Method for manufacturing photonic crystal gallium nitride light-emitting element, and lighting device
By forming photonic crystals on GaN layers using epitaxial growth and etching techniques on sapphire substrates, the method addresses inefficiencies and high costs associated with lens changes, achieving improved light directivity and luminous efficiency in GaN light emitting devices.
Patent Information
- Application Number
- JP2023112958
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2023-07-10
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-07-10
AI Technical Summary
Existing methods for forming photonic crystals on gallium nitride (GaN) layers in light emitting devices are not established, leading to inefficiencies and high costs due to the need for lens changes and expensive quartz lenses, especially for ultraviolet and deep ultraviolet rays.
A method involving epitaxial growth on a sapphire substrate, followed by electron beam lithography and inductively coupled plasma reactive ion etching to form photonic crystals on the GaN layer, allowing for efficient hole formation without the need for lenses.
This method enables reliable formation of photonic crystals on GaN layers, narrowing light directivity and increasing luminous efficiency, reducing costs by eliminating the need for lens changes and using less expensive materials.
Smart Images

Figure 2024163828000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a photonic crystal gallium nitride light emitting device. [Background technology]
[0002] In order to narrow the beam angle of light emitted from a light-emitting diode (LED) chip that uses gallium nitride (GaN), consideration is being given to equipping the LED device with a lens to concentrate the light and narrow the beam angle.
[0003] However, in the case of lenses, even a slight change in directivity requires changing the mold, which increases costs.In addition, in the case of ultraviolet and deep ultraviolet rays, quartz lenses are used in consideration of the lens absorption, which makes the lenses expensive.
[0004] Therefore, as a method of concentrating light and narrowing the directivity without equipping an LED device with a lens, the formation of photonic crystals with holes on the order of several hundred nanometers at a pitch of several hundred nanometers on the surface of the LED chip is being considered.
[0005] Patent Document 1 describes an invention relating to a gallium nitride photonic crystal and a manufacturing method thereof. That is, the invention aims to provide a high-performance gallium nitride semiconductor element, a gallium nitride semiconductor substrate, and a gallium nitride photonic crystal with a high yield by obtaining a nitride semiconductor with reduced dislocation density in a wide region during epitaxial growth, and the invention includes a process of forming a gallium nitride semiconductor layer on a substrate, a process of forming an array of trenches in the gallium nitride semiconductor layer, a process of performing a heat treatment in an atmosphere containing nitrogen to deform at least two or more adjacent trenches among the plurality of trenches, forming continuous cavities in the gallium nitride semiconductor layer corresponding to the positions of the deformed trenches, and a process of forming a gallium nitride semiconductor element on the gallium nitride semiconductor layer having the cavities.
[0006] Furthermore, Patent Document 2 describes a photonic crystal light-emitting diode having an objective of providing a photonic crystal light-emitting diode that is resistant to deterioration over a long period of time and has high energy efficiency and light-emitting efficiency, in which three layers, a first semiconductor layer, an active layer, and a second semiconductor layer, are stacked in that order, with a first electrode electrically connected to the first semiconductor layer and a second electrode electrically connected to the second semiconductor layer, in which voids penetrating at least the first semiconductor layer and the active layer out of the three layers are arranged two-dimensionally periodically to form a photonic crystal structure, and the first electrode covers the first semiconductor layer except for the voids and a first non-current injection region surrounding the voids. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2004-111766 A [Patent Document 2] JP 2011-54828 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, when light emitting devices such as LEDs are made of gallium nitride (GaN), the technology for forming photonic crystals in a GaN layer has not yet been established.
