Laminate film
A laminated film with a resin layer containing a chromic compound in microcapsules addresses the challenges of using chromic compounds decoratively, offering flexibility, scratch resistance, and color change, suitable for decorative applications.
Patent Information
- Application Number
- JP2023147848
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2023-09-12
- Publication Date
- 2024-11-08
AI Technical Summary
Chromic compounds, such as thermochromic and photochromic compounds, are not commonly used for decorative purposes due to issues like destruction under UV irradiation when mixed with a hard coat agent and the need to conform to complex surface shapes.
A laminated film structure is developed with a specific resin layer composition containing a binder resin and a chromic compound, which includes a chromic compound in microcapsules, providing a color tone change amount (ΔX) of 5.7 or more, and is designed for flexibility and scratch resistance.
The laminated film achieves appropriate hardness, flexibility, and excellent repeated bending characteristics while changing color tone in response to external stimuli, suitable for decorative applications.
Smart Images

Figure 2024159409000007 
Figure 2024159409000008 
Figure 2024159409000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminated film. [Background technology]
[0002] Laminated films with a functional layer on at least one side of a base film are used in various fields such as industrial compounds, optical compounds, electronic component compounds, and battery packaging materials. Polyethylene terephthalate (PET) films, which are representative polyester films, and biaxially oriented PET films in particular, are widely used as the base film for laminated films because of their excellent transparency, mechanical strength, heat resistance, flexibility, and other properties.
[0003] In recent years, thermochromic compounds and photochromic compounds have been used as light-adjusting materials, mainly for optical applications such as contact lenses, window glass, and liquid crystal displays (for example, Patent Document 1). There are also examples of their use as an anti-counterfeiting measure (Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2001-353801 A [Patent Document 2] Japanese Patent Application Publication No. 3-231394 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the above-mentioned chromic compounds have hardly been applied to decorative purposes. Furthermore, when applied to decorative purposes, it is common to provide an active energy curing type hard coat layer, so when a hard coat agent and a chromic compound are mixed and cured, there is a concern that the chromic compound may be destroyed by ultraviolet light irradiation. Furthermore, depending on the application, it may be necessary to be able to follow complex curved shapes.
[0006] Therefore, an object of the present invention is to propose a new laminated film that has appropriate hardness and flexibility, while having practical excellent repeated bending properties and abrasion resistance, and yet has the property of changing color tone in response to external stimuli. [Means for solving the problem]
[0007] In view of the above circumstances, the present inventors have conducted extensive research and found that the above problems can be easily solved by providing a laminated structure of resin layers having specific configurations, and have completed the present invention. That is, the present invention provides the following items [1] to
[27] .
[0008] [1] A laminate film comprising a base film and a resin layer provided on at least one surface of the base film, the resin layer containing a binder resin (A) and a chromic compound (B), and a color change (ΔX) of the surface of the resin layer calculated by the following formula (1) is 5.7 or more: ΔX=((ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2 ) 1 / 2 (1) ΔL * :L before and after external stimulation * Amount of change in value Δa * : a before and after external stimulation * Amount of change in value Δb * :b before and after external stimulation * Amount of change in value [2] The laminated film according to the above [1], wherein the binder resin (A) is an acrylic resin. [3] The laminate film according to the above [1], wherein the chromic compound (B) is a photochromic compound or a thermochromic compound. [4] The laminate film according to the above [1], wherein the content of the chromic compound (B) in the resin layer is 0.1% by mass to 5.0% by mass. [5] The laminate film according to the above [1], wherein the resin layer is formed by curing a resin composition containing a chromic compound (B) in microcapsules. [6] The laminate film according to the above [1], wherein the acrylic resin is an active energy ray-curable type. [7] The laminate film according to the above [1], wherein the base film is a polyester film. [8] The laminate film according to the above [2], wherein the base film is a polyethylene terephthalate (PET) film. [9] The laminate film according to the above [1], wherein the base film is a copolymer polyester film.
[10] The laminate film according to the above [1], which can be folded more than 200,000 times in a repeated bending test (outward bending, R=2.0 mm).
[11] The laminate film according to any one of the above [1] to
[10] , further comprising a functional layer A between the base film and the resin layer.
[12] The laminate film described in
[11] above, wherein the functional layer A is a printed layer.
[13] The laminated film described in
[11] above, wherein the functional layer A is a release layer.
[14] The laminate film described in [1] above, further comprising a functional layer B on the resin layer.
[15] The laminate film according to the above
[14] , wherein the functional layer B is a hard coat layer.
[16] The laminate film according to the above [1], wherein the resin layer has a thickness of 20 μm or less.
[17] A laminate film comprising a base film and a resin layer provided on at least one surface of the base film, the resin layer containing a binder resin (A) and a chromic compound (B), and a color change (ΔX) of the surface of the resin layer calculated by the following formula (1) is 5.7 or more; A laminate comprising other resin films bonded to both sides of the laminate film via adhesive layers. ΔX=((ΔL * ) 2 +(Δa * ) 2 +(Δb * )2 ) 1 / 2 (1) ΔL * :L before and after external stimulation * Amount of change in value Δa * : a before and after external stimulation * Amount of change in value Δb * :b before and after external stimulation * Amount of change in value
[18] A laminate film comprising a base film and a resin layer provided on at least one surface of the base film, the resin layer containing a binder resin (A) and a chromic compound (B), and a color change (ΔX) of the surface of the resin layer calculated by the following formula (1) is 5.7 or more; A laminate having a functional layer A between the base film and the resin layer, a printed layer or vapor deposition layer on the resin layer of the laminate film, and another resin film bonded on top of that via an adhesive layer. ΔX=((ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2 ) 1 / 2 (1) ΔL * :L before and after external stimulation * Amount of change in value Δa * : a before and after external stimulation * Amount of change in value Δb * :b before and after external stimulation * Amount of change in value
[19] The laminate according to
[18] above, wherein the functional layer A is a release layer.
[20] The laminate according to
[17] or
[18] above, further comprising another functional layer B on the resin layer.
[21] The laminate according to the above
[20] , wherein the other functional layer B is a hard coat layer.
[22] The laminate according to the above
[17] , wherein the other resin film attached to the resin layer side is a PMMA resin film.
[23] The laminate according to
[17] or
[18] above, wherein the other resin film is an ABS resin film.
[24] The laminate film according to any one of the above [1] to
[16] , which is for molding or decoration.
[25] The laminate according to any one of the above
[17] to
[19] , which is for molding or decoration.
[26] The laminate film according to
[24] above, which is used for decorating automobile parts.
[27] The laminate according to the above
[25] , which is used for decorating automobile parts. Effect of the Invention
[0009] According to the present invention, it is possible to provide a laminated film that has appropriate hardness and flexibility, is excellent in practical repeated bending properties and abrasion resistance, and yet has the property of changing color tone in response to an external stimulus. [Brief description of the drawings]
[0010] [Figure 1] 1 shows a structure (laminate 1) illustrating one example of an embodiment of the present invention. [Diagram 2] 1 shows a structure (laminate 2) illustrating one example of an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Next, the present invention will be described based on an embodiment, however, the present invention is not limited to the embodiment described below.
[0012] <<Laminated film>> A laminate film according to one embodiment of the present invention (hereinafter, sometimes referred to as "the present laminate film") is a laminate film having a structure in which a resin layer is laminated on at least one surface of a base film (hereinafter, sometimes referred to as "the present base film"). As long as the present laminate film has the above-mentioned structure, it may have other layers.
[0013] <Base film> The material and configuration of the base film are not limited as long as the film can provide sufficient rigidity and repeated folding properties. However, a polyester film is preferred because it has suitable hardness and flexibility while providing practical repeated folding properties and excellent abrasion resistance.
[0014] The base film may have a single layer structure or a multilayer structure. When the base film has a multilayer structure, it may have a two-layer or three-layer structure, or may have four or more layers other than the two-layer or three-layer structure as long as it does not deviate from the gist of the present invention.
[0015] The base film may be a single layer or a multilayer, and the main component resin of each layer is preferably polyester. Such a film is called a "polyester film." In this case, "main component resin" means the resin that is contained in the largest proportion among the resins constituting the base film, for example, a resin that accounts for 50 mass % or more, particularly 70 mass % or more, and even more particularly 80 mass % or more (including 100 mass %) of the resins constituting the base film. Each layer constituting the base film may contain a resin other than polyester or a component other than resin, so long as the main component resin is polyester.
[0016] (polyester) The polyester as the main component resin of each layer constituting the base film (hereinafter sometimes referred to as "the polyester") may be either a homopolyester or a copolymer polyester.
[0017] When the present polyester is a homopolyester, it is preferably one obtained by polycondensation of an aromatic dicarboxylic acid and an aliphatic glycol. Examples of the aromatic dicarboxylic acid include terephthalic acid and 2,6-naphthalenedicarboxylic acid. Examples of the aliphatic glycol include ethylene glycol, diethylene glycol, and 1,4-cyclohexanedimethanol.
[0018] When the polyester is a copolymer polyester, it may be one obtained by polycondensation of a dicarboxylic acid and a glycol, and examples of the dicarboxylic acid component include one or more of isophthalic acid, phthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, sebacic acid, etc. On the other hand, examples of the glycol component include one or more of ethylene glycol, diethylene glycol, propylene glycol, butanediol, 1,4-cyclohexanedimethanol, neopentyl glycol, etc.
[0019] As the polymerization catalyst for polyester, known catalysts such as antimony compounds, germanium compounds, titanium compounds, aluminum compounds, etc. can be used. Among these, in the present invention, polyesters polymerized using antimony compounds or titanium compounds as catalysts are preferred.
[0020] In addition, an alkaline earth metal compound may be used as the polymerization catalyst, and the alkaline earth metal compound is preferably used in combination with an antimony compound or a titanium compound. The alkaline earth metal compound may be an acetate, oxide, hydroxide, alkoxide, carbonate, etc. of an alkaline earth metal compound, and specifically may be magnesium acetate, magnesium oxide, magnesium hydroxide, magnesium alkoxide, magnesium carbonate, calcium oxide, calcium hydroxide, calcium acetate, calcium carbonate, etc. Among these, calcium compounds are preferred, and calcium acetate is particularly preferred. The alkaline earth metal compound may be a hydrate. When an alkaline earth metal compound is used, a phosphorus compound such as phosphoric acid, polyphosphoric acid, or a phosphoric acid ester may be used in combination.
