Toner and method for manufacturing toner

The toner composition with resin A and B addresses paper adhesion and charge-up issues by enhancing spatial arrangement and charge transfer, achieving stable image quality across varying environmental conditions.

JP2024163199AActive Publication Date: 2024-11-21CANON KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024150858
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-21
Estimated Expiration
2040-10-23

AI Technical Summary

Technical Problem

Existing toners exhibit paper adhesion issues in high-temperature, high-humidity environments and charge-up in low-temperature, low-humidity conditions, leading to image defects such as stains and fogging, while requiring both low-temperature fixability and heat-resistant storage stability.

Method used

A toner composition comprising resin A and resin B, where resin A has a specific structure represented by formula (1) and resin B has a monomer unit represented by formula (2), with a specific silicon-to-total ion count ratio, enhancing spatial arrangement and charge transfer properties to improve adhesion and reduce charge-up.

Benefits of technology

The toner achieves excellent low-temperature fixability, heat-resistant storage stability, and paper ejection adhesion in high-temperature, high-humidity environments, while suppressing image defects like fogging in low-temperature, low-humidity conditions, ensuring high-quality image formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163199000001
    Figure 2024163199000001
  • Figure 2024163199000002
    Figure 2024163199000002
  • Figure 2024163199000003
    Figure 2024163199000003
Patent Text Reader

Abstract

To provide a toner excellent in low-temperature fixability, heat-resistant storage properties and ejected paper adhesion properties in a high-temperature and high-humidity environment, and capable of forming a high-quality image when used in a low-temperature and low-humidity environment; and to provide a method for manufacturing the toner.SOLUTION: Provided is a toner with toner particles having a resin A and a resin B. A method for manufacturing the toner includes: a step for obtaining the toner in which the resin A has a structure represented by a prescribed general formula and the resin B has a monomer unit represented by a prescribed general formula, and toner slurry by having toner base particles containing the resin B dispersed in an aqueous medium; and a step for inputting a monomer composition containing a monomer represented by a prescribed general formula and a radical polymerization initiator to the obtained toner slurry, and forming the resin A on the surfaces of the toner base particles.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a toner used in electrophotography, electrostatic recording, and toner jet recording, and a method for producing the toner. [Background technology]

[0002] In recent years, in electrophotography, there has been a demand for energy saving in various electrophotographic processes in order to reduce power consumption. In the power consumption of laser beam printers, the thermal energy of the fixing device in the toner fixing process accounts for a large proportion, and efforts are being made to reduce power consumption by lowering the fixing temperature. In order to lower the fixing temperature, it is effective to improve the low-temperature fixing property of the toner. On the other hand, toners are also required to have storage stability (heat-resistant storage stability) to withstand high-temperature storage environments. In order to achieve both low-temperature fixability and heat-resistant storage stability of toners, a method of using a side-chain crystalline resin with a melting point of 50.0°C to 90.0°C as a binder resin has been considered (Patent Document 1). Patent Document 1 also describes that the image loading ability is good. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-130243 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, when continuous double-sided printing at a high printing rate was performed in a high-temperature, high-humidity environment using the toner described in Patent Document 1, it was found that the paper stacked on the paper output tray was sometimes soiled and the paper output adhesion (image loading ability) was sometimes insufficient. It was also found that such a toner is prone to charging up in a low-temperature, low-humidity usage environment, and image defects such as fogging may occur. The toner and the method for producing the toner disclosed herein are excellent in low-temperature fixability, heat-resistant storage stability, and adhesiveness at discharged paper in a high-temperature, high-humidity environment, and are capable of forming high-quality images when used in a low-temperature, low-humidity environment, and the method for producing the toner is also provided. [Means for solving the problem]

[0005] The toner of the present disclosure is A toner having toner particles having a resin A and a resin B, The resin A has a structure represented by the following formula (1): The resin B has a monomer unit represented by the following formula (2) and a monomer unit represented by the following formula (3), In a measurement of the surface of the toner particles using a time-of-flight secondary ion mass spectrometer, the ion count derived from silicon having a mass number of 28 relative to the total ion count in the mass numbers of 1 to 1800 is 0.0010 to 0.0050. It is characterized by:

[0006] [ka]

[0007] In formula (1), P 1 represents the polymer moiety, and R 1 ~R 3 each independently represents a hydrogen atom, an alkyl group having one or more carbon atoms, an alkoxy group having one or more carbon atoms, or a hydroxy group; R 1 ~R 3 at least one of represents an alkoxy group or a hydroxy group having one or more carbon atoms, and m represents a positive integer; L 1 is an alkylene group with 8 or less carbon atoms, *-O-**, *-OR 5 -**, *-NH-**, *-NH-R 6 -**, where * represents the bond to the carbonyl group in formula (1), ** represents the bond to the silicon atom, and R 5 , R 6 are each an alkylene group having up to 8 carbon atoms, each of which may have a hydroxyl group as a substituent; Multiple L when m is 2 or more 1 , multiple R 1 , multiple R 2 and multiple R 3 may be the same or different.

[0008] [ka]

[0009] In formula (2), R 4 represents a hydrogen atom or a methyl group, and n represents an integer of 11 to 35. [ka] In formula (3), R 7 represents a hydrogen atom or a methyl group. The present disclosure also provides A toner having toner particles having a resin A and a resin B, The resin A has a structure represented by the following formula (1): The resin B has a monomer unit represented by the following formula (2): When the content of the resin A in the toner particles is MA (mass%) and the content of the resin B in the toner particles is MB (mass%), MA / MB is 0.0050≦[MA / MB]≦0.2000, In a measurement of the surface of the toner particles using a time-of-flight secondary ion mass spectrometer, the ion count derived from silicon having a mass number of 28 relative to the total ion count in the mass numbers of 1 to 1800 is 0.0010 to 0.0050. It is characterized by: [ka] In formula (1), P 1 represents the polymer moiety, and R 1 ~R 3 each independently represents a hydrogen atom, an alkyl group having one or more carbon atoms, an alkoxy group having one or more carbon atoms, or a hydroxy group; R 1 ~R 3at least one of represents an alkoxy group or a hydroxy group having one or more carbon atoms, and m represents a positive integer; L 1 is an alkylene group with 8 or less carbon atoms, *-O-**, *-OR 5 -**, *-NH-**, *-NH-R 6 -**, where * represents the bond to the carbonyl group in formula (1), and ** represents the bond to the silicon atom, and R 5 , R 6 are each an alkylene group having up to 8 carbon atoms, each of which may have a hydroxyl group as a substituent; Multiple L when m is 2 or more 1 , multiple R 1 , multiple R 2 and multiple R 3 may be the same or different. [ka] In formula (2), R 4 represents a hydrogen atom or a methyl group, and n represents an integer of 11 to 35. Further, the present disclosure provides A toner having toner particles having a resin A and a resin B, The resin A has a structure represented by the following formula (1): The resin B has a monomer unit represented by the following formula (2): In a measurement of the surface of the toner particles using a time-of-flight secondary ion mass spectrometer, the ion count derived from silicon having a mass number of 28 relative to the total ion count in the mass numbers of 1 to 1800 is 0.0010 to 0.0050. It is characterized by: [ka] In formula (1), P 1 represents the polymer moiety, and R 1 ~R 3 each independently represents a hydrogen atom, an alkyl group having one or more carbon atoms, an alkoxy group having one or more carbon atoms, or a hydroxy group; R 1 ~R3 at least one of represents an alkoxy group or a hydroxy group having one or more carbon atoms, and m represents a positive integer; L 1 is an alkylene group with 8 or less carbon atoms, *-O-**, *-OR 5 -**, *-NH-**, *-NH-R 6 -**, where * represents the bond to the carbonyl group in formula (1), ** represents the bond to the silicon atom, and R 5 , R 6 are each an alkylene group having up to 8 carbon atoms, each of which may have a hydroxyl group as a substituent; Multiple L when m is 2 or more 1 , multiple R 1 , multiple R 2 and multiple R 3 may be the same or different. [ka] In formula (2), R 4 represents a hydrogen atom or a methyl group, and n represents an integer of 17 to 29. Effect of the Invention

[0010] According to the present disclosure, it is possible to provide a toner that is excellent in low-temperature fixing property, heat-resistant storage stability, and discharge adhesion in a high-temperature, high-humidity environment, and is capable of forming high-quality images when used in a low-temperature, low-humidity environment, and a method for producing the toner. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In the present invention, the description of "XX or more and YY or less" or "XX to YY" representing a numerical range means a numerical range including the endpoints, that is, the lower limit and the upper limit, unless otherwise specified. The monomer unit refers to the reacted form of a monomer substance in a polymer.

[0012] The toner of the present disclosure will be specifically described below. The toner of the present disclosure is A toner having toner particles having a resin A and a resin B, The resin A has a structure represented by the following formula (1): The resin B has a monomer unit represented by the following formula (2): It is characterized by:

[0013] [ka]

[0014] In formula (1), P 1 represents the polymer moiety, and R 1 ~R 3 each independently represents a hydrogen atom, an alkyl group having one or more carbon atoms, an alkoxy group having one or more carbon atoms, or a hydroxy group; R 1 ~R 3 at least one of represents an alkoxy group or a hydroxy group having one or more carbon atoms, and m represents a positive integer; L 1 is an alkylene group with 8 or less carbon atoms, *-O-**, *-OR 5 -**, *-NH-**, *-NH-R 6 -**, where * represents the bond to the carbonyl group in formula (1), ** represents the bond to the silicon atom, and R 5 , R 6 are each an alkylene group having up to 8 carbon atoms, each of which may have a hydroxyl group as a substituent; Multiple L when m is 2 or more 1 , multiple R 1 , multiple R 2 and multiple R 3 may be the same or different.

[0015] [ka]

[0016] In formula (2), R 4 represents a hydrogen atom or a methyl group, and n represents an integer of 11 to 35.

