Method for observing contact surface of rubber member
By using a transparent glass plate with a paper contact member and applying a median filter, the method enhances the accuracy of contact pressure distribution measurements on rubber members by correcting brightness distributions and converting them to pressure distributions.
Patent Information
- Application Number
- JP2023078350
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
AI Technical Summary
Existing methods for observing the contact surface of rubber members, such as tires, face challenges in accurately determining contact pressure distribution due to surface unevenness and interference from dirt or foreign objects, leading to unclear brightness differences and inaccurate pressure measurements.
A method involving a transparent glass plate with a paper contact member, where a rubber member is pressed against the paper, and images are taken from below the glass plate, using a pressure loading jig to apply varying pressures and apply a median filter to correct brightness distributions, converting brightness to pressure pixel-by-pixel to obtain accurate contact pressure distributions.
This method allows for a more precise determination of contact pressure distribution by minimizing the impact of surface unevenness and foreign objects, resulting in clearer and more accurate images of the contact surface.
Smart Images

Figure 2024162634000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for observing the contact surface of rubber members. [Background technology]
[0002] In the field of pneumatic tire (hereinafter referred to as "tire") design, the contact surface between a rubber member cut out from a tire and a glass plate is observed. For example, a rubber member is slid on a glass plate while changing temperature conditions, and the contact surface shape, contact area, or contact pressure distribution of the rubber member at each temperature is obtained, and the temperature dependency of the contact surface shape, etc. is investigated and utilized in the design.
[0003] Conventionally, methods for observing the contact surfaces of rubber members and the like have been known, such as those described in Patent Documents 1 and 2.
[0004] The method in Patent Document 1 involves placing a textured sheet with an uneven surface on top of a transparent plate, pressing a tire against the textured sheet to bring the tire and the uneven surface of the textured sheet into close contact, making the light reflectance different between the area where the tire and the uneven surface are in contact and the other areas so that the shape of the tire's contact surface can be seen, and then photographing that shape with a camera below the transparent plate.
[0005] In addition, the method of Patent Document 2 involves making light enter the interior of a transparent body and causing it to be totally reflected on the upper surface of the transparent body, so that when a rubber sample comes into contact with the upper surface of the transparent body, total reflection is no longer observed at the contact point, making it possible to identify the contact point when the transparent body is photographed with an imaging device.
[0006] However, in the method of using a textured sheet as in Patent Document 1, the unevenness on the surface of the textured sheet is relatively large, so the shape of the contact area between the tire and the uneven surface does not match the shape of the actual tire contact surface, making it difficult to observe the precise shape of the contact surface.
[0007] Furthermore, in the method of contacting a rubber sample with the upper surface of a transparent body as in Patent Document 2, there is a problem in that dirt, etc., adhering to the upper surface of the transparent body is captured in the image taken by the imaging device, making it difficult to distinguish between the contact area and the dirt, etc. In addition, with this method, light coming from above the upper surface of the transparent body also enters the imaging device, so there is a small difference in brightness between the contact area of the rubber sample and its surrounding area in the captured image, making it difficult to clearly distinguish the contact area of the rubber sample. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2003-14428 A [Patent Document 2] JP 2016-188767 A Summary of the Invention [Problem to be solved by the invention]
[0009] Recently, the applicant has been studying a new method for observing the contact surface of a rubber member, in particular a method for determining the contact pressure distribution on the contact surface. Specifically, this method involves placing a contact member such as paper on a transparent body such as a glass plate, pressing the rubber member from above the contact member, photographing the image of the pressed part from below the transparent body, and converting the brightness distribution of the photographed image into a contact pressure distribution. The contact pressure distribution also makes it possible to determine the contact surface shape, contact area, etc.
[0010] However, with this method, if the contact member is uneven or if there is a foreign object between the transparent body and the contact member, the brightness distribution of the captured image may be affected, making it impossible to obtain a correct contact pressure distribution.
[0011] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method that can obtain a more accurate contact pressure distribution on the contact surface of a rubber member. [Means for solving the problem]
[0012] The present invention includes the embodiments set forth below.
[0013] [1] A method for observing the contact surface of a rubber member, which involves pressing a rubber member against a contact member and taking an image of the contact surface between the rubber member and the contact member, comprising the steps of: placing the contact member on a transparent body; applying multiple levels of pressure from above the contact member using a pressure application tool and taking a first image from below the transparent body, which is an image with a luminance distribution when each pressure is applied; determining a relational equation between pressure and luminance for each pixel in the shooting range based on the first image for each pressure; pressing the rubber member from above the contact member and taking a second image from below the transparent body, which is an image with a luminance distribution; and obtaining a pressure distribution image, which is an image showing the contact pressure distribution at the contact surface between the rubber member and the contact member, by converting the luminance of the second image into pressure for each pixel based on the relational equation between pressure and luminance.