[0021] Representative examples of polyesters include polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), polybutylene naphthalate (PBN), and polyethylene furanoate (PEF). Among them, PET and PEN are preferred in terms of handling, and PET is the most preferred. Therefore, it is preferred to use PET or PEN as the main component resin, and it is most preferred to use PET as the main component resin. When the main component resin of each layer constituting the base film is, for example, polyethylene terephthalate, the film is called a “polyethylene terephthalate film.” The same applies when the main component resin is another resin.
[0022] (Other resin components) Each layer constituting the base film may be made of a resin other than polyester as the main component resin, such as epoxy, polyarylate, polyethersulfone, polycarbonate, polyetherketone, polysulfone, polyphenylene sulfide, polyester-based liquid crystal polymer, triacetyl cellulose, cellulose derivatives, polypropylene, polyamides, polycycloolefins, etc.
[0023] (particle) The base film may contain particles for the main purposes of imparting lubricity to the film surface and preventing scratches during each process. The type of the particles is not particularly limited as long as they are particles that can provide easy slipping. For example, inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, and titanium oxide, and organic particles such as acrylic resin, styrene resin, urea resin, phenol resin, epoxy resin, and benzoguanamine resin can be mentioned. These can be used alone or in combination of two or more kinds. Furthermore, precipitated particles obtained by precipitating and finely dispersing a part of a metal compound such as a catalyst during the polyester production process can also be used.
[0024] The shape of the particles is not particularly limited, and may be, for example, spherical, blocky, rod-like, flat, or the like. Furthermore, there is no particular limitation on the hardness, specific gravity, color, etc. of the above particles. Two or more kinds of these particles may be used in combination as necessary.
[0025] The average particle size of the particles is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 2.5 μm or less. If it is 5 μm or less, the surface roughness of the substrate film is not too rough, and no problems occur when forming a cured resin layer made of various curing compositions in a later process. On the other hand, the average particle size of the particles is preferably 0.01 μm or more, and even more preferably 0.5 μm or more.
[0026] The content of the particles in the base film is preferably 5% by mass or less, more preferably from 0.0003% to 3% by mass, and even more preferably from 0.01% to 2% by mass. When the average particle size of the particles is within the above range, the surface roughness of the base film is not too rough, and problems that may arise when forming a resin layer made of various curable compositions in a subsequent process can be suppressed.
[0027] When the particles are contained, the particles may be contained at least on the surface of the base film, and the surface of the base film may be adjusted to have the above content. In this case, the base film may be adjusted so that at least one of the surfaces has the above content, but it may be adjusted so that both surfaces have the above content. Therefore, for example, in the case of a multilayer structure, the particle content in at least one of the surface layers constituting the surface of the base film is preferably 5 mass % or less, more preferably 0.0003 mass % or more and 3 mass % or less, and even more preferably 0.01 mass % or more and 2 mass % or less.
[0028] The method of adding particles to the base film is not particularly limited, and any conventionally known method can be used. For example, the particles can be added at any stage of the production of raw material resin such as polyester. When the base film is polyester, it is preferable to add the particles after the completion of esterification or transesterification reaction.
[0029] (Other Ingredients) The substrate film may contain other components as required, such as conventionally known antioxidants, antistatic agents, heat stabilizers, lubricants, dyes, pigments, and ultraviolet absorbing agents. In particular, it is preferred that the laminate film contains an ultraviolet absorbing agent in order to ensure the weather resistance of the film.
[0030] (Thickness of base film) The thickness of the present base film is, for example, preferably 9 μm or more and 125 μm or less, more preferably 12 μm or more and 100 μm or less, and even more preferably 20 μm or more and 75 μm or less, in order to obtain sufficient rigidity and repeated folding properties.
[0031] (Production method) The substrate film can be formed, for example, from a resin composition by a melt casting method or a solution casting method. In the case of a multi-layer structure, it may be co-extruded. In addition, it may be uniaxially or biaxially stretched, and from the viewpoint of rigidity, a biaxially stretched film is preferable.
[0032] In general, first, undried or dried polyester chips are fed into a melt extrusion device by a known method, and heated to a temperature equal to or higher than the melting point of each polymer to melt it. The molten polymer is then extruded from a die and rapidly cooled to a temperature equal to or lower than the glass transition temperature on a rotating cooling drum to obtain a substantially amorphous unoriented sheet. In this case, in order to improve the flatness of the sheet, it is preferable to increase the adhesion between the sheet and the rotating cooling drum, and in the present invention, an electrostatic application adhesion method and / or a liquid application adhesion method are preferably adopted.
[0033] From the viewpoint of film strength, it is preferable to biaxially stretch the sheet obtained as described above to form a film. Specifically, the stretching conditions are as follows: the unstretched sheet is stretched in the longitudinal direction (machine direction) at 70 to 145°C, preferably 80 to 120°C, at a stretch ratio of 2.0 to 4.5 times, preferably 3.0 to 4.0 times, to form a uniaxially stretched film. Next, the film is stretched in the transverse direction (width direction) perpendicular to the longitudinal direction (machine direction) at a stretching ratio of 3.0 to 6.5 times or 3.5 to 6.0 times at 90 to 160° C. to obtain a biaxially stretched film. Subsequently, it is preferable to carry out a heat treatment (heat setting) for 10 to 600 seconds under tension or relaxation of 30% or less at 210 to 260° C. Then, it is preferable to relax the film by 1 to 10% in the longitudinal and / or transverse directions in the maximum temperature zone of the heat treatment and / or in the cooling zone at the exit of the heat treatment. The longitudinal direction (machine direction) of the film refers to the direction in which the film advances during the film manufacturing process, i.e., the direction in which the film roll is wound. The transverse direction (width direction) refers to the direction parallel to the film surface and perpendicular to the longitudinal direction, i.e., the direction parallel to the central axis of the roll when the film is in a roll shape.
[0034] (Characteristics of the base film) The tensile modulus of the base film (JIS K 7161) is preferably 2.0 GPa or more, and the upper limit is preferably 9.0 GPa or less, from the viewpoint of obtaining necessary and sufficient rigidity and repeated bending property, more preferably 3.0 GPa to 8.0 GPa, and even more preferably 3.0 GPa to 7.0 GPa.
[0035] <Resin layer> The laminated film has a resin layer provided on at least one surface of the substrate film. The resin layer contains a binder resin (A) and a chromic compound (B). The resin layer has the above-mentioned composition, and while having appropriate hardness and flexibility, it can have practical excellent repeated bending properties and abrasion resistance. The resin layer is preferably formed from a resin composition. The resin layer is preferably a cured resin layer formed from a curable resin composition. In addition, the curable resin composition is preferably a photocurable resin composition.
[0036] The components for forming the resin layer will be described in detail below. (A) Binder resin The binder resin can be any resin that is generally used together with a chromic material, and examples of the binder resin include polyester resins, polycarbonate resins, acrylic resins, and polyurethane resins. Among these, acrylic resins are preferred from the viewpoint of transparency, etc.
[0037] The mass average molecular weight of the resin composition is preferably 100 or more, more preferably 200 or more, and even more preferably 400 or more. On the other hand, the upper limit is preferably 500,000 or less, more preferably 400,000 or less, and even more preferably 250,000 or less.
[0038] (Acrylic resin) The acrylic resin is a polymer made of polymerizable monomers including acrylic and methacrylic monomers. These may be homopolymers or copolymers, or copolymers with polymerizable monomers other than acrylic and methacrylic monomers. Among the above, a polymer obtained by polymerizing a polymerizable monomer including an acrylic or methacrylic monomer is preferred, and it is more preferred that the polymerizable monomer includes an alkyl (meth)acrylic acid ester. In addition, in order to make it easier to dissolve or disperse the binder resin when the coating liquid is water-based, it is preferred that the polymerizable monomer has a hydrophilic group such as a hydroxyl group or a carboxyl group. Therefore, the acrylic resin is also preferably a polymer obtained by polymerizing a polymerizable monomer including an alkyl (meth)acrylic acid ester and a hydrophilic group-containing monomer such as a hydroxyl group-containing monomer or a carboxyl group-containing monomer. The acrylic resin may also be an emulsion polymer obtained by polymerizing a polymerizable monomer in the presence of a surfactant. The acrylic resin in the present invention is preferably an active energy ray curable type, and the coating film is cured by irradiation with active energy rays, thereby forming a cured coating film on the substrate.
[0039] Examples of the alkyl (meth)acrylic acid esters include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate. In addition, the alkyl (meth)acrylic acid esters may be hydroxyl group-containing alkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. These may be used alone or in combination of two or more. Among these, from the viewpoint of the effect of preventing oligomer precipitation by heat treatment, (meth)acrylic acid is preferable, and acrylic acid is more preferable. That is, the acrylic structure of the (meth)acrylic polymer is preferably a (meth)acrylic acid structure. The (meth)acrylic polymer may have a radically polymerizable double bond.
[0040] In the present invention, when the expression "(meth)acrylic" is used, it means one or both of "acrylic" and "methacrylic". The same applies to "(meth)acrylate" and "(meth)acryloyl". Furthermore, "(poly)propylene glycol" means one or both of "propylene glycol" and "polypropylene glycol". The same applies to "(poly)ethylene glycol". The same applies to other similar terms.
[0041] (Urethane (meth)acrylate) The resin composition preferably contains urethane (meth)acrylate. That is, the acrylic resin may be obtained by polymerizing a polymerizable monomer containing urethane (meth)acrylate. Examples of urethane (meth)acrylate include those obtained by reacting an isocyanate compound with a hydroxyl group-containing (meth)acrylate compound, and those obtained by reacting an isocyanate compound, a polyol compound, and a hydroxyl group-containing (meth)acrylate compound. The urethane (meth)acrylate can be used alone or in combination of two or more kinds. For example, those obtained by reacting an isocyanate compound with a hydroxyl group-containing (meth)acrylate compound, and those obtained by reacting an isocyanate compound, a polyol compound, and a hydroxyl group-containing (meth)acrylate compound may be used in combination.
[0042] Examples of the isocyanate-based compound include polyisocyanate-based compounds such as aromatic polyisocyanates, aliphatic polyisocyanates, and alicyclic polyisocyanates, and among these, diisocyanate compounds are preferred. Examples of the isocyanate-based compound include isocyanate-based compounds having an isocyanurate skeleton obtained by isocyanating a diisocyanate compound.
