Method for producing polyamic acid, and method for producing peeling layer-forming composition

By introducing terminal groups into polyamic acid using dicarboxylic anhydride and monoamine components, the method addresses the challenges of substrate damage and productivity in flexible electronic device manufacturing, achieving efficient and damage-free peeling of resin substrates.

JP2024179099APending Publication Date: 2024-12-26NISSAN CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023097645
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-14
Publication Date
2024-12-26

AI Technical Summary

Technical Problem

Existing methods for manufacturing flexible electronic devices using resin substrates face challenges such as the need for high-energy laser treatment, which can damage the substrate and reduce productivity, and the requirement for highly transparent substrates, limiting the scalability and efficiency of the process.

Method used

A method for producing polyamic acid with terminal groups introduced using specific dicarboxylic anhydride and monoamine components, which enhances the release properties of the release layer, allowing for easy peeling without substrate damage, even after high-temperature processes.

Benefits of technology

The method enables the production of a release layer with improved peelability, facilitating efficient separation of resin substrates from devices without damage, thereby enhancing manufacturing productivity and scalability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024179099000001
    Figure 2024179099000001
  • Figure 2024179099000002
    Figure 2024179099000002
  • Figure 2024179099000003
    Figure 2024179099000003
Patent Text Reader

Abstract

To provide a method for producing a polyamic acid that produces a polyamic acid suitable for forming a peeling layer with superior peelability.SOLUTION: A method for producing a polyamic acid includes a polyamic acid production step for producing polyamic acid. The polyamic acid is a reaction product of raw material components containing tetracarboxylic dianhydride, a diamine component, and at least one of a dicarboxylic anhydride and a monoamine component. In the polyamic acid production step, the reaction between the tetracarboxylic acid dianhydride and the diamine component is performed in the presence of at least one of the dicarboxylic anhydride and the monoamine component.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a polyamic acid, a method for producing a composition for forming a release layer, a method for producing a release layer, and a method for producing a flexible electronic device having a resin substrate. [Background technology]

[0002] In recent years, electronic devices are required to have functions such as flexibility and to be thin and lightweight, which requires the use of lightweight flexible plastic substrates instead of conventional heavy, fragile, and inflexible glass substrates.

[0003] In particular, new generation displays require the development of active matrix full color TFT (thin film transistor) display panels using lightweight flexible plastic substrates (hereafter referred to as resin substrates). The technology related to these new generation displays is expected to be applicable to various fields such as flexible displays, flexible smartphones, and mirror displays.

[0004] Therefore, various methods for manufacturing electronic devices using resin films as substrates have been studied, and for new generation displays, studies are being conducted on manufacturing processes that can be used with existing TFT equipment. For example, Patent Documents 1, 2, and 3 disclose a method in which an amorphous silicon thin film layer is formed on a glass substrate, a plastic substrate is formed on the thin film layer, and then a laser is irradiated from the glass surface side to peel off the plastic substrate from the glass substrate by hydrogen gas generated by crystallization of the amorphous silicon.

[0005] Furthermore, Patent Document 4 discloses a method for completing a liquid crystal display device by attaching a peelable layer (referred to as a "transferable layer" in Patent Document 4) to a plastic film using the techniques disclosed in Patent Documents 1 to 3.

[0006] However, the methods disclosed in Patent Documents 1 to 4, and especially the method disclosed in Patent Document 4, have problems in that it is essential to use a highly light-transmitting substrate to transmit the laser light, that it is necessary to irradiate the laser light with a relatively large energy sufficient to pass through the substrate and further release hydrogen contained in the amorphous silicon, and that the layer to be peeled off may be damaged by the irradiation of the laser light. Moreover, when the peeling layer has a large area, it takes a long time for the laser treatment, making it difficult to increase the productivity of device fabrication.

[0007] In view of this, a release layer-forming composition containing a specific polyamic acid and an organic solvent has been proposed as a composition for forming a release layer that can be peeled off without damaging the resin substrate of a flexible electronic device formed thereon and that provides a release layer whose releasability does not change even after heating treatment at relatively high temperatures in a TFT process or the like (e.g., Patent Document 5). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 10-125929 [Patent Document 2] Japanese Patent Application Publication No. 10-125931 [Patent Document 3] International Publication No. 2005 / 050754 [Patent Document 4] Japanese Patent Application Publication No. 10-125930 [Patent Document 5] International Publication No. 2017 / 204178 Summary of the Invention [Problem to be solved by the invention]

[0009] The release layer is required to have such releasability that it can be easily peeled off when peeling.

[0010] The present invention has been made in consideration of the above circumstances, and aims to provide a method for producing a polyamic acid useful for forming a release layer having excellent release properties, and a method for producing a composition for forming a release layer using the production method. [Means for solving the problem]

[0011] As a result of extensive research aimed at achieving the above object, the inventors discovered that a release layer having excellent releasability can be obtained by producing a polyamic acid having an introduced terminal group by a specific method, and thus completed the present invention.

[0012] That is, the present invention includes the following. [1] A method for producing a polyamic acid, comprising: a polyamic acid production step of producing a polyamic acid, the polyamic acid is a reaction product of raw material components including a tetracarboxylic dianhydride, a diamine component, and at least one of a dicarboxylic anhydride and a monoamine component; the reaction between the tetracarboxylic dianhydride and the diamine component in the polyamic acid production step is carried out in the presence of at least one of the dicarboxylic anhydride and the monoamine component. [2] The dicarboxylic acid anhydride includes an aromatic dicarboxylic acid anhydride, The monoamine component includes a monoamine having a ring structure. A method for producing the polyamic acid according to [1]. [3] The dicarboxylic acid anhydride is represented by the following formula (E1-1): The monoamine component is represented by the following formula (E2-1) or formula (E2-2): A method for producing the polyamic acid according to [1] or [2]. [ka] (In formula (E1-1), R 1 ~R 4each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 20 carbon atoms. [ka] (In formula (E2-1) and formula (E2-2), R 1 ~R 5 R each independently represents a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a halogen atom. 1 ~R 5 Adjacent two of may be joined together to form a ring structure. R 6 represents a single bond or an alkylene group having 1 to 4 carbon atoms. [4] The method for producing a polyamic acid according to any one of [1] to [3], wherein the tetracarboxylic dianhydride includes an aromatic tetracarboxylic dianhydride. [5] The method for producing a polyamic acid according to [4], wherein the aromatic tetracarboxylic dianhydride is represented by the following formula (1-1) or formula (1-2): [ka] (In formula (1-1), Ar 1 represents a tetravalent group obtained by removing two pairs of adjacent hydrogen atoms from a benzene ring which may have a substituent, or a tetravalent group obtained by removing two pairs of adjacent hydrogen atoms from a naphthalene ring which may have a substituent. In formula (1-2), X 1 represents a single bond, an ether bond, a carbonyl bond, an ester bond, a urethane bond, a urea bond, a thioether bond, a sulfonyl bond, -C(=O)N(-R)- (R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms), or a group represented by the following formula (1-2-1). R a each independently represents a halogen atom or an alkyl group having 1 to 4 carbon atoms. Each n independently represents an integer of 0 to 3. One (R a ) nWhen n is 2 or more, two or more R a may be the same or different.) [ka] (In formula (1-2-1), Y 1 and Y 2 each independently represents a single bond, an ether bond, a carbonyl bond, an ester bond, a urethane bond, a urea bond, a thioether bond, a sulfonyl bond, or -C(=O)N(-R)- (R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms). Ar 2 represents a divalent group obtained by removing two hydrogen atoms from a phenylene group which may have a substituent, or a biphenyl group which may have a substituent. * represents a bond.) [6] The method for producing a polyamic acid according to any one of [1] to [5], wherein the diamine component contains an aromatic diamine. [7] The method for producing a polyamic acid according to [6], wherein the aromatic diamine is represented by the following formula (2-1) or formula (2-2): [ka] (In formula (2-1), X 11 represents a single bond, an ether bond, a carbonyl bond, an ester bond, a urethane bond, a urea bond, a thioether bond, a sulfonyl bond, -C(=O)N(-R)- (R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms), or a group represented by the following formula (2-1-1). R b each independently represents a halogen atom or an alkyl group having 1 to 4 carbon atoms. Each m independently represents an integer of 0 to 4. One (R b ) m In the above, when m is 2 or more, two or more R b may be the same or different. In formula (2-2), X 12represents an -NH- group, an -O- group, or an -S- group. R c each independently represents a halogen atom or an alkyl group having 1 to 4 carbon atoms. p1 represents an integer of 0 to 3. p2 represents an integer of 0 to 4. (R c ) p1 In the above, when p1 is 2 or more, two or more R c may be the same or different. (R c ) p2 In this case, when p2 is 2 or more, two or more R c may be the same or different.) [ka] (In formula (2-1-1), Y 11 and Y 12 each independently represents a single bond, an ether bond, a carbonyl bond, an ester bond, a urethane bond, a urea bond, a thioether bond, a sulfonyl bond, or -C(=O)N(-R)- (R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms). Z 11 represents a divalent hydrocarbon group having 1 to 20 carbon atoms. * represents a bond.) [8] The raw material component includes the monoamine component, The method for producing a polyamic acid according to any one of [1] to [7], wherein the polyamic acid production step includes adding the tetracarboxylic dianhydride to an organic solvent solution containing the diamine component and the monoamine component, and reacting them. [9] The raw material component contains the dicarboxylic acid anhydride, The method for producing a polyamic acid according to any one of [1] to [7], wherein the polyamic acid production step includes adding the tetracarboxylic dianhydride and the dicarboxylic anhydride to an organic solvent solution containing the diamine component, and reacting them.

