Jelly roll electrode assembly and cylindrical lithium secondary battery including the same

The jelly roll electrode assembly addresses the issue of wrinkles and resistance in conventional cylindrical lithium secondary batteries by using protective tapes on the uncoated areas of the negative electrode current collector, ensuring proper contact and enhancing battery performance and safety.

JP2024535796AActive Publication Date: 2024-10-02LG ENERGY SOLUTION LTD

Patent Information

Application Number
JP2024515725
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-08
Filing Date
2022-12-07
Publication Date
2024-10-02
Estimated Expiration
2042-12-07

AI Technical Summary

Technical Problem

Conventional cylindrical lithium secondary batteries face issues with increased resistance and wrinkle formation in the jelly roll electrode assembly due to inadequate contact between the Cu foil and the battery outer can, particularly when the Cu foil serves as the negative electrode current collector, leading to variations in resistance and potential wrinkles during winding.

Method used

A jelly roll electrode assembly is designed with a negative electrode current collector that includes a negative electrode active material-coated and uncoated parts, featuring protective tapes on at least one side of the uncoated areas, adhering to a specific coverage ratio, to provide rigidity and prevent wrinkles during winding.

Benefits of technology

The assembly effectively prevents wrinkles, enhancing the life and efficiency of the cylindrical lithium secondary battery by ensuring proper contact and reducing resistance, thereby improving the overall performance and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024535796000001_ABST
    Figure 2024535796000001_ABST
Patent Text Reader

Abstract

The present application relates to a jelly roll electrode assembly and a cylindrical lithium secondary battery including the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of the filing date of Korean Patent Application No. 10-2021-0174846, filed with the Korean Intellectual Property Office on December 8, 2021, the entire contents of which are incorporated herein by reference.

[0002] The present application relates to a jelly roll electrode assembly and a cylindrical lithium secondary battery including the same. [Background technology]

[0003] The rapid increase in the use of fossil fuels has led to an increased demand for alternative and clean energy, and one of the most actively researched fields in this area is the field of power generation and storage using electrochemical reactions.

[0004] At present, a representative example of an electrochemical element that uses such electrochemical energy is a secondary battery, and the range of its use is tending to expand more and more.

[0005] As technological development and demand for mobile devices increases, the demand for secondary batteries as energy sources is rapidly increasing. Among such secondary batteries, lithium secondary batteries, which have high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used. In addition, research into methods for manufacturing high-density electrodes with higher energy density per unit volume as electrodes for such high-capacity lithium secondary batteries is being actively conducted.

[0006] In general, a secondary battery is composed of a positive electrode, a negative electrode, an electrolyte, and a separator. The negative electrode contains a negative electrode active material that inserts and removes lithium ions released from the positive electrode. Silicon-based particles having a large discharge capacity can be used as the negative electrode active material.

[0007] Such lithium secondary batteries are usually manufactured using a lithium-intercalated compound such as LiCoO2 or LiMn2O4 as the positive electrode and a non-lithium-intercalated material such as a carbon-based or Si-based material as the negative electrode. During charging, lithium ions inserted in the positive electrode move to the negative electrode via the electrolyte, and during discharging, lithium ions move again from the negative electrode to the positive electrode.

[0008] Lithium secondary batteries are used in various shapes, such as cylindrical, pouch, and square, depending on the application. Conventional cylindrical cells have a separator on the outermost side after winding, and have a separator shell structure that surrounds the entire cell and is electrically connected to the battery outer can via positive and negative electrode tabs.

[0009] Conventional cylindrical cells are wound in the order of positive electrode / separator / negative electrode / separator, with the separator exposed on the outermost surface, whereas the Cu foil outermost structure is wound in the order of negative electrode / separator / positive electrode / separator, with the Cu foil exposed on the outermost surface. This has the advantage that it can directly contact the inner wall of the battery outer can of the cylindrical cell, is electrically connected, and can replace the outer negative electrode tab.

[0010] However, if the contact between the Cu foil and the battery outer can is poor, the resistance increases, and a problem occurs in which the resistance varies depending on the outer diameter of the jelly roll. Unlike the conventional separator outer shell structure, the Cu foil is on the outermost shell, so two separators 2 are present inside, surrounding the positive electrode.

[0011] The thickness of the Cu foil, which is the negative electrode current collector, is gradually becoming thinner, and in particular, a tab is attached to the uncoated part of the core part of the negative electrode current collector, and the core part is used as the center for winding to form a jelly roll electrode assembly. At this time, wrinkles form on the uncoated part of the core part of the negative electrode current collector at the same time as winding, and the wrinkles propagate to the wrinkles of the negative electrode, and a problem occurs when the jelly roll electrode assembly is formed in this state.

