Particulate copolymer, aqueous dispersion, adhesive for lithium ion secondary battery, slurry for protective layer for lithium ion secondary battery, protective layer for lithium ion secondary battery, separator for lithium ion secondary battery, and lithium ion secondary battery
A particulate copolymer-based protective layer for lithium ion secondary batteries addresses heat shrinkage issues by controlling temperature-dependent behavior, ensuring safety through effective thermal shrinkage resistance.
Patent Information
- Application Number
- JP2023074775
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
AI Technical Summary
Existing lithium ion secondary battery separators face issues with heat shrinkage resistance, leading to potential short circuits between electrodes at high temperatures, especially as battery capacities increase.
A particulate copolymer with a specific composition, including units derived from acetoacetyl group-containing vinyl monomers, (meth)acrylic acid ester monomers, and carboxyl group-containing monomers, is used to form a protective layer that exhibits excellent heat shrinkage resistance by controlling the behavior of the separator based on temperature changes.
The protective layer suppresses thermal shrinkage of the separator even at high temperatures, preventing short circuits and enhancing the safety of lithium ion secondary batteries.
Smart Images

Figure 2024159043000001 
Figure 2024159043000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a particulate copolymer, an aqueous dispersion, an adhesive for lithium ion secondary batteries, a slurry for protective layers for lithium ion secondary batteries, a protective layer for lithium ion secondary batteries, a separator for lithium ion secondary batteries, and a lithium ion secondary battery. [Background technology]
[0002] In recent years, the development of power storage devices, such as lithium ion secondary batteries, has been actively carried out. In lithium ion secondary batteries, a separator is usually provided between positive and negative electrodes. The separator has the function of preventing direct contact between the positive and negative electrodes, and allowing the electrolyte held in the micropores to pass through and ions to pass through. In order to impart various properties to the separator while ensuring the electrical characteristics and safety of the lithium ion secondary battery, a separator has been proposed in which a protective layer containing an inorganic filler and a resin binder is arranged on the substrate surface of the separator. For example, Patent Document 1 proposes a battery separator in which a crosslinked polymer layer having an acetoacetyl group on the side chain of the polymer molecular chain is supported on a porous resin film. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-087795 A Summary of the Invention [Problem to be solved by the invention]
[0004] According to Patent Document 1, it is said that a separator can be obtained that captures metal ions dissolved in the electrolyte and reduces deposition on the negative electrode surface, thereby providing a nonaqueous lithium ion secondary battery with little deterioration in capacity even after repeated charging and discharging. On the other hand, in secondary batteries, the micropores in the separator substrate shrink when the battery heats up, hindering the passage of, for example, lithium ions, and suppressing runaway of the secondary battery. However, if runaway occurs at a higher temperature, such as 150°C or higher, there is a problem that the separator shrinks and the electrodes short-circuit. In particular, with the trend toward higher battery capacities in recent years, there is a tendency for the amount of heat generated during runaway to increase, and there is a demand for preventing the separator from shrinking when the temperature becomes high (hereinafter, such performance is also referred to as "heat shrinkage resistance"). According to the studies of the present inventors, it has become clear that there is still room for improvement in the technology described in Patent Document 1 from the viewpoint of heat shrinkage resistance when used as a separator.
[0005] The present invention has been made in consideration of the problems inherent in the above-mentioned conventional techniques, and has an object to provide a particulate copolymer or the like that exhibits excellent heat shrinkage resistance. [Means for solving the problem]
[0006] As a result of intensive research, the present inventors have found that the above problems can be solved by a particulate copolymer having a predetermined composition, and have thus completed the present invention.
[0007] That is, the present invention includes the following aspects. [1] A unit U1 derived from an acetoacetyl group-containing vinyl monomer M1; a unit U2 having one radically polymerizable double bond and derived from a (meth)acrylic acid ester monomer M2 different from M1; a unit U3 derived from a carboxyl group-containing monomer M3; a unit U4 derived from a monomer M4 which is different from the M1, M2 and M3 and is copolymerizable therewith; A particulate copolymer having in its molecule: A particulate copolymer, wherein a content C1 of the unit U1 in the particulate copolymer is 6% by mass or more relative to 100% by mass of the particulate copolymer. [2] The particulate copolymer according to [1], wherein the content C1 is 9% by mass or more and 99% by mass or less. [3] the unit U2 includes a unit U2' derived from an epoxy group-containing vinyl monomer, The particulate copolymer according to [1] or [2], wherein a content C2' of units U2' in the particulate copolymer is 2% by mass or more and 20% by mass or less, based on 100% by mass of the particulate copolymer. [4] The particulate copolymer according to any one of [1] to [3], wherein the particulate copolymer has a glass transition temperature of -40°C to 30°C. [5] The particulate copolymer according to any one of [1] to [4], wherein the particulate copolymer has a particle diameter of 40 to 600 nm. [6] The M2 further includes at least one selected from the group consisting of an epoxy group-containing vinyl monomer, a hydroxyl group-containing vinyl monomer, and a vinyl monomer having a hydrolyzable silyl group, The particulate copolymer according to any one of [1] to [5], wherein M4 includes at least one selected from the group consisting of a monomer having two or more radically polymerizable double bonds and an amide group-containing vinyl monomer. [7] An aqueous dispersion comprising the particulate copolymer according to any one of [1] to [6]. [8] The aqueous dispersion according to [7], further comprising an inorganic filler. [9] An adhesive for a lithium ion secondary battery for bonding an electrode and a separator, [7] An adhesive for lithium ion secondary batteries, comprising the aqueous dispersion according to [7].
[10] A slurry for a protective layer of a lithium ion secondary battery, comprising the aqueous dispersion according to [8].
[11] An inorganic filler; A particulate copolymer according to any one of [1] to [6], A protective layer for a lithium ion secondary battery comprising:
[12] A separator for a lithium ion secondary battery, comprising the protective layer for a lithium ion secondary battery according to
[11] .
[13] A lithium ion secondary battery comprising the separator for lithium ion secondary batteries according to
[12] . Effect of the Invention
[0008] According to the present invention, it is possible to provide a particulate copolymer or the like that exhibits excellent heat shrinkage resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention (hereinafter, also referred to as "the present embodiment") will be described in detail. Note that the present invention is not limited to the present embodiment, and various modifications can be made within the scope of the gist of the present invention.
[0010] In this specification, the terms "(meth)acrylic" and "(meth)acrylate" are used to encompass both "methacrylic and acrylic" and "methacrylate and acrylate".
[0011] [Particulate copolymer] The particulate copolymer of the present embodiment is a particulate copolymer having in its molecule a unit U1 derived from an acetoacetyl group-containing vinyl monomer M1 (hereinafter also simply referred to as "M1"); a unit U2 derived from a (meth)acrylic acid ester monomer M2 (hereinafter also simply referred to as "M2") having one radical polymerizable double bond and different from the M1; a unit U3 derived from a carboxyl group-containing monomer M3 (hereinafter also simply referred to as "M3"); and a unit U4 derived from a monomer M4 (hereinafter also simply referred to as "M4") different from the M1, M2, and M3 and copolymerizable therewith, and the content C1 of the unit U1 in the particulate copolymer is 6% by mass or more relative to 100% by mass of the particulate copolymer. The particulate copolymer of the present embodiment is thus configured, and can exhibit excellent heat shrinkage resistance.
