Modified fly ash
Heat-treated fly ash with controlled sulfur and nitrogen content addresses storage solidification and odor issues, enhancing pozzolanic reaction and concrete properties.
Patent Information
- Application Number
- JP2023082132
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional modified fly ash solidifies during storage and emits an ammonia odor when used as a concrete admixture, while also lacking sufficient pozzolanic reaction activation.
The modified fly ash is produced by heat treating fly ash to achieve an ignition loss of 1.0 wt% or less, an average particle size of 2.0 μm to 70.0 μm, and controlled sulfur and nitrogen contents, which enhances pozzolanic reaction, reduces ammonia odor, and improves concrete properties.
The modified fly ash prevents solidification during storage, eliminates ammonia odor during mixing, and activates pozzolanic reactions, resulting in improved concrete strength and durability.
Smart Images

Figure 2024165718000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to modified fly ash produced using fly ash generated from coal-fired power plants (coal-fired power plants) as a raw material. [Background technology]
[0002] Various proposals have been made so far regarding technologies for obtaining modified fly ash by removing carbon (unburned carbon) contained in fly ash generated from coal-fired power plants, etc., as well as modified fly ash made from fly ash as a raw material. One example of a proposal related to the present invention is "Industrial modified fly ash and its manufacturing method" described in Patent Document 1. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2008-126117 A Summary of the Invention [Problem to be solved by the invention]
[0004] The conventional modified fly ash obtained by implementing the invention described in Patent Document 1 is excellent in that it has a low unburned carbon content. However, the conventional modified fly ash has a problem in that it solidifies when stored in a silo or the like.
[0005] Furthermore, conventional modified fly ash has the problem that it can have an ammonia odor when used as a concrete admixture.
[0006] Therefore, the problem to be solved by the present invention is to provide a modified fly ash that is less likely to solidify during storage, does not give off an ammonia odor when mixed into concrete, and can activate the pozzolanic reaction. [Means for solving the problem]
[0007] The modified fly ash according to the present invention is a modified fly ash obtained by heat-treating fly ash raw powder generated in a coal-fired power plant, and is characterized in that the ignition loss is 1.0 wt% or less, the average particle size is 2.0 μm to 70.0 μm, the sulfur (SO3) content is 1.00 wt% or less, and the total nitrogen (N2) content is 0.05 wt% or less.
[0008] With this configuration, when the modified fly ash according to the present invention is used as a concrete admixture, the ignition loss (substitute value for the unburned carbon content) is 1.0 wt% or less, so that the unit water content (kg / m 3 ), air entrainment due to AE agent adsorption is well maintained, slump loss does not increase, the compressive strength of the concrete after hardening is improved and the amount of drying shrinkage is reduced, preventing cracks. In addition, the concrete structure becomes dense as the pozzolanic reaction is activated, so the strength develops over the long term and durability is improved.
[0009] The ignition loss was measured according to JISA6201, the average particle size was the volume average particle size, and was measured using a laser particle size distribution analyzer. The chemical components were measured using an X-ray fluorescence analyzer (XRF analyzer), and the nitrogen components were determined using an elemental analyzer (CHN coder method).
[0010] The AE agent is an abbreviation for "Air Entraining Agent", and is one of the admixtures that improves the efficiency of concrete pouring work and frost resistance, and is a type of surfactant. By mixing it into concrete in advance, it is possible to generate tiny air particles in the concrete, which increases the fluidity of the concrete, improving its ability to be filled into the formwork and reducing pouring defects.
[0011] In addition, because the average particle size is 2.0 μm to 70 μm, the fluidity of the concrete is good and the unit water content can be reduced, thereby reducing the drying shrinkage distortion and cracking of the concrete, and the structure is densified by the pozzolanic reaction, improving durability.
[0012] The sulfur content is preferably 1.00 wt% or less, and more preferably 0.01 wt% to 0.60 wt%. By keeping the sulfur content within this range, the solidification phenomenon during storage of the fly ash can be suppressed. Furthermore, if the sulfur content is too high, it can cause delay in the initial setting time of concrete or mortar, reduction in strength, expansion, etc., so by keeping the sulfur content within the above-mentioned range, it is possible to prevent such problems from occurring.
[0013] Furthermore, the nitrogen content is 0.05 wt% or less, and particularly preferably 0.01 wt% to 0.04 wt%. If the nitrogen content is within such a range, the odor of ammonia will not be felt during mixing of concrete.
[0014] Ammonia is generally used as a denitrification measure, and in that case, excess ammonia adheres to the fly ash particles (known as the ammonia slip phenomenon). It has been pointed out that if the amount of ammonia becomes too large, it can cause delays in the setting time of concrete or mortar, reduce the strength, and even have a negative effect on durability. However, since ammonia is desorbed at temperatures between 300℃ and 450℃, most of the ammonia can be removed by heat treatment.
[0015] In the modified fly ash, it is desirable that the content of the main component (SiO2+Al2O3) is 70.0wt% to 95.0wt%, and the vitrification rate relating to the pozzolanic reaction is 50.0wt% to 90.0wt%.
[0016] With this configuration, when the modified fly ash is used as a concrete admixture, the loss on ignition is reduced and the components that contribute to the vitrification rate, which contributes to the pozzolanic reaction, are increased accordingly, so that the pozzolanic reaction is more active than with conventional heat-modified fly ash, and the glass phase in the modified fly ash reacts with calcium hydroxide, a by-product of the hydration of cement, and the product produced by this reaction, which is similar to cement hydrate, densifies the hardened body structure, which is effective in long-term strength development.
[0017] The vitrification rate was calculated by quantifying the chemical components of the fly ash using fluorescent X-ray analysis, quantifying the crystalline components of quartz, mullite, and magnetite using powder X-ray analysis-Rietveld analysis, and subtracting these from the total.
[0018] In the modified fly ash, the basicity ((CaO+MgO+Al2O3) / SiO2) is desirably 0.2 to 0.8.
[0019] In the modified fly ash, the value of the network ratio Nr=(CaO+MgO+K2O+Na2O) / (SiO2+Al2O3) is preferably 0.02 to 0.15.
