Decorative film and manufacturing method of the same

The decorative film uses active energy ray-cured layers and waterless lithographic printing to overcome the limitations of traditional inks, achieving high-definition, three-dimensional patterns with enhanced productivity and reduced environmental impact.

JP2024168538AInactive Publication Date: 2024-12-05TORAY INDUSTRIES INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023085297
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Decorative films face challenges in forming high-definition, three-dimensional patterns with low environmental impact and high productivity due to the use of low-viscosity inks containing organic solvents, which emit VOCs and require lower curing temperatures, leading to bleeding and reduced productivity.

Method used

The decorative film employs active energy ray-cured layers for the pattern and backing layers, using rosin-modified resins, allyl resins, and acrylic resins, and a method involving direct ink transfer and curing without heating, combined with waterless lithographic printing to achieve high-definition and three-dimensional patterns.

Benefits of technology

This approach allows for the creation of high-definition, three-dimensional patterns with improved productivity and reduced environmental impact by eliminating the need for heating and solvent-based curing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168538000001_ABST
    Figure 2024168538000001_ABST
Patent Text Reader

Abstract

To provide a decorative film that can be used to produce high definition, three-dimensional patterns with high productivity.SOLUTION: A decorative film comprises a member having at least a film, a pattern layer, and a backing layer in that order, and the pattern layer and the backing layer are both activation energy line hardened films.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a decorative film and a method for manufacturing the decorative film. [Background technology]

[0002] Surface decoration using a decorative film is one method for imparting patterns such as letters and images to structures having three-dimensional or curved surfaces. In general, decorative films are given various designs by printing patterns on a film substrate using gravure printing, screen printing, or the like. Such decorative films are widely used to decorate the housings of mobile phone terminals, notebook PCs, digital cameras, and the like, as well as other home appliances, cosmetic containers, and interior and exterior parts of automobiles.

[0003] In recent years, decorative films are required to have design properties such as a three-dimensional effect, a sense of depth, and a sense of reality. For example, a decorative sheet for insert molding in which at least a colored layer, a resin layer, and a backer film are laminated in this order on a transparent base film, and embossing is performed from the colored layer toward the transparent base film, and the thickness of the resin layer is 0.3 to 2.5 times the embossing depth (see, for example, Patent Document 1); a decorative film formed by laminating a glossy layer, a patterned layer, and a concealing layer in this order on the surface of a base film, or the patterned layer, the glossy layer, and the concealing layer in this order, the base film is formed of a polyethylene terephthalate film or an acrylic film, the glossy layer and the concealing layer are laminated by silk screen printing, and the patterned layer is laminated by offset printing (see, for example, Patent Document 2), and the like are disclosed. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2010-82912 A [Patent Document 2] JP 2012-201006 A Summary of the Invention [Problem to be solved by the invention]

[0005] As mentioned above, decorative films generally have a pattern layer formed by gravure printing or screen printing. For such printing, inks that contain organic solvents and have low viscosity and high fluidity are generally used, and there are concerns about the environmental impact of VOCs, carbon dioxide, etc. that are emitted during the heating process to harden the ink. In addition, when using a film with a low glass transition temperature (Tg) that is easy to preform, it is necessary to lower the heating temperature to harden the ink, which poses a problem in productivity. Furthermore, in order to make designs such as line patterns, wood grain patterns, sand grain patterns, stone grain patterns, fabric patterns, pear-skin patterns, leather grain patterns, matte surface patterns, hairline patterns and geometric patterns look more realistic, there is a demand for higher definition (narrower halftone dots and fine lines) and three-dimensionality (thicker halftone dots and fine lines). However, with gravure printing and screen printing which use low-viscosity, highly fluid inks that contain organic solvents, it takes time for the ink to harden by heating, and the ink transferred to the film tends to spread and bleed, making it theoretically difficult to form a design layer that combines high definition and three-dimensionality.

[0006] Furthermore, in forming the backing layer, the lamination of a backer film as described in Patent Document 1 and the screen printing as described in Patent Document 2 have problems in terms of productivity.

[0007] Therefore, an object of the present invention is to overcome the problems of the conventional technology and to provide a decorative film on which high-definition, three-dimensional patterns can be formed with high productivity. [Means for solving the problem]

[0008] The decorative film of the present invention mainly has the following configuration. <1> A decorative film including a portion having at least a film, a design layer, and a backing layer in this order, the design layer and the backing layer both being active energy ray curable films. <2> The design layer contains a rosin-modified resin, an allyl-based resin, and / or an acrylic-based resin. <1> The decorative film according to claim 1. <3> The acrylic resin has a styrene group. <2> The decorative film according to claim 1. <4> The design layer further contains a compound having a urethane bond. <1> ~ <3> 13. The decorative film according to claim 12 . <5> The thickness of the backing layer is 5 μm or more and 100 μm or less. <1> ~ <4> 13. The decorative film according to claim 12 . <6> The method comprises, in order, at least: (1) a step of applying ink to the surface of a printing plate and transferring the ink onto a film directly or via a blanket; and (3a) a step of supplying a coating liquid for forming a backing layer onto the ink and curing the ink and the coating liquid for forming a backing layer by irradiating with active energy rays, thereby forming a design layer and a backing layer. <1> ~ <5> 13. A method for producing a decorative film according to any one of claims 1 to 12. <7> The method comprises, in order, at least: (1) a step of applying ink to the surface of a printing plate and transferring the ink onto a film directly or via a blanket; (2) a step of irradiating active energy rays to harden the ink to form a design layer; and (3b) a step of supplying a coating liquid for forming a backing layer onto the design layer, irradiating active energy rays to harden the coating liquid for forming the backing layer, and forming a backing layer. <1> ~ <5> 13. A method for producing a decorative film according to any one of claims 1 to 12. <8> The printing plate is a waterless lithographic printing plate. <6> or <7> A method for producing the decorative film according to claim 1. <9> In the step (3a) or (3b), a coating liquid for forming a backing layer is applied by a printing cylinder around which a lithographic printing plate having a silicone layer is wound. <6> ~ <8> 13. A method for producing a decorative film according to any one of claims 1 to 12. <10> The thickness of the silicone layer is 5 μm or more and 50 μm or less. <9> A method for producing the decorative film according to claim 1. <11> In the above (3a) or (3b), a coating liquid for forming a backing layer is supplied onto the ink or picture layer two or more times. <6> ~ <10> 13. A method for producing a decorative film according to any one of claims 1 to 12. Effect of the Invention

[0009] According to the present invention, a decorative film capable of forming a high-definition, three-dimensional pattern with high productivity can be obtained. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic cross-sectional view showing an example of a configuration of a decorative film according to the present invention. [Diagram 2] FIG. 4 is a schematic cross-sectional view showing another example of the configuration of the decorative film according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments, and can be modified in various ways depending on the purpose and application.