[0017] The toner having the above characteristics is excellent in low-temperature fixing property, heat-resistant storage stability, and adhesiveness at discharged paper in a high-temperature and high-humidity environment, and is capable of forming high-quality images when used in a low-temperature and low-humidity environment. The inventors believe that the effects are due to the following reasons. Resin B has a monomer unit represented by formula (2). The monomer unit represented by formula (2) has a high degree of freedom in the molecular chain and is easy to lower the glass transition point (Tg) of the resin during fixing, so that it can improve low-temperature fixing properties. However, when a resin having a monomer unit represented by formula (2) is used, the Tg of the image after fixing is easy to lower, so when the paper is stacked on the paper output tray in a heated state immediately after ejection, it is thought that ejection adhesion is likely to occur due to the heat and pressure from the weight of the paper itself.

[0018] The carbonyl group in resin A and the ester group in resin B have a high affinity, and it is believed that resin A and resin B tend to be arranged in close spatial positions in the fixed toner. If resin A and resin B are closer to each other in the spatial arrangement described above, the silane moiety in resin A and the long-chain alkyl moiety in resin B have a low affinity, so the long-chain alkyl moieties in resin B tend to gather locally, and the gathered long-chain alkyl moieties tend to be oriented in small regions. This is thought to result in the formation of domains in the toner particles. The formed domains restrict the movement of molecules, so the decrease in Tg of the image can be suppressed. 1 is an alkylene group having 8 or less carbon atoms, *-O-**, *-OR 5 -**, *-NH-**, *-NHR 6 -** (* represents the bond to the carbonyl group in formula (1), ** represents the bond to the silicon atom, and R 5 , R 6 each independently represents an alkylene group having 8 or less carbon atoms, and each carbon may have a hydroxyl group as a substituent.), the distance between the carbonyl group of resin A and the silane moiety is short, so that the above-mentioned effect becomes more remarkable, and it is believed that the effect of the present disclosure is achieved.

[0019] Resin A will be described in detail below. Resin A has a structure represented by the following formula (1).

[0020] [ka]

[0021] In formula (1), P 1 represents the polymer moiety, and R 1 ~R 3 each independently represents a hydrogen atom, an alkyl group having one or more carbon atoms, an alkoxy group having one or more carbon atoms, or a hydroxy group; R 1 ~R 3 at least one of represents an alkoxy group or a hydroxy group having one or more carbon atoms, and m represents a positive integer; L 1 is an alkylene group with 8 or less carbon atoms, *-O-**, *-OR 5 -**, *-NH-**, *-NH-R 6 -**, where * represents the bond to the carbonyl group in formula (1), ** represents the bond to the silicon atom, and R 5 , R 6 are each an alkylene group having up to 8 carbon atoms, each of which may have a hydroxyl group as a substituent; Multiple L when m is 2 or more 1 , multiple R 1 , multiple R 2 and multiple R 3 may be the same or different.

[0022] L in formula (1) 1 is an alkylene group having 8 or less carbon atoms, *-O-**, *-OR 5 -**, *-NH-**, *-NHR 6 -** (* represents the bond to the carbonyl group in formula (1), ** represents the bond to the silicon atom, and R 5 , R 6 are each an alkylene group having 8 or less carbon atoms, and each carbon may have a hydroxyl group as a substituent. When In addition, resins having a monomer unit represented by formula (2) tend to accumulate electric charge in low-temperature, low-humidity environments, and therefore tend to charge up, which may lead to image defects such as fogging. The toner particles according to the present disclosure contain resin B having a monomer unit represented by formula (2) and resin A having a structure represented by formula (1), and as described above, resin A and resin B tend to be arranged in close spatial positions, so that the electric charge of resin B is easily transferred to the carbonyl group of resin A through the ester moiety of resin B, and charge up can be suppressed in low-temperature, low-humidity environments. As a result, image defects such as fogging can be suppressed, and image quality can be improved. L in Equation (1) 1 *-NHR 6 -** is preferred. 1 *-NHR 6 In the case of -**, the above-mentioned effect is easily manifested, and the adhesiveness of discharged paper is easily improved. The image quality in the R 6 The alkylene group represented by the formula (I) preferably has 1 to 4 carbon atoms, and more preferably has 1 to 3 carbon atoms. In addition, in the resin A, L 1 *-OR 5 The effect of the present disclosure is also easily achieved in the -** case, which is also preferable. 5 The group preferably has 1 to 4 carbon atoms, and more preferably has 1 to 3 carbon atoms. In addition, L 1 When is an alkylene group, the alkylene group preferably has 1 to 4 carbon atoms, and more preferably 1 to 3 carbon atoms.

[0023] R in formula (1) 1 ~R 3 each independently represents a hydrogen atom, an alkyl group having one or more carbon atoms, an alkoxy group having one or more carbon atoms, or a hydroxy group; R 1 ~R 3 At least one of R represents an alkoxy group or a hydroxy group having one or more carbon atoms. 1 ~R 3Among the substituents which may be represented, the number of carbon atoms in the alkyl group is preferably 1 to 20, more preferably 1 to 4. The number of carbon atoms in the alkoxy group is preferably 1 to 20, more preferably 1 to 4, further preferably 1 to 3, and particularly preferably 1 or 2.

[0024] R in formula (1) 1 ~R 3 In order to make one or more of R into a hydroxy group, 1 ~R 3 Resin A in which one or more of the above groups are alkoxy groups may be hydrolyzed to convert the alkoxy groups into hydroxy groups. The hydrolysis may be carried out by any method, for example, the following method. R in the above formula (1) 1 ~R 3 Resin A, in which one or more of the above groups are alkoxy groups, is dissolved or suspended in a suitable solvent (which may be a polymerizable monomer), and the pH is adjusted to acidic using an acid or alkali, followed by mixing and hydrolysis. Further, hydrolysis may occur during the production of toner particles.

[0025] Any method may be used to form the structure represented by formula (1), and examples thereof include the following methods. They can be formed by reacting a carboxyl group in a resin with an amino silane coupling agent, polymerizing an ethylenically unsaturated bond site in a resin or a monomer having an ethylenically unsaturated bond with a (meth)acrylic silane coupling agent, reacting a hydroxyl group in a resin with an isocyanate silane coupling agent, or reacting an isocyanate group in a resin with an amino silane coupling agent. Examples of the aminosilane coupling agent include 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, and 3-aminopropyldimethoxymethylsilane. Examples of the (meth)acrylic silane coupling agent include 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-methacryloxypropyltriethoxysilane, 8-acryloxyoctyltriethoxysilane, 8-methacryloxyoctyltriethoxysilane, 3-[acrylate (triethoxysilyl)methyl, 3-methacrylate (triethoxysilyl)methyl, 3-[dimethoxy(methyl)silyl]propyl, 3-[dimethoxy(methyl)silyl]propyl, acrylate [dimethoxy(methyl)silyl]methyl, methacrylate [dimethoxy(methyl)silyl]methyl, 3-(methacryloyloxy)propyltris(trimethylsilyloxy)silane, and the like. Examples of the isocyanate coupling agent include isocyanatomethyltrimethoxysilane, isocyanatomethyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, and 3-isocyanatopropylmethyldimethoxysilane.

[0026] The content of the structure represented by the following formula (4) in the resin A is preferably 0.5% by mass or more and 10.0% by mass or less. When it is 0.5% by mass or more, the adhesiveness of discharged paper and the low temperature and low humidity are improved. When the content is 10.0% by mass or less, the hydrophilicity of the entire resin is prevented from increasing due to an excess of silane moieties in resin A, and the spatial arrangement of resin A and resin B is not hindered, so that discharged paper adhesion and image quality at low temperature and low humidity are easily improved. A more preferred range is 1.0% by mass or more and 7.0% by mass or less. The content of the structure represented by formula (4) in resin A can be controlled by adjusting the amount of silane coupling agent added or the amount of functional groups with which the silane coupling agent reacts.

[0027] [ka]

[0028] In formula (4), R 1 ~R 3 is R in formula (1). 1 ~R 3 is the same as L 1 is L in Eq. (1). 1 is the same as:

[0029] The weight average molecular weight MwA of the resin A is preferably 8000 or more and 50000 or less. When it is 8000 or more, the amount of low molecular weight components tends to be small, so that the heat-resistant storage stability tends to be improved. When MwA is 50000 or less, the mobility of the molecules is high after fixing, and spatial arrangement is easy, so that the adhesiveness at discharge tends to be improved. MwA is more preferably 12000 or more and 30000 or less. MwA can be controlled by changing the reaction temperature, reaction time, monomer composition, amount of initiator, etc. of the resin.

[0030] P in the above formula (1) 1 Examples of the resin moiety include, but are not limited to, a polyester resin moiety, a vinyl resin moiety, a polyurethane resin moiety, a polyurea resin moiety, a polycarbonate resin moiety, a phenol resin moiety, a polyolefin resin moiety, and an epoxy resin moiety. Among these, P in the resin A 1 When the resin contains a polyester resin moiety or a vinyl resin moiety, the adhesiveness to discharged paper is easily improved, which is preferable. For example, the resin may be a hybrid resin moiety of a polyester resin and a vinyl resin.

[0031] As the polymerization monomer that can be used in the production of the polyester resin portion, polyvalent carboxylic acids and polyhydric alcohols can be used. Examples of polyvalent carboxylic acids include oxalic acid, glutaric acid, succinic acid, maleic acid, adipic acid, β-methyladipic acid, azelaic acid, sebacic acid, nonanedicarboxylic acid, decanedicarboxylic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, fumaric acid, citraconic acid, diglycolic acid, cyclohexane-3,5-diene-1,2-dicarboxylic acid, hexahydroterephthalic acid, malonic acid, pimelic acid, phthalic acid, isophthalic acid, terephthalic acid, tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-carboxyphenylacetic acid, p-phenylene diacetic acid, m-phenylenediglycolic acid, p-phenylenediglycolic acid, o-phenylenediglycolic acid, diphenylacetic acid, diphenyl-p,p'-dicarboxylic acid, naphthalene-1,4-dicarboxylic acid, naphthalene-1,5-dicarboxylic acid, naphthalene-2,6-dicarboxylic acid, anthracene dicarboxylic acid, and cyclohexane dicarboxylic acid. Examples of polycarboxylic acids other than dicarboxylic acids include trimellitic acid, pyromellitic acid, naphthalene tricarboxylic acid, naphthalene tetracarboxylic acid, pyrene tricarboxylic acid, and pyrene tetracarboxylic acid. Polyhydric alcohols include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, neopentyl glycol, 1,4-butenediol, 1,5-pentane Diol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, isosorbide, trimethylolethane, trimethylolpropane, 1,3,5-trihydroxymethylbenzene, bisphenol A, bisphenol A ethylene oxide adduct, bisphenol A propylene oxide adduct, hydrogenated bisphenol A, hydrogenated bisphenol A ethylene oxide adduct, hydrogenated bisphenol A propylene oxide adduct, and the like.

