Threshold voltage tuning for gate-all-around FET architectures

JP2024503693A5Active Publication Date: 2024-11-26APPLIED MATERIALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023542923
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-01-25
Filing Date
2021-11-17
Publication Date
2024-11-26
Estimated Expiration
2041-11-17

AI Technical Summary

Technical Problem

Existing methods for tuning threshold voltage (Vt) in gate-all-around field effect transistors (GAA FETs) are incompatible with technology nodes below 10-15 nm, limiting the performance of semiconductor devices.

Method used

A method involving the formation of a dipole metal layer and work function adjustment layers on a high-k gate dielectric layer, combined with a metal gate electrode, to control the threshold voltage in GAA FETs.

Benefits of technology

Enables the manufacturing of smaller FET devices with improved performance by precisely tuning the threshold voltage, addressing the limitations of traditional methods in advanced technology nodes.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A method of forming a gate stack structure includes forming a dipole metal layer on a high-k gate dielectric layer on a semiconductor structure formed on a substrate, annealing the dipole metal layer, and removing the dipole metal layer, the dipole metal layer including a dopant in the high-k gate dielectric layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THE DISCLOSURE

[0001] Embodiments described herein relate generally to semiconductor device manufacturing, and more particularly to systems and methods for forming gate stacks in gate-all-around field effect transistors (FETs). [Background technology]

[0002]

[0002] To optimize metal-oxide-semiconductor field-effect transistors (MOSFETs) for power, timing, and area constraints, multiple threshold voltages V t (Multi V t ) technique is commonly adopted. t (Low V t ) modules switch quickly in response to input signals but consume more leakage power. High threshold voltage V t (High V t ) modules have slower switching speeds but consume less leakage power. A typical power-optimized design chooses a low V t Modules and High V t Modules are mixed.

[0003]

[0003] Threshold voltage V in MOSFET t is traditionally adjusted by inserting an interfacial dipole layer in a high-k / metal gate stack or by adding a work function tuning layer to the gate electrode. t The tuning method may be incompatible with architectures aimed at technology nodes below 10-15nm, such as gate-all-around FETs (GAA FETs), where the gate is placed on all four sides of the channel.

[0004]

[0004] Therefore, the adjusted threshold voltage V t What is needed is a system and method that can fabricate newer and smaller FET devices having Summary of the Invention

[0005]

[0005] Embodiments of the present disclosure provide a method of forming a gate stack structure, the method including forming a dipole metal layer on a high-k gate dielectric layer on a semiconductor structure formed on a substrate, annealing the dipole metal layer, and removing the dipole metal layer, the dipole metal layer including a dopant in the high-k gate dielectric layer.

[0006]

[0006] Some embodiments of the present disclosure also provide a method for forming a gate stack structure. The method includes forming a p-type work function adjustment layer on a high-k gate dielectric layer on a semiconductor structure formed on a substrate, forming an n-type work function adjustment layer on the high-k gate dielectric layer, and forming a metal gate electrode on the p-type work function adjustment layer and the n-type work function adjustment layer. The p-type work function adjustment layer includes a p-type doped conductive material, and the n-type work function adjustment layer includes an n-type doped conductive material.

[0007]

[0007] The embodiments of the present disclosure further provide a method for forming a gate stack structure on a semiconductor structure, the method includes forming an interface layer on the semiconductor structure, forming a high-k gate dielectric layer on the interface layer, forming a dipole metal layer on the high-k gate dielectric layer, the dipole metal layer including a dopant in the high-k gate dielectric layer, annealing the dipole metal layer, removing the dipole metal layer, forming a first high-k dielectric cap layer on the high-k gate dielectric layer, forming a p-type work function adjustment layer on the high-k gate dielectric layer, forming an n-type work function adjustment layer on the high-k gate dielectric layer, forming a second high-k dielectric cap layer on the p-type work function adjustment layer and the n-type work function adjustment layer, and forming a metal gate electrode on the second high-k dielectric cap layer. The p-type work function adjustment layer includes a p-type doped conductive material, and the n-type work function adjustment layer includes an n-type doped conductive material.

[0008]

[0008] In order to understand the features of the present disclosure in detail, a more particular description of the present disclosure briefly summarized above can be obtained by referring to the embodiments, some of which are illustrated in the accompanying drawings. However, it should be noted that the attached drawings illustrate only typical embodiments of the present disclosure, and the present disclosure may admit of other equally effective embodiments, and therefore the attached drawings should not be considered as limiting the scope of the present disclosure. [Brief description of the drawings]

[0009] [Figure 1] 1 is a top schematic view of an exemplary multi-chamber processing system according to one embodiment. [Figure 2A]

[0010] 2A and 2B depict a process flow diagram of a method for forming a semiconductor structure according to one embodiment. [Figure 2B] 2A and 2B depict a process flow diagram of a method for forming a semiconductor structure according to one embodiment. [Figure 3A]

[0011] FIG. 1 illustrates an isometric view of a semiconductor structure according to one embodiment. [Figure 3B] 3B, 3C, and 3D are cross-sectional views of a portion of a semiconductor structure according to one embodiment. [Figure 3C] 3B, 3C, and 3D are cross-sectional views of a portion of a semiconductor structure according to one embodiment. [Figure 3D] 3B, 3C, and 3D are cross-sectional views of a portion of a semiconductor structure according to one embodiment. [Figure 4A]

