Catalyst for olefin polymerization and olefin polymerization method
A catalyst system with a solid titanium component, organometallic compound, and specific organic compound enhances polyolefin stereoregularity and fluidity, addressing the limitations of conventional Ziegler-Natta catalysts and meeting the needs of lightweight automobile materials.
Patent Information
- Application Number
- JP2023079548
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
AI Technical Summary
Conventional Ziegler-Natta catalysts produce polyolefins with low stereoregularity due to residual titanium compounds, which are not suitable for producing high-stereoregular and high-fluidity polyolefins needed for lightweight, environmentally friendly automobile materials.
A catalyst system comprising a solid titanium catalyst component, an organometallic compound, and a specific organic compound, such as 9,9-bis(ethoxymethyl)-9H-fluorene, is used to enhance stereoregularity and fluidity of polyolefins, with prepolymerization steps to improve performance.
The catalyst system produces polyolefins with high stereoregularity and high fluidity, suitable for lightweight automobile materials, while minimizing low-stereoregularity by-products and reducing hydrogen usage.
Smart Images

Figure 2024163706000001 
Figure 2024163706000002 
Figure 2024163706000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an olefin polymerization catalyst and a method for polymerizing olefins. [Background technology]
[0002] Conventionally, Ziegler-Natta catalysts consisting of a titanium catalyst component and an organoaluminum compound have been widely used as catalysts for the production of polyolefins.
[0003] In particular, when producing highly stereoregular polyolefins such as polypropylene, a catalyst consisting of a solid titanium catalyst component containing an internal donor (internal electron donor), an organoaluminum compound, and an external donor (external electron donor) is usually used. For example, an olefin polymerization catalyst consisting of a magnesium chloride-supported solid titanium catalyst containing a carboxylic acid ester as an internal donor, an organoaluminum compound, and an organosilicon compound as an external donor is known (see, for example, Patent Documents 1 and 2).
[0004] However, when olefins are polymerized using a catalyst containing the above-mentioned solid titanium catalyst component, there is a problem that polyolefins with low stereoregularity are by-produced in addition to polyolefins with high stereoregularity due to so-called "excess titanium compounds" (Patent Document 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 08-003215 [Patent Document 2] Japanese Patent Application Publication No. 08-143620 [Patent Document 3] Japanese Patent Application Publication No. 59-124909 Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, the automotive industry has been actively developing environmentally friendly, fuel-efficient vehicles, and in the field of automotive materials, there is a demand for resinification of materials and further thinning of materials for the purpose of weight reduction. For this reason, there is a high expectation for improvement in olefin-based materials such as propylene-based materials, which have a long track record as automotive materials including bumper materials, and for example, propylene-based polymers having high stereoregularity and high fluidity are expected to be polymers having high rigidity, high heat resistance, and good moldability. Due to such needs, a catalyst capable of producing polyolefins having high stereoregularity and high fluidity is desired.
[0007] An object of the present invention is to provide a catalyst that can be used for producing polyolefins having high stereoregularity and high fluidity, and a method for producing polyolefins using the catalyst. [Means for solving the problem]
[0008] As a result of the inventor's research, it has been found that the above-mentioned problems can be solved by the following configuration examples. The configuration examples of the present invention are as shown in the following [1] to [4]. In this specification, the numerical range "A to B" indicates A or more and B or less. In the present invention, the term "polymerization" may be used to include not only homopolymerization but also random copolymerization or block copolymerization, and the term "polymer" may be used to include not only homopolymer but also random copolymer or block copolymer.
[0009] [1] A solid titanium catalyst component [A] containing magnesium, titanium, a halogen and an electron donor; An organometallic compound catalyst component [B]; An organic compound represented by the following formula (1): An olefin polymerization catalyst comprising:
[0010] [ka] (In the formula, R 1 ~R 8 is hydrogen and R 9 ~R 10 is an ethyl group.)
[0011] [2] A solid titanium catalyst component [A] containing magnesium, titanium, a halogen and an electron donor; An organometallic compound catalyst component [B]; An organic compound represented by the following formula (1): An olefin polymerization catalyst [II] obtained by prepolymerizing an olefin on a catalyst containing the above.
[0012] [ka] (In the formula, R 1 ~R 8 is hydrogen and R 9 ~R 10 is an ethyl group.)
[0013] [3] A solid titanium catalyst component [A] containing magnesium, titanium, a halogen and an electron donor, an organometallic compound catalyst component [B], and a prepolymerization catalyst component [P AB ]and, An organic compound represented by the following formula (1): An olefin polymerization catalyst comprising:
[0014] [ka] (In the formula, R 1 ~R 8 is hydrogen and R 9 ~R 10 is an ethyl group.)
[0015] [4] A method for polymerizing olefins, comprising polymerizing or copolymerizing an olefin in the presence of the olefin polymerization catalyst according to any one of [1] to [3]. Effect of the Invention
[0016] The present invention provides a catalyst that can be used to produce polyolefins having high stereoregularity and high fluidity, and a method for producing polyolefins using the catalyst. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] [Olefin polymerization catalyst] The first olefin polymerization catalyst [I] according to the present invention comprises a solid titanium catalyst component [A] containing magnesium, titanium, a halogen and an electron donor, an organometallic compound catalyst component [B], and a specific organic compound [C]. The second olefin polymerization catalyst [II] according to the present invention is a prepolymerization catalyst in which an olefin is prepolymerized in a catalyst comprising the solid titanium catalyst component [A], an organometallic compound catalyst component [B], and a specific organic compound [C]. The third olefin polymerization catalyst [III] according to the present invention is a catalyst comprising the solid titanium catalyst component [A], an organometallic compound catalyst component [B], and a prepolymerized catalyst component [P AB ] and a specific organic compound [C].
[0018] In each of the olefin polymerization catalysts [I] to [III], the electron donor contained in the solid titanium catalyst component [A] acts as an internal donor (internal electron donor), while the organic compound [C] acts as an external donor (external electron donor) in each of the olefin polymerization catalysts [I] to [III]. Hereinafter, each of the components constituting the olefin polymerization catalysts [I] to [III] will be described.
