Slurry composition for nonaqueous secondary battery adhesive layer pattern coating, adhesive layer for nonaqueous secondary battery and method of producing the same, member for nonaqueous secondary battery, and nonaqueous secondary battery

A slurry composition with specific particulate polymers and coating parameters forms an adhesive layer with improved pattern and cycle characteristics for non-aqueous secondary batteries, addressing the limitations of existing compositions.

JP2024159339APending Publication Date: 2024-11-08ZEON CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023075276
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing adhesive layer compositions for non-aqueous secondary batteries, such as lithium-ion batteries, fail to form a well-defined pattern and do not adequately improve the cycle characteristics of the batteries.

Method used

A slurry composition for coating an adhesive layer in non-aqueous secondary batteries is developed, containing at least two types of particulate polymers with different glass transition temperatures, applied at a high coating speed of 40 m/min, with a solid content concentration between 5% and 30% by mass and viscosity between 20 mPa·s and 70 mPa·s, forming an adhesive layer with improved pattern and cycle characteristics.

Benefits of technology

The solution results in an adhesive layer with a good pattern and enhanced cycle characteristics for non-aqueous secondary batteries, improving their performance and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159339000001
    Figure 2024159339000001
Patent Text Reader

Abstract

To provide a slurry composition for nonaqueous secondary battery adhesive layer pattern coating with which it is possible to form an adhesive layer that has an excellent pattern formed by pattern coating and that can increase cycle characteristics of an obtained nonaqueous secondary battery.SOLUTION: There is provided a slurry composition for nonaqueous secondary battery adhesive layer pattern coating, which contains at least two types of particulate polymers. Herein, the pattern coating is performed by gravure coating with a coating speed of 40 m / min or more. The at least two types of polymers include a particulate polymer A having a glass-transition temperature of 50°C or more and 110°C or less, and a particulate polymer B having a glass-transition temperature of less than 20°C. The slurry composition for nonaqueous secondary battery adhesive layer pattern coating has a solid content concentration of 5 mass% or more and less than 30 mass%. The viscosity measured under the conditions of a temperature of 25°C and a revolving speed of 60 rpm using a B type viscometer is 20 mPa s or more and 70 mPa s or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a slurry composition for pattern coating of an adhesive layer for a nonaqueous secondary battery, an adhesive layer for a nonaqueous secondary battery and a method for producing the same, a member for a nonaqueous secondary battery, and a nonaqueous secondary battery. [Background technology]

[0002] Non-aqueous secondary batteries such as lithium ion secondary batteries (hereinafter sometimes abbreviated as "secondary batteries") are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and are used in a wide range of applications. Secondary batteries generally include battery components such as a positive electrode, a negative electrode, and a separator that isolates the positive electrode and the negative electrode to prevent a short circuit between the positive electrode and the negative electrode.

[0003] In recent years, secondary batteries have used battery components that include a porous membrane layer for the purpose of improving heat resistance and strength, and an adhesive layer for the purpose of improving adhesion between battery components. Specifically, an electrode formed by forming an adhesive layer on an electrode substrate formed by providing an electrode mixture layer on a current collector, or a separator formed by forming an adhesive layer on a separator substrate is used as a battery component. The adhesive layer is usually formed by supplying a slurry-like non-aqueous secondary battery adhesive layer composition (hereinafter sometimes abbreviated as "adhesive layer composition") containing a binder component and a dispersion medium such as water onto an appropriate substrate such as an electrode substrate or a separator substrate, and drying the composition.

[0004] From the viewpoint of improving the performance of secondary batteries, various improvements have been attempted for adhesive layer compositions. For example, Patent Document 1 describes a pattern coating slurry containing a thermoplastic polymer or the like for pattern coating at least one side of a polyolefin porous substrate used as a substrate for a separator for an electric storage device, which is applied at a shear rate of 50,000 s -1In addition, for example, Patent Document 2 discloses a slurry composition for a non-aqueous secondary battery adhesive layer, which contains at least two kinds of particulate polymers, a water-soluble polymer, and a dispersion medium, and the at least two kinds of polymers include a particulate polymer A having a glass transition temperature of 30° C. or more and 100° C. or less, and a particulate polymer B having a glass transition temperature of 20° C. or less, and the solid content concentration of the slurry composition for a non-aqueous secondary battery adhesive layer is 1% by mass or more and 25% by mass or less. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2019-8882 [Patent Document 2] International Publication No. 2023 / 033088 Summary of the Invention [Problem to be solved by the invention]

[0006] However, when the adhesive layer is formed by pattern coating using the compositions described in Patent Documents 1 and 2, there is room for further improvement in terms of forming a good pattern. Furthermore, there is room for further improvement in the cycle characteristics of the obtained secondary cell.

[0007] Therefore, an object of the present invention is to provide a slurry composition for pattern coating of an adhesive layer for a non-aqueous secondary battery, which is capable of forming an adhesive layer that has a good pattern formed by pattern coating and can improve the cycle characteristics of the resulting non-aqueous secondary battery. Another object of the present invention is to provide an adhesive layer for a non-aqueous secondary battery that has a good pattern and can improve the cycle characteristics of the non-aqueous secondary battery, and a method for producing the same. Another object of the present invention is to provide a non-aqueous secondary battery member capable of providing a non-aqueous secondary battery having excellent cycle characteristics. It is yet another object of the present invention to provide a nonaqueous secondary battery having excellent cycle characteristics. [Means for solving the problem]

[0008] In view of this, the present inventors have conducted extensive research and have newly discovered that, when forming an adhesive layer pattern by gravure coating at a coating speed of 40 m / min or more, by setting the solid content concentration of an adhesive layer slurry composition containing at least two kinds of particulate polymers having different glass transition temperatures in the range of 5% by mass or more and less than 30% by mass, and setting the viscosity in the range of 20 mPa·s or more and 70 mPa·s or less, an adhesive layer having a good pattern can be formed and the cycle characteristics of the resulting nonaqueous secondary battery can be improved, thereby completing the present invention.

[0009] That is, the present invention aims to advantageously solve the above problems, and [1] the slurry composition for non-aqueous secondary battery adhesive layer pattern coating of the present invention is a slurry composition for non-aqueous secondary battery adhesive layer pattern coating, which contains at least two kinds of particulate polymers, the at least two kinds of polymers include particulate polymer A having a glass transition temperature of 50°C to 110°C and particulate polymer B having a glass transition temperature of less than 20°C, the solid content concentration of the slurry composition for non-aqueous secondary battery adhesive layer pattern coating is 5% by mass to less than 30% by mass, the viscosity measured at 25°C and a rotation speed of 60 rpm using a B-type viscometer is 20 mPa·s to 70 mPa·s, and the pattern coating is performed by gravure coating at a coating speed of 40 m / min or more. With such a slurry composition for non-aqueous secondary battery adhesive layer pattern coating, an adhesive layer can be formed that has a good pattern formed by pattern coating and can improve the cycle characteristics of the resulting non-aqueous secondary battery. In this specification, the glass transition temperature of the polymer can be measured by the method described in the Examples.

[0010] [2] In the slurry composition for coating a non-aqueous secondary battery adhesive layer pattern described in [1] above, the particulate polymer A preferably contains a (meth)acrylic acid ester monomer unit and has a volume average particle diameter in the range of 200 nm to 1,000 nm. If the particulate polymer A contains a (meth)acrylic acid ester monomer unit, swelling of the resulting non-aqueous secondary battery can be suppressed. If the volume average particle diameter of the particulate polymer A is in the range of 200 nm to 1,000 nm, the adhesive strength of the adhesive layer and the injectability of the secondary battery can be improved. In this specification, (meth)acrylic means acrylic and / or methacrylic. In this specification, "containing a monomer unit" means "a structural unit derived from the monomer is contained in the polymer obtained using the monomer". In addition, the "volume average particle diameter" refers to a particle diameter D50 at which the cumulative volume calculated from the small diameter side becomes 50% in a particle diameter distribution (volume basis) measured using a laser diffraction particle size distribution measurement device, and can be measured according to the method described in the examples of this specification.

[0011] [3] Furthermore, in the slurry composition for coating a pattern of an adhesive layer of a non-aqueous secondary battery according to the above [1] or [2], it is preferable that the particulate polymer B is a styrene-based polymer or an acrylic-based polymer and has a volume average particle diameter in the range of 80 nm to 400 nm. If the particulate polymer B is a styrene-based polymer or an acrylic-based polymer, the internal resistance of the obtained non-aqueous secondary battery can be further reduced. In addition, if the volume average particle diameter of the particulate polymer B is within the above range, the internal resistance of the obtained secondary battery can be reduced.

[0012] [4] Furthermore, in any one of the above slurry compositions for coating a nonaqueous secondary battery adhesive layer pattern [1] to [3], the content of the particulate polymer B is preferably 1 part by mass or more and 40 parts by mass or less, based on 100 parts by mass of the particulate polymer A. If the content ratio of the particulate polymer A to the particulate polymer B is within the above range, the cycle characteristics of the obtained secondary battery can be further improved.

[0013] [5] The present invention also aims to advantageously solve the above problems, and provides an adhesive layer for a nonaqueous secondary battery, which is formed using the slurry composition for pattern coating of an adhesive layer for a nonaqueous secondary battery according to any one of [1] to [4] above. Such an adhesive layer for a nonaqueous secondary battery has a good pattern formed by pattern coating, and can improve the cycle characteristics of a nonaqueous secondary battery.

[0014] [6] The present invention also aims to advantageously solve the above problems, and the method for producing an adhesive layer for a non-aqueous secondary battery of the present invention is characterized by comprising a coating step of applying a slurry composition for pattern coating of a non-aqueous secondary battery adhesive layer according to any one of [1] to [4] above onto a substrate by pattern coating. According to this production method, the adhesive layer for a non-aqueous secondary battery of the present invention can be efficiently produced.

[0015] [7] The present invention also aims to advantageously solve the above problems, and provides a non-aqueous secondary battery member of the present invention, which comprises a non-aqueous secondary battery adhesive layer according to [5] above on a substrate. By using such a non-aqueous secondary battery member, a non-aqueous secondary battery having excellent cycle characteristics can be provided.