[0012] 4A, 4B, 4C, 4D, 4E, 4F, 4G, and 4H are cross-sectional views of a portion of a gate stack structure according to one embodiment. [Figure 4B] 4A, 4B, 4C, 4D, 4E, 4F, 4G, and 4H are cross-sectional views of a portion of a gate stack structure according to one embodiment. [Figure 4C]4A, 4B, 4C, 4D, 4E, 4F, 4G, and 4H are cross-sectional views of a portion of a gate stack structure according to one embodiment. [Figure 4D] 4A, 4B, 4C, 4D, 4E, 4F, 4G, and 4H are cross-sectional views of a portion of a gate stack structure according to one embodiment. [Figure 4E] 4A, 4B, 4C, 4D, 4E, 4F, 4G, and 4H are cross-sectional views of a portion of a gate stack structure according to one embodiment. [Figure 4F] 4A, 4B, 4C, 4D, 4E, 4F, 4G, and 4H are cross-sectional views of a portion of a gate stack structure according to one embodiment. [Figure 4G] 4A, 4B, 4C, 4D, 4E, 4F, 4G, and 4H are cross-sectional views of a portion of a gate stack structure according to one embodiment. [Figure 4H] 4A, 4B, 4C, 4D, 4E, 4F, 4G, and 4H are cross-sectional views of a portion of a gate stack structure according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010]

[0013] For ease of understanding, the same reference numbers have been used, where possible, to designate identical elements common to the figures. It is believed that elements and features of one embodiment may be beneficially incorporated in other embodiments without additional recitation.

[0011]

[0014] The embodiments described herein provide an adjusted threshold voltage V t The present invention provides a system and method for forming transistor devices for extremely small process nodes, such as gate-all-around (GAA) FETs having a conventional silicon dioxide (SiO 2 ) gate dielectric, high-k dielectric materials (e.g., hafnium oxide (HfO 2) is used as the gate dielectric, and instead of the conventional polycrystalline silicon (polysilicon) gate, a metal layer (e.g., titanium (Ti), tantalum (Ta), tungsten (W)) or a conductive compound layer (e.g., titanium nitride (TiN), tantalum nitride (TaN)) is used as the gate electrode. t is adjusted by inducing a dipole layer in the high-k gate dielectric, adding a work function tuning layer to the gate electrode and adjusting their thickness, or a combination thereof.

[0012]

[0015] 1 is a schematic top view of one embodiment of a multi-chamber processing system 100 according to some embodiments of the present disclosure. The processing system 100 generally includes a factory interface 102, load lock chambers 104, 106, transfer chambers 108, 110 with respective transfer robots 112, 114, holding chambers 116, 118, and processing chambers 120, 122, 124, 126, 128, 130. As detailed herein, wafers in the processing system 100 may be processed in and transferred between the various chambers without exposing the wafers to an ambient environment outside the processing system 100 (e.g., an ambient atmospheric environment that may exist in a foundry, etc.). For example, wafers may be processed in and transferred between the various chambers in a low pressure (e.g., about 300 Torr or less) or reduced pressure environment without breaking the low pressure or reduced pressure environment during various processes performed on the wafers in the processing system 100. Thus, the processing system 100 may provide an integrated solution for several processing of wafers.

[0013]

[0016] Examples of processing systems that may be suitably modified in accordance with the teachings provided herein include the Endura®, Producer®, or Centura® integrated processing systems available from Applied Materials, Inc., Santa Clara, Calif., or other suitable processing systems. It is contemplated that other processing systems, including those from other manufacturers, may be adapted to benefit from aspects described herein.

[0014]

[0017] 1, the factory interface 102 includes a docking station 140 and a factory interface robot 142 to facilitate transfer of wafers. The docking station 140 is configured to receive one or more front opening unified pods (FOUPs) 144. In some embodiments, each factory interface robot 142 generally comprises a blade 148 disposed at one end of the respective factory interface robot 142 configured to transfer wafers from the factory interface 102 to the load lock chambers 104, 106.

[0015]

[0018] The load lock chambers 104, 106 have respective ports 150, 152 coupled to the factory interface 102 and respective ports 154, 156 coupled to the transfer chamber 108. The transfer chamber 108 further has respective ports 158, 160 coupled to the holding chambers 116, 118 and respective ports 162, 164 coupled to the processing chambers 120, 122. Similarly, the transfer chamber 110 has respective ports 166, 168 coupled to the holding chambers 116, 118 and respective ports 170, 172, 174, 176 coupled to the processing chambers 124, 126, 128, 130. Ports 154, 156, 158, 160, 162, 164, 166, 168, 170, 172, 174, 176 may be, for example, slit valve openings having slit valves for transferring wafers therethrough by transfer robots 112, 114 and for providing a seal between the respective chambers to prevent gas passing between the respective chambers. Generally, any port is opened to transfer a wafer therethrough. Otherwise, the port is closed.

[0016]

[0019] The load lock chambers 104, 106, the transfer chambers 108, 110, the holding chambers 116, 118, and the processing chambers 120, 122, 124, 126, 128, 130 may be fluidly coupled to a gas and pressure control system (not specifically shown). The gas and pressure control system may include one or more gas pumps (e.g., turbo pumps, cryopumps, roughing pumps), gas sources, various valves, and conduits fluidly coupled to the various chambers. In operation, the factory interface robot 142 transfers a wafer from the FOUP 144 through the port 150 or 152 to the load lock chamber 104 or 106. The gas and pressure control system then pumps down the load lock chamber 104 or 106. The gas and pressure control system further maintains the transfer chambers 108, 110 and the holding chambers 116, 118 at an internal low or reduced pressure environment (which may include an inert gas). Thus, pumping down the load lock chambers 104 or 106 may facilitate passing wafers between the atmospheric environment of the factory interface 102 and the low or reduced pressure environment of the transfer chamber 108, for example.

