Rubber composition for inner liner
A rubber composition for inner liners in tires, using specific ratios of butyl rubber, clay minerals, silica, and carbon black, addresses the imbalance in air permeation, moisture resistance, and fracture characteristics, enhancing tire durability.
Patent Information
- Application Number
- JP2023074660
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
AI Technical Summary
Existing rubber compositions for inner liners in high-pressure tires fail to balance air permeation prevention, moisture resistance, fracture characteristics, and embrittlement temperature due to the use of large amounts of platy clay minerals, which deteriorate other performance properties.
A rubber composition comprising 100% butyl rubber and/or recycled butyl rubber, with specific ratios of layered or plate-like clay minerals, silica, and carbon black, ensuring a CTAB adsorption specific surface area ratio that enhances air permeation prevention and moisture resistance while maintaining fracture properties and embrittlement temperature.
The composition achieves improved air permeation prevention and moisture resistance while maintaining fracture properties and embrittlement temperature, balancing performance without excessive filler amounts affecting basic properties.
Smart Images

Figure 2024158974000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition for an inner liner intended to be used primarily in an inner liner layer of a tire. [Background technology]
[0002] For tires filled with high air pressure, the inner liner layer is required to have high air permeation prevention performance. For example, Patent Document 1 proposes that a large amount of plate-like clay mineral is blended into a rubber composition for an inner liner to reduce air permeability. However, when a large amount of plate-like clay mineral is blended into a rubber composition for an inner liner, the breaking characteristics, brittle temperature, and moisture resistance are deteriorated, and there is a problem that basic performance other than the air permeation prevention performance required for the inner liner layer cannot be sufficiently ensured. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-24922 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a rubber composition for an inner liner which has improved air permeation prevention performance and moisture resistance while maintaining the breaking characteristics and brittle temperature, thereby enabling these performances to be simultaneously achieved in a well-balanced manner to a high degree. [Means for solving the problem]
[0005] The rubber composition for an inner liner of the present invention, which achieves the above object, comprises 100 parts by mass of a rubber component containing 70% by mass to 100% by mass of butyl rubber and / or recycled butyl rubber and 0% by mass to 30% by mass of isoprene rubber, 20 parts by mass to 40 parts by mass of a layered or plate-like clay mineral, and a CTAB adsorption specific surface area of 65 m 2 / g~100m2 / g, and 5 to 50 parts by mass of silica having a CTAB adsorption specific surface area of 20 m 2 / g~60m 2 The total amount of the clay mineral, the carbon black, and the silica is 35 parts by mass to 80 parts by mass, and the CTAB adsorption specific surface area C of the silica is 10 parts by mass to 55 parts by mass. Si and the CTAB adsorption specific surface area C of the carbon black CB Compared to C CB / C Si is 0.20 to 0.92. Effect of the Invention
[0006] The rubber composition for an inner liner of the present invention is composed of the above-mentioned compounding, and the ratio C of the CTAB adsorption specific surface area of silica and carbon black is CB / C Si By satisfying the above-mentioned relationship, it is possible to improve the air permeation prevention performance and moisture resistance while maintaining the breaking characteristics and brittle temperature. In particular, by blending a sufficient amount of layered or plate-shaped clay minerals, it is possible to improve the air permeation prevention performance. In addition, the ratio C CB / C Siis set within the above range, and the particle size of silica is smaller than that of carbon black, so that the small particle size silica penetrates into the gaps of the carbon black, increasing the filling rate of various particles in the rubber, which also improves the air permeation prevention performance. Furthermore, by blending hydrophilic silica, the inner liner layer can trap moisture in the air, improving the performance of preventing moisture from entering the tire (moisture resistance) (this makes the tire internal structure less susceptible to the effects of moisture, improving the tire casing durability). On the other hand, since the total blending amount of clay mineral, carbon black, and silica is controlled within the above range, it is possible to prevent the blending amount of these fillers from being excessive and affecting basic performance such as breaking characteristics and brittle temperature. Through these cooperations, the present invention can achieve the above-mentioned performances in a well-balanced manner. In the present invention, the CTAB adsorption specific surface areas of carbon black and silica are measured in accordance with JIS K6217-3, respectively.