[0020] In the modified fly ash, the value of the glass stability ratio GSR=SiO2 / (Na2O+K2O+CaO+MgO+Al2O3) is desirably 1.0 to 4.0.
[0021] The modified fly ash may have an average particle size of 2 μm to 10 μm.
[0022] With this configuration, the modified fly ash becomes suitable as an admixture for high-fluidity concrete, a water-stopping material, a crack injection material, and a substitute for silica fume.
[0023] The modified fly ash may have an average particle size of 10 μm to 40 μm.
[0024] With this configuration, the modified fly ash becomes suitable as a concrete admixture, a mortar admixture, a sprayed concrete admixture, a crack repair material, and a cross-section repair material.
[0025] The modified fly ash may have an average particle size of 40 μm to 70 μm.
[0026] With this configuration, the modified fly ash becomes suitable as a substitute for fine aggregate for concrete and as a sprayable concrete admixture. Effect of the Invention
[0027] The present invention makes it possible to provide a modified fly ash that is resistant to solidification during storage, and when used as a concrete admixture, does not give off an ammonia odor during mixing of concrete, and can activate the pozzolanic reaction. [Brief description of the drawings]
[0028] [Figure 1] 1 is a diagram showing the composition of modified fly ash according to an embodiment of the present invention. [Diagram 2] 1 is a schematic diagram showing a modified fly ash manufacturing facility according to an embodiment of the present invention. FIG. [Diagram 3] FIG. 3 is a schematic diagram showing a calcination device constituting the modified fly ash production facility shown in FIG. 2. [Figure 4] FIG. 4 is a cross-sectional view taken along line AA in FIG. [Diagram 5] FIG. 4 is a cross-sectional view taken along line BB in FIG. [Figure 6] FIG. 4 is a partial cross-sectional view showing a dam plate constituting the baking apparatus shown in FIG. [Figure 7] 4 is a partial cross-sectional view showing a stirring member constituting the baking apparatus shown in FIG. 3. [Figure 8] FIG. 8 is a partially enlarged view of FIG. [Figure 9] 3 is a vertical cross-sectional view of a pulverizing and classifying device that constitutes the modified fly ash production facility shown in FIG. 2. [Figure 10] FIG. 10 is a plan view of the crushing and classifying device shown in FIG. 9, with a portion thereof omitted. [Figure 11] FIG. 10 is a partially enlarged view of the vicinity of the crushing blades of the crushing and classifying device shown in FIG. [Figure 12] 3 is a partially cutaway front view of a classifier constituting the modified fly ash production facility shown in FIG. 2. [Figure 13] FIG. 13 is a partially enlarged view of the classification device shown in FIG. [Figure 14] 13 is a cross-sectional view taken along line CC in FIG. 12. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] Hereinafter, modified fly ash and a modified fly ash production facility according to an embodiment of the present invention will be described with reference to Figures 1 to 14. In addition, when the expression "to" is used in this specification, it is used as an expression including the numerical values before and after it.
[0030] Fig. 1 shows the compositions of modified fly ash FA2, FC1, FC2, and FC3 according to this embodiment. As shown in Figs. 2 and 3, modified fly ash FA2, FC1, FC2, and FC3 are produced using modified fly ash production equipment 90, using fly ash raw powder FA1 containing unburned carbon generated by coal combustion as a raw material.
[0031] As shown in Figure 1(a), the ignition loss (alternative value for unburned carbon content) of modified fly ash FA2 is 1.0% or less (0.53wt%), the sulfur (SO3) content is 0.01wt%-0.60wt%, the total nitrogen (N2) content is 0.01wt%-0.03wt%, the main component (SiO2+Al2O3) content is 70.0wt%-95.0wt%, the vitrification rate is 50.0wt%-90.0wt%, and the average particle size is 2.0μm-70.0μm. The average particle size (μm) was measured using a particle size distribution measuring device "Microtrac MT3000" manufactured by Microtrac Corporation (currently Microtrac Bell Corporation).
[0032] In order to compare the properties, effects, and the like of the modified fly ash according to this embodiment with those of a conventional fly ash, an experiment was carried out as described below. The contents and results of the experiment will now be described.
[0033] First, in order to compare the difference in the caking phenomenon during fly ash storage, the modified fly ash of this embodiment and the conventional fly ash were each placed in a container and stored under the same temperature and humidity, and then the presence or absence of the caking phenomenon was confirmed. As a result, while the caking phenomenon occurred in the conventional fly ash, the caking phenomenon hardly occurred in the modified fly ash FA2 of this embodiment.
[0034] This is presumably due to the fact that the sulfur (SO3) content of the modified fly ash FA2 according to this embodiment is a low value of 0.01 wt% to 0.60 wt%.
[0035] Next, in order to confirm the difference when the modified fly ash of the present embodiment and the conventional fly ash are used as concrete admixtures, aggregate, an air-enhancing agent, and water were added to the modified fly ash FA2 of the present embodiment and the conventional fly ash, respectively, and the concrete was formed and compared.
[0036] First, in the kneading process after adding water, the conventional fly ash generated an ammonia odor, whereas the modified fly ash FA2 of the present embodiment did not generate an ammonia odor. This is presumably because the modified fly ash of the present embodiment has a low total nitrogen (N2) content of 0.01wt% to 0.03wt%.
[0037] In addition, since the modified fly ash FA2 of this embodiment has an ignition loss (substitute value for the unburned carbon content) of 1.0 wt% or less, the unit water content (kg / m 3) was reduced. Furthermore, in the case of the modified fly ash FA2 of this embodiment, the air entrainment due to the adsorption of the AE agent was well maintained, the slump loss did not increase, and not only the compressive strength of the concrete after solidification was improved, but also the drying shrinkage was reduced. In addition, the modified fly ash FA2, which has a low unburned carbon content, is whitish in color compared to conventional fly ash, so that when used as a concrete admixture, it is possible to obtain a beautiful concrete that has a whiter appearance than conventional ones.
[0038] In addition, in modified fly ash FA2, the content of the main components (SiO2 + Al2O3) is 70.0wt%~95.0wt%, and the vitrification rate is 50wt%~90.0wt%. Therefore, when modified fly ash is used as a concrete admixture, the pozzolanic reaction is activated and the glass phase in the modified fly ash reacts with calcium hydroxide, a by-product of cement hydration. The product produced by this reaction, which is similar to cement hydrate, densifies the hardened body structure, and is therefore effective in increasing strength.
