Battery anode compositions comprising carbon and optionally silicon characterized by carbon domain size estimated by X-ray diffraction - Patents.com

The lithium ion battery anode composition with porous composite particles of carbon and silicon addresses the challenge of suboptimal electrode performance by enhancing capacity, charging speed, and stability, benefiting electric vehicles and energy storage.

JP2024535747APending Publication Date: 2024-10-02SILA NANOTECHNOLOGIES INC

Patent Information

Application Number
JP2024514113
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-07
Filing Date
2022-09-07
Publication Date
2024-10-02

AI Technical Summary

Technical Problem

Existing rechargeable batteries face challenges in achieving optimal electrode performance due to unclear selection of carbon types and properties in composite particles, leading to insufficient charge storage capacity, fast charging, and long cycle stability, which are crucial for applications in electric vehicles and energy storage.

Method used

A lithium ion battery anode composition is developed using porous composite particles comprising carbon and silicon, characterized by specific domain sizes and ratios of atom pair correlation functions, resulting in improved areal capacitance loading and cycling stability.

Benefits of technology

The anode composition enhances battery performance by increasing capacity, enabling faster charging and discharging, and improving long-term stability, thereby increasing energy density and reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024535747000001_ABST
    Figure 2024535747000001_ABST
Patent Text Reader

Abstract

In one embodiment, a lithium ion battery anode composition comprises porous composite particles comprising carbon (C) and an active material comprising silicon (Si), the carbon being characterized by a domain size (r) as inferred from an atomic pair correlation function G(r) obtained from synchrotron X-ray diffraction measurement of the porous composite particles ranging from about 10 Å (1 nm) to about 60 Å (6 nm). In another embodiment, a carbon material for use in making an anode composition for use in a Li-ion battery is characterized by a domain size (r) as inferred from an atomic pair correlation function G(r) obtained from synchrotron X-ray diffraction measurement of the carbon material ranging from about 10 Å (1 nm) to about 60 Å (6 nm).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This patent application claims the benefit of U.S. Provisional Application No. 63 / 241,407, entitled "BATTERY ELECTRODE COMPOSITION COMPRISING CARBON AND SILICON WITH SPECIFIC PROPERTIES FOR SUPERIOR PERFORMANCE," filed September 7, 2021, which is assigned to the assignee hereof and is expressly incorporated by reference in its entirety. [Background technology]

[0002] (Field) Aspects of the present disclosure relate generally to energy storage devices, and more particularly to battery technology, supercapacitor technology, and the like.

[0003] (background) Advanced rechargeable batteries are desirable for a wide range of electronic devices, electric vehicles, grid storage, and other important applications, in part, due to rechargeable batteries' relatively high energy density, relatively high specific energy, relatively high specific power, relatively fast charging, light weight, and potential for long life and cycle life.

[0004] However, despite the increasing commercial popularity of electrochemical energy storage technologies, further development of batteries is needed, particularly for low or zero emission, hybrid electric or fully electric vehicles, consumer electronics, energy efficient cargo ships and locomotives, aerospace applications, and potential applications in the power grid. In particular, further improvements are desired with respect to various rechargeable batteries, such as rechargeable metal and metal ion batteries (e.g., rechargeable Li and Li-ion batteries, rechargeable Na and Na-ion batteries, rechargeable Mg and Mg-ion batteries, rechargeable K and K-ion batteries, rechargeable Ca and Ca-ion batteries, etc.). The following energy storage devices may similarly benefit from additional improvements: rechargeable halogen-ion batteries (such as F-ion and Cl-ion batteries), rechargeable mixed-ion batteries, rechargeable aqueous batteries (e.g., rechargeable batteries having pH neutral or acidic or caustic electrolytes), electrochemical capacitors (e.g., supercapacitors or double layer capacitors), hybrid devices, rechargeable polymer electrolyte batteries and supercapacitors, rechargeable polymer gel electrolyte batteries and supercapacitors, rechargeable solid ceramic or solid glass electrolyte batteries, rechargeable composite electrolyte batteries, to name a few.

[0005] A wide range of active (charge storage) materials, a wide range of polymer binders, a wide range of conductive additives, and various mixing recipes can be utilized in the construction of battery electrodes. In some designs, the active materials can be utilized in the form of composite particles. However, the optimal composite formulation needs to be identified for improved electrode performance (low and stable resistance, high cycling stability, high rate capability, acceptable energy, good volumetric capacity, etc.). Furthermore, the selection of binders, additives, and mixing protocols needs to be found for the specific type, specific physical and chemical properties, and specific size of active particles. In many cases, the selection of the architecture and composition of the composite particles and the composition of the electrode is not straightforward and can be counterintuitive.

[0006] In many different types of rechargeable batteries, the charge storage material may be produced as a (nano)composite powder that may contain conductive carbon. As a subset of such particles, conductive carbon may be distributed not only on the surface of the (nano)composite particles but also within their bulk. In principle, such a class of charge storage (nano)composite particles may promise scalable (and in some cases sustainable) manufacturing and provide good charge storage performance characteristics. Unfortunately, it remains largely unclear which types and properties of carbon may be advantageous in such applications of composite ((nano)composite) particles. In addition, it is even more unclear how to achieve effective processing of such (nano)composite particles into electrodes that may provide good performance characteristics including high capacity, fast charging, fast discharging, and long cycling stability. The performance of battery electrodes constructed from similar (nano)composites has been shown to be stable at moderate electrode capacity loadings (2-4 mAh / cm for batteries). 2 ) may be insufficient, especially when the capacity is high (e.g., 4 to 16 mAh / cm 2 However, higher capacity loading is favorable for increasing battery cell energy density and reducing cell manufacturing costs. Summary of the Invention [Problem to be solved by the invention]

[0007] Thus, there is a continuing need for improved batteries, components, electrode materials, and other related materials and manufacturing processes. [Means for solving the problem]

[0008] The following provides a simplified summary of one or more aspects disclosed herein. Therefore, the following summary should not be considered an extensive summary of all contemplated aspects, nor should the following summary be considered to identify key or critical elements of all contemplated aspects or to delineate the scope associated with any particular aspect. Thus, the following summary has the sole purpose of presenting certain concepts of one or more aspects of the mechanisms disclosed herein in a simplified form prior to the detailed description provided below.

[0009] In one embodiment, a lithium ion battery anode composition comprises porous composite particles comprising carbon (C) and an active material comprising silicon (Si), the carbon characterized by a domain size (r) as inferred from an atomic pair distribution function G(r) obtained from synchrotron X-ray diffraction measurements of the porous composite particles ranging from about 10 Å (1 nm) to about 60 Å (6 nm).

[0010] In some embodiments, the carbon is characterized by one or more of the following: (1) domain sizes ranging between about 15 Å and about 19 Å, (2) domain sizes ranging between about 19 Å and about 22 Å, (3) domain sizes ranging between about 24 Å and about 28 Å, and (4) domain sizes ranging between about 28 Å and 55 Å, as estimated from the atomic pair correlation function G(r).

[0011] In some embodiments, the carbon comprises porous carbon.

[0012] In some embodiments, G(r=r1) is the value of the atomic pair correlation function at a real space position in the first coordination sphere of carbon, G(r=r2) is the value of the atomic pair correlation function at a real space position in the second coordination sphere of carbon, and the ratio G(r=r1) / G(r=r2) is in the range of about 0.700 to about 0.590.

[0013] In some embodiments, W(r=r1) is the value of the full width at half maximum of the atomic pair correlation function at a real space position in the first coordination sphere of carbon, and W(r=r2) is the value of the full width at half maximum of the atomic pair correlation function at a real space position in the second coordination sphere of carbon; the ratio W(r=r1) / W(r=r2) is in the range of about 0.700 to about 0.850.

[0014] In some embodiments, G(r=r1) is the value of the atomic pair correlation function at a real space position in the first coordination sphere of carbon, G(r=r3) is the value of the atomic pair correlation function at a real space position in the third coordination sphere of carbon, and the ratio G(r=r1) / G(r=r3) is in the range of about 1.100 to about 1.300.

[0015] In some embodiments, W(r=r1) is the value of the full width at half maximum of the atomic pair correlation function at a real space position in the first coordination sphere of carbon, W(r=r3) is the value of the full width at half maximum of the atomic pair correlation function at a real space position in the third coordination sphere of carbon, and the ratio W(r=r1) / W(r=r3) is in the range of about 0.600 to about 0.850.

[0016] In some embodiments, the anode comprising the anode composition has a current density of about 2 mAh / cm 2 to about 16mAh / cm 2 The areal capacitance load is shown to be

[0017] In some embodiments, about 10% to about 100% of the areal capacity loading of the anode is provided by composite particles each configured as a porous composite particle.

[0018] In some embodiments, the composite particles exhibit a weight ratio of silicon (Si) to carbon (C) ranging from about 5:1 to 1:5 on average.

[0019] In some embodiments, the porous composite particles are characterized by an average scattering domain size (r) as estimated from the atomic pair distribution function G(r), ranging from about 1 nm to about 40 nm.

[0020] In some embodiments, the porous composite particles are characterized by an average scattering domain size (r) ranging from about 1 nm to about 10 nm.

[0021] In some embodiments, the porous composite particles contain, on average, less than about 1% hydrogen (H), less than about 5% nitrogen (N), and less than about 2% oxygen (O) by weight.

[0022] In some embodiments, the porous composite particles exhibit, on average, about 1.5% to about 25% by weight nitrogen (N) uptake when heated in nitrogen gas (N2) at 1050° C. for 2 hours, as measured on a powder comprising the porous composite particles.

[0023] In some embodiments, the porous composite particles exhibit an average uptake of nitrogen (N) of about 0.5% to about 10% by weight when heated in nitrogen gas (N) at 850° C. for 2 hours, as measured on a powder comprising the porous composite particles.

[0024] In some embodiments, the porous composite particles form about 1% to about 100% by weight silicon carbide (SiC) when heated in nitrogen gas (N2) or argon gas (Ar) at a temperature range of about 750° C. to about 950° C. for 2 hours or longer, as detected by X-ray diffraction (XRD) or Fourier transform infrared spectroscopy (FTIR).

[0025] In some embodiments, the porous composite particles have a molecular weight of about 1 to about 40 m, as measured using a nitrogen adsorption isotherm on a powder comprising the porous composite particles. 2 The average Brunauer-Emmett-Teller (BET) specific surface area is in the range of 1 / g.

[0026] In some embodiments, the porous composite particles have a porous density of about 0.9 g / cm as measured using nitrogen or argon pycnometry on a powder comprising the porous composite particles. 3 to about 2.2 g / cm 3 The average density is in the range of

[0027] In some embodiments, the porous composite particles exhibit a volume average particle size in the range of about 0.2 microns to about 20 microns as measured using scanning electron microscope (SEM) image analysis or particle scattering techniques on a powder comprising the porous composite particles.

[0028] In some embodiments, the Raman spectrum of the porous composite particles exhibits carbon D and G peaks, with the ratio of the average intensities of the D and G peaks (ID / IG) ranging from about 0.7 to about 2.7.

[0029] In one embodiment, a Li-ion battery includes an anode comprising a lithium-ion battery anode composition, a cathode electrically isolated from the anode, and an electrolyte ionically connecting the anode and the cathode.

[0030] In some embodiments, the battery capacity ranges from about 0.2 Ah to about 400 Ah.

[0031] In some embodiments, R(r=rSi-C) is the value of the radial distribution function R(r) at the real space position of the first coordination sphere of the Si-C pair in the porous composite particle, and R(r=rC-C) is the value of the radial distribution function R(r) at the real space position of the first coordination sphere of the C-C pair in the porous composite particle, and the radial distribution function R(r) and the atomic pair correlation function are expressed as R(r)=G(r)r+4πr 2 They are related by ρ0, which is a constant related to the number density of the scatterers, and the ratio R(r=rSi-C) / R(r=rC-C) ranges from 0.050 to approximately 1.000.

[0032] In one aspect, a carbon material for use in making an anode composition for use in a Li-ion battery, the carbon material is characterized by a domain size (r) as estimated from an atomic pair distribution function G(r) obtained from synchrotron X-ray diffraction measurement of the carbon material ranging from about 10 Å (1 nm) to about 60 Å (6 nm).

[0033] In some embodiments, the domain size (r) corresponds to one of the following: (1) a first domain size ranging from about 15 Å to about 19 Å, (2) a second domain size ranging from about 19 Å to about 22 Å, (3) a third domain size ranging from about 24 Å to about 28 Å, and (4) a fourth domain size ranging from about 40 Å to 55 Å.

[0034] In some embodiments, the carbon material comprises porous carbon.

[0035] In some embodiments, G(r=r1) is the value of the atomic pair correlation function at a real space position in the first coordination sphere of the carbon material, G(r=r2) is the value of the atomic pair correlation function at a real space position in the second coordination sphere of the carbon material, and the ratio G(r=r1) / G(r=r2) is in the range of about 0.700 to about 0.590.

[0036] In some embodiments, W(r=r1) is the value of the full width at half maximum of the atomic pair correlation function at a real space position in the first coordination sphere of the carbon material, W(r=r2) is the value of the full width at half maximum of the atomic pair correlation function at a real space position in the second coordination sphere of the carbon material, and the ratio W(r=r1) / W(r=r2) is in the range of about 0.700 to about 0.850.

[0037] In some embodiments, G(r=r1) is the value of the atomic pair correlation function at a real space position in the first coordination sphere of the carbon material, G(r=r3) is the value of the atomic pair correlation function at a real space position in the third coordination sphere of the carbon material, and the ratio G(r=r1) / G(r=r3) is in the range of about 1.100 to about 1.300.

[0038] In some embodiments, W(r=r1) is the value of the full width at half maximum of the atomic pair correlation function at a real space position in the first coordination sphere of the carbon material, W(r=r3) is the value of the full width at half maximum of the atomic pair correlation function at a real space position in the third coordination sphere of the carbon material, and the ratio W(r=r1) / W(r=r3) is in the range of about 0.600 to about 0.850.

[0039] Other objects and advantages associated with the embodiments disclosed herein will become apparent to those skilled in the art upon review of the accompanying drawings and detailed description.

[0040] The accompanying drawings are presented to aid in the description of embodiments of the present disclosure and are provided solely to illustrate the embodiments, and not to limit them. Unless otherwise mentioned or implied by context, the various hatching, shading, and / or filling patterns in the drawings are merely meant to depict contrast between the various components, elements, features, etc., and do not convey the use of particular materials, colors, or other properties that may be defined outside of this disclosure with respect to the particular patterns employed. [Brief description of the drawings]

[0041] [Figure 1] FIG. 1 illustrates an example (e.g., Li-ion) battery to which the components, materials, and other techniques described herein, or combinations thereof, may be applied in accordance with various embodiments. [Figure 2A] 1 is a graphical plot of Si crystallite size as a function of the square root of the Raman D / G carbon peak intensity ratio for several carbon-based anode composite samples. [Figure 2B] 1 is a graphical plot of Si crystallite size as a function of temperature during one of the synthesis steps in making several carbon-based anode composite samples. [Figure 3A] 1 shows the X-ray diffraction patterns of two suitable porous carbon materials annealed at several vacuum annealing temperatures. [Figure 3B] 1 is an X-ray diffraction pattern of another suitable porous carbon material annealed at several vacuum annealing temperatures; [Figure 3C] FIG. 1 shows another example of a suitable porous carbon exhibiting (002) carbon spacing exceeding that of graphite. [Figure 4] 1 is a graphical plot of nitrogen uptake (change in mass) as a function of annealing temperature for carbon-containing composite powders. [Diagram 5] 4 is the X-ray diffraction patterns of suitable composite powders containing C and Si annealed in N2 at various temperatures. [Figure 6A] FIG. 1 shows a graphical plot of the atomic pair distribution function G(r) for several suitable carbon materials. [Figure 6B] FIG. 1 shows a graphical plot of the atomic pair distribution function G(r) for several suitable carbon materials. [Figure 7] FIG. 1 shows a graphical plot of the atomic pair distribution function G(r) for several suitable carbon materials. [Figure 8] FIG. 1 shows a graphical plot of the atomic pair distribution function G(r) for one suitable carbon material and two composite materials containing Si and C formed under various synthesis and processing conditions. [Figure 9A] FIG. 1 is a tabulated diagram of the ratio of peak amplitudes (values ​​of atomic pair distribution functions) of the first and second carbon-carbon coordination spheres for exemplary carbon materials. [Figure 9B] FIG. 1 shows the ratio of the full width at half maximum (FWHM) values ​​of the atomic pair correlation functions in the first and second carbon-carbon coordination spheres for an exemplary carbon material. [Figure 9C] FIG. 1 tabulates the ratio of peak amplitudes (values ​​of atomic pair distribution functions) of the first and third carbon-carbon coordination spheres for exemplary carbon materials. [Figure 9D] FIG. 1 shows the ratio of values ​​of FWHM of atomic pair correlation functions in the first and third carbon-carbon coordination spheres for an exemplary carbon material. [Figure 10] FIG. 1 shows a graphical plot of the atomic pair distribution function G(r) for a composite material containing carbon and silicon active materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0042] Aspects of the invention are disclosed in the following description and associated drawings directed to specific embodiments of the invention. The term "embodiments of the invention" does not require that all embodiments of the invention include the discussed features, advantages, processes, or modes of operation, and alternative embodiments may be devised without departing from the scope of the invention. Furthermore, well-known elements of the invention may not be described in detail or may be omitted so as not to obscure other more relevant details. Furthermore, the term "at least partially" is intended to be interpreted as "partially, substantially, or completely."

[0043] Any numerical range described herein with respect to any embodiment of the invention not only defines upper and lower bounds of the relevant numerical range, but also implicitly discloses each individual value within that range in units or increments consistent with the level of precision by which the upper and lower bounds are characterized. For example, a numerical distance range (i.e., a level of precision in one unit or increment) of 7 nm to 20 nm includes the set [7, 8, 9, 10, ..., 19, 20] (in nm), as if the intervening numbers 8 to 19 in one unit or increment were explicitly disclosed. In another example, a temperature range of about -120°C to about -60°C includes the set of temperature ranges of about -120°C to about -119°C, about -119°C to about -118°C, ..., about -61°C to about -60°C (in °C), as if the intervening numbers (in °C) between -120°C to -60°C in the incremental range were explicitly disclosed. In yet another example, a numerical percentage range from 30.92% to 47.44% (i.e., a level of precision in hundredths or increments) encompasses the set [30.92, 30.93, 30.94, ..., 47.43, 47.44] (units %), as if the intervening numerical values ​​between 30.92 and 47.44 in hundredths or increments were expressly disclosed. Thus, any of the intervening numerical values ​​encompassed by any disclosed numerical range shall be construed as if those intervening numerical values ​​were expressly disclosed, and any such intervening numerical values ​​may thereby constitute upper and / or lower bounds of a subrange that is included within its own broader range. Each subrange (e.g., each range that includes at least one intervening numerical value from the broader range as an upper and / or lower bound) shall thereby be construed as being implicitly disclosed by the descriptive disclosure of the broader range.

[0044] The following description may describe certain embodiments in the context of Li metal and Li ion batteries (for simplicity and convenience, and due to the current popularity of Li technology), however, various embodiments may also be used with other rechargeable primary batteries (e.g., Na metal and Na ion, Mg metal and Mg ion, K metal and K ion, Ca metal and Ca ion, and other metal and metal ion batteries, OH - It will be appreciated that the present invention may be applicable to a variety of devices, including batteries with different ions (such as alkaline batteries, mixed ion batteries, etc.), as well as electrochemical capacitors or hybrid devices (e.g., one electrode is battery-like and another electrode is electrochemical capacitor-like).

[0045] Although the following description may describe certain examples in the context of active ions contained within active particles, it will be understood that various aspects may be applicable to active ions present in an electrolyte at some stage of cell assembly or charging / discharging.

[0046] Additionally, although the following description may be described in terms of certain examples of active material formulations in a Li-containing (e.g., lithiated) state, it will be understood that various embodiments may be applicable to Li-free (e.g., non-lithiated) electrodes.

[0047] Additionally, although the following description may describe certain examples of active electrode materials belonging to so-called conversion type active material(s) (including so-called alloy type active materials, true conversion type active materials, chemical conversion type active materials, metal active materials, etc.), it will be understood that various aspects may be applicable to so-called intercalation type active material(s), so-called pseudocapacitive active materials, as well as mixed type active materials (or active material components) that may store charge by multiple mechanisms (e.g., active materials that exhibit both intercalation and conversion type electrochemical reactions during cell operation, among many other combinations).

[0048] Additionally, although the following description may describe certain specific examples of active (reversibly ion-storing) materials (as component(s) of (nano)composites) in the form of crystalline (or nanocrystalline) materials, it will be understood that various aspects are applicable to highly ordered or amorphous active materials.

[0049] Additionally, the following description is not limited to carbon-based (e.g., less than about 10 atomic % sp 2 In some designs, less than about 1 atomic percent sp 2 Although certain specific examples of active (reversibly ion-storing) materials may be described, such as carbon materials (90-100 atomic % sp 2 It will also be appreciated that materials containing carbon-containing composites (including materials containing bonded carbon) may reversibly store ions over certain potential ranges of battery operation (but generally exhibit substantially smaller volumetric and gravimetric capacities for ion storage). Thus, when discussing active materials in various embodiments of the present disclosure, the active material in a carbon-containing composite may be characterized as a material that is "substantially more active than carbon" (e.g., stores at least twice as many ions per atom of "active" material than carbon over an operable electrochemical potential range).

