Electrolyte for power storage device, reinforcing agent, electrolyte solution, and power storage device using the same

A complex compound electrolyte with halogenated boron and siloxy/thiosilane groups addresses solubility and performance issues in lithium-ion batteries, enhancing charge/discharge efficiency and high-temperature stability.

JP2024158180APending Publication Date: 2024-11-08TOMIYAMA PURE CHEM IND LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023073156
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing lithium-ion secondary batteries face challenges in achieving a balance of solubility in organic solvents, charge/discharge efficiency, -10°C resistance, cycle characteristics, capacity retention rate, and high-temperature performance, with insufficient improvements in electrolytes leading to suboptimal performance.

Method used

Development of a specific complex compound electrolyte containing one or more compounds represented by a defined formula, incorporating halogenated boron groups and siloxy/thiosilane groups, used in conjunction with an organic solvent and a reinforcing agent to enhance electrolytic solutions for power storage devices.

Benefits of technology

The electrolyte and reinforcing agent combination achieves an excellent balance of solubility, charge/discharge efficiency, low resistance at -10°C, improved cycle characteristics, and high-temperature stability, resulting in enhanced performance of power storage devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158180000001
    Figure 2024158180000001
  • Figure 2024158180000002
    Figure 2024158180000002
  • Figure 2024158180000003
    Figure 2024158180000003
Patent Text Reader

Abstract

PURPOSE: To provide: an electrolyte that can form a power storage device and has an excellent balance between solubility in organic solvents (non-aqueous solvents), charge / discharge efficiency, -10°C resistance value, cycle characteristics (volume change rate, capacity retention rate, resistance change rate), and high-temperature characteristics; a reinforcing agent; an electrolyte solution; a power storage device formed using them; and a method for producing a lithium boron fluoride complex compound and a lithium complex compound for the electrolyte or reinforcing agent.SOLUTION: An electrolyte for a power storage device contains a lithium boron fluoride complex compound having a specific substituent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrolyte, a reinforcing agent, and an electrolytic solution for an electricity storage device, an electricity storage device produced using these, and further to a method for producing these. [Background technology]

[0002] In recent years, with the spread of various electronic devices such as portable electronic terminals typified by smartphones and notebook computers, as well as hybrid cars and electric cars, secondary batteries play an important role as power sources for them. Examples of these secondary batteries include aqueous or nonaqueous electrolyte batteries, and furthermore, all-solid-state batteries. Among them, lithium ion secondary batteries using nonaqueous electrolyte, which are provided with positive and negative electrodes capable of absorbing and releasing lithium ions and the like, and a nonaqueous electrolyte, have high energy density at high voltages, are excellent in safety, and have various advantages over other secondary batteries in terms of environmental issues, etc.

[0003] In lithium-ion secondary batteries currently in practical use that use non-aqueous electrolytes, for example, a composite oxide of lithium and a transition metal is used as the positive electrode active material, and a material that can be doped and de-doped with lithium is used as the negative electrode active material. In order to improve these characteristics, there is a demand for improvements in the properties of the non-aqueous electrolyte that is responsible for the transport of lithium ions. Such a non-aqueous electrolyte is an aprotic organic solvent, LiBF 4 , LiPF 6 , LiClO 4 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 CF 2 CF 3 ) 2 An electrolyte solution containing an electrolyte such as the above is used.

[0004] These LiBF 4 , LiPF 6 The non-aqueous electrolyte, which contains electrolytes such as LiBF, has high conductivity, which indicates the transport of lithium ions. 4, LiPF 6 It is known that the high oxidative decomposition voltage of the lithium secondary battery leads to a stable high voltage, which contributes to bringing out the high voltage and high energy density characteristics of the lithium secondary battery. However, there is a demand for improvements in the non-aqueous electrolyte for such lithium secondary batteries, such as high conductivity of lithium ions to reduce electrical resistance, improved cycle characteristics that maintain high capacity even after repeated charging and discharging, low resistance characteristics at the initial stage, and maintenance of high characteristics at high temperatures. In order to achieve these objectives, various improvements have been proposed for the electrolyte contained in the non-aqueous electrolyte solution, and new materials have also been proposed for the electrolyte itself. In addition, lithium ion secondary batteries and all-solid-state lithium batteries have been developed that use aqueous electrolytes that are free from concerns about battery fires due to the flammability of organic solvents in non-aqueous electrolytes, and various improvements have been proposed for the solid electrolytes used therein, as well as new materials for the solid electrolytes themselves.

[0005] For example, Patent Document 1 proposes a non-aqueous electrolyte solution containing a complex compound represented by the following general formula as an electrolyte, which is disclosed to improve the initial resistance characteristics of an electricity storage device. X-(OA(Z)-OB - (Y)(F)M + -) n -R (X, Y, Z, and R are alkyl groups, A is P=O, and M is an alkali metal.)

[0006] In addition, Patent Document 2 discloses a compound having the general formula (1): M + PO 3 (F)A - (In the formula, M + is a monovalent metal, and A is a boron atom or a phosphorus atom.) It is disclosed that this complex compound has a partial structure represented by the following formula: where R is a monovalent metal, and A is a boron atom or a phosphorus atom. It is disclosed that this complex compound can improve the high-temperature charged storage characteristics of an electricity storage device, and in particular, can suppress an increase in resistance during storage.

[0007] Furthermore, Patent Document 3 discloses an electrolyte for an electricity storage device, which contains a lithium-containing complex compound represented by the following formula: (Li) m (A) n (U.F. x ) y (Li) m (Si) n (O) q (U.F. x ) y (A is O, S, P or N, U is B or P, m and n are 1 to 6, q is 1 to 12, x is 3 or 5, and y is 1 to 6.) (Li) m (O) n (B) p (OWF q ) x (W is B or P, m, p, and x are 1 to 15, n is 0 to 15, and q is 3 or 5.)

[0008] (Li) m (B) p (O) n (OR) y (OWF q ) x (W is B or P. n is 0 to 15, p, m, x, and y are 1 to 12, and q is 3 or 5. R is hydrogen, an alkyl group, or the like.) (Li) m (O) n (B) p (OOC-(A) z -COO) y (OWF q ) x (W is B or P. A is an alkylene group having 1 to 6 carbon atoms, etc. m, p, x, and y are 1 to 20, n is 0 to 15, z is 0 or 1, and q is 3 or 5.) It is disclosed that such an electrolyte can provide a nonaqueous electrolyte solution having low electrical resistance, and can provide an electricity storage device such as a lithium ion secondary battery having good initial characteristics and excellent cycle characteristics, and further, can provide an all-solid-state lithium secondary battery because the electrolyte itself has excellent lithium ion conductivity. However, sufficient improvements and new electrolytes have not yet been achieved. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. 2014 / 175225 [Patent Document 2] JP 2020-194771 A [Patent Document 3] International Publication No. 2019 / 180945 Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention aims to provide an electrolyte, a reinforcing agent, and an electrolytic solution capable of producing an electricity storage device having an excellent balance of solubility in organic solvents (nonaqueous solvents), charge / discharge efficiency, -10°C resistance, cycle characteristics (volume change rate, capacity retention rate, resistance change rate), and high-temperature characteristics, as well as an electricity storage device produced using these, and further a method for producing a lithium boron fluoride complex compound and a lithium complex compound for the above electrolyte or reinforcing agent. [Means for solving the problem]