[0012] (Decorative film) The decorative film according to the present invention includes a portion having at least a film, a pattern layer, and a backing layer in this order. The film has a function of holding the pattern layer and the backing layer as a support for the decorative film. The pattern layer has a function of imparting design to the object to be decorated with a desired pattern. The backing layer has a function of concealing the background of the pattern layer, improving the contrast of the pattern, and protecting the pattern layer when it comes into contact with a high-temperature molten resin. Two or more of these layers may be included. In addition, the pattern and the backing layer do not need to be formed on the entire surface, and for example, the pattern layer may be partially included depending on the desired pattern. In addition, an adhesive layer that bonds the object to be decorated and the backing layer may be further included on the backing layer, and an optional functional layer may be further included between each layer.

[0013] In the present invention, both the pattern layer and the backing layer are active energy ray cured films. Here, the active energy ray cured film refers to a film in which a compound having an ethylenically unsaturated bond is crosslinked and cured by active energy rays. Since both the pattern layer and the backing layer are active energy ray cured films, the decorative film of the present invention does not require a process of heating and curing an ink containing an organic solvent in forming the pattern layer, so that a highly detailed and three-dimensional pattern can be formed with high productivity. In addition, the backing layer can be formed with high productivity because it does not require a process of heating and curing an ink containing an organic solvent or a process of laminating with a backer film in forming the backing layer.

[0014] FIG. 1 shows a schematic cross-sectional view of an example of the configuration of the decorative film according to the present invention. The decorative film 100 according to the present invention has, from the top of the page, a film 1, a pattern layer 2, and a backing layer 3. The pattern layer 2 may be formed of two or more colors. For example, when the pattern layer is formed of two colors, it can be called a pattern layer 2a and a pattern layer 2b. The line width of each pattern layer may be the same or different, and the line width of the pattern layer with the smallest line width is defined as the minimum line width 2W. The height of each pattern layer may be the same or different, and the height of the pattern layer with the highest line width is defined as the maximum line height 2H. For example, when the object to be decorated is a resin molded product, the decorative film 100 can be suitably used for bonding the decorative film and the resin molded product by adhering the backing layer to the resin molten by injection molding or the like.

[0015] FIG. 2 shows a schematic cross-sectional view of another example of the configuration of the decorative film according to the present invention. The decorative film 200 according to the present invention has, from the top of the page, a film 1, a pattern layer 2 consisting of a pattern layer 2a and a pattern layer 2b, a backing layer 3, and an adhesive layer 4. As in FIG. 1, the line width of the pattern layer with the smallest line width is the minimum line width 2W, and the height of the pattern layer with the highest line height is the maximum line height 2H. For example, when the object to be decorated is a resin molded product, the decorative film 200 can be suitably used for bonding an injection-molded resin molded product and a decorative film via an adhesive layer.

[0016] The smaller the minimum line width 2W of the pattern layer 2, the more highly detailed the image can be reproduced, and the larger the maximum line height 2H, the more three-dimensional the expression becomes possible, so that patterns such as line patterns, grain patterns, sand grain patterns, stone grain patterns, cloth patterns, pear-skin patterns, leather grain patterns, matte surface patterns, hairline patterns, and geometric patterns can be made to look more realistic. From this viewpoint, the minimum line width 2W is preferably 60 μm or less, more preferably 30 μm or less, and even more preferably 23 μm or less. Moreover, the maximum line height 2H is preferably 2.0 μm or more, and more preferably 3.0 μm or more. Here, the line width and line height of the pattern layer can be measured by cross-sectional observation using a field emission scanning electron microscope (FE-SEM), and the line width of the thinnest part and the height of the highest part are measured for each of 10 randomly selected pattern layers, and the minimum line width is the minimum line width 2W, and the maximum height is the maximum line height 2H.

[0017] (film) Examples of the film include films of polyesters such as polyethylene terephthalate, polyolefins such as polyethylene and polypropylene, and resins such as polyamide, polyimide, polystyrene, polycarbonate, polyvinyl chloride, and polyvinyl acetal. Two or more of these may be used. Among these, polycarbonate, polyvinyl chloride, and polypropylene films are preferred. These films may contain additives in addition to the above-mentioned resins. The film may also be subjected to surface treatments such as primer resin coating, corona discharge treatment, and plasma treatment, which can improve the adhesion of the ink.

[0018] The glass transition temperature (Tg) of the film is preferably 110° C. or lower, more preferably 90° C. or lower, from the viewpoint of easy elongation during pre-shaping and excellent formability, while the Tg of the film is preferably 0° C. or higher from the viewpoint of maintaining the surface strength of the film.

[0019] (Picture layer) The design layer is an active energy ray cured film, for example, a film of an active energy ray curable ink (hereinafter sometimes abbreviated as "ink") containing a photopolymerization initiator and a compound having an ethylenic unsaturated bond described later is formed on a film, and the ink film is cured by irradiating the ink film with active energy rays. A part of the photopolymerization initiator and / or the compound having an ethylenic unsaturated bond remains in the design layer. The photopolymerization initiator and / or the compound having an ethylenic unsaturated bond in the design layer can be analyzed, for example, by GC-MS measurement of an extract obtained by extracting the free components in the design layer with dichloromethane.

[0020] Examples of active energy rays include ultraviolet rays (UV), electron beams (EB), infrared rays (IR), etc. Among these, UV rays can be preferably used.

[0021] As a method for forming an ink film that forms a pattern layer, active energy ray curing offset printing and flexographic printing are preferred because they do not require a heating process to remove organic solvents in the ink, have low environmental impact, can use a film with a low Tg, and are fast to print and have excellent productivity. Among them, offset printing that uses UV as active energy rays, i.e., UV offset printing, is preferably used because it has excellent design properties for the pattern layer. As a printing plate for offset printing, a waterless lithographic printing plate is preferred because it can form a more highly detailed and three-dimensional pattern by making the minimum line width smaller and the maximum line height larger.

[0022] The active energy ray curable ink preferably contains a colorant, a photopolymerization initiator, a compound having an ethylenic unsaturated bond, and a resin. It is also preferable to contain a compound having a urethane bond, which can improve the stretchability and followability of the decorative film and improve the moldability. Each component will be described.

[0023] (1) Coloring agent Examples of colorants include organic pigments and inorganic pigments. Examples of organic pigments and inorganic pigments include those exemplified as organic pigments and inorganic pigments in WO 2020 / 235557. Two or more of these may be contained.

[0024] The content of the colorant in the ink is preferably 5 to 40% by mass.

[0025] (2) Photopolymerization initiator The photopolymerization initiator is a component that generates radicals when irradiated with active energy rays and promotes crosslinking of a compound having an ethylenically unsaturated bond (3) described below, and is preferably used when UV is used as the active energy rays.