[0050] Additionally, while the following description may describe certain examples of particular sources (precursors) of carbon materials, it will be understood that various aspects may be applicable to other types of carbon material sources, including those produced from both organic and inorganic precursors, those that utilize templates (e.g., sacrificially) for the formation of some of the pores, and those that utilize organic waste products, among others.

[0051] Furthermore, although the following description may describe certain examples of (nano)composite particles or porous carbon particles having irregular or spherical or spheroidal three-dimensional (3D) shapes, it will be understood that the description is applicable to particles having a variety of shapes, including, for example, elongated, two-dimensional (2D, such as (nano)composite platelets or porous carbon sheets) or one-dimensional (1D, such as (nano)composite nanofibers and fibers or porous carbon nanofibers and fibers) shapes.

[0052] Furthermore, although the following description may also describe certain specific examples of liquid organic electrolytes as components of electrochemical cells (batteries or electrochemical capacitors) based on (nano)composite electrodes, it will be understood that various embodiments may be applicable to aqueous electrolytes, ionic salt electrolytes, molten salt electrolytes, solid ceramic electrolytes, solid glass electrolytes, solid polymer electrolytes (including single-ion conducting solid polymer electrolytes in which one ion (e.g., cation) is mobile while the counter ion (e.g., anion) is chemically bound to the polymer backbone), gel electrolytes, composite (e.g., glass-ceramic or glass-polymer or ceramic-polymer or liquid-ceramic-polymer or liquid-glass-polymer or liquid-glass-ceramic-polymer) electrolytes, and others. In some designs, multiple electrolytes may be used in a single cell structure (e.g., one electrolyte infiltrated / coating the surface of the electrode or active material, and another electrolyte interpenetrating the remaining pores of the electrode(s) or comprising at least a portion of the separator membrane; or, as another illustrative example, one electrolyte in contact with the anode and another electrolyte in contact with the cathode).

[0053] In some embodiments and designs, a solid (at device operating temperature) electrolyte may melt infiltrate at least some of the pores in the electrodes (e.g., at an elevated temperature where the electrolyte becomes liquid). In some embodiments and designs, a solid (at device operating temperature) electrolyte may be dissolved in a solvent and infiltrate at least some of the pores of the electrodes, followed by solvent evaporation (drying). In some embodiments and designs, a solid (at device operating temperature) electrolyte may infiltrate at least some of the pores of the electrodes, at an intermediate stage where such electrolyte is liquid, and then converted from liquid to solid. In some embodiments and designs, a polymer electrolyte may infiltrate at least some of the pores or active material in the electrolyte in a liquid state, and may be polymerized after infiltration (e.g., during heating, or after sufficient storage or UV treatment in an appropriate temperature range, etc.). In some designs, such polymerization may occur before cell use (application). In some designs, such polymerization may occur after cell assembly (e.g., or as a final stage thereof). In some designs, such polymerization may occur after cell sealing (e.g., as a final stage thereof). At some stages, the remaining pores (if any) after polymerization may be filled with another electrolyte for a fully assembled device (such as a Li-ion battery cell).

[0054] During battery (such as Li-ion batteries) operation, intercalation-type active materials operate by the insertion (intercalation) and extraction (deintercalation) of Li-ions into / from interstitial sites (nanoscale or sub-nanoscale voids) present in the crystalline or disordered or completely amorphous structures of such intercalation compounds. This intercalation / deintercalation process is accompanied by a change in the oxidation state of non-Li atoms (ions) (e.g., transition metal ions). Chemical bonds are typically not broken or reformed during such processes. Li-ions diffuse into / out of the active material.

[0055] During operation of a battery (such as a Li-ion battery), the conversion material changes (converts) from one crystal structure to another (hence the name "conversion" type). During operation of a (e.g., Li-ion) battery, Li ions are inserted into the alloy-type material (hence the name "alloy" type) forming a lithium alloy. Sometimes "alloy" type electrode materials (generally metals and metalloids) are considered a subclass of "conversion" type electrode materials. Known examples of "alloy" type active electrode materials suitable for metal-ion (e.g., Li-ion or Na-ion) batteries may include, but are not limited to, silicon (Si), tin (Sn), antimony (Sb), germanium (Ge), various alloys thereof, and combinations thereof, among others.

[0056] "Alloy" type electrode materials may contain other type(s) of conversion material (e.g., oxides, hydrides, nitrides, etc.) as additives in small amounts (e.g., about 0.1% to 50% by weight) as well as less active materials (which may represent significantly lower, e.g., about 0.01% to 30% of the alloy material weight capacity) that may help to increase the mechanical or electrochemical stability of the alloy materials or increase their electrical conductivity in the delithiated state (these may be intercalation type materials). The electrochemical reaction process between Li-ions and the alloy or conversion material may involve the destruction of some of the original chemical bonds and the formation of new chemical bonds. In the ideal case for some designs, the process is somewhat reversible, and only little (or no) loss of active material (or Li) occurs during battery operation (e.g., preferably no more than about 30% during the life of the battery).

[0057] While the following description may describe certain specific examples in the context of metal-ion batteries, other conversion type electrodes that may benefit from various aspects of the present disclosure include various chemistries used in a wide range of aqueous batteries, such as alkaline batteries, metal hydride batteries, lead acid batteries, etc. These include, but are not limited to, various metals (e.g., iron, zinc, cadmium, lead, indium, etc.), metal oxides, metal hydroxides, metal oxyhydroxides, and metal hydrides, to name a few.

[0058] FIG. 1 illustrates an example metal or metal-ion (e.g., Li or Li-ion) battery to which the components, materials, methods, and other techniques described herein, or combinations thereof, may be applied according to various embodiments. For illustrative purposes, a cylindrical battery is shown here, but other types of configurations, including prismatic or pouch (laminated) batteries, may be used as desired. The example battery 100 includes an anode 102, a cathode 103, a separator 104 interposed between the anode 102 and the cathode 103, an electrolyte (not shown) impregnated in the separator 104 (and typically impregnating both the anode 102 and the cathode 103), a battery case 105, and a sealing member 106 that seals the battery case 105. In some designs in the case of solid electrolyte(s), a solid electrolyte membrane may serve as the separator 104.

[0059] Both liquid and solid electrolytes may be used in the designs herein. Conventional electrolytes for Li or Na-based batteries of this type generally consist of a single Li or Na salt (such as LiPF6 for Li-ion batteries, and NaPF6 or NaClO4 salts for Na-ion batteries) in a mixture of organic solvents (such as a mixture of carbonates). Other common organic solvents that may be suitable in the context of one or more embodiments of the present disclosure include nitriles, esters, sulfones, sulfoxides, phosphorus-based solvents, silicon-based solvents, ethers, and others. In some designs, some of such solvents may be modified (e.g., sulfonated or fluorinated). The electrolyte may include an ionic liquid (in some designs, a neutral ionic liquid; in other designs, an acidic or basic ionic liquid). In some designs, a suitable electrolyte may include a mixture of various salts (e.g., a mixture of several Li salts or a mixture of Li and non-Li salts for rechargeable Li and Li-ion batteries). The most common salt used in certain conventional Li-ion battery electrolytes is, for example, LiPF, but less common salts that may be suitable in the context of one or more embodiments of the present disclosure include lithium tetrafluoroborate (LiBF), lithium perchlorate (LiClO), lithium bis(oxalato)borate (LiB(C2O4)2), lithium difluoro(oxalato)borate (LiBF2(C2O4)), various lithium imides (SO2FN), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium bis(oxalato)borate (LiB(C2O4)), lithium difluoro(oxalato)borate (LiBF2 ... - (Li + )SO2F, CF3SO2N - (Li + )SO2CF3, CF3CF2SO2N - (Li + )SO2CF3, CF3CF2SO2N - (Li + )SO2CF2CF3, CF3SO2N - (Li + )SO2CF2OCF3, CF3OCF2SO2N - (Li + )SO2CF2OCF3, C6F5SO2N - (Li + )SO2CF3, C6F5SO2N- (Li + )SO2C6F5, or CF3SO2N - (Li + )SO2PhCF3, and others). Electrolytes for Mg-ion, K-ion, Ca-ion, and Al-ion batteries are more unusual as these batteries are in the early stages of development. These unusual electrolytes may contain a variety of salts and solvents (in some cases ionic liquids are substituted for organic solvents for certain applications). In some designs, multiple Li salts may be advantageously used in the electrolyte. In some designs, electrolytes for Li-ion batteries may advantageously contain non-Li salt(s).

[0060] For aqueous Li-ion (or aqueous Na-ion, K-ion, Ca-ion, etc.) batteries, a suitable electrolyte may include a solution (e.g., an aqueous solution or a mixed aqueous-organic solution) of inorganic Li (or Na, K, Ca, etc.) salt(s) (e.g., Li2SO4, LiNO3, LiCl, LiBr, Li3PO4, H2LiO4P, C2F3LiO2, C2F3LiO3S, Na2O3Se, Na2SO4, Na2O7Si3, Na3O9P3, C2F3NaO2, etc.). In some designs, these electrolytes are solutions of organic Li (or Na, K, Ca, etc.) salts, such as metal salts of carboxylic acids (enumerated for Li for simplicity) (e.g., HCOOLi, CH3COOLi, CH3CH2COOLi, CH3(CH2)2COOLi, CH3(CH2)3COOLi, CH3(CH2)4COOLi, CH3(CH2)5COOLi, CH3(CH2)6COOLi, CH3(CH2)7COOLi, CH3(CH2)8COOLi, CH3(CH2)9COOLi, CH3(CH2) 10 COOLi, CH3 (CH2) 11 COOLi, CH3 (CH2) 12 COOLi, CH3 (CH2) 13 COOLi, CH3 (CH2) 14 COOLi, CH3 (CH2) 15 COOLi, CH3 (CH2) 16 COOLi, CH3 (CH2)17 COOLi, CH3 (CH2) 18 COOLi, and others having the formula CH3(CH2)xCOOLi, where x ranges up to 50; metal salts of sulfonic acids (e.g., RS(=O)2-OH, where R is a metal salt of an organic group, such as CH3SO3Li, CH3CH2SO3Li, C6H5SO3Li, CH3C6H4SO3Li, CF3SO3Li, [CH2CH(C6H4)SO3Li] n , and others) and other organometallic reactants (such as various organolithium reagents). Such solutions may include mixtures of inorganic and organic salts, mixtures of various other salts (e.g., mixtures of Li salts and salts of non-lithium metals and metalloids), in some cases hydroxide(s) (e.g., LiOH, NaOH, KOH, Ca(OH)2, etc.), and in some cases acids (including organic acids). In some designs, such aqueous electrolytes may include neutral or acidic or basic ionic liquids (about 0.00001 wt % to about 40 wt % based on the total weight of the electrolyte). In some designs, such "aqueous" (or water-containing) electrolytes may include, in addition to water, an organic solvent (about 0.00001 wt % to about 40 wt % based on the total weight of the electrolyte). Illustrative examples of suitable organic solvents may include carbonates (e.g., propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, fluoroethylene carbonate, vinylene carbonate, and the like), various nitriles (e.g., acetonitrile, and the like), various esters, various sulfones (e.g., propane sulfone, and the like), various sultones, various sulfoxides, various phosphorus-based solvents, various silicon-based solvents, various ethers, and the like.

[0061] Some electrolytes in some aqueous batteries (such as alkaline batteries, including nickel metal hydride batteries, among others) may include an alkaline solution (e.g., a mixture of KOH and LiOH solutions). Some electrolytes in aqueous batteries (such as lead-acid batteries) may include an acidic aqueous solution (e.g., an H2SO4 aqueous solution or an HCl aqueous solution). Some electrolytes in aqueous batteries may include an organic solvent as an additive. Some electrolytes in aqueous batteries may include two or more organic solvent(s) or ionic liquid(s) or surfactant(s) as additive(s) or substantial components of the electrolyte.

[0062] Conventional electrodes utilized in Li or Li-ion batteries may be produced by (i) forming a slurry containing active material, conductive additives, a binder solution, and possibly surfactants or other functional additives; (ii) casting the slurry onto a metal foil (e.g., Cu foil for most anodes used in Li or Li-ion batteries, and Al foil for most cathodes used in Li or Li-ion batteries and high potential anodes used in Li-ion batteries, such as lithium titanate); (iii) drying the cast slurry until the solvent is completely evaporated; and (iv) densifying the electrode, if necessary (e.g., by pressure calendaring). Instead of using such solvent-based processes for electrode fabrication, some designs may be advantageous to use dry electrode processing (solvent-free), including but not limited to electrostatic coating.

[0063] Some aspects of the present disclosure deal with the formation of carbon-containing composite electrode materials. A wide range of suitable active materials may be utilized in such composite electrode materials, illustrative examples of which are described below.

[0064] Conventional cathode materials utilized in Li and Li-ion batteries may be of the intercalation type, whereby metal ions are intercalated and occupy interstitial sites of such materials during charging and discharging of the battery. Such cathode materials typically experience very small volume changes (e.g., about 0.1-8 vol%) when used in battery electrodes during charging and discharging. Such cathode materials typically have high densities (e.g., about 3.8-6 g / cm 3 ) and are relatively easy to mix into a slurry. Polyvinylidene fluoride or polyvinylidene difluoride (PVDF) is one of the most common binders used in these electrodes. Carbon black is the most common conductive additive used in these electrodes. However, such cathodes exhibit relatively low gravimetric and volumetric reversible capacities (e.g., less than about 200-220 mAh / g and about 1000 mAh / cm, respectively). 3 less than).

[0065] Illustrative examples of suitable intercalation-type active cathode materials that may be utilized in the context of the present disclosure for Li or Li-ion cells include, but are not limited to: lithium nickel cobalt aluminum oxide (NCA - e.g., LiNi 0.8 Co 0.15 Al 0.05 O2, or LiNi x Co y Al z Lithium nickel cobalt manganese aluminum oxide (NCMA), lithium nickel oxide (LNO--e.g., LiNiO2 or others that may contain metals other than Ni for enhanced stability), various lithium manganese oxides (LMO--e.g., LiMnO2 or LMO, or Li2MnO3, or LiMn2O4, among others), various lithium nickel manganese cobalt oxides (NCM--e.g., LiNi 0.33 Co 0.33 Mn 0.33O2, or LiNi 0.8 Co 0.1 Mn 0.1 O2 or, more commonly, LiNi x Co y Mn z O2, where typically x+y+z≦1, or NCM, or NMC), various lithium nickel manganese oxides (LiNi 0.5 Mn 0.5 O2, LiNi 0.25 Mn 0.75 O2 or LiNi x Mn y O2, where typically x+y≦1; LiNi 0.5 Mn 0.15 O4 or LiNi x Mn y Lithium cobalt oxide (LCO--e.g., in the form of LiCoO2 or LiCo2O4, which may contain metals other than Co for enhanced performance or reduced cost), lithium cobalt aluminum oxide (LCAO), lithium manganese phosphate (LMP), lithium titanium sulfite (LiTiS2), or lithium iron phosphate (LiFePO4, LFP), lithium manganese phosphate (LiMnPO4), lithium manganese iron phosphate (LMFP), lithium cobalt phosphate (LiCoPO4), lithium nickel phosphate (LiNiPO4), lithium vanadium fluorophosphate (LiVFPO4), lithium iron fluorosulfate (LiFeSO4F), various Li-rich materials (e.g., lithium-rich (including rock salt) transition metal oxides and oxyfluorides, e.g., Li 1.211 Mo 0.467 Cr 0.3 O2, Li 1.3 Mn 0.4 Nb 0.3 O2, Li 1.2 Mn 0.4 Ti 0.4 O2, Li 1.2 Ni0.333 Ti 0.333 Mo 0.133 O2, and many others), various high capacity Li-ion based materials with partial substitution of fluorine or iodine for oxygen (e.g., rock salt Li2Mn 2 / 3 Nb 1 / 3 O2F, Li2Mn 1 / 2 Ti 1 / 2 O2F, Li 1.5 Na 0.5 MnO 2.85 I 0.12 ), and many other types of Li-containing disordered rock salts (including cation-disordered rock salts), layered, taborite, olivine, or spinel type active materials or mixtures thereof that contain at least oxygen or fluorine or sulfur and at least one transition metal, and other lithium transition metal (hereinafter "TM" e.g., Mn, Ni, Co, Nb, Ti, Ta, Fe, V, Mo, etc.) oxide or phosphate or sulfate (or mixed) cathode materials, relying on the intercalation of lithium (Li) and the change in the TM oxidation state. In some designs, such materials may be doped or heavily doped. In addition to Li-based intercalation type active materials, other examples of intercalation type active materials may be based on (e.g., similar) Na-ion intercalation compounds, K-ion intercalation compounds, Ca-ion intercalation compounds, among others. In addition to Li-containing (or Na-containing, K-containing, Ca-containing, etc.) intercalation compounds, Li-free (or Na-free, K-free, Ca-free, etc.) variety(s) of such or similar materials may be utilized (e.g., titanium oxide or oxyfluoride, niobium oxide or oxyfluoride, cobalt oxide or oxyfluoride, nickel oxide or oxyfluoride, nickel aluminum oxide or oxyfluoride, nickel cobalt manganese oxide or oxyfluoride, nickel cobalt aluminum oxide or oxyfluoride, iron oxide or oxyfluoride, iron phosphate, many others, and various mixtures thereof, etc.).

[0066] Some of such active intercalation materials may experience gradients in composition or core-shell particle morphology. Some of such materials may be partially fluorinated or may contain some significant percentage of fluorine (e.g., about 0.001-10 atomic %) in their composition. In some designs, in high voltage lithium transition metal oxide (or phosphate or sulfate or mixture or other) cathodes, TM and oxygen (O) are covalently bonded and both TM and O are oxidized in an electrochemical reduction-oxidation (redox) reaction during charging and discharging (including but not limited to oxide or phosphate or sulfate or mixed cathodes that may contain at least about 0.25 atomic % Mn, Fe, Ni, Co, Nb, Mg, Cr, Mo, Zr, W, Ta, Ti, Hf, Y, Sc, La, Sb, Sn, Si, or Ge). Note that Sc, Y, and various lanthanides may often be considered "inner transition metals."

[0067] In addition to or instead of intercalation type active materials, some designs of the present disclosure may include so-called pseudocapacitive (or mixed pseudocapacitive intercalation type) active materials. Suitable examples of pseudocapacitive (or mixed pseudocapacitive intercalation type) active materials include, but are not limited to, various (including mixed metal) oxides, hydroxides, oxyhydroxides, nitrides, oxynitrides, nitrates, phosphates, (oxy)phosphates, sulfides, sulfates, hydroxides, and other inorganic salts of Ru, Fe, Mn, Cu, Ti, Bi, V, Ni, Nb, Ce, Zr, Ta, Co, Sn, Sb, Si, In, Zn, Mo, Pb, La, Y, and various mixtures and derivatives thereof. Such compounds may include Li, Na, Ca, Cs, Mg, and K. In some designs, such compounds may include two, three, four, or more metals. In some designs, such compounds may include at least one transition metal.

[0068] Conventional anode materials utilized in Li-ion batteries are also of the intercalation type, whereby metal ions intercalate and occupy interstitial sites of such materials during charging and discharging of the battery. Such anodes undergo small or very small volume changes when used in electrodes (e.g., about 0.05-10% by volume). However, such anodes exhibit relatively small gravimetric and volumetric reversible capacities (typically less than about 200 mAh / g for lithium titanate (LTO), typically less than about 370-400 mAh / g for lithium vanadate, graphite or hard carbon-based anodes, and about 600 mAh / cm at the electrode level, not counting the volume of the current collector foil. 3 (Rechargeable volume capacity is less than 1000mAh).

