Clad material for wire bonding, joint structure using the same, and battery manufacturing method

A cladding material with an Al layer and Fe layer addresses the weak bonding issue by preventing intermetallic compound formation, enhancing bonding strength and conductivity in battery structures.

JP2024168857APending Publication Date: 2024-12-05PROTERIAL LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023085876
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The formation of fragile intermetallic compounds at the joint between Al-based wires and copper phosphate or nickel-plated steel bus bars weakens the bonding strength in conventional battery structures.

Method used

A cladding material composed of an Al layer and an Fe layer, where the Al layer is 20 μm or more, is used to bond with the Al-based wire, preventing the formation of fragile intermetallic compounds and enhancing bonding strength by ensuring both layers are of the same metal type.

Benefits of technology

The bonding strength between the Al-based wire and the cladding material is significantly improved, with a bonding strength of 9.8N or more, and the material maintains high conductivity and resistance to deformation under load.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168857000001_ABST
    Figure 2024168857000001_ABST
Patent Text Reader

Abstract

To provide a clad material for wire bonding which enables improvement of joint strength when an Al-based wire is joined.SOLUTION: A clad material 1 for wire bonding comprises: an Al layer 1a formed of pure aluminum or aluminum alloy; and an Fe layer 1b joined to the Al layer 1a by rolling and formed of iron-based alloy. A thickness t2 of the Al layer 1a is 20 μm or larger. An Al-based wire 2 for joint is joined to the Al layer 1a by wire bonding.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a clad material for wire bonding, a joint structure using the clad material for wire bonding, and a method for manufacturing a battery. [Background technology]

[0002] 2. Description of the Related Art Conventionally, batteries having a structure in which the battery and a bus bar are joined by wire bonding are known (see Patent Document 1).

[0003] The above-mentioned Patent Document 1 discloses an assembled battery consisting of a plurality of unit cells. In Patent Document 1, a plurality of unit cells are arranged and adjacent unit cells are electrically connected by a bus bar (lead plate). In Patent Document 1, one end of an aluminum wire is bonded to an end of the unit cell by wire bonding, and the other end of the aluminum wire is bonded to the bus bar by wire bonding, thereby bonding the unit cell and the bus bar by wire bonding. In Patent Document 1, the bus bar is made of copper phosphate or nickel-plated steel sheet. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2010-282811 A Summary of the Invention [Problem to be solved by the invention]

[0005] In the above-mentioned Patent Document 1, since the Al-based wire made of aluminum used for wire bonding and the other member (bus bar) made of copper phosphate or nickel-plated steel sheet to which the wire is bonded are made of different metals, a brittle intermetallic compound may be formed at the bonding portion between the Al-based wire and the other member, which may weaken the bonding strength between the wire and the other article. Therefore, there is a demand for improving the bonding strength when bonding the Al-based wire.

[0006] The present invention has been made to solve the above-mentioned problems, and one object of the present invention is to provide a clad material for wire bonding that is capable of improving the bonding strength when an Al-based wire is bonded by wire bonding, a bonding structure using the clad material for wire bonding, and a method for manufacturing a battery. [Means for solving the problem]

[0007] In order to achieve the above object, the inventors of the present application have intensively studied the placement of a clad material between an aluminum wire and another member such as a bus bar, and have found the following configuration: A clad material for wire bonding according to a first aspect of the present invention is a clad material for wire bonding to which an Al-based wire for bonding is bonded by wire bonding, and is composed of an Al layer made of pure aluminum or an aluminum alloy, and an Fe layer made of an iron-based alloy and roll-bonded to the Al layer, the thickness of the Al layer being 20 μm or more, and the Al-based wire for bonding is bonded to the Al layer by wire bonding.

[0008] As described above, the clad material for wire bonding according to the first aspect of the present invention is composed of an Al layer made of pure aluminum or an aluminum alloy, and an Fe layer made of an iron-based alloy and roll-bonded to the Al layer, the thickness of the Al layer is 20 μm or more, and an Al-based wire for bonding is bonded to the Al layer by wire bonding. Since the Al layer and the Al-based wire are the same metal, it is possible to suppress the formation of a brittle intermetallic compound at the bonded portion between the Al-based wire and the Al layer when they are bonded by wire bonding. As a result, it is possible to improve the bonding strength when the Al-based wire is bonded to the clad material for wire bonding. It has also been found through experiments described below that the thickness of the Al layer is 20 μm or more, which improves the bonding strength when the Al-based wire is bonded to the Al layer of the clad material for wire bonding.

[0009] In the clad material for wire bonding according to the first aspect, the thickness of the Al layer is preferably 60 μm or less. With this configuration, even if a load is applied when bonding an Al-based wire to the clad material for wire bonding by wire bonding, the Al layer is largely deformed due to the large thickness of the Al layer, which is softer than the Fe layer, and it is possible to suppress the formation of a gap between the Al-based wire and the Al layer. By suppressing the formation of a gap between the Al-based wire and the Al layer, it is possible to apply a load while the Al-based wire and the Al layer are in reliable contact with each other, so that the bonding can be more firmly performed. In addition, it has been found by an experiment described later that the bonding strength when the Al-based wire is bonded to the Al layer can be sufficiently increased by setting the thickness of the Al layer to 60 μm or less.