[0007] In the present invention, the entire rubber component is preferably a butyl rubber and / or a recycled butyl rubber. The clay mineral is preferably a flat talc having an aspect ratio of 2.0 to 4.5. Specifying the rubber component and the clay mineral in this way is advantageous in improving the air permeation prevention performance.
[0008] The rubber composition for innerliner of the present invention can be suitably used for the innerliner layer of a tire. A tire having an innerliner layer made of the rubber composition for innerliner of the present invention can exhibit excellent air permeation prevention performance and moisture resistance while satisfactorily ensuring the basic performance (breaking characteristics, brittle temperature) required for an innerliner layer due to the excellent physical properties of the rubber composition for innerliner of the present invention. [Brief description of the drawings]
[0009] [Figure 1] 1 is a meridian cross-sectional view showing an example of a pneumatic tire using the rubber composition for an inner liner of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The configuration of the present invention will be described in detail below with reference to the accompanying drawings.
[0011] As shown in FIG. 1, a pneumatic tire in which the rubber composition for an inner liner of the present invention is used includes a tread portion 1, a pair of sidewall portions 2 arranged on both sides of the tread portion 1, and a pair of bead portions 3 arranged on the tire radial inner side of the sidewall portions 2. In FIG. 1, the symbol CL indicates the tire equator. Although not depicted in FIG. 1 because it is a meridian cross section, the tread portion 1, the sidewall portions 2, and the bead portions 3 each extend in the tire circumferential direction to form an annular shape, thereby forming a toroidal basic structure of a pneumatic tire. The following explanation using FIG. 1 is basically based on the meridian cross section shown in the figure, but each tire component extends in the tire circumferential direction to form an annular shape.
[0012] A carcass layer 4 is installed between a pair of left and right bead portions 3. This carcass layer 4 includes a plurality of reinforcing cords extending in the tire radial direction, and is folded back from the inner side to the outer side in the tire width direction around a bead core 5 arranged in each bead portion 3. A bead filler 6 is arranged on the outer periphery of the bead core 5, and this bead filler 6 is wrapped by the main body and the folded back portion of the carcass layer 4. Meanwhile, a plurality of belt layers 7 (two layers in FIG. 1) are embedded on the outer periphery side of the carcass layer 4 in the tread portion 1. Each belt layer 7 includes a plurality of reinforcing cords inclined with respect to the tire circumferential direction, and the reinforcing cords are arranged so as to cross each other between the layers. In these belt layers 7, the inclination angle of the reinforcing cords with respect to the tire circumferential direction is set to, for example, a range of 10° to 40°. Furthermore, a belt reinforcing layer 8 (two layers, a full cover 8a covering the entire width of the belt layer 7 and an edge cover 8b locally covering the end portion of the belt layer 7) is provided on the outer periphery side of the belt layer 7. The belt reinforcing layer 8 includes organic fiber cords oriented in the tire circumferential direction. In the belt reinforcing layer 8, the organic fiber cords are set at an angle of, for example, 0° to 5° with respect to the tire circumferential direction.
[0013] An inner liner layer 9 is provided on the innermost surface of the tire along the carcass layer 4. This inner liner layer 9 is a layer for preventing air filled in the tire from permeating to the outside of the tire. The rubber composition for an inner liner of the present invention is used for the inner liner layer 9 of such a tire. Therefore, the basic structure of other parts is not limited to the above-mentioned structure.