[0043] Examples of the aromatic polyisocyanate include tolylene diisocyanate, diphenylmethane diisocyanate, polyphenylmethane polyisocyanate, modified diphenylmethane diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, phenylene diisocyanate, and naphthalene diisocyanate.
[0044] Examples of the aliphatic polyisocyanates include hexamethylene diisocyanate, pentamethylene diisocyanate, trimethylhexamethylene diisocyanate, lysine diisocyanate, and lysine triisocyanate.
[0045] Examples of the alicyclic polyisocyanate include hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, and 1,4-bis(isocyanatomethyl)cyclohexane.
[0046] Among these, aliphatic diisocyanates and alicyclic diisocyanates are preferred from the viewpoint of excellent yellowing resistance. Also, isocyanate-based compounds having an isocyanurate skeleton are preferred, and from the same viewpoint, isocyanate-based compounds having an isocyanurate skeleton obtained by isocyanating an aliphatic diisocyanate or an alicyclic diisocyanate are also preferred, and among these, isocyanate-based compounds having an isocyanurate skeleton are more preferred. The isocyanate compounds may be used alone or in combination of two or more kinds.
[0047] The hydroxyl group-containing (meth)acrylate compound is a compound having a hydroxyl group and a (meth)acryloyl group, and examples thereof include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 6-hydroxyhexyl (meth)acrylate, 2-hydroxyethyl acryloyl phosphate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, caprolactone-modified 2-hydroxyethyl (meth)acrylate, dipropylene glycol (meth)acrylate, fatty acid-modified glycidyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and 2-hydroxy-3-(meth)acrylate. Examples of the hydroxyl group-containing (meth)acrylate include monofunctional hydroxyl group-containing (meth)acrylates having one ethylenically unsaturated group such as acryloxypropyl (meth)acrylate; bifunctional hydroxyl group-containing (meth)acrylates having two ethylenically unsaturated groups such as glycerin di(meth)acrylate and 2-hydroxy-3-acryloyl-oxypropyl methacrylate; trifunctional or higher hydroxyl group-containing (meth)acrylates having three or more ethylenically unsaturated groups such as pentaerythritol tri(meth)acrylate, caprolactone-modified pentaerythritol tri(meth)acrylate, ethylene oxide-modified pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, caprolactone-modified dipentaerythritol penta(meth)acrylate, and ethylene oxide-modified dipentaerythritol penta(meth)acrylate. These can be used alone or in combination of two or more. Among these, (meth)acrylate compounds containing three or less ethylenically unsaturated groups are preferred, and polyfunctional (meth)acrylate compounds containing two or more ethylenically unsaturated groups are more preferred, with pentaerythritol tri(meth)acrylate being particularly preferred, because they have excellent reactivity and versatility and are well balanced with the scratch resistance of the cured coating film.
[0048] The polyol compound may be any compound having two or more hydroxyl groups (excluding the above hydroxyl group-containing (meth)acrylates). Examples of the polyol-based compound include aliphatic polyols, alicyclic polyols, polyether-based polyols, polyester-based polyols, polycarbonate-based polyols, polyolefin-based polyols, polybutadiene-based polyols, polyisoprene-based polyols, (meth)acrylic-based polyols, and polysiloxane-based polyols.
[0049] Examples of the aliphatic polyol include ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, trimethylene glycol, dimethylolpropane, neopentyl glycol, 2,2-diethyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,4-tetramethylenediol, 1,3-tetramethylenediol, 2-methyl-1,3-trimethylenediol, 1,5-pentamethylenediol, 1 Examples of such fatty alcohols include aliphatic alcohols containing two hydroxyl groups, such as 1,6-hexamethylenediol, 3-methyl-1,5-pentamethylenediol, 2,4-diethyl-1,5-pentamethylenediol, pentaerythritol diacrylate, 1,9-nonanediol, and 2-methyl-1,8-octanediol; sugar alcohols such as xylitol and sorbitol; and aliphatic alcohols containing three or more hydroxyl groups, such as glycerin, trimethylolpropane, and trimethylolethane.
[0050] Examples of the alicyclic polyol include cyclohexanediols such as 1,4-cyclohexanediol and cyclohexyldimethanol, hydrogenated bisphenols such as hydrogenated bisphenol A, and tricyclodecane dimethanol.
[0051] Examples of polyether polyols include alkylene structure-containing polyether polyols such as polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polybutylene glycol, polypentamethylene glycol, and polyhexamethylene glycol, and random or block copolymers of these polyalkylene glycols.
[0052] Examples of polyester-based polyols include condensation polymers of polyhydric alcohols and polycarboxylic acids, ring-opening polymers of cyclic esters (lactones), and reaction products of three components: polyhydric alcohols, polycarboxylic acids, and cyclic esters.
[0053] Examples of the polyhydric alcohol include ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, trimethylene glycol, 1,4-tetramethylene diol, 1,3-tetramethylene diol, 2-methyl-1,3-trimethylene diol, 1,5-pentamethylene diol, neopentyl glycol, 1,6-hexamethylene diol, 3-methyl-1,5-pentamethylene diol, 2,4-diethyl-1,5-pentamethylene diol, glycerin, trimethylolpropane, trimethylolethane, cyclohexanediols (such as 1,4-cyclohexanediol), bisphenols (such as bisphenol A), and sugar alcohols (such as xylitol and sorbitol).
[0054] Examples of the polyvalent carboxylic acid include aliphatic dicarboxylic acids such as malonic acid, maleic acid, fumaric acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, and dodecanedioic acid; alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid; and aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, orthophthalic acid, 2,6-naphthalenedicarboxylic acid, paraphenylenedicarboxylic acid, and trimellitic acid.
[0055] Examples of the cyclic ester include propiolactone, β-methyl-δ-valerolactone, and ε-caprolactone.
[0056] Examples of the polycarbonate-based polyol include a reaction product of a polyhydric alcohol with phosgene, and a ring-opening polymer of a cyclic carbonate (such as an alkylene carbonate).
[0057] Examples of the polyhydric alcohol used in the polycarbonate-based polyol include the polyhydric alcohols exemplified in the description of the polyester-based polyol, and examples of the alkylene carbonate include ethylene carbonate, trimethylene carbonate, tetramethylene carbonate, and hexamethylene carbonate.
[0058] The polycarbonate-based polyol may be any compound having a carbonate bond in the molecule and a hydroxyl group at the end, and may have an ester bond in addition to the carbonate bond.
[0059] The polyolefin polyols include those having a homopolymer or copolymer of ethylene, propylene, butene, or the like as a saturated hydrocarbon skeleton and having hydroxyl groups at the molecular terminals.
[0060] The polybutadiene-based polyols include those having a butadiene copolymer as a hydrocarbon skeleton and having hydroxyl groups at the molecular terminals. The polybutadiene-based polyol may be a hydrogenated polybutadiene polyol in which all or a part of the ethylenically unsaturated groups contained in the structure thereof have been hydrogenated.
[0061] The polyisoprene-based polyols include those having an isoprene copolymer as a hydrocarbon backbone and having hydroxyl groups at the molecular terminals. The polyisoprene-based polyol may be a hydrogenated polyisoprene polyol in which all or a part of the ethylenically unsaturated groups contained in the structure have been hydrogenated.
[0062] The (meth)acrylic polyols include those having at least two hydroxyl groups in the molecule of a (meth)acrylic acid ester polymer or copolymer, and examples of the (meth)acrylic acid ester include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, and octadecyl (meth)acrylate. More specifically, the (meth)acrylic polyol may be a copolymer of a (meth)acrylic acid ester and a hydroxyalkyl (meth)acrylate such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, or hydroxybutyl (meth)acrylate. Incidentally, the (meth)acrylic polyol excludes the above-mentioned hydroxyl group-containing (meth)acrylate compounds, which are compounds having a hydroxyl group and a (meth)acryloyl group.
[0063] Examples of the polysiloxane polyol include dimethylpolysiloxane polyol and methylphenylpolysiloxane polyol.
[0064] The above polyol compounds can be used alone or in combination of two or more.
[0065] In the reaction between the isocyanate compound and the hydroxyl group-containing (meth)acrylate compound, or the reaction between the isocyanate compound, the hydroxyl group-containing (meth)acrylate compound, and the polyol, the reaction is terminated when the residual isocyanate group content in the reaction system becomes 0.5 mass% or less, thereby obtaining a urethane (meth)acrylate. These reactions are typically addition reactions.
[0066] When the urethane (meth)acrylate includes one obtained by reacting an isocyanate compound, a polyol compound, and a hydroxyl group-containing (meth)acrylate compound, it is preferable to obtain the urethane (meth)acrylate by reacting a reaction product having an isocyanate group obtained by reacting an isocyanate compound with a polyol compound, or a mixture of the reaction product and an isocyanate compound, with a hydroxyl group-containing (meth)acrylate compound. The urethane (meth)acrylate obtained by such a reaction may be a mixture of one obtained by reacting an isocyanate-based compound with a hydroxyl group-containing (meth)acrylate-based compound and one obtained by reacting an isocyanate-based compound, a polyol-based compound, and a hydroxyl group-containing (meth)acrylate-based compound.
[0067] In the reaction between an isocyanate compound and a hydroxyl group-containing (meth)acrylate compound, it is also preferable to use a catalyst for the purpose of promoting the reaction. Examples of such catalysts include organometallic compounds such as dibutyltin dilaurate, dibutyltin diacetate, trimethyltin hydroxide, tetra-n-butyltin, zinc bisacetylacetonate, zirconium tris(acetylacetonate)ethylacetoacetate, and zirconium tetraacetylacetonate; metal salts such as tin octenate, zinc hexanoate, zinc octenate, zinc stearate, zirconium 2-ethylhexanoate, cobalt naphthenate, stannous chloride, stannous chloride, and potassium acetate; triethylamine, triethylenediamine, benzyldiethylamine, 1,4-diazabicyclo[2,2,2]octane, and 1,8-diazabicyclo[5,4,0]un. Decene, N,N,N',N'-tetramethyl-1,3-butanediamine, N-methylmorpholine, N-ethylmorpholine, and other amine catalysts, bismuth nitrate, bismuth bromide, bismuth iodide, bismuth sulfide, and other organic bismuth compounds such as dibutyl bismuth dilaurate and dioctyl bismuth dilaurate, and organic acid bismuth salts such as bismuth 2-ethylhexanoate, bismuth naphthenate, bismuth isodecanoate, bismuth neodecanoate, bismuth laurate, bismuth maleate, bismuth stearate, bismuth oleate, bismuth linoleate, bismuth acetate, bismuth bisneodecanoate, bismuth disalicylate, and bismuth digallate, and among these, dibutyltin dilaurate and 1,8-diazabicyclo[5,4,0]undecene are preferred. These can be used alone or in combination of two or more.
