Method for forming glass film having light shield, heat dissipation and conductivity of carbon black and transparency of amorphous powder glass or having thermal shock resistance and mechanical strength of crystalline powder glass

A glass film is produced by dispersing carbon black aggregates in methanol and combining them with powdered glass, achieving light shielding, heat dissipation, conductivity, and mechanical strength, addressing the challenges of combining these properties in a single film.

JP2024170188AInactive Publication Date: 2024-12-06小林 博
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023087211
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure 2024170188000001_ABST
    Figure 2024170188000001_ABST
Patent Text Reader

Abstract

To provide a method for forming a glass film having the light shield, heat dissipation and conductivity of carbon black and having the transparency of amorphous powder glass; or a method for forming a glass film having the thermal shock resistance and mechanical strength of crystalline powder glass.SOLUTION: A method for forming a glass film having the light shield, heat dissipation and conductivity of carbon black and having the transparency of amorphous powder glass comprises: weighing amorphous powder glass as an amount of the collection of aggregates forming an area larger than one half on the surface of the amorphous powder glass to mix the amorphous powder glass with a suspension having the collection of aggregates dispersed to methanol; applying vibration acceleration in three directions to superimpose the amorphous powder glasses through the suspension; and uniformly compressing the collection of the amorphous powder glasses and rising temperature to a softening point to form a glass film having the light shield, heat dissipation and conductivity of carbon black and the transparency of the amorphous powder glass. The use of crystalline powder glass as powder glass imparts the thermal shock resistance and mechanical strength of the crystalline powder glass to the glass film.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The first invention is an invention in which amorphous powdered glass is used as the powdered glass when creating a glass film. First, a carbon black cluster is pulverized to a limit size in excess methanol. Next, a homogenizer device is operated in excess methanol to create a suspension in which a cluster of aggregates in which the aggregates are entangled with each other through the methanol is dispersed in the excess methanol. Furthermore, a cluster of amorphous powdered glass is put into the suspension so that the cluster of aggregates forms a part wider than 1 / 2 of the surface of the amorphous powdered glass, not the entire surface of the amorphous powdered glass, and vibration acceleration is applied to the suspension in three directions, and the amorphous powdered glass is overlapped with each other through a film of the suspension having a thickness thinner than 1 μm, and the overlapped cluster of powdered glass is formed into a flat shape on the bottom surface of the container. After this, the entire cluster of amorphous powdered glass is evenly compressed and heated to the softening point of the amorphous powdered glass. At this time, first, methanol evaporates from the suspension, and aggregates are precipitated on the surface of the amorphous powdered glass with a thickness of less than 0.1 μm. On the other hand, since the aggregates form a region wider than 1 / 2 of the surface of the amorphous powdered glass, rather than the entire surface of the amorphous powdered glass, multiple regions where aggregates are not formed are formed on the surface of the amorphous powdered glass and have a certain area. Next, the overlapping powdered glass is softened, and the softened powdered glass is compressed evenly, and the softened amorphous powdered glass is deformed so as to fill the voids in the softened amorphous powdered glass, and a part of the softened amorphous powdered glass seeps out from the region where aggregates are not formed, and in the adjacent softened amorphous powdered glass, a region where the exuded softened amorphous powdered glass contacts each other appears, and the contacting regions are joined together. In addition, the contact portions of the softened powdered glass are frictionally welded via the aggregates.Thereafter, the collection of softened amorphous powdered glass is left at the cooling point of the amorphous powdered glass for 15 minutes or more and then slowly cooled to room temperature, whereby the distortion generated when the softened amorphous powdered glass pieces were joined together is released and the softened amorphous powdered glass solidifies. The joints between the amorphous powdered glass pieces also solidify, and the collection of amorphous powdered glass pieces joined together is produced as a glass film. The glass film has light blocking properties, heat dissipation properties, and electrical conductivity due to aggregates formed on the surface of the powdered glass. In addition, the glass film has the transparency of amorphous powdered glass because the surface of the powdered glass has many areas where aggregates are not formed. The second invention is an invention in which crystalline powdered glass is used as the powdered glass, and the glass film combines the light-blocking properties, heat dissipation properties, and electrical conductivity of carbon black, as well as the thermal shock resistance and mechanical strength of the crystalline powdered glass. Granular glass is variously called glass frit, glass particles, and glass powder, but in this invention it is described as powdered glass. According to the JIS packaging terminology, a film is defined as "a plastic film having a thickness of less than 250 μm," and a sheet is defined as "a thin plastic plate having a thickness of 250 μm or more." In this invention, in accordance with the JIS, a wide and thin film having a thickness of less than 250 μm is defined as a film.

[0002] The present inventor has filed two prior applications for inventions that are close to the present invention. The first prior application is for a method for molding a synthetic resin molded body that combines light-blocking properties, heat dissipation properties and electrical conductivity, and was filed as Patent Application No. 2023-011433. The second prior application is for a method for molding a thermoplastic elastomer molded body that combines light-blocking properties, heat dissipation properties, and electrical conductivity, and has been filed as Patent Application No. 2023-021915. The present invention is a method for producing a glass film using amorphous powdered glass, which has light-shielding properties, heat dissipation properties, and electrical conductivity, and also has transparency, or a method for producing a glass film using crystalline powdered glass, which has light-shielding properties, heat dissipation properties, electrical conductivity, thermal shock resistance, and mechanical strength, and uses powdered glass as a raw material to produce a glass film. In contrast, the prior application uses raw materials used in molding synthetic resin pellets or thermoplastic elastomer to mold molded bodies of various shapes. Therefore, the method of treating the powdered glass when producing the glass film is different from the method of treating the raw materials used in molding synthetic resin pellets or molded bodies made of thermoplastic elastomer.

[0003] Powdered glass is produced by mixing and blending several kinds of metal oxides as raw materials, melting them by heat to vitrify them, and then pulverizing them into fine powder by water quenching or roll quenching. For this reason, powdered glass has various compositions and composition ratios. Powdered glass is also divided into crystalline and amorphous (also called non-crystalline). Crystalline powdered glass has a molecular structure that is arranged three-dimensionally in a regular array, so light is reflected at the interface of the crystals and transparency is lost. On the other hand, since the molecular structure is arranged three-dimensionally in a regular array, it has superior thermal shock resistance and mechanical strength compared to amorphous powdered glass. In contrast, amorphous glass powder has transparency. In other words, amorphous glass powder has a non-crystalline structure that does not have a three-dimensional crystal lattice, so it has transparency that allows light to pass through. However, since it has a non-crystalline structure, it has inferior thermal shock resistance and mechanical strength compared to crystalline powdered glass. Furthermore, the size of the powdered glass varies depending on the application of the powdered glass, with the average particle size ranging from a few microns to tens of microns. On the other hand, from the viewpoint of the RoHS Directive, it is desirable to use lead-free powdered glass. Lead-free glass includes phosphate-based glass mainly composed of P2O5, bismuth-based glass mainly composed of Bi2O3, vanadate-based glass composed of V2O5, alkali metal oxide, alkaline earth metal oxide, zinc oxide, boron oxide, phosphorus pentoxide, tellurium oxide, etc., borosilicate-based glass composed of SiO2, B2O3, alkali metal oxide or alkaline earth metal oxide, and fluoride-based glass mainly composed of BeF2. Furthermore, the following metal oxides, which are the main raw materials of glass, each have their own unique functions, so the softening point and linear expansion coefficient of powdered glass can be freely changed by changing the ratio of metal oxides. Silicon oxide SiO2 creates a network structure of glass, which works to raise the softening point and lower the thermal expansion. On the other hand, boron oxide B2O3 creates a network structure of glass, which works to lower the softening point. Titanium oxide TiO2 promotes crystallization and raises the softening point. Alumina Al2O3 suppresses crystallization but raises the softening point. In contrast, sodium oxide Na2O lowers the softening temperature and increases thermal expansion, but is less resistant to hot water. On the other hand, potassium oxide K2O has the same properties as Na2O, but + Na + Since it is 1.4 times larger than Na2O, it is less mobile and provides hot water resistance. Furthermore, calcium oxide (CaO) has similar properties to Na2O, but improves the chemical durability of alkali glass.

[0004] Carbon black has excellent light blocking properties, with a light blocking rate of nearly 100% in the wavelength range from 250 nm to 2500 nm. In addition, carbon black has a high thermal emissivity of 0.95-0.97. On the other hand, the characteristics of carbon black vary greatly depending on the manufacturing method, and carbon black is classified according to the name of the manufacturing method. The properties of carbon black vary depending on the manufacturing method. Furnace black is carbon black produced by incomplete combustion of oil or gas in high-temperature gas, and is subdivided into oil furnaces and gas furnaces depending on the raw material burned. Among furnace blacks, Ketjen black uses oil made of hydrocarbons as the raw material, and produces carbon black by incomplete combustion of the oil. Among carbon blacks, Ketjen black has the largest specific surface area and DPB (dibutyl phthalate) absorption, and shows excellent light shielding properties, and its electrical conductivity is second only to acetylene black. In other words, Ketjen black has a hollow body formed by the structure of a circular arc, and the electrical conductivity of Ketjen black increases as electrons move through the circular arc structure. Other types of carbon black include channel black, which is made by burning natural gas and scraping off the deposits that form on channel steel; acetylene black, which is obtained by pyrolyzing acetylene gas; and thermal black, which is made by repeatedly burning and decomposing gas in a heat-storing furnace. Acetylene black is produced using acetylene gas, which has the highest purity of all carbon black raw materials, so it has the fewest impurities of all carbon blacks and also has the most developed structure and primary particles. For this reason, it has the best conductivity of all carbon blacks.

[0005] The smallest unit of carbon black is an aggregate, which is a primary agglomeration of carbon particles. An aggregate is a collection of carbon particles that are linked together in a bead-like shape and bonded together in an irregular, twisted structure (called a structure). On the other hand, the size of carbon particles in various types of carbon black varies greatly depending on the type of carbon black, and even in the same type of carbon black, there is a range in the size of carbon particles. The size of aggregates also varies greatly depending on the type of carbon black, and even in the same type of carbon black, there is a range in the size of aggregates. On the other hand, structures are formed when soft particles collide with each other at a speed close to the speed of sound in a manufacturing furnace, fuse together, and then are carbonized by heat treatment. For this reason, the primary particles are bonded together with a certain bonding force. When aggregates are generated, the aggregates are generated all at once, and the aggregates are intricately entangled by the structure to form a single aggregate. Furthermore, the aggregates are bonded to each other to form agglomerates, which are secondary aggregates of carbon particles and aggregate clumps. In other words, agglomerates are bonded to each other by the interaction of van der Waals forces. Therefore, the bond between aggregates is significantly smaller than the bond between primary particles. For this reason, when a load is applied to the bond between aggregates in liquid, the bonded aggregates are easily separated in the liquid, and the aggregates become a collection of entangled aggregates. The size of the agglomerates varies greatly depending on the type of carbon black, ranging from 1 to 100 μm. Furthermore, the agglomerates are bonded to each other by the interaction of van der Waals forces to form carbon black. Therefore, when a load is applied to the bonded portions of the agglomerates in a liquid, the bonded agglomerates are easily separated in the liquid. On the other hand, when handling carbon black, water is added to the carbon black to prevent the particles from scattering, causing the particles to solidify and become bead-shaped particles. Most carbon black currently on the market is bead-shaped particles. Note that carbon black made of bead-shaped particles is shipped after the moisture is removed from the carbon black. On the other hand, carbon black that does not solidify the particles forms loose particles. According to Non-Patent Document 1, the size of carbon particles in furnace black ranges from 10 to 100 nm, and the size of aggregates ranges from 40 to 200 ml / 100 g. The size of carbon particles in channel black ranges from 10 to 40 nm, and the size of aggregates ranges from 90 to 170 ml / 100 g. The size of carbon particles in thermal black ranges from 200 to 400 nm, and the size of aggregates ranges from 35 to 50 ml / 100 g. The size of carbon particles in acetylene black ranges from 20 to 50 nm, and the size of aggregates ranges from 140 to 220 ml / 100 g. In addition, the size of bead-shaped particles ranges from 100 to 3000 μm, and the size of loose particles ranges from 50 to 200 μm. [Background technology]

[0006] The prior art closest to the present invention is a technique for imparting light-shielding properties to glass. For example, Patent Document 1 describes an oxide glass in which the P ion content is 7-43 cation %, the Nb ion content is 10-21 cation %, the Li ion content is 20 cation % or more, the total content of Nb ion and Li ion is 48-70 cation %, the Bi ion content is more than 0 cation % and 6 cation % or less, the Ba ion content is 5 cation % or less, the Zr ion content is 2 cation % or less, the total content of Ti ion and W ion is 5 cation % or less, and the cation ratio of the Li content to the total content of Li ion, Na ion and K ion [Li ion / (Li ion + Na ion + K ion)] is 0.5 or more. It is described that the object of this invention is to realize a low specific gravity glass having a light-shielding part having excellent light-shielding properties against visible light and a light-transmitting part having excellent transparency by the glass composition. Patent Document 2 describes black quartz glass having a composition of 63-65 mass% SiO2, 18-24 mass% TiO2, and 12-17 mass% Al2O3 (wherein the total of SiO2, TiO2, and Al2O3 is 100 mass%). It describes that the object of this invention is to obtain black quartz glass having light blocking properties due to the glass composition, without cracks or bubbles in the glass. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2022-119440 A [Patent Document 2] Patent Publication No. 2022-061950 [Non-patent literature]

