Novel green lithium iron phosphate precursor, its preparation method and use

JP2024535003A5Active Publication Date: 2024-11-13SHANGHAI LIANGFU NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024515845
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-10
Filing Date
2022-09-09
Publication Date
2024-11-13
Estimated Expiration
2042-09-09

AI Technical Summary

Technical Problem

Conventional methods for producing lithium iron phosphate using iron phosphate or iron powder as raw materials face challenges such as low solid content concentration, high process costs, and difficulty in controlling reaction conditions, leading to increased energy consumption and viscosity issues.

Method used

A novel method involving the complete reaction of an iron source with phosphoric acid to form product A, followed by reaction with an organic acid, lithium source, and carbon source to form product B, which are then mixed and ground to achieve a lithium iron phosphate precursor with a solid content of over 50%, reducing energy consumption and viscosity.

Benefits of technology

The method results in a lithium iron phosphate precursor with high solid content and small particle size, enabling low-cost production with reduced energy consumption and improved charge/discharge rates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention discloses a novel green lithium iron phosphate precursor, and its preparation method and use. The preparation method of the lithium iron phosphate precursor includes the steps of: S1. reacting a mixture of an iron source and a phosphoric acid solution, and pulverizing the mixture to obtain product A after the reaction is completed; reacting a mixture of an organic acid solution, a lithium source, and a carbon source, and obtaining product B after the reaction is completed, and the preparation order of the product A and the product B is not limited; S2. pulverizing the mixture of the product A and the product B to obtain the lithium iron phosphate precursor. In the preparation process of the lithium iron phosphate precursor of the present invention, the solid content can be greatly improved, the energy consumption of the subsequent steps is low, the preparation method is simple, the cost is low, the particle size of the prepared lithium iron phosphate precursor is very small, and the charge and discharge c rate is fast.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority to Chinese patent application No. 2021110643549, filed on September 10, 2021. This application incorporates the above-mentioned Chinese patent application in its entirety.

[0002] The present invention provides a novel green lithium iron phosphate precursor, and methods for its preparation and use. [Background technology]

[0003] In recent decades, lithium-ion battery materials have been actively developed around the world for use in transportation such as electric cars and electric bicycles. In the development of motorized vehicles, research into power batteries used as on-board power sources has been a major bottleneck. Considering cost-effectiveness, lithium-ion batteries have great advantages. Lithium ferrous phosphate (LiFePO 4 ), also known as lithium iron phosphate, is a popular choice due to its cyclicality, price, safety, specific energy and other influencing factors. 4 The material has many advantages, including stable structure, abundant raw material sources, environmental friendliness, low cost, theoretical capacity of 170 mAh / g, and a stable discharge plateau at 3.5 V. In particular, its safety performance and cycle life are unmatched by other materials, making it the most attractive positive electrode material today.

[0004] Current LifePO 4 The synthesis method mainly focuses on the synthesis process using iron phosphate as a raw material. The synthesis method using iron phosphate as a raw material generally involves reacting iron phosphate with a lithium source and a carbon source, so the solid content of the obtained product is low (usually 35-40%) and there is a problem that the cost of the subsequent process is high.

[0005] In addition, LiFePO 4 can also be synthesized by reacting iron powder as a raw material with iron powder 6 powder, phosphoric acid, a lithium source, and a carbon source.

[0006] For example, WO2004036671A1 discloses using metallic iron to react with phosphoric acid in an aqueous solution, adding lithium carbonate or lithium hydroxide to prepare a lithium iron phosphate precursor, drying it, and after the first calcination, adding a carbon source and carrying out a second calcination to obtain the finished lithium iron phosphate product. However, in the reaction process between metallic iron powder and phosphoric acid, the main product is ferrous phosphate (Fe 2 O 3 ), an insoluble divalent iron compound. 3 (PO 4 ) 2 8H 2 O) is produced, which causes the solution to become a white paste-like, highly viscous substance, which is unfavorable for sufficient reaction of the metallic iron powder and subsequent mixing with the lithium source, and makes it impossible to improve the solids concentration of the synthesis product, which is unfavorable for improving productivity and reducing the cost of the drying process.It is described that the reaction of the metallic iron powder can be promoted by the process of adding hydrochloric acid, oxalic acid, etc., but hydrochloric acid induces oxidation of the product, and oxalic acid is prone to producing insoluble ferrous iron, making it difficult to mix the raw materials uniformly and making it difficult to successfully produce lithium iron phosphate.

[0007] As another example, JP2007305585A discloses a method of reacting iron powder in an aqueous solution containing phosphoric acid and citric acid, followed by the addition of lithium hydroxide to prepare a lithium iron phosphate precursor. However, in this method, the surface of the iron powder first reacts with phosphoric acid to form an insoluble divalent iron compound, ferrous phosphate (Fe 3 (PO 4 ) 2 8H 2 O) is produced, and the surface products prevent further reaction between the inside of the metallic iron powder and phosphoric acid, resulting in an insufficient reaction, and also preventing citric acid from exerting its full chelating effect.

