Optical film and image display device
The optical film with a retardation layer and alignment film addresses blue shift in organic LED displays by aligning liquid crystal compounds, maintaining brightness and color consistency across viewing angles.
Patent Information
- Application Number
- JP2023083332
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-29
AI Technical Summary
Existing organic LED display devices suffer from blue shift, which causes color tone changes within the viewing angle, deteriorating display quality, and increasing haze value to suppress this shift leads to a decrease in brightness.
An optical film comprising a retardation layer with unit pattern regions having different slow axis directions, a base material layer, and an alignment film with projections and depressions, all laminated in a specific order, and optionally including a polarizing plate to suppress blue shift while maintaining brightness.
The solution effectively reduces blue shift and maintains brightness by aligning liquid crystal compounds in a predetermined direction, ensuring consistent color tone across various viewing angles.
Smart Images

Figure 2024166907000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an optical film and an image display device. [Background technology]
[0002] 2. Description of the Related Art Organic LED (Organic Light Emitting Diode) display devices, which are an example of image display devices, are used in various fields.
[0003] In such an organic LED display device, a blue shift is likely to occur in an image viewed from an oblique direction. The blue shift is a phenomenon in which an image viewed from an oblique direction appears bluer than an image viewed from the front. In other words, even an image displayed by an organic LED display device may have a change in color within the viewing angle due to the blue shift. If the color changes within the viewing angle in this way, it may become a factor that reduces the display quality of the image.
[0004] Meanwhile, various techniques for improving the display quality of images have been proposed (for example, see Patent Document 1). Patent Document 1 discloses an image display device that can suppress color unevenness when observed from an oblique angle by increasing the haze value of an antiglare film. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2009-163216 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, when the haze value of a film is increased, the brightness of an image display device may decrease, and therefore, it is required to suppress the occurrence of blue shift while suppressing the decrease in brightness in the image display device.
[0007] The present disclosure has been made in consideration of the above points, and aims to provide an optical film and an image display device that can suppress the occurrence of blue shift while suppressing a decrease in luminance. [Means for solving the problem]
[0008] The embodiments of the present disclosure relate to the following [1] to [5].
[0009] [1] An optical film having a retardation layer, The retardation layer is composed of unit pattern regions arranged repeatedly, The unit pattern region has a plurality of optical axis pattern regions whose slow axis directions are different from each other, The pitch of the unit pattern regions is 15 μm or less.
[0010] [2] A base material layer; An alignment film laminated on the base layer, The optical film according to [1], wherein the base layer, the alignment film, and the retardation layer are laminated in this order.
[0011] [3] The alignment film contains a UV-curable resin; The optical film according to [2], wherein the alignment film has projections and recesses corresponding to the slow axis.
[0012] [4] An optical film according to any one of [1] to [3]; and a display device laminated on the optical film.
[0013] [5] The image display device according to [4], further comprising a polarizing plate disposed between the optical film and the display device, or on the opposite side of the optical film from the display device. Effect of the Invention
[0014] According to the embodiment of the present disclosure, it is possible to suppress the occurrence of blue shift while suppressing the decrease in luminance. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a cross-sectional view showing an image display device according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing an image display device according to an embodiment. [Diagram 3] FIG. 3 is a cross-sectional view showing an image display device according to an embodiment. [Figure 4] FIG. 4 is a cross-sectional view showing an optical film according to an embodiment. [Diagram 5] FIG. 5 is a plan view showing an alignment layer of an optical film according to an embodiment. [Figure 6] FIG. 6 is a cross-sectional view (a cross-sectional view taken along line VI-VI in FIG. 5) showing an alignment layer of an optical film according to an embodiment. [Figure 7] FIG. 7 is a plan view showing another example of the alignment layer of the optical film according to the embodiment. [Figure 8A] FIG. 8A is a plan view illustrating another example of an alignment layer of an optical film according to an embodiment. [Figure 8B] FIG. 8B is a plan view illustrating another example of the alignment layer of the optical film according to the embodiment. [Figure 9] FIG. 9 is a schematic diagram showing an exposure apparatus for producing an alignment film. [Figure 10] FIG. 10 is a plan view showing a retardation layer of an optical film according to an embodiment. [Figure 11A] FIG. 11A is a plan view showing another example of a retardation layer of an optical film according to an embodiment. [Figure 11B] FIG. 11B is a plan view showing another example of the retardation layer of the optical film according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. In the drawings attached to this specification, the scale and the aspect ratio are appropriately changed and exaggerated from those of the actual objects for the convenience of illustration and understanding.
[0017] The terms used in this specification that specify shapes and geometric conditions, as well as the degree thereof, such as "parallel," "perpendicular," "same," and the values of lengths and angles, are not to be bound by strict meanings, but are to be interpreted to include a range within which similar functions can be expected.
[0018] In this specification, terms such as "film," "sheet," and "plate" are not terms that are distinguished from one another solely on the basis of differences in name. For example, a "film" cannot be distinguished from a member called a sheet or plate solely on the basis of differences in name.
[0019] First, the configuration of an image display device according to the present embodiment will be described with reference to FIGS.
[0020] As shown in FIGS. 1 to 3, the image display device 1 according to the present embodiment includes an optical film 10 and a display device 50 laminated on the optical film 10. The image display device 1 may further include a polarizing plate 40. In this case, as shown in FIG. 1, the polarizing plate 40 may be disposed between the optical film 10 and the display device 50. As shown in FIG. 2, the polarizing plate 40 may be disposed on the opposite side of the optical film 10 to the display device 50. As shown in FIGS. 1 and 3, the image display device 1 may further include an ultraviolet ray cut film 60. Here, the optical film 10 will be first described.
[0021] As shown in FIG. 4, the optical film 10 includes a retardation layer 30. The optical film 10 may further include a base layer 11 and an alignment film 20 laminated on the base layer 11. The base layer 11, the alignment film 20, and the retardation layer 30 may be laminated in this order. In this case, the retardation layer 30 may be disposed closer to the viewer (the positive side of the lamination direction Z) than the base layer 11. Although not shown, a primer layer may be provided between the base layer 11 and the alignment film 20.
[0022] Next, each layer of the optical film 10 will be described in detail.
[0023] <Base material layer> The base layer 11 is a layer that plays a role of supporting and protecting the retardation layer 30. The base layer 11 may be an optically isotropic layer. The base layer 11 may be a layer formed from a polymer, or may be a layer formed from glass. As the polymer constituting the base layer 11, cellulose acylate, polycarbonate-based polymer, polyester-based polymer such as polyethylene terephthalate or polyethylene naphthalate, acrylic polymer such as polymethyl methacrylate, or styrene-based polymer such as polystyrene or acrylonitrile-styrene copolymer (AS resin), etc. can be used. In addition, examples of the polymer constituting the base layer 11 include polyolefins such as polyethylene and polypropylene, polyolefin-based polymers such as ethylene-propylene copolymers, vinyl chloride-based polymers, amide-based polymers such as nylon or aromatic polyamide, imide-based polymers, sulfone-based polymers, polyethersulfone-based polymers, polyetheretherketone-based polymers, polyphenylene sulfide-based polymers, vinylidene chloride-based polymers, vinyl alcohol-based polymers, vinyl butyral-based polymers, arylate-based polymers, polyoxymethylene-based polymers, epoxy-based polymers, and mixtures of these polymers. The in-plane retardation of the base layer 11 is preferably 20 nm or less, more preferably 5 nm or less, even more preferably 3 nm or less, even more preferably 1 nm or less, and most preferably 0 nm. The wavelength λ of light serving as the reference for the retardation is 550 nm. The measurement is performed in low retardation mode using a measuring device KOBRA-WR manufactured by Oji Scientific Instruments.
