Resin composition
A silicon-containing compound-based resin composition with tailored solvents addresses filterability and transparency issues in polyimide films, enhancing their suitability for high-temperature display processes like LTPS and LTPO.
Patent Information
- Application Number
- JP2024071687
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-04-25
- Publication Date
- 2024-11-08
AI Technical Summary
Existing polyimide resin compositions used in display manufacturing have insufficient filterability and transparency, failing to meet the requirements for high-temperature processes such as LTPS and LTPO.
A resin composition is developed using a silicon-containing compound as a monomer, combined with specific solvents that satisfy Hansen solubility parameters, enhancing filterability and transparency, suitable for forming polyimide films in display processes.
The composition achieves both high filterability and low yellowness (low YI) properties, enabling its application in resin manufacturing and display processes like LTPS and LTPO, improving productivity and quality.
Smart Images

Figure 2024159658000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition. The present invention further relates to a display using the resin composition, a method for producing the resin composition, and a method for producing a polyimide resin film, a display, and a laminate. [Background technology]
[0002] Polyimide resins are insoluble, infusible, and extremely heat-resistant resins, and have excellent properties such as thermal oxidation resistance, heat resistance, radiation resistance, low temperature resistance, and chemical resistance, etc. For these reasons, polyimide resins are used in a wide range of fields, including electronic materials. Examples of applications of polyimide resins in the field of electronic materials include insulating coating materials, insulating films, semiconductors, and electrode protective films for thin film transistor liquid crystal displays (TFT-LCDs). Recently, taking advantage of the lightness and flexibility of polyimide films, their use as flexible substrates, instead of the glass substrates that have traditionally been used in the field of display materials, has been considered. In particular, in recent years, there has been a demand for materials that can withstand high-temperature processes at 400° C. or higher, such as low-temperature polysilicon (LTPS) and low-temperature polycrystalline oxide (LTPO). In one embodiment of polyimide for display applications, the polyimide is shipped in a varnish state to a display manufacturer, which then forms the polyimide into a film. The manufacturing process of this varnish includes a filtration step for removing impurities, and good filterability is required from the viewpoint of productivity.
[0003] For example, Document 1 discloses a polyimide composition containing butyl benzoate as an aromatic solvent and γ-butyrolactone (hereinafter also referred to as GBL) as a polar solvent. Furthermore, for example, Document 2 discloses an insulating coating material that uses N-methylpyrrolidone (hereinafter also referred to as NMP) as the main solvent and butylbenzene as the co-solvent for polyamideimide varnish. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2010-155895 A [Patent Document 2] China Patent Application Publication No. 102559040 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the solvents used in the above patent documents are insufficient in filterability (filtration rate) required for producing polyimide. Furthermore, the varnishes of the above-mentioned patent documents are insufficient in terms of achieving both the properties required for display applications (low YI (transparency) and filterability, etc.).
[0006] Therefore, an object of the present invention is to provide a resin composition for forming a polyimide film that is applicable to a display process, by using a silicon-containing compound as a monomer and that has both filterability and low YI (transparency) properties that are applicable to a resin production process. A further object of the present invention is to provide a display using the resin composition, and methods for producing the resin composition, the polyimide resin film, the display, and the laminate. [Means for solving the problem]
[0007] That is, the above problems can be solved by the following technical means. [Section 1] The following general formula (1): [ka] {In the formula, P1 represents a divalent organic group, P2 represents a tetravalent organic group, and p represents a positive integer.} And / or general formula (2): [ka] {In the formula, P3 represents a divalent organic group, P4 represents a tetravalent organic group, and q represents a positive integer.} and The following general formula (3): [ka] {In the formula, R1 and R2 each independently represent a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200.} A resin composition comprising a resin having a structure derived from a silicon-containing compound represented by the formula: The solvent includes a main solvent and a co-solvent, The main solvent comprises at least one selected from the group consisting of: N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, γ-butyrolactone, γ-valerolactone, hexamethylphosphoric amide, dimethyl sulfoxide, sulfolane, picoline and pyridine The cosolvent has a Hansen solubility parameter satisfying the following: δD=16.5~18.9 δP = 0.1 to 8.2 δH=1.1~5.5 A resin composition, wherein the co-solvent is less than 50% by mass when the total amount of the solvent is taken as 100% by mass. [Section 2] The Hansen solubility parameter of the cosolvent satisfies the following: δD=16.5~18.4 δP = 0.1 to 5.6 δH=1.1~4.7 Item 1. The resin composition according to item 1. [Section 3] The co-solvent may be n-butylbenzene, cyclopropene, cyclopentene, ethylbenzene methyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, t-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, t-butoxybenzene Item 3. The resin composition according to item 1 or 2, comprising at least one selected from the group consisting of benzene, propoxybenzene, benzaldehyde dimethyl acetal, amylbenzene, butoxybenzene, benzyl isobutyl ether, t-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene, isobutyl benzoate, ethyl benzoate, propyl benzoate, diphenylacetylene, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate and benzyl benzoate. [Section 4] The co-solvent is n-butylbenzene, cyclopropene, cyclopentene, ethylbenzene methyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, t-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, t-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, amylbenzene, butoxybenzene, benzyl isobutyl ether, t-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene , isobutyl benzoate, ethyl benzoate, propyl benzoate, diphenylacetylene, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate, benzyl benzoate, 2-methyltetrahydrofuran, cyclopentyl methyl ether, p-xylene, isopropylbenzene, d-limonene, styrene, a-methylstyrene, 2-methylcyclohexanone, 3-methylcyclohexanone, 2-vinyltoluene, isophorone, diisodecyl phthalate, propylbenzene, isobutylbenzene, 4-methylstyrene, 2-ethylstyrene, 2-isopropylstyrene, isopropyl benzoate, 4-t-butylstyrene, cycloheptanone, 4-ethylstyrene, 4-isopropylstyrene, and 2-propylstyrene. The resin composition according to item 1 or 2, comprising at least one selected from the group consisting of styrene, ... [Section 5] Item 3. The resin composition according to item 1 or 2, wherein the cosolvent has a boiling point of less than 250° C. [Section 6] Item 3. The resin composition according to item 1 or 2, wherein the co-solvent comprises at least one selected from the group consisting of n-butylbenzene and ethoxybenzene. [Section 7] The P1 and / or P3 are represented by the following general formula (4): [ka] Item 7. The resin composition according to any one of items 1 to 6, comprising a structural unit derived from: [Section 8] The P2 and / or P4 are represented by the following general formula (5): [ka] 8. The resin composition according to any one of items 1 to 7, comprising a structural unit derived from: [Section 9] The P1 and / or P3 are represented by the following general formula (6): [ka] 9. The resin composition according to any one of items 1 to 8, comprising a structural unit derived from: [Section 10] 10. The resin composition according to any one of items 1 to 9, wherein the co-solvent is 5% by mass or more and 40% by mass or less when the total amount of the solvent is taken as 100% by mass. [Section 11] 10. The resin composition according to any one of items 1 to 9, wherein the co-solvent is present in an amount of 5% by mass or more and 30% by mass or less when the total amount of the solvent is taken as 100% by mass. [Section 12] Item 12. The resin composition according to any one of items 1 to 11, which is used for a substrate of a flexible display. [Section 13] 13. A display comprising a thin film transistor (TFT) substrate and / or a color filter substrate using the resin composition according to any one of items 1 to 12. [Section 14] The following general formula (1): [ka] {In the formula, P1 represents a divalent organic group, P2 represents a tetravalent organic group, and p represents a positive integer.} And / or general formula (2): [ka] {In the formula, P3 represents a divalent organic group, P4 represents a tetravalent organic group, and q represents a positive integer.} and The following general formula (3): [ka] {In the formula, R1 and R2 each independently represent a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200.} A method for producing a resin composition containing a resin having a structure derived from a silicon-containing compound represented by the formula: synthesizing the resin using at least one selected from the group consisting of N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, γ-butyrolactone, γ-valerolactone, hexamethylphosphoric amide, dimethylsulfoxide, sulfolane, picoline, and pyridine as a main solvent; After synthesis of the resin, the resin satisfies the following Hansen solubility parameters before filtration: δD=16.5~18.9 δP = 0.1 to 8.2 δH=1.1~5.5 Adding a co-solvent to prepare a resin composition; A method for producing a resin composition. [Section 15] A coating step of coating a surface of a support with the resin composition according to any one of items 1 to 12 or the resin composition obtained by the method according to item 14; a film-forming step of heating the resin composition to form a polyimide resin film; a peeling step of peeling the polyimide resin film from the support; a step of irradiating the polyimide resin film with a laser from the support side prior to the peeling step. [Section 16] A coating step of coating a surface of a support with the resin composition according to any one of items 1 to 12 or the resin composition obtained by the method according to item 14; a film-forming step of heating the resin composition to form a polyimide resin film; an element forming step of forming an element on the polyimide resin film; a peeling step of peeling the polyimide resin film on which the element is formed from the support; A method for manufacturing a display comprising: [Section 17] A coating step of coating a surface of a support with the resin composition according to any one of items 1 to 12 or the resin composition obtained by the method according to item 14; a film-forming step of heating the resin composition to form a polyimide resin film; an element forming step of forming an element on the polyimide resin film; A method for producing a laminate, comprising: [Section 18] A coating step of coating a surface of a support with the resin composition according to any one of items 1 to 12 or the resin composition obtained by the method according to item 14; a film-forming step of heating the resin composition to form a polyimide resin film; an element forming step of forming an element on the polyimide resin film; peeling the polyimide resin film on which the elements are formed from the support; A method for producing a laminate, comprising: [Section 19] The following general formula (1): [ka] {In the formula, P1 represents a divalent organic group, P2 represents a tetravalent organic group, and p represents a positive integer.} And / or general formula (2): [ka] {In the formula, P3 represents a divalent organic group, P4 represents a tetravalent organic group, and q represents a positive integer.} A structural unit represented by The following general formula (3): [ka] {In the formula, R1 and R2 each independently represent a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200.} A resin composition comprising a resin having a structure derived from a silicon-containing compound represented by the formula: The solvent comprises one or more mixed solvents, A resin composition, wherein the mixed solvent has a Hansen solubility parameter satisfying the following: δD=16.8~18.8 δP=6.8~9.8 δH=4.5~6.8 Effect of the Invention
[0008] According to the present invention, it is possible to provide a polyimide-containing resin composition that uses a silicon-containing compound as a monomer and that has both filterability and low YI (transparency) properties that are applicable to resin production processes. Specifically, it is possible to provide a resin composition for forming a polyimide film that has both filterability and low YI (transparency) properties and is applicable to display processes such as LTPS (low temperature polysilicon), LTPO (low temperature polycrystalline oxide), etc. The present invention can further provide a display using the resin composition, and methods for producing the resin composition, the polyimide resin film, the display, and the laminate.
[0009] It should be noted that the above description should not be construed as a disclosure of all embodiments of the present invention and all advantages related to the present invention. Further embodiments of the present invention and their advantages will become apparent by reference to the following description. [Brief description of the drawings]
[0010] [Figure 1]FIG. 1 is a schematic diagram showing the structure above a polyimide substrate of a top-emission type flexible organic EL display as an example of the display of this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] An exemplary embodiment of the present invention (hereinafter, abbreviated as "the present embodiment") will be described in detail below. The present invention is not limited to the present embodiment, and can be practiced with various modifications within the scope of the gist of the present invention. In the present specification, the upper and lower limits of each numerical range can be arbitrarily combined.
[0012] 《Resin composition》 In one aspect, the resin composition of the present embodiment is a compound represented by the following general formula (1): [ka] {In the formula, P1 represents a divalent organic group, P2 represents a tetravalent organic group, and p represents a positive integer.} The number p of repeating units in general formula (1) is not particularly limited, but may be an integer of 2-150. And / or general formula (2): [ka] {In the formula, P3 represents a divalent organic group, P4 represents a tetravalent organic group, and q represents a positive integer.} and a solvent described below. The number of repeating units q in the general formula (2) is not particularly limited, but may be an integer of 2-150.
[0013] In one aspect, the resin composition of the present embodiment comprises: The following general formula (1): [ka] {In the formula, P1 represents a divalent organic group, P2 represents a tetravalent organic group, and p represents a positive integer.} The number p of repeating units in general formula (1) is not particularly limited, but may be an integer of 2-150. And / or general formula (2): [ka] {In the formula, P3 represents a divalent organic group, P4 represents a tetravalent organic group, and q represents a positive integer.} The number of repeating units q in the general formula (2) is not particularly limited, but may be an integer of 2-150. and The following general formula (3): [ka] {In the formula, R1 and R2 each independently represent a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200.} The resin composition includes a resin having a structure derived from a silicon-containing compound represented by the following formula (I) and a solvent. Solvents include a main solvent and a co-solvent. The primary solvent comprises at least one selected from the group consisting of: N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, γ-butyrolactone, γ-valerolactone, hexamethylphosphoric amide, dimethyl sulfoxide, sulfolane, picoline and pyridine The Hansen solubility parameters of the cosolvent are: δD=16.5~18.9 δP = 0.1 to 8.2 δH=1.1~5.5 When the total amount of the solvent is taken as 100% by mass, the amount of the co-solvent is less than 50% by mass.
[0014] <Polyimide precursor / polyimide> The resin contained in the resin composition of the present embodiment can be used without any particular limitation on its structure as long as it contains the structural units represented by general formula (1) and / or (2). Hereinafter, a resin containing a structural unit represented by general formula (1) will be referred to as a polyimide precursor, and a resin containing a structural unit represented by general formula (2) will be referred to as a polyimide, and each component constituting the resin and each component constituting the resin composition will be described.
[0015] Polyimide can be obtained by thermal imidization of polyimide precursor (including partially imidized polyimide precursor), or by chemical imidization. From the viewpoint of transparency of the obtained polyimide film, thermal imidization is preferred. In addition, the resin composition can contain an imidization promoter.
[0016] In the resin having the structures of general formulae (1) and (2), when the structure derived from general formula (1) (amide unit) is L (mol) and the structure derived from general formula (2) (imide unit) is M (mol), the ratio of L to M, L / M, is (5 mol% / 95 mol%) to (95 mol% / 5 mol%), and preferably (10 mol% / 90 mol%) to (90 mol% / 10 mol%).
[0017] From the viewpoint of storage stability of the resin composition, the molar fraction of the imide unit M is preferably 5 mol % or more, more preferably 10 mol % or more, further preferably 15 mol % or more, and particularly preferably 20 mol % or more. From the viewpoint of suppressing clouding or whitening of the resin composition, the molar fraction of the amide unit L is preferably 95 mol % or less, more preferably 90 mol % or less, further preferably 85 mol % or less, and particularly preferably 80 mol % or less.
[0018] The ratio L / M of L to M can be calculated from the amount of each monomer charged and the synthesis conditions, or can be calculated by the following method. The resulting resin composition (e.g., a partially imidized polyimide precursor) 13Then, all polyimide precursors and all polyimide resins were synthesized using the same monomers as those constituting the resin in the same ratio (mol%), and each was similarly measured. 13 Measure C-NMR. By comparing the integral values of the obtained chart (for example, the integral value of the C peak of the carbonyl group of the amide / imide bond), the L / M ratio can be calculated.
[0019] (Diamine) In the general formulae (1) and (2), P1 and P3 each preferably independently have a structure derived from the following diamine. For example, diamines include 9,9-bis(4-aminophenyl)fluorene (BAFL), p,m-phenylenediamine (pPD, mPD), 3,3'-diaminodiphenyl sulfone (3,3-DAS), 4,4'-diaminodiphenyl sulfone (4,4-DAS), 3,5-diaminobenzoic acid, 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether, 4-aminophenyl-4'-aminobenzoate (APAB), 4,4'-diaminobenzanilide, 2,2'-bis(trifluoromethyl)benzidine (T FMB), 2,2'-dimethylbenzidine (mTB), 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3'-diaminobiphenyl, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 1,4-bis(4- aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,3-bis(3-aminophenoxy)benzene (APB), bis[4-(4-aminophenoxy)phenyl]sulfone, 4,4-bis(4-aminophenoxy)biphenyl, 4,4-bis(3-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene , 9,10-bis(4-aminophenyl)anthracene, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, and 1,4-bis(3-aminopropyldimethylsilyl)benzene, 1,3-bis[1-(4-aminophenyl)-1-methylethyl]benzene (BiSAM), 1,4-cyclohexanediamine (CHDA) and 4,4-diaminodiphenyl ether (ODA) and the like. These diamines may be used alone or in combination.