[0032] Vinyl monomers that can be used to manufacture the vinyl resin portion include styrene, α-methylstyrene, β-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, pn-dodecylstyrene, p-methoxystyrene, p-phenylstyrene, methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, n-amyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, n-nonyl acrylate, cyclohexyl acrylate, and the like. Examples of the acrylates include silyl acrylate, benzyl acrylate, dimethyl phosphate ethyl acrylate, diethyl phosphate ethyl acrylate, dibutyl phosphate ethyl acrylate, 2-hydroxyethyl acrylate, 2-benzoyloxyethyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, iso-propyl methacrylate, n-butyl methacrylate, iso-butyl methacrylate, tert-butyl methacrylate, n-amyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, n-octyl methacrylate, diethyl phosphate ethyl methacrylate, 2-hydroxyethyl methacrylate, dibutyl phosphate ethyl methacrylate, maleic acid, acrylic acid, and methacrylic acid.

[0033] The resin A may further have a monomer unit represented by the following formula (3).

[0034] [ka]

[0035] In formula (3), R 7 represents a hydrogen atom or a methyl group. When the resin A has a monomer unit represented by the formula (3), image quality in a low-temperature, low-humidity environment is likely to improve. The method for introducing the monomer unit represented by formula (3) into resin A is not particularly limited, but includes a method using acrylonitrile or methacrylonitrile as one of the polymerizable monomers capable of forming resin A. The monomer unit represented by formula (3) is preferably contained in resin A at 5.0 mass % to 60.0 mass %.

[0036] Resin A is added when polymerizing resin A during the production of toner particles, and is also used in the following manufacturing process. The method may be, but is not limited to, the method being introduced into the toner particles. A step of dispersing toner base particles containing resin B in an aqueous medium to obtain a toner slurry; a step of adding a monomer composition containing a monomer represented by the following formula (6) and a radical polymerization initiator to the obtained toner slurry to form the resin A on the surface of the toner base particles; Resin A can also be introduced into the toner particles via a method having the following formula:

[0037] [ka]

[0038] In formula (6), R 8 represents a hydrogen atom or a methyl group.

[0039] The formula (1) is preferably at least one selected from the group consisting of structures represented by the following formulas (7) to (12).

[0040] [ka]

[0041] R in equations (8) to (12) 1 ~R 3 ,R 5 ~R6 is R in formula (1). 1 ~R 3 ,R 5 ~R 6 and R 7 represents a hydrogen atom or a methyl group, and R in formulas (9) and (10) 9 , R 10 represents an alkylene group having 1 to 6 carbon atoms (preferably 1 to 4), and P in formulas (11) and (12) 2 represents the main chain skeleton of the polyester resin. The structure represented by formula (11) is not particularly limited, but specific examples include structures such as those shown in the following formulas (13) and (14). The structure represented by formula (12) is not particularly limited, but specific examples include structures such as those shown in the following formulas (15) and (16).

[0042] [ka]

[0043] [In formulas (13) to (16), R 1 ~R 3 ,R 6 is R in formula (1). 1 ~R 3 ,R 6 and X represents a residue obtained by removing a carboxy group from a polycarboxylic acid, and Y represents a residue obtained by removing a hydroxy group from a polyhydric alcohol. The residue obtained by removing a carboxy group from a polycarboxylic acid and the residue obtained by removing a hydroxy group from a polyhydric alcohol are obtained by condensing the polymerization monomers that can be used to produce the polyester resin portion described above.] Each of X and Y may be one type of structure or multiple types of structures. Among these, X is preferably at least one selected from the group consisting of an alkylene group (preferably having 1 to 12 carbon atoms), an alkenylene group (preferably having 2 to 4 carbon atoms), and a phenylene group (preferably having 6 to 12 carbon atoms). Y is preferably at least one selected from the group consisting of an alkylene group (preferably having 1 to 12 carbon atoms), a phenylene group (preferably having 6 to 12 carbon atoms), and a structure represented by the following formula (17).

[0044] [ka]

[0045] In formula (17), R 11 represents an ethylene group or a propylene group. x and y are each an integer of 0 or more, and the average value of x+y is 2 to 10. In formula (17), *** represents a bond to an oxygen atom in formulas (13) to (16).

[0046] Resin B will now be described in detail. Resin B has a monomer unit represented by formula (2).

[0047] [ka]

[0048] In formula (2), R 4 represents a hydrogen atom or a methyl group, and n represents an integer of 11 to 35. In formula (2), when n is 11 or more, a plasticizing effect is exhibited during fixing, and low-temperature fixing property is improved. When n is 35 or less, charging property in a low-temperature and low-humidity environment is good, and a high-quality image can be obtained. The preferred range of n is 17 to 29, and the more preferred range is 17 to 21.

[0049] The content of the monomer unit represented by formula (2) in the resin B is preferably 5.0% by mass or more and 95.0% by mass or less. Within this range, it is easy to achieve both low-temperature fixability and image quality in a low-temperature, low-humidity environment. More preferably, it is 8.0% by mass or more and 80.0% by mass or less.

[0050] As a method for introducing the monomer unit represented by formula (2) into resin B, for example, there is a method of polymerizing a vinyl monomer or a resin containing an ethylenically unsaturated bond with a monomer such as the following. Examples of monomers for introducing the monomer unit represented by formula (2) into resin B include dodecyl (meth)acrylate, tetradecyl (meth)acrylate, stearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, heneicosanyl (meth)acrylate, behenyl (meth)acrylate, lignoceryl (meth)acrylate, ceryl (meth)acrylate, octacosyl (meth)acrylate, myrisyl (meth)acrylate, dotriacontyl (meth)acrylate, hexadecyl (meth)acrylate, lauryl (meth)acrylate, and 2-decyltetradecyl (meth)acrylate.

[0051] Resin B preferably has a monomer unit represented by the following formula (3). [ka]

[0052] In formula (3), R 7 represents a hydrogen atom or a methyl group. When Resin B has a monomer unit represented by formula (3), the monomer unit represented by formula (2) is more likely to form a domain, and therefore discharged paper adhesion and heat-resistant storage stability are more likely to be improved. The method for introducing the monomer unit represented by formula (3) into resin B is not particularly limited, and examples thereof include a method of polymerizing at least one selected from the group consisting of acrylonitrile and methacrylonitrile with an ethylenically unsaturated bond in resin B, and a method of polymerizing a monomer having an ethylenically unsaturated bond with at least one selected from the group consisting of acrylonitrile and methacrylonitrile. The content of the monomer unit represented by formula (3) in resin B is preferably 5.0% by mass to 60.0% by mass.

[0053] The weight average molecular weight MwB of resin B is preferably 15,000 or more and 250,000 or less. When MwB is 15,000 or more, the amount of low molecular weight components tends to be small, so that the heat-resistant storage stability tends to be improved. When MwB is 100,000 or less, deformation during fixing tends to occur, so that the low-temperature fixing property tends to be improved. A more preferable range of MwB is 20,000 or more and 80,000 or less. MwB can be controlled by changing the reaction temperature, reaction time, monomer charging ratio, initiator amount, etc. when producing resin B.

[0054] Resin B is not particularly limited as long as it has a monomer unit represented by formula (2), and known resins such as vinyl resins, polyester resins, and epoxy resins can be used. Among these, resin B is preferably a vinyl resin. Examples of vinyl resins include polymers of monomers containing ethylenic unsaturated bonds. Examples of vinyl monomers that can be used to produce vinyl resins include monomers that can be used in the vinyl resin portion of resin A described above.

[0055] The method for introducing resin B into toner particles is not particularly limited, but in addition to adding synthesized resin B during the production of toner particles, the following methods can be mentioned. A step of dispersing and suspending a polymerizable monomer composition for obtaining resin B in water and polymerizing the polymerizable monomer composition to obtain resin B; a step of dispersing the toner base particles containing the resin B in an aqueous medium to obtain a toner slurry; a step of adding a monomer composition containing a monomer represented by the following formula (6) and a radical polymerization initiator to the obtained toner slurry to form the resin A on the surface of the toner base particles; The method according to claim 1,

[0056] [ka]

[0057] In formula (6), R 8 represents a hydrogen atom or a methyl group.

[0058] The toner particles will now be described in detail. The SP value of resin A in the Fedors method is SPA [(J / m 3 ) 0.5 ], and the SP value of resin B in the Fedors method is SPB[(J / m 3 ) 0.5 ], │SPA-SPB│≦2.00[(J / m 3 ) 0.5 │SPA-SPB│≦2.00[(J / m 3 ) 0.5 In the case of │SPA-SPB│, resin A and resin B are more likely to be spatially arranged after fixing, and therefore the effect of improving the adhesiveness of discharged paper is more likely to be realized. A more preferable range is │SPA-SPB│≦1.00[(J / m 3 ) 0.5 SPA and SPB can be controlled by changing the compositions of resins A and B. The lower limit of |SPA-SPB| ​​is not particularly limited, but is, for example, 0.00 or more. The SPA is preferably 19.00 [(J / m 3 ) 0.5 ]~23.00[(J / m 3 ) 0.5 The SPB is preferably 18.00 [(J / m 3 ) 0.5 ]~23.00[(J / m 3 ) 0.5 ].

[0059] When the content of resin A in the toner particles is MA (mass%) and the content of resin B in the toner particles is MB (mass%), it is preferable that MA / MB is 0.0050≦MA / MB≦0.2000. When MA / MB is 0.0050≦MA / MB, the adhesiveness at discharge is likely to be improved. When MA / MB is ≦0.2000, the heat-resistant storage stability is likely to be improved. MA / MB is more preferably 0.0050≦MA / MB≦0.1000. The content MA of the resin A in the toner particles is preferably 0.40% by mass to 4.0% by mass. Furthermore, the content MB of the resin B in the toner particles is preferably 40.0% by mass to 90.0% by mass.