[0069] Conversion-type active cathode materials can provide significantly higher specific capacity than intercalation-type materials. Suitable examples of these include, but are not limited to, metal fluorides, chlorides, sulfides, selenides, various mixtures, composites, and others. For example, fluoride-based cathodes can provide significantly higher specific capacity than intercalation-type materials, in some cases exceeding about 300 mAh / g (about 1200 mAh / cm at the electrode level) due to their very high capacity. 3These materials may offer extraordinary technological potential due to their capacity (greater than 1000 mAh / g). For example, in the absence of Li, FeF3 provides a theoretical specific capacity of 712 mAh / g; FeF2 provides a theoretical specific capacity of 571 mAh / g; MnF3 provides a theoretical specific capacity of 719 mAh / g; CuF2 provides a theoretical specific capacity of 528 mAh / g; NiF2 provides a theoretical specific capacity of 554 mAh / g; PbF2 provides a theoretical specific capacity of 219 mAh / g; BiF3 provides a theoretical specific capacity of 302 mAh / g; and BiF5 provides a theoretical specific capacity of 1000 mAh / g. 441mAh / g; SnF2 provides a theoretical specific capacity of 342mAh / g; SnF4 provides a theoretical specific capacity of 551mAh / g; SbF3 provides a theoretical specific capacity of 450mAh / g; SbF5 provides a theoretical specific capacity of 618mAh / g; CdF2 provides a theoretical specific capacity of 356mAh / g; ZnF2 provides a theoretical specific capacity of 519mAh / g; AlF3 also provides a high theoretical specific capacity, but at a low lithiation potential. AgF and AgF2 also provide a high theoretical specific capacity and also exhibit very high lithiation potentials. Mixtures of fluorides (e.g., in the form of alloys) can typically provide theoretical capacities that are approximately calculated according to the law of mixtures. The use of mixed metal fluorides can sometimes be advantageous (e.g., can provide higher rates, lower resistance, higher actual capacity, or longer stability). The use of metal fluorides mixed with the metal can sometimes be advantageous (e.g., can provide higher rates, lower resistance, higher actual capacity, or longer stability). In the fully lithiated state, the metal fluoride converts to a composite containing a mixture of metal and LiF clusters (or nanoparticles). Examples of totally reversible reactions of conversion-type metal fluoride cathodes may include 2Li+CuF2⇔2LiF+Cu for a CuF2-based cathode, or 3Li+FeF3⇔3LiF+Fe for a FeF3-based cathode. It will be understood that metal fluoride-based cathodes can be prepared without Li or in a partially lithiated or fully lithiated state.In addition to fluorides, other illustrative examples of converted active electrode materials include, but are not limited to, various metal oxy-fluorides, sulfo-fluorides, chloro-fluorides, oxy-chloro-fluorides, oxy-sulfo-fluorides, fluoro-phosphates, sulfo-phosphates, sulfo-fluoro-phosphates, mixtures and salts of metals (e.g., Fe, Cu, Ni, Co, Bi, Cr, other metals, various mixtures and alloys thereof, partially oxidized metals and metal alloys, etc.) (metal fluorides (including LiF or NaF), metal chlorides (including LiCl or NaF), metal oxy-fluorides, metal oxides, metal sulfo-fluorides, metal fluoro-phosphates, metal sulfides, metal oxy-sulfo-fluorides, various combinations thereof, etc.), and other salts containing halogens or sulfur or oxygen or phosphorus or combinations of these elements, among others. In some designs, F in the metal fluoride may be fully or partially replaced with another halogen (e.g., Cl or Br or I, etc.) or mixtures thereof to form the corresponding metal chloride or metal fluoride-chloride and other metal halide compositions. In some designs, the metal halide may be at least partially dissolved in the electrolyte. In some designs, at least a portion of the active material may be stored in liquid form (e.g., in the electrolyte).

[0070] Yet another example of a potential modified cathode (or, in some cases, anode) material is sulfur (S) (in the absence of Li) or lithium sulfide (LiS, fully lithiated). In some designs, selenium (Se) may be used together with S or by itself to form such cathode active materials.

[0071] In some designs, the conversion active cathode material may advantageously comprise a metal oxide or mixed metal oxide. In some designs, such (nano)composite may advantageously comprise a metal sulfide or mixed metal sulfide. In some examples, the mixed metal oxide or mixed metal sulfide may comprise lithium. In some examples, the mixed metal oxide may comprise titanium or vanadium or manganese or iron metal. In some examples, the lithium-containing metal oxide or metal sulfide may exhibit a layered structure. In some examples, the metal oxide or mixed metal oxide or metal sulfide or mixed metal sulfide may advantageously be ionically and electrically conductive (e.g., at about 10 -7 About 10 +4 In some embodiments, various other intercalation active materials may be utilized in place of or in addition to the metal oxides or metal sulfides. In some designs, such intercalation active materials may be utilized in a potential range close to that of S or Li2S (e.g., in the range of about 1.5 to 3.8 V vs. Li / Li + in the range), charge storage (e.g., Li insertion / extraction capacitance).

[0072] In some designs, the use of so-called Li-air cathodes (e.g., cathodes with active materials whose lithiation states are in the form of Li2O2, Li2O, LiOH), or similar metal-air cathodes based on Na, K, Ca, Al, Fe, Mn, Zn, and other metals (instead of Li), can be beneficial as well, due to their very high capacity. In some designs, such cathode active materials should ideally react reversibly with oxygen or oxygen-containing species in the electrochemical cell and can be completely lost upon complete delithiation (metal removal). These are also considered to belong to the conversion type cathodes.

[0073] Conversion type anode: nLi+M a X b ⇔aM+bLi nThrough reactions occurring with X, where M may be a metal or semimetal (intermetallic), and X is an anion (e.g., O for the anode, but may also be N, S, P, F, etc.) or hydrogen (H), they may provide much higher specific capacity than graphitic carbon. Suitable examples of such conversion-type active anode materials include, but are not limited to, various oxides, nitrides, sulfides, phosphides, fluorides, hydrides, etc. In some designs, these may include, among others, fully or partially oxidized non-carbon Group IV elements (e.g., oxides or nitrides or sulfides or phosphides of Si, Ge, Sn, or Pb), or fully or partially (e.g., oxides or nitrides or sulfides or phosphides) of Al, Ga, In, Sb, Bi, Fe, Ti, Mn, Cu, Ni, Co, V, and Zn.

[0074] Alloy-type active materials are sometimes considered a subclass of conversion-type active anode materials. The alloy-type materials used in Li-ion batteries also offer higher gravimetric and volumetric capacity compared to intercalation-type anodes. The alloy-type active anode materials may also offer lower irreversible first cycle losses compared to the conversion-type anode materials mentioned above (such as various oxides, nitrides, sulfides, phosphides, or hydrides). For example, earth-abundant silicon (Si) offers about 10 times higher gravimetric capacity and about 3 times higher volumetric capacity compared to intercalation-type graphite (or carbonaceous soft carbon, hard carbon, or graphite-like) anodes. In some designs, "Si-based" active materials may include Si, or Si doped or heavily doped with nitrogen (N), phosphorus (P), boron (B), or other elements, or alloyed with various other metals. As mentioned above, in addition to Si-based active materials, other Si-containing active materials, such as silicon oxide (SiO x ) or silicon oxynitride (SiO x N y ) or silicon nitride (SiN y) or hydrides, or other active materials containing the element Si (including those partially reduced by Li or Mg), and metal alloys containing Si may be utilized (e.g., some Si-containing active materials contain Si atoms in their composition, such as in Si-based ceramics or metal alloys, but are not considered Si-based in this context, and Si-based active materials generally encompass doped, heavily doped, or undoped Si). These Si-containing active materials offer lower capacity but reduced volume change relative to Si-based active materials, and typically improve cycling stability, but generally at the expense of higher first cycle loss or faster degradation or both. In addition to Si-based or (non-Si-based) Si-containing active anode materials, other examples of such high capacity (e.g., nanocomposite) anodes containing alloy-type (or, more broadly, conversion-type) active materials include, but are not limited to, those based on or containing germanium (Ge), antimony (Sb), aluminum (Al), magnesium (Mg), zinc (Zn), gallium (Ga), arsenic (As), phosphorus (P), silver (Ag), cadmium (Cd), indium (In), tin (Sn), lead (Sb), bismuth (Bi), various mixtures and alloys thereof (particularly by themselves or with Si or other "inert" metals, such as iron (Fe) or copper (Cu)), and others. Similarly, such materials may be doped or heavily doped and may take the form of oxides, oxynitrides, nitrides, hydrides, or compounds containing other metals or metalloids.

[0075] Alloy-type active anode materials are sometimes considered a subclass of conversion-type active anode materials. Alloy-type active anode materials used in Li-ion batteries also provide higher gravimetric and volumetric capacity compared to intercalation-type anodes. Alloy-type active anode materials may also provide lower irreversible first cycle losses compared to the conversion-type anode materials mentioned above (e.g., various oxides, nitrides, sulfides, phosphides, or hydrides, etc.). For example, earth-abundant silicon (Si) provides about 10 times higher gravimetric capacity and about 3 times higher volumetric capacity compared to intercalation-type graphite (or carbonaceous soft carbon, hard carbon, or graphite-like) anodes. In some designs, as mentioned above, "Si-based" active materials may include Si or Si doped or heavily doped with nitrogen (N), phosphorus (P), boron (B), or other elements, or may be alloyed with various other metals. In addition to Si-based materials, other Si-containing active materials, such as silicon oxide (SiO x ) or silicon oxynitride (SiO x N y ) or silicon nitride (SiN y) or hydrides or alloys containing Si or other active materials containing Si element (including those partially reduced with Li or Mg) may be utilized. These Si-containing active materials offer lower capacity but reduced volume change relative to Si-based active materials and typically improve cycling stability, but generally at the expense of higher first cycle loss or faster degradation or both. In addition to Si-based or (non-Si-based) Si-containing active anode materials, other examples of such high capacity (e.g., nanocomposite) anodes, including alloy-type (or, more broadly, conversion-type) active materials, include, but are not limited to, those based on or including germanium (Ge), antimony (Sb), aluminum (Al), magnesium (Mg), zinc (Zn), gallium (Ga), arsenic (As), phosphorus (P), silver (Ag), cadmium (Cd), indium (In), tin (Sn), lead (Sb), bismuth (Bi), various mixtures and alloys thereof (particularly those based on or including Si or other "inert" metals, such as iron (Fe) or copper (Cu)), and others. Similarly, such materials may be doped or heavily doped and may take the form of oxides, oxynitrides, nitrides, hydrides, or compounds containing other metals or metalloids.

[0076] In some designs, pure Li metal may be used as the active anode material in some embodiments of the present disclosure (e.g., used in combination with a porous carbon material in the anode). In some designs, such anodes may advantageously include other material(s) in addition to carbon and lithium metal (e.g., alloyed or converted anode materials, polymers, etc.). In some designs, such composites may be in the form of particles cast and formed into an electrode using a binder by a suitable mechanism. In some designs, such Li metal-C composite anodes may be at least partially formed during the first charge (after cell construction) using metal ions (e.g., Li ions) from a Li-containing cathode active material. For example, Li metal may be plated (electrodeposited) within the pores of a suitable carbon during the first charge. In some designs, it may be advantageous for at least a portion of such pores (e.g., about 10-100% of the pores) to remain free from the electrolyte and available for Li metal deposition during cell operation. In some designs, the pores in a suitable porous carbon may be closed by forming a shell around the porous carbon (and / or by incorporating a material that plugs the pores) before or after electrode fabrication. In some designs, a solid electrolyte (e.g., polymer or inorganic or polymer-inorganic composite) may be advantageously utilized to reduce side reactions, reduce first cycle capacity loss, reduce Li dendrite formation, and / or improve cell safety.

[0077] A wide range of alloy-type, metal, conversion-type active anode and cathode materials, as well as intercalation-type and pseudocapacitive-type active anode and cathode materials, may be successfully utilized in the context of the present disclosure. In some designs, such materials may be utilized in the formation of carbon-containing composites. In some designs (e.g., when the active material is loaded into the composite particles or into the electrode prior to assembly of the electrode into a cell), the active anode and cathode materials may exhibit a thermal conductivity of about 10 at about 400 K. -10 torr (preferably about 10 at 400K) -13It may be advantageous to use active materials that have a partial vapor pressure (less than 1000 psi torr). For example, in some designs, the electrodes may need to be dried at about 400 K prior to cell assembly; significant evaporation of the active materials may severely reduce the uniformity of the electrodes and the resulting cell performance as well as induce contamination and create safety hazards. In some designs, the electrodes may be assembled from the electrode composition (e.g., including composite particles) while in a discharged state.

[0078] In some designs, in the context of the present disclosure, the following polymer binders may be successfully used in electrodes including intercalation or conversion or mixed anode materials: polyvinylidene fluoride, or polyvinylidene difluoride (PVDF), various salts of carboxymethyl cellulose (CMC), such as Na-CMC and others, styrene-butadiene rubber (SBR), xanthan gum, polyvinyl chloride (PVC), polyacrylic acid (PAA) and its various derivatives, including various salts of PAA (e.g., Na-PAA, Li-PAA, NH4-PAA, and others), alginic acid and its various derivatives, including various salts of alginic acid (e.g., Na alginate, Li alginate, Ca alginate, Al alginate, etc.), chitosan, butyl acrylate, gum arabic, guar gum, carrageenan, gelatin, polyvinyl alcohol (PVA), and various mixtures and copolymers thereof. Carbon black is the most common conductive additive used in the anode, but single-walled, double-walled, and multi-walled carbon nanotubes, expanded graphite (multilayer graphene flakes), and metal nanowires may also be used in some designs.

[0079] For many applications and electrode designs, batteries with intercalation or conversion or mixed cathode materials or with intercalation or conversion (including alloys, such as Si or Sn) or mixed anode materials may exhibit sufficiently fast charge and discharge rates (e.g., charging to about 80% of maximum capacity within about 10-60 minutes). For some applications (e.g., for even faster rate performance (e.g., charging to about 80% of maximum capacity within about 1-600 seconds at "regular" areal capacity loads or 1-6000 seconds at "high" areal capacity loads), or for better cycle stability, or better calendar life, or better performance at low and high temperatures, or reduced reactivity with electrolytes, or higher capacity utilization, or other performance gains), it may be advantageous to produce composites containing such active materials for use in electrodes of batteries (e.g., Li-ion or Na-ion batteries, among others).

[0080] In some designs, composites (e.g., in the form of composite particles) including such active materials may further advantageously include carbon due to carbon's high electrical conductivity, acceptable mobility of Li and other no ions, good mechanical properties, and good chemical and electrochemical resistance.

[0081] In some designs, such composites (e.g., in the form of composite particles) that include both active (ion storage) materials (such as, but not limited to, intercalation-type materials, conversion-type materials, including alloy-type materials, pseudocapacitive materials, mixed-type active materials, etc.) and (inactive) carbon may be advantageous to have a significant weight percentage of (non-carbon) active material. In some designs, the percentage of such active material (e.g., to provide an illustrative example, the Si-based or Si-containing active material(s) in the case of an anode composite that includes C and Si) may preferably range from about 20% to about 98% by weight (in some designs, about 20% to about 40% by weight; in other designs, about 40% to about 60% by weight; in still other designs, about 60% to about 80% by weight; in still other designs, about 80% to about 98% by weight). In some designs, the weight ratio of active material to carbon may preferably range from about 1:4 to about 50:1 (in some designs, from about 1:1 to about 20:1). Too low a proportion of active material can result in undesirably low volumetric capacity, while too high a proportion of active material can result in reduced rate and stability.

[0082] It should be noted that in some designs, instead of or in addition to pure intercalation type active materials or pure conversion type active materials, mixed-type materials that undergo both intercalation and conversion type electrochemical reactions may be utilized. In some designs, the intercalation type active materials in the electrode may be in the form of individual particles bound together (e.g., with a binder and optional conductive additives) to form an electrode, or in the form of composite particles that include intercalation type active materials, which may be similarly bound together to form an electrode. Similarly, in some designs, the conversion type active materials in the electrode may be in the form of individual particles bound together (e.g., with a binder and optional conductive additives) to form an electrode, or in the form of composite particles that include conversion type active materials, which may be similarly bound together to form an electrode. In some designs, the electrodes are purposefully composed of multiple materials or material types (e.g., including both intercalation type active materials and conversion type active materials). In some designs, the particles that include intercalation type active materials and the particles that include conversion type active materials may exhibit sufficiently different sizes and / or BET specific surface areas. In addition to conversion-type and intercalation-type active materials, some of the materials may be of the pseudocapacitive type, or at least may experience a pseudocapacitive reaction in addition to other energy storage electrochemical reaction mechanisms.

[0083] In some designs, the active material distribution in the electrode may include 100% of such carbon-containing composites (e.g., in some designs, anode material composites containing Si in the case of an anode for a Li-ion battery), or may include a mixture of composites and "regular" active materials (e.g., graphite or soft carbon or hard carbon or various mixtures thereof in the case of an anode for a Li-ion battery). In some designs, the "regular" active materials may be intercalation-type active materials. In some designs, the appropriate mass percentage of composite particles in such "mixed" electrodes may range from about 1 to about 99% by weight (in some designs, about 1% to about 5% by weight; in other designs, about 5% to about 10% by weight; in still other designs, about 10% to about 20% by weight; or more) of all active material particles in a given electrode (i.e., without the weight of binders, conductive and other additives, and without the weight of current collectors), depending on the nature of such materials and the requirements and demands of the application. In still other designs, the weight percentage may range from about 20% to about 30%; in still other designs, from about 30% to about 40%; in still other designs, from about 40% to about 50%; in still other designs, from about 50% to about 60%; in still other designs, from about 60% to about 70%; in still other designs, from about 70% to about 80%; in still other designs, from about 80% to about 90%; in still other designs, from about 90% to about 99%. In some designs, percentages less than about 1% by weight are considered too small to make a substantial difference. Similarly, in other designs, percentages greater than about 99% by weight may result in an undesirable increase in the complexity and cost of the electrode mix, and may be better substituted with about 100% by weight of the composite(s) without any substantial sacrifice of electrode properties. However, any percentage (from about 0 to about 100% by weight) may be suitable for some applications.

[0084] In some designs, the performance characteristics and cycling stability of electrodes containing some of such carbon, including composite materials (e.g., in the form of composite particles), are particularly favorable for applications requiring ultra-fast charging (within about 1-600 seconds) or long calendaring life or long cycle life or low first cycle loss or other properties, particularly for electrode area capacity loadings of about 1-2 mAh / cm. 2 If the electrode area capacity exceeds 4 to 5 mAh / cm 2 If the electrode area capacity exceeds 6 to 8 mAh / cm 2 (For example, 6 to 18 mAh / cm 2 or even higher), may be particularly unsatisfactory. However, higher loadings are advantageous for reducing the cost of energy storage devices and increasing their energy density and specific energy. One or more embodiments of the present disclosure may achieve a loading of about 2 mAh / cm 2 to about 5mAh / cm 2 Electrode area loadings in the range of about 5 mAh / cm 2 to about 8mAh / cm 2 and even more so at loads in the range of about 8mAh / cm 2 to about 16, or even about 18 mAh / cm 2 loading (e.g., in some designs, the areal capacity loading of the electrode composition is about 2 mAh / cm 2 to about 18mAh / cm 2 The present invention is directed to synthesis processes, compositions, and various physical and chemical properties of carbon-containing composite electrodes that facilitate satisfactory performance with respect to the surface area, surface area, and surface area of ​​the electrode, which may range from 0.1 to 1.5 nm.

[0085] In some designs, degradation of Li-ion cells having some carbon-containing composite material (e.g., in the form of composite particles including both carbon and active material(s)) in at least one of their electrodes (e.g., in the anode or cathode or both) can be particularly undesirably fast in multi-layer (e.g., stacked or wound) medium sized cells (e.g., cells having cell capacities ranging from 0.2 Ah to about 10 Ah), even larger cells (e.g., cells having cell capacities ranging from about 10 Ah to about 40 Ah), and even extra-large cells (e.g., cells having capacities ranging from about 40 Ah to about 400 Ah) or jumbo cells (e.g., cells having capacities ranging from about 400 Ah to about 4,000 Ah or more). However, multi-layer medium or large sized cells can be attractive for some electronic devices, and multi-layer large, extra-large, or jumbo cells can be particularly attractive for use in some electronic transport or grid storage applications. One or more embodiments of the present disclosure facilitate the utilization of certain types of carbon with suitable microstructural, chemical, physical, and other properties to mitigate or overcome some or all of such limitations of carbon-containing composite materials and to substantially enhance the performance of such Li-ion cells.