[0010] In the wire bonding clad material according to the first aspect, the thickness of the Al layer is preferably smaller than the thickness of the Fe layer. With this configuration, the thickness of the Fe layer, which is harder than the Al layer, can be increased, so that the strength of the wire bonding clad material can be improved and deformation of the wire bonding clad material can be suppressed even when a load is applied when bonding an Al-based wire to the wire bonding clad material by wire bonding.

[0011] In the clad material for wire bonding according to the first aspect, the Fe layer is preferably made of ferritic stainless steel. With this configuration, the difference in hardness between the Fe layer and the Al layer can be reduced by using ferritic stainless steel, which is a stainless steel that is softer than other stainless steels. This allows the Fe layer to be stretched following the Al layer when the clad material for wire bonding is rolled, thereby suppressing the occurrence of thickness variations in the Fe layer.

[0012] In this case, the Fe layer is preferably made of SUS 430. By configuring in this way, the use of SUS 430, which is a versatile ferritic stainless steel with excellent workability, can improve the workability and productivity of the clad material for wire bonding.

[0013] In the wire bonding clad material according to the first aspect, the Al layer is preferably made of A1050. With this configuration, the use of A1050, which has high electrical conductivity, can improve the electrical conductivity of the wire bonding clad material. As a result, for example, when the wire bonding clad material is used between a unit cell and a bus bar that constitutes a battery pack, it is possible to suppress a decrease in electrical conductivity caused by the wire bonding clad material compared to when the unit cell and the bus bar are directly joined.

[0014] A bonding structure using a clad material for wire bonding according to a second aspect of the present invention includes an Al layer made of pure aluminum or an aluminum alloy, and an Fe layer made of an iron-based alloy and roll-bonded to the Al layer, the Al layer having a thickness of 20 μm or more, and a plate-shaped member made of pure aluminum or an aluminum alloy, in which one end of an Al-based wire for bonding is bonded to the Al layer by wire bonding, and the other end of the Al-based wire is bonded to the plate-shaped member.

[0015] The bonding structure using the clad material for wire bonding according to the second aspect of the present invention is composed of the clad material for wire bonding, which includes an Al layer made of pure aluminum or an aluminum alloy, and the thickness of the Al layer is 20 μm or more, and a plate-shaped member made of pure aluminum or an aluminum alloy, as described above. The plate-shaped member may be a bus bar or the like. Since the Al layer and the Al-based wire are the same metal, it is possible to suppress the formation of a brittle intermetallic compound at the bonding portion between the Al-based wire and the Al layer when they are bonded. As a result, it is possible to improve the bonding strength when the Al-based wire is bonded to the clad material for wire bonding. In addition, it has been found through an experiment described later that a bonding structure with high bonding strength can be obtained when the Al-based wire is bonded to the Al layer of the clad material for wire bonding by having a thickness of 20 μm or more.

[0016] In the bonding structure using the clad material for wire bonding according to the second aspect, the bonding strength between the Al-based wire and the Al layer is preferably 9.8 N or more. With this configuration, the bonding strength between the Al-based wire and the clad material for wire bonding can be made practically sufficient.

[0017] A battery manufacturing method according to a third aspect of the present invention includes the steps of: preparing a clad material for wire bonding by roll-bonding an Al plate material made of pure aluminum or an aluminum alloy and an Fe plate material made of an iron-based alloy, the clad material being composed of an Al layer and an Fe layer, the Al layer having a thickness of 20 μm or more; bonding a battery terminal member made of an iron-based alloy to the Fe layer; bonding one end of an Al-based wire for bonding to the Al layer by wire bonding; and bonding the other end of the Al-based wire to a bus bar made of pure aluminum or an aluminum alloy.

[0018] The method for manufacturing a battery according to the third aspect of the present invention includes the steps of preparing a clad material for wire bonding, in which the thickness of the Al layer is 20 μm or more, and bonding one end of an Al-based wire for bonding to the Al layer by wire bonding. Since the Al layer and the Al-based wire are the same metal, it is possible to suppress the formation of a brittle intermetallic compound at the bonding portion between the Al-based wire and the Al layer when they are bonded. As a result, it is possible to manufacture a clad material for wire bonding that can improve the bonding strength when the Al-based wire is bonded by wire bonding. It has also been found through experiments described below that the bonding strength between the Al-based wire and the Al layer of the clad material for wire bonding can be improved by having the Al layer have a thickness of 20 μm or more. Effect of the Invention

[0019] According to the present invention, it is possible to provide a clad material for wire bonding capable of improving the bonding strength when an Al-based wire is bonded by wire bonding, a bonding structure using the clad material for wire bonding, and a method for manufacturing a battery. [Brief description of the drawings]