[0008] As another example, Patent Document CN102348634A controls the amount of oxygen chemically bonded to iron powder in an oxidizing atmosphere, so that carboxylic acid coexists when the iron powder reacts with phosphoric acid, and the carboxylic acid chelate promotes the reaction between the iron powder and phosphoric acid, thereby reducing the amount of unreacted iron powder remaining. However, the control of the amount of oxygen bonded to the iron powder in this method is more complicated.

[0009] Therefore, in the conventional technology, when lithium iron phosphate is produced using iron phosphate as a raw material, the solid content is low, resulting in high process costs. In addition, when lithium iron phosphate is produced using iron powder as a raw material, it is difficult to control the solid content to smoothly advance the reaction and reduce energy consumption in the subsequent process. Summary of the Invention

[0010] The present invention provides a novel green lithium iron phosphate precursor, and a method for producing the same and use thereof, to solve the drawbacks of the prior art, that is, when lithium iron phosphate is produced using iron phosphate as a raw material, the process cost is high due to the low solid content, and when lithium iron phosphate is produced using iron powder as a raw material, it is difficult to control the solid content so as to smoothly proceed with the reaction and reduce energy consumption in the subsequent process.

[0011] The present inventor has found that in the conventional method for producing lithium iron phosphate, when an iron source is used as a raw material, in order to smoothly proceed with the reaction, the solid content is inevitably too low, which leads to the disadvantage of increasing the energy consumption in the subsequent process, and when the solid content is high, the viscosity becomes too high and stirring becomes impossible. The present inventor has unexpectedly discovered that by first completely reacting the iron source with phosphoric acid to obtain product A, then completely reacting the iron source with an organic acid, a lithium source, and a carbon source to obtain product B, and then mixing and reacting the product B, the solid content in the lithium iron phosphate precursor can reach 50% or more, even 60%, and the energy consumption in the process of producing lithium iron phosphate from the lithium iron phosphate precursor can be greatly reduced, and the production method is simple and inexpensive. Furthermore, the method of the present invention can produce a lithium iron phosphate precursor with a very small particle size, and the charge / discharge c rate is high. It has been experimentally proven that this effect cannot be obtained if an organic acid is not added to the reaction of product B.

[0012] The present invention solves the above technical problems through the following technical solutions.

[0013] The present invention provides a method for preparing a lithium iron phosphate precursor, comprising the steps of:

[0014] S1. React a mixture of an iron source and a phosphoric acid solution, and after the reaction is completed, grind it to obtain product A;

[0015] The organic acid solution, the lithium source, and the carbon source are reacted to obtain a product B after the reaction is completed; the order of preparing the product A and the product B is not limited.

[0016] S2. Grinding the mixture of product A and product B to obtain a lithium iron phosphate precursor.

[0017] In the present invention, in step S1, the completion state of the mixing reaction of the iron source and the phosphoric acid solution is generally when no gas is generated by the reaction, as is known to those skilled in the art.

[0018] In S1, the iron source is known to those skilled in the art, and since the present invention is a process method including the steps of preparing iron phosphate and then preparing lithium iron phosphate, it is known to those skilled in the art that the iron source does not include iron phosphate. Preferably, the iron source is a compound containing iron and oxygen elements, preferably one or more of iron powder, ferric oxide, ferric tetroxide, and ferric nitrate, more preferably one or more of iron powder, ferric oxide, and ferric tetroxide.

[0019] Here, the iron content in the iron powder is preferably 95 wt% or more, more preferably 99 wt% or more, and even more preferably 99.5 wt% or more, for example 99.7 wt%, and the iron powder is, for example, one or more of primary reduced iron powder, secondary reduced iron powder, carbonyl reduced iron powder, and electrolytic iron powder.

[0020] Here, the purity of the diiron trioxide is preferably 95 wt% or more, more preferably 99 wt% or more, and even more preferably 99.5 wt% or more.

[0021] Here, the purity of the triiron tetroxide is preferably 95 wt% or more, more preferably 99 wt% or more, and even more preferably 99.5 wt% or more.

[0022] In S1, the mesh of the iron source is preferably 200 to 1000 mesh, more preferably 200 to 500 mesh, for example, 250 mesh or 300 mesh.

[0023] In S1, the phosphoric acid solution generally refers to an aqueous phosphoric acid solution, and the mass percentage concentration of phosphoric acid in the phosphoric acid solution is preferably 20% to 85%, for example, 49%, 59%, or 62%.

[0024] In S1, the phosphoric acid in the phosphoric acid solution may be a conventional phosphoric acid in the art, such as industrial grade phosphoric acid, food grade phosphoric acid, electrical grade phosphoric acid, or electronic grade phosphoric acid, and the electrical grade phosphoric acid can be purchased from GUANGXI QINZHOU CHENGXING CHEMICAL TECHNOLOGY CO.,LTD.

[0025] In S1, the reaction temperature of the mixture of the iron source and the phosphoric acid solution is preferably 20 to 95°C, more preferably 30 to 90°C, for example, 35°C, 45°C, or 55°C.