[0086] In some designs (e.g., for faster charging rates or improved stability), it may be advantageous for such carbon-containing composites (e.g., carbon-containing composite particles) with (non-carbon) active materials to contain pores (e.g., surface pores, closed interior pores that are inaccessible to external materials such as electrolyte, open interior pores that are accessible to external materials such as electrolyte, interconnected open interior pores, etc.). In some designs, the "total" pore volume in the composite (including closed interior pores, if present) may be on the order of about 0.01 cm, depending on the volume change of the (non-carbon) active materials during cycling, the ionic conductivity of the composite components, the extent of side reactions with the electrolyte at operating conditions, and other factors. 3 / g to about 2.0 cm 3 / g (ranging from about 2 vol.% to about 75 vol.% in some designs) can be advantageous. In some designs (e.g., when the volume change of the active material is small and when side reactions are moderate), it may be advantageous for at least some fraction (e.g., about 0.1-100% by volume) of the total pores in the composite to be accessible to the electrolyte when the electrode composition constitutes part of an energy storage device cell (e.g., 100% by volume in this context means essentially no closed interior pores). In some designs, it may be advantageous for at least some fraction (e.g., about 1-100% by volume) of the pores to be interconnected to adjacent pores and accessible from the interior (or center) of the composite particle. In some designs, it may be advantageous for at least some fraction (e.g., about 1-100% by volume) of the pores to exhibit a characteristic dimension (e.g., diameter or width) that is in the range of about 0.3 nm to about 600 nm. In some designs, it may be advantageous for at least some fraction (e.g., about 0.1-30% by volume) of the total pores (including both those that are accessible and those that are not accessible to the electrolyte when the electrode composition constitutes part of an energy storage device cell) to be in the range of about 10 nm to about 20 nm. It may be advantageous in some designs for at least a portion (e.g., about 30-100% by volume) of the total pores (including both those accessible and those inaccessible to the electrolyte when the electrode composition constitutes part of an energy storage device cell) to exhibit a characteristic dimension in the range of about 0.3 nm to about 10 nm (e.g., to maximize the volumetric capacity of the electrode or to achieve high speed performance). In some designs, it may be advantageous (e.g., to maximize the volumetric capacity of the electrode or to improve stability) for at least a percentage (in the composite) of the total pores (e.g., about 10-100% by volume; in some designs, about 30-100% by volume - about 30-40% by volume or about 40-50% by volume or about 50-60% by volume or about 60-70% by volume or about 70-80% by volume or about 80-90% by volume or about 90-100% by volume) to exhibit a characteristic dimension in the range of about 0.3 nm to about 6 nm.In some designs (e.g., when the active material exhibits small (e.g., about 0.1-10 vol.%) or moderate (e.g., about 10-120 vol.%) volume changes during cycling and when it is desired to maximize the volumetric capacity and volumetric energy storage properties of the electrode), it may be advantageous for the volume fraction of total pores in such composites to be small (e.g., about 0.001-5 vol.%) or moderate (e.g., about 5-20 vol.%). In some designs (e.g., to maximize energy storage properties such as power or energy density or cycling stability, or to achieve a compromise between these or other features), the so-called Brunauer-Emmett-Teller (BET) specific surface area (SSA) or density functional theory (DFT) SSA (e.g., measured using N2 or Ar or CO2 or H2 sorption techniques and measured using BET or DFT methods) of the composite electrode material (particle) is less than about 0.25 m. 2 / g to about 1000m 2 / g (depending on, among other factors, the type of (non-carbon) active material and electrolyte used and the desired properties of the battery cell, in some designs it may be advantageous to have a 2 / g to about 2m 2 / g; in other designs, about 2m 2 / g to about 10m 2 / g; in other designs, about 10m 2 / g to about 40m 2 / g; in other designs, about 40m 2 / g to about 100m 2 / g; in other designs, about 100m 2 / g to about 400m 2 / g; in other designs, about 400m 2 / g to about 1000m 2 / g). A larger SSA may enable faster charge / discharge rate capability, but may also result in a higher rate of some undesirable side reactions (e.g., with the electrolyte). The rate of such undesirable (e.g., resulting in self-discharge or outgassing or deposit formation or irreversible consumption of electrolyte or electrode or cell swelling, faster decomposition, etc.) reactions may depend on the operating electrode potential, operating temperature, and electrolyte composition, among other factors. Acceptable rates will depend on the particular application. However, for many electrolyte systems, and for most cell designs and applications, the BET SSA is generally about 0.25 m 2 / g to about 1000m 2 / g. In some designs, the BET SSA is preferably in the range of about 1 m 2 / g to about 100m 2 / g. In some designs, the BET SSA is preferably in the range of about 1 m 2 / g to about 40m 2 It is believed preferable to range up to / g.

[0087] In some designs (especially in higher BET SSE complexes), it may be advantageous for the active (e.g., intercalation or conversion or mixed) material to be protected (from undesired interactions with the electrolyte) by a protective surface (shell) layer. In some designs, a suitable thickness for the protective surface layer may range from about 0.3 nm to about 60 nm (e.g., in some designs, about 0.3 nm to about 3 nm; in some designs, about 3 nm to about 6 nm; in some designs, about 6 nm to about 10 nm; in some designs, about 10 to about 20 nm; in some designs, about 20 nm to about 40 nm; and in some designs, about 40 nm to about 60 nm). Smaller thicknesses may be less effective in some applications, while larger thicknesses may result in reduced volumetric and gravimetric energy density and reduced performance in some applications. In some designs, the protective surface layer may directly coat at least a portion (e.g., about 1-100% of the exterior area) of the active material(s) / particle(s) that would otherwise be exposed to the electrolyte, at least during some of the battery assembly or operation. In some designs where a shell partially covers the exterior surface area (e.g., the protective material is selectively deposited to mostly cover the particle surface area, including the pores, such that what would otherwise be open pores are closed by the protective surface layer), the protective surface layer may instead be characterized as a pore plug material (rather than a shell). In some examples, the protective surface layer may include carbon. In some examples, the protective surface layer may include an oxide, a fluoride, an oxyfluoride, a sulfide, a nitride, an oxynitride, a nitridyl fluoride, a phosphate, a fluorophosphate (phosphate fluoride), or another material that includes metal or semimetal atoms.In some designs, the protective surface layer material is selected from the group consisting of the following elements: transition, alkali, or alkaline earth metals (such as iron (Fe), manganese (Mn), copper (Cu), yttrium (Y), zirconium (Zr), niobium (Nb), molybdenum (Mo), chromium (Cr), lithium (Li), sodium (Na), magnesium (Mg), potassium (K), calcium (Ca), strontium (Sr), cesium (Cs), barium (Ba), among others); lanthanum or lanthanoids. The metals may include one or more of: arsenic (La, Ce, Gd, Nd, Eu, etc.), beryllium (Be), aluminum (Al), silicon (Si), gallium (Ga), germanium (Ge), phosphorus (P), arsenic (As), tin (Sn), bismuth (Bi), lead (Pb), indium (In), cadmium (Cd), zinc (Zn), fluorine (F), iodine (I), oxygen (O), nitrogen (N), sulfur (S), selenium (Se), tellurium (Te), hydrogen (H), and carbon (C).

[0088] In some designs (e.g., to maximize electrode uniformity and battery stability), it may be advantageous for such carbon-containing composite electrode particles to exhibit volume average characteristic dimensions (e.g., diameters) ranging from about 5 nanometers (nm) to about 150 microns (about 200 nm to about 30 microns in some designs), as measured using a scanning electron microscope (SEM) or a laser particle size analyzer, or a combination of several characterization techniques and numerical analysis / modeling. Too small a particle size may lead to difficulties in achieving high packing density in some applications. At the same time, a high volume fraction of smaller particles may also lead to small interparticle pore sizes, which may slow the rate performance of the electrode and lead to faster cell degradation in some designs (especially when the battery is operated at higher speeds or lower temperatures). On the other hand, too large an average particle size may lead to local variations in electrode capacity loading and may lead to faster cell degradation in some designs (especially when the battery is operated at lower temperatures or higher speeds). Composite particle size, the interconnectivity of pores in the composite, and ion and electron transport in the composite material can affect particle-level rate performance. In some designs, too large an average particle size can also result in poor (or not good enough for a given application) charge and discharge rate performance. Although various electrode and electrolyte properties, battery cell operating conditions (e.g., current, rate, temperature, charging voltage, electrode operating potential, etc.), composite particle porosity and shape, and other parameters can affect the optimal composite particle size, in some designs, it is advantageous for such composite electrode particles to exhibit volume average characteristic dimensions in the range of about 200 nm to about 30 microns (in some designs - about 0.2 microns to about 1 micron; in other designs, about 1 to about 2 microns; in still other designs, about 2 microns to about 5 microns; in still other designs, about 5 microns to about 10 microns; in still other designs, about 10 microns to about 30 microns).The appropriate electrode-level porosity (e.g., the volume fraction of space in the electrode that is mostly-filled by electrolyte) can be influenced by the volume fraction of binder, the volume fraction of conductive and other additives, and the volume fraction of active (composite) particles (and their open porosity), the conductivity of the electrolyte, the thickness of the electrode, the battery operation, and other properties. Such porosity may change during cycling if the active material or a composite that includes the active material exhibits a substantial volume change during cycling. However, such electrode porosity values ​​ranging from about 1 vol.% to about 75 vol.% (e.g., in some designs - after 0-10 cycles after the so-called battery "formation" and quality control stage; in some designs - after electrode assembly / calendering and before electrolyte infiltration into the cell) are acceptable or advantageous for some applications (in some designs - from about 1 vol.% to about 10 vol.%; in other designs from about 10 vol.% to about 20 vol.%; in still other designs from about 20 vol.% to about 30 vol.%; in still other designs from about 30 vol.% to about 40 vol.%; in still other designs from about 40 vol.% to about 50 vol.%; in still other designs from about 50 vol.% to about 60 vol.%; in still other designs from about 60 vol.% to about 75 vol.%). Smaller volume fractions may result in slower charge / discharge rates and faster cell degradation in some applications. Larger fractions may undesirably reduce volumetric energy density, rate capability, and increase battery costs in some applications. In some designs, the volume fraction of the electrodes occupied (filled) with a suitable electrolyte may advantageously range from about 1% to about 755% by volume. In some designs, the suitable volume fraction of the electrodes occupied (filled) with a suitable electrolyte may be in an even narrower range, such as from about 5% to about 60% by volume (or even narrower ranges, such as from about 10% to about 40% by volume).

[0089] In some designs, the majority (e.g., about 70-100% by volume) of the (non-carbon) active material within the carbon-containing composite electrode particles may be in the form of smaller particles (e.g., rather than in the form of a continuous or discontinuous coating or a porous unibody filled with carbon or other (inert or less active) material). In some designs, the volume average size of the active material particles (within the carbon-containing composite electrode particles) may advantageously range from about 0.5 nm to about 200 nm (in some designs, from about 0.5 nm to about 5 nm; in other designs, from about 5 nm to about 10 nm; in still other designs, from about 10 nm to about 20 nm; in still other designs, from about 20 nm to about 40 nm; in still other designs, from about 40 nm to about 60 nm; in still other designs, from about 60 nm to about 100 nm; in still other designs, from about 100 nm to about 200 nm). Too large a size may not result in fast enough electrochemical reactions in some designs, while too small a size may result in undesirable side reactions or too low mass loading of the active material particles in such composites, thus limiting the energy performance of energy storage devices constructed with these composite particles in some designs. In some designs, the volume average size of the crystalline grains of the active material particles (composite electrode particles including the prepared carbon), as analyzed using diffraction or scattering techniques (e.g., X-ray diffraction, XRD) or transmission electron microscopy (TEM) or other suitable techniques, can advantageously range from about 0.5 nm to about 200 nm (in some designs, from about 0.5 nm to about 5 nm; in other designs, from about 5 nm to about 10 nm; in still other designs, from about 10 nm to about 20 nm; in still other designs, from about 20 nm to about 40 nm; in still other designs, from about 40 nm to about 60 nm; in still other designs, from about 60 nm to about 100 nm; in still other designs, from about 100 nm to about 200 nm).

[0090] In one illustrative example, a porous composite anode powder for Li-ion batteries was prepared having individual particles comprising porous carbon (i) infiltrated with (ii) silicon nanoparticles and (iii) encapsulated in a protective shelling material, such material containing closed pores. XRD measurements of the porous composite anode powder were performed using a Rigaku SmartLab diffractometer utilizing a Cu K-alpha radiation source at scan rates between 0.5 and 10 degrees / min from 3 to 158 degrees 2-theta. Powder XRD data were collected in a Bragg-Brentano geometry using an X-ray wavelength of 1.5406 Å. Various entrance and detector optics were used, specifically beam masks between 2 and 15 mm and Sollar slits between 0.5 and 5°. A 2D silicon detector was used for all measurements. Scherrer analysis of the Si(111) Bragg peak demonstrated that such porous composite anode powder samples had average Si crystallite sizes ranging from about 2 nm to about 100 nm (for some composite particle designs, from about 2 nm to about 20 nm; for other designs, from about 20 to about 40 nm; for still other designs, from about 40 to about 60 nm; and for still other designs, from about 60 to about 100 nm).

[0091] Figure 2A shows some suitable composite particle designs in which Si is embedded within a porous carbon matrix material, with average Si crystallite sizes ranging from about 5 nm to about 16 nm, as determined using Scherrer analysis of the Si(111) Bragg peak. In Figure 2A, the different color plots correspond to different experimental series of suitable Si- and C-containing composites that were produced.

[0092] FIG. 2B shows some other suitable composite particle designs in which Si is embedded within a porous carbon matrix material, where the average Si crystallite size, as determined using Scherrer analysis of the Si(111) Bragg peak, ranged from about 3.5 nm to about 8.5 nm.

[0093] Other suitable particle designs and still other processing conditions may result in either larger (in some designs, up to 60-100 nm) or smaller (down to about 2 nm) average Si grain sizes. In some suitable particle designs and processing conditions, at least a portion of the Si within the composite particles may be amorphous.

[0094] In some designs, the carbon in such carbon-containing compositions (e.g., composite particles that also contain active (non-carbon) materials) is predominantly (e.g., about 90-100%) sp 2 It may be advantageous to include -bonded carbon atoms (e.g., to obtain high electrical conductivity or for other performance benefits). In some designs, the carbon is sufficiently conductive (e.g., its electrical conductivity is about 1 S / m to about 10 6 S / m) can be advantageous (e.g., for faster speed performance).

[0095] In some designs, the active material particles (of the composite carbon-containing electrode particles) may be preferably located inside (e.g., confined by) the pores of suitable carbon particles, and in some designs, about 50% to about 100% by weight of the active material in the composite particles may be confined within the pores defined in the carbon particles.

[0096] In some designs, the composite carbon-containing and active material-containing electrode particles may comprise porous carbon. In some process designs, the porous carbon particles may be infiltrated with active material (or active material particles) during at least one of the processing (or synthesis) steps to form such carbon-containing and active material-containing electrode particles (e.g., Si-containing composite anode particles having Si-based and / or Si-containing active materials). In some designs, such porous carbon may exhibit certain properties that make the composite particles particularly functional in Li-ion batteries and other relevant applications.

[0097] In some designs, the porous carbon (e.g., used in the composite formation or ultimately produced during the composite formation) is approximately 400 m 2 / g to about 5,000m2 It may be advantageous for the porous carbon particles to exhibit an average so-called BET specific surface area (SSA) (as measured by CO, N, H, or Ar gas sorption) in the range of about 0.3 cm / g (prior to formation of the composite). In some designs, the porous carbon particles have an open porosity in the range of about 35% to about 93% by volume, and a specific surface area of ​​about 0.3 cm, as determined by gas sorption (e.g., CO, N, H, Ar, etc.) or other suitable measurement. 3 / g to about 6cm 3 It can be advantageous for the battery to exhibit a total open pore volume (e.g., void space) in the range of 100 / g. In some designs, a suitable BET SSA can be on the order of 400 m, depending on the chemistry and nature of the active materials in the battery, the cell fabrication procedure, the processing involved in infiltrating the active materials into the porous carbon, the cell fabrication procedure, and other factors. 2 / g to about 1,000m 2 / g range; in yet other designs, the appropriate BET SSA may be in the range of about 1000m 2 / g to about 2,000m 2 / g range; in yet other designs, the appropriate BET SSA may be in the range of about 2,000 m 2 / g to about 3,000m 2 / g range; in yet other designs, the appropriate BET SSA may be in the range of about 3,000 m 2 / g to about 4,000m 2 / g range; in yet other designs, the appropriate BET SSA may be in the range of about 4,000 m 2 / g to about 5,000m 2 / g range is also acceptable. 2 BET SSAs greater than 400 m / g can make the composite difficult to handle and produce, can result in poor performance in some designs, and in some cases can be too expensive to produce and handle (for battery applications). 2A BET SSA less than 0.1 / g may be undesirable and limit the rate performance and / or volumetric capacity (or capacitance) or other important properties of the composite in some electrochemical energy storage applications. In some designs, a suitable carbon pore volume may be on the order of 0.3 cm2 or less, depending on the chemistry and nature of the active materials in the battery, the cell fabrication procedure, the processing involved in infiltrating the active materials into the porous carbon, the cell fabrication procedure, and other factors. 3 / g to about 1 cm 3 / g range; in other designs, suitable pore volumes are in the range of about 1 cm 3 / g to about 2 cm 3 / g range; in yet other designs, suitable pore volumes are in the range of about 2 cm 3 / g to about 3 cm 3 / g range; in yet other designs, suitable pore volumes are in the range of about 3 cm 3 / g to about 4cm 3 / g range; in yet other designs, suitable pore volumes are in the range of about 4 cm 3 / g to about 5cm 3 / g range; in yet other designs, suitable pore volumes are in the range of about 5 cm 3 / g to about 6cm 3 / g range. Some designs have a 3 Pore ​​volumes greater than 0.4 cm / g can make the composite difficult to handle and produce, can result in poor performance in some designs, and in some cases can be too expensive to produce and handle (for battery applications). 3 Pore ​​volumes less than 100 / g may undesirably limit the rate performance and / or volumetric capacity (or capacitance) or other important properties of the composition in some electrochemical energy storage applications.

[0098] In some designs, it may be advantageous for the porous carbon (used in forming a suitable electrode composite; e.g., for infiltration of active material, or for making a composite with, e.g., an active material precursor and then converting the active material precursor to an active material, etc.) to contain approximately spherical (or approximately elliptical) pores. In some designs, such approximately spherical (or approximately elliptical) pores may advantageously exhibit an average pore size in the range of about 2 nm to about 100 nm (in some designs, about 2 nm to about 20 nm; in other designs, about 20 nm to about 100 nm). In some designs, such approximately spherical (or approximately elliptical) pores may advantageously be separated from each other by microporous (containing mostly pores of 2 nm or less) carbon material. Spherical (or approximately spherical) pores may exhibit better mechanical properties (e.g., compared to slit-shaped pores) and may better maintain mechanical integrity when filled with an active material that exhibits a volume change (e.g., Si or Sn, etc.). Separating such (e.g., relatively large) spherical pores from each other and from the surface of the composite particle can help seal them to prevent undesired interactions with the electrolyte. The approximately 2 nm or smaller pores in the material separating the individual spherical pores can, in some designs, exhibit an approximately slit shape. In some designs, the average thickness of the approximately microporous carbon "walls" separating the spherical pores can range from about 1 nm to about 100 nm (e.g., in some designs, from about 1 nm to about 10 nm; in other designs, from about 10 nm to about 20 nm; in other designs, from about 20 nm to about 50 nm; and in still other designs, from about 50 nm to about 100 nm). In some designs, the average pore volume of such microporous carbon "walls" may range from about 0.05 cc / g to about 1.20 cc / g (in some designs, from about 0.05 cc / g to about 0.25 cc / g; in other designs, from about 0.25 cc / g to about 0.5 cc / g; in other designs, from about 0.5 cc / g to about 0.75 cc / g; in still other designs, from about 0.75 cc / g to about 1.20 cc / g), as determined, for example, by gas (e.g., N2 or CO2 or H2 or Ar, etc.) sorption techniques.Too small a pore volume can undesirably reduce the total carbon pore volume or the ability to infiltrate such particles with active material (e.g., Si) or can reduce the rate performance or stability of the composite; whereas too large a pore volume can undesirably reduce the mechanical properties of the composite (e.g., including Si) or reduce the cycling stability.

[0099] In some designs, it may be advantageous for the porous carbon (used in forming a suitable electrode composite; e.g., for infiltration with an active material, or for making a composite with, e.g., an active material precursor, and then converting the active material precursor to an active material, etc.) to exhibit a compositional purity of greater than about 90% by weight (e.g., less than 10% by weight non-carbon species) prior to forming the composite, as determined by chemical composition, energy dispersive spectroscopy (EDS), thermogravimetric analysis (TGA), combustion analyzer, X-ray photoelectron spectroscopy (XPS), or other suitable mechanism. In some designs, a purity of greater than about 96% by weight may be even more advantageous in some designs. In some designs, a carbon purity of greater than about 98-99% by weight may be even more advantageous prior to use in a battery cell. In some designs, the so-called "ash" content in the carbon should preferably be less than about 10 wt% (e.g., preferably less than about 4 wt%, more preferably less than about 2 wt%, even more preferably less than about 1 wt%, and most preferably below about 0.25 wt%) before using such carbon in a battery electrode (in some designs, before infiltrating the active material). In some designs, higher contents of various impurities (e.g., K, S, Ca, Na, Zn, P, O, etc.) can induce side reactions, can significantly reduce cycling stability (especially at high temperatures), can induce premature failure, can reduce gravimetric and volumetric energy storage properties, can reduce power density, can lead to undesirable yet larger cell-to-cell or batch-to-batch variability, can reduce the performance characteristics of the electrochemical cell (e.g., Li-ion battery), and possibly induce some other type of undesirable result. In some designs, it may be advantageous to use a combination of chemical (e.g., treatment in acid) and thermal (e.g., heat treatment at temperatures from about 800° C. to about 2000° C. and evaporation of impurities) purification steps to obtain high purity porous carbon, or to use low ash content carbon precursors.

[0100] In some designs, it is considered important that the porous carbon contains less than about 10 wt. % (e.g., preferably less than about 2 wt. %, more preferably less than about 1 wt. %; even more preferably less than about 0.5 wt. %) of hydrogen atoms (e.g., present within its structure or as part of functional groups). In some designs, a higher hydrogen content (e.g., greater than about 2-10 wt. %) may result in undesirable gas formation and cell swelling, reduced capacity utilization, reduced cycling stability, higher first cycle loss, and / or other undesirable reductions in performance characteristics. In some designs, it is considered important that the composite carbon-containing electrode particles (e.g., in the case of anode materials, Si-containing particles, including Si-based and / or Si-containing active materials) contain less than about 10 wt. % (e.g., preferably less than about 2 wt. %, more preferably less than about 1 wt. %; even more preferably less than about 0.5 wt. %) of hydrogen atoms. The hydrogen content may be determined by using a hydrogen analyzer, titration, nuclear reaction analysis (NRA), Devanathan-Stachurski method, combustion carbon-hydrogen-nitrogen (CHN) analysis, instrumental gas analysis (IGA), scanning Kelvin probe force microscopy (SKPFM), and other suitable characterization mechanisms.

