Hydrophilic quantum dot, hydrophilic solvent-type quantum dot ink composition including the same, and light-emitting device and display including the same

Surface-modified quantum dots for polar solvent dispersion address viscosity and dispersibility issues, enabling efficient inkjet printing and cost-effective production of light-emitting devices and displays.

JP2024164835AActive Publication Date: 2024-11-27SAMSUNG ELECTRONICS CO LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024079418
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-05-15
Publication Date
2024-11-27
Estimated Expiration
2044-05-15

AI Technical Summary

Technical Problem

Existing quantum dot compositions face challenges in achieving low viscosity for inkjet printing, particularly with solvent-based inks, as non-polar solvents struggle with viscosity control and polar solvents have poor dispersibility, and non-polar solvent-based electron transport layers can etch light emitting layers.

Method used

Surface modification of quantum dots to enable dispersion in polar solvents, allowing for the formulation of hydrophilic quantum dot ink compositions with adjustable viscosity suitable for inkjet printing.

Benefits of technology

The modified quantum dots can be easily printed using inkjet methods, avoiding layer etching and reducing material waste, facilitating cost-effective production of light-emitting devices and displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164835000001_ABST
    Figure 2024164835000001_ABST
Patent Text Reader

Abstract

To provide a hydrophilic quantum dot, a hydrophilic solvent-type quantum dot ink composition including the same, and a light-emitting device and a display including the same.SOLUTION: The disclosure relates to hydrophilic quantum dots, a hydrophilic solvent-type quantum dot ink composition including the same, and a light-emitting device and a display that are manufactured by including the same, and more particularly, to hydrophilic quantum dots that are dispersible in a polar solvent with high viscosity, allowing for easy control of viscosity, a hydrophilic solvent-type quantum dot ink composition including the same, and a light-emitting device and a display that include the same.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to hydrophilic quantum dots, a hydrophilic solvent-based quantum dot ink composition containing the same, and a light-emitting device and a display manufactured using the same. More specifically, the present invention relates to hydrophilic quantum dots that can be dispersed in a highly viscous polar solvent and have easy-to-adjust viscosity, a hydrophilic solvent-based quantum dot ink composition containing the same, and a light-emitting device and a display including the same. [Background technology]

[0002] Quantum dots (QDs) are so-called semiconductor nanocrystals, and can produce various colors by generating light of different wavelengths according to particle size without changing the type of material. They have advantages of higher color purity and light stability than existing light-emitting bodies, so they are attracting attention as a next-generation light-emitting device.

[0003] In particular, quantum dots, which have become a new trend in the display field, are dispersed in a polymer matrix and can be applied in the form of a complex to various displays and electronic devices in addition to TVs and LEDs. Meanwhile, materials for color filters are required to have high sensitivity, adhesion to substrates, chemical resistance, heat resistance, etc. Conventionally, color filters applied to displays have generally been formed through a patterning process in which a desired pattern is formed using a photosensitive resist composition through an exposure process using a photomask, and then the non-exposed areas are dissolved and removed through a development process, but this has led to a problem of increased costs due to the waste of materials.

[0004] Recently, in order to solve the problem of increasing the quality of materials used for pixels and the associated cost increases, methods that use materials only in desired areas and minimize the use of materials have been attracting attention, rather than the conventional patterning methods such as spin coating or slit coating. The most representative method is the inkjet method, which can be broadly classified into the bubble jet method and the piezo method. The inkjet method uses materials only in desired pixels, thereby preventing unnecessary waste of materials. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Korean Patent No. 10-2340892 Summary of the Invention [Problem to be solved by the invention]

[0006] The quantum dot composition used in the inkjet method is required to have a viscosity of 100 cps or less, preferably 50 cps or less, so it is essential to achieve low viscosity. Since it is difficult to use solvent-free inks to develop ELQD ink materials for self-luminescence, the development of solvent-based inks is underway. However, there are technical limitations such as difficulty in adjusting viscosity with non-polar solvents used in solvent-based inks and reduced dispersibility with polar solvents, and related research is also insufficient.