[0012] (Unit U1) The particulate copolymer of the present embodiment has a unit U1 derived from an acetoacetyl group-containing vinyl monomer M1 in the molecule. Note that even if a monomer has a (meth)acrylic acid ester structure, if it contains an acetoacetyl group, it is classified as an acetoacetyl group-containing vinyl monomer M1, not as a (meth)acrylic acid ester monomer M2. The acetoacetyl group contained in the unit U1 contributes to the development of excellent heat shrinkage resistance.
[0013] The reason why heat shrinkage resistance is exhibited in this embodiment is presumed to be as follows, but the mechanism of action of this embodiment is not intended to be limited to the following content. In general, a separator for a lithium ion secondary battery is widely used that is composed of a separator substrate made of a microporous polyolefin film or the like and a protective layer disposed on the substrate. This protective layer is provided for the purpose of imparting a function such as suppressing thermal shrinkage. Examples of methods for forming the protective layer include a method of coating a polyolefin substrate with a composition containing an inorganic filler, latex, a dispersant, a thickener, water, etc. In this case, high adhesion is required between the separator substrate and the protective layer so that they do not peel off from each other. The present inventors conducted a study on the assumption that by increasing the adhesion, the protective layer would strongly support the separator substrate and thermal shrinkage would be suppressed. However, as a result of the study, it became clear that a protective layer whose adhesive strength was simply adjusted to increase the adhesion could not suppress thermal shrinkage. Here, as a result of further investigations by the present inventors, it was found that it is important to control the behavior of the protective layer according to temperature changes, and that by performing such control, the thermal shrinkage of the separator can be suppressed even at high temperatures such as 150°C. That is, it was inferred that the thermal shrinkage of the separator can be suppressed even at high temperatures such as 150°C by strengthening the interfacial adhesion between the separator substrate and the protective layer at a temperature lower than the temperature around where the shrinkage stress of the separator substrate increases (hereinafter also referred to as "low temperature"), and by making the fusion between the separator substrate and the protective layer occur at a temperature higher than the temperature around where the shrinkage stress of the separator substrate increases (hereinafter also referred to as "high temperature"). Based on such an inference, the present inventors conducted various investigations on the material for forming the protective layer, and found that by applying a particulate copolymer having an acetoacetyl group in its molecule, the coating layer exhibits the desired behavior at low and high temperatures, and excellent heat shrinkage resistance can be imparted to the protective layer at high temperatures such as 150°C.
[0014] From the above viewpoint, the content C1 of the unit U1 in the particulate copolymer of this embodiment is 6% by mass or more with respect to 100% by mass of the particulate copolymer. That is, when the content C1 is 6% by mass or more, the particulate copolymer of this embodiment exhibits excellent heat shrinkage resistance. If the content C1 is less than 6% by mass, it becomes difficult to ensure sufficient heat shrinkage resistance. From the same viewpoint as above, the content C1 is preferably 7% by mass or more, more preferably 9% by mass or more, even more preferably 15% by mass or more, and even more preferably 19% by mass or more. The upper limit of the content C1 is not particularly limited, but may be 99% by mass or less, 98% by mass or less, 96% by mass or less, 50% by mass or less, 45% by mass or less, 40% by mass or less, 35% by mass or less, or 30% by mass or less, based on 100% by mass of the particulate copolymer. In this embodiment, the content C1 is preferably 9% by mass or more and 99% by mass or less. As a method for adjusting the content C1 within the above range, for example, in the production method of the particulate copolymer described later, when carrying out emulsion polymerization, a method in which the blending ratio of the acetoacetyl group-containing vinyl monomer M1 is set to a predetermined amount relative to the total amount of monomers can be mentioned. The content C1 may be calculated from the blending ratio of the monomers when the particulate copolymer is produced, or may be calculated from various spectral data using IR (ATR method) or the like.
[0015] As described above, the particulate copolymer of the present embodiment can suppress the thermal shrinkage of the separator even at a high temperature such as 150°C. It is presumed that the particulate copolymer of the present embodiment can control the behavior of the protective layer in the separator according to temperature changes. In other words, the above behavior suggests that the flexibility of the protective layer increases at low temperatures and the protective layer becomes hard at high temperatures. When the flexibility of the protective layer increases at low temperatures, the adhesion between the separator substrate and the protective layer increases, and thermal shrinkage tends to be suppressed. In addition, when the protective layer remains hard even at high temperatures, the protective layer supports the separator substrate, and the thermal shrinkage of the separator tends to be suppressed even at high temperatures such as 150°C. As a result of the investigations by the present inventors, the acetoacetyl group in the particulate copolymer of this embodiment can form a coordinate bond with a metal ion in an inorganic filler that can coexist with the particulate copolymer, i.e., can form a complex structure, so that the binding strength between the particulate copolymer and the inorganic filler tends to be improved, and the protective layer does not collapse even at high temperatures and remains hard, so that the protective layer supports the separator substrate and suppresses thermal shrinkage of the separator even at high temperatures such as 150°C. As described above, when the particulate copolymer of this embodiment is used together with an inorganic filler as a protective layer, the effect of this embodiment, that is, the protective layer exhibits the desired behavior at low and high temperatures, tends to become more pronounced, and therefore the protective layer tends to be able to better suppress the thermal shrinkage of the separator even at high temperatures such as 150°C.
[0016] Examples of the acetoacetyl group-containing vinyl monomer M1 include, but are not limited to, acetoacetate alkenyl esters such as vinyl acetoacetate and allyl acetoacetate; (meth)acrylic acid acetoacetate diesters of alkylene glycols such as 2-acetoacetoxyethyl acrylate, 2-acetoacetoxyethyl methacrylate, 2-acetoacetoxypropyl acrylate, 2-acetoacetoxypropyl methacrylate, and 2-cyanoacetoacetoxyethyl methacrylate; crotonic acid acetoacetate diesters of alkylene glycols such as 2-acetoacetoxyethyl crotonate and 2-acetoacetoxypropyl crotonate; and acetoacetate esters of N-alkylol (meth)acrylamides such as N-(acetoacetoxymethyl)acrylamide, N-(acetoacetoxymethyl)methacrylamide, N-(acetoacetoxyethyl)acrylamide, and N-(acetoacetoxyethyl)methacrylamide. The acetoacetyl group-containing vinyl monomer M1 can be used alone or in combination of two or more. Of these, allyl acetoacetate, 2-acetoacetoxyethyl acrylate, 2-acetoacetoxyethyl methacrylate, 2-acetoacetoxypropyl acrylate, and 2-acetoacetoxypropyl methacrylate are preferred.
[0017] (Unit U2) The particulate copolymer of the present embodiment has one radically polymerizable double bond and has a unit U2 in the molecule that is derived from a (meth)acrylic acid ester monomer M2 different from M1. In this specification, the (meth)acrylic acid ester is also referred to as a (meth)acrylate. Examples of M2 include (meth)acrylates having an alkyl group such as methyl acrylate, ethyl acrylate, propyl acrylate, isopropyl acrylate, butyl acrylate, isobutyl acrylate, t-butyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, cyclohexyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl acrylate, butyl methacrylate, isobutyl methacrylate, t-butyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, cyclohexyl methacrylate, isobornyl acrylate, and t-butylcyclohexyl acrylate; (meth)acrylates having an aromatic ring such as benzyl acrylate, phenyl acrylate, benzyl methacrylate, and phenyl methacrylate. These (meth)acrylic acid ester monomers can be used alone or in combination of two or more. The (meth)acrylate having an alkyl group is preferably a (meth)acrylate comprising an alkyl group and a (meth)acryloyloxy group. The (meth)acrylate having an aromatic ring is preferably a (meth)acrylate comprising an aromatic ring and a (meth)acryloyloxy group.