[0039] In addition, since the average particle size of the modified fly ash FA2 of this embodiment is a small value of 2.0 μm to 70.0 μm, when the modified fly ash is used as a concrete admixture, the fluidity of the concrete is improved, the unit water content can be reduced, drying shrinkage distortion and cracks of the concrete are reduced, and the structure is densified by the pozzolanic reaction, thereby improving durability.
[0040] Next, a manufacturing facility for reformed fly ash FA2, FC1, FC2, and FC3 according to an embodiment of the present invention will be described with reference to Fig. 2 to Fig. 14. As shown in Fig. 2, the reformed fly ash manufacturing facility 90 includes a calciner 1 for burning and removing unburned carbon in the fly ash raw powder FA1, a pulverizing and classifying device 30 for pulverizing and classifying the reformed fly ash FA2 sent in after the unburned carbon has been burned and removed in the calciner 1 to form the reformed fly ash FC1, a classifying device 50 for further classifying the reformed fly ash FC1 pulverized and classified in the pulverizing and classifying device 30 to form the reformed fly ash FC2, and a bag filter 70 for filtering and collecting the gas from which the reformed fly ash FC2 classified in the classifying device 50 has been removed to form the reformed fly ash FC3. Also, a bypass path BP is provided that communicates between the pulverizing and classifying device 30 and the bag filter 70.
[0041] 2, a hot generator 80 capable of generating a plurality of types of air flows with different temperatures is disposed outside the baking apparatus 1. A plurality of air supply paths 81, 82, and 83 are provided from the hot generator 80 to the baking apparatus 1. The air supply path 81 is a path for supplying high-temperature air to a heating section region equipped with the outer shell furnace 6a and the burner 6b, the air supply path 82 is a path for supplying high-temperature air to a soaking section region equipped with the outer shell furnace 7a and the blower 7b, and the air supply path 83 is a path for supplying room-temperature air to a cooling section region equipped with the cooling water nozzle 8a and the water receiver 8b.
[0042] As shown in Fig. 3, the calcination device 1 is equipped with a rotary kiln 2, which is a cylindrical rotary furnace arranged so that the axis 2c slopes downward from the starting end 2a to the terminal end 2b. At the starting end 2a of the rotary kiln 2, as shown in Fig. 3, a screw conveyor 3, which is a means for charging the fly ash raw powder FA1, a supporting burner 4, which is a supplementary heating means, and an air blowing pipe 5, which is a path for blowing air into the rotary kiln 2, are arranged.
[0043] The air blowing pipe 5 is inserted from the starting end 2a of the rotary kiln 2 along the axis 2c to a position above the axis 2c, and an air blowing hole 5a opening toward the inner peripheral surface of the rotary kiln 2 is provided in the part near the tip of the air blowing pipe 5. The tip of the air blowing pipe 5 is closed by a partition wall 5b. A blower 16 for blowing air into the air blowing pipe 5 is disposed on the base end side of the air blowing pipe 5.
[0044] In addition, from the start end 2a to the end end 2b of the rotary kiln 2, an external heating means, a shell furnace 6a and a burner 6b, an external air cooling means, a shell furnace 7a and a blower 7b, and an external water cooling means, a cooling water nozzle 8a and a water receiver 8b, are arranged in series. At the end end 2b of the rotary kiln 2, an exhaust port 9 for discharging the reformed fly ash FA2 after the treatment and an exhaust pipe 10 as an exhaust path are arranged.
[0045] When the fly ash raw powder FA1 with an unburned carbon content of 3.90wt%-7.70wt% and an average particle size of 18.40μm-21.80μm is put into the hopper 3a of the screw conveyor 3, the fly ash raw powder FA1 is introduced into the rotary kiln 2 by the screw conveyor 3, and in the rotary kiln 2 in the area where the shell furnace 6a is arranged, the fly ash raw powder FA1 is heated by the auxiliary burner 4 and the burner 6b while air is supplied from the air blowing pipe 5. In this case, as shown in FIG. 5, the high-temperature gas flow generated from the burner 6b heats while swirling between the outer peripheral surface of the rotary kiln 2 and the shell furnace 6a, so that the fly ash raw powder FA1 in the rotary kiln 2 can be efficiently and uniformly heated.
[0046] When the temperature of the fly ash raw powder FA1 reaches 350°C, which is the spontaneous combustion temperature, through this heating process, the unburned carbon in the fly ash raw powder FA1 starts to burn at that point, and thereafter, the fly ash raw powder FA1 moves inside the rotary kiln 2 toward the area where the outer shell furnace 7a and the blower 7b are located, while maintaining and expanding the combustion of the unburned carbon by its own combustion heat. In the calciner 1, the air blowing hole 5a of the air blowing pipe 5 is provided at a position where air can be blown in when the temperature of the fly ash raw powder FA1 introduced into the rotary kiln 2 exceeds 350°C, which is the spontaneous combustion temperature of pulverized coal.
[0047] The fly ash raw powder FA1 that has reached the area where the shell furnace 7a and the blower 7b are arranged is controlled by the heat generated by the combustion of unburned carbon in the rotary kiln 2 in this area and the cooling effect of the air flow supplied from the blower 7b, and moves toward the end portion 2b in the rotary kiln 2 while maintaining a high temperature of about 600°C to 900°C (preferably about 700°C to 800°C). In this process, the combustion of unburned carbon progresses further, and most of it becomes the reformed fly ash FA2 that has been burned and removed. In addition, since the rotary kiln 2 in this process is cooled by the air flow supplied from the blower 7b, there is no risk of overheating.
[0048] In the area where the cooling water nozzles 8a and the water receivers 8b are arranged, the rotary kiln 2 is cooled by spraying cooling water from the cooling water nozzles 8a onto the outer peripheral surface of the rotary kiln 2. Therefore, the fly ash raw powder FA1 that has reached this area is cooled to about 200°C while moving toward the end of the rotary kiln 2, and then discharged from the discharge port 9 provided at the end 2b of the rotary kiln 2, and is collected via a hopper 11, and then sent to a crushing and classifying device 30, which will be described later.