[0014] [2] A method for observing the contact surface of a rubber member described in [1], comprising applying a median filter to each of the first images to obtain respective corrected first images, and determining the relationship between pressure and brightness for each pixel in the shooting range based on the corrected first images for each pressure.
[0015] [3] The method for observing the contact surface of a rubber member according to [2], wherein the size of the median filter is 3 x 3 pixels.
[0016] [4] A method for observing the contact surface of rubber members described in [1], comprising applying a median filter to the pressure distribution image.
[0017] [5] The method for observing the contact surface of a rubber member described in [4], wherein the size of the median filter is 3 x 3 pixels, 5 x 5 pixels, or 7 x 7 pixels.
[0018] [6] A method for observing the contact surface of a rubber member described in any of [1] to [5], comprising the steps of: irradiating light onto the transparent body and causing total reflection inside the transparent body; applying pressure from above the contact member to press the contact member against the transparent body so as to prevent total reflection of light at the pressed location, thereby taking the first image; and pressing the rubber member from above the contact member to press the contact member against the transparent body so as to prevent total reflection of light at the pressed location, thereby taking the second image. Effect of the Invention
[0019] According to the above method, it is possible to obtain a more accurate contact pressure distribution on the contact surface of the rubber member. [Brief description of the drawings]
[0020] [Figure 1] FIG. [Diagram 2] Top view of the glass plate and the light guide. [Diagram 3] The light guide viewed from the glass plate side. [Figure 4] FIG. [Diagram 5] Photos taken during the pre-test. (a) is a photo taken when the applied pressure is 100 kPa. (b) is a photo taken when the applied pressure is 200 kPa. (c) is a photo taken when the applied pressure is 300 kPa. [Figure 6] Top view of the arrangement of pressure application jigs used in the pre-test. (a) is a diagram showing how pressure is applied to multiple locations using a circular pressure application jig. (b) is a diagram showing how pressure is applied to multiple locations using a rectangular pressure application jig. (c) is a diagram showing how pressure is applied to one location using a circular pressure application jig. (d) is a diagram showing how pressure is applied to one location using a rectangular pressure application jig. [Figure 7] A diagram showing an image of calculating the relationship between pressure and brightness for each pixel. [Figure 8](a) is a diagram showing the state in which the rubber member is pressed against the paper. (b) is an image acquired when pressing (a). [Figure 9] (a) is the second image. (b) is the pressure distribution image obtained by converting the brightness of (a) into pressure. [Figure 10] (a) is the first image. (b) is a close-up of a portion of the first image. (c) is the image in (b) after applying a 3x3 pixel median filter. (d) is the image in (b) after applying a 7x7 pixel median filter. [Figure 11] (a) is a pressure distribution image. (b) is an image of (a) applied with a 3x3 pixel median filter. (c) is an image of (a) applied with a 7x7 pixel median filter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The embodiments will be described with reference to the drawings. Note that the embodiments described below are merely examples, and any appropriate modifications that do not depart from the gist of the present invention are included in the scope of the present invention.
[0022] 1 includes a glass plate 11 as a transparent body, a holder 12 that holds a rubber member 16 above the glass plate 11, a camera 13 arranged below the glass plate 11, light guides 14 as illumination devices provided on both the left and right sides (both lateral sides) of the glass plate 11, and an analysis device 17 connected to the camera 13. The imaging device 10 is a device that places paper 15 on the glass plate 11, and uses the camera 13 to capture an image of the contact state between the rubber member 16 and the paper 15 from below when the rubber member 16 is pressed onto the paper 15.
[0023] The glass plate 11 is a colorless and transparent glass plate. The glass plate 11 is rectangular when viewed from above and is a glass plate with a constant thickness. The upper surface 11b and the lower surface 11c of the glass plate 11 are flat. The glass plate 11 has an area required for the rubber member 16 to slide thereon and a thickness (length in the vertical direction) that does not break when the rubber member 16 is pressed. The specific size of the glass plate 11 is not limited, but is, for example, a depth (length in the depth direction in FIG. 1, length in the vertical direction in FIG. 2) of 320 mm to 400 mm, a width (length in the left-right direction in FIG. 1 and FIG. 2) of 90 mm to 110 mm, and a thickness of 10 mm to 30 mm. The glass plate 11 may be a plate made of one piece of glass, or may be a plate having the above thickness obtained by overlapping two pieces of glass.