[0008] [Non-Patent Document 1] Journal of the Japanese Society of Printing Science and Technology, Vol. 44 (2007) No. 3, pp. 133-143 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0009] The present invention aims to solve the following two problems. First, find a method for producing a glass film that has the light-shielding, heat-dissipating, and electrical conductivity of carbon black, and also has the transparency of amorphous powdered glass. Note that light-shielding and transparency are generally contradictory properties. This increases the added value of the glass film. Second, find a method for producing a glass film that has the light-shielding, heat-dissipating, and electrical conductivity of carbon black, and also has the thermal shock resistance and mechanical strength of crystalline powdered glass. This expands the applications of the glass film. [Means for solving the problem]

[0010] A method for producing a glass film having the light blocking, heat dissipation, and electrical conductivity of carbon black and the transparency of amorphous powdered glass is as follows: A container is charged with carbon black clumps and methanol having a weight 10 times greater than the weight of the carbon black clumps, the methanol is stirred, and the carbon black clumps are immersed in the excess methanol. Then, a plate that covers the entire surface of the carbon black clumps in the container is placed over the carbon black clumps. A compressive load is evenly applied to the entire surface of the plate to pulverize the carbon black clumps immersed in the excess methanol. Then, the plate is lifted from the container, and the container is fixed on a vibration table of a vibrator. The vibrator is operated to repeatedly apply vibration acceleration in three directions, front-back, left-right, and up-down, to the container to rearrange the pulverized carbon black clumps in the excess methanol. Then, the plate is placed on the container and the container is fixed on a vibration table of a vibrator. the plate is again covered with the carbon black mass, and the compressive load is applied evenly to the entire surface of the plate to further crush the carbon black mass immersed in the excess methanol; the plate is then again removed from the container, and the vibration acceleration in the three directions is applied repeatedly to the container; the pair of processes consisting of the process of applying the compressive load and the process of applying the vibration acceleration are repeated, and when a repulsive force is generated in the plate when the compressive load is applied to the plate, it is determined that the crushing of the carbon black mass immersed in the excess methanol is completed, and the pair of processes are stopped; thus, a first suspension is prepared in which the crushed carbon black mass is immersed in the excess methanol; thereafter, the first process is to remove the plate from the container; A homogenizer is placed in the container, and the homogenizer is operated in the first suspension, and shock waves are continuously applied to the pulverized carbon black mass via the excess methanol, whereby the shock waves are repeatedly irradiated to bonds between agglomerates in the pulverized carbon black mass, causing the bonds to dissociate and separate into individual agglomerates, and the shock waves are repeatedly irradiated to bonds between aggregates in the agglomerates, causing the bonds to dissociate and separate the entangled aggregates into individual agglomerates. a second step in which the aggregates are separated into individual aggregates, and as a result, the aggregates of carbon black that have been pulverized become aggregates of individual aggregates in which the aggregates are entangled with each other; the shock waves are repeatedly applied to the entangled aggregates, and the methanol is interposed between the entangled aggregates, and the entangled aggregates are gradually separated from the entangled aggregates, thereby creating a second suspension in which the aggregates are entangled with each other through the methanol and dispersed in the methanol; The aggregates are weighed so that the aggregates are formed on the surface of the amorphous powdered glass by a weight that is larger than 1 / 2 of the surface of the amorphous powdered glass, not on the entire surface of the amorphous powdered glass, and the weighed aggregate is placed in the container, the aggregate is stirred, and the aggregate is immersed in the second suspension. Furthermore, the container is placed on a vibration table of the vibrator. a third step of fixing the container on a surface of the container, operating the vibrator to repeatedly apply vibration acceleration in three directions, i.e., forward / backward, left / right, and up / down, to the container, thereby rearranging the clusters of amorphous powdered glass in the second suspension, whereby the clusters of amorphous powdered glass are overlapped with each other via a film made of the second suspension and having a thickness of less than 1 μm, and the overlapped clusters of amorphous powdered glass are formed on the bottom surface of the container as a cluster of amorphous powdered glass overlapped in a plane; A part of the amorphous powdered glass aggregate overlapping in a planar shape in the container is transferred to a new container as an amount required for producing a glass film, the new container is fixed on the vibration table of the vibrator, the vibrator is operated, and vibration acceleration in three directions, i.e., front-back, left-right, and up-down, is repeatedly applied to the new container, so that the amorphous powdered glass aggregates are overlapped with each other via the second suspension, and the overlapped aggregate of amorphous powdered glass is re-formed as an aggregate of amorphous powdered glass overlapping in a planar shape on the bottom surface of the new container. Furthermore, a new plate material that covers the entire surface of the amorphous powder glass aggregate in the new container is placed on the amorphous powder glass aggregate. After this, the new container is moved to a heat treatment device in a nitrogen atmosphere, and a compressive load smaller than the compressive strength of the amorphous powder glass is evenly applied to the entire surface of the new plate material, and the new container is heated to the softening point of the amorphous powder glass. As a result, first, methanol is evaporated from the second suspension, and the aggregate aggregate is formed on the surface of the amorphous powder glass at a temperature of 0.The amorphous powdered glass is precipitated with a thickness of less than 1 μm, and the aggregates form a region wider than 1 / 2 of the surface of the amorphous powdered glass, not the entire surface of the amorphous powdered glass, and also form a plurality of regions where the aggregates are not formed. Next, the amorphous powdered glass from which the aggregates are precipitated is softened, and the softened amorphous powdered glass is compressed and deformed so as to fill voids in the softened amorphous powdered glass, and a part of the softened amorphous powdered glass seeps out from the region where the aggregates are not formed in the softened amorphous powdered glass, and the softened amorphous powdered glass is compressed and deformed so as to fill voids in the softened amorphous powdered glass. a fourth step in which the softened amorphous powder glass particles are bonded to each other at contact points, and the contact points are bonded to each other through the aggregates by frictional heat; the softened amorphous powder glass particles are then left at the annealing point of the amorphous powder glass for 15 minutes or more, and then slowly cooled to room temperature, so that the strain generated in the amorphous powder glass particles when the softened amorphous powder glass particles are bonded to each other is released, and the softened amorphous powder glass particles are solidified, and the bonded parts of the amorphous powder glass particles are solidified, and the amorphous powder glass particles are bonded to each other to form a flat glass film on the bottom surface of the new container in the shape of the bottom surface; a fifth step of simultaneously applying an impact acceleration having the same magnitude to a plurality of points on the bottom surface of the new container, peeling off the glass film formed on the bottom surface of the new container from the bottom surface of the new container, and simultaneously applying an impact acceleration having the same magnitude as the impact acceleration to a plurality of points on the surface of the new plate, peeling off the glass film from the surface of the new plate, and removing the glass film; A method in which all of the above-mentioned five steps are carried out continuously is a method for producing a glass film that combines the light-blocking, heat-dissipating, and electrical conductivity of carbon black and the transparency of amorphous powdered glass.