[0016] [8] Here, in the nonaqueous secondary battery member of [7] above, it is preferable that the base material contains an organic separator material, and the adhesive layer for a nonaqueous secondary battery is disposed adjacent to at least one surface of the organic separator material, or is disposed adjacent to a surface of a heat-resistant layer provided on at least one surface of the organic separator material. By using such a nonaqueous secondary battery member, a nonaqueous secondary battery having even more excellent cycle characteristics can be provided.

[0017] [9] The present invention also aims to advantageously solve the above problems, and the nonaqueous secondary battery of the present invention is characterized in that it comprises the nonaqueous secondary battery member of the present invention. In this way, by providing the secondary battery with the nonaqueous secondary battery member of the present invention, the cycle characteristics of the secondary battery can be improved. Effect of the Invention

[0018] According to the present invention, it is possible to provide a slurry composition for pattern coating of a non-aqueous secondary battery adhesive layer, which is capable of forming an adhesive layer that has a good pattern formed by pattern coating and can improve the cycle characteristics of the resulting non-aqueous secondary battery. Furthermore, according to the present invention, it is possible to provide an adhesive layer for a non-aqueous secondary battery that has a good pattern and can improve the cycle characteristics of the non-aqueous secondary battery, and a method for producing the same. Moreover, according to the present invention, it is possible to provide a nonaqueous secondary battery member capable of providing a nonaqueous secondary battery having excellent cycle characteristics. Furthermore, according to the present invention, a nonaqueous secondary battery having excellent cycle characteristics can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, an embodiment of the present invention will be described in detail. Here, the slurry composition for pattern coating of a nonaqueous secondary battery adhesive layer of the present invention is used for the purpose of forming a pattern of an adhesive layer for bonding battery components such as separators and electrodes to each other, or for bonding components of battery components such as a separator substrate and a heat-resistant layer to each other, by gravure coating at a coating speed of 40 m / min or more. The non-aqueous secondary battery adhesive layer of the present invention is formed using the above-mentioned slurry composition for non-aqueous secondary battery adhesive layer pattern coating, preferably according to the method for producing a non-aqueous secondary battery adhesive layer of the present invention. The non-aqueous secondary battery member of the present invention comprises at least the non-aqueous secondary battery adhesive layer of the present invention. Furthermore, the non-aqueous secondary battery of the present invention comprises at least the non-aqueous secondary battery member of the present invention.

[0020] (Slurry composition for coating a non-aqueous secondary battery adhesive layer pattern) The slurry composition for coating a non-aqueous secondary battery adhesive layer pattern of the present invention is a slurry composition for forming an adhesive layer pattern by gravure coating at a coating speed of 40 m / min or more. The slurry composition contains at least two kinds of particulate polymers, and optionally contains other components such as a water-soluble polymer and an additive. More specifically, the slurry composition contains a particulate polymer A having a glass transition temperature of 50°C or more and 110°C or less, and a particulate polymer B having a glass transition temperature of less than 20°C. Furthermore, the slurry composition is characterized in that the solid content concentration is 5% by mass or more and less than 30% by mass, and the viscosity measured using a B-type viscometer under conditions of 25°C and a rotation speed of 60 rpm is 20 mPa·s or more and 70 mPa·s or less. Furthermore, an adhesive layer formed by high-speed gravure coating at a coating speed of 40 m / min or more using the slurry composition for pattern coating of a nonaqueous secondary battery adhesive layer of the present invention has a good pattern and can improve the cycle characteristics of the resulting nonaqueous secondary battery.

[0021] <Particulate polymer A> The particulate polymer A contained in the slurry composition needs to have a glass transition temperature of 50°C or more and 110°C or less. The particulate polymer A has the function of exerting adhesiveness on the adhesive layer formed using the slurry composition for non-aqueous secondary battery adhesive layer pattern coating. Here, the particulate polymer A preferably contains a (meth)acrylic acid ester monomer unit. If the particulate polymer A contains a (meth)acrylic acid ester monomer unit, swelling of the obtained non-aqueous secondary battery can be suppressed well. Furthermore, the particulate polymer A may contain an acid group-containing monomer unit. If the particulate polymer A contains an acid group-containing monomer unit, the coating property of the slurry composition for non-aqueous secondary battery adhesive layer pattern coating can be improved. If the slurry composition for adhesive layer pattern coating has excellent coating property, the occurrence of streaks and unevenness in the formed coating film can be suppressed.

[0022] [(Meth)acrylic acid ester monomer unit] Examples of (meth)acrylic acid ester monomers capable of forming a (meth)acrylic acid ester monomer unit include (meth)acrylic acid ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl acrylate, etc. These may be used alone or in combination of two or more kinds in any ratio.

[0023] The content ratio of the (meth)acrylic acid ester monomer unit in the particulate polymer A is preferably 15% by mass or more, more preferably 30% by mass or more, and even more preferably 60% by mass or more, and is preferably 99.0% by mass or less, and more preferably 95.0% by mass or less, when the total monomer units contained in the particulate polymer A is 100% by mass. If the content ratio of the (meth)acrylic acid ester monomer unit in the particulate polymer A is the above-mentioned lower limit or more, swelling of the obtained nonaqueous secondary battery can be suppressed.

[0024] [Acid group-containing monomer unit] Examples of acid group-containing monomers capable of forming acid group-containing monomer units include monomers having an acid group, such as monomers having a carboxylic acid group, monomers having a sulfonic acid group, monomers having a phosphoric acid group, and monomers having a hydroxyl group.

[0025] Examples of the monomer having a carboxylic acid group include monocarboxylic acid and dicarboxylic acid. Examples of the monocarboxylic acid include acrylic acid, methacrylic acid, and crotonic acid. Examples of the dicarboxylic acid include maleic acid, fumaric acid, and itaconic acid. Examples of monomers having a sulfonic acid group include vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allyl sulfonic acid, (meth)acrylic acid-2-ethyl sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-allyloxy-2-hydroxypropanesulfonic acid. Furthermore, examples of monomers having a phosphate group include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, and ethyl-(meth)acryloyloxyethyl phosphate. Examples of monomers having a hydroxyl group include 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate. In the present invention, (meth)allyl means allyl and / or methallyl, and (meth)acryloyl means acryloyl and / or methacryloyl. These may be used alone or in combination of two or more kinds in any ratio.

[0026] The content ratio of the acid group-containing monomer unit in the particulate polymer A is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1.0% by mass or more, and preferably 4.5% by mass or less, and more preferably 4.0% by mass or less, when the total monomer units contained in the particulate polymer A are taken as 100% by mass. If the content ratio of the acid group-containing monomer unit in the particulate polymer A is equal to or more than the lower limit, the cycle characteristics of the secondary battery can be further improved. In addition, if the content ratio of the acid group-containing monomer unit in the particulate polymer A is equal to or less than the upper limit, the internal resistance of the obtained secondary battery can be further reduced.

[0027] [Other monomer units] The particulate polymer A may contain, without being particularly limited, monomer units other than the above-mentioned (meth)acrylic acid ester monomer units and acid group-containing monomer units. Examples of monomers capable of forming such monomer units include aromatic vinyl monomers and crosslinkable monomers. Examples of aromatic vinyl monomers include styrene, α-methylstyrene, styrenesulfonic acid, butoxystyrene, vinylnaphthalene, and the like. These may be used alone or in combination of two or more at any ratio. The crosslinkable monomer is a monomer capable of forming a crosslinked structure during or after polymerization by heating or irradiation with energy rays. More specifically, examples of the crosslinkable monomer include polyfunctional monomers having two or more polymerization reactive groups in the monomer. Examples of such polyfunctional monomers include divinyl compounds such as divinylbenzene and allyl methacrylate, di(meth)acrylic acid ester compounds such as diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, diethylene glycol diacrylate, and 1,3-butylene glycol diacrylate, tri(meth)acrylic acid ester compounds such as trimethylolpropane trimethacrylate and trimethylolpropane triacrylate, and ethylenically unsaturated monomers containing an epoxy group such as allyl glycidyl ether and glycidyl methacrylate. These may be used alone or in combination of two or more at any ratio.

[0028] In preparing the particulate polymer A, the combination and mixing ratio of the various monomers can be changed as desired depending on the application of the slurry composition.

[0029] -Structure of particulate polymer A- The particulate polymer A may have any structure, for example, a core-shell structure having a core and a shell covering the outer surface of the core. The shell may partially cover the outer surface of the core. That is, the shell of the particulate polymer A may be in a covering mode in which the shell covers the outer surface of the core but does not cover the entire outer surface of the core. Furthermore, the particulate polymer A may have a non-uniform structure in which the polymer composition is different between the center and the surface. Whether the particulate polymer A has a core-shell structure or not can be confirmed by observing the particulate polymer with a scanning electron microscope.

[0030] In addition, when the particulate polymer A has a core-shell structure, it may have any constituent element other than the above-mentioned core part and shell part. For example, the particulate polymer A may have a part formed of a polymer other than the core part inside the core part. As a specific example, the seed particle used when producing the particulate polymer A by the seed polymerization method may remain inside the core part.

[0031] In the case where the particulate polymer A has a core-shell structure, that is, a so-called core-shell polymer, the aromatic vinyl monomer unit is preferably contained in an amount of 50.0% by mass or more, more preferably 65.0% by mass or more, even more preferably 80.0% by mass or more, preferably 99.0% by mass or less, and more preferably 97.0% by mass or less, based on the total repeating units constituting the shell portion being 100% by mass. If the content of the aromatic vinyl monomer unit in the shell is equal to or more than the lower limit, the blocking resistance can be improved. If the content of the aromatic vinyl monomer unit in the shell is equal to or less than the upper limit, the adhesiveness of the obtained non-aqueous secondary battery adhesive layer can be improved, and the cycle characteristics of the secondary battery can be further improved. Examples of the aromatic vinyl monomer unit contained in the shell portion include the aromatic vinyl monomer units listed above, and among them, styrene is preferred.

[0032] In addition, when the particulate polymer A has a core-shell structure, that is, a so-called core-shell polymer, the shell portion preferably contains a monomer unit having a carboxylic acid group as an acid group-containing monomer unit as a repeating unit. If the particulate polymer A is a core-shell polymer having a shell portion satisfying such composition conditions, the electrolyte injectability and cycle characteristics of the obtained secondary battery can be improved.

