Method for selecting composition of construction material including excavated clay soil and method and system for preparing such construction material

A computational algorithm optimizes the composition of construction materials with excavated clay soil, enhancing mechanical properties and reducing emissions, addressing the limitations of conventional cement production and excavated soil utilization.

JP2024163912AActive Publication Date: 2024-11-22MATERRUP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024122594
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-03-06
Filing Date
2024-07-29
Publication Date
2024-11-22
Estimated Expiration
2040-03-06

AI Technical Summary

Technical Problem

The cement industry contributes significantly to greenhouse gas emissions due to high energy consumption and carbon dioxide release during cement production, and the use of excavated clay soil in construction materials is limited by insufficient mechanical strength and suboptimal carbon footprint.

Method used

A method and system for selecting the composition of construction materials using excavated clay soil, involving a peptizer and activator, tailored through a computational algorithm to enhance mechanical properties, reducing energy consumption and emissions.

Benefits of technology

The method produces construction materials with mechanical properties comparable to conventional cement, significantly reducing greenhouse gas emissions and enabling widespread use of excavated clay soil in construction applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163912000001_ABST
    Figure 2024163912000001_ABST
Patent Text Reader

Abstract

To provide a system for preparing a construction material having mechanical characteristics at least equal to or higher than mechanical characteristics of cement commonly used in construction industries.SOLUTION: The disclosure relates to a method (100) for selecting a composition of a construction material including excavated clay soil, where the composition of the construction material includes amounts of a peptizer and an activating agent adapted to the excavated clay soil, and the method includes: a step (130) of receiving a measurement value of at least one of the physiochemical characteristics of the excavated clay soil and a step (170) of selecting the amount of the peptizer and the amount of the activating agent adapted to the excavated clay soil. The disclosure further relates to: a method (200) for calibrating a calculation algorithm for determining the composition of the construction material on site, and a system (400) for preparing the construction material formed from the excavated clay soil and the construction material including the excavated clay soil.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of construction materials, more particularly to the field of materials that can be used in construction, such as construction binders or concrete. The present invention relates to a method for selecting a composition of a construction material comprising excavated clayey soil. The present invention also relates to a method for calibrating a computational algorithm for determining the composition of an in-situ construction material comprising excavated clayey soil, a construction material formed from excavated clayey soil, and a system for preparing a construction material comprising excavated clayey soil. [Background technology]

[0002] Cement is the second most consumed resource in the world, with over 4 billion tonnes of the material produced worldwide each year, and this consumption is constantly increasing due to the growing demand for housing and infrastructure.

[0003] Cement is a binder, usually hydraulic, that hardens and hardens when mixed with water. After hardening, cement maintains its strength and stability even when exposed to water. There are many different types of cement used around the world. Also, cement preparation methods have become increasingly sophisticated, and automated systems have been developed to prepare various types of concrete (see Patent Documents 1 and 2 below).

[0004] Nevertheless, all conventional cements contain clinker in proportions that vary from 5% in some blast-furnace cements to a minimum of 95% in Portland cement, the most widely used cement in the world today. Clinker is the result of the calcination of a mixture consisting of about 80% limestone and 20% aluminosilicates (clays, etc.). This calcination (clinkerization) takes place at temperatures above 1200 °C, so such a cement preparation method implies high energy consumption. Moreover, the chemical conversion of limestone to lime also releases carbon dioxide. As a result, the cement industry generates about 8% of the world's CO2 emissions. In response to this challenge, industry and researchers are looking for ways to reduce the impact of carbon dioxide emissions from the cement industry.

[0005] In addition to these carbon emissions, the management of excavated soil is also problematic in the context of large urban development projects. This excavated soil is usually stored or used for quarry reclamation or park development, but the potential use is much smaller than the available amount. Furthermore, it has been proposed to use this excavated soil for the production of construction materials, but this application faces the problem of insufficient mechanical strength of the original soil structures on the one hand and, on the other hand, a suboptimal carbon footprint when using metakaolin.

[0006] Indeed, as described in the patent document 3 below, proposed cements based on raw soils either have too weak physical properties, such as increased mechanical strength, reduced capillary absorption or reduced liquid permeability, or require the addition of a portion of Portland cement to obtain acceptable mechanical properties.

[0007] In the case of metakaolin-based cements, the mixing of lime or sodium hydroxide with metakaolin during cement hydration induces a pozzolanic reaction. This reaction improves the binding properties of metakaolin cement. Due to these properties, metakaolin-based building materials have been proposed, including flash metakaolin, in particular in association with sodium hydroxide, as described in US Pat. No. 5,399,363. Nevertheless, the formation of metakaolin requires a thermal treatment of the kaolinite clay to bring about the dehydroxylation of the kaolinite crystal structure. This induces an unfavorable carbon balance, especially when taking into account the transport of excavated soil to thermal units.

[0008] There is therefore a need for new uses for excavated clay soils that can advantageously allow for the reduction of greenhouse gas emissions and the preparation of construction materials, such as construction binders or in-situ concrete, with mechanical properties at least equal to or better than those of cements commonly used in the construction industry, but with a low carbon footprint. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] French Patent Application Publication No. 2751911 [Patent Document 2] European Patent Application Publication No. 2296854 [Patent Document 3] French Patent Application Publication No. 3016376 [Patent Document 4] French Patent Application Publication No. 3034094 Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention therefore aims to overcome the disadvantages of the prior art, in particular to provide a method for selecting the composition of a construction material comprising excavated clay soil, which makes it possible, on the one hand, to form a construction material such as a construction binder in order to reduce the emission of greenhouse gases such as carbon dioxide, while at the same time giving it mechanical properties suitable for use in the construction industry, and, on the other hand, to propose an in-situ concrete comprising such a binder and capable of improving the comfort of the inhabitants compared to concrete made from Portland cement.

[0011] The present invention also aims to propose a construction material made from excavated clay soil, having mechanical properties suitable for use in the construction industry, whilst constituting a method for recycling excavated clay soil.

[0012] The present invention also aims to propose a method and a system for preparing a construction material comprising excavated clay soil in order to reduce greenhouse gas emissions compared to conventional construction materials of the Portland cement type. [Means for solving the problem]

[0013] To this end, the present invention provides a method for selecting a composition of a construction material comprising excavated clayey soil, the composition of the construction material comprising an amount of deflocculating agent and an activating agent adapted to the excavated clayey soil, the method being implemented by a computer device comprising a calculation module, - receiving measurements of at least one physicochemical property of the excavated clayey soil from a calculation module; - selecting by a calculation module an amount of deflocculating agent and an amount of activating agent applied to the excavated clayey soil based on a comparison of one or more measurements with a reference value, the reference value comprising a correlation between the measurement of at least one physicochemical property of the clayey soil and the amount of deflocculating agent and activating agent applied to the clayey soil to form a construction material; The present invention relates to a method comprising the steps of:

[0014] Such a selection method has the advantage that at least some of the components of a construction material based on excavated clayey soil can be selected to form a construction material, such as a construction binder or in-situ concrete, whose mechanical properties are comparable to those of conventional construction materials using clinker. Indeed, with the methods of the prior art, construction materials obtained from excavated soil are generally not efficient enough from a mechanical point of view to allow a wide range of uses.

[0015] Additionally, the components selected by the selection process (i.e., excavated clay soil, deflocculating agent and activator) allow for the formation of the construction material in a preparation process that consumes less energy.

[0016] Finally, the construction material comprises excavated clay soil and has preferably not undergone a combustion stage, thus advantageously retaining its hygrothermal properties and making it possible to improve the comfort of the inhabitants compared to concrete formed from Portland cement.

[0017] According to other optional features of the selection method: - at least one physicochemical property is selected from the clay content, the clay nature, the particle size, the content of impurities, the content of non-clay mineral fractions, the content of contaminants, the elemental analysis, the content of metal oxides, the salinity, the pH and the total exchange capacity of the clay in the excavated clay soil. Preferably, the at least one physicochemical property is selected from the clay content, the clay nature, the particle size, the content of non-clay mineral fractions, the elemental analysis, the content of metal oxides, the salinity, the pH and the total exchange capacity of the clay in the excavated clay soil. More preferably, the at least one physicochemical property is selected from the clay content, the clay nature, the particle size, the content of non-clay mineral fractions, the content of metal oxides and the total exchange capacity of the clay in the excavated clay soil. Such physicochemical properties are most likely to provide values ​​of deflocculants and activators adapted to the excavated clay soil considered. - at least one physicochemical property is measured on a pretreated excavated clayey soil, the pretreatment being selected from crushing, sorting, sieving and / or drying the excavated clayey soil, which advantageously minimizes the errors of the measurements taken. Preferably, the pretreatment comprises at least one fractionation, for example by sieving or sedimentation, more preferably fractionation at 50 μm, and fractionation at 20 μm, for example. - Preparing in advance for receiving the desired mechanical property values ​​of the construction material, the step of selecting the amount of deflocculating agent and activating agent further comprises excluding the amount of deflocculating agent and activating agent that does not allow the construction material to exhibit the desired mechanical property values. Thus, the operator can easily set objective performance criteria for the construction material that is expected to be composed. This saves time and improves performance in the process of reclaiming excavated soil for construction applications. The step of selecting by the calculation module the amount of deflocculating agent and the amount of activator adapted to the excavated clayey soil comprises implementing a pre-calibrated calculation algorithm. -Pre-calibrated computational algorithms are obtained by implementing statistical supervised learning methods.