[0019] <Solid titanium catalyst component [A]> The solid titanium catalyst component [A] (hereinafter sometimes simply referred to as "component [A]") constituting the olefin polymerization catalyst of the present invention contains magnesium, titanium, a halogen and an electron donor. The solid titanium catalyst component [A] is the main component constituting the titanium catalyst used as an olefin polymerization catalyst, and may be the same as the solid titanium catalyst component used in the conventionally known titanium catalysts. The solid titanium catalyst component [A] is, for example, (a) solid titanium containing magnesium, titanium, a halogen and an electron donor, from which titanium does not desorb upon washing with hexane at room temperature; (b) aromatic hydrocarbons, (c) liquid titanium, and (d) Electron donor The compound can be prepared by a method comprising the step of contacting
[0020] <(a) Solid titanium> The solid titanium (a) can be produced by contacting a magnesium compound, a titanium compound, an electron donor (internal donor), and the like by various methods, according to known methods for preparing solid titanium catalyst components (see, for example, JP-A-4-096911, JP-A-58-83006, JP-A-8-143580, and the like).
[0021] The magnesium compound is preferably used in a solid state. The magnesium compound in the solid state may be a magnesium compound itself in a solid state, or may be an adduct with an electron donor. The magnesium compound may be a magnesium compound described in JP-A-2004-2742, specifically, magnesium chloride, ethoxy magnesium chloride, butoxy magnesium, etc. The electron donor may be a compound having the ability to solubilize a magnesium compound described in JP-A-2004-2742, specifically, alcohol, aldehyde, amine, carboxylic acid, and mixtures thereof, etc. The amount of the magnesium compound and the electron donor used may vary depending on the type, the contact conditions, etc., but the magnesium compound may be used in an amount of 0.1 to 20 mol / L, preferably 0.5 to 5 mol / L, relative to the liquid electron donor.
[0022] The titanium compound is preferably used in a liquid state. Examples of such titanium compounds include tetravalent titanium compounds represented by the following formula (III). Ti(OR 5 ) g X 4-g (III) In formula (III), R 5 is a hydrocarbon group, X is a halogen atom, and 0≦g≦4. As the titanium compound, titanium tetrachloride is particularly preferable. The titanium compounds may be used in combination of two or more kinds.
[0023] The electron donor (internal donor) may, for example, be a compound represented by the following formula (IV) (hereinafter also referred to as "compound (IV)").
[0024] [ka]
[0025] In formula (IV), R represents a linear or branched alkyl group having 1 to 10 carbon atoms, preferably 2 to 8, and more preferably 3 to 6 carbon atoms, R' represents a linear or branched alkyl group having 1 to 10 carbon atoms, and n represents an integer of 0 to 4. In the present invention, a compound in which n is 0 is preferred.
[0026] Examples of alkyl groups for R and R' include methyl, ethyl, n-propyl, iso-propyl, n-butyl, iso-butyl, tert-butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl groups.
[0027] Specific examples of the compound (IV) include dimethyl phthalate, methyl ethyl phthalate, diethyl phthalate, di-n-propyl phthalate, diisopropyl phthalate, di-n-butyl phthalate, diisobutyl phthalate, di-n-pentyl phthalate, dineopentyl phthalate, di-n-hexyl phthalate, di-n-heptyl phthalate, di(methylhexyl) phthalate, di(dimethylpentyl) phthalate, di(ethylpentyl) phthalate, di(2,2,3-trimethylbutyl) phthalate, di-n-octyl phthalate, di-2-ethylhexyl phthalate, etc. Among these, diisobutyl phthalate is particularly preferred.
[0028] In the present invention, the electron donor (internal donor) may be an electron donor other than the compound (IV). Examples of the electron donor include a compound having two or more ether bonds that exist via a plurality of atoms (hereinafter, also referred to as a "polyether compound").
[0029] The polyether compound may be a compound in which the atom between the ether bonds is carbon, silicon, oxygen, nitrogen, sulfur, phosphorus, boron, or two or more atoms selected from these. Among these, a compound in which a relatively bulky substituent is bonded to the atom between the ether bonds and the atom between two or more ether bonds contains multiple carbon atoms is preferred. For example, a polyether compound represented by the following formula (2) is preferred.
[0030] [ka]
[0031] In the formula (2), m is an integer of 1 to 10, preferably an integer of 3 to 10, and more preferably an integer of 3 to 5. 11 , R 12 , R 31 ~R 36 R is independently a hydrogen atom or a substituent having at least one element selected from carbon, hydrogen, oxygen, fluorine, chlorine, bromine, iodine, nitrogen, sulfur, phosphorus, boron and silicon. 11 and R 12 are each independently preferably a hydrocarbon group having 1 to 10 carbon atoms, more preferably a hydrocarbon group having 2 to 6 carbon atoms. 31 ~R 36 are each independently preferably a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms.
[0032] R 11 and R 12 Specific examples of R include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, isopentyl, neopentyl, hexyl, heptyl, octyl, 2-ethylhexyl, decyl, cyclopentyl, and cyclohexyl. Of these, ethyl, n-propyl, isopropyl, n-butyl, and isobutyl are preferred. 31 ~R 36 Specific examples of R include a hydrogen atom, a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, and an isobutyl group. Among these, a hydrogen atom and a methyl group are preferred. 11 , R 12 , R 31 ~R 36 (Preferably R 11 , R 12 ) may combine together to form a ring other than a benzene ring, and the main chain may contain atoms other than carbon.