[0007] In this regard, a prior invention (Korean Patent No. 10-2340892, published on December 17, 2021) has been published relating to a quantum dot microcapsule ink that is capable of achieving a low viscosity of 10 cps or less and is electrically charged so that it can be dispersed in resins and binders, etc.; however, further processes were required, such as performing processes such as frictional charging to make the shell region of the quantum dot capsule positively or negatively charged, or coating the capsule surface with a charge regulator, etc.

[0008] In addition, in the case of a quantum dot light-emitting layer used in a self-luminous display for inkjet printing, the solvent type is not clear and many solvent types are being researched and developed, but when a non-polar solvent-based light-emitting layer is used, there is a technical problem that the light-emitting layer is etched when a non-polar solvent-based electron transport layer ink composition having the same properties is used. Therefore, there is a demand for hydrophilic quantum dots and hydrophilic solvent-based quantum dot ink compositions that can be dispersed in polar solvents.

[0009] The problem to be solved by the present invention is to provide a hydrophilic quantum dot and a hydrophilic solvent-type quantum dot ink composition that can be easily inkjet printed by modifying the surface of the quantum dot to induce dispersion in a highly viscous polar solvent, and has an easily adjustable viscosity. Effect of the Invention

[0010] According to an embodiment of the present invention, the quantum dots can be dispersed in a polar solvent through surface modification, and have properties (such as viscosity) that are suitable for inkjet printing.

[0011] The solvent-based quantum dot ink composition can be prepared using a polar solvent, making it easy to adjust the viscosity.

[0012] In addition, when a light-emitting layer is manufactured using the hydrophilic solvent-based quantum dot ink composition according to the present invention, even if a non-polar solvent-based electron transport layer is formed on the upper end of the light-emitting layer, no etching problem occurs in the light-emitting layer.

[0013] As a result, the polar solvent-based ink composition of the present invention can be effectively applied to the preparation of light-emitting devices, specifically, self-luminous displays, through an inkjet printing process, and can also be advantageously applied to commercialization and large-scale production through the application of a simple and inexpensive inkjet process.

[0014] The effects of the present invention are not limited to the above-mentioned examples, and more diverse effects are included in the present specification. [Brief description of the drawings]

[0015] [Figure 1] 1 is a graph showing the results of Experimental Example 4 for the ink composition of Example 4. [Diagram 2] 1 is a diagram showing the results of Experimental Example 4 for the ink composition of Example 4-a. [Diagram 3] 1 is a diagram showing the results of Experimental Example 4 for the ink composition of Example 4-b. [Figure 4] 1 is a diagram showing the results of Experimental Example 5. [Diagram 5] 1 is a diagram showing the results of Experimental Example 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will now be described. All terms (including technical and scientific terms) used in this specification may be used as commonly understood by those having ordinary knowledge in the technical field to which the present invention belongs, unless otherwise defined. Furthermore, terms defined in commonly used dictionaries should not be interpreted ideally or excessively unless otherwise clearly defined.

[0017] Furthermore, throughout this specification, when a part "comprises" a certain component, this does not mean to exclude other components, but means that it may further include other components, unless specifically stated to the contrary.

[0018] In this specification, the term "organic group" refers to a C1-C10 linear or branched alkyl group, a C2-C10 linear or branched alkenyl group, or a C2-C10 linear or branched alkynyl group, each of which may be substituted or unsubstituted.

[0019] As used herein, "alkyl" refers to a monovalent substituent derived from a straight or branched chain saturated hydrocarbon having 1 to 10 carbon atoms. Examples include, but are not limited to, methyl, ethyl, propyl, isobutyl, sec-butyl, pentyl, iso-amyl, or hexyl.

[0020] As used herein, "alkenyl" refers to a monovalent substituent derived from a straight or branched unsaturated hydrocarbon having 2 to 10 carbon atoms and one or more carbon-carbon double bonds. Examples include, but are not limited to, vinyl, allyl, isopropenyl, or 2-butenyl.

