiple α-glucose molecules through glycosidic bonds. Starch may be linear or branched.
[0027] Starch may be derived from various plants, for example. Examples of starch sources include cereals such as corn, wheat, and rice, beans such as broad beans, mung beans, and red beans, tubers such as potato, sweet potato, and tapioca, wild plants such as dogtooth violets, bracken, and kudzu, and palms such as sago palm.
[0028] The starch may be, for example, a modified starch, such as acetylated adipic acid cross-linked starch, acetylated starch, oxidized starch, sodium octenyl succinate starch, hydroxypropyl starch, hydroxypropylated phosphate cross-linked starch, phosphorylated starch, phosphate esterified phosphate cross-linked starch, urea phosphate esterified starch, sodium starch glycolate, or high amylose corn starch.
[0029] Metal stearates are mixed with the thermoplastic starch, and include calcium stearate, zinc stearate, magnesium stearate, aluminum stearate, and the like.
[0030] Of these, the metal stearate is preferably zinc stearate. With this configuration, a cushioning material having high cushioning performance can be realized at low cost.
[0031] The binder of the present embodiment may also contain binder materials other than thermoplastic starch and metal stearates, for example, binder materials made of various synthetic resins.
[0032] Examples of synthetic resins include AS resin, ABS resin, polypropylene, polyethylene, polyvinyl chloride, polystyrene, acrylic resin, polyester resin, polyethylene terephthalate, polyphenylene ether, polybutylene terephthalate, nylon, polyamide, polycarbonate, polyacetal, polyphenylene sulfide, and polyether ether ketone.
[0033] Of the synthetic resins, biodegradable resins such as polylactic acid, polybutylene succinate, and polyhydroxybutanoic acid may be used. By using a biodegradable resin, the cushioning material can be made more environmentally friendly. Furthermore, the resin may be, for example, copolymerized or modified.
[0034] When the cushioning material contains binder materials other than thermoplastic starch and metal stearates, the content of these binder materials in the cushioning material is preferably 1.0% by mass or less, more preferably 0.5% by mass or less, and even more preferably 0.1% by mass or less.
[0035] The proportion of the mass of the metal stearate to the total mass of the cellulose fibers and the binding material is preferably 10% by mass or more and 25% by mass or less. According to this configuration, it is possible to obtain a cushioning material having good cushioning performance, and to suppress the deterioration of the cushioning performance due to moisture absorption.
[0036] [1-3] Other ingredients The cushioning material of the present embodiment may contain cellulose fibers and a binder material made of thermoplastic starch and a metal stearate, but may also contain other components. Hereinafter, such components are also referred to as "other components."
[0037] Examples of other components include flame retardants, colorants, aggregation inhibitors, surfactants, antifungal agents, preservatives, antioxidants, ultraviolet absorbers, and oxygen absorbers.
[0038] The content of other components in the buffer material is preferably 7.0% by mass or less, more preferably 5.0% by mass or less, and even more preferably 3.0% by mass or less.
[0039] [1-4] Characteristics of cushioning material The cushioning material of the present embodiment may be of any size and shape, and may be, for example, in the form of a sheet or may have a three-dimensional shape.
[0040] In addition, the cushioning material of this embodiment may be, for example, a sheet-like cushioning material prepared in advance that is processed into a predetermined three-dimensional shape by molding using a mold, cutting, folding, incising, assembling, and other processes when necessary.
[0041] As described above, when the cushioning material has a three-dimensional shape and is manufactured from a sheet-like cushioning material, the cushioning material having a three-dimensional shape may be manufactured by stacking multiple sheets of cushioning material together.
[0042] [2] Manufacturing method of cushioning material Next, a method for manufacturing the cushioning material will be described.
[0043] [2-1] Composition for manufacturing cushioning material First, a composition for manufacturing a cushioning material used in the method for manufacturing a cushioning material of the present embodiment will be described.
[0044] [2-1-1] Cellulose fiber The composition for manufacturing a cushioning material of the present embodiment contains a plurality of cellulose fibers. As the cellulose fibers contained in the composition for manufacturing a cushioning material, those explained in the above [1-1] can be used. This provides the same effect as described above.
[0045] [2-1-2] Bonding material The composition for manufacturing a cushioning material of the present embodiment contains a binder. As the binder contained in the composition for manufacturing a cushioning material, those explained in the above [1-2] can be used. This provides the same effect as described above.