[0018] The (meth)acrylic acid ester monomer is more preferably a (meth)acrylic acid ester monomer consisting of an alkyl group having 4 or more carbon atoms and a (meth)acryloyloxy group, even more preferably a (meth)acrylic acid ester monomer consisting of an alkyl group having 6 or more carbon atoms and a (meth)acryloyloxy group, even more preferably one or more selected from the group consisting of methyl methacrylate, butyl acrylate, butyl methacrylate, 2-ethylhexyl acrylate, cyclohexyl methacrylate, isobornyl acrylate, and t-butylcyclohexyl acrylate, and even more preferably one or more selected from the group consisting of methyl methacrylate, cyclohexyl methacrylate, butyl acrylate, butyl methacrylate, and 2-ethylhexyl acrylate. The use of such a (meth)acrylic acid ester monomer is preferable from the viewpoint of improving the polymerization stability during emulsion polymerization and from the viewpoint of improving the adhesion to the electrode.
[0019] M2 may further include at least one selected from the group consisting of an epoxy group-containing vinyl monomer, a hydroxyl group-containing vinyl monomer, and a vinyl monomer having a hydrolyzable silyl group.
[0020] Examples of the epoxy group-containing vinyl monomer include glycidyl acrylate, glycidyl methacrylate, allyl glycidyl ether, methyl glycidyl acrylate, and methyl glycidyl methacrylate. The epoxy group-containing vinyl monomer may be used alone or in combination of two or more. In this embodiment, when the unit U2 contains a unit U2' derived from an epoxy group-containing vinyl monomer, the content C2' of the unit U2' in the particulate copolymer is preferably 2% by mass or more and 20% by mass or less with respect to 100% by mass of the particulate copolymer.
[0021] Examples of the hydroxyl group-containing vinyl monomer include hydroxyethyl (meth)acrylates such as 2-hydroxyethyl acrylate and 2-hydroxyethyl methacrylate, hydroxypropyl (meth)acrylates such as 2-hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylates such as 2-hydroxybutyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, di-(ethylene glycol) maleate, di-(ethylene glycol) itaconate, 2-hydroxyethyl maleate, bis(2-hydroxyethyl) maleate, and 2-hydroxyethyl methyl fumarate. The hydroxyl group-containing vinyl monomer may be used alone or in combination of two or more.
[0022] Examples of the hydrolyzable silyl group-containing vinyl monomer include vinyl silane, vinyl trimethoxy silane, γ-acryloxypropyl trimethoxy silane, γ-acryloxypropyl triethoxy silane, γ-methacryloxypropyl trimethoxy silane, γ-methacryloxypropyl triethoxy silane, 3-(methacryloyloxy)propyl trimethoxy silane, etc. As the hydrolyzable silyl group-containing vinyl monomer, one type may be used alone or two or more types may be used in combination.
[0023] The content of the unit U2 derived from the (meth)acrylic acid ester monomer M2 is not particularly limited, but can be, for example, 2% by mass or more and 90% by mass or less, preferably 10% by mass or more and 90% by mass or less, more preferably 20% by mass or more and 90% by mass or less, and even more preferably 30% by mass or more and 90% by mass or less, based on 100% by mass of the particulate copolymer of this embodiment. By the content of the (meth)acrylic acid ester monomer relative to the total amount of the particulate copolymer being in the range of 2% by mass or more and 90% by mass or less, the particulate copolymer is more likely to realize the behavior of increasing the flexibility of the coating layer at low temperatures (i.e., increasing the peel strength between the separator and the coating layer) and hardening the coating layer at high temperatures, and tends to be able to suppress the separator from shrinking even at high temperatures.
[0024] (Unit U3) The particulate copolymer of this embodiment has a unit U3 derived from a carboxyl group-containing monomer M3 in the molecule. Examples of the carboxyl group-containing monomer M3 include ethylenically unsaturated monomers having a carboxyl group. Note that even if a monomer has a (meth)acrylic acid ester structure, it is classified as a carboxyl group-containing monomer M3, not as a (meth)acrylic acid ester monomer M2, as long as it contains a carboxyl group. In this specification, a carboxyl group-containing monomer is also referred to as an unsaturated carboxylic acid. Examples of the ethylenically unsaturated monomer having a carboxyl group include monocarboxylic acid monomers such as acrylic acid, methacrylic acid, half ester of itaconic acid, half ester of maleic acid, and half ester of fumaric acid, and dicarboxylic acid monomers such as itaconic acid, fumaric acid, and maleic acid. These may be used alone or in combination of two or more. Of these, acrylic acid, methacrylic acid, and itaconic acid are preferred, and acrylic acid and methacrylic acid are more preferred.
[0025] The content of the unit U3 derived from the carboxyl group-containing monomer M3 can be, for example, 0.1% by mass or more and 10% by mass or less with respect to 100% by mass of the particulate copolymer of this embodiment. In this case, it is preferable that the content C2' of the unit U2' derived from the epoxy group-containing vinyl monomer is 2% by mass or more and 20% by mass or less with respect to 100% by mass of the particulate copolymer. In this embodiment, when the content of the unit U3 is 0.1% by mass or more and 10% by mass or less, and the content C2' of the unit U2' is 2% by mass or more and 20% by mass or less, the epoxy group and the carboxyl group are likely to undergo a crosslinking reaction at high temperatures in the protective layer (protective layer containing the particulate copolymer) on the separator substrate, the viscosity of the protective layer increases (i.e., the protective layer becomes hard at high temperatures), and the fusion between the separator substrate and the protective layer occurs more easily, and the effect of the protective layer to fix the separator substrate so as not to shrink tends to become more pronounced. From the viewpoint of further suppressing the thermal shrinkage of the separator, the content of the unit U3 is preferably 0.5% by mass or more and 5% by mass or less, and more preferably 1% by mass or more and 3% by mass or less. From the same viewpoint as above, the total amount of the content C2' of the unit U2' derived from the epoxy group-containing vinyl monomer and the content of the unit U3 is preferably more than 4% by mass, more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on 100% by mass of the particulate copolymer of this embodiment. The upper limit of the total amount may be 20% by mass or less, and is preferably 15% by mass or less. Furthermore, from the same viewpoint as above, the ratio of the content C2' of units U2' derived from the epoxy group-containing vinyl monomer to the content of units U3, expressed as content C2' / content of units U3, is preferably 0.5 or more and 10 or less, more preferably 1.0 or more and 10 or less, even more preferably 1.5 or more and 8.0 or less, and still more preferably more than 2 and less than 6.
[0026] (Unit U4) The particulate copolymer of the present embodiment has a unit U4 derived from a monomer M4 copolymerizable with the above M1, M2, and M3 in the molecule. M4 is a monomer that does not fall under any of the above M1, M2, and M3, and examples thereof include a monomer having two or more radically polymerizable double bonds and an amide group-containing vinyl monomer. These can be used alone or in combination of two or more. When these monomers are used as M4, for example, when the particulate copolymer of the present embodiment is applied as an adhesive for a lithium ion secondary battery to bond electrodes and separators, it is possible to bond while maintaining a suitable fluidity, and therefore tends to be excellent in handleability.