[0009] An object of the present invention is to provide a method for obtaining a photonic crystal GaN light-emitting device by efficiently forming a photonic crystal in a GaN layer that constitutes a light-emitting device, and a lighting device. [Means for solving the problem]
[0010] The present invention is a method for manufacturing a photonic crystal gallium nitride light-emitting device, comprising the steps of: epitaxially growing an n-type gallium nitride layer, a multiple quantum well layer, and a p-type gallium nitride layer, successively, on a sapphire substrate to form an epitaxial structure; forming a p-type electrode on the p-type gallium nitride layer; forming a metal substrate and a support substrate on the p-type electrode; inverting the epitaxial structure so that the support substrate is on the bottom and the sapphire substrate is on the top; peeling off the sapphire substrate located at the top by the inversion step to expose the n-type gallium nitride layer on the surface; etching the n-type gallium nitride layer exposed on the surface to adjust the film thickness; forming a photonic crystal on the etched surface of the n-type gallium nitride layer by electron beam lithography and inductively coupled plasma reactive ion etching;
[0011] In one embodiment of the present invention, the step of forming the photonic crystal comprises the steps of performing a hydrophobic treatment on the surface of the n-type gallium nitride layer, applying a resist to the surface of the n-type gallium nitride layer, irradiating the resist with an electron beam to perform drawing, and removing the resist with chlorine gas by inductively coupled plasma reactive ion etching.
[0012] In another embodiment of the present invention, the method includes the steps of growing a buffer layer and an undoped gallium nitride layer, in that order, on the sapphire substrate before growing the n-type gallium nitride layer on the sapphire substrate.
[0013] In yet another embodiment of the present invention, the photonic crystal gallium nitride light emitting device has an emission wavelength of 380 nm to 390 nm.
[0014] The present invention also provides an illumination device comprising a photonic crystal gallium nitride light emitting element manufactured by the above manufacturing method, and an illumination optical system that irradiates an object with light from the photonic crystal gallium nitride light emitting element. Effect of the Invention
[0015] According to the present invention, it is possible to reliably form photonic crystals in a gallium nitride (GaN) layer constituting a GaN light-emitting device. This makes it possible to narrow the directivity of light emitted from the light-emitting device. In addition, it is possible to increase the luminous efficiency of the gallium nitride light-emitting device. [Brief description of the drawings]
[0016] [Figure 1A] 1A to 1C are schematic cross-sectional views (part 1) illustrating a manufacturing method according to an embodiment. [Figure 1B] 4 is a schematic cross-sectional view (part 2) showing the manufacturing method of the embodiment. FIG. [Figure 1C] 4A to 4C are schematic cross-sectional views (part 3) illustrating the manufacturing method according to the embodiment. [Figure 1D] 4 is a schematic cross-sectional view (part 4) showing the manufacturing method of the embodiment. FIG. [Figure 1E] 5 is a schematic cross-sectional view (part 5) showing the manufacturing method of the embodiment. [Figure 1F] 6 is a schematic cross-sectional view (part 6) showing the manufacturing method of the embodiment. [Figure 1G] 7 is a schematic cross-sectional view (part 7) showing the manufacturing method of the embodiment. [Figure 1H] 8 is a schematic cross-sectional view showing the manufacturing method of the embodiment; FIG. [Figure 1I] 9 is a schematic cross-sectional view showing the manufacturing method of the embodiment; FIG. [Figure 1J] 10 is a schematic cross-sectional view showing the manufacturing method of the embodiment; FIG. [Diagram 2] FIG. 2 is a diagram showing the configuration of an illumination device and an exposure device according to the embodiment. [Diagram 3] FIG. 2 is a diagram showing a configuration of a light source unit. [Figure 4]1 is a SEM image after electron beam writing in an embodiment. [Diagram 5] 1A and 1B are SEM images after etching by inductively coupled plasma reactive ion etching according to an embodiment, where (a) is an SEM image of the