[0049] The cooling water sprayed from the cooling water nozzles 8a onto the outer peripheral surface of the rotary kiln 2 flows down along the outer peripheral surface to cool the rotary kiln 2, then falls into the water receiver 8b and is collected. After being cooled to a predetermined temperature in the cooling tower 12, the cooling water is sent back to the cooling water nozzles 8a and reused as cooling water.
[0050] On the other hand, the air supplied into the rotary kiln 2 from the air inlet pipe 5 and gases generated within the rotary kiln 2 by the combustion reaction of unburned carbon move within the rotary kiln 2 from the starting end 2a to the terminal end 2b, and are discharged as exhaust gas from the exhaust pipe 10 located near the terminal end 2b, and then sent to the bag filter 22.
[0051] In this case, in order to lower the temperature of the exhaust gas discharged from the exhaust pipe 10 to below the heat resistance temperature of the filter cloth in the bag filter 22, air introduced through the air supply path AP is mixed with the exhaust gas and sent in a diluted state to the bag filter 22. The exhaust gas is then rendered harmless through a dust removal process by the bag filter 22 and released into the atmosphere. The finely powdered coal ash collected by the bag filter 22 is transported upstream via the transport path R and then fed into the hopper 3a of the calcination device 1 for calcination again, so no residue is generated.
[0052] In this way, the unburned carbon in the fly ash raw powder FA1 introduced into the rotary kiln 2 is rapidly heated to 700°C in the heating region by the auxiliary burner 4 and burner 6b, and when the temperature reaches 700°C, it begins to burn spontaneously due to the high-temperature air blown in.The combustion reaction then progresses further as the unburned carbon moves through a high-temperature holding region controlled by the interaction of the combustion heat of the unburned carbon and the cooling by the blower 7b.
[0053] That is, since the combustion of unburned carbon proceeds while the fly ash raw powder FA1 is moved along the direction of heat transfer, the unburned carbon contained in the fly ash raw powder FA1 can be removed efficiently in a comparatively short time. In addition, the modified fly ash FA2 after the unburned carbon is burned and removed in the high temperature holding area is quenched by passing through a cooling area in which a cooling water nozzle 8a is arranged, and then discharged from a discharge port 9 and sent to a pulverizing and classifying device 30.
[0054] As shown in Fig. 3, a dam plate 17 protruding in the direction of the axis 2c is provided on the inner peripheral surface of the rotary kiln 2 at the boundary between the outer hull furnaces 6a, 7a and at the boundary between the outer hull furnace 7a and the cooling water nozzle 8a. As shown in Fig. 6, the dam plate 17 is doughnut-shaped, and a plurality of through holes 17a (rat holes) that contact the inner peripheral surface 2d of the rotary kiln 2 are provided in the dam plate 17 at equal intervals along the circumferential direction.
[0055] By providing such a dam plate 17 with through holes 17a on the inner peripheral surface 2d of the rotary kiln 2, the moving speed of the fly ash raw powder FA1 moving toward the terminal end inside the rotary kiln 2 is suppressed and the residence time can be increased, which enables complete combustion of unburned carbon and downsizing of the axial direction of the rotary kiln 2. In addition, since the through holes 17a of the dam plate 17 are in contact with the inner peripheral surface 2d of the rotary kiln 2, the fly ash raw powder FA1 moving along the inner peripheral surface 2d does not remain or accumulate on the dam plate 17.
[0056] These dam plates 17 are arranged on the inner peripheral surface 2d of the rotary kiln 2 at the boundary between the outer casing furnaces 6a, 7a and the boundary between the outer casing furnace 7a and the cooling water nozzle 8a, so that it is possible to retain the fly ash raw powder FA1 until the combustion start reaction in the area where the outer casing furnace 6a is arranged and the combustion reaction in the area where the outer casing furnace 7a is arranged are completed. Therefore, even if the rotary kiln 2 has a relatively short axial length, it is possible to completely combust unburned carbon.
[0057] Furthermore, as shown in Fig. 7, a number of shelf-like stirring members 18 are arranged at equal intervals along the circumferential direction on the inner peripheral surface 2d of the rotary kiln 2 in the region where the outer shell furnace 7a is arranged. As shown in Fig. 8, these stirring members 18 have a shape similar to the seating surface of a bench, and are attached to the inner peripheral surface 2d of the rotary kiln 2 by fixing members 19 formed by bending a round bar (or a tubular material) into an U-shape.
[0058] The rotation of the rotary kiln 2 also rotates these stirring members 18, stirring the fly ash raw powder FA1 by stirring it up and dropping it, so that sufficient oxygen is supplied to the fly ash raw powder FA1. Therefore, it becomes possible to rapidly advance the combustion reaction of unburned carbon, which is controlled by the diffusion of oxygen into the fly ash raw powder FA1, and to completely combust the unburned carbon in the fly ash raw powder FA1.
[0059] As shown in Fig. 8, a gap 20 through which the fly ash raw powder FA1 can pass is provided between each stirring member 18 and the inner peripheral surface 2d of the rotary kiln 2, so that the fly ash raw powder FA1 stirred up by the stirring member 8 can pass through the gap 20 and fall. This increases the chance (number of times) that the fly ash raw powder FA1 comes into direct contact with the inner peripheral surface 2d of the rotary kiln 2, increasing the efficiency of conduction between the inner peripheral surface 2d and improving the heating efficiency and cooling efficiency. In addition, by providing the gap 20, it is possible to prevent the fly ash raw powder FA1 moving along the inner peripheral surface 2d of the rotary kiln 2 from remaining or accumulating near the boundary between the inner peripheral surface 2d and the stirring member 18.
[0060] Furthermore, the high-temperature gas generated from the outer shell furnace 6a is mixed with outside air and sent to the heat exchanger 21, and the high-temperature air HA1 heated by heat exchange with the air introduced from the atmosphere into the heat exchanger 21 is supplied to the burner 6b. Also, a part of the high-temperature air HA2 heated in the outer shell furnace 7a is supplied from the blower 16 to the rotary kiln 2 via the air blowing pipe 5. In this way, air at a higher temperature than the outside air can be supplied to the air blowing pipe 5 and the burner 6b, thereby reducing the consumption of heating energy.