[0033] In particular, as the monomer unit having a carboxylic acid group contained in the shell portion, a monomer unit derived from the above-mentioned monocarboxylic acid is preferable, a monomer unit derived from acrylic acid or methacrylic acid is more preferable, and a monomer unit derived from methacrylic acid is even more preferable.

[0034] The content of the monomer unit having a carboxylic acid group in the shell portion is preferably 0.10% by mass or more, more preferably 0.50% by mass or more, even more preferably 0.90% by mass or more, and preferably 4.50% by mass or less, and even more preferably 4.00% by mass or less, based on 100% by mass of all repeating units constituting the shell portion. If the content of the monomer unit having a carboxylic acid group in the shell portion is equal to or more than the lower limit, the cycle characteristics of the obtained secondary battery can be further improved. Also, if the content of the monomer unit having a carboxylic acid group in the shell portion is equal to or less than the upper limit, the adhesion of the obtained secondary battery can be improved.

[0035] Furthermore, when the particulate polymer A has a core-shell structure, that is, a so-called core-shell polymer, the proportion of the polymer constituting the shell part is preferably 40% by mass or less, more preferably 35% by mass or less, preferably 15% by mass or more, and more preferably 20% by mass or more, based on 100% by mass of the total mass of the core part and the shell part. If the proportion of the polymer constituting the shell part is equal to or less than the upper limit, the adhesiveness of the obtained adhesive layer can be further improved, and as a result, the cycle characteristics of the secondary battery can be further improved. If the proportion of the polymer constituting the shell part is equal to or more than the lower limit, the electrolyte injection property and cycle characteristics of the obtained secondary battery can be further improved.

[0036] -Volume average particle size of particulate polymer A- The particulate polymer A preferably has a volume average particle diameter of 200 nm or more, more preferably 300 nm or more, even more preferably 450 nm or more, preferably 1,000 nm or less, more preferably 900 nm or less, and even more preferably 750 nm or less. Furthermore, from the viewpoint of achieving a good balance between the adhesiveness and blocking resistance (resistance to blocking) of the adhesive layer, the volume average particle diameter of the particulate polymer A is preferably larger than the volume average particle diameter of the particulate polymer B described later. If the volume average particle diameter of the particulate polymer A is equal to or greater than the above lower limit, the pourability can be improved. Furthermore, if the volume average particle diameter of the particulate polymer A is equal to or less than the above upper limit, the adhesiveness of the adhesive layer can be increased. The volume average particle diameter of the particulate polymer A is not particularly limited, but can be controlled based on the amount of polymerization initiator used when synthesizing the particulate polymer A, and the amount of emulsifier used when synthesizing the particulate polymer A by emulsion polymerization.

[0037] -Glass transition temperature of particulate polymer A- The particulate polymer A must have a glass transition temperature of 50°C or more and 110°C or less, more preferably 55°C or more, more preferably 58°C or more, preferably 100°C or less, and more preferably 90°C or less. If the glass transition temperature of the particulate polymer A is equal to or higher than the lower limit, it is possible to suppress mutual adhesion and blocking when the secondary battery members having an adhesive layer on the surface are stacked and stored, and it is possible to suppress deterioration of the injectability. In addition, if the glass transition temperature of the particulate polymer A is equal to or lower than the upper limit, it is possible to increase the adhesiveness of the adhesive layer, and it is possible to further improve the cycle characteristics of the obtained secondary battery. Note that, in cases where the particulate polymer A has the above-mentioned core-shell structure, etc., a plurality of glass transition temperatures may be detected when the glass transition temperature is measured by the method described in the examples of this specification. In such a case, the lowest glass transition temperature value is taken as the glass transition temperature of the particulate polymer A. The glass transition temperature of the particulate polymer A can be adjusted to a desired temperature by changing the composition of the particulate polymer A, etc.

[0038] -Method for preparing particulate polymer A- The particulate polymer A can be prepared by a known polymerization method without being particularly limited. The polymerization mode is not particularly limited, and any mode such as solution polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc. can be used. As the polymerization method, any method such as ionic polymerization, radical polymerization, living radical polymerization, etc. can be used. In addition, in emulsion polymerization, seed polymerization using seed particles may be adopted. Furthermore, when preparing the particulate polymer A having a core-shell structure, a continuous multi-stage suspension polymerization method and a multi-stage suspension polymerization method can be adopted, which are stepwise polymerization methods in which a polymer formed in a previous stage is successively covered with a polymer formed in a later stage.

[0039] The emulsifier, dispersant, polymerization initiator, polymerization aid, and the like used in the polymerization may be any commonly used agent, and the amounts used may be the amounts commonly used.

[0040] <Particulate polymer B> The particulate polymer B contained in the slurry composition must have a glass transition temperature of less than 20°C. The particulate polymer B, together with the particulate polymer A described above, serves to exert adhesiveness on the adhesive layer formed using the slurry composition for non-aqueous secondary battery adhesive layer pattern coating. The particulate polymer B is not particularly limited as long as it is dispersible in a dispersion medium such as water, and may be any polymer. Among them, styrene-based polymers and acrylic-based polymers are preferred as the particulate polymer B. This is because it is possible to further reduce the internal resistance of the resulting non-aqueous secondary battery. As the styrene-based polymer, there is a polymer in which the proportion of styrene units is 50% by mass or more, preferably more than 60% by mass, of the total repeating units. Specifically, as the styrene-based polymer, there is a styrene-butadiene copolymer (SBR), and among them, polar group-containing SBR is preferred. As the polar group-containing SBR, there is a polymer obtained by modifying SBR with a polar group such as an acid group. As a monomer that can be used to modify SBR with an acid group, there is an acid group-containing monomer described in the particulate polymer A section. The acrylic polymer refers to a polymer containing 50% by mass or more, preferably 60% by mass or more, of all repeating units of (meth)acrylic acid ester monomer units. Here, as the (meth)acrylic acid ester monomer capable of forming the (meth)acrylic acid ester monomer units, the same monomers as those described in the particulate polymer A section can be used. Among them, as the acrylic polymer, a polymer containing 50% by mass or more and 97% by mass or less of (meth)acrylic acid ester monomer units (particularly butyl acrylate units) is preferable. As the particulate polymer B, one type may be used alone, or two or more types may be used in combination.

[0041] -Glass transition temperature of particulate polymer B- The particulate polymer B must have a glass transition temperature of less than 20° C., preferably 10° C. or less, preferably −50° C. or more, more preferably −40° C. or more. If the glass transition temperature of the particulate polymer B is less than or equal to the upper limit, the adhesiveness of the adhesive layer can be ensured. It is preferable that the particulate polymer B has one glass transition temperature.

[0042] --Volume average particle size of particulate polymer B-- The particulate polymer B preferably has a volume average particle diameter of 80 nm or more, more preferably 100 nm or more, and preferably 400 nm or less, and more preferably 200 nm or less. If the volume average particle diameter of the particulate polymer B is equal to or greater than the lower limit, the internal resistance of the resulting secondary battery can be further reduced. If the volume average particle diameter of the particulate polymer B is equal to or less than the upper limit, the blocking resistance of the adhesive layer can be improved. The volume average particle diameter of the particulate polymer B is not particularly limited, but can be controlled based on the amount of polymerization initiator used when synthesizing the particulate polymer B, and the amount of emulsifier used when synthesizing the particulate polymer B by emulsion polymerization.

[0043] Examples of the method for producing the particulate polymer B include a solution polymerization method, a suspension polymerization method, and an emulsion polymerization method. Among them, the emulsion polymerization method and the suspension polymerization method are preferred because the polymerization can be carried out in water and the aqueous dispersion containing the particulate polymer B can be used as it is as a material for a slurry composition for adhesive layer pattern coating. In addition, when producing a polymer as the particulate polymer B, the reaction system preferably contains a dispersant. The particulate polymer B is usually formed by the polymer that substantially constitutes it, but may be accompanied by any component such as an additive used during polymerization.

[0044] <Mixing ratio of particulate polymers A and B> The blending ratio of the particulate polymer A and the particulate polymer B in the slurry composition is preferably 1 part by mass or more, more preferably 5 parts by mass or more, even more preferably 7 parts by mass or more, and preferably 40 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less, relative to 100 parts by mass of the particulate polymer A. If the blending ratio of the particulate polymers A and B is within the above range, the adhesiveness of the adhesive layer is improved, and the cycle characteristics of the obtained secondary battery can be further improved.

[0045] <Water-soluble polymer> The water-soluble polymer that may be optionally contained in the non-aqueous secondary battery adhesive layer pattern coating slurry composition adjusts the viscosity of the non-aqueous secondary battery adhesive layer pattern coating slurry composition to improve coatability. Preferably, the water-soluble polymer has adhesiveness and electrolyte resistance, and plays a role in assisting adhesion between components in the adhesive layer and between battery components in the secondary battery. In addition, in this specification, the term "water-soluble" for a polymer means that when 0.5 g of the substance is dissolved in 100 g of water at 25°C, the insoluble content is less than 1.0 mass%.

[0046] -Types of water-soluble polymers- Here, the water-soluble polymer is not particularly limited, and examples thereof include natural polymers, semi-synthetic polymers, and synthetic polymers.

[0047] [Natural polymer] Examples of natural polymers include polysaccharides and proteins derived from plants or animals, as well as fermentation products of these with microorganisms and heat treatment products of these. These natural polymers can be classified into plant-derived natural polymers, animal-derived natural polymers, and microbial-derived natural polymers. Examples of natural plant polymers include gum arabic, tragacanth gum, galactan, guar gum, carob gum, karaya gum, carrageenan, pectin, agar, quince seed, alkecolloids (gasso extract), starch (derived from rice, corn, potato, wheat, etc.), and glycyrrhizin. Examples of natural animal polymers include collagen, casein, albumin, and gelatin. Examples of natural microbial polymers include xanthan gum, dextran, succinoglucan, and pullulan.

[0048] [Semi-synthetic polymer] The semi-synthetic polymer includes a cellulose-based semi-synthetic polymer, which can be classified into a nonionic cellulose-based semi-synthetic polymer, an anionic cellulose-based semi-synthetic polymer, and a cationic cellulose-based semi-synthetic polymer.

[0049] Examples of nonionic cellulose-based semi-synthetic polymers include alkyl celluloses such as methyl cellulose, methyl ethyl cellulose, ethyl cellulose, and microcrystalline cellulose; and hydroxyalkyl celluloses such as hydroxyethyl cellulose, hydroxybutyl methyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose stearoxy ether, carboxymethyl hydroxyethyl cellulose, alkyl hydroxyethyl cellulose, and nonoxynyl hydroxyethyl cellulose.