inner diameter of the hole and (b) is an SEM image of the outer diameter of the hole. [Figure 6] 1 is a cross-sectional SEM image of a hole according to an embodiment. [Figure 7] FIG. 1 is a perspective view of a GaN wafer according to an embodiment. [Figure 8] FIG. 8 is a partially enlarged view of FIG. [Figure 9] FIG. 13 is a diagram showing the results of probe measurement of a reference chip. [Figure 10] FIG. 13 is a diagram showing the results of probe measurement of the LED chip (PhC-formed chip) of the embodiment. [Figure 11] FIG. 13 shows integrating sphere measurement results of a reference and a chip with PhC formed thereon. [Figure 12] FIG. 13 is an emission spectrum diagram of the reference and the PhC-formed chip. [Figure 13] FIG. 13 is an IV characteristic diagram of a reference and a PhC-formed chip. [Figure 14] FIG. 13 is a graph showing the IL characteristics of the reference and the PhC-formed chip. [Figure 15] FIG. 11 is a diagram showing the measurement results of the directional characteristics of a reference. [Figure 16] FIG. 13 is a diagram showing the measurement results of the directional characteristics of a PhC forming chip. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0018] The basic principle of this embodiment is to form photonic crystals in the GaN layer constituting a GaN light-emitting element by electron beam (EB) drawing and inductively coupled plasma reactive ion etching, taking into consideration that the etching rate of the GaN layer greatly differs depending on the structure and crystallinity of the substrate and the GaN layer, and to grow the GaN layer on a sapphire substrate rather than growing the GaN layer on a Si substrate or the like, and to form photonic crystals on the GaN layer thus grown by electron beam (EB) drawing and inductively coupled plasma reactive ion etching.
[0019] The present inventors have found that, compared with a GaN layer grown on a Si substrate, a GaN layer grown on a sapphire substrate has a significantly higher etching rate by electron beam (EB) lithography and inductively coupled plasma reactive ion etching, and that it is possible to very efficiently form holes at desired intervals and diameters on the surface of the GaN layer to form a photonic crystal.
[0020] 1A to 1J are cross-sectional views that typically show a method for producing a photonic crystal GaN light-emitting device (LED) in this embodiment.
[0021] As shown in FIG. 1A, a low-temperature buffer layer (not shown) and an undoped GaN (u-GaN) layer (not shown) are laminated on a sapphire substrate 10 using a metal-organic chemical vapor deposition (MOCVD) apparatus, and an n-GaN layer (n-type GaN layer) 12, a multiple quantum well (MQW) layer 14, and a p-GaN layer (p-type GaN layer) 16 are sequentially laminated thereon to grow an epitaxial structure that emits light at 385 nm (380 to 390 nm).
[0022] More specifically, the n-GaN layer 12 is composed of an (AlInGaN) / (InGaN;Si) n-SLS (superlattice structure) layer and a (GaN;Si) contact layer. Here, for example, (GaN;Si) indicates that Si is doped GaN.
[0023] Moreover, the multiple quantum well (MQW) layer 14 is composed of an (InGaN / AlGaN) MQW layer.
[0024] More specifically, the p-GaN layer 16 is composed of a p-GaN (GaN;Mg) contact layer and an (AlGaN;Mg / GaN;Mg) p-SLS (superlattice structure) layer.
[0025] In this embodiment, the term "GaN layer" does not necessarily mean a single layer having a GaN composition, but means a single layer or multiple layers having a composition containing GaN, such as AlInGaN, InGaN, AlGaN, etc. In short, it means a single layer or multiple layers having GaN as the main component.
[0026] In this embodiment, the emission wavelength of the epitaxial layer is 385 nm. When a wavelength longer than this is used, the basic epitaxial structure is the same, but in terms of band gap energy, the Al content of the (InGaN / AlInGaN) MQW emission layer 14 is made larger and the In content is made smaller for 385 nm than for longer wavelengths.
[0027] Next, as shown in Fig. 1B, a p-electrode (p-type electrode: ITO or the like) and a metal reflective film (Ag or the like) are evaporated onto the epitaxial structure layer emitting light at 385 nm. In Fig. 1B, the p-electrode and the metal reflective film are collectively shown as p-electrode and reflective film 18.
[0028] Next, as shown in FIG. 1C, a metal substrate (CuW, CuMo, or the like) 20 is bonded onto the p-electrode and the metal reflective film 18.