[0033] Specific examples of the polyether compound include 2,2-dicyclohexyl-1,3-dimethoxypropane, 2,2-diethyl-1,3-dimethoxypropane, 2,2-dipropyl-1,3-dimethoxypropane, 2,2-dibutyl-1,3-dimethoxypropane, 2-methyl-2-propyl-1,3-dimethoxypropane, 2-methyl-2-ethyl-1,3-dimethoxypropane, 2-methyl-2-isopropyl-1,3-dimethoxypropane, 2-methyl-2-cyclohexyl-1,3-dimethoxypropane, 2,2-bis(2-cyclohexyl ether), 2-methyl-2-isobutyl-1,3-dimethoxypropane, 2-methyl-2-(2-ethylhexyl)-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxypropane, 2,2-bis(cyclohexylmethyl)-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-diethoxypropane, 2,2-diisobutyl-1,3-dibutoxypropane, 2-isobutyl-2-isopropyl-1,3-dimethoxypropane, 2,2-di-s-butyl-1,3-dimethoxypropane, 2 ,2-Di-t-butyl-1,3-dimethoxypropane, 2,2-dineopentyl-1,3-dimethoxypropane, 2-isopropyl-2-isobutyl-1,3-dimethoxypropane, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, 2-cyclohexyl-2-cyclohexylmethyl-1,3-dimethoxypropane, 2,3-dicyclohexyl-1,4-diethoxybutane, 2,3-diisopropyl-1,4-diethoxybutane, 2,4-diisopropyl-1,5-dimethoxypentane, 2,4-diisobutyl-1,5-dimeth xypentane, 2,4-diisoamyl-1,5-dimethoxypentane, 3-methoxymethyltetrahydrofuran, 3-methoxymethyldioxane, 1,2-diisobutoxypropane, 1,2-diisobutoxyethane, 1,3-diisoamyloxyethane, 1,3-diisoamyloxypropane, 1,3-diisoneopentyloxyethane, 1,3-dineopentyloxypropane, 2,2-tetramethylene-1,3-dimethoxypropane, 2,2-pentamethylene-1,3-dimethoxypropane, 2,2-hexamethylene-1,3-dimethoxypropane, 1,2-Bis(methoxymethyl)cyclohexane, 2-cyclohexyl-2-ethoxymethyl-1,3-diethoxypropane, 2-cyclohexyl-2-methoxymethyl-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxycyclohexane, 2-isopropyl-2-isoamyl-1,3-dimethoxycyclohexane, 2-cyclohexyl-2-methoxymethyl-1,3-dimethoxycyclohexane, 2-isopropyl-2-methoxymethyl-1,3-dimethoxycyclohexane, 2-isobutyl-2-methoxymethyl-1 Examples of the cyclohexane include 2-cyclohexyl-2-ethoxymethyl-1,3-diethoxycyclohexane, 2-cyclohexyl-2-ethoxymethyl-1,3-dimethoxycyclohexane, 2-isopropyl-2-ethoxymethyl-1,3-diethoxycyclohexane, 2-isopropyl-2-ethoxymethyl-1,3-dimethoxycyclohexane, 2-isobutyl-2-ethoxymethyl-1,3-diethoxycyclohexane, and 2-isobutyl-2-ethoxymethyl-1,3-dimethoxycyclohexane.
[0034] Among these, 1,3-diethers are preferred, and 2-isopropyl-2-isobutyl-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxypropane, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, 2,2-dicyclohexyl-1,3-dimethoxypropane, and 2,2-bis(cyclohexylmethyl)-1,3-dimethoxypropane are more preferred. These compounds may be used alone or in combination of two or more.
[0035] <Preparation of solid titanium (a)> The solid titanium (a) can be prepared by contacting the magnesium compound, the titanium compound, and the electron donor. In this case, it is preferable to use a solid magnesium compound suspended in a hydrocarbon solvent. In addition, when contacting these components, a liquid titanium compound may be used once to produce a solid (s1), and the obtained solid (s1) may be further contacted with a liquid titanium compound to produce a solid (s2). Furthermore, it is preferable to prepare the solid titanium (a) after washing the solid (s1) or (s2) with a hydrocarbon solvent as necessary.
[0036] The contact of the above-mentioned components is usually carried out at a temperature of −70° C. to +200° C., preferably −50° C. to +150° C., and more preferably −30° C. to +130° C. The amount of each component used in preparing solid titanium (a) varies depending on the preparation method and cannot be generally specified, but for example, the electron donor can be used in an amount of 0.01 to 10 mol, preferably 0.1 to 5 mol, and the titanium compound can be used in an amount of 0.01 to 1000 mol, preferably 0.1 to 200 mol, per 1 mol of the magnesium compound.
[0037] The solid matter (s1) or (s2) thus obtained can be used as it is as solid titanium [A], but it is preferable to wash this solid matter with a hydrocarbon solvent at 0 to 150°C.
[0038] Examples of the hydrocarbon solvent include aliphatic hydrocarbon solvents such as hexane, heptane, octane, nonane, decane, cetane, etc., non-halogenated aromatic hydrocarbon solvents such as toluene, xylene, benzene, etc., and halogen-containing aromatic hydrocarbon solvents, etc. Among these, aliphatic hydrocarbon solvents or aromatic hydrocarbon solvents not containing halogens are preferably used.
[0039] When washing the solid, the hydrocarbon solvent is used in an amount of usually 10 to 500 ml, preferably 20 to 100 ml, per 1 g of the solid. The solid titanium (a) thus obtained contains magnesium, titanium, a halogen and an electron donor. In this solid titanium (a), the electron donor / titanium (weight ratio) is preferably 6 or less. The solid titanium (a) thus obtained does not lose titanium when washed with hexane at room temperature.
[0040] (b) Aromatic hydrocarbons Examples of the aromatic hydrocarbon (b) used in contact with the solid titanium (a) include benzene, toluene, xylene, ethylbenzene, and halogen-containing hydrocarbons thereof. Among these, xylene (particularly paraxylene) is preferred. By contacting the solid titanium (a) with such an aromatic hydrocarbon (b), it is possible to reduce the amount of so-called "excess titanium compound" that produces a low stereoregularity component as a by-product.
[0041] <(c) Liquid titanium> The liquid titanium (c) used for contact with the solid titanium (a) may be the same as the titanium compound used for preparing the solid titanium (a). Among them, titanium tetrahalides are preferred, and titanium tetrachloride is particularly preferred.
[0042] (d) Electron donor Examples of the electron donor (d) used for contact with the solid titanium (a) include the same as those exemplified as the electron donor (internal donor) described above. Among them, it is preferable to use the same electron donor as that used for preparing the solid titanium (a).
[0043] <<Method for preparing solid titanium catalyst component [A]>> The contact of the solid titanium (a), the aromatic hydrocarbon (b), the liquid titanium (c) and the electron donor (d) is carried out usually at a temperature of 110 to 160°C, preferably 115 to 150°C, for 1 minute to 10 hours, preferably 10 minutes to 5 hours. In this contact, the aromatic hydrocarbon (b) is used in an amount of usually 1 to 10,000 ml, preferably 5 to 5,000 ml, more preferably 10 to 1,000 ml, per 1 g of solid titanium (a). The liquid titanium (c) is used in an amount of usually 0.1 to 50 ml, preferably 0.2 to 20 ml, and particularly preferably 0.3 to 10 ml, per 100 ml of aromatic hydrocarbon (b). The electron donor (d) is used in an amount of usually 0.01 to 10 ml, preferably 0.02 to 5 ml, and particularly preferably 0.03 to 3 ml, per 100 ml of aromatic hydrocarbon (b).