[0011] That is, when the treatment in the five very simple steps described below is performed continuously, when the aggregates of carbon black are precipitated on the surface of the amorphous powder glass, they form a part wider than 1 / 2 of the surface, not on the entire surface of the amorphous powder glass, and also form a plurality of parts where aggregates are not formed. Furthermore, a compressive load is evenly applied to the entire aggregate of the amorphous powder glass, and the temperature is raised to the softening point of the amorphous powder glass. At this time, the amorphous powder glass softens, and the softened amorphous powder glass deforms so as to fill the voids in the aggregate of the softened amorphous powder glass, and a part of the softened amorphous powder glass exudes from the part where aggregates are not formed. At this time, in the adjacent softened powder glass, a part where the exuded softened amorphous powder glass contacts each other appears, and the contacting parts are bonded to each other. In addition, the contact parts of the softened amorphous powder glass are bonded to each other by frictional heat via the aggregate collection. As a result, a collection of amorphous glass powder, in which the amorphous glass powder particles are bonded together, is formed on the bottom surface of the new container as a planar glass film having the shape of the bottom surface. This glass film has, first, light-shielding and heat-dissipating properties due to the aggregates formed on the surface of the amorphous powdered glass, second, the transparency of the amorphous powdered glass is exhibited according to the occupancy rate of the area of ​​the portion on the surface of the amorphous glass where no aggregates are formed, and third, since the aggregates are continuously connected and formed on the surface of the amorphous powdered glass, the glass film has electrical conductivity according to the electrical conductivity of the aggregates. Here, the processing in the five steps and the effects of the processing will be described. The first step is a step of preparing a first suspension in which carbon black aggregates pulverized to a limit size are immersed in excess methanol. First, bead-shaped carbon black aggregates and methanol having a weight more than 10 times the weight of the carbon black aggregates are charged into a container, the methanol is stirred, and the carbon black aggregates, which have a density 2.3-2.7 times greater than that of methanol, are immersed in the excess methanol. In other words, the carbon black aggregates can be easily pulverized by compressing the bead-shaped carbon black aggregates immersed in the excess methanol. After this, a plate material that covers the entire surface of the carbon black aggregates in the container is placed on the carbon black aggregates, and a compressive load is evenly applied to the entire surface of the plate material to pulverize the carbon black aggregates immersed in the excess methanol. Furthermore, the plate material is lifted from the container, the container is fixed on the vibration table of the vibrator, the vibrator is operated, and vibration acceleration in three directions, front-back, left-right, and up-down, is repeatedly applied to the container at a vibration acceleration of 2-3G depending on the size of the container, and the crushed carbon black clusters are rearranged in excess methanol. That is, in the bead-shaped carbon black clusters, the size of the carbon black varies, and the size of the crushed carbon black also varies. For this reason, voids are formed in the crushed carbon black clusters. In order to fill these voids, vibration acceleration in three directions, front-back, left-right, and up-down, is repeatedly applied to the container, the crushed carbon black clusters are rearranged in excess methanol, and the rearranged carbon black clusters are crushed again, so that the crushing of all the carbon black proceeds and the size of the crushed carbon black approaches uniformity. Furthermore, the plate material is placed over the carbon black clusters in the container again, and the compression load is applied evenly to the entire surface of the plate material again, and the crushing of the carbon black clusters is further proceeded in excess methanol. The plate is then pulled out of the container again, and the vibration acceleration in the three directions is repeatedly applied to the container again. The pair of processes consisting of the process of applying a compressive load and the process of applying a vibration acceleration are repeated, and when a repulsive force is generated in the plate when the compressive load is applied to the plate, it is determined that the grinding of the carbon black aggregates immersed in the excess methanol is completed, and the pair of processes is stopped.After this, the plate is removed from the container. In other words, when the crushing of the carbon black by the compression of the plate reaches its limit, compressive stress is applied to the crushed carbon black when the crushed carbon black clusters are compressed, but the carbon black is not crushed and a repulsive force is generated in the plate. At this point, it is determined that the crushing of the carbon black clusters is completed. As a result, the bead-like carbon black is crushed to a size of about 1 / 25 of its original size and becomes a cluster of loose fine particles, and a first suspension is prepared in which the cluster of loose fine particles is immersed in excess methanol. The second step is a step of converting the first suspension into a second suspension in which each aggregate, which is entangled with each other, is dispersed in excess methanol. That is, in order to produce a glass film, it is necessary to overlap amorphous powdered glass on the surface of which aggregates are formed, and to make the overlapped powdered glass into a flat-shaped aggregate of powdered glass. For this reason, in the third step, the amorphous powdered glass is overlapped with each other via a film made of the second suspension and having a thickness of less than 1 μm, and the overlapped aggregate of amorphous powdered glass is stacked in a flat shape. Furthermore, in the fourth step, methanol is evaporated from the second suspension, and the aggregates are precipitated on the surface of the amorphous powdered glass, and the aggregates form a thickness of less than 0.1 μm on the surface of the amorphous powdered glass. In this way, in order to overlap amorphous powdered glass on which aggregates are formed, it is necessary to produce a second suspension in which each aggregate, which is entangled with each other, is dispersed in methanol. Meanwhile, a collection of loose fine particles is immersed in excess methanol in the container. Therefore, when the homogenizer device is operated in the first suspension, a collection of shock waves smaller than the aggregates is continuously generated in the excess methanol, and a collection of fine shock waves propagates through the excess methanol. As a result, a collection of fine shock waves continuously enters the inside of the loose fine particles immersed in the excess methanol. In the collection of agglomerates constituting the loose fine particles, the agglomerates are bonded to each other by the interaction of van der Waals forces. Therefore, the bonding force between the agglomerates is small. Furthermore, in the agglomerates, the aggregates are entangled with each other, and the aggregates are bonded to each other by the interaction of van der Waals forces. Therefore, the bonding force between the aggregates in the agglomerates is also small. For this reason, when a collection of fine shock waves continuously enters the interior of a loose particle, the bonds between the agglomerates are continuously irradiated with the shock waves propagating through the methanol, causing the bonds between the agglomerates to dissociate and separate into individual agglomerates.Similarly, the shock waves propagating through the methanol are continuously irradiated to the bonded portions of the aggregates in the agglomerates, dissociating the bonds between the aggregates and separating the entangled aggregates into individual aggregates. Furthermore, when the shock waves are repeatedly irradiated to the collection of aggregates, the collection of entangled aggregates becomes a second suspension dispersed in excess methanol. In other words, aggregates are easily entangled when they are formed because aggregates are formed by a collection of fine carbon particles. The number and size of the carbon particles that make up the aggregates and the length and shape of the aggregates vary, so the aggregates are intricately entangled, the number of entangled aggregates varies, and the entangled parts also vary. Such a collection of intricately entangled aggregates cannot be evenly dispersed in methanol. On the other hand, if shock waves smaller than the size of the aggregates are continuously irradiated to a collection of intricately entangled aggregates through excess methanol, the shock waves are first irradiated to the entangled parts of the aggregates, the entangled parts of the aggregates are temporarily released, and methanol is interposed in the entangled parts. Furthermore, shock waves are continuously irradiated to the aggregates in which the aggregates are entangled through methanol, and the entangled aggregates move slightly from the entangled parts. Furthermore, as the shock waves are continuously applied, the distance that the aggregates move from the entangled site increases. As this phenomenon of the aggregates moving from the entangled site gradually progresses and the distance from the entangled site of the aggregates continues to increase, the collection of aggregates in which the aggregates are entangled with each other through the methanol is evenly dispersed in the excess methanol. Based on this idea, shock waves smaller than the aggregates were continuously applied to the first suspension. That is, when a homogenizer device is placed in a container and operated in excess methanol, a collection of shock waves smaller than the aggregates is continuously generated in the excess methanol, the shock waves move through the methanol while exciting the methanol molecules. On the other hand, since the viscosity of methanol is low and the molecular weight is small, the proportion of energy consumed when the methanol molecules are excited by the shock waves is small, and the energy of the shock waves is not easily lost. Therefore, a collection of fine shock waves is continuously irradiated through the methanol into the inside of the loose particles. As a result, firstly, in the collection of agglomerates, shock waves are continuously irradiated through the methanol to the bond between the agglomerates, and the bonds between the agglomerates are dissociated, and the agglomerates are separated into individual agglomerates. Secondly, shock waves are continuously irradiated through the methanol to the bond between the aggregates in the agglomerates, and the bonds between the aggregates are dissociated, and the aggregates are separated into individual aggregates in which they are entangled. As a result, the collection of loose particles becomes a collection of aggregates in which aggregates are entangled with each other. Third, the shock wave is continuously irradiated to the aggregates in which aggregates are entangled with each other, the entangled portion of the aggregates is temporarily released, and methanol is interposed in the entangled portion of the aggregates. Fourth, the shock wave is continuously irradiated to the aggregates in which aggregates are entangled with each other, and the aggregates move slightly from the entangled portion. Fifth, the shock wave is continuously irradiated to the aggregates in which aggregates are entangled with each other, and the distance that the aggregates move from the entangled portion gradually increases. This phenomenon of the aggregates moving from the entangled portion progresses, and sixthly, the distance of the aggregates in which aggregates are entangled with each other gradually increases, and a second suspension in which the aggregates in which aggregates are entangled with each other through methanol are evenly dispersed in excess methanol is created. In addition, the aggregates are structures in which carbon particles are strung together, and have an irregular and complex shape. In addition, the number and size of the carbon particles, the length of the aggregates, and the shape of the structure vary, so the number of entangled aggregates and the positions at which the aggregates are entangled vary widely. For this reason, even if the shock waves emitted by the homogenizer device are repeatedly irradiated to a collection of aggregates in which aggregates are entangled, it is not easy to release all the entanglements between the aggregates, separate them into individual aggregates, and further disperse the separated aggregates one by one evenly in excess methanol. In other words, the separation of entanglement between aggregates by the homogenizer device is a process in which methanol is interposed at the site where the aggregates are directly entangled with each other, and the collection of aggregates entangled through methanol is dispersed in excess methanol. In other words, it is sufficient to create a second suspension in which the aggregates entangled through methanol are evenly dispersed in methanol. As a result, the density of the powdered glass is 3.2-9.3 times that of methanol and 1.2-4.1 times that of carbon black, so that the amorphous powdered glass can be overlapped with the second suspension by the third step, and the overlapped amorphous powdered glass can be stacked in a flat shape. Furthermore, when the methanol is evaporated from the second suspension in the fourth step, aggregates are precipitated on the surface of the amorphous powdered glass. The density of carbon black is 1.8-2.1 g / cm 3 The density of powdered glass varies greatly depending on the composition, ranging from 2.5 to 7.4 g / cm 3 It is. When an ultrasonic homogenizer is used as the homogenizer, a huge number of bubbles smaller than the size of the aggregates are generated at the same time, and then the bubbles disappear almost simultaneously. The generation and disappearance of the bubbles occurs repeatedly according to the frequency of the ultrasonic waves, and the generation and disappearance of the bubbles are repeated in the low-viscosity methanol (this phenomenon is called cavitation). Shock waves generated when the bubbles burst are continuously generated in the low-viscosity and low-density methanol, and most of the energy of the shock waves is not absorbed by the excitation of the methanol, but is continuously irradiated to the fine parts of the crushed carbon black. Therefore, the ultrasonic homogenizer repeats the generation and disappearance of the bubbles according to the frequency of the ultrasonic waves, so that the second suspension can be prepared in a relatively short time. The third step is a step of forming a collection of powdered glass, in which the amorphous powdered glass is overlapped with the second suspension, on the bottom surface of the container as a collection of powdered glass overlapped in a plane. Meanwhile, in order to provide the glass film to be formed with both the light-shielding property, heat dissipation property, and electrical conductivity of carbon black and the transparency of amorphous powdered glass, it is necessary to deposit the area where aggregates are formed on the surface of the amorphous powdered glass on a site wider than 1 / 2 of the surface of the amorphous powdered glass, rather than on the entire surface of the amorphous powdered glass. This ensures that a plurality of sites on the surface of the amorphous powdered glass where aggregates are not formed are reliably formed, and the plurality of sites have a certain area and ensure the transparency of the amorphous powdered glass by the plurality of sites where aggregates are not formed. In other words, among the plurality of sites where aggregates are not formed, there are sites where visible light does not pass through, even if the site where aggregates are not formed has a width shorter than the wavelength of visible light. However, if the total area of ​​a plurality of areas where aggregates are not formed has a certain area narrower than 1 / 2 of the surface of the amorphous powdered glass, there is certainly a portion that transmits visible light, and the presence of this portion ensures that the amorphous powdered glass exhibits transparency. As a result, the portion on the surface of the amorphous powdered glass where aggregates are formed provides the light blocking, heat dissipation, and electrical conductivity of carbon black. In addition, the plurality of portions on the surface of the amorphous powdered glass where aggregates are not formed provide transparency for the amorphous powdered glass. For this reason, first, the aggregates of the amorphous powdered glass are weighed so that the aggregates of the amorphous powdered glass form a portion wider than 1 / 2 of the surface of the amorphous powdered glass, not the entire surface of the amorphous powdered glass, and the weighed amorphous powdered glass is put into a container and the aggregates of the amorphous powdered glass are stirred. This causes the mass of amorphous powdered glass to become immersed in the second suspension since the density of amorphous powdered glass is 3.2-9.3 times the density of methanol and 1.2-4.1 times the density of carbon black.The volume of the aggregate of amorphous powdered glass calculated based on the weight and density is 1.2 to 4.1 times the volume of the aggregate of carbon black calculated based on the weight and density. In addition, whether the area where aggregates are formed on the surface of the amorphous powdered glass is not the entire surface of the amorphous powdered glass but is a part wider than 1 / 2 of the surface of the amorphous powdered glass is determined by continuously performing the treatments in the five steps of the present invention, and determining whether the area where aggregates are formed on the surface of the amorphous powdered glass is not the entire surface of the amorphous powdered glass but is a part wider than 1 / 2 of the surface of the amorphous powdered glass as an average surface area of ​​the amorphous powdered glass, based on the results of the light blocking rate, thermal emissivity, and visible light transmittance of the glass film produced. In other words, if the measurement results of the light blocking rate and thermal emissivity of the glass film are 50% or more and less than 100% of the light blocking rate and thermal emissivity of carbon black, it is determined that the occupancy rate of the average surface area where aggregates are formed on the surface of the amorphous powdered glass is greater than 50% and less than 100%. At the same time, if the measurement result of the visible light transmittance of the glass film is greater than 0% and less than 50%, it is determined that there are certainly areas on the surface of the amorphous powdered glass where aggregates are not formed. Next, the container is fixed on the vibration table of the vibrator, and the vibrator is operated to repeatedly apply vibration acceleration in three directions, front and back, left and right, and up and down, at a vibration acceleration of 2-3 G depending on the size of the container, to the container, and the amorphous powder glass aggregates are rearranged in the second suspension. As a result, the aggregates of the powder glass, in which the amorphous powder glass particles overlap each other via the second suspension, are formed on the bottom surface of the container as an aggregate of powder glass overlapped in a plane. As a result, the surface of all the amorphous powder glass is covered with the second suspension. Note that since the viscosity of methanol is low at 20°C, 0.59 mPa·sec, the thickness of the second suspension adsorbed on the surface of the amorphous powder glass is less than 1 μm. Meanwhile, in the second suspension, aggregates in which aggregates are entangled with each other via methanol are evenly dispersed in the methanol. Therefore, in the treatment of the fourth step, when methanol evaporates from the second suspension, aggregate clusters precipitate on the surface of the amorphous powdered glass, and the aggregate clusters do not form the entire surface of the amorphous powdered glass, but form areas that are larger than 1 / 2 of the surface of the amorphous powdered glass, and the areas where aggregates are not formed are formed on the surface of the powdered glass as multiple areas whose number corresponds to the weight of the carbon black clusters. The fourth step is to uniformly compress the entire amorphous powder glass having aggregates formed on its surface, soften the amorphous powder glass, and bring adjacent softened powder glass portions into contact with each other in the softened amorphous powder glass portions, and bond the contact portions. The contact portions of the softened powder glass portions are bonded by frictional heat via the aggregates. As a result, the bonded powder glass portions are formed on the bottom surface of a new container as a planar glass film having the shape of the bottom surface. For this reason, a portion of the planar overlapping amorphous powder glass portions formed in the third step is transferred to a new container in an amount required for the area and thickness of the glass film to be formed. Furthermore, a new container is fixed on the vibration table of the vibrator, the vibrator is operated, and vibration accelerations in three directions, front and back, left and right, and up and down, are repeatedly applied to the new container at a vibration acceleration of 2-3 G depending on the size of the container, so that the amorphous powdered glass overlaps with the second suspension, and the overlapped collection of powdered glass is formed again on the bottom surface of the new container as a collection of powdered glass overlapped in a flat shape. Furthermore, a new plate material that covers the entire surface of the collection of powdered glass is placed on top of the collection of powdered glass. After this, the new container is moved to a heat treatment device in a nitrogen atmosphere. Furthermore, a compressive load smaller than the compressive strength of the amorphous powdered glass is evenly applied to the entire surface of the new plate material, and the new container is heated to the softening point of the amorphous powdered glass. At this time, first, methanol evaporates from the second suspension, and aggregates are precipitated on the surface of the amorphous powdered glass with a thickness less than 0.1 μm, but the area formed on the surface of the amorphous powdered glass is not the entire surface of the amorphous powdered glass, but an area wider than 1 / 2 of the surface of the amorphous powdered glass, and areas where aggregates are not formed are formed on the surface of the amorphous powdered glass as a plurality of areas whose number corresponds to the weight of the carbon black aggregates. After this, the amorphous powdered glass on whose surface the aggregates are formed softens, and the softened amorphous powdered glass is compressed, and the softened amorphous powdered glass is deformed so as to fill the voids in the softened amorphous powdered glass aggregates.At this time, a part of the softened powder glass seeps out from the part where aggregates are not formed. In adjacent softened powder glass, there are parts where parts where aggregates are not formed contact each other, and the contact parts are bonded to each other by compressive stress. In addition, the contact parts of the softened powder glass are bonded to each other by frictional heat through a collection of aggregates. Note that the contact parts of the softened powder glass correspond to the convex parts of the unevenness on the surface of the softened powder glass, and since the contact parts are extremely numerous, the softened powder glass is firmly bonded to each other by frictional heat. On the other hand, since the volume of the contact parts is extremely small, the frictional heat is generated in a short time and disappears instantly. As a result, the bonded collection of amorphous powder glass is created on the bottom surface of the new container as a planar glass film having the shape of the bottom surface. That is, the size of the aggregate is smaller than that of the amorphous powdered glass by one order of magnitude or more, and the size and shape of the aggregate vary. Meanwhile, the amorphous powdered glass overlaps with each other through the second suspension having a thickness of less than 1 μm. Therefore, when methanol evaporates from the overlapping amorphous powdered glass, aggregates are precipitated on the surface of the powdered glass all at once, but the aggregates are not precipitated on the entire surface of the amorphous powdered glass, but on a portion wider than 1 / 2 of the surface of the amorphous powdered glass. At this time, the portion where no aggregates are formed is formed on the surface of the amorphous powdered glass as a plurality of portions consisting of a number according to the weight of the carbon black aggregates. After this, the powdered glass is softened by heating. Furthermore, the softened powdered glass aggregate is compressed evenly by a new plate material, and the softened powdered glass is deformed so as to fill the voids in the softened powdered glass aggregate. On the other hand, since a plurality of areas where aggregates are not formed are formed on the surface of the softened powdered glass, when the softened powdered glass is deformed under stress, a part of the softened powdered glass is preferentially exuded from the areas where aggregates are not formed on the surface of the softened powdered glass. Therefore, when adjacent pieces of softened powdered glass exuding from areas where aggregates are not formed come into contact with each other, the softened powdered glass exuding from the areas is bonded to each other at the contact area because stress is continuously applied to the softened powdered glass. In addition, the surface of the powdered glass except for the areas where aggregates are not formed has a thickness of less than 0.1 μm formed by the aggregate collection. Therefore, when the softened powdered glass collection is compressed, the softened powdered glass is bonded to each other at the contact area by frictional heat via the aggregate collection. After this, the softened collection of powdered glass is left at the annealing point of the powdered glass for more than 15 minutes and then annealed to room temperature. The distortion that occurred in the powdered glass when the softened powdered glass was joined together is released from the glass film, the softened powdered glass solidifies, and the joints between the powdered glass also solidify. As a result, a planar glass film made of the collection of solidified powdered glass is formed on the bottom surface of the new container in the shape of the bottom surface. The softening point of the powdered glass exceeds 500°C, which is the spontaneous ignition point of carbon black. Therefore, a new container was moved to a heat treatment device in a nitrogen atmosphere, and the collection of powdered glass in which the powdered glass was overlapped through the second suspension was heat-treated in a nitrogen atmosphere. In addition, since the compressive strength of the powdered glass is large at 45-55 MPa, the compressive stress compressing the collection of softened powdered glass is large, and the contact parts of the softened powdered glass are firmly bonded to each other by frictional heat through the collection of aggregates. The fifth step is a step of peeling off the flat glass film from the bottom of the new container, and peeling off the flat glass film from the surface of the new plate material to take out the flat glass film. For this purpose, an impact acceleration of the same magnitude is simultaneously applied to multiple locations on the bottom of the new container as an impact acceleration of 0.2-0.3G depending on the size of the new container, and the flat glass film is peeled off from the bottom of the new container. Furthermore, an impact acceleration of the same magnitude as the impact acceleration is simultaneously applied to multiple locations on the surface of the new plate material to peel off the flat glass film from the surface of the new plate material. As a result, the flat glass film is taken out. In addition, the glass film is bonded to the softened powder glass that has oozed out, and the contact parts of the softened powder glass are bonded to each other by frictional heat through the collection of aggregates, so that the bonding force between the powder glass is large, and further, since the glass film is lightweight, the glass film does not break even when subjected to an impact acceleration of 0.2-0.3G. On the other hand, the amorphous powdered glass constituting the glass film has a thickness of 0.1 μm or less and is formed as aggregates. Therefore, the glass film has the properties of aggregates. In addition, there are many areas on the surface of the amorphous powdered glass where aggregates are not formed. Therefore, the glass film has a slightly blackish color, but does not lose the transparency of the amorphous powdered glass. In other words, the glass film exhibits transparency depending on the occupancy rate of the area of ​​the area on the surface of the amorphous powdered glass where aggregates are not formed. Conversely, the glass film has a reduced light blocking property and heat dissipation property due to the aggregates depending on the occupancy rate of the area of ​​the area on the surface of the amorphous powdered glass where aggregates are not formed. The glass film thus produced has the following effects. First, the surface of the powdered glass, excluding the areas where the softened powdered glass has seeped out, is made up of aggregates thinner than 0.1 μm in thickness, so the flat glass film has the properties of an aggregate. On the other hand, carbon black has a total light transmittance close to 0% and has excellent light blocking properties. Therefore, the glass film has the function of filtering out ultraviolet rays. Also, carbon black absorbs far-infrared rays, so the glass film absorbs far-infrared rays. On the other hand, carbon black has a high thermal emissivity of 0.95-0.97, so the glass film acts as a heat dissipation film, and the glass film is resistant to thermal degradation even when exposed to far-infrared rays for a long period of time. Secondly, aggregates are formed in a region of the amorphous powdered glass that is wider than 1 / 2 of the surface, and the aggregates are connected to form a glass film. On the other hand, the resistivity of carbon black is six orders of magnitude greater than that of metals, but 13 orders of magnitude smaller than that of synthetic resins. Therefore, the glass film thus produced acts as a glass film that combines the functions of electrical conductivity, electromagnetic shielding, and antistatic properties based on the electrical conductivity of carbon black. In addition, carbon black has thermal conductivity based on electrical conductivity, so the glass film acts as a heat dissipation film as well as a heat conduction film, thereby enhancing the heat dissipation of the glass film. Thirdly, among the multiple areas where aggregates are not formed on the surface of the amorphous glass, there are certainly areas through which visible light passes, and the glass film exhibits the transparency of amorphous powdered glass depending on the total area of ​​the areas through which visible light passes. Fourth, a glass film made of an aggregate of powdered glass bonded together has higher mechanical strength than a synthetic resin film of the same thickness. In addition, since powdered glass and carbon black have better heat resistance, flame retardancy, and corrosion resistance than synthetic resin, the glass film produced has better heat resistance, flame retardancy, and corrosion resistance than synthetic resin films. Fifth, the surface of the glass film made of powdered glass bonded together is water-repellent, meaning that all liquids are repelled by surface tension. Sixth, since the area and shape of the glass film to be produced are determined by the shape of the bottom surface of the new container, the area and shape of the glass film to be produced can be freely changed. Seventh, since the thickness of the glass film to be produced is determined by the amount of suspension filled in a new container, the thickness of the glass film to be produced can be freely changed. Eighth, the aggregates constituting the glass film can be cut into primary particles. In addition, the powdered glass constituting the glass film has a thickness of submicrons, so the powdered glass can also be cut. Therefore, the glass film produced can be cut into glass films of various sizes and shapes. Ninth, carbon black and powdered glass are inexpensive industrial materials, and methanol is the most commonly used organic solvent. Furthermore, all of the five steps in the process of producing the glass film are extremely simple. Therefore, inexpensive glass films can be produced using inexpensive raw materials with low processing costs. Tenth, the glass film can be made safely: the carbon black is treated in methanol, so it does not scatter as dust, and the heat treatment is done in a nitrogen atmosphere, so the aggregates do not ignite. Eleventh, since the glass film is produced using amorphous powdered glass as a raw material, the glass film produced using amorphous powdered glass of various compositions as a raw material provides the first to tenth effects. As described above, the glass film produced has various excellent effects. This solves the first problem described in paragraph 9. In addition, the glass film produced can be used for various purposes based on the various effects.

