Separator, manufacturing method thereof, secondary battery, battery module, battery pack and power consumption device

The separator coating with specific organic particles and adhesive properties addresses adhesion and resistance issues, enhancing battery performance and safety by ensuring proper adhesion and reducing resistance.

JP2024535875AActive Publication Date: 2024-10-02CONTEMPORARY AMPEREX TECHNOLOGY (HONG KONG) LIMITED
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024517174
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2022-07-11
Publication Date
2024-10-02
Estimated Expiration
2042-07-11

AI Technical Summary

Technical Problem

The challenge in battery manufacturing lies in achieving suitable adhesion between electrode plates and separators without increasing resistance, which affects safety and dynamic performance due to misalignment, wrinkles, and excessive adhesion leading to separator layer adhesion during transportation and manufacturing processes.

Method used

A separator coating comprising 40-90 wt% first organic particles, 2-15 wt% pressure-sensitive adhesive, and optionally 0-50 wt% second organic particles, with specific particle diameters and vitrification transition temperatures, ensuring appropriate adhesion at different temperatures and pressures to prevent misalignment and resistance increase.

Benefits of technology

The solution enhances adhesion between electrode plates and separators, preventing misalignment and wrinkles, reducing resistance, and improving safety and dynamic performance while maintaining manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024535875000009
    Figure 2024535875000009
  • Figure 2024535875000010
    Figure 2024535875000010
  • Figure 2024535875000011
    Figure 2024535875000011
Patent Text Reader

Abstract

The present application provides a separator, a manufacturing method thereof, and a secondary battery, a battery module, a battery pack, and a power consumption device including the separator, wherein the separator includes a substrate and a coating applied to at least one surface of the substrate, the coating includes 40-90 wt% of first organic particles, 2-15 wt% of a pressure-sensitive adhesive, and optionally 0-50 wt% of second organic particles, wherein the first organic particles include an organic polymer and an inorganic material, and the pressure-sensitive adhesive includes an organic polymer and a plasticizer. The separator according to the present application has good ion conduction ability and adhesion performance at room temperature, and does not adhere under the action of a pressure of ≦1 MPa, but obviously adheres under the action of a pressure of ≧2 MPa, which can obviously improve the structural stability and ion conduction of electrochemical devices, and at the same time, can balance the manufacturing yield and dynamic performance requirements of battery cores.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the field of battery technology, and in particular to a separator, a manufacturing method thereof, and a secondary battery, a battery module, a battery pack and a power consuming device including the separator. [Background technology]

[0002] In the manufacturing process of the battery core of the electrochemical device, the electrode plate and the separator are inevitably misaligned during the transfer, and in the lightest case, the electrode plate will wrinkle after full charge, which will seriously affect the dynamic performance and reduce the safety performance of the battery core, and in the severest case, the electrode plates will contact each other and the dry battery core will be scrapped. Therefore, the technicians coat the separator with an adhesive coating, and generally in the first composite process of the electrode plate and the separator of the electrochemical device, pre-pressure is applied with an appropriate pressure action to ensure that the electrode plate and the separator of the electrochemical device have a certain adhesion before entering the next process, but due to the requirements of production efficiency, the pressure and the action time in the first process can not be satisfied to achieve the proper adhesion of the electrode plate and the separator of the electrochemical device. On the other hand, during the transportation of the separator, the separator and the separator also need to have a proper adhesion. If the adhesive force is too large, it may cause the separator layers to adhere to each other, which is disadvantageous to the subsequent high-speed composite of the electrode plate and the separator. Therefore, how to provide an appropriate adhesive effect between the separator and the electrode plate to improve safety performance, while preventing the adhesive force between the separator and the electrode plate from being too strong during transportation to affect the subsequent use of the separator, is a problem that engineers need to solve as soon as possible.

[0003] In addition, while solving the above problems, it is necessary to consider the following issues: whether the surface density of the adhesive material is too high will deteriorate the resistance of the separator; whether the adhesive material has appropriate adhesive strength at high temperatures and room temperatures; and whether the holes in the separator will be blocked, increasing the resistance of the separator and affecting the dynamic performance of the battery core.

[0004] As can be seen, it is very meaningful to develop a separator that can solve the above problems simultaneously. Summary of the Invention

[0005] The present invention has been made in view of the above problems, and an object of the present invention is to provide a separator, a manufacturing method thereof, and a secondary battery, a battery module, a battery pack, and a power consuming device each including the separator.

[0006] In order to achieve the above object, a first aspect of the present application provides a separator, the separator comprising: A substrate; a coating applied to at least one surface of the substrate, the coating comprising 40-90 wt % first organic particles, 2-15 wt % pressure sensitive adhesive, and optionally 0-50 wt % second organic particles; the first organic particles include an organic polymer and an inorganic material, and the pressure sensitive adhesive includes an organic polymer and a plasticizer; Optionally, the volume average particle diameter of the first organic particles satisfies (Dv90-Dv10) / Dv50≦2.5, optionally ≦2, further optionally ≦1.8, and the vitrification transition temperature of the first organic particles is 20-100° C., optionally 30-80° C.; Optionally, the separator has a density of 0.1 g m -2 Ω -1 ≦ρ / R≦1.0g m -2 Ω -1 , selectively 0.5g m -2 Ω -1 ≦ρ / R≦0.9g m -2 Ω -1 , and more selectively 0.6 g m -2 Ω -1 ≦ρ / R≦0.8g m -2 Ω -1 where ρ represents the areal density of the coating on the substrate and R represents the resistance of the separator at 25° C.

[0007] This separator contains a pressure-sensitive adhesive and has good pressure-sensitive properties, with an adhesive strength of 0.08 N / m or less at ≦1 MPa, which can prevent adhesion between separators during winding and storage of the separator. At the same time, it can have a clear adhesive action with the electrode plate at room temperature (generally 20-30°C, e.g. 25°C) and a pressure of ≧2 MPa, so that when this separator is used to manufacture a battery core, the electrode plate and the separator can be closely attached at room temperature and under an appropriate pressure. Optionally, the separator has an adhesive strength of 0.1 g m -2 Ω -1 ≦ρ / R≦1.0g m -2 Ω -1 Therefore, the separator has excellent adhesion performance and does not deteriorate dynamic performance due to an increase in the resistance of the separator.

[0008] In any embodiment, optionally, the first organic particles include (1) the volume average particle diameter Dv50 of the first organic particles is 3-36 μm, optionally 5-20 μm; (2) the vitrification transition temperature of the first organic particles is 20-100°C, optionally 30-80°C; (3) The weight average molecular weight of the organic polymer in the first organic particle is 500×10 3 g / mol-1000×10 3 g / mol, selectively 800×10 3 g / mol-1000×10 3 g / mol.

[0009] In any embodiment, optionally, the organic polymer in the first organic particles comprises at least a first polymerizable monomer having at least one ester bond and selectively one or more of methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, vinyl acetate, trifluoroethyl methacrylate, glycidyl methacrylate, or trimethylolpropane triacrylate, and further selectively one or more of methyl methacrylate, lauryl acrylate, lauryl methacrylate, or trimethylolpropane triacrylate; a second polymerizable monomer having at least one cyano bond and optionally one or more of acrylonitrile, methacrylonitrile, ethacrylonitrile, and further optionally one or more of acrylonitrile, methacrylonitrile; A monomer having at least one amide bond, optionally one or more of acrylamide, N-methylolacrylamide, and N-butoxymethacrylamide, and further optionally one or more of acrylamide and N-methylolacrylamide, polymerized with a third polymerizable monomer; Optionally, the weight ratio of the first polymerizable monomer to the second polymerizable monomer to the third polymerizable monomer is 1:0-0.8:0.05-0.75, and optionally 1:0.1-0.6:0.1-0.6.

[0010] When the organic polymer is formed by polymerizing the above-mentioned polymerizable monomer, the first organic particles produced have good adhesive properties and a relatively low vitrification transition temperature. In addition, when the sprayed surface density ρ of the adhesive material on the separator and the resistance R of the separator are 0.1 g m -2 Ω -1≦ρ / R≦1.0g m -2 Ω -1 Satisfying this ratio reduces the resistance of the separator and helps improve the dynamic performance of the battery employing this separator.

[0011] In any embodiment, optionally, the content of the organic polymer in the first organic particles is 50-99.9%, optionally 60-99%, and further optionally 70-99%, based on the total dry weight of the first organic particles; The content of inorganic matter in the first organic particles is 0.1-50%, alternatively 1-40%, more alternatively 1-30%, based on the total dry weight of the first organic particles.

[0012] In either embodiment, optionally the weight ratio of organic polymer to inorganic matter in the first organic particles is 99:1-1:1, optionally 70:30-1:1.

[0013] In any embodiment, optionally, based on the total weight of the organic polymer in the first organic particles, The content of the first polymerizable monomer is 35-80% by weight, and optionally 45-70% by weight; The content of the second polymerizable monomer is 0-30% by weight, optionally 5-25% by weight; and The content of the third polymerizable monomer is 5-40% by weight, optionally 8-35% by weight.

[0014] In any embodiment, optionally, the inorganic matter in the first organic particles is selected from one or more of oxides of silicon, aluminum, calcium, zinc, magnesium, sodium sulfate, sodium benzoate, calcium carbonate and modified materials thereof, optionally one or more of silicon dioxide, silica sol, aluminum oxide, zinc oxide, magnesium oxide, sodium benzoate, and further optionally one or more of fumed silicon dioxide, silicon fine powder, aluminum oxide, sodium benzoate.

[0015] In either embodiment, optionally, the surface of the first organic particles is uneven, and inorganic oxide clusters having a particle size of 10-200 nm are uniformly distributed thereon.

[0016] In either embodiment, optionally the weight ratio of the organic polymer to the plasticizer in the pressure sensitive adhesive is (4-25):1, optionally (4-11):1.

[0017] The relative contents of the organic polymer and the plasticizer in the pressure-sensitive adhesive within the above ranges ensures that a relatively large adhesive force is obtained between the electrode plate and the separator, which is advantageous for improving the adhesive performance and the cycle performance without significantly increasing the resistance of the separator.

[0018] In either embodiment, optionally, the pressure sensitive adhesive has a core-shell structure, and both the core and the housing of the core-shell structure comprise an organic polymer and a plasticizer, and wherein the weight ratio of the organic polymer to the plasticizer in the core is (3-4):1, optionally (3.2-3.8):1, and the weight ratio of the organic polymer to the plasticizer in the housing structure is (7-9):1, optionally (7.5-8.5):1.

[0019] The core and housing of the core-shell structure are mainly composed of organic polymers and plasticizers, which can further improve the pressure-sensitive performance of the pressure-sensitive adhesive, thereby improving the applicability of the separator to different pressure modes, and is favorable to reducing the resistance of the separator, thereby improving the dynamic performance of the separator.

[0020] In any embodiment, optionally in the pressure sensitive adhesive, a portion of the plasticizer is grafted to the organic polymer, and optionally in the pressure sensitive adhesive, at least 5 wt % of the plasticizer, based on the weight of the plasticizer, is grafted to the organic polymer.

[0021] When a part of the plasticizer is grafted to the organic polymer, it can prevent the plasticizer from migrating into the electrolyte in large amounts during cycling, thereby avoiding consuming various functional additives in the electrolyte, and further increasing the resistance of the separator, affecting the dynamic performance of the battery core.

[0022] In either embodiment, optionally the pressure sensitive adhesive has a volume average particle size Dv50 of 0.3-3.5 μm, optionally 0.8-2.0 μm.

[0023] A pressure-sensitive adhesive with an appropriate particle size helps to distribute uniformly on the first organic particles or on both the first organic particles and the second organic particles, and helps to exert adhesion between the core and the housing and the electrode plate under a certain pressure, and effectively improves the dynamic performance of the separator.

[0024] In either embodiment, optionally the pressure sensitive adhesive has a glass transition temperature of -50°C-100°C, optionally -45°C-60°C.

[0025] When the vitrification transition temperature of the pressure-sensitive adhesive is within the above range, it is advantageous to ensure the adhesive strength at room temperature, and to avoid an adhesive strength of more than 0.08 N / m at 1 MPa, which would cause the separator to adhere during storage and make it difficult to wind and unwind the separator, and to avoid an adhesive strength of less than 0.1 N / m at room temperature and 2 MPa, which would cause the adhesion between the separator and the electrode plate to be weak, which would be disadvantageous in shaping the battery core.