[0012] Therefore, research is being conducted on how to improve the wrinkles in the core electrode of a jelly roll electrode assembly in which the negative electrode current collector made of Cu foil forms the outermost layer. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] Japanese Patent Publication No. 2009-080971 Summary of the Invention [Problem to be solved by the invention]

[0014] The present application relates to a jelly roll electrode assembly and a cylindrical lithium secondary battery including the same. [Means for solving the problem]

[0015] One embodiment of the present specification provides a jelly roll electrode assembly including: a first separator; a positive electrode laminated on one side of the first separator and including a positive electrode current collector; a second separator provided on a side of the positive electrode opposite to a side that contacts the first separator; and a negative electrode including a negative electrode current collector provided on a side of the second separator opposite to a side that contacts the positive electrode; the jelly roll electrode assembly having a structure in which a jelly roll hollow portion is formed in a core portion and wound around the negative electrode, the negative electrode current collector including a negative electrode active material coated portion where a negative electrode active material is coated, and a negative electrode uncoated portion where the negative electrode active material is not coated, the negative electrode uncoated portion being formed on both ends of the negative electrode, at least one of the negative electrode uncoated portions at both ends having a negative electrode tab, and the negative electrode uncoated portion of the negative electrode current collector including a protective tape on at least one side, the protective tape satisfying the following formula 1:

[0016] [Formula 1] 50%≦a≦100% In the above formula 1, a is (length of protective tape attached to the negative electrode uncoated portion / total length of the negative electrode uncoated portion)×100%.

[0017] In another embodiment, a cylindrical lithium secondary battery is provided, comprising: a battery exterior material; a jelly roll electrode assembly according to the present application provided inside the battery exterior material; and an exterior cap having an electrode provided at an opening of the battery exterior material. Effect of the Invention

[0018] The jelly roll electrode assembly according to the present application is a jelly roll electrode assembly having a structure in which a jelly roll hollow portion is formed in a core portion and wound around the negative electrode to realize an outermost structure of the negative electrode current collector, and the negative electrode uncoated portion of the negative electrode current collector includes a protective tape that satisfies formula 1 on at least one side. As a result, even if a process of winding is included starting from the center of the thin negative electrode current collector, the protective tape gives rigidity to the negative electrode current collector to prevent wrinkles from being generated during winding, and thus wrinkles in the entire electrode can be improved, resulting in a jelly roll electrode assembly that is free of wrinkles.

[0019] In other words, the jelly roll electrode assembly according to the present application is characterized in that the protective tape is formed so as to cover at least 50% of one side of the negative electrode uncoated portion of the negative electrode current collector, and is formed on one or both sides of the uncoated portion, thereby improving wrinkles in the electrode and thereby increasing the life and efficiency of a cylindrical lithium secondary battery including the same. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a diagram illustrating a method for winding a jelly roll electrode assembly according to an embodiment of the present application. [Diagram 2] 1A and 1B are diagrams illustrating a method for manufacturing a jelly roll electrode assembly having an outermost separator structure. [Diagram 3] FIG. 2 is a side view of a jellyroll electrode assembly before winding according to an embodiment of the present application. [Figure 4] FIG. 2 is a diagram showing a core part of a negative electrode according to the present application. [Diagram 5]FIG. 2 shows a negative electrode according to Example 1 of the present application. [Figure 6] FIG. 2 is a diagram showing a negative electrode according to Comparative Example 1 of the present application. [Figure 7] FIG. 4 is a diagram showing the occurrence of wrinkles in a negative electrode according to Comparative Example 1 of the present application. [Explanation of symbols]

[0021] 1...Negative electrode 2 Second separator 3...Positive electrode 4. First separator 10 Negative electrode tab 11: Protective tape attached to the uncoated surface of the first negative electrode 12: Protective tape attached to the uncoated surface of the second negative electrode 13 Positive electrode tab 14 Positive electrode uncoated area 15 Negative electrode uncoated area 16...Negative electrode active material layer 17...Cathode active material layer 21 Overall length of first negative electrode uncoated portion 22 Overall length of second negative electrode uncoated portion 23: Length of protective tape attached to the uncoated surface of the first negative electrode 24: Length of protective tape attached to the uncoated surface of the second negative electrode 100 ··· Jelly roll hollow section DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Before describing the present invention, some terms will first be defined.

[0023] In this specification, when a part is said to "comprise" a certain component, this means that it may further include other components, not excluding other components, unless specifically stated to the contrary.

[0024] In this specification, "p to q" means a range of "not less than p and not more than q."

[0025] In this specification, the "specific surface area" is measured by the BET method, and specifically, is calculated from the amount of nitrogen gas adsorption at liquid nitrogen temperature (77K) using a BELSORP-mino II manufactured by BEL Japan Ltd. That is, in this application, the BET specific surface area may mean the specific surface area measured by the above-mentioned measurement method.

[0026] In this specification, "Dn" means the average particle size, which means the particle size at the n% point of the cumulative particle number distribution according to the particle size. That is, D50 is the particle size at the 50% point of the cumulative particle number distribution according to the particle size, D90 is the particle size at the 90% point of the cumulative particle number distribution according to the particle size, and D10 is the particle size at the 10% point of the cumulative particle number distribution according to the particle size. Meanwhile, the average particle size can be measured using a laser diffraction method. Specifically, the powder to be measured is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500), and the difference in the diffraction pattern according to the particle size is measured when the particles pass through a laser beam to calculate the particle size distribution.

[0027] In this specification, when a polymer contains a certain monomer as a monomer unit, it means that the monomer participates in a polymerization reaction and is contained as a repeating unit in the polymer. In this specification, when a polymer contains a monomer, this is interpreted as the same as when the polymer contains the monomer as a monomer unit.