[0011] Therefore, in order to solve the above problems, the present inventors have discovered a novel electrolyte for use in an electricity storage device, which contains a specific complex compound, and have arrived at the present invention based on this discovery. That is, the present invention is characterized in the following points. 1. An electrolyte for an electricity storage device, comprising a complex compound (A), The above electrolyte, wherein the complex compound (A) contains one or more complex compounds represented by the following formula (1): [ka] (In formula (1), X 1 is a P(=O) or P(=S) group, R 1 ~R 3 are each independently one group selected from the group consisting of a hydrogen atom, an alkyl group, an alkenyl group, a halogen atom, an alkoxy group, a siloxy group, a thiosilane group, and a group represented by the following formula (2), or R 1 ~R 3 one of the two groups selected from the group consisting of is an oxygen atom and is bonded to the other to form a ring structure, R 1 ~R 3 At least one of the above is a group containing a structure represented by the following formula (2): [ka] (Formula (2) represents an oligomer having a structure in which each repeating unit shown in [ ] is linked, and the linking order of each repeating unit is arbitrary. l is [ ] l represents the number of repeats of the repeating unit enclosed in (a) and is a number from 1 to 10, m is [ ] m represents the number of repeats of the repeating unit enclosed in (a) and is a number from 0 to 10. n is [ ] n represents the number of repeats of the repeating unit enclosed in (a) and is a number from 0 to 10. M + is an alkali metal cation or a quaternary ammonium cation, Y 1 ~Y 3 are each independently an oxygen atom or a sulfur atom, B is a boron atom, G is a halogen atom; X 2is a boron atom, a P(=O) group or a P(=S) group, Z indicates that the preceding and following groups are directly connected, or is a group selected from the group consisting of a substituted or unsubstituted alkylene group, an alkenylene group, a phenylene group, and an alkylene group having an ether group or a thioether group in the main chain; R 4 are each independently a hydrogen atom, an alkyl group, an alkenyl group, a halogen atom, an alkoxy group, a siloxy group, or a thiosilane group. 2. The electrolyte according to 1 above, characterized in that the complex compound has at least one boron halide group. 3. The electrolyte according to 1 above, characterized in that the complex compound has at least one of the siloxy group and / or the thiosilane group. 4. The complex compound is At least one boron halide group; At least one of the siloxy groups and / or thiosilane groups 2. The electrolyte according to claim 1, characterized in that it has 5. The electrolyte according to the above item 1, wherein the complex compound comprises one or more complex compounds selected from the group consisting of complex compounds represented by the following formulas (3) to (14): [ka] [ka] 6. A reinforcing agent for an electricity storage device, comprising the complex compound (A) according to any one of 1 to 5 above. 7. An electrolytic solution for an electricity storage device, comprising at least the complex compound (A) according to any one of 1 to 5 above and an organic solvent, The above electrolyte, characterized in that the concentration of the alkali metal cation or quaternary ammonium cation derived from the complex compound (A) in the entire electrolyte is 0.01 mol / L or more and 2.0 mol / L or less. 8. An electrolytic solution for an electricity storage device, comprising at least the complex compound (A) according to any one of 1 to 5 above and an organic solvent, The above electrolytic solution, characterized in that the concentration of the complex compound (A) in the entire electrolytic solution is 0.1 mass % or more and 30 mass % or less. 9. An electricity storage device produced using the electrolyte solution according to 7 or 8 above. 10. An electricity storage device produced using the electrolyte according to any one of 1 to 5 above and / or the reinforcing agent according to 6 above. 11. A solid-state electricity storage device produced using the electrolyte according to any one of 1 to 5 above and / or the reinforcing agent according to 6 above. 12. A method for synthesizing the complex compound (A) according to any one of 1 to 5 above, comprising the steps of: The complex compound (A) contains a P(=O) group or a P(=S) group and / or a boron halide group, The production method includes a step 1 of carrying out a bonding reaction between a boron halide salt (E) and a phosphorus compound (F) by dehalogenation of silyl, The boron halide salt (E) is a salt consisting of an anion having two or more halogen atoms bonded to boron and an alkali metal cation or a quaternary ammonium cation, The method for producing the phosphorus-based compound (F) is characterized in that it is a compound having a siloxy group or a thiosilane group bonded to a P(=O) group or a P(=S) group. 13. After the step 1, a boron halide salt (E) and / or a phosphorus compound (F) 13. The method according to claim 12, further comprising one or more steps 2: adding an additional reaction raw material consisting of the following and proceeding with a bonding reaction by dehalogenation silyl. Effect of the Invention

[0012] According to the present invention, it is possible to obtain an electrolyte, a reinforcing agent, and an electrolytic solution capable of producing an electricity storage device having an excellent balance of solubility in organic solvents (nonaqueous solvents), charge / discharge efficiency, -10°C resistance value, cycle characteristics (volume change rate, capacity retention rate, resistance change rate), and high-temperature characteristics, as well as electricity storage devices produced using these, and further, a method for producing a lithium boron fluoride complex compound and a lithium complex compound for the above-mentioned electrolyte or reinforcing agent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in more detail below. The following description of the constituent elements is an example of an embodiment of the present invention, and the present invention is not limited to these contents as long as it does not exceed the gist of the present invention.

[0014] <Electrolytes> The electrolyte of the present invention is an electrolyte for an electricity storage device, and contains a specific complex compound (A).

[0015] [Complex compound (A)] The complex compound (A) in the present invention is a complex compound used in an electrolyte for an electricity storage device, and preferably contains one or more complex compounds represented by the following formula (1).

[0016] [ka] (In formula (1), X 1 is a P(=O) or P(=S) group, R 1 ~R 3 are each independently one group selected from the group consisting of a hydrogen atom, an alkyl group, an alkenyl group, a halogen atom, an alkoxy group, a siloxy group, a thiosilane group, and a group represented by the following formula (2), or R 1 ~R 3 one of the two groups selected from the group consisting of is an oxygen atom and is bonded to the other to form a ring structure, R 1 ~R 3At least one of the above is a group containing a structure represented by the following formula (2): [ka] (Formula (2) represents an oligomer having a molecular structure in which each repeating unit shown in [ ] is linked, and the linking order of each repeating unit is arbitrary. l is [ ] l represents the number of repeats of the repeating unit enclosed in (a) and is a number from 1 to 10, m is [ ] m represents the number of repeats of the repeating unit enclosed in (a) and is a number from 0 to 10. n is [ ] n represents the number of repeats of the repeating unit enclosed in (a) and is a number from 0 to 10. M + is an alkali metal cation or a quaternary ammonium cation, Y 1 ~Y 3 are each independently an oxygen atom or a sulfur atom, B is a boron atom, G is a halogen atom; X 2 is a boron atom, a P(=O) group or a P(=S) group, Z indicates that the preceding and following groups are directly connected, or is a group selected from the group consisting of a substituted or unsubstituted alkylene group, an alkenylene group, a phenylene group, and an alkylene group having an ether group or a thioether group in the main chain; R 4 are each independently a hydrogen atom, an alkyl group, an alkenyl group, a halogen atom, an alkoxy group, a siloxy group, or a thiosilane group. Here, the halogenated boron group is a group in which at least one halogen atom is bonded to a boron atom. Moreover, it is more preferable that the complex compound (A) has at least one siloxy group and / or one thiosilane group. Furthermore, it is more preferable that the complex compound (A) has at least one or more boron halide groups and at least one or more siloxy groups and / or thiosilane groups.

[0017] In the above formula (1), M + Specific examples of alkali metal cations or quaternary ammonium cations represented by the formula: Li + ,Na + ,K + ,Rb + ,Cs + ,Fr + , NH4 + Among these, Li + ,NH 4 + is preferred.

[0018] R 1 ~R 3 , R 4 The alkyl groups in are each independently preferably a chain or cyclic alkyl group having 1 to 8 carbon atoms. Specific examples include a methyl group, an ethyl group, a propyl group, a butyl group, a hexyl group, a cyclopropyl group, a cyclobutyl group, a cyclohexyl group, a hydroxyethyl group, a trifluoromethyl group, and a hexafluoroethyl group.

[0019] R 1 ~R 3 , R 4 Each of the alkenyl groups in the formula (I) is preferably an alkenyl group having a carbon number of 2 to 5. Specific examples include a vinyl group, a propenyl group, a butenyl group, and a heptenyl group.

[0020] G, R 4 Specific examples of the halogen atom in include F, Cl, Br, I, and At. Among these, F and Cl are preferred because they have stable bonds with phosphorus and boron atoms.

[0021] R 1 ~R 3 , R 4The alkoxy groups in are each preferably an alkoxy group having a carbon number of 2 to 5. Specific examples include a methoxy group, an ethoxy group, and a butoxy group.

[0022] R 1 ~R 3 , R 4 Examples of the siloxy group in the formula (I) include a trimethylsiloxy group, a triethylsiloxy group, a triisopropylsiloxy group, a butyldimethylsiloxy group, a tributylsiloxy group, a trimethoxysiloxy group, a triethoxysiloxy group, and a tributoxysiloxy group.

[0023] R 1 ~R 3 , R 4 Examples of the thiosilane group in the formula (I) include a trimethylthiosilane group, a triethylthiosilane group, a triisopropylthiosilane group, a butyldimethylthiosilane group, a tributylthiosilane group, a trimethoxythiosilane group, a triethoxythiosilane group, and a tributoxythiosilane group.

[0024] [ ] m The repeating unit -Y 2 Z in -CO-Z-CO- represents a state in which CO and CO are directly bonded, or represents a substituted or unsubstituted alkylene group, alkenylene group, a phenylene group, and an alkylene group having an ether group or a thioether group in the main chain. Specific examples of Z include an alkylene group having 1 to 12 carbon atoms, an alkenylene group having an unsaturated bond containing 2 to 8 carbon atoms, a phenylene group, an ether group having 2 to 6 carbon atoms and containing oxygen in the main chain, and a thioether group having 2 to 6 carbon atoms and containing sulfur in the main chain. And -Y 2 Specific examples of CO-Z-CO- include -Y 2 CO-CO-, -Y 2 CO-(CH 2 )-CO-, -Y 2 CO-(CH 2 ) 2 -CO-, -Y 2 CO-(CH2 ) 3 -CO-, -Y 2 CO-(CH 2 ) 4 -CO-, -Y 2 CO-(CH 2 ) 8 -CO-, -Y 2 CO-(CH=CH)-CO-, -Y 2 CO-(C 6 H 4 )-CO-, -Y 2 CO-(CH 2 OCH 2 )-CO-, -Y 2 CO-(CH 2 CH 2 OCH 2 CH 2 )-CO-, -Y 2 CO-(CH 2 SCH 2 )-CO-, -Y 2 CO-(CH 2 CH 2 SCH 2 CH 2 )-CO-, etc.