[0012] A method for producing a glass film having the light-shielding, heat-dissipating and electrical conductivity of carbon black described in paragraph 10 and the transparency of amorphous powdered glass is as follows: The carbon black described in paragraph 10 is Ketjen black, and a method of using this Ketjen black as the carbon black described in paragraph 10 and continuously carrying out all of the five steps described in paragraph 10 according to the method described in paragraph 10 is a method for producing a glass film that combines the light-blocking, heat-dissipating, and electrical conductivity of the carbon black described in paragraph 10 and has the transparency of amorphous powdered glass.

[0013] In other words, among carbon blacks, Ketjenblack has the smallest primary particles, the largest number of primary particles per unit mass, and the largest BET surface area, and therefore has the best light blocking properties among carbon blacks. Therefore, when Ketjenblack is used as the carbon black, the glass film made by the method described in paragraph 10 acts as a glass film that is excellent at removing ultraviolet rays and absorbing far infrared rays. In addition, Ketjenblack has a high thermal emissivity of 0.97, and acts as an excellent heat dissipation film. Furthermore, Ketjenblack has the second highest electrical conductivity among carbon blacks after acetylene black, and therefore the glass film made by the method described in paragraph 10 acts as an electrically conductive glass film. That is, Ketjen Black has a primary particle diameter of 30-40 nm, and therefore the number of primary particles per unit mass is 1 x 10 7 / g and a BET surface area of ​​1270m 2 / g. In addition, Ketjenblack has a high thermal emissivity of 0.97. Therefore, the glass film described in paragraph 10 has better light blocking and heat dissipation properties than glass films made of other carbon black aggregates.

[0014] A method for producing a glass film having the light-shielding, heat-dissipating and electrical conductivity of carbon black described in paragraph 10 and the transparency of amorphous powdered glass is as follows: The carbon black described in paragraph 10 is acetylene black, and a method of using the acetylene black as the carbon black described in paragraph 10 and continuously carrying out all of the five steps described in paragraph 10 according to the method described in paragraph 10 is a method for producing a glass film that combines the light-blocking, heat-dissipating and electrical conductivity of the carbon black described in paragraph 10 and has the transparency of amorphous powdered glass.

[0015] In other words, acetylene black is produced using acetylene gas, which has the highest purity among the raw materials for carbon black, and therefore has the fewest impurities among all carbon blacks, and also has the most developed structure and primary particles. For this reason, it has the highest conductivity among all carbon blacks, and glass films using acetylene black have superior conductivity, electromagnetic shielding properties, and antistatic performance compared to glass films using other carbon blacks. In addition, because it has the most developed structure and primary particles, acetylene black aggregates are easily entangled. This increases the mechanical strength of the glass film. For example, acetylene black having a bulk density of 0.04 g / cm 3 There is a powder product with an electrical resistivity of 0.21 Ω cm. Although the light blocking and heat radiation properties of acetylene black are not as good as those of ketjen black, it has the light blocking and heat radiation properties of carbon black, so glass films have light blocking and heat radiation properties. Therefore, when acetylene black is used as the carbon black and a glass film is produced in accordance with the method described in paragraph 10, the glass film combines the electrical conductivity, electromagnetic shielding properties, and antistatic properties based on the electrical conductivity of acetylene black, while also possessing the light-blocking and thermal radiation properties of acetylene black.

[0016] A method for bonding a glass film prepared by the method described in any one of paragraphs 10, 12, or 14 to a surface of a substrate or part, comprising: a glass film prepared by the method described in any one of paragraphs 10, 12, and 14 is placed at a predetermined position on a surface of a substrate or a component, and a compressive load smaller than the compressive strength of the powdered glass described in any one of paragraphs 10, 12, and 14 is evenly applied to the entire surface of the glass film, compressing the entire surface of the glass film; thereby, frictional heat is generated at a portion where the back surface of the glass film contacts the surface of the substrate or the surface of the component, and the glass film is bonded to the surface of the substrate or the surface of the component by the frictional heat; Or, The method includes cutting a glass film prepared by the method described in any one of paragraphs 10, 12 or 14 into a predetermined shape, placing the cut glass film at a predetermined position on the surface of a substrate or a part, and evenly applying a compressive load smaller than the compressive strength of the powdered glass described in any one of paragraphs 10, 12 or 14 to the entire surface of the cut glass film, thereby compressing the entire surface of the cut glass film, thereby generating frictional heat at the location where the back surface of the cut glass film comes into contact with the surface of the substrate or the surface of the part, and the frictional heat bonds the cut glass film to the surface of the substrate or the surface of the part.