[0026] In S1, preferably, the mixture of the iron source and phosphoric acid solution is prepared by adding the iron source to a stirred phosphoric acid solution.

[0027] In S1, preferably, in the mixture of the iron source and the phosphoric acid solution, the molar ratio of iron element to phosphoric acid is (0.94-1.05):1, more preferably (0.96-1.0):1, for example, 0.98:1.

[0028] In S1, the grinding operation and conditions may be a conventional grinding operation, such as sand milling or ball milling.

[0029] Here, the grinding is preferably carried out by a sand mill. The sand mill is preferably a vertical sand mill, a horizontal sand mill (e.g., a nanoscale horizontal sand mill), a basket sand mill, or a double cone rod sand mill. The particle size of the grinding beads used in the sand mill is preferably 0.1 to 3.0 mm, for example, 0.3 mm or 0.4 mm. The grinding beads used in the sand mill are preferably zirconium oxide beads.

[0030] In S1, the viscosity of the product A is preferably 8000 to 20000 cps, more preferably 10000 to 20000 cps, for example, 15000 cps.

[0031] In S1, preferably, the organic acid solution generally refers to a solution of an organic acid, and the mass percentage concentration of the organic acid in the organic acid solution is more preferably 5% to 98%, for example, 55%, 62%, or 72%.

[0032] In S1, the organic acid in the organic acid solution is preferably a carboxylic acid compound and / or ascorbic acid, and the carboxylic acid compound is preferably one or more of formic acid, acetic acid, oxalic acid, citric acid, tartaric acid, and malic acid, and the organic acid is, for example, citric acid and / or oxalic acid, or malic acid and / or tartaric acid.

[0033] In S1, preferably, the lithium source is one or more of lithium hydroxide monohydrate, lithium carbonate, lithium dihydrogen phosphate, lithium phosphate and lithium acetate, more preferably lithium hydroxide monohydrate and / or lithium acetate, and the lithium carbonate is preferably industrial grade lithium carbonate or battery grade lithium carbonate.

[0034] In S1, the molar ratio of lithium element in the lithium source to phosphoric acid in the phosphoric acid solution is preferably 0.98 to 1.05, for example, 1.02, 1.03, or 1.04.

[0035] In S1, preferably, the carbon source includes one or more of glucose, sucrose, starch, phenolic resin, cyclodextrin, polyethylene, polyethylene glycol and polyvinyl alcohol, more preferably a mixture of polyvinyl alcohol, cyclodextrin and polyethylene glycol.

[0036] In S1, the amount of the carbon source added is preferably 1 to 60 mass %, more preferably 5 to 50 mass %, and further preferably 10 to 40 mass %, of the iron source.

[0037] In S1, the reaction temperature of the mixture of the organic acid, lithium source and carbon source is preferably 20 to 95°C, more preferably 30 to 90°C, for example 35°C, 40°C or 45°C.

[0038] In S1, preferably, the mixture of organic acid, lithium source and carbon source is prepared by adding the lithium source and carbon source to a stirred organic acid solution.

[0039] In S2, the mixture of product A and product B generally means mixing product A and product B.

[0040] In S2, the operation and conditions of said grinding may be conventional in the art, and the preferred embodiment of said grinding may be the same as S1.

[0041] In S2, the particle size of the lithium iron phosphate precursor is preferably 170 to 250 nm, for example, 200 nm or 220 nm.

[0042] The present invention further provides a lithium iron phosphate precursor produced by the method for producing a lithium iron phosphate precursor.

[0043] In the present invention, the lithium iron phosphate precursor preferably has a particle size of 170 to 250 nm.

[0044] The present invention further provides a method for preparing lithium iron phosphate, comprising the steps of spray drying, calcining and grinding said lithium iron phosphate precursor.

[0045] Here, the operations and conditions of the spray drying, calcination and grinding may be those common in the art.

[0046] Here, in the spray drying, the gas inlet temperature may be 280°C.

[0047] Here, in the spray drying, the outlet temperature may be 110°C.

[0048] Here, the firing conditions are as follows: in a nitrogen atmosphere of 99.999% purity, the temperature is gradually increased from room temperature to 650°C at a rate of 5°C / min, the material is kept at 650°C for 10 hours, and then cooled to obtain a sintered product.

[0049] Here, the pulverization conditions are as follows: the sintered product is treated with an airflow pulverizer to obtain the target final product positive electrode lithium iron phosphate material with a particle size D50 of 1.5-3 μm.

[0050] The present invention further provides lithium iron phosphate produced by the method for producing lithium iron phosphate.

[0051] The present invention further provides the use of the aforementioned lithium iron phosphate in the manufacture of a positive electrode material for a lithium ion battery.

[0052] Each of the preferred conditions described above can be combined in any manner without violating common knowledge in the art to obtain each of the preferred embodiments of the present invention.

[0053] All reagents and materials used in the present invention are commercially available.