[0044] The contact order of the solid titanium (a), aromatic hydrocarbon (b), liquid titanium (c) and electron donor (d) is not particularly limited, and they can be contacted simultaneously or sequentially. It is preferable that the solid titanium (a), aromatic hydrocarbon (b), liquid titanium (c) and electron donor (d) are contacted under an inert gas atmosphere and stirring. For example, it is desirable to contact the solid titanium (a), aromatic hydrocarbon (b), liquid titanium (c) and electron donor (d) in a glass flask equipped with a stirrer that is fully substituted with nitrogen, at the above temperature, with the stirrer rotating at 100 to 1000 rpm, preferably 200 to 800 rpm, for the above time, to contact the solid titanium (a), aromatic hydrocarbon (b), liquid titanium (c) and electron donor (d).
[0045] After the contact, the solid titanium (a) and the aromatic hydrocarbon (b) can be separated by filtration. By such contact between the solid titanium (a) and the aromatic hydrocarbon (b), a solid titanium catalyst component [A] having a reduced titanium content compared to the solid titanium (a) is obtained. Specifically, a solid titanium catalyst component [A] having a titanium content 25% or more by weight, preferably 30 to 95% by weight, more preferably 40 to 90% by weight, less than the solid titanium (a) is obtained.
[0046] The solid titanium catalyst component [A] obtained as described above contains magnesium, titanium, a halogen and an electron donor, and usually satisfies the following requirements (k1) to (k4), and preferably further satisfies the following requirement (k5).
[0047] (k1) The titanium content of the solid titanium catalyst component [A] is 2.5% by weight or less, preferably 2.2 to 0.1% by weight, more preferably 2.0 to 0.2% by weight, particularly preferably 1.8 to 0.3% by weight, and most preferably 1.5 to 0.4% by weight.
[0048] The content of the electron donor (k2) is 8 to 30% by weight, preferably 9 to 25% by weight, and more preferably 10 to 20% by weight.
[0049] (k3) The electron donor / titanium (weight ratio) is 7 or more, preferably 7.5-35, more preferably 8-30, and particularly preferably 8.5-25.
[0050] (k4) The solid titanium catalyst component [A] is not substantially desorbed of titanium by washing with hexane at room temperature. Washing the solid titanium catalyst component [A] with hexane means washing for 5 minutes with hexane in an amount of usually 10 to 500 ml, preferably 20 to 100 ml, per 1 g of the solid titanium catalyst component [A]. Room temperature is 15 to 25°C. Moreover, "not substantially desorbing of titanium" means that the titanium concentration in the hexane washing liquid is 0.1 g / L or less.
[0051] (k5) The solid titanium catalyst component [A] has an average particle size of 5 to 70 μm, preferably 7 to 65 μm, more preferably 8 to 60 μm, and particularly preferably 10 to 55 μm.
[0052] Here, the amounts of magnesium, halogen, titanium and electron donor are each expressed in weight percent per unit weight of the solid titanium catalyst component [A], and magnesium, halogen and titanium are quantified by inductively coupled plasma emission spectrometry (ICP method), and electron donor is quantified by gas chromatography. The average particle size of the catalyst is measured by centrifugal sedimentation method using decalin solvent.
[0053] When the above-mentioned solid titanium catalyst component [A] is used as a catalyst component for olefin polymerization, it is possible to polymerize propylene with high activity, and to stably produce polypropylene with high stereoregularity while reducing the amount of polypropylene with low stereoregularity produced.
[0054] <Organometallic compound catalyst component [B]> The organometallic compound catalyst component [B] is a component constituting a titanium catalyst used as an olefin polymerization catalyst, and may be the same as the organometallic compound component used in the conventionally known titanium catalyst. The organometallic compound catalyst component [B] is preferably an organometallic compound containing a metal belonging to Group 1, Group 2 or Group 13 of the periodic table, and examples thereof include organoaluminum compounds, alkyl complex compounds of Group 1 metals and aluminum, and organometallic compounds of Group 2 metals. The organometallic compound catalyst component [B] may be used in combination of two or more kinds.
[0055] <Organoaluminum compounds> The organoaluminum compound is, for example, represented by the following formula: R a n AIX 3-n In the formula, R a is a hydrocarbon group having 1 to 12 carbon atoms, X is a halogen or hydrogen, and n is 1 to 3. R acan be any hydrocarbon group having 1 to 12 carbon atoms, such as an alkyl group, a cycloalkyl group, or an aryl group, and specific examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an isobutyl group, a pentyl group, a hexyl group, an octyl group, a cyclopentyl group, a cyclohexyl group, a phenyl group, and a tolyl group.
[0056] Further, the organoaluminum compound may include a compound represented by the following formula: R a n AlY 3-n In the formula, R a is the same as above, and Y is -OR b Group, -OSiR c 3 groups, -OAlR d 2 units, -NR e 2 units, -SiR f 3 groups or -N(R g )AlR h 2 groups, n is 1 to 2, and R b , R c , R d and R h is a methyl group, an ethyl group, an isopropyl group, an isobutyl group, a cyclohexyl group, a phenyl group, etc., and R e is hydrogen, methyl, ethyl, isopropyl, phenyl, trimethylsilyl, etc., and R f and R g is a methyl group, an ethyl group, etc.
[0057] Specific examples of such organoaluminum compounds include the following compounds: ·R a n Al(OR b ) 3-n Examples of such compounds include dimethylaluminum methoxide, diethylaluminum ethoxide, and diisobutylaluminum methoxide. ·R a n Al(OSiR c ) 3-nCompounds represented by the formula: for example, Et2Al(OSiMe3), (iso-Bu)2Al(OSiMe3), (iso-Bu)2Al(OSiEt3), etc. ·R a n Al(OAlR d 2) 3-n Et2AlOAlEt2, (iso-Bu)2AlOAl(iso-Bu)2, etc. Among the above organoaluminum compounds, R a Organoaluminum compounds represented by 3Al (i.e., R a n AIX 3-n (where n=3) is preferably used. a Among the 3Al, trialkylaluminum such as triethylaluminum is preferred.
[0058] <Organic compound [C]> The organic compound [C] is 9,9-bis(ethoxymethyl)-9H-fluorene and is represented by the following formula (1).
[0059] [ka] (In the formula, R 1 ~R 8 is hydrogen and R 9 ~R 10 is an ethyl group.)