[0050] Examples of anionic cellulose-based semisynthetic polymers include those obtained by substituting the above-mentioned nonionic cellulose-based semisynthetic polymers with various derivative groups and their salts (sodium salts, ammonium salts, etc.).Specific examples include sodium cellulose sulfate, methyl cellulose, methyl ethyl cellulose, ethyl cellulose, carboxymethyl cellulose (CMC), and their salts.

[0051] Examples of cationic cellulose-based semi-synthetic polymers include low-nitrogen hydroxyethyl cellulose dimethyldiallyl ammonium chloride (polyquaternium-4), O-[2-hydroxy-3-(trimethylammonio)propyl]hydroxyethyl cellulose chloride (polyquaternium-10), and O-[2-hydroxy-3-(lauryldimethylammonio)propyl]hydroxyethyl cellulose chloride (polyquaternium-24).

[0052] [Synthetic polymer] The synthetic polymer is not particularly limited, and examples thereof include synthetic polymers containing acid group-containing monomer units in a ratio of 5% by mass to 50% by mass, vinyl acetate polymers such as polyvinyl alcohol, special ammonium polyacrylates (e.g., Aron (registered trademark) A6114, manufactured by Toagosei Co., Ltd.), acrylic acid / sulfonic acid monomer copolymers (e.g., AQUALIC (registered trademark) GL366, manufactured by Nippon Shokubai Co., Ltd.), and compounds well known as polyethylene glycol-type nonionic surfactants or propylene oxide / ethylene oxide copolymers (e.g., NOPTEX (registered trademark) ED052, manufactured by San Nopco Ltd.).

[0053] Here, the above-mentioned acid group-containing monomers can be used as the acid group-containing monomers for forming the acid group-containing monomer units. These may be used alone or in combination of two or more kinds in any ratio.

[0054] The monomer composition used to prepare the synthetic polymer preferably contains the above-mentioned acid group-containing monomer in an amount of 5% by mass or more, more preferably 25% by mass or more, preferably 50% by mass or less, and more preferably 45% by mass or less. By setting the ratio of the acid group-containing monomer in the monomer composition used to prepare the synthetic polymer within the above range, the cycle characteristics of the obtained secondary battery can be further improved. For the same reason, the content ratio of the acid group-containing monomer unit in the synthetic polymer synthesized using such a monomer composition is preferably 5% by mass or more, more preferably 25% by mass or more, preferably 50% by mass or less, and more preferably 45% by mass or less, based on the total repeating units constituting the synthetic polymer being 100% by mass. Furthermore, as the acid group-containing monomer unit contained in the synthetic polymer, a monomer having a carboxylic acid group is preferable, and a monocarboxylic acid such as acrylic acid, methacrylic acid, or crotonic acid is more preferable, and acrylic acid is particularly preferable. A synthetic polymer containing acrylic acid as an acid group-containing monomer unit within the above content range may be referred to as an acrylic synthetic polymer.

[0055] Furthermore, the monomer composition may contain other compounds copolymerizable with the acid group-containing monomer. Specifically, the other compounds include the above-mentioned (meth)acrylic acid ester monomers, the above-mentioned crosslinkable monomers, amide group-containing monomers such as (meth)acrylamide, and nitrile group-containing monomers such as acrylonitrile.

[0056] Examples of additives to be added to the monomer composition used for preparing the synthetic polymer include known additives that can be used in polymerization reactions, such as crosslinking agents such as ethylene glycol dimethacrylate, polymerization initiators such as potassium persulfate, and polymerization accelerators such as tetramethylethylenediamine. The type and amount of additive can be selected as desired depending on the polymerization method, etc.

[0057] As the polymerization solvent to be mixed with the monomer composition used for preparing the synthetic polymer, a known solvent capable of dissolving or dispersing the above-mentioned monomers can be used depending on the polymerization method, etc. Among them, it is preferable to use water as the polymerization solvent. Note that as the polymerization solvent, an aqueous solution of any compound or a mixed solution of a small amount of an organic medium and water may be used.

[0058] The synthetic polymer is obtained by, for example, radical polymerization of a monomer composition obtained by mixing the above-mentioned monomer, crosslinking agent, additive, and polymerization solvent by a known method. The solution containing the synthetic polymer and the polymerization solvent obtained by polymerizing the above-mentioned monomer composition may be used as it is for preparing a slurry composition for adhesive layer pattern coating, or may be used for preparing a slurry composition for adhesive layer pattern coating after performing solvent replacement or addition of any component.

[0059] Here, examples of the polymerization method for synthetic polymers include known polymerization methods such as aqueous solution polymerization, slurry polymerization, suspension polymerization, and emulsion polymerization, but aqueous solution polymerization using water as the polymerization solvent is preferred because it does not require a solvent removal operation, the solvent is highly safe, and there is no problem of contamination with a surfactant. Incidentally, aqueous solution polymerization is a method in which a monomer composition is adjusted to a predetermined concentration, dissolved oxygen in the reaction system is sufficiently replaced with an inert gas, a radical polymerization initiator is added, and, if necessary, heating or light irradiation such as ultraviolet light is performed to carry out a polymerization reaction.

[0060] When water is used as a polymerization solvent and the above-mentioned monomer composition is polymerized in water to prepare an aqueous solution containing a synthetic polymer, it is preferable to adjust the pH of the aqueous solution to 8 or more and 9 or less after polymerization.

[0061] - Weight average molecular weight of water-soluble polymers - The water-soluble polymer preferably has a weight average molecular weight of 300 or more, more preferably 500 or more, and preferably has a weight average molecular weight of 3,000,000 or less, more preferably 2,500,000 or less.

[0062] The weight-average molecular weight of the water-soluble polymer having a relatively large weight-average molecular weight (hereinafter, sometimes referred to as water-soluble polymer A) is preferably 100,000 or more, more preferably 150,000 or more, even more preferably 200,000 or more, and preferably 500,000 or less, more preferably 450,000 or less, and even more preferably 400,000 or less. If the weight-average molecular weight of the water-soluble polymer A is equal to or greater than the lower limit, the cycle characteristics of the obtained secondary battery can be further improved. If the weight-average molecular weight of the water-soluble polymer A is equal to or less than the upper limit, the adhesiveness of the adhesive layer can be increased.

[0063] The weight-average molecular weight of the water-soluble polymer having a relatively small weight-average molecular weight (hereinafter, sometimes referred to as water-soluble polymer B) is preferably 300 or more, more preferably 400 or more, and even more preferably 500 or more, and is preferably 90,000 or less, and more preferably 80,000 or less. If the weight-average molecular weight of water-soluble polymer B is equal to or more than the above lower limit, the cycle characteristics of the obtained secondary battery can be further improved. If the weight-average molecular weight of water-soluble polymer B is equal to or less than the above upper limit, the adhesiveness of the obtained adhesive layer can be increased.

[0064] - Blend ratio of water-soluble polymers - The blending ratio of the water-soluble polymer in the non-aqueous secondary battery adhesive layer pattern coating slurry composition is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.5 parts by mass or more, and is preferably 5.0 parts by mass or less, and more preferably 3.0 parts by mass or less, relative to 100 parts by mass of the particulate polymer A. By setting the blending ratio of the water-soluble polymer within the above range, the coatability of the slurry composition is improved, effectively suppressing the occurrence of streaks and unevenness in the adhesive layer, and further reducing the internal resistance of the resulting secondary battery.

[0065] <Other ingredients> The non-aqueous secondary battery adhesive layer pattern coating slurry composition may contain any other components in addition to the above-mentioned particulate polymers A and B and water-soluble polymer. The other components exclude the above-mentioned water-soluble polymer compounds. Examples of these other components include preservatives and antifoaming agents. These other components may be used alone or in combination of two or more. By optionally blending other components such as preservatives and antifoaming agents, the adhesive layer pattern coating slurry composition can be given desired attributes.

[0066] Among them, isothiazolinone compounds such as Navisite P40 and Acticide MBS can be preferably blended as preservatives. Also, DF6351 manufactured by Seiko PMC Corporation can be preferably blended as defoaming agents. The blending amount of these can be appropriately adjusted depending on the application. For example, the blending amount of these additives is preferably in the range of 1000 ppm or more and 3000 ppm or less in total relative to 100 parts by mass of particulate polymer A.

[0067] <Dispersion medium> Water can be used as the dispersion medium. The dispersion medium is not particularly limited as long as it can disperse the particulate polymers A and B and dissolve at least a part of the water-soluble polymer, and may be a mixed solvent of water and an organic solvent. From the viewpoint of coatability, it is preferable that the dispersion medium is water.

[0068] <Method for producing a slurry composition for coating a non-aqueous secondary battery adhesive layer pattern> The method for producing the slurry composition includes a step of mixing the particulate polymers A and B, the water-soluble polymer, and the dispersion medium with other components used as necessary. The mixing method is not particularly limited, but in order to efficiently disperse each component, mixing is usually performed using a disperser as a mixing device. The dispersing machine is preferably a machine capable of uniformly dispersing and mixing the above components. Examples include a ball mill, a sand mill, a pigment dispersing machine, a crushing machine, an ultrasonic dispersing machine, a homogenizer, a planetary mixer, etc. In addition, from the viewpoint of being able to apply a high shear force during dispersion, high dispersion machines such as a bead mill, a roll mill, and Filmix can also be used.

[0069] <Solid content concentration of slurry composition for coating non-aqueous secondary battery adhesive layer pattern> The solid content of the slurry composition must be 5% by mass or more and 30% by mass or less, preferably 26% by mass or less, preferably 12% by mass or more, and more preferably 17% by mass or more. If the solid content is within the above range, a good pattern can be formed in high-speed gravure coating at a coating speed of 40 m / min or more. More specifically, if the solid content is equal to or more than the lower limit, the pattern can be formed more favorably. If the solid content is equal to or less than the upper limit, the coatability of the slurry composition can be further improved. As a result, the cycle characteristics of the obtained secondary battery can be improved.