[0017] That is, when a glass film prepared by the method described in any one of paragraphs 10, 12, or 14 is placed at a predetermined position on a substrate or component, and a compressive load smaller than the compressive strength of the powdered glass described in any one of paragraphs 10, 12, or 14 is evenly applied to the entire surface of the glass film to compress the glass film, the aggregates formed on the surface of the glass film are slightly elastically deformed, and the back surface of the glass film is in close contact with the surface of the substrate or component, and frictional heat is generated for a short time at all contact sites that come into contact with the convex parts of the unevenness of the intimately contacted surface, and the frictional heat disappears instantly because the volume of the contact sites is small. This frictional heat bonds the lightweight glass film to the surface of the substrate or component. In addition, when a film produced by the method described in any one of paragraphs 10, 12, and 14 is cut into a predetermined shape, the cut glass film is placed at a predetermined position on a substrate or a component, and a compressive load smaller than the compressive strength of the powdered glass described in any one of paragraphs 10, 12, and 14 is applied to the entire surface of the glass film to compress the glass film, the aggregates formed on the surface of the glass film are slightly elastically deformed, the back surface of the glass film is in close contact with the surface of the substrate or the component, and frictional heat is generated for a short time at all contact sites that come into contact with the convex parts of the unevenness of the intimately contacted surface, and the frictional heat disappears instantaneously because the volume of the contact sites is small. This frictional heat bonds the lightweight glass film to the surface of the substrate or the component. The glass film is made of powdered glass with aggregates formed on the surface. On the other hand, aggregates are a collection of carbon particles that are bonded together in a beaded shape, and the carbon particles can be cut. In addition, most powdered glass is thin, at submicron thickness, so powdered glass can also be cut. Therefore, the glass film can be cut into any shape. That is, the unevenness of the surface of the substrate or part is small, at submicron size, but the number of protrusions that come into contact with the surface of the glass film is enormous. On the other hand, the surface of the glass film is formed of a collection of aggregates. When the entire glass film is compressed evenly with a compression load smaller than the compressive strength of the powdered glass, the collection of aggregates is slightly elastically deformed. For this reason, when the glass film arranged on the surface of the substrate or part is compressed, the glass film adheres to the surface of the substrate or part, and frictional heat is instantaneously generated at all contact points where the convex parts of the unevenness of the adhered surface come into contact with the surface of the glass film. This frictional heat bonds the glass film at the contact points to the convex parts of the unevenness of the surface of the substrate or part. Since the number of convex parts at the contact points is enormous, the distance between the contact points is short, and the glass film is lightweight, the surface of the glass film is firmly bonded to the surface of the substrate or part. The ignition temperature of carbon black in the atmosphere exceeds 500°C. On the other hand, frictional heat is generated in a short time and is cooled instantly because the contact area has an extremely small volume, so the temperature of the aggregates at the contact area is significantly lower than the ignition temperature of carbon black. In addition, the surface of the glass film is bonded to the surface of the substrate or part by the frictional heat generated in a short time and the frictional heat that is then instantaneously cooled. Therefore, even if the substrate or part is a synthetic resin with low heat resistance, or a cloth or nonwoven fabric, the lightweight glass film is bonded to the surface of the substrate or part. Furthermore, as explained in the third effect of the glass film described in the tenth paragraph, the area and shape of the glass film to be created can be freely changed. Furthermore, as explained in the fifth effect of the glass film described in the tenth paragraph, the glass film can be cut into various sizes and shapes. Therefore, the glass film can be bonded to substrates or parts made of various materials, and further to substrates or parts made of various sizes and shapes, by an extremely simple means called friction welding. As a result, glass films of various sizes and shapes having light shielding properties are formed on the surfaces of substrates or parts made of various materials. Also, glass films of various sizes and shapes having a certain thermal emissivity are formed on the surfaces of substrates or parts made of various materials. Furthermore, glass films of various sizes and shapes having the functions of conductivity, electromagnetic shielding, and antistatic properties based on the conductivity of carbon black are formed on the surfaces of substrates or parts made of various materials. In addition, the surface of the glass film bonded to the surface of the substrate or part has water repellency, which repels all liquids due to surface tension. This provides excellent corrosion resistance to the substrate or part to which the glass film is pressed using frictional heat. When the glass film is pressed against, for example, a window pane by frictional heat, it becomes a pane with a function of removing ultraviolet rays. Carbon black absorbs far-infrared rays, so when the glass film is pressed against, for example, a window pane by frictional heat, it becomes a pane that absorbs far-infrared rays. On the other hand, because the thermal emissivity of carbon black is as high as 0.95-0.97, the glass film acts as a heat dissipation film, and the glass film is not easily deteriorated by heat even if the pane is irradiated with far-infrared rays for a long period of time. The glass film also acts as a shatterproof film for the window pane. Furthermore, when the mixing ratio of carbon black to amorphous powdered glass is increased, the transparency of the glass film decreases, but the glass film exhibits the function of a privacy film for the window pane. Furthermore, the glass film is bonded to the surface of a substrate or part by the frictional heat generated in a short period of time and then instantaneous cooling. Therefore, the substrate or part is not limited to window glass sheets, and substrates or parts made of various materials with low heat resistance, and further substrates or parts of various sizes and shapes can be bonded by the extremely simple means of friction welding.

[0018] The method for producing the glass film described in paragraph 10 is a method for producing a glass film that combines the light blocking, heat dissipation, and electrical conductivity of carbon black, and the thermal shock resistance and mechanical strength of crystalline powder glass, and the method for producing the glass film is as follows: The first change in the process in the third step described in paragraph 10 is that the powdered glass put into the container in the third step is not amorphous powdered glass but crystalline powdered glass, the crystalline powdered glass is weighed to determine the weight at which aggregates are formed over the entire surface of the crystalline powdered glass, and the weighed crystalline powdered glass is put into the container. The second change in the process in the fourth step described in paragraph 10 is that the temperature to which the new container is heated in the fourth step described in paragraph 10 is the crystallization temperature of the crystalline powdered glass rather than the softening point of the amorphous powdered glass. The method of continuously carrying out the five steps described in paragraph 10 reflecting these two changes is a method for producing a glass film that has both the light-blocking, heat-dissipating, and electrical conductivity of carbon black and the thermal shock resistance and mechanical strength of crystalline powdered glass.

[0019] That is, when the crystalline glass powder is heated to the crystallization temperature, the crystals of the powdered glass grow and become crystalline powdered glass. The crystalline glass powder is divided into two types: one that has both a softening point and a crystallization temperature higher than the softening point (called DTA characteristics) by differential thermal analysis, and one that has a transition point but does not have a softening point higher than the transition point and has a crystallization temperature higher than the transition point. However, when any type of crystalline powdered glass is heated to the crystallization temperature, the powdered glass becomes crystalline powdered glass. The crystalline powdered glass does not have the transparency of the amorphous powdered glass, but has superior thermal shock resistance and mechanical strength to the amorphous powdered glass. For this reason, in the fourth step described in paragraph 10, the temperature to which the new container is heated is not the softening point of the amorphous powdered glass, but the crystallization temperature of the crystalline powdered glass. As a result, the glass film produced by the method described in paragraph 10 becomes a glass film that has both the thermal shock resistance and mechanical strength of the crystalline powdered glass. In addition, since crystalline powdered glass does not have the transparency of amorphous powdered glass, there is no need to form areas on the surface of the crystalline powdered glass where aggregates are not formed, as in the case of amorphous powdered glass. Therefore, in the third step described in paragraph 10, the aggregates of crystalline powdered glass are weighed to determine the weight of aggregates formed on the entire surface of the crystalline powdered glass, and the weighed aggregates of crystalline powdered glass are put into a container. As a result, aggregates are formed on the entire surface of the crystalline powdered glass, and the glass film is given the three properties of carbon black, namely light blocking, heat dissipation, and electrical conductivity, which are enhanced compared to the glass film made using the amorphous powdered glass described in paragraph 10. In addition, whether aggregates are formed on the entire surface of the crystalline powdered glass is determined by continuously performing the five steps of the present invention, and judging whether the area where aggregates are formed on the surface of the crystalline powdered glass is the entire surface of the crystalline powdered glass based on the results of the light blocking rate and thermal emissivity of the glass film produced. In other words, if the measurement results of the light blocking rate and thermal emissivity of the glass film are 100% of the light blocking rate and thermal emissivity of carbon black, it is determined that aggregates are formed on the entire surface of the crystalline powdered glass. Therefore, in the third step described in paragraph 10, the aggregates of the crystalline powdered glass are weighed to determine the weight of aggregates formed on the entire surface of the crystalline powdered glass, and the weighed aggregates of the crystalline powdered glass are placed in a container, and the aggregates precipitate on the entire surface of the crystalline powdered glass in the fourth step described in paragraph 10. As a result, a glass film that combines the light blocking, heat dissipation, and electrical conductivity of carbon black is produced by using the amorphous powdered glass. Therefore, in the method for producing a glass film that has both the light blocking, heat dissipation, and electrical conductivity of carbon black and the thermal shock resistance and mechanical strength of crystalline powdered glass, the powdered glass put into the container in the third step described in paragraph 10 is not amorphous powdered glass but crystalline powdered glass, and the crystalline powdered glass aggregates are weighed to represent the weight of aggregates formed on the entire surface of the crystalline powdered glass, and the weighed crystalline powdered glass aggregates are put into the container. This is a change in the process in the third step. By reflecting the first change and the second change in the processing in the fourth step described in paragraph 10, which is that the temperature to which the new container is heated in the fourth step described in paragraph 10 is the crystallization temperature of the crystalline powdered glass rather than the softening point of the amorphous powdered glass, in the processing method in the five steps described in paragraph 10 and continuously carrying out the processing method in the five steps described in paragraph 10 reflecting these two changes, a glass film is produced that combines the light-blocking, heat-dissipating, and electrical conductivity of carbon black, and the thermal shock resistance and mechanical strength of the crystalline powdered glass.

[0020] The method for bonding a glass film having the light-shielding, heat-dissipating, and electrical conductivity of carbon black described in paragraph 18 and the thermal shock resistance and mechanical strength of crystalline powdered glass to the surface of a substrate or part is as follows: a glass film prepared by the method described in paragraph 18 is placed at a predetermined position on a surface of a substrate or a component, and a compressive load smaller than the compressive strength of the crystalline powdered glass described in paragraph 18 is evenly applied to the entire surface of the glass film, thereby compressing the entire surface of the glass film, whereby frictional heat is generated at a portion where the back surface of the glass film contacts the surface of the substrate or the surface of the component, and the glass film is bonded to the surface of the substrate or the surface of the component by the frictional heat; Or, The method includes cutting a glass film prepared by the method described in paragraph 18 into a predetermined shape, placing the cut glass film at a predetermined position on the surface of a substrate or a part, and evenly applying a compressive load smaller than the compressive strength of the crystalline powdered glass described in paragraph 18 to the entire surface of the cut glass film, thereby compressing the entire surface of the cut glass film, thereby generating frictional heat at the location where the back surface of the cut glass film comes into contact with the surface of the substrate or the surface of the part, and the frictional heat bonds the cut glass film to the surface of the substrate or the surface of the part.

[0021] That is, when the glass film made by the method described in paragraph 18 is placed at a predetermined position on a substrate or component, and a compressive load smaller than the compressive strength of the crystalline powdered glass described in paragraph 18 is evenly applied to the entire surface of the glass film to compress the glass film, the aggregates formed on the surface of the glass film undergo slight elastic deformation, and the back surface of the glass film comes into close contact with the surface of the substrate or component, and frictional heat is generated for a short period of time at all contact sites that come into contact with the convex parts of the unevenness of the close contact surface, and then disappears instantaneously. This frictional heat bonds the glass film to the surface of the substrate or component. In addition, when the film produced by the method described in paragraph 18 is cut into a predetermined shape, the cut glass film is placed at a predetermined position on a substrate or component, and a compressive load smaller than the compressive strength of the crystalline powdered glass described in paragraph 18 is applied to the entire surface of the glass film to compress the glass film, the aggregates formed on the surface of the glass film undergo slight elastic deformation, the back surface of the glass film adheres to the surface of the substrate or component, and frictional heat is generated for a short period of time at all contact sites that come into contact with the convex parts of the unevenness of the adhered surface and then disappears instantaneously. This frictional heat bonds the glass film to the surface of the substrate or component. The glass film is a glass film in which powder glass is bonded together with aggregates formed on the surface. On the other hand, aggregates are a collection of carbon particles in which carbon particles are bonded together in a beaded shape, and the carbon particles can be cut. In addition, since most powder glass has a thickness of submicrons, crystalline powder glass is harder than amorphous powder glass, but can be cut. For this reason, the glass film can be cut into any shape. That is, the unevenness of the surface of the substrate or part is small, at submicron size, but the number of convex parts that come into contact with the surface of the glass film is enormous. On the other hand, the surface of the glass film is formed of aggregates. When the entire glass film is uniformly compressed with a compression load smaller than the compressive strength of the crystalline powdered glass, the aggregates are slightly elastically deformed. For this reason, when the glass film arranged on the surface of the substrate or part is compressed, the glass film adheres to the surface of the substrate or part, and frictional heat is instantaneously generated at all contact points where the convex parts of the unevenness of the adhered surface come into contact with the surface of the glass film. This frictional heat bonds the glass film at the contact points to the convex parts of the unevenness of the surface of the substrate or part. Since the number of convex parts at the contact points is enormous and the distance between the contact points is small, the surface of the glass film is firmly bonded to the surface of the substrate or part. The ignition temperature of carbon black in the atmosphere exceeds 500°C. On the other hand, frictional heat is generated in a short time and the contact area has a small volume, so the frictional heat is cooled instantly, and the temperature of the aggregates at the contact area is significantly lower than the ignition temperature of carbon black. In addition, the surface of the glass film is bonded to the surface of the substrate or part by the frictional heat generated in a short time and the frictional heat that is then instantaneously cooled. Therefore, even if the substrate or part is a synthetic resin with low heat resistance, or a cloth or nonwoven fabric, the glass film is bonded to the surface of the substrate or part. Furthermore, as explained in the third effect of the glass film described in the tenth paragraph, the area and shape of the glass film to be created can be freely changed. Furthermore, as explained in the fifth effect of the glass film described in the tenth paragraph, the glass film can be cut into various sizes and shapes. Therefore, the glass film can be bonded to substrates or parts made of various materials, and further to substrates or parts made of various sizes and shapes, by an extremely simple means called friction welding. As a result, glass films of various sizes and shapes having light shielding and thermal radiation properties are formed on the surfaces of substrates or parts made of various materials. Also, glass films of various sizes and shapes having excellent thermal shock resistance and mechanical strength, which are characteristics of crystalline powder glass, are formed on the surfaces of substrates or parts made of various materials. Furthermore, glass films of various sizes and shapes having both electrical conductivity, electromagnetic shielding properties, and antistatic properties based on the electrical conductivity of carbon black are formed on the surfaces of substrates or parts made of various materials. In addition, the surface of the glass film bonded to the surface of the substrate or part has water repellency, which repels all liquids due to surface tension. This provides excellent corrosion resistance to the substrate or part to which the glass film is pressed using frictional heat. [Brief description of the drawings]