[0024] The surface roughness of the upper surface 11b, the lower surface 11c, and the side surface 11a of the glass plate 11 is preferably 0.01 μm to 0.12 μm in terms of arithmetic mean roughness Ra. The method for measuring the arithmetic mean roughness Ra is in accordance with JIS B0601:2013 (ISO 4287:187, Amd.1:2009).
[0025] The holding unit 12 holds a jig 21 to which a rubber member 16 is attached. The holding unit 12 can move in the depth direction, lateral direction, and up and down direction of the glass plate 11 based on instructions from a control unit (not shown). The rubber member 16 is pressed against the paper 15 placed on the glass plate 11 by lowering the holding unit 12. The magnitude of the load on the rubber member 16 is adjusted by the amount of lowering of the holding unit 12. In addition, a sliding test of the rubber member 16 is performed by moving the holding unit 12 in the depth direction. The moving speed of the holding unit 12, which is also the moving speed of the rubber member 16, is controllable.
[0026] Camera 13 is, for example, a CCD camera capable of taking multiple pictures in succession. The pictures (images) taken by camera 13 are, for example, digital images consisting of 256 levels of brightness, with white being 255 and black being 0. Camera 13 is oriented so as to take pictures of glass plate 11 from below. The shooting direction of camera 13 is a direction perpendicular to bottom surface 11c of glass plate 11 as shown in FIG. 1. However, the shooting direction of camera 13 may be a direction slightly inclined with respect to the direction perpendicular to bottom surface 11c of glass plate 11.
[0027] Analysis device 17 is composed of a PC (Personal Computer) in which a predetermined analysis program is installed. Although not shown, analysis device 17 is composed of a processing device that performs analysis, an input device for an operator to input data, a display device that displays the analysis results, etc. Analysis device 17 performs a predetermined analysis on the photograph (image) taken by camera 13.
[0028] 2 and 3, the light guide 14 has a bundled fiber 22 in which a number of optical fibers are bundled together, and a housing 23 that houses one end of the bundled fiber 22. The light guide 14 is an illumination device that transmits light emitted from a light source (not shown) such as an LED through the bundled fiber 22 to the inside of the housing 23 and emits the light to the outside from a slit 24 formed in the housing 23. The light emitted from the light guide 14 is, for example, white light. Furthermore, light of uniform brightness is emitted from the entire slit 24.
[0029] The light guides 14 on both the left and right sides of the glass plate 11 are arranged so as to irradiate light toward the glass plate 11. That is, the light emitted from the slits 24 of the housing 23 is arranged so as to be incident on the glass plate 11. The incident direction (the direction of the optical axis of the light) is perpendicular to the side surface 11a of the glass plate 11 and parallel to the upper surface 11b and the lower surface 11c of the glass plate 11. The light incident on the glass plate 11 from the light guides 14 on both the left and right sides is totally reflected on the surface of the glass plate 11. However, the light is totally reflected when the surface of the glass plate 11 is in contact with air. In the totally reflected region, the light incident on the glass plate 11 does not pass above the upper surface 11b of the glass plate 11 or pass below the lower surface 11c of the glass plate 11. The two-dot chain line drawn in the glass plate 11 in FIG. 1 represents the totally reflected light.
[0030] The slits 24 of the left and right light guides 14 extend in the depth direction (depth direction in FIG. 1, up and down direction in FIG. 2) parallel to the left and right side surfaces 11a of the glass plate 11. A constant gap is provided between the slits 24 and the side surfaces 11a of the glass plate 11. The length L1 of the gap in the left and right direction (see FIGS. 1 and 2) is constant and is 0.1 mm to 1.0 mm.
[0031] The thickness L2 (length in the vertical direction, see Figs. 1 and 3) of the slit 24 is thinner than the thickness of the glass plate 11, for example, 10% or less of the thickness of the glass plate 11. A specific value of the thickness of the slit 24 is, for example, 0.2 mm to 1.0 mm. It is preferable that the center position of the slit 24 in the thickness direction (vertical direction) coincides with the center position of the glass plate 11 in the thickness direction (vertical direction).
[0032] Further, the length L3 (see FIG. 2) of the slit 24 in the depth direction is shorter than the length L4 (see FIG. 2) of the glass plate 11 in the depth direction. Further, the lower limit of the length of the slit 24 in the depth direction is not limited, but is, for example, half the length of the glass plate 11 in the depth direction. A specific value of the length of the slit 24 in the depth direction is, for example, 180 mm to 220 mm.