[0060] Each of the olefin polymerization catalysts [I] to [III] contains 9,9-bis(ethoxymethyl)-9H-fluorene as an external donor (external electron donor), and thus can stably produce polyolefins with high stereoregularity and high fluidity with high activity. In the case of 9,9-bis(ethoxymethyl)-9H-fluorene, R in formula (1) 9 and R 10 is an ethyl group, so R 9 and R 10The stereoregularity of polyolefins can be increased compared to cases other than ethyl groups. The reason for this effect is thought to be the steric restriction around the polymerization active species by the external donor. 9 and R 10 When both are ethyl groups, a specific configuration is formed that can achieve both steric control during the monomer insertion reaction and hydrogen insertion reaction, and R 9 and R 10 is an alkyl group other than an ethyl group, the stereoregularity and hydrogen responsiveness of the polyolefin are presumably improved.
[0061] Furthermore, by containing 9,9-bis(ethoxymethyl)-9H-fluorene as an external donor (external electron donor), each of the olefin polymerization catalysts [I] to [III] has good hydrogen responsiveness. Therefore, when any of the olefin polymerization catalysts [I] to [III] is used, even if the amount of hydrogen purged into the polymerization system is relatively small, the molecular weight of the polyolefin polymer polymerized by purging hydrogen tends to be small. Here, the smaller the molecular weight of the obtained polyolefin polymer, the lower the intrinsic viscosity and the higher the fluidity. Therefore, by using any of the olefin polymerization catalysts [I] to [III] having good hydrogen responsiveness as a catalyst, a polyolefin polymer with high fluidity can be obtained with a relatively small amount of hydrogen addition.
[0062] <Production method of organic compound [C]> The organic compound [C] can be prepared by a known preparation method (for example, the method described in Japanese Patent No. 4242932, B. WESSLEN, ACTA CHEM. SCAND. 21 (1967) 718-20, etc.). Specifically, 9H-fluorene is reacted with paraformaldehyde in the presence of sodium alcoholate to synthesize a 9H-fluorenedimethylol derivative, and then the resulting 9H-fluorenedimethylol derivative is reacted with a halogenated ethane in the presence of a strong base such as NaH in a suitable solvent such as tetrahydrofuran, thereby producing the organic compound [C]. The reaction conditions for producing the 9H-fluorenedimethylol derivative and for reacting with a halogenated ethane can be the conditions described in Japanese Patent No. 4242932 or conditions equivalent thereto.
[0063] [Olefin polymerization catalysts [I]] The olefin polymerization catalyst [I] contains a solid titanium catalyst component [A], an organometallic compound catalyst component [B], and an organic compound [C]. The amount of the organometallic compound catalyst component [B] contained in the olefin polymerization catalyst [I] is usually 1 to 1,000 mol, preferably 10 to 500 mol, and more preferably 50 to 250 mol per mol of the solid titanium catalyst component [A] in terms of titanium atom. The amount of the organic compound [C] contained in the olefin polymerization catalyst [I] is usually 1 to 1,000 mol, preferably 10 to 500 mmol, and more preferably 10 to 250 mol per mol of the solid titanium catalyst component [A] in terms of titanium atom.
[0064] <Method of producing olefin polymerization catalyst [I]> The olefin polymerization catalyst [I] is produced by a process comprising the step of contacting a solid titanium catalyst component [A], an organometallic compound catalyst component [B], and an organic compound [C]. The step of contacting the solid titanium catalyst component [A], the organometallic compound catalyst component [B], and the organic compound [C] is usually carried out at a temperature of 0 to 25°C, preferably 5 to 20°C, for 5 to 20 minutes, preferably 5 to 15 minutes.
[0065] [Olefin polymerization catalysts [II]] The olefin polymerization catalyst [II] is prepared by contacting a solid titanium catalyst component [A] with an organometallic compound catalyst component [B] and an organic compound [C], followed by prepolymerization of a polyolefin. In other words, the prepolymerization catalyst in which an olefin is prepolymerized on the olefin polymerization catalyst [I] is the olefin polymerization catalyst [II]. The olefin polymerization catalyst [II] is a prepolymerization catalyst component [P ABC In this case, the prepolymerization catalyst component [P ABC The olefin polymerization catalyst [II] can be used as a composite catalyst material in which one or more selected from an organometallic compound catalyst component [B] and an organic compound [C] are further added to the above-mentioned catalyst [II].
[0066] <Method of producing olefin polymerization catalyst [II]> The olefin polymerization catalyst [II] is produced by a process including a step of prepolymerizing an olefin using a catalyst (i.e., an olefin polymerization catalyst [I]) containing a solid titanium catalyst component [A], an organometallic compound catalyst component [B], and an organic compound [C]. The conditions for prepolymerizing an olefin can be arbitrarily set depending on the desired olefin polymerization catalyst [II].
[0067] [Olefin polymerization catalysts [III]] The olefin polymerization catalyst [III] is a catalyst obtained by prepolymerizing polyolefin with a solid titanium catalyst component [A] and an organometallic compound catalyst component [B]. AB ] and an organic compound [C]. [P] used in olefin polymerization catalysts [III] AB The amount of organometallic compound catalyst component [B] contained in [P AB The amount of the catalyst is usually 1 to 1,000 moles, preferably 10 to 500 moles, and more preferably 10 to 250 moles, per mole of titanium atom of the solid titanium catalyst component [A] contained in the catalyst [A]. The olefin polymerization catalyst [III] is a catalyst component for prepolymerization [PAB The catalyst may be a composite catalyst in which an organic compound [C] and an organometallic compound catalyst component [B] are further added to the catalyst.
[0068] <Method of producing olefin polymerization catalyst [III]> The olefin polymerization catalyst [III] is a catalyst comprising a solid titanium catalyst component [A] and an organometallic compound catalyst component [B], which is prepolymerized with an olefin to form a prepolymerization catalyst component [P AB and (P1) a step of preparing Prepolymerization catalyst component [P AB a step (P2) of contacting the organic compound [C] with the The present invention is produced by a method comprising the steps of: The prepolymerization conditions are the same as those for the preparation of the olefin polymerization catalyst [II]. AB The amount of organic compound [C] used per mole of titanium atom in the catalyst [I] is the same as the amount of organic compound [C] used per mole of titanium atom in the production method of the olefin polymerization catalyst [I].