[0060] In measurement of the surfaces of the toner particles by a time-of-flight secondary ion mass spectrometer (TOF-SIMS), the ion count derived from silicon having a mass number of 28 relative to the total ion count in mass numbers of 1 to 1800 is preferably 0.0010 to 0.0050, and more preferably 0.0020 to 0.0040. When the silicon-derived ion count is 0.0010 to 0.0050, it is considered that resin A is arranged near the surface of the toner particles. It is considered that the phenomenon of discharge adhesion is greatly influenced by the melting of the toner surface. Therefore, when resin A is arranged near the surface of the toner particles, it is considered that the effect of suppressing discharge adhesion as described above is more likely to be exhibited. The silicon-derived ion count can be controlled by changing the composition and amount of resin A, as well as by changing the manufacturing method of the toner particles for introducing the above-mentioned resin A.

[0061] The toner particles may contain a release agent. Examples of the release agent include aliphatic hydrocarbon waxes, oxides of aliphatic hydrocarbon waxes, block copolymers of aliphatic hydrocarbon waxes, waxes mainly composed of fatty acid esters, and partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax, partial esters of fatty acids and polyhydric alcohols, methyl ester compounds having hydroxyl groups obtained by hydrogenating vegetable oils and fats, and Fischer-Tropsch wax. The content of the release agent in the toner particles is preferably 1.50% by mass or more and 20.0% by mass or less.

[0062] A method for producing the toner particles will now be described. The toner particles can be produced by known methods. For example, a suspension polymerization method in which a polymerizable monomer composition containing a polymerizable monomer for obtaining resin B, resin A or a polymerizable monomer for obtaining resin A, and a release agent, etc., as required, is suspended and granulated in an aqueous medium, and the polymerizable monomer in the polymerizable monomer composition is polymerized; A kneading and grinding method in which various toner constituent materials such as resin B, resin A, and optionally a release agent are kneaded, ground, and classified; An emulsion aggregation method in which resin B and resin A are emulsified and dispersed, and the resulting dispersion is mixed with a dispersion liquid of a release agent or the like as necessary, and then aggregated and heated to fuse the mixture to obtain toner particles; An emulsion polymerization aggregation method in which a polymerizable monomer constituting resin B is emulsion-polymerized, the resulting dispersion is mixed with a dispersion in which resin A is emulsified and dispersed, and a dispersion of a release agent, etc., as necessary, and the mixture is aggregated and heat-fused to obtain toner particles; An organic solvent dispersion containing resin B, resin A, and optionally a release agent, etc., is added to water. Dissolution suspension method in which the drug is suspended in a system medium and granulated; etc. can be used.

[0063] The toner can also be produced by the following production method. a step of dispersing the toner base particles containing the resin B in an aqueous medium to obtain a toner slurry; a step of adding a monomer composition containing a monomer represented by the following formula (6) and a radical polymerization initiator to the obtained toner slurry to form the resin A on the surface of the toner base particles; The toner manufacturing method according to the present invention comprises the steps of:

[0064] [ka]

[0065] In formula (6), R 8 represents a hydrogen atom or a methyl group.

[0066] The toner particles may be used as a toner as it is, but an external additive may be added to the toner particles to improve the image quality of the toner. As the external additive, inorganic fine particles such as silica fine particles, titanium oxide fine particles, and aluminum oxide fine particles are preferably used. These inorganic fine particles are preferably hydrophobized with a hydrophobizing agent such as a silane coupling agent, silicone oil, and a mixture thereof. Furthermore, the toner may have an external additive other than the above added to the toner particles as necessary. The amount of the external additive added is preferably 0.5 parts by mass or more and 5.0 parts by mass or less with respect to 100 parts by mass of the toner particles.

[0067] The toner particles may contain a colorant. The colorant is not particularly limited, and the following known colorants can be used. Examples of yellow pigments that can be used include condensed azo compounds such as yellow iron oxide, navel yellow, naphthol yellow S, Hansa yellow G, Hansa yellow 10G, benzidine yellow G, benzidine yellow GR, quinoline yellow lake, permanent yellow NCG, and tartrazine lake, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Specific examples include the following. CI Pigment Yellow 12, 13, 14, 15, 17, 62, 74, 83, 93, 94, 95, 109, 110, 111, 128, 129, 147, 155, 168, 180 etc. Orange pigments include the following: Permanent Orange GTR, Pyrazolone Orange, Balkan Orange, Benzidine Orange G, Induthrene Brilliant Orange RK, Induthrene Brilliant Orange GK, etc. Examples of red pigments include condensed azo compounds such as red iron oxide, permanent red 4R, lithol red, pyrazolone red, watching red calcium salt, lake red C, lake red D, brilliant carmine 6B, brilliant carmine 3B, eosin lake, rhodamine lake B, and alizarin lake, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Specific examples include the following. CI Pigment Red 2, 3, 5, 6, 7, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 144, 146, 150, 166, 169, 177, 1 84, 185, 202, 206, 220, 221, 254, etc. Examples of blue pigments include alkali blue lake, Victoria blue lake, phthalocyanine blue, metal-free phthalocyanine blue, phthalocyanine blue partial chloride, fast sky blue, copper phthalocyanine compounds such as indanthrene blue BG and their derivatives, anthraquinone compounds, basic dye lake compounds, etc. Specific examples include the following. CI Pigment Blue 1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, 66, etc. Examples of black pigments include carbon black, aniline black, non-magnetic ferrite, magnetite, and pigments toned to black using the above-mentioned yellow, red and blue colorants. These colorants may be used alone or in combination of two or more, and may also be used in the form of a solid solution. The content of the colorant in the toner particles is preferably 3.0% by mass to 15.0% by mass.

[0068] The toner particles may contain a charge control agent. Any known charge control agent can be used as the charge control agent. There are charge control agents that control the toner to be negatively charged and charge control agents that control the toner to be positively charged. Examples of charge control agents that control the toner to be negatively charged include the following. Monoazo metal compounds, acetylacetone metal compounds, aromatic oxycarboxylic acids, aromatic dicarboxylic acids, oxycarboxylic and dicarboxylic acid-based metal compounds, aromatic oxycarboxylic acids, aromatic mono- and polycarboxylic acids and their metal salts, anhydrides, esters, phenol derivatives such as bisphenol, urea derivatives, metal-containing salicylic acid compounds, metal-containing naphthoic acid compounds, boron compounds, quaternary ammonium salts, calixarenes, and resin-based charge control agents. On the other hand, examples of toner that can be controlled to have a positive charge include the following. Nigrosine and nigrosine modifications such as fatty acid metal salts; guanidine compounds; imidazole compounds; onium salts such as quaternary ammonium salts such as tributylbenzylammonium-1-hydroxy-4-naphthosulfonate, tetrabutylammonium tetrafluoroborate, and their analogues such as phosphonium salts, and lake pigments thereof; triphenylmethane dyes and lake pigments thereof (lake agents include phosphotungstic acid, phosphomolybdic acid, phosphotungstomolybdic acid, tannic acid, lauric acid, gallic acid, ferricyanide, ferrocyanide, etc.); metal salts of higher fatty acids; resin-based charge control agents.

[0069] The methods for measuring the various physical properties of the toner will be described below. <Separation of toner and additives> First, in the case where the surface of the toner particles has been treated with an external additive or the like, the external additive is removed by the following method to obtain the toner particles. Add 160 g of sucrose (Kishida Chemical) to 100 mL of ion-exchanged water and dissolve in a hot water bath to prepare a concentrated sucrose solution. Add 31 g of the concentrated sucrose solution and 6 mL of Contaminon N (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments, consisting of nonionic surfactants, anionic surfactants, and organic builders, manufactured by Wako Pure Chemical Industries, Ltd.) to a centrifuge tube (50 mL capacity) to prepare a dispersion. Add 1.0 g of toner to this dispersion and break up the toner clumps with a spatula or similar. The centrifuge tube is shaken in a shaker at 350 strokes per minute (spm) for 20 minutes. After shaking, the solution is transferred to a glass tube for a swing rotor (capacity 50 mL) and separated in a centrifuge (H-9R, manufactured by Kokusan Co., Ltd.) at 3500 rpm for 30 minutes. This operation separates the toner particles from the removed external additives. Visually check that the toner and the aqueous solution are sufficiently separated, and collect the toner that has separated to the top layer with a spatula. The collected toner is filtered through a vacuum filter, and then dried in a dryer for at least one hour to obtain toner particles. This operation is repeated several times to ensure the required amount.

[0070] <Method of extracting Resin A and Resin B from toner particles> Resin A in the toner particles is extracted by separating the extract using tetrahydrofuran (THF) using a solvent gradient elution method. The preparation method is shown below. Weigh out 10.0 g of toner particles, place them in a cylindrical filter paper (Toyo Roshi No. 84) and place them in a Soxhlet extractor. Extract for 20 hours using 200 mL of THF as the solvent, and the solid obtained by removing the solvent from the extract is the THF-soluble fraction. The THF-soluble fraction contains resin A or resin B. Repeat this process multiple times to obtain the required amount of THF-soluble fraction. For the solvent gradient elution method, a gradient preparative HPLC (Shimadzu LC-20AP high pressure gradient preparative system, Waters SunFire preparative column 50 mm φ 250 mm) is used. The column temperature is 30°C, the flow rate is 50 mL / min, and the mobile phase uses acetonitrile as a poor solvent and THF as a good solvent. 0.02 g of the THF-soluble fraction obtained by extraction was dissolved in 1.5 mL of THF to prepare the sample for separation. The mobile phase started with a composition of 100% acetonitrile, and 5 minutes after the sample was injected, the ratio of THF was increased by 4% per minute until the mobile phase composition was 100% THF over 25 minutes. The components could be separated by drying the obtained fraction. This allowed the production of resin A or resin B. Which fraction is resin A or resin B? 13 It can be distinguished by C-NMR measurement.