[0014] In the rubber composition for innerliner of the present invention, the rubber component is a diene-based rubber, and necessarily contains a butyl-based rubber and / or a recycled butyl-based rubber. Also, it may contain an isoprene-based rubber optionally. The butyl-based rubber refers to butyl rubber or halogenated butyl rubber. Examples of the halogenated butyl rubber include brominated butyl rubber and chlorinated butyl rubber. As the butyl-based rubber (butyl rubber or halogenated butyl rubber), a rubber normally used in rubber compositions for tires can be used. The recycled butyl-based rubber is a recycled rubber whose main component is a butyl-based rubber obtained by desulfurizing rubber recovered from used tires and tubes. Examples of the isoprene-based rubber include various natural rubbers, epoxidized natural rubber, and various synthetic polyisoprene rubbers.
[0015] The butyl rubber and / or recycled butyl rubber may be contained in an amount of 70% by mass to 100% by mass, preferably 80% by mass to 100% by mass, based on 100% by mass of the rubber component. Particularly preferably, the total amount of the rubber component is butyl rubber and / or recycled butyl rubber (i.e., 100% by mass of the butyl rubber and / or recycled butyl rubber in 100% by mass of the rubber component). By containing a sufficient amount of butyl rubber and / or recycled butyl rubber in this way, it is possible to improve the air permeation prevention performance. If the content of butyl rubber and / or recycled butyl rubber is less than 70% by mass, it is difficult to ensure sufficient air permeation prevention performance. Note that, although the use of recycled butyl rubber can reduce the environmental load, there is a concern that defects (discoloration and shrinkage) may occur due to vulcanization accelerators remaining in the recycled butyl rubber, so considering the balance between these, the content of recycled butyl rubber may be, for example, 10% by mass to 40% by mass based on 100% by mass of the rubber component.
[0016] The isoprene-based rubber is preferably contained in an amount of 0% by mass to 30% by mass, and more preferably 0% by mass to 20% by mass, based on 100% by mass of the rubber component. In particular, as described above, it is particularly preferable that the entire rubber component is butyl-based rubber and / or recycled butyl-based rubber, and in this case, it is preferable that the rubber does not contain isoprene-based rubber. By suppressing the content of isoprene-based rubber in this way, it becomes possible to effectively exert the air permeation prevention performance of butyl-based rubber or recycled butyl-based rubber. If the content of isoprene-based rubber exceeds 30% by mass, the content of butyl-based rubber or recycled butyl-based rubber decreases, making it difficult to ensure sufficient air permeation prevention performance.
[0017] In the present invention, layered or plate-like clay mineral (hereinafter, sometimes simply referred to as "clay mineral"), silica, and carbon black are always blended as fillers into the diene rubber. When blending these fillers, the total blending amount of these three kinds is set to 35 parts by mass to 80 parts by mass, preferably 35 parts by mass to 70 parts by mass, per 100 parts by mass of the rubber component. This prevents the total amount of the filler from becoming excessive, and can suppress the influence on the basic performance required for the rubber composition for innerliner. If the total blending amount of these three kinds is less than 35 parts by mass, the breaking properties are reduced. If the total blending amount of these three kinds exceeds 80 parts by mass, the brittle temperature is increased. The blending amounts of these three kinds will be described later, but the total is always set to always satisfy the above-mentioned range.
[0018] The rubber composition for innerliner of the present invention can exhibit excellent air permeation prevention performance by blending layered or plate-like clay minerals. As the layered or plate-like clay minerals, either natural or synthetic products can be used. Specifically, talc, flat talc, graphite, flat clay, mica, etc. can be mentioned. Among these, flat talc can be preferably used. In particular, when flat talc is used, its aspect ratio is preferably 2.0 to 4.5, more preferably 2.0 to 4.0. An example of flat talc having an aspect ratio of 2.0 to 4.5 is HAR talc manufactured by Nippon Mistron Co., Ltd. By making the aspect ratio of the clay mineral (flat talc) 2.0 or more, the air permeation prevention performance can be improved. By making the aspect ratio of the clay mineral (flat talc) 4.5 or less, the dispersibility of the clay mineral (flat talc) in the rubber composition can be improved.
