Pattern formation method

The pattern forming method using a metal-containing resist composition with phosphorus and sulfur additives addresses sensitivity and edge roughness issues in traditional photoresists, enhancing etching resistance and resolution for smaller semiconductor features.

JP2024169310AActive Publication Date: 2024-12-05SAMSUNG SDI CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024059398
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-19
Filing Date
2024-04-02
Publication Date
2024-12-05
Estimated Expiration
2044-04-02

AI Technical Summary

Technical Problem

Traditional chemically amplified photoresists face challenges with reduced sensitivity, increased edge roughness, and poor etching resistance due to their elemental composition, making it difficult to meet the demands of semiconductor manufacturing for smaller feature sizes.

Method used

A pattern forming method involving a metal-containing resist composition applied to a substrate, followed by heat treatment and development using a developer composition containing additives like phosphoric acid compounds and sulfonic acid compounds, which increases the resist film thickness by 5 to 100% and incorporates phosphorus and sulfur elements on the surface.

Benefits of technology

The method enhances etching resistance, improves sensitivity and critical dimension uniformity, and reduces line edge roughness, enabling better resolution and miniaturization of semiconductor features.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169310000001_ABST
    Figure 2024169310000001_ABST
Patent Text Reader

Abstract

To provide a pattern formation method which includes a development step of coating a metal-containing resist composition, and forming a resist pattern.SOLUTION: A pattern formation method includes a step of coating a metal-containing resist composition onto a substrate, a heat treatment step of drying and heating the substrate, and forming a metal-containing resist film on the substrate, a step of exposing a metal-containing resist film using a patterned mask, and a development step of coating a developer composition, removing a non-exposure region and forming a resist pattern, wherein thickness of the metal-containing resist film after the development step is increased by 5 to 100% with respect to the thickness of the metal-containing resist film before the development step, and 5 to 20 at% of at least one of a phosphorus element and a sulfur element is contained on the surface of the metal-containing resist film after the development step.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pattern forming method. [Background technology]

[0002] In recent years, the semiconductor industry has experienced a continuous shrinkage of critical dimensions, which has led to a demand for new types of high performance photoresist materials and patterning methods to meet the demands of fabricating and patterning smaller and smaller features.

[0003] Traditional chemically amplified (CA) photoresists were designed for high sensitivity, but may be more challenging under EUV exposure, in part because their typical elemental composition (predominantly carbon (C) with additional small amounts of oxygen (O), fluorine (F), and sulfur (S)) reduces the absorbance of the photoresist at 13.5 nm wavelength, resulting in reduced sensitivity. CA photoresists are also challenged by roughness issues due to small feature sizes, and experimentally have shown increased line edge roughness (LER) due to reduced photospeed, in part due to the nature of the acid catalysis process. Due to the shortcomings and problems of CA photoresists, there is a demand for new types of high performance photoresists in the semiconductor industry.

[0004] In particular, in the photolithography process, there is a need to develop a photoresist that can guarantee excellent etching resistance and resolution, while at the same time improving sensitivity and CD (critical dimension) uniformity and improving LER characteristics. Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a pattern forming method which comprises a developing step of applying a metal-containing resist composition to form a resist pattern. [Means for solving the problem]

[0006] A pattern forming method according to one embodiment of the present invention includes a step of applying a metal-containing resist composition onto a substrate; a heat treatment step of drying and heating to form a metal-containing resist film on the substrate; a step of exposing the metal-containing resist film using a patterned mask; and a development step of applying a developer composition to remove unexposed areas of the metal-containing resist film to form a resist pattern. the thickness of the metal-containing resist film after the developing step is increased by 5 to 100% compared to the thickness of the metal-containing resist film before the developing step; After the developing step, the surface of the metal-containing resist film contains at least one of elemental phosphorus and elemental sulfur in an amount of 5 to 20 at %.

[0007] The developer composition may contain an additive including at least one selected from the group consisting of phosphoric acid compounds, phosphorous acid compounds, hypophosphorous acid compounds, and sulfonic acid compounds, and an organic solvent.

[0008] The above additives may be contained in an amount of 0.01 to 10% by mass, relative to 100% by mass of the total mass of the developer composition.