[0101] Surprisingly, it has been found that the thermal properties of the carbon (e.g., porous carbon) used for (or used in) forming the carbon-containing electrode composite are important indicators of its performance in Li-ion batteries and related applications. In some designs, the carbon (e.g., porous carbon) used for (or used in) forming the carbon-containing composite may exhibit a certain range of crystallization temperatures above which XRD forms graphitization (formation of graphite peaks) by annealing for several hours (e.g., about 1 hour to about 6 hours) in vacuum or in an inert environment such as Ar gas. In some designs, the crystallization onset temperature may preferably vary from about 1400°C to about 2400°C (in some designs, from about 1400°C to about 1600°C; in other designs, from about 1600°C to about 1800°C; in still other designs, from about 1800°C to about 2000°C; in still other designs, from about 2000°C to about 2200°C; in still other designs, from about 2200°C to about 2400°C). In some designs, the carbon XRD d(002) peak may shift from about 4.4-4.2 Å to about 3.4 Å as a function of increasing thermal annealing temperature. Crystallization onset temperatures of porous carbon lower than about 1400°C or higher than about 2400°C may undesirably result in inferior performance of carbon-containing composite particles in Li-ion batteries and related applications.

[0102] In some designs, it has been found that the microstructure of the carbon (e.g., porous carbon) used for (or used in) forming the carbon-containing electrode composite is an important indicator of its performance in Li-ion batteries and related applications. In some designs, it has been found that the (002) spacing of the carbon should preferably range from about 4.40 Å to about 3.45 Å (in some designs, from about 4.40 Å to about 4.00 Å; in other designs, from about 4.00 Å to about 3.80 Å; in still other designs, from about 3.80 Å to about 3.60 Å; in still other designs, from about 3.60 Å to about 3.45 Å), depending on various other parameters of the composite and its environment, as well as the electrochemical operating potential in Li-ion batteries.

[0103] Figure 3A shows examples of two suitable porous carbon samples that exhibit an onset temperature of crystallization between 1600°C and 1800°C upon annealing in vacuum for about 1 hour, as indicated by the formation of a sharp d(002) XRD peak upon annealing at 1800°C. Figure 3B shows another example of a suitable porous carbon that exhibits an onset temperature of crystallization between about 2100°C and about 2200°C upon annealing in vacuum for about 1 hour, as indicated by the formation of a sharp d(002) XRD peak upon annealing at 2200°C. Figure 3C shows another example of a suitable porous carbon that exhibits a (002) carbon spacing that exceeds that of graphite, which is about 3.34 Å.

[0104] Certain physical and chemical properties of carbon-containing compositions have been found to correlate well with their performance in cells. Such properties may be specific to the composition of the active material and the cell configuration and operating parameters (e.g., electrolyte, amount of such composition in the anode and cathode, areal capacity loading, cell operating temperature, charge rate, voltage range, among others). As a result, as an illustrative example, certain properties of carbon-containing composites with Si-based active material (e.g., nearly pure Si) are disclosed that facilitate their superior performance in anodes (e.g., either as a component of the anode together with graphitic carbon material or as the only Li storage material in the anode apart from the very small Li storage in the carbon-based conductive additive).

[0105] In some designs, such composites (e.g., in the form of composite particles) containing both active (ion storage) materials (including, e.g., Si-based active materials) and carbon may be advantageous to have a relatively small percentage of hydrogen. In some designs, the percentage of hydrogen may range preferably from about 0.00 wt.% to about 1.00 wt.% of the total weight of the composite particle (in some designs, below about 0.05 wt.%; in some designs, from about 0.05 wt.% to about 0.35 wt.%; in still other designs, from about 0.35 wt.% to about 1.00 wt.%). Too high a percentage of hydrogen may cause undesirably excessive first cycle losses and faster degradation. A very low percentage of H may make it difficult to obtain what are otherwise desirable structural, chemical, physical, and other properties of the carbon-containing composite provided.

[0106] In some designs, such composites (e.g., in the form of composite particles) containing both active (ion storage) materials (e.g., including Si-based active materials) and carbon may be advantageous to have a relatively small percentage of nitrogen. In some designs, the percentage of elemental nitrogen (N) may preferably range from about 0.00 wt% to about 5.00 wt% of the total weight of the composite particle (some designs below about 0.5 wt%; other designs from about 0.5 wt% to about 1 wt%; still other designs from about 1 wt% to about 2.50 wt%; still other designs from about 2.5 wt% to about 5.0 wt%). Too high a percentage of N may cause undesirably excessive first cycle losses and faster degradation. A very low percentage of N may make it difficult to obtain other desired structural, chemical, physical, and other properties of the carbon-containing composite.

[0107] In some designs, such composites (e.g., in the form of composite particles) containing both active (ion storage) materials (e.g., including Si-based active materials) and carbon may advantageously have a relatively small percentage of oxygen. In some designs, the percentage of oxygen (O) may preferably range from about 0.00% to about 5.00% by weight of the total weight of the composite particle (in some designs, below about 0.01% by weight; in other designs, from about 0.01% to about 0.25% by weight; in yet other designs, from about 0.25% to about 2% by weight; in yet other designs, from about 2% to about 5.0% by weight). Too high a percentage of O may cause undesirable excessive cycle loss and faster degradation. A very low percentage of O may make it difficult to obtain other desired structural, chemical, physical, and other properties of the provided carbon-containing composite.

[0108] It has been unexpectedly found that values ​​of nitrogen (N) incorporation during annealing of (e.g., porous) carbon-based composites with Si (or Si-based) active material in relatively inert nitrogen gas (N2) correlate well with the performance of the carbon-containing electrode composites in Li-ion batteries. For example, in some designs, it is believed that during annealing of suitable carbon-based and Si-containing composites (e.g., composite particles with Si-based and / or Si-containing active materials) in nitrogen gas (N2) at 1050°C for 2 hours, the composites may exhibit nitrogen incorporation (incorporation into the carbon structure) ranging from about 1.5 wt% to about 25 wt% nitrogen of the total weight of the composite, depending on the active material (e.g., Si-based and / or Si-containing active materials, etc.) particle size, percentage, cell design, and other factors (in some designs, about 1.5 wt% to about 2.5 wt%; in other designs, about 2.5 wt% to about 7.5 wt%; in still other designs, about 7.5 wt% to about 15 wt%; in still other designs, about 15 wt% to about 25 wt%). Either too little or too much nitrogen incorporation may cause undesirable cell performance (e.g., lower cycle life; lower performance; lower first cycle efficiency, etc.). In other examples, suitable carbon-based and Si-containing composites exhibit an average nitrogen (N) incorporation of about 1.5% to about 25% by weight when heated in nitrogen gas (N2) at 1050° C. for 2 hours, as measured on a powder containing the composite particles. For example, the powder may contain most (e.g., all or substantially all or a majority, etc.) of the carbon-based and Si-containing composite particles (e.g., a large statistical number of particles contributing to such a measurement).

[0109] In another example, in some designs, it is believed that during annealing of suitable carbon-based and Si-containing composites (e.g., composite particles with Si-based and / or Si-containing active materials) in nitrogen gas (N2) at 850°C for 2 hours, the composite particles may exhibit nitrogen incorporation (incorporation into the carbon structure) in the range of about 0.5 wt% to about 10 wt% nitrogen of the total weight of the composite (in some designs, about 0.5 wt% to about 2.5 wt%; in other designs, about 2.5 wt% to about 7.5 wt%; in still other designs, about 7.5 to about 10 wt%), depending on the size of the active material (e.g., Si-based and / or Si-containing active materials) granular particles in the composite, the weight percentage of the active material in the composite, the cell design, and other factors. Either too little or too much nitrogen incorporation may cause undesirable cell performance (e.g., lower cycle life; lower rate performance; lower first cycle efficiency, etc.). Carrying out such annealing in N2 may allow tailoring the processing and synthesis routes for the formation of such Si- and C-containing composites for superior performance in Li-ion battery anodes.

[0110] 4 shows an exemplary example of nitrogen (N) uptake by annealing an exemplary suitable carbon-containing composite powder (including Si-based active material) in N2 gas for 2 hours. Higher annealing temperature results in greater N2 uptake. The measurement error is estimated to be less than about 1.5% by weight.

[0111] Annealing of (e.g., porous) carbon-based composites with Si-based and / or Si-containing active materials in relatively inert nitrogen gas (N2) or argon gas (Ar), for example at elevated temperatures for 2 hours, typically results in the formation of silicon carbide (SiC) crystals, which can be detected by X-ray diffraction (XRD) or by Fourier transform infrared spectroscopy (FTIR) or other suitable techniques. In some implementations, the porous composite particles form about 1% to about 100% silicon carbide (SiC) by weight when heated in nitrogen gas (N2) or argon gas (Ar) at a temperature range of about 750°C to about 950°C for 2 hours or longer, as detected by XRD or FTIR or other suitable techniques. The total weight of SiC can be determined by using appropriate calibration standards. In some designs, it may be advantageous to oxidize any Si or C remaining in the sample to increase measurement accuracy. It has been unexpectedly found that the minimum temperature at which SiC forms correlates with the performance of the carbon-containing electrode composite in a Li-ion battery. For example, in some designs, it is believed that during annealing of a suitable carbon-based and Si-containing composite for 2 hours in N2 gas, the minimum temperature required to detect SiC by XRD (e.g., having a SiC(111) XRD peak at about 35 degrees 2-theta with at least 10% intensity of the Si(111) XRD peak at about 28 degrees after background subtraction) may preferably range from about 750°C to about 950°C (in some designs, about 750°C to about 875°C; in other designs, about 875°C to about 950°C). Too high or too low a SiC formation temperature typically results in poor performance of the Li-ion battery anode.

[0112] FIG. 5 shows illustrative examples of XRD patterns of suitable carbon-based Si-containing composites annealed in N2 at various temperatures and shows SiC formation at about 850°C.

[0113] It has been unexpectedly found that the reduction in specific capacity (measured in mAh / g) (in %) upon annealing suitable carbon-based silicon-containing anode composites (e.g., in the form of powder) in N2 gas at a relatively low temperature of 750°C for 2 hours correlates with their performance (e.g., cycle stability, calendar life, rate performance, etc.) in Li-ion batteries. For example, in some designs, it is believed that the capacity reduction during annealing in N2 for 2 hours ranges from about 2% to about 25% (in some designs, about 2 to about 12%; in other designs, about 12 to about 25%). Too low or too high reduction in specific capacity after annealing under such conditions may cause degraded performance characteristics in Li-ion battery anodes. Thus, the synthesis and processing conditions for the formation of suitable carbon-containing and silicon-containing composite anode particles may be adjusted to obtain the appropriate capacity reduction.

[0114] In some designs, it is believed that for superior performance of porous carbon-containing composites (e.g., containing Si, especially as part of a Si-based or Si-containing active material), it is preferred to exhibit variable porosity across the diameter (cross section) of the particle. In some designs (e.g., when the active material exhibits substantial volume change during cycling, such as Si-based and / or Si-containing active materials), it is believed that it is preferred that the central portion of the particle contains a larger pore volume (e.g., a larger volume fraction of pores relative to the active material fraction or the combined active material and carbon fraction) compared to portions of the particle closer to the surface.

[0115] In some designs, it is believed that good performance of a porous carbon-containing composite (e.g., containing Si as an active material, among others) preferably includes closed pores and a certain range of true density, as measured using argon (Ar) pycnometry or, in some designs, nitrogen (N2) pycnometry. In some designs, when the active material in the carbon-containing composite (particle) is a Si-based or Si-containing active material (e.g., Si or Si alloy or Si-based oxide or nitride or oxynitride or various combinations thereof, preferably with a BET SSA of about 1 m. 2 / g to about 40m2 / g), the true (measured by Ar pycnometry or N2 pycnometry) density of such a complex is about 0.9 g / cm 3 to about 2.2 g / cm 3 0.9g / cm3, with the optimum value believed to depend on the proportion and type of Si-based or Si-containing active material, the presence of other elements (e.g., metals), among other parameters. In some designs, such density is preferably in the range of about 0.9g / cm3. 3 to about 1.4 g / cm 3 ;approximately 1.4g / cm for other designs 3 to about 1.8 g / cm 3 ; and about 1.8 g / cm for other designs. 3 to about 2.2 g / cm 3 ) range. Density that is too low or too high can often result in poor performance (e.g., undesirable high speed degradation, slow speed performance, high loss, etc.).

[0116] In some designs, it is believed to be preferable (for superior performance in Li-ion battery anodes) that porous carbon-containing anode composites containing Si-based or Si-containing active materials (e.g., Si or Si-based active materials (among other suitable active anode materials)) exhibit a relatively uniform distribution of active material (e.g., Si) and C as measured by energy dispersive spectroscopy (EDS) on a cross-section of such composite particle. In particular, apart from a surface layer of 20-100 nm, it is believed to be preferable in some designs that EDS mapping of a cross-section of a composite particle (e.g., with a lateral resolution of about 2-50 nm) exhibits less than about 50% deviation from the average Si:C ratio (of total elemental Si and total elemental C in the composite particle) (which may, for example, range from 5:1 to 1:5 in some designs).

[0117] In some cell designs, it is believed that a porous carbon-containing anode composite (e.g., a composite that includes Si or Si-based or Si-containing active material, among other suitable active anode materials) is preferably used in combination with an intercalation-type anode material (e.g., synthetic / artificial or natural graphite, soft carbon, card carbon, and various combinations thereof) in forming the anode. In some designs, a suitable percentage of the areal capacity provided by the porous carbon-containing anode may range from about 10% to about 100%. For example, in some designs, a capacity of say 3.5 mAh / cm2 may be used. 2 For Li-ion battery anodes with areal capacity of about 0.35 mAh / cm, the porous carbon-containing anode composites 2 to about 3.5mAh / cm 2 In some designs, the porous carbon-containing anode composite may provide from about 10% to about 25% areal capacity, depending on, among other requirements, the volume change of the carbon-containing anode composite during cycling, the cell design (e.g., laminated vs. wound), the cell operating conditions (e.g., temperature, charge rate, discharge rate, pulse current requirements, etc.), areal capacity loading, requirements regarding cycle life and calendar life, requirements regarding charge rate, limitations of the choice of electrolyte or electrolyte additive, the type of copper foil used; total areal loading; in other designs, from about 25% to about 50% areal capacity; in still other designs, from about 50% to about 75% areal capacity; and in still other designs, from about 75% to about 100% areal capacity.

[0118] In some designs, it may be preferred (for superior performance in a Li-ion battery anode) that the porous carbon-containing anode composite with Si or Si-based active material exhibits certain microstructural, structural, thermal (or more generally, physical) and chemical properties, as well as certain microstructural, structural, thermal (or more generally, physical) and chemical properties of its components (e.g., Si-based or Si-containing active materials or carbons).

[0119] Unexpectedly, it has been found that the microstructural morphology of the carbon (e.g., porous carbon) used for (or used in) forming the carbon-containing electrode composite is an important indicator of its performance in Li-ion batteries and related applications. Therefore, appropriate processing of the carbon should preferably be performed to obtain certain microstructural morphologies for superior performance in some designs. Atomic pair distribution function analysis has been found to be particularly insightful.

[0120] Atomic pair distribution function (APDF) or atomic PDF analysis is an XRD technique also called "total scattering analysis". Herein, we sometimes refer to APDF as PFD. Most commonly, XRD experiments focus on the crystallographic information retained in the Bragg diffraction of X-rays from periodic structures within crystalline materials to perform, among other things, phase identification, composition, purity, lattice parameters, atomic dislocations, distortion, crystallite size, bond lengths, and angles. However, many engineered materials exhibit many aspects of their structure that deviate from the perfect crystalline case; for example, they exhibit very little or even no long-range structural coherence.

[0121] The total scattering approach to X-ray structural characterization considers both Bragg (coherent scattering for crystalline materials) and diffuse (incoherent scattering). When analyzing the total sum of scattering in a diffraction experiment, an additional correction is used to account for background that typically comes from Compton scattering, air scattering, and fluorescence, to name a few. This normalization function is called I(Q):

number

[0122] Subtraction of the Compton scattering from this function requires knowledge of the chemical composition of the sample. The intensity of the X-ray scattering as a function of the scattering vector I(Q) is typically further normalized to correct for the X-ray absorbance of the sample, resulting in a function S(Q), where S(Q) is:

number

[0123] X-ray diffraction is measured in units of Å -1 data, whereas the atomic pair correlation functions are real space functions with units of Å.

number

[0124] The pair distribution function G(r) is the Fourier transform of the total scattering structure function S(Q). The peaks of the pair distribution function G(r), whose positions are independent of the Fourier transform parameters, represent atom-atom pairs in real space, with the real space distance between them in Å. The presence of these peaks indicates that there is a statistically significant population of atoms, and indicates their real space atom-atom separation distance. Total scattering experiments require minimal structural coherence within the material, and are therefore the technique of choice for the analysis of amorphous, nanocrystalline, or low-order materials, including carbon (e.g., porous carbon). Detailed structural information may be obtained from the APDF when model-based approaches are not utilized. Some structural properties that can be probed by direct analysis of G(r) are: scattering domain size, coordination number, atomic density, as well as a wide variety of information from peak analysis and quantitative comparison across various atom-atom pairs. The scattering domain size may be determined by observing the radial distance at which structural coherence no longer exists. The coordination number is accessible through integration of the peak in G(r) since the intensity of that peak is a direct measure of the amount of atom-atom pairs. In the context of carbonaceous materials, this means, for example, that the coordination numbers for these are 3 and 4, respectively, so that 2 :sp 3 This can result in the determination of the carbon ratio. Atomic density, a value that is truly distinct from macroscopic measurement techniques in that it is unaffected by trapped porosity in the material, can be found through careful analysis of G(r). The determination of atomic density relies on the fact that G(r)=0 at radial distances below the first atom-atom interaction in the material. At these low radial distances, G(r)=-4πρ0r 2 The gradient of allows for the direct determination of the atomic number density by linear fitting of G(r). Finally, a rich set of information may be obtained by analysis of the peaks in G(r). Examples of salient peak metrics for structural analysis include: peak position, full width at half maximum, peak height, as well as width-to-height ratios across various atom-atom pairs.

[0125] It is also noted that in analyzing data, it is common to convert the pair distribution function, G(r), to a radial distribution function, R(r). The relationship between the pair distribution function, G(r), and the radial distribution function, R(r), is as follows (ρ0 is the number density of scatterers in the object): R(r)=G(r)r+4πr 2 ρ0 (Equation 4)

[0126] After mathematical conversion to R(r), it is straightforward to fit the peak in question using a Gaussian function, from which the area, width, height and position are available.

[0127] In some illustrative examples, synchrotron XRD data was collected on (i) suitable composite anode powders containing both carbon (porous carbon) and Si active materials, and (ii) suitable porous materials utilized in the formation of suitable composite electrode powders. Such XRD experiments were performed at the Advanced Photon Source at Argonne National Laboratory, beamline 11-ID. An X-ray wavelength of 0.21150 Å was used. The collected data were 2D plate images that were fitted and integrated using GSASII software for further analysis. Data was collected at detector distances of 1000 mm and 180 mm, with collection times ranging from 1 to 5 minutes.

[0128] Fourier transformation was performed using xPDFsuite with the following transformation conditions: Diffraction data were plotted against Q, a vector describing the scattering instants that discusses the diffraction data independent of the X-ray wavelength / energy (Q=4π·sin(theta) / λ), where λ is the X-ray wavelength. Q max (instrument) is the maximum Q cutoff (for a particular instrument) in terms of meaningful input intensity as reciprocal of Angstroms (some data files may contain trailing zeros or unreliable intensities at the upper bound of the detector range, thus Q max (Note that the (instrument) defines the threshold for reliable data.) This parameter is also used as an upper bound for the polynomial fit correction of the S(Q) data. Q max (Instrument) is the Q used in the Fourier transform max is defined independently of Q. min is the lower Q limit on the Fourier transform of the F(Q) curve in reciprocal Angstroms. Q max is the upper Q limit for the Fourier transform of the F(Q) curve in reciprocal Angstroms. ポリ is the r limit on the maximum frequency in the F(Q) correction polynomial. The pair distribution function (PDF) may not be reliable for shorter r, however for very small r ポリ does not allow for polynomial correction and may give a noisy PDF. Larger values ​​are believed to produce a closer fit with higher degree polynomials, but when too large they may smooth out useful signals in the data. The default was set to 0.9. r ステップ is the r lattice spacing for the PDF calculated in Angstroms (the number of points in G(r)).