[0026] In any embodiment, optionally, in the pressure sensitive adhesive, the organic polymer comprises a copolymer obtained by copolymerizing a mixture of at least one of the following first monomer group, at least one of the following second monomer group, at least one of the following third monomer group, and at least one of the following reactive dispersing agents, i.e. A first group of monomers includes acrylic acid, methacrylic acid, methyl methacrylate, tert-butyl methacrylate, isobornyl methacrylate, methylol acrylamide, acrylamide, styrene, and acrylonitrile; The second group of monomers is acrylic acid C4-C 22 Alkyl esters, such as isobutyl acrylate, isooctyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate (isooctyl acrylate), cyclohexyl acrylate, ethyl methacrylate, isobutyl methacrylate, 2-ethylhexyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, and benzyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, ethylene urea ethyl methacrylate, dicyclopentenyloxyethyl methacrylate, tetrahydrofuryl methacrylate, trifluoroethyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, acrylic methacrylate, and dicyclopentenyloxyethyl methacrylate; A third group of monomers includes 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, glycidyl acrylate, glycidyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, gamma-methacryloxypropyltrimethoxysilane, N-methylol acrylamide, N-butoxymethacrylamide, diacetone acrylamide (DAAM), ethyl acetoacetate methacrylate (AAEM), divinylbenzene, epoxy resins with an epoxy value of 0.35-0.50, divinylbenzene, and Reactive dispersants include polyvinyl alcohol, polypropylene alcohol, polypropylene glycol, polyethylene glycol, polyvinyl alcohol.

[0027] In any embodiment, optionally, the reactive dispersant has an alcoholysis degree of ≧85% and a number average polymerization degree of 400-2000, and preferably has an alcoholysis degree of ≧88% and a number average polymerization degree of 500-1600.

[0028] In any embodiment, optionally the plasticizer is glycerol C4-C 10 Alkyl di- or mono-ethers, glycerol C4-C 10 Carboxylic acid monoester or diester, propylene glycol C4-C 10 The alkyl ether or glycerol may be selected from one or more of the following: alkyl monoethers or glycerol.

[0029] In either embodiment, optionally the average thickness of the coating is 0.8-22 μm, optionally 2-15 μm.

[0030] In any embodiment, optionally, the second organic particles are polymers of one or more monomers containing halogen, phenyl, epoxy, cyano, ester and amide groups; Optionally, the second organic particles are selected from at least one of homopolymers or copolymers of fluorine-containing alkenyl monomer units, homopolymers or copolymers of olefin-based monomer units, homopolymers or copolymers of unsaturated nitrile-based monomer units, homopolymers or copolymers of alkylene oxide-based monomer units, dipolymers, homopolymers or copolymers of monosaccharide monomer units, and modified compounds of the above homopolymers or copolymers.

[0031] In any embodiment, optionally, the fluorine-containing alkenyl monomer unit is selected from one or more of difluoroethylene, vinylidene fluoride, trifluoroethylene, trifluorochloroethylene, tetrafluoroethylene, hexafluoropropylene, or derivatives thereof.

[0032] In any embodiment, optionally, the olefinic monomer units are selected from one or more of ethylene, propylene, butadiene, isoprene, styrene, or derivatives thereof.

[0033] In any embodiment, optionally, the unsaturated nitrile-based monomer units are selected from one or more of acrylonitrile, methacrylonitrile, or derivatives thereof.

[0034] In any embodiment, optionally, the alkylene oxide based monomeric units are selected from one or more of ethylene oxide, propylene oxide, or derivatives thereof.

[0035] In either embodiment, optionally, the monosaccharide monomer unit is selected from glucose or a derivative thereof.

[0036] In any embodiment, optionally, the second organic particles are selected from at least one of polyperfluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polystyrene-co-methyl methacrylate, polystyrene-co-butyl acrylate, styrene-butyl acrylate-isooctyl acrylate, polymethyl methacrylate, polyacrylonitrile, polyvinyl acetate, polyethylene-co-vinyl acetate, polyimide, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, and cyanoethyl sucrose.

[0037] In any embodiment, optionally, the second organic particles are selected from at least one of polyvinylidene fluoride-co-hexafluoropropylene, polystyrene-co-butyl acrylate, styrene-butyl acrylate-isooctyl acrylate, polyperfluoroethylene, polyvinylidene fluoride, and polyvinylidene fluoride-co-trichloroethylene.

[0038] In any embodiment, optionally, the second organic particles include (1) the volume average particle diameter Dv50 of the second organic particles is 2-20 μm, and optionally 6-15 μm; (2) the melting point of the second organic particles is 130-160°C, optionally 138-150°C; (3) The weight average molecular weight of the second organic particles is 400×10 3 g / mol-1000×10 3 g / mol, selectively 450×10 3 g / mol-650×10 3 g / mol, One or more of the following conditions are met:

[0039] The melting point of the second organic particles is within the above range, and can withstand the swelling of the electrolyte, on the one hand, does not consume excessive electrolyte, and is not likely to cause residual monomers to be bubbled by the electrolyte and block the separator, leading to an increase in the resistance of the separator and thus affecting the dynamic performance of the battery core, and on the other hand, the adhesion between the separator and the electrode plate is not significantly reduced, and the electrode plate is not likely to be pressure-damaged by the second organic particles and thus to deteriorate the safety performance.

[0040] In any embodiment, optionally, the separator comprises: (1) the porosity of the substrate is 10-95%; (2) the hole diameter of the substrate is 20-60 nm; (3) the thickness of the substrate is 3-12 μm, and optionally 5-9 μm; (4) The substrate is a film or nonwoven fabric selected from one or more of polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyether ether ketone, polyaryl ether ketone, polyetherimide, polyamide imide, polybenzimidazole, polyether sulfone, polyphenylene ether, cycloolefin copolymer, polyphenylene sulfide, and polyethylene naphthalene; One or more of the following conditions are met:

[0041] If the separator satisfies one or more of the above conditions, it is advantageous to further improve the adhesive performance of the separator and the dynamic performance and cycle performance of the corresponding secondary battery.

[0042] In any embodiment, optionally, in the separator, the mass ratio of the first organic particles to the second organic particles is 10-100:0-90, optionally 20-90:0-60; Optionally, the ratio of the sum of the mass of the first organic particles and the second organic particles to the mass of the pressure sensitive adhesive is 20-92:8-20, optionally 60-90:10-15.

[0043] A second aspect of the present application provides a method for producing the separator of the first aspect of the present application, the method comprising the steps of: Step S1: adding first organic particles and a dispersant to a solvent to form a first polymer solution; Step S2: adding a pressure sensitive adhesive to the first polymer solution obtained in step S1 and thoroughly mixing to form a second polymer solution; Optionally, step S3 of adding second organic particles to the second polymer solution obtained in step S2 and thoroughly mixing to form a third polymer solution; and step S4 of applying the second polymer solution obtained in step S2 or the third polymer solution obtained in step S3 to at least one surface of a substrate and obtaining a separator after drying; The separator comprises a substrate and a coating applied to at least one surface of the substrate, the coating comprising 40-90 wt % first organic particles, 2-15 wt % pressure sensitive adhesive, and optionally 0-50 wt % second organic particles, the first organic particles comprising an organic polymer and an inorganic material, the pressure sensitive adhesive comprising an organic polymer and a plasticizer, optionally a volume average particle size of the first organic particles satisfying (Dv90-Dv10) / Dv50≦2.5, optionally ≦2, further optionally ≦1.8, and a vitrification transition temperature of the first organic particles is 20-100° C., optionally 30-80° C., and optionally a viscosity of the separator is less than 0.1 g m -2 Ω -1 ≦ρ / R≦1.0g m -2 Ω -1 , selectively 0.5g m -2 Ω -1 ≦ρ / R≦0.9g m -2 Ω -1 , and more selectively 0.6 g m -2 Ω -1 ≦ρ / R≦0.8g m -2 Ω -1 where ρ represents the areal density of the coating on the substrate and R represents the resistance of the separator at 25° C.

[0044] A third aspect of the present application provides a secondary battery, the secondary battery including a positive electrode plate, a negative electrode plate, a separator located between the positive electrode plate and the negative electrode plate, and an electrolyte, the separator being the separator of the first aspect of the present application or a separator produced by the method of the second aspect of the present application.

[0045] In any embodiment, optionally, the adhesive strength between the positive electrode plate and the separator of the secondary battery satisfies 1.2≦F2 / F1≦4, optionally 1.5≦F2 / F1≦3.8, where F1 represents the adhesive strength between the positive electrode plate and the separator at 25° C. and ≧2 MPa, and F2 represents the adhesive strength between the positive electrode plate and the separator at 95° C. and ≧2 MPa.

[0046] A fourth aspect of the present application provides a battery module, the battery module including the secondary battery according to the third aspect of the present application. The battery module can be manufactured by adopting a manufacturing method commonly used in the art.

[0047] A fifth aspect of the present application provides a battery pack, which includes at least one of the secondary battery according to the third aspect of the present application or the battery pack according to the fourth aspect of the present application. The battery pack can be manufactured by adopting a manufacturing method commonly used in the art.

[0048] A sixth aspect of the present application provides a power consumption device, the power consumption device including at least one of the secondary battery according to the third aspect of the present application, the battery module according to the fourth aspect of the present application, or the battery pack according to the fifth aspect of the present application. The power consumption device can be manufactured by adopting a manufacturing method commonly used in the art. Effect of the Invention

[0049] The separator according to the present application comprises a substrate and a coating applied to at least one surface of the substrate, the coating comprising 40-90 wt% of first organic particles, 2-15 wt% of a pressure-sensitive adhesive polymer, and optionally 0-50 wt% of a second organic particle. The pressure-sensitive adhesive comprises an organic polymer and a plasticizer, and the pressure-sensitive adhesive can have good pressure-sensitive properties by the cooperation of both, so that the coating has good pressure-sensitive characteristics, and the separator also has good pressure-sensitive properties. In particular, the separator can have a slight adhesive action with the electrode plate at room temperature (generally 20-30°C, e.g. 25°C) and a pressure of ≦1 MPa, but can have a clear adhesive action with the separator electrode plate at room temperature and a pressure of ≧2 MPa, and the adhesion between the separator and the electrode plate is significantly improved, especially at 95°C and a pressure of ≧2 MPa. Thus, on the one hand, the electrode plate and the separator of the electrochemical device are closely attached at room temperature, which avoids the occurrence of misalignment between the electrode plate and the separator of the electrochemical device during production and transfer, effectively prevents wrinkles in the negative electrode caused by insufficient adhesion between the separator and the electrode plate, and further ensures the structural stability of the electrochemical device, which is favorable for increasing the yield of shell insertion, thereby improving the shaping performance and safety performance of the battery core and reducing production costs. On the other hand, the separator according to the present application does not adhere excessively during winding and storage, which is convenient for use in the subsequent manufacture of battery cores. Optionally, the first organic particles have a volume average particle size satisfying (Dv90-Dv10) / Dv50≦2.5 and a vitrification transition temperature of 20°C-100°C, which is favorable for improving the application of the adhesive coating and avoiding blocking of the separator holes, thereby avoiding an increase in the internal resistance of the separator. Finally, optionally, the separator described in the present application has a viscosity of 0.1 g m -2 Ω -1 ≦ρ / R≦1.0g m -2 Ω -1 By satisfying the above, it is advantageous to ensure a suitable separator coating surface density and to avoid excessive resistance of the separator, thereby achieving both the manufacturing yield and the dynamic performance requirements of the battery core.

[0050] The battery module, battery pack and power consuming device described in the present application include the separator according to the first aspect of the present application or the secondary battery according to the second aspect of the present application, and therefore have the same advantages as the separator or secondary battery according to the present application. [Brief description of the drawings]

[0051] In order to more clearly explain the technical solutions of the embodiments of the present application, the following briefly introduces the drawings that need to be used in the embodiments of the present application. It is obvious that the drawings described below are only some embodiments of the present application, and those skilled in the art can also obtain other drawings based on the drawings without exerting creative efforts. [Figure 1] 1 is a schematic diagram of a secondary battery according to an embodiment of the present application; [Diagram 2] FIG. 1 is a schematic diagram of a battery module according to an embodiment of the present application. [Diagram 3] 1 is a schematic diagram of a battery pack according to an embodiment of the present application. [Figure 4] FIG. 4 is an exploded schematic view of FIG. 3. [Diagram 5] 1 is a schematic diagram of a power consuming device according to an embodiment of the present application; [Figure 6] 6-a, 6-b and 6-c show topographical photographs of the pressure sensitive coating of a separator produced in one embodiment of the present application, which are scanning electron microscope images at different magnifications. [Figure 7] 7-a, 7-b and 7-c show topographical photographs of the pressure sensitive coating of a separator produced in one embodiment of the present application, and are scanning electron microscope images at different magnifications. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0052] Hereinafter, with reference to the drawings as appropriate, embodiments specifically disclosing the separator, the manufacturing method thereof, the secondary battery, the battery module, the battery pack, and the power consumption device of the present application will be described in detail. However, unnecessary detailed description may be omitted. For example, detailed description of well-known matters and duplicated description of structures that are actually the same may be omitted. This is to avoid the following description becoming unnecessarily long and to allow those skilled in the art to easily understand. Note that the drawings and the following description are provided to allow those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.

