Kneading method, electrode slurry manufacturing method, electrode manufacturing method, and battery manufacturing method
The hardening method with controlled solid content concentration and stainless steel kneading device minimizes metal contamination in electrode slurry, reducing short circuits and improving battery performance.
Patent Information
- Application Number
- JP2023079051
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Metal contamination during the electrode manufacturing process, particularly during the hardening process of electrode slurry, leads to the deposition of unintended metals inside lithium-ion batteries, causing short circuits.
A hardening method is employed with a solid content concentration of 76 to 87% by mass in the kneading step, using a stainless steel kneading device, and optionally coated with Ti or DLC, to minimize contamination from highly crystalline materials scraping off device components.
Reduces metal contamination in the electrode slurry and batteries, preventing short circuits and enhancing battery performance.
Smart Images

Figure 2024163450000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a kneading method, a method for producing an electrode slurry, a method for producing an electrode, and a method for producing a battery. [Background technology]
[0002] Secondary batteries such as lithium-ion batteries and nickel-metal hydride batteries are becoming increasingly important as power sources for a wide range of products, including portable devices, electric vehicles, unmanned aerial vehicles, etc. In particular, demand for lithium-ion secondary batteries is growing due to their light weight and high energy density.
[0003] A lithium-ion secondary battery basically comprises electrodes (positive and negative electrodes), an electrolyte, and a separator that separates the positive and negative electrodes. The electrodes are made of an electrode active material capable of absorbing and releasing lithium ions, which is held on a current collector such as copper foil or aluminum foil.
[0004] An electrode is manufactured by applying an electrode slurry containing an electrode active material, a conductive assistant, a binder that binds them, and a solvent to a current collector and drying it. A method for manufacturing such an electrode slurry is known in which an electrode active material, a solvent, and the like are kneaded to form a kneaded mixture, and then a solvent is further added to the kneaded mixture to form an electrode slurry (e.g., Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 7-161350 [Patent Document 2] JP 2000-353516 A Summary of the Invention [Problem to be solved by the invention]
[0006] If contamination of the electrodes occurs due to unintended metal contamination, the metal will be ionized inside the battery during use (charging and discharging), and will migrate to the negative electrode and deposit there. This can cause a short circuit inside the battery. Therefore, there is a need to reduce metal contamination in the electrodes.
[0007] An object of the present invention is to provide a kneading method capable of reducing metal contamination. [Means for solving the problem]
[0008] The present invention was made based on the finding that metal contamination of an electrode occurs during the electrode manufacturing process, particularly during the kneading step in producing an electrode slurry.
[0009] More specifically, the present invention has been made based on the following findings. The electrode material may contain a material with high crystallinity. If the viscosity of the kneaded material is high in the thickening process, the material with high crystallinity contained in the kneaded material scrapes off the components of the kneading device, which causes contamination. In order to reduce or prevent this, it is effective to set a threshold value for the solid content concentration of the kneaded material in the thickening process.
[0010] That is, the present invention has the following configuration. [1] A kneading method having a kneading step of kneading an electrode active material, a conductive assistant, a binder, and a solvent to obtain a kneaded material, The method for kneading, wherein the kneaded product in the kneading step has a solid content of 76 to 87 mass %. [2] The method for kneading the mixture according to [1], wherein a kneading device made of stainless steel is used as the kneading device for kneading the mixture. [3] A method for producing an electrode slurry, comprising mixing the kneaded mixture obtained by the kneading method according to [1] or [2] above with a solvent to produce an electrode slurry. [4] A method for producing an electrode, comprising applying the electrode slurry produced by the method for producing an electrode slurry according to the above [3] to a current collector and then drying the applied electrode slurry. [5] A method for producing a battery, comprising the steps of: producing a battery by using an electrode produced by the method for producing an electrode according to [4] above. Effect of the Invention
[0011] According to the present invention, a kneading method capable of reducing metal contamination can be provided.
[0012] According to the present invention, in the kneading step of kneading an electrode active material with a solvent or the like to form a kneaded material, it is possible to reduce metal contamination caused by a kneading device that kneads the kneaded material, thereby obtaining a kneaded material of an electrode active material, a solvent, or the like with reduced metal contamination.
[0013] Furthermore, by using this kneaded material with reduced metal contamination, it is possible to produce an electrode slurry, an electrode, and a battery with reduced metal contamination. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the following embodiment.
[0015] <Method of kneading> The kneading method of the present embodiment includes a kneading step of kneading an electrode active material, a conductive assistant, a binder, and a solvent to obtain a kneaded mixture.
[0016] (electrode active material) Examples of electrode active materials include positive electrode active materials and negative electrode active materials. These electrode active materials include materials with high crystallinity. As described above, if the viscosity of the kneaded material in the hard kneading process is high, the highly crystalline material contained in the kneaded material scrapes off the components of the kneading device such as a mixer, causing contamination. According to the present invention, even if a material with high crystallinity is used as the electrode active material, the effect of reducing contamination can be obtained. Therefore, when a material with high crystallinity is used as the electrode active material, the effect of the present invention can be enjoyed more.