[0027] Examples of monomers having two or more radically polymerizable double bonds include divinylbenzene and polyfunctional (meth)acrylates, etc. Among monomers having two or more radically polymerizable double bonds, polyfunctional (meth)acrylates are preferred because they exhibit better resistance to electrolyte even in small amounts. The polyfunctional (meth)acrylate may be a bifunctional (meth)acrylate, a trifunctional (meth)acrylate, or a tetrafunctional (meth)acrylate. More specifically, but not limited to, ethylene dimethacrylate, neopentyl glycol diacrylate, neopentyl glycol dimethacrylate, butanediol diacrylate, butanediol dimethacrylate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol tetraacrylate, and pentaerythritol tetramethacrylate may be mentioned. These may be used alone or in combination of two or more. Among these, trimethylolpropane triacrylate and trimethylolpropane trimethacrylate are preferred because they exhibit better resistance to electrolyte even in small amounts.
[0028] Examples of the amide group-containing vinyl monomer include acrylamide, N-methoxymethylacrylamide, N-methoxymethylmethacrylamide, N-butoxymethylacrylamide, and N-butoxymethylmethacrylamide. Other examples include methylol group-containing vinyl monomers such as N-methylol acrylamide, N-methylol methacrylamide, dimethylol acrylamide, and dimethylol methacrylamide. These may be used alone or in combination of two or more.
[0029] In this embodiment, from the viewpoint described above, it is preferable that M2 further contains at least one selected from the group consisting of an epoxy group-containing vinyl monomer, a hydroxyl group-containing vinyl monomer, and a vinyl monomer having a hydrolyzable silyl group, and that M4 contains at least one selected from the group consisting of a monomer having two or more radically polymerizable double bonds and an amide group-containing vinyl monomer.
[0030] The content of unit U4 can be, for example, 0.1% by mass or more and 10% by mass or less, preferably 0.1% by mass or more and 5% by mass or less, more preferably 0.2% by mass or more and 4% by mass or less, and even more preferably 0.2% by mass or more and 2.5% by mass or less, relative to 100% by mass of the particulate copolymer of this embodiment. When the content of units U4 is in the range of 0.2 mass % or more and 2.5 mass % or less, the protective layer (protective layer containing the particulate copolymer) provided on the separator substrate tends to be able to further suppress the thermal shrinkage of the separator substrate.
[0031] (glass transition temperature) The glass transition temperature of the particulate copolymer of the present embodiment is preferably -40°C or more and 30°C or less, more preferably -30°C or more and 20°C or less, and further preferably -25°C or more and 10°C or less. When the glass transition temperature is within the above range, the composition containing the particulate copolymer of the present embodiment tends to be easily applied onto a separator substrate. The glass transition temperature can be adjusted to a range of -40°C or more and 60°C or less, for example, by controlling the amount of the (meth)acrylic acid ester monomer M2 and / or the carboxyl group-containing monomer M3 used, which constitute the particulate copolymer. The glass transition temperature can be measured based on the method described in the Examples.
[0032] (particle size) The particle size of the particulate copolymer of the present embodiment is preferably 40 nm or more and 600 nm or less, more preferably 40 nm or more and 500 nm or less, and further preferably 50 nm or more and 300 nm or less. When the particle size is within the above range, the particulate copolymer of the present embodiment is applied as an adhesive for lithium ion secondary batteries as described below, and when a separator is bonded, a sufficient amount of voids can be left, and the function of the separator to allow ions in the electrolyte to pass through tends to be maintained. The particle size can be adjusted, for example, by using a seed latex and a surfactant in a desired ratio. Usually, the particle size (D 50 ) tends to be smaller. The particle size can be measured based on the method described in the Examples.
[0033] [Method of producing particulate copolymer] The particulate copolymer of the present embodiment can be produced by a known polymerization method, such as solution polymerization, emulsion polymerization, bulk polymerization, or the like.
[0034] In order to obtain the particulate copolymer of this embodiment as a dispersion (for example, an aqueous dispersion described later), it is preferable to use an emulsion polymerization method as the polymerization method. The emulsion polymerization method is not particularly limited, and a conventionally known method can be used. As the emulsion polymerization method, for example, in an aqueous medium, an acetoacetyl group-containing vinyl monomer M1, a (meth)acrylic acid ester monomer M2, a carboxyl group-containing monomer M3, a monomer M4 different from the above M1, M2, and M3 and copolymerizable therewith, a radical polymerization initiator, and other additive components (for example, a molecular weight regulator) used as necessary are polymerized to obtain a particulate copolymer. In the polymerization, various methods can be used as necessary, such as a method in which the composition of the monomers supplied into the reaction system is kept constant throughout the entire polymerization process, or a method in which the composition of the monomers supplied is changed gradually or continuously during the polymerization process to change the composition of the particles of the resin dispersion produced. When the copolymer is obtained by emulsion polymerization, for example, the obtained particulate copolymer may be in the form of an aqueous dispersion (latex) containing water and the particulate copolymer dispersed in the water.
[0035] The radical polymerization initiator is capable of initiating addition polymerization of monomers by radical decomposition with heat or a reducing substance. As the radical polymerization initiator, either an inorganic initiator or an organic initiator can be used. As the radical polymerization initiator, a water-soluble or oil-soluble polymerization initiator can be used. Examples of the water-soluble polymerization initiator include peroxodisulfates, peroxides, water-soluble azobis compounds, and redox systems of peroxides and reducing agents. Examples of peroxodisulfates include potassium peroxodisulfate (KPS), sodium peroxodisulfate (NPS), and ammonium peroxodisulfate (APS). Examples of peroxides include hydrogen peroxide, t-butyl hydroperoxide, t-butyl peroxymaleic acid, succinic acid peroxide, and benzoyl peroxide. Examples of water-soluble azobis compounds include 2,2-azobis(N-hydroxyethylisobutyramide), 2,2-azobis(2-amidinopropane) dihydrochloride, and 4,4-azobis(4-cyanopentanoic acid). Examples of peroxide-reducing agent redox systems include those in which the above-mentioned peroxides are combined with one or more reducing agents such as sodium sulfoxylate formaldehyde, sodium hydrogen sulfite, sodium thiosulfate, sodium hydroxymethanesulfinate, L-ascorbic acid and its salts, cuprous salts, and ferrous salts.
[0036] The radical polymerization initiator can be used in an amount of preferably 0.05 to 2 parts by mass based on 100 parts by mass of the total amount of monomers.
[0037] As the molecular weight regulator, for example, any of those usable in normal emulsion polymerization, such as halogenated hydrocarbons such as chloroform and carbon tetrachloride, mercaptans such as n-hexymercaptan, n-octylmercaptan, n-dodecylmercaptan, t-dodecylmercaptan, and thioglycolic acid, xanthogens such as dimethylxanthogen disulfide and diisopropylxanthogen disulfide, terpinolene, α-methylstyrene dimer, etc., can be used. Among these, n-dodecylmercaptan is preferably used.
[0038] The amount of the molecular weight modifier used is preferably 5 parts by mass or less per 100 parts by mass of the total amount of monomers used when polymerizing each part.
[0039] [Water dispersion] The aqueous dispersion of this embodiment includes the particulate copolymer of this embodiment. For example, the aqueous dispersion of this embodiment may have the form of a dispersion liquid in which the particulate copolymer (latex particles) of this embodiment is dispersed in water. The aqueous dispersion of this embodiment can be obtained by carrying out emulsion polymerization in the above-mentioned method for producing the particulate copolymer.
[0040] The solid content concentration of the aqueous dispersion of the present embodiment is not particularly limited, but the solid content concentration of the particulate copolymer of the present embodiment can be 10% by mass or more and 60% by mass or less. The solid content concentration can be measured based on the method described in the examples below.