[0068] In the reaction between an isocyanate compound and a hydroxyl group-containing (meth)acrylate compound, an organic solvent having no functional group reactive with an isocyanate group, for example, an ester such as ethyl acetate or butyl acetate, a ketone such as methyl ethyl ketone or methyl isobutyl ketone, an aromatic such as toluene or xylene, etc., can be used. A polymerization inhibitor or the like may also be used as appropriate.
[0069] In addition, the urethane (meth)acrylate is a reaction product of a hydroxyl group-containing (meth)acrylate compound and an isocyanate compound, or a hydroxyl group-containing (meth)acrylate compound, an isocyanate compound, and a polyol compound, but may be produced by reacting a mixture of a hydroxyl group-containing (meth)acrylate and a hydroxyl group-free (meth)acrylate with an isocyanate compound. Alternatively, it may be produced by reacting a mixture of a hydroxyl group-containing (meth)acrylate and a hydroxyl group-free (meth)acrylate with an isocyanate compound and a polyol compound. In this case, the hydroxyl group-free (meth)acrylate remains as an unreacted substance (a (meth)acrylate other than the urethane (meth)acrylate described later), but it is preferable to use it as it is by including it in the curable resin composition. In the reaction between the isocyanate compound and the hydroxyl group-containing (meth)acrylate compound described above, a part or all of the isocyanate compound may be a reaction product of the isocyanate compound and a polyol compound, as described above.
[0070] The mass average molecular weight of the urethane (meth)acrylate is, for example, 3,000 to 100,000, preferably 5,000 to 70,000, and more preferably 8,000 to 30,000. By forming a cured resin layer satisfying the above range in a laminate structure such as a laminate film, good film flatness can be ensured. When two or more types of urethane (meth)acrylate are contained in the resin composition, it is preferable that the weight average molecular weight of the entire urethane (meth)acrylate contained in the resin composition is within the above range. In addition, the resin composition may contain a (meth)acrylate other than the urethane (meth)acrylate. In that case, it is preferable that the weight average molecular weight of the entire (meth)acrylate including the urethane (meth)acrylate and the (meth)acrylate other than the urethane (meth)acrylate is within the above range.
[0071] The (meth)acryloyl group equivalent of the urethane (meth)acrylate is, for example, 120 g / eq or more and 250 g / eq or less, preferably 135 g / eq or more and 220 g / eq or less, more preferably 150 g / eq or more and 200 g / eq or less. When the (meth)acryloyl group equivalent of the urethane (meth)acrylate is within the above range, it is possible to form a cured resin layer having a suitable crosslinking density by adjusting the crosslinking points, and high hardness can be imparted by forming the cured resin layer in a laminate structure such as a laminate film. When two or more kinds of urethane (meth)acrylates are contained in the resin composition, it is preferable that the (meth)acryloyl group equivalent of the entire urethane (meth)acrylate contained in the resin composition is within the above range. In addition, the resin composition may contain a (meth)acrylate other than the urethane (meth)acrylate. In that case, it is preferable that the (meth)acryloyl group equivalent of the entire (meth)acrylate including the urethane (meth)acrylate and the (meth)acrylate other than the urethane (meth)acrylate is within the above range.
[0072] The ratio of the urethane (meth)acrylate in the resin composition is 50% by mass or more, preferably 60% by mass or more, based on the total solid content. The upper limit is not particularly limited, but is, for example, 99% by mass, preferably 95% by mass, and more preferably 85% by mass.
[0073] In the present invention, it is preferable to prepare a base polymer by polymerizing the above urethane (meth)acrylate alone or in combination of two or more kinds. The base polymer is preferably formed by dissolving or dispersing in a solvent or the like described below.
[0074] (solvent) The resin composition may be diluted with a solvent to form a coating liquid. The resin composition may be dissolved in a solvent to form a liquid coating liquid, or may be dispersed in the solvent. The solvent is preferably an organic solvent.Specific examples of the organic solvent include aromatic solvents such as toluene and xylene; ketone solvents such as methyl ethyl ketone (MEK), acetone, methyl isobutyl ketone (MIBK), cyclohexanone, and diisobutyl ketone; ether solvents such as diethyl ether, isopropyl ether, tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether (PGM), anisole, and phenetole; ester solvents such as ethyl acetate, butyl acetate, isopropyl acetate, and ethylene glycol diacetate; amide solvents such as dimethylformamide, diethylformamide, dimethylacetamide, and N-methylpyrrolidone; cellosolve solvents such as methyl cellosolve, ethyl cellosolve, and butyl cellosolve; alcohol solvents such as methanol, ethanol, propanol, isopropanol, and butanol; and halogen solvents such as dichloromethane and chloroform. These organic solvents may be used alone or in combination of two or more. Among these organic solvents, ester solvents, ether solvents, alcohol solvents and ketone solvents are preferably used.
[0075] The amount of the organic solvent used is not particularly limited, and is appropriately determined in consideration of the coatability of the prepared resin composition, the viscosity and surface tension of the liquid, the compatibility of the solid content, etc. The resin composition is prepared as a coating liquid having a solid content concentration of preferably 15 to 80 mass%, more preferably 20 to 70 mass%, using the above-mentioned solvent. Note that the "solid content" in the resin composition means the components excluding the solvent, which is a volatile component, and includes not only solid components but also semi-solid and viscous liquid substances.
[0076] (Other ingredients) The resin composition may contain, in addition to the above urethane (meth)acrylate, a photopolymerizable compound such as a (meth)acrylate other than the urethane (meth)acrylate. Examples of (meth)acrylates other than urethane (meth)acrylates include (meth)acrylates that do not have a hydroxyl group. Examples of (meth)acrylates that do not have a hydroxyl group include 1,2-di(meth)acryloxyethane, 1,2-di(meth)acryloxypropane, 1,3-di(meth)acryloxypropane, 1,4-di(meth)acryloxybutane, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)arylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ethoxylated tri(meth)acrylate, ethylene glycol di(meth)arylate ... Examples of the polyfunctional (meth)acrylates include polyfunctional (meth)acrylates having two or more (meth)acryloyl groups, such as trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, tris-2-hydroxyethyl isocyanurate tri(meth)acrylate, glycerin tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. These may be used alone or in combination of two or more.
[0077] In addition, various additives may be appropriately blended into the resin composition as necessary within the scope of the present invention. Examples of additives that may be used in combination include photoinitiators, light stabilizers, antioxidants, antistatic agents, flame retardants, leveling agents, dispersants, thixotropy-imparting agents (thickeners), and defoamers. Here, examples of the leveling agent include fluorine-based leveling agents, silicone-based leveling agents, and acrylic-based leveling agents. Among them, the surface of the resin layer can be given a function of repelling water and oil, and a function of preventing adhesion of dirt such as fingerprints. In this case, the leveling agent is preferably a fluorine-based leveling agent.
[0078] (Photoinitiator) When the resin composition is a photocurable resin composition, it is preferable to contain a photoinitiator in order to improve the curability. The photoinitiator is a photopolymerization initiator, and a known one can be used. Examples of the photopolymerization initiator include a photoradical generator and a photoacid generator.
[0079] Among the photopolymerization initiators that can be used in the resin composition, examples of the photoradical generator include benzoin and its alkyl ethers, such as benzoin, benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl ether; acetophenone, 2,2-dimethoxy-2-phenylacetophenone [e.g., trade name "Omnirad (registered trademark) 651", manufactured by IGM RESINS], 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone [e.g., trade name "Omnirad (registered trademark) 184", manufactured by IGM RESINS], 2-hydroxy-2-methyl-1-phenylpropan-1-one [e.g., trade name "Omnirad (registered trademark) 1173", manufactured by IGM RESINS], and the like. IGM RESINS], 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one [e.g., trade name "Omnirad® 127, IGM RESINS], 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one [e.g., trade name "Omnirad® 2959", IGM RESINS], 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one [e.g., trade name "Omnirad® 907", IGM alkylphenones such as 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone; phosphine oxides such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide [for example, trade name "Omnirad (registered trademark) TPO", manufactured by IGM RESINS] and bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide [for example, trade name "Omnirad (registered trademark) 819", manufactured by IGM RESINS]; anthraquinones such as 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, and 2-amylanthraquinone; benzophenone and various derivatives thereof; and formic acid derivatives such as methyl benzoylformate and ethyl benzoylformate.These may be used alone or in combination of two or more.
[0080] Among these photoradical generators, from the viewpoint of the light resistance of the cured product, preferred are alkylphenones, phosphine oxides, and formic acid derivatives, more preferred are 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, and methyl benzoylformate, and particularly preferred are 1-hydroxycyclohexyl phenyl ketone and 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one.
[0081] As the photoacid generator, known ones can be used, among which diaryliodonium salts and triarylsulfonium salts are preferred from the viewpoints of curability, acid generation efficiency, etc. Specific examples include anion salts of di(alkyl-substituted)phenyliodonium (specifically, PF 6 Salt, SbF 5 salts, tetrakis(perfluorophenyl)borate salts, etc. A specific example of an anion salt of (alkyl-substituted) phenyliodonium is dialkylphenyliodonium PF 6 The salt (trade name "Omniad (registered trademark) 250" manufactured by IGM RESINS) is particularly preferred. These photoacid generators may be used alone or in combination of two or more.
[0082] The content of the photoinitiator is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and particularly preferably 1 part by mass or more, based on 100 parts by mass of the total of the compounds having a (meth)acryloyl group in the resin composition, from the viewpoint of improving the curability. On the other hand, from the viewpoint of maintaining the stability of the coating solution when the resin composition is made into a solution and from the viewpoint of the flatness of the cured coating film, the content is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and particularly preferably 5 parts by mass or less.
[0083] (Viscosity of Resin Composition) In order to ensure good coatability, the resin composition for forming the resin layer preferably has a viscosity at 25°C measured with an E-type viscometer of 10 to 60 mPa·s, and more preferably 30 mPa·s or less, more preferably 20 mPa·s or less, more preferably 15 mPa·s or less, and even more preferably 12 mPa·s or less.