[0017]

[0020] With the wafer in the pumped down load lock chamber 104 or 106, the transfer robot 112 transfers the wafer from the load lock chamber 104 or 106 through ports 154 or 156 into the transfer chamber 108. The transfer robot 112 can then transfer the wafer to and / or between either the processing chambers 120, 122 through respective ports 162, 164 for processing and the holding chambers 116, 118 through respective ports 158, 160 for holding awaiting further transfer. Similarly, the transfer robot 114 can access wafers in the holding chambers 116 or 118 through ports 166 or 168 and can transfer wafers to and / or between either of the processing chambers 124, 126, 128, 130 through respective ports 170, 172, 174, 176 for processing and the holding chambers 116, 118 through respective ports 166, 168 for holding awaiting further transfer. Transferring and holding wafers in and between the various chambers can be performed in a low or reduced pressure environment provided by a gas and pressure control system.

[0018]

[0021] The processing chambers 120, 122, 124, 126, 128, 130 may be any suitable chambers for processing wafers. In some embodiments, the processing chamber 122 may perform a cleaning process, the processing chamber 120 may perform an etching process, and the processing chambers 124, 126, 128, 130 may perform respective epitaxial growth processes. The processing chamber 122 may be a SiCoNi™ Preclean chamber available from Applied Materials, Inc. of Santa Clara, Calif. The processing chamber 120 may be a Selectra™ Etch chamber available from Applied Materials, Inc. of Santa Clara, Calif.

[0019]

[0022] A system controller 190 is coupled to the processing system 100 for controlling the processing system 100 or components thereof. For example, the system controller 190 may control the operation of the processing system 100 using direct control of the chambers 104, 106, 108, 116, 118, 110, 120, 122, 124, 126, 128, 130 of the processing system 100 or by controlling controllers associated with the chambers 104, 106, 108, 116, 118, 110, 120, 122, 124, 126, 128, 130. In operation, the system controller 190 enables data collection and feedback from each chamber to regulate the performance of the processing system 100.

[0020]

[0023] The system controller 190 generally includes a central processing unit (CPU) 192, a memory 194, and support circuits 196. The CPU 192 may be one of any form of general-purpose processor that can be used in an industrial setting. The memory 194 or non-transitory computer-readable medium is accessible by the CPU 192 and may be one or more memories, such as a local or remote random access memory (RAM), a read-only memory (ROM), a floppy disk, a hard disk, or any other form of digital storage. The support circuits 196 are coupled to the CPU 192 and may include cache, clock circuits, input / output subsystems, power supplies, and the like. The various methods disclosed herein may generally be performed under the control of the CPU 192 by the CPU 192 executing computer instruction instruction codes stored in the memory 194 (or in the memory of a particular process chamber), for example, as software routines. When the computer instruction instruction codes are executed by the CPU 192, the CPU 192 controls the chamber to perform processes according to various methods.

[0021]

[0024] Other processing systems may have other configurations. For example, more or fewer processing chambers may be coupled to the transfer apparatus. In one illustrated embodiment, the transfer apparatus includes transfer chambers 108, 110 and holding chambers 116, 118. In other embodiments, more or fewer transfer chambers (e.g., one transfer chamber) and / or more or fewer holding chambers (e.g., no holding chambers) may be implemented as a transfer apparatus in a processing system.

[0022]

[0025] 2A and 2B depict a process flow diagram of a method 200 of forming a gate stack structure in a semiconductor structure 300 according to one or more embodiments of the present disclosure. FIG. 3A is an isometric view of the semiconductor structure 300. FIGS. 3B and 3C are cross-sectional views of a portion of the semiconductor structure 300 taken along lines B-B' and C-C', respectively, of FIG. 3A. FIG. 3D is an enlarged cross-sectional view of a portion of the semiconductor structure 300 taken along line D-D' of FIG. 3B. FIGS. 4A, 4B, 4C, 4D, 4E, 4F, 4G, and 4H are cross-sectional views of a portion of a gate stack structure formed in the semiconductor structure 300 corresponding to various stages of the method 200. It should be understood that FIGS. 3A, 3B, and 3C show only a partial schematic view of the semiconductor structure 300, and the semiconductor structure 300 may include any number of transistor sections and additional materials having multiple aspects as shown in the figures. It should also be noted that although the method steps shown in FIGS. 2A and 2B are described sequentially, other process sequences that include one or more method steps omitted and / or added and / or rearranged in another desired order are within the scope of the embodiments of the present disclosure provided herein.

[0023]

[0026] 3A, the semiconductor structure 300 may include a substrate 302 having a first region R1 and a second region R2. In R1, a first gate-all-around field effect transistor (GAA FET) module TR1 is formed, and in R2, a second GAA FET module TR2 is formed. The GAA FET module TR1 and the GAA FET module TR2 are electrically isolated from each other and from other GAA FET modules in the semiconductor structure 300, not shown in FIG. 3A, by an inter-module insulating layer 304.

[0024]

[0027] The term "substrate" as used herein refers to a layer of material that serves as a base for subsequent processing operations and includes a surface to be cleaned. The substrate 302 may be a silicon-based material or any suitable insulating or conductive material, as appropriate. The substrate 302 may be crystalline silicon (e.g., Si <100> or Si <111> ), silicon oxide, strained silicon, silicon germanium, doped or undoped polysilicon, doped or undoped silicon wafers and patterned or unpatterned wafers, silicon-on-insulator (SOI), carbon doped silicon oxide, silicon nitride, doped silicon, germanium, gallium arsenide, glass, or sapphire. The insulating layer 304 between the modules may be formed of a silicon-containing dielectric material, such as silicon oxide, silicon nitride, or silicon oxynitride.

[0025]

[0028] In one embodiment, the first region R1 is a high-voltage region and the second region R2 is a low-voltage region. In another embodiment, the first region R1 is a p-type MOSFET region and the second region R2 is an n-type MOSFET region. Each of the GAA FET modules TR1 and TR2 may include a channel region CH and a source / drain region SD separated in the X-direction by the channel region CH. The source / drain region SD may be wider in the Y-direction than the channel region CH.