[0028] In this specification, the term "polymer" is understood to be used in a broad sense including copolymers, unless otherwise specified as a "homopolymer."

[0029] In this specification, the weight average molecular weight (Mw) and number average molecular weight (Mn) are polystyrene-equivalent molecular weights measured by gel permeation chromatography (GPC) using commercially available monodisperse polystyrene polymers (standard samples) with various degrees of polymerization as standard substances for molecular weight measurement. In this specification, the molecular weight means the weight average molecular weight unless otherwise specified.

[0030] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings in order to enable those skilled in the art to easily carry out the present invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described below.

[0031] One embodiment of the present specification provides a jelly roll electrode assembly including: a first separator; a positive electrode laminated on one side of the first separator and including a positive electrode current collector; a second separator provided on a side of the positive electrode opposite to a side that contacts the first separator; and a negative electrode including a negative electrode current collector provided on a side of the second separator opposite to a side that contacts the positive electrode; the jelly roll electrode assembly having a structure in which a jelly roll hollow portion is formed in a core portion and wound around the negative electrode, the negative electrode current collector including a negative electrode active material coated portion where a negative electrode active material is coated and a negative electrode uncoated portion where no negative electrode active material is coated, the negative electrode uncoated portion being formed on both ends of the negative electrode, at least one of the negative electrode uncoated portions at both ends having a negative electrode tab, and the negative electrode uncoated portion of the negative electrode current collector including a protective tape on at least one side, the protective tape satisfying the following formula 1:

[0032] [Formula 1] 50%≦a≦100% In the above formula 1, a is (length of protective tape attached to negative electrode uncoated portion / total length of negative electrode uncoated portion)×100%.

[0033] The jelly roll electrode assembly according to the present application is a jelly roll electrode assembly having a structure in which a jelly roll hollow portion is formed in the center and wound around the negative electrode to realize the outermost structure of the negative electrode current collector, and the negative electrode uncoated portion of the negative electrode current collector includes a protective tape that satisfies formula 1 on at least one side. As a result, even if a process of winding is included starting from the center of the thin negative electrode current collector, the protective tape gives rigidity to the negative electrode current collector to prevent wrinkles from being generated during winding, and thus wrinkles in the entire electrode can be improved, resulting in a jelly roll electrode assembly that is free of wrinkles.

[0034] In one embodiment of the present application, a first separator, a positive electrode laminated on one side of the first separator and including a positive electrode current collector, a second separator laminated on one side of the positive electrode, and a negative electrode including a negative electrode current collector on the second separator can be expressed as an electrode sheet.

[0035] That is, a jelly roll electrode assembly including a first separator; a positive electrode laminated on one side of the first separator and including a positive electrode current collector; a second separator provided on the opposite side of the positive electrode that contacts the first separator; and a negative electrode including a negative electrode current collector provided on the opposite side of the second separator that contacts the positive electrode; and having a jelly roll hollow portion formed in a core portion and wound around the negative electrode, can be expressed as a jelly roll electrode assembly having a structure in which the electrode sheet is wound.

[0036] In one embodiment of the present application, the method for manufacturing a jelly roll electrode assembly includes the steps of respectively preparing and stacking a positive electrode, a negative electrode, a first separator, and a second separator.

[0037] In the above steps, the first separator, the positive electrode, the second separator, and the negative electrode are stacked in this order, and a jelly roll hollow portion is formed in the core portion and wound around the negative electrode. By the above stacking and winding method, a jelly roll electrode assembly having a negative electrode current collector as the outermost structure can be formed.

[0038] 1 is a diagram showing a method of winding an electrode sheet according to an embodiment of the present application into a jelly roll electrode assembly. Specifically, a first separator 4, a positive electrode 3 including a positive current collector laminated on one side of the first separator, a second separator 2 laminated on one side of the positive electrode 3, and a negative electrode 1 including a negative current collector laminated on the second separator 2 are laminated, and it can be seen that the jelly roll is wound around the negative electrode 1 with a jelly roll hollow part 100 formed in the center. Furthermore, as can be seen from FIG. 1, it can be seen that only the negative electrode 1 including the negative current collector is separately wound again to form a jelly roll electrode assembly with the negative current collector at the outermost edge.

[0039] FIG. 2 shows the outermost structure of a conventional separator, which has a positive electrode 3 / second separator 2 / negative electrode 1 / first separator 4 configuration, in which a jelly roll hollow portion 100 is formed in the center and wound around the positive electrode 3. The jelly roll electrode assembly finally produced from this has an outermost structure of the first separator 4.

[0040] In one embodiment of the present application, the positive electrode may include a positive electrode current collector, and a positive electrode active material layer formed on one or both sides of the positive electrode current collector and including a positive electrode active material.

[0041] In one embodiment of the present application, there is provided a jelly roll electrode assembly, in which the positive electrode current collector includes a positive electrode active material-coated portion on which a positive electrode active material is coated and a positive electrode uncoated portion on which no positive electrode active material is coated, and a positive electrode tab is provided on the positive electrode uncoated portion.

[0042] In one embodiment of the present application, the positive electrode active material layer is formed on an active material-coated portion of the positive electrode current collector, and a surface on which the positive electrode active material layer is not provided can be referred to as a positive electrode uncoated portion.