[0061] In this way, in the firing apparatus 1, an air blowing pipe 5 having an air blowing hole 5a is provided as an air blowing path into the rotary kiln 2, which is inserted from the starting end 2a of the rotary kiln 2 in the direction of its axis 2c and is located in the rotary kiln 2 in the area where the burner 6b and shell furnace 6a, which are external heating means, are located.
[0062] Therefore, air can be supplied from the air outlet 5a at the point when the fly ash raw powder FA1 introduced into the area where the burner 6b and the like are arranged reaches the spontaneous combustion start temperature of 700°C. Therefore, all of the heat from the auxiliary burner 4 and the burner 6b is used to raise the temperature of the fly ash raw powder FA1, which allows for a rapid temperature rise, and the subsequent process of burning unburned carbon can be performed for a long time, allowing the unburned carbon to be burned efficiently. In addition, since there is no need to heat the raw fly ash FA1 from the outside after the unburned carbon starts to burn, less energy is consumed.
[0063] The heating method of this process is a parallel flow in which the heating gas and the fly ash raw powder FA1 flow in parallel, and the temperature of the fly ash raw powder FA1 containing unburned carbon that progresses through the rotary kiln 2 increases, while the temperature of the heating gas gradually decreases. Since the temperature of the fly ash raw powder FA1 is the lowest at the start end 2a of the rotary kiln 2 where the heating gas temperature is the highest, the temperature of the rotary kiln 2 body is approximately the average value (about 600°C to 900°C) of the heating gas temperature and the temperature of the fly ash raw powder FA1, and does not become high. For this reason, it is possible to use general stainless steel materials (such as SUS310S) as the constituent material of the rotary kiln 2, and it is highly practical.
[0064] Meanwhile, in the calcination apparatus 1, an exhaust pipe 10 is provided as an exhaust path, which is inserted from the end 2b of the rotary kiln 2 along the axis 2c and opens into the rotary kiln 2 near the beginning of the area where the cooling water nozzles 8a and the like are arranged. This prevents the cooling effect of the cooling water sprayed from the cooling water nozzles 8a from reaching the exhaust gas, and the exhaust gas can pass through the exhaust pipe 10 and be discharged at a high temperature. This improves the combustion efficiency of the CO remaining in the exhaust gas, and also removes the fine powder of unburned carbon entrained in the exhaust gas by burning it.
[0065] Next, the pulverizing and classifying device 30 constituting the modified fly ash production facility 90 shown in FIG. 2 will be described with reference to FIGS.
[0066] As shown in Figures 9 and 10, the crushing and classifying device 30 includes a cylindrical portion 32 whose axis is held vertically, a conical portion 33 coaxially connected to the lower end of the cylindrical portion 32, an inlet path 34 connected tangentially to the upper peripheral wall of the cylindrical portion 32, an outlet path 35 connected near the upper end of the cylindrical portion 32, a collection box 45 connected to the lower end of the conical portion 33, a shelf-like portion 39 protruding from the inner peripheral surface 33a of the conical portion 33 in the axial direction, a rotating crushing blade 36 arranged adjacent to the upper surface of the shelf-like portion 39, a drive motor M for rotating the crushing blade 36 along the shelf-like portion 39, and a gas supply path 38 for supplying gas into the collection box 45.
[0067] A gas introduction pipe 23 incorporating a heater 49 and the introduction pipe 24 are connected upstream of the inflow path 34, and a hopper 25 for receiving the reformed fly ash FA2 sent from the calcination device 1 and an air ejection nozzle 26 for dispersing the introduced reformed fly ash FA2 are disposed upstream of the introduction path 24. The reformed fly ash FA2 discharged from the hopper 11 (see Figs. 2 and 3) of the calcination device 1 and introduced into the hopper 25 is dispersed by high-pressure air ejected from the air ejection nozzle 26, merges with the high-temperature gas flowing in from the gas introduction pipe 23, and flows into the cylindrical portion 32 via the inflow path 34.
[0068] The flat grinding blade 36 is attached near the upper end of a rotating shaft 37 disposed at the axis of the conical section 33, and the rotating shaft 37 is held in a vertical position by a bearing 40a and a holding member 41 disposed near the upper end of the rotating shaft 37, and a bearing 40b disposed at the lower end of the rotating shaft 37. The rotating shaft 37 is rotated by a driving motor M via a belt 44.
[0069] The holding members 41 are stretched radially around the rotating shaft 37 and are engaged with a holding stand 43 disposed externally through locking members 42 provided on the peripheral wall of the conical portion 33. The locking members 42 have a vibration-proof function that prevents the vibrations of the rotating grinding blades 36 from being transmitted to the conical portion 33 and the like, and a sealing function that prevents gas from inside the conical portion 33 from leaking to the outside.
[0070] In order to change the rotation direction and rotation speed of the grinding blades 36, a control device 27 having a rotation direction changing function and a rotation speed changing function is provided on the power supply wiring to the drive motor M, and a flow rate adjustment valve 28 for changing the amount of gas supplied into the collection box 45 is provided midway along the gas supply path 38. The gas supplied from the gas supply path 38 flows upward from the lower end of the conical section 33 via the collection box 45. The collection box 45, which is connected to the lower end of the conical section 33, is generally funnel-shaped with a diameter that gradually decreases downward, and a gate valve 47 and a rotary valve 48 are disposed at an outlet provided at its lower end.
[0071] As shown in Figures 10 and 11, the crushing blade 36, which is the crushing means, has a flat plate shape that rotates around a rotating shaft 37 disposed at the axis of the conical portion 33, and a standing portion 36a that faces the inner peripheral surface 33a of the conical portion 33 is provided at the tip of the crushing blade 36. A donut-shaped wear-resistant plate 46 is attached to the shelf-like portion 39, and a wear-resistant plate 29 is also attached to the inner peripheral surface 33a of the conical portion 33 that faces the standing portion 36a. Both the wear-resistant plates 46, 29 are detachable and can be replaced as necessary.