[0017] Examples of such a positive electrode active material include substances having a layered rock salt structure, an olivine structure, and a spinel structure.
[0018] Examples of the positive electrode active material having a layered rock salt structure include LiCoO2, lithium nickel cobalt manganese oxide (NCM), lithium nickel cobalt aluminum oxide (NCA), etc. NCM is a ternary material represented by LiNi x Co y Mn z O2 (x + y + z = 1). Examples of NCM include NCM111 (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2), NCM523 (LiNi 0.5 Co 0.2 Mn 0.3 O2), NCM622 (LiNi 0.6 Co 0.2 Mn 0.2 O2), NCM811 (LiNi 0.8 Co 0.2 Mn 0.2 O2). Also, NCA is a ternary material represented by LiNi x Co y Al z O2 (x + y + z = 1).
[0019] Examples of the positive electrode active material having an olivine structure include LiFePO4, etc. Examples of the positive electrode active material having a spinel structure include LiMn2O4, etc.
[0020] Examples of the negative electrode active material include Li-doped SiO x (0 < x < 2), etc.
[0021] (Conductive aid) Examples of the conductive aid include acetylene black, graphite, artificial graphite, carbon nanotube (CNT), etc. CNT may be a single-layer CNT or a multi-layer CNT.
[0022] (Binder) Examples of the binder (binding material) include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), styrene butadiene rubber (SBR), carboxymethyl cellulose (CMC), vinyl polymers, acrylic polymers, etc. As the binder, polyvinylidene fluoride (PVDF) is preferable.
[0023] (solvent) Examples of the solvent include N-methyl-2-pyrrolidone (NMP), pyrrolidone, N,N-dimethylformamide, tetrahydrofuran, dimethylacetamide, dimethylsulfoxide, hexamethylsulfoxide, tetramethylurea, acetone, methyl ethyl ketone, etc. The solvent is preferably N-methyl-2-pyrrolidone (NMP).
[0024] [Kneading process] In the kneading step, the electrode active material, the conductive assistant, the binder, and the solvent are kneaded to obtain a kneaded product. At this time, the kneading is performed in a state where the solid content concentration of the kneaded product is 76 to 87 mass%. In the kneading step, if the solid content concentration of the kneaded product exceeds 87 mass%, the viscosity of the kneaded product increases, and the electrode active material contained in the kneaded product scrapes off the components of the kneading device, causing contamination of the kneaded product with metal originating from the kneading device. The solid content concentration is preferably 79 mass% or more. In addition, the solid content concentration is preferably 85 mass% or less. The solid content concentration of the kneaded product can be calculated by the following formula. Solid content concentration of kneaded material (mass%) = (mass of solid content contained in kneaded material / mass of kneaded material) x 100
[0025] In the kneading process, the order of mixing the electrode active material, the conductive assistant, the binder, and the solvent is not particularly limited. For example, the electrode active material, the conductive assistant, and the binder, which are solid components, can be dry-mixed (dry-blended) first, and then the solvent can be added and kneaded. The conductive assistant can also be added in portions. In this case, the electrode active material, a part of the conductive assistant, and the binder can be dry-blended (dry-blended), and then the remaining conductive assistant can be added while adding the solvent and kneading. The solid content concentration of the kneaded product can be adjusted by adjusting the amount of solvent added (mixed amount).
[0026] When acetylene black is used as the conductive assistant, the former mixing order is preferred. That is, it is preferred to dry mix (dry blend) the electrode active material (positive electrode active material), acetylene black, and binder, and then add a solvent and knead. When CNT is used as the conductive assistant, the latter mixing order is preferred. That is, it is preferred to dry mix (dry blend) the electrode active material (positive electrode active material), a portion of the CNT, and the binder, and then add a solvent and knead while adding the remaining CNT and kneading.
[0027] The mixing ratio of the electrode active material, conductive assistant, and binder in the kneading step, in terms of mass ratio, when electrode active material:conductive assistant:binder=a:b:c (a+b+c=100), is preferably within the ranges of 40≦a≦99, 0.5≦b≦30, 0.5≦c≦30, and more preferably within the ranges of 80≦a≦98, 1≦b≦10, 1≦c≦10.
[0028] Examples of kneading devices used for kneading include planetary mixers, dispersers, kneaders, homogenizers, roll mills, and ball mills. A planetary mixer is preferable as the kneading device. A stainless steel kneading device is preferable as the kneading device. According to the present invention, even when a stainless steel kneading device is used, contamination of the kneaded material with stainless steel components originating from the kneading device can be reduced. Furthermore, by using a kneading device in which the surfaces of the kneading device members are coated, the contamination can be further reduced. As such coatings, Ti coating, DLC (diamond-like carbon) coating, Teflon (registered trademark) coating, and the like are preferable.
[0029] According to the kneading method of the present invention described above, even if a highly crystalline material is included in the kneaded product in the kneading process, contamination caused by the highly crystalline material scraping off the components of the kneading device can be reduced. As a result, contamination carried over to the electrode slurry, electrode, and battery manufacturing process after the kneading process can be reduced. This suppresses internal short circuits in the battery and improves battery performance.