[0054] Positive Progressive Effects of the Invention:

[0055] The lithium iron phosphate precursor produced by the present invention can greatly improve the solid content, reduce the energy consumption in the post-process, and produce a simple, green and environmentally friendly process without producing three types of waste material at low cost, making it possible to produce lithium iron phosphate, a positive electrode material, from an iron source at low cost. In addition, the lithium iron phosphate precursor produced by the present invention has an extremely small particle size and a high charge / discharge c rate. [Brief description of the drawings]

[0056] [Figure 1] 1 is an XRD spectrum of the lithium iron phosphate of Example 1. [Diagram 2] 1 is a scanning electron microscope photograph of the lithium iron phosphate of Example 1. [Diagram 3] 3 shows charge and discharge curves of the lithium iron phosphate of Example 1 at different c-rates. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0057] The present invention will be further described below with reference to examples, but the present invention is not limited to the scope of these examples. In the following examples, for the experimental methods for which no particular conditions are specified, conventional methods and conditions or product instructions are used.

[0058] Example 1

[0059] 1. According to the molar ratio of iron and phosphorus elements of 0.96:1, 6.895 kg of 85% industrial grade phosphoric acid was added to 5 L of deionized water, and diluted to a concentration of 49% by stirring. Then, slowly add 3.25 kg of 200 mesh, 99% purity secondary reduced iron powder while stirring, and react at 45°C. During the reaction, some gas was generated, and the color of the reactant gradually changed from gray-black to gray-white. When the reaction no longer generates gas, the material was put into a sand mill to carry out grinding. The grinding beads in the sand mill were 0.3 mm zirconium oxide beads. During the grinding, the viscosity of the material gradually increased to 15000cps, and the color gradually changed to pure white, and product A was obtained.

[0060] 2. According to the molar ratio of lithium and phosphorus of 1.04:1, 4 kg of citric acid is dissolved in 3.25 kg of deionized water to prepare a solution. While stirring, 2.3 kg of battery grade lithium carbonate and 1 kg of sucrose are added dropwise to the reaction solution, and reacted under the condition of 40°C, during which a large amount of gas is generated. The reaction is continued until no more gas is generated, forming a transparent solution, and product B is obtained.

[0061] 3. Product B was added to product A, and after mixing and stirring, the viscosity of the system rapidly decreased to 1000cps, followed by grinding. The material was ground until the particle size reached D50 of about 200nm, and the reaction was completed to obtain a slurry with a solid content of 50%.

[0062] 4. The reaction product slurry was spray-dried, sintered and ground to prepare lithium iron phosphate positive electrode material.

[0063] Here, spray drying conditions: the gas inlet temperature was 280°C, and the outlet temperature was 110°C. Sintering conditions: in a nitrogen gas atmosphere with a purity of 99.999%, the temperature was gradually increased from room temperature to 650°C at a rate of 5°C / min, and the product was kept at 650°C for 10 hours, and then cooled to obtain a sintered product. Crushing conditions: the sintered product was processed in an airflow crushing device to obtain a target finished product of positive electrode lithium iron phosphate material with a particle size D50 of 1.5 to 3 μm.

[0064] The lithium iron phosphate positive electrode material prepared in Example 1 was subjected to PXRD (powder X-ray diffraction) and scanning electron microscope (SEM) tests.

[0065] The PXRD data in Figure 1 was obtained by testing on a Bruker D8 ADVANCE, and the SEM images in Figure 2 were obtained by testing on a Hitachi SU8010.

[0066] Example 2

[0067] 1. According to the molar ratio of iron and phosphorus elements of 0.98:1, 13.8kg of 85% food-grade phosphoric acid was added to 5L of deionized water, and diluted to a concentration of 62.4% by stirring. Slowly add 6.6kg of 250 mesh, 99.5% purity secondary reduced iron powder while stirring, and react at 35℃. During the reaction, some gas was generated, and the color of the reactant gradually changed from gray-black to gray-white. When the reaction no longer generates gas, the material was put into a sand mill to carry out grinding. The grinding beads in the sand mill were 0.4mm zirconium oxide beads. During grinding, the viscosity of the material gradually increased to 20000cps, and the color gradually changed to pure white, and product A was obtained.

[0068] 2. According to the molar ratio of lithium and phosphorus of 1.03:1, 4 kg of citric acid and 4 kg of oxalic acid were dissolved in 5 kg of deionized water to prepare a solution, and 2 kg of glucose and 5.18 kg of industrial grade lithium hydroxide monohydrate were gradually added under stirring, and the reaction was carried out under the condition of 35°C, during which a large amount of gas was generated, and the reaction was continued until the gas generation stopped, forming a transparent and viscous solution, and product B was obtained.

[0069] 3. Product B was added to product A, and after mixing and stirring, the viscosity of the system rapidly decreased to 1200cps, followed by grinding. The material was ground to a particle size of about 220nm D50, and the reaction was completed to obtain a slurry with a solid content of 53%.

[0070] 4. The reaction product slurry was spray-dried, sintered and ground to obtain lithium iron phosphate positive electrode material.