[0053] The "ranges" disclosed in this application are defined in the form of lower and upper limits, and a given range is defined by selecting one lower limit and one upper limit, and the selected lower and upper limits define the boundaries of the particular range. Such defined ranges may be inclusive or exclusive of the extreme values, and may be arbitrarily combined, i.e., any lower limit may be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a particular parameter, it is understood that ranges of 60-110 and 80-120 are also contemplated. However, if 1 and 2 are listed as minimum range values, and 3, 4, and 5 are listed as maximum range values, the ranges 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5 are all contemplated. In this application, unless otherwise specified, a numerical range "ab" represents a shorthand representation of any combination of real numbers of ab, where a and b are both real numbers. For example, the numerical range "0-5" represents a list of all real numbers between "0-5" already listed in this specification, and "0-5" is just a shorthand representation of combinations of these numbers. Also, expressing a parameter as an integer ≧2 is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0054] Unless otherwise stated, all the embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0055] Unless otherwise stated, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0056] Unless otherwise stated, all steps in this application may be performed in sequence or randomly, and preferably in sequence. For example, the method includes steps (a) and (b) to mean that the method may include steps (a) and (b) performed in sequence, or may include steps (b) and (a) performed in sequence. For example, the method mentioned above may further include step (c) to mean that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), may include steps (a), (c) and (b), may include steps (c), (a) and (b), etc.

[0057] Unless otherwise specified, the terms "comprise" and "comprises" referred to in this application may be open ended or closed ended. For example, the terms "comprise" and "comprises" may further include or include other ingredients not listed, or may include or include only the ingredients listed.

[0058] Unless otherwise stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, "A or B" is satisfied if A is true (or exists) and B is false (or does not exist), if A is false (or does not exist) but B is true (or exists), or if both A and B are true (or exist).

[0059] In the description of this specification, it should be explained that unless otherwise specified, "more than or equal to" and "less than or equal to" are inclusive, and "multiple" in "one or more" means two or more than two.

[0060] It should be explained that in this application, the term "average degree of polymerization" means that the polymer is composed of homogeneous polymer molecules with different degrees of polymerization, and the degree of polymerization has a statistical average meaning. There are two most commonly used ways to express the average degree of polymerization: the degree of polymerization obtained by averaging the number of molecules is called the number average degree of polymerization, and the degree of polymerization obtained by averaging the weight is called the weight average degree of polymerization. In this application, the "average degree of polymerization" is the number average degree of polymerization.

[0061] It should be explained that in this application, the term "alcoholization degree" refers to the percentage of hydroxyl groups in the product obtained after alcoholysis to the original groups, and the unit is mole fraction %. For example, if the original groups (ester groups) are 100 and the hydroxyl groups after alcoholysis are 60, the alcoholysis degree is 60%.

[0062] It should be noted that in this application, the terms "primary particles" and "secondary particles" have the meanings commonly used in the art. Specifically, a "primary particle" is a particle that does not form an aggregate state, and a "secondary particle" is a particle that is formed by the aggregation of two or more primary particles. Primary particles and secondary particles can be easily distinguished from each other by scanning electron microscope (SEM) images.

[0063] Secondary batteries have the advantages of high energy density, good portability, no storage effect, and environmental friendliness, making them a preferred item for power sources of power consumption devices. In secondary batteries, the separator is an important part for ensuring the safety performance of the battery. However, on the other hand, in the manufacturing process of the battery core of the electrochemical device, the electrode plate and the separator inevitably undergo misalignment during production and transfer. In the lightest case, the electrode plate will wrinkle after full charge, which will seriously affect the dynamic performance and reduce the safety performance of the battery core, and in the more severe case, the electrode plates will come into contact with each other, leading to the disposal of the dry battery core. Therefore, engineers coat the separator with an adhesive coating, and generally in the first composite process of the electrode plate and the separator of the electrochemical device, pre-pressure is applied with an appropriate pressure action to ensure that the electrode plate and the separator of the electrochemical device have a certain adhesion before entering the next process. However, due to the requirements of production efficiency and considering that the material structure will deteriorate under a relatively large pressure, the pressure and action time in the first process generally cannot meet the electrode plate and the separator of the electrochemical device to achieve a proper adhesion effect. In addition, in order to guarantee the margin of the battery core group and the yield of the shell insertion, the electrode plate and the separator of the electrochemical device are generally baked in a tunnel furnace at 80-100°C for ≧700s, and then pressure is applied to make the electrode plate and the separator of the electrochemical device adhere to each other. Therefore, if the adhesive strength between the separator and the electrode plate at room temperature (25°C) and the adhesive strength at high temperature (e.g. 95°C) are not well matched, the adhesive strength of the battery core will be insufficient or too large, and the resistance of the separator will be greatly increased, which will deteriorate the dynamic performance of the battery core and even cause safety risks.

[0064] On the other hand, during the transportation of the separator, proper adhesion is also required between the separators. If the adhesive force is too large, it may cause the separator layers to adhere to each other, which is disadvantageous for the subsequent high-speed combination of the electrode plate and the separator. In addition, the inventors have found in the course of research that inappropriate adhesive materials and inappropriate surface density of adhesive materials may cause the blocking of separator holes, resulting in a decrease in the manufacturing yield of the battery core and a decrease in the dynamic performance of the battery core.

[0065] In order to solve the above problems, the inventors conducted extensive research and found that by applying a pressure-sensitive adhesive coating to the separator substrate, it is possible to relatively well achieve low viscosity at low pressure and high viscosity at high pressure, and furthermore, the coating density of the pressure-sensitive coating and the resistance of the separator are within 0.1 g m -2 Ω -1 ≦ρ / R≦1.0g m -2 Ω -1 It has been found that by adjusting the separator so as to satisfy the above condition, the resistance of the separator can be further reduced and the dynamic performance of a secondary battery using the separator can be improved.

[0066] Separator A first aspect of the present application provides a separator, the separator comprising: A substrate; a coating applied to at least one surface of the substrate, the coating comprising 40-90 wt % first organic particles, 2-15 wt % pressure sensitive adhesive, and optionally 0-50 wt % second organic particles; the first organic particles include an organic polymer and an inorganic material, and the pressure sensitive adhesive includes an organic polymer and a plasticizer; Optionally, the volume average particle diameter of the first organic particles satisfies (Dv90-Dv10) / Dv50≦2.5, optionally ≦2, further optionally ≦1.8, and the vitrification transition temperature of the first organic particles is 20-100° C., optionally 30-80° C.; Optionally, the separator has a density of 0.1 g m -2 Ω -1 ≦ρ / R≦1.0g m -2 Ω-1 , selectively 0.5g m -2 Ω -1 ≦ρ / R≦0.9g m -2 Ω -1 , and more selectively 0.6 g m -2 Ω -1 ≦ρ / R≦0.8g m -2 Ω -1 where ρ represents the areal density of the coating on the substrate and R represents the resistance of the separator at 25° C.

[0067] The present application provides a coating comprising 40-90 wt% of first organic particles, 2-15 wt% of pressure-sensitive adhesive, and optional 0-50 wt% of second organic particles on at least one surface of a porous separator substrate. The pressure-sensitive adhesive comprises an adhesive polymer and a plasticizer, and the pressure-sensitive adhesive polymer can have good pressure-sensitive properties through the cooperation of both, so that the coating has good pressure-sensitive properties, and the separator also has good pressure-sensitive properties. In particular, the separator can have a slight adhesive action with the electrode plate under a pressure of ≦1 MPa, but can have a clear adhesive action with the electrode plate under a pressure of ≧2 MPa, and the adhesion between the separator and the electrode plate is significantly improved, especially at 95° C. and a pressure of ≧2 MPa. Thus, on the one hand, the electrode plate and the separator of the electrochemical device are closely attached at room temperature, which avoids the occurrence of misalignment between the electrode plate and the separator of the electrochemical device during production and transfer, effectively prevents the wrinkles of the negative electrode caused by insufficient adhesion between the separator and the electrode plate, and further ensures the structural stability of the electrochemical device, which is favorable for increasing the yield of shell insertion, thereby improving the shaping performance and safety performance of the battery core and reducing the production cost. On the other hand, the separator according to the present application does not adhere during winding and storage, which is convenient for use in the subsequent manufacture of the battery core. Optionally, the volume average particle diameter of the first organic particles satisfies (Dv90-Dv10) / Dv50≦2.5 and has a vitrification transition temperature of 20°C-100°C, which is favorable for improving the application of the adhesive coating and avoiding the blocking of the separator holes. Finally, optionally, the separator described in the present application has a mass of 0.1 g·m -2 Ω -1 ≦ρ / R≦1.0g m -2 Ω -1 By satisfying the above, it is advantageous to ensure a suitable separator coating areal density and further reduce the internal resistance of the separator, thereby achieving both the manufacturing yield and the dynamic performance requirements of the battery core.

[0068] In some embodiments, optionally the weight ratio of the first organic particles to the second organic particles to the pressure sensitive adhesive on a dry weight basis is 20-90:0-60:8-20, optionally 30-80:30-50:10-15.

[0069] When the mass ratio of the first organic particles to the second organic particles to the pressure-sensitive adhesive is within the above range, the wetting and distribution uniformity of the electrolyte can be effectively improved, the synergistic advantages of each component can be fully exerted, and the adhesive performance, dynamic performance and cycle performance can be improved.

[0070] It should be explained that in this application, the first organic particles are generally designated as primary particles, while the second organic particles are generally designated as secondary particles. The cooperation of the first organic particles and the second organic particles can reinforce the adhesive force between the separator and the electrode plate, and can also effectively ensure that the separator has a moderate and non-uniform pore structure, and the coating surface density ρ of the coating on the separator and the resistance R of the separator at 25°C are 0.1 g m -2 Ω -1 ≦ρ / R≦1.0g m -2 Ω -1 For example, the ρ / R of the coating is preferably 0.52 g m -2 Ω -1 , 0.65g m -2 Ω -1 , 0.8gm -2 Ω -1 , 0.83g m -2 Ω -1 , 0.9g m -2 Ω -1 , 0.96g m -2 Ω -1 or 0.98 g m -2 Ω -1 and the range consisting of either or both of these.

[0071] It should be noted that in the present application, both the first organic particles and the pressure-sensitive adhesive include an organic polymer. For ease of distinction, the organic polymer contained in the first organic particles may be referred to as the "first organic polymer" and the organic polymer in the pressure-sensitive adhesive may be referred to as the "third organic polymer."

[0072] In some embodiments, the coating optionally has an areal density on the separator of 0.1-1.9 g / m 2 and optionally 0.25-1.5 g / m 2 and more selectively 0.65-1.2 g / m 2 It is.

[0073] In addition, in the manufacturing process of the battery core, the first organic particles are primary particles, which can help form a uniform coating interface, and can effectively improve the problem of tab misalignment during the manufacturing of the battery core.

[0074] [First organic particle] In some embodiments, the first organic particles have a volume average particle size Dv50 of 3-36 μm, optionally 5-20 μm, for example, in the range of 3 μm, 5 μm, 20 μm, 30 μm, or 36 μm, or any combination thereof.

[0075] When the volume average particle diameter Dv50 of the first organic particles is within the above range, the first organic particles have a relatively large average particle diameter, which on the one hand can increase the effective contact area between the electrode plate and the separator, and further greatly enhance the adhesive action between the electrode plate and the separator, and on the other hand can prevent these organic particles from penetrating into the holes formed on the separator substrate. At the same time, the existence of relatively large gaps in the large size can solve the problem of poor separator breathability, reduce the possibility of small particles blocking the separator holes, and reduce the risk of increased internal resistance. In addition, since it is difficult to combine the corners in the manufacturing process of the battery core (especially for rectangular housing batteries), the separator and the electrode plate here are not bonded, and the separator cannot effectively transfer and release the stress accumulated in the electrode plate to the surroundings, and the corners are poked due to the structural characteristics of the battery core module itself of the rectangular housing battery, and the stress formed by the expansion of the electrode plate is difficult to release. Therefore, if there is not enough space at the corners of the battery, after a certain number of cycles, i.e., when the stress is greater than the elongation rate of the copper-aluminum foil, the plate will break and even break through the separator, leading to serious safety risks. Meanwhile, in the present application, the first organic particles have a relatively large average particle size and a certain compressive ability, so that when they are present at the corners of the battery core, they can effectively provide stress relief space at the corners. At the same time, the first organic particles satisfy (Dv90-Dv10) / Dv50≦2.5, which ensures that the variation in the thickness of the separator is relatively small, and the deviation of the tab caused by the change in the thickness of the separator is not increased, and the manufacturing yield of the battery core is not reduced.