[0070] <Viscosity of Slurry Composition for Coating Non-Aqueous Secondary Battery Adhesive Layer Pattern> As described above, in order to improve the pattern formation in high-speed gravure coating, the viscosity of the slurry composition must be 20 mPa·s or more and 70 mPa·s or less, measured using a B-type viscometer at 25°C and a rotation speed of 60 rpm. Furthermore, in order to improve the pattern formation, the viscosity of the slurry composition is preferably 23 mPa·s or more. In order to improve the coatability of the slurry composition and form an adhesive layer without streaks or unevenness, the viscosity of the slurry composition is preferably 27 mPa·s or less. The viscosity of the slurry composition can be adjusted depending on the amount of solids of the solvent, particulate polymers A and B, and the amount of the water-soluble polymer, which is an optional component, that are blended in the slurry composition.

[0071] (Adhesive layer for non-aqueous secondary battery and non-aqueous secondary battery member having the same) The above-mentioned non-aqueous secondary battery adhesive layer pattern coating slurry composition can be used to form an adhesive layer on a suitable substrate. Specifically, the non-aqueous secondary battery adhesive layer pattern coating slurry composition can be dried on a suitable substrate to form a non-aqueous secondary battery adhesive layer. That is, the non-aqueous secondary battery adhesive layer of the present invention is made of a dried product of the above-mentioned non-aqueous secondary battery adhesive layer pattern coating slurry composition, and usually contains the above-mentioned particulate polymers A and B, and optionally contains the above-mentioned other components such as water-soluble polymers and additives. In addition, when the above-mentioned particulate polymers A and B and the optional water-soluble polymer contain crosslinkable monomer units, the crosslinkable monomer units may be crosslinked during drying of the slurry composition or during heat treatment optionally performed after drying (that is, the non-aqueous secondary battery adhesive layer may contain the above-mentioned particulate polymer A, particulate polymer B, and / or a crosslinked product of the water-soluble polymer). The preferred ratio of each component contained in the non-aqueous secondary battery adhesive layer is the same as the preferred ratio of each component in the slurry composition for coating a non-aqueous secondary battery adhesive layer pattern. In addition, the particulate polymers A and B present as particles in the slurry composition for coating a non-aqueous secondary battery adhesive layer pattern may maintain their original particle shape in the adhesive layer or may be deformed. In addition, when the particulate polymer A having a core-shell structure is blended in the slurry composition for coating an adhesive layer pattern, it is preferable that the core-shell structure itself is maintained even if the shape of the particulate polymer A as a whole is changed from the original particle shape. The adhesive layer for a non-aqueous secondary battery of the present invention has a good pattern and can improve the cycle characteristics of the non-aqueous secondary battery. Furthermore, a non-aqueous secondary battery member comprising the adhesive layer for a non-aqueous secondary battery of the present invention can improve the cycle characteristics of the resulting non-aqueous secondary battery.

[0072] <Base material> The substrate on which the adhesive layer is formed is not particularly limited, and for example, when the adhesive layer is used as a member constituting a part of the separator, a separator substrate can be used as the substrate, and when the adhesive layer is used as a member constituting a part of the electrode, an electrode substrate formed by forming an electrode mixture layer on a current collector can be used as the substrate. There is also no particular limit to the use of the adhesive layer formed on the substrate, and for example, the adhesive layer may be formed on a separator substrate or the like and used as a battery component such as a separator as it is, the adhesive layer may be formed on an electrode substrate and used as an electrode, or the adhesive layer formed on a release substrate may be peeled off from the substrate and attached to another substrate and used as a battery component. However, from the viewpoint of increasing the production efficiency of the battery component by omitting the step of peeling off the release substrate from the adhesive layer, it is preferable to use a separator substrate or an electrode substrate as the substrate.

[0073] [Separator substrate] The separator substrate is not particularly limited, and may be, for example, a separator substrate in which an arbitrary heat-resistant layer (for example, a layer containing a heat-resistant filler such as inorganic particles) is disposed on the surface of an organic separator material that is a microporous membrane made of a polyolefin resin such as polyethylene, polypropylene, polybutene, or polyvinyl chloride. In other words, the non-aqueous secondary battery member has a structure in which the non-aqueous secondary battery adhesive layer is disposed directly adjacent to at least one surface of the organic separator material, or is disposed adjacent to the surface of a heat-resistant layer provided on at least one surface of the organic separator material.

[0074] [Electrode base material] The electrode substrate (positive electrode substrate and negative electrode substrate) on which the adhesive layer is formed is not particularly limited, but may be an electrode substrate in which an electrode mixture layer is formed on a current collector. Here, the current collector, the components in the electrode mixture layer (e.g., electrode active materials (positive electrode active materials, negative electrode active materials) and binders for the electrode mixture layer (binders for the positive electrode mixture layer, binders for the negative electrode mixture layer)), and the method for forming the electrode mixture layer on the current collector may be any known method, and for example, the method described in JP 2013-145763 A may be used. The electrode base material may include, as a part thereof, any layer having a desired function other than the adhesive layer.

[0075] [Release base material] The release substrate on which the adhesive layer is formed is not particularly limited, and any known release substrate can be used.

[0076] <Weight of adhesive layer> The adhesive layer has a basis weight of 0.30 g / m 2 Preferably, it is 0.20 g / m or less. 2 More preferably, it is 0.15 g / m or less. 2 More preferably, it is 0.05 g / m or less. 2 It is preferable that the content is 0.08 g / m or more. 2 It is more preferable that the weight per unit area of ​​the adhesive layer is equal to or less than the upper limit. If the weight per unit area of ​​the adhesive layer is equal to or less than the upper limit, the injectability of the resulting adhesive layer is improved, the internal resistance of the resulting secondary battery is further reduced, and the cycle characteristics are further improved. If the weight per unit area of ​​the adhesive layer is equal to or more than the lower limit, the adhesiveness can be further improved.

[0077] (Method of manufacturing adhesive layer for non-aqueous secondary battery) The following methods can be used to form an adhesive layer on a substrate such as the separator substrate or electrode substrate described above: 1) A method in which the slurry composition is applied by gravure coating to the surface of a separator substrate or an electrode substrate (in the case of an electrode substrate, the surface on the electrode mixture layer side; the same applies below) and then dried; 2) A method in which the slurry composition is applied onto a release substrate by gravure coating, and dried to produce an adhesive layer, and the resulting adhesive layer is transferred to the surface of a separator substrate or electrode substrate. Among these, the method 1) is particularly preferred because it can improve pattern formability. Specifically, the method 1) includes a step of applying the slurry composition onto a separator substrate or an electrode substrate by gravure coating (application step), and a step of drying the slurry composition applied onto the separator substrate or the electrode substrate to form an adhesive layer (drying step).

[0078] The coating speed during gravure coating must be 40 m / min or more, preferably 60 m / min or more, and preferably 150 m / min or less, and more preferably 100 m / min or less. When the coating speed during high-speed gravure coating of the slurry composition of the present invention is within the above range, a good pattern can be efficiently produced.

[0079] In the drying step, the method for drying the slurry composition on the substrate is not particularly limited and may be any known method, such as drying with warm air, hot air, or low-humidity air, vacuum drying, or drying by irradiation with infrared rays or electron beams, etc. The drying conditions are not particularly limited, but the drying temperature is preferably 30 to 80° C., and the drying time is preferably 30 seconds to 10 minutes.

[0080] The thickness of the adhesive layer formed on the substrate is preferably 0.1 μm or more, more preferably 0.3 μm or more, and even more preferably 0.5 μm or more, and is preferably 3.0 μm or less, more preferably 1.5 μm or less, and even more preferably 1.0 μm or less. By having the thickness of the adhesive layer be equal to or more than the lower limit of the above range, the strength of the adhesive layer can be sufficiently ensured, and by having the thickness be equal to or less than the upper limit of the above range, the internal resistance of the secondary battery can be further reduced.

[0081] (Non-aqueous secondary battery) The nonaqueous secondary battery of the present invention includes the nonaqueous secondary battery member of the present invention described above. More specifically, in the nonaqueous secondary battery of the present invention, at least one of the positive electrode, the negative electrode, and the separator is the nonaqueous secondary battery member of the present invention. The nonaqueous secondary battery of the present invention has excellent cycle characteristics since it includes the nonaqueous secondary battery member of the present invention.

[0082] <Positive and negative electrodes> As described above, the secondary battery of the present invention is a non-aqueous secondary battery member of the present invention in which at least one of the positive electrode, negative electrode, and separator is provided with the adhesive layer of the present invention. That is, an electrode can be used in which an adhesive layer is provided on an electrode base material formed by forming an electrode mixture layer on a current collector. Note that the electrode base material and separator base material can be the same as those listed in the section "Adhesive layer for non-aqueous secondary battery". The positive electrode and the negative electrode having no adhesive layer are not particularly limited, and the electrodes made of the above-mentioned electrode base material can be used.

[0083] <Electrolyte> As the electrolyte, an organic electrolyte in which a supporting electrolyte is dissolved in an organic solvent is usually used. As the supporting electrolyte, for example, a lithium salt is used in a lithium ion secondary battery. As the lithium salt, for example, LiPF6, LiAsF6, LiBF4, LiSbF6, LiAlCl4, LiClO4, CF3SO3Li, C4F9SO3Li, CF3COOLi, (CF3CO)2NLi, (CF3SO2)2NLi, (C2F5SO2)NLi, etc. are listed. Among them, LiPF6, LiClO4, and CF3SO3Li are preferred because they are easily dissolved in a solvent and show a high degree of dissociation. Note that one type of electrolyte may be used alone, or two or more types may be used in combination. Usually, the lithium ion conductivity tends to be higher as the supporting electrolyte with a higher degree of dissociation is used, so the lithium ion conductivity can be adjusted by the type of supporting electrolyte.

[0084] The organic solvent used in the electrolyte is not particularly limited as long as it can dissolve the supporting electrolyte. For example, in a lithium ion secondary battery, carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), and methyl ethyl carbonate (MEC); esters such as γ-butyrolactone and methyl formate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; sulfur-containing compounds such as sulfolane and dimethyl sulfoxide; and the like are preferably used. A mixture of these solvents may also be used. Among them, carbonates are preferred because they have a high dielectric constant and a wide stable potential range. Usually, the lower the viscosity of the solvent used, the higher the lithium ion conductivity tends to be, so the lithium ion conductivity can be adjusted by the type of solvent. The concentration of the electrolyte in the electrolytic solution can be appropriately adjusted. Known additives may also be added to the electrolytic solution.