[10] A method for producing a composition for forming a release layer, comprising: producing a composition for forming a release layer comprising a polyamic acid and an organic solvent, A method for producing a composition, comprising producing a polyamic acid by the method for producing a polyamic acid according to any one of [1] to [9].

[11] A method for producing a release layer, comprising: A method for producing a release layer, comprising the step of forming a release layer using a composition for forming a release layer produced by the method for producing a composition according to

[10] .

[12] A method for producing a flexible electronic device having a resin substrate, comprising: A method for producing a flexible electronic device having a resin substrate, using a release layer produced by the method for producing a release layer according to

[11] .

[13] A release layer-forming composition comprising a polyamic acid and an organic solvent, the polyamic acid is a reaction product of raw material components including a tetracarboxylic dianhydride, a diamine component, and at least one of a dicarboxylic anhydride and a monoamine component; Regarding the components of the polyamic acid 1 a molar ratio of the total of the dicarboxylic acid anhydride and the monoamine component to the total of the tetracarboxylic acid dianhydride and the diamine component is 3 mol % or more in a H-NMR analysis of the composition for forming a release layer.

[14] The composition for forming a release layer according to

[13] , wherein the molar ratio is 50 mol % or less.

[15] The dicarboxylic acid anhydride comprises an aromatic dicarboxylic acid anhydride, The monoamine component includes a monoamine having a ring structure. The composition for forming a release layer according to

[13] or

[14] .

[16] A release layer formed from the composition for forming a release layer according to any one of

[13] to

[15] .

[17] A method for producing a flexible electronic device having a resin substrate, using the release layer according to

[16] . Effect of the Invention

[0013] According to the present invention, it is possible to provide a method for producing a polyamic acid useful for forming a release layer having excellent releasability, and a method for producing a release layer-forming composition using the production method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] (Method of producing polyamic acid) The method for producing a polyamic acid of the present invention includes a polyamic acid production step of producing a polyamic acid. Polyamic acid is a reaction product of raw material components. The raw material components include a tetracarboxylic dianhydride, a diamine component, and at least one of a dicarboxylic anhydride and a monoamine component. The reaction between the tetracarboxylic dianhydride and the diamine component in the polyamic acid production process is carried out in the presence of at least one of the dicarboxylic anhydride and the monoamine component.

[0015] When producing a polyamic acid having a group derived from at least one of a dicarboxylic anhydride and a monoamine component introduced as an end group, the reaction between a tetracarboxylic dianhydride and a diamine component is carried out in the presence of at least one of a dicarboxylic anhydride and a monoamine component, and the release layer formed from the release layer-forming composition containing the obtained polyamic acid and an organic solvent has excellent release properties. The present inventors consider the reason for this to be as follows. When end groups are to be introduced into the ends of a polyamic acid, even if the same amounts of raw material components that provide end groups are charged, the amount of end groups introduced varies depending on the method for producing the polyamic acid. Compared with the case where a polyamic acid is produced by reacting a tetracarboxylic dianhydride with a diamine component and then further reacting with at least one of a dicarboxylic anhydride and a monoamine component, the reaction between the tetracarboxylic dianhydride and the diamine component in the presence of at least one of a dicarboxylic anhydride and a monoamine component introduces more terminal groups (groups derived from the dicarboxylic anhydride and groups derived from the monoamine component) to the ends of the polyamic acid. As a result, the peelability is improved. In other words, peeling can be achieved with a smaller peeling force.

[0016] <<Tetracarboxylic acid dianhydride>> The tetracarboxylic dianhydride is not particularly limited, but preferably contains an aromatic tetracarboxylic dianhydride, since a release layer having excellent heat resistance can be obtained. Here, the aromatic tetracarboxylic dianhydride is a compound in which a total of two acid anhydride groups are bonded to the same or different aromatic rings. The aromatic ring may be an aromatic hydrocarbon ring or an aromatic heterocycle.

[0017] The aromatic tetracarboxylic dianhydride is not particularly limited, but is preferably represented by the following formula (1-1) or formula (1-2) in that a release layer having superior heat resistance can be obtained. [ka] (In formula (1-1), Ar 1 represents a tetravalent group obtained by removing two pairs of adjacent hydrogen atoms from a benzene ring which may have a substituent, or a tetravalent group obtained by removing two pairs of adjacent hydrogen atoms from a naphthalene ring which may have a substituent. In formula (1-2), X 1 represents a single bond, an ether bond, a carbonyl bond, an ester bond, a urethane bond, a urea bond, a thioether bond, a sulfonyl bond, -C(=O)N(-R)- (R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms), or a group represented by the following formula (1-2-1). R aeach independently represents a halogen atom or an alkyl group having 1 to 4 carbon atoms. Each n independently represents an integer of 0 to 3. One (R a ) n When n is 2 or more, two or more R a may be the same or different.) [ka] (In formula (1-2-1), Y 1 and Y 2 each independently represents a single bond, an ether bond, a carbonyl bond, an ester bond, a urethane bond, a urea bond, a thioether bond, a sulfonyl bond, or -C(=O)N(-R)- (R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms). Ar 2 represents a divalent group obtained by removing two hydrogen atoms from a phenylene group which may have a substituent, or a biphenyl group which may have a substituent. * represents a bond.)

[0018] In this specification, examples of halogen atoms include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0019] In this specification, examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group.

[0020] Ar in formula (1-1) 1 The substituents which the benzene ring and the naphthalene ring in the formula (I) may have are not particularly limited, but examples thereof include a halogen atom, an alkyl group having 1 to 4 carbon atoms, and an alkoxy group having 1 to 4 carbon atoms.

[0021] Ar in formula (1-1) 1 Examples of the aryl group include the following tetravalent groups: [ka] (In the formula, * represents a bond).

[0022] In the formula (1-2), n is an integer of 0 to 3, preferably an integer of 0 to 2, and more preferably 0.

[0023] Ar in formula (1-2-1) 2 In the above formula, the substituent that the phenylene group and the divalent group obtained by removing two hydrogen atoms from biphenyl may have is not particularly limited, but examples thereof include a halogen atom, an alkyl group having 1 to 4 carbon atoms, and an alkoxy group having 1 to 4 carbon atoms.

[0024] X in formula (1-2) 1 Examples of the group include the following groups. [ka] (In the formula, * represents a bond).

[0025] Specific examples of aromatic tetracarboxylic dianhydrides include pyromellitic dianhydride, benzene-1,2,3,4-tetracarboxylic dianhydride, naphthalene-1,2,3,4-tetracarboxylic dianhydride, naphthalene-1,2,5,6-tetracarboxylic dianhydride, naphthalene-1,2,6,7-tetracarboxylic dianhydride, naphthalene-1,2,7,8-tetracarboxylic dianhydride, and naphthalene-2,3,5,6-tetracarboxylic dianhydride. Naphthalene-2,3,6,7-tetracarboxylic dianhydride, naphthalene-1,4,5,8-tetracarboxylic dianhydride, biphenyl-2,2',3,3'-tetracarboxylic dianhydride, biphenyl-2,3,3',4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride, anthracene-1,2,3,4-tetracarboxylic dianhydride, anthracene-1,2,5,6-tetracarboxylic dianhydride, a Anthracene-1,2,6,7-tetracarboxylic dianhydride, Anthracene-1,2,7,8-tetracarboxylic dianhydride, Anthracene-2,3,6,7-tetracarboxylic dianhydride, Phenanthrene-1,2,3,4-tetracarboxylic dianhydride, Phenanthrene-1,2,5,6-tetracarboxylic dianhydride, Phenanthrene-1,2,6,7-tetracarboxylic dianhydride, Phenanthrene-1,2,7,8-tetracarboxylic dianhydride Examples of the dianhydride include, but are not limited to, phenanthrene-1,2,9,10-tetracarboxylic dianhydride, phenanthrene-2,3,5,6-tetracarboxylic dianhydride, phenanthrene-2,3,6,7-tetracarboxylic dianhydride, phenanthrene-2,3,9,10-tetracarboxylic dianhydride, phenanthrene-3,4,5,6-tetracarboxylic dianhydride, and phenanthrene-3,4,9,10-tetracarboxylic dianhydride. These may be used alone or in combination of two or more.

[0026] The structural formula of an example of an aromatic tetracarboxylic dianhydride is shown below. [ka] [ka]

[0027] The tetracarboxylic dianhydride may contain a tetracarboxylic dianhydride other than an aromatic tetracarboxylic dianhydride. Examples of such a tetracarboxylic dianhydride include 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2-dimethyl-1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-cyclopentane tetracarboxylic dianhydride, 1,2,4,5-cyclohexane tetracarboxylic dianhydride, 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene tetracarboxylic dianhydride, and 1,2,4,5-cyclohexane tetracarboxylic dianhydride. Examples of the compound include alicyclic tetracarboxylic dianhydrides such as 1,2-ene-1,2-dicarboxylic anhydride, 2,3,5-tricarboxy-2-cyclopentane acetic dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, 2,3,4,5-tetrahydrofuran tetracarboxylic dianhydride, and 3,5,6-tricarboxy-2-norbornane acetic dianhydride, and aliphatic tetracarboxylic dianhydrides such as 1,2,3,4-butane tetracarboxylic dianhydride.