[0024] When the base layer 11 is made of a polymer, the thickness of the base layer 11 may be about 25 μm or more and 125 μm or less. When the base layer 11 is made of glass, the thickness of the base layer 11 may be about 100 μm or more and 5 mm or less.
[0025] <Alignment film> The alignment film 20 plays a role in facilitating alignment of the liquid crystal compound in the retardation layer 30 when the retardation layer 30 is formed. After the retardation layer 30 is formed, the alignment film 20 may be removed. This makes it possible to obtain an optical film 10 without the alignment film 20.
[0026] As shown in FIG. 5 and FIG. 6, the alignment film 20 may have a concave-convex shape 21 corresponding to the slow axis of the optical axis pattern region Pa of the retardation layer 30, which will be described later. This allows the liquid crystal compound of the retardation layer 30 provided on the alignment film 20 to be aligned in a predetermined direction along the concaves 22 of the concave-convex shape 21. For example, when it is desired to change the direction of the in-plane slow axis for each optical axis pattern region Pa of the retardation layer 30, which will be described later, the alignment direction of the liquid crystal compound is changed by changing the longitudinal direction of the concaves 22 for each optical axis pattern region Pa. This allows the direction of the in-plane slow axis to be changed for each optical axis pattern region Pa. In this case, for example, the concave-convex shape 21 may be formed by an imprint method.
[0027] In the example shown in FIG. 5, the recesses 22 of the unevenness 21 extend linearly. The recesses 22 extend in a direction inclined in the first direction X and in a direction inclined in the second direction Y perpendicular to the first direction X. However, this is not limited thereto. For example, as shown in FIG. 7, the recesses 22 of the unevenness 21 may extend along the first direction X or the second direction Y, and as shown in FIGS. 8A and 8B, the recesses 22 of the unevenness 21 may extend in a curved shape. The first direction X and the second direction Y are directions perpendicular to the lamination direction Z of the optical film 10. Also, FIGS. 5, 7, and 8A show the alignment film 20 in the case where the number of optical axis pattern regions Pa of the retardation layer 30 described later is two, and FIG. 8B shows the alignment film 20 in the case where the number of optical axis pattern regions Pa of the retardation layer 30 described later is four.
[0028] The depth of the recesses 22 is preferably 2 nm or more and 200 nm or less, more preferably 10 nm or more and 100 nm or less, and even more preferably 20 nm or more and 50 nm or less. By making the depth of the recesses 22 2 nm or more, it is possible to more easily align a liquid crystal compound (liquid crystal molecules) described later along the recesses 22. By making the depth of the recesses 22 200 nm or less, it is possible to more easily peel the alignment film 20 from the shaping plate described later, and therefore it is possible to more easily and stably form the unevenness 21 of the alignment film 20.
[0029] The means for imparting an alignment regulating force to the alignment film 20 may be a conventionally known means. For example, the means for imparting an alignment regulating force to the alignment film 20 may be an imprinting method, a rubbing method, or a photoalignment method. Although any method can be used for fabrication, the imprinting method is preferred because roll processing can be efficiently performed when the shape is not linear. When fabricating the alignment film 20 by the imprinting method, it is preferred to use an electron beam curable resin in order to prevent deformation of the shape after curing. In addition, when fabricating the alignment film 20 by the imprinting method, the alignment film 20 may contain a UV curable resin. That is, the resin composition for forming the alignment film 20 may be a UV curable resin. Specific examples of UV curable resins include materials obtained by adding a photopolymerization initiator and any additive to a single material or a mixture of a polymerizable oligomer or monomer having an acryloyl group, such as urethane acrylate, epoxy acrylate, polyester acrylate, polyether acrylate, and melamine acrylate, and a polymerizable oligomer or monomer having a polymerizable vinyl group, such as acrylic acid, acrylamide, acrylonitrile, and styrene. The material of the alignment film 20 may be, for example, a thermosetting resin. When the alignment film 20 is produced by the photo-alignment method, first, a solution containing a thermosetting resin is dried to remove the solvent. Then, using a mask having a shape corresponding to the irregularities 21 of the present embodiment, intramolecular or intermolecular dimerization or isomerization is carried out by irradiating ultraviolet light through the mask, thereby producing the alignment film 20 having a desired shape.
[0030] <Imprint method> Next, a method for producing the alignment film 20 by an imprint method will be described. The unevenness of the alignment film 20 can be formed, for example, by shaping a layer containing a resin using a plate having a shape complementary to the surface shape of the alignment film 20. More specifically, the alignment film 20 can be formed, for example, by the following steps 1 and 2.
[0031] Step 1: A step of applying a coating liquid for forming an alignment film containing a resin onto a base layer 11 to form a layer containing a resin. Step 2: A step of shaping a layer containing a resin using a plate having a shape complementary to the surface shape of the alignment film 20.
[0032] When the alignment film 20 is produced by the imprint method, first, in step 1, a coating liquid for forming an alignment film containing a resin is applied onto the base layer 11 to form a layer containing a resin. When the coating liquid for forming an alignment film contains a solvent, it is preferable to dry the solvent in step 1.
[0033] When a curable resin is used as the resin, it is preferable to use a coating liquid for forming an alignment film containing a curable resin composition as the coating liquid for forming an alignment film in step 1. That is, when a curable resin is used as the resin, it is preferable that the curable resin in the coating liquid for forming an alignment film in step 1 is in an uncured state.
[0034] When a coating liquid for forming an alignment film containing an ionizing radiation curable resin composition is used as the coating liquid for forming an alignment film in step 1, it is preferable to cure the ionizing radiation curable resin composition contained in the shaped layer by irradiating with ionizing radiation simultaneously with the shaping in step 2.
[0035] When another layer such as a primer layer is provided between the substrate layer 11 and the alignment film 20, it is preferable to carry out a step of forming the other layer on the substrate layer 11 before step 1.
[0036] Next, in step 2, a layer containing a resin is shaped using a plate having a shape complementary to the surface shape of the alignment film 20. The plate used in step 2 can be produced by a general-purpose means such as laser lithography, electron beam lithography, or FIB (Focused Ion Beam). It is also preferable to produce many plates by duplicating the plate produced by the above-mentioned means, and arrange the many duplicated plates to form a multi-faceted plate. The plate duplication can be carried out by a general-purpose means such as electroforming.