[0029] Next, as shown in Fig. 1D, a support substrate (sapphire, Si substrate, etc.) 22 is bonded onto the metal substrate 20. The layered structure shown in Fig. 1D is, in order from the bottom, Sapphire substrate 10 / n-GaN layer 12 / MQW layer 14 / p-GaN layer 16 / p-electrode and reflective film 18 / metal substrate 20 / support substrate 22 It is.
[0030] Next, as shown in FIG. 1E, the epitaxial structure of FIG. 1D is flipped 180° upside down. The sapphire substrate 10 is placed at the top, and the sapphire substrate 10 is peeled off (lifted off) by a laser to expose the n-GaN layer 12 on the surface. That is, the epitaxial structure of FIG. 1D is inverted 180° up and down to form a layered structure, which is as follows, from the bottom: Support substrate 22 / metal substrate 20 / p-electrode and reflective film 18 / p-GaN layer 16 / MQW layer 14 / n-GaN layer 12 / sapphire substrate 10 The topmost sapphire substrate 10 (and buffer layer) is peeled off (lifted off) to expose the n-GaN layer 12 on the top surface.
[0031] Next, as shown in FIG. 1F, the n-GaN layer 12 on the surface is etched. Specifically, the total thickness of the epitaxial structure is adjusted to 1050 um by dry etching. Note that the total thickness of the epitaxial structure is not limited to this, and can be optimized depending on the emission wavelength.
[0032] 1G, a photonic crystal (PhC) is formed on the surface of the n-GaN layer 12 whose thickness has been adjusted by dry etching, as will be described in more detail below.
[0033] Next, as shown in FIG. 1H, trenches are formed from the surface of the n-GaN layer 12 down to the metal substrate 20 to separate the epitaxial structures.
[0034] Next, as shown in FIG. 1I, n-electrodes (n-type electrodes) 24 are formed on the n-GaN layer 12 in each of the separated regions.
[0035] Finally, as shown in FIG. 1J, the support substrate 22 is peeled off and diced to manufacture LED chips (V-chip structure LED chips: vertical LED chips in which electrodes are arranged in a vertical structure).
[0036] A method for producing the photonic crystal shown in FIG. 1G will now be described in more detail.
[0037] Photonic crystals (PhCs) are formed by developing a pattern in a resist using electron beam (EB) lithography and then etching using inductively coupled plasma reactive ion etching. Therefore, prior to forming a photonic crystal, it is necessary to set the EB lithography conditions and the etching conditions for inductively coupled plasma reactive ion etching.
[0038] <Etching conditions> The etching rate may vary depending on the substrate that is laminated on the Si substrate, sapphire substrate, etc., and on the structure and crystallinity of GaN.
[0039] Therefore, a GaN wafer with an emission wavelength of 385 nm grown on a sapphire substrate was rinsed and then dried for 2 minutes at 120°C. After that, a treatment (HMDS treatment) was performed to make the GaN wafer surface hydrophobic, and 950 nm of UV resist was applied using a spin coater, followed by pre-baking at 90°C for 90 seconds.
[0040] Next, a 100um x 100um pattern was printed using a high-speed maskless exposure tool at 150mJ / cm 2 The resist was then post-baked at 110° C. for 90 seconds and developed.
[0041] A GaN wafer with a UV resist was etched for 10 minutes with chlorine gas (30sccm) in an inductively coupled plasma reactive ion etching system. The etching depth was measured with a UV stylus step gauge, and a depth of 789.05nm was confirmed. The etching rate was 78.9nm / min.
[0042] On the other hand, when a GaN wafer with an emission wavelength of 385 nm grown on a Si substrate was used, the etching rate was confirmed in the same manner, and was found to be 16 nm / min. GaN layer grown on sapphire substrate: Etching rate = 78.9 nm / min GaN layer grown on Si substrate: Etching rate = 16 nm / min It is relatively difficult to form photonic crystals in a GaN layer using a Si substrate. However, it has been confirmed that photonic crystals can be efficiently formed in a GaN layer at a significantly high etching rate by growing a GaN layer on a sapphire substrate, that is, as in this embodiment, first growing a GaN layer on a sapphire substrate 10, then turning it upside down to remove the sapphire substrate 10, and etching the GaN layer on a metal substrate 20 by inductively coupled plasma reactive ion etching.