[0085] <Method of manufacturing non-aqueous secondary battery> A non-aqueous secondary battery can be produced, for example, by stacking a positive electrode and a negative electrode with a separator interposed therebetween, placing the resulting positive electrode-separator-negative electrode laminate in a battery container as is or, if necessary, by rolling or folding it, and injecting an electrolyte into the battery container and sealing it. Here, if necessary, an expand metal, a fuse, an overcurrent prevention element such as a PTC element, a lead plate, or the like may be placed in the battery container to prevent pressure rise inside the battery and overcharging and discharging. The shape of the battery may be, for example, any of a coin type, a button type, a sheet type, a cylindrical type, a square type, a flat type, and the like. EXAMPLES

[0086] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following description, the units "%" and "parts" expressing amounts are by mass unless otherwise specified. In addition, in a polymer produced by copolymerizing multiple types of monomers, the ratio of a structural unit formed by polymerizing a certain monomer in the polymer usually coincides with the ratio (feed ratio) of the certain monomer to all monomers used in the polymerization of the polymer, unless otherwise specified. In the examples and comparative examples, the measurement and evaluation of various attributes were carried out according to the following methods.

[0087] <Glass transition temperature> The glass transition temperatures of the particulate polymers A and B prepared in the examples and comparative examples were measured by measuring the DSC curves according to JIS K6240 using a differential thermal analyzer (SII NanoTechnology, EXSTAR DSC6220). Specifically, 10 mg of a dried measurement sample was weighed into an aluminum pan, and an empty aluminum pan was used as a reference. The DSC curves were measured at a temperature rise rate of 20°C / min within the measurement temperature range of -100°C to 200°C. During this temperature rise process, the endothermic peak temperature of the differential signal (DDSC) was obtained and used as the glass transition temperature of the particulate polymers A and B. Note that, for the particulate polymer A, two glass transition temperatures were detected, but the lower temperature was adopted as the glass transition temperature of the particulate polymer A.

[0088] <Viscosity of Slurry Composition> The viscosity of the slurry composition was measured using a Brookfield viscometer at 25° C. and a rotation speed of 60 rpm.

[0089] <Volume average particle size> The volume average particle diameter of the particulate polymers A and B prepared in the examples and comparative examples was measured by a laser diffraction method. Specifically, the aqueous dispersions (adjusted to a solid content concentration of 0.1% by mass) containing the prepared particulate polymers A and B were used as samples. Then, in the particle size distribution (volume basis) measured using a laser diffraction type particle size distribution measuring device (manufactured by Beckman Coulter, Inc., "LS-13320"), the particle diameter D50 at which the cumulative volume calculated from the small diameter side is 50% was taken as the volume average particle diameter.

[0090] <Weight average molecular weight of water-soluble polymer> The aqueous solutions containing the water-soluble polymers used in the examples and comparative examples were diluted to adjust the concentration to 0.5%. Then, the solutions were diluted to 0.025% with the following eluent to prepare samples. The samples were analyzed by gel permeation chromatography under the following conditions, and a molecular weight distribution curve was created to determine the weight average molecular weight of the water-soluble polymers. Apparatus: Gel permeation chromatography (GPC) (Agilent 1260 Infinity II HPLC) Detector: Differential refractive index detector RI (Agilent 1260 Infinity II) Column: 2 TSKgel GMPWXL (φ7.8mm×30cm, Tosoh) Solvent: For anionic polymers, 0.1M Tris buffer (with 0.1M potassium chloride) Flow rate: 0.7mL / min Column temperature: 40℃ Injection volume: 0.2mL Standard samples: Monodisperse polyethylene oxide (PEO) and polyethylene glycol (PEG) from Tosoh and Sigma-Aldrich

[0091] <Weight of adhesive layer> Ten test pieces with a width of 10 cm and a length of 10 cm were cut out from the substrate having the adhesive layer obtained in the examples and comparative examples, and the average value W1 (g) of the mass of the cut out test pieces was measured. In addition, the thickness of each test piece was measured at a total of five points, the four corners and the center of each test piece, and the average value was taken as the thickness T1 (μm) of each test piece. In addition, each substrate before applying the adhesive layer used in each of the examples and comparative examples was similarly cut out, and each mass W0 (g) and thickness T0 (μm) were measured by the same measurement method. From the obtained numerical value, the density ρ of the adhesive layer was calculated according to the following formula. ρ = (W1-W0) / (T1-T0) × 100

[0092] <Pattern formation evaluation> The pattern formation of the adhesive layer was evaluated as the ratio of the actual coverage to the designed coverage of the gravure plate (see formula below). The actual coverage was measured by observing the adhesive layer coated on the substrate with a scanning electron microscope (SEM), and the average coverage was obtained as the average value for 100 samples. Pattern formability = average coverage rate / design coverage rate calculated from gravure plate pattern A: 0.7 or more and less than 1.5 B: 0.6 or more and less than 0.7 or 1.5 or more and less than 2.5 C: 0.5 or more and less than 0.6 or 2.5 or more and less than 4.0 D: Outside the above range

[0093] <Coating ability of slurry composition (presence or absence of streaks)> The adhesive layers obtained in the examples and comparative examples were observed visually by applying light from the substrate side on which the adhesive layer was applied. Here, if the adhesive layer has "streaks" or "unevenness", the transmitted light amount will have a difference that can be visually determined. Here, in this specification, "streaks" refers to surface irregularities caused by the influence of the applicator used when applying the slurry composition. Also, "unevenness" refers to the variation in the layer thickness of the applied adhesive layer. Depending on the distribution pattern of the transmitted light amount, it is possible to visually determine whether "streaks" or "unevenness" has occurred in the adhesive layer to be observed. A slurry composition that can form an adhesive layer through which light can be uniformly transmitted, in other words, an adhesive layer without "streaks" and "unevenness", has good coatability, and a slurry composition that has "streaks" or "unevenness" in the formed adhesive layer has poor coatability. Therefore, the evaluation of the coatability of the slurry composition was performed according to the following criteria. The term "streaks" refers to areas where the amount of transmitted light changes in a line shape, and "unevenness" refers to areas where the boundary between the amount of transmitted light changes irregularly and is unclear. The "strong" or "weak" nature of "streaks" and "unevenness" is determined based on the degree of change in the amount of transmitted light. A: No streaks or unevenness were observed. B: Weak streaks and unevenness occurred. C: Strong streaks and unevenness were observed.

[0094] <Adhesive strength> The negative electrode with the functional layer and the separator thus prepared were cut into a width of 10 mm and a length of 50 mm. Next, the cut negative electrode with the functional layer and the separator were stacked so that the functional layer and the separator faced each other, and pressed for 1 minute with a flat plate press at a temperature of 90°C and a load of 1 MPa to obtain a test piece in which the negative electrode and the separator were integrated through the functional layer. The negative electrode (current collector) side of the obtained test piece was placed down, and cellophane tape was attached to the current collector surface. At this time, the cellophane tape specified in JIS Z1522 was used, and the cellophane tape was fixed to a horizontal test table. Then, the stress when one end of the test piece on the separator side was pulled in the vertical direction at a speed of 50 mm / min and peeled off was measured. The same measurement was performed three times, and the average value of the measurement results was taken as the peel strength, and the adhesiveness was evaluated according to the following criteria. The higher the peel strength value, the better the adhesiveness between the battery components via the functional layer. SA: Peel strength is 12N / m or more A: Peel strength is 10N / m or more and less than 12N / m B: Peel strength is 8N / m or more and less than 10N / m C: Peel strength is 3N / m or more and less than 8N / m D: Peel strength is less than 3N / m

[0095] <Electrolyte injection performance> An electrolyte solution (solvent: ethylene carbonate (EC) / diethyl carbonate (DEC) / vinylene carbonate (VC) (volume ratio) = 68.5 / 30 / 1.5, electrolyte: LiPF6 with a concentration of 1M) was injected into the lithium ion secondary batteries produced in the examples and comparative examples. The inside of the lithium ion secondary batteries was then reduced in pressure to -100 kPa and kept in that state for 1 minute. Thereafter, heat sealing was performed. After 10 minutes, the electrode (positive electrode) was disassembled, and the state of electrolyte impregnation in the electrode was visually confirmed. Evaluation was then performed according to the following criteria. The greater the portion of the electrode impregnated with electrolyte, the higher the electrolyte injectability. A: The electrolyte is impregnated on all sides of the electrode. B: The part of the electrode that is not impregnated with electrolyte is 1 cm 2Less than 100% of the surface area is impregnated (except that all surfaces are impregnated). C: The part of the electrode that is not impregnated with electrolyte is 1 cm 2 More than that remains.

[0096] <Secondary battery internal resistance> The lithium ion secondary batteries prepared in the examples and comparative examples were left to stand at 25°C for 5 hours after injecting the electrolyte. Next, the batteries were charged to a cell voltage of 3.65V at a constant current of 0.2C at 25°C, and then aged at 60°C for 12 hours. Then, the batteries were discharged to a cell voltage of 3.00V at a constant current of 0.2C at 25°C. Then, CC-CV charging (upper cell voltage 4.35V) was performed at a constant current of 0.2C, and CC discharging was performed at a constant current of 0.2C to a cell voltage of 3.00V. This charging and discharging at 0.2C was repeated three times. Next, in an environment at a temperature of 25°C, constant current charging and discharging was performed at 0.2C with a cell voltage between 4.2-3.00V, and the discharge capacity at this time was defined as C0. Thereafter, similarly, CC-CV charging was performed at a constant current of 0.2C, and discharge was performed to 3.0V at a constant current of 0.5C in an environment at a temperature of -10°C, and the discharge capacity at this time was defined as C1. Then, as the rate characteristic, the capacity retention rate represented by ΔC=(C1 / C0)×100(%) was calculated and evaluated according to the following criteria. The larger the value of this capacity retention rate ΔC, the lower the internal resistance, and the higher the discharge capacity at high current in a low temperature environment. A: Capacity retention rate ΔC is 70% or more (resistance: low) B: Capacity retention rate ΔC is 55% or more and less than 70% (resistance: medium) C: Capacity retention rate ΔC is less than 55% (resistance: large)