[0037] When the alignment film 20 is produced by the imprint method, the thickness of the alignment film 20 may be about 0.5 μm or more and 20 μm or less, or about 1 μm or more and 10 μm or less. Here, in the step 1 of applying the alignment film forming coating liquid, there is a possibility that foreign matter may be mixed into the alignment film forming coating liquid. Even if foreign matter is mixed into the alignment film forming coating liquid in this way, the alignment film 20 has a thickness of 0.5 μm or more, so that the foreign matter can be taken into the alignment film 20. That is, it is possible to prevent the foreign matter from being exposed from the surface of the alignment film 20. Therefore, it is possible to prevent a decrease in yield. Furthermore, since the alignment film 20 has a thickness of 0.5 μm or more, it is possible to easily produce the recesses 22 having a depth of 200 nm or less. Furthermore, since the alignment film 20 has a thickness of 20 μm or less, it is possible to prevent the occurrence of insufficient curing in the curable resin when irradiated with ultraviolet light. Therefore, it is possible to prevent the alignment film 20 from being unable to be released from the plate.
[0038] <Photo-alignment method> Next, a method for producing the alignment film 20 by a photo-alignment method will be described. Methods for producing the alignment film 20 by a photo-alignment method include a method using two-beam interference and a method of irradiating linearly polarized light using a light-shielding mask.
[0039] In the method using two-beam interference, first, a liquid in which a birefringence-inducing polymer is dissolved in a solvent is applied onto the base layer 11. Next, the liquid is dried to produce a coating film. Next, an orientation control force is imparted to the coating film by two-beam interference using highly coherent polarized beams such as laser beams.
[0040] The following two methods can be mentioned as a method using a light-shielding mask. In the first method, a light-shielding mask having a desired periodic pitch is used at least twice to irradiate at least two regions with linearly polarized light having different polarization characteristics and intensity. In the second method, first, a light-shielding mask having a desired periodic pitch is used to irradiate linearly polarized light. Next, linearly polarized light is irradiated without using a light-shielding mask to form regions with different irradiation energy amounts at a desired periodic pitch. This gives a periodic structure in which the molecular orientation directions differ by 90°. When comparing the first method with the second method, the second method has the advantage of being able to simplify the device.
[0041] Examples of photo-alignment materials used in the alignment film 20 according to the present embodiment include those described in JP-A-2006-285197, JP-A-2007-76839, JP-A-2007-138138, JP-A-2007-94071, JP-A-2007-121721, JP-A-2007-140465, and JP-A-2007-156439. azo compounds described in JP-A-2007-133184, JP-A-2009-109831, JP-A-3883848 and JP-A-4151746, aromatic ester compounds described in JP-A-2002-229039, and compounds having photoalignment units described in JP-A-2002-265541 and JP-A-2002-317013. photocrosslinkable polyimides, photocrosslinkable polyamides, and photocrosslinkable polyesters described in JP-T-2003-520878, JP-T-2004-529220, and JP-T-4162850; and photodimerizable compounds, particularly cinnamate compounds, chalcone compounds, and coumarin compounds, described in JP-A-9-118717, JP-T-10-506420, JP-T-2003-505561, WO 2010 / 150748, JP-A-2013-177561, and JP-A-2014-12823. Among these, photocrosslinkable polyimides, photocrosslinkable polyamides, photocrosslinkable polyesters, cinnamate compounds and chalcone compounds are preferred.
[0042] Next, an exposure device 70 for imparting an alignment regulating force to the alignment film 20 by a photo-alignment method will be described.
[0043] 9, the exposure device 70 includes a light source 71, a polarizing beam splitter 72, mirrors 73A and 73B, and λ / 4 plates 74A and 74B. Among these, the light source 71 includes a laser irradiation unit 75 and a λ / 2 plate (not shown). The light source 71 is configured to emit linearly polarized light P0 by changing the polarization direction of the laser light M emitted from the laser irradiation unit 75.
[0044] The polarizing beam splitter 72 serves to split the laser light M emitted from the light source 71 into two beams MA and MB.
[0045] The mirrors 73A and 73B are disposed on the optical paths of the two separated light beams MA and MB, respectively.
[0046] The λ / 4 plates 74A and 74B have parallel optical axes. The λ / 4 plate 74A converts the linearly polarized light P0 (light beam MA) into right-handed circularly polarized light P R The λ / 4 plate 74B converts the linearly polarized light P0 (light beam MB) into left-handed circularly polarized light P L It plays a role in converting
[0047] In such an exposure device 70, the alignment film 20a before the alignment pattern is formed is placed in an exposure section (not shown). Then, two light beams MA and MB are made to intersect on the alignment film 20a to cause interference. Due to this interference, the polarization state of the interference light periodically changes to an interference fringe pattern. Next, the alignment film 20a is exposed by being irradiated with the interference light. As a result, an alignment pattern in which the alignment state periodically changes is obtained in the alignment film 20.
[0048] In the exposure device 70, the period of the alignment pattern can be adjusted by changing the crossing angle α of the two light beams MA and MB. For example, when forming an alignment pattern on the alignment film 20 in which the slow axis of the liquid crystal compound rotates continuously by 180° in one direction, the length of one period in which the slow axis rotates by 180° can be adjusted by adjusting the crossing angle α. By forming a liquid crystal layer on the alignment film 20 having such an alignment pattern, it is possible to form a retardation layer 30 in which the slow axis of the liquid crystal compound rotates continuously in one direction. In addition, the rotation direction of the optical axis can be reversed by rotating the optical axes of the λ / 4 plates 74A and 74B by 90°, respectively.
[0049] When the alignment film 20 is produced by a photoalignment method, the thickness of the alignment film 20 may be about 1 nm or more and 1000 nm or less, or about 60 nm or more and 300 nm or less. When the thickness of the alignment film 20 is 1 nm or more, foreign matter can be taken into the alignment film 20, and a decrease in yield can be suppressed. Furthermore, when the thickness of the alignment film 20 is 1000 nm or less, a deterioration in the sensitivity of the alignment film 20 due to polarized light exposure can be suppressed. Therefore, a decrease in the liquid crystal alignment control force can be suppressed.
[0050] The alignment film 20 may be produced by a roll-to-roll method. By producing the alignment film 20 by the roll-to-roll method, the alignment film 20 can be mass-produced in a short time. The alignment film 20 may be produced from a single sheet. When producing the alignment film 20 from a sheet, the alignment film 20 can be produced from a metal plate or a resin plate by an imprint method, and can be produced by using a light-shielding mask by a photoalignment method.
[0051] <Retardation layer> The retardation layer 30 may contain a liquid crystal compound. The retardation layer 30 may be made of a composition further containing a photopolymerization initiator, a surfactant, and a solvent. Here, the liquid crystal compound, the photopolymerization initiator, the surfactant, and the solvent of the retardation layer 30 will be described first.
[0052] <<Liquid crystal compounds>> The liquid crystal compound of the retardation layer 30 may be a rod-shaped liquid crystal compound such as a nematic liquid crystal compound and a smectic liquid crystal compound, or a discotic liquid crystal compound. In this embodiment, the liquid crystal compound of the retardation layer 30 may be a rod-shaped liquid crystal compound or a discotic liquid crystal compound. In addition, the liquid crystal compound may be a polymerizable liquid crystal compound. In other words, the retardation layer 30 may be a cured product of a composition containing a polymerizable liquid crystal compound.