[0069] <Olefin Polymerization Method> An olefin can be polymerized in the presence of any one or more of the olefin polymerization catalysts [I] to [III]. In a preferred and exemplary embodiment of the present invention, the olefin includes propylene. In this embodiment, the method for producing the obtained olefin polymer includes a step of polymerizing propylene in the presence of any one or more of the olefin polymerization catalysts [I] to [III] described above. Here, an example of the polymerization of propylene is homopolymerization of propylene. In addition, when olefin polymerization is performed, in addition to the olefin that derives the main structural unit of the polyolefin to be polymerized, a small amount of other olefin or a small amount of diene compound can be coexisted in the polymerization system as another comonomer to produce a random copolymer. Examples of such olefins other than propylene include olefins having 2 to 8 carbon atoms such as ethylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, and 3-methyl-1-butene. Among these, ethylene is preferred. In the case of a random copolymer, the content of other comonomers is preferably 6 mol% or less, more preferably 3 mol% or less.
[0070] The polymerization can be carried out by any of liquid phase polymerization methods such as solution polymerization and suspension polymerization, or gas phase polymerization methods. When the polymerization is carried out in the form of a slurry polymerization reaction, an inert organic solvent can be used as the reaction solvent, or an olefin that is liquid at the reaction temperature can be used.
[0071] Specific examples of the inert organic solvent include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene; alicyclic hydrocarbons; aromatic hydrocarbons; halogenated hydrocarbons; and contact products thereof. Of these, it is particularly preferable to use aliphatic hydrocarbons.
[0072] In the polymerization, the olefin polymerization catalysts [I] to [III] are usually used in an amount of about 1×10 titanium atom per liter of polymerization volume. -5 ~1 mmol, preferably about 1×10 -4 Used in amounts of ~0.1 millimolar.
[0073] If hydrogen is used during polymerization, the molecular weight, intrinsic viscosity, fluidity, etc. of the resulting polyolefin can be adjusted. The more hydrogen is added, the smaller the molecular weight of the resulting polyolefin tends to be. Similarly, the more hydrogen is added, the smaller the intrinsic viscosity of the resulting polyolefin tends to be, and the greater the fluidity of the resulting polyolefin tends to be. Here, since the olefin polymerization catalysts [I] to [III] all have good hydrogen responsiveness, the molecular weight and intrinsic viscosity of the resulting polyolefin tend to be small, and the fluidity of the resulting polyolefin tends to be high, even if the amount of hydrogen added is small compared to the case of using other catalysts. Therefore, when polymerization is performed using the olefin polymerization catalysts [I] to [III] as a catalyst, the amount of hydrogen used to obtain a polyolefin with the desired fluidity and the partial pressure of hydrogen in the system can be smaller than when using other catalysts.
[0074] The polymerization of polyolefins is usually carried out at a temperature of about 20 to 150°C, preferably about 50 to 100°C, and at a pressure of normal pressure to 100 kg / cm. 2 , preferably about 2 to 50 kg / cm 2 This is carried out under pressure.
[0075] When polymerization is carried out using one or more of the olefin polymerization catalysts [I] to [III] as a catalyst, the polymerization of polyolefins can be carried out in any of batch, semi-continuous, and continuous methods. Furthermore, the polymerization can be carried out in two or more stages by changing the reaction conditions. In addition, in the present invention, olefin homopolymers and block copolymers may be produced.
[0076] The propylene polymer obtained by the polymerization method using any one or more of the olefin polymerization catalysts [I] to [III] as a catalyst may contain a structural unit derived from biomass-derived propylene. The propylene constituting the propylene polymer may be only biomass-derived propylene, or may be a mixture of biomass-derived propylene and fossil fuel-derived propylene. Biomass-derived propylene is propylene obtained from any renewable natural raw material, such as a plant-derived or animal-derived raw material including fungi, yeast, algae, and bacteria, and its residue, and contains as carbon the propylene polymer. 14 C isotope 10 -12 The biomass-derived propylene is contained in a ratio of about 100 (pMC) as measured in accordance with ASTM D 6866. Biomass-derived propylene can be obtained by a conventionally known method. It is preferable from the viewpoint of reducing the environmental load (mainly reducing greenhouse gas emissions) that a propylene polymer obtained by a polymerization method using any one or more of the olefin polymerization catalysts [I] to [III] as a catalyst contains a constitutional unit derived from biomass-derived propylene. If the polymer production conditions such as the polymerization catalyst, polymerization process, and polymerization temperature are the same, even if the raw material propylene of the propylene polymer contains biomass-derived propylene, 14 C isotope 10 -12 ~10 -14 The molecular structure of the propylene polymer is the same as that of a propylene polymer made only from fossil fuel-derived propylene, except for the proportion of propylene in the propylene polymer. Therefore, the performance of these propylene polymers is said to be the same.
[0077] The propylene polymer obtained by the polymerization method using any one or more of the olefin polymerization catalysts [I] to [III] as a catalyst may contain a structural unit derived from chemically recycled propylene. The propylene used as a raw material for the propylene polymer may be only chemically recycled propylene, or may be a mixture of chemically recycled propylene and fossil fuel-derived propylene and / or biomass-derived propylene. Chemically recycled propylene is obtained by a conventionally known method. It is preferable from the viewpoint of reducing environmental load (mainly reducing waste) that the propylene polymer obtained by the polymerization method using any one or more of the olefin polymerization catalysts [I] to [III] as a catalyst contains chemically recycled propylene. In general, even if the raw material monomer contains a chemically recycled monomer, the chemically recycled monomer is a monomer obtained by depolymerizing or pyrolyzing a polymer such as waste plastic back into a monomer unit such as propylene, or a monomer produced using such a monomer as a raw material, and therefore, if the polymer production conditions such as the polymerization catalyst, polymerization process, and polymerization temperature are the same, the molecular structure is the same as that of a propylene polymer in which the raw material propylene is made only of fossil fuel-derived monomers. Therefore, the performance of these propylene polymers is considered to be the same.
[0078] When the raw material monomer of the polymer obtained by the polymerization method using any one or more of the olefin polymerization catalysts [I] to [III] as a catalyst is ethylene, the raw material monomer may be only biomass-derived ethylene or a mixture of biomass-derived ethylene and fossil fuel-derived ethylene, as in the case of propylene. In addition, the raw material monomer may be only chemically recycled ethylene or a mixture of chemically recycled ethylene and fossil fuel-derived ethylene and / or biomass-derived ethylene. The same applies to the case where an olefin other than propylene and ethylene is used as a raw material monomer. EXAMPLES
[0079] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0080] [raw materials] In the examples and comparative examples, the solid titanium catalyst component [A-1] prepared in Preparation Example 2 described below was used as the solid titanium catalyst component [A]. As the organometallic compound catalyst component [B], triethylaluminum [B-1] (manufactured by Toso Finechem Co., Ltd.) was used. In the examples, 9,9-bis(ethoxymethyl)-9H-fluorene was used as the organic compound [C].