[0009] The above phosphorous compounds include phosphonic acid, methylphosphonic acid, ethylphosphonic acid, butylphosphonic acid, hexylphosphonic acid, n-octylphosphonic acid, tetradecylphosphonic acid, octadecylphosphonic acid, phenylphosphonic acid, vinylphosphonic acid, aminomethylphosphonic acid, methylenediaminetetramethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid, 1-amino1-phosphonooctylphosphonic acid, etidronic acid, 2-aminoethylphosphonic acid, 3-aminopropylphosphonic acid, 4-methylphenylphosphonic acid, 3-methylphenylphosphonic acid, 2-methylphenylphosphonic acid, 4-aminoethylphosphonic acid, 5-aminopropylphosphonic acid, 6-aminopropylphosphonic acid, 7-aminopropylphosphonic acid, 8-aminopropylphosphonic acid, 9-aminopropylphosphonic acid, 10-aminopropylphosphonic acid, 11-aminopropylphosphonic acid, 12-aminopropylphosphonic acid, 13-aminopropylphosphonic acid, 14-aminopropylphosphonic acid, 15-aminopropylphosphonic acid, 16-aminopropylphosphonic acid, 17-aminopropylphosphonic acid, 18-aminopropylphosphonic acid, 19-aminopropylphosphonic acid, 20-aminopropylphosphonic acid, 21-aminopropylphosphonic acid, 22-aminopropylphosphonic acid, 23-aminopropylphosphonic acid, 24-aminopropylphosphonic acid, 25-aminopropylphosphonic acid, 26-aminopropylphosphonic acid, 27-aminopropylphosphonic acid, 28-aminopropylphosphonic acid, 29-aminopropylphosphonic acid, 30-aminopropylphosphonic acid, 31-aminopropylphosphonic acid, 32-aminopropylphosphonic acid, 33-aminopropylphosphonic acid, 34-aminopropylphosphonic acid, 35-aminopropylphosphonic acid, 36-aminopropylphosphonic acid, 37-aminopropylphosphonic acid, 38-aminopropylphosphonic acid, and may be at least one selected from the group consisting of aminophenylphosphonic acid, 3-aminophenylphosphonic acid, 2-aminophenylphosphonic acid, 3-hydroxyphenylphosphonic acid, 4-hydroxyphenylphosphonic acid, 2-hydroxyphenylphosphonic acid, 6-hydroxyhexylphosphonic acid, decylphosphonic acid, diphosphonic acid, methylene diphosphonic acid, nitrilotrimethylene triphosphonic acid, 1H,1H,2H,2H-perfluorooctanephosphonic acid, cyclohexylmethylphosphonic acid, 2-thienylmethylphosphonic acid, 4-fluorophenylphosphonic acid, and benzylphosphonic acid.

[0010] The hypophosphorous acid compound may be at least one selected from the group consisting of diphenylphosphinic acid, bis(4-methoxyphenyl)phosphinic acid, phosphinic acid, bis(hydroxymethyl)phosphinic acid, phenylphosphinic acid, and p-(3-aminopropyl)-p-butylphosphinic acid.

[0011] The sulfonic acid compound may be at least one selected from the group consisting of p-toluenesulfonic acid, benzenesulfonic acid, p-dodecylbenzenesulfonic acid, 1,4-naphthalenedisulfonic acid, methanesulfonic acid, phenylmethanesulfonic acid, 1-octane sulfonic acid, 4-ethenylbenzenesulfonic acid, 2-methylbenzenesulfonic acid, ethanesulfonic acid, 2,5-dimethylbenzenesulfonic acid, 2,4-dimethylbenzenesulfonic acid, allylsulfonic acid, 1-butanesulfonic acid, 1-propanesulfonic acid, 2-propanesulfonic acid, vinylbenzenesulfonic acid, hexanesulfonic acid, and heptanesulfonic acid.

[0012] The metal compound contained in the metal-containing resist composition can include at least one of an organic oxy group-containing tin compound and an organic carbonyloxy group-containing tin compound.

[0013] The metal compound preferably includes a compound represented by the following chemical formula 1 or a condensate thereof.

[0014] [ka]

[0015] In the above chemical formula 1, R 1 is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 7 to 31 carbon atoms, and L a -OR a (Here, L a is a substituted or unsubstituted alkylene group having 1 to 20 carbon atoms, R a is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms; R 2 ~R 4each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 7 to 31 carbon atoms, -OR b , and -OC(=O)R c and R 2 ~R 4 At least one of the is -OR b and -OC(=O)R c is selected from among R b is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof; R c is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof. Effect of the Invention

[0016] According to the present invention, there can be provided a pattern forming method including a development step of applying a metal-containing resist composition to form a resist pattern. [Brief description of the drawings]

[0017] [Figure 1] 1A to 1C are schematic cross-sectional views illustrating the pattern formation method of the present invention, shown in order of steps. [Diagram 2] 1A to 1C are schematic cross-sectional views illustrating the pattern formation method of the present invention, shown in order of steps. [Diagram 3]1A to 1C are schematic cross-sectional views illustrating the pattern formation method of the present invention, shown in order of steps. [Figure 4] FIG. 1 shows scanning electron micrographs comparing the thickness of metal-containing resist films after a development process. [Diagram 5] 1 is a graph showing the results of an XPS analysis of a metal-containing resist film after a development process. [Figure 6] FIG. 2 is a scanning electron microscope photograph showing a resist pattern after a development process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, the embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, in describing the present invention, descriptions of already known functions or configurations will be omitted in order to clarify the gist of the description.