[0018] According to another aspect, the present invention further provides a method for calibrating a computational algorithm for determining a composition of a construction material, such as a construction binder or in-situ concrete, implemented, for example, by a digital device including a learning module, comprising: a first step of receiving from a learning module measurements of at least one physicochemical property of the excavated clayey soil; a second step of receiving from the learning module a value of the amount of deflocculating agent and a value of the amount of activating agent that can be added to the excavated clayey soil to form a construction material; a third step of receiving from the learning module at least one measured value of a mechanical property of a construction material formed from the excavated clayey soil, at least one value of a physicochemical property received during the first receiving step, and amounts of deflocculating agent and activating agent received during the second receiving step; - creating by a learning module correlations between the measurements received in order to calibrate a calculation algorithm; The present invention relates to a method comprising the steps of:

[0019] The combination of excavated clayey soil, deflocculating agent and activating agent allows the production of a construction material with considerable mechanical properties, and the selection method according to the invention allows the selection of suitable quantity values. However, taking into account the complexity and variability of the physicochemical properties of excavated clayey soil, the inventors have developed a method for calibrating the calculation algorithm that allows to overcome this complexity. Such a calibration method allows to propose quantity values ​​of deflocculating agent and activating agent that are highly adapted to the excavated clayey soil. It should be noted that the order of receipt is not important and allows the description of the method to be clear.

[0020] According to another aspect, the present invention further provides a method for preparing a construction material from excavated clay soil, comprising the steps of: - measuring at least one physicochemical property of the excavated clayey soil; - a selection step according to the method according to the invention for selecting the composition of a construction material comprising excavated clay soil, - mixing the excavated clay soil, the deflocculating agent and the activator according to the selected composition; The present invention relates to a method comprising the steps of:

[0021] Such a simple and rapid method makes it possible to reduce greenhouse gas emissions during its implementation, as compared to the implementation of methods for preparing conventional construction materials of the Portland cement type.

[0022] According to another optional feature of the preparation method, the preparation method comprises: - measuring the physicochemical or mechanical properties of the resulting construction material during the mixing step; - comparing the measured values ​​with predetermined values ​​of physicochemical or mechanical properties of the resulting construction material; adding at least one complementary component when the measured value differs from a predetermined value of a physicochemical or mechanical property of the resulting building material; Further includes:

[0023] Verification of the properties of the resulting construction material therefore allows a quality control to be performed online, i.e. preferably in real time, to ensure that the resulting construction material has mechanical properties as close as possible to the expected mechanical properties, in fact deviations may be identified during mixing and corrected before the construction material is used as well as before it is completed.

[0024] According to another aspect, the invention relates to a computer program product arranged to carry out the selection method according to the invention.

[0025] According to another aspect, the invention relates to a computer program product arranged to carry out the calibration method according to the invention.

[0026] According to another aspect, the present invention further relates to a construction material formed from excavated clayey soil, the construction material comprising a deflocculating agent and the excavated clayey soil. Preferably, the present invention further relates to a construction material formed from excavated clayey soil, the construction material comprising the excavated clayey soil, an activator and a deflocculating agent, the deflocculating agent comprising at least 0.1% by weight of the construction material, preferably at least 0.25% by weight of the construction material.

[0027] Activators are not systematically found in construction binders or in-situ concrete because they may react with and transform the components of the excavated clay soil. Nevertheless, in some cases, construction materials according to the invention formed from excavated clay soil may further include an activator.

[0028] Such construction materials formed from excavated clay soil have mechanical properties suitable for use in the construction industry whilst constituting a method of reclaiming excavated clay soil.

[0029] According to another optional feature of the construction material according to the invention, the construction material comprises a mixture of different types of clay.

[0030] Furthermore, the construction material may comprise at least 2% by weight, preferably at least 4% by weight, more preferably at least 6% by weight of silt particles, in particular particles with a diameter between 2 μm and 50 μm.

[0031] The construction material according to the invention may comprise metal oxide in a content of at least 2% by weight of the construction material.

[0032] The construction material according to the invention may further comprise blast furnace slag.

[0033] The construction material according to the invention may comprise 30% to 80% by weight of excavated clay soil, 0.1% to 10% by weight of deflocculating agent and 5 to 10% by weight of blast furnace slag, in which case the construction material preferably corresponds to a construction binder.

[0034] The construction material according to the invention comprises: - between 5 and 20% by weight of raw clay from excavated clay soil; - between 0.1 and 3 wt. % of a deflocculating agent; - between 3 and 15 wt. % of an activator; - between 25 and 45% by weight of sand; - between 35 and 55% by weight of aggregates It may include, The construction material therefore preferably corresponds to in-situ concrete.

[0035] As shown in the examples, the construction material according to the invention has improved mechanical performance.

[0036] Furthermore, the excavated clayey soil may advantageously be pre-treated, the pre-treatment being selected from crushing, screening, sieving and / or drying the excavated clayey soil. Pre-treatment may, for example, include fractionation.

[0037] According to another aspect, the present invention relates to a method for preparing a construction material according to the invention from excavated clay soil, comprising the steps of: - excavating clay soil; - screening the excavated clay soil, if necessary, when the excavated clay soil contains stones retained by 2 cm screening; - mixing the excavated clayey soil, preferably the fraction less than 50 μm, a deflocculating agent and an activator; The present invention relates to a method comprising the steps of:

[0038] According to another aspect, the present invention further provides a system for preparing a construction material comprising excavated clay soil, the system comprising: - at least one container containing excavated clay soil; at least one container containing a deflocculating agent; at least one container containing an activator; a mixing device having automated transport means between the container and the mixing device, a control module configured to generate an output signal that is used by an automated transport means to transport the determined amount of deflocculating agent and activating agent to a mixing device; The present invention relates to a system comprising:

[0039] Advantageously, the system for preparing a construction material according to the invention comprises communication means configured to receive data relating to the determined amount of deflocculating agent and the determined amount of activating agent adapted to the excavated clayey soil, the control module being configured to generate an output signal to be used by the automated transport means to transport the determined amounts of deflocculating agent and activating agent to the mixing device.

[0040] Preferably, the system for preparing a building material according to the present invention comprises means for measuring at least one physicochemical property of the excavated clayey soil and a calculation means, the calculation means being capable of implementing a computer program configured to perform the steps of obtaining measurements of at least one physicochemical property of the excavated clayey soil and determining the amount of deflocculating agent and the amount of activator adapted to the excavated clayey soil based on a comparison of the one or more measurements with reference values.

[0041] In particular, the present invention further provides a system for preparing a construction material comprising excavated clay soil, the system comprising: - at least one container containing excavated clay soil; at least one container containing a deflocculating agent; at least one container containing an activator; a mixing device having automated transport means between the container and the mixing device, - a means for measuring at least one physicochemical property of the excavated clayey soil; - a computational means, obtaining measurements of at least one physicochemical property of the excavated clayey soil; determining an appropriate amount of deflocculating agent and an appropriate amount of activating agent for the excavated clay soil based on a comparison of the one or more measurements with a reference value; a computing means adapted to execute a computer program configured to execute a control module configured to generate an output signal for use by an automated transport means to transport the determined amount of deflocculating agent and activating agent to a mixing device; The present invention relates to a system comprising:

[0042] Such systems can automatically form construction binders or even in-situ concrete (with added fillers) from excavated clay soil, construction materials with mechanical properties comparable to traditional materials that have a much larger carbon footprint.

[0043] Other advantages and features of the present invention will become apparent upon reading the following description, given by way of illustrative and non-limiting example, with reference to the attached figures, in which: [Brief description of the drawings]

[0044] [Figure 1] 1 depicts method steps for selecting a composition of a construction material comprising excavated clay soil according to one embodiment of the present invention. The dashed steps are optional. [Diagram 2] 2 represents the steps of a method for calibrating a computational algorithm for determining the composition of an in-situ construction material. The dotted steps are optional. [Diagram 3] 3 depicts steps of a method for preparing a construction material from excavated clay soil. The dotted steps are optional. [Figure 4] FIG. 4 depicts a method for preparing a construction material according to one embodiment of the present invention. [Diagram 5] 5 depicts a method for preparing a construction material according to one embodiment of the present invention. The dotted steps are optional. [Figure 6] 6 represents a diagram showing the functional structure of a system for preparing construction material comprising excavated clay soil according to the invention, the solid arrows represent the means of transport and the dotted arrows represent data transfer or instructions, particularly to the means of transport. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0045] Aspects of the present invention will be described with reference to flowcharts and / or block diagrams of methods, apparatus (systems) and computer program products according to embodiments of the invention. In the figures, the flowcharts and block diagrams illustrate the architecture, functionality, and operation of possible implementations of systems, methods and computer program products according to various embodiments of the invention.

[0046] In this regard, each block of the flowcharts or block diagrams may represent a system, device, module, or code that comprises one or more executable instructions for implementing one or more specified logical functions. In some implementations, the functions associated with the blocks may appear in a different order than that shown in the figures. For example, two blocks shown in succession may in fact be executed substantially simultaneously, or the blocks may be executed in the reverse order depending on the functionality involved. Each block in the flow diagrams and / or flowcharts, and combinations of blocks in the flow diagrams and / or flowcharts, may be implemented by a specialized hardware system that performs a particular function or operation, or a combination of specialized hardware and computer instructions.

[0047] Description of the Invention In the remainder of the description, the expression "clay soil" must be understood as corresponding to a soil derived from clay (clay-containing soil) or, more generally, to a soil derived from loose strata of fine particle size and thus containing one or more rock materials based on hydrated silicates or aluminosilicates of lamellar structure. In particular, clay soils can correspond to soils such as sandy clay silt soils, clay silt soils, clay sand soils, clay soils, etc. Preferably, the clay soils contain at least 25% by weight of clay, preferably at least 30% by weight of clay, more preferably at least 40% by weight of clay. The clay content by weight can be determined by standard methods of the prior art, such as the particle size method described in the NF X31-107 standard. Moreover, preferably, clay soils in the framework of the present invention contain at most 95% by weight of clay, preferably at most 90% by weight of clay, more preferably at least 80% by weight of clay.