[0026]

[0029] 3A, 3B, and 3C, the source / drain region SD may include a first semiconductor layer 306 and a second semiconductor layer 308 stacked alternately and repeatedly on the substrate 302. The first semiconductor layer 306 is formed of a first material having an etch selectivity with respect to a second material from which the second semiconductor layer 308 is formed (i.e., the etch rate of the first material is higher than the etch rate of the second material). The etch selectivity (i.e., the etch rate of the first material relative to the etch rate of the second material) is between about 10:1 and 200:1. Exemplary combinations of the first and second materials include silicon germanium (SiGe) / silicon (Si), silicon germanium (SiGe) / germanium (Ge), and germanium tin (GeSn) / silicon (Si). The portions of the first semiconductor layer 306 of the source / drain region SD may be separated in the X-direction by a gate electrode GE. Each of the GEs is surrounded by a gate stack 310 formed in a channel region CH. The second semiconductor layer 308 in the channel region CH may act as a nanowire or nanotube having a width between a few nanometers and a few hundred nanometers.

[0027]

[0030] The first and second semiconductor layers 306 and 308 may be formed using any suitable deposition technique, such as chemical vapor deposition (CVD), atomic layer deposition (ALD), or physical vapor deposition (PVD), and patterning techniques, such as lithography and etching processes.

[0028]

[0031] The first and second semiconductor layers 306 and 308 may each have a thickness of about 6 nm to about 14 nm, for example about 10 nm.

[0029]

[0032] 3D , the gate stack 310 includes an interfacial layer 312, a high-k gate dielectric layer 314, a first high-k dielectric capping layer 316, a p-type work function tuning layer 318, an n-type work function tuning layer 320, and a second high-k dielectric capping layer 322, sequentially formed on the second semiconductor layer 308. A gate electrode GE is formed on the second high-k dielectric capping layer 322.

[0030]

[0033] The method 200 begins with an interface formation process at block 205 to form an interface layer 312 on the second semiconductor layer 308, as shown in FIG. 2 The interfacial layer 312 formed in block 205 may include a suitable thermal oxidation process, such as an enhanced in situ steam generation (eISSG) process utilizing O gas. The interfacial layer 312 formed in block 205 may be a thin amorphous silicon oxide (SiO ) layer having a thickness between about 3 Å and about 10 Å (e.g., about 5 Å), corresponding to one or more monolayers of silicon oxide. 2 In some embodiments, the interface layer 312 is a H 2 and O 2 In-situ steam generation (ISSG) process using gas, or NH 3 and O 2 The interface layer 312 may be formed by a gas-assisted rapid thermal oxidation (RTO) process. The interface layer 312 may act as a nucleation layer for the high-k gate dielectric layer 314 deposited thereon, improving the quality of the interface (e.g., interface state density, storage capacitance, frequency dispersion, leakage current, etc.) between the second semiconductor layer 308 and the high-k gate dielectric layer 314. The interface formation process may be performed in a processing chamber, such as the processing chambers 120, 122, 124, 126, 128, or 130 shown in FIG. 1.

[0031]

[0034] In some embodiments, the interface formation process in block 205 is omitted, and the interface layer 312 is not formed before the deposition of the high-k gate dielectric layer 314 on the second semiconductor layer 308. In that case, the interface layer 312 is formed by a subsequent thermal oxidation process that thermally oxidizes the second semiconductor layer 308 through the high-k gate dielectric layer 314 deposited on the second semiconductor layer 308. The interface layer 312 formed by the subsequent thermal oxidation process may be thick enough to ensure reliable device characteristics (e.g., interface state density, storage capacitance, frequency dispersion, and leakage current, etc.) and reduce atomic diffusion from the high-k gate dielectric layer 314 to the second semiconductor layer 308, and has a thickness between about 0.3 nm and about 1 nm, for example 0.5 nm.

[0032]

[0035] In block 210, a deposition process is performed to deposit a high-k gate dielectric layer 314 on the interfacial layer 312, as shown in FIG. 4B. The high-k gate dielectric layer 314 is made of hafnium dioxide (HfO 2 ), zirconium dioxide (ZrO 2 ), ytterbium oxide (Y 2 O 3 ), aluminum oxide (Al 2 O 3 ), high-k dielectric materials such as HfZrO, HfLaO xThe high-k dielectric film may be formed of a ternary high-k dielectric film having a third element doped into an existing metal oxide high-k dielectric host material such as HfTiO. The deposition process may include an atomic layer deposition (ALD) process. In the ALD process, a metal-containing precursor and an oxygen-containing precursor are alternately delivered to the interfacial layer 312. In some embodiments, the metal-containing precursor is purged before delivering the oxygen-containing precursor. The metal may be a transition metal such as hafnium (Hf), zirconium (Zr), or titanium (Ti), a rare earth metal such as lanthanum (La), ytterbium (Yb), or yttrium (Y), an alkaline earth metal such as strontium (Sr), or another metal such as aluminum (Al). For the oxidizer, any oxygen-containing precursor that may react with the metal may be used. For example, the oxygen-containing precursor may be or may include water, diatomic oxygen, ozone, a hydroxyl-containing precursor or alcohol, a nitrogen- and oxygen-containing precursor, plasma-enhanced oxygen, including locally or remotely enhanced oxygen, or any other material containing oxygen that may be incorporated into a metal to produce a layer of oxide of the metal on the interfacial layer 312. In one embodiment, the metal-containing precursor is hafnium tetrachloride (HfCl 4 ) and the oxidant is water (H 2 O) and hafnium dioxide (HfO 2 ) layer. The ALD process may be performed at a temperature between 200° C. and about 400° C., for example about 270° C. The high-k gate dielectric layer 314 deposited by the ALD process may be amorphous and may have a thickness between about 10 Å and about 30 Å. The deposition process may be performed in a processing chamber, such as processing chambers 120, 122, 124, 126, 128, or 130 shown in FIG. 1.