[0025] Specific examples of the complex compound (A) represented by the above formula (1) include complex compounds represented by the following formulae (3) to (14) and complex compounds containing a P(=O) group or a P(=S) group and / or a boron halide group. The electrolyte of the present invention preferably contains one or more complex compounds (A) selected from the group consisting of these. [ka] [ka]

[0026] The above formulas (3), (4), and (14) are O and B - This shows that the and are bonded to form a ring structure.

[0027] <Method for producing complex compound (A)> A method for producing the complex compound (A) will be described below when the complex compound (A) is a complex compound containing a P(=O) group or a P(=S) group, and / or a boron halide group. A complex compound containing a P(=O) group or a P(=S) group, and / or a boron halide group can be synthesized by a method including the following step 1, or a method including step 1 and one or more steps 2 in this order.

[0028] (Process 1) A step of carrying out a bonding reaction between the boron halide salt (E) and the phosphorus compound (F) by dehalogenation of silyl. (Process 2) A step of adding additional reaction raw materials consisting of a boron halide salt (E) and / or a phosphorus compound (F) after the step 1 to advance a bonding reaction by dehalogenation of silyl. The above-mentioned dehalogenation silyl reaction proceeds even in the absence of a solvent, but a suitable solvent may be used as necessary. In addition, the dehalogenation silyl reaction can be efficiently carried out by controlling the reaction temperature. The reaction temperature is not particularly limited as long as it is a temperature at which the dehalogenation silyl reaction can be efficiently carried out. For example, it can be selected in the range of 10 to 150°C depending on the solvent used, and the reaction can be suitably promoted in the range of 20 to 120°C. In addition, from the viewpoint of ease of control of the reaction rate, the range of 40 to 100°C is more preferable, but is not limited to these conditions.

[0029] The molar ratio of the boron atoms in the boron halide salt (E) to the silyl groups in the phosphorus compound (F) [boron atoms in (E) / silyl groups in (F)] in step 1 can be appropriately selected depending on the chemical structure of the complex compound (A) to be obtained, and is not particularly limited. For example, the molar ratio [boron atom (E) / silyl group (F)] is preferably 0.2 or more and 5 or less, more preferably 0.3 or more and 3.0 or less. If the molar ratio [boron atom (E) / silyl group (F)] is smaller than the above range, the amount of unreacted silyl groups increases, and the solubility of the complex compound (A) is likely to decrease. If it is larger than the above range, the amount of unreacted boron halide salt (E) increases, which may reduce the life performance of the battery.

[0030] In step 2, the amount of the boron halide salt (E) or the phosphorus compound (F) to be added can be appropriately selected depending on the chemical structure of the complex compound (A) to be obtained. The type, amount and order of addition of the boron halide salt (E) or the phosphorus compound (F) are not particularly limited. For example, in step 1, the molar ratio of the silyl group in the added phosphorus compound (F) or the boron atom in the added boron halide salt (E) to the unreacted boron atom in the boron halide salt (E) or the unreacted silyl group in the phosphorus compound (F), respectively [{silyl group in the added (F)+boron atom in the added (E)} / {unreacted boron atom in (E)+unreacted silyl group in (F)}] is preferably 0.2 or more and 5 or less, more preferably 0.3 or more and 3.0 or less.

[0031] The molar ratio [boron atom (E) / silyl group (F)] in all steps including step 1 and step 2 is, for example, preferably 0.2 or more and 5.0 or less, more preferably 0.3 to 3.0 or less.

[0032] (Boron halide salts (E)) The boron halide salt (E) is a salt that comprises an anion having two or more halogen atoms bonded to boron and an alkali metal cation or a quaternary ammonium cation, and is capable of undergoing a dehalogenation silyl reaction. Examples of the boron halide salt (E) include, but are not limited to, complex salts containing a boron dihalide or boron trihalide functional group in the molecule, tetrahalide borates, monohalide phosphates, dihalide phosphates, and hexahalide phosphates.

[0033] Specific examples of boron halide salts (E) include tetrahalogenated boron salts, lithium oxide·bis(boron trihalide) salts, lithium sulfide·bis(boron trihalide) salts, oxalate·boron trihalide complex salts, maleate·boron trihalide complex salts, fumarate·boron trihalide complex salts, citraconate·boron trihalide complex salts, adipate·boron trihalide complex salts, glutarate·boron trihalide complex salts, succinate·boron trihalide complex salts, tartrate·boron trihalide complex salts, malonate·boron trihalide complex salts, glycolate·boron trihalide complex salts, diglycolate·boron trihalide complex salts, thiodiacetate·boron trihalide complex salts, thiodipropion ... Carboxylic acid complex salts such as phosphinate-boron trihalide complex salts, phosphinate-boron trihalide complex salts, dimethylphosphinate-boron trihalide complex salts, difluorophosphate-boron trihalide complex salts, phosphonate-boron trihalide complex salts, methylphosphonate-boron trihalide complex salts, vinylphosphonate-boron trihalide complex salts, fluorophosphate-boron trihalide complex salts, phosphate-boron trihalide complex salts, methyl phosphate-boron trihalide complex salts, ethyl phosphate-boron trihalide complex salts, diphosphate-boron trihalide complex salts, polyphosphate-boron trihalide complex salts Examples of the phosphoric acid complex salt include, but are not limited to, condensed phosphoric acid complex salts such as uranyl complex salts, thiophosphate complex salts such as monothiophosphate-boron trihalide complex salts, dithiophosphate-boron trihalide complex salts, trithiophosphate-boron trihalide complex salts, and tetrathiophosphate-boron trihalide complex salts, and reaction products of these with a phosphorus compound (F) containing an anion having two or more halogen atoms bonded to boron.

[0034] The halogen is preferably fluorine, and the cation is preferably a lithium cation or a sodium ion. Specific examples of such a compound include lithium tetrafluoroborate, lithium oxide bis(boron trifluoride) salt, lithium sulfide bis(boron trifluoride) salt, lithium tetrafluoroborate salt, lithium oxalate bis(boron trifluoride) complex salt, lithium maleate bis(boron trifluoride) complex salt, lithium fumarate bis(boron trifluoride) complex salt, lithium citraconic acid bis(boron trifluoride) complex salt, lithium aconitic acid bis(boron trifluoride) complex salt, and lithium thiodiacetate bis(boron trifluoride) complex salt. , lithium thiopropionate bis(boron trifluoride) complex salt, lithium adipate bis(boron trifluoride) complex salt, lithium glutarate bis(boron trifluoride) complex salt, lithium succinate bis(boron trifluoride) complex salt, lithium tartrate bis(boron trifluoride) complex salt, lithium malonate bis(boron trifluoride) complex salt, lithium glycolate bis(boron trifluoride) complex salt, lithium diglycolate bis(boron trifluoride) complex salt, lithium borate tris(boron trifluoride) complex salt, Lithium phosphate tris(boron trifluoride) complex salt, Lithium monothiophosphate tris(boron trifluoride) complex salt, Lithium dithiophosphate tris(boron trifluoride) complex salt, Lithium trithiophosphate tris(boron trifluoride) complex salt, Lithium tetrathiophosphate tris(boron trifluoride) complex salt, Lithium phosphinate boron trifluoride complex salt, Lithium dimethylphosphinate boron trifluoride complex salt, Lithium difluorophosphate boron trifluoride complex salts, lithium fluorophosphate boron trifluoride complex salts, lithium phosphonate bis(boron trifluoride) complex salts, lithium methylphosphonate bis(boron trifluoride) complex salts, lithium vinylphosphonate bis(boron trifluoride) complex salts, and reaction products of these with a phosphorus compound (F) containing an anion having two or more halogen atoms bonded to boron, but are not limited to these. Among these, lithium sulfide bis(boron trifluoride) complex salt, lithium oxide bis(boron trifluoride) complex salt, lithium tetrafluoroborate salt, lithium oxalate bis(boron trifluoride) complex salt, lithium maleate bis(boron trifluoride) complex salt, lithium citraconic acid bis(boron trifluoride) complex salt, lithium adipate bis(boron trifluoride) complex salt, lithium thiodiacetate bis(boron trifluoride) complex salt, lithium borate tris(boron trifluoride) complex salt, lithium difluorophosphate boron trifluoride complex salt, lithium fluorophosphate tris(boron trifluoride) complex salt, Preferred are boron fluoride complex salts, lithium phosphonate bis(boron trifluoride) complex salts, lithium methylphosphonate bis(boron trifluoride) complex salts, lithium vinylphosphonate bis(boron trifluoride) complex salts, lithium phosphate tris(boron trifluoride) complex salts, lithium monothiophosphate tris(boron trifluoride) complex salts, lithium dithiophosphate tris(boron trifluoride) complex salts, lithium trithiophosphate tris(boron trifluoride) complex salts, lithium tetrathiophosphate tris(boron trifluoride) complex salts, and reaction products of these with a phosphorus compound (F).