[0072] In the crushing and classifying device 30 with the crushing blades 36 rotated by the drive motor M, when gas containing the reformed fly ash FA2 from which unburned carbon has been burned off in the firing device 1 shown in Figure 2 is caused to flow into the cylindrical section 32 from the inflow path 34, a swirling flow revolving around the axis is generated within the cylindrical section 32, and the reformed fly ash FA2 contained in the gas moves toward the inner surface 32a of the cylindrical section 32 due to the action of the centrifugal force generated by the swirling flow, and after coming into contact with the inner surface 32a, it descends while drawing a spiral flow along the inner surface 32a of the cylindrical section 32 and the inner surface 33a of the conical section 33.
[0073] Then, as shown in FIG. 11, when the modified fly ash FA2 that has fallen along the inner surface 33a of the conical portion 33 reaches the wear-resistant plate material 29, 46 attached near the shelf-like portion 39, it is impact-crushed mainly by the hammering action of the crushing blades 36 having the upright portions 36a that rotate at high speed, and is then finely crushed by the impact action and friction action based on the inertial force of the modified fly ash FA2 particles themselves, and then falls from the inner edge of the wear-resistant plate material 46.
[0074] The modified fly ash FC1 that falls from the inner edge of the wear-resistant plate material 46 descends along the inner surface 33a of the conical section 33, again drawing a spiral flow together with the swirling flow, but since the gas flow reverses and rises within the recovery box 45, the modified fly ash FC1 separated from the gas flow is recovered in the recovery box 45, and the gas after the modified fly ash FC1 has been removed is discharged from the outflow path 35.
[0075] Meanwhile, the reformed fly ash FC1 collected in the collection box 45 is discharged through the gate valve 47 and the rotary valve 48 and collected in a specified container as reformed fly ash FC1. As shown in Fig. 1(b), the reformed fly ash FC1 has an average particle size of 40.0 μm to 70.0 μm, and other items are equivalent to the reformed fly ash FA2 shown in Fig. 1(a), and meets the requirements for Class IV fly ash specified in the JIS standard.
[0076] In this way, the swirl flow generated in the cylindrical portion 32, the conical portion 33, and the collection box 45 constituting the pulverizing and classifying device 30 exerts a cyclone function, and the classification function of the modified fly ash FA2, which is the material to be pulverized, can also be obtained. In this embodiment, as shown in FIG. 11, the inner diameter d of the doughnut-shaped wear-resistant plate material 46 is set to be smaller than the inner diameter D of the shelf-like portion 39, and it is preferable that d / D is 100% to 70%. Note that, when the inner diameter d is made small, the retention area of the modified fly ash FA2 on the wear-resistant plate material 46 increases, so that the pulverization action tends to increase, but when the inner diameter d is too small, the downward swirl flow is suppressed, the classification point increases, and the classification performance tends to deteriorate.
[0077] In the crushing and classifying device 30, it is possible to change the rotation direction and rotation speed of the crushing blades 36 by operating the control device 27 to change the rotation direction and rotation speed of the drive motor M, thereby adjusting the crushing action and classification point.
[0078] For example, if the pulverizing blade 36 is rotated (reverse rotation) in the opposite direction to the swirling flow generated in the cylindrical portion 32 and the conical portion 33, the relative speed between the modified fly ash FA2 and the pulverizing blade 36 increases, and the pulverizing action increases, but the swirling force of the gas is suppressed, so the classification point increases. Also, if the pulverizing blade 36 is rotated (normal rotation) in the same direction as the swirling flow, the relative speed between the modified fly ash FA2 and the pulverizing blade 36 decreases, and the pulverizing action decreases, but the swirling force of the gas is not suppressed, so the classification point decreases.
[0079] In this way, when the crushing action is increased or decreased by rotating the crushing blade 36 in the forward or reverse direction, the classification point also increases or decreases, but the classification point can be adjusted by increasing or decreasing the amount of gas supplied into the collection box 45. That is, when the crushing blade 36 is rotated in the reverse direction, the crushing action increases, the swirl force decreases, and the classification point increases, but the classification point can be lowered by decreasing the amount of gas supplied into the collection box 45. Also, when the crushing blade 36 is rotated in the forward direction, the crushing action decreases, the swirl force increases, and the classification point decreases, but the classification point can be raised by increasing the amount of gas supplied into the collection box 45.
[0080] As described above, by operating the control device 27 to change the rotation direction of the drive motor M and the pulverizing blades 36, it is possible to set the working conditions (strength of the pulverizing action, size of the classification point) according to the type and properties of the modified fly ash FA2 to be pulverized. In addition, by changing the rotation speed of the drive motor M to change the rotation speed of the pulverizing blades 36, it is possible to increase or decrease the effect on the pulverizing action and the swirling force, so that it is possible to set even more detailed conditions.
[0081] Next, the classifier 50 constituting the modified fly ash production facility 90 shown in FIG. 2 will be described with reference to FIGS.
[0082] 2 and 12, the classifier 50 includes a cylindrical section 52 whose axis is held vertically, a conical section 53 coaxially connected to the lower end of the cylindrical section 52, an inflow path 57 connected to the tangential direction of the peripheral wall of the cylindrical section 52, an outflow path 58 connected to the upper end of the cylindrical section 52, and a collection box 54 connected to the lower end 61 of the conical section 53. As shown in FIG. 12, the inner peripheral surface 53a of the conical section 53 is provided with a plurality of vanes 59 for controlling swirling flow protruding in the axial direction, and a support shaft 64 whose tip is fixed to the vane 59 and which rotatably passes through the peripheral wall and bearing 63 of the conical section 53, and an operation handle 60 fixed to the base end of the support shaft 64 are provided as gradient changing means for these vanes 59.
[0083] As shown in Figures 13 and 14, each vane 59 has a flat plate shape, and the gradient (tilt angle) of each vane 59 can be changed by rotating an operating handle 60 exposed to the outside around a support shaft 64. As shown in Figure 12, a plurality of gas introduction paths 56 are connected to the upper surface of the recovery box 54, and flow rate adjustment valves 56a are provided for each of them to change the amount of gas introduced into the recovery box 54 via these gas introduction paths 56. In addition, a plurality of flap valves 55a, 55b are arranged in sequence below the recovery box 54.