[0030] <Method of manufacturing electrode slurry> In a method for producing an electrode slurry according to one embodiment of the present invention, the kneaded mixture obtained by the above-mentioned hard kneading method is mixed with a solvent to produce an electrode slurry.
[0031] In the method for producing an electrode slurry of this embodiment, for example, a known method for producing an electrode slurry can be adopted. As the solvent, the same solvent as that used in the above-mentioned kneading step can be used. In addition, as the mixing device, the same device as the above-mentioned kneading device can be used.
[0032] In this embodiment, after the above-mentioned kneading process, a solvent may be added and mixed while continuing kneading with the kneading device to produce an electrode slurry, or the kneaded material obtained in the kneading process may be transferred to another mixing device, and then a solvent may be added to and mixed with the kneaded material to produce an electrode slurry.
[0033] The amount of the solvent added can be appropriately adjusted taking into consideration the coatability of the electrode slurry, etc. Preferably, the solvent is added so that the solid content concentration of the electrode slurry becomes 40 to 74 mass %.
[0034] When the solvent is added and mixed, a disperser may be used as necessary. After mixing, the mixture may be degassed.
[0035] <Electrode manufacturing method> In the method for producing an electrode according to one embodiment of the present invention, the above-mentioned electrode slurry is applied to a current collector and then dried to produce an electrode.
[0036] In the method for producing an electrode according to the present embodiment, for example, a known method for producing an electrode can be adopted. For example, the electrode can be produced by applying the above-mentioned electrode slurry to the surface of a current collector using a coating device such as a die coater or a slit coater, and then drying the applied slurry. After drying, a pressing process may be carried out as appropriate.
[0037] In the case of producing a positive electrode, an electrode slurry containing a positive electrode active material as an electrode active material is produced, and this is applied to a current collector such as aluminum foil, and then dried. In the case of producing a negative electrode, an electrode slurry containing a negative electrode active material as an electrode active material is produced, and this is applied to a current collector such as copper foil, and then dried.
[0038] <Battery manufacturing method> A battery manufacturing method according to one embodiment of the present invention is a method for manufacturing a battery by using an electrode manufactured by the above-described electrode manufacturing method.
[0039] In the method for manufacturing a battery according to the present embodiment, for example, a known method for manufacturing a battery can be adopted. For example, a battery can be manufactured by disposing and assembling the electrodes manufactured by the above-described electrode manufacturing method, an electrolyte, and a separator in an exterior body.
[0040] According to the manufacturing method of the electrode slurry, electrode, and battery of the present invention, the same effects as those described above can be obtained. EXAMPLES
[0041] The present invention will be described below with reference to examples, but the present invention is not limited to the following examples.
[0042] Example 1 LiCoO2 was used as an electrode active material, carbon nanotubes (CNT) as a conductive assistant, polyvinylidene fluoride (PVDF) as a binder, and N-methyl-2-pyrrolidone (NMP) as a solvent, and kneaded in a kneading device. A stainless steel planetary mixer was used as the kneading device. First, LiCoO2, a portion of the CNT, and PVDF were dry-mixed (dry-blended). Then, NMP was added to the blend and kneaded, while the remaining CNT was added and kneaded to produce a kneaded product (kneading process). The solid content of the kneaded product in the kneading process was 85% by mass.
[0043] Example 2 A kneaded product was produced in the same manner as in Example 1, except that the amount of NMP added was changed and the solid content concentration of the kneaded product in the hard kneading step was set to 83 mass %.
[0044] Comparative Example 1 A kneaded product was produced in the same manner as in Example 1, except that the amount of NMP added was changed and the solid content concentration of the kneaded product in the hard kneading step was set to 89 mass %.
[0045] The kneaded materials produced in Examples 1 and 2 and Comparative Example 1 were subjected to elemental mapping by scanning transmission electron microscope-energy dispersive X-ray analysis (STEM-EDX) to examine the presence of Fe and Cr elements derived from the stainless steel kneading machine. The results are shown in Table 1.
[0046] [Table 1]
[0047] As shown in Table 1, according to the kneading method of the present invention, by setting the solid content concentration of the kneaded material in the kneading step within a predetermined range, it is possible to reduce metal contamination originating from the kneading device.
Claims
1. A kneading method having a kneading step of kneading an electrode active material, a conductive assistant, a binder, and a solvent to obtain a kneaded material, The method for kneading, wherein the solid content concentration of the kneaded product in the kneading step is 76 to 87% by mass.
2. 2. The method for kneading according to claim 1, wherein a kneading device made of stainless steel is used as the kneading device for kneading the mixture.
3. A method for producing an electrode slurry, comprising mixing a kneaded mixture obtained by the method for kneading according to claim 1 or 2 with a solvent to produce an electrode slurry.
4. A method for producing an electrode, comprising applying the electrode slurry produced by the method for producing an electrode slurry according to claim 3 onto a current collector and then drying the applied electrode slurry.
5. A method for producing a battery, comprising the steps of: producing a battery by using an electrode produced by the method for producing an electrode according to claim 4.
Citation Information
Patent Citations
Manufacture of electrode slurry for lithium battery
JP1995161350A
Manufacture of nonaqueous electrolyte secondary battery
JP2000353516A