[0041] The pH of the aqueous dispersion of the present embodiment is not particularly limited, but can be 6 or more and less than 10, and preferably 7 or more and less than 9. When the pH of the aqueous dispersion of the present embodiment is 7 or more and less than 9, for example, even if the particulate copolymer of the present embodiment contains a unit U2' derived from an epoxy group-containing vinyl monomer, the ring-opening reaction of the epoxy group that may occur over time tends to be suppressed, and the long-term stability of the dispersion liquid can be maintained. The pH of the aqueous dispersion of this embodiment is preferably adjusted using ammonia, sodium hydroxide, potassium hydroxide, and amines such as dimethylaminoethanol, and more preferably adjusted using ammonia (water) or sodium hydroxide. The pH of the aqueous dispersion of this embodiment can be measured based on the method described in the Examples.
[0042] The aqueous dispersion of the present embodiment can contain the particulate copolymer of the present embodiment in a dispersed state in water, but the aqueous dispersion may contain, in addition to water and the copolymer, a solvent such as methanol, ethanol, isopropyl alcohol, a dispersant, a lubricant, a thickener, a bactericide, etc. The aqueous dispersion of the present embodiment may further contain an inorganic filler. The inorganic filler is not particularly limited, and the inorganic filler described later can be appropriately adopted.
[0043] [Adhesive for lithium-ion secondary batteries] The adhesive for lithium ion secondary batteries of the present embodiment is an adhesive for lithium ion secondary batteries for bonding an electrode and a separator, and includes the aqueous dispersion of the present embodiment. The adhesive for lithium ion secondary batteries of the present embodiment is used, for example, to bond a separator and an electrode in a lithium ion secondary battery. More specifically, the adhesive for lithium ion secondary batteries of the present embodiment is used, for example, when forming an adhesive layer on a separator or an electrode of a lithium ion secondary battery. That is, a separator with an adhesive layer for lithium ion secondary batteries can be manufactured by applying the adhesive for lithium ion secondary batteries of the present embodiment on a separator and forming an adhesive layer. For more detailed battery configurations when a separator with an adhesive layer for lithium ion secondary batteries is applied to a lithium ion secondary battery, reference can be made to, for example, those described in JP 2015-41603 A.
[0044] [Slurry for protective layer of lithium-ion secondary battery] The slurry for a lithium ion secondary battery protective layer of this embodiment (hereinafter also referred to as "slurry of this embodiment") contains the aqueous dispersion of this embodiment. The slurry of this embodiment may further contain an inorganic filler.
[0045] The slurry of the present embodiment is a dispersion liquid used for forming a protective layer containing the particulate copolymer of the present embodiment and, if necessary, an inorganic filler on the separator substrate by applying the slurry to the surface of a separator substrate for a lithium ion secondary battery, for example, and then drying the slurry. The slurry of the present embodiment may further contain a conductive assistant, a thickener, a non-aqueous solvent, etc., if necessary.
[0046] [Lithium-ion secondary battery protective layer] The lithium ion secondary battery protective layer of this embodiment (hereinafter also referred to as "filler protective layer") contains an inorganic filler and the particulate copolymer of this embodiment. That is, in this embodiment, the filler protective layer is the slurry of this embodiment and can be obtained from an inorganic material.
[0047] (Inorganic filler) The inorganic filler that can be contained in the slurry or filler protection layer of this embodiment is not particularly limited, but it is preferable that the filler has a melting point of 200°C or higher, has high electrical insulation properties, and is electrochemically stable within the range of use of lithium ion secondary batteries.
[0048] The inorganic filler is not particularly limited, but examples thereof include oxide ceramics such as alumina, silica, titania, zirconia, magnesia, ceria, yttria, zinc oxide, and iron oxide; nitride ceramics such as silicon nitride, titanium nitride, and boron nitride; ceramics such as silicon carbide, calcium carbonate, magnesium sulfate, aluminum sulfate, aluminum hydroxide, aluminum oxide hydroxide, potassium titanate, talc, kaolinite, dickite, nacrite, halloysite, pyrophyllite, montmorillonite, sericite, mica, amesite, bentonite, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, and silica sand; and glass fibers. These may be used alone or in combination.
[0049] Among these, from the viewpoint of improving the electrochemical stability and heat resistance of the separator, aluminum oxide compounds such as alumina, aluminum hydroxide, and aluminum oxide hydroxide (AlO(OH)); and aluminum silicate compounds having no ion exchange capacity such as kaolinite, dickite, nacrite, halloysite, and pyrophyllite are preferred.
[0050] Alumina has many crystal forms, such as α-alumina, β-alumina, γ-alumina, and θ-alumina, and any of these can be suitably used. Among these, α-alumina is preferred from the viewpoint of thermal and chemical stability.
[0051] The aluminum oxide compound is preferably aluminum oxide hydroxide (AlO(OH)). From the viewpoint of preventing internal short circuits caused by the generation of lithium dendrites, boehmite is more preferable as the aluminum oxide hydroxide. By employing particles mainly composed of boehmite as the inorganic filler constituting the protective layer, a very lightweight protective layer can be realized while maintaining high permeability, and even in a thinner protective layer, the thermal shrinkage of the protective film at high temperatures is suppressed, and excellent heat resistance tends to be exhibited. Synthetic boehmite, which can reduce ionic impurities that may affect the characteristics of the electrochemical device, is even more preferable.
[0052] As the aluminum silicate compound having no ion exchange capacity, kaolin, which is mainly composed of kaolin mineral, is more preferable because it is inexpensive and easily available. Kaolin includes wet kaolin and calcined kaolin obtained by calcining wet kaolin. In this embodiment, calcined kaolin is more preferable. Calcined kaolin tends to have excellent electrochemical stability because water of crystallization is released during the calcination process and impurities are also removed.
[0053] The average particle size of the inorganic filler is preferably more than 0.01 μm and not more than 4.0 μm, more preferably more than 0.1 μm and not more than 3.5 μm, and even more preferably more than 0.2 μm and not more than 3.0 μm. Adjusting the average particle size of the inorganic filler to the above range is preferable from the viewpoint of suppressing thermal shrinkage at high temperatures even when the filler protection layer is thin (for example, 7 μm or less). Examples of methods for adjusting the particle size and its distribution of the inorganic filler include a method of pulverizing the inorganic filler using an appropriate pulverizing device such as a ball mill, a bead mill, a jet mill, etc. to reduce the particle size.
[0054] Examples of the shape of the inorganic filler include plate-like, scaly, needle-like, columnar, spherical, polyhedral, block-like, etc. A combination of inorganic fillers having these shapes may be used.
[0055] The proportion of the inorganic filler in the filler protection layer can be appropriately determined from the viewpoints of the binding property of the inorganic filler, the permeability of the separator, heat resistance, etc. The proportion of the inorganic filler in the filler protection layer is preferably 20% by mass or more and less than 100% by mass, more preferably 50% by mass or more and 99.99% by mass or less, still more preferably 80% by mass or more and 99.9% by mass or less, and particularly preferably 90% by mass or more and 99% by mass or less.
[0056] The thickness of the filler protection layer is preferably 0.5 μm or more from the viewpoint of improving heat resistance and insulating properties, and is preferably 5 μm or less from the viewpoint of increasing the capacity and improving the permeability of the battery.