[0026] Examples of photopolymerization initiators include 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl-phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, 1-[4-(2-hydroxyethoxyl)-phenyl]-2-hydroxy-methylpropanone, 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone, and 2-dimethylamino)-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one. alkylphenone-based photopolymerization initiators such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide; intramolecular hydrogen abstraction type photopolymerization initiators such as methylbenzoyl formate; oxime ester-based photopolymerization initiators such as 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(o-benzoyloxime), ethenone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(o-acetyloxime); cationic photopolymerization initiators such as iodonium, (4-methylphenyl)[4-(2-methylpropyl)phenyl]-, hexafluorophosphate(1-)in propylene carbonate, sulfonium hexafluorophosphate, and sulfonium tetrakis[pentafluorophenyl]borate. Two or more of these may be contained.

[0027] The content of the photopolymerization initiator in the ink is preferably 0.1 to 30% by mass.

[0028] (3) Compounds having an ethylenically unsaturated bond Compounds having ethylenically unsaturated bonds are components that crosslink by radicals and are called monomers, oligomers, etc. Since they also function as a solvent for other ink components, the inclusion of a compound having an ethylenically unsaturated bond eliminates the need for organic solvents.

[0029] Examples of the monomer include a monofunctional monomer having one ethylenically unsaturated bond in the molecule and a difunctional or higher monomer having two or more ethylenically unsaturated bonds in the molecule. From the viewpoint of promoting curing by active energy rays and increasing the strength of the pattern layer, a difunctional or higher monomer is preferred.

[0030] Examples of the difunctional or higher monomer include trimethylolpropane triacrylate (TMPTA), ditrimethylolpropane tetraacrylate (DITMPTA), pentaerythritol tetra(meth)acrylate, dipentaerythritol propionate triacrylate, dipentaerythritol hexaacrylate (DPHA), glycerin propoxy triacrylate (GPTA), hexanediol diacrylate (HDDA; bifunctional), and ethylene oxide adducts thereof. Two or more of these may be contained. Here, (meth)acrylate is a general term for acrylate and methacrylate.

[0031] Examples of oligomers include epoxy-modified (meth)acrylates, which are exemplified by the ester of hydroxyl groups and (meth)acrylic acid generated after ring-opening of epoxy groups contained in epoxy compounds such as epoxy resins with acid or base, rosin-modified epoxy acrylates, polyester-modified (meth)acrylates, which are exemplified by the ester of terminal hydroxyl groups and (meth)acrylic acid of condensation polymers of dibasic acids and diols, polyether-modified (meth)acrylates, which are exemplified by the ester of terminal hydroxyl groups and (meth)acrylic acid of polyether compounds, and urethane-modified (meth)acrylates, which are exemplified by the ester of terminal hydroxyl groups and (meth)acrylic acid in condensation polymers of polyisocyanate compounds and polyol compounds. Two or more of these may be contained. Here, (meth)acrylic acid is a general term for acrylic acid and methacrylic acid.

[0032] The content of the compound having an ethylenically unsaturated bond in the ink is preferably 30 to 80% by mass.

[0033] (4) Resin Examples of the resin include alkyd resins, rosin-modified resins, allyl resins, acrylic resins, etc. Two or more of these may be contained.

[0034] Examples of rosin-modified resins include rosin-modified phenolic resins and rosin-modified maleic acid resins. Examples of allyl-based resins include diallyl phthalate resins. Examples of acrylic-based resins include methacrylic acid alkyl ester resins, acrylic acid alkyl ester resins, and styrene-acrylic resins. Here, the styrene-acrylic resin refers to a copolymer of (A) styrene and / or α-methylstyrene and (B) (meth)acrylic acid and / or (meth)acrylic acid alkyl ester.

[0035] Among these, styrene-acrylic resins are preferred from the viewpoint of achieving higher definition of the design layer. Styrene-acrylic resins contain (A) styrene and / or α-methylstyrene residues, which strengthen the interaction between the resins and reduce the spinnability of the ink, thereby suppressing the wetting and spreading of the ink in a fine design and achieving higher definition of the design layer.

[0036] The total content of (A) styrene and / or α-methylstyrene residues in the styrene-acrylic resin is preferably 40% by mass or more from the viewpoint of suppressing the spinnability of the ink and achieving higher definition of the design layer, while the total content of (A) styrene and / or α-methylstyrene residues in the styrene-acrylic resin is preferably 65% ​​by mass or less from the viewpoint of improving the flexibility of the resin and suppressing cracks in the design layer.

[0037] The content of the resin in the ink is preferably from 5 to 30% by mass.

[0038] (5) Compounds containing urethane bonds Examples of compounds having a urethane bond include polyurethane resins, urethane (meth)acrylate monomers and oligomers, etc. In the present invention, compounds having a urethane bond are classified as (5) compounds having a urethane bond even if they are compounds or resins having an ethylenically unsaturated bond.

[0039] The polyurethane resin is preferably one having a urethane bond formed by reacting an isocyanate compound with a polyol compound. The urethane bond contained in the polyurethane resin forms a hard segment by hydrogen bonding, and can impart toughness to the pattern layer. The polyol contained in the polyurethane resin forms a soft segment, and can impart flexibility to the pattern layer. This makes it difficult for cracks to occur in the pattern layer even if the decorative film is stretched during pre-shaping, and improves formability.

[0040] Examples of polyurethane resins include those exemplified as (a) polyurethane in WO 2020 / 235556.

[0041] The urethane (meth)acrylate is preferably one obtained by reacting a (meth)acrylic acid having a hydroxyl group, an isocyanate compound, and a polyol compound. The urethane bond contained in the urethane (meth)acrylate forms a hard segment by hydrogen bonding, and can impart toughness to the pattern layer. In addition, the polyol contained in the urethane (meth)acrylate forms a soft segment, and can impart flexibility to the pattern layer. This makes it difficult for cracks to occur in the pattern layer even if the decorative film is stretched during pre-shaping, and can improve formability. Furthermore, the (meth)acryloyl group contained in the urethane (meth)acrylate causes a curing reaction by irradiation with active energy rays, and can impart heat resistance to the pattern layer.

[0042] Examples of urethane (meth)acrylates include those exemplified as (a) urethane (meth)acrylates in WO 2020 / 235557.

[0043] The content of the compound having a urethane bond in the ink is preferably 3 to 20% by mass.

[0044] (Backing layer) The backing layer hides the background of the pattern layer to improve the contrast of the pattern, and also has the function of protecting the pattern layer when it comes into contact with a high-temperature molten resin, so unlike the pattern layer which expresses design with a fine pattern, it is preferable that the backing layer is present on almost the entire surface of the decorative film. In the present invention, the backing layer refers to a layer which is located in the order of the film, the pattern layer, and the backing layer, and occupies 95 to 100% by area of ​​the decorative film. The backing layer is an active energy ray cured film, for example, a film of an active energy ray curable ink containing a photopolymerization initiator and a compound having an ethylenic unsaturated bond is formed on a pattern layer, and the ink film is cured by irradiating the ink with active energy rays. In this case, the photopolymerization initiator may be, for example, the one exemplified as (2) above, and the compound having an ethylenic unsaturated bond may be, for example, the one exemplified as (3) above. Part of these (2) and / or (3) remains in the backing layer. (2) and / or (3) in the backing layer can be analyzed, for example, by GC-MS measurement of the extract obtained by extracting the free components in the backing layer with dichloromethane.