[0033]

[0036] In block 215, an optional post-deposition anneal process is performed to harden and densify the as-deposited high-k gate dielectric layer 314. Crystallization of the as-deposited amorphous high-k gate dielectric layer 314 may occur. The post-deposition anneal process is performed in a rapid thermal processing (RTP) chamber, such as a RADOX™ chamber available from Applied Materials, Inc., located in Santa Clara, Calif., using nitrogen (N 2 1. The post-deposition anneal process may include a thermal anneal process in an inert atmosphere, such as a SiO 2 (SiO 2 ) and Argon (Ar) atmosphere. The RTP chamber may be any of the processing chambers 120, 122, 124, 126, 128, and 130 shown in FIG. 1. The post-deposition anneal process may thermally harden and densify the interfacial layer 312 and the high-k dielectric layer 314.

[0034]

[0037] The post-deposition anneal process may be performed for between about 1 second and about 60 seconds, at a temperature between about 500° C. and about 800° C., and at a pressure between about 0.01 Torr and 100 Torr.

[0035]

[0038] In block 220, a plasma nitridation process is performed to insert nitrogen atoms into vacancies and defects in the high-k gate dielectric layer 314. The plasma nitridation process may be a decoupled plasma nitridation (DPN) process performed in a DPN chamber, such as a CENTURA® DPN chamber available from Applied Materials, Inc., Santa Clara, Calif. The DPN chamber may be any of the processing chambers 120, 122, 124, 126, 128, and 130 shown in FIG. 1. The plasma nitridation process exposes the high-k gate dielectric layer 314 to a nitrogen plasma. This may allow nitrogen radicals or nitrogen atoms to be incorporated into the high-k gate dielectric layer 314 throughout the thickness of the high-k gate dielectric layer 314. During the plasma nitridation process, the nitrogen atoms may form metastable bonds with oxygen (O). Gases that may be used in the plasma process include nitrogen (N 2 ), ammonia (NH 3), or mixtures thereof. In one embodiment, the nitrogen gas is about 3% to about 8% nitrogen (N 2 ) and ammonia (NH 3 ) The plasma nitridation process may not change the thickness of the high-k gate dielectric layer 314 as a result of nitrogen being incorporated into vacancies and defects in the as-deposited high-k gate dielectric layer 314.

[0036]

[0039] The nitridation process may be carried out at a temperature between about 0° C. and about 500° C. for between about 10 seconds and about 300 seconds.

[0037]

[0040] In block 225, an optional thermal nitridation process is performed to further insert nitrogen atoms into vacancies and defects in the plasma nitrided high-k gate dielectric layer 314. The thermal nitridation process is performed in a rapid thermal processing (RTP) chamber, such as a RADOX™ chamber available from Applied Materials, Inc., located in Santa Clara, Calif., using an ammonia (NH 3 The RTP chamber may include a thermal annealing process in a SiO 2 (SiO 2 ) atmosphere. The RTP chamber may be any of the processing chambers 120, 122, 124, 126, 128, and 130 shown in FIG.

[0038]

[0041] The thermal nitridation process may be carried out for between about 10 seconds and about 300 seconds, at a temperature between about 700° C. and about 900° C., and at a pressure between about 10 Torr and 740 Torr.

[0039]

[0042] At block 230, a post-nitridation anneal process is performed to passivate remaining chemical bonds in the plasma nitrided high-k gate dielectric layer 314. The post-nitridation anneal process is performed in a rapid thermal processing (RTP) chamber, such as a RADOX™ chamber available from Applied Materials, Inc., located in Santa Clara, Calif., using nitrogen (N 2) and argon (Ar) ambient. The RTP chamber may be any of the processing chambers 120, 122, 124, 126, 128, and 130 shown in FIG. 1. The post-nitridation anneal process may passivate metastable nitrogen bonds formed in the plasma nitridation process in block 220 and may result in crystallization of the amorphous high-k gate dielectric layer 314.

[0040]

[0043] The spike thermal anneal process may be performed for between about 1 second and about 30 seconds, at a temperature between about 700° C. and about 850° C., and at a pressure between about 10 Torr and 740 Torr.

[0041]

[0044] 4C, a dipole formation process is performed to form a dipole metal layer 402 on the high-k gate dielectric layer 314. The dipole formation process in block 235 includes blanket deposition of the dipole metal layer 402 over the entire exposed surface of the high-k gate dielectric layer 314 in the semiconductor structure 300, and subsequent lithography and etching processes to pattern the dipole metal layer 402 (i.e., to form the dipole metal layer 402 in some areas of the semiconductor structure 300 and not form the dipole metal layer 402 in other areas of the semiconductor structure 300).

[0042]

[0045] In some embodiments, the dipole metal layer 402 is made of hafnium dioxide (HfO 2 The semiconductor device is formed of a material containing an n-type dopant in a high-k dielectric material such as lanthanum oxide (La). Suitable n-type dopants include rare earth metals such as lanthanum (La), yttrium (Y), and ytterbium (Yb), or any metallic substance having a higher Fermi level than hafnium (Hf), such as magnesium (Mg). Suitable lanthanum (La)-containing materials include lanthanum oxide (La). 2 O 3), lanthanum nitride (LaN), lanthanum (La), and titanium lanthanum nitride (TiLaN). In a subsequent annealing process, the n-type dopant species from the dipole metal layer 402 diffuses and becomes incorporated into the underlying high-k gate dielectric layer 314. This reduces the threshold voltage V t The amount of n-type dopant species reduces the threshold voltage V t For example, the incorporation of lanthanum (La) species between about 1 atomic % and about 5 atomic % into the high-k gate dielectric layer 314 determines a change in the threshold voltage V t is changed by about 10 eV.