[0019] The aspect ratio Ar of the plate-like mineral is measured by the following formula (1). Ar = (Ds - Dl) / Ds (1) (In the formula, Ar is the aspect ratio, Ds is the 50% particle diameter obtained from the cumulative distribution measured by the centrifugal sedimentation method, and Dl is the 50% particle diameter obtained from the cumulative distribution measured by the coherent light laser diffraction method. The 50% particle diameter Ds measured by the centrifugal sedimentation method can be measured using, for example, a SediGrag 5100 particle diameter measuring device manufactured by Micromeritics Instruments. The 50% particle diameter Dl measured by the coherent light laser diffraction method can be measured using a Laser Malvern Mastersizer 2000 diffraction type particle distribution measuring device manufactured by Malvern Instruments.)
[0020] From the viewpoint of improving air permeation prevention performance, the clay mineral used in the present invention preferably has an average particle size of 3.0 μm to 9.0 μm, more preferably 4.0 μm to 8.0 μm. By making the average particle size of the clay mineral 3.0 μm or more, the dispersibility of the clay mineral in the rubber composition can be improved. By making the average particle size of the clay mineral 9.0 μm or less, the breaking properties can be improved. In the present invention, the average particle size of the clay mineral is the median size (D50: particle size of 50% in the cumulative particle size distribution) measured by a laser diffraction method.
[0021] The amount of the clay mineral is 20 to 40 parts by mass, preferably 20 to 35 parts by mass, per 100 parts by mass of the rubber component. By blending an appropriate amount of the clay mineral in this manner, the air permeation prevention performance of the clay mineral can be ensured. If the amount of the clay mineral is less than 20 parts by mass, the air permeation prevention performance decreases. If the amount of the clay mineral is more than 40 parts by mass, the brittle temperature increases.
[0022] The carbon black used in the present invention may be any carbon black that is commonly used in rubber compositions for tires. However, the CTAB adsorption specific surface area of the carbon black must be less than 20 m. 2 / g~60m 2 / g, preferably 20m 2 / g~50m 2 / g. By using such carbon black, it is possible to achieve both air permeation prevention performance and basic performance. The CTAB adsorption specific surface area of carbon black is 20m 2 If the CTAB adsorption specific surface area of the carbon black is less than 60 m 2 If it exceeds 1 / g, the low heat generation performance and the air permeation prevention performance decrease.
[0023] The amount of carbon black is 10 to 55 parts by mass, preferably 10 to 50 parts by mass, per 100 parts by mass of the rubber component. By adding an appropriate amount of carbon black in this way, it is possible to achieve both breaking properties and brittle temperature. If the amount of carbon black is less than 10 parts by mass, the breaking properties decrease. If the amount of carbon black is more than 55 parts by mass, the brittle temperature increases.
[0024] The silica used in the present invention may be, for example, a silica normally used in rubber compositions for tires, such as wet-process silica, dry-process silica, or surface-treated silica. However, the silica may have a specific surface area of 65 m2 or less for CTAB adsorption. 2 / g~100m 2 / g, preferably 75m 2 / g~100m 2 / g of silica is always used. Using silica with this particle size is advantageous in improving air permeation prevention performance. In addition, the hydrophilicity of silica can improve moisture resistance (the incorporation of hydrophilic silica allows moisture in the air to be trapped by the inner liner layer, preventing moisture from entering the inside of the tire). The CTAB adsorption specific surface area of silica is 65 m 2 If the CTAB adsorption specific surface area of the silica is less than 100 m 2 If it exceeds 1 / g, the low heat generation performance and the air permeation prevention performance decrease.
[0025] In the present invention, the CTAB adsorption specific surface area of silica is set to be sufficiently larger than the CTAB adsorption specific surface area of carbon black. In other words, the silica used in the present invention has a smaller particle size than carbon black. This allows the silica with a small particle size to enter the gaps in the carbon black, increasing the filling rate of various particles in the rubber, and also improving the air permeation prevention performance in this respect. Specifically, the CTAB adsorption specific surface area C Si and the CTAB adsorption specific surface area C of the carbon black mentioned above CB Comparison with C CB / C Siis set to 0.20 to 0.92, preferably 0.20 to 0.67. CB / C Si If the ratio C is less than 0.20, the breaking properties and low heat generation properties are reduced. CB / C Si If the particle size ratio exceeds 0.92, there is almost no difference between the particle sizes of the silica and carbon black, and therefore the silica cannot penetrate into the gaps in the carbon black, as described above, and the effect of increasing the particle filling rate and improving the air permeation prevention performance cannot be expected.