[0019] In order to clearly explain the present invention, parts that are not relevant to the description are omitted, and the same or similar components are given the same reference numerals throughout the specification. In addition, the size and thickness of each component shown in the drawings are arbitrarily shown for the convenience of explanation, and the present invention is not necessarily limited to those shown in the drawings.

[0020] In the drawings, the thicknesses of the layers and regions are exaggerated to clearly show the layers and regions. Also, for the convenience of explanation from the drawings, the thicknesses of some layers and regions are exaggerated. When a part such as a layer, film, region, plate, etc. is "on" or "on" another part, this includes not only the case where it is "directly on" the other part, but also the case where there is another part therebetween.

[0021] In this specification, "substituted" means that a hydrogen atom is substituted with a deuterium atom, a halogen group, a hydroxy group, an amino group, a substituted or unsubstituted alkylamino group having 1 to 30 carbon atoms, a nitro group, a substituted or unsubstituted organic silyl group having 1 to 40 carbon atoms, an alkyl group having 1 to 30 carbon atoms, a haloalkyl group having 1 to 10 carbon atoms, an alkylsilyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or a cyano group. "Unsubstituted" means that a hydrogen atom is not substituted with another substituent and remains a hydrogen atom.

[0022] In this specification, unless otherwise defined, the term "alkyl group" refers to a straight-chain or branched-chain aliphatic hydrocarbon group. The alkyl group may be a "saturated alkyl group" that does not contain any double bonds or triple bonds.

[0023] The alkyl group may be an alkyl group having 1 to 20 carbon atoms. More specifically, the alkyl group may be an alkyl group having 1 to 10 carbon atoms or an alkyl group having 1 to 6 carbon atoms. For example, an alkyl group having 1 to 4 carbon atoms means that the alkyl chain contains 1 to 4 carbon atoms, and indicates that the alkyl group is selected from the group consisting of, for example, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group.

[0024] Specific examples of the above alkyl group or the below cycloalkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, a pentyl group, a hexyl group, a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group.

[0025] In this specification, unless otherwise defined, a "cycloalkyl group" refers to a monovalent cyclic aliphatic hydrocarbon group.

[0026] In this specification, unless otherwise defined, the term "alkenyl group" refers to a straight-chain or branched-chain aliphatic hydrocarbon group and an aliphatic unsaturated alkenyl group containing one or more double bonds.

[0027] As used herein, unless otherwise defined, the term "alkynyl group" refers to a straight-chain or branched-chain aliphatic hydrocarbon group and an aliphatic unsaturated alkynyl group containing one or more triple bonds.

[0028] As used herein, an "aryl group" refers to a substituent in which all elements of the cyclic substituent have p-orbitals and these p-orbitals form conjugation, and includes monocyclic or fused polycyclic (i.e., rings which share adjacent pairs of carbon atoms) functional groups.

[0029] Hereinafter, a pattern forming method according to one embodiment of the present invention will be specifically described with reference to the drawings.

[0030] A pattern forming method according to one embodiment of the present invention includes a step of applying a metal-containing resist composition onto a substrate, a heat treatment step of drying and heating the substrate to form a metal-containing resist film on the substrate, a step of exposing the metal-containing resist film using a patterned mask, and a development step of applying a developer composition to remove unexposed areas of the metal-containing resist film to form a resist pattern. The thickness of the metal-containing resist film after the development process is increased by 5 to 100% compared to the thickness of the metal-containing resist film before the development process, After the development step, the surface of the metal-containing resist film contains 5 to 20 at % of at least one of phosphorus and sulfur.

[0031] When the spacing between mask patterns is narrowed to reduce the resist spacing, light diffraction during exposure causes bridges to form between the lines of the resist pattern, resulting in an increase in LER.

[0032] Furthermore, when a developer with high solubility is used, the spacing between the spaces will become wider even with the same irradiation energy, whereas when a developer with low solubility is used, undissolved material will remain in some of the spaces, which may cause bridging between the lines.

[0033] However, in the resist pattern formed by the pattern forming method according to the present invention, at least one of phosphorus element and sulfur element is contained in an amount of 5 to 20 at % on the surface of the metal-containing resist film after the development process, so that the thickness of the metal-containing resist film after the development process is increased by 5 to 100% compared to the thickness of the metal-containing resist film before the development process. Therefore, the effect of reducing the space interval without bridging can be realized, and the LER characteristics can be improved.