[0020] [Figure 1] 1A and 1B are diagrams showing a battery pack according to the present embodiment, in which FIG. 1A is a perspective view and FIG. 1B is a cross-sectional view. [Diagram 2] 1 is a diagram showing an example of a clad material for wire bonding according to an embodiment of the present invention; [Diagram 3] 1 is a diagram showing a state in which a clad material for wire bonding according to the present embodiment and a bus bar are bonded together by an Al-based wire. FIG. [Figure 4] FIG. 2 is a diagram showing an example of a unit cell according to the present embodiment. [Diagram 5] 1A to 1C are diagrams illustrating a method for manufacturing a clad material for wire bonding according to the present embodiment. [Figure 6] 1A to 1C are diagrams for explaining a method of joining the clad material for wire bonding according to the present embodiment to a battery terminal. [Figure 7] 1 is a diagram showing a laser irradiation position when the clad material for wire bonding according to the present embodiment is laser-welded to a battery terminal. FIG. [Figure 8] 1A to 1C are diagrams for explaining a wire bonding method according to an embodiment of the present invention. [Figure 9] 1 is a graph showing the bonding strength of SUS430 wire-bonded with an Al-based wire and a clad material for wire bonding. [Figure 10] 1 is a graph showing the results of a thermal shock test of SUS430 wire-bonded with an Al-based wire and a clad material for wire bonding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0022] As shown in FIG. 1, a clad material for wire bonding 1 according to an embodiment of the present invention is used in a battery pack 100. The battery pack 100 is configured by electrically connecting a plurality of lithium ion secondary batteries 10 via a bus bar 20. Note that, although the battery pack 100 is illustrated in a simplified manner in FIG. 1, the number of lithium ion secondary batteries 10 constituting the battery pack 100 for vehicle use or the like is greater than the number illustrated in FIG. 1. The battery pack 100 for vehicle use is a large battery system mounted on an electric vehicle (EV) or a hybrid electric vehicle (HEV). Note that the battery pack 100 is an example of a "battery" as defined in the claims. Also, the bus bar 20 is an example of a "plate-shaped member" as defined in the claims.

[0023] As shown in Fig. 2, the clad material for wire bonding 1 is composed of an Al layer 1a and an Fe layer 1b. In Fig. 2, the clad material for wire bonding 1 has a circular shape, but the shape of the clad material for wire bonding 1 is not limited to this.

[0024] The Al layer 1a is made of pure aluminum or an aluminum alloy. The pure aluminum has an aluminum content of 99% or more and 100% or less, such as the A1000 series of JIS standards including A1050. The aluminum alloy is an alloy in which other elements such as Mn or Mg are added to Al, such as the A3000 series of JIS standards including A3003 and the A5000 series of JIS standards including A5052.

[0025] The Fe layer 1b is made of an iron-based alloy. The iron-based alloy is an alloy in which Fe is the largest among the constituent metal elements. Among the iron-based alloys, those containing about 10 mass% or more of Cr are called stainless steel. The iron-based alloy constituting the Fe layer 1b is preferably a stainless steel that is an iron-based alloy containing 10 mass% or more of Cr from the viewpoint of durability. Moreover, the iron-based alloy constituting the Fe layer 1b is preferably a ferritic stainless steel that is a stainless steel that does not contain Ni in order to reduce the difference in hardness with the Al layer 1a. The ferritic stainless steel is a stainless steel that contains 16 mass% to 18 mass% of Cr and has a main metal structure at room temperature that is a ferrite phase with a body-centered cubic lattice structure, such as SUS430.

[0026] The total thickness t1 of the clad material for wire bonding 1 is 200 μm or more and 400 μm or less. The thickness t2 of the Al layer 1a is 20 μm or more. From the viewpoint of improving the bonding strength with the Al-based wire 2 by wire bonding, the thickness t2 of the Al layer 1a is preferably 60 μm or less. From the viewpoint of improving the strength of the clad material for wire bonding 1, the thickness t2 of the Al layer 1a is preferably smaller than the thickness t3 of the Fe layer 1b.

[0027] 3, one end of an Al-based wire 2 for bonding is bonded to the Al layer 1a by wire bonding. The other end of the Al-based wire 2 for bonding is bonded to the bus bar 20 by wire bonding. The Al-based wire 2 is made of pure aluminum or an aluminum alloy.

[0028] A terminal (negative electrode terminal or positive electrode terminal) of the lithium ion secondary battery 10 is joined to the Fe layer 1b. The joining method is, for example, laser welding. In the case of laser welding, the joining is performed, for example, by irradiating a laser from the Al layer 1a side.

[0029] (Lithium-ion secondary battery) 4, lithium ion secondary battery 10 includes cylindrical housing 11, a cover member 12 that seals an opening of housing 11, and an electricity storage element 13 disposed within housing 11. Housing 11 is made of Ni-plated steel sheet, and also serves as the negative terminal of lithium ion secondary battery 10.

[0030] The housing 11 contains an electricity storage element 13 and an electrolyte (not shown). The cover member 12 is made of an iron-based alloy and also serves as the positive electrode terminal of the lithium-ion secondary battery 10. The electricity storage element 13 is formed by winding a positive electrode 14, a negative electrode 15, and an insulating separator 16 disposed between the positive electrode 14 and the negative electrode 15. The positive electrode 14 includes a positive electrode current collector (not shown) made of aluminum foil, and a positive electrode active material layer (not shown) disposed on the surface of the positive electrode current collector. The positive electrode active material layer has a positive electrode active material such as lithium manganate, and a binder made of a resin material.

[0031] The lithium ion secondary battery 10 further includes a positive electrode lead material 17 for connecting the positive electrode 14 and the positive electrode terminal (lid material 12), and a negative electrode lead material 18 for connecting the negative electrode 15 and the negative electrode terminal (casing 11). The positive electrode lead material 17 is made of aluminum foil, and is joined to the positive electrode current collector of the positive electrode 14 and the lid material 12 by resistance welding or the like. The negative electrode lead material 18 is made of copper foil, and is joined to the negative electrode current collector of the negative electrode 15 and the casing 11 by resistance welding or the like.