[0035] (phosphorus compound (F)) The phosphorus-based compound (F) is a compound having a siloxy group or a thiosilane group bonded to a P(=O) group or a P(=S) group, and preferably has two or more of the siloxy groups or thiosilane groups. Specific examples of the phosphorus compound (F) include bis(trimethylsilyl) vinyl phosphonate, tris(trimethylsilyl) phosphate, trimethylsilyl phosphinate, trimethylsilyl dimethyl phosphinate, bis(trimethylsilyl) phosphonate, and bis(aryl phosphonate). Examples of the reaction products of these with a boron halide salt (E) include, but are not limited to, tris(trimethylsilyl) diphosphate, hexa(trimethylsilyl) diphosphate, tris(trimethylsilyl) polyphosphate, tris(trimethylsilyl) monothiophosphate, tris(trimethylsilyl) dithiophosphate, tris(trimethylsilyl) trithiophosphate, tris(trimethylsilyl) tetrathiophosphate, and reaction products of these with a boron halide salt (E) having a siloxy group or a thiosilane group bonded to a P(=O) group or a P(=S) group. Among these, bis(trimethylsilyl) vinylphosphonate, bis(trimethylsilyl) phosphonate, tris(trimethylsilyl) phosphate, hexa(trimethylsilyl) diphosphate, tris(trimethylsilyl) polyphosphate, and the like are preferred.

[0036] <Reinforcement agent> In the present invention, the reinforcing agent is a compound that imparts effects such as increasing the charge / discharge efficiency of the battery, extending the battery life, and lowering the resistance. The strengthening agents of the present invention may be used with the electrolytes of the present invention. Additionally, the reinforcing agent of the present invention may be used with lithium-based electrolytes other than those of the present invention. Furthermore, the reinforcing agent of the present invention can be used in combination with a general-purpose reinforcing agent. As long as the reinforcing agent and the general-purpose reinforcing agent are mutually compatible, they can be used in any ratio. There is no limitation here. For example, the content of the reinforcing agent of the present invention in the total reinforcing agents contained in the battery is preferably 0.1 mass% or more and 100 mass% or less, more preferably 0.2 mass% or more and 70 mass% or less. Specific examples of general-purpose toughening agents include, but are not limited to, sulfur-containing compounds, cyclic acid anhydrides, nitrile compounds, and isocyanate compounds.

[0037] Examples of the sulfur-containing compound include 1,3-propane sultone (PS), propene sultone, ethylene sulfite, hexahydrobenzo[1,3,2]dioxathiolane-2-oxide (also referred to as 1,2-cyclohexanediol cyclic sulfite), 5-vinyl-hexahydro-1,3,2-benzodioxathiol-2-oxide, 1,4-butanediol dimethanesulfonate, 1,3-butanediol dimethanesulfonate, methylenemethane disulfonic acid, ethylenemethane disulfonic acid, N,N-dimethylmethanesulfonamide, N,N-diethylmethanesulfonamide, divinyl sulfone, and 1,2-bis(vinylsulfonyl)methane.

[0038] Examples of the cyclic acid anhydrides include glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, succinic anhydride, diglycolic anhydride, cyclohexanedicarboxylic anhydride, cyclopentanetetracarboxylic dianhydride, 4-cyclohexene-1,2-dicarboxylic anhydride, 3,4,5,6-tetrahydrophthalic anhydride, 5-norbornene-2,3-dicarboxylic anhydride, phenylsuccinic anhydride, 2-phenylglutaric anhydride, phthalic anhydride, pyromellitic anhydride, fluorosuccinic anhydride, and tetrafluorosuccinic anhydride. carboxylic acid anhydrides such as 1,2-ethanedisulfonic acid anhydride, 1,3-propanedisulfonic acid anhydride, 1,4-butanedisulfonic acid anhydride, 1,2-benzenedisulfonic acid anhydride, tetrafluoro-1,2-ethanedisulfonic acid anhydride, hexafluoro-1,3-propanedisulfonic acid anhydride, octafluoro-1,4-butanedisulfonic acid anhydride, 3-fluoro-1,2-benzenedisulfonic acid anhydride, 4-fluoro-1,2-benzenedisulfonic acid anhydride, and 3,4,5,6-tetrafluoro-1,2-benzenedisulfonic acid anhydride.

[0039] Examples of the nitrile compound include pentanenitrile, octanenitrile, decanenitrile, dodecanenitrile, crotononitrile, succinonitrile, glutaronitrile, adiponitrile, pimelonitrile, suberonitrile, and glutaronitrile.

[0040] Examples of the isocyanate compound include alkyl isocyanates such as methyl isocyanate, ethyl isocyanate, propyl isocyanate, isopropyl isocyanate, butyl isocyanate, and tertiary butyl isocyanate, cycloalkyl isocyanates such as cyclohexyl isocyanate, allyl isocyanate, propargyl isocyanate, monomethylene diisocyanate, dimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, octamethylene diisocyanate, decamethylene diisocyanate, and 1,4-diisocyanate. Examples of compounds include anthra-2-butene, toluene diisocyanate, xylylene diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 1,4-diisocyanatocyclohexane, dicyclohexylmethane-4,4'-diisocyanate, bicyclo[2.2.1]heptane-2,5-diylbis(methylisocyanate), bicyclo[2.2.1]heptane-2,6-diylbis(methylisocyanate), isophorone diisocyanate, carbonyl diisocyanate, 1,4-diisocyanatobutane-1,4-dione, and trimethylhexamethylene diisocyanate.

[0041] <Electrolyte> The electrolyte solution of the present invention is a liquid for use in an electricity storage device that contains an electrolyte and an organic solvent (non-aqueous solvent), and may further contain a reinforcing agent.

[0042] The electrolytic solution of the present invention may contain the complex compound (A) as an electrolyte and / or a reinforcing agent. The electrolytic solution of the present invention may contain an electrolyte other than the complex compound (A) and / or a reinforcing agent.

[0043] Cations are present in the electrolyte solution, and these cations preferably include lithium cations, sodium cations, or quaternary ammonium cations, more preferably include lithium cations or sodium cations, and particularly preferably include lithium cations. is more preferred.

[0044] A specific example of the electrolyte other than the complex compound (A) is LiPF 6 , LiBF 4 , LiN(FSO 2 ) 2 , LiN(CF 3 SO 2 ) 2 , LiN(C 2 F 5 SO 2 ) 2 , LiN(CF 3 SO 2 )(C 2 F 5 SO 2 ) or LiN(CF 3 SO 2 )(C 4 F 9 SO 2 ) and the like, but are not limited to these.

[0045] The concentration of all cations in the entire electrolyte, particularly the concentration of all lithium cations, is preferably 0.1 mol / L or more and 5.0 mol / L or less, more preferably 0.7 mol / L or more and 2.5 mol / L or less. If the concentration of alkali metal cations or quaternary ammonium cations in the entire electrolyte is lower than the above range, it is difficult to have sufficient charge / discharge characteristics, and even if it is higher than the above range, the internal resistance is likely to increase and the charge / discharge characteristics are not significantly improved.

[0046] The concentration of all cations derived from complex compound (A) in the entire electrolyte, particularly lithium cations, is preferably 0.01 mol / L or more and 3.0 mol / L or less, more preferably 0.1 mol / L or more and 2.0 mol / L or less, in the entire electrolyte. If the concentration of all cations derived from complex compound (A) in the electrolyte, particularly lithium cations, is lower than the above range, the protection of the electrode surface of the electricity storage device is likely to be insufficient. If the concentration is higher than the above range, the lithium ion conductivity of the electrolyte is not significantly improved.

[0047] The mass% of the complex compound (A) in the entire electrolyte is 0.01 mass% or more and 30 mass% or more. If the mass % of the complex compound (A) in the entire electrolyte is lower than the above range, the protection of the electrode surface of the electricity storage device is likely to be insufficient, and if it is higher than the above range, the lithium ion conductivity of the electrolyte is not significantly improved.

[0048] [Organic solvents] As the organic solvent for the electrolyte of the present invention, various organic solvents can be used. For example, aprotic polar solvents can be preferably used. Among aprotic polar solvents, from the viewpoint of increasing ion conductivity, it is more preferable to use carbonate-based solvents such as cyclic carbonates and chain carbonates, and it is even more preferable to use a combination of cyclic carbonates and chain carbonates. In addition, it is particularly preferable to use saturated cyclic carbonates and unsaturated cyclic carbonates as cyclic carbonates, and to contain three kinds of carbonates. When cyclic carbonates and / or chain carbonates are used, other non-aqueous solvents such as lactones, sulfones, ethers, nitriles, chain carboxylate esters, chain glycol ethers, fluorine-containing ethers, and phosphate esters can be further added as necessary.