[0046] When the binder material is contained in the composition for producing a cushioning material as particles, it is preferable that the volume average particle size of the binder material is smaller than the thickness of the cellulose fibers. This makes it easier to mix the binder material and the cellulose fibers more uniformly, and more effectively prevents unintended variations in composition within the cushioning material.
[0047] The volume average particle size of the binding material is preferably 0.8 μm or more and 100 μm or less, and more preferably 1.5 μm or more and 50 μm or less.
[0048] The particulate binding material can be obtained by kneading the material using, for example, a kneader, a Banbury mixer, a single-screw extruder, a multi-screw extruder, a two-roll mill, a three-roll mill, a continuous kneader, a continuous two-roll mill, or the like, and then pelletizing and pulverizing the material by an appropriate method. The binding material may contain particles of various sizes, which may be classified using a known classification device. The outer shape of the particles of the binding material is not particularly limited, and may be spherical, disc-shaped, fibrous, amorphous, or the like.
[0049] In this embodiment, the ratio of the mass of the binding material to the total mass of the cellulose fiber and the binding material contained in the total solid content constituting the composition for manufacturing a cushioning material is preferably 20 mass % or more and 50 mass % or less. According to this configuration, a cushioning material having good cushioning performance can be obtained. The total mass of the cellulose fiber and the binding material contained in the total solid content constituting the cushioning material manufacturing composition corresponds to the mass of the total solid content constituting the cushioning material manufacturing composition minus the mass of the total solid content constituting the other components described later.
[0050] In this embodiment, the ratio of the mass of the metal stearate to the total mass of the cellulose fiber and binding material contained in the total solid content constituting the composition for manufacturing a cushioning material is preferably 10 mass % or more and 25 mass % or less. According to this configuration, it is possible to obtain a cushioning material having good cushioning performance, and to suppress the deterioration of the cushioning performance due to moisture absorption.
[0051] In the composition for manufacturing a cushioning material, the binding material may be present in any state, for example, dissolved in other components, but it is preferable that the binding material be present in a dispersed state, particularly dispersed as a powder.
[0052] This makes it possible to favorably form voids in the manufactured cushioning material, and thus makes it possible to more reliably improve the cushioning performance of the cushioning material.
[0053] [2-1-3]Liquid component The composition for manufacturing a cushioning material of the present embodiment may contain, for example, a liquid component.
[0054] By including a liquid component, for example, it is possible to favorably disintegrate the cellulose fibers in the composition for manufacturing a cushioning material, and to favorably prevent unintended uneven distribution of each component in the composition for manufacturing a cushioning material.
[0055] When the composition for manufacturing a buffer material contains a liquid component, the binding material may be contained in a dissolved state in the liquid component, or may be contained in a dispersed state in the liquid component.
[0056] Examples of the liquid component include water, various organic solvents such as alcohol solvents such as methanol, ethanol, ethylene glycol, and glycerin, and ketone solvents such as acetone and methyl ethyl ketone, and one or more selected from these can be used in combination.
[0057] When the composition for producing a buffer material contains a liquid component, the content of the liquid component in the composition for producing a buffer material can be, for example, 10% by mass or more and 70% by mass or less.
[0058] [2-1-4] Other ingredients The composition for manufacturing a cushioning material of the present embodiment may contain components other than those described above. As such components, those described in [1-3] above can be used.
[0059] The proportion of other components in the total solid content constituting the composition for manufacturing a buffer material is preferably 7.0 mass % or less, more preferably 5.0 mass % or less, and even more preferably 3.0 mass % or less.
[0060] [2-1-5] Properties of the composition for manufacturing cushioning materials The composition for producing a cushioning material may be in any form, for example, a powder, a dispersion, a web, or the like.
[0061] [2-1-6] Preparation of composition for manufacturing cushioning material The composition for producing a buffer material can be prepared, for example, by mixing the components of the composition for producing a buffer material.
[0062] More specifically, for example, the composition for manufacturing a cushioning material can be prepared by stirring and mixing defibrated cellulose fibers, powdered thermoplastic starch, and powdered metal stearate. In such a case, for example, the composition for manufacturing a cushioning material can be suitably prepared using an apparatus as described in detail later.
[0063] [2-2] Manufacturing equipment Next, a manufacturing apparatus that can be used to manufacture the cushioning material will be described.