[0021] As used herein, "alkynyl" refers to a monovalent substituent derived from a straight or branched unsaturated hydrocarbon having 2 to 10 carbon atoms and one or more carbon-carbon triple bonds. Examples include, but are not limited to, ethynyl, n-propynyl, n-but-2-enyl, or n-hex-3-enyl.

[0022] <Hydrophilic Solvent-Based Quantum Dot Ink Composition> The quantum dot ink composition according to an embodiment of the present invention is an ink composition that can form a light-emitting layer by discharging it by inkjet printing, roll-to-roll coating, screen printing, spray coating, dip coating, or spin coating.

[0023] A quantum dot ink composition according to an embodiment of the present invention includes hydrophilic quantum dots that have been surface-modified with a ligand and a polar solvent, and the hydrophilic quantum dots can be dispersed in the polar solvent.

[0024] The composition of the quantum dot composition will be specifically described below.

[0025] Quantum dots Quantum dots (QDs) are nano-sized semiconductor materials that can have different energy band gaps depending on their size and composition, and can therefore emit light of various emission wavelengths.

[0026] Such quantum dots may have a homogeneous single layer structure, a multilayer structure such as a core-shell structure, a gradient structure, or a mixture of these. In the core-shell structure, the shell may be multilayered (e.g., core / shell / shell), where each layer may contain different components, e.g., (semi)metal oxides.

[0027] The quantum dots can be freely selected from II-VI group compounds, III-V group compounds, IV-VI group compounds, group IV elements, group IV compounds, and combinations thereof. When the quantum dots have a core-shell structure, the core and shell can be freely composed of the following exemplified components.

[0028] By way of example, the II-VI compound may be a binary compound selected from the group consisting of CdO, CdS, CdSe, CdTe, ZnO, ZnS, ZnSe, ZnTe, HgS, HgSe, HgTe, MgSe, MgS and mixtures thereof; CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdH ternary compounds selected from the group consisting of CdZnSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, MgZnSe, MgZnS, and mixtures thereof; and quaternary compounds selected from the group consisting of CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe, HgZnSTe, and mixtures thereof. As another example, the III-V compound may be selected from the group consisting of binary compounds selected from the group consisting of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, and mixtures thereof; ternary compounds selected from the group consisting of GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, and mixtures thereof; and quaternary compounds selected from the group consisting of GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, InAlPSb, and mixtures thereof.

[0029] As another example, the IV-VI compound may be selected from the group consisting of binary compounds selected from the group consisting of SnS, SnSe, SnTe, PbS, PbSe, PbTe, and mixtures thereof; ternary compounds selected from the group consisting of SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, and mixtures thereof; and quaternary compounds selected from the group consisting of SnPbSSe, SnPbSeTe, SnPbSTe, and mixtures thereof.

[0030] As another example, the group IV element may be selected from the group consisting of Si, Ge, and mixtures thereof. The group IV compound may also be a binary compound selected from the group consisting of SiC, SiGe, and mixtures thereof.

[0031] As another example, the alloy type compound is a ternary compound selected from InZnP, etc.

[0032] The surface of the quantum dots may contain a divalent to tetravalent metal, for example, a metal from group 2 to group 14, such as Mg, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Cd, In, or Sn. By adding more metal to the surface of the quantum dots before surface modification, the sites to which the ligands are attached can be expanded, and thus the surface modification of the quantum dots can be effectively performed.

[0033] The two-element compound, three-element compound, or four-element compound may be present in a particle at a uniform concentration, or may be present in the same particle with a concentration distribution that is partially different. A quantum dot may also have a core / shell structure in which one quantum dot surrounds another. The interface between the core and the shell may have a concentration gradient in which the concentration of the element present in the shell decreases toward the center.

[0034] The shape of the quantum dots is not particularly limited as long as it is a shape commonly used in the art. For example, the shapes of the quantum dots may be spherical, rod-shaped, pyramidal, disk-shaped, multi-arm, or cubic nanoparticles, nanotubes, nanowires, nanofibers, nanoplate particles, and the like.