[0028] The molar ratio of aromatic tetracarboxylic dianhydride in the tetracarboxylic dianhydride is not particularly limited, but is preferably 50 mol % or more, more preferably 70 mol % or more, and particularly preferably 90 mol % or more. The molar ratio of the aromatic tetracarboxylic dianhydride in the tetracarboxylic dianhydride may be 100 mol % or less, or may be less than 100 mol %.

[0029] <<Diamine component>> The diamine component is not particularly limited, but preferably contains an aromatic diamine, since a release layer having excellent heat resistance can be obtained. Here, the aromatic diamine is a compound in which a total of two amino groups (-NH2) are bonded to the same or different aromatic rings. The aromatic ring may be an aromatic hydrocarbon ring or an aromatic heterocycle.

[0030] The aromatic diamine is not particularly limited, but is preferably represented by the following formula (2-1) or (2-2) in that a release layer having superior heat resistance can be obtained. [ka] (In formula (2-1), X 11 represents a single bond, an ether bond, a carbonyl bond, an ester bond, a urethane bond, a urea bond, a thioether bond, a sulfonyl bond, -C(=O)N(-R)- (R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms), or a group represented by the following formula (2-1-1). R b each independently represents a halogen atom or an alkyl group having 1 to 4 carbon atoms. Each m independently represents an integer of 0 to 4. One (R b ) m In the above, when m is 2 or more, two or more R b may be the same or different. In formula (2-2), X 12 represents an -NH- group, an -O- group, or an -S- group. R c each independently represents a halogen atom or an alkyl group having 1 to 4 carbon atoms. p1 represents an integer of 0 to 3. p2 represents an integer of 0 to 4. (R c ) p1 In the above, when p1 is 2 or more, two or more R c may be the same or different. (R c ) p2 In this case, when p2 is 2 or more, two or more R c may be the same or different.) [ka] (In formula (2-1-1), Y 11 and Y 12 each independently represents a single bond, an ether bond, a carbonyl bond, an ester bond, a urethane bond, a urea bond, a thioether bond, a sulfonyl bond, or -C(=O)N(-R)- (R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms). Z 11 represents a divalent hydrocarbon group having 1 to 20 carbon atoms. * represents a bond.)

[0031] Z in formula (2-1-1) 11 Examples of the divalent hydrocarbon group having 1 to 20 carbon atoms include alkylene groups having 1 to 20 carbon atoms. The alkylene group having 1 to 20 carbon atoms may be either linear or branched, and specific examples thereof include, but are not limited to, methylene, ethylene, propylene, trimethylene, tetramethylene, pentylene, hexylene, heptylene, octylene, nonylene, decylene, undecylene, dodecylene, tridecylene, tetradecylene, pentadecylene, hexadecylene, heptadecylene, octadecylene, nonadecylene, and eicosanylene. In the present invention, an alkylene group having 2 to 6 carbon atoms is preferred, and a linear alkylene group having 2 to 6 carbon atoms is more preferred.

[0032] Z in formula (2-1-1) 11 The divalent hydrocarbon group having 1 to 20 carbon atoms may be, for example, a divalent hydrocarbon group having a fluorene skeleton.

[0033] In formula (2-1), an amino group (-NH2) and X are bonded to one benzene ring. 11 In order to preferably obtain the effects of the present invention, the position is preferably para.

[0034] In the formula (2-1), m is an integer of 0 to 4, preferably an integer of 0 to 2, and more preferably 0. In the formula (2-2), p1 is an integer of 0 to 3, preferably an integer of 0 to 2, and more preferably 0. In the formula (2-2), p2 is an integer of 0 to 4, preferably an integer of 0 to 2, and more preferably 0.

[0035] Examples of aromatic diamines include o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 2-methyl-1,4-phenylenediamine, 5-methyl-1,3-phenylenediamine, 4-methyl-1,3-phenylenediamine, 2-(trifluoromethyl)-1,4-phenylenediamine, 2-(trifluoromethyl)-1,3-phenylenediamine and 4-(trifluoromethyl)-1,3-phenylenediamine, benzidine, 2,2'-dimethylbenzidine, 3,3 '-dimethylbenzidine, 2,3'-dimethylbenzidine, 2,2'-bis(trifluoromethyl)benzidine, 3,3'-bis(trifluoromethyl)benzidine, 2,3'-bis(trifluoromethyl)benzidine, 4,4'-diaminophenyl ether, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-diaminobenzanilide, 5-amino-2-(3-aminophenyl)-1H-benzimidazole, 9,9-bis(4-aminophenyl)fluorene, and the like.

[0036] The structural formula of one example of an aromatic diamine is shown below. [ka] [ka] [ka] [ka]

[0037] The molar ratio of the aromatic diamine in the diamine component is not particularly limited, but is preferably 50 mol % or more, more preferably 70 mol % or more, and particularly preferably 90 mol % or more. The molar proportion of the aromatic diamine in the diamine component may be 100 mol % or less, or may be less than 100 mol %.

[0038] <<Dicarboxylic acid anhydride>> The dicarboxylic acid anhydride is not particularly limited, but preferably contains an aromatic dicarboxylic acid anhydride, since a release layer having excellent heat resistance can be obtained. Here, the aromatic dicarboxylic acid anhydride is a compound in which one acid anhydride group is bonded to the same or different aromatic rings. The aromatic ring may be an aromatic hydrocarbon ring or an aromatic heterocycle.

[0039] The aromatic dicarboxylic acid anhydride is preferably represented by the following formula (E1-1), since a release layer having superior heat resistance can be obtained. [ka] (In formula (E1-1), R 1 ~R 4 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 20 carbon atoms.

[0040] Specific examples of aromatic dicarboxylic anhydrides include phthalic anhydride, 2,3-naphthalenedicarboxylic anhydride, and 1,8-naphthalenedicarboxylic anhydride, etc. Among these, phthalic anhydride is particularly suitable in the present invention, taking into consideration safety, ease of handling, reactivity, etc.

[0041] The molar ratio of aromatic dicarboxylic anhydride in dicarboxylic anhydride is not particularly limited, but is preferably 50 mol % or more, more preferably 70 mol % or more, and particularly preferably 90 mol % or more. The molar ratio of the aromatic dicarboxylic anhydride in the dicarboxylic anhydride may be 100 mol % or less, or may be less than 100 mol %.

[0042] <<Monoamine components>> The monoamine component is not particularly limited, but preferably contains a monoamine having a ring structure, since a release layer having excellent heat resistance can be obtained. The ring structure may be a non-aromatic ring or an aromatic ring. The number of members in the ring structure is not particularly limited, and examples include 5- to 7-membered rings. The ring structure may be a monocyclic or polycyclic ring. Examples of the non-aromatic ring include an aliphatic hydrocarbon ring. The aromatic ring may be an aromatic hydrocarbon ring or an aromatic heterocycle.

[0043] The monoamine component is preferably represented by the following formula (E2-1) or formula (E2-2), since a release layer having superior heat resistance can be obtained. [ka] (In formula (E2-1) and formula (E2-2), R 1 ~R 5 R each independently represents a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a halogen atom. 1 ~R 5 Adjacent two of may be joined together to form a ring structure. R 6 represents a single bond or an alkylene group having 1 to 4 carbon atoms.

[0044] Examples of the monoamine component include aniline, 1-naphthylamine, 2-naphthylamine, 1-aminoanthracene, 2-aminoanthracene, 9-aminoanthracene, 9-aminophenanthracene, 2-aminobiphenyl, 3-aminobiphenyl, and 4-aminobiphenyl.

[0045] The structural formula of an example of the monoamine represented by formula (E2-1) is shown below. [ka]

[0046] The structural formula of an example of the monoamine represented by formula (E2-2) is shown below. [ka]

[0047] The molar ratio of monoamines having a ring structure in the monoamine component is not particularly limited, but is preferably 50 mol % or more, more preferably 70 mol % or more, and particularly preferably 90 mol % or more. The molar proportion of monoamines having a ring structure in the monoamine component may be 100 mol % or less, or may be less than 100 mol %.

[0048] The polyamic acid production process preferably includes adding a tetracarboxylic dianhydride to an organic solvent solution containing a diamine component and reacting the tetracarboxylic dianhydride. Since the tetracarboxylic dianhydride is often in a powder form and is difficult to dissolve in an organic solvent, the reaction is more likely to proceed uniformly when the tetracarboxylic dianhydride is added to an organic solvent solution containing a diamine component. The polyamic acid production process preferably includes adding a tetracarboxylic dianhydride to an organic solvent solution containing a diamine component and a monoamine component, and reacting the components. The polyamic acid production process preferably includes adding a tetracarboxylic dianhydride and a dicarboxylic anhydride to an organic solvent solution containing a diamine component and reacting them. In this case, the tetracarboxylic dianhydride and the dicarboxylic anhydride may be added to the organic solvent solution at the same time, or the tetracarboxylic dianhydride may be added to the organic solvent solution after the dicarboxylic anhydride is added to the organic solvent solution, or the dicarboxylic anhydride may be added to the organic solvent solution after the tetracarboxylic dianhydride is added to the organic solvent solution.