[0071] <Measurement of Resin A Content and Resin B Content in Toner Particles> The contents of resin A and resin B in the toner particles can be calculated from the amounts of each resin or polymerizable monomers capable of forming each resin charged when producing the toner particles. In addition, by identifying and extracting resin A and resin B from each fraction obtained by a method for extracting resin A and resin B from toner particles, the respective contents can be calculated for the toner particles subjected to a Soxhlet extractor.

[0072] <How to confirm the structure of Resin A and Resin B> Polymer moiety P in formula (1) of resin A 1 , L 1 Part, R 1 ~R 3 The monomer unit structures in resin B represented by the moiety and formula (2) and formula (3) are 1 H-NMR analysis, 13 C-NMR analysis, 29 This is carried out using Si-NMR. The measurement sample is either resin A or resin B itself, or resin A or resin B extracted from toner particles by the above-mentioned extraction method. R in formula (1) 1 ~R 3 The alkoxy group or hydroxy group in 29 The valence of the alkoxy group or hydroxy group relative to the silicon atom can be determined by the method shown in "Si-NMR (solid) measurement conditions."

[0073] ( 29 Si-NMR (solid state) measurement conditions Equipment: JEOL RESONANCE JNM-ECX500II Sample tube: 3.2mmφ Sample size: 150mg Measurement temperature: room temperature Pulse mode: CP / MAS Measurement nuclear frequency: 97.38MHz ( 29 Si) Reference material: DSS (external standard: 1.534ppm) Sample rotation speed: 10kHz Contact time: 10ms Delay time: 2s Number of times: 2000 to 8000 From the above measurement, the abundance ratio of multiple silane components according to the number of oxygen atoms bonded to Si can be calculated by peak separation and integration using curve fitting. In this way, R in formula (1) 1 ~R 3 The valence of the alkoxy group or hydroxy group relative to the silicon atom can be confirmed. P in formula (1) 1 , L 1 and R 1 ~R 3 The structure of the monomer unit in resin B represented by formula (2) and formula (3) is 13 This can be confirmed by C-NMR (solid state) measurement. The measurement conditions are as follows.

[0074] ( 13 C-NMR (solid state) measurement conditions Equipment: JEOL RESONANCE JNM-ECX500II Sample tube: 3.2mmφ Sample size: 150mg Measurement temperature: room temperature Pulse mode: CP / MAS Measurement nuclear frequency: 123.25MHz ( 13 C) Reference substance: Adamantane (external standard: 29.5ppm) Sample rotation speed: 20kHz Contact time: 2ms Delay time: 2s Number of times accumulated: 1024 P in formula (1) 1 , L 1 , R 1 ~R 3 The peaks are separated according to the types of monomer units in resin B represented by formulas (2) and (3), and each peak is identified to obtain P 1 , L 1 , R 1 ~R 3 To determine the structures of formula (2) and formula (3).

[0075] <Method of measuring weight average molecular weight (Mw)> The weight average molecular weight (Mw) of a polymer, resin or toner particle is measured by gel permeation chromatography (GPC) as follows. First, the sample is dissolved in tetrahydrofuran (THF) at room temperature for 24 hours. The resulting solution is then filtered through a solvent-resistant membrane filter "Myshoridisc" (manufactured by Tosoh Corporation) with a pore size of 0.2 μm to obtain a sample solution. The sample solution is prepared so that the concentration of components soluble in THF is approximately 0.8 mass%. This sample solution is used to perform measurements under the following conditions. Equipment: HLC8120 GPC (detector: RI) (Tosoh Corporation) Column: Shodex KF-801, 802, 803, 804, 805, 806, 807 (Showa Denko) Eluent: tetrahydrofuran (THF) Flow rate: 1.0mL / min Oven temperature: 40.0℃ Sample injection volume: 0.10 mL In calculating the molecular weight of the sample, a molecular weight calibration curve prepared using standard polystyrene resins (product names: "TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500", manufactured by Tosoh Corporation) is used.

[0076] <Calculation Methods of SPA and SPB> SPA and SPB are obtained as follows according to the calculation method proposed by Fedors. For each atom or atomic group in the molecular structure, the evaporation energy (Δei) (cal / mol) and molar volume (Δvi) (cm / mol) are obtained from the table described in "polym.Eng.Sci., 3 14(2), 147 - 154(1974)", and (4.184×ΣΔei / ΣΔvi) 0.5 is taken as the SP value (J / cm 3 ) 0.5 That is. Specifically, the evaporation energy (Δei) and molar volume (Δvi) of the monomer units derived from the monomers constituting resin A or resin B are obtained for each monomer unit, and the product with the molar ratio (j) of each monomer unit in resin A is calculated respectively. Then, the sum of the evaporation energies of each monomer unit is divided by the sum of the molar volumes to obtain the value calculated from the following formula (5). SPA or SPB = {4.184×(Σj×ΣΔei) / (Σj×ΣΔvi)} 0.5 (5)

[0077] <Measurement Method of Ion Count Derived from Silicon with Mass Number 28 with Respect to Total Ion Count in Mass Numbers 1 to 1800 in TOF - SIMS Measurement> In the measurement of the surface of toner particles by a time - of - flight secondary ion mass spectrometer (TOF - SIMS), the ion count derived from silicon with mass number 28 with respect to the total ion count in mass numbers 1 to 1800 is measured under the following apparatus and measurement conditions. Measuring apparatus: TOFSIMS TRIFT IV (manufactured by ULVAC - PHI, Inc.) Primary ion species: Gold ion (Au + ) Primary ion acceleration voltage: 30 keV Primary ion current value: 2 pA Analysis area: 300×300 μm 2 Number of pixels: 256 x 256 pixels Analysis time: 3min Repetition frequency: 8.2kHz Charge neutralization: on Secondary ion polarity: Positive Secondary ion mass range (m / z): 0.5 to 1850 The analysis was performed using standard software (Win Cadense) from ULVAC-PHI, Inc. The ion count derived from silicon with mass number 28 was calculated as the intensity ratio of the ion count derived from silicon with mass number 28 to the total ion count from mass numbers 1 to 1850.

[0078] <Method of measuring toner particles and weight average particle size (D4) of toner> The toner particles and the weight average particle size (D4) of the toner are measured using a precision particle size distribution measuring device "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.). The measurement is performed under the following conditions. Effective number of measurement channels: 25,000 Total number of control motors: 50,000 Aperture: 100μm Current: 1600μA Gain; 2 The Kd value is measured using a "Standard particle size of 10.0 μm" (Beckman Coulter, Inc.). The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume %, the "Average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen is the weight-average particle size (D4).

[0079] <Method for measuring the content of the structure represented by formula (4) in resin A> The content of the structure represented by formula (4) in resin A is measured using a wavelength dispersive X-ray fluorescence analyzer "Axios" (PANalytical) and the accompanying dedicated software "SuperQ ver.4.0F" (PANalytical) for setting measurement conditions and analyzing measurement data. Rh is used as the anode of the X-ray tube, the measurement atmosphere is vacuum, the measurement diameter (collimator mask diameter) is 27 mm, and the measurement time is 10 seconds. When measuring, a proportional counter (PC) is used, and when measuring heavy elements, a scintillation counter (SC) is used for detection. The measurement sample is prepared by placing 4 g of resin A or tetrahydrofuran soluble matter obtained by the method of isolating resin A from the toner particles in a dedicated aluminum ring for pressing, flattening it, and pressing it at 20 MPa for 60 seconds using a tablet molding compression machine "BRE-32" (manufactured by Maekawa Test Machinery Manufacturing Co., Ltd.) to form a pellet with a thickness of 2 mm and a diameter of 39 mm. In addition, binder particles [product name: Spectro Blend, components: C81.0% by mass, O2.9% by mass, H13.5% by mass, N2.6% by mass, chemical formula: C 19 H 38 SiO2 particles (hydrophobic fumed silica) [product name: AEROSIL NAX50, specific surface area: 40±10 m2] per 100 parts by mass of SiO2 particles (hydrophobic fumed silica) [product name: AEROSIL NAX50, specific surface area: 40±10 m2] 2 0.5 parts by mass of SiO2 particles (carbon content: 0.45% to 0.85%; manufactured by Nippon Aerosil Co., Ltd.) was added and thoroughly mixed using a coffee mill. Similarly, 5.0 parts by mass and 10.0 parts by mass of the SiO2 particles were mixed with the binder particles, respectively, to prepare samples for the calibration curve. For each sample, a pellet of the calibration curve sample is prepared as described above using a tablet press, and the count rate (unit: cps) of the Si-Kα ray observed at a diffraction angle (2θ) = 109.08° when PET is used as the analyzing crystal is measured. In this case, the acceleration voltage and current value of the X-ray generator are 24 kV and 100 mA, respectively. A linear function calibration curve is obtained by plotting the obtained X-ray count rate on the vertical axis and the amount of SiO2 particles added in each calibration curve sample on the horizontal axis. Next, the resin A to be analyzed or the tetrahydrofuran soluble matter obtained by the method of isolating resin A from the toner particles is pelletized as described above using a tablet molding compression machine, and the count rate of the Si-Kα radiation is measured. Then, the content of silicon atoms in the calibration curve is obtained. From the obtained silicon atom content and the structure of resin A obtained by the method for confirming the structure of resin A described above, the content of the structure represented by formula (4) can be obtained. EXAMPLES

[0080] The present disclosure will be specifically described below with reference to examples, but the present disclosure is not limited to these examples. Unless otherwise specified, the "parts" of each material in the examples and comparative examples are all based on mass.

[0081] <Production of Resin S1> Resin S1 was prepared according to the following procedure. The following materials were charged into an autoclave equipped with a pressure reducing device, a water separating device, a nitrogen gas introducing device, a temperature measuring device, and a stirrer, and the reaction was carried out under a nitrogen atmosphere at normal pressure and 200°C. When the desired molecular weight was obtained, the reaction was stopped by cooling. Bisphenol A-propylene oxide 2 mole adduct: 71.3 parts Terephthalic acid: 14.0 parts Isophthalic acid: 14.0 parts Tetrabutoxytitanate: 0.1 parts Trimellitic acid 0.9 parts Thereafter, the mixture was reacted for 2 hours under a reduced pressure of 10 mmHg to 20 mmHg to obtain resin S1. The weight average molecular weight (Mw) of the obtained resin S1 was 19,000.