[0043]

[0046] In some embodiments, the dipole metal layer 402 is made of hafnium dioxide (HfO 2 The semiconductor device is formed of a material containing a p-type dopant in a high-k dielectric material such as aluminum (Al), niobium (Nb), tantalum (Ta), or any metallic material having a Fermi level lower than that of hafnium (Hf). Suitable aluminum (Al)-containing materials include aluminum oxide (Al 2 O 3 Suitable niobium (Nb)-containing materials include niobium nitride (NbN), niobium oxide (NbO x ), and titanium niobium nitride (TiNbN). In a subsequent annealing process, the p-type dopant species diffuse and become incorporated into the underlying high-k gate dielectric layer 314. This reduces the threshold voltage V t The amount of p-type dopant species reduces the threshold voltage V t For example, the incorporation of aluminum (Al) species between about 1 atomic % and about 5 atomic % into the high-k gate dielectric layer 314 determines a change in the threshold voltage V t For example, the incorporation of between about 1 atomic % and about 5 atomic % niobium (Nb) species into the high-k gate dielectric layer 314 changes the threshold voltage V t is changed by about 120 eV.

[0044]

[0047] The blanket deposition process may include an atomic layer deposition (ALD) process. The ALD process may be performed at a temperature between 200° C. and about 400° C., such as about 300° C. The dipole metal layer 402 deposited by the ALD process may have a thickness between about 3 Å and about 20 Å, such as about 10 Å. The deposition process may be performed in a processing chamber, such as processing chambers 120, 122, 124, 126, 128, or 130 shown in FIG. 1.

[0045]

[0048] In block 240, an annealing process is performed to diffuse the dopant species (lanthanum (La), aluminum (Al), or niobium (Nb)) into the underlying high-k gate dielectric layer 314. The annealing process in block 240 is performed in a rapid thermal processing (RTP) chamber, such as a RADOX™ chamber available from Applied Materials, Inc., located in Santa Clara, Calif., using nitrogen (N 2 ) and a thermal annealing process in an inert atmosphere, such as an argon (Ar) atmosphere. The RTP chamber may be any of the processing chambers 120, 122, 124, 126, 128, and 130 shown in FIG.

[0046]

[0049] The annealing process in block 240 may be performed for between about 1 second and about 30 seconds, at a temperature between about 600° C. and about 1000° C., for example about 900° C., and at a pressure between about 0.1 Torr and 100 Torr.

[0047]

[0050] At block 245, a removal process is performed to strip the dipole metal layer 402. The removal process may include a dry plasma etching process.

[0048]

[0051] In block 250, a deposition process is performed to deposit a first high-k dielectric cap layer 316 on the gate dielectric layer 314 of the semiconductor structure 300, as shown in FIG. 4D. The first high-k dielectric cap layer 316 may be formed of a metal nitride material including titanium (Ti) or tantalum (Ta), such as TiN or TaN. The first high-k dielectric cap layer 316 is used as a protective layer for the high-k gate dielectric layer 314 during subsequent patterning and etching processes. The deposition process in block 250 may include an atomic layer deposition (ALD) process. In ALD, a metal-containing precursor including titanium (Ti) or tantalum (Ta), a nitrogen-containing precursor, and a dopant-containing precursor are delivered to the surface of the gate dielectric layer 314. Examples of metal-containing precursors include titanium (Ti) or tantalum (Ta), and an example of a nitrogen-containing precursor is ammonia (NH 3 ), Diazene (N 2 H 2 ), and hydrazine (N 2 H 4 ).

[0049]

[0052] The ALD process in block 250 may be performed at a temperature between about 200° C. and about 700° C., such as between about 300° C. and about 600° C. The first high-k dielectric cap layer 316 deposited by the ALD process in block 250 may be amorphous and may have a thickness between about 2 Å and about 200 Å, such as between 10 Å and about 15 Å. The deposition process may be performed in a processing chamber, such as processing chambers 120, 122, 124, 126, 128, or 130 shown in FIG.

[0050]

[0053] In block 255, an optional metal cap anneal process is performed to harden and densify the as-deposited first high-k dielectric cap layer 316. Crystallization of the as-deposited first high-k dielectric cap layer 316 may occur. The optional metal cap anneal process in block 255 may be performed in a rapid thermal processing (RTP) chamber, such as a RADOX™ chamber available from Applied Materials, Inc., located in Santa Clara, Calif., using nitrogen (N 2 ) and a thermal annealing process in an inert atmosphere, such as an argon (Ar) atmosphere. The RTP chamber may be any of the processing chambers 120, 122, 124, 126, 128, and 130 shown in FIG.

[0051]

[0054] The optional metal cap anneal process in block 255 may be performed for between about 1 second and about 10 seconds, at a temperature between about 700° C. and about 850° C., and at a pressure between about 0.1 Torr and 100 Torr.

[0052]

[0055] In block 260, a deposition process is performed to deposit a sacrificial silicon cap layer 404 on the first high-k dielectric cap layer 316, as shown in FIG. 4E. The sacrificial silicon cap layer 404 may physically and chemically protect the underlying high-k gate dielectric layer 314 and the first high-k dielectric cap layer 316 during a subsequent annealing process in block 265. The sacrificial silicon cap layer 404 is formed of amorphous silicon, such as hydrogenated amorphous silicon (a-Si:H). Amorphous silicon may have less atomic diffusion compared to polycrystalline silicon, where grain boundaries provide a pathway for diffusion. The deposition process in block 260 may be an atomic layer deposition (ALD) process or a chemical vapor deposition (CVD) process. In that case, the semiconductor structure 300 having the first high-k dielectric cap layer 316 formed thereon is exposed to a silicon precursor. An example of a silicon precursor is polysilane (Si x H yFor example, polysilanes include disilane (Si 2 H 6 ), trisilane (Si 3 H 8 ), tetrasilane (Si 4 H 10 ), isotetrasilane, neopentasilane (Si 5 H 12 ), cyclopentasilane (Si 5 H 10 ), hexasilane (C 6 H 14 ), cyclohexasilane (Si 6 H 12 ), or generally, Si x H y where x=2 or more x H y , and combinations thereof.