[0129] The Fourier transformation performed on the collected data using the xPDF software complies with the following conditions and assumptions: (i) before transformation, the collected data was corrected by subtracting from an empty polyimide (KAPTON) capillary sample holder to remove contributions from the sample holder and air scattering effects; (ii) a suitable high purity porous carbon material was assumed to contain only carbon (the following values ​​used in the analysis: Q max (equipment)=29.0;Q min =0.99984;Q max =23.4697;Q max is chosen so that spurious artifacts in F(Q) are truncated and F(Q) ends at 0; ステップ =0.01;r ポリ =0.8898); (iii) a suitable composite anode powder containing both high purity carbon and high purity Si active materials is deemed to contain only carbon and silicon in atomic ratios carefully determined by a combination of other techniques such as inductively coupled plasma mass spectroscopy (ICP-MS), inductively coupled plasma optical emission spectroscopy (ICP-OES), gravimetric burnout data, mass gain recording during synthesis, and other methods (the following values ​​used for analysis: Q max (equipment)=28.998;Q min =0.71731;Q max =23.0;Q max is chosen so that spurious artifacts in F(Q) are truncated and F(Q) ends at 0; ステップ =0.01;r ポリ = 0.9); (iv) ρ determination for the conversion of G(r) to R(r) in Equation 4 was realized through a nonlinear least squares (nls) fit of the gradient of G(r) between r = 0 and r = 0.75 Å; some adjustments were made to account for any convergence errors built up at low radial distances so that R(r) did not fall below R(r) = 0. The domain size (size of the coherently scattering structural domain, averaged over the entire material in the beam path) was calculated from the PDF data. The domain size (r) was estimated as defined by the function G(r) that falls below about ± 0.01, the dimension (r) above which substantial coherence loss is observed. Note that for crystalline nanoparticles, the interference length is equal to the nanoparticle size, but for nanoparticles with defects or diameter-dependent structural relaxation, the interference length is not equal to the nanoparticle size. Thus, the scattering interference length places a robust lower bound on the average nanoparticle size, which can be larger ("at least this size"). This is particularly useful for materials that do not exhibit Bragg scattering (eg, amorphous or highly distorted) that typically cannot be analyzed using Scherrer analysis.

[0130] The average domain size of suitable carbon (e.g., porous carbon) used for (or used in) the formation of a carbon-containing electrode composite (e.g., composite particle) may preferably (for good performance in a cell) range from about 10 Å to about 60 Å, with the most preferred domain size depending on the composite composition and microstructure (e.g., type and amount of active material (e.g., Si vs. LTO vs. LiF / Fe vs. NaCl vs. FeF3, etc.), size of active material particles, volumetric expansion of active material, pore volume left during side reactions, pore size, etc.), as well as the particular cell design and cell operating conditions (e.g., electrochemical potential during cycling, type of active ion (e.g., Li + Against Na + ), operating temperature, etc. In some designs, such suitable domain sizes in carbon may preferably range from about 10 Å to about 15 Å; in other designs, from about 15 Å to about 25 Å; in still other designs, from about 25 Å to about 30 Å; in still other designs, from about 30 Å to about 40 Å; in still other designs, from about 40 Å to about 50 Å; in still other designs, from about 50 Å to about 60 Å. Such synchrotron XRD measurements and PDF analyses may be performed on either carbon materials (e.g., to select proper synthesis / processing conditions) or carbon-containing composites (e.g., having Si-based or Si-containing active materials) (e.g., to detect the presence or retention of suitable carbon in the composite).

[0131] 6A-6B show exemplary examples of PDF analysis of suitable carbons with scattering domain sizes of (601) between about 15 Å and about 19 Å (loss of interference defined as a function falling below G(r)=±0.01); (602) between about 19 Å and about 22 Å; (603) between about 24 Å and about 28 Å; (604) between 40 Å and 55 Å. Such synchrotron XRD measurements and PDF analysis may be performed on either carbon materials (e.g., to select proper synthesis / processing conditions) or carbon-containing composites (e.g., Si-based or Si-containing active materials, among others) (e.g., to detect the presence or retention of suitable carbon in the composite).

[0132] FIG. 7 shows an illustrative example of a PDF analysis of suitable carbon with scattering domain sizes of about 17.5 Å, about 21 Å, about 26 Å, and about 45 Å.

[0133] In some designs, the average scattering domain size of the suitable carbon-containing and suitable active material-containing electrode composite (e.g., composite particle) preferably ranges from about 1 nm to about 40 nm (for good performance in a cell), with the most preferred domain size depending on the composition and microstructure of the composite (e.g., type and amount of active material (e.g., Si-based vs. Si-containing vs. LTO vs. LiF / Fe vs. NaCl vs. FeF3, etc.), size of the active material particles, volume expansion of the active material, pore volume remaining in the composite, pore size, etc.) and the particular cell design and cell operating conditions (e.g., electrochemical potential during cycling, type of active ion (e.g., Li + Against Na + ), operating temperature, etc. In some designs, such suitable domain sizes may range from about 1 nm (10 Å) to about 5 nm (50 Å); in other designs, from about 5 nm to about 10 nm; in yet other designs, from about 10 nm to about 20 nm; and in yet other designs, from about 20 nm to about 40 nm.

[0134] The average scattering domain size of the active material (e.g., in the case of an anode for a Li-ion battery, the Si-based and / or Si-containing active material) in a suitable carbon-containing electrode composite (e.g., composite cathode or anode particle) may preferably (for good performance in the cell) range from about 1 nm to about 40 nm, with the most preferred domain size depending on the composition and microstructure of the composite, the particular cell design, and the cell operating conditions. In some designs, such suitable domain sizes may range from about 1 nm (10 Å) to about 5 nm (50 Å); in other designs, from about 5 nm to about 10 nm; in yet other designs, from about 10 nm to about 20 nm; and in yet other designs, from about 20 nm to about 40 nm.

[0135] FIG. 8 shows exemplary examples of PDF analysis of two carbon-containing anode composites including (i) a suitable carbon (in this example, a suitable porous carbon) used in the formation of a carbon-containing electrode composite and (ii) a Si-based active material. In one exemplary example, the composite domain size is on the order of about 2.5 nm (limited by the Si domain size). In another exemplary example, the domain size is on the order of about 3.5 nm (limited by the Si domain size; the increased Si scattering domain size relative to the first example was due to deviations from the synthesis / processing conditions). Other suitable processing conditions may further increase the Si scattering domain size (e.g., up to 5 nm in some cases, or up to 10 nm in other cases, or up to 20 nm in still other cases, or up to 40 nm in still other cases).

[0136] For perfectly crystalline graphite, the real space central maxima for the three first coordination spheres of carbon are 1.42, 2.45, and 2.85 Å. The first coordination sphere is defined as the sphere bounded by the atoms with the shortest real space distance to the central reference atom. Atoms at real space positions at greater distances from the central reference atom will be encompassed in the second, third, up to n-th coordination spheres, defined by their distance from the central atom. However, these bond lengths or peak central maxima may vary when the structure of carbon is substantially distorted (e.g., as in some porous or structured or partially distorted carbons) or when the structure of the Sp 2 :Sp 3 If the carbon ratio is significantly changed, it may shift substantially. In perfectly crystalline graphite, the ratio of the heights of the real space peaks in the first and second coordination spheres should be equal to 0.5. However, distorted carbons (e.g., depleted or non-hexagonal rings) may show higher ratios. In some designs of suitable carbons (e.g., porous carbons) used for (or used in) the formation of carbon-containing electrode composites (e.g., in the form of composite particles), the synchrotron PDF peak heights and their full width at half maximum (FWHM) in the three first coordination spheres may preferably be within a certain range of values ​​(for good performance in cells). In some designs, the ratio of real space peak heights for the first and second coordination spheres in a suitable carbon (e.g., as a component of a suitable carbon-containing electrode composite) may preferably range from about 0.700 to about 0.590 (about 0.700 to about 0.650 in some designs; about 0.650 to about 0.620 in other designs; and about 0.620 to about 0.590 in still other examples, depending on the chemistry, microstructure, and electrode operating conditions of the composite particle). Such synchrotron XRD measurements and PDF analyses may be performed on either carbon materials (e.g., to select suitable synthesis / processing conditions) or carbon-containing composites (e.g., having Si-based and / or Si-containing active materials, among others) (e.g., to detect the presence or retention of suitable carbon in the composite).

[0137] In perfectly ordered crystalline graphite, the ratio of the FWHM values ​​for the first and second coordination spheres should be 1. In some artificial graphite samples with significant degrees of distortion, such values ​​may be even smaller, such as in the range of about 0.850 to about 0.950. However, in some designs, in suitable carbons, the ratio of the FWHM values ​​may preferably be even smaller (related to certain degrees of variation in bond lengths and distortions that are beneficial to the carbon performance in the composite, and may potentially be related to various distortions such as vacancies, non-membered rings, etc.). In some designs, the ratio of FWHM values ​​for the first and second coordination spheres in suitable carbons may preferably range from about 0.700 to about 0.850 (in some designs, about 0.700 to about 0.760; in other designs, about 0.760 to about 0.810; in still other designs, about 0.810 to about 0.830; in still other designs, about 0.830 to about 0.850), depending on the composite electrode particle active material and composition and electrode operating conditions, among other factors. Such synchrotron XRD measurements and PDF analyses may be performed on either carbon materials (e.g., to select proper synthesis / processing conditions) or carbon-containing composites (e.g., Si-based and / or Si-containing active materials, among others) (e.g., to detect the presence or retention of suitable carbon in the composite).

[0138] For perfectly crystalline graphite, the ratio of the real space peak heights for the first and third coordination spheres should be 1. However, in some designs, the ratio of the real space peak heights for the first and third coordination spheres in suitable carbons may preferably be even larger (which may be related to certain disorders that benefit the carbon performance in the composite, and potentially related to various distortions such as vacancies, non-membered rings, etc.). In some designs, the ratio of the real space peak heights for the first and third coordination spheres in suitable carbons should preferably range from about 1.100 to about 1.300 (in some designs, about 1.100 to about 1.150; in other designs, about 1.150 to about 1.180; in still other designs, about 1.180 to about 1.240; in still other designs, about 1.240 to about 1.300), depending on the composite electrode particle active material and composition and electrode operating conditions, among other factors. Such synchrotron XRD measurements and PDF analyses may be performed on either carbon materials (e.g., to select proper synthesis / processing conditions) or carbon-containing composites (e.g., Si-based and / or Si-containing active materials, among others) (e.g., to detect the presence or retention of suitable carbon in the composite).

[0139] For perfectly ordered crystalline graphite, the ratio of the FWHM values ​​for the first and third coordination spheres should be 1. However, in suitable carbons, the ratio of the FWHM values ​​may preferably be smaller (related to a certain degree of variation in bond lengths and disorder that benefits the carbon performance in the composite, potentially related to various distortions such as vacancies, non-membered rings, etc.). In some designs, the ratio of the FWHM values ​​for the first and third coordination spheres in suitable carbons may preferably range from about 0.600 to about 0.850 (in some designs, about 0.0600 to about 0.700; in some designs, about 0.700 to about 0.760; in other designs, about 0.760 to about 0.810; in still other designs, about 0.810 to about 01830; in still other designs, about 0.830 to about 0.850), depending on the composite electrode particle active material and composition and electrode operating conditions, among other factors. Such synchrotron XRD measurements and PDF analyses may be performed on either carbon materials (e.g., to select proper synthesis / processing conditions) or carbon-containing composites (e.g., having Si-based and / or Si-containing active materials, among others) (e.g., to detect the presence or retention of suitable carbon in the composite).

[0140] FIG. 9A shows an exemplary embodiment of the structural properties of a suitable carbon (e.g., porous carbon in this embodiment) that can be used in the formation of a suitable high-performance carbon-containing electrode composite (e.g., Si-based and / or Si-containing active material). In such an exemplary embodiment, the ratios of the real space peak heights for the first and second coordination spheres in the suitable carbon are: 0.660, 0.625, 0.596, and 0.595. Lower values ​​of the ratio indicate a higher degree of order in the suitable carbon embodiment. The top inset of FIG. 9A shows five-membered, six-membered, and seven-membered rings. Arrows are shown that generally represent the second and third coordination spheres in the case of the six-membered ring. It will be understood that the second and third coordination spheres (as well as the first and higher coordination spheres) can vary in the case of the five-membered and seven-membered rings.

[0141] 9B shows exemplary examples of suitable (e.g., in this example, porous carbon) structural properties that can be used in forming suitable high performance carbon-containing electrode composites (e.g., having Si-based and / or Si-containing active materials). In such exemplary examples, the ratios of FWHM values ​​for the first and second coordination spheres in suitable carbons are 0.773, 0.771, 0.795, 0.814, and 0.830.

[0142] 9C shows an illustrative example of structural properties for a suitable carbon (e.g., in this example, porous carbon) that may be used in forming a suitable high performance carbon-containing electrode composite (e.g., having a Si-based and / or Si-containing active material). In such an illustrative example, the ratios of the real space peak heights for the first and third coordination spheres in the suitable carbon are 1.237, 1.210, 1.194, and 1.230.

[0143] 9D shows an exemplary embodiment of structural properties for a suitable carbon (e.g., in this embodiment, porous carbon) that may be used in forming a suitable high performance carbon-containing electrode composite (e.g., having a Si-based and / or Si-containing active material). In such an exemplary embodiment, the ratio of FWHM values ​​for the first and second coordination spheres in the suitable carbon is 0.657, 0.625, 0.650, 0.695, 0.839.

[0144] Surprisingly, certain values ​​of the relative strength of the C-C bonds in the first coordination sphere in the radial distribution function, R(r), with the case of bonds between C and the active material (e.g., Si-C bonds, Si in the case of Si-based anodes for Li-ion batteries) can be correlated to the performance of carbon-containing and active material-containing composites. Thus, the processing conditions for the formation of such carbon-containing composites can be optimized. In crystalline SiC, the first atom-atom (Si-C) pair is located at about r = 1.9 Å. In crystalline graphite (and many graphitic carbons, even when disordered), the first carbon atom-atom (C-C) pair is located at about r = 1.42 Å, and the second C-C bond is found at about r = 2.47 Å. In crystalline Si, the first atom-atom (Si-Si) pair bond is located at about r = 2.37 Å, which is close to the second C-C bond of graphitic carbon. In composites containing both carbon (C) and Si, the intensity of the corresponding peak in R(r) can be used to optimize performance. However, the first Si-Si bond distance overlaps with the second CC bond distance. In some designs of composites containing both Si and C, the ratio of the intensity of the first SC pair bond to the intensity of the first CC pair bond in R(r) should preferably range from about 0.050 to about 1.000 (in some designs, about 0.050 to about 0.350; in other designs, about 0.350 to about 0.700; in still other designs, about 0.700 to about 1.000). Too large an intensity ratio (e.g., in some examples, substantially above 1.000, e.g., 1.25 or 1.95) can typically cause the cell to have significantly poorer performance (e.g., lower capacity, stability, speed performance, etc.). In general, lower intensity ratio values ​​(reduced Si-C bond formation) are often considered preferable; however, too small an intensity ratio (e.g., substantially lower than about 0.050) may also reduce some aspects of performance (e.g., first cycle efficiency, stability, etc.). Although the first coordination sphere of silicon (at about r=2.37 Å) and the second coordination sphere of graphitic carbon (at about r=2.47 Å) are enmeshed with each other, the location of the real-space peak maximum of this complex peak in composites containing both Si and C may be used for performance optimization during adjustment of synthesis / processing conditions.For example, in some designs, the location of the maximum of this complex peak may preferably range from about 2.375 Å to about 2.425 Å (in some designs, from about 2.375 Å to about 2.395 Å; in other designs, from about 2.395 Å to about 2.405 Å; in yet other designs, from about 2.405 Å to about 2.425 Å). The ratio of the intensity of the complex (first Si-Si and second CC) to the intensity of the first CC peak should preferably be within a certain range for optimal performance of the carbon-based composite with Si as the active material. In some designs, such intensity ratio may preferably range from about 1.500 to about 6.500 (in some designs, from about 1.500 to about 3.000; in other designs, from about 3.000 to about 4.500; in yet other designs, from about 4.500 to about 6.500).

[0145] FIG. 10 shows examples of G(r) for exemplary suitable carbon-containing composites containing Si as the active material. In these particular examples, the ratios of the strength of the first Si-C pair bond to the strength of the first CC pair bond in R(r) are about 0.642 and 0.522, respectively (0.522 provides slightly better performance in this example). In these particular examples, the positions of the maxima of the (first Si-Si and second CC-) complex peaks are about r=2.391 Å and about r=2.385 Å, respectively (r=2.385 Å provides slightly better performance in this example). In these particular examples, the ratios of the intensity of the complex (first Si-Si and second CC) to the intensity of the first CC peak are about 3.333 and 3.363, respectively (a peak intensity ratio of 3.363 provides slightly better performance in this example).

[0146] In some designs, it may be advantageous (with respect to various performance characteristics) for the carbon-containing composite (e.g., composite particle) to exhibit certain spectral signatures as detected in Raman spectroscopy studies. In particular, in some designs, the ratio of the intensities of the carbon D band and the carbon G band (I D / I G ) (e.g., measured using a laser wavelength of about 532 nm; e.g., from about 1000 to about 2000 cm -1 (analyzed by fitting two Gaussian peaks after subtraction of the linear background in this range) has an I of about 0.7. D / I G From about 2.7 I D / I G It is believed to be advantageous to range from about 0.9 to about 2.1 in some designs. Note that these ranges use the ratio of absolute intensities of the D and G peaks (obtained by fitting the spectrum with two G peaks and two D peaks using a Gaussian model and using the intensity / height of the highest G peak and the highest D peak), not the ratio of integrated intensities (area under each of the D and G peaks). However, some designs may use the ratio of integrated intensities (area under the corresponding peaks) of the D and G peaks (obtained by fitting the spectrum with two G peaks and two D peaks using a Gaussian model and using the sum of the areas under both Gaussian model G peaks (I G合計面積 ) and calculate the sum of the areas under both Gaussian model D peaks (I D合計面積 ) and calculate the ratio of these two sums: I D合計面積 / I G合計面積 It is believed that the ratio of (obtained by calculating (a) from (b)) to (c) ranges advantageously from about 0.7 to about 2.7 (or in some designs, 4).

[0147] In some designs, the full width at half maximum (FWHM) of the carbon G band in the Raman spectrum of most carbon-containing composite particles (e.g., measured using a laser wavelength of about 532 nm; e.g., by fitting two Gaussian peaks after linear background subtraction in this range) is between about 1000 and about 2000 cm. -1 (analyzed over a spectral wavenumber range spanning approximately 10 cm -1 About 150cm from -1 (Some designs are approximately 50cm -1 About 100cm from -1 ) is considered advantageous.

[0148] In some designs, sources of carbon for forming suitable carbon-containing composites include, by way of a few illustrative examples and without limitation: (i) various carbon-containing gases (e.g., various hydrocarbons (e.g., CH), among others); 12 , C5H 10 , C5H8, C6H6, etc.) vapors; hydrocarbon gases (e.g., CH4, C2H2, C2H4, C2H6, C3H6, C3H8, C3H4, C4H 10 , C4H8, C4H6, etc., or combinations thereof), (ii) various carbon-containing liquids (e.g., solutions of monosaccharides, disaccharides, and polysaccharides, such as glucose, fructose, galactose, ribose, deoxyribose, sucrose, lactose, maltose, starch, alginates, amylose, amylopectin, glycogen, lignin, among others), crude oil, coal tar pitch, petroleum pitch, bio-pitch and various solutions thereof, vegetable-derived oils, propane, butane, ethane, various olefins, and many other liquid hydrocarbons), and (iii) Various carbon-containing solids (e.g., various nut shells (e.g., coconut shells, apricot shells, almond shells, among others), various pits (e.g., olive pits, cherry kernels, apricot kernels, peach kernels, avocado kernels, among others), various wood and waste wood products (e.g., sawdust), bamboo, grass / straw and (dried) leaves (e.g., banana fiber, rice husks, corn cobs, kelp, among others), coal and various sugars and sugar-containing natural compounds, including monosaccharides, disaccharides and polysaccharides (e.g., glucose, fructose, galactose, ribose, deoxyribose, among others). , sucrose, lactose, maltose, starch, gum arabic, lignin, cellulose, chitin, alginates, amylose, amylopectin, glycogen), various human wastes, various food processing wastes and food wastes, waste paper products, various polymers (e.g., natural glycoproteins and mixtures thereof, phenolic and furfural resins including poly(furfuryl alcohol), rayon, polyethylene, polypropylene, nylon, polyurethane, polylactide, polypropylene, among many other known carbon polymer precursors). glycolide, polyamide, polyaramid, polyethylene terephthalate, polyacrylonitrile, poly(p-phenylene vinylene), various polyoxymethylenes, various vinyl polymers), and various combinations thereof, ammonium (NH3) salts of various metals (e.g., Mg, Al, Si, Zn, Sn, Sb, or Ti, etc.), or various organic acids (e.g., lactic acid, acetic acid, formic acid, citric acid, oxalic acid, uric acid, malic acid, tartaric acid, carboxylic acids, etc.),carboxylic acids, etc., and combinations thereof. In some designs, inorganic residues (e.g., oxides or other) produced by (e.g., thermal) decomposition (by carbonization) of some of such carbon precursors or carbon-containing precursors may be dissolved (e.g., by weak acids) or bases, or in some designs may be converted to active materials (e.g., Si) by known means (e.g., by magnesiothermal reduction of silicon oxide residues and subsequent dissolution into magnesium oxide, or by other suitable means).