[0032] As shown in FIG. 1, the busbar 20 is made of pure aluminum or an aluminum alloy. In general, a busbar electrically connects the terminals (negative electrode terminal, positive electrode terminal) of a plurality of unit cells. In this embodiment, the busbar 20 electrically connects the positive electrode terminals of a plurality of unit cells (lithium ion secondary batteries 10). In this embodiment, the clad material 1 for wire bonding is disposed between the busbar 20 and the positive electrode terminal of the lithium ion secondary battery 10. As shown in FIG. 1, the busbar 20 has a plate-like shape.

[0033] As shown in FIG. 1, a recess 20a is provided on the X1 side of the busbar 20. Although FIG. 1 shows an example in which the recess 20a is provided on one side (X1 side) in the short side direction, the recess 20a may be provided on one side and the other side (X1 side and X2 side) in the short side direction. An end of an Al-based wire 2 is bonded to the recess 20a by wire bonding. A single busbar 20 can simultaneously connect a plurality of terminals. Although not shown in FIG. 1, negative electrode terminals are also connected to each other by another busbar. The negative electrode terminals and the other busbar are joined by laser welding, spot welding, or the like. In addition, the battery pack 100 shown in FIG. 1 is intended to show a configuration example of a portion where positive electrode terminals are connected to each other by the busbar 20, and configurations of other connection portions are omitted. In addition, the battery pack may be configured to join the positive electrode terminal and the negative electrode terminal by a busbar. The battery pack may also have a configuration in which the positive electrode terminals are connected to each other by a bus bar and the negative electrode terminals are connected to each other by a bus bar, and a configuration in which the positive electrode terminals and the negative electrode terminals are joined by a bus bar.

[0034] (Battery manufacturing method) As shown in FIG. 5, a clad material 1 for wire bonding is prepared by rolling-bonding an Al sheet material 50a and an Fe sheet material 50b, the clad material 1 being composed of an Al layer 1a and an Fe layer 1b, and the thickness of the Al layer 1a is 20 μm or more. The Al sheet material 50a is a sheet material composed of the same pure aluminum or aluminum alloy as the Al layer 1a. The Fe sheet material 50b is a sheet material composed of the same iron-based alloy as the Fe layer 1b. In the roll-bonding, the rolling ratio (degree of processing) is set so that the thicknesses of the Al sheet material 50a and the Fe sheet material 50b before rolling are the same as the thicknesses of the Al layer 1a and the Fe layer 1b after rolling. Although not shown in FIG. 5, diffusion annealing may be performed after the roll-bonding of the Al sheet material 50a and the Fe sheet material 50b. In addition, softening annealing may be performed before the roll-bonding of the Al sheet material 50a and the Fe sheet material 50b. In addition, after the Al sheet material 50a and the Fe sheet material 50b are roll-bonded, further rolling may be performed to obtain a desired thickness for the Al layer 1a and a desired thickness for the Fe layer 1b. In addition, softening annealing may be performed before further rolling. The produced clad material for wire bonding 1 is then processed into, for example, a circular shape. The method of processing into a circular shape may be performed by punching the clad material for wire bonding 1. The diameter of the clad material for wire bonding 1 formed into a circular shape is set to be suitable for the diameter of the terminal to be bonded.

[0035] When constructing the battery pack 100 shown in FIG. 1, the Fe layer 1b of the wire bonding clad material 1 is joined to the battery terminal member as shown in FIG. 6. In FIG. 6, the battery terminal member is a cover material 12 (positive terminal). Depending on the configuration of the battery pack, the negative terminal (outer bottom surface of the housing 11) can also be joined to the Fe layer 1b of the wire bonding clad material 1. A method for joining the Fe layer 1b of the wire bonding clad material 1 to the battery terminal member is, for example, laser welding. In the case of laser welding, the laser irradiation unit 40 is disposed on the Al layer 1a side and laser irradiation is performed. For example, the laser is irradiated so as to form a circular locus along the outer periphery of the circular wire bonding clad material 1 as shown by the dashed line in FIG. 7.

[0036] After the Fe layer 1b of the wire bonding clad material 1 is joined to the battery terminal member by laser welding or the like, the Al layer 1a of the wire bonding clad material 1 is joined to the bus bar 20. The method of joining the Al layer 1a of the wire bonding clad material 1 to the bus bar 20 is as follows, as shown in Fig. 8, in which one end of an Al-based wire 2 for bonding is joined to the Al layer 1a by wire bonding, and the other end of the Al-based wire 2 is joined to the recess 20a of the bus bar 20 by wire bonding.

[0037] Wire bonding can be performed in two ways: one in which one end and the other end of the Al-based wire 2 are melted to form a ball-shaped joint, and the other in which a ball-shaped joint is not formed. In addition, the methods of bonding one end and the other end of the Al-based wire 2 to the Al layer 1a and the bus bar 20, respectively, include a method using heat, a method using pressure, a method using ultrasonic waves, or a method using a suitable combination of heat, pressure, ultrasonic waves, and the like. When ultrasonic waves are used, for example, one end of the wire is pressed against the Al layer 1a of the wire bonding clad material 1 by the tool 50, ultrasonic vibration is applied to generate heat inside, and the one end of the wire and the vicinity of the surface of the Al layer 1a are melted and bonded. This forms a joint structure consisting of the wire bonding clad material 1 and the bus bar 20. At this time, the bonding strength between the Al-based wire 2 and the Al layer 1a of the wire bonding clad material 1 is preferably 9.8 N or more.

[0038] <Effects of this embodiment> In this embodiment, the following effects can be obtained.