[0048] The expression "excavated clay soil" in the sense of the present invention corresponds to a clay soil obtained after a step of excavating the soil, for example during land preparation and / or earthworks, for construction, building or backfilling purposes. In particular, within the meaning of the present invention, the excavated clay soil may or may not be removed from the production site. Preferably, according to the advantages of the present invention, the excavated clay soil is used at the production site or at a distance of less than 200 km. Moreover, advantageously, the excavated clay soil within the framework of the present invention is raw excavated clay soil, i.e. it has not undergone a calcination step. In particular, it has not undergone a thermal pretreatment. For example, this corresponds to a clay soil that has not undergone an increase in temperature above 300°C, preferably above 200°C, more preferably above 150°C. In fact, raw clay can be subjected to a heating step, which generally requires a temperature increase substantially equal to 150°C, but without a calcination step. Clays used conventionally have a relatively constant particle size profile with sizes below 2 μm. Excavated clay soils can have different particle size profiles. In the framework of the present invention, the excavated clay soil may contain particles with a size of more than 2 μm, preferably more than 20 μm, more preferably more than 50 μm, more than 75 μm, for example as determined according to the ASTM D422-63 standard. Preferably, the excavated clay soil does not contain aggregates larger than 2 cm, as determined according to the NF EN 933-1 standard.

[0049] The term "wt. %" in relation to excavated clay soil, composition, binder or in-situ concrete should be understood as being relative to the dry weight of the composition, binder or in-situ concrete. The dry weight corresponds, for example, to the weight before the addition of water required to form the construction material.

[0050] The expression "construction material" within the meaning of the present invention corresponds to construction binders or in-situ concrete, which in particular comprises fillers such as aggregates and / or sand.

[0051] "Depeptizer" means any compound that dissociates aggregates and colloids in an aqueous suspension. Deflocculants have been used, for example, in the context of oil drilling or extraction to make clay more fluid and easier to extract or drill.

[0052] By "activator" is meant any composition that functions to promote the dispersion of an aluminosilicate source, promoting the formation of stable hydrates with low solubility and the formation of compact structures with these hydrates, thereby improving the mechanical strength of materials incorporating such activating compositions.

[0053] The term "particle size" in the sense of the present invention corresponds to the distribution of clayey soil elements and particles according to the relative proportion by weight of the different classes of particles distinguished by their size and constituting the mineral skeleton of the soil. There are five particle size classes: - clay (0-2 micrometers), - fine silt (2-20 micrometers), - coarse silt (20-50 micrometers), - fine sand (50-200 micrometers), - coarse sand (200-2000 micrometers).

[0054] The expression "nature of clay" within the meaning of the present invention corresponds to the chemical and / or mineralogical characteristics of the clay. It particularly corresponds to the chemical composition of the clay, but also to the mineralogical and physical properties of the clay (specific surface, porosity, morphology, etc.). For example, it may correspond to the identification of the clay by its common name (for example kaolinite, illite, montmorillonite, smectite, bentonite, chlorite and vermiculite).

[0055] The expression "metallic trace elements" corresponds to metallic chemical elements, in particular they correspond to metals, in the sense of the present invention, selected from iron, lead, mercury, uranium, chromium, copper, cadmium, silver, gold, zinc, nickel or titanium.

[0056] The term "substantially equal" within the meaning of the present invention corresponds to a value that varies from a comparison value by less than 20%, preferably by less than 10%, and even more preferably by less than 5%.

[0057] By "model" or "rule" or "calculation algorithm" is understood within the meaning of the present invention a finite sequence of operations or instructions that makes it possible to select values ​​of the amounts of deflocculating agent and activating agent, i.e. for example to form predefined groups Y associated with scores or categories, as a function of the correlation between the amounts of deflocculating agent D and activating agent A on the one hand, and one or more values ​​of physicochemical properties of the excavated clayey soil E. The implementation of this finite sequence of operations makes it possible, for example, to assign a label Y0 to an observation described by a set of properties D0, A0, E0. This is for example thanks to the implementation of a function f that makes it possible to reproduce Y with the observed D, A and E. Y=f(D,A,E)+e where e represents the noise or measurement error. Here, Y can be, for example, the ability to form building materials (yes / no).

[0058] Advantageously, the calculation algorithm can establish predefined groups and associate other values, such as values ​​of mechanical properties M of construction materials that can be formed from these quantities. Thus, using the formula "M=f(D,A,E)+e" it is possible to select values ​​of quantities for forming construction materials with predetermined mechanical properties.

[0059] A “supervised learning method” within the meaning of the present invention is a method for learning n labeled observations (X 1…n ,Y 1…n ,D 1…n ,,A 1…n ,,E 1…n ) where, for example, Y=f(D,A,E)+e or M=f(D,A,E)+e.

[0060] "Process", "calculate", "determine", "display", "extract", "compare" or more broadly "executable operations" refer, within the meaning of the present invention, to operations performed by a device or a processor, unless the context indicates otherwise. In this respect, operations refer to operations and / or processes in a data processing system, such as a computer system or an electronic computing device, that manipulate and transform data represented as physical (electronic) quantities in the memory of the computer system or other device in order to store, transmit or display information. In particular, computational operations are performed by the processor of the device, the generated data are written to corresponding fields in the data memory, and this or these fields can be returned to the user, for example, via an adapted human-machine interface, such as the screen of a connected object, as a non-limiting example, formatting such data. These operations may be based on applications or software.

[0061] The terms or expressions "application," "software," "program code," and "executable code" refer to any expression, code, or notation of a set of instructions intended to cause a data processing system to perform a particular function, either directly or indirectly (e.g., after translation into another code). Exemplary program code may include, but is not limited to, subprograms, functions, executable applications, source code, object code, libraries, and / or any other sequence of instructions designed to be executed on a computer system.

[0062] By "processor" is meant, within the meaning of the present invention, at least one hardware circuit configured to carry out operations according to instructions contained in a code. The hardware circuit may be an integrated circuit. Examples of processors include, but are not limited to, central processing units, graphic processors, application specific integrated circuits ("ASIC" in Anglo-Saxon terminology) and programmable logic circuits. The invention can be implemented using a single processor or several other units.

[0063] "Coupled" within the meaning of the present invention means directly or indirectly connected to one or more intermediate elements. Two elements may be mechanically, electrically coupled, or linked by a communication channel.

[0064] The expression "human-machine interface" within the meaning of the present invention corresponds to any element allowing a human being to communicate with a computer, in particular, and without this list being exhaustive, to a keyboard and means for responding to commands entered via the keyboard, displaying the screen and, optionally, selecting items displayed on the screen with a mouse or a touchpad. Another embodiment is a touchscreen for directly selecting elements on the screen touched by a finger or an object, with the possibility of optionally displaying a virtual keyboard.

[0065] In the claims, the term "comprise" or "include" does not exclude other elements or steps.

[0066] In the following description, the same references are used to designate the same elements. The reference signs should not be understood as limiting the scope of the invention. Furthermore, different features which are presented and / or claimed may be advantageously combined. Their presence in the specification or in different dependent claims does not exclude this possibility.

[0067] As mentioned above, currently there are large volumes of excavated soils, which are often considered waste and therefore constitute an additional burden for developers when developing sites. The pollution that may be generated by such management, and in particular the transportation of these excavated soils, is in addition to the pollution generated by the preparation of conventional cements (e.g. Portland).

[0068] Faced with this observation, the inventors have identified a method that allows the use of excavated clay soil to select the composition of the construction material and obtain a construction binder with mechanical properties similar to those of traditional cement (e.g., Portland). Using this method, construction binders can be produced that can be advantageously used as, but not limited to, substitutes for Portland cement, lime, or CSA, as shown in the examples. Thus, waste material (i.e., excavated clay) combined in specific proportions with deflocculating agents and activators can become a raw material for construction processes.

[0069] Moreover, considering on the one hand its preparation method and on the other hand the use of excavated clay soil, the construction material according to the invention has the advantage of having a carbon footprint at least two times lower than most of the construction materials or hydraulic binders most used in the world today (i.e. Portland cement). In fact, the construction material according to the invention is mainly made of clay soil and has zero or less clinker content than comparable products, which allows reducing CO2 emissions and production costs with comparable mechanical properties. Moreover, preferably, the clay soil has not undergone a calcination step, which is an energy-consuming step that also generates the emission of greenhouse gases, more specifically carbon dioxide.

[0070] Finally, advantageously, as shown in the examples, the construction binder according to the invention makes it possible to produce construction materials having mechanical properties at least comparable to those of Portland cement and significantly better than those of the "low carbon" materials described above.

[0071] Thus, according to a first aspect, the present invention relates to a method 100 for selecting a composition of a construction material comprising excavated clay soil. Since the construction binder can then be used to form an in-situ concrete, e.g. following the addition of a filler, the selection method 100 can alternatively correspond to a method 100 for selecting a composition of an in-situ concrete.

[0072] In particular, to enable the preparation of a construction material from excavated clay soil, the composition of the construction material must contain deflocculating agents and activating agents in amounts adapted to the excavated clay soil.

[0073] For this purpose, the method according to the invention, preferably implemented by a computer device including a calculation module, may comprise a step 130 of receiving from the calculation module measurements of at least one physicochemical property of the excavated clayey soil, and a step 170 of selecting by the calculation module an amount of deflocculating agent and an amount of activator adapted to the excavated clayey soil.