[0022] [Figure 1] FIG. 2 is an enlarged schematic diagram of a portion of the surface of a glass film, in which the surface of the glass film has a mottled pattern of areas where aggregates of Ketjen Black are formed and areas where they are not formed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Example 1 In this embodiment, Ketjen black is used as carbon black, and aggregates of Ketjen black are precipitated on the surface of amorphous powdered glass to create a glass film in which amorphous powdered glass pieces are bonded together. Ketjen Black (Lion Corporation's product EC600JD) has a small average primary particle diameter of 34 nm and a specific surface area of ​​1270 m 2 / g, which shows excellent light-shielding properties. In addition, the amount of dibutyl phthalate required to fill the gaps between Ketjen Black particles is 495 cm 3 / 100g, which is large, and the degree of particle connection and particle aggregation is large. This promotes the entanglement of the Ketjen Black aggregates, increasing the mechanical strength of the glass film. The bulk density is 120g / L. In addition, amorphous powdered glass containing SnO and P2O5 as main components was used as the powdered glass (product FP67 from Asahi Glass Co., Ltd.). This powdered glass has a specific gravity of 3.6 g / cm 3 It has a transition point of 285°C, a softening point of 390°C, and a D50 of 20μm. As a powdered glass, it has a large particle size, low transition point and softening point, and a thermal expansion coefficient of 79×10 -7 / ℃, which is relatively small. First, the clusters of Ketjen Black were crushed in excess methanol to the limit size, and a suspension was created in which the crushed clusters of Ketjen Black were dispersed in excess methanol. For this purpose, 20 g of Ketjen Black and 240 g of industrial grade 1 methanol were filled into a container, and the methanol was stirred to immerse the Ketjen Black in the methanol. Furthermore, a flat plate was placed on the container, and 13 weights of 5 kg were placed on the flat plate at approximately equal intervals. After this, the weight and the flat plate were removed, and the container was fixed on the vibration table of the vibration exciter, and a vibration acceleration of 2 G was repeatedly applied to the container in three directions: front and back, left and right, and up and down. This pair of processes of applying a compression load and applying a vibration acceleration was repeated five times. After this, a weight was placed on the flat plate, but since no movement of the flat plate sinking in the direction of gravity was observed, it was determined that the clusters of Ketjen Black had been crushed to the limit size, and the process was stopped. In addition, an ultrasonic homogenizer (LUH150, product of Yamato Scientific Co., Ltd.) was operated in the methanol in the container, and a 20 kHz ultrasonic signal was applied for 30 minutes to create a suspension in which aggregates in which the aggregates were entangled with each other were dispersed in methanol. Next, 54 g of amorphous powdered glass was put into the container, and the collection of powdered glass was stirred to immerse the collection of powdered glass in the suspension. The container was then fixed on the vibration table of the vibration exciter, and the vibration exciter was operated to repeatedly apply vibration acceleration of 2 G in three directions, front-back, left-right, and up-down, to the container, arranging the collection of powdered glass in the suspension. The volume of the collection of amorphous powdered glass, calculated based on the weight and density, was 15 cm. 3 The volume of a cluster of Ketjen Black calculated based on its mass and density is 10 cm 3 Therefore, the volume occupied by the aggregate of amorphous powdered glass in the suspension is 1.5 times the volume occupied by the aggregate of Ketjen Black in the suspension. After that, a container measuring 20 cm x 20 cm was filled with 10 g of the powdered glass arranged in the suspension, and the container was fixed on the vibration table and repeatedly subjected to an acceleration of 2 G in three directions, i.e., forward / backward, left / right, and up / down. After that, a flat plate that covers the entire powdered glass in the container was placed over the suspension, and 13 weights weighing 5 kg were placed on the flat plate at approximately equal intervals, and the container was moved to a heat treatment device in a nitrogen atmosphere, where the container was heated to 390°C to soften the powdered glass and apply a compressive stress evenly to the softened powdered glass, bonding the powdered glass together, and creating a flat glass film on the bottom surface of the container in the shape of the bottom surface. After that, the weight was removed from the container, and a vertical impact acceleration of 0.3G was simultaneously applied to nine discrete points on the bottom of the container, peeling off the glass film with a slightly blackish color and transparency from the bottom of the container, and then a vertical impact acceleration of 0.3G was simultaneously applied to nine discrete points on the surface of the flat plate, peeling off the glass film from the surface of the flat plate. Note that the surface of the glass film was formed in a mottled pattern of areas where a blackish substance was formed and areas where it was not formed. Ten such glass films were created. Next, the glass film was observed using an electron microscope. An extremely low accelerating voltage SEM owned by JFE Techno-Research Corporation was used. This device allows surface observation at extremely low accelerating voltages starting from 100 volts, and allows the film surface to be observed directly without forming a conductive coating. First, observations of the side of the film revealed that the film was 10 μm thick. Furthermore, the reflected electron beam from the blackish substance formed in a speckled pattern on the surface of the glass film was subjected to image processing to extract energies between 900-1000 volts, and the material of the blackish substance was analyzed based on the shade of the image. As no shade was observed, it was found to be composed of a single atom. Furthermore, the energy and intensity of characteristic X-rays from multiple points on the surface were subjected to image processing to analyze the type of elements that made up the blackish substance. The blackish substance was composed only of carbon atoms. From the above observation results, it was found that the surface of the glass film had a patchy pattern of areas where aggregates of Ketjen Black were formed and areas where they were not. Therefore, the glass film created has the light blocking, heat radiation, and electrical conductivity based on the properties of Ketjen Black, and also has the transparency of amorphous powdered glass. Figure 1 shows a schematic enlarged view of a part of the surface of the glass film. 1 is the aggregates and 2 is the amorphous powdered glass. Next, the light-shielding property of the glass film was measured based on the JIS-L-1055A method, and it was found that the light-shielding rate was about 60%, and that the glass film had light-shielding properties. From the light-shielding property of the glass film, it is believed that Ketjen Black is formed on the surface of the glass film at an average rate of nearly 60%. Furthermore, the thermal emissivity of the glass film was measured using an analyzer consisting of a Fourier transform infrared spectrophotometer and a radiation measurement unit (equipment owned by Kobelco Research Institute Co., Ltd.), and it was found that the thermal emissivity was about 0.57, and that the glass film had heat dissipation properties. From the thermal emissivity of the glass film, it is believed that Ketjen Black is formed on the surface of the glass film at an average rate of nearly 60% of the area. Next, the visible light transmittance of the glass film was measured using a measuring instrument PT-50 manufactured by Komyo Rikagaku Kogyo. A glass film with a thickness of 30 μm, manufactured by Nippon Electric Glass Co., Ltd., G-Leaf, was used as the glass film that transmits 100% of visible light. The visible light transmittance of the glass film was around 35%. Therefore, the glass film had the transparency of amorphous powdered glass. The visible light transmittance of the glass film is expected to be 40% due to the light blocking property and thermal radiation property of the glass film, but the visible light transmittance was 35%. This result is considered to be due to the existence of a relatively narrow area where visible light cannot pass among the multiple areas on the surface of the amorphous powdered glass where aggregates are not formed, resulting in a visible light transmittance of 35%. Therefore, the occupancy rate of the aggregates formed on the surface of the amorphous powdered glass is considered to be close to 60% on average. Furthermore, the surface resistance of the glass film was measured at multiple points using a surface resistance meter (for example, a surface resistance meter ST-4 from Simco Japan Co., Ltd.). The surface resistivity was around 19 Ω, meaning that the glass film had a resistance close to the resistivity of Ketjen black, which is 3.9 Ω·cm. Therefore, based on the resistivity of Ketjen black, the film that was created also acts as a thin film that combines the functions of conductivity, electromagnetic shielding, and antistatic properties. Furthermore, based on the surface resistance of the glass film, it is believed that clusters of Ketjen black are connected in a continuous manner and formed on the surface of the glass film. In addition, the tensile strength of the glass film was measured based on the tensile strength test for plastic films (ISO527-3:2012), and the result was 130±10MPa. This tensile strength is greater than the tensile strength of a 50μm-thick transparent acrylic resin film, which is 50-60MPa. Therefore, even though the glass film is only 10μm thick, it has a greater tensile strength than a 50μm-thick transparent acrylic resin film. From the above results, in Example 1, the surface of the glass film was formed with a collection of Ketjen Black with an average area occupancy rate of about 60%. On the other hand, by increasing the weight ratio of Ketjen Black to the weight of amorphous powdered glass, the light-shielding property and heat radiation property of the glass film are increased, but the transparency of the glass film is decreased. On the other hand, by decreasing the weight ratio of Ketjen Black to the weight of amorphous powdered glass, the light-shielding property and heat radiation property of the glass film are decreased, but the transparency of the glass film is increased.