[0045] Examples of active energy rays include ultraviolet rays (UV), electron beams (EB), infrared rays (IR), etc. Among these, UV rays can be preferably used.

[0046] The active energy ray-curable ink used to form the backing layer (hereinafter, sometimes abbreviated as "ink for forming the backing layer") preferably contains the above-mentioned (2) photopolymerization initiator, (3) compound having an ethylenically unsaturated bond, colorant, and resin.

[0047] As the colorant used in the ink for forming the backing layer, among the above-mentioned (1) colorants, those that do not denature even when in contact with a high-temperature molten resin are preferred, and inorganic pigments with high heat resistance can be suitably used. In addition, two or more types of colorants may be used.

[0048] Examples of resins used in the ink for forming the backing layer include acrylic resins, ABS resins, polyolefin resins, styrene resins, vinyl chloride resins, polycarbonate resins, etc. Two or more of these may be included. When the object to be decorated is a resin molded product, such as the decorative film shown in FIG. 1, and the backing layer is adhered to the molten resin by injection molding or the like to adhere the decorative film to the resin molded product, it is preferable that the backing layer is formed from a material that easily adheres or bonds to the molten resin, and more preferably is the same type of material as the resin that constitutes the resin molded product.

[0049] Examples of the ink for forming the backing layer include UV-curable flexographic ink, UV-curable screen ink, UV-curable offset ink, EB-curable flexographic ink, and EB-curable offset ink. Two or more of these may be used. These active energy ray-curable inks may be diluted with a compound having an ethylenically unsaturated bond to reduce the viscosity.

[0050] The thickness of the backing layer is preferably 3.5 μm or more, more preferably 5.0 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more from the viewpoint of improving the strength of the decorative film, while the thickness of the backing layer is preferably 100 μm or less from the viewpoint of improving productivity.

[0051] The reflection density of the backing layer is preferably 1.20 or more, more preferably 1.30 or more, more preferably 1.50 or more, and even more preferably 2.00 or more, from the viewpoint of concealing the decorated object that is the background of the pattern layer and improving the contrast of the pattern. Here, the reflection density of the backing layer can be measured using a reflection spectrophotometer for the area that does not overlap with the pattern layer. More specifically, the reflection density is measured using a reflection spectrophotometer under the condition of color filter: black for 10 points randomly selected from the backing layer, and the average value is calculated. The reflection density of the backing layer can be adjusted to a desired range, for example, by selecting the colorant concentration of the ink for forming the backing layer and the thickness of the backing layer.

[0052] (Adhesive layer) Examples of materials for the adhesive layer include two-component curing urethane resins using isocyanate as a curing agent, chlorinated polyolefins such as chlorinated polypropylene, (meth)acrylic resins, vinyl chloride-vinyl acetate copolymers, etc. Two or more of these may be used.

[0053] The thickness of the adhesive layer is preferably 1 μm or more and 50 μm or less.

[0054] The decorative film of the present invention can be pre-shaped by being sandwiched between a heated mold. In this case, the breaking elongation of the decorative film, the formability of the decorative film, can be indexed by the breaking elongation measured using a universal testing machine for the area where the solid image part of the picture layer and the backing layer overlap. From the viewpoint of ease of pre-shaping (formability), it is preferably 120% or more, more preferably 150% or more, and even more preferably 200% or more. Here, the breaking elongation of the decorative film can be measured using a universal testing machine for a portion having at least the film, the picture layer, and the backing layer in this order. More specifically, test specimens are prepared from the aforementioned parts using a test specimen punching blade (dumbbell-shaped No. 4, compliant with JIS K 6251 (2017)), and the 150°C breaking point of the prepared test specimens is measured using a universal testing machine and a thermostatic chamber under conditions of temperature: 150°C, chuck distance: 20 mm, and tensile speed: 200 mm / min. Each measurement is performed three times, and the breaking elongation (%) is calculated using the following formula (α), and the average value is calculated. Breaking elongation (%) = (breaking point (mm) - 20 (mm)) / 20 (mm) × 100 (α).

[0055] (Method of manufacturing decorative film) The method for producing a decorative film according to an embodiment of the present invention may, for example, include a method which sequentially comprises at least (1) a step of attaching ink to the surface of a printing plate and transferring the ink onto a film directly or via a blanket (hereinafter, may be abbreviated as "step (1)") and (3a) a step of supplying a coating liquid for forming a backing layer onto the ink and curing the ink and the coating liquid for forming a backing layer by irradiating with active energy rays to form a design layer and a backing layer (hereinafter, may be abbreviated as "step (3a)"); or a method which sequentially comprises at least steps (1) and (2) a step of irradiating with active energy rays to cure the ink to form a design layer (hereinafter, may be abbreviated as "step (2)"). )") and (3b) a process for forming a backing layer by applying active energy rays to the backing layer-forming coating liquid to form a backing layer (hereinafter sometimes abbreviated as "process (3b)"). In either case, the formation of the design layer does not require a process for heat-curing an ink containing an organic solvent, so that a highly detailed, three-dimensional design layer can be formed with high productivity. In addition, the formation of the backing layer does not require a process for heat-curing an ink containing an organic solvent or a process for laminating with a backer film, so that the backing layer can be obtained with high productivity.

[0056] In the method for producing the decorative film according to the present invention, a publicly known offset printing machine, flexographic printing machine, resin letterpress printing machine, etc., equipped with an active energy ray irradiation device can be used. Among them, a UV offset printing machine can be preferably used from the viewpoint of excellent design of the picture layer and the viewpoint of widespread use of printing machines. An example of the method for producing the decorative film is shown below.

[0057] In step (1), ink is applied to the surface of a printing plate, and the ink is transferred onto a film directly or via a blanket.

[0058] In the method for producing a decorative film using a UV offset printing machine, the printing plate used for UV offset printing includes a water-based lithographic printing plate and a waterless lithographic printing plate. Among these, a waterless lithographic printing plate that does not require dampening water is preferred, and the picture layer can be made more precise. When a decorative film is produced using a multicolor UV offset printing machine equipped with an inline coater as the UV offset printing machine, in step (1), a waterless lithographic printing plate obtained by making a waterless lithographic printing plate precursor into a predetermined image pattern is mounted on the front cylinder (e.g., cylinders 1 to 4) of the multicolor UV offset printing machine equipped with an inline coater, and the ink exemplified as the ink for forming the picture layer of the decorative film described above is preferably supplied to the image portion of the waterless lithographic printing plate to adhere thereto, and the image-wise ink is preferably transferred to the film via a blanket.