[0074] Furthermore, the method according to the invention may comprise the steps of: pre-treating 110 the excavated clayey soil, measuring 120 the physicochemical properties of the excavated clayey soil, receiving 140 a desired mechanical property value of the construction material, generating 150 a plurality of combinations of values ​​of the amounts of deflocculating agent and activating agent, determining 160 a desired mechanical property value of the construction material or determining at least one physicochemical or mechanical property value of the construction material to be formed.

[0075] As shown in Figure 1, the selection method according to the invention may include a step of pre-treating the excavated clayey soil 110. Advantageously, therefore, one or more measurements are obtained from a sample of the excavated clayey soil that has been subjected to the excavated clayey soil pre-treatment step 110.

[0076] This pre-treatment step may, for example, include or consist of separating, crushing, sorting (eg by color), sieving and / or drying the excavated clay soil.

[0077] In particular, within the framework of the present invention, clay soil is an excavated soil and therefore may contain coarse elements or high-dimensional fractions that will be advantageously removed in the first stage of the method. In particular, the method according to the present invention may therefore comprise removing elements having at least one dimension greater than 1 cm (centimeter), preferably removing elements having at least one dimension greater than 0.2 cm. Preferably, the method according to the present invention may comprise removing elements having a size greater than at least 1 cm, preferably greater than 475 μm (micrometer), more preferably greater than 75 μm, as determined according to the ASTM D422-63 standard.

[0078] Furthermore, the method according to the invention may comprise a step 120 of measuring at least one physicochemical property of the excavated clayey soil. This step is preferably carried out on a sample of the excavated clayey soil and can be carried out on-site or in a specialized laboratory. Indeed, depending on the physicochemical property or properties measured, it may or may not have a portable instrument.

[0079] The measuring step 120 may, for example, - the clay content in the excavated clayey soil, measured by the particle size method, for example as described in the NF X31-107 standard; - the properties of clay, e.g. obtained by X-ray diffraction; - the content of impurities, in particular the content of metallic trace elements, obtained by elemental analysis, for example using an ICP-MS instrument; -Salinity by conductivity meter measuring the conductivity of clay soil washing water; -pH using a pH meter to measure the pH of the clay soil wash water; and - the total exchange capacity of clay in excavated clay soils, determined for example by the so-called methylene blue method according to the NF EN 933-9+A1 standard The method may include measuring

[0080] Thus, the measuring step 120 may involve, for example, using a pH meter, an X-ray diffractometer, a conductivity meter, an electron microscope, a mercury porosimeter, a spectrofluorometer, an ICP-MS (English: Inductively Coupled Plasma Mass Spectrometry), an HPLC-MS (liquid chromatography coupled to mass spectrometry), a GC-MS (gas chromatography coupled to mass spectrometry), a measurement of the specific surface by the BET method (specific surface measurement of Brunauer-Emmett-Teller), a granulometer or a TGA (for thermogravimetric analysis) rheometer.

[0081] The method according to the invention comprises a step 130 of receiving measurements of at least one physicochemical property of the excavated clayey soil. In particular, this step can be performed by a computing module of a digital device.

[0082] The physicochemical properties of the excavated soil for which measurements are received may be selected from the clay content in the excavated clay soil, the nature of the clay, the particle size, the content of impurities, the presence of contaminants, the flow limit, the plasticity limit, the content of metal oxides, the salinity, the pH, and the total exchange capacity of the clay in the excavated clay soil. For example, the physicochemical properties of the excavated soil for which measurements are received may be selected from the clay content in the excavated clay soil, the nature of the clay, the particle size, the content of impurities, the content of metal oxides, the salinity, the pH, and the total exchange capacity of the clay in the excavated clay soil. Preferably, the physicochemical properties of the excavated soil for which measurements are received may be selected from, for example, the clay content in the excavated clay soil, the flow limit, and the plasticity limit. More preferably, the physicochemical properties of the excavated soil for which measurements are received include the clay content in the excavated clay soil.

[0083] In particular, the impurity content may correspond to the metal content and advantageously to the metal oxide content, such as iron oxide or aluminum oxide.

[0084] Preferably, measurements of at least two physicochemical properties of the excavated clayey soil are received, more preferably at least three, even more preferably at least four measurements are received. Indeed, depending on the number of physicochemical properties considered, the results of the selection method may be of better quality.

[0085] The one or more physicochemical properties are widely studied soil physicochemical properties such as pH, particle size, clay content, etc.

[0086] In particular, the method according to the invention comprises: -Clay content and clay properties in the excavated clay soil; -Clay content and total clay exchange capacity in excavated clay soils; - clay content and amount of contaminants; -The pH and clay content of excavated clay soils; or - Total exchange capacity and particle size of clay in excavated clayey soil and receiving 130 a combination of measurements selected from:

[0087] Additionally, as shown in FIG. 1, the method according to the present invention may include receiving 140 a desired mechanical property value of the construction material.

[0088] Indeed, in addition to selecting a composition of the construction material, the method according to the invention can advantageously make it possible to select a composition of the construction material that allows the preparation of a construction material that gives mechanical properties, allowing the user to select the optimal amount to obtain a construction material that meets his needs.

[0089] The desired mechanical properties of the construction material may be selected from, for example, compressive strength, drying shrinkage, setting time, flexural strength, tensile strength, Young's modulus, Poisson's ratio.

[0090] For example, a method according to the present invention may include receiving a desired compressive strength value for a construction material, which may comprise, for example, a lower limit (e.g., 20 MPa (megapascals) or 30 MPa) or a fixed value (e.g., 40 MPa).

[0091] Preferably, when the method according to the invention comprises receiving 140 a desired mechanical property value of a construction material, the step of selecting 170 the amounts of deflocculating agent and activating agent further comprises excluding 171 amounts of deflocculating agent and activating agent that do not enable the construction material to exhibit the desired mechanical property value. For example, this may correspond to the selection by the calculation algorithm of all values ​​of A and D that are able to generate, from the measured value of E, a value of M=40 MPa. Alternatively, in the absence of a calculation algorithm, this may comprise excluding all values ​​from the database with a value of M less than 30 MPa.

[0092] The step 130 of receiving measurements of at least one physicochemical property of the excavated clayey soil may be followed by a step 150 of generating a plurality of combinations of values ​​of the amount of deflocculating agent on the one hand and values ​​of the amount of activating agent on the other hand. Following the generation of this plurality of values, the calculation module may perform a value selection step 170, as described below.

[0093] Furthermore, the method according to the invention may comprise a step 160 of determining the value of at least one physicochemical or mechanical property expected for the construction material, this step being carried out for example by a calculation module.

[0094] From the measured values ​​of the physicochemical properties of the excavated clayey soil and the values ​​of the amounts of deflocculating agent and activating agent produced, it is possible to determine the values ​​of the mechanical properties of the construction material formed from the excavated soil and the amounts of deflocculating agent and activating agent considered.

[0095] The method according to the invention comprises a step 170 of selecting an amount of deflocculating agent and an amount of activating agent adapted to the excavated clayey soil, which step can be performed, for example, by a calculation module.

[0096] The amount of deflocculating agent and activating agent may correspond to a volume, a mass or a ratio. Preferably, the amount corresponds to a ratio to the amount of excavated clay soil added to the composition of the construction material. Alternatively, if the amount corresponds to a volume or mass, it is related to the amount of excavated clay soil added to the composition of the construction material.

[0097] Additionally, selecting 170 the amount of deflocculating agent and the amount of activating agent may include determining the nature of the deflocculating agent and / or activating agent to be added. For example, the nature of these agents may correspond to a family of chemical molecules or a particular chemical molecule or combination of molecules.

[0098] In fact, the peptizer may be a combination of molecules, and the selection of the amount of peptizer may correspond to the selection of the amount of each molecule that makes up the peptizer. The same applies to the activator, which may be one molecule or multiple molecules.

[0099] Advantageously, the selection is based on a comparison of one or more measurements of physicochemical properties of the excavated clay soil with a reference value, in particular the reference value comprising a correlation between the measurement of at least one physicochemical property of the clay soil and the amount of deflocculating agent and activating agent applied to the clay soil to form the construction material.

[0100] Deflocculating agent Many compounds can act as peptizers and many are commonly known to those skilled in the art.

[0101] In the framework of the present invention, the deflocculating agent is in particular a non-ionic surfactant, such as a polyoxyethylene ether, which may be chosen, for example, from poly(oxyethylene) lauryl ether.

[0102] The deflocculating agent may also be an anionic agent, such as an anionic surfactant. In particular, the anionic agent may be selected from alkylarylsulfonates, amino alcohols, carbonates, silicates, fatty acids, humates (e.g., sodium humate), carboxylic acids, lignosulfonates (e.g., sodium lignosulfonate), polyacrylates, phosphates, or polyphosphates, such as sodium hexametaphosphate, sodium tripolyphosphate, sodium orthophosphate, carboxymethylcellulose, and mixtures thereof.

[0103] The peptizer can also be a polyacrylate, and thus may be selected, for example, from sodium polyacrylate and ammonium polyacrylate.

[0104] The peptizer may also be an amine selected from, for example, 2-amino-2-methyl-1-propanol, mono-, di-, or triethanolamine, isopropanolamine (1-amino-2-propanol, diisopropanolamine, and triisopropanolamine), and N-alkylated ethanolamines.

[0105] The peptizer can also be a silicate, such as sodium silicate, sodium metasilicate, or sodium trisilicate.

[0106] Alternatively, as noted above, the deflocculating agent can be a mixture of compounds, such as a mixture comprising at least two compounds selected from nonionic surfactants, anionic agents, polyacrylates, amines, and organophosphorus compounds.

[0107] In particular, the peptizer may be a mixture of sodium silicate and sodium carbonate.