[0071] Here, spray drying conditions: the gas inlet temperature was 280°C, and the outlet temperature was 110°C. Sintering conditions: in a nitrogen gas atmosphere with a purity of 99.999%, the temperature was gradually increased from room temperature to 650°C at a rate of 5°C / min, and the product was kept at 650°C for 10 hours, and then cooled to obtain a sintered product. Crushing conditions: the sintered product was processed in an airflow crushing device to obtain a target finished product of positive electrode lithium iron phosphate material with a particle size D50 of 1.5 to 3 μm.

[0072] Example 3

[0073] 1. According to the molar ratio of iron and phosphorus elements of 1:1, add 27.6kg of 85% food-grade phosphoric acid to 12L of deionized water, dilute to a concentration of 59.2% by stirring, slowly add 13.5kg of 300 mesh, 99.7% purity electrolytic iron powder while stirring, react at 55℃, some gas is generated during the reaction, and the color of the reactant gradually changes from gray-black to gray-white. When the reaction no longer generates gas, the material is put into a sand mill to carry out grinding, and its viscosity gradually increases to 10000cps during grinding, and the color gradually changes to pure white, and product A is obtained.

[0074] 2. According to the molar ratio of lithium and phosphorus of 1.02:1, 6 kg of malic acid and 7 kg of tartaric acid are dissolved in 5 kg of deionized water to prepare a solution. While stirring, 4 kg of polyethylene glycol and 9.03 kg of industrial grade lithium carbonate are gradually added to the reaction solution, and reacted under the condition of 45°C, during which a large amount of gas is generated, and the reaction is continued until gas generation stops, forming a transparent and viscous solution, and obtaining product B.

[0075] 3. Product B was added to product A, and after mixing and stirring, the viscosity of the system rapidly decreased, followed by grinding. The material was ground to a particle size of about 170 nm, D50, and the reaction was completed to obtain a slurry with a solid content of 60%.

[0076] 4. The reaction product slurry was spray-dried, sintered and ground to obtain lithium iron phosphate positive electrode material.

[0077] Here, spray drying conditions: the gas inlet temperature was 280°C, and the outlet temperature was 110°C. Sintering conditions: in a nitrogen gas atmosphere with a purity of 99.999%, the temperature was gradually increased from room temperature to 650°C at a rate of 5°C / min, and the product was kept at 650°C for 10 hours, and then cooled to obtain a sintered product. Crushing conditions: the sintered product was processed in an airflow crushing device to obtain a target finished product of positive electrode lithium iron phosphate material with a particle size D50 of 1.5 to 3 μm.

[0078] Example 4

[0079] 1. According to the molar ratio of iron and phosphorus of 0.98:1, 13.8kg of 85% food-grade phosphoric acid was added to 5L of deionized water, and diluted to a concentration of 62.4% by stirring. Then, 9.11kg of 250 mesh, 99.5% purity triferric oxide was slowly added while stirring, and the reaction was carried out at 35℃. During the reaction, some gas was generated, and the color of the reactant gradually changed from gray-black to gray-white. When the reaction no longer generated gas, the material was put into a sand mill to carry out grinding. The grinding beads in the sand mill were 0.4mm zirconium oxide beads. During grinding, its viscosity gradually increased to 20000cps, and the color gradually changed to pure white, and product A was obtained.

[0080] 2. According to the molar ratio of lithium and phosphorus of 1.03:1, 4 kg of citric acid and 4 kg of oxalic acid were dissolved in 5 kg of deionized water to prepare a solution, and 2 kg of glucose, 4 kg of industrial grade lithium hydroxide monohydrate, and 3.43 kg of lithium acetate were added dropwise with stirring, and the mixture was reacted at 35°C. During the reaction, a large amount of gas was generated. The reaction was continued until no more gas was generated, forming a transparent and viscous solution, and product B was obtained.

[0081] 3. Product B was added to product A, and after mixing and stirring, the viscosity of the system rapidly decreased to 1200cps, followed by grinding. The material was ground to a particle size of about 220nm D50, and the reaction was completed to obtain a slurry with a solid content of 53%.

[0082] 4. The reaction product slurry was spray-dried, sintered and ground to obtain lithium iron phosphate positive electrode material.

[0083] Here, spray drying conditions: the gas inlet temperature was 280°C, and the outlet temperature was 110°C. Sintering conditions: in a nitrogen gas atmosphere with a purity of 99.999%, the temperature was gradually increased from room temperature to 650°C at a rate of 5°C / min, and the product was kept at 650°C for 10 hours, and then cooled to obtain a sintered product. Crushing conditions: the sintered product was processed in an airflow crushing device to obtain a target finished product of positive electrode lithium iron phosphate material with a particle size D50 of 1.5 to 3 μm.