[0059] If necessary, in step (2), the ink is irradiated with active energy rays to harden the ink and form a pattern layer. When a decorative film is produced using a multicolor UV offset printing machine equipped with an in-line coater as the UV offset printing machine, it is preferable to harden the ink by irradiating it with UV light from a UV lamp installed between the cylinders of the printing machine (for example, between cylinders 4 and 5).

[0060] Next, in step (3a) or (3b), a coating liquid for forming a backing layer is supplied onto the ink or the design layer, and the coating liquid for forming the backing layer is cured by irradiating with active energy rays to form a backing layer. In the case of step (3a) not including step (2), the coating liquid for forming the backing layer is supplied onto the ink, and then active energy rays are irradiated to combine and cure the ink and the coating liquid for forming the backing layer, thereby forming the design layer and the backing layer simultaneously. In the case of step (3b) provided after step (2), the coating liquid for forming the backing layer is supplied onto the design layer, and then active energy rays are irradiated to cure the coating liquid for forming the backing layer, thereby forming the backing layer.

[0061] Examples of the method for supplying the coating liquid for forming the backing layer include coating using coating equipment such as a chamber coater, a roll coater, a bar coater, a slit die coater, and a gap applicator, coating using a printing cylinder of a gravure printing machine, a flexographic printing machine, a resin letterpress printing machine, and an offset printing machine, and screen printing. Among these, coating using a chamber coater that is widely used as an in-line coating equipment of a printing machine, and coating using a printing cylinder that is not used for forming a pattern layer among the printing cylinders of a multi-color printing machine are preferred, and the pattern layer and the backing layer can be formed continuously, thereby further increasing productivity. In the coating using a printing cylinder, a waterless lithographic printing plate is preferred as the printing plate. That is, it is preferred to use a printing cylinder wrapped with a waterless lithographic printing plate as a coater to coat the coating liquid for forming the backing layer. The waterless lithographic printing plate preferably has a silicone layer on the substrate, and the thickness of the silicone layer is preferably 5 μm or more and 50 μm or less. By making the thickness of the silicone layer 5 μm or more, the cells to which the backing layer forming coating liquid adheres can be made deeper, and the backing layer forming coating liquid can be applied thickly, so that a backing layer having a thickness of 5 μm or more can be easily formed. The thickness of the silicone layer is more preferably 10 μm or more. On the other hand, the thickness of the silicone layer is more preferably 20 μm or less. In order to make the thickness of the backing layer within the desired range, the backing layer forming coating liquid may be supplied two or more times in step (3a) or (3b). In this case, the backing layer forming coating liquid may be supplied two or more times and then irradiated with active energy rays to harden the backing layer forming coating liquid, or a cycle of supplying the backing layer forming coating liquid and then irradiating with active energy rays to harden the backing layer forming coating liquid may be performed two or more times.

[0062] When a decorative film is manufactured using a multicolor UV offset press equipped with an inline coater as the UV offset press, in step (3a) or (3b), it is preferable to mount a waterless lithographic printing plate obtained by processing a waterless lithographic printing plate precursor into a predetermined image pattern (e.g., a solid image pattern) on the rear cylinder (e.g., cylinder 5 to 7) of the multicolor UV offset press equipped with an inline coater, and to supply the above-mentioned backing layer forming coating liquid to the image portion of the waterless lithographic printing plate and transfer it onto the ink or picture layer via a blanket. Then, it is preferable to cure the backing layer forming coating liquid by UV irradiation using a UV lamp installed after the rear cylinder of the press.

[0063] When forming an adhesive layer on a backing layer, it is preferable to form the adhesive layer by supplying the above-mentioned adhesive layer material on the backing layer. Examples of the method for supplying the adhesive layer material include the methods exemplified as the method for supplying the coating liquid for forming the backing layer in step (3a) or (3b). EXAMPLES

[0064] The present invention will now be described in more detail with reference to examples. First, the materials used in the examples and comparative examples will be described.

[0065] <Preparation Example 1: Ink-1> Varnish-1 was obtained by mixing and dissolving 30 parts by mass of alkyd resin "Arakyd" (registered trademark) 3145-80 (manufactured by Arakawa Chemical Industries, Ltd.), 70.0 parts by mass of trimethylolpropane triacrylate ethylene oxide adduct "Miramer" (registered trademark) M3130 (manufactured by MIWON Co., Ltd.) as a compound having an ethylenically unsaturated bond, and 0.1 parts by mass of 4-methoxyphenol (manufactured by Tokyo Chemical Industry Co., Ltd.) as a polymerization inhibitor. This varnish-1 was mixed with the following components in the following ratios and kneaded using a three-roll mill to obtain ink-1. (a) Varnish-1: 40 parts by weight (b) Dipentaerythritol propionate triacrylate: 30 parts by mass (c) Titanium oxide "Tipake" (registered trademark) CR-50 (manufactured by Ishihara Sangyo Kaisha, Ltd.): 20 parts by mass (d) Alkylphenone-based photopolymerization initiator “Omnirad” (registered trademark) 907 (manufactured by IGM Resins BV): 5 parts by mass (e) Acylphosphine oxide photopolymerization initiator “Omnirad” TPO-L (manufactured by IGM Resins BV): 5 parts by mass.

[0066] <Preparation Example 2: Ink-2> Ink-2 was obtained in the same manner as in Preparation Example 1, except that varnish-2 in which the alkyd resin "Arakido" 3145-80 (manufactured by Arakawa Chemical Industries, Ltd.) was replaced with rosin-modified phenolic resin OR-581 (manufactured by Seiko PMC Co., Ltd.) was used.

[0067] <Preparation Example 3: Ink-3> Ink-3 was obtained in the same manner as in Preparation Example 1, except that varnish-3 in which the alkyd resin "Arakyd" 3145-80 (manufactured by Arakawa Chemical Industries, Ltd.) was replaced with diallyl phthalate resin "Daiso DAP" (registered trademark) (manufactured by Osaka Soda Co., Ltd.) was used.

[0068] <Preparation Example 4: Ink-4> Ink-4 was obtained in the same manner as in Preparation Example 1, except that varnish-4 in which the alkyd resin "Arakyd" 3145-80 (manufactured by Arakawa Chemical Industries, Ltd.) was replaced with acrylic resin "Beamset" (registered trademark) 700" (manufactured by Arakawa Chemical Industries, Ltd.) was used.

[0069] <Preparation Example 5: Ink-5> Varnish-4 obtained in Preparation Example 4 and the following components were mixed in the following ratios and kneaded using a three-roll mill to obtain Ink-5. (a) Varnish-4: 40 parts by weight (b) Dipentaerythritol propionate triacrylate: 20 parts by mass (c) Titanium oxide "Tipake" CR-50 (manufactured by Ishihara Sangyo Kaisha, Ltd.): 20 parts by weight (d) Alkylphenone photopolymerization initiator “Omnirad” 907 (manufactured by IGM Resins BV): 5 parts by mass (e) Acylphosphine oxide photopolymerization initiator “Omnirad” TPO-L (manufactured by IGM Resins BV): 5 parts by mass (f) Compound having a urethane bond: Aliphatic urethane acrylate “EBECRYL” (registered trademark) 4858 (manufactured by Daicel-Allnex Co., Ltd.): 10 parts by mass.