[0043] Specifically, as can be seen from FIG. 3, the positive electrode 3 is provided between a first separator 4 and a second separator 2, and the positive electrode 3 includes a positive electrode uncoated portion 14 where a positive electrode active material layer 17 is not applied, and a positive electrode tab 13 is provided on the uncoated portion.

[0044] In the positive electrode, the positive electrode current collector is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity, and may be, for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The positive electrode current collector may generally have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the adhesive strength of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0045] The positive electrode active material may be a commonly used positive electrode active material. Specifically, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2) or a compound substituted with one or more transition metals; a lithium iron oxide such as LiFe3O4; 1+c1 Mn 2-c1 O4 (0≦c1≦0.33), lithium manganese oxides such as LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7; chemical formula LiNi 1-c2 Ni-site type lithium nickel oxide represented by the chemical formula LiMn 2-c3 M c3Examples of the lithium manganese composite oxide include, but are not limited to, lithium manganese oxide represented by Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01≦c3≦0.1) or Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn); and LiMn2O4 in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion. The positive electrode may be Li-metal.

[0046] The positive electrode active material layer may contain a positive electrode conductive material and a positive electrode binder in addition to the above-mentioned positive electrode active material.

[0047] In this case, the positive electrode conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it has electronic conductivity without causing chemical changes in the battery that is constructed.Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like, and one or more of these may be used alone or in mixture.

[0048] In addition, the positive electrode binder plays a role of improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector.Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination.

[0049] In one embodiment of the present application, the positive electrode current collector may include a positive electrode uncoated portion and a positive electrode tab formed on the positive electrode uncoated portion, and the jelly roll electrode assembly according to the present application may include one positive electrode tab.

[0050] In this case, the positive electrode uncoated portion may be formed in the center of the positive electrode.

[0051] In one embodiment of the present application, the negative electrode may include a negative electrode current collector; and a negative electrode active material layer, and the negative electrode current collector may include a negative electrode active material-coated portion to which the negative electrode active material is coated, and a negative electrode uncoated portion to which the negative electrode active material is not coated.

[0052] Specifically, as can be seen from FIG. 3, the negative electrode 1 is provided on a second separator 2, and the negative electrode 1 includes negative electrode uncoated areas 15 at both ends of the negative electrode where the negative electrode active material layer 16 is not applied, and at least one of the negative electrode uncoated areas at both ends is provided with a negative electrode tab 10.

[0053] The jelly roll electrode assembly according to the present application includes negative electrode uncoated portions at both ends of a negative electrode, and at least one of the negative electrode uncoated portions at both ends includes a negative electrode tab. Specifically, the negative electrode uncoated portion on the winding core side of the negative electrode uncoated portions may include a negative electrode tab.

[0054] In one embodiment of the present application, the negative electrode active material layer may include a negative electrode active material including one or more selected from the group consisting of a silicon-based material and a carbon-based material.

[0055] In one embodiment of the present application, the negative electrode active material layer may include a negative electrode conductive material; and a negative electrode binder.

[0056] In one embodiment of the present application, the negative electrode active material, the negative electrode conductive material, and the negative electrode binder may be any materials used in the art without limitation.

[0057] In one embodiment of the present application, the negative electrode current collector is not particularly limited as long as it does not induce a chemical change in the battery and has electrical conductivity. For example, the current collector may be made of copper, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel whose surface is treated with carbon, nickel, titanium, silver, or the like. Specifically, a transition metal that easily adsorbs carbon, such as copper or nickel, may be used as the current collector. The thickness of the current collector may be 6 μm to 20 μm, but the thickness of the current collector is not limited thereto.

[0058] The negative electrode binder may include at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, and substances in which hydrogen is substituted with Li, Na, Ca, or the like, or may include various copolymers thereof.

[0059] The negative electrode conductive material is not particularly limited as long as it does not induce a chemical change in the battery and has conductivity, and examples of the negative electrode conductive material that can be used include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive tubes such as carbon nanotubes; metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0060] In one embodiment of the present application, the first separator and the second separator are used to separate the negative electrode and the positive electrode and provide a path for lithium ion migration. Any separator that is generally used as a separator in a secondary battery can be used without any particular limitation, and it is particularly preferable that the separator has low resistance to ion migration of the electrolyte and has excellent electrolyte moisture absorption ability. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof may be used. In addition, a normal porous nonwoven fabric, for example, a nonwoven fabric made of a high-melting point glass fiber, a polyethylene terephthalate fiber, or the like, may be used. In addition, in order to ensure heat resistance or mechanical strength, a coated separator containing a ceramic component or a polymeric substance may be used, and may be selectively used as a single layer or a multilayer structure.

[0061] In one embodiment of the present application, there is provided a jelly roll electrode assembly, wherein the negative electrode current collector includes a negative electrode active material-coated portion on which a negative electrode active material is coated, and a negative electrode uncoated portion on which no negative electrode active material is coated, the negative electrode uncoated portion is formed on both ends of the negative electrode, at least one of the negative electrode uncoated portions on both ends has a negative electrode tab, and the negative electrode uncoated portion of the negative electrode current collector includes a protective tape on at least one side, and the protective tape satisfies the following Formula 1:

[0062] [Formula 1] 50%≦a≦100% In the above formula 1, a is (length of the protective tape attached to the negative electrode uncoated portion / total length of the negative electrode uncoated portion)×100%.