[0034] The phosphorus (P) and sulfur (S) components contained in the developer are adsorbed onto the resist surface, increasing the thickness of the pattern while maintaining the shape of the pattern, thereby reducing the space interval.

[0035] More specifically, the process of forming a pattern using the metal-containing resist composition can include a process of applying the metal-containing resist composition onto a substrate on which a thin film has been formed by a method such as spin coating, slit coating, inkjet printing, etc., and a process of drying the applied metal-containing resist composition to form a metal-containing resist film. The metal-containing resist composition can include a tin-based compound, and for example, the tin-based compound can include at least one of an organic oxy group-containing tin compound and an organic carbonyloxy group-containing tin compound.

[0036] For example, the metal compound contained in the metal-containing resist composition preferably contains a compound represented by the following chemical formula 1 or a condensate thereof.

[0037] [ka]

[0038] In the above chemical formula 1, R 1 is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 7 to 31 carbon atoms, and L a -OR a (Here, L a is a substituted or unsubstituted alkylene group having 1 to 20 carbon atoms, R a is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms; R 2 ~R 4 each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 7 to 31 carbon atoms, -OR b , and -OC(=O)R c and R 2 ~R 4 At least one of the is -OR b , and -OC(=O)R c is selected from among R b is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof; R cis a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof.

[0039] R in the above Chemical Formula 1 b and R c may each independently be a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms.

[0040] Furthermore, the metal compound contained in the metal-containing resist composition may include a condensate of the compound represented by Chemical Formula 1 above.

[0041] Subsequently, a first heat treatment step is performed in which the substrate on which the metal-containing resist film is formed is heated. The first heat treatment step can be performed at a temperature of 80° C. to 120° C., during which the solvent evaporates and the metal-containing resist film can be more firmly attached to the substrate.

[0042] The metal-containing resist film is then selectively exposed to light using a patterned mask.

[0043] For example, examples of light that can be used in the exposure process include light having short wavelengths such as i-line (wavelength 365 nm), KrF excimer laser (wavelength 248 nm), and ArF excimer laser (wavelength 193 nm), as well as light having high energy wavelengths such as EUV (Extreme Ultra Violet; wavelength 13.5 nm) and E-Beam (electron beam).

[0044] More specifically, the exposure light in one embodiment may be short wavelength light having a wavelength range of 5 nm to 150 nm, or may be light having a high energy wavelength such as EUV (Extreme UltraViolet; wavelength 13.5 nm) or E-Beam (electron beam).

[0045] In the step of forming a resist pattern, a negative pattern can be formed.

[0046] The exposed areas of the metal-containing resist film form polymers through crosslinking reactions such as condensation between organometallic compounds, and thus have a different solubility from the unexposed areas of the metal-containing resist film.

[0047] Subsequently, the substrate is subjected to a second heat treatment step. The second heat treatment step can be performed at a temperature of 90° C. to 200° C. By performing the second heat treatment step, the exposed area of ​​the metal-containing resist film becomes less soluble in a developer.

[0048] This is followed by a developing step using a developer composition.

[0049] Specifically, a developer composition is applied to dissolve the metal-containing resist film in the unexposed area, and then the metal-containing resist film is removed, completing a resist pattern corresponding to a negative tone image.

[0050] 1 to 3 are schematic cross-sectional views showing the process steps in order to explain the pattern formation method of the present invention.

[0051] Referring to FIG. 1, the exposed metal-containing resist film is developed to form a resist pattern 130P.

[0052] In an exemplary embodiment, the exposed metal-containing resist film can be developed to remove the unexposed areas of the metal-containing resist film to form a resist pattern 130P consisting of the exposed areas of the metal-containing resist film. The resist pattern 130P can include a plurality of openings (OP).

[0053] In an exemplary embodiment, the development of the metal-containing resist film can be performed by a negative-tone development (NTD) process. In this case, the developer composition for the metal-containing resist according to an embodiment of the present invention can be used as the developer composition.

[0054] Referring to FIG. 2, the feature layer 110 is processed using the resist pattern 130P resulting from FIG.

[0055] For example, in order to process the feature layer 110, various processes can be performed, such as a process of etching the feature layer 110 exposed through the openings (OP) of the resist pattern 130P, a process of implanting impurity ions into the feature layer 110, a process of forming an additional film on the feature layer 110 through the openings (OP), a process of deforming a part of the feature layer 110 through the openings (OP), etc. Fig. 2 shows, as an exemplary process of processing the feature layer 110, etching the feature layer 110 exposed through the openings (OP) to form a feature pattern 110P.