[0097] <Cycle characteristics> After injecting the electrolyte, the lithium ion secondary batteries produced in the examples and comparative examples were left to stand for 24 hours in an environment of 25° C. Thereafter, at 25° C., the batteries were charged to 4.2 V (cutoff condition: 0.02 C) in a constant voltage constant current (CC-CV) mode at a charge rate of 1 C, and discharged to 3.0 V in a constant current (CC) mode at a discharge rate of 1 C, and the initial capacity C2 was measured. Furthermore, the same charge / discharge operation was repeated in a 45°C environment, and the capacity C3 after 300 cycles was measured. The capacity retention rate ΔC' = (C3 / C2) × 100 (%) was calculated and evaluated according to the following criteria. The higher the capacity retention rate, the less the secondary battery's discharge capacity declines and the better its cycle characteristics. SA: Capacity retention rate ΔC´90% or more A: Capacity retention rate ΔC' is 85% or more and less than 90% B: Capacity retention rate ΔC´ is 75% or more and less than 85% C: Capacity retention rate ΔC´ is 65% or more and less than 75% D: Capacity retention rate ΔC´ is less than 65%

[0098] Example 1 <Preparation of Particulate Polymer A> As the particulate polymer A, organic particles 1-1 having a core-shell structure were prepared. First, in order to form a core portion, 45 parts of methyl methacrylate monomer and 21.83 parts of butyl acrylate as (meth)acrylic acid ester monomers, 2.8 parts of methacrylic acid monomer as an acid group-containing monomer, and 0.07 parts of allyl methacrylate as a crosslinkable monomer were added to a 5 MPa pressure-resistant container equipped with a stirrer. Furthermore, 1 part of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.5 parts of potassium persulfate as a polymerization initiator were added, and after sufficient stirring, the inside of the container was heated to 60°C to start polymerization. When the polymerization conversion rate reached 96%, 29 parts of styrene, 0.3 parts of methacrylic acid monomer, and 1 part of acrylonitrile were continuously added to the above container in order to form a shell portion, and the inside of the container was heated to 70°C to continue polymerization, and when the polymerization conversion rate reached 96%, the reaction was stopped by cooling. As a result, an aqueous dispersion (polymer 1-1) containing organic particles 1-1 was obtained. The glass transition temperature and volume average particle size of the obtained polymer (1-1) as particulate polymer A were measured according to the above-mentioned method. The results are shown in Table 1. When the obtained polymer (1-1) as particulate polymer A was observed with a scanning electron microscope, it was confirmed that it had a core-shell structure.

[0099] <Preparation of Particulate Polymer B> In a 5 MPa pressure vessel equipped with a stirrer, 65 parts of styrene, 32.5 parts of 1,3-butadiene, 1 part of methacrylic acid monomer, 1 part of hydroxyethyl acrylate, 0.5 parts of allyl methacrylate, 0.4 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.5 parts of potassium persulfate as a polymerization initiator were placed, thoroughly stirred, and then heated to 50°C to initiate polymerization. When the polymerization conversion rate reached 96%, the reaction was stopped by cooling to obtain a mixture containing polymer (2-1) as particulate polymer B. A 5% aqueous sodium hydroxide solution was added to the mixture containing the polymer (2-1) to adjust the pH to 8. Thereafter, unreacted monomers were removed from the mixture by heating and reduced pressure distillation, and the mixture was cooled to 30°C or less to obtain an aqueous dispersion containing the desired polymer (2-1). The glass transition temperature and volume average particle size of polymer (2-1) as particulate polymer B were measured according to the above-mentioned method. The results are shown in Table 1.

[0100] <Preparation of Water-soluble Polymer A> As the water-soluble polymer A, synthetic water-soluble polymer 1 (synthetic WP1) was prepared. In a 5 MPa pressure vessel equipped with a stirrer, 34 parts of methacrylic acid as an acid group-containing monomer, 65 parts of ethyl acrylate as a (meth)acrylic acid ester monomer, 1.0 parts of ethylene glycol dimethacrylate as a crosslinkable monomer, 1.0 parts of polyoxyalkylene alkenyl ether ammonium sulfate, 150 parts of ion-exchanged water, and 0.5 parts of potassium persulfate as a polymerization initiator were added, and after sufficient stirring, the vessel was heated to 60 ° C. to start polymerization. When the polymerization conversion rate reached 96%, the reaction was stopped by cooling, and an aqueous dispersion containing synthetic water-soluble polymer 1 (synthetic WP1) as the water-soluble polymer A was obtained. Next, the aqueous dispersion containing the synthetic WP1 and a 5% by mass aqueous sodium hydroxide solution were added to a container equipped with a stirrer and charged with ion-exchanged water, with the pH of the resulting solution being 8 and the concentration of synthetic WP1 in the resulting solution being 1% by mass, and the mixture was sufficiently stirred to dissolve the synthetic WP1. In this way, an aqueous solution of water-soluble polymer A was prepared. The weight average molecular weight of the resulting water-soluble polymer A was measured as described above and found to be 280,000.

[0101] <Preparation of Slurry Composition for Coating Non-Aqueous Secondary Battery Adhesive Layer Pattern> 100 parts by mass (solids equivalent) of particulate polymer A, 10 parts by mass (solids equivalent) of particulate polymer B, and 1.5 parts by mass (solids equivalent) of the water-soluble polymer A aqueous solution were added to a container equipped with a stirrer and mixed. 2000 ppm of preservative (Navisite P40) and 150 ppm of defoamer (DF6351 manufactured by Seiko PMC Co., Ltd.) were added thereto, and the mixture was further diluted with ion-exchanged water to obtain a slurry composition for adhesive layer pattern coating with a solids concentration of 25% by mass. The viscosity of the obtained slurry composition was measured according to the above. The results are shown in Table 1.

[0102] <Formation of adhesive layer for non-aqueous secondary battery> The adhesive layer pattern coating slurry composition obtained as described above was pattern coated onto a separator substrate (polypropylene, Celgard 2500) at a coating speed of 80 m / min using a gravure coater (manufactured by Fuji Kikai Kogyo Co., Ltd.), and dried at 50°C for 10 seconds. This operation was performed on both sides of the separator substrate to obtain a separator equipped with an adhesive layer having a thickness of 1 μm on each side. For the separator equipped with the obtained adhesive layer, the basis weight of the adhesive layer was measured as described above, and the pattern was evaluated. The results are shown in Table 1.

[0103] <Preparation of negative electrode> In a 5 MPa pressure vessel equipped with a stirrer, 33 parts of 1,3-butadiene, 3.5 parts of itaconic acid, 63.5 parts of styrene, 0.4 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.5 parts of potassium persulfate as a polymerization initiator were placed, and after thorough stirring, the vessel was heated to 50°C to initiate polymerization. When the polymerization conversion rate reached 96%, the reaction was stopped by cooling to obtain a mixture containing a particulate binder (SBR). A 5% by mass aqueous solution of sodium hydroxide was added to the mixture containing the particulate binder to adjust the pH to 8, and unreacted monomers were removed by heating and reduced pressure distillation, and then the mixture was cooled to 30°C or less to obtain an aqueous dispersion containing a particulate binder. 100 parts of artificial graphite (average particle size: 15.6 μm), 1 part of a 2% aqueous solution of carboxymethylcellulose (manufactured by Nippon Paper Industries Co., Ltd., "MAC350HC") as a thickener in terms of solid content, and ion-exchanged water were used to adjust the solid content concentration to 68% by mass, and then mixed at 25 ° C. for 60 minutes. The solid content concentration was further adjusted to 62% by mass with ion-exchanged water, and then mixed for another 15 minutes at 25 ° C. The above-mentioned particulate binder was added to the obtained mixture in terms of solid content equivalent to 1.5 parts, and ion-exchanged water was further added to adjust the final solid content concentration to 52% by mass, and then mixed for another 10 minutes. This was defoamed under reduced pressure to obtain a negative electrode slurry composition with good fluidity. The slurry composition for negative electrode obtained above was applied to a copper foil having a thickness of 20 μm as a current collector using a comma coater so that the film thickness after drying was about 150 μm, and then dried. This drying was performed by conveying the copper foil at a speed of 0.5 m / min in an oven at 60° C. for 2 minutes. Then, the copper foil was heated at 120° C. for 2 minutes to obtain a negative electrode raw sheet before pressing. This negative electrode raw sheet before pressing was rolled with a roll press to obtain a negative electrode after pressing with a negative electrode active material layer having a thickness of 80 μm (single-sided negative electrode).

[0104] <Preparation of positive electrode> As a positive electrode active material, 100 parts of LiCoO2 having a volume average particle diameter of 12 μm, 2 parts of acetylene black ("HS-100" manufactured by Denka Co., Ltd.) as a conductive material, 2 parts (solid content equivalent) of PVDF (manufactured by Kureha Corporation, #7208) as a binder, and N-methyl-2-pyrrolidone (NMP) were mixed to adjust the total solid content concentration to 70 mass %. These were mixed by a planetary mixer to prepare a positive electrode slurry composition. The slurry composition for positive electrode obtained as described above was applied to a 20 μm thick aluminum foil current collector using a comma coater so that the film thickness after drying was about 150 μm, and then dried. This drying was performed by conveying the copper foil at a speed of 0.5 m / min in an oven at 60° C. for 2 minutes. Then, the copper foil was heated at 120° C. for 2 minutes to obtain a pre-press positive electrode raw material. This pre-press positive electrode raw material was rolled using a roll press to obtain a post-press positive electrode with a positive electrode active material layer thickness of 80 μm (single-sided positive electrode).

[0105] <Manufacturing lithium-ion secondary batteries> The pressed positive electrode obtained as described above was cut into a square piece of 4 cm square. The separator having the adhesive layer for a non-aqueous secondary battery obtained as described above was cut into a square piece of 5 cm square. Then, a square piece of the separator was placed on the surface of the positive electrode composite layer side of the cut square piece of the positive electrode. Furthermore, the pressed negative electrode prepared as described above was cut into a square piece of 4.2 cm square, and this was further placed on the square piece of the separator so that the surface of the negative electrode composite layer side faces. Next, the obtained laminate was pressed at a temperature of 60 ° C. and 0.5 MPa to be bonded. The bonded laminate was then wrapped in an aluminum packaging exterior as the exterior of the battery, and an electrolyte (solvent: ethylene carbonate (EC) / diethyl carbonate (DEC) / vinylene carbonate (VC) (volume ratio) = 68.5 / 30 / 1.5, electrolyte: LiPF6 with a concentration of 1M) was injected so that no air remained. Then, the opening of the aluminum packaging exterior was heat-sealed at 150°C, and the aluminum packaging exterior was hermetically closed to produce a 40mAh laminated lithium-ion secondary battery. The obtained laminated lithium ion secondary battery was subjected to various evaluations as described above. The results are shown in Table 1.