[0035] In addition, the size of the quantum dots is not particularly limited and can be appropriately adjusted within a normal range known in the art. As an example, the average particle size (D50) of the quantum dots is about 2 to 10 nm. In this way, when the particle size of the quantum dots is controlled in the range of about 2 to 10 nm, light of a desired hue can be emitted. For example, when the particle size of the quantum dot core / shell containing InP is about 5 to 6 nm, light of a wavelength of about 520 to 550 nm can be emitted, while when the particle size of the quantum dot core / shell containing InP is about 7 to 8 nm, light of a wavelength of about 620 to 640 nm can be emitted. For example, as the blue light-emitting QD, non-cadmium (Cd)-based III-V group QD (e.g., InP, InGaP, InZnP, GaN, GaAs, GaP) can be used.

[0036] In addition, the quantum dots may have a full width of half maximum (FWHM) of an emission wavelength spectrum of about 40 nm or less, and color purity and color reproducibility may be improved within this range. In addition, the light emitted through such quantum dots is emitted in all directions, and thus a wide viewing angle may be improved.

[0037] Organic ligands such as oleic acid, myristic acid, lauric acid, palmitic acid, stearic acid, oleylamine, n-octylamine, hexadecylamine, hexylphosphonic acid, n-octylphosphonic acid, tetradecylphosphonic acid, octadecylphosphonic acid, or combinations thereof may be attached to the surface of the quantum dots.

[0038] According to one embodiment of the present invention, the content of the quantum dots is 1 to 20 wt %, preferably 1 to 10 wt %, and more preferably 1 to 5 wt %, based on the total weight of the quantum dot composition, depending on the properties of the quantum dots.

[0039] The quantum dot solution may contain a metal that constitutes the surface of the quantum dots. The content of the metal to be added is 1 to 20% by weight, preferably 1 to 10% by weight, and more preferably 1 to 5% by weight, based on the total weight of the quantum dot composition. For example, when Zn metal is contained on the surface of the quantum dots, ZnCl 2 can be added.

[0040] The weight ratio of the quantum dots to the metal compound that constitutes the surface of the quantum dots and is added to the quantum dots is 3:1 to 1:3, preferably 2:1 to 1:2, and more preferably 1:1.

[0041] Ligand In the quantum dot composition according to the present invention, the ligand serves to modify the surface of the quantum dots. Quantum dots have a barrier to dispersion in hydrophilic or polar solvents due to their hydrophobic surface characteristics, but the surface of the quantum dots can be modified with an appropriate ligand to improve the miscibility of the quantum dots in hydrophilic solvents and adjust the viscosity, making it possible to use the quantum dots in inkjet printing.

[0042] According to one embodiment of the present invention, the ligand comprises a reactive group capable of binding to the surface of the quantum dot and an organic group having hydrophilic properties, preferably comprises a reactive group capable of binding to the surface of the quantum dot on one side and an organic group having hydrophilic properties on the other side, and more preferably comprises one or more reactive groups capable of binding to the surface of the quantum dot on one side and one or more organic groups having hydrophilic properties at an end.

[0043] Non-limiting examples of functional groups that can be attached to the surface of a quantum dot include -COOH, -CN, NH 2 , NH, N, SH, PO, P, OH, COOR' (where R' is an alkyl group), -C(=O)-, PO(OH) 2 , POOH, and combinations thereof.

[0044] The hydrophilic organic group contained in the ligand is an organic group having 3 to 10 carbon atoms, and preferably contains one or more elements selected from the group containing nitrogen (N), oxygen (O) and sulfur (S). Specific examples thereof include a carboxy group, a hydroxy group, a sulfo group, a sulfonyl group, an ammonium group, an amine group, ethylene glycol, and polyethylene glycol (PEG).

[0045] The hydrophilic organic group contained in the ligand is contained in the ligand as 1 to 20 independently selected moieties as a part of the ligand.