[0043] Next, an illumination device including the GaN light emitting element manufactured by the manufacturing method shown in the above embodiment and an exposure device including the illumination device will be described with reference to FIGS.
[0044] Fig. 2 is a diagram showing a schematic configuration of an exposure apparatus equipped with an illumination device IU using the GaN light-emitting element manufactured by the manufacturing method according to the embodiment described above as a light source. Fig. 3(A) is a plan view showing a schematic configuration of a light source unit 120 that supplies exposure light to the illumination device IU, and Fig. 3(B) is a diagram showing a schematic internal configuration of the light source unit 120 and the output optical system 130.
[0045] In FIG. 2, the illumination device IU includes a first focusing optical system 140 that focuses the exposure light from the light source unit 120 via the output optical system 130, a fly's eye lens FEL onto which the exposure light from the first focusing optical system 140 is incident, and a second focusing optical system 160 that focuses the exposure light from the fly's eye lens FEL to illuminate a reticle REI as an irradiated surface.
[0046] The exposure apparatus also includes an illumination device IU, and a projection optical system PO that forms an image of a pattern on a reticle illuminated by the illumination device IU onto a wafer serving as an exposed substrate.
[0047] Next, the light source unit 120 and the output optical system 130 will be described with reference to FIG.
[0048] In FIG. 3(A), the light source unit 120 includes a plurality of LED (Light Emitting Diode) chips 123 (5×5 in FIG. 3(A)) arranged on a substrate 121, for example. These LED chips are GaN light emitting elements manufactured by the manufacturing method of the above-mentioned embodiment. The number of LED chips 123 may be appropriately changed as necessary. Each of the plurality of LED chips 123 has a light emitting portion 231, and the peak wavelength of the light emitted from the light emitting portion 231 is within a range of 380 to 390 nm. That is, the light emitting portion 231 is an ultraviolet LED (UV LED). It is more preferable that the peak wavelength of the light emitted from the light emitting portion 231 is 385 nm. The light emitting surface of the light emitting portion 231 may be a square, or may be a polygon such as a rectangle or a hexagon. The LED chips 123 may be arranged on a heat sink, for example, instead of on a substrate.
[0049] The configuration of the light source unit 120 and the output optical system 130 will be described with reference to Fig. 3(B). In Fig. 3(B), the two directions in which the LED chips 123 are arranged are the X direction and the Y direction. The X direction and the Y direction are perpendicular to each other. The direction perpendicular to the X direction and the Y direction is the Z direction. The Z direction approximately coincides with the traveling direction of the light emitted from the light emitting section 231. Note that, in Fig. 3(B), for clarity of the drawing, only four LED chips 123 aligned in a row along the Y direction are shown.
[0050] As shown in FIG. 3B, the output optical system 130 includes a plurality of magnifying optical systems for forming magnified images of the light emitting parts 231 of the LED chips 123. The magnifying optical systems are arranged to correspond to the arrangement of the LED chips 123, and are bilaterally telecentric optical systems that magnify and project the light emitting parts 231 under a magnification ratio. Although FIG. 3B illustrates each magnifying optical system of the output optical system 130 as two positive lenses, the number of lenses constituting the magnifying optical system is not limited to two. The magnifying optical system may be a reflective system or a catadioptric system. The output optical system 130 may include a unity magnification optical system or a reduction optical system instead of or in addition to the magnifying optical system.
[0051] 2 and 3, each magnifying optical system of the output optical system 130 forms a magnified image of the light emitting unit 231 near the final optical member of the output optical system 130. As a result, a plurality of light source images that are densely arranged are located near the final optical member of the output optical system 130.
[0052] Returning to FIG. 2, each component of the illumination device IU will be described.