[0026] The amount of silica to be mixed is 5 to 50 parts by mass, preferably 5 to 35 parts by mass, per 100 parts by mass of the rubber component. By mixing an appropriate amount of silica in this way, air permeation prevention performance, moisture resistance, and brittle temperature can be all achieved. If the amount of silica to be mixed is less than 5 parts by mass, the moisture resistance and air permeation prevention performance decrease. If the amount of silica to be mixed exceeds 50 parts by mass, the brittle temperature increases.
[0027] In the rubber composition for innerliner of the present invention, a silane coupling agent can be added when compounding the above-mentioned silica. By compounding the silane coupling agent, the dispersibility of silica in diene rubber can be improved. Examples of silane coupling agents include bis-(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)disulfide, 3-trimethoxysilylpropylbenzothiazoletetrasulfide, γ-mercaptopropyltriethoxysilane, and 3-octanoylthiopropyltriethoxysilane. Among these, those having a tetrasulfide bond in the molecule can be preferably used. The compounding amount of the silane coupling agent is preferably less than 10 mass %, more preferably 3 mass % to 9 mass %, based on the compounding amount of silica. If the compounding amount of the silane coupling agent is 10 mass % or more of the silica compounding amount, the silane coupling agents condense with each other, and the desired hardness and strength of the rubber composition cannot be obtained.
[0028] Other compounding agents than those mentioned above can be added to the rubber composition of the present invention. Examples of other compounding agents include various compounding agents generally used in rubber compositions for tires, such as vulcanizing or crosslinking agents, vulcanization accelerators, antiaging agents, and liquid polymers. The compounding amounts of these compounding agents can be conventional general compounding amounts as long as they do not go against the object of the present invention. In addition, as the kneading machine, a normal rubber kneading machine, such as a Banbury mixer, a kneader, or a roll, can be used.
[0029] The present invention will be further described below with reference to examples, but the scope of the present invention is not limited to these examples. EXAMPLES
[0030] In preparing 21 types of rubber compositions for inner liners (Standard Example 1, Comparative Examples 1-7, Examples 1-13) with the materials shown in Table 4 as a common blend and the blends shown in Tables 1-3, the blending components except for the vulcanization accelerator and sulfur were weighed and kneaded for 5 minutes in a 1.8 L closed Banbury mixer, and the master batch was discharged and cooled at room temperature. After that, this master batch was fed to a 1.8 L closed Banbury mixer, and the vulcanization accelerator and sulfur were added and mixed for 2 minutes to obtain each rubber composition for inner liners.
[0031] The obtained rubber composition for inner liners was vulcanized at 170°C for 10 minutes in a mold of a specified shape (inner dimensions: length 150 mm, width 150 mm, thickness 2 mm) to prepare vulcanized rubber test pieces. The vulcanized rubber test pieces were used to evaluate the air permeation prevention performance, moisture resistance, brittle temperature, and breaking elongation using the methods described below.
[0032] Air permeation prevention performance Using each rubber composition for inner liners (vulcanized rubber test piece), the air permeability coefficient was measured at a test temperature of 30°C using air-equivalent test gas (nitrogen:oxygen=8:2) in accordance with Method A (differential pressure method) of JIS K7126 "Gas permeability test method for plastic films and sheets". The results obtained are shown in the "Air permeability prevention performance" column as an index using the reciprocal of the measured value, with the value of Conventional Example 1 being 100. The larger this index value, the smaller the air permeability coefficient and the more excellent the air permeability prevention performance.