[0046] Examples of ligands include bifunctional molecules containing a carboxylic acid-containing organic group and a thiol group, such as, but not limited to, 3-mercaptopropionic acid, 6-mercaptohexanoic acid, 7-mercaptoheptanoic acid, 8-mercaptooctanoic acid, 12-mercaptododecanoic acid, mercaptosuccinic acid, or dimercaptosuccinic acid.

[0047] According to one embodiment of the present invention, the content of the ligand is 1 to 40 wt %, preferably 1 to 20 wt %, and more preferably 1 to 10 wt %, based on the total weight of the quantum dot composition, depending on the properties of the quantum dots.

[0048] Furthermore, the weight ratio of the quantum dots to the ligand is 1:1 to 1:5, preferably 1:1 to 1:3, and more preferably 1:1.5 to 1:2.5.

[0049] Polar Solvents Highly viscous polar solvents have excellent properties for producing ink compositions suitable for use in inkjet printing processes, but have presented problems in uniformly dispersing quantum dots.

[0050] According to one embodiment of the present invention, the polar solvent includes two or more kinds, preferably includes propylene glycol, more preferably includes one or more solvents including one or more functional groups selected from the group including carboxyl group, hydroxyl group, sulfo group, ester group, and ketone group. At this time, the volume ratio of propylene glycol to the remaining polar solvent is 1:0.5 to 1:5, preferably 1:1 to 1:3. The optimal volume ratio may vary depending on the physical properties of the remaining polar solvent to be added.

[0051] The viscosity of the quantum dot ink composition according to the present invention is about 2 to 20 cps, preferably 2 to 16 cps, and more preferably 2.1 to 15 cps, and within this range, the quantum dot ink composition is suitable for use in an inkjet printing method.

[0052] In addition, the quantum dot ink composition according to the present invention has a roughness of 0.5 to 5 nm, preferably 1 to 3 nm, and more preferably 1 to 2 nm. The more uniform the roughness after thinning, the more uniform the thin film can be realized when applied to a light emitting device and a display device, and therefore the more uniform the color reproduction rate can be. Furthermore, leakage does not occur when the device is operated, and the driving characteristics of the device can be improved.

[0053] <Light Emitting Device and Display Device> The light emitting device according to one embodiment of the present invention is distinguished from conventional light emitting devices in that it includes a light emitting layer formed from the quantum dot ink composition described above.

[0054] The light emitting device according to an embodiment of the present invention may be, but is not limited to, a quantum dot light emitting device, an organic light emitting device, or the like, and may be applied to various types of light emitting devices.

[0055] In general, the light emitting device includes a first electrode, a second electrode facing the first electrode, a light emitting layer disposed between the first electrode and the second electrode and formed by inkjet printing the quantum dot ink composition, a hole transport layer disposed between the first electrode and the light emitting layer, and an electron transport layer disposed between the light emitting layer and the second electrode. If necessary, the light emitting device may further include at least one layer selected from the group consisting of a hole injection layer and an electron injection layer.

[0056] The present invention also provides a display device including the quantum dot ink composition, where the display device can be, but is not limited to, a liquid crystal display (LCD), an electroluminescent display (EL), a plasma display panel (PDP), a field emission display (FED), an organic light emitting device (OLED), and the like. EXAMPLES

[0057] The present invention will be described in more detail with reference to the following Preparations and Examples. However, the following Preparations and Examples are for illustrating the present invention, and the scope of the present invention is not limited to the Preparations and Examples.

[0058] <Production Example 1. Polar Solvent A> Propylene glycol (hereinafter referred to as PG), butanol and propylene glycol monomethyl acetate (hereinafter referred to as PGMEA) were mixed in a volume ratio of 1:1:1 to a total volume of 2 ml to prepare polar solvent A.

[0059] <Production Example 2. Polar Solvent B> Polar solvent B was prepared by mixing PG and butanol in a volume ratio of 1:3.

[0060] <Production Example 3. Polar Solvent C> Polar solvent C was prepared by mixing PG and PGMEA in a volume ratio of 1:1.

[0061] <Production Example 4. Polar Solvent D> Polar solvent D was prepared by mixing PG and hexanol in a volume ratio of 1:1.