[0049] The volume ratio of cyclic carbonates / chain carbonates in the electrolyte can be any ratio as long as the lithium ion conductivity is sufficiently high. It is not particularly limited. For example, the volume ratio of saturated cyclic carbonates / chain carbonates is preferably 10 / 90 to 70 / 30, more preferably 20 / 80 to 50 / 50. As the cyclic carbonates, unsaturated cyclic carbonates can be used. The content of the unsaturated cyclic carbonates is preferably from 0.01 to 10% by volume, and more preferably from 0.1 to 5% by volume, in the total amount of the organic solvent.

[0050] If the amount of the cyclic carbonates is less than the above range, the degree of dissociation and solubility of the complex compound as an electrolyte tend to decrease, and the ionic conductivity of the electrolyte tend to decrease. Conversely, if the amount of the cyclic carbonates is more than the above range, the electrolyte tend to have a high viscosity and tend to solidify at low temperatures, making it difficult to obtain sufficient charge / discharge characteristics.

[0051] If the amount of the chain carbonate is less than the above range, the electrolyte solution tends to have a high viscosity and tends to solidify at low temperatures, making it difficult to obtain sufficient charge / discharge characteristics.On the other hand, if the amount of the chain carbonate is more than the above range, the dissociation degree and solubility of the complex compound, which is the electrolyte, tend to decrease, making the ionic conductivity of the electrolyte solution prone to decrease.

[0052] If the amount of the unsaturated cyclic carbonate is less than the above range, it is difficult to form a good coating on the surface of the negative electrode, which leads to a deterioration in cycle characteristics, whereas if the amount of the unsaturated cyclic carbonate is more than the above range, it is easy for gas to be generated from the electrolyte during high-temperature storage, which leads to an increase in pressure inside the electricity storage device, which is undesirable for practical use.

[0053] Specific examples of aprotic polar solvents include cyclic carbonates, chain carbonates, lactones, sulfones, cyclic ethers, chain ethers, nitriles, chain carboxylates, chain glycol ethers, fluorine-containing ethers, phosphorus-containing compounds, dimethyl sulfoxide, dichloroethane, chlorobenzene, and nitrobenzene. These can be used alone or in combination of two or more.

[0054] Specific examples of cyclic carbonates include ethylene carbonate, propylene carbonate, 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, trifluoromethylethylene carbonate, fluoroethylene carbonate, and 4,5-difluoroethylene carbonate. Among these, ethylene carbonate, propylene carbonate, and fluoroethylene carbonate are preferred. When propylene carbonate is used, a stable electrolyte solution can be obtained in a wide temperature range. These specific compounds can be used alone or in combination of two or more.

[0055] Examples of the chain carbonates include chain carbonates having 3 to 9 carbon atoms, and specific examples include ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, methyl propyl carbonate, dipropyl carbonate, methyl butyl carbonate, dibutyl carbonate, ethyl propyl carbonate, and methyl trifluoroethyl carbonate. In the above, the propyl groups may be independently n-propyl or isopropyl groups, and the butyl groups may be independently n-butyl, isobutyl, or t-butyl groups. Among these, ethyl methyl carbonate, dimethyl carbonate, and diethyl carbonate are preferred. These specific compounds may be used alone or in combination of two or more.

[0056] Specific examples of unsaturated cyclic carbonates include vinylene carbonate derivatives and alkenyl ethylene carbonate.

[0057] Specific examples of vinylene carbonate derivatives include vinylene carbonate, fluorovinylene carbonate, methylvinylene carbonate, fluromethylvinylene carbonate, ethylvinylene carbonate, propylvinylene carbonate, butylvinylene carbonate, dimethylvinylene carbonate, diethylvinylene carbonate, and dipropylvinylene carbonate.

[0058] Specific examples of alkenyl ethylene carbonate include 4-vinyl ethylene carbonate, 4-vinyl-4-methyl ethylene carbonate, 4-vinyl-4-ethyl ethylene carbonate, 4-vinyl-4-n-propyl ethylene carbonate, etc. These specific compounds can be used alone or in combination of two or more.

[0059] Examples of cyclic carboxylates (lactones) include those having 3 to 9 carbon atoms, such as γ-butyrolactone, γ-valerolactone, γ-caprolactone, and ε-caprolactone. Among these, γ-butyrolactone and γ-valerolactone are more preferred. These specific compounds can be used alone or in combination of two or more.

[0060] The chain carboxylates include those having 3 to 9 carbon atoms, and specific examples thereof include methyl acetate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, t-butyl acetate, methyl propionate, ethyl propionate, n-propyl propionate, isopropyl propionate, n-butyl propionate, isobutyl propionate, and t-butyl propionate. Among these, ethyl acetate, methyl propionate, and ethyl propionate are preferred. These specific compounds can be used alone or in combination of two or more.

[0061] The chain glycol ethers include those having 3 to 6 carbon atoms, and specific examples thereof include dimethoxymethane, dimethoxyethane, diethoxymethane, diethoxyethane, ethoxymethoxymethane, ethoxymethoxyethane, etc. Among these, dimethoxyethane and diethoxyethane are more preferable. These specific compounds can be used alone or in combination of two or more.

[0062] Specific examples of fluorine-containing ethers include 1,1,2,2-tetrafluoroethyl-2, Examples of the compounds include 2,3,3-tetrafluoropropyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3,3-pentafluoropropyl ether, ethoxy-2,2,2-trifluoroethoxy-ethane, etc. These specific compounds may be used alone or in combination of two or more.

[0063] Specific examples of sulfones include dimethyl sulfone, diethyl sulfone, ethyl methyl sulfone, methyl propyl sulfone, sulfolane, 2-methyl sulfolane, and 3-methyl sulfolane. Specific examples of cyclic ethers include tetrahydrofuran, 2-methyltetrahydrofuran, dioxane, dioxolane, and 4-methyldioxolane. Specific examples of chain ethers include dimethyl ether. Specific examples of nitriles include acetonitrile, succinonitrile, adiponitrile, and benzonitrile. Specific examples of amides include N,N-dimethylformamide and dimethylacetamide. Specific examples of phosphorus-containing compounds include diethyl vinyl phosphate, allyl diethyl phosphate, propargyl diethyl phosphate, trivinyl phosphate, triallyl phosphate, tripropargyl phosphate, diallyl ethyl phosphate, dipropargyl ethyl phosphate, 2-acryloyloxyethyl diethyl phosphate, and tris(2-acryloyloxyethyl)phosphate.

[0064] <Electricity storage device> The electricity storage device of the present invention is an electricity storage device produced using the electrolytic solution of the present invention, or an electricity storage device produced using the electrolyte and / or reinforcing agent of the present invention. The electricity storage device of the present invention may be any of a liquid-based electricity storage device, a semi-solid-based electricity storage device, and a solid-based electricity storage device. Specific examples of the electricity storage device of the present invention include various electricity storage devices such as a lithium ion secondary battery, an electric double layer capacitor, and a hybrid battery in which one of the positive electrode or negative electrode is a battery and the other is a double layer. The shape of the electricity storage device of the present invention is not particularly limited, and it may be in various shapes such as a cylindrical shape, a square shape, an aluminum laminate shape, a coin shape, a button shape, or the like. The electricity storage device of the present invention is produced using the electrolyte, electrolytic solution, reinforcing agent, etc. of the present invention, and therefore has low electrical resistance and is excellent in initial characteristics, cycle characteristics, and high-temperature characteristics. The electricity storage device of the present invention can also be produced by using electrolytes, electrolytic solutions, reinforcing agents, etc. other than the electrolyte, electrolytic solution, and reinforcing agent of the present invention in combination.

[0065] Hereinafter, a lithium ion secondary battery will be described as an example. A lithium-ion secondary battery is a secondary battery that charges and discharges by the movement of lithium ions between a positive electrode and a negative electrode, and is composed of a positive electrode, a negative electrode, a separator, an electrolyte (electrolytic solution), etc.

[0066] (Negative electrode) The negative electrode may have a configuration in which a negative electrode active material is formed on a current collector such as copper foil, expanded metal, carbon material, or a composite material thereof. Examples of negative electrode active materials constituting the negative electrode include carbon materials capable of being doped / dedoped with lithium ions, metallic lithium, lithium-containing alloys, or silicon capable of being alloyed with lithium, silicon alloys, tin, tin alloys, tin oxides capable of being doped / dedoped with lithium ions, silicon oxides, transition metal oxides capable of being doped / dedoped with lithium ions, transition metal nitrogen compounds capable of being doped / dedoped with lithium ions, and mixtures thereof.

[0067] In order to improve the adhesion of the negative electrode active material to the current collector, for example, a polyvinylidene fluoride binder, a latex binder, or the like may be contained, and carbon black, amorphous whisker carbon, carbon nanofiber, or the like may be contained as a conductive assistant.

[0068] Examples of carbon materials constituting the negative electrode active material include pyrolytic carbons, cokes (pitch coke, needle coke, petroleum coke, etc.), graphites, fired organic polymer compounds (phenolic resins, furan resins, etc., fired at an appropriate temperature to be carbonized), carbon fibers, activated carbon, graphite (natural graphite, artificial graphite, carbon-coated graphite, graphite-coated graphite, resin-coated graphite, etc.), and the like.