[0056] 3, the resist pattern 130P remaining on the feature pattern 110P in the resultant structure of FIG. 2 is removed. To remove the resist pattern 130P, an ashing and stripping process can be used.

[0057] According to one embodiment, the thickness of the metal-containing resist film after the development process may be increased by 5 to 100% compared to the thickness of the metal-containing resist film before the development process.

[0058] The thickness of the metal-containing resist film after the development step can be increased by the inclusion of at least one of phosphorus and sulfur elements in the surface of the resist pattern.

[0059] For example, at least one of phosphorus and sulfur may be contained at 5 to 20 at %.

[0060] For example, the developer composition may contain an additive including at least one selected from the group consisting of phosphoric acid compounds, phosphorous acid compounds, hypophosphorous acid compounds, and sulfonic acid compounds, and an organic solvent.

[0061] The phosphorus and sulfur elements contained on the surface of the metal-containing resist film after the development step may originate from additives in the developer composition.

[0062] The additives may be contained in an amount of 0.01 to 10% by mass relative to the total mass (100% by mass) of the developer composition. Specifically, the content of the additives may be 0.01 to 7% by mass, 0.01 to 5% by mass, 0.01 to 3% by mass, or 0.01 to 1% by mass relative to the total mass (100% by mass) of the developer composition.

[0063] For example, the phosphorous acid compounds include phosphonic acid, methylphosphonic acid, ethylphosphonic acid, butylphosphonic acid, hexylphosphonic acid, n-octylphosphonic acid, tetradecylphosphonic acid, octadecylphosphonic acid, phenylphosphonic acid, vinylphosphonic acid, aminomethylphosphonic acid, methylenediaminetetramethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid, 1-amino1-phosphonooctylphosphonic acid, etidronic acid, 2-aminoethylphosphonic acid, 3-aminopropylphosphonic acid, 4-methylphenylphosphonic acid, 3-methylphenylphosphonic acid, 2-methylphenylphosphonic acid, 4 ... and may be at least one selected from the group consisting of 1H,1H,2H,2H-perfluorooctanephosphonic acid, cyclohexylmethylphosphonic acid, 2-thienylmethylphosphonic acid, 4-fluorophenylphosphonic acid, and benzylphosphonic acid.

[0064] For example, the hypophosphorous acid compound may be at least one selected from the group consisting of diphenylphosphinic acid, bis(4-methoxyphenyl)phosphinic acid, phosphinic acid, bis(hydroxymethyl)phosphinic acid, phenylphosphinic acid, and p-(3-aminopropyl)-p-butylphosphinic acid.

[0065] For example, the sulfonic acid compound may be at least one selected from the group consisting of p-toluenesulfonic acid, benzenesulfonic acid, p-dodecylbenzenesulfonic acid, 1,4-naphthalenedisulfonic acid, methanesulfonic acid, phenylmethanesulfonic acid, 1-octane sulfonic acid, 4-ethenylbenzenesulfonic acid, 2-methylbenzenesulfonic acid, ethanesulfonic acid, 2,5-dimethylbenzenesulfonic acid, 2,4-dimethylbenzenesulfonic acid, allylsulfonic acid, 1-butanesulfonic acid, 1-propanesulfonic acid, 2-propanesulfonic acid, vinylbenzenesulfonic acid, hexanesulfonic acid, and heptanesulfonic acid.

[0066] Examples of the organic solvent contained in the developer composition include at least one selected from the group consisting of ethers, alcohols, glycol ethers, aromatic hydrocarbon compounds, ketones, and esters, but are not limited thereto. For example, the organic solvent may be ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol methyl ether, diethylene glycol ethyl ether, propylene glycol, propylene glycol methyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), propylene glycol ethyl ether, propylene glycol ethyl ether acetate, propylene glycol propyl ether acetate, propylene glycol butyl ether, propylene glycol butyl ether acetate, ethanol, propanol, isopropyl alcohol, isobutyl alcohol, 4-methyl-2-pentanol (or may be written as methyl isobutyl carbinol (MIBC)), hexanol, 1-methoxy-2-propanol, 1-ethoxy ... Examples of suitable alkoxysilanes include, but are not limited to, ethanol, ethylene glycol, propylene glycol, heptanone, propylene carbonate, butylene carbonate, toluene, xylene, methyl ethyl ketone, cyclopentane, cyclohexane, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, gamma-butyrolactone, methyl 2-hydroxyisobutyrate, methoxybenzene, n-butyl acetate, 1-methoxy-2-propyl acetate, methoxyethoxypropionate, ethoxyethoxypropionate, or mixtures thereof.