[0053] The first light-collection optical system 140 is disposed so that its front focal point is located at or near the position of the light source image formed by the light source unit 120 and the output optical system 130, and provides Koehler illumination to the entrance surface of the fly's eye lens FEL.
[0054] The fly-eye lens FEL is formed by, for example, arranging a plurality of lens elements having positive refractive power vertically and horizontally and densely so that their optical axes are parallel to the reference optical axis AX. Each lens element constituting the fly-eye lens FEL has a rectangular cross section similar to the shape of the illumination field to be formed on the reticle REI (and thus the shape of the exposure area to be formed on the wafer W).
[0055] Therefore, the light beam incident on the fly-eye lens FEL is wavefront-split by the multiple lens elements, and one light source image is formed on or near the rear focal plane (exit surface) of each lens element. In other words, a substantial surface light source consisting of multiple light source images, that is, a secondary light source, is formed on or near the rear focal plane (exit surface) of the fly-eye lens FEL.
[0056] Here, when focusing on one lens element of the fly-eye lens FEL, a plurality of light source images formed by the light source unit 120 and the output optical system 130 are formed on the rear focal plane (exit surface) of this one lens element or in its vicinity, and these plurality of light source images are distributed in an area having a similar shape to the area where the plurality of LED chips 123 are arranged. For this reason, the area where the plurality of LED chips 123 are arranged and the cross section of each lens element of the fly-eye lens FEL may have a similar shape to each other.
[0057] Now, the light beam from the secondary light source formed on or near the rear focal plane (exit surface) of the fly-eye lens FEL is incident on the aperture stop 150 arranged nearby. In this embodiment, the rear focal plane (exit surface) of the fly-eye lens FEL and the LED chip array surface of the light source unit 120 are optically conjugate.
[0058] The aperture stop 150 is disposed at a position that is nearly optically conjugate with the entrance pupil plane of the projection optical system PO, and has a variable aperture for defining the range that contributes to the illumination of the secondary light source. The exposure light from the secondary light source that passes through the aperture stop 150 is subjected to the focusing action of the second focusing optical system 160, and then illuminates a reticle REI on which a predetermined pattern is formed in a superimposed manner.
[0059] Then, the exposure light from the reticle REI illuminated by the illumination device IU (exposure light passing through a pattern located within the illumination field on the reticle REI) is incident on the projection optical system PO and forms an image of the pattern of the reticle REI on the wafer W as the exposed substrate. As a result, the pattern of the reticle REI is exposed onto the exposure area of the wafer W. The projection magnification of the projection optical system PO may be a reduction magnification, an enlargement magnification, or an equal magnification. The projection optical system PO may also be a refractive optical system, a reflective optical system, or a catadioptric optical system. EXAMPLES
[0060] A GaN wafer with an emission wavelength of 385 nm was rinsed and then dried for 2 minutes at 120° C. Then, a treatment (HMDS treatment) was performed to make the wafer surface hydrophobic, and EB resist was applied to a thickness of 500 nm using a spin coater, followed by pre-baking at 180° C. for 3 minutes.
[0061] Next, a high-speed, high-precision electron beam lithography system was used to measure the exposure dose (μC / cm 2 The dose (μC / cm) was changed under nine conditions. 2 ) were 150, 160, 170, 180, 190, 200, 210, 220, and 230, respectively.
[0062] After development, the hole diameter was confirmed using a scanning electron microscope (SEM). As a result, the relationship between the exposure dose and the hole diameter was as follows: Dose amount: 150→293.3nm Dose amount: 160→296.00nm Dose amount: 170→309.33nm Dose amount: 180→314.67nm Dose amount: 190→320.00nm Dose amount: 200→325.33nm Dose amount: 210→330.67nm Dose amount: 220→338.67nm Dose amount: 230→352.00nm It was confirmed that there is a positive correlation between the exposure dose and the hole diameter.
[0063] From the results of the above EB lithography conditions, a high-speed, high-precision electron beam lithography system was used to determine the EB lithography conditions at 140μC / cm 2 After development, the hole diameter was confirmed by SEM.