[0076] In some embodiments, the vitrification transition temperature of the first organic particles is optionally 20-100° C., optionally 30-80° C. Examples include ranges of 20° C., 30° C., 40° C., 60° C., 80° C., or 100° C., and any and all of the foregoing.

[0077] When the vitrification transition temperature of the first organic particles is within the above range, the particles can withstand the swelling of the electrolyte, on the one hand, the electrolyte is not consumed excessively, and the residual monomer is not easily bubbled by the electrolyte to block the separator, which affects the dynamic performance of the battery core, and on the other hand, the adhesion between the separator and the electrode plate is not significantly reduced, and the electrode plate is not easily pressure-damaged by the first organic particles, which reduces the safety performance.

[0078] In some embodiments, optionally, the weight average molecular weight of the organic polymer in the first organic particles is 500×10 3 g / mol-1000×10 3 g / mol, and selectively 800×10 3 g / mol-1000×10 3 The weight average molecular weight is g / mol. The weight average molecular weight can be measured by a method commonly used in the art, for example, by gel permeation chromatography, with reference to GB / T 21863-2008.

[0079] In some embodiments, optionally, the first organic particles in the separator of the present application include an organic polymer and an inorganic material, wherein the organic polymer in the first organic particles comprises at least: a first polymerizable monomer having at least one ester bond and selectively one or more of methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, vinyl acetate, trifluoroethyl methacrylate, glycidyl methacrylate, or trimethylolpropane triacrylate, and further selectively one or more of methyl methacrylate, lauryl acrylate, lauryl methacrylate, or trimethylolpropane triacrylate; a second polymerizable monomer having at least one cyano bond and optionally one or more of acrylonitrile, methacrylonitrile, ethacrylonitrile, and further optionally one or more of acrylonitrile, methacrylonitrile; A monomer having at least one amide bond, optionally one or more of acrylamide, N-methylolacrylamide, and N-butoxymethacrylamide, and further optionally one or more of acrylamide and N-methylolacrylamide, polymerized with a third polymerizable monomer; Optionally, the weight ratio of the first polymerizable monomer to the second polymerizable monomer to the third polymerizable monomer is 1:0-0.8:0.05-0.75, and optionally 1:0.1-0.6:0.1-0.6.

[0080] When the organic polymer is formed by polymerizing the above-mentioned polymerizable monomer, the first organic particles produced have good adhesive properties and a relatively low vitrification transition temperature. In addition, when the sprayed surface density ρ of the adhesive material on the separator and the resistance of the separator are R0.1g m -2 Ω -1≦ρ / R≦1.0g m -2 Ω -1 Satisfying this requirement reduces the resistance of the separator and helps improve the dynamic performance of the battery employing this separator.

[0081] In some embodiments, the organic polymer content of the first organic particles is preferably 50-99.9%, more preferably 60-99%, and even more preferably 70-99%, based on the total dry weight of the first organic particles; The content of inorganic matter in the first organic particles is 0.1-50%, alternatively 1-40%, more alternatively 1-30%, based on the total dry weight of the first organic particles.

[0082] If the content of the organic polymer in the first organic particles is too low or the content of the inorganic substance is too high, the adhesive performance of the first organic particles as a whole may be insufficient, and the organic polymer and the inorganic substance may not be held together. If the content of the inorganic substance in the first organic particles is too low, the flame retardancy of the first organic particles may be relatively poor.

[0083] In some embodiments, optionally the weight ratio of organic polymer to inorganic matter in said first organic particles is 99:1-1:1, optionally 70:30-1:1.

[0084] When the weight ratio of the organic polymer to the inorganic material in the first organic particles is within the above range, the synergistic function of the organic polymer and the inorganic material is fully exerted, which is advantageous for imparting good adhesive performance and flame retardancy to the first organic particles.

[0085] In some embodiments, the content of the first polymerizable monomer is 35-80 wt %, and optionally 45-70 wt %, based on the total weight of the organic polymer in the first organic particles; The content of the second polymerizable monomer is 0-30% by weight, optionally 5-25% by weight; and The content of the third polymerizable monomer is 5-40% by weight, optionally 8-35% by weight.

[0086] When the contents of the first polymerizable monomer, the second polymerizable monomer and the third polymerizable monomer are all within the above ranges, the synergistic advantages of each monomer are fully exerted, which is advantageous for improving the adhesive performance of the organic polymer, while providing an appropriate glass transition temperature, and further improving the adhesive performance of the first organic particles.

[0087] In some embodiments, optionally, the inorganic matter in the first organic particles is selected from one or more of oxides of silicon, aluminum, calcium, zinc, magnesium, and sodium sulfate, sodium benzoate, calcium carbonate, and modifications thereof, optionally one or more of silicon dioxide, silica sol, aluminum oxide, zinc oxide, magnesium oxide, sodium benzoate, and further optionally one or more of fumed silicon dioxide, silicon powder, aluminum oxide, and sodium benzoate.

[0088] In some embodiments, the surface of the first organic particles is optionally uneven and has inorganic oxide clusters with a particle size of 10-200 nm uniformly distributed thereon.

[0089] The present application further provides a method for producing the first organic particles of the present application, the method including at least the following steps:

[0090] Step 1: providing a first polymerizable monomer, a second polymerizable monomer and a third polymerizable monomer, wherein the weight ratio of the first polymerizable monomer to the second polymerizable monomer and the third polymerizable monomer is 1:0-0.8:0.05-0.75, optionally 1:0.1-0.6:0.1-0.6; Step 2: Polymerizing the polymerizable monomer to obtain an organic polymer; Step 3: adding an organic solvent and an inorganic substance to the organic polymer of step 2, and obtaining a mixed slurry after stirring; and Step 4: The mixed slurry of step 3 is dried, polished and pulverized to obtain the organic first particles described in the present application.

[0091] It should be explained that the polymerization of the polymerizable monomer may be carried out by any polymerization method commonly used in the art, for example, by emulsion polymerization or suspension polymerization.

[0092] In some embodiments, additives may be optionally added to the polymerization system of the polymerizable monomer, such as emulsifiers, for example, sodium lauryl sulfate, and polymerization initiators, for example, ammonium persulfate.

[0093] [Pressure-sensitive adhesive] The pressure sensitive adhesives described in this application include an organic polymer and a plasticizer.

[0094] In some embodiments, optionally the weight ratio of the organic polymer to the plasticizer in the pressure sensitive adhesive is (4-25):1, optionally (4-11):1.

[0095] The relative content of the plasticizer in the pressure-sensitive adhesive is within the above range, which ensures that a relatively large adhesive force is obtained between the electrode plate and the separator, and is advantageous for improving adhesion performance and cycle performance without a significant increase in the resistance of the separator.

[0096] In some embodiments, optionally, the pressure sensitive adhesive has a core-shell structure, and both the core and the housing of the core-shell structure comprise an organic polymer and a plasticizer, and wherein the weight ratio of the organic polymer to the plasticizer in the core is (3-4):1, optionally (3.2-3.8):1, and the weight ratio of the organic polymer to the plasticizer in the housing structure is (7-9):1, optionally (7.5-8.5):1.

[0097] The core and the housing of the core-shell structure are both composed of organic polymers and plasticizers, which can further improve the pressure-sensitive performance of the pressure-sensitive adhesive, thereby improving the applicability of the separator to different pressure modes, and is favorable for reducing the resistance of the separator, thereby improving the dynamic performance of the separator. On the other hand, the pressure-sensitive adhesive contains a plasticizer, and under a certain pressure action (e.g., 1-2 MPa), the plasticizer can rapidly migrate between the organic polymer and the separator base material, plasticize the adhesive polymer, extend its molecular chain, and generate intermolecular hydrogen bonding action with the thickener of the styrene butadiene rubber (SBR)-based adhesive and sodium carboxymethyl cellulose (CMC) in the negative electrode plate, and the adhesive of the positive electrode plate, such as polyvinylidene fluoride (PVDF), to enhance the wetting of the interface and reinforce the riveting action between the two interfaces. Under the action of ≧2 MPa, the core structure is broken, and the plasticizer in the core is released, which can further improve the above action.

[0098] In some embodiments, optionally in the pressure sensitive adhesive, a portion of the plasticizer is grafted to the organic polymer, optionally in the pressure sensitive adhesive, at least 5 wt% of the plasticizer is grafted to the organic polymer, based on the weight of the plasticizer. For example, 0 wt%, 3 wt%, 5 wt% or 8 wt% of the plasticizer is grafted to the organic polymer, optionally 8 wt% of the plasticizer is grafted to the organic polymer.

[0099] When a part of the plasticizer is grafted to the organic polymer, it can prevent the plasticizer from migrating into the electrolyte in large quantities during cycling, which would consume various functional additives in the electrolyte, and further avoid the increase in the resistance of the separator, affecting the dynamic performance of the battery core. In particular, when at least 5 wt% of the plasticizer is grafted to the organic polymer backbone, the separator and the plate can form a "disconnected yet connected" action, which can further improve the durability of the room temperature adhesion, reduce the rebound, and further ensure that the excess plasticizer does not migrate into the electrolyte during cycling and affect the performance of the battery core.

[0100] It should be noted that the grafting rate can be adjusted by methods well known in the art, such as adjusting the synthesis time to change the grafting rate. For details, refer to PCT application number PCT / CN2021 / 143069.

[0101] The graft ratio may be tested by a method commonly used in the art, such as an infrared test method. For example, it may be performed by the following steps: Obtain Fourier infrared spectrograms from each test of organic polymer, plasticizer, and pressure-sensitive adhesive; -1 A peak different from that of the organic polymer and the plasticizer alone appears at this position, and this peak represents the grafted plasticizer. The area under the peak represents the amount of the grafted plasticizer, and the graft rate of the plasticizer can be calculated based on this.

[0102] In some embodiments, the pressure sensitive adhesive optionally has a volume average particle size Dv50 of 0.3-3.5 μm, optionally 0.8-2.0 μm, for example, in the range of 0.3 μm, 0.5 μm, 0.8 μm, 1.0 μm, 2.0 μm, 3.0 μm, or 3.5 μm, or any combination thereof.

[0103] A pressure-sensitive adhesive having an appropriate particle size helps to distribute uniformly on the first or second organic particles, and helps to exert adhesion between the core and the housing and the electrode plate under a certain pressure, and effectively improves the resistance value of the separator.

[0104] In some embodiments, the pressure sensitive adhesive optionally has a glass transition temperature of -50°C-100°C, optionally -45°C-60°C.

[0105] When the glass transition temperature of the pressure-sensitive adhesive polymer is within the above range, it is advantageous to ensure the adhesive strength at room temperature, and to avoid the adhesive strength being greater than 0.08 N / m at room temperature and 1 MPa, which would cause the separator to adhere when wound, and the adhesive strength being less than 0.1 N / m at room temperature and 2 MPa, which would result in weak adhesion between the separator and the electrode plate, which would be disadvantageous in shaping the battery core.

[0106] In some embodiments, optionally, in the pressure sensitive adhesive, the organic polymer comprises a copolymer obtained by copolymerizing a mixture of at least one of the following first monomer group, at least one of the following second monomer group, at least one of the following third monomer group, and at least one reactive dispersant, i.e. The first group of monomers generally has a melting point greater than 80° C. and includes acrylic acid, methacrylic acid, methyl methacrylate, tert-butyl methacrylate, isobornyl methacrylate, methylol acrylamide, acrylamide, styrene, acrylonitrile; The second group of monomers generally has a melting point below 80° C. and is represented by the formula: 22Alkyl esters, such as isobutyl acrylate, isooctyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate (isooctyl acrylate), cyclohexyl acrylate, ethyl methacrylate, isobutyl methacrylate, 2-ethylhexyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, and benzyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, ethylene urea ethyl methacrylate, dicyclopentenyloxyethyl methacrylate, tetrahydrofuryl methacrylate, trifluoroethyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, acrylic methacrylate, and dicyclopentenyloxyethyl methacrylate; The third monomer group is a crosslinkable monomer, which contains at least one of a hydroxyl group, an amino group, and a double bond, and includes 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, glycidyl acrylate, glycidyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, γ-methacryloxypropyltrimethoxysilane, N-methylol acrylamide, N-butoxymethacrylamide, diacetone acrylamide (DAAM), ethyl acetoacetate methacrylate (AAEM), divinylbenzene, an epoxy resin having an epoxy value of 0.35-0.50, and divinylbenzene; and Reactive dispersants include polyvinyl alcohol, polypropylene alcohol, polypropylene glycol, polyethylene glycol, polyvinyl alcohol.