[0082] <Production of Resins S2 to S6> As shown in Table 1, resins S2 to S6 were produced in the same manner as resin S1, except that the alcohol component and the acid component were changed and the reaction time was appropriately changed according to the desired molecular weight.

[0083] [Table 1] In Table 1, BPA-PO2 mol represents a bisphenol A-propylene oxide 2 mol adduct, TPA represents terephthalic acid, IPA represents isophthalic acid, and TMA represents trimellitic acid.

[0084] <Production of Resin V1> Resin V1 was prepared according to the following procedure. 100.0 parts of propylene glycol monomethyl ether was heated while replacing with nitrogen, and refluxed at a liquid temperature of 120° C. or higher. A mixture of 97.0 parts of styrene as a polymerizable monomer, 3.0 parts of methacrylic acid, and 0.50 parts of tert-butyl peroxybenzoate (manufactured by NOF Corporation, product name: Perbutyl Z) as a polymerization initiator was added dropwise thereto over a period of 3 hours. After the dropwise addition was completed, the solution was stirred for 3 hours, and then distilled at normal pressure while increasing the liquid temperature to 170°C. After the liquid temperature reached 170°C, the pressure was reduced to 1 hPa, and distillation was performed for 1 hour to remove the solvent, and a resin solid was obtained. The resin solid was dissolved in tetrahydrofuran, reprecipitated with n-hexane, and the precipitated solid was filtered to obtain resin V1. The weight average molecular weight (Mw) of the obtained resin V1 was 24,500.

[0085] <Manufacture of Resins V2 to V6> Resins V2 to V6 were produced in the same manner as in the production of Resin V1, except that the polymerizable monomers were changed as shown in Table 2.

[0086] [Table 2]

[0087] <Production Example of Resin A1> Resin A1 was prepared according to the following procedure. 100.0 parts of resin S1 was dissolved in 400.00 parts of N,N-dimethylacetamide, and 1.6 parts of 3-aminopropyltrimethoxysilane as a silane compound, 3.0 parts of triethylamine, and 2.4 parts of DMT-MM [4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride] as a condensation agent were added, and the mixture was incubated at room temperature for 5 hours. Stirred. After the reaction was completed, the solution was dropped into methanol to reprecipitate and filter, thereby obtaining resin A1. The weight average molecular weight MwA of resin A1 was 20000. The physical properties of the obtained resin A1 are shown in Table 4.

[0088] <Production examples of resins A2, A4, and A7-14> Resins A2, A4, and A7 to 14 were obtained in the same manner as in Production Example for Resin A1, except that the base resin, the type and amount of silane compound added, and the amount of DMT-MM added were changed as shown in Table 3. The structures and physical properties of the obtained Resins A2, A4, and A7 to 14 are shown in Table 4.

[0089] [Table 3]

[0090] <Production example of resin A3> Resin A3 was prepared according to the following procedure. 100.0 parts of resin V2 was dissolved in 500.00 parts of chloroform, and 2.0 parts of 3-isocyanatepropyltrimethoxysilane and 0.50 parts of titanium (IV) tetraisopropoxide were added under a nitrogen atmosphere and stirred at room temperature for 5 hours. After the reaction was completed, the solution was dropped into methanol, reprecipitated, and filtered to obtain resin A3. The structure and physical properties of the obtained resin A3 are shown in Table 4.

[0091] <Resin A5 manufacturing example> Resin A5 was obtained in the same manner as in the production example of Resin V1, except that methacrylic acid was replaced with 3-methacryloxypropyltrimethoxysilane. The structure and physical properties of the obtained Resin A5 are shown in Table 4.

[0092] <Production example of resin A6> 100.0 parts of resin S2 was dissolved in 1000.0 parts of toluene, and 2.5 parts of 3-methacryloxypropyltrimethoxysilane and 0.6 parts of tert-butyl peroxybenzoate [manufactured by NOF Corp., trade name: Perbutyl Z] were added under a nitrogen atmosphere, and the mixture was reacted at 100°C for 5 hours. The resulting solution was reprecipitated in methanol, filtered and washed, and then vacuum dried to obtain resin A6. The structure and physical properties of the resulting resin A6 are shown in Table 4.

[0093] <Production example of resin A15> Resin A15 was obtained in the same manner as in the production example of Resin V1, except that 97.0 parts of styrene were replaced with 98.0 parts of styrene and 3.0 parts of methacrylic acid were replaced with 2.0 parts of vinyltriethoxysilane. The structure and physical properties of the obtained Resin A15 are shown in Table 4.

[0094] <Production example of resin A16> A solution of 10.0 parts of resin A2 dissolved in 90.0 parts of toluene was mixed with 400.0 parts of pure water and stirred, the pH was adjusted to 4.0 using dilute hydrochloric acid, and the mixture was stirred at room temperature for 10.8 hours. The stirring was then stopped and the mixture was transferred to a separatory funnel to extract the oil phase. The oil phase was concentrated and reprecipitated with methanol to obtain resin A16. The obtained resin A16 29 When analyzed by Si-NMR (solid state) measurement, R in formula (1) 1 ~R 3 The structure and physical properties of the obtained resin A16 are shown in Table 4.

[0095] [Table 4] Production examples of resins A17 to A23 will be described later.

[0096] <Production Example of Toner Particle 1> Into a reaction vessel, 390.0 parts of ion-exchanged water and 14.0 parts of sodium phosphate (12-hydrate) (manufactured by Rasa Kogyo Co., Ltd.) were added, and the mixture was kept warm at 65°C for 1 hour while purging with nitrogen. Next, an aqueous calcium chloride solution in which 9.2 parts of calcium chloride (2-hydrate) was dissolved in 10.0 parts of ion-exchanged water was added all at once using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) while stirring at 12,000 rpm, to prepare an aqueous medium containing a dispersion stabilizer. Furthermore, hydrochloric acid was added to the aqueous medium to adjust the pH to 6.0, and aqueous medium 1 was obtained. Next, the following materials were mixed: Behenyl acrylate 60.0 parts Methacrylonitrile 30.0 parts Styrene 10.0 parts Resin A1 2.0 parts Wax (Fischer-Tropsch wax, melting point: 78°C) 9.0 parts ·CIPIGMENT BLUE 15:3 6.0 copies The mixture was kept at 65° C. and uniformly dissolved and dispersed using a TK homomixer at 500 rpm to prepare a polymerizable monomer composition 1. While maintaining the temperature of the aqueous medium 1 at 70° C. and the rotation speed of the stirring device at 12,000 rpm, the polymerizable monomer composition 1 was charged into the aqueous medium 1, and 8.0 parts of t-butyl peroxypivalate was added as a polymerization initiator. Granulation was continued for 10 minutes while maintaining the stirring speed at 12,000 rpm. The stirring device was changed to a stirrer equipped with a propeller stirring blade, and polymerization was carried out for 5 hours while stirring at 150 rpm and maintaining the temperature at 70°C. The temperature was then increased to 85°C and maintained at that temperature for 2 hours, and then cooled to room temperature, thereby obtaining toner particle dispersion 1. Hydrochloric acid was added to the obtained toner particle dispersion 1 to adjust the pH to 1.4 or less, the dispersion stabilizer was dissolved, and the mixture was filtered, washed, and dried to obtain toner particles 1. Table 5 shows the physical properties of resin B1 of toner particles 1. Table 8 shows the physical properties of toner particles 1.

[0097] <Production Examples of Toner Particles 2 to 31, 34 to 36, and Comparative Toner Particles 1 to 4> Toner particles 2 to 31, 34 to 36 and comparative toner particles 1 to 4 were produced in the same manner as in the production example of toner particle 1, except that the types and amounts of raw materials were changed as shown in Table 6. Table 8 shows the physical properties of resins B1 to B17 of toner particles 2 to 31, 34 to 36 and comparative toner particles 1 to 4.

[0098] [Table 5]

[0099] [Table 6]

[0100] In Table 6, BHA stands for behenyl acrylate, OCA stands for octacosyl acrylate, STA stands for stearyl acrylate, LA stands for lauryl acrylate, OA stands for octyl acrylate, nBA stands for n-butyl acrylate, MN stands for methacrylonitrile, and AN stands for acrylonitrile.

[0101] <Production Example of Toner Particles 32> (Manufacture of Resin B18) Behenyl acrylate 60.0 parts Methacrylonitrile 30.0 parts Styrene 10.0 parts Toluene 100.0 parts Mix the above materials, heat to 70℃, and then add t-butyl as a polymerization initiator while stirring. 1.0 part of peroxypivalate was added. The mixture was then maintained at 70°C for 5 hours to polymerize, and was then heated to 85°C and maintained for 2 hours. After cooling, the mixture was reprecipitated in methanol, filtered, and dried to obtain resin B18. The physical properties of the obtained resin B18 are shown in Table 5.

[0102] Resin B18 100.0 parts ·CIPIGMENT BLUE 15:3 7.0 copies ·Resin A2 2.0 parts Paraffin wax (DSC peak temperature: 80°C) 5.0 parts The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.), and then mixed in a twin-screw mixer (PCM-30, manufactured by Ikegai Iron Works Co., Ltd.) at a rotation speed of 3.3 s. -1 The mixture was mixed at a mixing temperature of 120°C. The mixture was cooled and coarsely pulverized to 1 mm or less using a hammer mill to obtain a coarsely pulverized product. The coarsely pulverized product was finely pulverized using a mechanical pulverizer (T-250 manufactured by Turbo Kogyo Co., Ltd.). The finely pulverized powder was further classified using a multi-division classifier utilizing the Coanda effect to obtain toner particles 32 having a weight average particle size of 6.1 μm. The MA / MB of the obtained toner particles 32 was 0.0200.