[0067] When other additives described later are contained, the organic solvent may be contained in an amount that is the balance excluding the contained components.

[0068] The developer composition may further contain at least one other additive selected from the group consisting of a surfactant, a dispersant, a moisture absorbent, and a coupling agent.

[0069] The surfactant can play a role in improving the coating uniformity of the developer composition and improving the wettability. In an exemplary embodiment, the surfactant may be, but is not limited to, a sulfate salt, a sulfonate salt, a phosphate ester, a soap, an amine salt, a quaternary ammonium salt, a polyethylene glycol, an alkylphenol ethylene oxide adduct, a polyhydric alcohol, a nitrogen-containing vinyl polymer, or a combination thereof. For example, the surfactant may include an alkylbenzene sulfonate salt, an alkylpyridinium salt, a polyethylene glycol, or a quaternary ammonium salt. When the developer composition includes a surfactant, the surfactant may be included in an amount of 0.001% by weight to 3% by weight based on the total weight of the developer composition.

[0070] The dispersant can serve to make each component of the developer composition uniformly disperse in the developer composition. In an exemplary embodiment, the dispersant can be, but is not limited to, an epoxy resin, polyvinyl alcohol, polyvinyl butyral, polyvinylpyrrolidone, glucose, sodium dodecyl sulfate, sodium citrate, oleic acid, linoleic acid, or a combination thereof. When the developer composition includes a dispersant, the dispersant can be included in an amount of 0.001% by mass to 5% by mass based on the total mass of the developer composition.

[0071] The moisture absorbent can prevent adverse effects of moisture in the developer composition. For example, the moisture absorbent can prevent metals contained in the developer composition from being oxidized by moisture. In an exemplary embodiment, the moisture absorbent can be, but is not limited to, polyoxyethylene nonylphenol ether, polyethylene glycol, polypropylene glycol, polyacrylamide, or a combination thereof. When the photoresist composition includes a moisture absorbent, the moisture absorbent is included in an amount of 0.001% by weight to 10% by weight based on the total weight of the developer composition.

[0072] The coupling agent can improve the adhesion to the lower film when the developer composition is coated on the lower film. In an exemplary embodiment, the coupling agent can include a silane coupling agent. The silane coupling agent can be, but is not limited to, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltrichlorosilane, vinyltris(β-methoxyethoxy)silane, 3-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, or trimethoxy[3-(phenylamino)propyl]silane. When the developer composition includes a coupling agent, the coupling agent can be included in an amount of 0.001% to 5% by weight based on the total weight of the developer composition.

[0073] As described above, the resist pattern formed by exposure to light having a wavelength such as i-line (wavelength 365 nm), KrF excimer laser (wavelength 248 nm), ArF excimer laser (wavelength 193 nm), and high-energy light such as EUV (extreme ultraviolet, Extreme UltraViolet; wavelength 13.5 nm) and E-Beam (electron beam) can have a thickness width of 5 nm to 100 nm. As an example, the resist pattern can be formed with a width of 5 nm to 90 nm, 5 nm to 80 nm, 5 nm to 70 nm, 5 nm to 60 nm, 5 nm to 50 nm, 5 nm to 40 nm, 5 nm to 30 nm, or 5 nm to 20 nm.

[0074] Alternatively, the resist pattern may have a half-pitch of 50 nm or less, such as 40 nm or less, for example 30 nm or less, such as 20 nm or less, for example 15 nm or less, and a pitch with a linewidth roughness of 10 nm or less, 5 nm or less, 3 nm or less, 2 nm or less. EXAMPLES

[0075] The present invention will be described in more detail below with reference to examples of the preparation of the above-mentioned metal-containing resist developer composition, but the technical features of the present invention are not limited to the following examples.

[0076] (Production of developer composition for metal-containing resist) The organic solvent and additives were mixed in the compositions shown in Table 1 below in a PP bottle, and then the bottle was shaken at room temperature (25°C) to completely dissolve the mixture. The mixture was then filtered using a PTFE filter with a pore size of 1 μm to obtain a developer composition.

[0077] [Table 1]

[0078] (Preparation of Metal-Containing Resist Composition) An organometallic compound having a structural unit represented by the following chemical formula C was dissolved in 4-methyl-2-pentanol at a concentration of 1% by mass, and then filtered using a 0.1 μm PTFE syringe filter to prepare a metal-containing resist composition.

[0079] [ka]

[0080] (Evaluation 1: Pattern thickness measurement and XPS analysis) An 8-inch silicon wafer was spin-coated with hexamethyldisilazane to form a hydrophobic surface. The metal-containing resist composition prepared above was then spin-coated on the wafer with the hydrophobic surface at 1,500 rpm for 30 seconds, and heat-treated at 160° C. for 60 seconds to produce a coated wafer.