[0081] In the comparative example, the following organic compound [CC] was used in place of the organic compound [C]. 9,9-Bis(methoxymethyl)-9H-fluorene [CC-1] 9,9-Bis(propoxymethyl)-9H-fluorene [CC-2] 9,9-Bis(isopropoxymethyl)-9H-fluorene [CC-3] 2,7-Di-tert-butyl-9,9-bis(ethoxymethyl)-9H-fluorene [CC-4] 12,12-Bis(ethoxymethyl)-1,1,4,4,7,7,10,10-octamethyl-2,3,4,7,8,9,10,12-octahydro-1H-dibenzo[b,h]fluorene [CC-5]
[0082] [Example 1] <Preparation Example 1: Preparation of solid titanium (a-1)> After thoroughly replacing the air in a 2-liter high-speed stirring apparatus (manufactured by Tokushu Kika Kogyo Co., Ltd.), 700 ml of refined kerosene, 10 g (0.11 mol) of magnesium chloride, 24.2 g (0.53 mol) of ethanol, and 3 g of sorbitan distearate ("Emersol 320" manufactured by Kao Atlas Co., Ltd.) were charged into the apparatus. The temperature of this system was raised under stirring, and the mixture was stirred for 30 minutes under conditions of 120°C and 800 rpm. Under high-speed stirring, the mixture was transferred to a 2-liter glass flask (with stirrer) containing 1 liter of refined kerosene previously cooled to -10°C, using a Teflon (registered trademark) tube with an inner diameter of 5 mm. The obtained solid was filtered and thoroughly washed with refined n-hexane, to obtain a solid adduct in which 2.8 mol of ethanol was coordinated to 1 mol of magnesium chloride.
[0083] Next, the solid adduct (45 mmol in terms of magnesium atom) was suspended in 20 ml of decane, and the entire amount was introduced into 195 ml (1.77 mol) of titanium tetrachloride kept at -20°C under stirring. The mixture was heated to 80°C over 5 hours, and 1.8 ml (6.2 mmol) of diisobutyl phthalate was added. The mixture was then heated to 110°C and stirred for 1.5 hours.
[0084] After the reaction was completed for 1.5 hours, the solid portion was collected by hot filtration and washed with decane at 100°C and hexane at room temperature until titanium was no longer detected in the filtrate. In this way, solid titanium (a-1) containing 3.8% by weight of titanium, 16% by weight of magnesium, 18.2% by weight of diisobutyl phthalate, and 1.1% by weight of ethanol residue was obtained. The contents of magnesium, halogen and titanium were quantified by plasma emission spectrometry (ICP method, Shimadzu Corporation, ICPE-9820). The contents of electron donors were quantified by gas chromatography (Shimadzu Corporation, GC-2010Plus).
[0085] <Preparation Example 2: Preparation of solid titanium catalyst component [A-1]> In a 200 ml glass reactor that had been thoroughly purged with nitrogen, 6.8 g of the obtained solid titanium (a-1), 113 ml of paraxylene, 11 ml of decane, 2.5 ml (23 mmol) of titanium tetrachloride, and 0.34 ml (1.2 mmol) of diisobutyl phthalate were placed. The temperature inside the reactor was raised to 130°C, and the mixture was stirred at that temperature for 1 hour for contact treatment, after which the solid portion was collected by hot filtration. This solid portion was resuspended in 101 ml of paraxylene, and 1.7 ml (15 mmol) of titanium tetrachloride and 0.22 ml (0.8 mmol) of diisobutyl phthalate were added.
[0086] Then, the temperature was raised to 130°C, and the mixture was stirred for 1 hour while maintaining the temperature to react. After the reaction was completed, solid-liquid separation was again performed by hot filtration, and the obtained solid portion was washed with decane at 100°C and hexane at room temperature until the paraxylene in the catalyst was 1% by weight or less. In this way, a solid titanium catalyst component [A-1] containing 1.3% by weight of titanium, 20% by weight of magnesium, and 13.8% by weight of diisobutyl phthalate was obtained. The analysis method of each component contained in the solid titanium catalyst component [A-1] was the same as that in Preparation Example 1.
[0087] <Preparation Example 3: Preparation of olefin polymerization catalyst [I-1]> In a 30 ml glass vessel containing 7 ml of heptane, 0.35 mmol of triethylaluminum [B-1], 0.07 mmol of 9,9-bis(ethoxymethyl)-9H-fluorene [C] as an external electron donor, and 0.0028 mmol of the solid titanium catalyst component [A-1] obtained in Preparation Example 2 in terms of titanium atom were charged, and the mixture was contacted at 20°C for 10 minutes to prepare an olefin polymerization catalyst [I-1].
[0088] <Main polymerization using olefin polymerization catalyst [I-1] (polymerization of propylene)> In order to confirm the performance of the olefin polymerization catalyst [I-1], the main polymerization was carried out as follows using propylene as the olefin. The olefin polymerization catalyst [I-1] was charged into a 2-liter autoclave containing 500 g of propylene, and polymerization was carried out at 20° C. for 10 minutes. Then, 7.5 liters of hydrogen was further charged, and the temperature in the system was raised to 70° C. to carry out polymerization for 1 hour. Then, ethanol was added to terminate the polymerization, and unreacted propylene was purged to obtain polypropylene.
[0089] <Analysis of polypropylene obtained by this polymerization> [Mesopentad fraction (mmmm)] The pentad fraction (mmmm,%), which is an index of the stereoregularity of a polymer and indicates its microtacticity, is 13 The C-NMR spectrum was assigned according to Macromolecules 8, 687 (1975). 13 It was calculated from the peak intensity ratio of the C-NMR spectrum.
[0090] 13 C-NMR spectra were measured using a Burker BioSpin Corp. AVANCE III Cryo-500 nuclear magnetic resonance spectrometer. The solvent was a mixture of orthodichlorobenzene and heavy benzene (80 / 20% by volume), the sample concentration was 50 mg / 0.6 mL, the measurement temperature was 120 °C, and the observed nuclei were 13 The measurement was performed with C (125 MHz), sequence single pulse proton broadband decoupling, pulse width 45° (5.00 μsec), repetition time 5.5 sec, number of integrations 5,000, and chemical shift reference value 21.59 ppm. The results are shown in Table 1.