[0020] Among these, from the viewpoint of being applicable to LTPS (low temperature polysilicon) and LTPO (low temperature polycrystalline oxide) processes and achieving both low YI (transparency) and low Rth of the resulting polyimide film, at least one selected from the group consisting of 9,9-bis(4-aminophenyl)fluorene (BAFL), p,m-phenylenediamine (pPD, mPD), 3,3'-diaminodiphenyl sulfone (3,3-DAS), 4,4'-diaminodiphenyl sulfone (4,4-DAS), 3,5-diaminobenzoic acid, and 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether is preferred, and 9,9-bis(4-aminophenyl)fluorene (BAFL), 3,3'-diaminodiphenyl sulfone (3,3-DAS), and 4,4'-diaminodiphenyl sulfone (4,4-DAS) are more preferred.
[0021] In the present disclosure, YI (yellowness index) refers to the depth of yellowness of the color of a polyimide resin film, and the lower the value, the higher the transparency of the polyimide resin film. The YI value at a thickness of 10 μm of the polyimide film obtained from the resin composition of this embodiment is preferably 16 or less, more preferably 13 or less, even more preferably 10 or less, particularly preferably 5 or less, and most preferably 3 or less, from the viewpoint of transparency. The YI of the resin composition is measured by the method described in the Examples.
[0022] In the present disclosure, Rth refers to retardation in the thickness direction when the resin composition is made into a film, and in the case of a display in which an image or subject is viewed (by the human eye or a camera, etc.) through a polyimide resin film (specifically, a bottom-emission type OLED, liquid crystal, transmissive display, under-display camera, etc.), the closer to 0 the Rth value is, the lower the value is, preferably. Rth (converted to a film thickness of 10 μm) is determined by measuring five locations on each sample using a retardation birefringence measuring device (manufactured by Oji Scientific Instruments, product name: KOBRA-WR) (wavelength of measuring light: 589 nm).
[0023] In the resin, P1 and / or P3 are each represented by the following general formula (4): [ka] It is preferable that the copolymer contains a structural unit derived from the following formula: It is preferable that the resin contains a constitutional unit derived from formula (4) since this makes it possible to achieve low YI, high heat resistance and low Rth while maintaining the solvent solubility of the resin. On the other hand, when the ratio of the general formula (4) in the resin in the resin composition of this embodiment is high, the chemical resistance tends to be poor. The reason for this is not clear, but it is thought that the compound of the general formula (4) has an alicyclic part, which has poor chemical resistance. Similarly, resins using alicyclic monomers (e.g., CpODA, etc.) also tend to have poor chemical resistance.
[0024] In the resin, P1 and / or P3 are each represented by the following general formula (6): [ka] It is preferable that the copolymer contains a structural unit derived from the following formula: Such a resin is preferred from the viewpoint of the transparency (in one embodiment, low yellowness index: low YI) and low Rth of the resulting resin.
[0025] (acid dianhydride) In the above general formulae (1) and (2), P2 and P4 each preferably independently have a structure derived from the following acid dianhydride. For example, the acid dianhydride may be 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF), pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 4,4'-oxydiphthalic dianhydride (ODPA), norbornane 2-spiro-α-cyclopentanone-α'-spiro-2''-norbornane-5,5'',6,6'' -tetracarboxylic dianhydride (CpODA), 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride (6FDA), 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-cyclohexene-1,2 dicarboxylic anhydride, 1,2,3,4-benzenetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 3,3',4, 4'-Diphenylsulfonetetracarboxylic dianhydride, methylene-4,4'-diphthalic dianhydride, 1,1-ethylidene-4,4'-diphthalic dianhydride, 2,2-propylidene-4,4'-diphthalic dianhydride, 1,2-ethylene-4,4'-diphthalic dianhydride, 1,3-trimethylene-4,4'-diphthalic dianhydride, 1,4-tetramethylene-4,4'-diphthalic dianhydride, 1,5-pentamethylene-4,4'-diphthalic dianhydride, 4,4'- Oxydiphthalic dianhydride, p-phenylenebis(trimellitate anhydride), thio-4,4'-diphthalic dianhydride, sulfonyl-4,4'-diphthalic dianhydride, 1,3-bis(3,4-dicarboxyphenyl)benzene dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,3-bis[2-(3,4-dicarboxyphenyl)-2-propyl]benzene benzene dianhydride, 1,4-bis[2-(3,4-dicarboxyphenyl)-2-propyl]benzene dianhydride, bis[3-(3,4-dicarboxyphenoxy)phenyl]methane dianhydride, bis[4-(3,4-dicarboxyphenoxy)phenyl]methane dianhydride, 2,2-bis[3-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, bis(3,4-dicarboxyphenoxy)dimethylsilane dianhydride, 1,3-bis(3,4-dicarboxyphenyl)-1,1,3,3-tetramethyldisiloxane dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, and 1,2,7,8-phenanthrenetetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride (HPMDA), and 1,2,3,4-cyclobutanetetracarboxylic dianhydride (CBDA), the following structure: [ka] The compound represented by the formula (BzDA): The structure: [ka] Examples of the compound include the compound represented by the formula (BNBDA). Among these acid dianhydrides, from the viewpoint of being applicable to LTPS (low temperature polysilicon) and LTPO (low temperature polycrystalline oxide) processes and achieving both low YI and low Rth in the resulting polyimide film, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF), pyromellitic anhydride (PMDA), and 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), which are represented by the following general formula (5), are preferred, and BPAF is more preferred. In one embodiment, a polyimide resin composition containing 4,4'-oxydiphthalic dianhydride (ODPA) can be cured at a low temperature of about 260°C to form a polyimide resin film, and therefore 4,4'-oxydiphthalic dianhydride (ODPA) is preferred as the dianhydride. These acid dianhydrides can be used alone or in combination.
[0026] In the resin composition of the present embodiment, P2 and / or P4 is a compound represented by the general formula (5): [ka] It can contain structural units derived from:
[0027] Furthermore, in the resin composition of the present embodiment, P2 and / or P4 is a group represented by the following general formula (7): [ka] It can contain structural units derived from:
[0028] In one aspect, in the resin composition of the present embodiment, P1 and / or P3 may contain at least a structural unit derived from general formula (4), and P2 and / or P4 may contain a structural unit derived from general formula (5). In one aspect, the resin composition of the present embodiment can be one in which the structural units derived from general formula (4) account for 80 mol % or less of all diamine monomers, or the structural units derived from general formula (5) account for 15 mol % or more of all dianhydride monomers. By making the structural unit derived from general formula (4) 80 mol % or less of all diamine monomers, the YI of the resulting polyimide film can be reduced, and by making the structural unit derived from general formula (5) 15 mol % or more of all acid dianhydride monomers, the heat resistance and Young's modulus of the resulting polyimide film can be increased.
[0029] In the resin composition of the present embodiment, P1 and / or P3 may contain at least a structural unit derived from general formula (3) described below, and P2 and / or P4 may contain a structural unit derived from general formula (7).
[0030] In one aspect, the resin composition of the present embodiment may be such that P1 and / or P3 contain at least one or more structural units derived from general formula (3) and general formula (4), P2 and / or P4 contain a structural unit derived from general formula (5), and the structural unit derived from general formula (3) accounts for 20 mol % or more of all diamine monomers. By making the constitutional unit derived from general formula (3) 20 mol % or more of all diamine monomers, the YI and Rth of the obtained polyimide film can be reduced.
[0031] In one aspect, in the resin composition of the present embodiment, P1 and / or P3 may contain at least one or more structural units derived from general formula (3) and general formula (4), and P2 and / or P4 may contain at least one or more structural units derived from general formula (5) and general formula (7).
[0032] <Silicon-containing compounds> In the resin according to the present embodiment, the structural unit of the general formula (2) is The following general formula (3): [ka] {In the formula, R1 and R2 each independently represent a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200.} The silicon-containing compound may include a structure derived from the silicon-containing compound represented by the formula:
[0033] Therefore, the silicon-containing compound used in the synthesis of the polyimide precursor in this embodiment may be a compound having a reactive group capable of co-condensing with at least one of a tetracarboxylic dianhydride and a diamine.
[0034] The silicon-containing compound in this embodiment is, for example, a compound represented by the following formula (17) (hereinafter, also simply referred to as (17)): [ka] {In the formula, R1 each independently represents a single bond or a divalent organic group having 1 to 10 carbon atoms; R2 and R3 each independently represent a monovalent organic group having 1 to 10 carbon atoms, and at least one of R2 and R3 represents a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms; R4 and R5 each independently represent a monovalent organic group having 1 to 10 carbon atoms, and at least one of R4 and R5 represents a monovalent aromatic group having 6 to 10 carbon atoms; R6 and R7 each independently represent a monovalent organic group having 1 to 10 carbon atoms, and at least one of R6 and R7 represents an organic group containing an unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms. L1 and L2 each independently represent a monovalent organic group having an acid anhydride structure, an amino group, an isocyanate group, a carboxyl group, an alkoxycarbonyl group, a halogenated carbonyl group, a hydroxyl group, an epoxy group, or a mercapto group; i is an integer from 1 to 200; j and k each independently represent an integer of 0 to 200, and j represents an integer of 1 to 200; and 0≦j / (i+j+k)≦0.50 and satisfy the relationship of 0.05≦j / (i+j+k)≦0.50.
[0035] Each R1 in formula (17) is independently a single bond or a divalent organic group having 1 to 10 carbon atoms. The divalent organic group having 1 to 10 carbon atoms may be linear, cyclic, or branched, and may be saturated or unsaturated (in one embodiment, an aromatic hydrocarbon group). When R1 is a divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, examples of the alkylene groups include linear or branched alkylene groups such as a methylene group (in one embodiment, a trimethylene group), an ethylene group, a propylene group (in one embodiment, an n-propylene group, an i-propylene group), a butylene group (in one embodiment, an n-butylene group, an s-butylene group, or a t-butylene group), a pentylene group (in one embodiment, an n-pentylene group, or a neopentylene group), an n-hexylene group, an n-heptylene group, an n-octylene group, an n-nonylene group, or an n-decylene group; Examples of the cycloalkylene groups include a cyclopropylene group, a cyclobutylene group, a cyclopentylene group, a cyclohexylene group, a cycloheptylene group, and a cyclooctylene group. When R1 is a divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, it is preferably at least one selected from the group consisting of a trimethylene group, an ethylene group, an n-propylene group, and an i-propylene group. When R1 is an unsaturated aliphatic hydrocarbon group, specific examples thereof include an alkenyl group and an allyl group.
[0036] In formula (17), R2 and R3 are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of R2 and R3 is a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms. The monovalent organic group having 1 to 10 carbon atoms may be linear, cyclic, or branched, and may be saturated or unsaturated (in one embodiment, an aromatic hydrocarbon group). For example, when R2 and R3 are monovalent organic groups having 1 to 10 carbon atoms, linear or branched alkyl groups such as a methyl group, an ethyl group, a propyl group (in one embodiment, an n-propyl group, an i-propyl group), a butyl group (in one embodiment, an n-butyl group, an s-butyl group, or a t-butyl group), a pentyl group (in one embodiment, an n-pentyl group, or a neopentyl group), an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, or an n-decyl group; cycloalkyl groups such as a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group; Examples of the aromatic groups include a phenyl group, a tolyl group, a xylyl group, an α-naphthyl group, and a β-naphthyl group. The monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms may be linear, cyclic, or branched, and may be saturated or unsaturated (in one embodiment, an aromatic hydrocarbon group). For example, when R2 and R3 are a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms, a straight-chain or branched-chain alkyl group such as a methyl group, an ethyl group, a propyl group (in one embodiment, an n-propyl group, an i-propyl group), a butyl group (in one embodiment, an n-butyl group, an s-butyl group, or a t-butyl group), or a pentyl group (in one embodiment, an n-pentyl group, or a neopentyl group); Examples of the cycloalkyl group include a cyclopropyl group, a cyclobutyl group, and a cyclopentyl group. When R2 and R3 are monovalent aliphatic hydrocarbon groups having 1 to 5 carbon atoms, they are preferably at least one type selected from the group consisting of a methyl group, an ethyl group, and an n-propyl group.
[0037] In formula (17), R4 and R5 are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of R4 and R5 is a monovalent aromatic group having 6 to 10 carbon atoms. The monovalent organic group having 1 to 10 carbon atoms may be linear, cyclic, or branched, and may be saturated or unsaturated (in one embodiment, an aromatic hydrocarbon group). For example, when R4 and R5 are a monovalent organic group having 1 to 10 carbon atoms, linear or branched alkyl groups such as a methyl group, an ethyl group, a propyl group (in one embodiment, an n-propyl group, an i-propyl group), a butyl group (in one embodiment, an n-butyl group, an s-butyl group, or a t-butyl group), a pentyl group (in one embodiment, an n-pentyl group, or a neopentyl group), an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, or an n-decyl group; cycloalkyl groups such as a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group; Examples of the aromatic groups include a phenyl group, a tolyl group, a xylyl group, an α-naphthyl group, and a β-naphthyl group. When R4 and R5 are monovalent aromatic groups having 6 to 10 carbon atoms, examples thereof include a phenyl group, a tolyl group, a xylyl group, an α-naphthyl group, and a β-naphthyl group, and it is preferable that the group is at least one selected from the group consisting of a phenyl group, a tolyl group, and a xylyl group.
[0038] In formula (17), R6 and R7 are each independently a monovalent organic group having 1 to 10 carbon atoms, and at least one of R6 and R7 is preferably an organic group having an unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms. The monovalent organic group having 1 to 10 carbon atoms may be linear, cyclic, or branched, and may be saturated or unsaturated (in one embodiment, an aromatic hydrocarbon group). When R6 and R7 are each a monovalent organic group having 1 to 10 carbon atoms, for example, a straight-chain or branched-chain alkyl group such as a methyl group, an ethyl group, a propyl group (in one embodiment, an n-propyl group, an i-propyl group), a butyl group (in one embodiment, an n-butyl group, an s-butyl group, or a t-butyl group), a pentyl group (in one embodiment, an n-pentyl group, or a neopentyl group), an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, or an n-decyl group; cycloalkyl groups such as a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group; Examples of the aromatic groups include a phenyl group, a tolyl group, a xylyl group, an α-naphthyl group, and a β-naphthyl group. When R6 and R7 are monovalent organic groups having 1 to 10 carbon atoms, they are preferably at least one type selected from the group consisting of a methyl group, an ethyl group, and a phenyl group. The organic group having an unsaturated aliphatic hydrocarbon group may be an unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms, and may be linear, cyclic, or branched. When R6 and R7 are each an unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms, examples of such alkenyl groups include a vinyl group, an allyl group, a 1-propenyl group, a butenyl group (in one embodiment, a 3-butenyl group or a 2-butenyl group), a pentenyl group, a hexenyl group, a heptenyl group, an octenyl group, a nonenyl group, and a decenyl group; Alkynyl groups such as ethynyl, propynyl, butynyl, pentynyl, and hexynyl groups; Examples of such cycloalkenyl groups include cyclopentenyl and cyclohexenyl groups. When R6 and R7 are each an unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms, it is preferably at least one selected from the group consisting of a vinyl group, an allyl group, and a 3-butenyl group.
[0039] Some or all of the hydrogen atoms of R1 to R7 in formula (17) may be substituted with a substituent such as a halogen atom, eg, F, Cl, or Br, or may be unsubstituted.
[0040] In formula (17), L1 and L2 are each independently a monovalent organic group containing an acid anhydride structure (also referred to as an acid anhydride group), an amino group, an isocyanate group, a carboxyl group, an alkoxycarbonyl group, a halogenated carbonyl group, a hydroxyl group, an epoxy group, or a mercapto group. Examples of the monovalent organic group containing an acid anhydride structure include a group represented by the following formula: [ka] {wherein "*" represents a bond.}
[0041] Among these, an amino group and an acid anhydride group are preferred, and from the viewpoint of viscosity stability of the resin composition, an amino group is more preferred.
[0042] The alkoxyl group in the alkoxycarbonyl group may be an alkoxyl group having 1 to 6 carbon atoms, such as a methoxyl group, ethoxyl group, n-propoxyl group, i-propoxyl group, n-butoxyl group, i-butoxyl group, or t-butoxyl group.