[0064] Figure 4 shows an SEM image after development, confirming that holes with diameters in the range of 286-292 nm were formed.
[0065] Next, etching was performed with chlorine gas (30sccm) in an inductively coupled plasma reactive ion etching device, and the hole diameter was confirmed with an SEM after EB resist removal. As a result, it was confirmed that the outer diameter was 262-269nm, the inner diameter was 213-220nm, and the taper angle was sufficiently suppressed to 70 degrees-80 degrees.
[0066] Figure 5 shows SEM images after etching with an inductively coupled plasma reactive ion etching system. Figure 5(a) is an SEM image of the inner diameter, and Figure 5(b) is an SEM image of the outer diameter. It was confirmed that holes on the order of several hundred nm were formed with a pitch of several hundred nm on the surface of the GaN wafer, and that photonic crystals were formed.
[0067] Figure 6 shows an SEM image of the cross section of a GaN wafer after etching with an inductively coupled plasma reactive ion etching apparatus. The taper angle of the holes that make up the photonic crystal is 70 degrees to 80 degrees. In order to narrow the directional angle of the light emitted from the LED chip, it is desirable for the holes that make up the photonic crystal to have no taper, i.e., a taper angle of 90 degrees. In this embodiment, a good result was obtained with a taper angle of 70 degrees to 80 degrees.
[0068] Fig. 7 shows a perspective view of the appearance of a GaN wafer on which photonic crystals are formed, and Fig. 8 shows an enlarged view of a portion of the wafer. It was confirmed that the illumination light illuminating the GaN wafer (fluorescent light from the room and halogen light from the microscope) was trapped in the area where the photonic crystals were formed, making the area brighter than other areas.
[0069] Figures 9 and 10 respectively show the electrical characteristic measurement results by a probe of a reference chip and the LED chip (PhC formation chip) of the present embodiment. Here, the reference chip shown in Figure 9 is an LED chip in which a photonic crystal is not formed in the GaN layer, and is a total of 10 LED chips A1 to A10 with different positions on the wafer from each other. Also, the LED chip of the present embodiment shown in Figure 10 is an LED chip in which a photonic crystal (PhC) is formed in the GaN layer, and is a total of 11 LED chips B1 to B11 with different positions on the wafer from each other. Although good electrical characteristics are obtained for both the reference chip and the PhC formation chip, for example, when comparing the half-value width (WH) and the optical output (Po) of the reference chip A1 and the PhC chip, <Reference chip A1> Half-value width WH = 16.87 (nm) Optical output Po = 166.86 (mW) <PhC formation chip B1> Half-value width WH = 11.55 (nm) Optical output Po = 445.70 (mW) and the LED chip of the present embodiment has a significantly reduced half-value width and a significantly increased optical output compared to the reference chip. On average, the half-value width WH decreased by about 5.9 nm, and the optical output Po increased by about 2.68 times.
[0070] Figure 11 shows the integrating sphere measurement results of the reference chip and the LED chip (PhC formation chip) of the present embodiment. These are the results of mounting each chip on an aluminum substrate and measuring the characteristics with an integrating sphere. Figure 11(A) shows the measurement results at a forward current IF = 500 mA, and Figure 11(B) shows the measurement results at IF = 700 mA.
[0071] When comparing the reference chips (A1 to A3) and the PhC formation chips (B4 to B6), the LED chips of the present embodiment showed the same results as the measurement results by the probe shown in Figures 9 and 10 when compared with the reference chips.
[0072] Figures 12, 13, and 14 respectively show the emission spectrum, IV characteristics, and IL characteristics of the reference chips (A1 to A3) and the PhC-formed chips (B4 to B6). Figure 12(A) shows the emission spectrum of the reference chips (A1 to A3), and Figure 12(B) shows the emission spectrum of the PhC-formed chips (B4 to B6). The same is true for Figures 13 and 14. Note that the IL characteristics in Figure 14 are graphed with the intensity of IF (100 mA) set to 1. As shown in Fig. 12, the emission spectra are almost the same for the reference and the chip with PhC formed thereon, and as shown in Fig. 13, the IV characteristics are good for both the reference and the chip with PhC formed thereon.