[0084] Example 4

[0085] 1. According to the molar ratio of iron and phosphorus of 0.98:1, 13.8kg of 85% food-grade phosphoric acid was added to 5L of deionized water, and diluted to a concentration of 62.4% by stirring. Slowly add 2.2kg of 250 mesh, 99.5% purity secondary reduced iron powder, 3.03kg of triferric oxide, and 3.14kg of diferric oxide while stirring, and react at 35℃. During the reaction, some gas was generated, and the color of the reactant gradually changed from gray-black to gray-white. When the reaction no longer generates gas, the material was put into a sand mill to carry out grinding. The grinding beads in the sand mill were 0.4mm zirconium oxide beads. During grinding, its viscosity gradually increased to 20000cps, and the color gradually changed to pure white, and product A was obtained.

[0086] 2. According to the molar ratio of lithium and phosphorus of 1.03:1, 4 kg of citric acid and 4 kg of oxalic acid were dissolved in 5 kg of deionized water to prepare a solution. While stirring, 2 kg of a mixture of polyvinyl alcohol, cyclodextrin and polyethylene glycol and 5.18 kg of industrial grade lithium hydroxide monohydrate were added dropwise to the solution, and reacted under the condition of 35°C. During the reaction, a large amount of gas was generated. The reaction was continued until no more gas was generated, forming a transparent and viscous solution, and product B was obtained.

[0087] 3. Product B was added to product A, and after mixing and stirring, the viscosity of the system rapidly decreased to 1200cps, followed by grinding. The material was ground to a particle size of about 220nm D50, and the reaction was completed to obtain a slurry with a solid content of 50%.

[0088] 4. The reaction product slurry was spray-dried, sintered and ground to obtain lithium iron phosphate positive electrode material.

[0089] Here, spray drying conditions: the gas inlet temperature was 280°C, and the outlet temperature was 110°C. Sintering conditions: in a nitrogen gas atmosphere with a purity of 99.999%, the temperature was gradually increased from room temperature to 650°C at a rate of 5°C / min, and the product was kept at 650°C for 10 hours, and then cooled to obtain a sintered product. Crushing conditions: the sintered product was processed in an airflow crushing device to obtain a target finished product of positive electrode lithium iron phosphate material with a particle size D50 of 1.5 to 3 μm.

[0090] Comparative Example 1

[0091] 1. According to the molar ratio of iron and phosphorus elements of 0.96:1, 6.895 kg of 85% industrial grade phosphoric acid was added to 5 L of deionized water, and diluted to a concentration of 49% by stirring. While stirring, 3.25 kg of secondary reduced iron powder with 200 mesh and purity of 99% was slowly added, and reacted at 45°C. During the reaction, some gas was generated, and the color of the reactant gradually changed from gray-black to gray-white. When the reaction no longer generated gas, the material was put into a sand mill to carry out grinding. The grinding beads in the sand mill were 0.3 mm zirconium oxide beads. During grinding, its viscosity gradually increased to 15000cps, and the color gradually changed to pure white, and product A was obtained.

[0092] 2. According to the molar ratio of lithium and phosphorus of 1.04:1, 2.3 kg of battery grade lithium carbonate and 1 kg of sucrose were added dropwise with stirring to 3.25 kg of deionized water at 40°C to prepare a slurry (the solubility of lithium carbonate in water is low) to obtain Product B.

[0093] 3. After adding product B to product A and mixing and stirring, the viscosity of the system increased suddenly, the slurry solidified, and grinding could not be carried out.

[0094] Comparative Example 2

[0095] 1. According to the molar ratio of iron and phosphorus elements of 0.96:1, 6.895 kg of 85% industrial grade phosphoric acid was added to 5 L of deionized water, and diluted to a concentration of 49% by stirring. While stirring, 3.25 kg of secondary reduced iron powder with 200 mesh and purity of 99% was slowly added, and reacted at 45°C. During the reaction, some gas was generated, and the color of the reactant gradually changed from gray-black to gray-white. When the reaction no longer generated gas, the material was put into a sand mill to carry out grinding. The grinding beads in the sand mill were 0.3 mm zirconium oxide beads. During grinding, its viscosity gradually increased to 15000cps, and the color gradually changed to pure white, and product A was obtained.

[0096] 2. To avoid the problem of solidification when mixing with Product B, 25 kg of deionized water was added to Product A to dilute it.

[0097] 3. According to the molar ratio of lithium and phosphorus of 1.04:1, 2.3 kg of battery grade lithium carbonate and 1 kg of sucrose were added dropwise with stirring to 3.25 kg of deionized water at 40°C to prepare a slurry (the solubility of lithium carbonate in water is low) to obtain Product B.

[0098] 4. Product B was added to product A, mixed and stirred, the system showed no hardening problem, and grinding was then carried out. When the primary particle size of the material finally reached a D50 of about 800 nm, the system was stable, and the primary particle size did not show any tendency to decrease when grinding was carried out. The reaction was stopped, and a slurry with a solid content of 17% was obtained at the completion of the reaction.

[0099] 5. The reaction product slurry was spray-dried, sintered and ground to obtain lithium iron phosphate positive electrode material.