[0057] The layer density of the filler protection layer is 0.5 g / cm 3 More than 3.0g / cm 3 It is preferable that the concentration is 0.7 g / cm or less. 3 More than 2.0g / cm 3 It is more preferable that the layer density of the filler protection layer is 0.5 g / cm or less. 3 When the layer density of the filler protection layer is 3.0 g / cm or more, the heat shrinkage rate at high temperatures tends to be good. 3 When the thickness is less than 100 mm, the air permeability tends to decrease.
[0058] An example of a method for forming the filler protective layer is a method of applying a coating liquid containing an inorganic filler and the aqueous dispersion of the present embodiment to at least one surface of the separator substrate. In this case, the coating liquid may contain a solvent other than water, a dispersant, a thickener, etc., in order to improve dispersion stability, coatability, and storage properties. In this embodiment, after the coating liquid is applied, the coating liquid may be dried to remove water and the like, and the filler protective layer may be substantially composed of only solids. That is, in one aspect of this embodiment, the lithium ion secondary battery protective layer may contain the particulate copolymer of this embodiment and the inorganic filler, and water may or may not remain.
[0059] [Separator for lithium-ion secondary batteries] The separator for a lithium ion secondary battery of this embodiment (hereinafter also referred to as "the separator of this embodiment") includes a protective layer for a lithium ion secondary battery of this embodiment. The separator of this embodiment may include a porous substrate as a separator substrate, and a filler protective layer disposed on at least a portion of at least one side of the porous substrate. As described above, the filler protective layer includes an inorganic filler and the particulate copolymer of this embodiment. The separator of this embodiment may be composed of only the separator substrate and the filler protective layer, or may further include an adhesive layer for bonding to the electrode in addition to these.
[0060] In the separator of this embodiment, the filler protection layer can be disposed on one or both sides of the separator substrate, such as a polyolefin porous substrate.
[0061] Each member constituting the separator of the present embodiment and a preferred embodiment of a method for producing the separator of the present embodiment will be described in detail below.
[0062] (Separator substrate) As the separator substrate, for example, a porous substrate can be used. The porous substrate is a substrate having pores or gaps inside, and the substrate itself can be a substrate that has been used as a conventional separator. Among these, a polyolefin porous substrate (e.g., a polyolefin microporous film) containing a polyolefin resin as a main component is preferred from the viewpoint of excellent applicability of the coating liquid described later, making the separator film thinner, increasing the active material ratio in an electricity storage device such as a battery, and increasing the capacity per volume. Here, "containing as a main component" means containing more than 50% by mass, preferably 75% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, still more preferably 95% by mass or more, particularly preferably 98% by mass or more, and may be 100% by mass.
[0063] For example, by subjecting the surface of a separator substrate such as a polyolefin microporous membrane to a surface treatment, it becomes easier to apply a coating liquid thereafter and also improves the adhesion between the polyolefin microporous membrane and the filler protective layer or protective layer, so that the surface treatment is preferably performed. Examples of the surface treatment method include a corona discharge treatment method, a plasma treatment method, a mechanical roughening method, a solvent treatment method, an acid treatment method, and an ultraviolet oxidation method.
[0064] [Method of forming filler protection layer] The filler protection layer can be disposed on the separator substrate by, for example, applying a coating liquid containing the particulate copolymer of this embodiment and an inorganic filler, and further containing additional components such as a solvent other than water and a dispersant as necessary, to at least one surface of the separator substrate.
[0065] The method of applying the coating liquid to the separator substrate is not particularly limited as long as the required layer thickness and coating area can be achieved. Examples of the coating method include gravure coater method, small diameter gravure coater method, reverse roll coater method, transfer roll coater method, kiss coater method, dip coater method, knife coater method, air doctor coater method, blade coater method, rod coater method, squeeze coater method, cast coater method, die coater method, screen printing method, spray coating method, inkjet coating method, etc. Among them, the gravure coater method is preferred because it has a high degree of freedom in the coating shape.
[0066] The method for removing the solvent from the coating liquid after coating is not limited, and any method that has little effect on the separator substrate and the filler protective layer can be used, such as a method of drying the separator substrate at a temperature equal to or lower than the melting point of the separator substrate while fixing the separator substrate, or a method of drying under reduced pressure at a low temperature.
[0067] [How to place the protective layer] In this embodiment, for example, the aqueous dispersion of this embodiment can be applied to a separator substrate as a coating liquid (which may or may not contain an inorganic filler), thereby forming a protective layer on the separator substrate. The coating liquid preferably contains, in addition to water and the particulate copolymer of this embodiment, a poor solvent such as a mixed solvent with a water-soluble organic medium (e.g., methanol or ethanol).
[0068] The method for applying the aqueous dispersion of the present embodiment as a coating liquid onto the separator substrate is preferably a gravure coater coating method or a die coater coating method.
[0069] The method of removing the solvent from the coating liquid after coating to form the protective layer is not particularly limited, and any method that has little effect on the separator substrate and the protective layer can be used. For example, there is a method of drying the separator substrate at a temperature below its melting point while fixing it, a method of drying under reduced pressure at a low temperature, a method of immersing the separator substrate in a poor solvent for the particulate copolymer to solidify the particulate copolymer into particles and simultaneously extract the solvent, etc.
[0070] [Lithium-ion secondary battery] The lithium ion secondary battery of the present embodiment includes the separator of the present embodiment. The lithium ion secondary battery of the present embodiment may have a configuration similar to that of a conventionally known lithium ion secondary battery, for example, as described in JP 2018-92701 A, except that the lithium ion secondary battery of the present embodiment includes the separator of the present embodiment.
[0071] The heat shrinkage rate of the separator of this embodiment at 150° C. is not particularly limited, but is preferably 0% or more and less than 30%, more preferably 0% or more and 20% or less, and even more preferably 0% or more and 10% or less, in both MD and TD. By having the heat shrinkage rate at 150° C. in both MD and TD of 10% or less, it is possible to prevent the separator from rupturing even when the battery abnormally heats up, and it is possible to suppress contact between the positive and negative electrodes, which tends to result in better safety performance. EXAMPLES
[0072] The present embodiment will be described in more detail below using examples and comparative examples, but the present embodiment is not limited to the following examples in any way.