[0049] The polyamic acid production process may, for example, be the following modes (1) and (2). (1): A process for obtaining a polyamic acid by adding a diamine component, a monoamine component, and an organic solvent to a reaction vessel, and then adding a tetracarboxylic dianhydride to the reaction vessel and carrying out a reaction. (2): A step of adding a diamine component and an organic solvent to a reaction vessel, and then adding a tetracarboxylic dianhydride and a dicarboxylic anhydride to the reaction vessel and carrying out a reaction to obtain a polyamic acid.

[0050] The charge ratio (molar ratio) of the tetracarboxylic dianhydride (M1) and the diamine component (M2) can be appropriately set in consideration of the molecular weight of the desired polyamic acid, the ratio of monomer units, and the like, and the molar ratio (M1:M2) is, for example, 100:150 to 150:100. The molar amounts of the tetracarboxylic dianhydride, the diamine component, the dicarboxylic anhydride, and the monoamine component to be charged can be appropriately set taking into consideration the molecular weight of the desired polyamic acid, the ratio of the monomer units, and the like, but it is preferable that the following formula is satisfied. 0.8≦[M1+(0.5×M3)] / [M2+0.5×M4]≦1.2 M1: Molar amount of tetracarboxylic dianhydride M2: Molar amount of diamine component M3: Molar amount of dicarboxylic anhydride M4: Molar amount of monoamine component In the formula, the molar amount of either the dicarboxylic anhydride or the diamine component may be 0 moles.

[0051] The organic solvent used in the above-mentioned reaction is not particularly limited as long as it does not adversely affect the reaction, and specific examples thereof include m-cresol, 2-pyrrolidone, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-vinyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, 3-methoxy-N,N-dimethylpropylamide, 3-ethoxy-N,N-dimethylpropylamide, 3-propoxy-N,N-dimethylpropylamide, 3-isopropoxy-N,N-dimethylpropylamide, 3-butoxy-N,N-dimethylpropylamide, 3-sec-butoxy-N,N-dimethylpropylamide, 3-tert-butoxy-N,N-dimethylpropylamide, γ-butyrolactone, etc. The organic solvent may be used alone or in combination of two or more kinds.

[0052] In particular, the organic solvent used in the reaction preferably contains at least one selected from the group consisting of amides represented by the following formula (S1), amides represented by the following formula (S2), and amides represented by the following formula (S3), since the organic solvent dissolves the raw materials (diamine component, tetracarboxylic dianhydride, dicarboxylic anhydride, monoamine component) and the product (polyamic acid) well. [ka] (In formulas (S1) to (S3), R 51 , and R 53 each independently represents an alkyl group having 1 to 10 carbon atoms; R 54 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; R 52 represents an alkylene group having 1 to 5 carbon atoms.

[0053] Examples of the alkyl group having 1 to 10 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a s-butyl group, a t-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, etc. Among these, an alkyl group having 1 to 3 carbon atoms is preferred, and an alkyl group having 1 or 2 carbon atoms is more preferred.

[0054] Examples of the alkylene group having 1 to 5 carbon atoms include a methylene group, a 1,2-ethylene group, a 1,3-propylene group, a 1,4-butylene group, a 1,5-pentylene group, etc. Among these, a methylene group, a 1,2-ethylene group, and a 1,3-propylene group are preferred, and a methylene group and a 1,2-ethylene group are more preferred.

[0055] The reaction temperature may be appropriately set within the range from the melting point to the boiling point of the solvent used, and is usually about 0 to 100°C. In order to prevent imidization of the resulting polyamic acid and maintain a high content of polyamic acid units, the reaction temperature is preferably about 0 to 70°C, more preferably about 0 to 60°C, and even more preferably about 0 to 50°C. The reaction time cannot be generally defined since it depends on the reaction temperature and the reactivity of the raw materials, but it is usually about 1 to 100 hours.

[0056] By the method described above, a reaction solution containing a polyamic acid can be obtained.

[0057] (Polyamic acid) The polyamic acid of the present invention is a reaction product of raw material components including a tetracarboxylic dianhydride, a diamine component, and at least one of a dicarboxylic anhydride and a monoamine component. In other words, the polyamic acid of the present invention includes, as constituent components, a tetracarboxylic dianhydride, a diamine component, and at least one of a dicarboxylic anhydride and a monoamine component. About the components of polyamic acid 1 In H-NMR analysis, the molar ratio of the total of the dicarboxylic acid anhydride and the monoamine component to the total of the tetracarboxylic acid dianhydride and the diamine component (hereinafter sometimes referred to as "molar ratio") is 3 mol % or more. The larger the molar ratio, the better the releasability of the release layer obtained by using the polyamic acid, i.e., the smaller the peeling force required for peeling.

[0058] The molar proportion is 3 mol % or more, and more preferably 5 mol % or more. The upper limit of the molar ratio is not particularly limited, and the molar ratio may be, for example, 50 mol % or less, 30 mol % or less, or 15 mol % or less. In addition, when the polyamic acid contains a dicarboxylic anhydride, the polyamic acid may or may not contain a monoamine component. In addition, when the polyamic acid contains a monoamine component, the polyamic acid may or may not contain a dicarboxylic anhydride. Therefore, in the "total of dicarboxylic anhydride and monoamine component", one of the dicarboxylic anhydride and the monoamine component may be 0.

[0059] The molar ratio of polyamic acid is 1 H-NMR analysis, 13 It can be determined by C-NMR analysis or IR (infrared spectroscopy) analysis. The molar ratio of the polyamic acid is, for example, 1 It can be determined by H-NMR analysis. 1 In the H-NMR analysis, for example, in the group derived from the tetracarboxylic dianhydride, the group derived from the diamine component, the group derived from the dicarboxylic anhydride, and the group derived from the monoamine component in the polyamic acid, hydrogen atoms (protons: 1 Identify H) 1 These hydrogen atoms (protons: 1 The molar ratio can be calculated from the integrated intensity of the chemical shift of H. An example of this will be described in detail in the Examples below.

[0060] Specific and preferred examples of the tetracarboxylic dianhydride constituting the polyamic acid include the specific and preferred examples of the tetracarboxylic dianhydride given in the description of the method for producing the polyamic acid of the present invention. Specific and preferred examples of the diamine component constituting the polyamic acid include the specific and preferred examples of the diamine component given in the description of the method for producing the polyamic acid of the present invention. Specific and preferred examples of the dicarboxylic anhydride constituting the polyamic acid include the specific and preferred examples of the dicarboxylic anhydride given in the description of the method for producing the polyamic acid of the present invention. Specific and preferred examples of the monoamine component constituting the polyamic acid include the specific and preferred examples of the monoamine component given in the description of the method for producing the polyamic acid of the present invention.

[0061] The polyamic acid of the present invention is preferably produced by the method for producing a polyamic acid of the present invention. As described above, compared to the case where a polyamic acid is produced by reacting a tetracarboxylic dianhydride with a diamine component and then further reacting with at least one of a dicarboxylic anhydride and a monoamine component, the reaction between the tetracarboxylic dianhydride and the diamine component in the presence of at least one of a dicarboxylic anhydride and a monoamine component introduces more terminal groups (groups derived from the dicarboxylic anhydride and groups derived from the monoamine component) to the terminals of the polyamic acid. Therefore, according to the method for producing a polyamic acid of the present invention, a polyamic acid having a molar ratio of 3 mol % or more can be produced.

[0062] The weight average molecular weight of the polyamic acid of the present invention and the polyamic acid obtained by the method for producing a polyamic acid of the present invention is not particularly limited, but is preferably 3,000 or more, more preferably 5,000 or more, and even more preferably 10,000 or more. On the other hand, the upper limit of the weight average molecular weight of the polyamic acid is usually 2,000,000. However, in consideration of preventing the viscosity of the composition for forming the release layer from becoming excessively high and of reproducibly obtaining a highly flexible resin thin film, the weight average molecular weight of the polyamic acid is preferably 1,000,000 or less, and more preferably 200,000 or less.

[0063] (Composition for forming a release layer and method for producing the composition for forming a release layer) The release layer-forming composition of the present invention contains the polyamic acid of the present invention and an organic solvent. The method for producing a release layer-forming composition of the present invention is a method for producing a release layer-forming composition containing a polyamic acid and an organic solvent. The method for producing the release layer-forming composition includes producing a polyamic acid by the method for producing a polyamic acid of the present invention. The release layer-forming composition may contain other components in addition to the polyamic acid and the organic solvent.

[0064] The concentration of the polyamic acid relative to the total mass of the composition for forming the release layer is appropriately set taking into consideration the thickness of the thin film (release layer) to be produced and the viscosity of the composition, but is usually about 0.5 to 30 mass %, preferably about 2 to 25 mass %.

[0065] <Organic solvent> In the present invention, the reaction solution is usually filtered, and the filtrate can be used as it is, or the solution obtained by diluting or concentrating the filtrate can be used as the composition for forming a peeling layer of the present invention. By doing so, not only can the inclusion of impurities that may cause deterioration of the adhesion, peelability, etc. of the obtained peeling layer be reduced, but also the composition for forming a peeling layer can be efficiently obtained. The solvent used for dilution or concentration is not particularly limited, and examples thereof include the same as the specific examples of the reaction solvent for the above reaction, which may be used alone or in combination of two or more kinds.