[0107] Optionally, in some embodiments, the weight ratio of the first monomer group monomers to the second monomer group monomers to the third monomer group monomers to the reactive dispersant is 35-45:45-60:4-8:2-5.

[0108] In the present application, the reactive dispersant plays a dispersing role while copolymerizing with the first monomer, the second monomer and the third monomer in the synthesis of the pressure-sensitive adhesive. Optionally, the alcoholysis degree of these reactive dispersants is ≧85%, and the number average polymerization degree is 400-2000, and optionally, the alcoholysis degree is ≧88%, and the number average polymerization degree is 500-1600.

[0109] In some embodiments, the plasticizer is optionally glycerol C4-C 10 Alkyl di- or mono-ethers, glycerol C4-C 10 Carboxylic acid monoester or diester, propylene glycol C4-C 10 The alkyl ether or glycerol may be selected from one or more of the following: alkyl monoethers or glycerol.

[0110] In some embodiments, the pressure sensitive adhesive polymer can optionally be prepared with reference to PCT Application No. PCT / CN2021 / 143069, the entire disclosure of which is incorporated herein by reference.

[0111] In some embodiments, the pressure sensitive adhesive polymer may optionally be synthesized according to a method comprising the steps of:

[0112] Step 1: Add emulsifier and oligomer to the solvent, and obtain a first mixed solution after uniform dispersion; Step 2: Add a stabilizer to the first mixed solution, and after uniform dispersion, obtain a second mixed solution; Step 3: Add aqueous initiator to the second mixed solution, mix uniformly, and react at 60-80°C for 20-60 minutes to obtain a third mixed solution; Step 4: Add the reactant monomer mixture dropwise evenly to the third mixed solution while stirring, and obtain a fourth mixed solution after 80-100 minutes, for example 80 minutes; Step 5: The fourth mixed solution is heated to 80-90° C., for example 84° C., and stirred for 120-240 minutes, for example 180 minutes, to obtain a fifth mixed solution; Step 6: Add a plasticizer to the fifth mixed solution, and react at 80-90°C, for example 84°C, for 120-240 minutes, for example 180 minutes to obtain a sixth mixed solution; Step 7: Add an aqueous initiator to the sixth mixed solution, and react at 60-80°C, for example 72°C, for 20-60 minutes, for example 30 minutes, to obtain a seventh mixed solution; Step 8: Add the reactant monomer mixture dropwise evenly to the seventh mixed solution while stirring, and obtain a fourth mixed solution after 100-160 minutes, for example 120 minutes; Step 9: Add a plasticizer to the eighth mixed solution, and react at 80-90°C, for example 84°C, for 120-240 minutes, for example 180 minutes to obtain a ninth mixed solution; Step 10: The ninth mixed solution is cooled to below 50°C and filtered to obtain a pressure-sensitive adhesive.

[0113] Optionally, in some embodiments, the solvent used in step 1 is deionized water.

[0114] In some embodiments, optionally, 0.1-1 wt % of an emulsifier and 2-3 wt % of an oligomer are added in step 1, in sequence, based on the total weight of the reactive monomer mixture (including monomers of the first monomer group, monomers of the second monomer group, monomers of the third monomer group, and reactive dispersant), co-agents (including emulsifiers, stabilizers, aqueous initiators), and plasticizers added in synthesizing the pressure sensitive adhesive, and so forth.

[0115] In some embodiments, the emulsifier is optionally selected from one or more of propyl sulfonate, polyoxyethylene alkyl ether, polyoxyethylene aryl ether, and sorbitol.

[0116] Optionally, in some embodiments, the stabilizer is selected from one or more of polyethylene oxide, allyl polyether sulfate, methylene succinic acid (itaconic acid), styrene sulfonic acid, sodium vinyl sulfonate, and sodium nanocellulose.

[0117] In some embodiments, the aqueous initiator is optionally selected from one or more of sodium bicarbonate, benzoyl peroxide, lauroyl peroxide, cumene hydroperoxide, t-butyl hydroperoxide, di-t-butyl peroxide, dicumyl peroxide, t-butyl peroxybenzoate, t-butyl peroxypivalate, methyl ethyl ketone peroxide, cyclohexanone peroxydiisopropyl carbonate, dicyclohexyl peroxydicarbonate, potassium persulfate, sodium persulfate, ammonium persulfate, azobisisobutyronitrile, azobisisoheptonitrile, ammonium persulfate-sodium bicarbonate.

[0118] Optionally, in some embodiments, the oligomer has a number average molecular weight of ≦1000 and a melting point of 0-30° C.

[0119] In some embodiments, the oligomer is optionally selected from, for example, stearyl methacrylate.

[0120] In some embodiments, optionally, in step 1, the dispersion is performed at a rotation speed of 8000-12000 r / min (revolutions per minute), for example 10000 r / min, for 20-60 minutes, for example 50 minutes, to achieve uniform dispersion.

[0121] In some embodiments, optionally the operating temperature in step 1 is 20-40°C, for example 25°C.

[0122] In some embodiments, optionally, in step 2, 1-4 wt % of a stabilizer is added to the first mixture solution.

[0123] In some embodiments, optionally, in step 2, mixing is performed at 6000-8000 r / min, e.g., 6500 r / min, for 20-60 minutes, e.g., 30 minutes, to achieve uniform mixing.

[0124] In some embodiments, optionally the operating temperature in step 2 is 20-60°C, for example 45°C.

[0125] In some embodiments, optionally, in step 3, 0.05-0.5 wt % of an aqueous initiator is added to the second mixture solution.

[0126] In some embodiments, optionally, in step 3, mixing is performed at 8000-12000 r / min, for example 8000 r / min, for 20-60 minutes, for example 30 minutes, to achieve uniform mixing.

[0127] In some embodiments, optionally the operating temperature in step 3 is 60-80°C, for example 72°C.

[0128] In some embodiments, optionally, in step 4, 35%-45% by weight of the reacting monomer mixture is added dropwise to the third mixture solution.

[0129] In some embodiments, optionally, the stirring speed in step 4 is 100-1000 r / min, for example 400 r / min.

[0130] In some embodiments, optionally, in step 4, the dropping is preferably completed exactly at 60 minutes.

[0131] In some embodiments, optionally, the stirring speed in step 5 is 12000-18000 r / min, for example 15000 r / min.

[0132] In some embodiments, optionally, in step 6, 10-20 wt % of a plasticizer, such as glycerol, is added to the fifth mixture solution.

[0133] In some embodiments, optionally, the stirring speed in step 6 is 12000-18000 r / min, for example 15000 r / min.

[0134] In some embodiments, optionally, in step 7, 0.05-0.5% by weight of an aqueous initiator is added to the sixth mixture solution.

[0135] In some embodiments, optionally, the stirring speed in step 7 is 8000-12000 r / min, for example 8000 r / min.

[0136] In some embodiments, optionally, in step 8, 30%-40% by weight of the reacting monomer mixture is added dropwise to the seventh mixture solution.

[0137] In some embodiments, optionally, the stirring speed in step 8 is 100-1000 r / min, for example 400 r / min.

[0138] In some embodiments, optionally, in step 8, the dripping of the reacting monomer mixture is completed at exactly 60 minutes.

[0139] In some embodiments, optionally, in step 9, 5-20% by weight of a plasticizer, such as glycerol, is added to the eighth mixed solution.

[0140] In some embodiments, optionally, the stirring speed in step 9 is 12000-18000 r / min, for example 15000 r / min.

[0141] It should be noted that those skilled in the art can also refer to the above method (omitting steps 7-9 and changing the mass fractions of the plasticizer and reacting monomer mixture added accordingly) to synthesize and obtain non-core-shell structured pressure-sensitive adhesive polymers.

[0142] [Second organic particle] The separator coating described in the present application optionally further includes a second organic particle.

[0143] Optionally, in some embodiments, the second organic particles are polymers of one or more monomers containing halogens, phenyl groups, epoxy groups, cyano groups, ester groups and amide groups.

[0144] In some embodiments, optionally, the second organic particles are selected from at least one of homopolymers or copolymers of fluorine-containing alkenyl monomer units, homopolymers or copolymers of olefin-based monomer units, homopolymers or copolymers of unsaturated nitrile-based monomer units, homopolymers or copolymers of alkylene oxide-based monomer units, dipolymers, homopolymers or copolymers of monosaccharide monomer units, and modified compounds of the above homopolymers or copolymers.

[0145] In some embodiments, the fluorine-containing alkenyl monomeric units are selected from one or more of difluoroethylene, vinylidene fluoride, trifluoroethylene, trifluorochloroethylene, tetrafluoroethylene, hexafluoropropylene, or derivatives thereof.

[0146] In some embodiments, the olefinic monomer units are selected from one or more of ethylene, propylene, butadiene, isoprene, styrene, or derivatives thereof.

[0147] In some embodiments, the unsaturated nitrile-based monomer units are selected from one or more of acrylonitrile, methacrylonitrile, or derivatives thereof.

[0148] In some embodiments, the alkylene oxide based monomeric units are selected from one or more of ethylene oxide, propylene oxide, or derivatives thereof.

[0149] In some embodiments, the monosaccharide monomer units are selected from glucose or derivatives thereof.

[0150] In some embodiments, the second organic particles are selected from at least one of polyperfluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polystyrene-co-methyl methacrylate, polystyrene-co-butyl acrylate, styrene-butyl acrylate-isooctyl acrylate, polymethyl methacrylate, polyacrylonitrile, polyvinyl acetate, polyethylene-co-vinyl acetate, polyimide, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, and cyanoethyl sucrose.

[0151] In some embodiments, the second organic particles may be at least one selected from polyvinylidene fluoride-co-hexafluoropropylene, polystyrene-co-butyl acrylate, styrene-butyl acrylate-isooctyl acrylate, polyperfluoroethylene, polyvinylidene fluoride, and polyvinylidene fluoride-co-trichloroethylene.

[0152] The second organic particles are similar to the first organic particles and may be produced by a polymerization method commonly used in the art, for example, by emulsion polymerization or suspension polymerization.

[0153] In some embodiments, the second organic particles comprise: (1) the volume average particle diameter Dv50 of the second organic particles is 2-20 μm, and optionally 6-15 μm; (2) the melting point of the second organic particles is 130-160°C, optionally 138-150°C; (3) The weight average molecular weight of the second organic particles is 400×10 3 g / mol-1000×10 3 g / mol, selectively 450×10 3 g / mol-650×10 3 g / mol, One or more of the following conditions are met:

[0154] By adopting the second organic particles within the above particle size range, the secondary battery can further form sufficient and non-uniformly distributed gaps between the first organic particles and the second organic particles during normal operation, and can ensure the smoothness of ion transmission channels, so that the battery has better cycle performance. The cooperation between the first organic particles and the second organic particles can reinforce the adhesive force between the separator and the electrode plate, and can also effectively ensure that the separator has a moderate and non-uniform pore structure.

[0155] The melting point of the second organic particles is within the above range, and can withstand the swelling of the electrolyte, while not consuming excessive electrolyte, and the residual monomer is not easily bubbled by the electrolyte to block the separator, which affects the dynamic performance of the battery core, while the adhesion between the separator and the electrode plate is not significantly reduced, and the electrode plate is not easily pressure-damaged by the second organic particles, which reduces the safety performance.

[0156] For example, the volume average particle size Dv50 of the second organic particles may be 2 μm, 8 μm, 10 μm, or 12 μm.

[0157] In some embodiments, the separator comprises: (1) the porosity of the substrate is 10-95%; (2) the hole diameter of the substrate is 20-60 nm; (3) the thickness of the substrate is 3-12 μm, and optionally 5-9 μm; (4) The substrate is a film or nonwoven fabric selected from one or more of polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyether ether ketone, polyaryl ether ketone, polyetherimide, polyamide imide, polybenzimidazole, polyether sulfone, polyphenylene ether, cycloolefin copolymer, polyphenylene sulfide, and polyethylene naphthalene; One or more of the following conditions are met:

[0158] If the separator satisfies one or more of the above conditions, it is advantageous to further improve the adhesive performance of the separator and the dynamic performance and cycle performance of the corresponding secondary battery.

[0159] In some embodiments, optionally in the separator, the mass ratio of the first organic particles to the second organic particles is 10-100:0-90, optionally 20-90:0-60; Optionally, the ratio of the sum of the mass of the first organic particles and the second organic particles to the mass of the pressure sensitive adhesive is 20-92:8-20, optionally 60-90:10-15.

[0160] As examples, the weight ratio of the first organic particles to the second organic particles may be 100:0, 90:10, 70:30, 50:50, 40:60, 65:25, or 75:10, and ranges consisting of any and both of these ratios.