[0033] The paper 15 placed on the glass plate 11 is a member (contact member) that the rubber member 16 comes into contact with. The paper 15 is a sheet-like material produced by agglutinating natural fibers such as those of plants, and a specific example is photographic printing paper. The paper 15 preferably has a smooth surface, high reflectance, is white, is as thin as possible while still ensuring adequate strength, and is homogeneous throughout. Specifically, the arithmetic mean roughness Ra of the surface of the paper 15 is preferably 0.1 μm to 2.0 μm. The whiteness of the surface of the paper 15 is preferably 85 to 102%. Here, the whiteness is a value determined by a diffuse illumination method (JISP8148) that complies with the international standard ISO whiteness (ISO12470). The thickness of the paper 15 is preferably 0.2 mm to 0.5 mm, and more preferably 0.2 mm to 0.3 mm.
[0034] Such paper 15 is cut to the same shape and size as glass plate 11. Then, the cut paper 15 is attached to the upper surface 11b of glass plate 11 with double-sided tape on the four sides of glass plate 11. The double-sided tape has enough adhesive strength to prevent paper 15 from shifting relative to glass plate 11 when rubber member 16 slides over paper 15. Paper 15 attached to glass plate 11 floats slightly above upper surface 11b of glass plate 11. Therefore, a thin air layer is formed between upper surface 11b of glass plate 11 and paper 15 attached thereto.
[0035] As described above, the light incident on the glass plate 11 is totally reflected by the surface of the glass plate 11 when the surface of the glass plate 11 is in contact with the air. However, when the rubber member 16 is pressed against the paper 15, the air layer between the glass plate 11 and the paper 15 becomes very thin under the contact surface between the rubber member 16 and the paper 15, or the glass plate 11 and the paper 15 come into close contact with each other. As a result, the light reflection conditions on the surface of the glass plate 11 change in the part where the rubber member 16 is pressed (pressed part), and the light is no longer totally reflected. Therefore, at the position of the camera 13 below the glass plate 11, the pressed part appears bright, and the other parts appear almost black. Also, the parts where the pressure of the press is greater and the air layer between the glass plate 11 and the paper 15 is thinner appear brighter, and the part where the glass plate 11 and the paper 15 are in close contact with each other appears the brightest.
[0036] The reason why total reflection occurs at the boundary between glass plate 11 and air but not at the boundary between glass plate 11 and paper 15 is because the refractive indexes of glass, air, and paper are approximately 1.52, 1.00, and 1.50, respectively, and as a result, the critical angles at the boundary between glass and air and the boundary between glass and paper are different.
[0037] Furthermore, since rubber member 16 and paper 15 naturally come into contact at the pressed portion of rubber member 16, the shape and size of the portion that appears bright as the pressed portion of rubber member 16 coincides with the shape and size of the contact surface between rubber member 16 and paper 15. Furthermore, the shape and size of the contact surface between rubber member 16 and paper 15 can be considered to be approximately the same as the shape and size of the contact surface between rubber member 16 and glass plate 11 when it is assumed that rubber member 16 is pressed directly against glass plate 11.
[0038] The rubber member 16 used in the observation method using the imaging device 10 is prepared by removing plies, belts, etc. from a tire and then cutting out a portion of the tread rubber. For example, one rubber member 16 may be a single block cut out from a tire, or a group of multiple blocks cut out.
[0039] When performing the observation method using the imaging device 10, the operator attaches and fixes the paper 15 to the upper surface 11b of the glass plate 11 with double-sided tape. Next, the operator turns off the lights in the test room in which the imaging device 10 is placed. The operator also prevents light such as sunlight from entering the test room, and prevents devices in the test room from emitting light as much as possible. In this state, the operator turns on the light guides 14 on both the left and right sides. The light emitted from the slits 24 of the light guides 14 enters the glass plate 11 and is totally reflected inside the glass plate 11.
[0040] Next, the worker performs a preliminary test to determine the relationship between brightness and pressure in a photograph (image) taken by camera 13. In the preliminary test, the worker applies multiple levels of pressure from above paper 15, and photographs are taken by camera 13 when each level of pressure is applied.
[0041] For the preliminary test, the worker prepares a pressure application jig 25 (see FIG. 6) for applying pressure. The pressure application jig 25 is circular or rectangular when viewed from above, and applies a certain pressure to the circular or rectangular pressure application range. In detail, as shown in FIG. 4, a circular or rectangular (circular in the case of FIG. 4) rubber packing 27 is provided along the edge of the lower surface 26 of the pressure application jig 25. Furthermore, the pressure application jig 25 is provided with a flow path (not shown) for introducing air into the inside of the rubber packing 27, and an air compressor (not shown) connected to the flow path. In addition, a pressing tool such as a weight or a mechanism for pressing down the pressure application jig 25 from above is attached to the pressure application jig 25. With this structure, air is sent from the air compressor to the inside of the rubber packing 27, and the pressure increases in the pressure application range inside the rubber packing 27. The pressure application range is not limited, but in the case of a circle, the diameter is, for example, about 60 mm to 70 mm, and in the case of a rectangle, the depth is, for example, 260 mm to 270 mm and the width is, for example, 25 mm to 35 mm. Even if the pressure in the pressure application range increases, the pressure application jig 25 will not float up due to the action of the holding tool.