[0053] The polymerizable liquid crystal compound is a liquid crystal compound having a polymerizable group, and examples thereof include monofunctional liquid crystal compounds having one polymerizable group and polyfunctional liquid crystal compounds having two or more polymerizable groups. Among these, polyfunctional liquid crystal compounds are preferred, polyfunctional liquid crystal compounds having 2 to 3 polymerizable groups are more preferred, and polyfunctional liquid crystal compounds having 2 polymerizable groups are even more preferred. The polymerizable group is one that can be polymerized by irradiation with active energy rays such as ultraviolet rays, and examples thereof include ethylenically unsaturated double bonds such as vinyl groups, methacryloyl groups, and acryloyl groups.
[0054] In the retardation layer 30, the liquid crystal compound may be fixed in any of the alignment states of horizontal alignment, hybrid alignment, and tilt alignment. For example, the long axis of the rod-shaped liquid crystal compound may be substantially horizontal to the surface of the retardation layer 30. The rod-shaped liquid crystal compound being substantially horizontal means that the angle between the surface of the retardation layer 30 and the director of the rod-shaped liquid crystal compound is in the range of 0° to 20°. The angle may be 0° to 10°, or 0° to 5°.
[0055] The discotic liquid crystal compound may have a substantially perpendicular surface to the film surface (optically anisotropic layer surface). The discotic liquid crystal compound is substantially perpendicular to the film surface (optically anisotropic layer surface). The average angle between the surface of the retardation layer 30 and the discotic liquid crystal compound is within the range of 70° to 90°. The angle may be 80° to 90°, or 85° to 90°.
[0056] As the rod-shaped liquid crystal compound, azomethines, azoxys, cyanobiphenyls, cyanophenyl esters, benzoates, cyclohexane carboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolanes, or alkenylcyclohexylbenzonitriles can be used. As the rod-shaped liquid crystal compound, not only these low molecular weight liquid crystal compounds but also polymeric liquid crystal compounds can be used. In addition, the rod-shaped liquid crystal compound may have a polymerizable group. The number of polymerizable groups in one molecule of the rod-shaped liquid crystal compound may be 2 or 3, or may be 2.
[0057] Discotic liquid crystal compounds are described in various documents (C. Destrade et al., Mol. Crysr. Liq. Cryst., vol. 71, page 111 (1981); Quarterly Chemistry Review, No. 22, Chemistry of Liquid Crystals, Chapter 5, Chapter 10, Section 2 (1994), edited by the Chemical Society of Japan; B. Kohne et al., Angew. Chem. Soc. Chem. Comm., page 1794 (1985); J. Zhang et al., J. Am. Chem. Soc., vol. 116, page 2655 (1994)). Polymerization of discotic liquid crystal compounds is described in JP-A-8-27284.
[0058] The discotic liquid crystal compound may have a polymerizable group. In this case, for example, a structure in which a polymerizable group is bonded as a substituent to the discotic core of the discotic liquid crystal compound is considered. On the other hand, if the polymerizable group is directly bonded to the discotic core, it may be difficult to maintain the alignment state during the polymerization reaction. Therefore, the discotic liquid crystal compound may have a linking group between the discotic core and the polymerizable group. That is, the discotic liquid crystal compound having a polymerizable group may be a compound represented by the following formula: D(-LP)n In the formula, D is a discotic core, L is a divalent linking group, P is a polymerizable group, and n is an integer of 1 to 12. Specific examples of the discotic core (D), the divalent linking group (L), and the polymerizable group (P) in the formula are (D1) to (D15), (L1) to (L25), and (P1) to (P18) described in JP-A-2001-4837, respectively, and the contents described in the same publication can be used. The phase transition temperature of the discotic liquid crystal compound may be 30° C. or more and 300° C. or less, or 30° C. or more and 170° C. or less.
[0059] In addition, as described later, the retardation layer 30 may exhibit reverse dispersion. In this case, as a liquid crystal compound exhibiting reverse dispersion, compounds described in each publication such as JP-T-2010-537954, JP-T-2010-537955, JP-T-2010-522892, JP-T-2010-522893, or JP-T-2013-509458, or each patent publication such as Japanese Patent No. 5892158, Japanese Patent No. 5979136, Japanese Patent No. 5994777, or Japanese Patent No. 6015655 may be used.
[0060] The liquid crystal compound may be used alone or in combination of two or more. When using one liquid crystal compound alone, the liquid crystal compound may be a polymerizable liquid crystal compound. When using two or more liquid crystal compounds in combination, at least one may be a polymerizable liquid crystal compound, or all may be polymerizable liquid crystal compounds. The content of the polymerizable liquid crystal compound in the composition constituting the retardation layer 30 may be 60% by mass or more and 99.9% by mass or less, or 65% by mass or more and 98% by mass or less, based on the total solid matter in the composition.
[0061] <<Photopolymerization initiator>> Examples of the photopolymerization initiator of the retardation layer 30 include acetophenone, benzophenone, α-hydroxyalkylphenone, Michler's ketone, benzoin, benzyl dimethyl ketal, benzoyl benzoate, α-acyloxime ester, and thioxanthones. The content of the photopolymerization initiator in the composition constituting the retardation layer 30 may be 0.01% by mass or more and 20% by mass or less, or 0.5% by mass or more and 5% by mass or less, based on the total solid matter in the composition.
[0062] <<Surfactants>> The surfactant of the retardation layer 30 may be a fluorine-based surfactant having a polymerizable group or a silicon-based surfactant having a polymerizable group. The fluorine-based surfactant and the silicon-based surfactant may be used in combination. The content of the surfactant in the composition constituting the retardation layer 30 may be 0.01% by mass or more and 2.0% by mass or less, or 0.1% by mass or more and 1.0% by mass or less, based on the total solid matter in the composition.
[0063] <<Solvent>> Examples of the solvent for the retardation layer 30 include ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.), ethers (dioxane, tetrahydrofuran, etc.), aliphatic hydrocarbons (hexane, etc.), alicyclic hydrocarbons (cyclohexane, etc.), aromatic hydrocarbons (toluene, xylene, etc.), halogenated carbons (dichloromethane, dichloroethane, etc.), esters (methyl acetate, ethyl acetate, butyl acetate, etc.), alcohols (butanol, cyclohexanol, etc.), cellosolves (methyl cellosolve, ethyl cellosolve, etc.), cellosolve acetates, sulfoxides (dimethyl sulfoxide, etc.), or amides (dimethylformamide, dimethylacetamide, etc.), and mixtures thereof may also be used. The content of the solvent in the composition constituting the retardation layer 30 may be 50% by mass or more and 90% by mass or less, or 70% by mass or more and 80% by mass or less, in the composition.