[0033] Moisture resistance The inner liner rubber composition (vulcanized rubber test piece) was used to measure the moisture absorption amount of the test piece under high humidity conditions, and the moisture trapping ability of the inner liner was evaluated. Specifically, the vulcanized rubber test piece cut into a 2 mm thick, 5 cm square was first vacuum dried for 3 days, and the weight before moisture absorption (dry weight) was measured. Next, the vulcanized rubber test piece was left to stand in a constant temperature and humidity chamber at a temperature of 30°C and a humidity of 86% for 2 weeks. Thereafter, the vulcanized rubber test piece was taken out of the chamber and the weight after moisture absorption (moisture absorption weight) was measured. The moisture absorption amount obtained by subtracting the dry weight from the moisture absorption weight was recorded in the "moisture resistance" column as an index with the value of Standard Example 1 being 100. The higher the index, the higher the moisture absorption amount and the better the moisture resistance (high ability to trap moisture).
[0034] Low temperature embrittlement Using each rubber composition for inner liners (vulcanized rubber test piece), the brittleness temperature [°C] was measured according to the low-temperature impact embrittlement test of JIS K6261 "Vulcanized rubber and thermoplastic rubber - Determination of low-temperature properties". The results are shown in the "Low-temperature embrittlement" column as an index with the value of Conventional Example 1 being 100. The higher the index, the lower the brittleness temperature and the better the crack resistance at low temperatures.
[0035] Elongation at break Using each rubber composition for inner liners (vulcanized rubber test pieces), dumbbell JIS No. 3 test pieces were prepared in accordance with JIS K6251, and tensile tests were performed at room temperature (20°C) at a pulling rate of 500 mm / min to measure the tensile elongation at break. The results are shown in the "Elongation at break" column as an index with the value of Reference Example 1 being 100. A higher index value means a higher tensile elongation at break (better tensile properties).
[0036] [Table 1]
[0037] [Table 2]
[0038] [Table 3]
[0039] [Table 4]
[0040] The types of raw materials used in Tables 1 to 4 are shown below. NR: Natural rubber, TSR20 ·IIR: Butyl rubber, Japan Butyl Co., Ltd. BROMOBUTYL 2255 CB1: Carbon black, Nitelon #10N (CTAB adsorption specific surface area: 40 m 2 / g) CB2: Carbon black, manufactured by Tokai CB Co., Ltd. SEAT3 (CTAB adsorption specific surface area: 70 m 2 / g) CB3: Cabot Japan Co., Ltd. SHOWBLACK N762 (CTAB adsorption specific surface area: 20 m 2 / g) CB4: Tokai Carbon Co., Ltd., Seast 116HM (CTAB adsorption specific surface area: 60 m 2 / g) Silica 1: Solvay ZEOSIL 1085GR (CTAB adsorption specific surface area: 80 m 2 / g) Silica 2: EVONIK ULTRASIL 4000GR (CTAB adsorption specific surface area: 70m 2 / g) Silica 3: Solvay ZEOSIL 115GR (CTAB adsorption specific surface area: 105 m 2 / g) Plate-like clay mineral: MISTRON HAR manufactured by Imerys (aspect ratio: 3.0, average particle size: 5.0 μm) Layered clay mineral: Austin Black 325 bituminous coal crushed material manufactured by Coal Fillers Inc. (aspect ratio: 3.0, average particle size: 6.0 μm) Calcium carbonate: MSK-V manufactured by Maruo Calcium Co., Ltd. (a filler that does not meet the condition of "layered or plate-like") Zinc oxide: 3 types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd. Stearic acid: Industrial stearic acid 50S manufactured by Nisshin Rika Co., Ltd. Sulfur: Tsurumi Chemical Industry Co., Ltd. Kinkaji Oil-filled Powdered Sulfur Vulcanization accelerator: Sancerer DM-PO manufactured by Sanshin Chemical Industry Co., Ltd.