[0024] Example 2 In this embodiment, acetylene black is used as carbon black, and aggregates of acetylene black are precipitated on the surface of amorphous powdered glass to create a glass film in which amorphous powdered glass pieces are bonded together. Acetylene black (Denka Li-100) has an average particle size of 35 nm and a specific surface area of ​​68 m 2 It is composed of primary particles with a molecular weight of 1.01g / g and an iodine adsorption capacity of 92mg / g. In addition, it has a bulk density of 40g / L and an electrical resistivity of 0.21Ω·cm, making it the most conductive of all carbon blacks. The powdered glass is the amorphous powdered glass used in Example 1. First, 20 g of acetylene black and 240 g of industrial grade 1 methanol were filled into a container, and the excess methanol was stirred to soak the acetylene black in the methanol. A flat plate was then placed on the container, and 13 5 kg weights were placed on the plate at approximately equal intervals. After this, the weights and the flat plate were removed, and the container was fixed on the vibration table of a vibration exciter, and a vibration acceleration of 2 G was repeatedly applied to the container in three directions: forward / backward, left / right, and up / down. This pair of processes of applying a compressive load and applying a vibration acceleration was repeated five times. After this, a weight was placed on the flat plate, but since there was no movement of the flat plate sinking in the direction of gravity, it was determined that the acetylene black aggregates had been crushed to the limit size, and the process was stopped. Furthermore, an ultrasonic homogenizer (LUH150, manufactured by Yamato Scientific Co., Ltd.) was operated in the methanol in the container, and a 20 kHz ultrasonic signal was applied for 30 minutes to create a suspension in which aggregates in which the aggregates were entangled with each other were dispersed in the methanol. Next, 43 g of amorphous powdered glass was put into the container, and the collection of powdered glass was stirred and immersed in the suspension. The container was then fixed on the vibration table of the vibration exciter, and the vibration exciter was operated to repeatedly apply vibration acceleration of 2 G in three directions, front-back, left-right, and up-down, to the container, arranging the collection of powdered glass in the suspension. The volume of the collection of amorphous powdered glass, calculated based on the weight and density, was 12 m. 3 The volume of a lump of acetylene black converted into density is 10 cm 3 Therefore, the volume occupied by the aggregate of amorphous powdered glass in the suspension is 1.2 times the volume occupied by the aggregate of acetylene black in the suspension. After that, in the same manner as in Example 1, a container with a size of 20 cm x 20 cm was filled with 10 g of the powdered glass arranged in the suspension, and the container was fixed on the vibration table and repeatedly subjected to an acceleration of 2 G in three directions, i.e., forward / backward, left / right, and up / down. After that, a flat plate covering the entire powdered glass in the container was placed on the suspension, and 13 weights of 5 kg were placed on the flat plate at approximately equal intervals. Furthermore, the container was moved to a heat treatment device in a nitrogen atmosphere, and the container was heated to 390°C to soften the powdered glass, and a compressive stress was evenly applied to the softened powdered glass, bonding the powdered glass together, and a flat glass film was created on the bottom surface of the container in the shape of the bottom surface. After that, the weight was removed from the container, and a vertical impact acceleration of 0.3G was simultaneously applied to nine discrete points on the bottom of the container, peeling off the glass film with a slightly blackish color and transparency from the bottom of the container, and then a vertical impact acceleration of 0.3G was simultaneously applied to nine discrete points on the surface of the flat plate, peeling off the glass film from the surface of the flat plate. Note that the surface of the glass film was formed in a mottled pattern of areas where a blackish substance was formed and areas where it was not formed. Ten such glass films were created. Next, the glass film was observed with an electron microscope in the same manner as in Example 1. From the observation of the side of the film, the thickness of the film was 8.5 μm. Furthermore, the energy between 900-1000 volts was extracted from the reflected electron beam from the blackish substance formed in a mottled pattern on the surface of the glass film, and image processing was performed to analyze the material of the blackish substance based on the shade of the image. Since no shade was observed, it was found to be composed of a single atom. Furthermore, the energy and intensity of characteristic X-rays from multiple points on the surface were image processed to analyze the type of elements that constitute the blackish substance. The blackish substance was composed only of carbon atoms. From the above observation results, it was found that the surface of the glass film had a mottled pattern of areas where acetylene black aggregates were formed and areas where they were not formed. Therefore, the glass film thus produced has the light-shielding properties, heat radiation properties, and electrical conductivity based on the properties of acetylene black, and also has the transparency of amorphous powdered glass. Furthermore, as in Example 1, the light blocking property of the glass film was measured, and it was found to be a light blocking glass film with a light blocking rate of about 75%. From the light blocking property of the glass film, it is considered that acetylene black is formed on the surface of the glass film at a rate close to 75% on average. From the thermal emissivity of the glass film, it was found to be a heat dissipating glass film with a thermal emissivity of about 0.71. From the thermal emissivity of the glass film, it is considered that acetylene black is formed on the surface of the glass film at a rate close to 75% on average. Next, the visible light transmittance of the glass film was measured in the same manner as in Example 1. The visible light transmittance of the glass film was about 22%. The visible light transmittance of the glass film was expected to be 25% due to the light blocking property and thermal radiation property of the glass film, but the visible light transmittance was 22%. This result is considered to be due to the existence of a relatively narrow portion through which visible light cannot pass among the multiple portions on the surface of the amorphous powdered glass where aggregates are not formed, resulting in a visible light transmittance of 22%. Therefore, the occupancy rate of the aggregates formed on the surface of the amorphous powdered glass is considered to be close to 75% on average. Furthermore, similarly to Example 1, the surface resistance of the prepared glass film was measured at multiple points on the surface. Since the surface resistivity was 1.0Ω, the glass film had a resistance close to the resistivity of acetylene black, 0.21Ω·cm. Therefore, based on the resistivity of acetylene black, the prepared film also acts as a thin film that combines the functions of conductivity, electromagnetic shielding, and antistatic properties. In addition, based on the surface resistance of the glass film, it is considered that the collection of acetylene black is continuously connected and formed on the surface of the glass film. Moreover, the tensile strength of the glass film was measured in the same manner as in Example 1, and the result was 130±10 MPa, which is greater than the tensile strength of a transparent film made of acrylic resin having a thickness of 50 μm. From the above results, in Example 2, acetylene black aggregates were formed with an average area occupancy rate of about 75% of the surface of the glass film. When the weight ratio of acetylene black to the weight of amorphous powdered glass is reduced, the light-shielding and thermal radiation properties of the glass film are reduced, but the transparency of the glass film is increased. On the other hand, when the weight ratio of acetylene black to the weight of amorphous powdered glass is further increased, the light-shielding and thermal radiation properties of the glass film are increased, but the transparency of the glass film is further decreased.

[0025] Example 3 In this example, the glass film produced in Example 1 is pressure-bonded to a transparent window glass sheet by frictional heat. For this purpose, the window glass sheet is cut to a size of 20 cm x 20 cm, which is the same size as the glass film produced in Example 1, and then washed and dried. First, the glass film prepared in Example 1 was superimposed on a window glass plate, and thirteen weights of 4 kg were placed on the glass film at approximately equal intervals. Five such samples were prepared. Next, the bonding strength of the laminated glass films was measured based on the tensile adhesion strength test method of JIS-K6849:1994, and was found to be 32 MPa. Therefore, the glass film having a thickness of 10 μm was bonded to the window glass plate with sufficient bonding strength. This provides the window glass plate with the light-shielding property, heat radiation property, and electrical conductivity of the glass film prepared in Example 1.

[0026] Example 4 In this example, the glass film prepared in Example 1 was cut to 10 cm x 10 cm, and the glass film was pressed onto the surface of the window glass plate used in Example 3 by frictional heat. For this purpose, the glass film prepared in Example 1 was cut to 10 cm x 10 cm, washed, dried, and the glass film was superimposed on the surface of the window glass plate measuring 20 cm x 20 cm so that the center positions of both were aligned. Furthermore, five weights of 2.6 kg were placed on the glass film at approximately equal intervals, and the cut glass film was pressed onto the surface of the window glass plate by frictional heat. Five such samples were prepared. The bonding strength of the overlapped glass films was measured in the same manner as in Example 3. The bonding strength was 1 / 4 of that in Example 3, but it was sufficient to bond a lightweight glass film to a window glass sheet. This result shows that the bonding strength is proportional to the area of ​​the overlapping bonding surfaces compared to the bonding strength in Example 3. In other words, the entire surface of the glass film is compressed evenly, the surface of the glass film is in close contact with the surface of the window glass sheet, and the number of contacts formed on both surfaces is proportional to the surface area of ​​both surfaces, so that the bonding strength is proportional to the surface area of ​​both surfaces.

[0027] Example 5 In this example, acetylene black is used as the carbon black, and aggregates of acetylene black are precipitated over the entire surface of crystalline powdered glass. The temperature is then raised to the crystallization temperature of the crystalline powdered glass, and a glass film is created in which the crystalline powdered glass is bonded together. The acetylene black used here is the same as that used in Example 2. Crystalline powdered glass (a product of Asahi Glass Co., Ltd., product name LS-5-300M) is mainly composed of SiO2, RO (R is an alkaline earth metal), and RO (R is an alkali metal), and has a density of 2.9 g / cm 3 and the thermal expansion coefficient is 105×10 -7 / ℃, with a transition temperature of 490℃, a softening point of 610℃, a crystallization temperature of 675℃, and a median particle size D50 of 10μm, which is relatively large among crystalline powder glasses. First, as in Example 1, the acetylene black aggregates were crushed in excess methanol to a limit size, and a suspension was prepared in which the crushed acetylene black aggregates were dispersed in excess methanol. For this purpose, 40 g of acetylene black and 450 g of industrial grade 1 methanol were filled into a container, and the excess methanol was stirred to immerse the acetylene black in the excess methanol. Furthermore, a flat plate was placed on the container, and 17 weights of 4 kg were placed on the flat plate at approximately equal intervals. After this, the weight and the flat plate were removed, and the container was fixed on the vibration table of the vibration exciter, and a vibration acceleration of 2 G in three directions, front and back, left and right, and up and down, was repeatedly applied to the container. Such a pair of processes of applying a compression load and applying a vibration acceleration was repeated five times. After this, a weight was placed on the flat plate, but since there was no movement of the flat plate sinking in the direction of gravity, it was determined that the acetylene black aggregates had been crushed to a limit size, and the process was stopped. Next, similarly to Example 1, an ultrasonic homogenizer (LUH150, product of Yamato Scientific Co., Ltd.) was operated in the methanol in the container, and a 20 kHz ultrasonic signal was applied for 30 minutes to create a suspension in which aggregates, in which the aggregates were entangled with each other through the methanol, were dispersed in the methanol. Further, 43.9 g of crystalline powdered glass was put into the container, and the aggregate of powdered glass was stirred to immerse the aggregate of powdered glass in the suspension. The container was then fixed on the vibration table of the vibration exciter, and the vibration exciter was operated to repeatedly apply vibration acceleration of 2 G in three directions, front-back, left-right, and up-down, to the container, thereby arranging the aggregate of powdered glass in the suspension. The volume of the aggregate of crystalline powdered glass, calculated based on the weight and density, was 15 cm. 3 The volume of a lump of acetylene black converted into density is 20 cm 3 Therefore, the volume of the suspension occupied by the aggregate of crystalline powdered glass is 0.75 times the volume of the suspension occupied by the aggregate of acetylene black. Then, in the same manner as in Example 1, a container measuring 20 cm x 20 cm was filled with 10 g of the powdered glass arranged in the suspension, and the container was fixed on the vibration table and repeatedly subjected to an acceleration of 2 G in three directions, i.e., forward / backward, left / right, and up / down. Then, a flat plate covering the entire powdered glass in the container was placed on the suspension, and 13 weights weighing 5 kg were placed on the flat plate at approximately equal intervals. The container was then moved to a heat treatment device in a nitrogen atmosphere, where the container was heated to 675°C to crystallize the powdered glass, and compressive stress was applied evenly to the crystallized powdered glass to bond the powdered glass together, forming a flat glass film on the bottom surface of the container in the shape of the bottom surface. After that, the weight was removed from the container, and a vertical impact acceleration of 0.3 G was simultaneously applied to nine mutually separated points on the bottom surface of the container, peeling off the blackish glass film from the bottom surface of the container, and furthermore, a vertical impact acceleration of 0.3 G was simultaneously applied to nine mutually separated points on the surface of the flat plate, peeling off the glass film from the surface of the flat plate. Ten such glass films were created. Next, the glass film was observed with an electron microscope in the same manner as in Example 1. From the observation of the side of the film, the thickness of the film was 11.3 μm. Furthermore, the energy between 900-1000 volts was extracted from the reflected electron beam from the blackish substance formed on the surface of the glass film, and image processing was performed to analyze the material of the blackish substance based on the shade of the image. Since no shade was observed, it was found to be composed of a single atom. Furthermore, the energy and intensity of characteristic X-rays from multiple points on the surface were image processed to analyze the type of elements that constitute the blackish substance. The blackish substance was composed only of carbon atoms. From the above observation results, it was found that acetylene black aggregates were formed on the entire surface of the glass film. Therefore, the glass film thus produced has the light-shielding, heat-radiating, and electrical conductivity properties of acetylene black, as well as the heat resistance and mechanical strength of crystalline powdered glass. Furthermore, as in Example 1, the light blocking property of the glass film was measured, and it had a light blocking rate of 0.95. Therefore, acetylene black is formed on the entire surface of the glass film. Furthermore, as in Example 1, the thermal emissivity of the glass film was measured, and it had a light blocking rate of 0.95. Therefore, the result of the thermal emissivity of the glass film also shows that acetylene black is formed on the entire surface of the glass film. Furthermore, similarly to Example 1, the surface resistance of the prepared glass film was measured at multiple points on the surface. Since the surface resistivity was 1.0Ω, the glass film had a resistance close to the resistivity of acetylene black, 0.21Ω·cm. Therefore, based on the resistivity of acetylene black, the prepared film also acts as a thin film that combines the functions of conductivity, electromagnetic shielding, and antistatic properties. In addition, based on the surface resistance of the glass film, it is considered that the collection of acetylene black is continuously connected and formed on the surface of the glass film. Moreover, the tensile strength of the glass film was measured in the same manner as in Example 1, and the tensile strength was 260±20 MPa. Since crystalline powdered glass was used in Example 5, the tensile strength was twice as high as that of the glass film made of amorphous powdered glass used in Example 2. This tensile strength was even higher than that of a transparent film made of acrylic resin having a thickness of 50 μm. Next, the bending strength of the glass film was measured based on the ring bending test of ASTM-C1499-01. The bending strength was 30 MPa. Furthermore, the bending strength of the glass film produced in Example 2 was measured by the same ring bending test. The bending strength was 15 MPa. Since crystalline powdered glass was used in Example 5, it had twice the bending strength of the glass film made of amorphous powdered glass used in Example 2. Furthermore, the glass film was heated to 250°C and then immersed in water, but there was no change in the surface of the glass film. Similarly, the glass film produced in Example 2 was heated to 200°C and then immersed in water, resulting in the occurrence of many cracks on the surface of the glass film. Since crystalline powdered glass was used in Example 5, the thermal shock resistance was improved compared to the glass film made of amorphous powdered glass used in Example 2. From the above results, in Example 5, acetylene black aggregates were formed on the entire surface of the glass film. Therefore, the glass film has the functions of electrical conductivity, electromagnetic shielding, and antistatic properties based on the electrical conductivity of acetylene black, and also has the light blocking and thermal radiation properties of acetylene black. Furthermore, the glass film has the thermal shock resistance and mechanical strength of crystalline powdered glass.