[0062] <Production Example 5. Polar Solvent E> Polar solvent E was prepared by mixing PG and ethanol in a volume ratio of 1:3.

[0063] <Production Example 6. Polar Solvent F> Polar solvent F was prepared by mixing PG and butyl acetate in a volume ratio of 1:1.

[0064] <Production Example 7. Polar Solvent G> Polar solvent G was prepared by mixing PG and heptanol in a volume ratio of 1:1.

[0065] <Production Example 8. Polar Solvent H> Polar solvent H was prepared by mixing PG and acetone in a volume ratio of 1:1.

[0066] Example 1 Hydrophilic Solvent-Based Quantum Dot Ink Composition The quantum dots used were a green quantum dot solution dispersed in colloidal form in toluene, with a core of indium phosphide (InP), a shell of zinc selenide (ZnSe) and zinc sulfide (ZnS), and a ligand of oleic acid, about 0.025 g of which was used.

[0067] The green quantum dots solution dispersed in toluene was mixed with ZnCl 2 After adding about 0.025 g of (5 wt % in ethanol), the mixture was stirred for about 10 minutes. After stirring, ethanol was poured in and the mixture was centrifuged.

[0068] After centrifugation, the mixture was redispersed in toluene, and about 0.05 g of mercaptosuccinic acid was added as a surface-modifying ligand, followed by stirring for 10 minutes. Finally, hexane was poured in, followed by centrifugation to obtain only the surface-modified quantum dots, which were then dispersed in the polar solvent A.

[0069] <Example 2> The preparation was carried out in the same manner as in Example 1, except that the surface-modified quantum dots were dispersed in polar solvent B.

[0070] <Example 3> The preparation was carried out in the same manner as in Example 1, except that the surface-modified quantum dots were dispersed in polar solvent C.

[0071] <Example 4> The preparation was carried out in the same manner as in Example 1, except that the surface-modified quantum dots were dispersed in polar solvent D.

[0072] <Example 5> The preparation was carried out in the same manner as in Example 1, except that the surface-modified quantum dots were dispersed in polar solvent E.

[0073] <Example 6> The preparation was carried out in the same manner as in Example 1, except that the surface-modified quantum dots were dispersed in polar solvent F.

[0074] <Example 7> The preparation was carried out in the same manner as in Example 1, except that the surface-modified quantum dots were dispersed in the polar solvent G.

[0075] <Example 8> The preparation was carried out in the same manner as in Example 1, except that the surface-modified quantum dots were dispersed in the polar solvent H.

[0076] <Comparative Example> A solution of green quantum dots dispersed in colloidal form in cyclohexylbenzene was used without surface modification. The core was made of indium phosphide (InP), the shell was made of zinc selenide (ZnSe) and zinc sulfide (ZnS), and the ligand was oleic acid.

[0077] <Experimental Example 1. Quantum Efficiency Evaluation> Using a QE 2100 device, the quantum efficiency (QE) was measured (excitation wavelength 450 nm) for the ink compositions prepared in Examples 1 to 8 under absorption conditions of 0.6 to 0.8. The results are shown in Table 1 below.

[0078] [Table 1]

[0079] In all the examples, the quantum efficiency was 70% or more, and Examples 3 to 8 showed extremely excellent quantum efficiencies of about 98 to 100%.

[0080] <Experimental Example 2. Viscosity Evaluation> The viscosity of the ink composition was measured using a rheometer (MARS-40). At this time, the CP (con&plate) measurement method was applied, the set temperature was 25°C, and the shear rate was Start 10 sec -1 ~End 20sec -1 I did.

[0081] In addition to Examples 1 to 8, further polar solvents were produced by varying the mixing ratio of each polar solvent, and the mixing ratios and viscosity results for each are shown in Table 2 below.

[0082] [Table 2]

[0083] The remaining solvents other than PG have a lower polarity than PG, so the viscosity tends to decrease as the specific gravity of the mixture ratio increases. The viscosities of the examples shown in Table 2 all fall within the range of 2 to 16 cps, and are considered to be suitable for use in inkjet printing.