[0053]

[0056] The sacrificial silicon cap layer 404 may have a thickness between about 30 Å and about 50 Å. The deposition process in block 260 may be performed in a processing chamber, such as processing chambers 120, 122, 124, 126, 128, or 130 shown in FIG.

[0054]

[0057] In block 265, a post cap anneal (PCA) process is performed to harden and densify the first high-k dielectric cap layer 316. Crystallization of the as-deposited first high-k dielectric cap layer 316 and the as-deposited sacrificial silicon cap layer 404 may occur. The PCA process in block 265 may be performed in a rapid thermal processing (RTP) chamber, such as a RADOX™ chamber available from Applied Materials, Inc., located in Santa Clara, Calif., using nitrogen (N 2 ) and a thermal annealing process in an inert atmosphere, such as an argon (Ar) atmosphere. The RTP chamber may be any of the processing chambers 120, 122, 124, 126, 128, and 130 shown in FIG.

[0055]

[0058] The PCA process in block 265 may be carried out for between about 1 second and about 10 seconds, at a temperature between about 900° C. and about 1000° C., for example about 900° C., and at a pressure between about 0.1 Torr and 100 Torr.

[0056]

[0059] At block 270, a removal process is performed to strip the sacrificial silicon cap layer 404. The removal process may include a dry plasma etch process.

[0057]

[0060] In block 275, a deposition process is performed to deposit a p-type work function tuning layer 318 on the hardened and densified first high-k dielectric cap layer 316, as shown in Figure 4F. The p-type work function tuning layer 318, in conjunction with the high-k gate dielectric layer 314, acts as an effective gate electrode in the p-type MOSFET region.

[0058]

[0061] The p-type work function adjustment layer 318 is made of a p-type doped conductive material, such as titanium nitride (TiN), titanium silicon nitride (TiSiN), tantalum silicon nitride (TaSiN), molybdenum nitride (MoN), tungsten nitride (W 3 N 2 ), niobium nitride (NbN), molybdenum niobium nitride (MoNbN), and titanium niobium nitride (TiNbN). In some embodiments, the p-type work function adjusting layer 318 may have a doping amount between about 1 atomic % and about 20 atomic %, for example about 10 atomic %. The thickness of the p-type work function adjusting layer 318 is determined by the threshold voltage V t For example, the change in the thickness of the p-type work function adjustment layer 318 determines the change in the threshold voltage V t by about 80 eV. The total thickness of the p-type work function adjusting layer 318 may be between about 5 Å and about 30 Å, for example about 10 Å.

[0059]

[0062] The deposition process may include an atomic layer deposition (ALD) process. In an ALD process, a metal-containing precursor and ammonia (NH 3) are alternately delivered to the exposed layer of the semiconductor structure 300. In some embodiments, the metal-containing precursor is purged before delivering the nitrogen-containing precursor. This sequence is repeated until the desired thickness is reached. The metal may be titanium (Ti), molybdenum (Mo), niobium (Nb), tantalum (Ta), or tungsten (W). The ALD process may be performed at a temperature of about 200° C. to about 400° C., for example about 300° C. The deposition process may be performed in a process chamber, such as process chambers 120, 122, 124, 126, 128, or 130 shown in FIG. 1.

[0060]

[0063] In block 280, a deposition process is performed to deposit an n-type work function adjusting layer 320 on the p-type work function adjusting layer 318, as shown in Figure 4G. The n-type work function adjusting layer 320, in conjunction with the high-k gate dielectric layer 314, acts as an effective gate electrode in the n-type MOSFET region.

[0061]

[0064] The n-type work function adjustment layer 320 is made of titanium aluminum carbide (Ti 3 AlC 2 ), zinc nitride (Zn 3 N 2 ), vanadium nitride (VN), magnesium nitride (Mg 3 N 2 ), yttrium nitride (YN), strontium nitride (Sr 3 N 2 ), or any metallic species that has an average work function higher than that of silicon. In some embodiments, the n-type work function tuning layer 320 may have a doping amount between about 1 atomic % and about 20 atomic %, for example about 10 atomic %. The thickness of the n-type work function tuning layer 320 is determined by the threshold voltage V t For example, the change in the thickness of the n-type work function adjustment layer 320 determines the change in the threshold voltage V t by about 80 eV. The total thickness of the n-type work function adjusting layer 320 may be between about 5 Å and about 30 Å, for example about 10 Å.

[0062]

[0065] The deposition process may include an atomic layer deposition (ALD) process. In an ALD process, a metal-containing precursor and ammonia (NH 3 ) are alternately delivered to the exposed layer of the semiconductor structure 300. In some embodiments, the metal-containing precursor is purged before delivering the nitrogen-containing precursor. The metal may be titanium (Ti), aluminum (Al), zinc (Zn), vanadium (V), magnesium (Mg), yttrium (Y), or strontium (Sr). The ALD process may be performed at a temperature of about 200° C. to about 400° C., for example, about 300° C. The deposition process may be performed in a process chamber, such as process chambers 120, 122, 124, 126, 128, or 130 shown in FIG. 1.