[0106] (Examples 2 to 3) The same operations, measurements, and evaluations as in Example 1 were carried out, except that the solid content concentration in preparing the adhesive layer pattern coating slurry composition was changed as shown in Table 1. The results are shown in Table 1.

[0107] (Examples 4 to 5) The same operations, measurements, and evaluations as in Example 1 were carried out, except that the viscosity in preparing the adhesive layer pattern coating slurry composition was changed as shown in Table 1. The results are shown in Table 1.

[0108] (Examples 6 to 7) The same operations, measurements, and evaluations were carried out as in Example 1, except that the gravure plate used in forming the non-aqueous secondary battery adhesive layer was changed so that the basis weight was as shown in Table 1. The results are shown in Table 1.

[0109] Example 8 The same operations, measurements and evaluations as in Example 1 were carried out, except that polymer (1-2) was prepared by changing the composition of the particulate polymer A as shown in Table 1. The results are shown in Table 1. <Preparation of Polymer (1-2)> As the particulate polymer A, a polymer (1-2) having a core-shell structure was prepared. First, in order to form a core portion, 35 parts of 2-ethylhexyl acrylate as a (meth)acrylic acid ester monomer, 31.1 parts of styrene as an aromatic vinyl monomer, 2.8 parts of methacrylic acid monomer as an acid group-containing monomer, and 0.8 parts of ethylene glycol dimethacrylate as a crosslinkable monomer were added to a 5 MPa pressure vessel equipped with a stirrer. Furthermore, 1 part of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.5 parts of potassium persulfate as a polymerization initiator were added, and after sufficient stirring, the vessel was heated to 60°C to initiate polymerization. When the polymerization conversion rate reached 96%, 30 parts of styrene and 0.3 parts of methacrylic acid monomer were continuously added to the vessel to form a shell portion, and the vessel was heated to 70°C to continue polymerization, and when the polymerization conversion rate reached 96%, the vessel was cooled to stop the reaction. This resulted in an aqueous dispersion containing the polymer (1-2) as the particulate polymer A. When the obtained polymer (1-2) as the particulate polymer A was observed with a scanning electron microscope, it was confirmed that the polymer had a core-shell structure.

[0110] Example 9 The composition of the particulate polymer B was changed as shown in Table 1, and a polymer (2-2) was prepared as follows, but the same operations, measurements, and evaluations as in Example 1 were carried out. The results are shown in Table 1. <Preparation of Polymer (2-2)> To a reactor equipped with a stirrer, 90 parts of ion-exchanged water, 0.05 parts of sodium dodecylbenzenesulfonate (manufactured by Kao Chemical Corporation, "Neopelex G-15") as an emulsifier, and 0.23 parts of ammonium persulfate were supplied, the gas phase was replaced with nitrogen gas, and the temperature was raised to 70°C. On the other hand, in another vessel, 50 parts of ion-exchanged water, 0.1 parts of sodium dodecylbenzenesulfonate as an emulsifier, 2 parts of methacrylic acid (MAA) as an acid group-containing monomer, 2.5 parts of acrylonitrile (AN) as a nitrile group-containing monomer, and 95 parts of n-butyl acrylate (BA) as a (meth)acrylic acid ester monomer and 0.5 parts of allyl methacrylate (AMA) as a crosslinkable monomer were mixed to obtain a monomer composition. This monomer composition was continuously added to the reactor over 4 hours to perform polymerization. During the addition, the reaction was carried out at 80°C. After the addition was completed, the mixture was stirred at 80°C for another 3 hours to terminate the reaction, and an aqueous dispersion containing polymer (2-2) as particulate polymer B was obtained.

[0111] Example 10 The same operations, measurements, and evaluations were carried out as in Example 1, except that no water-soluble polymer A was added, and 1.5 parts of a special polyacrylic acid ammonium salt (Aron (registered trademark) A6114, manufactured by Toagosei Co., Ltd.; weight average molecular weight: 8000 (nominal value)) was used as the water-soluble polymer B. The results are shown in Table 1.

[0112] (Examples 11 to 12) The amount of the polymerization initiator was adjusted, specifically, in Example 11, the amount was greater than that in Example 1, and in Example 12, the amount was less than that in Example 1. In Example 11, a polymer (1-3) having a volume average particle diameter of 200 nm was obtained. In Example 12, a polymer (1-4) having a volume average particle diameter of 1000 nm was obtained. Except for these points, the same operations, measurements, and evaluations were performed as in Example 1. The results are shown in Table 1. When the obtained polymers (1-3) and (1-4) as the particulate polymer A were observed with a scanning electron microscope, it was confirmed that they had a core-shell structure.

[0113] (Comparative Examples 1 to 2) The same operations, measurements, and evaluations as in Example 1 were carried out, except that the solid content concentration in preparing the adhesive layer pattern coating slurry composition was changed as shown in Table 1. The results are shown in Table 1.

[0114] (Comparative Examples 3 to 4) The same operations, measurements, and evaluations as in Example 1 were carried out, except that the viscosity in preparing the adhesive layer pattern coating slurry composition was changed as shown in Table 1. The results are shown in Table 1.

[0115] In addition, in Table 1 shown below, "MMA" stands for methyl methacrylate. "BA" stands for butyl acrylate. "ST" stands for styrene. "MAA" stands for methacrylic acid; "AMA" stands for allyl methacrylate; "EDMA" stands for ethylene glycol dimethacrylate, "2EHA" indicates 2-ethylhexyl acrylate, "AN" indicates acrylonitrile, "BD" indicates 1,3-butadiene; "HEA" refers to 2-hydroxyethyl acrylate.

[0116] [Table 1]

[0117] According to Examples 1 to 12, when forming an adhesive layer pattern by high-speed gravure coating, it is found that when the solid content concentration of the slurry composition for coating an adhesive layer pattern, which contains at least two types of particulate polymers having different glass transition temperatures, is in the range of 5% by mass or more and less than 30% by mass, and the viscosity is in the range of 20 mPa·s or more and 70 mPa·s or less, an adhesive layer having a good pattern can be formed, and the cycle characteristics of the resulting nonaqueous secondary battery can be improved. [Industrial Applicability]

[0118] According to the present invention, it is possible to provide a slurry composition for pattern coating of a non-aqueous secondary battery adhesive layer, which is capable of forming an adhesive layer that has a good pattern formed by pattern coating and can improve the cycle characteristics of the resulting non-aqueous secondary battery. Furthermore, according to the present invention, it is possible to provide an adhesive layer for a non-aqueous secondary battery that has a good pattern and can improve the cycle characteristics of the non-aqueous secondary battery, and a method for producing the same. Moreover, according to the present invention, it is possible to provide a nonaqueous secondary battery member capable of providing a nonaqueous secondary battery having excellent cycle characteristics. Furthermore, according to the present invention, a nonaqueous secondary battery having excellent cycle characteristics can be provided.

Claims

1. A slurry composition for coating a non-aqueous secondary battery adhesive layer pattern, comprising at least two types of particulate polymers, The at least two kinds of polymers include a particulate polymer A having a glass transition temperature of 50° C. or more and 110° C. or less, and a particulate polymer B having a glass transition temperature of less than 20° C., the solid content concentration of the nonaqueous secondary battery adhesive layer pattern coating slurry composition is 5% by mass or more and less than 30% by mass, and the viscosity measured using a B-type viscometer under conditions of 25° C. and a rotation speed of 60 rpm is 20 mPa s or more and 70 mPa s or less, The pattern coating is performed by gravure coating at a coating speed of 40 m / min or more. A slurry composition for coating a non-aqueous secondary battery adhesive layer pattern.

2. 2. The slurry composition for coating a non-aqueous secondary battery adhesive layer pattern according to claim 1, wherein the particulate polymer A contains (meth)acrylic acid ester monomer units and has a volume average particle diameter in the range of 200 nm to 1,000 nm.

3. 2. The slurry composition for coating a non-aqueous secondary battery adhesive layer pattern according to claim 1, wherein the particulate polymer B is a styrene-based polymer or an acrylic-based polymer and has a volume average particle diameter in the range of 80 nm to 400 nm.

4. The slurry composition for coating a non-aqueous secondary battery adhesive layer pattern according to claim 1, wherein the content of the particulate polymer B is 1 part by mass or more and 40 parts by mass or less, based on 100 parts by mass of the particulate polymer A.

5. 5. A non-aqueous secondary battery adhesive layer formed using the slurry composition for pattern coating of a non-aqueous secondary battery adhesive layer according to claim 1.

6. A method for producing an adhesive layer for a non-aqueous secondary battery, comprising a coating step of applying the slurry composition for pattern coating of a non-aqueous secondary battery adhesive layer according to any one of claims 1 to 4 onto a substrate by pattern coating.

7. A member for a non-aqueous secondary battery comprising the adhesive layer for a non-aqueous secondary battery according to claim 5 on a substrate.

8. 8. The non-aqueous secondary battery member according to claim 7, wherein the substrate comprises an organic separator material, and the adhesive layer for a non-aqueous secondary battery is disposed adjacent to at least one surface of the organic separator material, or is disposed adjacent to a surface of a heat-resistant layer provided on at least one surface of the organic separator material.

9. A non-aqueous secondary battery comprising the member for non-aqueous secondary batteries according to claim 7.

Citation Information

Patent Citations

  • Binder composition for nonaqueous secondary battery functional layer, slurry composition for nonaqueous secondary battery functional layer, functional layer for nonaqueous secondary battery, nonaqueous secondary battery, and manufacturing method thereof

    JP2016154108A

  • Battery separator and method of manufacturing same

    WO2017094486A1

  • Method for producing laminated body and coating system

    WO2021153165A1

  • Slurry composition for nonaqueous secondary battery adhesive layer, nonaqueous secondary battery adhesive layer and manufacturing method therefor, nonaqueous secondary battery member, and nonaqueous secondary battery