[0084] (B) Chromic Compound A chromic compound is a compound whose optical properties (e.g., transmittance, color, hue, fluorescence intensity, refractive index, reflectance) change reversibly or irreversibly in response to an external stimulus, such as temperature, light, water, pH, pressure, or electricity.
[0085] As the chromic compound, for example, a thermochromic compound, a photochromic compound, a hydrochromic compound, a pH-responsive compound (for example, a halochromic compound or an acidichromic compound), a piezochromic compound, and an electrochromic compound can be used. The chromic compound may be used alone or in combination of two or more kinds. Among these, the chromic compound is preferably at least one of a photochromic compound and a thermochromic compound.
[0086] The content of the chromic compound in the resin layer (i.e., relative to the solid content of the resin composition) is usually 0.1 to 5.0 mass %, preferably 0.5 to 3.5 mass %, from the viewpoint of changing the color to the desired color without impairing the performance of the resin layer.
[0087] (Thermochromic compounds) Thermochromic compounds generally change color in the range of −5° C. to 65° C. In the present invention, one type of thermochromic compound may be used, or two or more types of thermochromic compounds having different color change temperatures and color tones may be used in combination.
[0088] As each compound, various known compounds can be used. For example, examples of thermochromic compounds and microcapsules encapsulating thermochromic compounds and color developers described below include "TC Color" (reversible) from Sakura Cray-Pas Corporation, "Chromicolor" (reversible) from Matsui Pigment Chemical Industry Co., Ltd., and "Thermolock" (semi-irreversible) from Matsui Pigment Chemical Industry Co., Ltd. Examples of photochromic compounds include Matsui Pigment Chemical Industry's "Photopia Color" (reversible), Matsui Pigment Chemical Industry's "Photolock" (irreversible), and Recording Materials Research Institute's "Thermo Color" (reversible). These are just a few examples, and various chromic compounds such as irreversible type, heat accumulation type, quasi-reversible type, and reversible type can be selected according to the purpose. For example, in thermochromic compounds, examples of irreversible types include inorganic compounds using metal salts and organic compounds using a thermal recording method. Examples of reversible types include inorganic compounds using metal complex salts, organic compounds using condensed aromatic ring-substituted ethylene derivatives, organic compounds using liquid crystals (e.g., cholesteric liquid crystals), and organic compounds using Metamocolor (registered trademark).
[0089] As an example of a thermochromic compound, a leuco dye will be described. Leuco dyes are dyes that irreversibly change their chemical structure through an oxidation-reduction reaction with a developer to develop a color, and are themselves colorless or light-colored dye precursors. Leuco dyes can be classified into two types: those that act as electron donors and those that act as electron acceptors and react with the developer. Either type is acceptable, but those that act as electron donors and react are preferred. Examples of leuco dyes include triphenylmethanephthalide-based leuco compounds, triarylmethane-based leuco compounds, fluoran-based leuco compounds, phenothidian-based leuco compounds, thiofluoran-based leuco compounds, xanthene-based leuco compounds, indophthalyl-based leuco compounds, spiropyran-based leuco compounds, azaphthalide-based leuco compounds, chromenopyrazole-based leuco compounds, methine-based leuco compounds, rhodamine anilinolactam-based leuco compounds, rhodamine lactam-based leuco compounds, quinazoline-based leuco compounds, diazaxanthene-based leuco compounds, and bislactone-based leuco compounds. Among these, triphenylmethanephthalide-based leuco compounds, fluoran-based leuco compounds, or azaphthalide-based leuco compounds are preferred from the viewpoint of color development. The leuco dye may be one type, or two or more types may be used in combination.
[0090] The thermochromic compound is preferably a compound represented by the following general formula (I): The compound represented by the following general formula (I) is typically a leuco compound, and is preferably a fluoran-based leuco compound. [ka]
[0091] In formula (I), X is a carbon atom or a nitrogen atom, and R 1 , R 2 R represents a substituted or unsubstituted aromatic group or a group having a substituted or unsubstituted heterocycle. 1 and R 2 may form part of the fluoran skeleton. 3represents a hydrogen atom, a halogen atom, a substituted or unsubstituted acyl group, an alkyl group, an alkoxy group, a nitro group, an aryl group, or an amino group. 3 is preferably a hydrogen atom. Also, if X is nitrogen, R 1 and R 2 is preferably an aromatic group which may have a substituent, and when X is carbon, R 1 and R 2 Each of R is preferably a group having a substituted or unsubstituted heterocycle. 1 and R 2 may be the same or different from each other, but considering ease of production, R 1 and R 2 are preferably the same. Also, if X is carbon, R 1 and R 2 Preferably, R forms part of the fluoran skeleton. 1 and R 2 When forms part of the fluoran skeleton, R 1 and an aromatic group of R 2 The aromatic group may be bonded via *-O-*, where * is the bonding site to the aromatic ring constituting the aromatic group. For example, the following are examples of thermochromic compounds:
[0092] [Table 1]
[0093] (Temperature regulator) The temperature regulator is a substance having a melting point, and is solid at temperatures lower than the melting point, but melts and becomes liquid when the temperature rises to the melting point. The melted temperature regulator functions as a solvent for the leuco dye, and the leuco dye moves to the surface of the developer and develops color. Examples of such substances include aliphatic alcohols and fatty acid alkyl esters.
[0094] Examples of the aliphatic alcohol include methyl alcohol, ethyl alcohol, 1-propyl alcohol, 1-butyl alcohol, 1-pentyl alcohol, and 1-hexyl alcohol. Examples of fatty acid alkyl esters include methyl formate, ethyl formate, isopropyl formate, isopropyl formate, methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, isopropyl propionate, isopropyl butyrate, isopropyl valerate, isopropyl caprylate, methyl laurate, ethyl laurate, and propyl laurate.
[0095] (Developer) The color developer is preferably an inorganic compound, and specific examples of the color developer include silica, alumina, and zeolite. The amount of developer to be used should be the amount necessary to react with the leuco dye to produce color, and is preferably 10 to 100 parts by weight, more preferably 30 to 200 parts by weight, and even more preferably 50 to 150 parts by weight, per part by weight of the leuco dye.
[0096] (Microcapsules) In the present invention, from the viewpoint of preventing the deterioration of the chromic compound due to the irradiation of active energy rays, the chromic compound (B) may be contained in the microcapsule, and preferably the chromic compound (B) and the color developer may be contained in the microcapsule. It is more preferable to encapsulate the chromic compound, the temperature regulator, and the color developer and microencapsulate them. Conventionally known methods can be used for microencapsulation. Examples of the thermosetting resin that forms the coating of the microcapsules include melamine resin, benzoguanamine resin, cycloguanamine resin, urea resin, thermosetting acrylic resin, polyurethane resin, polyester resin, and epoxy resin.
[0097] The content of the microcapsules in the resin layer (i.e., relative to the solid content of the resin composition) is, from the viewpoint of changing the color to the desired color without impairing the performance of the resin layer, for example, 0.5 to 20 mass %, preferably 1 to 15 mass %, and more preferably 3 to 12 mass %.
[0098] (Coloring agent) The resin composition of the present invention may contain a colorant. The colorant may be a pigment or a dye. By containing a colorant, it becomes easier to increase the color tone change amount (ΔX) described later. As the colorant, various color pigments such as red pigments, blue pigments, green pigments, yellow pigments, purple pigments, orange pigments, and brown pigments, and various color dyes such as red dyes, blue dyes, green dyes, yellow dyes, purple dyes, orange dyes, and brown dyes can be used. For example, as the red colorant, Sudan Red-based colorants such as Sudan I, Sudan II, Sudan III, Sudan IV, Sudan Red 7B, and Sudan Red G can be mentioned. The content of the colorant in the resin layer (that is, relative to the solid content of the resin composition) is not particularly limited, but is, for example, 0.001 to 1 mass %, preferably 0.01 to 0.4 mass %, and more preferably 0.2 to 0.2 mass %.
[0099] (Photochromic Compound) Specific examples of photochromic compounds include naphthopyran, chromene, spiropyran, spirooxazine and thiospiropyran, benzopyran, stilbene, azobenzene, thioindigo, bisimidazole, spirodihydroindolizine, quinine, perimidine spirocyclohexadienone, viologen, fulgide, fulgimide, diarylethene, hydrazine, aniline, aryl disulfide, arylthiosulfonate, spiroperimidine, triarylmethane, and derivatives of these compounds. The photochromic compound may also be in the form of a capsule in which these compounds or derivatives are conjugated. The photochromic compound may be used alone or in combination of two or more types.
[0100] (Thickness of resin layer) The thickness of the resin layer is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less. When the thickness of the resin layer is equal to or less than the above upper limit, curling and heat wrinkles can be prevented in a laminate structure having a resin layer such as a laminate film, and good flatness can be ensured. On the other hand, there is no particular lower limit to the thickness of the resin layer, but it is preferably 1.0 μm or more in terms of adequately protecting the base film. The thickness of the resin layer is preferably 0.05 to 0.8 relative to the thickness of the substrate, more preferably 0.1 to 0.5, and even more preferably 0.15 to 0.4.
[0101] <Surface condition of resin layer> The surface of the resin layer may be uneven or flat, but is preferably flat from the viewpoint of appearance (surface gloss). On the other hand, it is preferable that the surface is uneven from the viewpoint of imparting antiglare properties. It can be arbitrarily selected according to the required properties.
[0102] [Functional Layer] The laminated film may have a functional layer between the base film and the resin layer or on the resin layer. Hereinafter, the functional layer between the base film and the resin layer may be referred to as functional layer A, and the functional layer provided on the resin layer may be referred to as functional layer B.
[0103] [Release layer] The laminated film may include a release layer between the base film and the resin layer. The release layer may be formed on the base film by a known coating method.
[0104] [Print layer] The laminated film may have a printed layer between the base film and the resin layer. The printed layer may be formed by printing on the base film with toner, ink, or the like by a known printing method. The printed layer may be formed by solid printing, or may be partially printed on the base film to form characters, designs, patterns, or the like. The printed layer is formed and combined with the color change of the resin layer to improve the design.
[0105] [Hard coat layer] The laminated film may have a hard coat layer on the resin layer. The hard coat layer may be formed on the resin layer by a known coating method.