[0063] In one embodiment of the present application, the negative electrode uncoated portion may be formed at both ends of the negative electrode, one of which may be formed in the hollow portion of the jelly roll. Specifically, this corresponds to the position 100 in Fig. 1, and may refer to the portion of the end of the negative electrode where winding begins, as can be seen in Fig. 3.

[0064] In one embodiment of the present application, there is provided a jelly roll electrode assembly, wherein the negative electrode current collector includes a negative electrode active material-coated portion on which a negative electrode active material is coated, and a negative electrode uncoated portion on which no negative electrode active material is coated, the negative electrode uncoated portion is formed on both ends of the negative electrode, one of the negative electrode uncoated portions at both ends has a negative electrode tab, and the negative electrode uncoated portion of the negative electrode current collector includes a protective tape on at least one side, and the protective tape satisfies Formula 1.

[0065] In one embodiment of the present application, there is provided a jelly roll electrode assembly, wherein the negative electrode current collector includes a negative electrode active material-coated portion on which a negative electrode active material is coated, and a negative electrode uncoated portion on which no negative electrode active material is coated, the negative electrode uncoated portion is formed on both ends of the negative electrode, one of the negative electrode uncoated portions at both ends has a negative electrode tab, and the negative electrode tab is located at an end of the negative electrode uncoated portion that is located in a hollow portion of the negative electrode jelly roll, among the ends of the negative electrode uncoated portion, and the negative electrode uncoated portion of the negative electrode current collector includes a protective tape on at least one side, and the protective tape satisfies Formula 1.

[0066] In one embodiment of the present application, there is provided a jelly roll electrode assembly, in which the negative electrode uncoated portion of the negative electrode current collector includes a protective tape on at least one surface thereof, and the protective tape satisfies Formula 1 above.

[0067] In another embodiment, there is provided a jelly roll electrode assembly, wherein the negative electrode uncoated portion of the negative electrode current collector includes a protective tape on one side, and the protective tape satisfies Formula 1.

[0068] In yet another embodiment, there is provided a jelly roll electrode assembly, wherein the negative electrode uncoated portion of the negative electrode current collector includes protective tapes on both sides thereof, and the protective tapes satisfy Formula 1.

[0069] The jelly roll electrode assembly according to the present application includes a protective tape that satisfies the formula 1 on at least one surface of the negative uncoated portion of the negative current collector, and therefore, even if a winding process is performed starting from the center of the thin negative current collector, the protective tape can impart rigidity to the negative current collector and prevent wrinkles from being generated during winding. This can improve the wrinkles in the entire electrode, and thus provides a jelly roll electrode assembly that is free of wrinkles.

[0070] That is, the present invention has a feature that can solve the problem of wrinkles being formed in conventional electrodes when a protective tape having the above-mentioned length is attached to at least one surface of the negative electrode uncoated portion of the jelly roll electrode assembly according to the present application.

[0071] In one embodiment of the present application, there is provided a jelly roll electrode assembly, in which the negative electrode uncoated portion includes a first negative electrode uncoated surface on which the negative electrode tab is provided; and a second negative electrode uncoated surface that is an opposite surface to the first negative electrode uncoated surface, the protective tape is formed on the first negative electrode uncoated surface and the second negative electrode uncoated surface, and the protective tape satisfies the following Formulas 2 and 3:

[0072] [Formula 2] 25%≦a1≦100% [Formula 3] 25%≦b1≦100% In the above formula 2 and formula 3, a1 is (length of protective tape attached to first negative-electrode uncoated portion / total length of first negative-electrode uncoated portion) × 100%, b1 is (length of protective tape attached to second negative-electrode uncoated portion / total length of second negative-electrode uncoated portion) × 100%, At least one of a1 and b1 is 50% or more.

[0073] Specifically, the above can be seen from Fig. 4. Fig. 4 is a diagram showing a core part of a negative electrode according to the present application. Specifically, a negative electrode tab 10 is provided on a negative electrode uncoated part included in the core part at both ends of the negative electrode, and the length 23 of the protective tape attached to the first negative electrode uncoated part and the total length 21 of the first negative electrode uncoated part can be seen, and the length 24 of the protective tape attached to the second negative electrode uncoated part and the total length 22 of the second negative electrode uncoated part can be seen.

[0074] In one embodiment of the present application, the formula 2 may satisfy the range of 25%≦a1≦100%, may satisfy the range of 50%≦a1≦100%, or may satisfy the range of 70%≦a1≦100%.

[0075] In one embodiment of the present application, the protective tape attached to the first negative electrode uncoated portion is formed in a structure that covers the negative electrode tab, and has a feature that it can fix the negative electrode tab and improve the wrinkle phenomenon in the uncoated portion of the negative electrode current collector when it is wound up.

[0076] In one embodiment of the present application, the formula 3 may satisfy the range of 25%≦b1≦100%, may satisfy the range of 50%≦b1≦100%, or may satisfy the range of 70%≦b1≦100%.