[0064] Such a retardation layer 30 can be formed, for example, by applying a composition constituting the retardation layer 30 onto the alignment film 20, and then drying and curing the composition. Specific drying conditions vary depending on the composition constituting the retardation layer 30, but the drying temperature may be 40° C. or higher and 150° C. or lower. In order to suppress deformation of the base layer 11, the drying temperature is preferably 40° C. or higher and 100° C. or lower. The drying time may be 30 seconds or higher and 250 seconds or lower, or 50 seconds or higher and 200 seconds or lower. When polymerizing the polymerizable liquid crystal compound, ultraviolet rays may be used. The irradiation energy of the ultraviolet rays varies depending on the thickness of the retardation layer 30, etc., but is preferably 50 mJ / cm. 2 More than 1J / cm 2 or less, 150 mJ / cm 2 More than 900mJ / cm 2 It may be the following.
[0065] The retardation layer 30 is most preferably a layer that gives a retardation of λ / 2 at a measurement wavelength of 550 nm, but may also be a layer that gives a retardation of n times λ / 4 (nλ / 4). The retardation layer 30 may be a λ / 2 retardation layer or a λ / 4 retardation layer. When the retardation layer 30 is a λ / 2 retardation layer, the in-plane retardation at a wavelength of 550 nm may be 220 nm or more and 300 nm or less, 230 nm or more and 280 nm or less, or 240 nm or more and 275 nm or less. When the retardation layer 30 is a λ / 4 retardation layer, the in-plane retardation at a wavelength of 550 nm may be 90 nm or more and 160 nm or less, 100 nm or more and 150 nm or less, or 110 nm or more and 150 nm or less. In this specification, the in-plane phase difference (in-plane retardation, Re) can be expressed by the following formula, where the refractive index in the in-plane slow axis direction is nx, the refractive index in the in-plane direction perpendicular to nx is ny, the refractive index in the direction perpendicular to nx and ny is nz, and the film thickness is d (nm). In-plane phase difference (Re)=(nx-ny)×d The in-plane retardation of the retardation layer 30 means the average value of five in-plane retardations obtained by excluding the maximum value and the minimum value from the in-plane retardations at seven locations within the in-plane of the retardation layer 30. The wavelength λ of the light serving as the reference for the retardation is set to 550 nm. As a measuring device for the in-plane retardation, the product name "AxoStep" manufactured by AXOMETRICS can be mentioned.
[0066] The retardation layer 30 may exhibit positive dispersion or negative dispersion. Note that negative dispersion is a characteristic in which the retardation imparted to the transmitted light increases as the wavelength of the transmitted light becomes longer. Specifically, negative dispersion is a characteristic in which the relationship between the retardation (Re450) at a wavelength of 450 nm and the retardation (Re550) at a wavelength of 550 nm is Re450 < Re550. On the other hand, positive dispersion is a characteristic in which the relationship between Re450 and Re550 is Re450 > Re550.
[0067] The thickness of the retardation layer 30 can be appropriately adjusted within the range of 0.1 μm or more and 10 μm or less in consideration of the retardation to be imparted.
[0068] Here, as shown in FIG. 10, in the present embodiment, the retardation layer 30 is composed of unit pattern regions 31 arranged in a repeating manner. A plurality of unit pattern regions 31 of the retardation layer 30 are arranged along the first direction X. Note that a plurality of unit pattern regions 31 of the retardation layer 30 may be arranged along a curve (for example, a meandering curve). In this case, it is possible to suppress the deterioration of visibility caused by diffracted light due to reflection in one direction.
[0069] The unit pattern region 31 has a plurality of optical axis pattern regions Pa (first optical axis pattern region Pa1 and second optical axis pattern region Pa2) whose slow axis directions are different from each other. The plurality of optical axis pattern regions Pa are arranged along the first direction X. In the illustrated example, each unit pattern region 31 has two optical axis pattern regions Pa. The widths of the optical axis pattern regions Pa are equal to each other. The unit pattern region 31 may have a plurality of optical axis pattern regions Pa whose widths are close to each other. For example, the unit pattern region 31 may have an optical axis pattern region Pa whose width is 5 μm (median value) and an optical axis pattern region Pa whose width is 4 μm or 6 μm. The straight lines in the optical axis pattern region Pa in FIG. 10 indicate the direction of the in-plane slow axis. The curves in the optical axis pattern region Pa in FIG. 11A and FIG. 11B described later indicate the direction in which the liquid crystal compounds are arranged.
[0070] In addition, as shown in FIG. 8A and FIG. 8B, when the direction in which the unevenness 21 of the alignment film 20 extends changes continuously, the direction in which the optical axis extends changes continuously as shown in FIG. 11A and FIG. 11B. In addition, FIG. 11A shows a retardation layer 30 formed on the alignment film 20 shown in FIG. 8A, and in the retardation layer 30 shown in FIG. 11A, each unit pattern region 31 has two optical axis pattern regions Pa. FIG. 11B shows a retardation layer 30 formed on the alignment film 20 shown in FIG. 8B, and in the retardation layer 30 shown in FIG. 11B, each unit pattern region 31 has four optical axis pattern regions Pa. In these cases, depending on the width of the optical axis pattern region Pa, when the width of each optical axis pattern region Pa is 5 μm or more, the number of optical axis pattern regions Pa in the unit pattern region 31 may be 3 to 90 as follows. In this case, the number of optical axis pattern regions Pa in the unit pattern region 31 is preferably 10 to 60, more preferably 20 to 30. By having the number of optical axis pattern regions Pa in the unit pattern region 31 be 3 or more, a sudden change in the direction in which the optical axis extends can be suppressed. Therefore, the deterioration of the liquid crystal alignment can be suppressed. Furthermore, by having the number of optical axis pattern regions Pa in the unit pattern region 31 be 90 or less, it is possible to suppress the number of boundary portions between adjacent optical axis pattern regions Pa from increasing too much. Therefore, it is possible to suppress the generation of unnecessary diffracted light at the boundary portions. When the width of each optical axis pattern region Pa is 5 μm or less, there is no problem when the alignment film 20 is produced by the photoalignment method, but when the alignment film 20 is produced by the imprint method, it is preferable that the number of optical axis pattern regions Pa in the unit pattern region 31 be 3 to 20. By making the number of optical axis pattern regions Pa in the unit pattern region 31 20 or less, it is possible to prevent the width of the uneven shape of the alignment film 20 from becoming too narrow. Therefore, the resin constituting the unevenness 21 of the alignment film 20 can maintain the shape of the convex portions in a good condition.
[0071] Here, the unit pattern regions 31 have the same optical axis pattern region Pa. In the illustrated example, each unit pattern region 31 has a first optical axis pattern region Pa1 and a second optical axis pattern region Pa2. Therefore, in the example shown in Fig. 10, the first optical axis pattern region Pa1 and the second optical axis pattern region Pa2 are alternately arranged along the first direction X.
[0072] As described above, the directions of the slow axes of the optical axis pattern regions Pa are different from each other. In the illustrated example, the directions of the slow axes correspond to the longitudinal directions of the concaves and convexes 21 and the concaves 22 formed on the alignment film 20 described above. On the other hand, the directions of the slow axes within each optical axis pattern region Pa are the same as each other.