[0084] In the reformed fly ash production equipment 90 shown in Fig. 2, the gas from which the reformed fly ash FC1 discharged together with the gas from the outflow path 35 of the pulverizing and classifying device 30 has been removed flows into the cylindrical section 52 via the inflow path 57 of the classifying device 50, and a swirling flow around the axis is generated in the cylindrical section 52. The gas from which the reformed fly ash FC1 has been removed diffuses and moves toward the inner peripheral surface 52a of the cylindrical section 52 due to the action of the centrifugal force generated by this swirling flow, and comes into contact with the inner peripheral surface 52a, and then, together with the swirling flow, descends while drawing a downward spiral flow along the inner peripheral surface 52a. Then, the reformed fly ash FC2 separated from the swirling flow that reverses and rises in the collection box 54 is collected in the collection box 54, while the gas from which the reformed fly ash FC2 has been removed is discharged from the outflow path 58.
[0085] The reformed fly ash FC2 collected in the collection box 54 is discharged by opening the flap valves 55a and 55b. As shown in Fig. 1(c), the reformed fly ash FC2 has an average particle size of 10.0 μm to 40.0 μm, and other properties are equivalent to those of the reformed fly ash FA2 shown in Fig. 1(a), and it meets the requirements for Class II fly ash specified in the JIS standard.
[0086] Here, by rotating the operating handle 60 protruding outward from the peripheral wall of the conical section 53 of the classifier 50 to make the gradient of the vanes 59 steeper (closer to vertical), the vortex flow rate of the outer peripheral portion (portion close to the inner peripheral surface 53a of the conical section 53) of the swirling flow generated in the conical section 53 is suppressed, and the centrifugal force is reduced, lowering the classification point. Conversely, by rotating the operating handle 60 to make the gradient of the vanes 59 gentler (closer to horizontal), the suppression of the vortex flow rate of the outer peripheral portion (portion close to the inner peripheral surface 53a of the conical section 53) of the swirling flow generated in the conical section 53 is released, increasing the centrifugal force and raising the classification point.
[0087] That is, by rotating the operating handle 60 to change the gradient of the vane 59, the vortex flow speed at the outer periphery of the swirling flow changes, and the centrifugal force changes, so that the classification point of the modified fly ash FC2 that falls along with the swirling flow while drawing a downward spiral flow along the inner circumferential surface 53a of the cone section 53 can be easily changed. In this way, the classification point can be lowered or raised by operating the operating handle 60 to change the gradient of the vane 59. Therefore, in the classification work of powder and granular material in a dry state such as modified fly ash FC2, the classification point can be changed relatively easily.
[0088] In addition, in the classification device 50, a gas introduction path 56 having a flow rate control valve 56a for changing the amount of gas supplied is provided in the collection box 54. Therefore, by operating the flow rate control valve 56a to increase or decrease the amount of gas supplied to the collection box 54, the swirling flow in the collection box 54 decreases or increases accordingly, and the classification point can be changed.
[0089] That is, if the flow rate control valve 56a is opened to increase the amount of gas supplied to the collection box 54, the swirling flow in the collection box 54 decreases and the centrifugal force also decreases, so the amount of the modified fly ash FC2 with a large particle size that falls increases and the classification point increases. Conversely, if the flow rate control valve 56a is closed to decrease the amount of gas supplied to the collection box 54, the swirling flow in the collection box 54 increases and the centrifugal force also increases, so the amount of the modified fly ash FC2 with a small particle size that falls increases and the classification point decreases.
[0090] 13, in the classifier 50, a gap 62 is provided between the inner peripheral surface 53a of the conical portion 53 and the vane 59. Therefore, the modified fly ash FC2 that falls along the inner peripheral surface 53a of the conical portion 53 together with the swirling flow can move through the gap 62 between the inner peripheral surface 53a of the conical portion 53 and the vane 59, thereby ensuring the smooth fall of the modified fly ash FC2.
[0091] 14, four vanes 59 are arranged at equal intervals along the circumferential direction of the conical section 53, so that the swirling flow can be suppressed evenly along the circumferential direction of the conical section 53 without localized turbulence of the swirling flow. This allows smooth classification point control and reduces re-scattering of the modified fly ash FC2 that falls along the inner circumferential surface 53a of the conical section 53. The number of vanes 59 is not limited to four, so an appropriate number can be set within the range of about 2 to 10.
[0092] On the other hand, the gas from which the reformed fly ash FC2 discharged together with the gas from the outflow path 58 of the classifier 50 has been removed is sent into the bag filter 70 via the inflow path 71 shown in Fig. 2. The coal ash that has flowed into the bag filter 70 is filtered and collected therein, and then discharged as the reformed fly ash FC3 from a hopper 72 provided at the lower end. As shown in Fig. 1(d), the average particle size of the reformed fly ash FC3 is 2.0 μm to 10.0 μm, and other items are equivalent to the reformed fly ash FA2 shown in Fig. 1(a), and it meets the requirements for Class I fly ash as specified in the JIS standard.
[0093] As described above, by processing the fly ash raw powder FA1 containing unburned carbon in the modified fly ash production equipment 90 shown in Fig. 2, four types of modified fly ash FA2, FC1, FC2, and FC3 can be obtained, and the unburned carbon contents of these modified fly ash FA2, FC1, FC2, and FC3 are much lower than the values stipulated for Class IV ash, Class II ash, and Class I ash in the JIS standard, respectively. That is, the modified fly ash production equipment 90 can produce modified fly ash FA2, FC1, FC2, and FC3 with an extremely low unburned carbon content and appropriately adjusted particle size according to requirements, using the fly ash raw powder FA1 as a raw material.
[0094] These modified fly ash FA2, FC1, FC2, and FC3 can be widely used as concrete admixtures, construction materials, ship fitting materials, fillers, etc. For example, when modified fly ash FA2 or FC2 is used as a cement substitute as a concrete material, the mixing amount is 60 kg / m 3 ~100kg / m 3 If the modified fly ash FA2 or FC2 is used, or the fly ash replacement rate is about 15% to 25%, it is possible to produce concrete with almost the same fluidity, air entrainment, and strength development performance as the standard concrete, even if the concrete is made using the same mix as the standard concrete that does not use the modified fly ash FA2 or FC2.