[0041] As is clear from Tables 1 to 3, Examples 1 to 13 maintained or improved the low-temperature embrittlement resistance and breaking elongation to levels equal to or greater than those of Control Example 1, while improving the air permeation prevention property and moisture resistance compared to Control Example 1, thereby achieving a good balance between these performance properties.
[0042] On the other hand, in Comparative Example 1, the content of butyl rubber was low, so the air permeation prevention performance was reduced. In Comparative Example 2, the amount of silica blended was low, so none of the performances could be improved. In Comparative Example 3, the amount of silica blended was high, so the low-temperature embrittlement property and the breaking elongation were deteriorated. In Comparative Example 4, the amount of carbon black blended was low, so the air permeation prevention property and the breaking elongation were reduced. In Comparative Example 5, the CTAB adsorption specific surface area of silica was large, so the air permeation prevention property could not be improved and the breaking elongation was reduced. In Comparative Example 6, the CTAB adsorption specific surface area of carbon black was large, so the low-temperature embrittlement property was reduced. In Comparative Example 7, calcium carbonate (a filler that does not satisfy the condition of "layered or plate-like") was blended instead of the layered or plate-like clay mineral, so the air permeation prevention property was reduced.
[0043] The present disclosure includes the following inventions. Invention [1] A rubber component containing 70% to 100% by mass of butyl rubber and / or recycled butyl rubber and 0% to 30% by mass of isoprene rubber, 20 to 40 parts by mass of layered or plate-like clay mineral, and a CTAB adsorption specific surface area of 65 m 2 / g~100m 2 / g, and 5 to 50 parts by mass of silica having a CTAB adsorption specific surface area of 20 m 2 / g~60m 2 The total amount of the clay mineral, the carbon black, and the silica is 35 parts by mass to 80 parts by mass, and the CTAB adsorption specific surface area C of the silica is 10 parts by mass to 55 parts by mass. Si and the CTAB adsorption specific surface area C of the carbon black CB Comparison with C CB / C Si The rubber composition for an inner liner, wherein the modulus is 0.20 to 0.92. Invention [2] The rubber composition for inner liners according to invention [1], characterized in that the entirety of the rubber component is butyl-based rubber and / or recycled butyl-based rubber. Invention [3] The rubber composition for an inner liner according to invention [1] or [2], wherein the clay mineral is a flat talc having an aspect ratio of 2.0 to 4.5. Invention [4] A tire comprising an inner liner layer made of the rubber composition for an inner liner according to any one of inventions [1] to [3]. [Explanation of symbols]
[0044] 1 Tread section 2 Sidewall 3 Bead section 4 Carcass layer 5 Bead Core 6 Bead Filler 7 Belt layer 8 Belt cover layer 9 Inner liner layer CL Tire Equator
Claims
1. A rubber component containing 70% by mass to 100% by mass of butyl rubber and / or recycled butyl rubber and 0% by mass to 30% by mass of isoprene rubber, 20% by mass to 40% by mass of a layered or plate-like clay mineral, and a CTAB adsorption specific surface area of 65 m 2 / g to 100m 2 / g, and 5 to 50 parts by mass of silica having a CTAB adsorption specific surface area of 20 m 2 / g to 60m 2 / g, the total amount of the clay mineral, the carbon black, and the silica is 35 parts by mass to 80 parts by mass, and the CTAB adsorption specific surface area C Si and the CTAB adsorption specific surface area C of the carbon black CB Comparison with C CB / C Si The rubber composition for an inner liner is characterized in that the modulus is 0.20 to 0.
92.
2. 2. The rubber composition for an inner liner according to claim 1, wherein the entire rubber component is a butyl-based rubber and / or a reclaimed butyl-based rubber.
3. 3. The rubber composition for an inner liner according to claim 1, wherein the clay mineral is a flat talc having an aspect ratio of 2.0 to 4.
5.
4. A tire comprising an inner liner layer made of the rubber composition for an inner liner according to claim 1 or 2.
Citation Information
Patent Citations
JP2014‐24922A