[0042] The worker uses a pressing tool to press the pressure application jig 25 against the paper 15 from above, sealing the inside of the rubber packing 27, and increases the pressure in the pressure application range by introducing air into the inside of the rubber packing 27, thereby applying pressure from above the paper 15. While applying pressure from above the paper 15 in this way, the worker takes a photograph from below the glass plate 11 with the camera 13. Since total reflection of light is inhibited in the pressure application range (i.e., light is not totally reflected and passes through the upper surface 11b of the glass plate 11 and hits the paper 15), the pressure application range appears bright in the photograph taken by the camera 13, and the other parts appear almost black. Also, as shown in Figures 5(a) to (c), the greater the applied pressure, the thinner the air layer between the glass plate 11 and the paper 15 becomes, and the pressure application range appears brighter. In addition, there are small irregularities on the surface of the paper 15, and sometimes foreign matter is present between the glass plate 11 and the paper 15, so that in the photograph taken, the brightness will not be uniform across the entire pressure load area, but will vary from pixel to pixel.
[0043] The worker applies multiple levels of pressure to the paper 15, and takes pictures with the camera 13 while applying each pressure. The magnitude of the pressure is set to include the pressure of the pressing by the rubber member 16 in the main test described below. There are at least three levels of pressure, and preferably eight levels or more. For example, the worker gradually increases the applied pressure from 100 kPa, to 200 kPa, to 300 kPa, and takes pictures with the camera 13 each time the pressure is changed.
[0044] Even if the applied pressure changes, the positions of the paper 15 and the camera 13 do not change. Therefore, the same area of the paper 15 is always captured in the photograph (image).
[0045] The photographs (images) taken by the camera 13 at each pressure are acquired by the analysis device 17. The photographs (images) thus acquired at each pressure are each referred to as a first image.
[0046] The pressure application range by one pressure application jig 25 is limited. Therefore, when the rubber member 16 is to be pressed over a wide range in the main test described later, the worker applies the same pressure at multiple locations using one pressure application jig 25 as shown in Figs. 6(a) and 6(b) and takes photos of the multiple locations. Then, the data of the photos of the multiple locations is combined to obtain a wide range of the first image for that pressure. The photo data is brightness matrix data, and the data is combined, for example, by using rows 1 to 400 of the matrix as data for the first photo and rows 401 to 1000 as data for the second photo. The rubber member 16 is pressed during the main test within the range of the first image obtained in this way. Of course, when the range to press the rubber member 16 in the main test is narrow, it is sufficient for the worker to apply pressure at one location using the pressure application jig 25 at each pressure as shown in Figs. 6(c) and 6(d).
[0047] Next, analysis device 17 obtains a relational expression between pressure and brightness for each pixel from each pressure applied in the preliminary test and the brightness for each pixel in the first image acquired at each pressure.
[0048] Specifically, the analysis device 17 performs fitting using a function such as a linear function or a quadratic function for data on each pressure applied in the preliminary test and the brightness in the first image acquired at each pressure. The analysis device 17 performs this fitting for each pixel in the first image. The fitting method is a known method such as the least squares method. The function obtained as a result is used as a relational expression between the pressure and brightness in each pixel.
[0049] Fig. 7 shows an image of how the relational equation between pressure and brightness at each pixel is obtained. As shown in this figure, analysis device 17 fits data (points in each graph) showing the relationship between pressure and brightness for each pixel of the first image with a function (straight line in each graph), and uses the function as the relational equation between pressure and brightness at that pixel. Although only three pixels are shown in Fig. 7, analysis device 17 actually obtains the relational equation for all pixels in this manner.
[0050] The reason why the relational expression is found for each pixel in this way is that the relationship between pressure and brightness is different for each pixel. In detail, even if the same pressure is applied, the brightness in the photograph is different for each pixel due to the influence of the unevenness of the surface of the paper 15, foreign matter (e.g., dust, dirt, etc.) between the paper 15 and the glass plate 11, the intrusion of ambient light, etc. Therefore, the relationship between pressure and brightness is different for each pixel.