[0095] In addition, when modified fly ash FC1 is used as a substitute for fine aggregate in concrete materials, if the amount mixed is about 20% of the fine aggregate volume, it is possible to produce concrete with almost the same fluidity, air entrainment, and strength development performance as standard concrete, even if the mixture is the same as that of concrete (standard concrete) that does not use modified fly ash FC1. In addition, modified fly ash FA2, FC2, and FC3 can also be used as a substitute for fine aggregate in concrete materials.
[0096] Furthermore, since the modified fly ash FC3 has a very fine particle size and is spherical, it can be suitably used as a filler.
[0097] In addition, as shown in FIG. 2, the modified fly ash manufacturing equipment 90 is provided with a bypass route BP for allowing the modified fly ash FC1 removed from the modified fly ash FA2 flowing out from the outlet path 35 of the crushing and classifying device 30 to flow into the bag filter 70 without passing through the classifying device 50, and a switch 73 for opening and closing the flow path toward the bypass route BP.
[0098] Therefore, when the switch 73 is closed, the coal ash flows from the crushing and classifying device 30, via the classifying device 50, to the bag filter 70. However, by opening the switch 73, the coal ash flowing out from the outflow path 35 of the crushing and classifying device 30 can be made to flow directly into the bag filter 70.
[0099] Therefore, when it is desired to selectively produce any one of the modified fly ashes FC1, FC2, and FC3, for example, when it is desired to produce the modified fly ashes FC1 and FC3 but it is not necessary to produce the modified fly ash FC2 formed by the classification device 50, it is possible to concentrate and efficiently produce only the modified fly ashes FC1 and FC3.
[0100] The modified fly ash described with reference to Figures 1 to 14 is merely an example of the fly ash according to the present invention, and the modified fly ash according to the present invention is not limited to the modified fly ash described above. Furthermore, the facility for producing the modified fly ash according to the present invention is not limited to the modified fly ash production facility described with reference to Figures 2 to 14. [Industrial Applicability]
[0101] The modified fly ash according to the present invention can be widely used as a concrete admixture, a concrete repair material, a concrete filler, etc. in various industrial fields such as the civil engineering and construction industries. [Explanation of symbols]
[0102] 1. Baking equipment 2. Rotary Kiln 2a Starting end 2b Termination section 2c axis center 2d inner surface 3. Screw conveyor 3a,11 Hopper 4. Auxiliary burner 5 Air inlet tube 5a Air outlet 5b Bulkhead 6a, 7a Shell furnace 6b Burner 7b,16 Blower 8 Stirring member 8a Cooling water nozzle 8b Water tray 9 Outlet 10 Exhaust pipe 12 Cooling Tower 17 Dam Plate 17a Through hole 18 Stirring member 19 Fixing member 20 Gap 21 Heat exchanger 22 Bag filter 30 Crushing and classifying device 32 Cylindrical section 32a,33a Inner surface 33 Cone 34 Inflow route 35 Outflow route 36 Crushing blade 36a Standing part 37 Rotational Axis 38 Gas supply path 39 Shelf 40a, 40b Bearings 41 Retaining member 42 Locking member 43 Support stand 44 Belt 45 Collection Box 29,46 Wear-resistant plate material 47 Gate Valve 48 Rotary Valve 49 Heater 25 Hopper 26 Air jet nozzle 24 Introduction route 23 Gas inlet pipe 27 Control Device 28 Flow Control Valve 50 Classifier 52 Cylindrical part 52a,53a Inner surface 53 Cone 54 Collection Box 55a, 55b Flap valve 56 Gas introduction path 56a Flow control valve 57 Inflow route 58 Outflow route 59 Vane 60 Operating handle 61 Bottom end 62 Gap 63 Bearings 64 Spindle 70 Bag Filter 71 Inflow route 72 Hopper 73 Switchgear 80 Hot Generator 81, 82, 83 Air supply route 90 Fly ash production facility AP air supply route BP bypass route D, d Inner diameter FA1 Fly ash raw powder FA2, FC1, FC2, FC3 Modified fly ash HA1,HA2 Hot air M Drive motor R Transport route
Claims
1. This modified fly ash is made by heat-treating fly ash raw powder generated in coal-fired power plants. The ignition loss is 1.0 wt% or less, the average particle size is 2.0 μm to 70.0 μm, and sulfur (SO 3 ) content is 1.00 wt% or less, and the total nitrogen (N 2 ) content is 0.05 wt% or less.
2. The main component is (SiO 2 +Al 2 O 3 2. The modified fly ash according to claim 1, wherein the content of said vitrification agent is 70.0 wt % to 95.0 wt % and the vitrification rate relating to the pozzolanic reaction is 50.0 wt % to 90.0 wt %.
3. Basicity (CaO+MgO+Al 2 O 3 ) / SiO 2 The modified fly ash according to claim 1 or 2, wherein the value of (a) is 0.2 to 0.
8.
4. Network ratio Nr = (CaO + MgO + K 2 O+Na 2 O) / (SiO 2 +Al 2 O 3 The modified fly ash according to claim 1 or 2, wherein the value of (a) is 0.02 to 0.
15.
5. Glass Stability Ratio GSR = SiO 2 / (Na 2 O+K 2 O+CaO+MgO+Al 2 O 3 The modified fly ash according to claim 1 or 2, wherein the value of (a) is 1.0 to 4.
0.
6. The modified fly ash according to claim 1 or 2, having an average particle size of 2 μm to 10 μm.
7. The modified fly ash according to claim 1 or 2, having an average particle size of 10 μm to 40 μm.
8. The modified fly ash according to claim 1 or 2, having an average particle size of 40 μm to 70 μm.
Citation Information
Patent Citations
Method for removing carbon contained in fly ash
JP1994134435A
Industrial modified fly ash and its manufacturing method
JP2008126117A
Method for promptly evaluating coal ash containing cement and method for manufacturing coal ash containing cement
JP2017111087A
Modified fly ash, manufacturing method of modified fly ash and fly ash modification device
JP2018043910A
Method for manufacturing modified fly ash, and apparatus for manufacturing modified fly ash
JP2019107620A