[0039] In this embodiment, the wire bonding clad material 1 is composed of an Al layer 1a made of pure aluminum or an aluminum alloy, and an Fe layer 1b made of an iron-based alloy and roll-bonded to the Al layer 1a. The thickness t2 of the Al layer 1a is 20 μm or more, and an Al-based wire 2 for bonding is bonded to the Al layer 1a by wire bonding. Since the Al layer 1a and the Al-based wire 2 are the same metal, it is possible to suppress the formation of a brittle intermetallic compound at the bonded portion between the Al-based wire 2 and the Al layer 1a when they are bonded by wire bonding. As a result, it is possible to improve the bonding strength when the Al-based wire 2 is bonded to the wire bonding clad material 1. It has been found through an experiment described later that the thickness t2 of the Al layer 1a is 20 μm or more, which improves the bonding strength when the Al-based wire 2 is bonded to the Al layer 1a of the wire bonding clad material 1.

[0040] In addition, in this embodiment, the thickness of the Al layer 1a is 60 μm or less. As a result, even if a load is applied when bonding the Al-based wire 2 to the wire bonding clad material 1 by wire bonding, the Al layer 1a is largely deformed due to the large thickness of the Al layer 1a, which is softer than the Fe layer 1b, and the formation of a gap between the Al-based wire 2 and the Al layer 1a can be suppressed. Since the formation of a gap between the Al-based wire 2 and the Al layer 1a is suppressed, a load can be applied in a state where the Al-based wire 2 and the Al layer 1a are in reliable contact with each other, and therefore the bonding can be more firmly performed. In addition, it has been found through an experiment described later that the bonding strength when the Al-based wire 2 is bonded to the Al layer 1a can be sufficiently increased by setting the thickness of the Al layer 1a to 60 μm or less.

[0041] In this embodiment, the thickness t2 of the Al layer 1a is smaller than the thickness t3 of the Fe layer 1b. This allows the thickness of the Fe layer 1b, which is harder than the Al layer 1a, to be increased, thereby improving the strength of the clad material for wire bonding 1 and suppressing deformation of the clad material for wire bonding 1 even when a load is applied when joining the Al-based wire 2 to the clad material for wire bonding 1 by wire bonding.

[0042] In this embodiment, the Fe layer 1b is made of ferritic stainless steel. By using ferritic stainless steel, which is a stainless steel that is softer than other stainless steels, the difference in hardness between the Fe layer 1b and the Al layer 1a can be reduced. This allows the Fe layer 1b to be stretched following the Al layer 1a when the wire bonding clad material 1 is rolled, thereby suppressing the occurrence of thickness variations in the Fe layer 1b.

[0043] In addition, in this embodiment, the Fe layer 1b is made of SUS 430. By using SUS 430, which is a versatile ferritic stainless steel with excellent workability, the workability and productivity of the clad material for wire bonding 1 can be improved.

[0044] In this embodiment, the Al layer 1a is made of A1050. By using A1050, which has high electrical conductivity, the electrical conductivity of the wire bonding clad material 1 can be improved. As a result, when the wire bonding clad material 1 is used between the unit cells and the bus bar 20 constituting the battery pack 100, for example, it is possible to suppress a decrease in electrical conductivity caused by the wire bonding clad material 1 compared to a case where the unit cells and the bus bar 20 are directly bonded to each other.

[0045] In addition, the bonding structure using the clad material for wire bonding 1 of this embodiment includes the clad material for wire bonding 1 including the Al layer 1a made of pure aluminum or an aluminum alloy, and the thickness t2 of the Al layer 1a is 20 μm or more, as described above, and the bus bar 20 made of pure aluminum or an aluminum alloy. As a result, since the Al layer 1a and the Al-based wire 2 are the same type of metal, it is possible to suppress the formation of a brittle intermetallic compound at the bonding portion between the Al-based wire 2 and the Al layer 1a when they are bonded. As a result, it is possible to improve the bonding strength when the Al-based wire 2 is bonded to the clad material for wire bonding 1. In addition, it has been found through an experiment described later that, since the thickness of the Al layer 1a is 20 μm or more, a bonding structure with high bonding strength can be obtained when the Al-based wire 2 is bonded to the Al layer 1a of the clad material for wire bonding 1.

[0046] In this embodiment, the bonding strength between the Al-based wire 2 and the Al layer 1a is 9.8 N or more. This makes it possible to sufficiently increase the bonding strength between the Al-based wire 2 and the clad material for wire bonding 1.

[0047] In addition, the manufacturing method of the battery of this embodiment includes the steps of preparing the clad material 1 for wire bonding, in which the thickness of the Al layer 1a is 20 μm or more, and bonding one end of the Al-based wire 2 for bonding to the Al layer 1a by wire bonding. Since the Al layer 1a and the Al-based wire 2 are the same metal, it is possible to suppress the formation of a brittle intermetallic compound at the bonding portion between the Al-based wire 2 and the Al layer 1a when they are bonded. As a result, it is possible to manufacture the clad material 1 for wire bonding, which can improve the bonding strength when the Al-based wire 2 is bonded by wire bonding. In addition, it has been found by an experiment described later that the bonding strength between the Al-based wire 2 and the Al layer 1a of the clad material for wire bonding 1 can be improved by the thickness of the Al layer 1a being 20 μm or more.

[0048] [Example] An experiment (Example) in which the bonding strength between the Al-based wire 2 and the Al layer 1a of the wire bonding clad material 1 was measured by changing the thickness of the Al layer 1a will be described.