[0070] <Preparation Example 6: Ink-6> Ink-6 was obtained in the same manner as in Preparation Example 1, except that varnish-6 in which the alkyd resin "Arakido" 3145-80 (manufactured by Arakawa Chemical Industries, Ltd.) was replaced with styrene-acrylic resin MS-2225 (styrene residue: 30% by mass, manufactured by Seiko PMC Co., Ltd.) was used.

[0071] <Preparation Example 7: Ink-7> Ink-7 was obtained in the same manner as in Preparation Example 1, except that varnish-7 in which the alkyd resin "Arakido" 3145-80 (manufactured by Arakawa Chemical Industries, Ltd.) was replaced with styrene acrylic resin YS-1274 (styrene and α-methylstyrene residues: 50% by mass, manufactured by Seiko PMC Corporation) was used.

[0072] <Preparation Example 8: Ink-8> Ink-8 was prepared in the same manner as in Preparation Example 5, except that the varnish-4 obtained in Preparation Example 4 was changed to the varnish-7 obtained in Preparation Example 7.

[0073] <Preparation Example 9: Ink-9> Varnish 7 obtained in Preparation Example 7 and the following components were mixed in the following ratios and kneaded using a three-roll mill to obtain Ink 9. (a) Varnish-7: 40 parts by weight (b) Dipentaerythritol propionate triacrylate: 20 parts by mass (c) Titanium oxide "Tipake" CR-50 (manufactured by Ishihara Sangyo Kaisha, Ltd.): 20 parts by weight (d) Alkylphenone photopolymerization initiator “Omnirad” 907 (manufactured by IGM Resins BV): 5 parts by mass (e) Acylphosphine oxide photopolymerization initiator “Omnirad” TPO-L (manufactured by IGM Resins BV): 5 parts by mass (f) Compound having a urethane bond: polyurethane resin “Yuliano” (registered trademark) W600 (manufactured by Arakawa Chemical Industries, Ltd.): 10 parts by mass.

[0074] <Production Example 1: Waterless Planographic Printing Plate Precursor-1> Waterless lithographic printing plate precursor-1 was prepared by the following method.

[0075] The following heat insulating layer composition solution was applied onto a 0.24 mm thick degreased aluminum substrate (manufactured by Mitsubishi Aluminum Co., Ltd.) and dried at 200° C. for 90 seconds to provide a heat insulating layer with a thickness of 10.0 μm. The heat insulating layer composition solution was obtained by mixing the following components with stirring at room temperature.

[0076] [Thermal insulation layer composition solution] (i) Epoxy resin “jER” (registered trademark) 1010 (manufactured by Mitsubishi Chemical Corporation): 29.2 parts by mass (ii) Polyurethane "Sanprene" (registered trademark) LQ-T1331D (manufactured by Sanyo Chemical Industries, Ltd., solid content concentration: 20% by mass): 51.7 parts by mass (iii) Aluminum chelate ALCH-TR (Kawaken Fine Chemical Co., Ltd.): 4.5 parts by mass (iv) Leveling agent "Disparlon" (registered trademark) LC951 (manufactured by Kusumoto Chemicals Co., Ltd., solid content: 10% by mass): 0.1 parts by mass (v) Dispersion of titanium oxide "Tipake" (registered trademark) CR-50 (manufactured by Ishihara Sangyo Kaisha, Ltd.) in N,N-dimethylformamide (50% by mass of titanium oxide): 14.5 parts by mass (vi) N,N-dimethylformamide: 450 parts by mass (vii) Methyl ethyl ketone: 150 parts by mass.

[0077] Next, the following heat-sensitive layer composition solution was applied onto the heat insulating layer and dried by heating at 140° C. for 90 seconds to provide a heat-sensitive layer having a thickness of 1.5 μm. The heat-sensitive layer composition solution was obtained by mixing the following components by stirring at room temperature.

[0078] [Thermosensitive layer composition solution] (i) Infrared absorbing dye NK5559 (manufactured by Hayashibara Co., Ltd., maximum absorption wavelength: 774 nm): 12.0 parts by mass (ii) Phenol formaldehyde novolak resin "SUMILITE RESIN" (registered trademark) PR53195 (manufactured by Sumitomo Bakelite Co., Ltd.): 70.4 parts by mass (iii) Titanium-n-butoxide bis(acetylacetonate) “Nacem” (registered trademark) titanium (manufactured by Nippon Kagaku Sangyo Co., Ltd., concentration: 73% by mass, containing 27% by mass of n-butanol as a solvent): 17.6 parts by mass (iv) Tetrahydrofuran: 900 parts by mass.

[0079] Next, the following silicone layer composition solution, prepared immediately before coating, was coated on the heat-sensitive layer and heated at 140° C. for 80 seconds to provide a silicone layer with a thickness of 5 μm, thereby obtaining waterless lithographic printing plate precursor 1. The silicone layer composition solution was obtained by mixing the following components by stirring at room temperature.

[0080] [Silicone layer composition solution] (i) α,ω-divinylpolydimethylsiloxane: DMS-V35 (weight average molecular weight 49,500, manufactured by GELEST Inc.): 87.0 parts by mass (ii) Methylhydrogensiloxane-dimethylsiloxane copolymer RD-1 (manufactured by Dow Corning Toray Co., Ltd.): 4.2 parts by mass (iii) Vinyltris(methylethylketoxyimino)silane: 2.6 parts by mass (iv) Platinum catalyst SRX212 (manufactured by Dow Corning Toray Co., Ltd.): 6.2 parts by mass (v) “Isopar” (registered trademark) E (manufactured by Esso Chemical Co., Ltd.): 900 parts by mass.

[0081] <Production Examples 2 to 5: Waterless Planographic Printing Plate Precursors-2 to 5> Waterless lithographic printing plate precursor-2 to waterless lithographic printing plate precursor-5 were obtained in the same manner as in Production Example 1, except that the thickness of the silicone layer was changed as follows. Production Example 2: Waterless lithographic printing plate precursor-2: Silicone layer thickness 3 μm Production Example 3: Waterless lithographic printing plate precursor-3: Silicone layer thickness 10 μm Production Example 4: Waterless lithographic printing plate precursor-4: Silicone layer thickness 20 μm Production Example 5: Waterless lithographic printing plate precursor-5: Silicone layer thickness 50 μm.