[0084] <Experimental Example 3. Evaluation of organic matter content / TGA analysis> TGA analysis is a thermal analysis method that measures the mass change of a sample due to temperature change. The temperature at which a sudden change in weight occurs can be interpreted as the decomposition temperature of the organic matter, and the weight percentage occupied by the organic matter can be numerically confirmed based on the degree of total weight loss.

[0085] The ink compositions prepared in Example 1 (ZC-MSA GQD) and Comparative Example (Ref GQD) were dried in a vacuum oven for at least 1 hour to form powder, and the organic content was evaluated using a TGA 550. The results are shown in Table 3 and the graph below. Measurement conditions: Mass flow 240mL / min, equilibrate 40℃, ramp 10℃ / min to 700℃ / min

[0086] [Table 3]

[0087] Referring to Table 3 and the first graph, in the quantum dots manufactured in the comparative example, only oleic acid (3rd peak) attached to the initial quantum dots was observed, and there was a weight loss of about 16% of the organic matter. From this, it can be determined that about 16.3% of the total weight of oleic acid was attached to the initial quantum dots.

[0088] In the case of Example 1, there is a weight loss of about 15% of the organic matter, and peaks (1st to 3rd peaks) are observed in three parts. The first peak is related to oleic acid that has been substituted with the ligand and separated from the quantum dots, the second peak is related to the ligand newly attached to the surface of the quantum dots, and the third peak is related to oleic acid that has not yet been substituted.

[0089] While the weight loss of the total organic matter in Example 1 and the comparative example is almost similar, the third peak values ​​are 2.767 and 14.348, respectively, which is about 5.2 times different. This shows that the ligand substitution on the surface of the quantum dots in Example 1 is very good.

[0090] Also, referring to the second graph, in Example 1, a rapid weight loss occurs at about 180°C, while in the Comparative Example, a rapid weight loss occurs at about 400°C, so it can be seen that the combustion points of the main organic materials are different from each other.

[0091] <Experimental Example 4. Roughness Evaluation> After cleaning the ITO glass, the prepared ink composition was applied to a spin coater (3500 rpm / 20 s) to form a thin film, which was then dried on a hot plate at 70° C. for about 15 minutes and the roughness value of the thin film was measured using a Zygo NewView 9000 device.

[0092] For the roughness evaluation, an ink composition containing a polar solvent shown in Table 4 below was used, and the results are shown in FIGS.

[0093] [Table 4]

[0094] 1 to 3, the roughness value of the thickest part of an arbitrary cross section of each thin film was measured and displayed. In the case of Example 4 (FIG. 1), the maximum roughness value was measured to be about 2.73 nm, in the case of Example 4-a (FIG. 2), it was measured to be about 2.02 nm, and in the case of Example 4-b (FIG. 3), it was measured to be about 1.73 nm.

[0095] This indicates that the roughness value of the ink composition can be uniformly adjusted by adjusting the mixing ratio of the polar solvent.

[0096] <Experimental Example 5. Evaluation of ejection properties> After mounting on a Fuji Film Dimatix 2.4pl (DMC-11610) head, an Omnijet 200 device was used to evaluate the ejection properties. The ink composition of Example 1 was used and ejected in the form of one drop. Time-division photography was performed according to the time it took for one drop of ink to be ejected, and the results are shown in FIG.

[0097] Referring to FIG. 4, it can be seen that a tail is formed in the ink at the beginning of ejection, but it can be seen that the ink is gradually ejected in a well-balanced spherical shape, the diameter of which is about 18.307 μm.

[0098] <Experimental Example 6. Inkjet Shape (CRF) Evaluation> As in Experimental Example 5, after mounting on a Fuji Film Dimatix 2.4pl (DMC-11610) head, the ink composition of Example 1 was ejected using an Omnijet 200 device, and pattern evaluation was performed.