[0108] Preferably, the deflocculating agent is selected from lignosulfonates (eg, sodium lignosulfonate), polyacrylates, humates, and mixtures thereof.

[0109] The peptizer is preferably in the form of a salt.

[0110] However, the present invention is not limited to the above deflocculating agents, and any type of deflocculating agent known to those skilled in the art may be used in place of the above deflocculating agents.

[0111] Activator It is the activator that, in conjunction with the excavated clay soil and the deflocculating agent, gives the construction material its desired mechanical properties.

[0112] Without being limited by theory, the activator may enable the formation of a network between the clay sheets that gives the construction material according to the invention its mechanical properties.

[0113] In particular, the activator may include a metal oxide and / or may be an alkaline activating composition.

[0114] Preferably, the metal oxide is a transition metal oxide. More preferably, the metal oxide may be selected from iron oxides such as FeO, Fe3O4, Fe2O3, Fe2O3, alumina Al2O3, manganese (II) oxide MnO, titanium (IV) oxide TiO2, and mixtures thereof.

[0115] The metal oxides may preferably be derived, for example, from the composition of blast furnace slag formed during the production of pig iron from iron ore.

[0116] The metal oxide is present in a content of at least 2% by weight of the construction material, preferably at least 5% by weight of the construction material, more preferably at least 10% by weight of the construction material.

[0117] When the activator is an alkaline activating composition, the alkaline composition may comprise a compound having a pKa preferably greater than or equal to 10, more preferably greater than or equal to 12, even more preferably substantially equal to 14.

[0118] The alkaline composition may include an organophosphorus compound, such as, for example, sodium tripolyphosphate, which is designated by the acronym NaTPP.

[0119] In particular, the activator may include a mixture of sodium hydroxide and sodium silicate.

[0120] Advantageously, the activator may be an alkaline activating composition further comprising a metal oxide. As shown in the examples, the construction binder prepared from such an activator has good mechanical properties. Therefore, preferably, the activator may comprise a metal oxide and at least one compound having a pKa of 10 or more.

[0121] Furthermore, the selection step 170 may include determining 172 the amount of additives to be incorporated into the composition of the construction material. Indeed, the selection method according to the invention may result in a composition of the construction material containing determined concentrations of several additives, which may modify the chemical and / or mechanical properties of the final construction material.

[0122] The additives are, for example, selected from flow agents, synthetic or natural rheology retaining agents, shrinkage inhibitors, water retention agents, air entraining agents, synthetic resins, pigments and mixtures thereof.

[0123] The flow agent can be, for example, a polyacrylate, a polynaphthalenesulfonate, a polycarboxylate, or a polyphosphonate.

[0124] Additionally, the selection step 170 may include determining 173 the amount of fillers to be incorporated into the mix to form the in-situ concrete. These fillers may modify the mechanical properties of the final construction material.

[0125] The fillers may be selected, for example, from recycled or non-recycled aggregates, powders, sand, gravel, crushed concrete and / or fibers.

[0126] The fibers may be selected from vegetable fibers, such as, for example, cotton, flax, hemp, cellulose, bamboo, miscanthus fibers, synthetic fibers, such as metal, glass, carbon, polypropylene fibers, and mixtures thereof. The presence of fibers may allow the formation of building materials with improved mechanical and insulating properties.

[0127] Advantageously, and as previously mentioned, step 170 of determining the amount of deflocculating agent and the amount of activator adapted to the excavated clay soil involves implementing a pre-calibrated computational algorithm.

[0128] This computational algorithm may be built from various learning models, in particular partitioning, supervised or unsupervised models.

[0129] The unsupervised statistical learning model may be selected, for example, from an unsupervised Gaussian mixture model, a hierarchical bottom-up classification (Hierarchical clustering Agglomerative in the Anglo-Saxon terminology), a hierarchical top-down classification (Hierarchical clustering divisive in the Anglo-Saxon terminology).

[0130] Statistical supervised learning models may be selected from among kernel methods (such as support vector machines (SVM), kernel ridge regression) as described, for example, in Burgess, 1998 (Data Mining and Knowledge Discovery, A Tutorial on Support Vector Machines for Pattern Recognition), set methods (such as bagging, boosting, decision trees, random forests) as described, for example, in Breiman, 2001 (Machine Learning, Random Forests), or neural networks as described, for example, in Rosenblatt, 1958 (Perceptrons: a Probabilistic Model for the Storage and Organization of Information in the Brain).

[0131] Preferably, the pre-calibrated computational algorithm has been obtained by implementing a statistical supervised learning method.

[0132] Thus, according to another aspect, the invention relates to a method 200 for calibrating a calculation algorithm, which calculation algorithm is in particular dedicated to the determination of the composition of construction materials. The calibration method according to the invention can in particular be implemented by a digital device including a learning module.

[0133] As shown in FIG. 2, such a calibration method according to the present invention includes a step 230 of receiving measurements of at least one physicochemical property of an excavated clayey soil.

[0134] Preferably, several measurements of the excavated clayey soil are received, in particular values ​​of at least two, more preferably at least three and even more preferably at least four physico-chemical properties. Indeed, depending on the number of physico-chemical properties considered, the calibration method will be of better quality.

[0135] The calibration method according to the invention also includes receiving 240 a deflocculating agent amount value and an activator amount value, which correspond to the amounts of agents that, when added to the excavated clay soil, allow the formation of a construction material.

[0136] The amount of deflocculating agent and activating agent may correspond to a volume, a mass or a ratio. Preferably, the amount corresponds to a ratio to the amount of excavated clay soil added to the composition of the construction material. Alternatively, if the amount corresponds to a volume or mass, it is related to the amount of excavated clay soil added to the composition of the construction material.

[0137] Additionally, receiving 240 values ​​for the amounts of deflocculating agent and activating agent may include receiving properties of the deflocculating agent and / or activating agent, which may correspond to, for example, a family of chemical molecules or a particular chemical molecule or combination of molecules.

[0138] These values ​​may be obtained through tests described in the Examples section. Only the amount of agent that allows the formation of the building material is included in the calibration method.

[0139] In fact, the calibration method may include a step 250 of forming the construction material according to the received values. Alternatively, and preferably, multiple combinations of values ​​of the amount of agent have been tested for multiple excavated clays to form a database that can be used as input data to the calibration method.

[0140] The method then includes a step 270 of making a correlation between the received measurements in order to calibrate the computation algorithm. This correlation step based on the measurements allows the computation algorithm to be built from a statistical learning model. The computation algorithm may thus take the form of a function f of the following type of equation: Y=f(E,A,D)

[0141] 2, before the preparation step 270, the calibration method according to the invention may further comprise a step 260 of receiving a measurement of at least one mechanical property of the formed construction material. Indeed, in addition to using the value of the amount of agent and one or more values ​​of the physicochemical properties of the excavated clayey soil, the calibration method according to the invention may use one or more measurements of the resulting construction material. The calculation algorithm may thus take the form of a function f of the following type of equation: M = f(E, A, D)

[0142] Preferably, several measurements are received 260, in particular values ​​of at least two, more preferably at least three, even more preferably at least four physicochemical properties of the construction material.

[0143] 2, the calibration method according to the present invention may include a step 210 of pre-treating a sample of clayey soil. Step 210 may precede a step 220 of measuring at least one physicochemical property of the clayey soil. Furthermore, once the correlation is established, the correlation may be stored 280 in a storage medium such as a RAM or non-volatile memory.

[0144] Advantageously, the calibration method according to the invention may comprise a step 290 of updating the calculation algorithm by repeating the above-mentioned and at least the following preceding steps: receiving 230 measurements of at least one physicochemical property of the excavated clayey soil, receiving 240 an amount of deflocculating agent and an amount of activating agent which when added to the excavated clayey soil form a construction material, and creating 270 a correlation between the received measurements in order to calibrate the calculation algorithm.

[0145] According to another aspect, the present invention relates to a method 300 for preparing construction material from excavated clay soil.

[0146] Such a process according to the invention, as shown in Figure 3, has the advantage that it is a so-called low-carbon process, i.e. a process in which the greenhouse gas emissions, such as in particular carbon dioxide emissions, are reduced compared to the greenhouse gas emissions of known processes for preparing construction binders, such that the reduction in greenhouse gas emissions is in particular linked to the absence of an energy-intensive calcination stage.

[0147] Furthermore, the preparation of the construction binder according to the invention may allow the preparation of an in-situ concrete made at least in part from raw materials from the construction site. Such properties further reduce the environmental footprint of the concrete produced. Once the amount of deflocculating agent and the amount of activating agent adapted to the excavated clayey soil have been selected, it is possible to proceed with the preparation of the construction material from the excavated clayey soil according to conventional methods.

[0148] The preparation method according to the present invention may include a step 310 of measuring at least one physicochemical property of the excavated clayey soil.

[0149] Such a step can be carried out well before the mixing step 340. This is the case, for example, when a preliminary investigation is carried out and the excavated soil does not need to be used quickly. Alternatively, the step 310 of measuring at least one physicochemical property of the excavated clay soil may be carried out immediately before the step 100 of selecting the composition of the construction material corresponding to the step of carrying out the method 100 according to the invention and the mixing 340. This is the case, for example, of an automated method for preparing a construction material from excavated clay soil, where the excavated clay soil is analyzed along with a portable measuring device and then continuously mixed with selected amounts of agents to form a construction material in a very short time.

[0150] Preferably, several measurements of the excavated clayey soil are received, in particular values ​​of at least two, more preferably at least three, even more preferably at least four physico-chemical properties.

[0151] Further, as shown in FIG. 3 and FIG. 4, the preparation method according to the present invention may include selecting 100 a composition of the construction material including excavated clay soil according to the present invention.