[0066] Among the above specific examples, in consideration of obtaining a highly flat resin thin film with good reproducibility, the following solvents are preferred: N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, N-ethyl-2-pyrrolidone, γ-butyrolactone, ethyl lactate, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cycloheptane, cyclohexane, diethylene glycol ethyl methyl ether, and ethylene glycol.

[0067] <Other ingredients> The other components are not particularly limited, and examples thereof include a crosslinking agent (hereinafter also referred to as a crosslinkable compound).

[0068] <<Crosslinkable compound>> Examples of crosslinkable compounds include, but are not limited to, compounds containing two or more epoxy groups, melamine derivatives, benzoguanamine derivatives, and glycolurils having a group in which the hydrogen atom of an amino group is substituted with a methylol group, an alkoxymethyl group, or both.

[0069] Specific examples of the crosslinkable compound are listed below, but the invention is not limited thereto. Examples of the compound containing two or more epoxy groups include the following compounds. Epolead GT-401, Epolead GT-403, Epolead GT-301, Epolead GT-302, Celloxide 2021, Celloxide 3000 (all manufactured by Daicel Corporation), and other epoxy compounds having a cyclohexene structure; Bisphenol A type epoxy compounds such as Epicoat 1001, Epicoat 1002, Epicoat 1003, Epicoat 1004, Epicoat 1007, Epicoat 1009, Epicoat 1010, and Epicoat 828 (all manufactured by Japan Epoxy Resins Co., Ltd. (currently manufactured by Mitsubishi Chemical Corporation, jER (registered trademark) series)); Bisphenol F type epoxy compounds such as Epicoat 807 (manufactured by Japan Epoxy Resins Co., Ltd. (now Mitsubishi Chemical Corporation)); Phenol novolac epoxy compounds such as Epicoat 152, Epicoat 154 (both manufactured by Japan Epoxy Resins Co., Ltd. (currently manufactured by Mitsubishi Chemical Corporation, jER (registered trademark) series)), EPPN201, EPPN202 (both manufactured by Nippon Kayaku Co., Ltd.); Cresol novolac epoxy compounds such as ECON-102, ECON-103S, ECON-104S, ECON-1020, ECON-1025, and ECON-1027 (all manufactured by Nippon Kayaku Co., Ltd.), and Epicoat 180S75 (manufactured by Japan Epoxy Resins Co., Ltd. (currently manufactured by Mitsubishi Chemical Corporation, jER (registered trademark) series)); Naphthalene-type epoxy compounds such as V8000-C7 (manufactured by DIC Corporation); Alicyclic epoxy compounds such as Denacol EX-252 (manufactured by Nagase ChemteX Corporation), CY175, CY1770, CY179, Araldite CY-182, Araldite CY-192, Araldite CY-184 (all manufactured by BASF), Epiclon 200, Epiclon 400 (all manufactured by DIC Corporation), Epicoat 871, Epicoat 872 (all manufactured by Japan Epoxy Resins Co., Ltd. (currently manufactured by Mitsubishi Chemical Corporation, jER (registered trademark) series)), ED-5661, ED-5662 (all manufactured by Celanese Coatings Co., Ltd.); Aliphatic polyglycidyl ether compounds such as Denacol EX-611, Denacol EX-612, Denacol EX-614, Denacol EX-622, Denacol EX-411, Denacol EX-512, Denacol EX-522, Denacol EX-421, Denacol EX-313, Denacol EX-314, and Denacol EX-312 (all manufactured by Nagase ChemteX Corporation).

[0070] Examples of melamine derivatives, benzoguanamine derivatives, or glycolurils in which the hydrogen atom of an amino group has been substituted with a methylol group, an alkoxymethyl group, or both include the following compounds. MX-750, which has an average of 3.7 methoxymethyl groups substituted per triazine ring, and MW-30, which has an average of 5.8 methoxymethyl groups substituted per triazine ring (both manufactured by Sanwa Chemical Co., Ltd.); Methoxymethylated melamines such as Cymel 300, Cymel 301, Cymel 303, Cymel 350, Cymel 370, Cymel 771, Cymel 325, Cymel 327, Cymel 703, and Cymel 712 (all manufactured by Mitsui Cyanamid Co., Ltd. (currently Nippon Cytec Industries Co., Ltd.)); Methoxymethylated butoxymethylated melamines such as Cymel 235, Cymel 236, Cymel 238, Cymel 212, Cymel 253, and Cymel 254 (all manufactured by Mitsui Cyanamid Co., Ltd. (currently Nippon Cytec Industries Co., Ltd.)); Butoxymethyl melamine such as Cymel 506 and Cymel 508 (both manufactured by Mitsui Cyanamid Co., Ltd. (currently Nippon Cytec Industries Co., Ltd.)); Carboxylic acid-containing methoxymethylated isobutoxymethylated melamine such as Cymel 1141 (manufactured by Mitsui Cyanamid Co., Ltd. (now Nippon Cytec Industries Co., Ltd.)); Methoxymethylated and ethoxymethylated benzoguanamines such as Cymel 1123 (manufactured by Mitsui Cyanamid Co., Ltd. (now Nippon Cytec Industries Co., Ltd.)); Methoxymethylated butoxymethylated benzoguanamines such as Cymel 1123-10 (manufactured by Mitsui Cyanamid Co., Ltd. (now Nippon Cytec Industries Co., Ltd.)); Butoxymethylated benzoguanamines such as Cymel 1128 (manufactured by Mitsui Cyanamid Co., Ltd. (now Nippon Cytec Industries Co., Ltd.)); Carboxy group-containing methoxymethylated and ethoxymethylated benzoguanamines such as Cymel 1125-80 (manufactured by Mitsui Cyanamid Co., Ltd. (currently Nippon Cytec Industries Co., Ltd.)); Butoxymethylated glycoluril such as Cymel 1170 (manufactured by Mitsui Cyanamid Co., Ltd. (now Nippon Cytec Industries Co., Ltd.)); Methylol glycoluril such as Cymel 1172 (manufactured by Mitsui Cyanamid Co., Ltd. (now Nippon Cytec Industries Co., Ltd.))

[0071] The viscosity of the composition for forming the release layer is appropriately set taking into consideration the thickness of the thin film to be produced, and when the objective is to obtain a resin thin film having a thickness of about 0.05 to 5 μm with good reproducibility, the viscosity is usually about 3 to 10,000 mPa·s at 25°C, preferably about 5 to 1,000 mPa·s, and more preferably about 8 to 200 mPa·s. Here, the viscosity can be measured using a commercially available viscometer for measuring the viscosity of liquids, for example, by referring to the procedure described in JIS K7117-2, under the condition of a composition temperature of 25°C. Preferably, a cone-plate type (corn-plate type) rotational viscometer is used as the viscometer, and preferably, the same type of viscometer is used with a standard cone rotor of 1°34'×R24, and the composition temperature can be measured under the condition of a composition temperature of 25°C. An example of such a rotational viscometer is TVE-25H manufactured by Toki Sangyo Co., Ltd.

[0072] (Release layer and method for producing release layer) The release layer of the present invention is formed from the release layer-forming composition of the present invention. The method for producing a release layer of the present invention includes, for example, a step of forming a release layer using a composition for forming a release layer produced by the method for producing a composition of the present invention.

[0073] For example, a thin film (release layer) can be obtained by applying the release layer forming composition of the present invention or a release layer forming composition produced by the composition production method of the present invention to a substrate and heating it.

[0074] Examples of the substrate (base material) include glass, plastic (polycarbonate, polymethacrylate, polystyrene, polyester, polyolefin, epoxy, melamine, triacetyl cellulose, ABS, AS, norbornene-based resin, etc.), metal (silicon wafer, etc.), metal compound (silicon nitride, etc.), wood, paper, slate, etc., and those containing glass, silicon nitride or silicon wafer are preferred. In particular, glass and silicon nitride are more preferred because the release layer obtained from the release layer forming composition according to the present invention has sufficient adhesion thereto. The substrate surface may be composed of a single material, or may be composed of two or more materials. The substrate surface may be composed of two or more materials in a certain range of the substrate surface and the remaining surface is composed of another material, or in a certain pattern such as a dot pattern or a line and space pattern on the entire substrate surface, among other materials.

[0075] The coating method is not particularly limited, but examples thereof include cast coating, spin coating, blade coating, dip coating, roll coating, bar coating, die coating, inkjet printing, and printing methods (relief printing, intaglio printing, planographic printing, screen printing, etc.).

[0076] Methods for imidizing the polyamic acid contained in the composition for forming a release layer include thermal imidization, in which the composition applied to a substrate is heated as is, and catalytic imidization, in which a catalyst is added to the composition and then heated.

[0077] The catalytic imidization of polyamic acid can be carried out by adding a catalyst to a composition for forming a release layer, stirring the mixture to prepare a catalyst-added composition, and then applying the composition to a substrate and heating the composition. The amount of the catalyst is 0.1 to 30 times by mole, preferably 1 to 20 times by mole, the amount of the amic acid group. In addition, acetic anhydride or the like can be added as a dehydrating agent to the catalyst-added composition, and the amount is 1 to 50 times by mole, preferably 3 to 30 times by mole, the amount of the amic acid group.