[0149] In some designs, carbon-containing composite particles may be produced by first producing porous carbon and then infiltrating the pores with an intercalation-type or transformation-type (including alloy-type) active material. In some designs, such infiltration processes include vapor deposition techniques (such as CVD, atomic layer deposition (ALD), among others) or solution infiltration techniques (including sol-gel or hydrothermal synthesis or layer-by-layer deposition or electrodeposition or electroless deposition or electrophoretic deposition or salt infiltration, among others, followed by solvent evaporation and decomposition or transformation in a controlled environment), or melt infiltration (e.g., infiltration of a precursor or components of a precursor from a melt), or various combination(s) of multiple such techniques (e.g., infiltration of a precursor (e.g., inorganic or metal-based) from a solution or vapor phase or melt). This may be performed by using a reducing (e.g., in H2 or hydrogen-containing gases, e.g., hydrocarbon gases or vapors, among others) or oxidizing (e.g., O or F or Cl or S-containing gases, among others) or neutralizing (e.g., N2 or Ar or He gas or vacuum)) salt infiltration and subsequent annealing or heat treatment in a controlled gaseous environment, which may contain molecules containing fluorine or hydrogen or oxygen or sulfur or phosphorus or lithium or sodium or potassium or calcium atoms, etc. Thus, in some designs, the precursor may first be infiltrated and then converted to the appropriate intercalation-type or pseudocapacitive-type active material, e.g., by heat treatment in a suitable gaseous (or vaporous) environment.

[0150] In some designs, as previously mentioned, an additional shelling (or pore plug) material layer may at least partially close (or coat) the active material, carbon, or entire composite particle. The maximum heat treatment (e.g., in a controlled environment) temperature of such a process during composite formation may vary depending on the nature of the composite and the composition of the intercalation-type active material (e.g., its thermal stability, mobility, reactivity when in contact with carbon, etc.), but in some designs may range from about 100° C. to about 1,100° C. (sometimes from about 300 to about 800° C.). In some designs, multiple heat treatments in various gaseous environments (e.g., first in O or F-containing, then in Ar or N) at various temperatures (e.g., from about 50° C. to about 1,100° C.) or pressures (e.g., from about 0.0001 Torr to 20,000 Torr; in some designs - near atmospheric pressure) and / or for various durations (e.g., from about 0.0001 seconds to about 240 hours) may be accomplished to tailor the material synthesis (e.g., for the formation of a composite with a desired active grain size that resides primarily within the carbon pores, as well as with the desired phases and stoichiometry of active material particles).

[0151] In some designs, synthesis of the carbon-containing composite may include mixing carbon powder (e.g., expanded carbon, graphene, activated carbon, carbon black, dendritic carbon, carbon nanotubes, etc.) with organic carbon precursors (e.g., starch, various sugars, cellulose and cellulose-derived products, alginates and alginate-derived products, pitches (e.g., mesophase, plant-derived pitches, coal tar pitches, etc.) and various components thereof, coal, coal tar, lignin, gum arabic, various other polysaccharides, natural glycoproteins and mixtures thereof, phenolic and furfural resins including poly(furfuryl alcohol), anions, polyethylene, polyacrylonitrile, poly(p-phenylenevinylene), various vinyl polymers, among many other known carbon precursors) and active material (nano)particles (e.g., silicon or silicon oxides or nitrides, as illustrative examples, in the case of the formation of Si-based composites) or active material precursors (e.g., oxides and other salts; including salt solutions) (either in a dry state or in solution / suspension) and carbonizing such mixture to obtain the carbon-containing composite. In some designs, such a mixture may just include an organic carbon precursor (e.g., polymer) and an active material (or active material precursor) (without carbon particles). In examples, the temperature of the carbonization (pyrolysis) or subsequent (e.g., spraying or particle formation) heat treatment may vary depending on the composition of the active material and may range from about 300° C. to about 1200° C. (in some designs, about 450° C. to about 1000° C.). In some designs, higher temperatures may result in undesirable reactions of the active material, or the active material with carbon to form chars and other undesirable compositions. In some designs, lower temperatures may limit the rate performance and capacity of the composite produced.

[0152] In some designs, it may be advantageous to utilize spray drying or spray pyrolysis techniques as at least one of the steps in the composite synthesis. In some designs, it may be advantageous to utilize hydrothermal (or solvothermal) treatment during at least one of the steps in the composite synthesis (e.g., to induce oxidation or crystallization of the precursor at relatively low temperatures without burning / over-oxidizing the carbon). In some designs, it may be advantageous to utilize hydrothermal treatment in combination with thermal treatment in a controlled environment (e.g., reactive environments such as oxygen-containing or fluorine-containing at low temperatures (e.g., from about room temperature to about 350-400°C), or inert at higher temperatures (e.g., from about 400°C to about 600-1200°C depending on the particular chemistry and stability of its active material when in contact with carbon), or both).

[0153] In some designs, the carbon / active material composite particles so produced may be at least partially milled to produce a desired particle size distribution.

[0154] In some designs, the carbon / active material composite particles thus produced may be further (at least partially) encapsulated in a functional shelling (or pore plug) layer (e.g., to increase electrical conductivity, or to increase ionic conductivity, or to increase wettability by the electrolyte, or to prevent undesirable interactions between the electrolyte and the active material, or for other advantageous purposes). In some designs, the shelling material layer may preferentially cover either the active material or the carbon layer (e.g., by having a different wettability or a different nucleation time on the carbon surface than that of the active material). In some designs, the volume fraction of the functional shelling layer may range from about 0.001 vol.% to about 20 vol.% of the volume of the composite particle. In some designs, the functional shelling material layer may also act as the "active" material in terms of its ion storage capacity (e.g., exhibiting a capacity in the range of about 0.1% to about 75% of that of the active material, when expressed in units of capacity per unit mass, mAh / g, or capacity per unit volume, mAh / cc). In some designs, such shelling material layers may be deposited by using vapor deposition techniques (such as CVD, ALD, among others), electrochemical deposition, electrodeposition, electroless deposition, electrophoretic deposition, layer-by-layer deposition, or various other solution-based deposition techniques, or a combination of both solution and vapor deposition. In some designs, after shelling material deposition, the composite may be heat treated (e.g., at a temperature of about 100 to about 1000° C.) in a suitable gaseous environment (e.g., inert gas such as N2 or Ar or He, among others) or vacuum to enhance the properties of the composite. In some designs, the average thickness of the shelling material layer may vary depending on the grain size, ionic and electrical conductivity, and / or other properties of such layer. In some designs, a suitable thickness (e.g., average thickness) of the shelling material layer may range from about 0.2 nm to about 200 nm, although larger thicknesses may be acceptable in some applications (although perhaps at the expense of reduced volumetric capacity of the electrode or reduced electrode porosity). In some designs, the shelling material layer may include carbon (C) (e.g., in some designs, mostly conductive sp-type carbon, such as in graphite or graphitic carbon or turbostratic carbon or mostly amorphous carbon). 2 -bonded carbon). In some designs, solvents containing a variety of carbon atoms or a variety of hydrocarbons (e.g., CH 12 , C5H 10 , C5H8, C6H6, etc.) vapors may be used as precursors for carbon deposition. In some designs, hydrocarbon gases (e.g., CH4, C2H2, C2H4, C2H6, C3H6, C3H8, C3H4, C4H 10 , C4H8, C4H6, etc.) or combinations thereof may be advantageously used as precursors for carbon deposition. In some designs, viscoelastic polymers (including bio-derived ones such as pitch) may be used as precursors for carbon layer formation. In some designs, pitch may be derived from petroleum, coal tar, plants (including wood). In some designs, the shelling material layer may further be a composite of two materials. In some designs, the shelling material may include flake-shaped particles. In some designs, the shelling material may be selected from the following elements: transition, alkali, or alkaline earth metals (e.g., iron (Fe), manganese (Mn), copper (Cu), yttrium (Y), zirconium (Zr), niobium (Nb), molybdenum (Mo), chromium (Cr), lithium (Li), sodium (Na), magnesium (Mg), potassium (K), calcium (Ca), strontium (Sr), cesium (Cs), barium (Ba), among others), lanthanum or lanthanides. The metals may include one or more of the following: (La, Ce, Gd, Nd, Eu, etc.), beryllium (Be), aluminum (Al), silicon (Si), gallium (Ga), germanium (Ge), phosphorus (P), arsenic (As), tin (Sn), bismuth (Bi), lead (Pb), indium (In), cadmium (Cd), zinc (Zn), fluorine (F), iodine (I), oxygen (O), nitrogen (N), sulfur (S), selenium (Se), tellurium (Te), hydrogen (H), and carbon (C). In some designs, the shelling material layer may include a polymer. In some designs, the polymer used in the shelling material layer may exhibit high electrical and / or ionic conductivity (e.g., above about 10 -7 About 10 +4 In such designs, the polymer layer of the shelling material layer may be at least partially carbonized. In some designs, the shelling material layer may include a glass or ceramic layer. In some designs, the glass or ceramic layer may exhibit high electrical and / or ionic conductivity (e.g., in the range of about 10 -7 About 10 +4 In some designs, the shelling material layer may include a metal or metal alloy.

[0155] In some designs, the formation of suitable porous carbon may involve carbonization of a suitable organic precursor (e.g., by thermal annealing or by hydrothermal treatment or other means) followed by chemical or physical activation and / or dissolution or conversion of inorganic residues. In some designs, the formation of so-called hydrocarbons (carbons produced by hydrothermal treatment of hydrocarbon precursors) may be advantageous over other carbonization techniques due to high carbon conversion efficiency, uniform distribution of oxygen in the material, and other favorable features. Suitable examples of hydrochar precursors include, but are not limited to, various nut shells (e.g., coconut shells, apricot shells, almond shells, among others), various pits (e.g., olive pits, cherry kernels, apricot kernels, peach kernels, avocado kernels, among others), various wood and waste wood products (e.g., sawdust), bamboo, grass / straw and (dried) leaves (e.g., banana fiber, rice husks, corn cobs, kelp, among others), various human waste, various food processing wastes and food waste, waste paper products, coal and coal tar pitch, petroleum pitch, crude oil, various sugars including monosaccharides, disaccharides and polysaccharides (glucose, fructose, galactose, ribose, deoxyribose, sucrose, lactose, maltose, starch, lignin, cellulose, amylose, amylopectin, glycogen, among other suitable precursors). In some designs, the hydrochar may be annealed in an inert environment (e.g., in vacuum, or in N2 or Ar or He gas, etc.) prior to (e.g., first) activation. Suitable temperatures may range from about 500° C. to about 2000° C. depending on the precursor and the desired porosity after activation. In some designs, heat treatment at temperatures below about 500° C. is believed to have little effect on activation and not remove (desired) amounts of impurities (e.g., as effluent(s)). In some designs, heat treatment at temperatures above about 2000° C. is very effective in obtaining high purity material, but may prevent high BET SSA from being achieved and may prevent the retention of (sometimes desirable) small pores after activation.

[0156] In some designs, it may be advantageous to use so-called physical activation techniques (such as activation in CO2 or H2O or both streams, among others) to induce additional pores and increase the pore volume and surface area of ​​the carbon produced by carbonization. Suitable activation temperatures may vary depending on the type of carbon and its pretreatment history. However, by way of example, suitable temperatures may range from about 700°C to about 1300°C (-800 to about 1150°C in some designs). By way of example, temperatures higher than about 1300°C may make the activation process very difficult to control to the desired uniformity and may further induce undesirable pore size distribution in the carbon. In another example, temperatures lower than about 700°C may make the activation process too slow to achieve the desired pore size and surface area characteristics in the produced activated carbon.

[0157] In some designs, the formation of suitable porous carbon (eg, when obtaining larger pore volumes) may involve the use of a sacrificial template material prior to carbonization and activation.

[0158] In some designs, the formation of so-called hydrochar (carbon produced by hydrothermal treatment of hydrocarbon precursors, including various biomaterials such as shells, wood waste, etc.) may be advantageous prior to activation.

[0159] In some designs, the carbon precursor may be annealed in an inert environment (e.g., in vacuum, N2 or Ar or He gas, etc.) prior to activation. In some designs, suitable temperatures may range from about 500°C to about 2800°C, depending on the precursor and the desired porosity after activation (in some designs, about 500°C to about 800°C; in other designs, about 800°C to about 1200°C; in still other designs, about 1200°C to about 1600°C; in still other designs, about 1600°C to about 2000°C; in still other designs, about 2000°C to about 2800°C). In some designs, heat treatment at temperatures below about 500°C may have little effect on activation and may not remove as much impurity (e.g., effluent(s)) as is sometimes desired. In some designs, heat treatment at temperatures above about 2800° C. is very effective in obtaining high purity material, but can prevent achieving high BET SSA and forming small pores after activation (which is sometimes desired).

[0160] In some designs, chemical activation may be used instead of or in addition to physical activation. Examples of suitable chemical activators include, but are not limited to, KOH, NaOH, ZnCl2, H3PO4, K2CO3, or H2SO4. In some designs, the carbonization step proceeds simultaneously with chemical activation. In other designs, after carbonization of the precursor, the resulting carbon may then be mixed with a chemical activator, heat treated to activate, and then purified.

[0161] In some designs (e.g., to maximize rate performance or battery stability), the porous carbon may be annealed in an inert environment (e.g., in vacuum or in N2 or Ar or He gas, etc.) after activation. The annealing process may provide additional purification, may increase the electrical conductivity of the carbon, may increase the mechanical properties of the carbon, may reduce the number of nucleation sites (for active material deposition), and may provide reduced self-discharge and other performance benefits to the cell (e.g., battery rate, battery stability, etc.). In some designs, suitable temperatures may range from about 800°C to about 2800°C, depending on the precursor and the desired porosity after activation (in some designs, about 800°C to about 1200°C; in still other designs, about 1200°C to about 1400°C; in still other designs, about 1400°C to about 1800°C; in still other designs, about 1800°C to about 2800°C). In some designs, heat treatment at temperatures below about 800° C. may have little effect on the infiltration of active material into the porous structure or on the bonding of active material with the carbon, or on the conductivity or purity of the carbon. In some designs, heat treatment at temperatures above about 2800° C. may prevent the realization of high BET SSA and may induce excessive pore closers after activation.

[0162] In some designs, the porous carbon may be annealed and activated more than once (e.g., two or three or more times) to obtain the most desired characteristics for use in carbon-containing electrode composites. In some designs, different heat treatment (annealing) temperatures may be purposefully used prior to the different activation procedures.

[0163] In some designs, electrodes containing conversion-type (including alloy-type or metal-type) active materials or intercalation-type or pseudocapacitive-type active materials may be advantageously prepared in certain ways or contain certain conductive or other additives.

[0164] In some designs, it may be advantageous to use nanoparticles (e.g., carbon black, including those that include carbon particles linked into larger aggregates) or one-dimensional (1D) conductive additives (e.g., single-walled carbon nanotubes, double-walled carbon nanotubes, multi-walled carbon nanotubes, carbon (nano)fibers, compatible metal nanofibers, nanotubes and nanowires, etc. (e.g., copper, nickel, titanium, iron nanowires / nanofibers, aluminum nanowires / nanofibers, nickel nanowires / nanofibers, etc.)), or combinations thereof, in electrodes that include carbon-containing composite electrode materials.

[0165] In some designs, it may be advantageous to attach the conductive additive to the (nano)composite electrode particles by several mechanisms. In one example, the conductive additive (e.g., carbon nanotubes or graphene or metal nanoparticles or metal nanowires) may be directly on the surface of the electrode particles (e.g., by CVD or by solution chemical route). In another example, the conductive particles (of various shapes and sizes) may be strongly attached to the surface of the electrode particles by charging the surface of each (or most) particle(s) and using an opposite charge on the electrode particles as the conductive additive particles. In yet another example, the conductive particles may be attached to the surface of the electrode particles by using an organic (e.g., polymer) binder and by carbonizing the binder, which forms a conductive carbon interlayer (e.g., effectively acting as a conductive glue) between the conductive additive(s) and the electrode particle(s). In yet another example, a carbon layer may be CVD-deposited on the mixture of conductive additive particles and active electrode particles, thereby preferentially depositing carbon at the contact points between the electrode particles and the conductive additive. In an embodiment, the CVD carbon layer may act similarly to a conductive glue to strongly attach the conductive additive(s) to the electrode particle(s).

[0166] In some designs, the optimal weight percentage of the slurry components, given as the ratio of the mass of the inactive components to the external surface area of ​​the composite electrode particles, is from about 1 to about 5,000 m 2 Values ​​ranging from about 5 to about 200 m activity / g inactivity may be observed. 2 In some designs, the optimal weight percentage of the slurry components for a particular electrode composition may depend on the size of the active particles, the type of conductive additive, the surface chemistry of the conductive additive, the surface chemistry of the active particles, the density of the particles, the volume change during cycling, the type and molecular weight of the binder(s), the thickness of the electrode, the density of the electrode, and / or other parameters.

[0167] In some applications, it may be advantageous to induce opposite charges on the surfaces of the conductive additive and the (composite) electrode particles to increase their contact area and strength and to achieve a more uniform mixture. For example, a positive charge may be introduced on the surface of the composite particles and a negative charge may be introduced on the surface of the conductive additive. In another example, a negative charge may be introduced on the surface of the composite particles and a positive charge may be introduced on the surface of the conductive additive. In some applications, it may be advantageous to induce a chemical reaction between the conductive additive and the electrode particles during or after electrode drying.

[0168] In some designs, it may be advantageous to use multiple types of conductive additives (e.g., with various dimensions, aspect ratios, or morphologies) for the most optimal performance. In some designs, it may be even more advantageous to chemically bond one type of conductive additive to the surface of the electrode particles. In this case, as an example, the requirement for lack of swelling to maintain the stability of the electrode particle / conductive additive interface may be substantially reduced or even completely avoided. In one example, short (e.g., about 0.01-10 microns) carbon nanofibers, carbon nanotubes, or graphene / graphite ribbons may be grown (e.g., by using catalytically assisted vapor deposition, CVD, or other mechanisms) from the surface of the electrode particles. In another example, a mixture of conductive carbon additive particles (e.g., carbon black, carbon nanotubes, etc.) with one charge and the electrode particles with the opposite charge may be further mixed with a small sacrificial binder content and then carbonized. In some designs, the carbonized binder may firmly and permanently attach some of the carbon additive to the surface of the electrode particles. In examples, such electrode particle / carbon additive composites may be used in slurries with various suitable binders and additional conductive additives (e.g., as applicable in the context of one or more embodiments of the present disclosure) to form (or mold) more stable electrodes that experience moderate volume changes during cycling.

[0169] In some applications, it may be advantageous to use two or more conductive additives with different surface charges or different surface chemistries. In particular, in some designs, when one type of additive exhibits a higher affinity for the electrode particles, such additive may be selected to form a uniform coating around the electrode particles. In some designs, such additives may be selected to form chemical bonds with the electrode particles at some stage of electrode assembly or slurry preparation. As an example, the second additive may be incorporated into the binder at a significantly higher percentage than the first additive, and thus optimized to form a robust and uniform binder / additive (nano)composite resulting in a stable electrode.

[0170] In some applications, the two or more additives may be selected to perform different functions. In one example, one type of additive (e.g., having larger dimensions or higher conductivity, e.g., carbon nanofibers, other conductive nanofibers, long (e.g., having lengths greater than about 10 microns) carbon nanotubes, graphite, or graphene flakes having linear dimensions greater than about 5-10 microns, other conductive flakes, metal nanowires, etc.) may be selected to provide higher electrical conductivity within the electrode as a whole, while a second type of conductive additive (e.g., carbon black and other conductive nanoparticles, shorter (e.g., having average lengths of about 0.25-10 microns) carbon nanotubes or conductive nanowires or (e.g., chopped) conductive nanofibers, smaller graphene or graphite flakes, shorter graphite ribbons, etc.) may be selected to ensure that each individual electrode particle is effectively electrically connected to multiple adjacent electrode particles and the first type of additive, thereby forming an efficient conductive network that results in high volume utilization of the electrode material. In another example, one type of additive may be selected to perform multiple functions (e.g., to increase both the conductivity and mechanical stability of the electrode, or to increase the conductivity of the electrode and provide a faster ion path (e.g., if porous or to prevent closure of the electrode pores)). In some designs, one type of conductive additive may aid in better dispersion of a second type during slurry mixing.In particular, in some designs, it may be advantageous to use a mixture of two of the following types of conductive additives in the same slurry: (i) various types of single-walled carbon nanotubes (SWCNTs), with or without a surface coating; (ii) various types of double-walled (DWCNTs), triple-walled (TWCNTs), and other types of multi-walled carbon nanotubes (MWCNTs), with or without a surface coating; (iii) various types of carbon blacks, including those annealed above 1000° C. in an inert environment; (iv) various types of carbon fibers, including those annealed above 1000° C. in an inert environment; (v) various types of carbon nanofibers; (vi) various types of metal nanowires, with or without a protective or functional surface coating layer (e.g., Cu, Fe, Ti, or Ni for low potential anodes in Li-ion batteries, such as anodes containing Si). nanowires; such as Al nanowires for the cathode or high voltage anode of Li-ion batteries, or other nanowires for various aqueous batteries (e.g., Ni or Ti nanowires); (vii) various types of carbon-coated or metal (e.g., Cu, Fe, Ni, Ti, or Al) coated ceramic nanowires or fibers (e.g., Al2O3 nanowires or fibers); (viii) various types of carbon onions; (ix) various types of graphite ribbons (including metal-coated graphite ribbons); (x) various types of metal (e.g., Cu, Fe, Ni, Ti, or Al) nanoparticles (with or without a protective or functional surface layer coating); and (xi) various types of metal (e.g., Cu, Fe, Ni, Ti, or Al) (nano)flakes (with or without a protective or functional surface layer coating). In some designs, the surface chemistry of each type of such additive can be individually optimized for optimal performance in the cell.