[0081] The coated wafer was exposed to EUV light (Lawrence Berkeley National Laboratory Micro Exposure Tool, MET) and pad exposure time was adjusted so that an incremental dose of EUV was applied to each pad.

[0082] The metal-containing resist composition and the substrate were then post-exposure baked (PEB) on a hot plate at 180° C. for 90 seconds. The baked metal-containing resist film and substrate were immersed in the developer according to Examples 1-7 and Comparative Examples 1-3 for 30 seconds, respectively, and then washed with the same developer for an additional 15 seconds to form a negative tone image, i.e., remove the unexposed coating portion. Finally, the process was terminated by baking on a hot plate at 240° C. for 60 seconds.

[0083] The coated wafers were exposed to a wavelength range of 280 nm to 1,000 nm at an angle of 70° using a J. A. Woolam M2000 ellipsometer to measure the thickness of the metal-containing resist film remaining on the pads.

[0084] The thickness measurement results are shown in Table 2 and FIG.

[0085] The increase in the thickness of the resist film before and after development was calculated using the following formula 1.

[0086]

number

[0087] In addition, the components of the remaining metal-containing resist film were analyzed by X-ray photoelectron spectroscopy (XPS) (instrument used: AXISSUPRA, manufactured by KRATOS Analytical), and the results are shown in Table 2 and Figure 5. Specifically, the beam size was set to 700 μm, the source power was set to 150 W for wide scan and 225 W for narrow scan, and analysis was performed in XPS-monochromatic mode, and the resolution was set to 20 eV at 0.1 eV intervals for C1s, O1s, P2p, Sn3d, and S3p during narrow scan, and the phosphorus content was measured.

[0088] Evaluation 2: CD measurement The developer composition is evaluated by injecting it in the development process during the coating-exposure-development process for manufacturing a patterned wafer. The patterned wafer, which has completed the process, has a line / space CD pattern formed, and is then transferred to a Hitachi High-Tech CG-5000 (high-resolution FEB measuring device, CD-SEM) to measure the CD (Critical Dimension) size of the part of the mask pattern with a half-pitch of 14 nm. The minimum value of the space CD between the lines is shown in Table 2 and Figure 6.

[0089] [Table 2]

[0090] Referring to Table 2, when the metal-containing resist developer compositions of Examples 1 to 7 are used, the space CD due to the increase in thickness of the metal-containing resist film after development is reduced, and there is less residue at the dissolved space portion, compared to the cases where the metal-containing resist developer compositions of Comparative Examples 1 to 3 are used, so that excellent resolution and reduced bridges and residues can be realized.

[0091] FIG. 4 shows scanning electron microscope images comparing the thickness of metal-containing resist films after the development process.

[0092] Referring to FIG. 4, it can be seen that when development was performed using a developer composition containing a sulfonic acid compound (Example 5), the thickness of the metal-containing resist film after the development process was increased compared to when no developer treatment was performed (Comparative Example 1) and when development was performed using a developer composition containing an organic acid (Comparative Example 2).

[0093] FIG. 5 is a graph showing the results of XPS analysis of the metal-containing resist film after the development process.

[0094] 5, the XPS analysis of the metal-containing resist film after the development process shows that it contains phosphorus (P) components, which indicates that the additive components in the developer composition are adsorbed onto the surface of the metal-containing resist film.

[0095] FIG. 6 is a scanning electron microscope photograph showing the resist pattern after the development process.

[0096] 6, when phosphorus or sulfur is included in the additive components, the phosphorus or sulfur is adsorbed on the surface of the metal-containing resist film, increasing the thickness of the resist pattern, but even with a narrow space CD (10.5 nm), there is little generation of dissolved residue and bridges are reduced, resulting in a pattern with excellent resolution. This effect allows the semiconductor line width to be minimised by minimising the size of the space part pattern.

[0097] Although specific embodiments of the present invention have been described and illustrated above, it is obvious to those skilled in the art that the present invention is not limited to the described embodiments, and various modifications and variations can be made without departing from the spirit and scope of the present invention. Therefore, the modifications or variations should not be understood individually from the technical spirit and perspective of the present invention, and the modified embodiments should belong to the scope of the claims of the present invention. [Explanation of symbols]

[0098] OP opening, 100 boards, 110 feature layers, 130 Metal-containing resist film, 110P feature pattern, 130P resist pattern.