[0073] In addition, when the number of optical axis pattern regions Pa in the unit pattern region 31 is three or more, each optical axis pattern region Pa may be configured so that the direction of the in-plane slow axis changes stepwise along the first direction X. For example, although not shown, the angle of the in-plane slow axis of the optical axis pattern region Pa with respect to the second direction Y may change stepwise as it moves toward the positive side of the first direction X. For example, when the number of optical axis pattern regions Pa in the unit pattern region 31 is 180, the angle of the slow axis in each optical axis pattern region Pa with respect to the second direction Y may change stepwise by 1°. By changing the direction of the slow axis stepwise, alignment defects of the liquid crystal compound between the optical axis pattern regions Pa can be suppressed, which is preferable.
[0074] The shape of each optical axis pattern region Pa may be, for example, a quadrilateral such as a square, a rectangle, or a diamond, or a polygon such as a triangle or a hexagon. The width (length in the first direction X) of each optical axis pattern region Pa may be, for example, 0.001 mm or more and 1 mm or less. The widths of each optical axis pattern region Pa may be the same as each other or may be different from each other.
[0075] The pitch P of the unit pattern regions 31 is 15 μm or less. This makes it possible to suppress a decrease in the brightness of the optical film 10 and to suppress the occurrence of a blue shift even when the image display device 1 is viewed from an oblique angle. The pitch P of the unit pattern regions 31 may be 2 μm or more. When the pitch P of the unit pattern regions 31 is 2 μm or more, the formability of the irregularities 21 can be improved when the alignment film 20 is produced by an imprint method.
[0076] The optical film 10 according to the present embodiment may further include other layers such as a functional layer or a pressure-sensitive adhesive layer.
[0077] <Functional layer> The functional layer may have a function as, for example, a hard coat layer, an antiglare layer, an antireflection layer, etc. The functional layer may be formed on, for example, the base layer 11 or the like.
[0078] <Adhesive layer> The adhesive layer may be a layer for bonding each layer of the optical film 10 to each other. The adhesive constituting the adhesive layer may be a general-purpose adhesive such as an acrylic adhesive, a polyester adhesive, a urethane adhesive, or a vinyl adhesive. The adhesive layer formed from these general-purpose adhesives usually has optical isotropy. The thickness of the adhesive layer may be about 2 μm or more and 30 μm or less.
[0079] <Specific layer structure of optical film> The layer structure of the optical film 10 is not particularly limited, but the optical film 10 may have the following structures (1) to (15), where " / " indicates the interface between layers. (1) Base layer / Alignment film / Retardation layer (2) Functional layer / base layer / alignment film / retardation layer (3) Base layer / adhesive layer / retardation layer / alignment film / base layer (4) Base layer / adhesive layer / retardation layer / alignment film / base layer / functional layer (5) Functional layer / base layer / adhesive layer / retardation layer / alignment film / base layer (6) Functional layer / base layer / adhesive layer / retardation layer / alignment film / base layer / functional layer (7) Base material layer / adhesive layer / retardation layer / adhesive layer / base material layer (8) Base material layer / adhesive layer / retardation layer / adhesive layer / base material layer / functional layer (9) Functional layer / base layer / adhesive layer / retardation layer / adhesive layer / base layer (10) Base layer / adhesive layer / retardation layer / alignment film / adhesive layer / base layer (11) Base layer / adhesive layer / retardation layer / alignment film / adhesive layer / base layer / functional layer (12) Functional layer / base layer / adhesive layer / retardation layer / alignment film / adhesive layer / base layer (13) Base layer / adhesive layer / alignment film / retardation layer / adhesive layer / base layer (14) Base layer / adhesive layer / alignment film / retardation layer / adhesive layer / base layer / functional layer (15) Functional layer / base layer / adhesive layer / alignment film / retardation layer / adhesive layer / base layer
[0080] Next, the polarizing plate 40 and the display device 50 of the image display device 1 will be described.
[0081] [Polarizing plate] The polarizing plate 40 plays a role of exhibiting light absorption performance or anti-reflection performance by being disposed on a display element such as an organic EL element or a touch panel such as a resistive film type touch panel (not shown). The polarizing plate may be a linear polarizing plate or a circular polarizing plate.
[0082] The polarizer of the polarizing plate 40 may be an iodine-based polarizer, a dye-based polarizer using a dichroic dye, or a polyene-based polarizer. Iodine-based polarizers and dye-based polarizers can generally be manufactured using a polyvinyl alcohol-based film. The absorption axis of the polarizer corresponds to the stretching direction of the film. Therefore, a polarizer stretched in the vertical direction (transport direction) has an absorption axis extending parallel to the longitudinal direction. On the other hand, a polarizer stretched in the horizontal direction (direction perpendicular to the transport direction) has an absorption axis extending perpendicular to the longitudinal direction.
[0083] [Display device] The display device 50 is, for example, an organic EL (Electro Luminescence) display device. The display device 50 may include, for example, a metal layer, a support substrate, a resin substrate, a thin film transistor (TFT), and an organic EL layer, all of which are not shown. A touch panel, not shown, may be disposed on the display device 50. The touch panel may be a resistive touch panel, a capacitive touch panel, an optical touch panel, an ultrasonic touch panel, an electromagnetic induction touch panel, or the like. These touch panels may have a pressure detection function. Although not shown, the display device 50 may be housed in a housing, not shown, together with a control unit (not shown) electrically connected to the display device 50.
[0084] <Size, shape, etc.> When manufacturing the display device 50, the optical film 10 and the polarizing plate 40 may be made of a sheet-like material cut to a predetermined size, or a roll-like material obtained by winding a long sheet into a roll. When using a sheet-like material, the size of the optical film 10, etc. is not particularly limited, but the maximum diameter may be about 0.5 inches or more and 500 inches or less. The "maximum diameter" refers to the maximum length when any two points of the optical film 10, etc. are connected. For example, when the optical film 10, etc. is rectangular, the diagonal line of the rectangle is the maximum diameter. When the optical film 10, etc. is circular, the diameter of the circle is the maximum diameter.
[0085] When using a material in a roll form, the width and length of the optical film 10 are not particularly limited, but generally, the width may be about 300 mm or more and 8000 mm or less, and the length may be about 50 m or more and 10000 m or less. The optical film 10 in a roll form can be cut into sheets according to the size of the image display device 1 or the like. When cutting, it is preferable to remove the end of the roll, which has unstable physical properties. When cutting into sheets, the shape of the cut material is not particularly limited, and for example, the shape of the material may be a polygon such as a triangle, a rectangle, or a pentagon, a circle, or a random, indefinite shape.
[0086] Next, a method for producing the optical film 10 according to the present embodiment will be described.
[0087] First, the base layer 11 is prepared.
[0088] Next, an alignment film 20 is formed on the base material layer 11. In this case, first, for example, a UV curable resin is applied onto the base material layer 11, and then the unevenness 21 is formed by, for example, an imprint method. Thereafter, the UV curable resin is irradiated with ultraviolet rays to cure the UV curable resin.
[0089] Next, the retardation layer 30 is formed on the alignment film 20. In this case, for example, a composition constituting the retardation layer 30 is applied onto the alignment film 20, and then the composition is dried and cured to form the retardation layer 30.
[0090] In this manner, the optical film 10 shown in FIG. 4 is obtained.