[0082] <Production Example 6: Waterless planographic printing plate for forming a pattern layer> The waterless lithographic printing plate precursor-1 obtained in Production Example 1 was exposed to light using a CTP exposure machine PlateRite 8900N-E (manufactured by SCREEN Co., Ltd.) at an exposure energy of 125 mJ / cm 2 Exposure was performed under the condition of (drum rotation speed: 210 rpm). The exposed image was provided in the center of a lithographic printing plate precursor having a length of 550 mm and a width of 650 mm, with 10 fine lines each having a length of 100 mm and a line width of 200, 150, 100, 90, 80, 70, 60, 50, 40, 30, 20, and 10 μm spaced at 100 μm intervals, and a belt-shaped solid image having a length of 20 mm and a width of 650 mm was provided. The exposed waterless lithographic printing plate precursor-1 was passed through an automatic developing machine TWL-1160F (manufactured by Toray Industries, Inc.) at a speed of 40 cm / min, and the plate surface was pretreated with a pretreatment liquid DP-1 (manufactured by Toray Industries, Inc.), and then the plate surface was rubbed with a rotating brush while showering tap water to produce a waterless lithographic printing plate for forming a pattern layer. When the fine lines formed on the waterless lithographic printing plate for forming a design layer were observed using a 100x loupe, they were reproduced without breaks up to a line width of 20 μm. Therefore, the minimum line width and maximum line height of the design layer produced using the waterless lithographic printing plate for forming a design layer in each example were evaluated for fine lines with a line width of 20 μm or more.

[0083] <Production Examples 7 to 11: Waterless Planographic Printing Plates for Forming Backing Layer-1 to 5> The waterless lithographic printing plate precursors-1 to -5 obtained in Production Examples 1 to 5 were each exposed using a CTP exposure machine PlateRite 8900N-E (manufactured by SCREEN Co., Ltd.) with an exposure energy of 125 mJ / cm 2Exposure was performed under the condition of (drum rotation speed: 210 rpm). The exposed image was a solid image of 200 mm long x 400 mm wide in the center of a lithographic printing plate precursor of 550 mm long x 650 mm wide. The exposed plate was passed through an automatic developing machine TWL-1160F (manufactured by Toray Industries, Inc.) at a speed of 40 cm / min, and the plate surface was pretreated with a pretreatment liquid DP-1 (manufactured by Toray Industries, Inc.), and then the plate surface was rubbed with a rotating brush while showering tap water to produce waterless lithographic printing plates-1 to 5 for forming a backing layer as follows.

[0084] <Production Example 12: Gravure Cylinder> On the copper-plated cylinder, 10 thin lines each having a length of 100 mm and a line width of 300, 200, 100, 50, and 20 μm were engraved at 100 μm intervals, and a solid image in the shape of a strip having a length of 20 mm and a width of 650 mm was engraved using an electronic engraving machine for gravure cylinders, Vision 3 (manufactured by OHIO Co., Ltd.). After that, the cylinder was chrome-plated to increase the strength of the surface, and a gravure cylinder was manufactured. When the thin lines formed on the gravure cylinder were observed using a 100x magnifying glass, they were reproduced without breakage up to a line width of 200 μm. Therefore, the minimum line width and maximum line height of the pattern layer produced using the gravure cylinder in each comparative example were evaluated for thin lines having a line width of 200 μm or more.

[0085] Next, the evaluation methods used in the examples and comparative examples will be described.

[0086] (1) Measurement of minimum line width and maximum line height The decorative films obtained in each of the examples and comparative examples were embedded in resin, and then cross sections were prepared using the cross-section polisher method (CP method). Using a field emission scanning electron microscope (FE-SEM), the thinnest line width and the highest line height were measured for 10 randomly selected patterns under conditions of an acceleration voltage of 3.0 kV and a magnification of 5,000x. The minimum line width and maximum line height were determined as the minimum line width and maximum line height, respectively.

[0087] (2) Evaluation of concealment Of the decorative films obtained in each of the examples and comparative examples, 10 randomly selected locations in the solid image area measuring 200 mm in length x 400 mm in width where the backing layer of the decorative film is provided and not overlapping with the picture layer were measured for reflection density using a reflection spectrophotometer "SpectroEye" (registered trademark) (manufactured by X-rite Co., Ltd.) under the condition of a black color filter, and the average value was taken as the concealing property.

[0088] (3) Evaluation of formability Of the decorative films obtained in each of the Examples and Comparative Examples, the areas where the solid image areas of the picture layer and the backing layer overlap were punched out using a test specimen punching blade (dumbbell-shaped No. 4, JIS K 6251 (2017) compliant) to prepare test specimens.

[0089] Using a universal testing machine Autograph AGS-J 500N (Shimadzu Corporation) and a thermostatic chamber TCE-N300A (Shimadzu Corporation), the 150°C breaking point of the prepared test pieces was measured under the conditions of temperature: 150°C, chuck distance: 20 mm, and tensile speed: 200 mm / min. The measurement was performed three times for each decorative film, and the breaking elongation (%) was calculated using the following formula (α), and the average value was taken as the formability (%). Breaking elongation (%) = (breaking point (mm) - 20 (mm)) / 20 (mm) × 100 (α).

[0090] <Example 1> We prepared a 7-color UV offset printing press "LITHRONE" (registered trademark) GX40 advance (manufactured by Komori Corporation) equipped with an inline double coater, which has 7 cylinders capable of offset printing, two chamber coaters behind the 7th cylinder that allow for inline coating, and UV irradiation devices in two locations, between cylinders 4 and 5 and behind the coaters.

[0091] To form a picture layer, the waterless lithographic printing plate for forming a picture layer obtained in Production Example 6 was attached to the first plate cylinder, and Ink-1 obtained in Preparation Example 1 was placed in the ink fountain of the first cylinder. In addition, to form a backing layer, UV-curable screen ink UV FLX-972 black (manufactured by Teikoku Ink Mfg. Co., Ltd.) was placed in one chamber coater as a coating liquid for forming a backing layer.

[0092] Using the printing machine under the above conditions, polycarbonate film NF-2000 (Tg: 150°C, thickness: 300μm, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was cut into sheets of film measuring 467mm x 632mm, and ink-1 was printed on the film at a printing speed of 8,000 sheets per hour, followed by UV irradiation to form a pattern layer. Subsequently, a coating liquid for forming a backing layer was applied, and then a backing layer was formed by UV irradiation, producing a decorative film at a speed of 8,000 sheets per hour.

[0093] <Examples 2 to 9> A decorative film was produced in the same manner as in Example 1, except that the ink for forming the design layer was changed as shown in Table 1.

[0094] <Example 10> A decorative film was produced in the same manner as in Example 7, except that the polycarbonate film NF-2000 was changed to a polycarbonate film "DURABIO" (registered trademark) (Tg: 102°C, manufactured by Mitsubishi Chemical Corporation).

[0095] <Example 11> A decorative film was produced in the same manner as in Example 9, except that the polycarbonate film NF-2000 was changed to DURABIO.

[0096] <Example 12> A decorative film was produced in the same manner as in Example 9, except that the polycarbonate film NF-2000 was changed to a polyvinyl chloride film "Achilles Salaria" (registered trademark) (Tg: 80°C, manufactured by Achilles Corporation).