[0103] <Production Example of Toner Particle 33> (Production of dispersion of resin B18 resin particles) 60 parts of resin B18 was added to 200 g of toluene (manufactured by Wako Pure Chemical Industries), heated to 90°C, and then stirred for 3 hours to dissolve. 180 parts of ion-exchanged water in which 6 parts of anionic surfactant (manufactured by Daiichi Kogyo Seiyaku: Neogen RK) and 3 parts of anionic surfactant (manufactured by Nippon Oil & Fats: Nonsar LN1) were dissolved were added to the toluene solution in which resin B18 was dissolved. Then, the mixture was thoroughly stirred at 4000 rpm using an ultra-high speed stirring device TK Robomix (manufactured by Primix Co., Ltd.). After that, the mixture was dispersed for about 1 hour using a high-pressure impact type dispersing machine Nanomizer (manufactured by Yoshida Kikai Kogyo Co., Ltd.), and then the toluene was removed using an evaporator to obtain a dispersion of resin B18 resin fine particles.

[0104] (Preparation of Dispersion of Resin A2) A dispersion of Resin A2 was obtained in the same manner as in the production of the dispersion of Resin B18 fine particles, except that Resin B18 was changed to Resin A2.

[0105] (Production of dispersion of release agent particles) Release agent (HNP-51, melting point 78°C, made by Nippon Seiro) 20.0 parts Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK) 1.0 part -Ion-exchanged water 79.0 parts The above formulation was placed in a mixing vessel equipped with a stirrer, heated to 90°C, and circulated through a Clearmix W Motion (manufactured by M Technique) while being stirred at a shear stirring section with a rotor outer diameter of 3 cm and a clearance of 0.3 mm under conditions of a rotor rotation speed of 19,000 r / min and a screen rotation speed of 19,000 r / min. After dispersing for 60 minutes, the mixture was cooled to 40°C under cooling treatment conditions of a rotor rotation speed of 1,000 r / min, a screen rotation speed of 0 r / min, and a cooling rate of 10°C / min, to obtain a dispersion of release agent fine particles.

[0106] (Production of pigment dispersion) ·CIPigment BLUE 15:3 10.0 copies 78.0 parts of ion-exchanged water Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK) 2.0 parts The above materials were mixed and then dispersed for 1 hour using a high-pressure impact disperser Nanomizer (manufactured by Yoshida Kikai Kogyo Co., Ltd.) to prepare a pigment dispersion liquid.

[0107] Resin B18 fine particle dispersion (solid content 28%) 320.0 parts Pigment dispersion (solid content 11%) 50.0 parts Dispersion of release agent particles (20% solids) 50.0 parts Dispersion of Resin A2 (28% solids) 3.2 parts The above materials were put into a round stainless steel flask and mixed. An aqueous solution of 8 parts of magnesium sulfate dissolved in 98.0 parts of ion-exchanged water was added thereto, and dispersed for 10 minutes at 5000 r / min using a homogenizer (IKA Ultra Turrax T50). After that, the mixture was heated to 50°C in a heating water bath using a stirring blade while appropriately adjusting the rotation speed so that the mixture was stirred. After holding at 50°C for 1 hour, the weight average particle diameter of the formed aggregated particles was measured. As a result, it was confirmed that aggregated particles with a weight average particle diameter of about 6.0 μm were formed. To the dispersion of the obtained aggregated particles, an aqueous solution in which 40 parts of sodium ethylenediaminetetraacetate was dissolved in 360 parts of ion-exchanged water was added, and then 2800 parts of ion-exchanged water was added. The mixture was heated to 80°C while continuing to stir, and kept in a sealed state for 2 hours to obtain fully fused particles. After that, after filtration and solid-liquid separation, the filtered matter was thoroughly washed with ion-exchanged water and dried using a vacuum dryer, toner particles 33 having a weight average particle size of 5.8 μm were obtained. The MA / MB of the obtained toner particles 33 was 0.0100.

[0108] <Production Example of Toner Particle 37> 98.5 parts of styrene and 1.5 parts of 3-methacryloxypropyltrimethoxysilane (MPTMS) were mixed using a stirrer until a homogeneous phase was formed, obtaining a monomer solution 1. Next, 50 parts of ion-exchanged water was measured out, and 50 parts of the monomer solution 1 was added thereto, and a dispersion treatment was carried out using an ultrasonic homogenizer (manufactured by SONICS & MATERIAL) at 97% intensity and 25°C for 1 minute, obtaining a monomer suspension 1. Toner base particle dispersion 37 was obtained in the same manner as in the production example of toner particle 1, except that resin A1 was not added, the steps from adding hydrochloric acid to drying were not performed, and the solid content concentration of the toner particle dispersion was adjusted to 20.0 mass % by adding ion exchanged water, decanting, and filtering. 500 parts of the obtained toner base particle dispersion 37 was placed in a reaction vessel equipped with a stirrer, heated to 70°C while stirring, and purged with nitrogen for 1 hour. 2.0 parts of the monomer suspension 1 and 0.1 parts of potassium persulfate (KPS) were added to the reaction vessel, and a reaction was carried out at 70°C for 3 hours to form resin A17 on the surface of the toner base particles. After cooling to room temperature, hydrochloric acid was added to adjust the pH to 1.4 or less, and stirring was performed for 1 hour. Thereafter, filtration, washing, and drying were performed in the same manner as in the production example of toner particles 1, and toner particles 37 were obtained. The physical properties of the obtained toner particles 37 are shown in Table 8.

[0109] <Production Examples of Toner Particles 38 to 44> Toner particles 38 to 44 were produced in the same manner as in the production example of toner particle 37, except that the composition of resin B, the composition of the monomer solution, and the number of parts of the monomer suspension added were changed as shown in Tables 7-1 and 7-2. The physical properties of the obtained toner particles 38 to 44 are shown in Table 8.

[0110] <Production Example of Toner Particle 45> Toner base particle dispersion 45 was obtained in the same manner as in the production example of toner particle 33, except that no dispersion of resin A2 was added, the processes of filtering, washing and drying the fused particles were not performed, and the fused particles were subjected to addition of ion exchanged water, decantation and filtration, and the solids concentration of the toner particle dispersion was adjusted to 20.0 mass %. Toner particles 45 were obtained in the same manner as in the production example of toner particles 37, except that toner base particle dispersion liquid 37 was changed to toner base particle dispersion liquid 45. The physical properties of toner particles 45 obtained are shown in Table 8.

[0111] <Production Example of Toner Particle 46> Toner base particles 46 were obtained in the same manner as in the production example of toner particles 32, except that resin A2 was not added. 100 parts by mass of toner base particles 46 and 1.0 part by mass of Contaminon N were weighed out and added to 400 parts by mass of ion-exchanged water, and dispersed using an ultrasonic disperser to obtain toner base particle dispersion liquid 46. Thereafter, toner particles 46 were obtained in the same manner as in the production example of toner particles 37 above, except that toner base particle dispersion liquid 37 was changed to toner base particle dispersion liquid 46 and that the monomer dissolving liquid was changed as shown in Table 7-2. The physical properties of the obtained toner particles 46 are shown in Table 8.

[0112] [Table 7-1] (In Table 7-1, BHA stands for behenyl acrylate, nBA stands for n-butyl acrylate, and MN stands for methacrylonitrile.)

[0113] [Table 7-2] (In Table 7-2, MPTMS represents 3-methacryloxypropyltrimethoxysilane, MOTMS represents 8-methacryloxyoctyltrimethoxysilane, and MN represents methacrylonitrile.)

[0114] [Table 8] *: Ion count derived from silicon with mass number 28 relative to total ion count with mass numbers 1 to 1800 in TOF-SIMS measurements of the toner particle surface

[0115] <Production Examples of Toners 1 to 46 and Comparative Toners 1 to 4> For 100.0 parts of each of the obtained toner particles 1 to 46 and the comparative toner particles 1 to 4, the BET value was 200 m 2 / g and 0.6 parts of hydrophobic silica fine particles having a number average particle size of primary particles of 8 nm were mixed in a Henschel mixer (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.). After the above-mentioned mixing treatment, the mixture was sieved through a mesh having an opening of 150 μm to obtain toners 1 to 46 and comparative toners 1 to 4, respectively.

[0116] <Examples 1 to 46> In Examples 1 to 46, evaluations were carried out using Toners 1 to 46, respectively. The evaluation methods and results are shown below.

[0117] <Comparative Examples 1 to 4> In Comparative Examples 1 to 4, evaluation was carried out using Comparative Toners 1 to 4, respectively. The evaluation was carried out in the same manner as in Examples 1 to 46.

[0118] <Evaluation method for adhesiveness of discharged paper> The evaluation was carried out in a high temperature and high humidity environment (30℃ / 80%RH) using a modified LBP712Ci (Canon) color laser printer. The modifications were as follows: The gear and software of the evaluation machine were changed to set the process speed to 350 mm / sec and the fixing temperature to 180°C. The cartridge used for the evaluation was a cyan cartridge. That is, the product toner was removed from a commercially available cyan cartridge, the inside was cleaned with an air blower, and then 50 g of the toner to be evaluated was filled in. In addition, the product toner was removed from each of the magenta, yellow, and black stations, and magenta, yellow, and black cartridges with the toner remaining amount detection mechanism disabled were inserted. Under the above conditions, the toner loading amount is 0.45 mg / cm 2 An image measuring 25.0 cm in length and 20.0 cm in width was printed in continuous double-sided mode, and the media (XEROX4200 paper (75 g / m 2 The evaluation was carried out while changing the number of sheets loaded. After printing a specified number of sheets on the output tray and leaving it for one minute, the toner stains on the bottom sheet of the stack (the first printed sheet) were evaluated according to the following criteria. The evaluation results are shown in Table 9. (Evaluation Criteria) A: With a capacity of 250 sheets, there is no toner staining on the paper. B: Toner stains on paper occurred when the number of sheets loaded was between 150 and 250. C: Toner stains on paper occurred when the number of sheets loaded was between 50 and 150. D: Toner stains on paper occur when the number of sheets loaded is less than 50