[0078] As the imidization catalyst, a tertiary amine is preferably used, and examples of the tertiary amine include pyridine, substituted pyridines, imidazole, substituted imidazoles, picoline, quinoline, and isoquinoline.

[0079] The heating temperature during thermal imidization and catalytic imidization is usually appropriately determined within the range of 50 to 550°C, but is preferably 200°C or higher, and preferably 450°C or lower. By setting the heating temperature in this manner, it becomes possible to prevent the obtained film from becoming brittle and to allow the imidization reaction to proceed sufficiently. The heating time cannot be generally specified because it varies depending on the heating temperature, but is usually 5 minutes to 5 hours. The imidization rate may be, for example, in the range of 50 to 100%.

[0080] A preferred example of the heating mode in the present invention, taking into consideration the heat resistance of the resulting release layer and the versatility of the apparatus used, is a method in which the applied composition is heated at 50 to 100° C. for 1 to 30 minutes, then heated at 110 to 150° C. for 3 minutes to 1 hour, and then the heating temperature is gradually increased to finally heat at 200 to 300° C. for 10 minutes to 2 hours. In particular, it is preferable to heat at 80 to 120° C. for 5 to 30 minutes, and then at 230 to 300° C. for 30 minutes to 1 hour.

[0081] Examples of the heating device include a hot plate, an oven, etc. The heating atmosphere may be air or an inert gas, and may be normal pressure or reduced pressure.

[0082] The thickness of the release layer is usually about 0.01 to 10 μm, and preferably about 0.05 to 5 μm, and the thickness of the coating film before heating is adjusted to achieve a release layer of the desired thickness.

[0083] The release layer described above has excellent adhesion to a substrate, particularly a substrate such as glass or silicon nitride, and has appropriate adhesion to and appropriate release properties with a resin substrate. Therefore, the release layer according to the present invention can be suitably used in a manufacturing process for a flexible electronic device to release the resin substrate together with a circuit or the like formed on the resin substrate from the substrate without damaging the resin substrate.

[0084] (Method of manufacturing a flexible electronic device having a resin substrate) In the method of the present invention for producing a flexible electronic device having a resin substrate, for example, the release layer of the present invention is used. In the method of the present invention for producing a flexible electronic device having a resin substrate, for example, a release layer produced by the method of the present invention for producing a release layer is used.

[0085] An example of a method for producing a flexible electronic device using the release layer of the present invention will now be described. A release layer is formed on a substrate by the above-mentioned method using the composition for forming a release layer according to the present invention. A resin solution for forming a resin substrate is applied onto the release layer, and the coating is heated to form a resin substrate fixed to the substrate via the release layer according to the present invention. At this time, a resin substrate is formed with an area larger than that of the release layer so as to cover the entire release layer. Examples of the resin substrate include resin substrates made of polyimide resin, acrylic resin, and cycloolefin resin, which are typical resin substrates for flexible electronic devices, and examples of resin solutions for forming the resin substrate include polyimide solutions, polyamic acid solutions, acrylic polymer solutions, cycloolefin polymer solutions, and cycloolefin copolymer solutions. The resin substrate may be formed according to a conventional method.

[0086] Next, a desired circuit is formed on the resin substrate fixed to the base via the release layer according to the present invention, and then the resin substrate is cut, for example, along the release layer, and the resin substrate together with the circuit is peeled off from the release layer to separate the resin substrate from the base. At this time, a part of the base may be cut together with the release layer.

[0087] The present invention also provides the following method for producing an object to be peeled. A step of applying the composition for forming a release layer of the present invention onto a substrate and baking it to form a release layer; forming an object to be peeled on the peeling layer; and A step of peeling the object to be peeled from the peeling layer. The present invention provides a method for producing an object to be peeled, comprising the steps of:

[0088] In the above-mentioned manufacturing method, the firing conditions for forming the release layer can be the same as those described above. The "object to be peeled" may be a single layer or multiple layers. The layer immediately above the peeling layer of the "object to be peeled" (usually a resin substrate) should have good peelability from the peeling layer, or in other words, poor adhesion to the peeling layer, depending on the peeling layer used.

[0089] Furthermore, the present invention relates to a laminate for use in a flexible electronic device, comprising: A substrate; a release layer formed on the substrate; A resin substrate formed on the release layer; A laminate having the following structure is provided: EXAMPLES

[0090] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The abbreviations of the compounds used in the following examples, and the methods for measuring the weight average molecular weight and molecular weight distribution are as follows.

[0091] <Abbreviation of compound> <<Tetracarboxylic acid dianhydride>> PMDA: Pyromellitic dianhydride BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride NADA: 2,3,6,7-naphthalenetetracarboxylic acid 2,3:6,7-dianhydride <<Diamine>> ODA: 4,4'-oxydianiline 34ODA: 3,4'-oxydianiline BAPB: 1,4-bis(4-aminophenoxy)benzene DABA: 4,4'-diaminobenzanilide APAB: 4-aminophenyl 4-aminobenzoate DADPM: 4,4'-methylenedianiline DABA-Me: 4-amino-N-(4-aminophenyl)-N-methylbenzamide DABP: 4,4'-diaminobenzophenone ABI: 5-amino-2-(4-aminophenyl)benzimidazole ABO: 5-amino-2-(4-aminophenyl)benzoxazole p-PDA: p-phenylenediamine <<Monoamine (end group)>> An: Aniline BzAn: Benzylaniline ·TI: m-Toluidine DMAn: 3,5-Dimethylaniline EAn: p-Ethylaniline HxAn: p-Hexylaniline FAn: p-Fluoroaniline 3FAn: m-(trifluoromethyl)aniline APy: m-aminopyridine <<Dicarboxylic anhydride (end group)>> ·PA: Phthalic anhydride <<Solvent>> ·NMP: N-methyl-2-pyrrolidone NEP: N-ethyl-2-pyrrolidone EL: Ethyl lactate

[0092] <Measurement of weight average molecular weight and molecular weight distribution> The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the polymer were measured using a GPC apparatus manufactured by JASCO Corporation (column: KD803 and KD805 manufactured by Shodex; eluent: dimethylformamide / LiBr·H2O (30 mM) / H3PO4 (30 mM) / THF (1%); flow rate: 1.0 mL / min; column temperature: 50°C; Mw: standard polyethylene oxide equivalent value) (the same applies in the following Examples and Comparative Examples).

[0093] [1] Polymer synthesis Polyamic acid was synthesized by the following method. The polymer was not isolated from the resulting polymer-containing reaction liquid, but was diluted as described below to prepare a composition for forming a resin substrate or a composition for forming a release layer.

[0094] [Synthesis Example 1] Synthesis of polyamic acid A1 1.73 g (8.6 mmol) of ODA and 0.18 g (1.9 mmol) of An were dissolved in 29 g of NEP, and then cooled to 5 to 15°C in an ice bath under a nitrogen atmosphere. 2.09 g (9.6 mmol) of PMDA and 7 g of NEP were added to the resulting solution, and reacted at 23°C for 24 hours to obtain polyamic acid A1. The Mw of polyamic acid A1 was 13,570, and the Mw / Mn was 1.7.

[0095] [Synthesis Examples 2 to 22] Synthesis of polyamic acids A2 to A22 Polyamic acids A2 to A22 were obtained in the same manner as in Synthesis Example 1, except that the types and amounts of tetracarboxylic dianhydride, diamine, and end group, as well as the type and reaction temperature of the solvent were changed to the combinations shown in Tables 1-1 to 1-4. The Mw and Mw / Mn of the resulting polyamic acids A2 to A22 are shown in Tables 1-1 to 1-4.

[0096] [Synthesis Example 23] Synthesis of polyamic acid A23 1.88 g (9.4 mmol) of ODA was dissolved in 29 g of NEP, and then cooled to 5 to 15°C in an ice bath under a nitrogen atmosphere. 1.84 g (8.4 mmol) of PMDA, 0.28 g (1.9 mmol) of PA, and 7 g of NEP were added to the resulting solution, and reacted at 23°C for 24 hours to obtain polyamic acid A23. The Mw of polyamic acid A23 was 13,400, and the Mw / Mn was 1.7.

[0097] [Synthesis Example 24] Synthesis of polyamic acid A24 1.81 g (9.1 mmol) of ODA was dissolved in 29 g of NEP, and then cooled to 5 to 15°C in an ice bath under a nitrogen atmosphere. 1.38 g (6.3 mmol) of PMDA, 0.80 g (5.4 mmol) of PA, and 7 g of NEP were added to the resulting solution, and reacted at 23°C for 24 hours to obtain polyamic acid A24. The Mw of polyamic acid A24 was 4,550, and the Mw / Mn was 1.5.

[0098] [Synthesis Example 25] Synthesis of polyamic acid A25 9.11 g (45.5 mmol) of ODA and 0.45 g (4.8 mmol) of An were dissolved in 144 g of NMP, and then cooled to 5 to 15°C in an ice bath under a nitrogen atmosphere. 10.44 g (47.9 mmol) of PMDA and 7 g of NMP were added to the resulting solution, and after stirring for 30 minutes, the mixture was reacted at 50°C for 24 hours to obtain polyamic acid A25. The Mw of polyamic acid A25 was 19,370, and the Mw / Mn was 1.8.