[0043] The halogen atom in the halogenated carbonyl group is preferably a halogen atom other than a fluorine atom, and more preferably a chlorine atom or an iodine atom.
[0044] In the formula (17), i is an integer of 1 to 200, preferably an integer of 2 to 100, more preferably an integer of 4 to 80, and further preferably an integer of 8 to 40. In the formula (17), j and k each independently represent an integer of 0 to 200. j is preferably an integer of 1 to 200, more preferably an integer of 0 to 50, and further preferably an integer of 0 to 20. In formula (17), it is preferable that the relationship 0≦j / (i+j+k)≦0.50, and 0.05≦j / (i+j+k)≦0.50 is satisfied.
[0045] The functional group equivalent weight of the silicon-containing compound represented by formula (17) is preferably 800 or more, more preferably 1000 or more, and even more preferably 1500 or more, from the viewpoint of the filterability of the resin composition of the present disclosure. On the other hand, if the functional group equivalent is 500 or less, the filterability tends to be poor. Here, the functional group equivalent in the present disclosure is the molecular weight of the silicon-containing compound per 1 mole of functional group (unit: g / mol). The functional group equivalent can be measured by a known method according to existing standards and the like. Furthermore, it is preferable that the functional group equivalent of the silicon-containing compound is 800 or more, since the residual stress of the polyimide film in a nitrogen atmosphere is small. The reason for this is believed to be that when the functional group equivalent is a certain value or more, the silicone domain increases, and stress is relieved. The filterability (filtration rate) of the resin composition of the present disclosure is measured by the method described in the Examples.
[0046] The resin in the resin composition of the present disclosure is preferably one having a structure derived from formula (17), since the polyimide film has a small residual stress measured under a nitrogen atmosphere and has good performance. The reason for measuring under a nitrogen atmosphere is that in the display manufacturing process, when an inorganic film such as SiO or SiN is formed on the polyimide film, the film may be exposed to a nitrogen atmosphere, and therefore low residual stress under a nitrogen atmosphere is required.
[0047] From the viewpoints of the type of monomer, cost, and increasing the molecular weight of the resulting polyimide precursor, the silicon-containing compound having a structure represented by general formula (17) is preferably a silicon-containing diamine. Examples of silicon-containing diamines include those represented by the following formula (18): [ka] {In the formula, P5 each independently represents a divalent hydrocarbon group having 1 to 10 carbon atoms and may be the same or different, P3 and P4 are the same as R2 and R3 defined in general formula (17), and 1 represents an integer of 1 to 200.} Preferred is a diamino(poly)siloxane represented by the following formula:
[0048] Preferred structures of P3 and P4 in the general formula (18) include a methyl group, an ethyl group, a propyl group, a butyl group, and a phenyl group, etc. Among these, the most preferred is a methyl group. Furthermore, P5 in the general formula (18) may be a trimethylene group (-CH2CH2CH2-).
[0049] In the above general formula (18), l is an integer of 1 to 200, and is preferably an integer of 3 to 200 from the viewpoint of the heat resistance of the polyimide obtained by using the silicon-containing diamine represented by formula (18).
[0050] The preferred range of the functional group equivalent of the compound represented by the general formula (18) is the same as that of the silicon-containing compound represented by the above-mentioned general formula (17).
[0051] The copolymerization ratio of the silicon-containing diamine is preferably 0.5 to 30 mass %, more preferably 1.0 mass % to 25 mass %, and even more preferably 1.5 mass % to 20 mass %, based on the total mass of the polyimide precursor / polyimide. When the silicon-containing diamine is 0.5% by mass or more, the residual stress generated between the support, which will be described later, can be effectively reduced. When the silicon-containing diamine content is 30% by mass or less, the resulting polyimide film has good transparency, which is preferable from the viewpoint of achieving low haze, high total light transmittance, and high glass transition temperature (hereinafter referred to as Tg).
[0052] As described above, the silicon-containing compound used as a monomer for the polyimide precursor / polyimide may be synthesized using the common general technical knowledge at the time of filing, or a commercially available product may be used. Commercially available products include methylphenyl silicone oil modified with amines at both ends: X22-1660B-3 (functional group equivalent: 2200), X22-9409 (functional group equivalent: 670) (both manufactured by Shin-Etsu Chemical Co., Ltd.); Methylphenyl silicone oil modified with acid anhydrides at both ends (Shin-Etsu Chemical Co., Ltd.: X22-168-P5-B (functional group equivalent: 2100)), Methylphenyl silicone oil modified with epoxy at both ends (Shin-Etsu Chemical Co., Ltd.: X22-2000 (functional group equivalent: 620)), Amino-modified dimethyl silicone at both ends: PAM-E (functional group equivalent: 130), X22-161A (functional group equivalent: 800), X22-161B (functional group equivalent: 1500), KF8012 (functional group equivalent: 2200) (all manufactured by Shin-Etsu Chemical Co., Ltd.); Toray Dow Corning: BY16-853U (functional group equivalent: 450), JNC Corporation: Silaplane FM3311 (number average molecular weight 1000), Both ends of epoxy-modified dimethyl silicone (Shin-Etsu Chemical Co., Ltd.: X-22-163A (functional group equivalent: 1750), Dimethyl silicone modified with alicyclic epoxy at both ends (X-22-169B (functional group equivalent: 1700) manufactured by Shin-Etsu Chemical Co., Ltd.), Dimethyl silicone modified with hydroxyl groups at both ends (Shin-Etsu Chemical Co., Ltd.: KF-6000), Both ends of mercapto-modified dimethyl silicone (Shin-Etsu Chemical Co., Ltd.: X-22-167B (functional group equivalent: 1700)), Examples thereof include dimethyl silicone modified with acid anhydrides at both ends (manufactured by Shin-Etsu Chemical Co., Ltd.: X-22-168A (functional group equivalent: 1000)). Among these, from the viewpoints of cost, improved chemical resistance, and improved Tg, dimethyl silicone oil modified with amines at both ends is preferred.
[0053] <solvent> The resin composition of the present embodiment includes a solvent. In one embodiment, the solvent includes a main solvent and a co-solvent.
[0054] Main solvent In the present disclosure, a primary solvent refers to the component having the largest mass relative to the total amount of the solvent including the primary solvent and the co-solvent, and a co-solvent refers to the component having the smallest mass relative to the total amount of the solvent including the primary solvent and the co-solvent. The content of the main solvent is 50% by mass or more, preferably 60% by mass or more, and particularly preferably 70% by mass or more, when the total amount of the solvent is taken as 100% by mass.
[0055] The main solvent of the present disclosure is preferably one that has good solubility for polyimide / polyimide precursor and can appropriately control the solution viscosity of the resin composition of the present disclosure. In the present disclosure, for example, the main solvent is an amide such as N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, and hexamethylphosphoric amide; Lactones such as 1,3-dimethylimidazolidinone, tetramethylurea, γ-butyrolactone, and γ-valerolactone; The solvent contains at least one selected from the group consisting of dimethyl sulfoxide, sulfolane, picoline, and pyridine. These main solvents may be used alone or in combination of two or more. Among them, it is preferable to use at least one selected from the group consisting of N-methyl-2-pyrrolidone (NMP), hexamethylphosphoric amide, and N,N-dimethylacetamide.
[0056] Specific examples of the main solvent composition include N-methyl-2-pyrrolidone (NMP) alone, or Combinations of two types (for example, main solvent 1 and main solvent 2) include combinations of N-methyl-2-pyrrolidone (NMP) and γ-butyrolactone (GBL), GBL and dimethylsulfoxide, and GBL and 3-methoxy-N,N-dimethylpropanamide, etc. When two types of main solvents are combined, the mass ratio of main solvent 1:main solvent 2 is preferably 10:90 to 90:10. The mass ratio of NMP to GBL may be, for example, NMP:GBL=10:90 to 90:10, and is preferably 50:50.
[0057] The numerical range of the Hansen solubility parameter (hereinafter also referred to as the SP value) of the main solvent is not particularly limited as long as it can dissolve the monomer, which is the raw material of the polyimide, and the polymer, which is the product. In one embodiment, the primary solvent has a Hansen solubility parameter of δD=16.5~19.0 δP=8.0~17.5 ΔH may be in the range of 5.7 to 12.3. When the SP value of the main solvent is within the above range, the solubility of the polyimide / polyimide precursor is good. In addition, when the main solvent is used as a synthesis solvent for synthesizing the resin of the present disclosure, it is preferable because the molecular weight of the polyimide / polyimide precursor can be increased.
[0058] Co-solvent As a cosolvent, the Hansen solubility parameter is δD=16.5~18.9 δP = 0.1 to 8.2 It is preferable that the co-solvent has an ΔH value in the range of 1.1 to 5.5, has a good solubility of polyimide / polyimide precursor when mixed with the main solvent, and can appropriately control the solution viscosity of the resin composition of the present disclosure. When the SP value of the co-solvent is within the above range, the filterability of the resin composition can be improved. Two or more solvents may be mixed and used as a co-solvent. In this case, the Hansen solubility parameter is calculated by multiplying the Hansen solubility parameter of each solvent by the volume fraction (vol%) of each solvent.
[0059] The Hansen solubility parameter of the cosolvent is preferably within the following ranges, since it provides better filterability: δD=16.5~18.4 δP = 0.1 to 5.6 δH=1.1~4.7
[0060] In the present disclosure, a mixed solvent refers to a solvent containing one or more main solvents and one or more co-solvents. The resin composition of the present embodiment may contain a solvent containing one or more mixed solvents. The Hansen solubility parameter of the mixed solvent containing the main solvent and the cosolvent is in the following range: ΔD = 16.8 to 18.8 δP=6.8~9.8 When ΔH is 4.5 to 6.8, the filterability of the resin composition is good, which is preferable. Good filterability is considered to be correlated with the Hansen solubility parameter of the polymer constituting the resin.
[0061] Hansen solubility parameters are parameters developed by Charles M. Hansen as a way to predict whether one substance will dissolve in another to form a solution. They are based on the idea that like will dissolve if one molecule is "similar" to another, by definition, if it bonds to itself in a similar way. Specifically, each molecule is given the following three Hansen solubility parameters, each measured in units of MPa: 0.5 It is. δD: Energy from intermolecular dispersion forces δP: Energy from dipole-dipole intermolecular forces between molecules δH: Energy from hydrogen bonds between molecules. These three parameters can be treated as the coordinates of a three-dimensional point, also known as Hansen space: the closer two molecules are in this three-dimensional space, the more likely they are to dissolve in each other. The SP values of the main solvent and the cosolvent are measured by the method described in the Examples. When the main solvent or the co-solvent is a combination of two or more solvents, the solubility parameter is a value calculated from each solvent and its charging ratio.
[0062] The present inventors have found that a polyimide precursor obtained by using, in addition to a specific main solvent, a co-solvent satisfying all of the specific Hansen solubility parameters is excellent in properties required for display applications, particularly filterability and low YI (transparency) of the polyimide precursor. In addition, by using a specific cosolvent in a specific ratio, it is possible to provide a polyimide-containing resin composition that is applicable to displays (particularly displays using LTPS (low temperature polysilicon) and LTPO (low temperature polycrystalline oxide)).
[0063] Specific examples of cosolvents include n-butylbenzene, cyclopropene, cyclopentene, ethylbenzene methyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, t-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, t-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, amylbenzene, butoxybenzene, benzyl isobutyl ether, t-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, and cyclohexyl. Benzene, isobutyl benzoate, ethyl benzoate, propyl benzoate, diphenylacetylene, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate, benzyl benzoate, 2-methyltetrahydrofuran, cyclopentyl methyl ether, p-xylene, isopropylbenzene, d-limonene, toluene, styrene, a-methylstyrene, 2-methylcyclohexanone, 3-methylcyclohexanone, 2-vinyltoluene, isophorone, diisodecyl phthalate, propylbenzene, isobutylbenzene, 4-methylstyrene, 2-ethylstyrene, 2-isopropylstyrene, isopropyl benzoate, 4-t-butylstyrene, cycloheptanone, 4-ethylstyrene, 4-isopropylstyrene, 2-propylstyrene, n-butyl benzoate, and dibutyl sebacate. These co-solvents may be used alone or in combination.
[0064] Examples of the cosolvent having a more preferable SP value include n-butylbenzene, cyclopropene, cyclopentene, ethylbenzene methyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, 2-methyltetrahydrofuran, cyclopentyl methyl ether, p-xylene, isopropylbenzene, d-limonene, toluene, diphenylacetylene, dibutyl sebacate, t-butylbenzene, 1,4-cineole, benzyl methacrylate, ether, isopropoxybenzene, t-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, amylbenzene, butoxybenzene, benzyl isobutyl ether, t-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene, isobutyl benzoate, propylbenzene, isobutylbenzene, 4-methylstyrene, 2-ethylstyrene, 2-isopropylstyrene, isopropyl benzoate, and 4-t-butylstyrene. The use of these solvents as co-solvents is preferable because it improves the filterability of the resin composition of the present embodiment.
[0065] In one embodiment, the co-solvent of the present disclosure is n-butylbenzene, cyclopropene, cyclopentene, ethylbenzene methyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, t-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, t-butoxybenzene, propanediol, tert-butylbenzene ... From the viewpoint of preventing a decrease in the filtration rate over time, it is preferable that the filtration agent contains at least one selected from the group consisting of benzene, benzaldehyde dimethyl acetal, amylbenzene, butoxybenzene, benzyl isobutyl ether, t-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene, isobutyl benzoate, ethyl benzoate, propyl benzoate, diphenylacetylene, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate, and benzyl benzoate.
[0066] In one embodiment, the co-solvent of the present disclosure is n-butylbenzene, cyclopropene, cyclopentene, ethylbenzene methyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, t-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, t-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, amylbenzene, butoxybenzene, benzyl isobutyl ether, t-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene From the viewpoint of low YI, a polyimide obtained by containing at least one selected from the group consisting of benzoic acid, isobutyl benzoate, ethyl benzoate, propyl benzoate, diphenylacetylene, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate, benzyl benzoate, 2-methyltetrahydrofuran, cyclopentyl methyl ether, p-xylene, isopropylbenzene, d-limonene, styrene, a-methylstyrene, 2-methylcyclohexanone, 3-methylcyclohexanone, 2-vinyltoluene, isophorone, diisodecyl phthalate, propylbenzene, isobutylbenzene, 4-methylstyrene, 2-ethylstyrene, 2-isopropylstyrene, isopropyl benzoate, 4-t-butylstyrene, cycloheptanone, 4-ethylstyrene, 4-isopropylstyrene, and 2-propylstyrene is preferable.
[0067] Even if the boiling point of the cosolvent of the present disclosure is 250° C. or higher, it can be suitably used as the cosolvent of the present embodiment. However, it is preferable that the cosolvent of the present disclosure has a boiling point of less than 250° C., because this can reduce the YI value when a polyimide resin composition is prepared by adding a resin to the cosolvent and the composition is heated to form a polyimide resin film.
[0068] Examples of co-solvents having a boiling point of 250° C. or higher include diphenylacetylene, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate, benzyl benzoate, butyl benzoate, and butyl sebacate.
[0069] Cosolvents with a boiling point of less than 250°C include n-butylbenzene, cyclopropene, cyclopentene, ethylbenzene methyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, t-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, t-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, amylbenzene, butoxybenzene, benzyl isobutyl ether, and t-benzoate. butyl, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene, isobutyl benzoate, ethyl benzoate, propyl benzoate, 2-methyltetrahydrofuran, cyclopentyl methyl ether, p-xylene, isopropylbenzene, d-limonene, styrene, a-methylstyrene, 2-methylcyclohexanone, 3-methylcyclohexanone, 2-vinyltoluene, isophorone, diisodecyl phthalate, propylbenzene, isobutylbenzene, 4-methylstyrene, 2-ethylstyrene, 2-isopropylstyrene, isopropyl benzoate, 4-t-butylstyrene, cycloheptanone, 4-ethylstyrene, 4-isopropylstyrene, and 2-propylstyrene.
[0070] Among the co-solvents, at least one selected from the group consisting of n-butylbenzene and ethoxybenzene is particularly preferred from the viewpoint of achieving both filterability and a low YI value.