[0171] In some applications, it may be advantageous to limit the overall volume fraction of all conductive additive particles in the electrode to less than about 5% by volume (even more preferably, below about 2% by volume). In some designs, the percentage of all conductive additive particles in the electrode by mass may be preferably less than about 7% by weight (e.g., even more preferably, below about 3% by weight) when only carbon materials are used as conductive additives, and less than about 10% by weight (e.g., even more preferably, below about 5% by weight) when part of the conductive additive comprises a suitable metal. In examples, a higher volume fraction of conductive additives may reduce the ion transport and volumetric capacity of the electrode, and may increase the scope of undesirable side reactions. In further examples, a higher weight (mass) fraction of conductive additives may reduce the specific capacity of the electrode.

[0172] In the above detailed description, it is seen that various features are grouped together in the embodiments. This disclosure approach should not be understood as intending that the exemplary items have more features than are expressly stated in each item. Rather, various aspects of the present disclosure may include less than all features of each exemplary item disclosed. Thus, the following items should be considered hereby incorporated into this description, and each item can stand on its own as a separate embodiment. Although each dependent item may refer to a specific combination with one of the other items within that item, the aspect(s) of that dependent item are not limited to a specific combination. It will be understood that other exemplary items may also include combinations of the aspect(s) of the dependent item with the subject matter of any other dependent item or independent item, or combinations of any feature with other dependent and independent items. Various aspects disclosed herein expressly include these combinations unless expressly expressing or readily inferring that a particular combination is not intended (e.g., inconsistent aspects such as defining an element as both an insulator and a conductor). It is further contemplated that aspects of an item may be included in any other independent item, even if that item is not directly dependent on the independent item.

[0173] An implementation is described in the following numbered items:

[0174] Item 1. A lithium ion battery anode composition comprising porous composite particles comprising carbon (C) and an active material comprising silicon (Si), wherein the carbon is characterized by a domain size (r) as estimated from an atomic pair correlation function G(r) obtained from synchrotron X-ray diffraction measurements of the porous composite particles ranging from about 10 Å (1 nm) to about 60 Å (6 nm).

[0175] Item 2. The lithium ion battery anode composition of item 1, wherein the carbon is characterized by one or more of the following: (1) domain sizes ranging between about 15 Å and about 19 Å, (2) domain sizes ranging between about 19 Å and about 22 Å, (3) domain sizes ranging between about 24 Å and about 28 Å, and (4) domain sizes ranging between about 28 Å and 55 Å, the domain sizes as estimated from an atomic pair correlation function, G(r).

[0176] Item 3. The lithium ion battery anode composition of any of items 1 to 2, wherein the carbon comprises porous carbon.

[0177] Item 4. The lithium ion battery anode composition of any of items 1 to 3, wherein G(r=r1) is the value of the atomic pair correlation function at the real space positions of the first coordination sphere of carbon, G(r=r2) is the value of the atomic pair correlation function at the real space positions of the second coordination sphere of carbon, and the ratio G(r=r1) / G(r=r2) is in the range of about 0.700 to about 0.590.

[0178] Item 5. The lithium ion battery anode composition of any of items 1 to 4, wherein W(r=r1) is the value of the full width at half maximum of the atomic pair correlation function at real space positions in the first coordination sphere of carbon, W(r=r2) is the value of the full width at half maximum of the atomic pair correlation function at real space positions in the second coordination sphere of carbon, and the ratio W(r=r1) / W(r=r2) is in the range of about 0.700 to about 0.850.

[0179] Item 6. The lithium ion battery anode composition of any of items 1 to 5, wherein G(r=r1) is the value of the atomic pair correlation function at the real space positions of the first coordination sphere of carbon, G(r=r3) is the value of the atomic pair correlation function at the real space positions of the third coordination sphere of carbon, and the ratio G(r=r1) / G(r=r3) is in the range of about 1.100 to about 1.300.

[0180] Item 7. The lithium ion battery anode composition of any of items 1 to 6, wherein W(r=r1) is the value of the full width at half maximum of the atomic pair correlation function at real space positions in the first coordination sphere of carbon, W(r=r3) is the value of the full width at half maximum of the atomic pair correlation function at real space positions in the third coordination sphere of carbon, and the ratio W(r=r1) / W(r=r3) is in the range of about 0.600 to about 0.850.

[0181] Item 8. An anode comprising the anode composition has a capacity of about 2 mAh / cm 2 to about 16mAh / cm 2 8. The lithium ion battery anode composition of any of items 1 to 7, exhibiting an areal capacity loading ranging from

[0182] Item 9. The lithium ion battery anode composition of item 8, wherein about 10% to about 100% of the areal capacity loading of the anode is provided by composite particles each configured as a porous composite particle.

[0183] Item 10. The lithium ion battery anode composition of any of items 8 to 9, wherein the composite particles exhibit a weight ratio of silicon (Si) to carbon (C) ranging from about 5:1 to 1:5 on average.

[0184] Item 11. The lithium ion battery anode composition of any of items 1 to 10, wherein the porous composite particles are characterized by an average scattering domain size (r) as estimated from the atomic pair correlation function G(r), ranging from about 1 nm to about 40 nm.

[0185] Item 12. The lithium ion battery anode composition of item 11, wherein the porous composite particles are characterized by an average scattering domain size (r) ranging from about 1 nm to about 10 nm.

[0186] Item 13. The lithium ion battery anode composition of any of items 1 to 12, wherein the porous composite particles contain, on average, less than about 1 wt. % hydrogen (H), less than about 5 wt. % nitrogen (N), and less than about 2 wt. % oxygen (O).

[0187] Item 14. The lithium ion battery anode composition of any of items 1 to 13, wherein the porous composite particles exhibit, on average, about 1.5% by weight to about 25% by weight of nitrogen (N) uptake when heated in nitrogen gas (N2) at 1050° C. for 2 hours, as measured on a powder containing the porous composite particles.

[0188] Item 15. The lithium ion battery anode composition of any of items 1 to 14, wherein the porous composite particles exhibit an average uptake of nitrogen (N) of about 0.5% by weight to about 10% by weight when heated in nitrogen gas (N2) at 850°C for 2 hours, as measured on a powder comprising the porous composite particles.

[0189] Item 16. The lithium ion battery anode composition of any of items 1 to 15, wherein the porous composite particles form about 1% by weight to about 100% by weight of silicon carbide (SiC) when heated in nitrogen gas (N2) or argon gas (Ar) at a temperature range of about 750°C to about 950°C for 2 hours or longer, as detected by X-ray diffraction (XRD) or Fourier transform infrared spectroscopy (FTIR).

[0190] Item 17. The porous composite particles have a molecular weight of about 1 to about 40 m when measured using a nitrogen adsorption isotherm on a powder containing the porous composite particles. 2 17. Any of the lithium ion battery anode compositions of items 1 to 16, wherein the lithium ion battery anode composition exhibits an average Brunauer-Emmett-Teller (BET) specific surface area in the range of 1 / g.

[0191] Item 18. The porous composite particles have a particle size of about 0.9 g / cm when measured using nitrogen or argon pycnometry on a powder containing the porous composite particles. 3 to about 2.2 g / cm 3 18. The lithium ion battery anode composition of any of items 1 to 17, wherein the composition exhibits an average density in the range of

[0192] Item 19. The lithium ion battery anode composition of any of items 1 to 18, wherein the porous composite particles exhibit a volume average particle size in the range of about 0.2 microns to about 20 microns when measured using scanning electron microscope (SEM) image analysis or particle scattering techniques on a powder comprising the porous composite particles.

[0193] Item 20. The lithium ion battery anode composition of any of items 1 to 19, wherein the Raman spectrum of the porous composite particles exhibits carbon D and G peaks, and the ratio of the average intensity of the D peak to the G peak (ID / IG) ranges from about 0.7 to about 2.7.

[0194] Item 21. A Li-ion battery comprising an anode comprising the lithium-ion battery anode composition of any of items 1 to 20, a cathode electrically isolated from the anode, and an electrolyte ionically connecting the anode and the cathode.

[0195] Item 22. The Li-ion battery of item 21, having a battery capacity ranging from about 0.2 Ah to about 400 Ah.

[0196] Item 23. R(r = rSi-C) is the value of the radial distribution function R(r) at the real space position of the first coordination sphere of the Si-C pair in the porous composite particle, R(r = rC-C) is the value of the radial distribution function R(r) at the real space position of the first coordination sphere of the C-C pair in the porous composite particle, and the radial distribution function R(r) and the atomic pair correlation function are R(r) = R(r) = G(r)r + 4πr 2 23. Any of the Li-ion batteries of items 21 to 22, related by ρ0, where ρ0 is a constant related to the number density of the scatterers, and the ratio R(r=rSi-C) / R(r=rC-C) is in the range of 0.050 to about 1.000.

[0197] Item 24. A carbon material for use in preparing an anode composition for use in a Li-ion battery, the carbon material being characterized by a domain size (r) as estimated from an atomic pair distribution function G(r) obtained from synchrotron X-ray diffraction measurement of the carbon material ranging from about 10 Å (1 nm) to about 60 Å (6 nm).

[0198] Item 25. The carbon material of item 24, wherein the domain size (r) is one of the following: (1) a first domain size ranging from about 15 Å to about 19 Å, (2) a second domain size ranging from about 19 Å to about 22 Å, (3) a third domain size ranging from about 24 Å to about 28 Å, and (4) a fourth domain size ranging from about 40 Å to 55 Å.

[0199] Item 26. The carbon material of any one of items 24 to 25, wherein the carbon material comprises porous carbon.

[0200] Item 27. Any of the carbon materials of items 24 to 26, wherein G(r=r1) is the value of an atomic pair correlation function at a real space position in the first coordination sphere of the carbon material, G(r=r2) is the value of an atomic pair correlation function at a real space position in the second coordination sphere of the carbon material, and the ratio G(r=r1) / G(r=r2) is in the range of about 0.700 to about 0.590.

[0201] Item 28. Any of the carbon materials of items 24 to 27, wherein W(r=r1) is a value of the full width at half maximum of the atomic pair correlation function at a real space position in the first coordination sphere of the carbon material, W(r=r2) is a value of the full width at half maximum of the atomic pair correlation function at a real space position in the second coordination sphere of the carbon material, and the ratio W(r=r1) / W(r=r2) is in the range of about 0.700 to about 0.850.

[0202] Item 29. Any of the carbon materials of items 24 to 28, wherein G(r=r1) is the value of an atomic pair correlation function at a real space position in the first coordination sphere of the carbon material, G(r=r3) is the value of an atomic pair correlation function at a real space position in the third coordination sphere of the carbon material, and the ratio G(r=r1) / G(r=r3) is in the range of about 1.100 to about 1.300.

[0203] Item 30. Any of the carbon materials of items 24 to 29, wherein W(r=r1) is a value of the full width at half maximum of the atomic pair correlation function at a real space position in the first coordination sphere of the carbon material, W(r=r3) is a value of the full width at half maximum of the atomic pair correlation function at a real space position in the third coordination sphere of the carbon material, and the ratio W(r=r1) / W(r=r3) is in the range of about 0.600 to about 0.850.

[0204] The present description is provided to enable any person skilled in the art to make or use embodiments of the invention. It will be understood, however, that the invention is not limited to the specific formulations, process steps, and materials disclosed herein, since various modifications of these embodiments will be readily apparent to those skilled in the art. That is, the generic principles defined herein may be applied to other embodiments without departing from the spirit or scope of the invention.

Claims

1. The porous composite particle includes carbon (C) and an active material includes silicon (Si), 1. A lithium ion battery anode composition, wherein the carbon is characterized by a domain size (r) estimated from an atomic pair distribution function G(r) obtained from synchrotron x-ray diffraction measurements of the porous composite particles ranging from about 10 Å (1 nm) to about 60 Å (6 nm).

2. the carbon is characterized by one or more of the following: (1) a domain size in the range of about 15 Å to about 19 Å, (2) a domain size in the range of about 19 Å to about 22 Å, (3) a domain size in the range of about 24 Å to about 28 Å, and (4) a domain size in the range of about 28 Å to 55 Å; The domain size is estimated from the atomic pair distribution function G(r).

10. The lithium ion battery anode composition of claim 1.

3. 10. The lithium ion battery anode composition of claim 1, wherein the carbon comprises porous carbon.

4. G(r=r 1 ) is the value of the atomic pair correlation function at a real space position of the first coordination sphere of the carbon; G(r=r 2 ) is the value of the atomic pair correlation function at a real space position of the second coordination sphere of the carbon; Ratio G (r=r 1 ) / G(r = r 2 ) is in the range of about 0.700 to about 0.590; 10. The lithium ion battery anode composition of claim 1.

5. W(r=r 1 ) is the full width at half maximum value of the atomic pair correlation function at the real space position of the first coordination sphere of the carbon; W(r=r 2 ) is the full width at half maximum value of the atomic pair correlation function at the real space position of the second coordination sphere of the carbon; Ratio W(r=r 1 ) / W(r = r 2 ) is in the range of about 0.700 to about 0.850; 10. The lithium ion battery anode composition of claim 1.

6. G(r=r 1 ) is the value of the atomic pair correlation function at a real space position of the first coordination sphere of the carbon; G(r=r 3 ) is the value of the atomic pair correlation function at a real space position of the third coordination sphere of the carbon; Ratio G (r=r 1 ) / G(r = r 3 ) is in the range of about 1.100 to about 1.300; 10. The lithium ion battery anode composition of claim 1.

7. W(r=r 1 ) is the full width at half maximum value of the atomic pair correlation function at the real space position of the first coordination sphere of the carbon; W(r=r 3 ) is the full width at half maximum value of the atomic pair correlation function at the real space position of the third coordination sphere of the carbon, Ratio W(r=r 1 ) / W(r = r 3 ) is in the range of about 0.600 to about 0.850; 10. The lithium ion battery anode composition of claim 1.

8. The anode comprising the anode composition has a capacitance of about 2 mAh / cm 2 to about 16 mAh / cm 2 13. The lithium ion battery anode composition of claim 1, which exhibits an areal capacity loading in the range of

9. 10. The lithium ion battery anode composition of claim 8, wherein about 10% to about 100% of the areal capacity loading of the anode is provided by composite particles each configured as the porous composite particles.

10. 9. The lithium ion battery anode composition of claim 8, wherein the composite particles exhibit an average weight ratio of silicon (Si) to carbon (C) ranging from about 5:1 to 1:

5.

11. 10. The lithium ion battery anode composition of claim 1, wherein the porous composite particles are characterized by an average scattering domain size (r) estimated from an atomic pair distribution function G(r) in the range of about 1 nm to about 40 nm.

12. 12. The lithium ion battery anode composition of claim 11, wherein the porous composite particles are characterized by an average scattering domain size (r) in the range of about 1 nm to about 10 nm.

13. 2. The lithium ion battery anode composition of claim 1, wherein the porous composite particles contain, on average, less than about 1 wt. % hydrogen (H), less than about 5 wt. % nitrogen (N), and less than about 2 wt. % oxygen (O).

14. The porous composite particles are heated to 1050° C. on average in nitrogen gas (N 2 2. The lithium ion battery anode composition of claim 1, wherein a powder comprising said porous composite particles exhibits a nitrogen (N) uptake of about 1.5% to about 25% by weight when heated in a 200 MPa (100 MPa) atmosphere for 2 hours.

15. The porous composite particles are heated to 850° C. in nitrogen gas (N 2 2. The lithium ion battery anode composition of claim 1, wherein the composition exhibits an average nitrogen (N) uptake of about 0.5% to about 10% by weight as measured on a powder comprising the porous composite particles when heated in a 200 MPa (100 MPa) atmosphere for 2 hours.

16. The porous composite particles are heated in nitrogen gas (N ) at a temperature range of about 750° C. to about 950° C. as detected by X-ray diffraction (XRD) or Fourier transform infrared spectroscopy (FTIR). 2 13. The lithium ion battery anode composition of claim 1, which forms about 1 wt. % to about 100 wt. % silicon carbide (SiC) when heated in nitrogen or argon gas (Ar) for 2 hours or longer.

17. The porous composite particles have a particle size of about 1 m as measured using a nitrogen adsorption isotherm on a powder including the porous composite particles. 2 / g to about 40m 2 13. The lithium ion battery anode composition of claim 1, exhibiting an average Brunauer-Emmett-Teller (BET) specific surface area in the range of 100 / g.

18. The porous composite particles have a density of about 0.9 g / cm as measured using nitrogen or argon pycnometry on a powder including the porous composite particles. 3 to about 2.2 g / cm 3 13. The lithium ion battery anode composition of claim 1 , which exhibits an average density in the range of

19. 10. The lithium ion battery anode composition of claim 1, wherein the porous composite particles exhibit a volume average particle size in the range of about 0.2 microns to about 20 microns as measured using scanning electron microscope (SEM) image analysis or particle scattering techniques on a powder comprising the porous composite particles.

20. The Raman spectrum of the porous composite particle exhibits carbon D and G peaks, and the ratio of the average intensities of the D and G peaks (I D / I G 2. The lithium ion battery anode composition of claim 1, wherein Mn is in the range of about 0.7 to about 2.

7.

21. an anode comprising the lithium ion battery anode composition of claim 1; a cathode electrically isolated from the anode; an electrolyte ionically connecting the anode and the cathode; A Li-ion battery comprising:

22. 22. The Li-ion battery of claim 21, wherein the battery capacity ranges from about 0.2 Ah to about 400 Ah.

23. R (r = r Si-C ) is the value of the radial distribution function R(r) at the real space position of the first coordination sphere of the Si—C pair in the porous composite particle; R (r = r C-C ) is the value of the radial distribution function R(r) at the real space position of the first coordination sphere of the C—C pair in the porous composite particle, The radial distribution function R(r) and the atomic pair correlation function are R(r)=G(r)r+4πr 2 ρ 0 and ρ 0 is a constant related to the number density of scatterers, and the ratio R (r = r Si-C ) / R (r = r C-C 22. The Li-ion battery of claim 21 , wherein R is in the range of 0.050 to about 1.

000.

24. 1. A carbon material for use in making an anode composition for use in a Li-ion battery, said carbon material being characterized by a domain size (r) estimated from an atomic pair distribution function G(r) obtained from a synchrotron x-ray diffraction measurement of said carbon material in the range of about 10 Å (1 nm) to about 60 Å (6 nm).

25. 25. The carbon material of claim 24, wherein the domain size (r) corresponds to one of the following: (1) a first domain size ranging from about 15 Å to about 19 Å, (2) a second domain size ranging from about 19 Å to about 22 Å, (3) a third domain size ranging from about 24 Å to about 28 Å, and (4) a fourth domain size ranging between about 40 Å and 55 Å.

26. The carbon material of claim 24 , wherein the carbon material comprises porous carbon.

27. G(r=r 1 ) is the value of the atomic pair correlation function at a real space position of the first coordination sphere of the carbon material; G(r=r 2 ) is the value of the atomic pair distribution function at a real space position of the second coordination sphere of the carbon material; Ratio G (r=r 1 ) / G(r = r 2 25. The carbon material of claim 24, wherein the MnO2 content is in the range of about 0.700 to about 0.

590.

28. W(r=r 1 ) is the full width at half maximum value of the atomic pair correlation function at a real space position of the first coordination sphere of the carbon material; W(r=r 2 ) is the full width at half maximum of the atomic pair correlation function at a real space position of the second coordination sphere of the carbon material; Ratio W(r=r 1 ) / W(r = r 2 25. The carbon material of claim 24, wherein the MnO2 content is in the range of about 0.700 to about 0.

850.

29. G(r=r 1 ) is the value of the atomic pair correlation function at a real space position of the first coordination sphere of the carbon material; G(r=r 3 ) is the value of the atomic pair correlation function at a real space position of the third coordination sphere of the carbon material; Ratio G (r=r 1 ) / G(r = r 3 25. The carbon material of claim 24, wherein Mn is in the range of about 1.100 to about 1.

300.

30. W(r=r 1 ) is the full width at half maximum value of the atomic pair correlation function at a real space position of the first coordination sphere of the carbon material; W(r=r 3 ) is the full width at half maximum value of the atomic pair correlation function at a real space position of the third coordination sphere of the carbon material; Ratio W(r=r 1 ) / W(r = r 3 25. The carbon material of claim 24, wherein the MnO2 content is in the range of about 0.600 to about 0.850.

Citation Information

Patent Citations

  • Method for controlling terminal with earphone cable, apparatus, device, program and recording medium for controlling terminal with earphone cable

    JP2016502723A

  • Positive electrode active material for lithium ion secondary battery, method for preparing the same, positive electrode sheet for lithium ion secondary battery, and lithium ion secondary battery

    JP2016526262A

  • Electroactive Materials for Metal-Ion Batteries

    JP2022533387A

Cited By

  • Computing device, method and program

    JP7716143B1