[0097] <Example 13> A decorative film was produced in the same manner as in Example 9, except that the polycarbonate film NF-2000 was changed to a polypropylene film P2111 (Tg: 0° C., manufactured by Toyobo Co., Ltd.).

[0098] <Example 14> A decorative film was produced in the same manner as in Example 13, except that the coating liquid for forming the backing layer was fed into two chamber coaters instead of one chamber coater, and the coating liquid for forming the backing layer was applied twice to form the backing layer.

[0099] <Example 15> The coating method of the coating liquid for forming the backing layer was changed from the chamber coater to the printing cylinder. The waterless lithographic printing plate-2 for forming the backing layer obtained in Production Example 8 was attached to each of the fifth and sixth plate cylinders, UV-curable screen ink UV FLX-972 was poured into each ink fountain, and the coating liquid for forming the backing layer was applied twice. Except for this, the decorative film was produced in the same manner as in Example 13.

[0100] <Example 16> A decorative film was produced in the same manner as in Example 15, except that the waterless lithographic printing plate-2 was changed to the waterless lithographic printing plate-1 for forming a backing layer obtained in Production Example 7.

[0101] <Example 17> A decorative film was produced in the same manner as in Example 15, except that the waterless lithographic printing plate-3 for forming a backing layer obtained in Production Example 9 was attached to the fifth plate cylinder, no printing plate was attached to the sixth plate cylinder, and the coating liquid for forming a backing layer was applied once.

[0102] <Example 18> A decorative film was produced in the same manner as in Example 15, except that the waterless lithographic printing plate-2 was changed to the waterless lithographic printing plate-3 for forming a backing layer obtained in Production Example 9.

[0103] <Example 19> A decorative film was produced in the same manner as in Example 15, except that the waterless lithographic printing plate-3 for forming a backing layer obtained in Production Example 9 was attached to each of the fifth, sixth, and seventh plate cylinders, and the coating liquid for forming a backing layer was applied three times.

[0104] <Examples 20 to 22> Decorative films were produced in the same manner as in Examples 17 to 19, except that the waterless lithographic printing plate-3 was changed to the waterless lithographic printing plate-4 for forming a backing layer obtained in Production Example 10.

[0105] <Examples 23 to 25> Decorative films were produced in the same manner as in Examples 17 to 19, except that the waterless lithographic printing plate-3 was changed to the waterless lithographic printing plate-5 for forming a backing layer obtained in Production Example 11.

[0106] <Comparative Example 1> The gravure cylinder obtained in Production Example 12 was attached to an FB type gravure printing machine (manufactured by Fuji Machine Industry Co., Ltd.), and continuous printing was performed on a polycarbonate film NF-2000 using gravure ink LSNT (manufactured by Toyo Ink Co., Ltd.) to form a pattern layer.

[0107] Furthermore, on the pattern layer, "Takelac" (registered trademark) A-626 / "Takenate" (registered trademark) A-65 (mixed at a mass ratio of 16 / 1, both manufactured by Mitsui Chemicals, Inc.) was applied as an adhesive by the bar coating method, and after drying at 80°C for 1 minute, the coating amount was 4.0 g / m 2 The adhesive layer was then formed so that the adhesive layer was as follows. Then, a black ABS film (thickness: 200 μm, manufactured by Towa Kako Co., Ltd.) was laminated onto the adhesive layer using a laminator MPK-600 to form a backing layer, and the decorative film was produced at a speed of about 10 sheets per hour. Since the backing layer was formed offline, the productivity was low.

[0108] <Comparative Example 2> In the same manner as in Comparative Example 1, a design layer was formed on the polycarbonate film NF-2000.

[0109] Furthermore, on the pattern layer, using a screen printing plate BS (manufactured by Asada Mesh Co., Ltd., mesh: 325, opening rate: 41%, mesh thickness: 60 μm), solvent screen ink HAS 911 black (manufactured by Teikoku Ink Mfg. Co., Ltd.) diluted to 30% by mass with G-002 solvent (manufactured by Teikoku Ink Mfg. Co., Ltd.) was supplied in the form of a solid image, and a backing layer was formed by drying at 80°C for 60 minutes, and a decorative film was produced at a speed of about 0.85 sheets per hour. Since the backing layer was formed offline, productivity was low.

[0110] The decorative films obtained in the respective Examples and Comparative Examples were evaluated by the above-mentioned methods, and the results are summarized in Tables 1 and 2.

[0111] [Table 1]

[0112] [Table 2] [Explanation of symbols]

[0113] 1. Film 2. Picture layer 2a Picture layer 2b Picture layer 2W Minimum line width 2H Maximum line height 3 Backing layer 4 Adhesive layer 100 Decorative Film 200 Decorative film with adhesive layer

Claims

1. A decorative film including a portion having at least a film, a design layer, and a backing layer in this order, the design layer and the backing layer both being active energy ray curable films.

2. 2. The decorative film according to claim 1, wherein the design layer comprises a rosin-modified resin, an allyl-based resin, and / or an acrylic-based resin.

3. The decorative film according to claim 2 , wherein the acrylic resin has a styrene group.

4. 3. The decorative film according to claim 1, wherein the design layer further comprises a compound having a urethane bond.

5. 3. The decorative film according to claim 1, wherein the backing layer has a thickness of 5 μm or more and 100 μm or less.

6. 2. A method for producing a decorative film according to claim 1, comprising the steps of: (1) applying ink to the surface of a printing plate and transferring the ink onto a film directly or via a blanket; and (3a) supplying a coating liquid for forming a backing layer onto the ink and irradiating the ink with active energy rays to harden the ink and the coating liquid for forming the backing layer, thereby forming a pattern layer and a backing layer.

7. 2. A method for producing a decorative film according to claim 1, comprising the steps of: (1) applying ink to the surface of a printing plate and transferring the ink onto a film, either directly or via a blanket; (2) irradiating active energy rays to harden the ink to form a pattern layer; and (3b) supplying a coating liquid for forming a backing layer onto the pattern layer, irradiating active energy rays to harden the coating liquid for forming the backing layer, thereby forming a backing layer.

8. The method for producing a decorative film according to claim 6 or 7, wherein the printing plate is a waterless planographic printing plate.

9. 8. The method for producing a decorative film according to claim 6 or 7, wherein in the step (3a) or (3b), the coating liquid for forming the backing layer is applied by a printing cylinder around which a lithographic printing plate having a silicone layer is wound.

10. The method for producing a decorative film according to claim 9, wherein the silicone layer has a thickness of 5 μm or more and 50 μm or less.

11. 8. The method for producing a decorative film according to claim 6 or 7, wherein in the step (3a) or (3b), the coating liquid for forming a backing layer is supplied onto the ink or design layer two or more times.

Citation Information

Patent Citations

  • Decoration sheet for insert molding and decoration resin molding

    JP2010082912A

  • Decorative film and decorative molded article

    JP2012201006A