[0069] The carbon material is preferably one in which the interplanar spacing (d002) of the (002) plane measured by X-ray diffraction is 0.340 nm or less. And the true density is 1.70g / cm 3 Graphite having the above properties or a highly crystalline carbon material having properties similar thereto is preferred. By using such carbon materials in the negative electrode, the energy density of the nonaqueous electrolyte storage device can be increased.

[0070] Further, the carbon material may contain boron, be coated with a metal such as gold, platinum, silver, copper, Sn, or Si, or be coated with a salt such as a magnesium salt or a calcium salt, etc. These carbon materials may be used alone or in combination of two or more.

[0071] In addition, when silicon, silicon alloys, tin, tin alloys, which can be alloyed with lithium, tin oxide, silicon oxide, which can be doped and dedoped with lithium ions, transition metal oxides, which can be doped and dedoped with lithium ions, etc. are used, they all have a higher theoretical capacity per weight than the above-mentioned carbon materials and are therefore preferable.

[0072] (positive electrode) The positive electrode may have a configuration in which a positive electrode active material is formed on a current collector such as aluminum, titanium, or stainless steel foil, or an expanded metal, a carbon material, or a composite material thereof. The positive electrode active material constituting the positive electrode can be formed from various materials capable of charging and discharging, such as lithium-containing transition metal oxides, lithium-containing transition metal composite oxides using one or more transition metals, transition metal oxides, transition metal sulfides, metal oxides, and olivine-type metal lithium salts.

[0073] For example, LiCoO 2 , LiNiO 2 , LiMn 2 O 4 , LiMnO 2 Li, etc. x MO 2 (where M is one or more transition metals, and x is a value that varies depending on the charge / discharge state of the power storage device, and is usually 0.05≦x≦1.20) composite oxides of lithium and one or more transition metals (lithium transition metal composite oxides), metal composite oxides in which some of the transition metal atoms that are the main components of these lithium transition metal composite oxides are replaced with other metals such as Al, Ti, V, Cr, Mn, Fe, Co, Li, Ni, Cu, Zn, Mg, Ga, Zr, Si, Yb, etc., FeS 2 , TiS 2 , V 2 0 5 , MoO 3 , MoS 2 or a polymer such as polyacetylene or polypyrrole. Among these, materials such as lithium transition metal composite oxides that can be doped and dedoped with Li, and metal composite oxides in which some of the transition metal atoms are substituted with other metals, are preferred.

[0074] In addition, it is also possible to use a positive electrode active material having a substance of a different composition attached to the surface of the positive electrode active material. Examples of the substance attached to the surface include metal oxides, Examples of the metal sulfide include metal carbonate. Specific examples of metal oxides include aluminum oxide, silicon oxide, titanium oxide, zirconium oxide, magnesium oxide, calcium oxide, boron oxide, antimony oxide, and bismuth oxide. Specific examples of metal sulfides include lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, and aluminum sulfate. Specific examples of metal carbonates include carbonates such as lithium carbonate, calcium carbonate, and magnesium carbonate.

[0075] In order to improve the adhesion of the positive electrode active material to the current collector, for example, a polyvinylidene fluoride binder, a latex binder, or the like may be contained, and in order to improve the electronic conductivity within the positive electrode, carbon black, amorphous whiskers, graphite, carbon nanofibers, or the like may be contained.

[0076] (Separator) The separator serves to electrically insulate the positive electrode from the negative electrode, and is preferably a film that is permeable to lithium ions. Specific examples of the separator include porous membranes such as microporous polymer films. As the microporous polymer film, a porous polyolefin film is preferable, and specifically, a porous polyethylene film, a porous polypropylene film, or a multi-layer film of a porous polyethylene film and a porous polypropylene film is preferable. The separator may also be made of a polymer electrolyte, such as, but not limited to, a polymer substance having a lithium salt dissolved therein, or a polymer substance swollen with an electrolytic solution. EXAMPLES

[0077] <Synthesis of raw materials> [Production Example 1] In an argon atmosphere, 500 ml of methanol is placed in an Erlenmeyer flask and 20 g of lithium oxide (Li 2 O) was added to prepare a slurry. The slurry obtained above was cooled and BF 3 After the mixture was dropped into the flask, the mixture was stirred at 25° C. for 3 hours to obtain a reaction solution. Using an evaporator, methanol was removed from the reaction solution obtained, which was then washed three times with dibutyl ether and dried under reduced pressure to obtain 75 g of lithium oxide boron trifluoride complex salt (LiF 3 BOBF 3 Li) was obtained.

[0078] [Manufacturing Examples 2-10] The lithium oxide in Production Example 1 was changed to the compounds and amounts added as shown in Table 1, and the same procedure as in Production Example 1 was carried out to prepare each of the boron trifluoride complex salts of Production Examples 2 to 10.

[0079] [Table 1]

[0080] <Battery Construction> A battery for evaluating the electrolyte or the electrolyte solution containing the additive of the present invention was fabricated as follows.

[0081] (Preparation of positive electrode) The binder is polyvinylidene fluoride, the conductive agent is acetylene black, and the positive electrode active material is a composite oxide powder of lithium, nickel, manganese, and cobalt (LiNi 0.8 Mn 0.1 Co 0.1 O 2 ) was mixed in the ratio shown below to prepare a positive electrode mixture, to which N-methylpyrrolidone was added to prepare a paste. Polyvinylidene fluoride 2.0g Acetylene black 2.5g Cathode active material 95.5g The obtained paste was applied onto both sides of an aluminum foil current collector having a thickness of 18 μm, and after the solvent was dried and removed, the resulting mixture was rolled with a roll press to obtain a positive electrode.

[0082] (Preparation of negative electrode) The following ingredients were mixed together to prepare a slurry using water as a dispersion medium. Artificial graphitizable carbon powder 95.8g Styrene butadiene rubber (SBR) 2.0g Carboxymethylcellulose 2.2g The slurry obtained above was applied onto both sides of a copper foil having a thickness of 12 μm, and after the solvent was removed by drying, the resultant was rolled with a roll press to obtain a negative electrode.

[0083] (Battery cell manufacturing) The positive and negative electrodes obtained above were wound with a separator (F23DHA manufactured by Toray Battery Separator Film Co., Ltd.) having a thickness of 23 μm between them to prepare a flat wound electrode group, which was then placed in a case (50 mm long). The battery cells were then fabricated by placing the electrodes in a rectangular parallelepiped shape (40 mm wide x 40 mm wide x 2.0 mm thick).

[0084] (Production of lithium-ion secondary batteries) Using the battery cell produced above, a lithium ion secondary battery (laminate battery) was produced according to the following procedure. 1) 1.0 g of electrolyte was poured into the inlet of the battery cell, and after the pressure was reduced, the inlet was sealed. 2) The sealed battery cell was kept in an atmosphere of 25°C and charged to 4.2V at 20mA, and then discharged to 3.0V at 20mA. 3) The internal gas of the battery cell was removed by reducing pressure to obtain a battery.

[0085] <Various evaluation methods> [Initial charge / discharge efficiency] The battery cell thus prepared, filled and sealed, was charged in an atmosphere at 25° C. with a current of 20 mA until the voltage from 0 V rose to 4.2 V. Then, while maintaining the voltage at 4.2 V, charging was continued until the current value reached 4 mA, and the total current value consumed until the current value reached 4 mA was defined as the initial charge capacity value. Next, the charged electricity storage device was discharged to 3.0 V by applying a current of 20 mA in an atmosphere at 25° C., and the total current value consumed until the voltage reached 3.0 V was defined as the initial discharge capacity value. Then, the initial charge / discharge efficiency (%) was calculated using the following formula. Initial charge / discharge efficiency (%) = (initial discharge capacity / initial charge capacity value) x 100

[0086] [-10℃ resistance value] The lithium ion secondary battery prepared above was charged to a SOC (State of Charge) of 50% in an atmosphere of 25°C, and discharged at a rate of 0.2C for 10 seconds in an atmosphere of -10°C. The voltage after the 10-second discharge was measured to determine the DC resistance value. Then, following the same procedure, the voltage after discharging for 10 seconds at rates of 0.5C, 1.0C, and 2.0C in an atmosphere of -10°C was measured, and the DC resistance was calculated.