[0071] From the viewpoint of achieving both the filterability of the resin composition and a low YI of the polyimide resin film, the content of the co-solvent is less than 50% by mass, preferably 40% by mass or less, and particularly preferably 30% by mass or less, when the total amount of the solvent is taken as 100% by mass. From the viewpoint of the filterability of the resin composition, the content of the co-solvent is preferably 5% by mass or more, when the total amount of the solvent is taken as 100% by mass. When the total amount of the solvent is taken as 100% by mass, the content of the cosolvent is preferably from 5% by mass to 40% by mass, and more preferably from 5% by mass to 30% by mass.
[0072] Specific examples of compositions in which cosolvents are mixed include a combination of two types (for example, cosolvent 1 and cosolvent 2) such as n-butylbenzene and ethoxybenzene, and n-butylbenzene and n-butyl benzoate. When cosolvents are combined as described above, the mass ratio of cosolvent 1:cosolvent 2 is preferably 10:90 to 90:10. The mass ratio of n-butylbenzene to ethoxybenzene may be, for example, n-butylbenzene:ethoxybenzene=10:90 to 90:10, and is preferably 50:50.
[0073] A specific example of the composition of the solvent of the present disclosure is a mixed solvent of N-methyl-2-pyrrolidone (NMP) as a main solvent and n-butylbenzene as a co-solvent, etc. The mass ratio of the main solvent to the co-solvent may be, for example, main solvent:co-solvent=95:5 to 51:49.
[0074] Additional Ingredients The resin composition of the present embodiment may further contain additional components in addition to the polyimide / polyimide precursor and the solvent, such as a surfactant and an alkoxysilane compound.
[0075] (Surfactant) By adding a surfactant to the resin composition of the present embodiment, the coatability of the resin composition can be improved. Specifically, the occurrence of streaks in the coating film can be prevented.
[0076] Examples of the surfactant include silicone-based surfactants, fluorine-based surfactants, and other nonionic surfactants. Examples of silicone surfactants include organosiloxane polymers KF-640, 642, 643, KP341, X-70-092, and X-70-093 (all manufactured by Shin-Etsu Chemical Co., Ltd.); SH-28PA, SH-190, SH-193, SZ-6032, SF-8428, DC-57, DC-190 (all manufactured by Toray Dow Corning Silicone Co., Ltd.); SILWET L-77, L-7001, FZ-2105, FZ-2120, FZ-2154, FZ-2164, FZ-2166, L-7604 (all manufactured by Nippon Unicar); DBE-814, DBE-224, DBE-621, CMS-626, CMS-222, KF-352A, KF-354L, KF-355A, KF-6020, DBE-821, DBE-712 (Gelest), BYK-307, BYK-310, BYK-378, BYK-333 (all manufactured by BYK Japan); Granol (manufactured by Kyoeisha Chemical Co., Ltd.) and the like.
[0077] Examples of fluorine-based surfactants include Megafac F171, F173, and R-08 (manufactured by Dainippon Ink and Chemicals, Inc.); Examples include Fluorad FC4430 and FC4432 (Sumitomo 3M Limited). Other nonionic surfactants include, for example, polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, and polyoxyethylene octylphenol ether.
[0078] Among these surfactants, from the viewpoint of the coatability (streak prevention) of the resin composition, silicone-based surfactants and fluorine-based surfactants are preferred, and from the viewpoint of reducing the effect of the oxygen concentration during the curing process on the YI value and total light transmittance, silicone-based surfactants are preferred. When a surfactant is used, the content thereof is preferably 0.001 to 5 parts by mass, and more preferably 0.01 to 3 parts by mass, based on 100 parts by mass of the polyimide precursor in the resin composition.
[0079] (Alkoxysilane compounds) When the polyimide film obtained from the resin composition of the present embodiment is used for a flexible substrate or the like, from the viewpoint of obtaining good adhesion between a support and the polyimide film in the production process, the resin composition of the present disclosure may contain 0.01 to 20 parts by mass of an alkoxysilane compound per 100 parts by mass of the polyimide precursor. By making the content of the alkoxysilane compound 0.01 parts by mass or more relative to 100 parts by mass of the polyimide precursor, good adhesion between the support and the polyimide film can be obtained. In addition, it is preferable that the content of the alkoxysilane compound is 20 parts by mass or less from the viewpoint of storage stability of the resin composition of the present disclosure. The content of the alkoxysilane compound is preferably 0.02 to 15 parts by mass, more preferably 0.05 to 10 parts by mass, and even more preferably 0.1 to 8 parts by mass, relative to 100 parts by mass of the polyimide precursor. By using the alkoxysilane compound, in addition to improving the adhesion, the coatability of the resin composition of the present disclosure is improved (suppression of streaks), and the effect of the oxygen concentration during curing on the YI value of the polyimide film can also be reduced.
[0080] Examples of the alkoxysilane compound include 3-ureidopropyltriethoxysilane, bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltripropoxysilane, γ-aminopropyltributoxysilane, γ-aminoethyltriethoxysilane, γ-aminoethyltripropoxysilane, γ-aminoethyltributoxysilane, γ-aminobutyltriethoxysilane, γ-aminobutyltrimethoxysilane, γ-aminobutyltripropoxysilane, γ-aminobutyltributoxysilane, phenylsilanetriol, trimethoxyphenylsilane, trimethoxy(p-tolyl)silane, diphenylsilanediol, dimethoxydiphenylsilane, diethoxydiphenylsilane, dimethoxydi-p-tolylsilane, triphenylsilanol, and compounds having the following structure: [ka] The alkoxysilane compounds may be used alone or in combination of two or more.
[0081] <<Method for producing resin composition>> In one aspect of the present embodiment, a method for producing a resin composition includes the steps of: synthesizing a resin using one selected from the group consisting of the following as a main solvent; These include N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, gamma-butyrolactone, gamma-valerolactone, hexamethylphosphoric amide, dimethylsulfoxide, sulfolane, picoline, and pyridine. In one embodiment, a method for producing a resin composition includes preparing a solvent including a primary solvent and a co-solvent. In one embodiment, the method for producing the resin composition includes the steps of: preparing a resin composition by adding a co-solvent after synthesis of the resin and before filtration; A cosolvent having a Hansen solubility parameter of: δD=16.5~18.9 δP = 0.1 to 8.2 δH=1.1~5.5 Includes.
[0082] The method for producing the resin composition in the present embodiment is not particularly limited, and can be, for example, by the following steps. Resin synthesis process This step is a step of synthesizing a resin (in one embodiment, a polyimide / polyimide precursor) using, as a main solvent, one selected from the group consisting of N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, γ-butyrolactone, γ-valerolactone, hexamethylphosphoric amide, dimethyl sulfoxide, sulfolane, picoline, and pyridine.
[0083] Synthesis of Polyimide / Polyimide Precursor The polyimide / polyimide precursor of the present embodiment can be synthesized by polycondensation reaction of polycondensation components including acid dianhydride and diamine. Also, the polyimide / polyimide precursor of the present disclosure may be synthesized by adding a silicon-containing compound as a polycondensation component. It is preferable to use the silicon-containing compound purified by the method described below. In a preferred embodiment, the polycondensation component comprises an acid dianhydride, a diamine, and a silicon-containing compound. The polycondensation reaction is preferably carried out in a suitable solvent. Specifically, for example, a method may be used in which a predetermined amount of a diamine component and a silicon-containing compound are dissolved in a solvent, and then a predetermined amount of an acid dianhydride is added to the resulting diamine solution and stirred. The imidization in synthesizing a polyimide may be thermal imidization or chemical imidization using an imidization catalyst. The acid dianhydride, diamine and silicon-containing compound are the same as those described above.
[0084] The molar ratio of acid dianhydride to diamine when synthesizing a polyimide / polyimide precursor is preferably in the range of acid dianhydride:diamine=100:90 to 100:110 (0.90 to 1.10 molar parts of diamine per 1 molar part of acid dianhydride), and more preferably in the range of 100:92 to 100:101 (0.92 to 1.01 molar parts of diamine per 1 molar part of acid dianhydride), from the viewpoints of increasing the molecular weight of the resin composition, which is the polyimide precursor, and of the slit coating properties of the resin composition.
[0085] The weight average molecular weight of the polyimide / polyimide precursor can be controlled by adjusting the types of acid dianhydride, diamine and silicon-containing compound, the molar ratio of the acid dianhydride to the diamine, the addition of an end-capping agent, adjusting the reaction conditions, etc. The closer the molar ratio of the acid dianhydride component to the diamine component is to 1:1 and the smaller the amount of end-capping agent used, the higher the molecular weight of the polyimide precursor can be.
[0086] It is recommended to use high-purity products as the acid dianhydride component and the diamine component. The purity is preferably 98% by mass or more, more preferably 99% by mass or more, and even more preferably 99.5% by mass or more, respectively. The acid dianhydride component and the diamine component can also be highly purified by reducing the water content in the component. When multiple types of acid dianhydride components and / or multiple types of diamine components are used, it is preferable that the acid dianhydride components as a whole and the diamine components as a whole have the above-mentioned purity, and it is more preferable that all types of acid dianhydride components and diamine components used have the above-mentioned purity.
[0087] <Synthesis solvent for polyimide / polyimide precursor> The synthesis solvent for polyimide / polyimide precursor is not particularly limited as long as it can dissolve the acid dianhydride component, the diamine component, and the resulting polyimide / polyimide precursor, and can give a high molecular weight polymer. In one embodiment, the main solvent and / or the co-solvent of the present disclosure can be used as a synthesis solvent for polyimide / polyimide precursor. That is, the main solvent or the co-solvent of the present disclosure can be used alone as a synthesis solvent, or the main solvent and the co-solvent of the present disclosure can be used in combination as a mixed solvent.
[0088] The main solvent that can be used as the synthesis solvent preferably includes at least one selected from the group consisting of, for example, N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, γ-butyrolactone, γ-valerolactone, hexamethylphosphoric amide, dimethylsulfoxide, sulfolane, picoline, and pyridine. Co-solvents that can be used as synthesis solvents include, for example, n-butylbenzene, n-butyl benzoate, and ethoxybenzene.
[0089] The main solvent and the co-solvent that can be used as the synthesis solvent are the same as those described above. When a mixed solvent obtained by mixing a main solvent and a co-solvent is used as a synthesis solvent, the mass ratio of main solvent:co-solvent is preferably 10:90 to 90:10.
[0090] The water content in the synthesis solvent is preferably, for example, 3,000 ppm by mass or less in order to allow the polycondensation reaction to proceed smoothly. In the resin composition of the present disclosure, the content of molecules with a weight average molecular weight of less than 1,000 is preferably less than 5% by mass. The presence of molecules with a molecular weight of less than 1,000 in the resin composition of the present disclosure is believed to be due to the moisture content of the solvent and raw materials (acid dianhydride and diamine) used during synthesis. In other words, it is believed that the acid anhydride groups of some acid dianhydride monomers are hydrolyzed by moisture to become carboxyl groups, and remain in a low molecular weight state without becoming high molecular weight. Therefore, the less moisture content of the solvent used in the polycondensation reaction, the more preferable. The water content in the synthesis solvent is preferably 3,000 ppm by mass or less, more preferably 1,000 ppm by mass or less. Similarly, the water content in the raw material is preferably 3,000 ppm by mass or less, more preferably 1,000 ppm by mass or less.
[0091] The moisture content of the synthetic solvent is considered to be related to the grade of the solvent used (dehydrating grade, general-purpose grade, etc.), the solvent container (bottle, 18L can, canister, etc.), the storage condition of the synthetic solvent (whether rare gas is enclosed, etc.), the time from opening to use (whether it is used immediately after opening, or after aging after opening, etc.), etc. It is also considered to be related to the rare gas replacement of the reactor before synthesis, the presence or absence of rare gas circulation during synthesis, etc. Therefore, when synthesizing a polyimide precursor, it is recommended to use high-purity raw materials, to use a solvent with a low water content, and to take measures to prevent moisture from the environment from being mixed into the system before and during the reaction.
[0092] When each polycondensation component is dissolved in the synthesis solvent, heating may be performed as necessary. From the viewpoint of obtaining a polyimide precursor having a high degree of polymerization, the reaction temperature during the synthesis of the polyimide precursor may be preferably 0° C. to 120° C., 40° C. to 100° C., or 60° C. to 100° C. The polymerization time during the synthesis of the polyimide precursor may be preferably 1 to 100 hours, or 2 to 10 hours. The reaction temperature during polyimide synthesis may be preferably 130 to 200° C., 150 to 190° C., or 160 to 180° C. The polymerization time during polyimide synthesis may be preferably 1 to 100 hours, or 2 to 10 hours. By setting the polymerization time to 1 hour or more, a polyimide precursor / polyimide having a uniform degree of polymerization can be obtained, and by setting the polymerization time to 100 hours or less, a polyimide precursor / polyimide having a high degree of polymerization can be obtained.
[0093] The resin composition of the present embodiment may contain any other polyimide precursor in addition to the polyimide / polyimide precursor of the present embodiment. However, the mass ratio of the any polyimide / polyimide precursor is preferably 30 mass% or less, more preferably 10 mass% or less, based on the total amount of the polyimide / polyimide precursor in the resin composition of the present disclosure, from the viewpoint of reducing the oxygen dependency of the YI value and total light transmittance of the polyimide film.
[0094] The polyimide precursor in this embodiment may be partially imidized (partially imidized). By partially imidizing the polyimide precursor, the viscosity stability during storage of the resin composition of the present disclosure can be improved. In the case where the polyimide precursor is partially imidized, the imidization rate is preferably 5% or more, more preferably 8% or more, and preferably 90% or less, more preferably 80% or less, and even more preferably 70% or less, from the viewpoint of balancing the solubility of the polyimide precursor in the resin composition of the present disclosure and the storage stability of the solution. This partial imidization is obtained by heating the polyimide precursor to dehydrate and ring-close it. The heating for partial imidization can be carried out at a temperature of preferably 120 to 200° C., more preferably 150 to 185° C., and even more preferably 150 to 180° C., for preferably 15 minutes to 20 hours, and more preferably 30 minutes to 10 hours.
[0095] The polyimide / polyimide precursor obtained by the above reaction may be heated with N,N-dimethylformamide dimethyl acetal or N,N-dimethylformamide diethyl acetal to esterify a part or all of the carboxylic acid, and the resulting product may be used as the polyimide precursor of this embodiment. The viscosity stability during storage can be improved by the esterification. These ester-modified polyamic acids can also be obtained by reacting the above-mentioned acid dianhydride component with one equivalent of a monohydric alcohol relative to the acid anhydride group, and a dehydration condensing agent such as thionyl chloride or dicyclohexylcarbodiimide, in that order, and then condensing the resulting mixture with a diamine component.
[0096] Synthesis of Polyimide The synthesis of the polyimide of the present embodiment may include a thermal imidization step, in which an azeotropic solvent, such as a co-solvent of the present embodiment, such as toluene, may be used as the thermal imidization solvent, but the azeotropic solvent is usually removed (under reduced pressure) at the end of the thermal imidization step. In a more preferred embodiment of polyimide synthesis, the acid dianhydride component and the diamine component are dissolved in the above-mentioned synthesis solvent, an azeotropic solvent such as toluene is added, and water generated during imidization is removed from the system to produce a polyimide solution (also called polyimide varnish) containing polyimide and solvent. By performing (reduced pressure) distillation using a cosolvent as the azeotropic solvent, the content of the cosolvent is usually 5% by mass or less relative to 100% by mass of the resin composition, which is preferable because it provides the effects of this embodiment (such as improved filterability). Here, the reaction conditions are not particularly limited, but for example, the reaction temperature is 0° C. to 190° C., and the reaction time is 3 to 72 hours. In one embodiment, when the diamine component contains a sulfone group, in order to sufficiently proceed with the reaction, it is preferable to heat the reaction at 180° C. for about 12 hours. In addition, it is preferable to conduct the reaction in an inert atmosphere such as argon or nitrogen.
[0097] Purification of silicon-containing compounds The resin composition of the present embodiment may be produced by polycondensation reaction of polycondensation components including an acid dianhydride, a diamine, and a silicon-containing compound. As a method for reducing the total amount of cyclic silicon-containing compounds contained in the resin composition of the present embodiment, for example, the silicon-containing compounds are purified before polycondensation reaction to reduce the total amount of cyclic silicon-containing compounds. Alternatively, the resin composition may be purified after the polycondensation reaction of the present disclosure to reduce the total amount of cyclic silicon-containing compounds.