[0152] Additionally, it may include a step 340 of mixing the excavated clay soil, the deflocculating agent, and the activating agent according to a selected composition.

[0153] In the mixing step, water can be added so that the ratio of the mass of water to the mass of the construction material is less than 1, for example between 0.4 and 0.8. Furthermore, water can be advantageously added after the excavated clay soil and the peptizer are dry mixed.

[0154] Thus, preferably, the method according to the invention may include a mixing step to obtain a suspension of dispersed or deflocculated excavated clayey soil. When mixing, the deflocculating agent is preferably added before the activating agent so that the dispersed or deflocculated excavated clayey soil and the activating agent are mixed.

[0155] This mixing step 340 of the clay suspension can be advantageously, but not exclusively, carried out in equipment selected from mixers and truck mixers or more generally any equipment adapted to mix clayey soils.

[0156] Preferably, the preparation method may include a step 330 of screening the excavated clay soil, which is carried out before the mixing step 340 and before or after the measuring step 310, in particular to remove aggregates with a diameter of more than 20 mm (millimeters).

[0157] In a broader sense, the preparation method may include preparing excavated clay soil, where the preparation may include, for example, drying, grinding, sieving, and storing.

[0158] Preferably, the pretreatment or screening step comprises at least one fractionation such as sieving, more preferably fractionation such as sieving at 50 μm. Advantageously, but not exclusively, the elements or particles thus sieved (such as the sand and / or aggregate fraction) can be reused in the mix of construction materials, in particular in-situ concrete. The fractions of most interest in the preparation of construction materials are those not retained by the sieve. Thus, the method 300 according to the invention for preparing construction materials from excavated clayey soil advantageously comprises a step 335 of fractionating the optionally sieved excavated clayey soil, the fractionation being preferably carried out at 50 μm.

[0159] Alternatively, the excavated clay soil may not be pretreated and all of the clay soil may be used to obtain a construction material, in which case the method may be used to produce in-situ concrete.

[0160] This advantageously allows for the reclamation of all excavated clay soil, especially when the physicochemical properties associated with the excavated clay soil are sufficient to obtain a construction material with the desired mechanical properties. In this way, all soil can be reclaimed from the beginning, without the need to separate and process the clay and blend the material.

[0161] As shown in FIG. 5, a method 300 according to the present invention for preparing a construction material from excavated clay soil includes: - Step 320 of excavating clay soil; a step 330 of screening the excavated clayey soil if the excavated clayey soil contains stones retained by 2 cm screening, - step 340 of mixing the excavated clayey soil, preferably the fraction below 50 μm, the deflocculating agent and the activator; Advantageously,

[0162] Furthermore, the preparation method can advantageously include a step of treating contaminants, which can reduce the concentration of contaminants in the excavated clay soil, such as trace metal elements, hydrocarbons (e.g. polycyclic aromatic hydrocarbons, C10-C40, etc.), PCBs (polychlorinated biphenyls), BTEX (benzene, toluene, ethylbenzene, xylene), TOC (total organic carbon), etc.

[0163] Furthermore, conventionally, before, concomitantly with or after the addition of the activating composition, the method according to the invention may comprise the addition of additives or fillers for modifying the mechanical properties of the final construction material.

[0164] Advantageously, the preparation method may comprise measuring 350 one or more values ​​of a physicochemical or mechanical property of the construction material during the mixing step (i.e. while the construction material is being formed) and comparing 360 the measured values ​​with predetermined values ​​of the physicochemical or mechanical property of the construction material being formed.

[0165] This allows quality control of the construction material being formed.

[0166] Furthermore, when the measured value differs from a predefined value of the physicochemical or mechanical property of the resulting construction material, the preparation method may comprise a step 370 of adding at least one complementary ingredient.

[0167] In this specification, the complementary components may be selected from, for example, deflocculants, activators, and excavated clay soils to modify the desired composition. The complementary components may also be selected from additives or fillers as described above.

[0168] This ensures that the resulting construction material has mechanical properties as close as possible to the expected mechanical properties: in fact, deviations are identified during mixing and corrected before the material is used.

[0169] Further, as shown in FIG. 4, the method is completed by step 380 of recovering the formed building material.

[0170] According to another aspect, the present invention relates to a system 400 for preparing a construction material comprising excavated clay soil. Alternatively, as discussed, the present invention relates to a system 400 for preparing in-situ concrete comprising excavated clay soil.

[0171] Such a method according to the invention, as shown in Fig. 5, may include containers 410, 420, 430 for the various components of the construction material. For example, it may include at least one container 410 for excavated clay soil, at least one container 420 for a deflocculating agent, and at least one container 430 for an activating agent. Furthermore, it may include at least one container 440 for fillers and / or additives. Furthermore, the system may include a washing container for holding a washing liquid.

[0172] In particular for excavated clay soil, the container 410 may not be an object but simply a place where the excavated clay soil is stored. The container may also be selected from a tank, a container, a bin, or a silo.

[0173] Furthermore, the system according to the invention comprises a mixing device 450. In particular, such a device is capable of homogenizing and / or mixing the precursor components of the construction binder.

[0174] This mixing device 450 is in particular coupled to automated transport means (represented by arrows between the containers 410, 420, 430, 440, respectively, and the mixing device 450) arranged between the containers 410, 420, 430 and the mixing device 450. These transport means can be, for example, flexible or inflexible pipes, belts, conveyors or augers. Furthermore, in combination with the transport means, the system may include pumps, valves, solenoid valves and flow restrictors. In particular, the flow restrictors may be arranged to functionally switch with each of the transport means in order to independently regulate the amount of each component delivered to the mixing device 450.

[0175] Furthermore, the system according to the invention may comprise means 460 for measuring at least one physicochemical property of the excavated clay soil. Such measuring means 460 may be, for example, a pH meter, an X-ray diffractometer, a conductivity meter, an electron microscope, a mercury porosimeter, a spectrofluorometer, an ICP-MS, an HPLC-MS, a GC-MS, measurement of the specific surface area by the BET method, a granulometer or a rheometer.

[0176] Furthermore, the system according to the present invention comprises: - obtaining measurements of at least one physicochemical property of the excavated clayey soil; - determining an amount of deflocculating agent and an amount of activating agent suitable for the excavated clay soil based on a comparison of the one or more measurements with a reference value; The method may include a computing means 470 adapted, preferably configured, to execute a computer program configured to perform the steps of:

[0177] Furthermore, the system according to the present invention includes a control module 480 configured to generate output signals for use by the automated transport means. Such output signals would enable the system to transport determined amounts of deflocculating agent and activating agent to the mixer 450. Furthermore, they may enable a predetermined amount of excavated clay soil to be transported to the mixer 450.

[0178] Preferably, the system for preparing a construction material according to the invention may further comprise a screen (preferably a compact one), a soil breaker, a planetary mixer.

[0179] More preferably, it may include a soil breaker. In particular, the soil breaker makes it possible to eliminate the presence of agglomerate particles that may affect the construction binder and the quality of the in-situ concrete. Moreover, the powdered clayey soil will provide a uniform appearance to the in-situ concrete.

[0180] Even more preferably, the system for preparing a construction material according to the invention comprises a sieve for isolating pebbles having a diameter of more than 10 cm, preferably more than 2 cm. The system for preparing a construction material may also comprise a sorting means, for example of the sieve type, for isolating particles having a diameter of less than 50 μm, preferably particles having a diameter of less than 20 μm. Advantageously, but not exclusively, the elements or particles thus separated, such as the sand and / or aggregate fraction, can be reused in the mix of construction materials, in particular in-situ concrete.

[0181] Alternatively, the excavated clay soil may not need to be pretreated and all of the clay soil may be used to obtain the construction material, in which case the method may be used to produce in-situ concrete.

[0182] It may also include pollution control equipment for treating excavated soil before use.

[0183] Thus, according to another aspect, the present invention relates to a construction material formed from excavated clay soil. In particular, this construction material may be prepared according to the preparation method according to the invention described above. For example, this construction material is directly prepared according to the preparation method according to the invention described above.

[0184] The construction material according to the present invention is characterized in that it comprises a deflocculating agent and excavated clay soil. It should be noted that the preparation of the construction material comprises adding an activator. However, this activator is not systematically found in the construction material, since it may react with the excavated clay soil. Nevertheless, sometimes the construction material according to the present invention may comprise a deflocculating agent, an activator and excavated clay soil.

[0185] Considering the possible addition of fillers, the present invention also relates to an in-situ concrete characterized in that it comprises a deflocculating agent and an excavated clay soil.

[0186] Alternatively, when no filler is added, the present invention also relates to a construction binder characterized in that it comprises a deflocculating agent and excavated clay soil.

[0187] Advantageously, the construction material according to the invention comprises a mixture of different types of clay, in particular - illite and kaolinite, - illite and kaolinite and bentonite, - illite and bentonite, - kaolinite and bentonite, - illite and montmorillonite, or - combinations of kaolinite, illite, smectite, bentonite, chlorite, montmorillonite, muscovite, hallosite, sepiolite, attapulgite and vermiculite; The clay may include a combination of clays selected from:

[0188] Moreover, advantageously, the construction material is formed from excavated clay soil characterized in that it contains up to 80% by weight of particles larger than 2 μm, preferably up to 60% by weight of particles larger than 2 μm. The content of particles larger than 2 μm can be measured, for example, according to the NF X31-107 standard. Thus, the excavated soil preferably undergoes a pretreatment step to result in a particle size centered on a fraction with a size diameter of 50 μm or less, preferably 20 μm or less.