[0087] [Volume change rate] For the lithium ion secondary batteries prepared above, the volume value of the lithium ion secondary batteries in an uncharged state in an atmosphere at 25° C. was measured and used as the initial volume value. Next, the battery was charged to 4.2 V at a rate of 0.2 C, and left in the charged state in an atmosphere at 60° C. for 4 weeks. Then, the lithium ion secondary battery was discharged to 3.0 V at a rate of 0.2 C in an atmosphere of 25° C., and the volume value of the lithium ion secondary battery was measured, which was taken as the volume value after high-temperature storage. Then, the volume change rate (%) was calculated from the following formula. Volume change rate (%) = (volume after high temperature storage / initial volume) x 100

[0088] [Capacity maintenance rate] The lithium ion secondary battery prepared above was charged to 4.2 V at a rate of 1 C in an atmosphere of 45° C., and then discharged to 3.0 V at a rate of 1 C in the same atmosphere. This was regarded as the first cycle, and the discharge capacity value was taken as the initial capacity value. Next, under the same conditions, charge and discharge were repeated 200 cycles, and the discharge capacity value at the 200th cycle was taken as the post-cycle capacity value. The capacity retention rate (%) was calculated from the following formula. Capacity retention rate (%) = (capacity after cycling / initial capacity) x 100

[0089] [Resistance change rate] The lithium-ion secondary battery prepared above was subjected to SOC (Sta The battery was charged to 50% (at the time of Charge) and discharged for 10 seconds at rates of 0.2C, 0.5C, 1.0C, and 2.0C, and the DC resistance was measured and used as the initial resistance. Next, the battery was charged to 4.2 V at a rate of 1 C in an atmosphere at 45° C., and then discharged to 3.0 V at a rate of 1 C in the same atmosphere. This cycle was repeated 200 times, and the DC resistance was measured to obtain the post-cycle resistance. Then, the resistance change rate was calculated from the following formula. Resistance change rate (%) = (resistance after cycling / initial resistance) x 100

[0090] <<Experiment 1: Synthesis of Complex Compounds>> <Synthesis of Complex Compound (A) 1> [Example 1] (Process 1) As a boron fluoride-based lithium salt (C), 18.2 g of lithium sulfide bis(boron trifluoride) complex salt was dissolved in 200 ml of ethyl methyl carbonate in an Erlenmeyer flask under a nitrogen atmosphere, and then cooled to prepare a lithium sulfide bis(boron trifluoride) / ethyl methyl carbonate solution. Then, 25.2 g of bis(trimethylsilyl)vinylphosphonate as a phosphorus compound (D) was added with stirring to the lithium sulfide bis(boron trifluoride) / ethyl methyl carbonate solution prepared above, and after the addition was completed, the mixture was stirred for 3 hours while maintaining the temperature at 80°C to obtain a reaction liquid.

[0091] (concentrated) Next, ethyl methyl carbonate was removed from the reaction liquid obtained above using an evaporator, and the reaction liquid was washed three times with dibutyl ether and dried under reduced pressure to obtain 22 g of complex compound (A1) (vinylphosphonic acid / lithium sulfide-bis(boron trifluoride) condensation salt) represented by the following formula (3). [ka]

[0092] [Example 2] The same procedure as in Example 1 was repeated except for using 16.6 g of lithium oxide-bis(boron trifluoride) complex salt as the boron fluoride-based lithium salt (C) and 31.4 g of tris(trimethylsilyl) phosphate as the phosphorus-based compound (D), to obtain 25 g of complex compound (A2) ((trimethylsilyl)phosphate / lithium oxide-bis(boron trifluoride) condensation salt) represented by the following formula (4). [ka]

[0093] [Example 3] (Process 1) As the boron fluoride-based lithium salt (C), 18.8 g of lithium tetrafluoroborate was dissolved in 200 ml of ethyl methyl carbonate in an Erlenmeyer flask under a nitrogen atmosphere, and the solution was cooled to obtain a lithium tetrafluoroborate / ethyl methyl carbonate solution. Then, 31.4 g of tris(trimethylsilyl) phosphate as a phosphorus-based compound (D) was added to the lithium tetrafluoroborate / ethyl methyl carbonate solution obtained above with stirring, and the mixture was stirred for 1 hour while maintaining the temperature at 50° C., thereby obtaining reaction solution 1.

[0094] (Process 2) As boron fluoride-based lithium salt (C), 16.6 g of lithium oxide·bis(boron trifluoride) complex salt was dissolved in 100 ml of ethyl methyl carbonate, and the resulting solution was added little by little at normal pressure to reaction solution 1 obtained in step 1, and the reaction was carried out under reduced pressure several times until the entire amount was added and the reaction was carried out under reduced pressure. The mixture was then stirred for 2 hours while maintaining at 50°C, and further maintained at 80°C for 3 hours to obtain reaction solution 2.

[0095] (concentrated) Next, the ethyl methyl carbonate was removed using an evaporator, the residue was washed three times with dibutyl ether, and dried under reduced pressure to obtain 32 g of complex compound (A3) (lithium phosphate bis(boron trifluoride) / lithium oxide bis(boron trifluoride) condensation salt) represented by the following formula (5). [ka]

[0096] [Examples 4 to 12] The same procedure as in Example 3 was carried out except that the boron fluoride-based lithium salt (C) and the phosphorus-based compound (D) in steps 1 and 2 were changed to the contents and reaction conditions shown in Tables 2 and 3, and 39 g of complex compound (A4) (lithium phosphate bis(boron trifluoride) / lithium oxalate bis(boron trifluoride) condensed salt), 41 g of complex compound (A5) (lithium phosphate bis(boron trifluoride) / lithium maleate bis(boron trifluoride) condensed salt), 42 g of complex compound (A6) (lithium phosphate bis(boron trifluoride) / lithium thiodiacetate bis(boron trifluoride) condensed salt), and 43 g of complex compound (A7) (lithium phosphate bis(boron trifluoride) / lithium borate bis(boron trifluoride) condensed salt), each of which is represented by the following formulas (6) to (14), were obtained. 52 g of complex compound (A8) (lithium phosphate·bis(boron trifluoride) condensed salt / lithium phosphate·tris(boron trifluoride) condensed salt), 55 g of complex compound (A9) (lithium phosphate·bis(boron trifluoride) / lithium monothiophosphate·tris(boron trifluoride) condensed salt), 56 g of complex compound (A10) (lithium phosphate·bis(boron trifluoride) condensed salt / lithium monothiophosphate·tris(boron trifluoride) condensed salt), From the obtained mixture, 60 g of complex compound (A11) (lithium phosphate·boron trifluoride / lithium dithiophosphate·tris(boron trifluoride) condensed salt), 49 g of complex compound (A12) (lithium phosphate·boron trifluoride / lithium oxalate·bis(boron trifluoride) condensed salt), and 30 g of complex compound (A13) (lithium phosphate·boron trifluoride / lithium oxalate·bis(boron trifluoride) condensed salt) were obtained. [ka] [ka]

[0097] [Table 2]

[0098] [Table 3]

[0099] <<Experiment 2: Evaluation of complex compound (A) as an electrolyte>> <Other electrolyte-free systems> [Example 13] (Preparation of electrolyte) The complex compound (A3) obtained above was added to a mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and vinylene carbonate (VC) (volume ratio = 30:69:1) so that the lithium cation concentration was 1.5 mol / L, and the mixture was mixed in the mass ratio shown below and dissolved uniformly to prepare an electrolyte solution. Complex compound (A3) 12.8 parts by mass Mixed solvent 87.2 parts by mass The volume of the obtained electrolyte was 0.0836 L, so the electrolyte (complexation) in the electrolyte was The mass concentration of compound (A3) is calculated as follows: Mass concentration: 12.8 / 0.0836=153g / L Complex compound (A3) is represented by the following formula (5), has a molecular weight of 408, and generates four lithium cations per molecule. Therefore, the molar concentration of lithium cations derived from complex compound (A3) in the electrolyte solution is calculated as follows: Molar concentration of lithium cations derived from complex compound (A3): (12.8 / 408) x 4 / 0.0836 = 1.5 mol / L [ka]

[0100] (Battery production and evaluation) The above-obtained electrolyte solution was used to fabricate the above-mentioned lithium ion secondary battery, and the initial charge / discharge efficiency and the −10° C. resistance value were evaluated. The manufacturing specifications and evaluation results are shown in Table 3 below.

[0101] [Examples 14 to 19, Comparative Example 1] The same procedure and evaluation were performed as in Example 13, except that the complex compound (A3) was changed to the complex compound (A) shown in Table 4 in terms of the parts by mass.