[0049] A plate material made of SUS430 and a SUS430 single plate having a plate thickness of 300 μm was prepared as a bonded material of Comparative Example 1 in which the thickness of the Al layer 1a to which the Al-based wire 2 is bonded by wire bonding is 0 μm. In addition, a wire bonding clad material 1 composed of an Al layer 1a made of A1050 and an Fe layer 1b made of SUS430 and having a total thickness of 300 μm was prepared as a bonded material of Examples 1 to 5 and Comparative Example 2 in which the thickness of the Al layer 1a exceeds 0 μm. The bonded materials of Examples 1 to 5 and Comparative Example 2 are wire bonding clad materials 1 having different ratios (layer thickness ratios) of the thickness of the Al layer 1a to the thickness of the Fe layer 1b, and the thicknesses of the Al layers 1a were 10 μm (Comparative Example 2), 20 μm (Example 1), 40 μm (Example 2), 60 μm (Example 3), 90 μm (Example 4), and 140 μm (Example 5).

[0050] The Al layer 1a of the clad material 1 for wire bonding in Examples 1 to 5 and Comparative Example 2 was bonded to one end of the Al-based wire 2 by wire bonding to prepare a bonded structure. Also, the SUS430 single plate in Comparative Example 1 was bonded to one end of the Al-based wire 2 by wire bonding to prepare a bonded structure. The wire bonding was performed by using an Al-based wire 2 having a diameter of 300 μm, pressing one end of the Al-based wire 2 with a tool 50 to apply a load of 2 N, 3 N or 4 N, and oscillating ultrasonic waves with an output of 2 W for 100 ms (milliseconds) to bond the materials to be bonded. Note that, before wire bonding, the bonded surfaces of the bonded materials in Examples 1 to 5 and Comparative Example 1 and Comparative Example 2 were polished to a mirror finish.

[0051] A wire bond strength evaluation test was performed on each of the joint structures of Examples 1 to 5 and Comparative Example 1 and Comparative Example 2. A shear test was used for the wire bond strength evaluation test. Specifically, in accordance with JIS Z3198-7 (2003) "Lead-free solder test method - Part 7: Shear test method for solder joints of chip components", a shear jig was applied to the Al-based wire 2, and the shear jig was moved at a speed of 5 mm / min to 30 mm / min to measure the maximum shear load. In addition, the clearance (gap) between the shear jig and the Al layer 1a of Examples 1 to 5 and Comparative Example 2 was set to 3 μm. Similarly, the clearance (gap) between the shear jig and the SUS single plate of Comparative Example 1 was set to 3 μm. In addition, for Examples 1 to 5, Comparative Example 1 and Comparative Example 2, multiple test specimens were prepared for the wire bond strength evaluation test, and the average value of the maximum shear load was calculated to be the average bond strength. The results of the wire bond strength evaluation test are shown in Table 1 and FIG. 9. In Fig. 9, the average bonding strength is plotted as bonding strength on the vertical axis, and the thickness of the Al layer 1a is plotted on the horizontal axis. Also, in Fig. 9, the bonding strength of the SUS single plate of Comparative Example 1 is plotted at the position where the thickness of the Al layer 1a is 0 μm.

[0052] [Table 1] TIFF2024168857000002.tif173156

[0053] As shown in Table 1, when wire bonding was performed with a load of 2N using the SUS430 single plate of Comparative Example 1 (thickness t2 of Al layer 1a shown in FIG. 2 is 0 μm) as the joined material, the average bond strength of the bonded structure was 5.8N. When wire bonding was performed with a load of 3N, it was 8.2N. When wire bonding was performed with a load of 4N, it was 8.3N.

[0054] When wire bonding was performed with a load of 2N using the clad material for wire bonding 1 of Comparative Example 2 having an Al layer 1a with a thickness t2 of 10 μm as the bonded material, the average bond strength of the bonded structure was 9.7N. When wire bonding was performed with a load of 3N, the average bond strength was 8.9N. When wire bonding was performed with a load of 4N, the average bond strength was 7.9N.

[0055] When wire bonding was performed with a load of 2N using the clad material for wire bonding 1 of Example 1 having an Al layer 1a with a thickness t2 of 20 μm as the bonded material, the average bond strength of the bonded structure was 10.3N. When wire bonding was performed with a load of 3N, the average bond strength was 10.6N. When wire bonding was performed with a load of 4N, the average bond strength was 11.3N.

[0056] When wire bonding was performed with a load of 2N using the clad material for wire bonding 1 of Example 2 having an Al layer 1a with a thickness t2 of 40 μm as the bonded material, the average bond strength of the bonded structure was 10.2N. When wire bonding was performed with a load of 3N, the average bond strength was 10.9N. When wire bonding was performed with a load of 4N, the average bond strength was 11.2N.

[0057] When wire bonding was performed with a load of 2N using the clad material for wire bonding 1 of Example 3 having an Al layer 1a with a thickness t2 of 60 μm as the bonded material, the average bond strength of the bonded structure was 10.6N. When wire bonding was performed with a load of 3N, the average bond strength was 11.7N. When wire bonding was performed with a load of 4N, the average bond strength was 11.3N.

[0058] When wire bonding was performed with a load of 2N using the clad material for wire bonding 1 of Example 4 having an Al layer 1a with a thickness t2 of 90 μm as the bonded material, the average bond strength of the bonded structure was 7.8N. When wire bonding was performed with a load of 3N, the average bond strength was 9.8N. When wire bonding was performed with a load of 4N, the average bond strength was 9.6N.