[0189] Preferably, the construction material according to the invention comprises at least 50% by weight of excavated clay soil, at least 60% by weight of excavated clay soil, at least 70% by weight of excavated clay soil, at least 80% by weight of excavated clay soil, most preferably at least 90% by weight of excavated clay soil, which is advantageous when the construction material is a construction binder.

[0190] In fact, selecting the amount of deflocculating agent and activator provides the advantage of being able to form a construction binder with a large amount of excavated clay soil without changing the mechanical properties of the resulting construction material. When the construction material is in-situ concrete, it may comprise at least 10% by weight of excavated clay soil, at least 15% by weight of excavated clay soil, at least 20% by weight of excavated clay soil, at least 30% by weight of excavated clay soil, at least 40% by weight of excavated clay soil, at least 50% by weight of excavated clay soil.

[0191] The deflocculating agent may comprise at least 0.1% by weight of the construction material, at least 0.20% by weight of the construction material, at least 0.25% by weight of the construction material, preferably at least 0.5% by weight of the construction material, more preferably at least 1% by weight of the construction material, even more preferably at least 1.5% by weight of the construction material, and for example at least 2% by weight of the construction material, which is advantageous when the construction material is in-situ concrete.

[0192] The deflocculating agent may represent at least 0.30% by weight of the construction material, at least 0.5% by weight of the construction material, preferably at least 1% by weight of the construction material, more preferably at least 1.5% by weight of the construction material, even more preferably at least 2% by weight of the construction material, and for example at least 2.5% by weight of the construction material, which is advantageous when the construction material is a construction binder.

[0193] Further, the deflocculating agent may comprise up to 20% by weight of the construction material, preferably up to 15% by weight of the construction material, and more preferably up to 10% by weight of the construction material.

[0194] In particular, the deflocculating agent may represent between 0.25 and 10% by weight of the construction material, preferably between 0.5 and 10% by weight of the construction material, more preferably between 1 and 10% by weight of the construction material, even more preferably between 2 and 8% by weight, and for example between 2 and 5% by weight of the construction binder.The deflocculating agent may thus preferably represent between 0.1 and 5% by weight of the construction material.

[0195] In particular, the deflocculating agent comprises at least 0.5% by weight of the excavated clayey soil, preferably at least 1% by weight of the excavated clayey soil, more preferably at least 2% by weight of the excavated clayey soil, even more preferably at least 3% by weight, and for example at least 4% by weight of the excavated clayey soil. Indeed, at such a deflocculating agent concentration, the binder formulation according to the invention can then be used in combination with an activating composition to form a material having advantageous mechanical properties.

[0196] Furthermore, the deflocculating agent comprises up to 20% by weight of the excavated clayey soil, preferably up to 10% by weight of the excavated clayey soil. Indeed, too high a concentration is not necessary to form a material with advantageous mechanical properties.

[0197] In particular, the deflocculating agent comprises between 0.5 and 20% by weight of the excavated clayey soil, preferably between 1 and 10% by weight of the excavated clayey soil, more preferably between 3 and 10% by weight of the excavated clayey soil, and even more preferably between 4 and 10% by weight of the excavated clayey soil.

[0198] The activator is present, for example, in a content of at least 5% by weight of the construction material, preferably at least 7% by weight of the construction material, more preferably at least 8% by weight of the construction material, which is advantageous when the construction material is in-situ concrete.

[0199] The activator may be present in a content of at least 10% by weight of the construction material, preferably at least 15% by weight of the construction material, more preferably at least 20% by weight of the construction material, even more preferably at least 25% by weight of the construction binder, and for example at least 30% by weight of the construction binder.

[0200] Furthermore, the activator may comprise up to 50% by weight of the construction material, preferably up to 45% by weight of the construction material, and more preferably up to 40% by weight of the construction material, which is advantageous when the construction material is a construction binder.

[0201] The activator may also comprise up to 15% by weight of the construction material, preferably up to 12% by weight of the construction material, and more preferably up to 10% by weight of the construction material, which is advantageous when the construction material is in-situ concrete.

[0202] In particular, the activator may represent between 3 and 12% by weight of the construction material, preferably between 4 and 10% by weight of the construction material, more preferably between 5 and 10% by weight of the construction material, which is advantageous when the construction material is in-situ concrete.

[0203] In particular, the activator may represent between 10 and 80% by weight of the construction material, preferably between 15 and 80% by weight of the construction material, more preferably between 20 and 80% by weight of the construction material, even more preferably between 30 and 80% by weight of the construction material, and for example between 40 and 60% by weight of the construction material, which is advantageous when the construction material is a construction binder.

[0204] In one particular embodiment, the construction material according to the invention, preferably the construction binder, comprises: - 30% to 80% by weight of excavated clay soil; - 1% to 10% by weight of a deflocculating agent; -10% to 50% by weight of activator; Equipped with.

[0205] Preferably, the construction material according to the invention, preferably the construction binder, comprises: - 50% to 75% by weight of excavated clay soil; - 1% to 10% by weight of a deflocculating agent; -15% to 50% by weight of activator; Equipped with.

[0206] More preferably, the construction material according to the invention, preferably the construction binder, comprises: - 50% to 70% by weight of excavated clay soil; - 2% to 5% by weight of a deflocculating agent; -15% to 45% by weight of activator; Equipped with.

[0207] More preferably, the construction material according to the invention, preferably the construction binder, comprises: - 50% to 60% by weight of excavated clay soil; - 2% to 5% by weight of a deflocculating agent; -25% to 45% by weight of metal oxides; Equipped with.

[0208] Even more preferably, the construction material according to the invention, preferably the construction binder, - 30% to 80% by weight of excavated clay soil; - 1% to 10% by weight of a deflocculating agent; - 10% to 40% by weight of a metal oxide; -2% to 15% by weight of a strong base; Equipped with.

[0209] Even more preferably, the construction material according to the invention, preferably the construction binder, - 30% to 80% by weight of excavated clay soil; - 0.1% to 10% by weight of a deflocculating agent; -15% to 50% by weight of blast furnace slag Equipped with.

[0210] Even more preferably, the construction material according to the invention, preferably the construction binder, - 30% to 80% by weight of excavated clay soil; - 0.1% to 10% by weight of a deflocculating agent; - 10% to 45% by weight of blast furnace slag; - 5% to 20% by weight of an alkaline composition such as triphosphate; Equipped with.

[0211] Preferably, the construction material according to the invention comprises: - between 5 and 45% by weight, preferably between 5 and 30% by weight, more preferably between 10 and 20% by weight of a construction binder according to the invention, - between 25 and 45% by weight, preferably between 30 and 40% by weight, of sand, for example from in situ soil, preferably from excavated clayey soil; - between 35 and 55% by weight, preferably between 40 and 50% by weight, of aggregates, for example from in situ soils, preferably from excavated clayey soils; -preferably from 2 to 10% by weight of water It is a site-concrete structure equipped with

[0212] More preferably, the construction material according to the invention comprises: - between 5 and 20% by weight of raw clay from excavated clay soil, preferably between 5 and 15% by weight of raw clay from excavated clay soil; - between 0.1 and 3 wt. % of a deflocculating agent; - between 3 and 15% by weight, preferably between 5 and 12% by weight, of an activator, for example between 5% and 10% by weight of blast furnace slag; - between 25 and 45% by weight, preferably between 30 and 40% by weight, of sand, for example from in situ soil, preferably from excavated clayey soil; - between 35 and 55% by weight, preferably between 40 and 50% by weight, of aggregates, for example from in situ soils, preferably from excavated clayey soils; -preferably between 2 and 10% by weight of water It is a site-concrete structure equipped with

[0213] The sand and aggregates may be obtained from a quarry, and the binder may further include quarry clay to supplement the clay from the excavated clay soil.

[0214] Additionally, the in-situ concrete may include admixtures such as flow enhancers, superplasticizers, rheology retention agents, or air entraining agents.

[0215] Furthermore, the water to dry matter weight ratio of the construction binder is advantageously controlled, preferably less than 1, and more preferably substantially equal to 0.6.

[0216] Furthermore, according to another aspect, the present invention relates to a construction material formed from the construction binder according to the present invention.

[0217] Furthermore, the present invention relates to a construction material obtainable from the preparation process according to the invention.The present invention relates to a construction material obtainable from the preparation process according to the invention.

[0218] The invention in particular enables the production of: - Thermal insulating building materials: from construction binders according to the invention with the addition of light aggregates of the "vegetable or porous" type; - lightweight concrete: from construction binders according to the invention with the addition of a foaming agent of the aluminum powder type, which will trap air in the material and improve its insulating properties; - prefabricated elements: concrete blocks or slabs manufactured in a factory from the construction binder according to the invention; and -Separation module.

[0219] As shown by the following examples, the present invention provides a solution based on a mixture of raw clay matrix, deflocculating agent and activating composition, providing a construction material with similar mechanical properties to the standard while reducing the carbon footprint. EXAMPLES

[0220] Methodology for determining physicochemical properties of clayey soils: The clay soil is pre-screened to remove all elements or particles having a diameter of more than 20 μm. Such pre-treated clay soil is particularly suitable for forming a construction binder according to the invention.

[0221] The pH is measured using 20 g of pretreated clay soil mixed with 100 mL of distilled water. After stirring for 20 minutes at 150 rpm ("revolutions per minute" in Anglo-Saxon terminology), the suspension is filtered and the pH of the filtered solution is measured.

[0222] The clay content is conventionally measured by the particle size distribution method described in the NF X31-107 standard.

[0223] Clay properties are conventionally measured by X-ray diffraction techniques.

[0224] Generating Similarity Values As indicated above, the values ​​include a correlation between a measurement of at least one physicochemical property of the clay soil and values ​​of the amount of deflocculating agent and activator.