[0077] In one embodiment of the present application, when a protective tape is included in a first negative electrode uncoated portion where a negative electrode tab is provided among the negative electrode uncoated portions, and a protective tape satisfying the above range is also included in a second negative electrode uncoated portion on the opposite side, the negative electrode uncoated portion has a feature that the core wrinkle occurrence rate is significantly reduced compared to a case where a protective tape is provided only on one side.

[0078] That is, when a protective tape having the above length is attached to one surface of the negative electrode uncoated portion of the jelly roll electrode assembly, the problem of wrinkles in the conventional electrodes can be solved. At the same time, in particular, when protective tape is provided on both the first negative electrode uncoated portion and the second negative electrode uncoated portion of the negative electrode uncoated portions, in addition to the problem of wrinkles, the jelly roll-shaped core portion has rigidity, which provides an excellent effect of preventing collapse of the core portion.

[0079] In one embodiment of the present application, there is provided a jelly roll electrode assembly, wherein a1 is 100% and b1 is 100%.

[0080] In the present application, the a1 being 100% and the b1 being 100% may mean that both sides of the negative electrode uncoated portion on which the negative electrode tab is provided are entirely covered with the protective tape.

[0081] In one embodiment of the present application, a jellyroll electrode assembly is provided that includes one each of the positive electrode tab and the negative electrode tab.

[0082] As can be seen from FIG. 3, the negative electrode tab of the jelly roll electrode assembly according to the present invention is located at the end of the negative electrode that is located at the core portion of the negative electrode, and the positive electrode tab is formed at the center of the positive electrode, not at the outer periphery of the positive electrode. Thus, one positive electrode tab and one negative electrode tab may be included.

[0083] When one positive electrode tab and one negative electrode tab are included as described above, the resistance may be higher than when two or more are included. However, by including one each, the uncoated area is reduced and more positive electrode active material and negative electrode active material can be included, resulting in a significant increase in capacity.

[0084] That is, the jelly roll electrode assembly according to the present invention includes one positive electrode tab and one negative electrode tab, and is used for high capacity applications rather than high output applications. The purpose can be determined according to the number of positive electrode tabs and negative electrode tabs.

[0085] In one embodiment of the present application, there is provided a jelly roll electrode assembly including: a positive electrode active material layer provided on both sides of the positive electrode active material-coated portion of the positive electrode current collector; and a negative electrode active material layer provided on both sides of the negative electrode active material-coated portion of the negative electrode current collector.

[0086] When the active material layers are formed on both sides as described above, the active material can be contained in a larger amount, which maximizes the capacity.

[0087] In one embodiment of the present application, there is provided a jelly roll electrode assembly, in which a negative electrode current collector is an outermost structure.

[0088] A manufacturing method having an outermost structure of a negative electrode current collector can be seen in Fig. 1. As can be seen from Fig. 1, a jelly roll hollow part 100 is formed in the center, and the negative electrode 1 is wound around the negative electrode 1. Finally, only the negative electrode current collector included in the negative electrode 1 is wound again around the outer edge of the jelly roll electrode assembly to form an outermost exposed structure of the negative electrode current collector.

[0089] That is, the outermost structure of the negative electrode current collector is a structure in which the winding order of the positive electrode and the negative electrode are reversed so that the negative electrode current collector is exposed at the outermost edge, and the negative electrode current collector can be in direct contact with the inner wall of the battery exterior material described below, and can be electrically connected to the can even without an outer negative electrode tab. That is, as described above, the jelly roll electrode assembly according to the present invention has one positive electrode tab and one negative electrode tab, thereby realizing a high-capacity battery, and the negative electrode current collector is formed at the outermost edge, thereby realizing the above-mentioned features.

[0090] In one embodiment of the present application, there is provided a jelly roll electrode assembly, wherein the protective tape is any one selected from the group consisting of polyethylene terephthalate (PET), polypropylene (PP), polyester, polycarbonate (PC), polyimide (PI), polyethylene naphthalate (PEN), polyether ether ketone (PEEK), polyarylate (PAR), polycylicolefin (PCO), polynorbornene (polynorbornene), polyethersulphone (PES), and cycloolefin polymer (COP).

[0091] The protective tape can be any tape that can fix the negative electrode tab and has a rigidity sufficient to prevent bending of the negative electrode uncoated portion during winding. Specifically, PET may be used.

[0092] In one embodiment of the present application, there is provided a jelly roll electrode assembly, wherein the protective tape has a thickness of 10 μm or more and 100 μm or less.

[0093] In one embodiment of the present application, a cylindrical lithium secondary battery is provided, comprising: a battery exterior material; a jelly roll electrode assembly according to the present application provided inside the battery exterior material; and an exterior cap having an electrode provided at an opening of the battery exterior material.

[0094] The contents of the jelly roll electrode assembly are as described above.

[0095] In one embodiment of the present application, the inside of the battery exterior material may contain an electrolyte.

[0096] Examples of the electrolyte include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries, but are not limited to these.

[0097] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.

[0098] Examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.

[0099] In particular, ethylene carbonate and propylene carbonate, which are cyclic carbonates among the carbonate-based organic solvents, can be preferably used as high-viscosity organic solvents, because they have a high dielectric constant and dissociate lithium salts well. When such cyclic carbonates are mixed in an appropriate ratio with linear carbonates having low viscosity and low dielectric constant, such as dimethyl carbonate and diethyl carbonate, an electrolyte having high electrical conductivity can be prepared, and therefore such a mixture can be used even more preferably.