[0099] In pattern evaluation, ITO glass was used as the lower substrate, and the size and height of the pattern on the substrate were measured using a Zygo New View 9000 device. In this case, the following Equation 1 was introduced to quantify the degree of the coffee-ring effect, and the results are shown in Figure 5. [Formula 1] CRF (Coffee Ring Factor)=Hmax / Hmin In the above formula, Hmax indicates the maximum thickness of the pattern, Hmin indicates the minimum thickness of the pattern, and the CRF value indicates the degree of the coffee ring effect, i.e., CRF=1 indicates that the coffee ring effect is completely removed.

[0100] 5, the Hmax of the inkjet shape of Example 1 was about 41.62 nm, and the Hmin was about 39.78 nm. Therefore, the CRF was about 1.047, which is very close to 1, and it was determined that the coffee ring effect had almost no effect. Also, when looking at the three-dimensional shape, it was confirmed that the shape was uniform overall, not just one cross section.

[0101] It will be obvious to those having ordinary skill in the art to which the present invention pertains that the present invention is not limited to the above-described embodiments and can be modified or altered in various ways without departing from the technical scope of the present invention.

Claims

1. 1. A surface-modified quantum dot, comprising: A hydrophilic quantum dot, the surface of which is modified with a ligand comprising a reactive group capable of binding to the surface of the quantum dot and an organic group having hydrophilicity.

2. The hydrophilic quantum dot of claim 1 , wherein the quantum dot can be used for inkjet printing.

3. The reactive groups are COOH, CN, NH 2 , NH, N, SH, PO, P, OH, COOR', -C(=O)-, PO(OH) 2 2. The hydrophilic quantum dot of claim 1, wherein the hydrophilic quantum dot is selected from the group consisting of POOH, POOH, and combinations thereof.

4. The hydrophilic quantum dot according to claim 1 , wherein the organic group is an organic group having 3 to 10 carbon atoms.

5. The hydrophilic quantum dot of claim 4 , wherein the organic group comprises one or more elements selected from the group consisting of nitrogen (N), oxygen (O) and sulfur (S).

6. The hydrophilic quantum dot of claim 1 , wherein the ligand is mercaptosuccinic acid.

7. 2. The hydrophilic quantum dot of claim 1, wherein the surface of the quantum dot comprises Mg, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Cd, In or Sn.

8. A quantum dot having a surface modified with a ligand; a polar solvent, The quantum dot ink composition includes two or more polar solvents.

9. The quantum dot ink composition of claim 8 , wherein the polar solvent comprises propylene glycol.

10. The quantum dot ink composition of claim 9 , wherein the polar solvent further comprises one or more functional groups selected from the group consisting of a carboxy group, a hydroxy group, a sulfo group, an ester group, and a ketone group.

11. The quantum dot ink composition according to claim 9, wherein in the polar solvent, the total volume ratio of propylene glycol to other solvents is 1:0.5 to 1:

5.

12. The quantum dot ink composition according to claim 8, wherein the viscosity of the ink composition is 2 to 20 cps.

13. The quantum dot ink composition according to claim 8, wherein the roughness of the ink composition is 0.5 to 5 nm.

14. The quantum dot ink composition of claim 8 , wherein the quantum dots are dispersible in the polar solvent.

15. The quantum dot ink composition of claim 8 , wherein the ink composition is for inkjet printing.

16. 9. The quantum dot ink composition of claim 8, wherein the ink composition has a quantum efficiency (QE) of 70% or more.

17. 17. A light emitting device comprising a light emitting layer produced by the composition of any one of claims 8 to 16.

18. A display comprising the light-emitting element according to claim 17.

Citation Information

Patent Citations

  • Water-soluble luminescent quantum dots and their biomolecular conjugates

    JP2002530630A

  • Novel fluorescent probe for labelling biosample and its preparation method

    JP2005283254A

  • Production method of quantum dot dispersion and quantum dot dispersion

    JP2020055911A

  • Photoresponsive quantum dot drug delivery system

    JP2020519565A

  • Application of multifunctional ligands to improve the performance and stability of quantum dot inks

    JP2021501230A