[0098] As a method for purifying a silicon-containing compound, for example, stripping can be performed while blowing an inert gas, such as nitrogen gas, into the silicon-containing compound in an arbitrary vessel. The stripping temperature is preferably 200°C or higher and 300°C or lower, more preferably 220°C or higher and 300°C or lower, and even more preferably 240°C or higher and 300°C or lower. The lower the stripping vapor pressure, the more preferable, and it is 1000 Pa or less, more preferably 300 Pa or less, even more preferably 200 Pa or less, and still more preferably 133.32 Pa (1 mmHg) or less. The stripping time is preferably from 4 hours to 12 hours, more preferably from 6 hours to 10 hours. By adjusting the conditions as described above, the cyclic silicon-containing compounds can be efficiently removed, and the total amount of the cyclic silicon-containing compounds can be controlled within a preferred range (in one embodiment, 1000 ppm or less based on the total amount of the silicon-containing compounds and the cyclic silicon-containing compounds).
[0099] A process for preparing a resin composition This step is performed after the step of synthesizing the resin described above, and before filtration, a solvent having a Hansen solubility parameter of: δD=16.5~18.9 δP = 0.1 to 8.2 δH=1.1~5.5 This is a process for preparing a resin composition. One embodiment of the resin composition of the present disclosure is used for displays, and from the viewpoint of productivity, filtration is performed to remove impurities, etc., so the resin composition of the present disclosure is required to have good filterability. The filterability of the resin composition of the present disclosure is improved by adding a solvent (in one embodiment, a co-solvent) that satisfies the above-mentioned specific Hansen solubility parameter before filtration to dilute a solution (in one embodiment, a polyimide / polyimide precursor solution or varnish) containing the resin of the present disclosure and a solvent (in one embodiment, a main solvent and / or a co-solvent).
[0100] The solvent to be added to the polyimide / polyimide precursor solution for dilution is not particularly limited as long as it satisfies the above-mentioned specific Hansen solubility parameters. In one embodiment, the cosolvent of the present disclosure can be used as a dilution solvent for the polyimide / polyimide precursor solution, and the description of the cosolvent is the same as above. These co-solvents may be used alone or in combination of two or more. A specific example of a composition containing a co-solvent is a mixed solvent of n-butylbenzene and ethoxybenzene, etc. The mass ratio of n-butylbenzene to ethoxybenzene may be, for example, n-butylbenzene:ethoxybenzene=10:90 to 90:10, and preferably 50:50. In one aspect, the co-solvents of the present disclosure may be used as synthesis solvents or diluent solvents. Examples of cosolvents that can be used as dilution solvents include n-butylbenzene, cyclopropene, cyclopentene, ethylbenzene methyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, tert-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, t-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, amylbenzene, butoxybenzene, benzyl isobutyl ether, t-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cineole, Preferred examples of the benzenediamine include cyclohexylbenzene, isobutyl benzoate, ethyl benzoate, propyl benzoate, diphenylacetylene, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate, benzyl benzoate, 2-methyltetrahydrofuran, cyclopentyl methyl ether, p-xylene, isopropylbenzene, d-limonene, toluene, styrene, a-methylstyrene, 2-methylcyclohexanone, 3-methylcyclohexanone, 2-vinyltoluene, isophorone, diisodecyl phthalate, propylbenzene, isobutylbenzene, 4-methylstyrene, 2-ethylstyrene, 2-isopropylstyrene, isopropyl benzoate, 4-t-butylstyrene, cycloheptanone, 4-ethylstyrene, 4-isopropylstyrene, 2-propylstyrene, n-butyl benzoate, and dibutyl sebacate.
[0101] Preparation of Resin Composition When the synthesis solvent (in one embodiment, a main solvent and / or a co-solvent) used in synthesizing the polyimide precursor is the same as the solvent (in one embodiment, a co-solvent) contained in the polyimide / polyimide precursor solution when diluting the polyimide / polyimide precursor solution, the synthesized polyimide / polyimide precursor solution can be used as it is as a resin composition. If necessary, the resin composition may be prepared by adding any solvent and one or more additional components to the polyimide precursor and stirring and mixing at a temperature range of room temperature (in one embodiment, 25°C) to 80°C. This stirring and mixing may be performed using an appropriate device such as a Three-One Motor (manufactured by Shinto Chemical Co., Ltd.) equipped with stirring blades, a planetary centrifugal mixer, etc. If necessary, the resin composition may be heated to 40°C to 100°C.
[0102] On the other hand, when the synthesis solvent (in one embodiment, the main solvent and / or the co-solvent) used when synthesizing the polyimide / polyimide precursor is different from the solvent (in one embodiment, the co-solvent) contained when diluting the polyimide / polyimide precursor solution, the polyimide / polyimide precursor may be isolated by removing the solvent in the synthesized polyimide precursor solution by an appropriate method such as reprecipitation, solvent distillation, etc. Next, a desired solvent and additional components as necessary may be added to the isolated polyimide precursor at a temperature range of room temperature (25°C) to 80°C, and the mixture may be stirred and mixed to prepare a resin composition.
[0103] After preparing the resin composition as described above, the resin composition may be heated, for example, at 130 to 200°C for 5 minutes to 2 hours to dehydrate and imidize a part of the polyimide precursor to an extent that the polymer does not precipitate (partial imidization). The imidization rate can be controlled by controlling the heating temperature and heating time. By partially imidizing the polyimide precursor, the viscosity stability during storage of the resin composition can be improved.
[0104] From the viewpoint of slit coating performance, the solution viscosity of the resin composition is preferably 500 to 100,000 mPa·s, more preferably 1,000 to 50,000 mPa·s, and even more preferably 3,000 to 20,000 mPa·s. Specifically, the viscosity is preferably 500 mPa·s or more, more preferably 1,000 mPa·s or more, and even more preferably 3,000 mPa·s or more in order to prevent leakage from the slit nozzle.The viscosity is preferably 100,000 mPa·s or less, more preferably 50,000 mPa·s or less, and even more preferably 20,000 mPa·s or less in order to prevent clogging of the slit nozzle.
[0105] Regarding the solution viscosity of the resin composition during polyimide / polyimide precursor synthesis, if the value is higher than the above range, stirring during synthesis tends to be difficult. However, even if the solution becomes highly viscous during synthesis (1000 mPa·s or higher in this disclosure), it is possible to obtain a resin composition with a viscosity that is easy to handle by adding a solvent after the reaction is completed and stirring. The solution viscosity of the resin composition in this embodiment is a value measured at 23° C. using an E-type viscometer (for example, VISCONICEHD, manufactured by Toki Sangyo Co., Ltd.).
[0106] From the viewpoint of viscosity stability during storage of the resin composition, the water content of the resin composition of this embodiment is preferably 3,000 ppm by mass or less, more preferably 2,500 ppm by mass or less, even more preferably 2,000 ppm by mass or less, still more preferably 1,500 ppm by mass or less, particularly preferably 1,000 ppm by mass or less, particularly preferably 500 ppm by mass or less, particularly preferably 300 ppm by mass or less, and particularly preferably 100 ppm by mass or less.
[0107] The polyimide / polyimide precursor may be synthesized in a main solvent and a co-solvent may be added before filtration to obtain a resin composition, or the polyimide / polyimide precursor may be synthesized in a mixed solvent of a main solvent and a co-solvent to obtain a resin composition.
[0108] A step of preparing a solvent containing a main solvent and a co-solvent. This step is a step of preparing a solvent containing a main solvent and a co-solvent. The preparation conditions of the solvent are the same as those described above for the main solvent and the co-solvent. The solvent may be used in the synthesis of the polyimide / polyimide precursor or may be used to dilute the polyimide / polyimide precursor solution before filtration. The resin composition is filtered by setting a membrane filter (pore size 0.5 μm) in a stainless steel holder with a tank, pouring in the varnish, sealing it, and filtering with air gas under pressure (about 0.3 MPa).
[0109] <Polyimide film and its manufacturing method> A polyimide film (hereinafter, also referred to as a polyimide resin film) can be provided using the resin composition of the present embodiment. A method for producing a polyimide resin film according to one aspect of this embodiment includes a coating step of coating the resin composition of this embodiment on a surface of a support. In one embodiment, a method for producing a polyimide resin film includes a film forming step of heating a resin composition to form a polyimide resin film. In one embodiment, a method for producing a polyimide resin film includes a peeling step of peeling the polyimide resin film from a support. In one embodiment, the method for producing a polyimide resin film includes, prior to the peeling step, an irradiation treatment of irradiating the polyimide resin film with a laser from the support side.
[0110] <Coating process> The coating step is a step of coating the resin composition of the present embodiment onto the surface of a support. The support is not particularly limited as long as it has heat resistance against the heating temperature in the film formation process after the coating process and has good releasability in the peeling process. Examples of the support include glass substrates (e.g., alkali-free glass substrates); silicon wafers; resin substrates such as PET (polyethylene terephthalate), OPP (oriented polypropylene), polyethylene glycol terephthalate, polyethylene glycol naphthalate, polycarbonate, polyimide, polyamideimide, polyetherimide, polyetheretherketone, polyethersulfone, polyphenylenesulfone, and polyphenylenesulfide; and metal substrates such as stainless steel, alumina, copper, and nickel.
[0111] When a thin-film polyimide molded product is to be formed, for example, a glass substrate or a silicon wafer is preferred, and when a thick-film or sheet-like polyimide molded product is to be formed, a support made of, for example, PET (polyethylene terephthalate), OPP (oriented polypropylene), etc. is preferred.
[0112] Generally, the coating method includes a coating method using a doctor blade knife coater, an air knife coater, a roll coater, a rotary coater, a flow coater, a die coater, a bar coater, etc. Application methods such as slit coating, spin coating, spray coating, dip coating, etc.; Examples of printing techniques include screen printing and gravure printing. The resin composition of the present embodiment is preferably applied by slit coating. The thickness of the coating film (referred to as film thickness) should be appropriately adjusted depending on the desired thickness of the polyimide film and the content of the polyimide precursor in the resin composition, but is preferably about 1 to 1,000 μm. The temperature in the coating step may be room temperature, or the resin composition may be heated to, for example, 40° C. to 80° C. in order to reduce the viscosity and improve workability.
[0113] Optional drying process The coating step may be followed by a drying step, or the drying step may be omitted and the process may proceed directly to the next film formation step (heating step). The drying step is carried out for the purpose of removing the organic solvent from the resin composition. When carrying out the drying step, for example, a suitable device such as a hot plate, a box-type dryer, a conveyor-type dryer, or a reduced pressure dryer can be used. The temperature in the drying step is preferably 80°C to 200°C, and more preferably 100°C to 150°C. The pressure in the drying step is preferably 40 Pa to 140 Pa, and more preferably 60 Pa to 120 Pa. The drying step is preferably carried out for 1 minute to 10 hours, more preferably 3 minutes to 1 hour. In this manner, a coating film containing a polyimide precursor is formed on the surface of the support.
[0114] <Film formation process> Next, a film forming step (hereinafter also referred to as a heating step) is carried out. The film-forming step is a step in which the organic solvent contained in the coating film obtained in the coating step is removed by heating, and the imidization reaction of the polyimide precursor in the coating film is advanced to form a polyimide resin film. As the heating method, hot air drying, infrared heater, hot air drying and infrared heater, etc. can be used. Far infrared rays can also be used as infrared rays. The heating step can be performed using an apparatus such as an inert gas oven, a hot plate, a box-type dryer, a conveyor-type dryer, etc. The heating step can be performed simultaneously with the drying step, or both steps can be performed sequentially.
[0115] The heating step may be carried out in an air atmosphere, but from the viewpoints of safety and obtaining a polyimide film with good transparency, low retardation in the thickness direction (Rth) and low YI value, it is preferable to carry out the heating step in an inert gas atmosphere, such as nitrogen or argon. The heating temperature may be appropriately set depending on the type of polyimide precursor and the type of solvent in the resin composition, but is preferably 250° C. to 550° C., more preferably 300° C. to 450° C. If the temperature is 250° C. or higher, the imidization proceeds well, and if the temperature is 550° C. or lower, inconveniences such as a decrease in transparency and a decrease in heat resistance of the obtained polyimide film can be avoided. The heating time is preferably about 0.1 to 10 hours.
[0116] In this embodiment, the oxygen concentration of the ambient atmosphere in the heating step is preferably 2,000 ppm by mass or less, more preferably 300 ppm by mass or less, and even more preferably 10 ppm by mass or less, from the viewpoint of a low YI value and transmittance of the resulting polyimide film. By carrying out heating in an atmosphere having an oxygen concentration of 2,000 mass ppm or less, the YI value of the resulting polyimide film can be made 16 or less.
[0117] <Peeling process> In the peeling step, the polyimide resin film on the support is peeled off after being cooled to, for example, about 25° C. (room temperature) to 50° C. The peeling step may, for example, be the following treatments (1) to (4).
[0118] (1) After preparing a construct containing a polyimide resin film / support by the above-mentioned method, a laser is irradiated from the support side of the construct to ablate the interface between the support and the polyimide resin film, thereby peeling off the polyimide resin (in one embodiment, an irradiation treatment). The type of laser includes a solid (YAG) laser, a gas (UV excimer) laser, etc. It is preferable to use a spectrum with a wavelength of 308 nm, etc. (see JP-T-2007-512568 and JP-T-2012-511173, etc.). The irradiation treatment is a treatment in which a laser is irradiated onto the polyimide resin film from the support side. From the viewpoint of the refractive index difference between the front and back of the resulting polyimide resin film, it is preferable to carry out an irradiation treatment prior to the peeling step.
[0119] (2) A treatment in which a release layer is formed on the support before the resin composition is applied to the support, and then a structure including a polyimide resin film / release layer / support is obtained, and the polyimide resin film is peeled off. Examples of the release layer include Parylene (registered trademark, manufactured by Japan Parylene LLC) and tungsten oxide; release agents such as vegetable oil-based, silicone-based, fluorine-based, and alkyd-based release agents may also be used (see JP 2010-067957 A and JP 2013-179306 A, etc.). The treatment (2) and the laser irradiation of the treatment (1) may be used in combination.
[0120] (3) A process in which an etchable metal substrate is used as a support to obtain a structure including a polyimide resin film / support, and then the metal is etched with an etchant to obtain a polyimide resin film. Examples of metals that can be used include copper (specifically, electrolytic copper foil "DFF" manufactured by Mitsui Mining & Smelting Co., Ltd.), aluminum, etc. Examples of etchants that can be used include ferric chloride for copper, and dilute hydrochloric acid for aluminum.
[0121] (4) After obtaining a construct including a polyimide resin film / support by the above-mentioned method, a process is performed in which an adhesive film is attached to the surface of the polyimide resin film, the adhesive film / polyimide resin film is separated from the support, and then the polyimide resin film is separated from the adhesive film.
[0122] Among these peeling treatments, from the viewpoints of the refractive index difference between the front and back of the resulting polyimide resin film, a low YI value, and the elongation of the resin film, treatment (1) or (2) is preferred, and treatment (1) is more preferred. In the process (3), when copper is used as the support, the YI value of the resulting polyimide resin film tends to be large and the elongation of the resin film tends to be small. This is thought to be due to the effect of copper ions.
[0123] The thickness of the polyimide film obtained after the peeling step is not limited, but is preferably 1 to 200 μm, and more preferably 5 to 100 μm.
[0124] <Polyimide resin film (resin film after curing of resin composition)> The structure of the polyimide contained in the polyimide resin film formed from the polyimide precursor of the present embodiment is represented by the following general formula (20): [ka] {In general formula (20), P1 and P2 are the same as P1 and P2 in general formula (1) or general formula (2), or P3 and P4 in general formula (2), and m is a positive integer.} Preferred P1 and P2 in the general formula (20) are also preferred in the polyimide of the general formula (20) for the same reasons as in the general formula (1) or (2). The number m of repeating units in the general formula (20) is not particularly limited, but may be an integer of 2-150.
[0125] The structure of the polyimide contained in the polyimide resin film formed from the polyimide precursor composition of the present embodiment is represented by the following general formula (21): [ka] {In general formula (21), P3 and P4 are the same as P1 and P2 in general formula (1), P5 and P6 in general formula (21) are the same as P3 and P4 in general formula (2), and m and n are positive integers.} Preferred P3 and P4, and P5 and P6 in general formula (21) are also preferred in the polyimide of general formula (21) for the same reasons as preferred P1 and P2 in general formula (1) and preferred P3 and P4 in general formula (2). The numbers of repeating units m and n in the general formula (21) are not particularly limited, but may be integers of 2-150.