[0064] FIG. 1 is a diagram showing a schematic diagram of an example of a manufacturing apparatus capable of manufacturing a cushioning material. As shown in FIG. 1, the manufacturing apparatus 100 has a supply section 10, a crushing section 12, a defibrating section 20, a sorting section 40, a first web forming section 45, a rotating body 49, a mixing section 50, a deposition section 60, a second web forming section 70, and a cushioning material forming section 80.
[0065] The supply unit 10 supplies a raw material containing cellulose fibers to the crushing unit 12. The supply unit 10 is, for example, an automatic supply unit for continuously supplying the raw material to the crushing unit 12.
[0066] The crushing unit 12 cuts the raw material supplied by the supply unit 10 in air or the like to make small pieces. The small pieces have a shape and size of, for example, several centimeters square. In the illustrated example, the crushing unit 12 has crushing blades 14, which can cut the input raw material. For example, a shredder is used as the crushing unit 12. The raw material cut by the crushing unit 12 is received in a hopper 1 and then transported to the defibrating unit 20 via a pipe 2.
[0067] The defibrating unit 20 defibrates the raw material cut by the coarse crushing unit 12, i.e., the raw material containing cellulose fibers. Here, "defibrate" refers to unraveling the raw material consisting of multiple cellulose fibers bound together, i.e., the defibrated material, into individual cellulose fibers. The defibrating unit 20 also has the function of separating substances such as resin particles, ink, toner, fillers, and anti-bleeding agents adhering to the raw material from the cellulose fibers.
[0068] The material that has passed through the defibrating unit 20 is called the "defibrated material." In addition to the defibrated cellulose fibers, the "defibrated material" may contain resin particles that have separated from the cellulose fibers when the cellulose fibers are defibrated, colorants such as ink, toner, and fillers, and additives such as anti-bleeding agents and paper strength agents. An example of the resin particles separated from the cellulose fibers is particles that contain a resin for bonding multiple cellulose fibers together.
[0069] The defibrator unit 20 performs defibration in a dry manner. A method of performing defibration and other processes in air, such as air, is called a dry method, as opposed to a wet method in which the material is dissolved in a liquid such as water to form a slurry. In this embodiment, an impeller mill is used as the defibrator unit 20. The defibrator unit 20 has a function of generating an airflow that sucks in the raw material and discharges the defibrated material. This allows the defibrator unit 20 to suck in the raw material together with the airflow from the inlet 22 using the airflow it generates, defibrate the raw material, and transport the defibrated material to the outlet 24. The defibrated material that has passed through the defibrator unit 20 is transferred to the sorting unit 40 via the pipe 3. Note that the airflow generated by the defibrator unit 20 may be used as the airflow for transporting the defibrated material from the defibrator unit 20 to the sorting unit 40, or an airflow generating device such as a blower may be provided and the airflow may be used.
[0070] The sorting section 40 introduces the defibrated material defibrated by the defibration section 20 from an inlet 42 and sorts it according to the length of the cellulose fibers. The sorting section 40 has a drum section 41 and a housing section 43 that houses the drum section 41. The drum section 41 has a net and can separate a first sorted material, which is cellulose fibers or particles that are smaller than the mesh size of the net and pass through the net, from a second sorted material, which is cellulose fibers, undefibrated pieces, and lumps that are larger than the mesh size of the net and do not pass through the net. The first sorted material is transferred to the mixing section 50, for example, via a pipe 7 described below. The second sorted material is returned to the defibration section 20 from the discharge port 44 via a pipe 8. The drum section 41 is specifically a cylindrical sieve formed by a net, and is rotated by a motor. For example, a wire net, an expanded metal made by stretching a metal plate with slits, or a punched metal made by forming holes in a metal plate by a press or the like is used as the net of the drum section 41.
[0071] The first web forming section 45 transports the first sorted material that has passed through the sorting section 40 to the mixing section 50. The first web forming section 45 includes a mesh belt 46, a plurality of tension rollers 47, and a suction section .
[0072] The suction unit 48 is disposed below the sorting unit 40 with the mesh belt 46 in between, and sucks the first sorted material that has passed through the mesh of the drum unit 41 in the sorting unit 40 and been dispersed into the air onto the mesh belt 46. The first sorted material is deposited on the moving mesh belt 46 to form a web V. The basic configurations of the mesh belt 46, tension roller 47, and suction unit 48 are similar to those of the mesh belt 72, tension roller 74, and suction mechanism 76 of the second web forming unit 70, which will be described later.