[0100] The metal salt may be a lithium salt, which is a substance that is easily dissolved in the non-aqueous electrolyte. For example, the anion of the lithium salt may be F - , Cl - , I - , NO3 -, N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , and (CF3CF2SO2)2N - One or more selected from the group consisting of may be used.

[0101] In addition to the constituents of the electrolyte, the electrolyte may further include one or more additives such as a haloalkylene carbonate compound such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing a decrease in battery capacity, and improving the discharge capacity of the battery.

[0102] The jelly roll electrode assembly according to the present invention may be included in a cylindrical battery. The cylindrical battery may mean that the battery itself, which includes an assembly including a positive electrode, a negative electrode, a separator, and an electrolyte, has a cylindrical shape. Specifically, the cylindrical battery may be composed of a cylindrical can, a battery assembly provided inside the cylindrical can, and a top cap. EXAMPLES

[0103] Below, preferred examples are presented to aid in understanding the present invention. However, these examples are merely illustrative of the present description, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope and technical spirit of the present description. Naturally, such changes and modifications fall within the scope of the appended claims.

[0104] <Example 1> As shown in FIG. 3, a first separator / positive electrode / second separator / negative electrode were laminated, a negative electrode tab was provided on the center of the uncoated part of the negative electrode current collector when it was wound, and protective tapes in which a was 100%, specifically a1 was 100% and b1 was 100%, were attached to both sides of the uncoated part of the negative electrode current collector where the negative electrode tab was provided, and then wound up to form a jelly roll electrode assembly.

[0105] <Example 2> A jelly roll electrode assembly was formed in the same manner as in Example 1, except that a protective tape in which a was 100%, specifically a1 was 100%, was attached to one side of the negative electrode current collector uncoated portion on which the negative electrode tab was provided.

[0106] <Example 3> A jelly roll electrode assembly was formed in the same manner as in Example 1, except that protective tapes in which a was 80%, specifically, a1 was 80% and b1 was 30%, were attached to both sides of the negative electrode current collector uncoated portion on which the negative electrode tab was provided.

[0107] <Example 4> A jelly roll electrode assembly was formed in the same manner as in Example 1, except that protective tapes in which a was 80%, specifically, a1 was 30% and b1 was 80%, were attached to both sides of the negative electrode current collector uncoated portion on which the negative electrode tab was provided.

[0108] <Comparative Example 1> A jelly roll electrode assembly was formed in the same manner as in Example 1, except that a protective tape in which a was 40%, specifically a1 was 40%, was attached to one side of the negative electrode current collector uncoated portion on which the negative electrode tab was provided.

[0109] <Comparative Example 2> A jelly roll electrode assembly was formed in the same manner as in Example 1, except that protective tapes in which a was 40%, specifically, a1 was 40% and b1 was 30%, were attached to both sides of the negative electrode current collector uncoated portion on which the negative electrode tab was provided.

[0110] <Comparative Example 3> A jelly roll electrode assembly was formed in the same manner as in Example 1, except that no protective tape was attached to both sides of the negative electrode current collector uncoated portion where the negative electrode tab was provided.

[0111] In the jelly roll electrode assemblies of Examples 1 to 4, a protective tape is formed to cover at least 50% of one side of the negative electrode uncoated portion of the negative electrode current collector, and is formed on one or both sides of the uncoated portion. As a result, it has been confirmed that the jelly roll electrode assemblies have the characteristic of improving the life and efficiency of a cylindrical lithium secondary battery including the same by improving wrinkles in the electrode.

[0112] Specifically, in the case of Example 1, the protective tape was attached to 100% of both sides of the uncoated portion of the negative electrode current collector on which the negative electrode tab was provided, and in the case of Example 2, the protective tape was attached to 100% of the side of the uncoated portion of the negative electrode current collector on which the negative electrode tab was provided.

[0113] Comparing Example 1 and Example 2, it was confirmed that Example 1 had a greater effect of improving wrinkles on the electrodes than Comparative Examples 1 to 3, and was particularly superior in improving wrinkles on the electrodes compared to Example 2 (protective tape formed on one side). This is due to the formation of rigid protective tape on both sides of the plain area.

[0114] In particular, Fig. 5 is a diagram showing a negative electrode according to Example 1 of the present application. Specifically, it can be seen that protective tape was attached to both sides of the negative electrode uncoated area (shown by the dotted line) so that a was 100%. In this case, it was confirmed that no wrinkles were generated in the negative electrode, and therefore it was found that there was an effect of improving wrinkles in the electrode.

[0115] In the above-mentioned Examples 3 and 4, protective tapes are provided on both sides of the negative electrode current collector uncoated portion where the negative electrode tab is provided, with the proviso that a1 and b1 are not 100%. Although a small amount of wrinkles are generated in the electrode compared to Example 1, it was confirmed that the wrinkles in the electrode are improved to the extent that they do not affect the operation of the electrode.