[0099] [Synthesis Example 26 (Comparative Synthesis Example 1)] Synthesis of polyamic acid C1 1.86 g (9.3 mmol) of ODA was dissolved in 29 g of NEP, and then cooled to 5 to 15° C. in an ice bath under a nitrogen atmosphere. 2.14 g (9.8 mmol) of PMDA and 7 g of NEP were added to the resulting solution, and reacted at 23° C. for 24 hours to obtain polyamic acid C1. The Mw of polyamic acid C1 was 44,850, and the Mw / Mn was 1.9.

[0100] [Synthesis Example 27 (Comparative Synthesis Example 2)] Synthesis of polyamic acid C2 1.97 g (9.8 mmol) of ODA was dissolved in 29 g of NEP, and then cooled to 5 to 15° C. in an ice bath under a nitrogen atmosphere. 2.03 g (9.3 mmol) of PMDA and 7 g of NEP were added to the resulting solution, and reacted at 23° C. for 24 hours to obtain polyamic acid C2. The Mw of polyamic acid C2 was 31,520, and the Mw / Mn was 2.1.

[0101] [Synthesis Example 28 (Comparative Synthesis Example 3)] Synthesis of polyamic acid C3 1.73 g (8.6 mmol) of ODA was dissolved in 26 g of NEP, and the solution was cooled to 5 to 15°C in an ice bath under a nitrogen atmosphere. 2.09 g (9.6 mmol) of PMDA and 6 g of NEP were added to the resulting solution, and the mixture was reacted at 23°C for 24 hours. 0.18 g (1.9 mmol) of An and 4 g of NEP were added to the resulting solution, and the mixture was reacted at 23°C for an additional 6 hours to obtain polyamic acid C3. The Mw of polyamic acid C3 was 57,930, and the Mw / Mn was 1.6.

[0102] [Table 1-1]

[0103] [Table 1-2]

[0104] [Table 1-3]

[0105] [Table 1-4]

[0106] [Synthesis Example F1] Synthesis of polyamic acid F1 16.37 g (151.3 mmol) of p-PDA was dissolved in 240 g of NMP. 43.64 g (148.3 mmol) of BPDA was added to the resulting solution, and the mixture was reacted at 23° C. for 24 hours under a nitrogen atmosphere to obtain polyamic acid F1. The polyamic acid F1 had an Mw of 107,300 and an Mw / Mn of 3.6.

[0107] [2] Preparation of composition for forming release layer [Example 1-1] EL and NEP were added to the reaction liquid obtained in Synthesis Example 1, and the mixture was diluted so that the polymer concentration was 5 mass % and the EL concentration was 20 mass %, to obtain a composition 1 for forming a release layer.

[0108] [Examples 1-2 to 1-25] Compositions 2 to 25 for forming a release layer, each having a polymer concentration of 5 mass% and an EL concentration of 20 mass%, were obtained in the same manner as in Example 1-1, except that the reaction liquids obtained in Synthesis Examples 2 to 25 were used instead of the reaction liquid obtained in Synthesis Example 1. When the polymer solution was NEP, it was diluted with NEP, and when the polymer solution was NMP, it was diluted with NMP.

[0109] [Comparative Examples 1-1 to 1-3] Compositions 25 to 29 for forming a peeling layer, each having a polymer concentration of 5% by mass and an EL of 20% by mass, were obtained in the same manner as in Example 1-1, except that the reaction liquid obtained in Comparative Synthesis Examples 1 to 3 was used instead of the reaction liquid obtained in Synthesis Example 1.

[0110] Table 2 shows the type of polyamic acid in each of the release layer-forming compositions of Examples 1-1 to 1-25 and Comparative Examples 1-1 to 1-3.

[0111] [Table 2]

[0112] [3] Formation of peeling layer [Example 2-1] Using a spin coater, the composition for forming a release layer obtained in Example 1-1 was applied onto a 100 mm x 100 mm glass substrate (same below). The obtained coating film was heated at 100°C for 2 minutes using a hot plate, and then at 300°C for 30 minutes using an oven under a nitrogen atmosphere, and the heating temperature was increased to 450°C (10°C / min), and further heated at 450°C for 30 minutes to form a release layer with a thickness of 100 to 200 nm on the glass substrate, thereby obtaining a glass substrate with a release layer. During the temperature increase, the glass substrate with the coating film was heated in the oven without being taken out of the oven.

[0113] [Examples 2-2 to 2-25] A release layer was formed in the same manner as in Example 2-1, except that the compositions for forming a release layer obtained in Examples 1-2 to 1-25 were used instead of the composition for forming a release layer obtained in Example 1-1, and a glass substrate with a release layer was obtained.

[0114] [Comparative Examples 2-1 to 2-3] A release layer was formed in the same manner as in Example 2-1, except that the compositions for forming a release layer obtained in Comparative Examples 1-1 to 1-3 were used instead of the composition for forming a release layer obtained in Example 1-1, and a glass substrate with a release layer was obtained.

[0115] [4] Formation of resin substrate and evaluation of peelability [Example 3-1] Using a spin coater, the resin substrate forming composition F1 was applied onto the release layer (resin thin film) on the glass substrate with the release layer obtained in Example 2-1.Then, the obtained coating film was heated using a hot plate to form a resin substrate layer.The baking conditions of the resin substrate forming composition F1 are described below. The glass substrate was heated at 80° C. for 10 minutes using a hot plate, then heated at 120° C. for 10 minutes using an oven under a nitrogen atmosphere, the heating temperature was increased to 180° C. (10° C. / min, the same applies below), further heated at 180° C. for 60 minutes, the heating temperature was increased to 250° C., further heated at 250° C. for 10 minutes, the heating temperature was increased to 450° C., and further heated at 450° C. for 10 minutes to form a resin substrate having a thickness of 10 μm on the release layer. During the temperature increase, the glass substrate with the coating was heated in the oven without being taken out of the oven.

[0116] [Examples 3-2 to 3-25, Comparative Examples 3-1 to 3-3] A resin substrate was formed on a release layer in the same manner as in Example 3-1, except that the glass substrates with a release layer obtained in Examples 2-2 to 2-25 and Comparative Examples 2-1 to 2-3 were used instead of the glass substrate with a release layer obtained in Example 2-1.

[0117] <Evaluation of peel strength of resin substrate> The resin substrates and the glass substrates with a release layer obtained in Examples 3-1 to 3-25 and Comparative Examples 3-1 to 3-3 were cut together with the release layer to prepare strips of 25 mm x 70 mm. Furthermore, Cellotape (registered trademark) (CT-24, manufactured by Nichiban Co., Ltd.) was applied onto the strips, and then the resin substrates were peeled off from the release layer at a peel angle of 90° and a peel speed of 300 mm / min using an autograph AGS-X500N (manufactured by Shimadzu Corporation), and the peel force was measured. Those that could not be peeled off were deemed not peelable. The results are shown in Table 3. [Evaluation Criteria] a: Peel force less than 0.30N / 25mm b: Peeling force of 0.30N / 25mm or more and less than 0.50N / 25mm c: Peeling force of 0.50N / 25mm or more

[0118] [5] Heat resistance evaluation of the peeling layer The release layer was scraped off from the glass substrates with the release layer obtained in Examples 2-1 to 2-25 and Comparative Examples 2-1 to 2-3, and the temperature at which the weight loss was 1% when heated at a rate of 10° C. / min in a nitrogen atmosphere was determined by thermogravimetry. The results are shown in Table 3. <Evaluation criteria> A: 500℃ or higher B: 450℃ or higher and less than 500℃ C: 450℃ or more

[0119] [Table 3]

[0120] [7] Composition analysis of polyamic acid The reaction solutions of the polyamic acids obtained in Synthesis Example 1-1 and Comparative Synthesis Example 1-3 were purified by reprecipitation with chloroform to recover solid polyamic acid. The solid thus obtained was dissolved in deuterated DMSO, 1 H-NMR analysis was performed. The results are shown in Table 4. The calculation method for each unit is described below. < 1 Calculation method using H-NMR> Among the hydrogen atoms of the groups derived from PMDA in the polyamic acids A1 and C3, hydrogen atoms that can be distinguished from the hydrogen atoms of the groups derived from ODA and the hydrogen atoms of the groups derived from An (proton: 1 The integrated intensity A of the chemical shift of 2H (chemical shift A; 7.99 ppm + 8.35 ppm (s, 2H)) was calculated. Among the hydrogen atoms of the groups derived from ODA in the polyamic acids A1 and C3, hydrogen atoms that can be distinguished from the hydrogen atoms of the groups derived from PMDA and the hydrogen atoms of the groups derived from An (proton: 1 H) (chemical shift B; (7.04 ppm (m, 4H)-7.10 (m, 1H peak due to An)) was calculated. Among the hydrogen atoms of the groups derived from An in the polyamic acids A1 and C3, hydrogen atoms that can be distinguished from the hydrogen atoms of the groups derived from PMDA and the hydrogen atoms of the groups derived from ODA (proton: 1 The integrated intensity C of the chemical shift of 2H (chemical shift C; 7.35 ppm (m, 2H)) was calculated. Here, the chemical shift A is the chemical shift of two hydrogen atoms of the group derived from PMDA. Therefore, the integral intensity A per one hydrogen atom is 1 / 2 of the integral intensity A. And, 1 / 2 of the integral intensity A is related to the molar ratio of the group derived from PMDA in the polyamic acid. The chemical shift B is the chemical shift of four hydrogen atoms of the group derived from ODA. Therefore, the integral intensity B per one hydrogen atom is 1 / 4 of the integral intensity B. And, 1 / 4 of the integral intensity B is related to the molar ratio of the group derived from ODA in the polyamic acid. The chemical shift C is the chemical shift of two hydrogen atoms of the group derived from An. Therefore, the integral intensity C per one hydrogen atom is 1 / 2 of the integral intensity C. And, 1 / 2 of the integral intensity C is related to the molar ratio of the group derived from An in the polyamic acid.