Claims

1. applying a metal-containing resist composition onto a substrate; a heat treatment step of drying and heating to form a metal-containing resist film on the substrate; exposing the metal-containing resist film using a patterned mask; and a developing step of applying a developer composition and removing unexposed areas to form a resist pattern; Including, the thickness of the metal-containing resist film after the developing step is increased by 5 to 100% relative to the thickness of the metal-containing resist film before the developing step; The pattern forming method, wherein the surface of the metal-containing resist film after the developing step contains at least one of phosphorus element and sulfur element in an amount of 5 to 20 at %.

2. 2. The pattern formation method according to claim 1, wherein the developer composition comprises an additive containing at least one selected from the group consisting of phosphoric acid compounds, phosphorous acid compounds, hypophosphorous acid compounds, and sulfonic acid compounds, and an organic solvent.

3. The pattern formation method according to claim 2, wherein the additive is contained in an amount of 0.01 to 1.0% by mass based on the total mass of the developer composition.

4. The phosphorous acid compounds include phosphonic acid, methylphosphonic acid, ethylphosphonic acid, butylphosphonic acid, hexylphosphonic acid, n-octylphosphonic acid, tetradecylphosphonic acid, octadecylphosphonic acid, phenylphosphonic acid, vinylphosphonic acid, aminomethylphosphonic acid, methylenediaminetetramethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid, 1-amino1-phosphonooctylphosphonic acid, etidronic acid, 2-aminoethylphosphonic acid, 3-aminopropylphosphonic acid, 4-methylphenylphosphonic acid, 3-methylphenylphosphonic acid, 2-methylphenylphosphonic acid, 4-amino ... The pattern formation method according to claim 2, wherein the phosphoric acid is at least one selected from the group consisting of phosphonic acid, 3-aminophenylphosphonic acid, 2-aminophenylphosphonic acid, 3-hydroxyphenylphosphonic acid, 4-hydroxyphenylphosphonic acid, 2-hydroxyphenylphosphonic acid, 6-hydroxyhexylphosphonic acid, decylphosphonic acid, diphosphonic acid, methylene diphosphonic acid, nitrilotrimethylene triphosphonic acid, 1H,1H,2H,2H-perfluorooctanephosphonic acid, cyclohexylmethylphosphonic acid, 2-thienylmethylphosphonic acid, 4-fluorophenylphosphonic acid, and benzylphosphonic acid.

5. 3. The pattern formation method according to claim 2, wherein the hypophosphorous acid compound is at least one selected from the group consisting of diphenylphosphinic acid, bis(4-methoxyphenyl)phosphinic acid, phosphinic acid, bis(hydroxymethyl)phosphinic acid, phenylphosphinic acid, and p-(3-aminopropyl)-p-butylphosphinic acid.

6. 3. The pattern formation method according to claim 2, wherein the sulfonic acid compound is at least one selected from the group consisting of p-toluenesulfonic acid, benzenesulfonic acid, p-dodecylbenzenesulfonic acid, 1,4-naphthalenedisulfonic acid, methanesulfonic acid, phenylmethanesulfonic acid, 1-octane sulfonic acid, 4-ethenylbenzenesulfonic acid, 2-methylbenzenesulfonic acid, ethanesulfonic acid, 2,5-dimethylbenzenesulfonic acid, 2,4-dimethylbenzenesulfonic acid, allylsulfonic acid, 1-butanesulfonic acid, 1-propanesulfonic acid, 2-propanesulfonic acid, vinylbenzenesulfonic acid, hexanesulfonic acid, and heptanesulfonic acid.

7. 2. The pattern formation method according to claim 1, wherein the metal compound contained in the metal-containing resist composition includes at least one of an organic oxy group-containing tin compound and an organic carbonyloxy group-containing tin compound.

8. 2. The pattern forming method according to claim 1, wherein the metal compound contained in the metal-containing resist composition includes a compound represented by the following Chemical Formula 1 or a condensate thereof: 【Chemistry 1】 In the above Chemical Formula 1, R 1 is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 7 to 31 carbon atoms, and L a -O-R a (Here, L a is a substituted or unsubstituted alkylene group having 1 to 20 carbon atoms, R a is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms; R 2 ~R 4 each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 7 to 31 carbon atoms, -OR b and -OC(=O)R c and R 2 ~R 4 At least one of the groups is -OR b and -OC(=O)R c is selected from among R b is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof; R c is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof.

Citation Information

Patent Citations

  • Photoresist developer compositions

    CN1503064A

  • Agent for raising image sharpness added into developing solution dependent on dissolution speed difference and developing composition containing it

    JP1984142547A

  • Photoresist developer

    JP2003195517A

  • Developing solution and pattern forming method

    JP2008176098A

  • Photoresist developer and method of manufacturing a semiconductor device

    US20210364924A1