[0161] As examples, the ratio of the sum of the mass of the first organic particles and the second organic particles to the mass of the pressure-sensitive adhesive may be 60:10, 80:10, 85:15, 90:10, or 110:10, and ranges consisting of any and both of these ratios.

[0162] In some embodiments, the average thickness of the coating is 0.8-22 μm, optionally 2-15 μm. By way of example, the average thickness may be in the range of 0.8 μm, 2 μm, 3 μm, 4 μm, 6 μm, 10 μm, 12 μm, 15 μm, 20 μm, or 22 μm, and any and all of the foregoing.

[0163] Manufacturing method of separator A second aspect of the present application provides a method for producing the separator according to the first aspect of the present application, the method comprising: Step S1: adding first organic particles and a dispersant to a solvent to form a first polymer solution; Step S2: adding a pressure sensitive adhesive to the first polymer solution obtained in step S1 and thoroughly mixing to form a second polymer solution; Optionally, step S3 of adding second organic particles to the second polymer solution obtained in step S2 and thoroughly mixing to form a third polymer solution; Step S4 of applying the second polymer solution obtained in step S2) or the third polymer solution obtained in step S3 to at least one surface of the substrate and drying to obtain a separator; Including, The separator comprises a substrate and a coating applied to at least one surface of the substrate, the coating comprising 40-90 wt % first organic particles, 2-15 wt % pressure sensitive adhesive, and optionally 0-50 wt % second organic particles, the first organic particles comprising an organic polymer and an inorganic material, the pressure sensitive adhesive comprising an organic polymer and a plasticizer, optionally a volume average particle size of the first organic particles satisfying (Dv90-Dv10) / Dv50≦2.5, optionally ≦2, further optionally ≦1.8, and a vitrification transition temperature of the first organic particles is 20-100° C., optionally 30-80° C., and optionally a viscosity of the separator is less than 0.1 g m -2 Ω -1 ≦ρ / R≦1.0g m -2 Ω -1 , selectively 0.5g m -2 Ω -1 ≦ρ / R≦0.9g m-2 Ω -1 , and more selectively 0.6 g m -2 Ω -1 ≦ρ / R≦0.8g m -2 Ω -1 where ρ represents the areal density of the coating on the substrate and R represents the resistance of the separator at 25° C.

[0164] In some embodiments, non-limiting examples of dispersants used in step S1 may include acrylates (e.g., BYK brand 22136), branched alcohol polyethers (e.g., Dow brand TMN-6), polyethylene glycol trimethyl nonyl ether, or mixtures thereof.

[0165] In some embodiments, non-limiting examples of the solvent used in step S1 may include acetone, tetrahydrofuran, dichloromethane, chloroform, dimethylformamide, N-methyl-2-pyrrolidone, cyclohexane, water, or mixtures thereof.

[0166] In some embodiments, non-limiting examples of the coating method used in step S4 may include dip coating, die coating, roller coating, comma coating, spray coating, or a combination thereof. The double-sided coating area density after drying is 0.32-1.92 g / m 2 may be also possible.

[0167] [Secondary battery] A third aspect of the present application provides a secondary battery, which has good safety and dynamic performance.

[0168] Generally, a secondary battery includes a positive electrode plate, a negative electrode plate, an electrolyte, and a separator. During battery charging, active ions shuttle between the positive electrode plate and the negative electrode plate to store and release. The electrolyte serves to conduct ions between the positive electrode plate and the negative electrode plate. Secondary batteries using electrolyte and some secondary batteries using semi-solid electrolyte further include a separator. The separator is disposed between the positive electrode plate and the negative electrode plate, and mainly serves to prevent short circuit between the positive electrode and the negative electrode, while allowing ions to pass through.

[0169] In the secondary battery according to the present application, the separator may be the separator according to the first aspect of the present application, which has good ion conductivity and adhesive performance at room temperature, and its resistance at room temperature (generally 20-30°C, e.g. 25°C) is 1.6Ω or less, particularly 1.2Ω or less, its adhesive strength at a pressure of ≦1MPa is 0.1N / m or less, particularly 0.08N / m or less, and its adhesive strength with the electrode plate at room temperature of ≧2MPa is 0.15N / m or more, particularly 0.4N / m or more, and its adhesive strength with the electrode plate at ≧2MPa, 95°C is 4.9N / m or less, particularly 1.8N / m or less.

[0170] When a secondary battery is manufactured using the separator according to the first embodiment of the present application, the adhesive strength F1 between the positive electrode plate and the separator at room temperature of 25° C. and ≧2 MPa and the adhesive strength F2 between the positive electrode plate and the separator at 95° C. and ≧2 MPa satisfy 1.2≦F2 / F1≦4, optionally 1.5≦F2 / F1≦3.8. At the same time, the surface density ρ of the coating on the substrate and the resistance R of the separator at 25° C. are less than 0.1 g m -2 Ω -1 ≦ρ / R≦1.0g m -2 Ω -1 , selectively 0.5g m -2 Ω -1 ≦ρ / R≦0.9g m -2 Ω -1 , and more selectively 0.6 g m -2 Ω -1 ≦ρ / R≦0.8g m -2 Ω -1If F2 / F1>4, the pre-cold pressing is insufficient during winding of the battery core, the battery core swells, the separator and the electrode plate are misaligned, and the inner electrode plate slips, which may cause the safety risk of short-circuiting of the electrode plate. In addition, the hot pressing adhesion is inappropriately excessive, which may cause the electrolyte to be difficult to infiltrate, affecting the chemical formation efficiency of the battery core, and may even cause black spots to form after full charge, leading to lithium precipitation, which will severely affect the dynamics and safety performance of the battery core. If F2 / F1<1.2, the pre-cold pressing meets the process requirements, but in the process of passing through the tunnel furnace to perform hot pressing, the thickness and width of the battery core may exceed the standard, swell, or the battery core may swell after being left for a certain period of time, which may reduce the yield of the battery core and reduce the production efficiency. In addition, the greater risk is that after being put into the shell and injected with the electrolyte, the hardness of the battery core may be extremely reduced, the electrode plate may be separated from the separator, and the expansion force of the battery core may increase. More seriously, the adhesion between the separator and the electrode plate is too low, and the repulsion of the negative electrode cannot be restrained, which may cause wrinkles and lithium precipitation problems, leading to deterioration of the battery core cycle performance.

[0171] [Positive electrode plate] The positive electrode plate includes a positive electrode current collector and a positive electrode film that is disposed on at least one surface of the positive electrode current collector and includes a positive electrode active material. For example, the positive electrode current collector has two surfaces that face each other in the thickness direction of the positive electrode current collector, and the positive electrode film is disposed on either one or both of the two facing surfaces of the positive electrode current collector.

[0172] The positive electrode current collector may be made of a material having good electrical conductivity and mechanical strength, and in some embodiments, may be made of aluminum foil.

[0173] The present application is not specifically limited to a specific type of positive electrode active material, and any material that can be used for the positive electrode of a secondary battery known in the art may be adopted, and those skilled in the art can select it according to actual needs.

[0174] In some embodiments, the secondary battery according to the present application is a lithium-ion secondary battery. The positive electrode active material includes positive electrode active materials for lithium-ion secondary batteries known in the art. For example, the positive electrode active material may include at least one material selected from the group consisting of lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other conventional materials that can be used as battery positive electrode active materials may be used. Here, examples of lithium transition metal oxides include lithium cobalt oxide (e.g., LiCoO2), lithium nickel oxide (e.g., LiNiO2), lithium manganese oxide (e.g., LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (e.g., LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM 333 (may be abbreviated as LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM 523 (may be abbreviated as LiNi 0.5 Co 0.25 Mn 0.25 O2(NCM 211 (may be abbreviated as LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM 622 (may be abbreviated as LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM 811 Lithium nickel cobalt aluminum oxide (e.g., LiNi 0.85 Co 0.15 Al 0.05Examples of the lithium-containing phosphate having an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (e.g., LiFePO4 (which may be abbreviated as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (e.g., LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, and a composite material of lithium manganese iron phosphate and carbon.

[0175] In some embodiments, the mass percentage of the positive electrode film that is made up of the positive electrode active material is optionally 75% to 99%, optionally 80% to 97%.

[0176] In some embodiments, the positive electrode membrane further includes an adhesive. The type of adhesive is not specifically limited, and those skilled in the art can select it according to actual needs. For example, the adhesive used in the positive electrode membrane may include one or more of polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE).

[0177] In some embodiments, optionally the adhesive occupies a mass percentage of the positive electrode membrane between 0.1% and 3.5%, optionally between 0.5% and 3%.

[0178] In some embodiments, the positive electrode film further includes a conductive agent. The type of the conductive agent is not specifically limited, and a person skilled in the art can select it according to actual needs. For example, the conductive agent used in the positive electrode film may include one or more of graphite, superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0179] In some embodiments, the conductive agent optionally comprises a mass percentage of the positive electrode membrane of 0.05% to 5%, optionally 0.5% to 3%.

[0180] In some embodiments, the step of employing the positive active material to manufacture a positive plate may include dispersing the positive active material, adhesive, and optional conductive agent in a solvent, which may be N-methylpyrrolidone, and uniformly stirring with a vacuum mixer to obtain a positive slurry, uniformly coating the positive slurry on a positive current collector aluminum foil, drying at room temperature, and then transferring to an oven for drying, and cold pressing and slitting to obtain a positive plate.

[0181] [Negative electrode plate] The negative electrode plate includes a negative electrode current collector and a negative electrode film disposed on at least one surface of the negative electrode current collector. For example, the negative electrode current collector has two surfaces facing each other in the thickness direction of the negative electrode current collector, and the negative electrode film layer is disposed on either one or both of the two facing surfaces of the negative electrode current collector.

[0182] The negative electrode current collector may be made of a material having good electrical conductivity and mechanical strength, and may be made of copper foil in some embodiments.

[0183] The negative electrode film includes a negative electrode active material, and the step of manufacturing a negative electrode plate by using the negative electrode active material may include a step of dispersing the negative electrode active material, an adhesive, and an optional thickener and a conductive agent in a solvent, which may be deionized water, to form a uniform negative electrode slurry, and a step of coating the negative electrode slurry on a negative electrode current collector, and obtaining a negative electrode plate after processes such as drying and cold pressing.

[0184] In some embodiments, the present application is not specifically limited to a specific type of negative electrode active material, and the negative electrode plate selectively includes a negative electrode active material that can be used in a secondary battery negative electrode. The negative electrode active material may be one or more of graphite materials (e.g., artificial graphite, natural graphite), mesocarbon microbeads (abbreviated as MCMB), hard carbon, soft carbon, silicon-based materials, and tin-based materials.

[0185] In some embodiments, the mass percentage of the negative electrode active material in the positive electrode film is optionally 75% to 99%, optionally 80% to 97%.

[0186] In some embodiments, the adhesive may be selected from one or more of polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), styrene butadiene rubber (SBR), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0187] In some embodiments, the adhesive optionally comprises a mass percentage of the negative electrode film of 0.1% to 3.5%, optionally 0.5% to 2.5%.

[0188] In some embodiments, the viscosity increasing agent may be sodium carboxymethylcellulose (CMC-Na).

[0189] In some embodiments, the thickener optionally comprises a mass percentage of the negative electrode film of 0.04% to 5%, optionally 0.5% to 3%.

[0190] In some embodiments, the conductive agent used in the negative plate may be selected from one or more of graphite, superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0191] In some embodiments, the weight percentage of the conductive agent in the negative electrode film is optionally 0.04% to 5%, optionally 0.5% to 3%.

[0192] [Electrolyte] The electrolyte serves to conduct ions between the positive and negative electrodes. The present application is not specifically limited to the type of electrolyte, which can be selected according to need. For example, the electrolyte may be liquid, gel, or all solid.

[0193] In some embodiments, the electrolyte is an electrolytic solution, which includes an electrolyte salt and a solvent.

[0194] In some embodiments, the electrolyte salt may be selected from one or more of LiPF6 (lithium hexafluorophosphate), LiBF4 (lithium tetrafluoroborate), LiClO4 (lithium perchlorate), LiAsF6 (lithium hexafluoroarsenate), LiFSI (lithium bis(fluorosulfonyl)imide), LiTFSI (lithium bis(trifluoromethanesulfonate), LiTFS (lithium trifluoromethanesulfonate), LiDFOB (lithium difluoro(oxalato)borate), LiBOB (lithium bis(oxalato)borate), LiPO2F2 (lithium difluorophosphate), LiDFOP (lithium difluorobis(oxalato)phosphate), and LiTFOP (lithium tetrafluoro(oxalato)phosphate).

[0195] In some embodiments, the concentration of the electrolyte salt in the non-aqueous electrolyte solution is, for example, 0.3 mol / L (moles / liter) or more, optionally 0.7 mol / L or more, optionally 1.7 mol / L or less, and further optionally 1.2 mol / L or less.