[0102] [Table 4]

[0103] <<Experiment 3: Evaluation of complex compounds as reinforcing agents>> <Without other strengthening agents> [Example 20] (Preparation of electrolyte) A mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and vinylene carbonate (VC) (volume ratio = 30:68:2) and LiPF as the electrolyte. 6 and a complex compound (A1) serving as a reinforcing agent were mixed in the following mass ratio and dissolved uniformly to prepare an electrolyte solution. LiPF 6 12.3 parts by mass Complex compound (A1) 2.0 parts by mass Mixed solvent 85.7 parts by mass Since the volume of the obtained electrolyte solution was 0.0827 L, the mass concentration of each electrolyte in the electrolyte solution was calculated as follows. LiPF 6 Mass concentration: 12.3 / 0.827=149g / L Mass concentration of complex compound (A1): 2 / 0.827 = 24 g / L In addition, complex compound (A1) is represented by the following formula (3), has a molecular weight of 250, and generates two lithium cations from one molecule. Therefore, the molar concentration of lithium cations derived from complex compound (A1) in the electrolyte solution is calculated as follows. Molar concentration of lithium cations derived from complex compound (A1): (2 / 250) x 2 / 0.0827 = 0.16 mol / L [ka] Similarly, LiPF 6 The molecular weight of LiPF is 152, and one molecule generates one lithium cation. 6 The molar concentration of the resulting lithium cations is calculated as follows: LiPF 6Molar concentration of lithium cations derived: (12.3 / 152) x 1 / 0.0827 = 0.98 mol / L

[0104] (Battery production and evaluation) The above-mentioned lithium ion secondary battery was produced using the electrolytic solution obtained above, and the volume value of the battery in an uncharged state in an atmosphere at 25° C. was then measured and used as the initial volume value. Next, the battery was charged to 4.2 V at a rate of 0.2 C, and left in the charged state for 4 weeks in an atmosphere at 60° C. Then, the battery was discharged to 3.0 V at a rate of 0.2 C in an atmosphere at 25° C., and the volume of the battery was measured in the same atmosphere at 25° C. to obtain the volume after high-temperature storage. Then, the volume change rate, capacity retention rate, and resistance change rate were evaluated. The manufacturing specifications and evaluation results are shown in Table 5 below.

[0105] [Examples 21 to 25, Comparative Example 2] The procedure was the same as in Example 20, and evaluation was performed in the same manner, except that the reinforcing agent was changed to the compound and parts by mass shown in Table 5.

[0106] [Table 5]

[0107] <Combined with other strengthening agents> [Example 26] (Preparation of electrolyte) The electrolyte was a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and vinylene carbonate (VC) (volume ratio = 30:69:1) and LiPF 6 The above, complex compound (A1) as a reinforcing agent, and 1,3-propane sultone were mixed and dissolved in the following ratio to prepare an electrolyte solution. LiPF 6 12.3 parts by mass Complex compound (A1) 1.0 part by mass 1,3-propane sultone 1.0 parts by mass Mixed solvent 85.7 parts by mass Since the volume of the obtained electrolyte solution was 0.827 L, the mass concentration of each electrolyte in the electrolyte solution was calculated as follows. LiPF 6 Mass concentration: 12.3 / 0.0827=149g / L Mass concentration of complex compound (A1): 1.0 / 0.0827 = 12 g / L In addition, complex compound (A1) is represented by the following formula (3), has a molecular weight of 250, and generates two lithium cations from one molecule. Therefore, the molar concentration of lithium cations derived from complex compound (A1) in the electrolyte solution is calculated as follows. Molar concentration of lithium cations derived from complex compound (A1): (1.0 / 250) x 2 / 0.827 = 0.1 mol / L [ka] Similarly, LiPF 6 The molecular weight of LiPF is 152, and one molecule generates one lithium cation. 6 The molar concentration of the resulting lithium cations is calculated as follows: LiPF 6 Molar concentration of lithium cations derived: (12.3 / 152) x 1 / 0.827 = 0.98 mol / L

[0108] (Battery production and evaluation) A battery was fabricated using the electrolyte solution obtained above, and the initial resistance was measured in an atmosphere at 25°C. Then, in an atmosphere of 45° C., the battery was first charged to 4.2 V at a rate of 1 C, and then discharged to 3.0 V at a rate of 1 C to measure the discharge capacity, and this first discharge capacity was taken as the initial capacity. Subsequently, similarly, charging and discharging was repeated 200 times between 3.0 V and 4.2 V to measure the discharge capacity, and the capacity retention rate after 200 cycles was calculated. The resistance value was then measured in an atmosphere at 25° C., and the rate of change in resistance after 200 cycles was calculated. The manufacturing specifications and evaluation results are shown in Table 6 below.

[0109] [Examples 27 to 29, Comparative Example 3] The procedure was the same as in Example 26, except that the reinforcing agent was changed to the compound and the parts by mass shown in Table 6, and the evaluation was performed in the same manner.

[0110] [Table 6]

[0111] <Summary of results> The electrolyte, reinforcing agent, and electrolytic solution of the present invention used in the examples, and the energy storage device produced using these, exhibited excellent balance of solubility in organic solvents (nonaqueous solvents), charge / discharge efficiency, -10°C resistance value, cycle characteristics (volume change rate, capacity retention rate, resistance change rate), and high-temperature characteristics. In contrast, the comparative examples showed poor results in any of the following: excellent solubility in organic solvents (non-aqueous solvents), charge / discharge efficiency, -10°C resistance, cycle characteristics (volume change rate, capacity retention rate, resistance change rate), and high-temperature characteristics.

Claims

1. An electrolyte for an electricity storage device, comprising a complex compound (A), The above electrolyte, wherein the complex compound (A) contains one or more complex compounds represented by the following formula (1): [Formula 1] (In formula (1), X 1 is a P(=O) or P(=S) group, R 1 ~R 3 are each independently one group selected from the group consisting of a hydrogen atom, an alkyl group, an alkenyl group, a halogen atom, an alkoxy group, a siloxy group, a thiosilane group, and a group represented by the following formula (2), or R 1 ~R 3 one of the two groups selected from the group consisting of is an oxygen atom and is bonded to the other to form a ring structure, R 1 ~R 3 At least one of the above is a group containing a structure represented by the following formula (2): [chemical 2] (Formula (2) represents an oligomer having a structure in which each repeating unit shown in [ ] is linked, and the linking order of each repeating unit is arbitrary. l is [ ] l represents the number of repeats of the repeating unit bracketed with , and is a number from 1 to 10, m is [ ] m represents the number of repeats of the repeating unit enclosed in (a) and is a number from 0 to 10, n is [ ] n represents the number of repeats of the repeating unit enclosed in (a) and is a number from 0 to 10, M + is an alkali metal cation or a quaternary ammonium cation, Y 1 ~Y 3 are each independently an oxygen atom or a sulfur atom, B is a boron atom; G is a halogen atom; X 2 is a boron atom, a P(=O) group or a P(=S) group, Z indicates that the preceding and following groups are directly connected, or is a group selected from the group consisting of a substituted or unsubstituted alkylene group, an alkenylene group, a phenylene group, and an alkylene group having an ether group or a thioether group in the main chain; R 4 are each independently a hydrogen atom, an alkyl group, an alkenyl group, a halogen atom, an alkoxy group, a siloxy group, or a thiosilane group.

2. 2. The electrolyte according to claim 1, wherein the complex compound has at least one boron halide group.

3. 2. The electrolyte according to claim 1, wherein the complex compound has at least one of the siloxy group and / or the thiosilane group.

4. The complex compound is At least one boron halide group; At least one of the siloxy groups and / or thiosilane groups 2. The electrolyte of claim 1, comprising:

5. The electrolyte according to claim 1, characterized in that the complex compound contains one or more complex compounds selected from the group consisting of complex compounds represented by the following formulas (3) to (14): [C3] [C4]

6. A reinforcing agent for an electricity storage device, comprising the complex compound (A) according to any one of claims 1 to 5.

7. An electrolyte solution for an electricity storage device, comprising at least the complex compound (A) according to any one of claims 1 to 5 and an organic solvent, The concentration of the alkali metal cation or quaternary ammonium cation derived from the complex compound (A) in the entire electrolyte is 0.01 mol / L or more and 2.0 mol / L or less. The above electrolyte.

8. An electrolyte solution for an electricity storage device, comprising at least the complex compound (A) according to any one of claims 1 to 5 and an organic solvent, The concentration of the complex compound (A) in the entire electrolyte is 0.1% by mass or more and 30% by mass or less. The above electrolyte.

9. An electricity storage device produced using the electrolyte solution according to claim 7 or 8.

10. An electricity storage device produced using the electrolyte according to any one of claims 1 to 5 and / or the reinforcing agent according to claim 6.

11. A solid-state electricity storage device produced using the electrolyte according to any one of claims 1 to 5 and / or the reinforcing agent according to claim 6.

12. A method for synthesizing the complex compound (A) according to any one of claims 1 to 5, comprising the steps of: The complex compound (A) contains a P(=O) group or a P(=S) group, and / or a boron halide group, The production method includes a step 1 of carrying out a bonding reaction between a boron halide salt (E) and a phosphorus compound (F) by dehalogenation of silyl, The boron halide salt (E) is a salt consisting of an anion having two or more halogen atoms bonded to boron and an alkali metal cation or a quaternary ammonium cation, The phosphorus-based compound (F) is a compound having a siloxy group or a thiosilane group bonded to a P(=O) group or a P(=S) group. A manufacturing method comprising:

13. The method according to claim 12, further comprising one or more steps: (a) after the step 1, adding an additional reaction raw material consisting of a boron halide salt (E) and / or a phosphorus compound (F) to promote a bonding reaction by dehalogenation of silyl;

Citation Information

Patent Citations

  • Non-aqueous electrolyte and storage device using the same

    JP2020194771A

  • Nonaqueous electrolyte solution for batteries, novel compound, polymer electrolyte, and lithium secondary battery

    WO2014175225A1

  • Electrolyte for power storage devices and nonaqueous electrolyte solution

    WO2019180945A1