[0028] Example 6 In this example, the glass film produced in Example 5 is thermocompression bonded to a synthetic resin film. An acrylic resin film having a thickness of 50 μm was used as the film. For this purpose, the acrylic resin film was cut to a size of 20 cm x 20 cm, which is the same size as the glass film produced in Example 5, and then washed and dried. First, the glass film prepared in Example 5 was superimposed on an acrylic resin film, and thirteen weights of 3 kg were placed on the glass film at approximately equal intervals to prepare five such samples. Next, the bonding strength of the laminated glass films was measured based on the tensile adhesion strength test method of JIS-K6849:1994 in the same manner as in Example 3, and the tensile strength was 80±5 MPa. This tensile strength is greater than the tensile strength of the acrylic resin film, which is 50-60 MPa. Therefore, by pressing the glass film to the acrylic resin film, the tensile strength of the acrylic resin film is increased. Furthermore, the acrylic resin film is provided with the functions of conductivity, electromagnetic shielding, and antistatic properties based on the conductivity of acetylene black, and is also provided with the light shielding and heat radiation properties of acetylene black. The reason why the tensile adhesive strength of Example 6 is higher than that of Example 3 is considered to be due to the following reasons. The glass film is bonded to an acrylic resin film in Example 6, whereas it is bonded to a window glass plate in Example 3. When the entire surface of the acrylic resin film is compressed evenly through the glass film, the convex part of the surface of the acrylic resin film that contacts the surface of the glass film is more likely to elastically deform than the convex part of the surface of the window glass plate. Therefore, the convex part of the surface of the acrylic resin film that contacts the surface of the glass film is elastically deformed, and the volume of the surface that contacts the surface of the glass film is increased. In contrast, the convex part of the surface of the window glass plate is less likely to deform, so the volume of the surface that contacts the surface of the glass film is smaller than that of the acrylic resin film. It is considered that the increase in the volume of the convex part corresponding to this bonding part increases the bonding force of the surface of the acrylic resin film to the surface of the glass film. [Explanation of symbols]

[0029] 1. Aggregate clusters 2. Amorphous powdered glass

Claims

1. A method for producing a glass film having the light blocking, heat dissipation, and electrical conductivity of carbon black and the transparency of amorphous powdered glass is as follows: A container is charged with carbon black clumps and methanol having a weight 10 times greater than the weight of the carbon black clumps, the methanol is stirred, and the carbon black clumps are immersed in the excess methanol. Then, a plate that covers the entire surface of the carbon black clumps in the container is placed over the carbon black clumps. A compressive load is evenly applied to the entire surface of the plate to pulverize the carbon black clumps immersed in the excess methanol. Then, the plate is lifted from the container, and the container is fixed on a vibration table of a vibrator. The vibrator is operated to repeatedly apply vibration acceleration in three directions, front-back, left-right, and up-down, to the container to rearrange the pulverized carbon black clumps in the excess methanol. Then, the plate is placed on the container and the container is fixed on a vibration table of a vibrator. the plate is again covered with the carbon black mass, and the compressive load is applied evenly to the entire surface of the plate to further crush the carbon black mass immersed in the excess methanol; the plate is then again removed from the container, and the vibration acceleration in the three directions is applied repeatedly to the container; the pair of processes consisting of the process of applying the compressive load and the process of applying the vibration acceleration are repeated, and when a repulsive force is generated in the plate when the compressive load is applied to the plate, it is determined that the crushing of the carbon black mass immersed in the excess methanol is completed, and the pair of processes are stopped; thus, a first suspension is prepared in which the crushed carbon black mass is immersed in the excess methanol; thereafter, a first process of removing the plate from the container; A homogenizer is placed in the container, and the homogenizer is operated in the first suspension, and shock waves are continuously applied to the pulverized carbon black mass via the excess methanol, whereby the shock waves are repeatedly irradiated to bonds between agglomerates in the pulverized carbon black mass, causing the bonds to dissociate and separate into individual agglomerates, and the shock waves are repeatedly irradiated to bonds between aggregates in the agglomerates, causing the bonds to dissociate and separate the entangled aggregates into individual agglomerates. a second step in which the aggregates are separated into individual aggregates, and the aggregates are entangled with each other, and the shock waves are repeatedly applied to the entangled aggregates, and the entangled aggregates are gradually separated from the entangled aggregates, thereby forming a second suspension in which the aggregates are entangled with each other and dispersed in methanol; The aggregates are weighed so that the aggregates are formed on the surface of the amorphous powdered glass by a weight that is larger than half of the surface of the amorphous powdered glass, not on the entire surface of the amorphous powdered glass. The weighed aggregate of the amorphous powdered glass is put into the container, the aggregate of the amorphous powdered glass is stirred, and the aggregate of the amorphous powdered glass is immersed in the second suspension. Furthermore, the container is placed on a vibration table of the vibrator. a third step of fixing the container on a surface of the container, operating the vibrator to repeatedly apply vibration acceleration in three directions, i.e., forward / backward, left / right, and up / down, to the container, thereby rearranging the clusters of amorphous powdered glass in the second suspension, whereby the clusters of amorphous powdered glass overlap each other via a film made of the second suspension and having a thickness of less than 1 μm, and the overlapped clusters of amorphous powdered glass are formed on the bottom surface of the container as a cluster of amorphous powdered glass overlapped in a plane; A part of the amorphous powdered glass aggregate overlapping in a planar shape in the container is transferred to a new container as an amount required for producing a glass film, the new container is fixed on the vibration table of the vibrator, the vibrator is operated, and vibration accelerations in three directions, i.e., forward / backward, left / right, and up / down, are repeatedly applied to the new container, so that the amorphous powdered glass aggregates are overlapped with each other via the second suspension, and the overlapped aggregate of amorphous powdered glass is re-formed on the bottom surface of the new container as an aggregate of amorphous powdered glass overlapping in a planar shape; and A new plate material covering the entire surface of the amorphous powder glass aggregate is placed on the amorphous powder glass aggregate, and then the new container is moved to a heat treatment device in a nitrogen atmosphere, and a compressive load smaller than the compressive strength of the amorphous powder glass is evenly applied to the entire surface of the new plate material, and the new container is heated to the softening point of the amorphous powder glass. As a result, first, methanol is evaporated from the second suspension, and the aggregate aggregate is precipitated on the surface of the amorphous powder glass with a thickness of less than 0.1 μm, and the aggregate aggregate is precipitated on the surface of the amorphous powder glass. A region wider than 1 / 2 of the surface of the amorphous powdered glass is formed, not on the entire surface of the amorphous powdered glass, and a plurality of regions where the aggregates are not formed are formed. Next, the amorphous powdered glass on which the aggregates are precipitated is softened, and the softened amorphous powdered glass is compressed, and the softened amorphous powdered glass is deformed so as to fill voids in the softened amorphous powdered glass, and a part of the softened amorphous powdered glass seeps out from the region where the aggregates are not formed in the softened amorphous powdered glass. In adjacent softened amorphous glass powder, the oozing softened amorphous glass powder comes into contact with each other at a portion, and the contacting portions are bonded to each other. The contacting portions of the softened amorphous glass powder are bonded to each other by frictional heat via the aggregate collection. Thereafter, the collection of softened amorphous glass powder is left at the annealing point of the amorphous glass powder for 15 minutes or more, and then slowly cooled to room temperature. This releases distortion generated in the amorphous glass powder when the softened amorphous glass powder is bonded to each other, and the softened amorphous glass powder is solidified.A fourth step in which the joints between the softened amorphous powder glass are also solidified, and the solidified amorphous powder glass is joined to the bottom of the new container to form a flat glass film having a shape of the bottom of the new container; a fifth step of simultaneously applying an impact acceleration having the same magnitude to a plurality of points on the bottom surface of the new container, peeling off the glass film formed on the bottom surface of the new container from the bottom surface of the new container, and simultaneously applying an impact acceleration having the same magnitude as the impact acceleration to a plurality of points on the surface of the new plate, peeling off the glass film from the surface of the new plate, and removing the glass film; A method in which all of the above-mentioned five steps are carried out continuously is a method for producing a glass film that combines the light-blocking, heat-dissipating, and electrical conductivity of carbon black and the transparency of amorphous powdered glass.

2. A method for producing a glass film having the light-shielding, heat-dissipating and electrical conductivity of carbon black as described in claim 1 and the transparency of amorphous powdered glass, comprising the steps of: The carbon black described in claim 1 is Ketjen black, and a method of using this Ketjen black as the carbon black described in claim 1 and continuously carrying out all of the five steps described in claim 1 according to the method described in claim 1 is a method for producing a glass film that combines the light-blocking, heat-dissipating, and electrical conductivity of the carbon black described in claim 1 and has the transparency of amorphous powdered glass.

3. A method for producing a glass film having the light-shielding, heat-dissipating and electrical conductivity of carbon black as described in claim 1 and the transparency of amorphous powdered glass, comprising the steps of: The carbon black described in claim 1 is acetylene black, and a method of using the acetylene black as the carbon black described in claim 1 and continuously carrying out all of the five steps described in claim 1 according to the method described in claim 1 is a method of producing a glass film that combines the light-blocking, heat-dissipating, and electrical conductivity of the carbon black described in claim 1 and has the transparency of amorphous powdered glass.

4. A method for bonding a glass film produced by the method according to any one of claims 1, 2 and 3 to a surface of a substrate or a part, comprising the steps of: A method for bonding the glass film to the surface of a substrate or a component, the method comprising: placing a glass film prepared by the method according to any one of claims 1, 2, or 3 at a predetermined position on the surface of a substrate or a component; uniformly applying a compressive load smaller than the compressive strength of the powdered glass according to any one of claims 1, 2, or 3 to the entire surface of the glass film, and compressing the entire surface of the glass film; thereby generating frictional heat at a portion where the back surface of the glass film contacts the surface of the substrate or the surface of the component, and bonding the glass film to the surface of the substrate or the surface of the component by the frictional heat, Or, A method for bonding the cut glass film to the surface of the substrate or the surface of the component by cutting a glass film prepared by the method according to any one of claims 1, 2 or 3 into a predetermined shape, placing the cut glass film at a predetermined position on the surface of a substrate or a component, and evenly applying a compressive load smaller than the compressive strength of the powdered glass according to any one of claims 1, 2 or 3 to the entire surface of the cut glass film, thereby generating frictional heat at the location where the back surface of the cut glass film comes into contact with the surface of the substrate or the surface of the component, and the frictional heat bonds the cut glass film to the surface of the substrate or the surface of the component.

5. The method for producing the glass film according to claim 1 is a method for producing a glass film having both the light blocking properties, heat dissipation properties, and electrical conductivity of carbon black, and the thermal shock resistance and mechanical strength of crystalline powder glass, and the method for producing the glass film is as follows: The first change in the process in the third step described in claim 1 is that the powdered glass to be put into the container in the third step is not amorphous powdered glass but crystalline powdered glass, and the crystalline powdered glass is weighed to determine the weight of aggregates formed on the entire surface of the crystalline powdered glass, and the weighed crystalline powdered glass is put into the container. The second change in the process in the fourth step described in claim 1 is that the temperature to which the new container is heated in the fourth step described in claim 1 is the crystallization temperature of the crystalline powdered glass, not the softening point of the amorphous powdered glass. The method of continuously carrying out the five-step process described in claim 1 reflecting these two changes is a method for producing a glass film that has both the light-shielding, heat-dissipating, and electrical conductivity of carbon black, and the thermal shock resistance and mechanical strength of crystalline powdered glass.

6. A method for bonding a glass film having the light-shielding, heat-dissipating, and electrical conductivity of carbon black and the thermal shock resistance and mechanical strength of crystalline powdered glass to a surface of a substrate or a part, comprising the steps of: The method includes disposing a glass film prepared by the method described in claim 5 at a predetermined position on a surface of a substrate or a component, and uniformly applying a compressive load smaller than the compressive strength of the crystalline powdered glass described in claim 5 to the entire surface of the glass film, thereby compressing the entire surface of the glass film, whereby frictional heat is generated at a portion where the back surface of the glass film contacts the surface of the substrate or the surface of the component, and the glass film is bonded to the surface of the substrate or the surface of the component by the frictional heat, Or, A method comprising cutting a glass film prepared by the method described in claim 5 into a predetermined shape, placing the cut glass film at a predetermined position on the surface of a substrate or a component, and evenly applying a compressive load smaller than the compressive strength of the crystalline powdered glass described in claim 5 to the entire surface of the cut glass film, thereby compressing the entire surface of the cut glass film, thereby generating frictional heat at the site where the back surface of the cut glass film comes into contact with the surface of the substrate or the surface of the component, and the frictional heat bonds the cut glass film to the surface of the substrate or the surface of the component.

Citation Information

Patent Citations

  • Black quartz glass and its manufacturing method

    JP2022061950A

  • Glass and optical element

    JP2022119440A