[0073] The web V is formed into a soft and puffy state containing a lot of air by passing through the screening section 40 and the first web forming section 45. The web V accumulated on the mesh belt 46 is input into the pipe 7 and transported to the mixing section 50.
[0074] The rotor 49 is disposed near the inlet of the pipe 7, and cuts the web V before it is transported to the mixer 50. In the illustrated example, the rotor 49 has a base 49a and a plurality of protrusions 49b radially protruding from the base 49a. The protrusions 49b have, for example, a plate shape. In the illustrated example, four protrusions 49b are provided, and the four protrusions 49b are provided at equal intervals. The rotor 49 cuts the web V with the protrusions 49b by rotating in the direction R around the base 49a as the rotation axis. By cutting the web V with the rotor 49, for example, it is possible to reduce the fluctuation in the amount of defibrated material supplied per unit time to the deposition section 60.
[0075] The rotating body 49 is provided in the vicinity of the first web forming unit 45. In the illustrated example, the rotating body 49 is provided next to the tension roller 47 that is located most downstream of the transport path of the web V in the first web forming unit 45, among the multiple tension rollers 47. The rotating body 49 is provided at a position where the protrusions 49b can come into contact with the web V, but does not come into contact with the mesh belt 46 on which the web V is deposited. The shortest distance between the protrusions 49b and the mesh belt 46 is, for example, 0.05 mm or more and 0.5 mm or less.
[0076] The mixing section 50 mixes the first sorted material that has passed through the screening section 40, in other words, the web V transported by the first web forming section 45, with additives including a binder material in the air. This produces a mixture of cellulose fibers and binder material. The mixing section 50 has an additive supply section 52 that supplies additives, a pipe 54 that transports the first sorted material and additives, and a blower 56. The pipe 54 is continuous with the pipe 7, and the first sorted material that has been input into the pipe 7 as the web V is transported to the pipe 54 via the pipe 7. In the illustrated example, the additives are supplied from the additive supply section 52 to the pipe 54 via a hopper 9.
[0077] In the mixing section 50, an air flow is generated by the blower 56, so that the first sorted material and the additives can be mixed and transported in the pipe 54. The mechanism for mixing the first sorted material and the additives is not particularly limited, and may be one that uses a blade that rotates at high speed to mix, or one that uses the rotation of a container, such as a V-type mixer.
[0078] The additive supply unit 52 may be a screw feeder as shown in FIG. 1 or a disk feeder (not shown). The additives supplied from the additive supply unit 52 include the above-mentioned binding material. When the binding material is supplied, the cellulose fibers are not bound together. When the binding material passes through the cushioning material forming unit 80, a part of the binding material melts, and binds together the cellulose fibers in the surface region of the cushioning material WS.
[0079] The additives supplied from the additive supply unit 52 may contain, in addition to the binding material, a colorant for coloring the cellulose fibers, an aggregation inhibitor for inhibiting aggregation of the cellulose fibers and the binding material, and a flame retardant for making the cellulose fibers etc. less flammable, depending on the type of cushioning material WS to be manufactured. The mixture that has passed through the mixing unit 50, i.e., the composition for manufacturing cushioning material which is a mixture of the first sorted material and the additives, is transferred to the deposition unit 60 via the pipe 54.
[0080] The depositing unit 60 introduces the mixture transported from the mixing unit 50 through an inlet 62, loosens the defibrated material of entangled cellulose fibers, and drops it while dispersing it in the air. This allows the depositing unit 60 to deposit the mixture in the second web forming unit 70 with good uniformity.
[0081] The deposition unit 60 has a drum unit 61 and a housing unit 63 that houses the drum unit 61. A rotating cylindrical sieve is used as the drum unit 61. In other words, the drum unit 61 has a mesh and causes cellulose fibers or particles smaller than the mesh size of the mixture that has passed through the mixing unit 50 to fall. The configuration of the drum unit 61 is the same as that of the drum unit 41, for example.
[0082] The "sieve" of the drum unit 61 does not have to have the function of selecting a specific object. In other words, the "sieve" used as the drum unit 61 means one equipped with a net, and the drum unit 61 may allow all of the mixture introduced into the drum unit 61 to fall.
[0083] The second web forming section 70 accumulates the material that has passed through the accumulation section 60 to form a web W, which is a pile that will become the cushioning material WS. At this time, a forming die (not shown in Fig. 1) can be placed on the mesh belt 72 and used as a tray to form the web W inside the forming die. The second web forming section 70 has, for example, the mesh belt 72, a plurality of tension rollers 74, and a suction mechanism 76.