[0126] The polyimide resin film of the present embodiment has the following characteristics: -YI (yellowness index) 16 or less (film thickness 10μm equivalent) -Degassing start temperature (TDS) is 420℃ or higher Residual stress is 35MPa or less (under nitrogen atmosphere), or Rth (thickness retardation) is 100nm or less (10μm film thickness equivalent) It is preferable that the following is satisfied. This makes the polyimide resin film of this embodiment suitable for use in displays (particularly displays using LTPS (low temperature polysilicon) and LTPO (low temperature polycrystalline oxide)).
[0127] <<Uses of Polyimide Film>> The polyimide film obtained from the resin composition of the present embodiment can be used, for example, as a semiconductor insulating film, a thin film transistor liquid crystal display (TFT-LCD) insulating film, an electrode protective film, and also as a transparent substrate for display devices such as flexible displays, liquid crystal displays, organic electroluminescence displays, field emission displays, and electronic paper. The polyimide film obtained from the resin composition of the present embodiment can be suitably used as a display including a thin film transistor (TFT) substrate and / or a color filter substrate. In particular, the polyimide film obtained from the resin composition of this embodiment can be suitably used as a thin film transistor (TFT) substrate, a color filter substrate, a touch panel substrate, and a substrate for a transparent conductive film (ITO, indium thin oxide) in the production of flexible devices. Examples of flexible devices to which the polyimide film of the present embodiment can be applied include TFT devices for flexible displays, flexible solar cells, flexible touch panels, flexible lighting, flexible batteries, flexible printed circuit boards, flexible color filters, and surface cover lenses for smartphones.
[0128] The process of forming a TFT on a flexible substrate using a polyimide film is typically carried out at a wide temperature range of 150° C. to 650° C. Specifically, when manufacturing a TFT device using amorphous silicon, a process temperature of 250° C. to 350° C. is generally required, and the polyimide film of this embodiment must be able to withstand this temperature, so specifically, it is necessary to appropriately select a polymer structure having a glass transition temperature and a thermal decomposition onset temperature equal to or higher than the process temperature.
[0129] When fabricating a TFT device using a metal oxide semiconductor (such as IGZO), a process temperature of 320°C to 400°C is generally required. The polyimide film of this embodiment must be able to withstand this temperature, and therefore it is necessary to appropriately select a polymer structure having a glass transition temperature and a thermal decomposition onset temperature that are equal to or higher than the maximum temperature of the TFT fabrication process.
[0130] When manufacturing a TFT device using LTPS (low temperature polysilicon) or LTPO (low temperature polycrystalline oxide), a process temperature of 380°C to 520°C is generally required. Since the polyimide film of this embodiment needs to be able to withstand such temperatures, it is necessary to appropriately select a glass transition temperature and a thermal decomposition onset temperature that are equal to or higher than the maximum temperature of the TFT manufacturing process. On the other hand, due to the thermal history, the optical properties (particularly the light transmittance, retardation properties and YI value) of the polyimide film tend to decrease as it is exposed to a high-temperature process. However, the polyimide obtained from the polyimide precursor of the present embodiment has good optical properties even after being subjected to a thermal history.
[0131] As examples of applications of the polyimide film of this embodiment, a display and a method for producing a laminate will be described below.
[0132] <Display manufacturing method> A method for producing a display according to one aspect of this embodiment includes a coating step of coating the resin composition of this embodiment onto a surface of a support. In one embodiment, the method for producing a display includes a film-forming step of heating a resin composition to form a polyimide resin film. In one embodiment, the method for producing a display includes an element forming step of forming an element on a polyimide resin film. In one embodiment, the method for producing a display includes a peeling step of peeling the polyimide resin film on which the elements are formed from the support. The display of the present disclosure comprises elements formed on the polyimide resin film of the present disclosure.
[0133] In the display manufacturing method of the present disclosure, the preferred specific procedures for the coating step and the film forming step are the same as those described above with respect to the polyimide film manufacturing method.
[0134] In the display manufacturing method of the present disclosure, the element forming step is a step of forming an element on a polyimide resin film. Examples of elements in the display of the present disclosure include organic EL elements, liquid crystal elements, and micro LED elements. The element formation process can be carried out under known manufacturing conditions, for example, through an organic EL substrate manufacturing process, a sealing substrate manufacturing process, and an assembly process, which will be described later.
[0135] In the display manufacturing method of the present disclosure, the peeling step is a step of peeling the polyimide resin film and the element from the support. In the display manufacturing method of the present disclosure, the preferred specific procedure of the peeling step is the same as that described above with respect to the polyimide film manufacturing method.
[0136] - Flexible OLED display manufacturing example FIG. 1 is a schematic diagram showing the structure above a polyimide substrate of a top-emission type flexible organic EL display as an example of the display of this embodiment. The organic EL structure 25 in FIG. 1 will be described. For example, an organic EL element 250a that emits red light, an organic EL element 250b that emits green light, and an organic EL element 250c that emits blue light are arranged in a matrix as one unit, and a partition (bank) 251 defines the light-emitting region of each organic EL element. Each organic EL element is composed of a lower electrode (anode) 252, a hole transport layer 253, a light-emitting layer 254, and an upper electrode (cathode) 255. On the lower layer 2a that shows a CVD multi-layer film (multi-barrier layer) made of silicon nitride (SiN) or silicon oxide (SiO), a TFT 256 (selected from low-temperature polysilicon (LTPS) or metal oxide semiconductor (IGZO, etc.)) for driving the organic EL element, an interlayer insulating film 258 having a contact hole 257, and a lower electrode 259 are provided in plurality. The organic EL elements are sealed with a sealing substrate 2b, and a hollow portion 261 is formed between each organic EL element and the sealing substrate 2b.
[0137] The manufacturing process of a flexible organic EL display includes a step of preparing a polyimide film on a glass substrate support, a step of preparing an organic EL substrate shown in FIG. 1 on the upper part of the polyimide film, a step of preparing a sealing substrate, an assembly step of bonding the two substrates together, and a peeling step of peeling the organic EL display prepared on the polyimide film from the glass substrate support. The organic EL substrate manufacturing step, the sealing substrate manufacturing step, and the assembly step can be performed using well-known manufacturing steps. An example is given below, but the present invention is not limited to this. The step of preparing the polyimide film and the peeling step are the same as the above-mentioned polyimide film coating step, film formation step, and peeling step.
[0138] For example, referring to FIG. 1, first, a polyimide film is prepared on a glass substrate support by the above-mentioned method, and a multi-barrier layer (lower substrate 2a in FIG. 1) consisting of a multi-layer structure of silicon nitride (SiN) and silicon oxide (SiO) is prepared on the upper part by a CVD method or a sputtering method, and a metal wiring layer for driving a TFT is prepared on the upper part by using a photoresist or the like. An active buffer layer such as SiO is prepared on the upper part by a CVD method, and a TFT device (TFT 256 in FIG. 1) such as a metal oxide semiconductor (IGZO) or low temperature polysilicon (LTPS) is prepared on the upper part. After preparing a TFT substrate for a flexible display, an interlayer insulating film 258 having a contact hole 257 is formed by a photosensitive acrylic resin or the like. An ITO film is formed by a sputtering method or the like, and a lower electrode 259 is formed so as to be paired with the TFT.
[0139] Next, after forming partitions (banks) 251 using photosensitive polyimide or the like, a hole transport layer 253 and a light-emitting layer 254 are formed in each space partitioned by the partitions. An upper electrode (cathode) 255 is formed so as to cover the light-emitting layer 254 and partitions (banks) 251. Thereafter, using a fine metal mask or the like as a mask, an organic EL material that emits red light (corresponding to the organic EL element 250a that emits red light in FIG. 1), an organic EL material that emits green light (corresponding to the organic EL element 250b that emits green light in FIG. 1), and an organic EL material that emits blue light (corresponding to the organic EL element 250c that emits blue light in FIG. 1) are deposited by a known method to prepare an organic EL substrate. The organic EL substrate is sealed with a sealing film or the like (sealing substrate 2b in FIG. 1), and the device above the polyimide substrate is peeled off from the glass substrate support by a known peeling method such as laser peeling, thereby preparing a top-emission type flexible organic EL display. When the polyimide of this embodiment is used, a see-through type flexible organic EL display can be produced. A bottom emission type flexible organic EL display may also be produced by a known method.
[0140] Flexible LCD manufacturing example A flexible liquid crystal display can be produced using the polyimide film of this embodiment. As a specific production method, a polyimide film is produced on a glass substrate support by the above-mentioned method, and a TFT substrate made of, for example, amorphous silicon, metal oxide semiconductor (IGZO, etc.), and low-temperature polysilicon is produced by using the above-mentioned method. Separately, a polyimide film is produced on a glass substrate support according to the coating process and film formation process of this embodiment, and a color filter glass substrate (CF substrate) equipped with a polyimide film is produced using a color resist or the like according to a known method. A seal material made of a thermosetting epoxy resin or the like is applied by screen printing to one of the TFT substrate and the CF substrate in a frame-shaped pattern lacking a liquid crystal injection port, and spherical spacers made of plastic or silica having a diameter equivalent to the thickness of the liquid crystal layer are scattered on the other substrate.
[0141] Next, the TFT substrate and the CF substrate are bonded together, and the sealing material is cured. Then, liquid crystal material is injected into the space surrounded by the TFT substrate, the CF substrate, and the sealing material by decompression, a thermosetting resin is applied to the liquid crystal injection port, and the liquid crystal material is sealed by heating to form a liquid crystal layer. Finally, the glass substrate on the CF side and the glass substrate on the TFT side are peeled off at the interface between the polyimide film and the glass substrate by laser irradiation or the like, thereby producing a flexible liquid crystal display.
[0142] In particular, in this embodiment, a process is included in which a laminate including a polyimide resin film / inorganic film with a YI (yellowness index) of 16 or less (calculated at a film thickness of 10 μm) is heated at 260° C. or higher or 430° C. or higher, thereby making it possible to manufacture a display having sufficient characteristics required for a display (a balance between characteristics such as glass transition temperature when cured at 260° C. or higher or 430° C. or higher, low YI, Young's modulus, chemical resistance, and heat resistance of the laminate).
[0143] Furthermore, in this embodiment, the polyimide film has the following properties: -Degassing start temperature (TDS) is 420℃ or higher Residual stress is 35MPa or less (under nitrogen atmosphere), or Rth (thickness retardation) is 100nm or less (10μm film thickness equivalent) By satisfying the above, it is possible to manufacture a display having sufficient characteristics as the characteristics required for a display as described above. Therefore, the resin composition of the present embodiment is suitably used for producing a display substrate, preferably a flexible display substrate.
[0144] <<Method for manufacturing laminate>> A method for producing a laminate according to one aspect of this embodiment includes a coating step of coating the resin composition of this embodiment onto a surface of a support. In one embodiment, the method for producing a laminate includes a film forming step of heating a resin composition to form a polyimide resin film. In one embodiment, the method for producing a laminate includes an element forming step of forming an element on the polyimide resin film. In one embodiment, the method for producing a laminate includes a step of peeling off the polyimide resin film on which the element is formed from the support. The laminate of the present disclosure is formed by forming an element on the polyimide resin film of the present disclosure. In one embodiment, the laminate includes a polyimide resin film and an inorganic film. The inorganic film may be a SiO2 film, a SiN X Membrane and SiON X Membranes and the like.
[0145] In the method for producing a laminate according to the present disclosure, the preferred specific procedures for the coating step, film formation step, element formation step and peeling step are the same as those described for the above-mentioned method for producing a polyimide film and method for producing a display.
[0146] Examples of the element in the laminate of the present disclosure include an organic EL element, a liquid crystal element, and a micro LED element. In the method for producing a laminate according to the present disclosure, a peeling step may be optionally carried out. EXAMPLES
[0147] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples and comparative examples, but the present invention is not limited to these examples and comparative examples.
[0148] <<Measurement and evaluation methods of physical properties>> <Boiling point of cosolvent (℃)> The boiling points of the co-solvents are listed in Table 1 with reference to the websites of the reagent manufacturers. For solvents listed on the website of Tokyo Chemical Industry Co., Ltd. (hereinafter also referred to as TCI), the boiling points listed on TCI were adopted as the boiling points of the co-solvents in the present disclosure. When two or more co-solvents are used in combination, the boiling point of the solvent with the highest boiling point is listed in Table 1.
[0149] How to calculate SP value The values obtained by the following method were defined as the Hansen solubility parameters (HSPiP) of the primary solvent and the cosolvent of the present disclosure; 1) Using the application available for download at the following website; https: / / www.hansen-solubility.com / buy-HSPiP-software.php 2) Using HSPiP 5th Edition or later application 3) For solvents included in the application (included in Solvent Optimizer), the solubility parameters (δD, δP, δH values) listed there were used. 4) For solvents not included in the application, the simplified molecular input line entry system (SMILES) notation was obtained from the structure of the solvent, and the SMILES was entered in the "DIY" section of the application to calculate the solubility parameters (δD, δP, and δH values).
[0150] <Yellowness (YI)> The resin compositions of the Examples and Comparative Examples were applied to an alkali-free glass substrate (hereinafter also referred to as "glass substrate" or simply "substrate") having dimensions of 100 mm length x 100 mm width x 0.5 mm thickness in an area 5 mm inward from the edge of the glass substrate, so that the film thickness after curing would be 10 μm. A slit coater (LC-R300G, manufactured by SCREEN Finetech Solutions) was used for application. The solvent was removed from the obtained glass substrate with the coating film using a reduced pressure dryer (manufactured by Tokyo Ohka Kogyo Co., Ltd.) under conditions of 80°C, 100 Pa, and 30 minutes, to obtain a glass substrate having a coating film of the resin composition.
[0151] The glass substrate having the obtained coating film of the resin composition was heated in an oven (INH-9N1, manufactured by Koyo Thermo Systems Co., Ltd.) until the temperature reached 100° C. Examples in which an acid anhydride other than ODPA was used as the acid anhydride 1 include Examples 1 to 115, even-numbered Examples 151 to 162, even-numbered Examples 171 to 184, odd-numbered Examples 191, 193, and Examples 210 to 223, and even-numbered Examples 228 and Examples 229 to 234, and In Comparative Examples 2 to 4, which are comparative examples in which an acid anhydride other than ODPA was used as the acid anhydride 1, samples were prepared by heating at 430° C. for 30 minutes in a nitrogen atmosphere (oxygen concentration 300 ppm or less).
[0152] The obtained sample was used as a specimen and the yellowness index (YI) value was measured using a spectrophotometer (manufactured by Nippon Denshoku Industries Co., Ltd., model name "SE600") with a D65 light source. The results obtained are expressed as the following values converted into a film thickness of 10 μm: Examples 1 to 115, the even-numbered examples among Examples 151 to 162, the even-numbered examples among Examples 171 to 184, the odd-numbered examples among Examples 191, 193, and Examples 210 to 223, Example 228, and the even-numbered examples among Examples 229 to 234, and Comparative Examples 2 to 4 were evaluated according to the following criteria. A: YI is 10 or less "Excellent" B: YI is between 10 and 13. "Excellent" C: YI is between 13 and 16. "Good" D: YI is over 16 "bad" If the evaluation is A, B, or C, the resin composition can be suitably used as a resin composition for forming a display.
[0153] Examples in which ODPA was used as acid anhydride 1, that is, Examples 116 to 151, the odd-numbered examples among Examples 153 to 162, the odd-numbered examples among Examples 163 to 171, and the odd-numbered examples among Examples 173 to 184, Examples 185 to 190, Example 192, Examples 194 to 210, and the even-numbered examples among Examples 212 to 223, and the odd-numbered examples among Examples 224 to 227, and Examples 229 to 234, and Comparative Example 1 in which ODPA was used as acid anhydride 1, were heated in an oven (INH-9N1, manufactured by Koyo Thermo Systems Co., Ltd.) at 260°C for 30 minutes in an air atmosphere to form a polyimide resin film sample on a glass substrate.