[0106] <<Laminated film manufacturing method>> The resin layer can be formed by curing a resin composition, for example, by applying a curable resin composition having a mass average molecular weight in the range of 1,000 to 500,000 onto a substrate film and curing the composition. More specifically, the present laminated film can be produced by applying a resin composition to at least one surface of a substrate film and curing the composition to form a resin layer. In addition, when the laminated film has a printed layer, it is preferable to form a printed layer on one surface of the substrate film by printing or the like, and then apply a curable resin composition for forming a resin layer onto the substrate film and cure the composition. However, the method for producing the laminated film is not limited to the above method.
[0107] <Method of forming resin layer> As described above, the resin layer can be obtained by applying a resin composition to the surface of a substrate film, drying the composition to form a coating layer, and curing the coating layer. Examples of a method for applying the resin composition include air doctor coating, blade coating, rod coating, bar coating, knife coating, squeeze coating, impregnation coating, reverse roll coating, transfer roll coating, gravure coating, kiss roll coating, cast coating, spray coating, curtain coating, calendar coating, and extrusion coating. The drying conditions are not particularly limited, and the drying may be performed at about room temperature or by heating, for example, at about 25 to 120° C., preferably 50 to 100° C., and more preferably 60 to 90° C. The drying time is not particularly limited as long as the solvent can be sufficiently evaporated, and is, for example, about 10 seconds to 30 minutes, and preferably about 15 seconds to 10 minutes.
[0108] The method for curing the resin composition may be appropriately selected depending on the curing mechanism of the resin composition, and if the resin composition is a thermosetting resin composition, it may be cured by heating, and if it is a photocurable resin composition, it may be cured by irradiating it with energy rays. In the laminated film of the present invention, active energy rays that can be used when curing the photocurable resin composition include ultraviolet rays, electron beams, X-rays, infrared rays, and visible light. Among these active energy rays, ultraviolet rays and electron beams are preferred from the viewpoints of curability and prevention of resin deterioration.
[0109] The resin composition is preferably cured by irradiation with energy rays from the viewpoints of molding time and productivity, and of preventing thermal shrinkage and thermal deterioration of each member due to heating, etc. The energy rays may be irradiated from either side, and may be irradiated from the substrate film side or the opposite side of the substrate film. When the resin composition is cured by ultraviolet irradiation in producing the laminated film of the present invention, various ultraviolet irradiation devices can be used, and as the light source, a xenon lamp, a high-pressure mercury lamp, a metal halide lamp, an LED-UV lamp, etc. can be used. The amount of ultraviolet irradiation (unit: mJ / cm 2 ) is usually 50 to 3,000 mJ / cm 2 From the viewpoints of the curability of the curable resin composition, the flexibility of the cured product (cured film), etc., it is preferably 100 to 1,000 mJ / cm 2 From the viewpoint of the flatness of the laminated film, it is more preferably 100 to 500 mJ / cm 2 and is appropriately determined depending on the reaction rate of the (meth)acryloyl group required in each curing step. When the resin composition is used in a particularly severe environment, it is preferable to increase the amount of ultraviolet light to adjust the surface hardness of the cured product of the resin composition.
[0110] In addition, when the resin composition is cured by electron beam irradiation during the production of the laminated film of the present invention, various electron beam irradiation devices can be used. The irradiation dose (Mrad) of the electron beam is usually 0.5 to 20 Mrad, and is preferably in the range of 1 to 15 Mrad from the viewpoints of the curability of the resin composition, the flexibility of the cured product, and prevention of damage to the substrate, but is appropriately determined depending on the reaction rate of the (meth)acryloyl group required in each curing step.
[0111] <<Physical properties of laminated film>> (Discoloration) In the present invention, it is necessary that the color tone change (ΔX) of the surface of the resin layer, calculated by the following formula (1), is 5.7 or more. ΔX=((ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2 ) 1 / 2 (1) ΔL * :L before and after external stimulation * Amount of change in value Δa * : a before and after external stimulation * Amount of change in value Δb * :b before and after external stimulation * Amount of change in value If ΔX is less than 5.7, the color tone cannot be changed sufficiently by external stimuli. ΔX is preferably 6.0 or more, more preferably 6.5 or more. The upper limit of ΔX is not particularly limited, but may be, for example, 197 or less, 150 or less, 100 or less, or 50 or less. In addition, ΔX is the L before and after applying an external stimulus using a color difference meter in a transmission method. * , a * , b * and calculate it according to the above formula (1).
[0112] As mentioned above, external stimuli are stimuli such as temperature, light, water, pH, pressure, and electricity.* , a * , b * The external stimulus during measurement is an external stimulus that changes the optical properties of the chromic compound contained in the resin layer, for example, if it is a thermochromic compound, the temperature may be changed, and if it is a photochromic compound, light may be irradiated. The level and type of the external stimulus are not particularly limited, but if any external stimulus is applied so that the chromic compound changes, and ΔX becomes equal to or greater than the lower limit, ΔX is deemed to satisfy the above-mentioned requirement. For example, when the external stimulus is temperature, ΔX can be obtained when the temperature of the laminated film is changed from a first temperature to a second temperature. In this case, the first temperature and the second temperature can be set so that ΔX is maximized. For example, the first temperature is set to room temperature (25° C.), and the second temperature is raised or lowered from the room temperature, and L * , a * , b * As an example, the first temperature may be set to room temperature (25°C) and the second temperature may be set to 35°C.
[0113] In addition, each component (i.e., a before or after external stimulation) * Value, b * Value, L * When we focus on the value of L * The value is preferably 0 to 100. * The value is 0 * ≦60 is preferable. * The value is 0≦b * < 60 is preferred. By satisfying this range, for example, when a composition of a resin layer containing a chromic compound / printed layer / substrate film is applied to the decoration of an automobile part, when the color changes from one tone (tone 1) to another tone (tone 2), when the interior part (such as the instrument panel) is viewed from the outside, the color change provides not only a decorative function but also an indication function, for example, that the temperature inside the vehicle is rising. Also, when used in the housing of a smartphone, the heat generation state of the device can be visually confirmed. In another embodiment, when the hard coat layer / chromic compound-containing resin layer / substrate film configuration is applied to the sunroof of an automobile part, the color tone changes from one tone (tone 1) to another tone (tone 2) during the day as the amount of sunlight from outside increases, and the color tone changes to provide light blocking properties. Then, in the evening, the color tone can be restored to the original tone as the amount of sunlight from outside decreases. This is an example of the application of reversible color tone changes due to changes in the amount of ultraviolet light irradiation. Since it can be replaced like conventional automobile window films, it can be easily installed.
[0114] (Pencil hardness) In accordance with JIS K5600-5-4, the pencil hardness of the resin layer is H or more, preferably 2H or more.
[0115] (Repeated bending ability) The laminated film having the above-mentioned structure has a resin layer on the surface of the base film, and the structure of the resin layer is designed within a specific range, thereby further improving the practical repeated bending property. Specifically, the laminated film has enough durability to not crack even when folded more than 200,000 times in a repeated bending property evaluation (outward bending, R=1.5).
[0116] The present laminated film has a light transmittance of, for example, 40 to 97%, preferably 50 to 95%, and more preferably 55 to 90%. When the light transmittance is within the above range, a certain level of transparency can be ensured, and the film can be easily used suitably for decorative purposes. The light transmittance referred to here is preferably the higher value measured at wavelengths of 500 nm and 600 nm.
[0117] <<Characteristics and uses of laminated film>> This laminated film is capable of achieving both a high level of surface hardness and repeated bending resistance (flexural durability, outward bending, the ability to bend 200,000 times under conditions of R=2.0). It is presumed that this is because adjusting the composition of the resin layer makes it possible to reduce the stress transmission into the resin layer when the laminated film is bent. Furthermore, by containing a chromic compound, a desired color change can be achieved by a predetermined external stimulus. For example, by containing a thermochromic compound, a desired color change can be achieved in a predetermined temperature range.
[0118] Furthermore, by using such a resin layer, it is not necessary to extremely increase the tensile modulus of elasticity of the substrate film used. In the past, when designing a laminate film having a surface layer with high surface hardness to achieve the desired surface hardness (pencil hardness of 2H or more), it was necessary to review the structural design of the raw materials that make up the base film used and further increase the tensile modulus, if necessary. In contrast, when the resin layer is configured as described above, it is possible to appropriately select a general-purpose base film available on the market, which has the advantage of increasing the freedom in the selection of the base film.
[0119] This laminated film has excellent abrasion resistance, practical repeated folding properties, and colorfastness, and can be used for molding, decoration, and other applications. For example, it can be suitably used for decorating automobile interiors. However, the applications of this laminated film are not limited to these applications.
[0120] [Laminate 1] The laminate 1 of the present invention includes a laminate film having a base film, a resin layer provided on at least one side of the base film, the resin layer containing a binder resin (A) and a chromic compound (B), and other resin films attached to both sides of the laminate film via adhesive layers. Here, the base film, the resin layer, and the laminate film are as described above.
[0121] (adhesive layer) The adhesive layer in the laminate 1 of the present invention is formed from a pressure-sensitive adhesive, a pressure-sensitive adhesive sheet, an adhesive, etc., but from the viewpoint of excellent adhesiveness, an adhesive is preferably used. As the adhesive, for example, a polyolefin adhesive, an acrylic adhesive, a polyester adhesive, an epoxy adhesive, a polyurethane adhesive, etc. can be used.
[0122] (Other resin films) The other resin film in the laminate 1 of the present invention is not particularly limited and is appropriately determined depending on the application. Specific examples include acrylic resin film, polyester film, polyolefin film, etc. Among these, the other resin film attached to the resin layer side is preferably an acrylic resin film, and among them, a polymethyl methacrylate resin (PMMA resin) film is preferable in terms of conformity to a mold during injection molding. In addition, as the other resin film, an ABS resin (acrylonitrile-butadiene-styrene copolymer resin) film is also preferable in terms of conformity to a mold during injection molding.
[0123] More specifically, an example is a laminate 10 shown in Fig. 1. The laminate 10 is made of PMMA 11, a dry laminate 12, a chromic dye + HC layer (hard coat layer), an easily moldable PET film 14, a dry laminate 15, and a molded member such as ABS (ABS).