[0084] The second web forming section 70 deposits the passing material that has passed through the mesh of the drum section 61 in the depositing section 60 onto the forming mold on the mesh belt 72 while moving the mesh belt 72. The mesh belt 72 and the forming mold are tensioned by tension rollers 74, and are configured to be hard to pass through the passing material but allow air to pass through. The mesh belt 72 moves as the tension rollers 74 rotate. As the mesh belt 72 moves continuously, the passing material that has passed through the depositing section 60 continuously falls and accumulates, forming a web W on the forming mold on the mesh belt 72. The mesh belt 72 and the forming mold are formed of, for example, metal, resin, cloth, nonwoven fabric, etc.
[0085] The suction mechanism 76 is provided below the deposition unit 60 across the mesh belt 72. The suction mechanism 76 can generate a downward airflow, i.e., an airflow from the deposition unit 60 toward the mesh belt 72. The suction mechanism 76 can suck the mixture dispersed in the air by the deposition unit 60 onto the mesh belt 72. This can increase the discharge speed from the deposition unit 60. Furthermore, the suction mechanism 76 can form a downflow in the fall path of the mixture, which can prevent the defibrated material and additives from becoming entangled during the fall.
[0086] As described above, the web W containing a lot of air and in a soft and swollen state is formed through the web forming process performed in the deposition unit 60 and the second web forming unit 70. The web W deposited on the mold on the mesh belt 72 is transported to the cushioning material forming unit 80.
[0087] The cushioning material forming unit 80 heats the web W accumulated in the forming mold on the mesh belt 72 to form the cushioning material WS. In the cushioning material forming unit 80, the web W, which is an accumulation of the mixture of defibrated material and additives mixed in the second web forming unit 70, is heated to soften and melt the binding material, thereby binding multiple cellulose fibers together.
[0088] The cushioning material forming section 80 includes a heating section 84 that heats the web W. As the heating section 84, for example, a heat press, a heating roller, or the like is used, but the following description will be given using an example in which a heating roller is used. The number of heating rollers 86 in the heating section 84 is not particularly limited. In the illustrated example, the heating section 84 includes a pair of heating rollers 86. By configuring the heating section 84 as heating rollers 86, the cushioning material WS can be formed while continuously transporting the web W.
[0089] The pair of heating rollers 86 are arranged, for example, with their rotation axes parallel to each other on the front and back sides of the web W. The heating rollers 86 come into contact with the web W on both the front and back sides, and heat the web W while conveying the web W by sandwiching it therebetween.
[0090] The manufacturing apparatus 100 of this embodiment may have a cutting section 90 as necessary. In the illustrated example, the cutting section 90 is provided downstream of the heating section 84. The cutting section 90 cuts the mold including the buffer material WS formed by the buffer material forming section 80. In the illustrated example, the cutting section 90 has a first cutting section 92 that cuts the mold of the buffer material WS in a direction intersecting the conveying direction of the buffer material WS, and a second cutting section 94 that cuts the buffer material WS in a direction parallel to the conveying direction. The second cutting section 94 cuts the mold including the buffer material WS that has passed through the first cutting section 92, for example. The buffer material WS cut by the second cutting section 94 is discharged to the discharge section 96.
[0091] Thereafter, the cushioning material WS is removed from the mold in which it was formed, thereby obtaining the cushioning material WS as a three-dimensional molded body.
[0092] [2-3] Manufacturing process FIG. 2 is a flow chart showing the manufacturing process of the cushioning material of this embodiment. The cushioning material of this embodiment is manufactured through the steps shown in Fig. 2 by the manufacturing apparatus shown in Fig. 1. Specifically, the manufacturing method for the cushioning material of this embodiment includes a fiber-defibrating step S1, a mixing step S2, and a molding step S3.
[0093] The defibration step S1 is a step in which a raw material containing cellulose fibers is defibrated by the defibration unit 20 in a dry manner. The mixing step S2 is a step of mixing the cellulose fibers defibrated in the defibration step S1 with a binder material in the air by the mixer 50 to produce a mixture. Here, the binder material mixed with the cellulose fibers includes thermoplastic starch and a metal stearate. The forming step S3 is a step of forming the cushioning material by heating the mixture in the cushioning material forming section 80. The cushioning material of this embodiment is formed by this forming step S3.