[0225] These reference values ​​are generated from a number of clay soil samples combined with various amounts of deflocculating agent and activating agent in the process for preparing a construction binder described below.

[0226] The generation of the reference value may be carried out by implementing an experimental design such as, for example, a simplex design, a screening design, a factorial design, a response surface design, a mixture design, a Taguchi design, or the like.

[0227] Table 1 below shows the physicochemical properties of the different excavated soil samples and Table 2 shows an example of an experimental design to generate the reference values.

[0228] [Table 1]

[0229] [Table 2]

[0230] Preparation of construction binder: The construction binders, especially when generating reference values, are prepared according to the same protocol: a premix of a given amount between clayey soil and deflocculant is made, for example according to an experimental design, then water is added and the suspension is mixed at low speed, i.e. substantially at 600 revolutions per minute, for 30 seconds, then an activator is added to the premix, then the premix is ​​mixed at high speed, i.e. approximately at 1500 revolutions per minute, for 3 minutes.

[0231] The water to dry matter weight ratio of the composition (also called construction binder) is adjusted to a value less than 1 and more preferably substantially equal to 0.6.

[0232] The construction binder thus formed is then poured into a mould and left to harden for 28 days at room temperature, i.e. around 20 degrees Celsius.

[0233] Next, the mechanical properties of the construction binder are evaluated.

[0234] Methodology for measuring mechanical properties of construction binders: After hardening is complete, the construction binder is removed from the form and its mechanical strength is measured. By mechanical strength of a construction binder is meant its compressive strength, such compression is measured according to the NF EN 196-1 standard.

[0235] The results of the measurements performed in the experiments described in Table 2 are shown in Table 3 below.

[0236] [Table 3]

[0237] These results show that the performance of the binder formed, especially its mechanical strength, differs depending on the amount of activator and deflocculator used.

[0238] Furthermore, they show that the presence of a deflocculating agent makes it possible to obtain mechanical strengths of more than 30 MPa.

[0239] Selection of the composition of the construction binder: After providing the reference values ​​and, if necessary, the calculation algorithm, the method for selecting appropriate amounts of deflocculator and activator for a given excavated clayey soil can be implemented.

[0240] First, an excavated clay soil sample is sieved to remove all elements or particles greater than 20 μm in diameter.

[0241] The physicochemical properties of the pretreated excavated clayey soil samples are then analyzed as described above.

[0242] The obtained values ​​are then transmitted to a computing device configured to implement the method according to the invention.

[0243] The latter then generates values ​​for the amounts of deflocculant and activator that will form a construction binder when combined with a given amount of excavated soil.

[0244] Formation of the construction binder according to the invention The excavated clay soil is then sieved to remove any elements or particles greater than 2 cm in diameter, and a predetermined amount of the pretreated excavated clay soil is then mixed simultaneously or sequentially with the selected deflocculating agent and activation amount values.

[0245] The construction binder or in-situ concrete formed according to the invention has a compressive strength comparable to that obtained with concrete formed with Portland cement.The invention therefore makes it possible to select a suitable composition, which makes it possible to form, from excavated clay soils, a low-carbon construction binder with sufficient mechanical properties to make it a construction material that meets the majority of the sector's needs.

Claims

1. 1. A method (100) for selecting a composition of a construction material comprising excavated clay soil, the composition of the construction material comprising an amount of deflocculating agent and an activating agent adapted to the excavated clay soil, the method being implemented by a computer device including a calculation module, - receiving (130) from said calculation module measurements of at least one physico-chemical property of the excavated clayey soil; - selecting (170) by the calculation module an amount of deflocculating agent and an amount of activating agent applied to the excavated clayey soil based on a comparison of the one or more measurements with a reference value, the reference value comprising a correlation between the measurement of at least one physicochemical property of the clayey soil and the amount of deflocculating agent and activating agent applied to the clayey soil to form a construction material; A method comprising:

2. The at least one physicochemical property is selected from the clay content in the excavated clayey soil, the nature of the clay, the particle size, the impurity content, the non-clay mineral fraction content, the contaminant content, the elemental analysis, the metal oxide content, the salinity, the pH and the total exchange capacity of the clay in the excavated clayey soil. The method of claim 1.

3. The at least one physicochemical property is measured on a pretreated excavated clayey soil, the pretreatment being selected from crushing, sorting, sieving and / or drying the excavated clayey soil. The method according to claim 1 or 2.

4. Firstly, a desired mechanical property value of the construction material is received (140), The step of selecting (170) the amount of deflocculating agent and activating agent further comprises eliminating (171) amounts of the deflocculating agent and activating agent that do not enable the building material to exhibit the desired mechanical property values.

4. The method according to any one of claims 1 to 3.

5. The step of selecting (170) by the calculation module an amount of deflocculating agent and an amount of activating agent adapted to the excavated clayey soil includes implementing a pre-calibrated calculation algorithm.

5. The method according to any one of claims 1 to 4.

6. The pre-calibrated computation algorithm is obtained by implementing a statistical supervised learning method. The method according to claim 5.

7. A method (200) for calibrating a computational algorithm for determining a composition of a construction material implemented by a digital device including a learning module, comprising: a first step (230) of receiving measurements of at least one physicochemical property of an excavated clayey soil from said learning module; a second step (240) of receiving from said learning module values ​​of the amount of deflocculating agent and values ​​of the amount of activating agent that can be added to said excavated clay soil to form a construction material; a third step (260) of receiving from the learning module the measurements of at least one mechanical property of the construction material formed from the excavated clayey soil, the values ​​of the at least one physicochemical property received during the first receiving step (230), and the amounts of the deflocculating agent and the activating agent received during the second receiving step (240); - creating (270) by said learning module a correlation between said received measurements in order to calibrate a calculation algorithm; A method comprising:

8. A method (300) for preparing construction material from excavated clay soil, comprising: - measuring (310) at least one physicochemical property of the excavated clayey soil; - a selection step according to a method (100) according to any one of claims 1 to 6 for selecting a composition of a construction material comprising excavated clay soil, - mixing (340) the excavated clay soil, the deflocculating agent and the activator according to the selected composition; A method comprising:

9. - measuring (350) the physicochemical or mechanical properties of the resulting construction material during the mixing step; - comparing (360) said measurements with predetermined values ​​of physicochemical or mechanical properties of the resulting construction material; - adding (370) at least one complementary component when said measured value differs from a predetermined value of a physicochemical or mechanical property of said resulting construction material; 9. The method for preparing according to claim 8, further comprising:

10. 1. A construction material formed from excavated clay soil, comprising: excavated clay soil, an activator, and a deflocculating agent, said deflocculating agent comprising at least 0.1% by weight of said construction material, preferably at least 0.25% by weight of said construction material.

11. Contains a mixture of different types of clay, 11. The construction material of claim 10.

12. said construction material containing metal oxides in a content of at least 2% by weight, said construction material preferably corresponding to a construction binder; 12. A construction material according to claim 10 or 11.

13. Including blast furnace slag A construction material according to any one of claims 10 to 12.

14. - 30% to 80% by weight of excavated clay soil; - 0.1% to 10% by weight of a deflocculating agent; - 5 to 10% by weight of blast furnace slag; Including, Preferably corresponding to a construction binder, 14. The construction material of claim 13.

15. - between 5 and 20% by weight of raw clay from the excavated clay soil; - between 0.1 and 3 wt. % of a deflocculating agent; Between 3 and 15 wt. % of an activator; Between 25 and 45% by weight of sand; - between 35 and 55% by weight of aggregate; Including, Preferably corresponding to in-situ concrete, 14. The construction material of claim 13.

16. Contains at least 2% by weight of silt particles; 16. A construction material according to any one of claims 10 to 15.

17. The excavated clayey soil is pretreated, the pretreatment being selected from crushing, screening, sieving and / or drying the excavated clayey soil; 17. A construction material according to any one of claims 10 to 16.

18. A method (300) for preparing a construction material according to any one of claims 10 to 17 from excavated clay soil, comprising the steps of: - excavating (320) clay soil; screening (330) the excavated clay soil when the excavated clay soil contains stones retained by -2 cm screening; - mixing (340) the excavated clay soil, the deflocculating agent and the activator; A method comprising:

19. 1. A system (400) for preparing construction material comprising excavated clay soil, comprising: - at least one container (410) containing excavated clay soil; - at least one container (420) containing a deflocculating agent; at least one container (430) containing an activating agent, a mixing device (450) having automated transport means between said containers (410, 420, 430) and the mixing device (450); a control module (480) configured to generate output signals used by said automated transport means to transport determined amounts of said deflocculating agent and said activating agent to said mixing device (450); A system comprising:

20. a communication means configured to receive data relating to the determined amount of deflocculating agent and the determined amount of activating agent applied to the excavated clayey soil; the control module (480) is configured to generate an output signal that is used by the automated transport means to transport the determined amount of deflocculator and activator to the mixing device (450).

20. A system (400) for preparing a construction material according to claim 19.

21. - means (460) for measuring at least one physicochemical property of said excavated clayey soil; - a calculation means (470); Equipped with The calculation means (470) - obtaining measurements of at least one physico-chemical property of the excavated clayey soil; - determining an amount of deflocculating agent and an amount of activator suitable for the excavated clayey soil based on a comparison of the one or more measurements with reference values; adapted to execute a computer program configured to perform 20. A system (400) for preparing a construction material according to claim 19.

Citation Information

Patent Citations

  • Method for building additive composition for soil cement and consolidated material for soil cement

    JP1999254425A

  • Method of preparing soil cement slurry

    JP2007217255A

  • Mixing design method and soil cement

    JP2008031769A

  • Method for preparing soil cement slurry

    JP2008037891A

  • Concrete slump measurement and control system

    EP2296854A2