[0124] [Laminate 2] The laminate 2 of the present invention includes a laminate film having a base film, a release layer, and a resin layer in this order, the resin layer containing a binder resin (A) and a chromic compound (B), and another resin film having a printed layer or a vapor deposition layer on the resin layer of the laminate film and bonded thereon via an adhesive layer. Here, the base film, the resin layer, the laminate film, and the other resin film are as described above. More specifically, an example of the laminate 20 is shown in Fig. 2. The laminate 20 is made of an easily moldable PET film 21, a release layer 22, a chromic dye + HC layer (hard coat layer) 23, a printed layer and / or a vapor deposition layer 24, a dry laminate 25, and a molded member such as ABS (ABS).
[0125] <<Explanation of terms>> In the present invention, the term "film" includes the term "sheet", and the term "sheet" includes the term "film". In addition, in this specification, when it is written "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". In addition, when it is stated that the amount is "X or more" (X is any number), it also means that the amount is "preferably greater than X" unless otherwise specified, and when it is stated that the amount is "Y or less" (Y is any number), it also means that the amount is "preferably smaller than Y" unless otherwise specified. EXAMPLES
[0126] The present invention will be specifically described below with reference to examples, although the present invention is not limited to the following examples in any way. The measurement and evaluation methods used in the present invention are as follows.
[0127] (1) Resin layer thickness measurement method Each laminated film was attached to a glass slide using "Aron Alpha Series" manufactured by Toa Gosei Co., Ltd., to prepare a sample for SAICS. The obtained sample for SAICS was set in a SAICS (DN-01 type manufactured by Daipla Wintes Co., Ltd.), and a cut of 300 μm wide and 1 μm deep was made in advance with a diamond cutting edge. The cut was made using a single crystal diamond blade with a V-angle dimension of 80°, a rake angle of 5°, and a relief angle of 5°. The measurement was performed by setting a borazon cutting blade with a width of 300 μm on the sample with a 300 μm wide cut in advance, and measuring the film thickness of each cured resin layer at an arbitrary depth, horizontal speed of 1 μm / s, and vertical speed of 0.5 μm / s. A boron nitride blade with a blade width dimension of 0.3 mm, a rake angle of 20°, and a relief angle of 10° was used for the measurement. The compound strength was measured from the vertical displacement position and cutting force, and the thickness of each layer was confirmed.
[0128] (2) Pencil hardness The pencil hardness of the resin layer was measured in accordance with JIS K5600-5-4.
[0129] (3) Flexural durability Using a folding tester (Yuasa System Co., Ltd., DLDMLH-FS), the test was performed with a minimum radius R=1.5 so that the resin layer of the laminated film was the inner surface (referred to as Out-fold in Tables 2 to 4), and the presence or absence of cracks in the resin layer on the inner surface was visually confirmed. The number of times until cracks occurred was taken as the number of repeated foldings, and the results were judged according to the following criteria. In addition, the test was performed with a minimum radius R=2.0 so that the resin layer of the laminated film was the outer surface (referred to as In-fold in Tables 2 to 4), and the presence or absence of cracks in the resin layer on the outer surface was visually confirmed. The number of times until cracks occurred was taken as the number of repeated foldings, and the results were judged according to the following criteria. (Judgment criteria) ◎: Can be repeatedly folded 200,000 times ○: Repeated bending times: over 100,000 to less than 200,000 △: Repeated folding times: over 1,000 to 100,000 ×: Repeated folding times less than 1000
[0130] (4) Color difference change rate (before and after discoloration) Using a color difference meter (SD6000 manufactured by Nippon Denshoku Industries Co., Ltd.), the color difference was measured by the transmission method before and after the application of an external stimulus (in this example and comparative example, when the temperature was raised from room temperature to 35°C), and the amount of change in color tone (ΔX) was calculated using the following formula (1). ΔX=((ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2 ) 1 / 2 (1) ΔL * :L before and after external stimulation * Amount of change in value Δa * : a before and after external stimulation * Amount of change in value Δb * :b before and after external stimulation * Amount of change in value
[0131] (5)Light transmittance Using a spectrophotometer (U-3900H, manufactured by Hitachi High-Technologies Corporation), the light transmittance at room temperature in the wavelength region of 380 nm to 780 nm was measured, and the light transmittance (Δ) at wavelengths of 600 nm and 500 nm was calculated.
[0132] The various compounds used in the examples and comparative examples were prepared as follows.
[0133] <Polyester raw materials> <Polyester (A)> 100 mol% dimethyl terephthalate, 100 mol% ethylene glycol, and 0.07 parts by mass of calcium acetate monohydrate were placed in a reactor, and the mixture was heated to a high temperature while distilling off methanol to carry out an ester exchange reaction. After the reaction started, the temperature was raised to 230°C in about 4.5 hours, and the ester exchange reaction was essentially completed. Next, 0.04 parts by mass of phosphoric acid and 0.035 parts by mass of antimony trioxide were added, and polymerization was carried out according to a conventional method. That is, the reaction temperature was gradually increased to a final temperature of 280°C, while the pressure was gradually reduced to a final temperature of 0.05 mmHg. After 4 hours, the reaction was terminated, and the mixture was chipped according to a conventional method to obtain polyester (A). The resulting intrinsic viscosity was 0.63. <Polyester (B)> Silica particles having an average particle size of 2 μm were added to the polyester (A) to obtain polyester (B) containing 0.2% by mass of silica particles. The intrinsic viscosity was 0.65.
[0134] <Base film> <Base film PET> The mixed raw material obtained by mixing polyesters (A) and (B) at a ratio of 90% by mass and 10% by mass, respectively, was used as the raw material for the outermost layer (surface layer), and only polyester (A) was used as the raw material for the intermediate layer. Each was fed to two extruders, melted at 285°C, and then co-extruded on a cooling roll set at 40°C in a layer configuration of two types and three layers (surface layer / intermediate layer / surface layer = 1 / 8 / 1 discharge amount (mass ratio)), cooled and solidified to obtain an unstretched sheet. Next, the film was stretched 3.4 times in the longitudinal direction at a film temperature of 85°C using the roll peripheral speed difference, then introduced into a tenter, stretched 4.3 times in the transverse direction at 110°C, heat-treated at 235°C, and then relaxed 2% in the transverse direction to obtain a polyester film (base film) with a thickness of 50 μm.
[0135] <Resin composition> <Production Example 1: Mixture (A-1) containing urethane (meth)acrylate> Into a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a nitrogen gas inlet, 29.3 parts by mass of an isocyanurate compound whose main component is a trimer of hexamethylene diisocyanate (product name: Coronate HX, manufactured by Tosoh Corporation, isocyanate group content: 21.0% by mass) and 70.7 parts by mass of a mixture of pentaerythritol triacrylate and pentaerythritol tetraacrylate (hydroxyl value 120 mg KOH / g) (b1-1 / b1-2 = 0.25 / 0. 75 (mol / mol)), 0.06 parts by mass of 2,6-di-tert-butylcresol as a polymerization inhibitor, and 0.02 parts by mass of dibutyltin dilaurate as a reaction catalyst were charged and reacted at 60°C. The reaction was terminated when the residual isocyanate groups reached 0.3% by mass or less, yielding a mixture (A-1) of 70 parts by mass of urethane (meth)acrylate and 30 parts by mass of pentaerythritol tetraacrylate (acryloyl group equivalent 134 g / eq, weight average molecular weight 10,000).
[0136] <Production Example 2: Urethane (meth)acrylate (A-2)> A four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a nitrogen gas inlet was charged with 37.7 parts by mass of isophorone diisocyanate, 24.5 parts by mass of polytetramethylene glycol (hydroxyl value 175 mg KOH / g; molecular weight calculated from the hydroxyl value 641), 14.1 parts by mass of polyester triol (hydroxyl value 250 mg KOH / g; molecular weight calculated from the hydroxyl value 673), and 0.02 parts by mass of dibutyltin dilaurate as a reaction catalyst, and the mixture was reacted at 80°C. When the residual isocyanate groups reached 11% or less, 23.7 parts by mass of 2-hydroxyethyl acrylate and 0.04 parts by mass of methoxyphenol as a polymerization inhibitor were further charged and reacted at 60°C. When the residual isocyanate groups reached 0.3% by mass or less, the reaction was terminated to obtain urethane (meth)acrylate (A-2) (acryloyl group equivalent: 493 g / eq; weight average molecular weight: 3,400).
[0137] <Acrylate (A)> 90 parts by mass of mixture (A-1) and 10 parts by mass of urethane (meth)acrylate (A-2) were charged into a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a nitrogen gas inlet, and the mixture was stirred at 60°C until homogenous, obtaining acrylate (A). The (meth)acryloyl group equivalent of the entire acrylate (A) was 145 g / eq.
[0138] (Resin composition 1) Resin composition 1 was prepared by adding 10 parts by mass of (Y) Thermochromic ("Thermocolor" manufactured by Recording Materials General Research Institute, 35°C, blue color), 0.06 parts by mass of (Y2) Sudan III (red pigment), 5 parts by mass of a photopolymerization initiator (Omnirad127 manufactured by IGM Resins BV), and 233 parts by mass of methyl ethyl ketone to 90 parts by mass of acrylate (A).
[0139] (Resin composition 2) Acrylate (B); bifunctional: Viscoat #230, manufactured by Osaka Organic Chemical Industry Co., Ltd. Acrylate (C); Trifunctional: TMPTA, trimethylolpropane triacrylate Resin composition 2 was prepared by adding 10 parts by mass of (Y) photochromic (CAS No. 1498-89-1), 5 parts by mass of photopolymerization initiator (Omnirad 127 manufactured by IGM Resins BV), and 233 parts by mass of methyl ethyl ketone to 45 parts by mass of acrylate (B) and 45 parts by mass of acrylate (C). The (Y) photochromic has the following structure.
[0140] [ka] 1′,3′-Dihydro-8-methoxy-1′,3′,3′-trimethyl-6-nitrospiro[2H-1-benzopyran-2,2′-(2H)-indole]
[0141] (Resin composition 3) Resin composition 3 was prepared by adding 8 parts by mass of (Y) Photochromic (CAS No. 1498-89-1) and 239 parts by mass of methyl ethyl ketone to 125 parts by mass of acrylic polyol (UVG301, manufactured by Nippon Shokubai Co., Ltd.), 15 parts by mass of hexamethylene diisocyanate (D165N, manufactured by Mitsui Chemicals, Inc.).