[0121] Polyamic acid A1 1 In the H-NMR analysis, when 1 / 2 of the integrated intensity A was taken as 100, 1 / 4 of the integrated intensity B was 92, and 1 / 2 of the integrated intensity C was 14. These values ​​correspond to the molar ratios of the group derived from PMDA, the group derived from ODA, and the group derived from An in the polyamic acid A1. The molar ratio (%) of the terminal group An can be calculated as follows. Molar ratio of end groups (%) = C m / (A m +B m ) A m : 1 / 2 of integral intensity A B m : 1 / 4 of integral intensity B C m : 1 / 2 of integral intensity C As a result, the molar proportion of the monoamine component (An) in the polyamic acid A1 was 7.3 mol %.

[0122] Polyamic acid C3 1In the H-NMR analysis, when 1 / 2 of the integrated intensity A was taken as 100, 1 / 4 of the integrated intensity B was 95, and 1 / 2 of the integrated intensity C was 4. These values ​​correspond to the molar ratios of the group derived from PMDA, the group derived from ODA, and the group derived from An in polyamic acid C3. The molar proportion of the monoamine component (An) in the polyamic acid C3 was 2.1 mol %.

[0123] [Table 4]

[0124] From the results in Table 3, it was confirmed that the release layers prepared from the release layer-forming compositions of the Examples have the property of being easily peeled off from the resin substrate. On the other hand, it was confirmed that the release layers prepared from the release layer-forming compositions of Comparative Examples 1-1 and 1-2 containing a polyamic acid having no terminal group, and the release layer-forming composition of Comparative Example 1-3 containing a polyamic acid synthesized by a method different from that of the Examples, are difficult to peel off from the resin substrate.

Claims

1. A method for producing a polyamic acid, comprising a polyamic acid production step of producing a polyamic acid, the polyamic acid is a reaction product of raw material components including a tetracarboxylic dianhydride, a diamine component, and at least one of a dicarboxylic anhydride and a monoamine component; the reaction between the tetracarboxylic dianhydride and the diamine component in the polyamic acid production step is carried out in the presence of at least one of the dicarboxylic anhydride and the monoamine component.

2. the dicarboxylic acid anhydride comprises an aromatic dicarboxylic acid anhydride, The monoamine component includes a monoamine having a ring structure. A method for producing the polyamic acid according to claim 1 .

3. The dicarboxylic acid anhydride is represented by the following formula (E1-1): The monoamine component is represented by the following formula (E2-1) or formula (E2-2): A method for producing the polyamic acid according to claim 1 . 【Chemistry 1】 (In formula (E1-1), R 1 ~R 4 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 20 carbon atoms. 【Chemistry 2】 (In formula (E2-1) and formula (E2-2), R 1 ~R 5 R each independently represents a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a halogen atom. 1 ~R 5 Adjacent two of may be joined together to form a ring structure. R 6 represents a single bond or an alkylene group having 1 to 4 carbon atoms.

4. The method for producing a polyamic acid according to claim 1 , wherein the tetracarboxylic dianhydride includes an aromatic tetracarboxylic dianhydride.

5. The method for producing a polyamic acid according to claim 4, wherein the aromatic tetracarboxylic dianhydride is represented by the following formula (1-1) or formula (1-2): 【Chemistry 3】 (In formula (1-1), Ar 1 represents a tetravalent group obtained by removing two pairs of adjacent hydrogen atoms from a benzene ring which may have a substituent, or a tetravalent group obtained by removing two pairs of adjacent hydrogen atoms from a naphthalene ring which may have a substituent. In formula (1-2), X 1 represents a single bond, an ether bond, a carbonyl bond, an ester bond, a urethane bond, a urea bond, a thioether bond, a sulfonyl bond, -C(=O)N(-R)- (R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms), or a group represented by the following formula (1-2-1). R a each independently represents a halogen atom or an alkyl group having 1 to 4 carbon atoms. Each n independently represents an integer of 0 to 3. One (R a ) n When n is 2 or more, two or more R a may be the same or different.) 【Chemistry 4】 (In formula (1-2-1), Y 1 and Y 2 each independently represents a single bond, an ether bond, a carbonyl bond, an ester bond, a urethane bond, a urea bond, a thioether bond, a sulfonyl bond, or -C(=O)N(-R)- (R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms). Ar 2 represents a divalent group obtained by removing two hydrogen atoms from a phenylene group which may have a substituent, or a biphenyl group which may have a substituent. * represents a bond.)

6. The method for producing a polyamic acid according to claim 1 , wherein the diamine component comprises an aromatic diamine.

7. The method for producing a polyamic acid according to claim 6, wherein the aromatic diamine is represented by the following formula (2-1) or formula (2-2): 【Chemistry 5】 (In formula (2-1), X 11 represents a single bond, an ether bond, a carbonyl bond, an ester bond, a urethane bond, a urea bond, a thioether bond, a sulfonyl bond, -C(=O)N(-R)- (R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms), or a group represented by the following formula (2-1-1). R b each independently represents a halogen atom or an alkyl group having 1 to 4 carbon atoms. Each m independently represents an integer of 0 to 4. One (R b ) m In the formula, when m is 2 or more, two or more R b may be the same or different. In formula (2-2), X 12 represents an -NH- group, an -O- group, or an -S- group. R c each independently represents a halogen atom or an alkyl group having 1 to 4 carbon atoms. p1 represents an integer of 0 to 3. p2 represents an integer of 0 to 4. (R c ) p1 When p1 is 2 or more, two or more R c may be the same or different. (R c ) p2 When p2 is 2 or more, two or more R c may be the same or different.) 【Chemistry 6】 (In formula (2-1-1), Y 11 and Y 12 each independently represents a single bond, an ether bond, a carbonyl bond, an ester bond, a urethane bond, a urea bond, a thioether bond, a sulfonyl bond, or -C(=O)N(-R)- (R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms). Z 11 represents a divalent hydrocarbon group having 1 to 20 carbon atoms. * represents a bond.)

8. the raw material components include the monoamine component, 2. The method for producing a polyamic acid according to claim 1, wherein the polyamic acid production step comprises adding the tetracarboxylic dianhydride to an organic solvent solution containing the diamine component and the monoamine component, and reacting the tetracarboxylic dianhydride with the diamine component and the monoamine component.

9. The raw material component contains the dicarboxylic acid anhydride, 2. The method for producing a polyamic acid according to claim 1, wherein the polyamic acid production step comprises adding the tetracarboxylic dianhydride and the dicarboxylic anhydride to an organic solvent solution containing the diamine component, and reacting the tetracarboxylic dianhydride and the dicarboxylic anhydride.

10. A method for producing a composition for forming a release layer, comprising: producing a composition for forming a release layer comprising a polyamic acid and an organic solvent, A method for producing a composition, comprising producing a polyamic acid by the method for producing a polyamic acid according to any one of claims 1 to 9.

11. A method for producing a release layer, comprising the steps of: A method for producing a release layer, comprising the step of forming a release layer using a composition for forming a release layer produced by the method for producing a composition according to claim 10.

12. A method for producing a flexible electronic device having a resin substrate, comprising: A method for producing a flexible electronic device having a resin substrate, using a release layer produced by the method for producing a release layer according to claim 11.

13. A release layer-forming composition comprising a polyamic acid and an organic solvent, the polyamic acid is a reaction product of raw material components including a tetracarboxylic dianhydride, a diamine component, and at least one of a dicarboxylic anhydride and a monoamine component; Regarding the components of the polyamic acid 1 a molar ratio of the total of the dicarboxylic acid anhydride and the monoamine component to the total of the tetracarboxylic acid dianhydride and the diamine component is 3 mol % or more in a H-NMR analysis of the composition for forming a release layer.

14. The composition for forming a release layer according to claim 13 , wherein the molar ratio is 50 mol % or less.

15. the dicarboxylic acid anhydride comprises an aromatic dicarboxylic acid anhydride, The monoamine component includes a monoamine having a ring structure. The release layer forming composition according to claim 13 .

16. A release layer formed from the composition for forming a release layer according to any one of claims 13 to 15.

17. A method for producing a flexible electronic device having a resin substrate, using the release layer according to claim 16.

Citation Information

Patent Citations

  • Separation method

    JP1998125929A

  • Separation method

    JP1998125930A

  • Transfer of thin film element, thin film element, thin film integrated circuit device, active materix substrate and liquid crystal display device

    JP1998125931A

  • Active matrix displays and other electronic devices having plastic substrates

    WO2005050754A1

  • Detachable layer-forming composition and detachable layer

    WO2017204178A1