[0091] As described above, according to the present embodiment, the retardation layer 30 of the optical film 10 is composed of unit pattern regions 31 arranged repeatedly. Moreover, the unit pattern region 31 has a plurality of optical axis pattern regions Pa whose slow axis directions are different from each other. The pitch P of the unit pattern regions 31 is 15 μm or less. This makes it possible to suppress the occurrence of blue shift even when the image display device 1 is viewed obliquely while suppressing the decrease in luminance of the optical film 10. Note that, by making the pitch P of the unit pattern regions 31 15 μm or less, it is possible to suppress the occurrence of blue shift even when the image display device 1 is viewed obliquely while suppressing the decrease in luminance of the optical film 10, as will be described in the examples below. EXAMPLES
[0092] Next, a specific example of the above embodiment will be described.
[0093] Example 1 The optical film 10 shown in Fig. 4 was produced. First, the alignment film 20 shown in Fig. 8B was produced by an imprint method. The pitch P of the unit pattern regions 31 was set to 0.5 µm. The number of optical axis pattern regions Pa was set to four.
[0094] When producing the optical film 10, first, a plate for forming the alignment layer 20 was produced. At this time, a master mold having a surface shape designed by simulation was first produced. At this time, a synthetic quartz plate having a size of 6 inches square was used to produce the quartz master mold by an electron beam lithography process using an electron beam drawing device and a dry etching device.
[0095] Next, an ultraviolet-curable resin was poured into the mother mold, and then the ultraviolet-curable resin was irradiated with ultraviolet light to cure the ultraviolet-curable resin. The ultraviolet-curable resin was then peeled off from the mother mold to obtain a resin plate having a shape complementary to the surface shape of the mother mold. Next, a plurality of replica molds of the mother mold, which are molds having a shape complementary to the shape of the resin plate, were produced by electroforming. Next, the plurality of replica molds were wound around a roll to produce a roll-shaped plate.
[0096] Next, a primer layer having the following formulation was applied onto the substrate layer 11 (a cycloolefin polymer having a thickness of 40 μm, Zeon Corporation's trade name "ZEONOR") and dried to form a primer layer having a thickness of 0.5 μm.
[0097] Next, a coating liquid for forming a pattern layer having the following formulation was applied onto the primer layer and dried to form a layer containing an uncured resin.
[0098] Next, the above-mentioned roll-shaped plate was used to form a layer containing uncured resin by the roll-to-roll method, and at the same time, ultraviolet light was irradiated from the side of the base layer 11 to cure the layer containing the formed resin. At this time, the integrated light amount of the ultraviolet light was 500 mJ / cm. 2 Next, the shaped layer was peeled off from the plate to obtain a laminate having the primer layer and the pattern layer (alignment film 20) on the base layer 11.
[0099] Next, the following liquid crystal layer (retardation layer) forming coating solution was applied onto the pattern layer by a continuous roll-to-roll method, dried, and then irradiated with ultraviolet light to form a liquid crystal layer (retardation layer 30). At this time, the integrated light amount of the ultraviolet light was 150 mJ / cm. 2 It was decided.
[0100] The liquid crystal layer was made of liquid crystal with an in-plane birefringence (Δn) of 0.15, and the thickness was adjusted so that the in-plane retardation was 275 nm. In Example 1, in which the pitch P of the unit pattern region 31 was 0.5 μm, the liquid crystal layer forming coating liquid was applied four times to obtain the desired film thickness. In Example 2 to Comparative Example 3 described later, when the pitch P was 10 μm, the liquid crystal layer forming coating liquid was applied two times to obtain the desired film thickness, and when the pitch P was 20 μm, the liquid crystal layer forming coating liquid was applied in one time. This is because the liquid crystal orientation differs depending on the size of the pitch P.
[0101] By the above steps, the optical film 10 according to Example 1 was produced.
[0102] <Coating solution for forming primer layer> Polyolefin resin: 70 parts by weight (Mitsubishi Chemical Corporation, product name: Surflen P-1000) Silica-based lubricant: 5 parts by weight (Manufactured by CIK Nanotech, product name: SIRMIBK15WT%-E65) Methyl ethyl ketone: 25 parts by weight
[0103] <Coating solution for forming pattern layer> Pentaerythritol triacrylate: 96 parts by weight (Manufactured by Nippon Kayaku Co., Ltd., product name: PET-30) Photopolymerization initiator: 4 parts by weight (IGM, product name: Omnirad184)
[0104] <Liquid crystal layer coating solution> Surfactant: 0.04 parts by weight (BYK-361N (product name), manufactured by BYK-Chemie) ·Rod-shaped liquid crystal molecules: 10 parts by mass (LC242 (product name), manufactured by BASF, in-plane birefringence (Δn)=0.15) Photopolymerization initiator: 0.4 parts by weight (IGM, product name: Omnirad184) Methyl ethyl ketone: 89.6 parts by weight
[0105] Measurement sample preparation After confirming that there was no protective film or the like on the screen of a smartphone (Samsung Electronics' Galaxy Z Fold3 5G), a 25 μm-thick optical adhesive film (Panac Corp.'s PD-R5) was laminated onto the screen. Then, the optical film 10 was laminated onto the optical adhesive film so that the retardation layer faced the optical adhesive film. In this way, a measurement sample was prepared.
[0106] Next, the luminance was measured for the obtained optical film 10. The luminance of the optical film 10 was measured as follows using a color luminance meter (BM-5A, manufactured by Topcon Technohouse Corporation) in order to accurately measure the front luminance. (1) The height of the color luminance meter is set so that the distance from the top surface of the measurement sample to the focusing lens of the color luminance meter is 50 cm. At this time, in order to accurately measure the front luminance, the axis of the color luminance meter is adjusted using a reflector such as a mirror so that the lens part is reflected in the image seen through the lens. Thereafter, the measurement sample is placed at a predetermined position and observed again through the lens to adjust the focus to the top surface of the measurement sample. Note that the top surface of the measurement sample means the surface of the substrate layer 11 of the optical film 10 opposite to the retardation layer 30. (2) Set the brightness of your smartphone screen to maximum. (3) Set the measurement angle to 0.2°. (4) The measurement room was kept dark to prevent external light from entering, and the luminance was measured 30 seconds later when the amount of light had stabilized. The measurement was performed in an environment with a temperature of 25°C and a relative humidity of 45%. (5) For each measurement sample, the measurement in (4) above is repeated five times at one-minute intervals, the maximum and minimum values obtained from the five measurements are deleted, and the average value of the remaining values is determined as the brightness of the optical film 10.
[0107] The color coordinates x and y of the optical film 10 were also measured. The color coordinates x and y are the color coordinates x and y in an xy chromaticity diagram defined in the CIE 1931 color space. The color coordinates x and y were measured using EZ Contrast 160R manufactured by ELDIM. The measurement procedure was as follows. (1) Set the distance from the top surface of the measurement sample to the condenser lens of the color luminance meter device. At this time, set the height of the color luminance meter device so that it is in focus on the color filter of the smartphone (approximately 5 mm). (2) Set the brightness of your smartphone screen to maximum. (3) The measurement room was kept dark to prevent outside light from entering. The measurement environment was 25°C and 45% relative humidity. (4) Measurements and calculation of color coordinates x and y were performed using EZ Com V5.20.