[0119] <Evaluation method for low-temperature fixability> A color laser printer (HP Color LaserJet 3525dn, manufactured by HP) with the fixing unit removed was prepared, the toner was removed from the cyan cartridge, and the toner to be evaluated was replaced. Next, a medium (GF-C081, basis weight 81.4 g / m 2 ) was used to create an unfixed toner image (0.45 mg / cm2) measuring 4.0 cm in length and 10.0 cm in width. 2 ) was formed at a position 1.0 cm from the upper end in the paper feed direction. Next, the removed fixing unit was modified so that the fixing temperature and process speed could be adjusted, and the process speed was set to 230 mm / s under a normal temperature and humidity environment (23°C, 60% RH). The surface temperature of the fixing sleeve was changed from 100°C to 180°C in increments of 5°C to fix the unfixed image. The minimum fixing temperature was set to 5°C higher than the temperature at which the fixed image would cold off, and the toner was ranked according to the following evaluation criteria. A rating of C or higher was deemed to indicate good low-temperature fixing ability. The results are shown in Table 9. [Evaluation Criteria] A: The minimum fixing temperature is 115℃ or less B: Minimum fixing temperature is 120℃ or 125℃ C: Minimum fixing temperature is 130℃ or 135℃ D: Minimum fixing temperature is 140℃ or higher

[0120] <Method for evaluating heat resistance storage stability> 5 g of each toner was placed in a 50 cc resin cup and left for 72 hours at a temperature of 50°C / humidity of 10% RH and at a temperature of 55°C / humidity of 10% RH. The toner was examined for the presence or absence of agglomerates. In this disclosure, a rating of C or higher was deemed to indicate good heat-resistant storage stability. The results are shown in Table 9. [Evaluation Criteria] A: No clumps formed B: Slight clumps formed, crumbles when lightly pressed with fingers C: Agglomerates form, but do not crumble when lightly pressed with fingers D: Completely aggregated

[0121] <Image quality evaluation in low temperature and low humidity environments> As an index for evaluating image quality, fogging in non-image areas was evaluated. The fog was evaluated in a low temperature and low humidity environment (15°C / 10% RH). XEROX 4200 paper (75 g / m, manufactured by XEROX) was used as the evaluation paper. 2) was used. The evaluation machine and toner cartridge used were the same as those used in the evaluation of paper discharge adhesion. A solid white image was output, and the worst reflection density of the white background was taken as Ds, the average reflection density of the transfer material before image formation was taken as Dr (%), and [Dr-Ds (%)] was taken as the fog value. The reflection density of the white background was measured using a reflection densitometer (Reflectometer Model TC-6DS, manufactured by Tokyo Denshoku Co., Ltd.) and an amber light filter was used. The smaller the value, the better the evaluation. The evaluation criteria are as follows. The evaluation results are shown in Table 9. (Evaluation Criteria) A: Less than 0.50% B: 0.50% or more and less than 1.50% C: 1.50% or more and less than 3.00% D: 3.00% or more

[0122] [Table 9]

Claims

1. A toner having toner particles having a resin A and a resin B, The resin A has a structure represented by the following formula (1): The resin B has a monomer unit represented by the following formula (2) and a monomer unit represented by the following formula (3), The toner is characterized in that, when the surface of the toner particles is measured with a time-of-flight secondary ion mass spectrometer, the ion count derived from silicon having a mass number of 28 relative to the total ion count in the mass numbers of 1 to 1,800 is 0.0010 to 0.0050. 【Chemistry 1】 [In formula (1), P 1 represents a polymer moiety, R 1 ~R 3 each independently represents a hydrogen atom, an alkyl group having one or more carbon atoms, an alkoxy group having one or more carbon atoms, or a hydroxy group; R 1 ~R 3 at least one of represents an alkoxy group or a hydroxy group having one or more carbon atoms, and m represents a positive integer; L 1 is an alkylene group having 8 or less carbon atoms, *-O-**, *-OR 5 -**, *-NH-**, *-NH-R 6 -**, where * represents the bond to the carbonyl group in formula (1), ** represents the bond to the silicon atom, and R 5 , R 6 are each an alkylene group having up to 8 carbon atoms, each of which may have a hydroxyl group as a substituent; When m is 2 or more, a plurality of L 1 , multiple R 1 , multiple R 2 and multiple R 3 may be the same or different. 【Chemistry 2】 [In formula (2), R 4 represents a hydrogen atom or a methyl group, and n represents an integer of 11 to 35. 【Chemistry 3】 [In formula (3), R 7 represents a hydrogen atom or a methyl group.

2. A toner having toner particles having a resin A and a resin B, The resin A has a structure represented by the following formula (1): The resin B has a monomer unit represented by the following formula (2): the content of the resin A in the toner particles is MA (mass%) and the content of the resin B in the toner particles is MB (mass%), MA / MB satisfies 0.0050≦[MA / MB]≦0.2000, In the measurement of the surface of the toner particles by a time-of-flight secondary ion mass spectrometer, the mass number The ion count derived from silicon having a mass number of 28 relative to the total ion count in the range of 1 to 1800 is 0.0010 to 0.0050. A toner characterized by: 【Chemistry 4】 [In formula (1), P 1 represents a polymer moiety, R 1 ~R 3 each independently represents a hydrogen atom, an alkyl group having one or more carbon atoms, an alkoxy group having one or more carbon atoms, or a hydroxy group; R 1 ~R 3 at least one of represents an alkoxy group or a hydroxy group having one or more carbon atoms, and m represents a positive integer; L 1 is an alkylene group having 8 or less carbon atoms, *-O-**, *-OR 5 -**, *-NH-**, *-NH-R 6 -**, where * represents the bond to the carbonyl group in formula (1), ** represents the bond to the silicon atom, and R 5 , R 6 are each an alkylene group having up to 8 carbon atoms, each of which may have a hydroxyl group as a substituent; When m is 2 or more, a plurality of L 1 , multiple R 1 , multiple R 2 and multiple R 3 may be the same or different. 【Chemistry 5】 [In formula (2), R 4 represents a hydrogen atom or a methyl group, and n represents an integer of 11 to 35.

3. A toner having toner particles having a resin A and a resin B, The resin A has a structure represented by the following formula (1): The resin B has a monomer unit represented by the following formula (2): In a measurement of the surface of the toner particles using a time-of-flight secondary ion mass spectrometer, the ion count derived from silicon having a mass number of 28 relative to the total ion count in the mass numbers of 1 to 1800 is 0.0010 to 0.0050. A toner characterized by: 【Chemistry 6】 [In formula (1), P 1 represents a polymer moiety, R 1 ~R 3 each independently represents a hydrogen atom, an alkyl group having one or more carbon atoms, an alkoxy group having one or more carbon atoms, or a hydroxy group; R 1 ~R 3 at least one of represents an alkoxy group or a hydroxy group having one or more carbon atoms, and m represents a positive integer; L 1 is an alkylene group having 8 or less carbon atoms, *-O-**, *-OR 5 -**, *-NH-**, *-NH-R 6 -**, where * represents the bond to the carbonyl group in formula (1), and ** represents the bond to the silicon atom, R 5 , R 6 are each an alkylene group having up to 8 carbon atoms, each of which may have a hydroxyl group as a substituent; When m is 2 or more, a plurality of L 1 , multiple R 1 , multiple R 2 and multiple R 3 may be the same or different. 【Chemistry 7】 [In formula (2), R 4 represents a hydrogen atom or a methyl group, and n represents an integer of 17 to 29.

4. Said L 1 However, *-NHR 6 The toner according to any one of claims 1 to 3, wherein the toner is represented by -**.

5. Said L 1 But *-OR 5 The toner according to any one of claims 1 to 3, wherein the toner is represented by -**.

6. The toner according to any one of claims 1 to 5, wherein the content of the structure represented by the following formula (4) in the resin A is 0.5% by mass or more and 10.0% by mass or less. 【Chemistry 8】 [In formula (4), R 1 ~R 3 is R in formula (1) 1 ~R 3 is the same as L 1 is L in formula (1). 1 is the same as:

7. The SP value of the resin A in the Fedors method is SPA [(J / m 3 ) 0.5 ], and the SP value of the resin B in the Fedors method is SPB [(J / m 3 ) 0.5 ], |SPA-SPB|≦2.00[(J / m 3 ) 0.5 7. The toner according to claim 1, wherein

8. The toner according to any one of claims 1 to 7, wherein the resin A has a weight average molecular weight MwA of 8,000 or more and 50,000 or less.

9. The toner according to any one of claims 1 to 8, wherein the weight average molecular weight MwB of the resin B is 15,000 or more and 250,000 or less.

10. The toner according to any one of claims 1 to 9, wherein the resin A further has a monomer unit represented by the following formula (3): 【Chemistry 9】 [In formula (3), R 7 represents a hydrogen atom or a methyl group.

11. The P 1 The toner according to any one of claims 1 to 10, wherein represents a polyester resin moiety.

12. The P 1 The toner according to any one of claims 1 to 10, wherein represents a vinyl resin moiety.

13. The toner according to any one of claims 1 to 12, wherein the formula (1) is at least one selected from the group consisting of structures represented by the following formulas (7) to (12): 【Chemistry 10】 (R in formulas (7) to (12) 1 ~R 3 , R 5 ~R 6 is R in formula (1) 1 ~R 3 , R 5 ~R 6 and R 7 represents a hydrogen atom or a methyl group, and R in formulas (9) and (10) 9 , R 10 represents an alkylene group having 1 to 6 carbon atoms, and P in formulas (11) and (12) 2 represents the main chain skeleton of the polyester resin.)

14. A method for producing the toner according to any one of claims 1 to 13, comprising the steps of: The method comprises: a step of dispersing the toner base particles containing the resin B in an aqueous medium to obtain a toner slurry; With a step of adding a monomer composition containing a monomer represented by the following formula (6) and a radical polymerization initiator to the obtained toner slurry to form the resin A on the surface of the toner base particles; The toner manufacturing method according to the present invention comprises the steps of: 【Chemistry 11】 [In formula (6), R 8 represents a hydrogen atom or a methyl group.

Citation Information

Patent Citations

  • Emulsion particle and toner prepared by using the same

    JP2002249530A

  • Resin particles for electrophotographic toner and method for manufacturing the same

    JP2008287088A

  • Toner for developing electrostatic charge image, electrostatic charge image developer, process cartridge, image forming method, and image forming apparatus

    JP2010181439A

  • Resin particle and method for producing the same

    JP2011026540A

  • Toner

    JP2015075662A