[0073] On the other hand, as shown in Figure 14, the IL characteristics of the chip with PhC suppressed the output drop when the current increased compared to the reference. This is thought to be due to the fact that heat generation is small due to the improvement of the external quantum efficiency (EQE).
[0074] 15 and 16 show the directional characteristic measurement results of the reference chips (A1 to A3) and the PhC-formed chips (B4 to B6), respectively. It was confirmed that the chips had directional characteristics, and in this embodiment, the PhC-formed chips showed a tendency for the intensity to increase in four directions.
[0075] As described above, according to this embodiment, photonic crystals can be manufactured by forming holes of the order of several hundreds of nanometers at a pitch of several hundreds of nanometers on the surface of a GaN layer grown on a sapphire substrate. This makes it possible to provide directivity with the LED chip alone without using a lens, and eliminates the need to create a mold, reducing costs. In addition, the light emission efficiency of the LED chip can be increased by more than twice as much as when a photonic crystal is not formed, and output reduction when the current increases can be suppressed, allowing for flexible response to specification changes. [Explanation of symbols]
[0076] 10 sapphire substrate, 12 n-GaN layer, 14 MQW layer, 16 p-GaN layer, 18 p-electrode and reflective film, 20 metal substrate, 22 support substrate, 24 n-electrode.
Claims
1. forming an epitaxial structure by epitaxially growing an n-type gallium nitride layer, a multiple quantum well layer, and a p-type gallium nitride layer on a sapphire substrate in this order; forming a p-type electrode on the p-type gallium nitride layer; forming a metal substrate and a support substrate on the p-type electrode; inverting the epitaxial structure so that the support substrate is on the bottom and the sapphire substrate is on the top; peeling off the sapphire substrate located at the top by the inversion step to expose the n-type gallium nitride layer to the surface; adjusting the thickness of the n-type gallium nitride layer by etching the n-type gallium nitride layer exposed on the surface; forming a photonic crystal on the etched surface of the n-type gallium nitride layer using electron beam lithography and inductively coupled plasma reactive ion etching; forming an n-type electrode on the n-type gallium nitride layer; peeling off the support substrate; A method for manufacturing a photonic crystal gallium nitride light-emitting device comprising the steps of:
2. The step of forming the photonic crystal includes: a step of subjecting a surface of the n-type gallium nitride layer to a hydrophobic treatment; applying a resist to a surface of the n-type gallium nitride layer; irradiating the resist with an electron beam to perform writing; removing the resist with chlorine gas by inductively coupled plasma reactive ion etching; The method for manufacturing a photonic crystal gallium nitride light emitting device according to claim 1 , comprising:
3. Prior to growing the n-type gallium nitride layer on the sapphire substrate, a buffer layer and an undoped gallium nitride layer are sequentially grown on the sapphire substrate. The method for manufacturing a photonic crystal gallium nitride light emitting device according to claim 1 , comprising:
4. The method for producing a photonic crystal gallium nitride light-emitting device according to any one of claims 1 to 3, wherein the emission wavelength of the photonic crystal gallium nitride light-emitting device is 380 nm to 390 nm.
5. A photonic crystal gallium nitride light emitting device manufactured by the manufacturing method according to any one of claims 1 to 3; an illumination optical system that illuminates an object with light from the photonic crystal gallium nitride light emitting device; A lighting device comprising:
Citation Information
Patent Citations
High-power and high-brightness LED (Light Emitting Diode) chip
CN202259401U
Light emitting device and fabrication method thereof
JP2007305998A
Pyramidal photonic crystal light emitting device
US20080121912A1
Light emitting device having auto-cloning photonic crystal structures and manufacturing method thereof
US20120175654A1
Light-emitting diode with local photonic crystals
US20150069443A1