[0154] The obtained sample was used as a specimen and the yellowness index (YI) value was measured using a spectrophotometer (manufactured by Nippon Denshoku Industries Co., Ltd., model name "SE600") with a D65 light source. The results obtained are expressed as the following values converted into a film thickness of 10 μm: Examples 116 to 151, the odd-numbered examples among Examples 153 to 162, the odd-numbered examples among Examples 163 to 171, and Examples 173 to 184, the even-numbered examples among Examples 185 to 190, Example 192, Examples 194 to 210, and Examples 212 to 223, the odd-numbered examples among Examples 224 to 227, and Examples 229 to 234, and Comparative Example 1 were evaluated according to the following criteria. A: YI is 3 or less "Excellent" B: YI is between 3 and 5. "Excellent" C: YI is between 5 and 10. "Good" D: YI is over 10 "Poor" If the evaluation is A, B, or C, the resin composition can be suitably used as a resin composition for forming a substrate for a color filter.
[0155] <Filterability> An Advantech membrane filter (mesh size: 0.5 μm) was set in an Advantech stainless steel holder with tank (model number KST-47), and the varnish prepared as described below was poured into it. The filter was then sealed and pressure-filtered with air gas at a pressure of 0.3 MPa. The filtrate was received in a container, and the amount of filtration per hour was measured 30 minutes after the start of filtration to calculate the filtration rate. "5": Filtration speed is 10g / Hr or more "Excellent" "4": Filtration rate is 5g / Hr or more but less than 10g / Hr "Excellent" "3": Filtration rate is 3g / Hr or more but less than 5g / Hr. "Good" "2": Filtration rate is 1g / Hr or more but less than 3g / Hr. "Fair" "1": Filtration rate is less than 1g / Hr "Not acceptable" If the evaluation score is "2" or higher, the resin composition can be suitably used for forming a display.
[0156] <Filtration speed> Pressure filtration was carried out in the same manner as described in <Filterability>, the amount of filtration was measured 5 hours after the start of filtration, and the filtration rate 5 hours after the start of filtration was calculated. "a": Filtration rate is 5g / Hr or more (Excellent) "b": Filtration rate is 3g / Hr or more but less than 5g / Hr (Excellent) "c": Filtration rate is 1g / Hr or more but less than 3g / Hr (good) "d": Filtration rate is less than 1g / Hr (poor) If the evaluation is a, b, or c, the resin composition can be suitably used as a resin composition for forming a display.
[0157] Example 1 In a separable flask equipped with a stirring rod and a Dean-Stark tube and reflux tube, NMP (200g) as the main solvent, toluene (150g), BAFL (13.52g; 38.8mmol) as the diamine, and SiDA (7g) as the Si element-containing monomer were added while stirring, followed by PMDA (3.27g; 15mmol), BPDA (4.41g; 15mmol), and BPAF (9.2g; 20mmol) as the acid dianhydrides at room temperature. The internal temperature was then raised to 180°C and the mixture was heated to reflux at 180°C for 3 hours to perform imidization. Then, the mixture was cooled to room temperature, and pPD (6.29 g; 58.2 mmol) was added as a diamine with stirring, followed by BPAF (22.9 g; 50.0 mmol) as an acid dianhydride. The mixture was stirred at room temperature for 24 hours, and the toluene was removed under reduced pressure to obtain an NMP solution (hereinafter also referred to as varnish) of a partially imidized (L / M=60 / 40 mol%) polyimide precursor (hereinafter also referred to as PAI). The obtained varnish was stored in a freezer (set temperature: -20°C). When evaluating its performance, it was thawed and n-butylbenzene was added as a co-solvent to make it 30 wt% of the total solvent and to make the solid content 15 wt%.
[0158] Examples 2 to 5 A varnish was obtained in the same manner as in Example 1, except that the content of the co-solvent was changed as shown in Table 1.
[0159] Examples 6 to 18 and 24 A varnish was obtained in the same manner as in Example 1, except that the main solvent shown in Table 1 was used instead of NMP as the main solvent.
[0160] Example 19 In a separable flask equipped with a stirring rod, a Dean-Stark tube and a reflux tube, NMP (200g) as the main solvent, toluene (150g), APAB (4.6g; 20mmol) as the diamine, and SiDA (7g) were added with stirring while introducing nitrogen gas, followed by CpODA (38.44g; 100mmol) as the acid dianhydride at room temperature. The internal temperature was then raised to 180°C and heated to reflux at 180°C for 3 hours to carry out imidization. The mixture was then cooled to room temperature, and APAB (17.43 g; 76.5 mmol) was added as a diamine with stirring. The mixture was stirred at room temperature for 24 hours, and the toluene was removed under reduced pressure to obtain an NMP solution of a partially imidized (L / M=20 / 80 mol%) polyimide precursor (PAI) (hereinafter also referred to as a varnish). The obtained varnish was stored in a freezer (set temperature: -20°C). When evaluating its performance, it was thawed and n-butylbenzene was added as a co-solvent to make it 30 wt% of the total solvent and to make the solid content 15 wt%.
[0161] Example 20 A varnish was obtained in the same manner as in Example 19, except that the diamine was changed as shown in Table 1.
[0162] Example 21 In a separable flask equipped with a stirring rod and a Dean-Stark tube and reflux tube, NMP (200g) as the main solvent, toluene (150g), BAFL (13.52g; 38.8mmol), pPD (6.29g; 58.2mmol), and SiDA (7g) as diamines were added with stirring while introducing nitrogen gas, followed by PMDA (3.27g; 15mmol), BPDA (4.41g; 15mmol), and BPAF (32.09g; 70mmol) as acid dianhydrides at room temperature. The internal temperature was then raised to 180°C and the mixture was heated to reflux at 180°C for 3 hours to perform imidization. The mixture was then cooled to room temperature, stirred at room temperature for 24 hours, and the toluene was removed under reduced pressure to obtain a polyimide (hereinafter also referred to as PI) NMP solution (hereinafter also referred to as varnish). The obtained varnish was stored in a freezer (set temperature: -20°C), and when evaluating its performance, it was thawed and n-butylbenzene was added as a co-solvent to make it 30 wt% of the total solvent and to make the solid content 15 wt%.
[0163] Example 22 Except for changing the amount of PMDA to 3.71 g, the same components as in Example 21 were added at room temperature, and the mixture was stirred at room temperature for 24 hours. The mixture was then heated to 180°C and the toluene was distilled off under reduced pressure in the same manner as in Example 1 to obtain an NMP solution (hereinafter also referred to as varnish) of a polyimide precursor (hereinafter also referred to as PAA).
[0164] Example 23 In a separable flask equipped with a stirring rod and a Dean-Stark tube and reflux tube, NMP (200g) as the main solvent, toluene (80g), BAFL (13.52g; 38.8mmol) and SiDA (7g) as diamines were added while stirring, followed by PMDA (3.27g; 15mmol), BPDA (4.41g; 15mmol), and BPAF (9.2g; 20mmol) as acid dianhydrides at room temperature. The internal temperature was then raised to 180°C and the mixture was heated to reflux at 180°C for 3 hours to perform imidization. The mixture was then cooled to room temperature, and n-butylbenzene (70 g) was added as a co-solvent to serve as a synthesis solvent. pPD (6.29 g; 58.2 mmol) was added as a diamine with stirring, followed by BPAF (22.9 g; 50.0 mmol) as an acid dianhydride. The mixture was stirred at room temperature for 24 hours, and the toluene was removed under reduced pressure to obtain a solution of a partially imidized (L / M=60 / 40 mol%) polyimide precursor (PAI) dissolved in NMP (hereinafter also referred to as a varnish). The obtained varnish was stored in a freezer (set temperature: -20°C). When evaluating its performance, it was thawed and n-butylbenzene was added as a co-solvent to make it 30 wt% of the total solvent and to make the solid content 15 wt%.
[0165] Examples 25 to 38, 40, 42, 44, 46, 48, 50 to 59, 61, 63, 65, 67, 69, 71, 73 to 77, 79, 81 to 97, 99, 101, 103, 105, 107, 109, and 111 to 114 A varnish was obtained in the same manner as in Example 1, except that a cosolvent shown in Table 1 was used instead of n-butylbenzene.
[0166] Example 39 In a separable flask equipped with a stirring rod and a Dean-Stark tube and reflux tube, NMP (400g) as the main solvent, toluene (250g), TFMB (12.81g; 40mmol) as the diamine, and SiDA (7.7g) as the Si element-containing monomer were added while stirring, followed by PMDA (3.27g; 15mmol) and 6FDA (6.66g; 15mmol) as the acid dianhydride at room temperature. The internal temperature was then raised to 180°C and heated to reflux at 180°C for 3 hours to perform imidization. The mixture was then cooled to room temperature, and TFMB (18.25 g; 57 mmol) was added as a diamine with stirring, followed by PMDA (15.27 g; 70.0 mmol) as an acid dianhydride. The mixture was stirred at room temperature for 24 hours, and the toluene was removed under reduced pressure to obtain an NMP solution (hereinafter also referred to as varnish) of a partially imidized (L / M=70 / 30 mol%) polyimide precursor (hereinafter also referred to as PAI). The obtained varnish was stored in a freezer (set temperature: -20°C). When evaluating its performance, it was thawed and n-butylbenzene was added as a co-solvent to make it 30 wt% of the total solvent and to make the solid content 10 wt%.
[0167] Examples 41, 43, 45, 47, 49, 60, 62, 64, 66, 68, 70, 72, 78, 80, 98, 100, 102, 104, 106, 108, 110, 115, 152, 154, 156, 158, 160, 162, 172, 174, 176, 178, 180, 182, 184, 191, 193, 211, 213, 215, 217, 219, 221, 223, 228, 230, 232, and 234 A varnish was obtained in the same manner as in Example 39, except that a cosolvent shown in Table 1 was used instead of n-butylbenzene.
[0168] Example 116 In a separable flask equipped with a stirring rod, a Dean-Stark tube and a reflux tube, NMP (200g) as the main solvent, toluene (150g), 4,4-DAS (12.4g; 50mmol), 3,3-DAS (7.4g; 30mmol), and SiDA (7g) as diamines were added with stirring while introducing nitrogen gas, followed by ODPA (31.0g; 100mmol) as an acid dianhydride at room temperature. The internal temperature was then raised to 180°C and heated to reflux at 180°C for 3 hours to carry out imidization. The mixture was then cooled to room temperature, and 4,4-DAS (14.42 g; 58.1 mmol) and 3,3-DAS (9.61 g; 38.7 mmol) were added as diamines with stirring. The mixture was stirred at room temperature for 24 hours, and the toluene was removed by distillation under reduced pressure to obtain an NMP solution of a partially imidized (L / M=80 / 20 mol%) polyimide precursor (PAI) (hereinafter also referred to as varnish). The obtained varnish was stored in a freezer (set temperature: -20°C). When evaluating its performance, it was thawed and ethoxybenzene was added as a co-solvent to make it 30 wt% of the total solvent and to make the solid content 15 wt%.
[0169] Examples 117 to 123, 128 to 133, and 137 A varnish was obtained in the same manner as in Example 116, except that the main solvent shown in Table 1 was used instead of NMP as the main solvent.
[0170] Examples 124 to 127 A varnish was obtained in the same manner as in Example 116, except that the content of the co-solvent was changed as shown in Table 1.
[0171] Example 134 In a separable flask equipped with a stirring rod, a Dean-Stark tube and a reflux tube, GBL (200g) as the main solvent, toluene (150g), 4,4-DAS (14.42g; 58.1mmol) and 3,3-DAS (9.61g; 38.7mmol) as diamines, and SiDA (7g) were added with stirring while introducing nitrogen gas, followed by ODPA (31.02g; 100mmol) as an acid dianhydride at room temperature. The internal temperature was then raised to 180°C and heated to reflux at 180°C for 3 hours to carry out imidization. The mixture was then cooled to room temperature, stirred at room temperature for 24 hours, and the toluene was removed under reduced pressure to obtain a polyimide (hereinafter also referred to as PI) GBL solution (hereinafter also referred to as varnish). The obtained varnish was stored in a freezer (set temperature: -20°C), and when evaluating its performance, it was thawed and ethoxybenzene was added as a co-solvent to make it 30 wt% of the total solvent and to make the solid content 15 wt%.
[0172] Example 135 The same components as in Example 134 were added at room temperature, and the mixture was stirred at room temperature for 24 hours. The procedure was the same as in Example 116, except for the heating step at 180°C and the removal of toluene by distillation under reduced pressure, to obtain a GBL solution (hereinafter also referred to as varnish) of polyimide precursor (hereinafter also referred to as PAA).
[0173] Example 136 In a separable flask equipped with a stirring rod, a Dean-Stark tube and a reflux tube, GBL (200g) as the main solvent, toluene (80g), 4,4-DAS (12.4g; 50mmol), 3,3-DAS (7.4g; 30mmol) and SiDA (7g) as diamines were added with stirring while introducing nitrogen gas, followed by ODPA (31.02g; 100mmol) as an acid dianhydride at room temperature. The internal temperature was then raised to 180°C and heated to reflux at 180°C for 3 hours to carry out imidization. The mixture was then cooled to room temperature, and ethoxybenzene (70 g) was added as a co-solvent to serve as a synthesis solvent. Then, 4,4-DAS (2.01 g; 8.1 mmol) and 3,3-DAS (2.16 g; 8.7 mmol) were added as diamines with stirring. The mixture was stirred at room temperature for 24 hours, and the toluene was removed under reduced pressure to obtain a solution of a partially imidized (L / M=80 / 20 mol%) polyimide precursor (PAI) dissolved in GBL (hereinafter also referred to as varnish). The obtained varnish was stored in a freezer (set temperature: -20°C). When evaluating its performance, it was thawed and ethoxybenzene was added as a co-solvent to make it 30 wt% of the total solvent and to make the solid content 15 wt%.
[0174] Examples 138 to 151, 153, 155, 157, 159, 161, 163 to 171, 173, 175, 177, 179, 181, 183, 185 to 190, 192, 194 to 210, 212, 214, 216, 218, 220, 222, and 224 to 227 A varnish was obtained in the same manner as in Example 116, except that GBL was used instead of NMP as the main solvent, and a cosolvent shown in Table 1 was used instead of ethoxybenzene as the cosolvent.
[0175] Comparative Example 1 A 2 L separable 3-neck flask equipped with a stainless steel anchor stirrer was fitted with a ball condenser equipped with a water separation trap. 67.96g (360mmol) of bis-(3,4-dicarboxyphenyl)ether dianhydride (manufactured by Manac Co., Ltd.) (hereinafter abbreviated as ODPA), 165.24g (180mmol) of diaminosiloxane compound BY16-853U (manufactured by Toray Dow Corning Co., Ltd.) (amino group equivalent 459, hereinafter abbreviated as BY16), 4.33g (43mmol) of γ-valerolactone, 6.83g (86mmol) of pyridine, 235.2g of n-butyl benzoate, and 100.8g of γ-butyrolactone were charged. After stirring at room temperature under a nitrogen atmosphere at 180 rpm for 30 minutes, the mixture was heated to 180°C and stirred for 1 hour. Water was removed during the reaction. Then, after cooling, 22.34g (72mmol) of ODPA, 63.15g (216mmol) of 1,3-bis(3-aminophenoxy)benzene (manufactured by Mitsui Chemicals, Inc.) (hereinafter abbreviated as APB), 10.52g (36mmol) of 1,3-bis(4-aminophenoxy)benzene (manufactured by Wakayama Seika Kogyo Co., Ltd.) (hereinafter abbreviated as TPE-R), and a mixed solvent of 140g of n-butyl benzoate as a co-solvent and 60g of γ-butyrolactone as a main solvent were added to the second stage, and the mixture was reacted for 5 hours at 180°C while stirring at 180 rpm. By removing reflux materials such as water from the system during the reaction, an organosilicon group-containing polyimide solution with a concentration of 41% by mass was obtained. 325 g of n-butyl benzoate was added to 900 g of the synthesized organosilicon group-containing polyimide solution to obtain a composition, the content of which was 77.9 wt %. The resin composition of Comparative Example 1 corresponds to the composition described in Patent Document 1.
[0176] Comparative Example 2 A varnish was obtained in the same manner as in Example 1, except that sulfolane was used as the co-solvent.
[0177] Comparative Example 3 A varnish was obtained in the same manner as in Example 1, except that n-butylbenzene was not used as a co-solvent.
[0178] Comparative Example 4 A varnish was obtained in the same manner as in Example 1, except that cyclohexanone was used instead of NMP as the main solvent.