[0196] In some embodiments, the solvent may be selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS), and diethyl sulfone (ESE).

[0197] In some embodiments, the electrolyte solution further includes optional additives, for example, the additives may include an anode film-forming additive, may include a cathode film-forming additive, and may further include additives that can improve some performance of the battery, such as an additive that improves the overcharge performance of the battery, an additive that improves the high temperature performance of the battery, an additive that improves the low temperature performance of the battery, etc.

[0198] [Exterior body] In some embodiments, the secondary battery may include an exterior body for packaging the positive electrode plate, the negative electrode plate, the separator, and the electrolyte. As an example, the positive electrode plate, the negative electrode plate, and the separator may be stacked or wound to form a stacked structure battery core or a wound structure battery core, and the battery core is packaged in the exterior body, and the electrolyte may employ an electrolyte solution, which is infiltrated into the battery core. The number of battery cores in the secondary battery may be one or more, and can be adjusted according to demand.

[0199] In some embodiments, the exterior of the secondary battery may be a pouch, such as a bag-shaped pouch. The material of the pouch may be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc. The exterior of the secondary battery may be a hard case, such as an aluminum case.

[0200] In some embodiments, the positive plates, negative plates and separators can be fabricated into an electrode assembly by a winding or lamination process.

[0201] The present application is not particularly limited to the shape of the secondary battery, which may be cylindrical, rectangular or any other shape. Figure 1 shows a secondary battery 5 with a rectangular structure as an example.

[0202] [Battery modules, battery packs and power consuming devices] A fourth aspect of the present application provides a battery module, the battery module including the secondary battery according to the third aspect of the present application.

[0203] In some embodiments, the secondary battery according to the present application may be assembled into a battery module, and the number of secondary batteries included in the battery module may be multiple, with the specific number being adjustable according to the application and capacity of the battery module.

[0204] Fig. 2 shows an example of a battery module 4. Referring to Fig. 2, in the battery module 4, the multiple secondary batteries 5 may be arranged in sequence along the longitudinal direction of the battery module 4. Of course, they may be arranged in any other manner. Furthermore, the multiple secondary batteries 5 may be fixed by fasteners.

[0205] Optionally, the battery module 4 may further include a case having an accommodating space, and the multiple secondary batteries 5 are accommodated in the accommodating space.

[0206] A fifth aspect of the present application provides a battery pack, the battery pack including at least one of the secondary battery according to the third aspect of the present application or the battery module according to the fourth aspect of the present application.

[0207] In some embodiments, battery modules assembled from secondary batteries may be assembled into a battery pack, and the number of battery modules included in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0208] 3 and 4 show an example of a battery pack 1. Referring to Fig. 3 and 4, the battery pack 1 may include a battery box and a plurality of battery modules 4 installed in the battery box. The battery box may include an upper housing 2 and a lower housing 3, and the upper housing 2 may be covered by the lower housing 3 to form a sealed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner.

[0209] A sixth aspect of the present application provides a power consumption device, comprising at least one of the secondary battery according to the third aspect of the present application, the battery module according to the fourth aspect of the present application, or the battery pack according to the fifth aspect of the present application, and providing a power source to the power consumption device. The power consumption device may be, but is not limited to, a mobile device (e.g., a mobile phone, a laptop, etc.), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.

[0210] The power consumption device can select a secondary battery, a battery module or a battery pack according to its usage demand.

[0211] 5 shows an example of a power consuming device, such as a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. A battery pack or a battery module can be employed to meet the demand for high power and high energy density of the secondary battery of the power consuming device.

[0212] Other examples of power consuming devices include mobile phones, tablet computers, notebook computers, etc. These power consuming devices generally require thinness and can employ secondary batteries as their power source.

[0213] Working Example The following describes the examples of the present application. The examples described below are illustrative and are used only to interpret the present application, and should not be understood as limitations to the present application. If no specific techniques or conditions are specified in the examples, they are performed according to the techniques described in the literature in the field or according to the specifications of the conditions or products. If no manufacturer is specified, the reagents or instruments used are all ordinary products available on the market.

[0214] Example 1 Preparation of the first organic particles (P1) At room temperature, the necessary monomers were mixed uniformly with stirring in the weight percentage ratio of 25% by weight of 2-hydroxyethyl acrylate, 20% by weight of n-butyl acrylate, 5% by weight of methyl methacrylate, 5% by weight of trimethylolpropane triacrylate, 20% by weight of acrylonitrile, and 25% by weight of acrylamide. 2 kg of mixed monomers, 60 g of sodium lauryl sulfate emulsifier, 20 g of ammonium persulfate initiator, and 2.40 kg of deionized water were added to a 10 L four-neck flask containing a mechanical stirrer, a thermometer, and a condenser. The mixture was emulsified by stirring for 30 minutes at a rotation speed of 1600 rpm. Then, the temperature was raised to 75°C under nitrogen gas protection and reacted for 4 hours, after which the pH was adjusted to 6.5 with 1 wt% NaOH aqueous solution, and the temperature was immediately lowered to below 40°C and discharged, obtaining an organic polymer in an emulsion state, the solid content of which was about 45%.

[0215] The organic polymer and silicon dioxide were added to an appropriate amount of deionized water in a dry weight ratio of 9:1, and thoroughly mixed by stirring for 1 hour. The solvent was then removed by spray drying to obtain a powder. The powder was then polished and pulverized to obtain a Dv50 particle size of 8 μm, a particle size distribution (Dv90-Dv10) / Dv50 of 1.76, a DSC glass transition temperature of 60°C, and a weight average molecular weight of approximately 600×10 3 g / mol of primary organic particles were obtained.

[0216] Pressure sensitive adhesive manufacturing The pressure-sensitive adhesive includes an organic polymer and a plasticizer, where the organic polymer is 30 wt% isobutyl acrylate + 25 wt% isooctyl acrylate + 5 wt% 2-hydroxypropyl methacrylate + 15 wt% styrene + 22 wt% acrylonitrile + 3 wt% polyvinyl alcohol copolymer, the plasticizer is glycerol, and the graft rate is 8 wt%. It can be prepared by referring to the patent document having PCT application number PCT / CN2021 / 143069.

[0217] Separator manufacturing 1) A polyethylene microporous membrane (purchased from Shanghai Enji Co., Ltd.) with a thickness of about 9 μm, a hole diameter of about 50 nm, and a porosity of about 38% was used as the separator substrate. 2) 3.3 kg of a pressure-sensitive adhesive having a glass transition temperature of about 10° C., a volume average particle diameter Dv50 of about 1.1 μm, and a mass ratio of an organic polymer and a plasticizer of 5:1 (wherein, with respect to the weight of the plasticizer, about 8 wt % of the plasticizer is grafted onto the organic polymer), where the organic polymer is a copolymer of 30 wt % isobutyl acrylate + 25 wt % isooctyl acrylate + 5 wt % 2-hydroxypropyl methacrylate + 15 wt % styrene + 22 wt % acrylonitrile + 3 wt % polyvinyl alcohol, and the plasticizer is glycerol) is added to 23.6 kg of deionized water to obtain a first polymer solution; 3) Add an appropriate amount of first organic particles (P1, 25 wt% 2-hydroxyethyl acrylate + 20 wt% n-butyl acrylate + 5 wt% methyl methacrylate + 5 wt% trimethylolpropane triacrylate + 20 wt% acrylonitrile + 25 wt% acrylamide, Dv50 particle size is 6 μm, (Dv90-Dv10) / Dv50 is 1.76, glass transition temperature is 60° C., and weight average molecular weight is about 600×10 3 g / mol) and 18 g of a dispersant (BYK-22136, BYK Chemical, brand 22136) and thoroughly mixed to form a second polymer solution, wherein the second polymer solution has a mass ratio of the first organic particles to the pressure sensitive adhesive of 90:10 based on the dry weight; 4) The second polymer solution obtained in step 3) was made into an aqueous coating slurry, which was then coated on two surfaces of the separator substrate by spin spraying. After drying, 32 locations were selected, and the change in gram weight per unit area of ​​the separator before and after spin spraying was measured at each location. The average value was calculated, and the areal density ρ of the separator coating was determined to be 0.97 g / m 2 The produced separator includes a separator substrate and a pressure-sensitive coating applied to two surfaces of the separator substrate, the pressure-sensitive coating having a thickness of about 3 μm, and includes first organic particles and a pressure-sensitive adhesive in a mass ratio of 90:10 based on dry weight, and the pressure-sensitive adhesive includes an organic polymer and a plasticizer in a mass ratio of 5:1 (wherein about 8 wt % of the plasticizer is grafted to the organic polymer, based on the weight of the plasticizer).

[0218] Secondary battery manufacturing The active material is LiNi 1 / 3 Mn 1 / 3 Co 1 / 3O2, acetylene black as a conductive agent, and polyvinylidene fluoride (PVDF, weight average molecular weight 1.2 million g / mol) as an adhesive were mixed in a weight ratio of 94:3:3 in N-methylpyrrolidone solvent by thorough and uniform stirring to obtain a positive electrode slurry. This slurry was then coated on aluminum (Al) foil, dried, and cold pressed to obtain a positive electrode plate. The amount of positive electrode active material carried on the positive electrode plate was 0.32 g / 1540.25 mm 2 and the density is 3.45 g / cm 3 It is.

[0219] The active material, artificial graphite, the conductive agent, acetylene black, the adhesive, styrene butadiene rubber (SBR), and the thickener, sodium carbomethylcellulose (CMC), were mixed in a weight ratio of 95:2:2:1 in deionized water to obtain a negative electrode slurry. The slurry was then coated on copper (Cu) foil, dried, and cold pressed to obtain a negative electrode plate. The amount of graphite supported on the negative electrode plate was 0.18 g / 1540.25 mm. 2 and the density is 1.65 g / cm 3 It is.

[0220] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 3:5:2, and LiPF6 was uniformly dissolved in the above solution to obtain an electrolyte solution, in which the concentration of LiPF6 was 1 mol / L.

[0221] The separators produced in each of the Examples and Comparative Examples were used as separators for secondary batteries.

[0222] The positive electrode plate, separator, and negative electrode plate were stacked in order, with the separator positioned between the positive and negative electrodes to play the role of isolation, and then rewound to obtain a bare battery core. The bare battery core was placed in an exterior body, and electrolyte was injected and packaged to obtain a secondary battery. It should be noted that when the separator coating is single-sided, the coating surface faces the negative electrode (i.e., the positive electrode plate) side.

[0223] How we tested 1.Volume average particle size test Standard GB / T 19077-2016 / ISO 13320:2009 Particle size distribution laser diffraction method was referred to. Tested using a laser granulometer (Marvin 3000, MasterSizer 3000), with a helium-neon red light source as the main light source. Take one clean small beaker, add 1g of sample to be measured, add one drop of surfactant to promote sample dispersion, add 20ml of deionized water (ensure sample concentration is 8-12% light shielding), and sonicate at 53KHz / 120W for 5 minutes to ensure the sample is completely dispersed. Turn on the laser granulometer, clean the optical path system, and then automatically test the background. Stir the already sonicated solution to be measured, disperse it evenly, and put it into the sample pool as required, and start measuring the particle size. The measurement result can be read from the instrument.

[0224] 2. Vitrification transition temperature It may be measured by a method commonly used in the art, for example, by differential scanning calorimetry with reference to GB / T 19466.2. The temperature rise rate was 10° C. / min, and the atmosphere was air.

[0225] 3. Graft rate test of plasticizer in pressure-sensitive adhesive It may be detected by an infrared test method, specifically, by obtaining Fourier infrared spectrograms from each test of organic polymers, plasticizers, and pressure-sensitive adhesives, and detecting the Fourier infrared spectrum of the pressure-sensitive adhesive at 1500-1700 cm -1 A peak different from that of the organic polymer and the plasticizer alone appears at the position, and this peak represents the grafted plasticizer. The area under the peak represents the amount of the grafted plasticizer, and the graft ratio of the plasticizer (representing the peak area corresponding to the characteristic peak of the grafted plasticizer / peak area of ​​the plasticizer %100%) can be calculated.

[0226] 4. Evaluation of separator adhesion performance The test process is as follows:

[0227] 1. The prepared separator with a length of 300 mm and a width of 100 mm and the prepared positive and negative electrode plates were selected.

[0228] 2. The top and bottom surfaces of the separator were wrapped in paper, and then cut into samples measuring 54.2 mm x 72.5 mm using a knife die and press.

[0229] 3. Stack the cut separator sample and positive or negative electrode plate in an orderly manner, taking care that the separator is on top (when coating one side, the coating faces the positive electrode plate), and place 130mm x 130mm Teflon (registered trademark: Teflon) on the top and bottom. Place the stacked sample in the middle of a 200mm x 200mm piece of cardboard, and cover it with a piece of 150mm x 160mm cardboard.