[0051] Next, the worker performs the main test. The main test is performed by using the paper 15 attached to the glass plate 11 in the preliminary test as it is. The positional relationship between the glass plate 11, the paper 15, the camera 13, and the light guide 14 does not change between the preliminary test and the main test. Therefore, in the main test, a photograph is taken under the same lighting conditions and with the same shooting range as in the preliminary test.
[0052] In this test, an operator attaches rubber member 16 to a jig 21 and holds the jig 21 in the holder 12 of the imaging device 10. When the holder 12 holds the rubber member 16 via the jig 21, it presses the rubber member 16 against the paper 15 on the glass plate 11 and then moves and slides the rubber member 16 at a constant speed on the paper 15. The sliding causes the rubber member 16 to undergo shear deformation.
[0053] While the holding part 12 is moving in this way, the camera 13 takes a number of photographs from below the glass plate 11. The photographing range is an area that includes the pressed part of the rubber member 16. Total reflection of light is inhibited in the pressed part of the rubber member 16 (that is, the light is no longer totally reflected and passes through the upper surface 11b of the glass plate 11 to hit the paper 15), so in the photograph taken by the camera 13, the pressed part appears bright and the other parts appear almost black. In addition, there is a brightness distribution in the photograph. Specifically, the parts where the pressure of the pressure is greater and the air layer between the glass plate 11 and the paper 15 is thinner appear brighter, and the part where the glass plate 11 and the paper 15 are in close contact appears the brightest.
[0054] As an example, Fig. 8(b) shows an image captured when the left side of rubber member 16 is pressed against paper 15 as shown in Fig. 8(a). From Figs. 8(a) and (b), it can be seen that the image captured shows the pressed part of rubber member 16 as bright, and the other parts as black. It can also be seen that the parts that are pressed harder against paper 15 and therefore have greater pressure are brighter.
[0055] One sliding test is performed from when the rubber member 16 is pressed against the paper 15 on the glass plate 11 until the sliding of the rubber member 16 ends and the taking of a plurality of photographs by the camera 13 is completed.
[0056] In the main test, the photographs (images) taken by the camera 13 are acquired by the analysis device 17. Each photograph (image) acquired in the main test is referred to as a second image. The second image acquired by the analysis device 17 is associated with the time when the second image was taken.
[0057] Next, the analysis device 17 converts the luminance of each second image into pressure for each pixel using the above-mentioned relational expression between pressure and luminance. As a result, the second image, which was a luminance distribution image, is converted into a pressure distribution image, which is an image showing the contact pressure distribution on the contact surface between the rubber member 16 and the paper 15.
[0058] For reference, an example of the second image is shown in Fig. 9(a), and a pressure distribution image obtained by converting the brightness of the second image into pressure is shown in Fig. 9(b). As can be seen from Fig. 9(a) and (b), the mottled pattern seen in the second image is reduced in the pressure distribution image.
[0059] The analysis device 17 can perform various analyses using the pressure distribution image. For example, like the second image, the pressure distribution image is also linked to the photographing time. Therefore, based on a plurality of pressure distribution images photographed over a predetermined period of time, it is possible to clarify the time series change in the contact pressure distribution in the rubber member 16 during sliding. In addition, it is also possible to perform the test under a plurality of different temperature conditions and clarify the difference in the contact pressure distribution due to the difference in temperature. It is also possible to obtain the contact area between the rubber member 16 and the paper 15 from the pressure distribution image and clarify the time series change in the contact area.
[0060] As described above, the observation method of this embodiment includes the steps of placing paper 15 on glass plate 11 as a preliminary test, applying multiple levels of pressure from above paper 15, and photographing from below glass plate 11 first images that are images with luminance distributions when each level of pressure is applied, and determining a relational equation between pressure and luminance for each pixel in the photographed range based on the first images for each pressure. This makes it possible to grasp the relationship between pressure and luminance for each pixel as an equation, even if the relationship between pressure and luminance differs for each pixel due to the presence of unevenness on the surface of paper 15, foreign matter (e.g., dust, dirt, stains, etc.) between paper 15 and glass plate 11, intrusion of ambient light, etc.
[0061] Furthermore, the observation method of this embodiment includes, as a main test, a step of pressing rubber member 16 from above paper 15 and capturing a second image, which is an image with a luminance distribution of paper 15, from below glass plate 11. The second image captured at this time has unevenness due to unevenness on the surface of paper 15, foreign matter between paper 15 and glass plate 11, intrusion of surrounding light, and the like.