[0059] When wire bonding was performed with a load of 2N using the clad material for wire bonding 1 of Example 5 having an Al layer 1a with a thickness t2 of 140 μm as the bonded material, the average bond strength of the bonded structure was 9.0N. When wire bonding was performed with a load of 3N, the average bond strength was 9.1N. When wire bonding was performed with a load of 4N, the average bond strength was 10.0N.

[0060] From the above results, the inventors of the present application found that in the bonded structures using the clad materials for wire bonding 1 of Examples 1 to 5 in which the thickness t2 (see FIG. 2) of the Al layer 1a is 20 μm or more as the bonded material, the bond strength (average bond strength) between the bonded material and the Al wire 2 is improved compared to the bonded structure using the SUS430 single plate of Comparative Example 1 as the bonded material, that is, the bonded structure in which the Al wire 2 is directly bonded to the SUS430 single plate by wire bonding. In particular, in the bonded structure using the bonded material in which the thickness t2 of the Al layer 1a is in the range of 20 μm or more and 60 μm or less as the bonded material, the average bond strength of the bonded structure was 9.8 N or more when the load during wire bonding was 4 N or less, that is, in all cases of 2N, 3N, and 4N. From this, the inventors of the present application found that using a clad material for wire bonding 1 having an Al layer 1a with a thickness t2 of 20 μm or more and 60 μm or less as the joined material is preferable because it provides a sufficiently large bond strength between the joined material and the Al-based wire 2. In addition, as shown in the graph of Fig. 9, the inventors found that the bond strength (average bond strength) is highest when the thickness t2 of the Al layer 1a is 60 μm.

[0061] Next, a thermal shock test was performed on each of the bonded structures in the case of wire bonding under a load of 3N for Examples 1 to 5 and Comparative Example 1 and Comparative Example 2. The thermal shock test was performed 1000 cycles, with one cycle consisting of a combination of a high-temperature holding part at 80°C for 20 minutes and a low-temperature holding part at -40°C for 20 minutes, in accordance with ISO 16750-4 (environmental testing of electrical and electronic equipment for automobiles - mechanical load). In addition, for Examples 1 to 5 and Comparative Example 1 and Comparative Example 2, a plurality of test specimens were prepared for the thermal shock test, and the average value of the maximum shear load was calculated as described above, and used as the average bond strength. The results of the thermal shock test are shown in Table 2 and FIG. 10. In FIG. 10, the average bond strength is plotted as the bond strength on the vertical axis, and the thickness of the Al layer 1a is plotted on the horizontal axis. In addition, in FIG. 10, the bond strength of the SUS single plate of Comparative Example 1 is plotted at the position where the thickness of the Al layer 1a is 0 μm.

[0062] [Table 2] TIFF2024168857000003.tif124158

[0063] As shown in Table 2, when the SUS430 single plate of Comparative Example 1 (where the thickness t2 of the Al layer 1a shown in Figure 2 is 0 μm) was used as the material to be joined, the average joining strength before the thermal shock test (when the number of cycles was 0) was 8.2 N, but after the thermal shock test (when the number of cycles was 1000) it was 10.6 N.

[0064] In addition, when the wire bonding clad material 1 in Comparative Example 2 having an Al layer 1a with a thickness t2 of 10 μm was used as the material to be joined, the average bonding strength before the thermal shock test (when the number of cycles was 0) was 8.9 N, but after the thermal shock test (when the number of cycles was 1000) it was 8.8 N.

[0065] In addition, when the wire bonding clad material 1 in Example 1 having an Al layer 1a with a thickness t2 of 20 μm was used as the material to be joined, the average bonding strength before the thermal shock test (when the number of cycles was 0) was 10.6 N, but after the thermal shock test (when the number of cycles was 1000) it was 13.8 N.

[0066] In addition, when the wire bonding clad material 1 in Example 2 having an Al layer 1a with a thickness t2 of 40 μm was used as the material to be joined, the average bonding strength before the thermal shock test (when the number of cycles was 0) was 10.9 N, but after the thermal shock test (when the number of cycles was 1000) it was 13.5 N.

[0067] In addition, when the wire bonding clad material 1 in Example 3 having an Al layer 1a with a thickness t2 of 60 μm was used as the material to be joined, the average joining strength was 11.7 N before the thermal shock test (when the number of cycles was 0), but was 13.5 N after the thermal shock test (when the number of cycles was 1000).

[0068] In addition, when the wire bonding clad material 1 in Example 4 having an Al layer 1a with a thickness t2 of 90 μm was used as the material to be joined, the average bonding strength before the thermal shock test (when the number of cycles was 0) was 9.8 N, but after the thermal shock test (when the number of cycles was 1000) it was 11.7 N.

[0069] In addition, when the wire bonding clad material 1 in Example 5 having an Al layer 1a with a thickness t2 of 140 μm was used as the material to be joined, the average bonding strength before the thermal shock test (when the number of cycles was 0) was 9.1 N, but after the thermal shock test (when the number of cycles was 1000) it was 11.7 N.