[0073] [Example 1] (Production of particulate copolymer) A reaction vessel equipped with a stirrer, a reflux condenser, a dropping tank, and a thermometer was charged with 759 parts by mass of ion-exchanged water and, as emulsifiers, 0.6 parts by mass of "Aqualon KH1025" (registered trademark, 25% aqueous solution manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.; hereinafter also referred to as "KH1025") and 0.6 parts by mass of "Adeka Reasoap SR1025" (registered trademark, 25% aqueous solution manufactured by ADEKA Corporation; hereinafter also referred to as "SR1025"). Next, the temperature inside the reaction vessel was raised to 80° C., and 1.5 parts by mass of a 2% aqueous solution of ammonium persulfate (hereinafter also referred to as "APS") was added while maintaining the temperature at 80° C. Five minutes after the addition of the aqueous ammonium persulfate solution was completed, the following emulsion was dropped from the dropping tank into the reaction vessel over 150 minutes. The emulsion was prepared by mixing a mixture of the following acetoacetyl group-containing vinyl monomer M1, (meth)acrylic acid ester monomer M2, carboxyl group-containing monomer M3, monomer M4 which is different from M1, M2 and M3 and is copolymerizable therewith, an emulsifier and ion-exchanged water in a homomixer for 5 minutes. That is, As an acetoacetyl group-containing vinyl monomer M1, 100 parts by mass of 2-acetoacetoxyethyl methacrylate (hereinafter also referred to as "AAEM"), As the (meth)acrylic acid ester monomer M2, 73 parts by mass of methyl methacrylate (hereinafter also referred to as "MMA"), 34 parts by mass of cyclohexyl methacrylate (hereinafter also referred to as "CHMA"), 1.5 parts by mass of butyl methacrylate (hereinafter also referred to as "BMA"), Butyl acrylate (hereinafter also referred to as "BA") 296 parts by mass, 313 parts by mass of 2-ethylhexyl acrylate (hereinafter also referred to as "2EHA"), 100 parts by mass of glycidyl methacrylate (hereinafter also referred to as "GMA"), 58 parts by weight of 2-hydroxyethyl methacrylate (hereinafter also referred to as "HEMA"), and 3 parts by mass of 3-(methacryloyloxy)propyltrimethoxysilane (manufactured by The Dow Chemical Company; hereinafter also referred to as "AcSi"), As the carboxyl group-containing monomer M3, 10 parts by mass of methacrylic acid (hereinafter also referred to as "MAA"), and 15 parts by mass of acrylic acid (hereinafter also referred to as "AA"), As a monomer M4 different from the M1, M2 and M3 and copolymerizable therewith, 0.2 parts by mass of acrylamide (hereinafter also referred to as "AAm"), and 20 parts by mass of trimethylolpropane triacrylate (ATMPT, product name of Shin-Nakamura Chemical Co., Ltd.; hereinafter also referred to as "A-TMPT"), As an emulsifier 7.5 parts by weight of KH1025, 7.5 parts by weight of SR1025, 0.5 parts by mass of sodium p-styrenesulfonate (hereinafter also referred to as "NaSS"), and 0.5 parts by mass of a 2% aqueous solution of ammonium persulfate; 703 parts by mass of ion-exchanged water; The mixture was mixed for 5 minutes using a homomixer to prepare an emulsion. After the dropwise addition of the emulsion was completed, the temperature inside the reaction vessel was maintained at 80° C. for 120 minutes, and then the reaction vessel was cooled to room temperature. The pH of the resulting emulsion was adjusted to 8.0 using an aqueous solution of ammonium hydroxide (25% aqueous solution) to obtain an aqueous dispersion of the particulate copolymer (solid content concentration: 40%). The particulate copolymer in the obtained aqueous dispersion was measured for pH, viscosity, Tg, average particle size, and swelling degree in electrolyte by the methods described below, and was also evaluated by a tensile test described below. The results are shown in Table 1.
[0074] (solid content concentration) Approximately 1 g of the aqueous dispersion of the particulate copolymer was precisely weighed out on an aluminum dish, and the weight (g) of the aqueous dispersion weighed out at this time was designated as a. This was dried for 1 hour in a hot air dryer at 130°C, and the dry weight (g) of the dried film (particulate copolymer) after drying was designated as b. The solid content concentration was calculated by the following formula. Solid content concentration (mass%) = b / a × 100
[0075] (pH) The electrodes of a pH meter (glass electrode type hydrogen ion concentration indicator, manufactured by DDK Toa Corp.) were immersed in the aqueous dispersion of the particulate copolymer (solid content concentration: approximately 40%), and the displayed value was read.
[0076] (viscosity) The viscosity was measured using a Brookfield viscometer at 25° C., a rotation speed of 60 rpm, and for 1 minute.
[0077] (glass transition temperature) An appropriate amount of the aqueous dispersion containing the particulate copolymer (solid content concentration: 38 to 42% by mass, pH 8.0) was placed on an aluminum dish and dried in a hot air dryer at 130° C. for 30 minutes. Approximately 17 mg of the dried film was placed in an aluminum container for measurement, and a DSC curve and a DDSC curve were obtained under a nitrogen atmosphere using a DSC measurement device (Shimadzu Corporation, model number: DSC6220). The measurements were performed using the following program. (1st stage heating program) The temperature started at 70°C and was increased at a rate of 15°C per minute. After reaching 110°C, it was maintained for 5 minutes. (2nd stage cooling program) The temperature was decreased from 110°C at a rate of 30°C per minute. After reaching -50°C, it was maintained at this temperature for 4 minutes. (Third stage heating program) The temperature was increased from -50°C to 130°C at a rate of 15°C per minute. DSC and DDSC data were collected during this third temperature increase. The glass transition temperature (Tg) was determined as the intersection point between a straight line extending from the baseline of the obtained DSC curve to the higher temperature side and a tangent to the inflection point.
[0078] (Average particle size of particulate copolymer) Using a particle size measuring device using a light scattering method (manufactured by LEED & NORTHRUP, product name "MICROTRAC UPA150"), the 50% particle size (nm) of an aqueous dispersion (solid content concentration approximately 40%) containing a particulate copolymer was measured and used as the average particle size.
[0079] (Electrolyte swelling degree) 3 g of the particulate copolymer aqueous dispersion (solid concentration 38-42%, pH 8.0) was placed on an aluminum dish and dried for 60 minutes in a hot air dryer at 130 ° C. The dried film was cut into 0.5 g pieces and placed in a 50 mL vial together with 10 g of a mixed solvent of ethylene carbonate: ethyl methyl carbonate = 1: 2 (volume ratio), and shaken for 3 hours. The sample was then taken out, washed with the above mixed solvent, and the mass (Wa) was measured. After that, the sample was left to stand in an oven at 150 ° C. for 1 hour, and the mass (Wb) was measured, and the swelling degree of the particulate copolymer in the electrolyte was measured by the following formula. Although the mixed solvent does not contain an electrolyte, it was confirmed that there was no difference in the degree of swelling of the particulate copolymer regardless of the presence or absence of an electrolyte. Swelling degree of particulate copolymer in electrolyte (times) = (Wa-Wb) / Wb
[0080] (Preparation of separator) A dispersion for forming a protective layer was prepared by uniformly dispersing 100 parts by mass of aluminum hydroxide oxide particles (average particle size 1.0 μm) as an inorganic filler (solid concentration of aluminum hydroxide oxide particles 50%), 3.0 parts by mass of a water dispersion (solid concentration of particulate copolymer 40%) as a resin binder, and 0.5 parts by mass of an amine polyphosphate salt (solid concentration of amine polyphosphate salt 1%) as an ion dissociative inorganic dispersant. The dispersion for forming a protective layer was applied to the surface of a polyethylene substrate (porous substrate; film thickness 11 μm) that had been corona-treated in advance using a bar coater. Thereafter, the substrate was dried at 60° C. for 1 minute to remove water, and a separator with a total film thickness of 12.9 μm was obtained in which a protective layer with a thickness of 1.9 μm was formed on the polyethylene substrate. As the "polyphosphoric acid", tripolyphosphoric acid was used.