[0062] However, the observation method of this embodiment includes a step of converting the luminance of the second image into pressure for each pixel based on the above relational expression, thereby acquiring a pressure distribution image that shows the contact pressure distribution on the contact surface between the rubber member 16 and the paper 15. In this way, by converting the luminance of the second image into pressure for each pixel using the above relational expression, it is possible to acquire the contact pressure distribution in a form in which unevenness due to the unevenness of the surface of the paper 15 contained in the second image has been removed. Therefore, it is possible to acquire a more accurate contact pressure distribution on the contact surface of the rubber member 16.
[0063] In the observation method of this embodiment, the worker applies light to the glass plate 11 and causes total reflection inside the glass plate 11. The worker also places paper 15 on the glass plate 11. The holder 12 then presses the rubber member 16 from above the paper 15, thereby creating a contact surface between the rubber member 16 and the paper 15 and preventing total reflection of light below the contact surface (i.e., the light is transmitted through the upper surface 11b of the glass plate 11 and strikes the paper 15). The camera 13 photographs the pressed portion from below the glass plate 11, thereby acquiring an image of the contact surface between the rubber member 16 and the surface of the paper 15.
[0064] With this method, as described above, it is possible to obtain an image in which the pressed portion is bright and the other portion is black, and to more accurately observe the contact surface of the rubber member 16. Moreover, the bright portion in the image can be regarded as being substantially the same as the shape and size of the contact surface between the rubber member 16 and the glass plate 11 when they come into contact with each other.
[0065] In addition, because the paper 15 is placed on the glass plate 11, even if sunlight is shining into the test room or the lights are on in the test room, the light can be prevented from passing through the glass plate 11 and entering the camera 13. In other words, the paper 15 blocks external light such as sunlight. Therefore, the light entering the camera 13 can be limited to indirect lighting from the light guide 14. In addition, because the paper 15 is placed on the glass plate 11, the rubber member 16, the jig 21, etc. located above the paper 15 can be prevented from entering the image captured by the camera 13. Due to the effect of the paper 15, only the pressed part appears bright in the image, and the contact surface of the rubber member 16 can be observed more accurately.
[0066] Various modifications can be made to the above embodiment. Any one of the modifications described below may be applied to the above embodiment, or any two or more may be selected and combined and applied to the above embodiment. For example, with respect to the median filter, both the following modification example 1 and modification example 2 may be applied, modification example 2 may be applied without applying modification example 1, or modification example 1 may be applied without applying modification example 2.
[0067] <Change Example 1> The first image acquired in the preliminary test may contain noise. In such a case, it is effective to apply a median filter to the first image. A median filter converts the brightness of a pixel into the median value of the brightness of the surrounding pixels. The size of the median filter applied to the first image is preferably 3x3 pixels (i.e., a square with the pixel to be converted at the center, 3 pixels high and 3 pixels wide).
[0068] As described above, the first images are acquired for each of a plurality of pressure levels, and the analysis device 17 applies a median filter to each of the plurality of first images. The first image applied with the median filter is regarded as a corrected first image. In this manner, the corrected first images are acquired for each of a plurality of pressure levels.
[0069] The analysis device 17 obtains a relational expression between pressure and brightness for each pixel in the photographed range based on the corrected first images for each of the multiple pressures. Using the relational expression, the analysis device 17 converts the brightness of the second image obtained in the main test into pressure for each pixel, and obtains a pressure distribution image that represents the contact pressure distribution on the contact surface between the rubber member 16 and the paper 15. This makes it possible to reduce the effect of noise even if it is included in the first image, and is expected to improve the accuracy of the contact pressure distribution.
[0070] Applying a median filter to the first image is effective not only when there is noise in the first image, but also when there is concern that paper 15 may shift slightly relative to glass plate 11 between the preliminary test and the main test. Even if there is such a slight shift, applying a median filter to the first image can smooth the luminance distribution of the first image, thereby reducing the effect of the shift on the relational equation between pressure and luminance calculated for each pixel.
[0071] However, applying a median filter may result in losing the effect on the first image of small irregularities on the surface of paper 15. Therefore, if there is little need to apply a median filter, such as when there is little noise in the first image or when there is no possibility of misalignment of paper 15, it is better not to apply a median filter to the first image.
[0072] As an example of this modification, an example of the first image is shown in Fig. 10(a), and the rectangular area in Fig. 10(a) is enlarged and shown in Fig. 10(b). Fig. 10(c) shows an image obtained by applying a 3x3 pixel median filter to the image in Fig. 10(b), and Fig. 10(d) shows an image obtained by applying a 7x7 pixel median filter to the image in Fig. 10(b). These figures show that the larger the size of the median filter, the more the image is smoothed, but fine information is lost.