[0100] Here, spray drying conditions: the gas inlet temperature was 280°C, and the outlet temperature was 110°C. Sintering conditions: in a nitrogen gas atmosphere with a purity of 99.999%, the temperature was gradually increased from room temperature to 650°C at a rate of 5°C / min, and the product was kept at 650°C for 10 hours, and then cooled to obtain a sintered product. Crushing conditions: the sintered product was processed in an airflow crushing device to obtain a target finished product of positive electrode lithium iron phosphate material with a particle size D50 of 1.5 to 3 μm.

[0101] Comparative Example 3

[0102] 1. According to the molar ratio of iron and phosphorus elements of 0.96:1, 6.895 kg of 85% industrial grade phosphoric acid was added to 5 L of deionized water, and diluted to a concentration of 49% by stirring. While stirring, 3.25 kg of secondary reduced iron powder with 200 mesh and purity of 99% was slowly added, and 4 kg of citric acid was further added, and the reaction was carried out at 45°C. During the reaction, some gas was generated, and the color of the reactant gradually changed from gray-black to yellow-green. When the reaction no longer generated gas, the material was put into a sand mill to carry out grinding. The grinding beads in the sand mill were 0.3 mm zirconium oxide beads. During grinding, its viscosity gradually increased to 15000cps, and the color gradually changed to yellow-green, and product A was obtained.

[0103] 2. According to the molar ratio of lithium and phosphorus of 1.04:1, 2.3 kg of battery grade lithium carbonate and 1 kg of sucrose were added dropwise with stirring to 3.25 kg of deionized water at 40°C to prepare a slurry (the solubility of lithium carbonate in water is low) to obtain Product B.

[0104] 3. Product B was added to product A, and after mixing and stirring, the viscosity of the system gradually increased to more than 20,000cps. In order to make the process run smoothly, another 10L of deionized water was added to reduce the viscosity to 1,200cps. When the material was ground to a particle size of about 500nm, D50, the reaction was completed to obtain a slurry with a solid content of 35%.

[0105] 4. The reaction product slurry was spray-dried, sintered and ground to obtain lithium iron phosphate positive electrode material.

[0106] Here, spray drying conditions: the gas inlet temperature was 280°C, and the outlet temperature was 110°C. Sintering conditions: in a nitrogen gas atmosphere with a purity of 99.999%, the temperature was gradually increased from room temperature to 650°C at a rate of 5°C / min, and the product was kept at 650°C for 10 hours, and then cooled to obtain a sintered product. Crushing conditions: the sintered product was processed in an airflow crushing device to obtain a target finished product of positive electrode lithium iron phosphate material with a particle size D50 of 1.5 to 3 μm.

[0107] The lithium iron phosphate powders prepared in Examples 1 to 5 and Comparative Examples 2 to 3 were each taken and mixed with carbon black and polyvinylidene fluoride (PVDF) in a mass ratio of 80:10:10 until uniform, then coated on aluminum foil and dried to prepare a suitable positive electrode test piece, which was then assembled with metallic lithium to prepare a 2032 button battery, and a charge / discharge cycle experiment was performed using a charge / discharge machine (LAND CT2001A) at a charge / discharge range of 2.0V to 4.2V and at charge / discharge rates of C / 10, C / 5, C / 2, 1C, 2C, and 5C. The results are shown in FIG. 3 and Table 1.

[0108] [Table 1]

[0109] [Table 2]

[0110] As shown in Table 2, in Examples 1 to 5, the amount of dehydration required for preparing the precursor can be significantly reduced compared to Comparative Examples 2 and 3, and the energy consumption required for dehydration can be significantly reduced. In Comparative Example 1, the production method based on the conventional technology had a problem that only the solid content increased and the viscosity was too high to stir. In Comparative Examples 2 to 3, the effect of the present invention was not obtained because an organic acid was not added to the reaction of Product B.

[0111] Although specific embodiments of the present invention have been described above, it should be understood by those skilled in the art that these are merely examples and that various changes and modifications can be made to these embodiments without departing from the principles and essence of the present invention. Accordingly, the scope of the present invention is defined by the appended claims.

Claims

1. S1. React a mixture of an iron source and a phosphoric acid solution, and after the reaction is completed, grind the mixture to obtain product A; reacting a mixture of an organic acid solution, a lithium source, and a carbon source, and obtaining a product B after the reaction is completed, the order of producing the product A and the product B is not limited; S2. Grinding the mixture of product A and product B to obtain a lithium iron phosphate precursor; A method for producing a lithium iron phosphate precursor, comprising: The mass percentage concentration of phosphoric acid in the phosphoric acid solution is 20% to 85%, The organic acid solution has a mass percentage concentration of the organic acid of 55% to 72%; The organic acid in the organic acid solution is one of a carboxylic acid compound and / or ascorbic acid; the carboxylic acid compound is one or more of formic acid, acetic acid, oxalic acid, citric acid, tartaric acid, and malic acid; The lithium iron phosphate precursor has a solid content of 50% or more, The particle size of the lithium iron phosphate precursor is 170 to 250 nm. A method for producing a lithium iron phosphate precursor.