[0081] (Heat shrinkable) In addition to the above-mentioned separator, the following separator was also produced. That is, a separator having a layer thickness of 13.3 μm was produced in the same manner as above, except that the amount of the water dispersion used was changed from 3.0 parts by mass to 3.25 parts by mass, and the thickness of the protective layer was changed from 1.9 μm to 2.1 μm. In addition to the above separator, the following separator was also produced: A separator with a total thickness of 13.2 μm was produced in the same manner as above, except that the amount of the aqueous dispersion was changed from 3.0 parts by mass to 3.5 parts by mass, and the thickness of the protective layer was changed from 1.9 μm to 2.2 μm. In addition to the above separator, the following separator was also prepared: A separator with a total thickness of 13.5 μm was prepared in the same manner as above, except that the amount of the aqueous dispersion was changed from 3.0 parts by mass to 4.0 parts by mass, and the thickness of the protective layer was changed from 1.9 μm to 2.5 μm. The heat shrinkage was evaluated using each separator. That is, the separator was cut into a size of 100 mm in the MD direction and 100 mm in the TD direction to prepare a sample, and the sample was left to stand in an oven at 150°C for 1 hour. At this time, the sample was sandwiched between two pieces of paper so that the hot air would not directly hit the sample. After removing the sample from the oven and cooling it, the length (mm) was measured and the heat shrinkage rate was calculated using the following formula. The measurement was performed in the MD direction and the TD direction, and the larger value was taken as the heat shrinkage rate. Heat shrinkage rate (%) = {(100 - length after heating) / 100} x 100 The thermal shrinkage rates obtained were evaluated based on the following evaluation criteria, and the results are shown in Table 1. S: The shrinkage rate is less than 10% even if the protective layer thickness is less than 2.1 μm. A: Protective layer thickness is 2.1μm or more and less than 2.2μm, and shrinkage rate is less than 10% B: Protective layer thickness is 2.2μm to 2.3μm and shrinkage rate is less than 10% C: Protective layer thickness is over 2.3 μm and shrinkage rate is less than 10%
[0082] (peel strength) The separator was attached to a 15mm x 75mm preparation with double-sided tape. Then, a 12mm wide mending tape was attached on top of the protective layer, and one end of the mending tape was pulled vertically at a pulling speed of 100mm / min to measure the stress when peeled off. The measurement was carried out three times, and the average value was calculated and used as the peel strength. A higher peel strength value indicates better adhesion between the polyethylene substrate and the protective layer. The obtained peel strength values were evaluated based on the following evaluation criteria, and the results are shown in Table 1. S:350 or more A: 250 or more and less than 350 B: 120 or more and less than 250 C: Less than 120
[0083] [Examples 2 to 12, Comparative Examples 1 to 5] Except for the types and amounts of the raw material monomers and the amount of the emulsifier used being as shown in Table 1, emulsion polymerization was carried out in the same manner as in Example 1 to obtain an aqueous dispersion. The particulate copolymer in the obtained aqueous dispersion was measured for pH, viscosity, Tg, average particle size, and swelling degree in electrolyte by the above-mentioned methods. The results are shown in Table 1. Also, a separator including a polyethylene substrate and a protective layer was produced in the same manner as in Example 1. The heat shrinkability and peel strength of the obtained separator were evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0084] [Table 1]
[0085] (Tensile test 1) The particulate copolymer of each example (solid content concentration of particulate copolymer: 40%) was used as dispersion A for tensile tests (for evaluation of single films). Dispersion A was applied to a glass plate using a 0.25 mm applicator, and after natural drying for about 5 hours in a room adjusted to 23°C and 50% humidity, the coating film was cut into a size of 10 mm wide and 80 mm long, and a tensile test of the obtained coating film test piece was performed using a Tensilon UTM-III-500 manufactured by Toyo Baldwin Co., Ltd. under the conditions shown below, and the measurement results of 5% modulus and 10% modulus were obtained. Such measurements were performed six times, and the obtained average values are shown in Table 2 as the values of 5% modulus and 10% modulus. Tripolyphosphoric acid was used as the above-mentioned "polyphosphoric acid". (Test conditions for Tensilon UTM-III-500) Tensile speed: 50mm / min Test conditions: Humidity 23°C, humidity 50%
[0086] (Tensile test 2) Dispersion B for tensile tests (for composite membrane evaluation) was prepared by uniformly dispersing 30 parts by mass of an aqueous dispersion of particulate copolymer of each example (solid concentration of particulate copolymer: 40%) as a binder, 69.5 parts by mass of an aqueous dispersion of aluminum oxide hydroxide particles (solid concentration of aluminum oxide hydroxide particles: 50%) as an inorganic filler, and 0.5 parts by mass of an amine polyphosphate salt (solid concentration of amine polyphosphate salt: 1%) as an ion dissociative inorganic dispersant. Two sheets of 0.23 mm thick PTFE tape were attached to a PP board to create a square mold, dispersion B was poured into it, and the mold was dried overnight in a room adjusted to 23°C and 50% humidity. Thereafter, a dumbbell-shaped No. 8 sample was cut out as a tensile test sample, and a tensile test was performed on the obtained coating test piece using a Toyo Baldwin Tensilon UTM-III-500 at a tensile speed of 3 mm / min, test temperature of 23°C, and test humidity of 50%. The 1% modulus was measured, and the average value was also obtained, which is shown in Table 2. As the "polyphosphoric acid" mentioned above, tripolyphosphoric acid was used.
[0087] [Table 2]
Claims
1. A unit U1 derived from an acetoacetyl group-containing vinyl monomer M1; a unit U2 having one radically polymerizable double bond and derived from a (meth)acrylic acid ester monomer M2 different from M1; a unit U3 derived from a carboxyl group-containing monomer M3; a unit U4 derived from a monomer M4 which is different from the M1, M2 and M3 and is copolymerizable therewith; A particulate copolymer having in its molecule: A particulate copolymer, wherein a content C1 of the unit U1 in the particulate copolymer is 6% by mass or more relative to 100% by mass of the particulate copolymer.
2. The particulate copolymer according to claim 1 , wherein the content C1 is 9% by mass or more and 99% by mass or less.
3. the unit U2 includes a unit U2' derived from an epoxy group-containing vinyl monomer, 2. The particulate copolymer according to claim 1, wherein the content C2' of the units U2' in the particulate copolymer is 2% by mass or more and 20% by mass or less, based on 100% by mass of the particulate copolymer.
4. 2. The particulate copolymer according to claim 1, wherein the particulate copolymer has a glass transition temperature of -40°C to 30°C.
5. 2. The particulate copolymer according to claim 1, wherein the particle size of the particulate copolymer is 40 to 600 nm.
6. The M2 further includes at least one selected from the group consisting of an epoxy group-containing vinyl monomer, a hydroxyl group-containing vinyl monomer, and a vinyl monomer having a hydrolyzable silyl group, 2. The particulate copolymer according to claim 1, wherein said M4 comprises at least one selected from the group consisting of a monomer having two or more radically polymerizable double bonds and an amide group-containing vinyl monomer.
7. An aqueous dispersion comprising the particulate copolymer according to any one of claims 1 to 6.
8. The aqueous dispersion according to claim 7 , further comprising an inorganic filler.
9. An adhesive for a lithium ion secondary battery for bonding an electrode and a separator, An adhesive for lithium ion secondary batteries, comprising the aqueous dispersion according to claim 7 .
10. A slurry for a protective layer of a lithium ion secondary battery, comprising the aqueous dispersion according to claim 8 .
11. An inorganic filler; A particulate copolymer according to any one of claims 1 to 6, A protective layer for a lithium ion secondary battery comprising:
12. A separator for a lithium ion secondary battery comprising the protective layer for a lithium ion secondary battery according to claim 11.
13. A lithium ion secondary battery comprising the separator for lithium ion secondary batteries according to claim 12.
Citation Information
Patent Citations
Microgel-containing anionic water-dispersible resin composition and electrodeposition coating material containing same
JP1996003489A
Reactive resin particle
JP1999124508A
Polymer solution
JP2009007572A
Battery separator and lithium-ion secondary battery
JP2009266557A
Separator for battery, and nonaqueous lithium-ion secondary battery comprising to use this
JP2009087795A