[0063]

[0066] 4H, a formation process is performed to form a second high-k dielectric cap layer 322 on the n-type work function tuning layer 320. The formation process in block 285 is substantially the same as the deposition process in block 250, the metal cap anneal process in block 255, the deposition process in block 260, the post cap anneal (PCA) process in block 265, and the removal process in 270.

[0064]

[0067] In block 290, a deposition process is performed to deposit a gate electrode GE on the second high-k dielectric cap layer 322, as shown in FIG. 3D. The gate electrode GE may be formed of a metal, such as tungsten (W) or cobalt (Co). The gate electrode GE may be p-type doped or n-type doped. The deposition process in block 290 may be performed using WF 6 The process may include a chemical vapor deposition (CVD) process using a tungsten-containing precursor such as SiO 2 or a cobalt-containing precursor such as SiO 2 .

[0065]

[0068] The embodiments described herein provide an adjusted threshold voltage V tThe present invention provides a system and method for forming a gate stack structure in a gate-all-around (GAA) FET having a high-k dielectric material (e.g., hafnium oxide (HfO 2 )) and a gate electrode formed of a metal layer (e.g., titanium (Ti), tantalum (Ta), tungsten (W)) or a conductive compound layer (e.g., titanium nitride (TiN), tantalum nitride (TaN)). t is controllably adjusted by inducing a dipole layer in the high-k gate dielectric, by adding a work function tuning layer to the gate electrode and adjusting their thickness, or a combination thereof.

[0066]

[0069] The gate stack structures described herein may be advantageously used in any metal gate application and / or any barrier application in MOSFETs, dynamic random access memories (DRAMs), and flash memories.

[0067]

[0070] While the forgoing is directed to several embodiments of the present disclosure, other and further embodiments of the present disclosure may be devised without departing from the basic scope of the disclosure, the scope of the present disclosure being defined by the following claims.

Claims

1. A method for forming a gate stack structure, Forming a dipole metal layer on a high dielectric constant gate dielectric layer on a semiconductor structure formed on a substrate, Annealing the aforementioned dipole metal layer, and This includes removing the aforementioned dipole metal layer, The method wherein the dipole metal layer includes a dopant in the high dielectric constant gate dielectric layer.

2. Forming the aforementioned dipole metal layer is The process involves blanket-depositing the dipole metal layer onto the semiconductor structure, and The method according to claim 1, comprising patterning the dipole metal layer.

3. The aforementioned high dielectric constant gate dielectric layer is made of hafnium oxide (HfO 2 The method according to claim 1, including )

4. The method according to claim 3, wherein the dipole metal layer includes lanthanum (La).

5. The method according to claim 3, wherein the dipole metal layer comprises aluminum (Al).

6. The method according to claim 3, wherein the dipole metal layer comprises niobium (Nb).

7. The method according to claim 1, wherein the dipole metal layer has a thickness between 3 Å and 20 Å.

8. A method for forming a gate stack structure, Forming a p-type work function adjustment layer on a high-dielectric-constant gate dielectric layer on a semiconductor structure formed on a substrate, Forming an n-type work function adjustment layer on the aforementioned p-type work function adjustment layer, Forming a high dielectric constant gate dielectric cap layer on the n-type work function adjustment layer, and This includes forming a metal gate electrode on the high dielectric constant gate dielectric cap layer, The p-type work function adjustment layer includes a p-type doped conductive material. The method wherein the n-type work function adjustment layer comprises an n-type doped conductive material.

9. The method according to claim 8, wherein the metal gate electrode comprises tungsten (W).

10. The method according to claim 8, wherein the p-type work function adjusting layer comprises a p-type doped conductive material and has a thickness between 5 Å and 30 Å.

11. The method according to claim 8, wherein the n-type work function adjusting layer comprises an n-type doped conductive material and has a thickness between 5 Å and 30 Å.

12. A method for forming a gate stack structure on a semiconductor structure, Forming an interface layer on a semiconductor structure, Forming a high dielectric constant gate dielectric layer on the interface layer, A dipole metal layer containing a dopant within the high dielectric constant gate dielectric layer is formed on the high dielectric constant gate dielectric layer. Annealing the aforementioned dipole metal layer, Removing the aforementioned dipole metal layer, A first high dielectric constant dielectric cap layer is formed on the high dielectric constant gate dielectric layer. Forming a p-type work function adjustment layer on the high dielectric constant gate dielectric layer, Forming an n-type work function adjustment layer on the high dielectric constant gate dielectric layer, Forming a second high dielectric constant dielectric cap layer on the p-type work function adjustment layer and the n-type work function adjustment layer, and This includes forming a metal gate electrode on the second high dielectric constant dielectric cap layer, The p-type work function adjustment layer includes a p-type doped conductive material. The method wherein the n-type work function adjustment layer comprises an n-type doped conductive material.

13. Forming the aforementioned dipole metal layer is The process involves blanket-depositing the dipole metal layer onto the high dielectric constant gate dielectric layer, and The method according to claim 12, comprising patterning the dipole metal layer.

14. The aforementioned high dielectric constant gate dielectric layer is made of hafnium oxide (HfO 2 The method according to claim 12, including )

15. The method according to claim 14, wherein the dipole metal layer includes lanthanum (La).

16. The method according to claim 14, wherein the dipole metal layer comprises aluminum (Al) or niobium (Nb).

17. The method according to claim 12, wherein the metal gate electrode comprises tungsten (W).

18. The method according to claim 17, wherein the p-type work function adjusting layer comprises a p-type doped conductive material and has a thickness between 5 Å and 30 Å.

19. The method according to claim 17, wherein the n-type work function adjusting layer comprises an n-type doped conductive material and has a thickness between 5 Å and 30 Å.

20. The method according to claim 12, wherein the first high dielectric constant dielectric cap layer and the second high dielectric constant dielectric cap layer each contain titanium nitride (TiN).