[0091] <Molecular weight distribution> The Mw / Mn value, which is an index of molecular weight distribution, was obtained by analyzing the chromatogram measured under the following conditions by a known method. The results are shown in Table 1. Apparatus: Waters gel permeation chromatograph Alliance GPC2000 Column: Tosoh TSKgel GMH6-HT x2 + TSKgel GMH6-HTL x2 Mobile phase: o-dichlorobenzene (containing 0.025% BHT) Flow rate: 1.0ml / min Temperature: 140℃ Column calibration: Tosoh monodisperse polystyrene Sample concentration: 0.15% (w / v) Injection volume: 0.4ml
[0092] <Intrinsic viscosity [η]> The intrinsic viscosity [η] was measured at 135°C using decalin as a solvent. That is, about 20 mg of polypropylene sample was weighed out, dissolved in 15 mL of decalin, and the specific viscosity η was measured in an oil bath at 135°C. sp The decalin solution was diluted with 5 mL of decalin solvent, and the specific viscosity η was measured in the same manner. sp This dilution procedure was repeated two more times, and the η sp The value of / C was calculated as the intrinsic viscosity (see the formula below). The results are shown in Table 1. [η]=lim(η sp / C) (C→0)
[0093] <Amount of decane solubles> Approximately 6 grams of polypropylene (this weight is represented as b (grams) in the formula below), 500 ml of decane, and a small amount of a heat-resistant stabilizer soluble in decane were placed in a glass measuring vessel, and the vessel was heated to 150°C in 2 hours while stirring with a stirrer under a nitrogen atmosphere to dissolve the polypropylene, and then the vessel was kept at 150°C for 2 hours, and then slowly cooled to 23°C over 8 hours. The resulting liquid containing polypropylene precipitate was filtered under reduced pressure using a glass filter of 25G-4 standard manufactured by Asahi Seisakusho. 100 ml of the filtrate was collected and dried under reduced pressure to obtain a part of the decane-soluble component. This weight was represented as a (grams) in the formula below. After this operation, the amount of the decane-soluble component was determined by the formula below. The results are shown in Table 1. Decane soluble component content (wt%)=100×(500×a) / (100×b)
[0094] [Comparative Example 1] An olefin polymerization catalyst [CI-1] was prepared using the same method as in Preparation Example 3, except that the external donor charged in Preparation Example 3 was changed from 9,9-bis(ethoxymethyl)-9H-fluorene [C] to 9,9-bis(methoxymethyl)-9H-fluorene [CC-1]. Thereafter, polypropylene was polymerized and evaluated in the same manner as in Example 1, except that the olefin polymerization catalyst [CI-1] was used instead of the olefin polymerization catalyst [I-1]. The obtained results are shown in Table 1.
[0095] [Comparative Example 2] An olefin polymerization catalyst [CI-2] was prepared in the same manner as in Preparation Example 3, except that the external donor charged in Preparation Example 3 was changed to 9,9-bis(propoxymethyl)-9H-fluorene [CC-2]. Thereafter, polypropylene was polymerized and evaluated in the same manner as in Example 1, except that the olefin polymerization catalyst [CI-2] was used instead of the olefin polymerization catalyst [I-1]. The obtained results are shown in Table 1.
[0096] [Comparative Example 3] An olefin polymerization catalyst [CI-3] was prepared in the same manner as in Preparation Example 3, except that the external donor charged in Preparation Example 3 was changed to 9,9-bis(isopropoxymethyl)-9H-fluorene [CC-3]. Thereafter, polypropylene was polymerized and evaluated in the same manner as in Example 1, except that the olefin polymerization catalyst [CI-3] was used instead of the olefin polymerization catalyst [I-1]. The obtained results are shown in Table 1.
[0097] [Comparative Example 4] An olefin polymerization catalyst [CI-4] was prepared using the same method as in Preparation Example 3, except that the external donor charged in Preparation Example 3 was changed to 2,7-di-tert-butyl-9,9-bis(ethoxymethyl)-9H-fluorene [CC-4]. Thereafter, polypropylene was polymerized and evaluated in the same manner as in Example 1, except that the olefin polymerization catalyst [CI-4] was used instead of the olefin polymerization catalyst [I-1]. The obtained results are shown in Table 1.
[0098] [Comparative Example 5] An olefin polymerization catalyst [CI-5] was prepared using the same method as in Preparation Example 3, except that the external donor charged in Preparation Example 3 was changed to 12,12-bis(ethoxymethyl)-1,1,4,4,7,7,10,10-octamethyl-2,3,4,7,8,9,10,12-octahydro-1H-dibenzo[b,h]fluorene [CC-5]. Thereafter, polypropylene was polymerized and evaluated in the same manner as in Example 1, except that the olefin polymerization catalyst [CI-5] was used instead of the olefin polymerization catalyst [I-1]. The obtained results are shown in Table 1.
[0099] [Table 1]
Claims
1. A solid titanium catalyst component [A] containing magnesium, titanium, a halogen and an electron donor; An organometallic compound catalyst component [B]; An organic compound [C] represented by the following formula (1): An olefin polymerization catalyst [I] comprising: [Case 1] (In the formula, R 1 ~R 8 is hydrogen, R 9 ~R 10 is an ethyl group.)
2. A solid titanium catalyst component [A] containing magnesium, titanium, a halogen and an electron donor; An organometallic compound catalyst component [B]; An organic compound [C] represented by the following formula (1): An olefin polymerization catalyst [II], which is obtained by prepolymerizing an olefin on a catalyst containing the above. [chemical 2] (In the formula, R 1 ~R 8 is hydrogen, R 9 ~R 10 is an ethyl group.)
3. A solid titanium catalyst component [A] containing magnesium, titanium, a halogen and an electron donor, and an organometallic compound catalyst component [B] are mixed with a prepolymerized catalyst component [P] obtained by prepolymerizing an olefin. AB ]and, An organic compound [C] represented by the following formula (1): An olefin polymerization catalyst comprising: [C3] (In the formula, R 1 ~R 8 is hydrogen, R 9 ~R 10 is an ethyl group.)
4. A method for polymerizing olefins, comprising polymerizing or copolymerizing olefins in the presence of the olefin polymerization catalyst according to any one of claims 1 to 3.
Citation Information
Patent Citations
Production of olefin polymerization catalyst
JP1984124909A
Method for polymerizing alpha-olefin
JP1996003215A
Polymerization of alpha-olefin
JP1996143620A