[0070] From the above results, the inventors of the present application found that when the wire bonding clad material 1 in which the thickness t2 of the Al layer 1a in Examples 1 to 5 is 20 μm or more is used as the joined material, the average bonding strength of the joined structure after the thermal shock test is improved compared to when the SUS430 single plate in Comparative Example 1 (the thickness t2 of the Al layer 1a is 0 μm) is used as the joined material, that is, the joined structure in which the Al-based wire 2 is directly bonded to the SUS430 single plate by wire bonding. In particular, when the thickness t2 of the Al layer 1a is within the range of 20 μm or more and 60 μm or less, the average bonding strength after the thermal shock test is 13.5 N or more, so the bonding strength of the joined structure is sufficiently large. As a result, the inventors of the present application have discovered that a bonding structure using a wire bonding clad material 1 as the bonded material, in which the thickness t2 of the Al layer 1a is 20 μm or more (preferably, the thickness t2 of the Al layer 1a is in the range of 20 μm or more and 60 μm or less), maintains its bonding strength even when repeatedly subjected to thermal shock due to the passage of a large current, etc.

[0071] [Variations] The embodiments and examples disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is indicated by the claims, not by the description of the embodiments and examples described above, and further includes all modifications (variations) within the meaning and scope of the claims.

[0072] For example, in the present embodiment, a configuration example in which the clad material for wire bonding 1 is used in the assembled battery 100 has been shown, but the present invention is not limited to this. In the present invention, for example, the clad material for wire bonding 1 may be used in other than the assembled battery 100, and may be used in, for example, electric / electronic circuit boards for in-vehicle use, etc.

[0073] In the present embodiment, the clad material for wire bonding 1 and the cover material 12, which is the positive electrode terminal of the lithium ion secondary battery 10, are laser welded to each other, and the clad material for wire bonding 1 and the bus bar 20 are joined by wire bonding using the Al-based wire 2. However, the present invention is not limited to this. For example, the clad material for wire bonding 1 and the housing 11, which is the negative electrode terminal of the lithium ion secondary battery 10, may be laser welded to each other, and the clad material for wire bonding 1 and the bus bar 20 may be joined by wire bonding using the Al-based wire 2. For example, the clad material for wire bonding 1 may be laser welded to the terminal (positive electrode terminal) of one battery, and another clad material for wire bonding 1 may be laser welded to the terminal (positive electrode terminal) of the other battery, and the Al layers 1a of the clad materials for wire bonding 1 and the other clad materials for wire bonding 1 may be joined by wire bonding using the Al-based wire 2.

[0074] In the present embodiment, the clad material 1 for wire bonding has a configuration example in which the thickness t2 of the Al layer 1a is smaller than the thickness t3 of the Fe layer 1b shown in Fig. 2, but the present invention is not limited to this. In the present invention, the clad material 1 for wire bonding may have a thickness t2 of the Al layer 1a that is equal to or larger than the thickness t3 of the Fe layer 1b, for example.

[0075] In the present embodiment, the clad material for wire bonding 1 is used in a cylindrical lithium ion secondary battery 10 as shown in Fig. 4, but the present invention is not limited to this. In the present invention, the clad material for wire bonding 1 may be used in a prismatic lithium ion secondary battery 10. [Explanation of symbols]

[0076] 1 Cladding material for wire bonding 1a Al layer 1b Fe layer 2. Aluminum Wire 10 Lithium-ion secondary battery 11 Housing (negative terminal) 12 Lid material (positive terminal) 20 Bus bar (plate-shaped member)

Claims

1. A clad material for wire bonding to which an Al-based wire for bonding is bonded by wire bonding, An Al layer made of pure aluminum or an aluminum alloy; an Fe layer made of an iron-based alloy and roll-bonded to the Al layer; The thickness of the Al layer is 20 μm or more, The clad material for wire bonding, in which an Al-based wire for bonding is bonded to the Al layer by wire bonding.

2. 2. The clad material for wire bonding according to claim 1, wherein the thickness of the Al layer is 60 μm or less.

3. The clad material for wire bonding according to claim 1 , wherein the thickness of the Al layer is smaller than the thickness of the Fe layer.

4. 2. The clad material for wire bonding according to claim 1, wherein the Fe layer is made of ferritic stainless steel.

5. 5. The clad material for wire bonding according to claim 4, wherein the Fe layer is made of SUS430.

6. The clad material for wire bonding according to claim 5 , wherein the Al layer is made of A1050.

7. A clad material for wire bonding, comprising: an Al layer made of pure aluminum or an aluminum alloy; and an Fe layer made of an iron-based alloy and roll-bonded to the Al layer, the Al layer having a thickness of 20 μm or more; a plate-shaped member made of pure aluminum or an aluminum alloy; One end of an Al-based wire for bonding is bonded to the Al layer by wire bonding; The other end of the Al-based wire is bonded to the plate-like member, forming a bonding structure using a clad material for wire bonding.

8. 8. The bond structure using the clad material for wire bonding according to claim 7, wherein a bond strength between the Al-based wire and the Al layer is 9.8 N or more.

9. A step of preparing a clad material for wire bonding, the clad material being composed of an Al layer and an Fe layer, by rolling and bonding an Al plate material made of pure aluminum or an aluminum alloy and an Fe plate material made of an iron-based alloy, the Al layer having a thickness of 20 μm or more; a step of joining a battery terminal member made of an iron-based alloy to the Fe layer; a step of bonding one end of an Al-based wire for bonding to the Al layer by wire bonding; and joining the other end of the Al-based wire to a bus bar made of pure aluminum or an aluminum alloy.

Citation Information

Patent Citations

  • Battery pack

    JP2010282811A