[0179] Comparative Example 5 A varnish was obtained in the same manner as in Example 1, except that the amounts of the main solvent and the co-solvent were changed to the content ratios shown in Table 1. In addition, the note *1 in Table 1 indicates that in Examples 24 and 137, the mixing ratio of the main solvent was 50 wt% / 50 wt%, and the note *2 indicates that in Examples 25 and 138, the mixing ratio of the cosolvent was 50 wt% / 50 wt%.
[0180] (Components used in the Examples and Comparative Examples) <Acid dianhydride> BPAF: 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride PMDA: Pyromellitic anhydride BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride ODPA: 4,4'-oxydiphthalic dianhydride (bis-(3,4-dicarboxyphenyl) ether dianhydride) CpODA: Norbornane 2-spiro-α-cyclopentanone-α'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic dianhydride 6FDA: 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride
[0181] <Diamine> BAFL: 9,9-bis(4-aminophenyl)fluorene pPD: p-phenylenediamine mPD: m-phenylenediamine 3,3-DAS: 3,3-diaminodiphenyl sulfone 4,4-DAS: 4,4-diaminodiphenyl sulfone APAB: 4-aminophenyl-4-aminobenzoate TFMB: 2,2'-bis(trifluoromethyl)benzidine APB: 1,3-bis(3-aminophenoxy)benzene TPE-R: 1,3-bis(4-aminophenoxy)benzene
[0182] <Si-containing monomer> SiDA: (In general formula (17), L1 and L2 are amino groups (-NH2), R1 is a trimethylene group (-CH2CH2CH2-), R2 and R3 are methyl groups, (i is a positive integer, j and k are 0, and the compound has a functional group equivalent of 2200) General formula (17): [ka]
[0183] <Main solvent> NMP: N-methyl-2-pyrrolidone DMF: N,N-dimethylformamide DMAc: N,N-dimethylacetamide 1,3-Dimethylimidazolidinone Tetramethylurea 3-Methoxy-N,N-dimethylpropanamide 3-Butoxy-N,N-dimethylpropanamide γ-Butyrolactone γ-Valerolactone Hexamethylphosphoric amide Dimethyl sulfoxide Sulfolane Picholine Pyridine
[0184] <Co-solvent> n-Butylbenzene Cyclopropene Cyclopentene Ethylbenzene methyl sulfide Cyclohexene Diethyl sulfide Cycloheptane Ethylbenzene 1,8-Cineole Dipentene Tributyl borate Benzyl methacrylate Fran Phenylacetylene Ethoxybenzene Dihexyl Phthalate Methyl benzoate 1-Menthone Dioctyl adipate 1-Menthyl acetate Diisononyl adipate t-Butylbenzene 1,4-Cineole Benzyl methyl ether Isopropoxybenzene t-Butoxybenzene Propoxybenzene Benzaldehyde dimethyl acetal Amylbenzene Butoxybenzene Benzyl isobutyl ether t-Butyl benzoate Benzyl Butyl Ether Benzaldehyde diethyl acetal Hexylbenzene Cyclohexylbenzene Isobutyl Benzoate Ethyl Benzoate Propyl benzoate Diphenylacetylene Ethyl cinnamate Diethylhexyl phthalate Diisoheptyl Phthalate Diisononyl Phthalate Benzyl benzoate 2-Methyltetrahydrofuran Cyclopentyl methyl ether p-Xylene Isopropyl benzene d-Limonene toluene styrene a-Methylstyrene 2-Methylcyclohexanone 3-Methylcyclohexanone 2-Vinyltoluene Isophorone Diisodecyl Phthalate Propylbenzene Isobutylbenzene 4-Methylstyrene 2-Ethylstyrene 2-Isopropylstyrene Isopropyl Benzoate 4-t-Butylstyrene Cycloheptanone 4-Ethylstyrene 4-Isopropylstyrene 2-Propylstyrene n-Butyl benzoate Dibutyl Sebacate
[0185] <Polymer type name> PAA: Polyimide precursor PI: Polyimide PAI: Partially imidized polyimide precursor
[0186] [Table 1-1]
[0187] [Table 1-2]
[0188] [Table 1-3]
[0189] [Table 1-4]
[0190] [Table 1-5]
[0191] [Table 1-6]
[0192] [Table 1-7]
[0193] [Table 1-8]
[0194] [Table 1-9]
[0195]
Table 1-10
[0196]
Table 1-11
[0197]
Table 1-12
[0198]
Table 1-13
[0199]
Table 1-14
[0200]
Table 1-15
[0201]
Table 1-16
[0202]
Table 1-17
[0203]
Table 1-18
[0204]
Table 1-19
[0205] [Table 1-20]
[0206] [Table 1-21]
[0207] [Table 1-22]
[0208] [Table 1-23]
[0209] [Table 1-24]
[0210] As shown in Table 1, the polyimides obtained from the resin compositions of the Examples had both low YI (transparency) and filterability properties compared to the Comparative Examples, and were excellent in the properties required for display applications. The resin composition of Comparative Example 1 corresponds to the composition described in Patent Document 1, but the low YI (transparency), filterability and filtration rate were D, “1”, and “d”, and the respective properties could not be achieved simultaneously. The resin composition of Comparative Example 2 is a resin composition in which a cosolvent whose Hansen solubility parameter does not satisfy the specific range was used. Although the low YI (transparency) and filterability were A in terms of the YI value, the filterability and filtration rate were rated as "1" and "d", respectively, and the respective properties were not compatible. The resin composition of Comparative Example 3 is a resin composition without using a cosolvent, and although the low YI (transparency) and filterability were A in terms of the YI value, the filterability and filtration rate were "1" and "d", respectively, and the respective properties could not be achieved at the same time. Comparative Example 3, in which a cosolvent was not used, did not achieve the effects of this embodiment (filterability, etc.). The resin composition of Comparative Example 4 is a resin composition in which a solvent other than a specific solvent selected from the group consisting of N-methyl-2-pyrrolidone (NMP) and the like is used as the main solvent, and the low YI (transparency) was D. In addition, in the resin composition of Comparative Example 4, polyimide polymer precipitated, and the filterability was poor at "1," so that all the characteristics could not be achieved at the same time. In Comparative Example 5, the content of the co-solvent n-butylbenzene was 55 wt % or more of the total solvent, and the YI value was A. However, the filterability was "1" and the filtration rate was "d," which were poor, and the respective characteristics could not be achieved simultaneously.
[0211] The reason for the deterioration of filterability in Comparative Examples 3 and 4 is unclear, but it is believed to be due to the presence of a trace amount of ultra-high molecular weight polymer. When the solubility of the polymer is calculated from the viewpoint of the Hansen solubility parameter, it is close to the SP value used in the main solvent, and it is found that the polymer has a property of being easily dissolved in the main solvent. However, the cosolvents in Comparative Examples 3 and 4 had poor filterability despite their high solubility in the polymer. It is generally known that the solubility of a polymer decreases as the molecular weight increases. For this reason, it is believed that ultra-high molecular weight polymers turn into a fine gel even in a good solvent, filling the pores inside the filter paper and causing poor filterability. As a solution to this problem, a co-solvent is added as shown in the examples. The co-solvent in the examples is a poor solvent for the polymer from the viewpoint of the Hansen solubility parameter, but the solubility of the polymer can be maintained by adjusting the addition ratio with the main solvent, which is a good solvent. However, it is believed that the gel-like ultra-high molecular weight polymer, which is thought to be the cause of the deterioration of filterability, was condensed due to the influence of the cosolvent, which is a poor solvent. The condensed ultra-high molecular weight polymer remained on the surface of the filter paper and did not block the pores, which is why it is believed that filterability improved. In the present disclosure, a resin composition obtained by using a specific main solvent and a co-solvent having a Hansen solubility parameter within a specific range achieves both filterability and low YI (transparency) properties, and can be suitably used as a polyimide film applicable to display processes such as LTPS (low temperature polysilicon) and LTPO (low temperature polycrystalline oxide). [Explanation of symbols]
[0212] 2a Lower Board 2b Sealing substrate 25 Organic EL structure 250a Red light emitting organic EL element 250b Green light-emitting organic electroluminescence element 250c Blue light emitting organic electroluminescence element 251 Partition (bank) 252 Lower electrode (anode) 253 Hole transport layer 254 Light-emitting layer 255 Upper electrode (cathode) 256 TFT 257 Contact Hole 258 Interlayer insulating film 259 Lower Electrode 261 Hollow part
Claims
1. The following general formula (1): [Formula 1] {In the formula, P 1 represents a divalent organic group, P 2 represents a tetravalent organic group, and p represents a positive integer. And / or general formula (2): [chemical 2] {In the formula, P 3 represents a divalent organic group, P 4 represents a tetravalent organic group, and q represents a positive integer. and The following general formula (3): [C3] {In the formula, R 1 and R 2 each independently represents a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200. A resin composition comprising a resin having a structure derived from a silicon-containing compound represented by the formula: The solvent includes a main solvent and a co-solvent, The main solvent comprises at least one selected from the group consisting of: N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, γ-butyrolactone, γ-valerolactone, hexamethylphosphoric amide, dimethyl sulfoxide, sulfolane, picoline and pyridine The cosolvent has a Hansen solubility parameter of: δD=16.5~18.9 δP=0.1 to 8.2 δH=1.1 to 5.5 A resin composition, wherein the co-solvent is less than 50% by mass when the total amount of the solvent is taken as 100% by mass.
2. The Hansen solubility parameter of the cosolvent satisfies the following: δD=16.5~18.4 δP=0.1 to 5.6 δH=1.1 to 4.7 The resin composition according to claim 1.
3. The co-solvent may be n-butylbenzene, cyclopropene, cyclopentene, ethylbenzene methyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, t-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, t-butoxybenzene 3. The resin composition according to claim 1 or 2, comprising at least one selected from the group consisting of benzene, propoxybenzene, benzaldehyde dimethyl acetal, amylbenzene, butoxybenzene, benzyl isobutyl ether, t-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene, isobutyl benzoate, ethyl benzoate, propyl benzoate, diphenylacetylene, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate, and benzyl benzoate.
4. The co-solvent may be n-butylbenzene, cyclopropene, cyclopentene, ethylbenzene methyl sulfide, cyclohexene, diethyl sulfide, cycloheptane, ethylbenzene, 1,8-cineole, dipentene, tributyl borate, benzyl methacrylate, furan, phenylacetylene, ethoxybenzene, dihexyl phthalate, methyl benzoate, 1-menthone, dioctyl adipate, 1-menthyl acetate, diisononyl adipate, t-butylbenzene, 1,4-cineole, benzyl methyl ether, isopropoxybenzene, t-butoxybenzene, propoxybenzene, benzaldehyde dimethyl acetal, amylbenzene, butoxybenzene, benzyl isobutyl ether, t-butyl benzoate, benzyl butyl ether, benzaldehyde diethyl acetal, hexylbenzene, cyclohexylbenzene, Isobutyl benzoate, ethyl benzoate, propyl benzoate, diphenylacetylene, ethyl cinnamate, diethylhexyl phthalate, diisoheptyl phthalate, diisononyl phthalate, benzyl benzoate, 2-methyltetrahydrofuran, cyclopentyl methyl ether, p-xylene, isopropylbenzene, d-limonene, styrene, a-methylstyrene, 2-methylcyclohexanone, 3-methylcyclohexanone, 2-vinyltoluene, isophorone, diisodecyl phthalate, propylbenzene, isobutylbenzene, 4-methylstyrene, 2-ethylstyrene, 2-isopropylstyrene, isopropyl benzoate, 4-t-butylstyrene, cycloheptanone, 4-ethylstyrene, 4-isopropylstyrene and 2-propylstyrene. The resin composition according to claim 1 or 2, which comprises at least one selected from the group consisting of styrene.
5. The resin composition according to claim 1 or 2, wherein the co-solvent has a boiling point of less than 250°C.
6. The resin composition according to claim 1 or 2, wherein the co-solvent comprises at least one selected from the group consisting of n-butylbenzene and ethoxybenzene.
7. The P 1 and / or P 3is represented by the following general formula (4): [C4] The resin composition according to claim 1 or 2, comprising a structural unit derived from:
8. The P 2 and / or P 4 is represented by the following general formula (5): [C5] The resin composition according to claim 1 or 2, comprising a structural unit derived from:
9. The P 1 and / or P 3 is represented by the following general formula (6): [C6] The resin composition according to claim 1 or 2, comprising a structural unit derived from:
10. The resin composition according to claim 1 or 2, wherein the co-solvent is present in an amount of 5% by mass or more and 40% by mass or less when the total amount of the solvent is taken as 100% by mass.
11. The resin composition according to claim 1 or 2, wherein the co-solvent is present in an amount of 5% by mass or more and 30% by mass or less when the total amount of the solvent is taken as 100% by mass.
12. The resin composition according to claim 1 or 2, which is used for a substrate of a flexible display.
13. A display comprising a thin film transistor (TFT) substrate and / or a color filter substrate using the resin composition according to claim 1 or 2.
14. The following general formula (1): [C7] {In the formula, P 1 represents a divalent organic group, P 2 represents a tetravalent organic group, and p represents a positive integer. And / or general formula (2): [C8] {In the formula, P 3represents a divalent organic group, P 4 represents a tetravalent organic group, and q represents a positive integer. and The following general formula (3): [C9] {In the formula, R 1 and R 2 each independently represents a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200. A method for producing a resin composition containing a resin having a structure derived from a silicon-containing compound represented by the formula (I) and a solvent, the method comprising the steps of: synthesizing the resin using, as a main solvent, at least one selected from the group consisting of N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), 1,3-dimethylimidazolidinone, tetramethylurea, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, γ-butyrolactone, γ-valerolactone, hexamethylphosphoric amide, dimethylsulfoxide, sulfolane, picoline, and pyridine; After synthesis of the resin, the resin has the following Hansen solubility parameters before filtration: δD=16.5~18.9 δP=0.1 to 8.2 δH=1.1 to 5.5 Adding a co-solvent to prepare a resin composition; A method for producing a resin composition.
15. A coating step of coating a surface of a support with the resin composition according to claim 1 or 2, or a resin composition obtained by the method according to claim 14; a film-forming step of heating the resin composition to form a polyimide resin film; a peeling step of peeling the polyimide resin film from the support; a step of irradiating the polyimide resin film with a laser from the support side prior to the peeling step.
16. A coating step of coating a surface of a support with the resin composition according to claim 1 or 2, or a resin composition obtained by the method according to claim 14; a film-forming step of heating the resin composition to form a polyimide resin film; an element forming step of forming an element on the polyimide resin film; a peeling step of peeling the polyimide resin film on which the element is formed from the support; A method for manufacturing a display comprising:
17. A coating step of coating a surface of a support with the resin composition according to claim 1 or 2, or a resin composition obtained by the method according to claim 14; a film-forming step of heating the resin composition to form a polyimide resin film; an element forming step of forming an element on the polyimide resin film; A method for producing a laminate, comprising:
18. A coating step of coating a surface of a support with the resin composition according to claim 1 or 2, or a resin composition obtained by the method according to claim 14; a film-forming step of heating the resin composition to form a polyimide resin film; an element forming step of forming an element on the polyimide resin film; peeling the polyimide resin film on which the elements are formed from the support; A method for producing a laminate, comprising:
19. The following general formula (1): [C10] {In the formula, P 1 represents a divalent organic group, P 2 represents a tetravalent organic group, and p represents a positive integer. And / or general formula (2): [C11] {In the formula, P 3 represents a divalent organic group, P 4 represents a tetravalent organic group, and q represents a positive integer. A structural unit represented by The following general formula (3): [C12] {In the formula, R 1 and R 2 each independently represents a monovalent aliphatic hydrocarbon group having 1 to 5 carbon atoms or a monovalent aromatic group having 6 to 10 carbon atoms, and m represents an integer of 1 to 200. A resin composition comprising a resin having a structure derived from a silicon-containing compound represented by the formula: The solvent comprises one or more mixed solvents, The resin composition, wherein the mixed solvent has a Hansen solubility parameter satisfying the following: δD=16.8~18.8 δP=6.8 to 9.8 δH=4.5 to 6.8
Citation Information
Patent Citations
Polyamide-imide insulating varnish and preparation method thereof
CN102559040A
Composition, coated film comprising the composition, laminate containing the coated film, and electronic equipment in which the laminate is incorporated
JP2010155895A
Cited By
Polyamic acid composition, production method for said polyamic acid composition, polyimide, polyimide film, laminate, and production method for said laminate
WO2026141464A1