[0142] (Resin composition 4) Resin composition 4 was prepared by adding 5 parts by mass of a photopolymerization initiator (Omnirad127 manufactured by IGM Resins BV) to 50 parts by mass of the acrylate (B) and 50 parts by mass of the acrylate (C).
[0143] [Example 1] The resin composition 1 was applied to the substrate film PET using a bar coater (#20) so that the coating thickness (after drying) was 12 μm. The resin layer was dried by heating at 90° C. for 1 minute to obtain a resin layer (before curing). The integrated light amount was 400 mJ / cm 2 The resin layer was cured by irradiation with ultraviolet light in a nitrogen atmosphere to obtain a laminated film having a laminated structure of a substrate film PET / resin layer. The results of evaluation by the above-mentioned methods are shown in Table 2.
[0144] [Example 2] The resin composition 2 was applied to the substrate film PET using a bar coater (#4) so that the coating thickness (after drying) was 2 μm. The resin layer was obtained by heating and drying at 90° C. for 1 minute. The integrated light amount was 200 mJ / cm 2 The resin layer was cured by irradiation with ultraviolet light in a nitrogen atmosphere to obtain a laminated film having a laminated structure of a substrate film PET / resin layer. The results of evaluation by the above-mentioned methods are shown in Table 3.
[0145] [Example 3] The resin composition 3 was applied to the base film PET using a bar coater (#8) so that the coating thickness (after drying) was 2 μm. The resin layer was obtained by heating and drying at 80° C. for 1 min. Next, the resin composition 4 was applied onto the resin layer using a bar coater (#4) so that the coating thickness (after drying) was 3 μm. The integrated light amount was 400 mJ / cm 2 The functional layer was cured by irradiation with ultraviolet light in a nitrogen atmosphere to obtain a laminated film having a laminated structure of base film PET / resin layer / functional layer B. The results of evaluation by the above-mentioned methods are shown in Table 4.
[0146] [Example 4] The resin composition 3 was applied to the base film PET with a bar coater (#10) so that the coating thickness (after drying) was 3 μm. The resin layer was obtained by heating and drying at 80° C. for 1 minute. Next, the resin composition 4 was applied onto the resin layer with a bar coater (#4) so that the coating thickness (after drying) was 3 μm. The integrated light amount was 400 mJ / cm 2 The resin layer (functional layer B) was cured by irradiating it with ultraviolet light in a nitrogen atmosphere to obtain a laminated film having a laminated structure of base film PET / resin layer / functional layer B. The results of evaluation by the above-mentioned methods are shown in Table 4.
[0147] [Comparative Example 1] A laminated film was obtained by producing in the same manner as in Example 1, except that Sudan III (red pigment) was not added. The results were evaluated in the same manner as in Example 1 and are shown in Table 2.
[0148] [Comparative Example 2] A laminated film was obtained by producing in the same manner as in Example 1, except that no thermochromic was added in Example 1. The results of evaluation in the same manner as in Example 1 are shown in Table 2.
[0149] [Comparative Example 3] In Example 2, no photochromic was added and the integrated light amount was 400 mJ / cm 2 Except for the above, a laminated film was produced in the same manner as in Example 2. The results of evaluation in the same manner as in Example 1 are shown in Table 3.
[0150] <Evaluation Results> The properties of each of the laminated films obtained in the above Examples and Comparative Examples are shown in Tables 2 to 4 below.
[0151] [Table 2]
[0152] [Table 3]
[0153] [Table 4]
[0154] <Consideration> From the results of the above examples and comparative examples, it was found that a resin layer is laminated on the surface of a base film, and the resin layer contains a binder resin (A) and a chromic compound (B), so that while having flexibility, it is possible to achieve a high level of surface hardness (H or more) and repeated bending resistance (the ability to bend 200,000 times under the condition of outward bending, R = 2.0). In contrast, it was found that it is difficult to achieve the desired hard coat properties, repeated bending properties, and chromic properties (discoloration properties) simultaneously by simply providing a resin layer, as shown in Comparative Examples 1 and 2. In addition, as an additional effect, it was found that the surface hardness was higher and yet bending was possible under harsher conditions compared to the case where the chromic compound was not contained, probably because the chromic compound used was in a microencapsulated form.
[0155] It was also found that by setting the constituent compounds and thickness ratio of the resin layer within a specific range, it is not necessary to extremely increase the tensile modulus of the base film used, and it is not necessary to use a customized base film. Conventionally, when designing a laminate film having a surface layer with high surface hardness, it has been necessary to review the structural design of the raw materials that make up the base film used and further increase the tensile modulus, if necessary. In contrast, if the cured resin layer has a specific structure, it is possible to appropriately select a general-purpose base film available on the market, which provides the advantage of increased freedom in the selection of the base film. In addition, the more negative the b* value, the stronger the blue component tends to be, and it can be seen that the blue component disappeared at 35°C in Example 1 and Comparative Example 1. On the other hand, the more positive the a* value, the stronger the red component, with the value in Example 1 being larger than in Comparative Examples 1 and 2, confirming the presence of red. It was also found that this value hardly changes even when heated. From the above, it can be seen from the values that Example 1 exhibits blue + red = purple at room temperature, and changes color to red at 35°C. Furthermore, it was found that in Examples 2 to 4 in which a photochromic compound was combined, good chromic properties (color change properties) were also exhibited. [Industrial Applicability]
[0156] The laminated film of the present invention has a high level of surface hardness (H or more) and repeated bending resistance (can be bent 200,000 times under the condition of outward bending, R = 2.0), and yet has good chromic properties (discoloration), and can be used for various substrate films. It can be used for various purposes such as decorative purposes, optical purposes, and packaging purposes. It is particularly suitable for decorative purposes used in automobile parts, and can be given an indicating function in addition to decoration. [Explanation of symbols]
[0157] 10 Laminate 1 11 PMMA 12 Dry lamination 13 Chromic pigment + HC layer 14 Easy-to-form PET film 15 Dry lamination 16 Molded parts (ABS) 20 Laminate 2 21 Easy-to-form PET film 22 Release layer 23 Chromic dye + HC layer 24 Printed and / or vapor-deposited layers 25 Dry Lamination 26 Molded parts (ABS)
Claims
1. A laminate film comprising a base film and a resin layer provided on at least one surface of the base film, the resin layer containing a binder resin (A) and a chromic compound (B), and a color tone change (ΔX) of the surface of the resin layer calculated by the following formula (1) is 5.7 or more: ΔX=((ΔL * ) 2 + (Δa * ) 2 + (Δb * ) 2 ) 1/2 ...(1) ΔL * : L before and after external stimulation * Amount of change in value Δa * : a before and after external stimulation * Amount of change in value Δb * : before and after external stimulation * Amount of change in value
2. The laminated film according to claim 1 , wherein the binder resin (A) is an acrylic resin.
3. The laminate film according to claim 1 , wherein the chromic compound (B) is a photochromic compound or a thermochromic compound.
4. The laminate film according to claim 1, wherein the content of the chromic compound (B) in the resin layer is 0.1% by mass to 5.0% by mass.
5. The laminate film according to claim 1 , wherein the resin layer is formed by curing a resin composition containing a chromic compound (B) in microcapsules.
6. The laminated film according to claim 2 , wherein the acrylic resin is an active energy ray curable type.
7. The laminate film according to claim 1 , wherein the base film is a polyester film.
8. The laminate film according to claim 1 , wherein the base film is a polyethylene terephthalate (PET) film.
9. The laminate film according to claim 1 , wherein the base film is a copolymer polyester film.
10. The laminated film according to claim 1, which can be folded 200,000 times or more in a repeated bending test (outward bending, R=2.0 mm).
11. The laminate film according to claim 1 , further comprising a functional layer A between the base film and the resin layer.
12. The laminate film according to claim 11 , wherein the functional layer A is a printed layer.
13. The laminate film according to claim 11 , wherein the functional layer A is a release layer.
14. The laminate film according to claim 1 , further comprising a functional layer B on the resin layer.
15. The laminate film according to claim 14 , wherein the functional layer B is a hard coat layer.
16. The laminated film according to claim 1 , wherein the resin layer has a thickness of 20 μm or less.
17. A laminated film comprising a base film and a resin layer provided on at least one surface of the base film, the resin layer containing a binder resin (A) and a chromic compound (B), and a color tone change (ΔX) of the surface of the resin layer calculated by the following formula (1) is 5.7 or more; A laminate comprising other resin films bonded to both sides of the laminate film via adhesive layers. ΔX=((ΔL * ) 2 + (Δa * ) 2 + (Δb * ) 2 ) 1/2 ...(1) ΔL *: L before and after external stimulation * Amount of change in value Δa * : a before and after external stimulation * Amount of change in value Δb * : before and after external stimulation * Amount of change in value
18. A laminated film comprising a base film and a resin layer provided on at least one surface of the base film, the resin layer containing a binder resin (A) and a chromic compound (B), and a color tone change (ΔX) of the surface of the resin layer calculated by the following formula (1) is 5.7 or more; A laminate comprising a functional layer A between the base film and a resin layer, a printed layer or a vapor deposition layer on the resin layer of the laminate film, and another resin film bonded onto the printed layer or a vapor deposition layer via an adhesive layer. ΔX=((ΔL * ) 2 + (Δa * ) 2 + (Δb * ) 2 ) 1/2 ...(1) ΔL * : L before and after external stimulation * Amount of change in value Δa * : a before and after external stimulation * Amount of change in value Δb * : before and after external stimulation * Amount of change in value
19. The laminate according to claim 18 , wherein the functional layer A is a release layer.
20. The laminate according to claim 17 or 18, further comprising another functional layer B on the resin layer.
21. The laminate according to claim 20 , wherein the other functional layer B is a hard coat layer.
22. The laminate according to claim 17 or 18, wherein the other resin film attached to the resin layer side is a PMMA resin film.
23. The laminate according to claim 17 or 18, wherein the other resin film is an ABS resin film.
24. The laminate film according to any one of claims 1 to 16, which is for molding or decoration.
25. The laminate according to any one of claims 17 to 19, which is for molding or decoration.
26. The laminate film according to claim 24, which is used for decorating automobile parts.
27. The laminate according to claim 25, which is used for decorating automobile parts.
Citation Information
Patent Citations
Forgery preventive printed matter and forgery preventive information detecting method
JP1991231394A
Method for manufacturing thermochromic dimming element
JP2001353801A
Cited By
Preparation method of cyclic chiral nitro compound
CN119930562A