[0073] <Change Example 2> In general, minute specks in a pressure distribution image are often treated as unnecessary information in various analyses using the pressure distribution image. Therefore, if there are minute specks in a pressure distribution image, they are considered as noise, and it is preferable to remove the minute specks by applying a median filter to the pressure distribution image. The size of the median filter applied to the pressure distribution image is preferably 3×3 pixels, 5×5 pixels, or 7×7 pixels.
[0074] Furthermore, if a foreign object that was not present in the preliminary test gets between the paper 15 and the glass plate 11 during the actual test, the foreign object will affect the pressure distribution image. In such a case, it is effective to apply a median filter to the pressure distribution image.
[0075] As an example of this modification, an example of a pressure distribution image is shown in Fig. 11(a). Fig. 11(b) shows an image obtained by applying a 3x3 pixel median filter to this pressure distribution image, and Fig. 11(c) shows an image obtained by applying a 7x7 pixel median filter to this pressure distribution image. It can be seen from these figures that the larger the median filter size, the more the image is smoothed.
[0076] <Change Example 3> The structure of the photographing device 10 is not limited to that of the above embodiment. For example, an acrylic plate or the like may be used as the transparent body instead of the glass plate 11. Also, a camera capable of photographing a moving image may be used as the camera 13, and an image may be acquired from the moving image.
[0077] <Change Example 4> The rubber member 16 does not have to be cut out from a tire, but may be prepared as a sample using a sample mold.
[0078] <Change Example 5> The pressure application jig used to apply pressure from above the paper 15 in the preliminary test is not limited to that in the above embodiment. Any pressure application jig may be used as long as it can apply pressure from above the paper 15. However, it is preferable that the pressure application jig be one that applies uniform pressure to the paper 15 by introducing a fluid such as air into an enclosed space formed between the paper 15 and the pressure application jig, like the pressure application jig 25 in the above embodiment.
[0079] <Change Example 6> Instead of the paper 15 made of natural fibers such as plants, other sheet-like materials can be used as the contact member. For example, paper made of a fibrous polymer material or a fibrous inorganic material, or a synthetic resin sheet formed into a sheet-like material rather than a fibrous material can be used as the contact member.
[0080] In any of the contact members, the preferred ranges of the arithmetic mean roughness of the surface, the whiteness of the surface, and the thickness are the same as those of the paper 15 in the above embodiment. [Explanation of symbols]
[0081] 10...imaging device, 11...glass plate, 11a...side surface, 11b...upper surface, 11c...lower surface, 12...holding portion, 13...camera, 14...light guide, 15...paper, 16...rubber member, 17...analysis device, 21...jig, 22...bundled fiber, 23...casing, 24...slit, 25...pressure loading jig, 26...lower surface, 27...rubber packing
Claims
1. A method for observing a contact surface of a rubber member, comprising pressing a rubber member against a contact member and taking an image of the contact surface between the rubber member and the contact member, placing the contact member on a transparent body; A step of applying a plurality of levels of pressure from above the contact member using a pressure application tool, and photographing a first image, which is an image having a luminance distribution when each pressure is applied, from below the transparent body; A step of obtaining a relational expression between pressure and brightness for each pixel in the photographing range based on the first image for each pressure; pressing the rubber member from above the contact member and capturing a second image, which is an image having a luminance distribution, from below the transparent body; a step of converting the luminance of the second image into pressure for each pixel based on the relational expression between pressure and luminance to obtain a pressure distribution image which is an image representing a contact pressure distribution on a contact surface between the rubber member and the contact member; The method for observing a contact surface of a rubber member comprises:
2. 2. A method for observing the contact surface of a rubber member as described in claim 1, further comprising applying a median filter to each of the first images to obtain respective corrected first images, and determining the relationship between pressure and brightness for each pixel in the shooting range based on the corrected first images for each pressure.
3. 3. The method for observing the contact surfaces of rubber members according to claim 2, wherein the size of the median filter is 3 x 3 pixels.
4. The method for observing the contact surfaces of rubber members according to claim 1 , further comprising applying a median filter to the pressure distribution image.
5. 5. The method for observing the contact surface of a rubber member according to claim 4, wherein the size of the median filter is 3x3 pixels, 5x5 pixels, or 7x7 pixels.
6. Light is incident on the transparent body and totally reflected inside the transparent body; applying pressure from above the contact member to press the contact member against the transparent body, thereby preventing total reflection of light at the pressed location, and capturing the first image; The rubber member is pressed from above the contact member to press the contact member against the transparent body, thereby preventing total reflection of light at the pressed location, and capturing the second image. The method for observing the contact surface of a rubber member according to any one of claims 1 to 5.
Citation Information
Patent Citations
Display method of tire contact shape and display device of tire contact shape
JP2003014428A
Observation device and method of contact surface of rubber
JP2016188767A