[0094] According to such a production method, it is possible to produce a cushioning material in which the deterioration of cushioning performance due to moisture absorption is suppressed due to the hydrophobicity of the metal stearate. The manufacturing apparatus and manufacturing process of the cushioning material of this embodiment are not limited to the above-mentioned apparatus and process. In other words, the cushioning material of this embodiment may be manufactured by an apparatus different from the above-mentioned manufacturing apparatus, or may be manufactured through a process different from the above-mentioned manufacturing process.
[0095] [3] Evaluation The results of various evaluations performed using the cushioning material of this embodiment will be described below.
[0096] [3-1] Basic characteristics First, as basic characteristics of the cushioning material, the stress-strain curve and the cushioning coefficient-strain curve will be described.
[0097] [3-1-1] Stress-strain curve FIG. 3 is a graph showing an example of the relationship between the stress applied to the cushioning material and the strain generated in the cushioning material, where the horizontal axis corresponds to the strain and the vertical axis corresponds to the stress. The stress-strain curve shown in this graph was obtained by compressing a sample of a cushioning material made of cellulose fiber, thermoplastic starch, and metal stearate in the thickness direction, i.e., the graph shows the relationship between the ratio of the thickness of the cushioning material when compressed to the thickness of the cushioning material in its natural state and the applied stress.
[0098] The sample used contains 70% by mass of cellulose fiber, 15% by mass of thermoplastic starch, and 15% by mass of metal stearate, respectively. That is, the ratio of the mass of the binding material to the total mass of the cellulose fiber and the binding material is 30% by mass, and the ratio of the mass of the metal stearate to the total mass of the cellulose fiber and the binding material is 15% by mass. In this evaluation, zinc stearate is used as the metal stearate.
[0099] As shown in Figure 3, after the stress starts to increase at a relatively steep rate after compression begins, the slope becomes smaller and the stress increase becomes gradual before the strain reaches 0.1. After that, when the strain exceeds 0.3, the stress increase gradually becomes larger, and when the strain exceeds 0.7, the slope of the curve becomes steep.
[0100] Cushioning materials are required to have a high stress required to produce a certain distortion. The higher this stress, the smaller the area that receives the load can be made, and the smaller the package size can be. In other words, it is preferable that the various components that make up the cushioning material and their respective blending ratios are determined so that this stress is high.
[0101] [3-1-2] Buffer coefficient-distortion curve FIG. 4 is a graph showing an example of the relationship between the damping coefficient and the distortion, where the horizontal axis corresponds to the distortion and the vertical axis corresponds to the damping coefficient. The cushioning coefficient is the ratio of the stress to the energy absorbed by deformation when stress is applied to the cushioning material. The cushioning coefficient is a value that indicates the cushioning efficiency, and the smaller the value, the higher the cushioning efficiency. The cushioning coefficient-strain curve can be derived from the relationship between stress and strain shown in Figure 3.
[0102] As shown in Figure 4, the cushioning coefficient-distortion curve shown in this graph is a downward convex curve. In other words, the cushioning coefficient decreases as the strain increases, reaches a minimum value, and then increases as the strain increases. When determining the thickness of the cushioning material, the optimal dimensions can be obtained by using the minimum cushioning coefficient, which is the minimum value of the cushioning coefficient.
[0103] Cushioning materials are required to have a small minimum cushioning coefficient. The smaller the minimum cushioning coefficient, the thinner the cushioning material can be, and the smaller the packaging size can be. In other words, it is preferable that the various components that make up the cushioning material and their respective mixing ratios are determined so that the minimum cushioning coefficient is small.
[0104] [3-2] Determining the mixing ratio of bonding materials Next, an evaluation performed to determine the blend ratio of the binder material will be described.
[0105] [3-2-1] Relationship between mixture ratio and stress FIG. 5 is a graph showing the relationship between the blend ratio of the bonding material and the stress when the strain is 0.2, where the horizontal axis corresponds to the blend ratio of the bonding material and the vertical axis corresponds to the stress when the strain is 0.2.
[0106] This graph was generated based on the relationship between stress and strain obtained by compressing a number of samples with different blending ratios of the binding material. Here, the blending ratio of the binding material is the ratio of the mass of the binding material to the total mass of the cellulose fiber and the binding material containing thermoplastic starch. In this evaluation, the graph was generated using seven types of samples with blending ratios of 0 mass%, 5 mass%, 10 mass%, 20 mass%, 30 mass%, 40 mass%, and 50 mass%. In other words, the graph in FIG. 5 plots the stress when the strain of each sample with blending ratios of 0 mass%, 5 mass%, 10 mass%, 20 mass%, 30 mass%, 40 mass%, and 50 mass% is 0.2.