[0108] In order to evaluate the change in color when viewed from a planar view and from an oblique direction, the color coordinates x and y when viewed from a planar view (0 degrees) and from a direction tilted by 60 degrees from the planar view were measured. Note that the color coordinates x and y when viewed from a direction tilted by 60 degrees from the planar view were taken as the average value of the color coordinates x and y measured from the left and right directions.
[0109] The above-mentioned measurements and evaluations were performed on areas without defects such as foreign matter, scratches, or wrinkles. The above-mentioned measurements and evaluations were performed in an atmosphere with a temperature of 23°C ± 5°C and a relative humidity of 40% to 65%, unless otherwise specified. Furthermore, the measurement sample was exposed to the atmosphere for 30 minutes to 60 minutes before each measurement, unless otherwise specified.
[0110] Example 2 An optical film 10 was produced in the same manner as in Example 1, except that the pitch P of the unit pattern region 31 was 1 μm and the number of optical axis pattern regions Pa was 8. In addition, the luminance and color coordinates of the optical film 10 were measured in the same manner as in Example 1.
[0111] Example 3 An optical film 10 was produced in the same manner as in Example 1, except that the pitch P of the unit pattern region 31 was 2 μm and the number of optical axis pattern regions Pa was 8. In addition, the luminance and color coordinates of the optical film 10 were measured in the same manner as in Example 1.
[0112] Example 4 An optical film 10 was produced in the same manner as in Example 1, except that the pitch P of the unit pattern region 31 was 3 μm and the number of optical axis pattern regions Pa was 8. In addition, the luminance and color coordinates of the optical film 10 were measured in the same manner as in Example 1.
[0113] Example 5 An optical film 10 was produced in the same manner as in Example 1, except that the pitch P of the unit pattern region 31 was 7 μm and the number of optical axis pattern regions Pa was 30. In addition, the luminance and color coordinates of the optical film 10 were measured in the same manner as in Example 1.
[0114] Example 6 An optical film 10 was produced in the same manner as in Example 1, except that the pitch P of the unit pattern region 31 was 15 μm and the number of optical axis pattern regions Pa was 30. In addition, the luminance and color coordinates of the optical film 10 were measured in the same manner as in Example 1.
[0115] Comparative Example 1 An optical film was produced in the same manner as in Example 1, except that an optical film in which the retardation layer was not composed of unit pattern regions was produced. The luminance and color coordinates of the optical film were measured in the same manner as in Example 1. In the optical film according to Comparative Example 1, the directions of the respective slow axes in the plane of the retardation layer were the same as each other.
[0116] Comparative Example 2 An optical film was produced in the same manner as in Example 1, except that the pitch P of the unit pattern region 31 was 20 μm and the number of optical axis pattern regions Pa was 30. In addition, the luminance and color coordinates of the optical film were measured in the same manner as in Example 1.
[0117] Comparative Example 3 An optical film was produced in the same manner as in Example 1, except that the pitch P of the unit pattern region 31 was 30 μm and the number of optical axis pattern regions Pa was 30. In addition, the luminance and color coordinates of the optical film were measured in the same manner as in Example 1.
[0118] The above results are shown in Tables 1 and 2.
[0119] [Table 1]
[0120] [Table 2]
[0121] In Table 1, "A" in the "formability" column means that the concaves and convexes of the alignment film could be formed with extremely high precision. In Table 1, "B" in the "formability" column means that the concaves and convexes of the alignment film could be formed with high precision.
[0122] In addition, in Table 2 above, "brightness ratio" means the ratio of the luminance of the optical films according to Examples 1 to 6, Comparative Examples 2 and 3 to the luminance of the optical film according to Comparative Example 1. In addition, in Table 2 above, "chromaticity variation amount" is an amount calculated by the following formula. Chromaticity fluctuation amount = (Δx 2 +Δy 2 ) 1 / 2 Note that Δx and Δy refer to the difference between the color coordinates x, y in planar view (0 degrees) and the color coordinates x, y when viewed from a direction tilted by 60 degrees with respect to the planar view.
[0123] As a result, as shown in Tables 1 and 2, in the optical films 10 according to Examples 1 to 6, even when the pitch was set to 15 μm or less, the unevenness 21 of the alignment film 20 could be formed with high precision. In particular, in the optical films 10 according to Examples 3 to 6, by setting the pitch to 2 μm or more, the unevenness 21 of the alignment film 20 could be formed with extremely high precision.
[0124] Furthermore, as shown in Tables 1 and 2, the luminance ratio was 93% or more in the optical films 10 according to Examples 1 to 6. Therefore, in the optical films 10 according to Examples 1 to 6, even when the pitch was 15 μm or less, a decrease in the luminance of the optical films 10 could be suppressed.
[0125] Furthermore, as shown in Tables 1 and 2, the optical films according to Comparative Examples 1 to 3 had a chromaticity coordinate difference Δx of 0.0463 or more. In contrast, the optical films 10 according to Examples 1 to 6 had a chromaticity coordinate difference Δx of 0.0407 or less. In particular, the optical films 10 according to Examples 1 to 5 had a chromaticity coordinate difference Δx of 0.0320 or less. Here, when the chromaticity coordinate x changes (approaches 0), the image tends to become blue. Therefore, it was found that the optical films 10 according to Examples 1 to 6 can reduce the chromaticity coordinate difference Δx, thereby suppressing the occurrence of blue shift in the image display device 1.
[0126] Furthermore, as shown in Tables 1 and 2, the optical films according to Comparative Examples 1 to 3 had a chromaticity variation of 0.0467 or more. In contrast, the optical films 10 according to Examples 1 to 6 had a chromaticity variation of 0.0412 or less. Therefore, the optical films 10 according to Examples 1 to 6 were able to reduce the color change between when viewed from a planar view and when viewed from an oblique direction. Therefore, it was found that the optical films 10 according to Examples 1 to 6 were able to suppress the occurrence of blue shift in the image display device 1 even when the image display device 1 was viewed from an oblique direction.
[0127] It is also possible to combine the multiple components disclosed in the above embodiment and each modification as necessary. Alternatively, some components may be deleted from all the components shown in the above embodiment and each modification.
Claims
1. An optical film having a retardation layer, The retardation layer is composed of unit pattern regions arranged repeatedly, The unit pattern region has a plurality of optical axis pattern regions whose slow axis directions are different from each other, The pitch of the unit pattern regions is 15 μm or less.
2. A base layer; An alignment film laminated on the base layer, The optical film according to claim 1 , wherein the base layer, the alignment film, and the retardation layer are laminated in this order.
3. The alignment film includes a UV curable resin, The optical film according to claim 2 , wherein the alignment film has projections and recesses corresponding to the slow axis.
4. The optical film according to claim 1 , and a display device laminated on the optical film.
5. The image display device according to claim 4 , further comprising a polarizing plate disposed between the optical film and the display device, or on the opposite side of the optical film to the display device.
Citation Information
Patent Citations
Set of polarizing plate, and liquid crystal panel and liquid crystal display using the same
JP2009163216A