[0116] In Comparative Example 1, protective tape was formed on one side of the negative electrode uncoated region, and in Comparative Example 2, protective tape was formed on both sides of the negative electrode uncoated region, but the coverage was less than 50% in each case. It was confirmed that even when protective tape was provided, wrinkles in the electrode still occurred when the electrode assembly was wound up, which may cause a decrease in performance of the lithium secondary battery and a safety issue due to lithium precipitation.

[0117] 6 is a diagram showing a negative electrode according to Comparative Example 1 of the present application. Specifically, in the negative electrode uncoated portion (shown by a thin dotted line), a protective tape is attached to one side so that a is 40% and 60% of the negative electrode uncoated portion is exposed. In this case, as can be seen from FIGS. 6 and 7, the length of the protective tape cannot be filled, and wrinkles are generated in the negative electrode uncoated portion (enlargement of the thick dotted line), which causes wrinkles in the entire negative electrode, which leads to a decrease in the performance of the lithium secondary battery.

[0118] In Comparative Example 3, the protective tape was not provided on both sides. In this case, many wrinkles were generated when the electrode assembly was wound up, which may cause early performance deterioration of the lithium secondary battery and safety problems due to lithium precipitation.

Claims

1. A first separator; a positive electrode including a positive electrode current collector, the positive electrode current collector being laminated on one side of the first separator; a second separator provided on the surface of the positive electrode opposite to the surface in contact with the first separator; and a negative electrode including a negative electrode current collector provided on a surface of the second separator opposite to the surface in contact with the positive electrode; and a jelly roll electrode assembly having a structure in which a jelly roll hollow portion is formed in a core portion and wound around the negative electrode, the negative electrode current collector includes a negative electrode active material-coated portion on which a negative electrode active material is coated, and a negative electrode uncoated portion on which the negative electrode active material is not coated, The negative electrode uncoated portion is formed on both ends of the negative electrode, and at least one of the negative electrode uncoated portions at both ends has a negative electrode tab; The negative electrode uncoated portion of the negative electrode current collector includes a protective tape on at least one surface thereof, and the protective tape satisfies the following formula 1: [Formula 1] 50%≦a≦100% In the above formula 1, a is (length of protective tape attached to the negative electrode uncoated portion / total length of the negative electrode uncoated portion)×100%.

2. the negative electrode uncoated portion includes a first negative electrode uncoated surface on which the negative electrode tab is provided; and a second negative electrode uncoated surface opposite to the first negative electrode uncoated surface, the protective tape is formed on the first negative electrode uncoated surface and the second negative electrode uncoated surface, The jelly roll electrode assembly of claim 1, wherein the protective tape satisfies the following formulas 2 and 3: [Formula 2] 25%≦a1≦100% [Formula 3] 25%≦b1≦100% In the formula 2 and the formula 3, a1 is (length of protective tape attached to first negative-electrode uncoated portion / total length of the first negative-electrode uncoated portion)×100%, b1 is (length of protective tape attached to second negative-electrode uncoated portion / total length of the second negative-electrode uncoated portion)×100%, At least one of the a1 and the b1 is 50% or more.

3. the positive electrode current collector includes a positive electrode active material-coated portion on which a positive electrode active material is coated, and a positive electrode non-coated portion on which the positive electrode active material is not coated, 10. The jellyroll electrode assembly of claim 1, further comprising a positive tab on the positive non-coating portion.

4. 3. The jelly roll electrode assembly of claim 2, wherein a1 is 100% and b1 is 100%.

5. 4. The jellyroll electrode assembly of claim 3, comprising one each of the positive and negative electrode tabs.

6. a positive electrode active material layer provided on both sides of the positive electrode active material-coated portion of the positive electrode current collector; and 4. The jelly roll electrode assembly of claim 3, further comprising: a negative electrode active material layer provided on both sides of the negative electrode active material-coated portion of the negative electrode current collector.

7. 2. The jelly roll electrode assembly of claim 1, wherein the protective tape is any one selected from the group consisting of polyethylene terephthalate (PET), polypropylene (PP), polyester, polycarbonate (PC), polyimide (PI), polyethylene naphthalate (PEN), polyethylene ether ketone (PEEK), polyarylate (PAR), polycylicolefin (PCO), polynorbornene, polyethylene sulphone (PES), and cycloolefin polymer (COP).

8. 2. The jelly roll electrode assembly of claim 1, wherein the protective tape has a thickness of 10 μm or more and 100 μm or less.

9. 2. The jelly roll electrode assembly of claim 1, wherein the jelly roll electrode assembly is an outermost structure of a negative electrode current collector.

10. Battery casing materials; The jelly roll electrode assembly according to any one of claims 1 to 9, which is provided inside the battery exterior material; and an exterior cap having an electrode provided at an opening of the battery exterior material; A cylindrical lithium secondary battery comprising:

Citation Information

Patent Citations

  • Wound nonaqueous electrolyte secondary battery

    JP2008277207A

  • Electrode assembly having protection tape and rechargeable battery including the same

    US20160149221A1

  • Secondary battery using non-aqueous electrolyte

    WO2018180748A1

  • Anode for lithium ion battery

    JP2009080971A

Cited By

  • Jelly roll electrode assembly and cylindrical lithium secondary battery including the same

    JP2025169418A

  • Jelly roll electrode assembly and cylindrical lithium secondary battery containing the same