[0107] As shown in Fig. 5, as the blending ratio of the bonding material increases from 0 mass%, the stress increases, and is maximum when the blending ratio is 30 mass%. Thereafter, the stress decreases as the blending ratio increases, but the stress when the blending ratio is 50 mass% is greater than the stress when the blending ratio is 10 mass%. For this reason, from the viewpoint of stress, the blending ratio of the bonding material is preferably 20 mass% or more and 50 mass% or less, and more preferably 20 mass% or more and 30 mass% or less.
[0108] [3-2-2] Relationship between mixture ratio and minimum buffer coefficient FIG. 6 is a graph showing the relationship between the blend ratio of the binder material and the minimum cushioning coefficient, where the horizontal axis corresponds to the blend ratio of the binder material and the vertical axis corresponds to the minimum cushioning coefficient.
[0109] This graph is derived from the stress-strain relationship that was the basis for the graph in Figure 5, and like Figure 5, it plots the minimum cushioning coefficient when the blend ratio is 0 mass%, 5 mass%, 10 mass%, 20 mass%, 30 mass%, 40 mass%, and 50 mass%.
[0110] As shown in Fig. 6, the minimum cushioning coefficient decreases as the blending ratio of the bonding material increases from 0 mass%, and is minimum when the blending ratio is 10 mass%. Thereafter, the minimum cushioning coefficient increases slightly as the blending ratio increases, and decreases slightly when the blending ratio exceeds 40 mass%, but the minimum cushioning coefficient when the blending ratio is 40 mass% is smaller than the minimum cushioning coefficient when the blending ratio is 5 mass%. For this reason, from the viewpoint of the minimum cushioning coefficient, the blending ratio of the bonding material is preferably 10 mass% or more and 50 mass% or less, and more preferably 10 mass% or more and 30 mass% or less.
[0111] Based on the above results, taking into consideration both stress and minimum cushioning coefficient, the mixing ratio of the binder material is preferably 20% by mass or more and 50% by mass or less, and more preferably 20% by mass or more and 30% by mass or less.
[0112] [3-3] Determination of the metal stearate content Next, the evaluation carried out to determine the blending ratio of the metal stearate will be described.
[0113] [3-3-1] Relationship between mixture ratio and stress FIG. 7 is a graph showing the relationship between the blending ratio of metal stearate and the stress at which the strain is 0.2, where the horizontal axis corresponds to the blending ratio of metal stearate and the vertical axis corresponds to the stress at which the strain is 0.2.
[0114] This graph was created based on the relationship between stress and strain obtained by compressing a number of samples with different blending ratios of metal stearate. Here, the blending ratio of metal stearate is the ratio of the mass of metal stearate to the total mass of cellulose fiber and a binding material made of thermoplastic starch and metal stearate. In this evaluation, the blending ratio of the binding material is fixed at 30% by mass, and zinc stearate is used as the metal stearate. Then, a graph was created using a number of samples for each of seven blending ratios of metal stearate: 0%, 5%, 10%, 15%, 20%, 25%, and 30% by mass. That is, the graph in FIG. 7 plots the stress when the strain of each sample with blending ratios of 0%, 5%, 10%, 15%, 20%, 25%, and 30% by mass is 0.2.
[0115] 7, as the blending ratio of metal stearate increases from 0% by mass, the stress increases, reaching a maximum when the blending ratio is 15% by mass. Thereafter, the stress decreases as the blending ratio increases. For this reason, from the viewpoint of stress, the blending ratio of metal stearate is preferably 5% by mass or more and 25% by mass or less, and more preferably 10% by mass or more and 20% by mass or less.
[0116] [3-3-2] Relationship between mixture ratio and minimum buffer coefficient FIG. 8 is a graph showing the relationship between the blending ratio of metal stearate and the minimum cushioning coefficient, with the horizontal axis corresponding to the blending ratio of metal stearate and the vertical axis corresponding to the minimum cushioning coefficient.
[0117] This graph is derived from the stress-strain relationship that was the basis for the graph in Figure 7, and like Figure 7, it plots the minimum cushioning coefficient when the blend ratio is 0 mass%, 5 mass%, 10 mass%, 15 mass%, 20 mass%, 25 mass%, and 30 mass%.