2. (1) the iron source is one or more of iron powder, ferric oxide, ferric oxide, and ferric nitrate; (2) the mesh of the iron source is 200 to 500 mesh; 2. A method for producing a lithium iron phosphate precursor according to claim 1, characterized in that one or more of the following conditions are met:

3. The iron content in the iron powder is 95 wt % or more, and / or the iron powder being one or more of primary reduced iron powder, secondary reduced iron powder, carbonyl reduced iron powder, and electrolytic iron powder; and / or The purity of the iron trioxide is 95 wt % or more, and / or The purity of the iron trioxide is 95 wt% or more. The method for producing the lithium iron phosphate precursor according to claim 2 .

4. The iron content in the iron powder is 99.5 wt % or more, and / or The purity of the iron trioxide is 99.5 wt % or more, and / or The purity of the iron trioxide is 99.5 wt% or more. The method for producing the lithium iron phosphate precursor according to claim 2 .

5. (1) The mass percentage concentration of phosphoric acid in the phosphoric acid solution is 49%, 59%, or 62%; (2) the phosphoric acid in the phosphoric acid solution is industrial grade phosphoric acid, food grade phosphoric acid, electrical grade phosphoric acid, or electronic grade phosphoric acid; (3) the reaction temperature of the mixture of the iron source and the phosphoric acid solution is 20 to 95° C.; (4) In the mixture of the iron source and the phosphoric acid solution, the molar ratio of elemental iron to phosphoric acid is (0.94-1.05):1; 2. A method for producing a lithium iron phosphate precursor according to claim 1, characterized in that one or more of the following conditions are met:

6. The reaction temperature of the mixture of the iron source and the phosphoric acid solution is 35° C., 45° C., or 55° C.; and / or In the mixture of the iron source and phosphoric acid solution, the molar ratio of elemental iron to phosphoric acid is 0.98:1; A method for producing the lithium iron phosphate precursor according to claim 1 .

7. (1) the grinding is carried out using a sand mill; (2) The viscosity of the product A is 8,000 to 20,000 cps; (3) the mass percentage concentration of the organic acid in the organic acid solution is 62%; (4) The organic acid is citric acid and / or oxalic acid, or malic acid and / or tartaric acid; 2. A method for producing a lithium iron phosphate precursor according to claim 1, characterized in that one or more of the following conditions are met:

8. The sand mill is a vertical sand mill, a horizontal sand mill, a basket sand mill, or a double cone rod sand mill; and / or The particle size of the grinding beads used in the sand mill is 0.1 to 3.0 mm, and / or the grinding beads used in the sand mill are zirconium oxide beads, and / or The viscosity of the product A is 10,000 to 20,000 cps; The method for producing the lithium iron phosphate precursor according to claim 7 .

9. The grain size of the grinding beads used in the sand mill is 0.3 mm or 0.4 mm, and / or The viscosity of the product A is 15,000 cps. The method for producing the lithium iron phosphate precursor according to claim 7 .

10. (1) the lithium source is one or more of lithium hydroxide monohydrate, lithium carbonate, lithium dihydrogen phosphate, lithium phosphate, and lithium acetate; (2) the molar ratio of lithium element in the lithium source to phosphoric acid in the phosphoric acid solution is 0.98 to 1.05; (3) the carbon source comprises one or more of glucose, sucrose, starch, phenolic resin, cyclodextrin, polyethylene, polyethylene glycol, and polyvinyl alcohol; (4) the amount of the carbon source added is 1 to 60% by mass of the iron source; (5) the reaction temperature of the mixture of the organic acid solution, the lithium source and the carbon source is 20 to 95° C.; (6) The particle size of the lithium iron phosphate precursor is 200 nm or 220 nm; 2. A method for producing a lithium iron phosphate precursor according to claim 1, characterized in that one or more of the following conditions are met:

11. the lithium source is lithium hydroxide monohydrate and / or lithium acetate; and / or and / or the molar ratio of lithium element in the lithium source to phosphoric acid in the phosphoric acid solution is 1.02, 1.03 or 1.04; and / or the carbon source is a mixture of polyvinyl alcohol, cyclodextrin and polyethylene glycol; and / or The amount of the carbon source added is 5 to 50% by mass of the iron source, and / or The reaction temperature of the mixture of the organic acid solution, the lithium source and the carbon source is 30 to 90° C.; A method for producing the lithium iron phosphate precursor according to claim 1 .

12. The amount of the carbon source added is 10 to 40% by mass of the iron source, and / or The reaction temperature of the mixture of the organic acid solution, the lithium source and the carbon source is 35° C., 40° C. or 45° C.; A method for producing the lithium iron phosphate precursor according to claim 1 .

13. A lithium iron phosphate precursor, characterized in that it is produced by the method for producing a lithium iron phosphate precursor according to any one of claims 1 to 12.

14. A method for producing lithium iron phosphate, comprising the steps of spray drying, calcining and grinding the lithium iron phosphate precursor of claim 13.