[0118] As shown in Fig. 8, the minimum cushioning coefficient decreases as the blending ratio of metal stearate increases from 0% by mass, and is minimum when the blending ratio is 20% by mass. Thereafter, the minimum cushioning coefficient increases slightly as the blending ratio increases. For this reason, from the viewpoint of the minimum cushioning coefficient, the blending ratio of metal stearate is preferably 10% by mass or more and 30% by mass or less, and more preferably 15% by mass or more and 25% by mass or less.
[0119] [3-3-3] Relationship between blending ratio and water repellency FIG. 9 is a table showing the relationship between the blending ratio of metal stearate and water repellency. In this evaluation, the contact angle of the free surface of a stationary liquid is used as an index of water repellency. Here, the contact angle is the angle on the inner side of the droplet among the angles between the free surface of a droplet dropped on the surface of the buffer material and the surface of the buffer material. In other words, the larger the contact angle, the closer the droplet is to a sphere, and the higher the water repellency. In other words, the larger the contact angle, the more the moisture absorption of the buffer material is suppressed, and the more the deterioration of the buffer performance due to moisture absorption is suppressed. In this evaluation, the blending ratio of the binding material is fixed at 30 mass%, and zinc stearate is used as the metal stearate.
[0120] Fig. 9 shows the results of measuring the contact angle for seven types of samples with different metal stearate blending ratios. In the figure, the comparative example is a buffer material that does not contain metal stearate, i.e., a buffer material with a metal stearate blending ratio of 0 mass%. Moreover, Examples 1 to 6 are buffer materials that contain metal stearate, and are buffer materials with metal stearate blending ratios of 30 mass%, 25 mass%, 20 mass%, 15 mass%, 10 mass%, and 5 mass%, respectively.
[0121] As shown in Fig. 9, the cushioning material containing metal stearate tends to have a larger contact angle and is more water repellent than cushioning materials that do not contain metal stearate. In particular, when the blending ratio of metal stearate is 10 mass% or more, a large difference in contact angle appears compared to binding materials that do not contain metal stearate. Therefore, from the viewpoint of water repellency, the blending ratio of metal stearate is preferably 10 mass% or more and 30 mass% or less.
[0122] In consideration of the above results and all of the stress, minimum cushioning coefficient, and water repellency, the blending ratio of metal stearate is preferably 10% by mass or more and 25% by mass or less, and more preferably 15% by mass or more and 20% by mass or less. [Explanation of symbols]
[0123] 1...hopper, 2,3,7,8...pipe, 9...hopper, 10...supply section, 12...crushing section, 14...crushing blade, 20...defibration section, 22...inlet, 24...discharge outlet, 40...screening section, 41...drum section, 42...inlet, 43...housing section, 44...discharge outlet, 45...first web forming section, 46...mesh belt, 47...tension roller, 48...suction section, 49...rotating body, 49a...base, 49b...projection, 50...mixing section, 5 2...additive supply section, 54...pipe, 56...blower, 60...deposition section, 61...drum section, 62...inlet, 63...housing section, 70...second web forming section, 72...mesh belt, 74...tension roller, 76...suction mechanism, 80...cushion forming section, 84...heating section, 86...heating roller, 90...cutting section, 92...first cutting section, 94...second cutting section, 100...manufacturing equipment, V,W...web, WS...cushion.
Claims
1. A cushioning material comprising cellulose fibers and a binder material that binds the cellulose fibers, The cushioning material is characterized in that the binder material includes thermoplastic starch and metal stearate.
2. 2. The cushioning material of claim 1, wherein the metallic stearate is zinc stearate.
3. The cushioning material according to claim 1 , wherein a ratio of a mass of the binder material to a total mass of the cellulose fibers and the binder material is 20 mass % or more and 50 mass % or less.
4. 4. The cushioning material according to claim 3, wherein a ratio of a mass of the metal stearate to a total mass of the cellulose fibers and the binding material is 10% by mass or more and 25% by mass or less.
5. A defibration process for dry defibrating a raw material containing cellulose fibers; a mixing step of mixing the cellulose fibers defibrated in the defibration step with a binder material in air to generate a mixture; and a molding step of heating the mixture to form a cushioning material. The method for producing a cushioning material, wherein the binding material includes thermoplastic starch and a metal stearate.