[0230] 4. The laminated sample was placed in a plate press and the pressure was adjusted. The air pressure was adjusted, and the plate press pressure was 350KG±10KG (the contact area was approximately 54.2mm×72.5mm, and the actual pressure after conversion was approximately 0.87MPa). The temperature was set to 25°C, and the time was set to 15 seconds, and the sample was pressed.

[0231] 5. The hot pressed samples were cut into small pieces of 72.5 mm × 15 mm using a knife die and a press.

[0232] 6. One side of the electrode plate was attached to a steel plate with double-sided tape and a separator was attached to the other side. The separator was then attached to a 15 mm wide piece of A4 paper using double-sided tape to complete the production of the test sample.

[0233] 7. The Gotech tensile machine was turned on and the parameters were set as follows: adhesion test, speed 50mm / min, starting fixture pitch 40mm.

[0234] 8. The test sample was placed between the jigs, the end of the steel plate was fixed to the lower collet, and the A4 paper was fixed to the upper collet. The upper and lower end collets were clamped by the jigs, respectively.

[0235] 9. Click on the computer desktop stretching operation interface, clear the force, displacement, etc., and then click "Start" to perform a pre-stretch of about 5mm. After pre-stretching, clear the force, displacement, etc. again and start the test. During the test, the steel plate that holds the electrode plate is fixed, and the tension machine pulls the A4 paper upward to peel off the separator and electrode plate. After the test is completed, the complete data is exported and saved.

[0236] 10. Each set should measure at least 5 test samples, and if the repeatability of the adhesive strength test curve of the 5 test samples is relatively good, the next set should be tested, otherwise the test should be re-run until the repeatability of the 5 test samples is relatively good.

[0237] 11. After the test was completed, an adhesive strength (N / m)-displacement curve was created, and the average value of the 100th to 300th data points was taken as the adhesive strength, and the measured adhesive strength was taken as F0.

[0238] 12. Steps 1 to 11 were repeated, where in step 4, the pressure was changed to 850 Kg±10 KG (the actual pressure after conversion corresponds to about 2.24 MPa) and the temperature T was changed to 25° C. The obtained adhesive strength was designated as F1.

[0239] 13. Steps 1 to 11 were repeated, where in step 4, the pressure was changed to 850 Kg±10 KG (the actual pressure after conversion corresponds to about 2.24 MPa) and the temperature T was changed to 95° C. The obtained adhesive strength was designated as F2.

[0240] 5. Evaluation of separator resistance performance The test process is as follows:

[0241] (1) Preparation of separator: Cut each separator to be measured into samples of the same size (45.3mm x 33.7mm), bake the samples in an environment of 60°C for at least 4 hours, and then quickly transfer them into a 100-grade cleaning glove box at 25°C as spares. (2) Manufacture of Symmetrical Battery Confinement Pocket Bag (Symmetrical Battery Confinement Aluminum Plastic Bag (Aluminum Plastic Bag is a general-purpose product that combines polypropylene and aluminum foil for pouch cells)): A blank symmetrical battery assembled with Cu Foil vs. Cu Foil (copper foil vs. copper foil) as a current collector was adopted. The confinement of this Pocket bag was realized by green adhesive intermediate punching. The Pocket bag needs to be baked in a 60°C environment for at least 4 hours before use, and then quickly transferred into the 25°C 100-class cleaning glove box described in (1) above for preparation. (3) Assembly of symmetrical batteries: Using the negative electrode plate as an electrode, 5 sets of symmetrical battery samples each having a different number of separator layers (1, 2, 3, 4, 5 layers) were assembled in the original position in the glove box described in (1) above. Each set of samples had 5 parallel samples. The pocket bags were side-sealed using a simple packaging machine, and electrolyte (300 μL) (electrolyte, same composition as battery electrolyte) was injected using a pipette gun, and the bottles were sealed. (4) Attachment of a jig to the assembled symmetric battery: To allow the electrolyte to sufficiently infiltrate the separator, the assembled symmetric battery is placed in the glove box described in (1) above overnight, and the next day, a metal jig is attached and the pressure of the jig is controlled to 0.7 MPa. (5) Electrochemical impedance spectroscopy (EIS) measurement: Before the measurement, the symmetric batteries with different numbers of separator layers were placed in a high and low temperature box and kept at a constant temperature of 25°C for half an hour, and the EIS was measured at the set temperature (25°C). (For low temperatures (e.g., -25°C to 0°C), the constant temperature time can be extended, for example, by about 2 hours.) (6) The French Bio-Logic VMP3 electrochemical working station is used, with voltage <5V, current <400mA, and current accuracy: 0.1%*100μA. During the measurement, the EIS measurement conditions were set as voltage frequency 1MHz-1kHz, disturbance voltage 5MV, and fixture pressure was controlled at 0.7MPa.

[0242] (7) A scattergram was created by plotting the real part of the EIS data against the negative imaginary part, and the EIS diagrams obtained by plotting the data of parallel samples with different and the same number of layers on one graph were compared with the EIS raw data.

[0243] (8) A new EIS diagram was obtained by removing points other than the first quadrant from the EIS diagram obtained in (7) above. The plot in the first quadrant in the new EIS diagram was linearly fitted to obtain a related equation, and when y = 0, the x value was obtained, which is the resistance value of the required separator in the electrolyte. By analogy, the resistance value between parallel samples with different numbers of layers can be obtained by linearly fitting the EIS data obtained by measurement. The parallel samples with five resistance values ​​were designated as R.

[0244] 6. Performance evaluation of secondary batteries Cycle Performance Test: Five secondary batteries were taken out from each set, and the secondary batteries were repeatedly charged and discharged according to the following steps, and the cycle capacity retention rate of the secondary batteries at 25° C. or 45° C. was calculated.

[0245] The first charge and discharge was performed in a 25°C environment, and constant current and constant voltage charging was performed with a charge current of 0.7C (i.e., the current value that completely releases the theoretical capacity within 2 hours) until the upper limit voltage reached 4.4V, and constant current discharging was performed with a discharge current of 0.5C until the final voltage reached 3V, and the discharge capacity of the first cycle was recorded, and then 1000 charge and discharge cycles were performed, and the discharge capacity of the 1000th cycle was recorded. Cycle capacity retention = (discharge capacity of the 1000th cycle / discharge capacity of the first cycle) x 100%.

[0246] The first charge and discharge was performed in a 45°C environment, and constant current and constant voltage charging was performed with a charge current of 0.7C (i.e., the current value that completely releases the theoretical capacity within 2 hours) until the upper limit voltage reached 4.4V, and constant current discharging was performed with a discharge current of 0.5C until the final voltage reached 3V, and the discharge capacity of the first cycle was recorded, and then 1000 charge and discharge cycles were performed, and the discharge capacity of the 1000th cycle was recorded. Cycle capacity retention = (discharge capacity of the 1000th cycle / discharge capacity of the first cycle) x 100%.

[0247] Example 2-3 Except for the difference in the ratio of the first organic particles (Dv90-Dv10) / Dv50 in the separator coating, it is the same as Example 1. Specifically, the ratio of the first organic particles (Dv90-Dv10) / Dv50 of the separator produced in Example 2 is 2.

[0248] The (Dv90-Dv10) / Dv50 of the first organic particles of the separator produced in Example 3 is 2.5.

[0249] Comparative Example 1 The same as Example 1, except that the first organic particles in the separator coating have a (Dv90-Dv10) / Dv50 of 3.5.

[0250] Examples 4-8 Except that the first organic particles used are different and have different vitrification transition temperatures, they are the same as Example 1. Specifically, the vitrification transition temperatures of the first organic particles used in Examples 4-8 are 20°C, 30°C, 40°C, 80°C and 100°C, respectively.

[0251] Comparative Example 2-3 The procedure was the same as in Example 1, except that the first organic particles P5 and P11, which have vitrification transition temperatures of 10° C. and 110° C., respectively, were used.

[0252] Examples 9-13 The areal density of the separator coating, ρ / R, is 0.52 g m -2 Ω-1 , 0.65g m -2 Ω -1 , 0.83g m -2 Ω -1 , 0.96g m -2 Ω -1 and 0.98 g m -2 Ω -1 Other than that, this is the same as in Example 1.

[0253] Comparative Example 4-6 The areal density of the separator coating, ρ / R, is 0.26 g m -2 Ω -1 , 0.29g m -2 Ω -1 and 0.41 g m -2 Ω -1 Other than that, this is the same as in Example 1.

[0254] Examples 14-15 The same as Example 1, except that the first organic particles used were P12 and P13, respectively.

[0255] Example 16 Separator manufacturing 1) A polyethylene microporous membrane (purchased from Shanghai Enji Co., Ltd.) with a thickness of about 9 μm, a hole diameter of about 50 nm, and a porosity of about 38% was used as the separator substrate. 2) 21 kg of the first organic particles P1 is added to 140 kg of deionized water and mixed uniformly to form a first polymer solution; 3) 23.5 kg of an aqueous emulsion of a pressure-sensitive adhesive (whose glass transition temperature is about 10° C., whose volume average particle diameter Dv50 is about 1.1 μm, and which comprises an organic polymer and a plasticizer in a mass ratio of 5:1 (wherein, based on the weight of the plasticizer, about 8 wt % of the plasticizer is grafted onto the organic polymer, where the organic polymer is 30 wt % isobutyl acrylate + 25 wt % isooctyl acrylate + 5 wt % 2-hydroxypropyl methacrylate + 15 wt % styrene + 22 wt % acrylonitrile + 3 wt % polyvinyl alcohol copolymer, and the plasticizer is glycerol) is added to the first polymer solution obtained in step 2) and mixed uniformly to obtain a second polymer solution; 4) adding an appropriate amount of second organic particles (polyvinylidene fluoride, weight average molecular weight 500,000 g / mol) to the second polymer solution obtained in step 3) so that the mass ratio of the first organic particles to the second organic particles is 90:10 based on the dry weight, and uniformly mixing to obtain a third polymer solution, in which the mass ratio of all organic particles (including the first organic particles and the second organic particles having a mass ratio of 90:10 based on the dry weight) to the pressure-sensitive adhesive is 85:15 based on the dry weight; 5) The third polymer solution obtained in step 4) was made into an aqueous coating slurry, which was applied to one surface of a separator substrate by spin spraying, and dried to obtain a separator. The separator thus manufactured includes a separator substrate and a coating applied to one surface of the separator substrate, the coating having a thickness of about 3 μm, and including organic particles (including first organic particles and second organic particles having a mass ratio of 90:10 based on the dry weight) in a mass ratio of 85:15 based on the dry weight, and a pressure-sensitive adhesive, and the pressure-sensitive adhesive includes an organic polymer and a plasticizer (including about 8 wt % of the plasticizer grafted to the organic polymer based on the weight of the plasticizer) in a mass ratio of 5:1. The coating has a surface density of 0.97 g / m 2 As shown in FIG. 6, the coating topography of the separator produced in this example is shown.

[0256] Examples 17-19 The same as in Example 16, except that the mass ratios of the first organic particles to the second organic particles in the coating based on the dry weight were 70:30, 50:50 and 40:60, respectively.

[0257] Comparative Example 7 The same as Example 16, except that the first organic particles were not used.

[0258] The compositions of the first organic particles used in the examples and comparative examples are as shown in Table 1 below.

[0259] The adhesive performance and resistance of the separators prepared in Examples 1-19 and Comparative Examples 1-7 and the cycle performance of the secondary batteries prepared using these separators were evaluated, and the results are shown in Table 2 below.

[0260] [Table 1] JPEG2024535875000002.jpg254157JPEG2024535875000003.jpg254111

[0261] [Table 2] JPEG2024535875000005.jpg249148

[0262] As can be seen from the results of Tables 1 and 2, by combining organic particles with a pressure-sensitive adhesive made from an organic polymer and a plasticizer when manufacturing a separator, the separator can be effectively given high adhesive performance and ion-conducting ability at room temperature. Specifically, the resistance of the separators manufactured at room temperature is 1.89Ω or less. At room temperature and under the action of ≧2MPa, the adhesive strength with the positive electrode is 0.15N / m or more, especially 0.4N / m or more, while the adhesive strength with the electrode is ≦1MPa. Therefore, the manufactured separator can avoid excessive adhesion between layers during the winding and storage process of the separator, and at the same time, when the separator is used to manufacture a battery core, the electrode plate and the separator can be closely attached at room temperature. On the one hand, it can avoid the occurrence of misalignment between the electrode plate and the separator, which leads to the scrapping of the battery core, which affects the battery core performance and creates safety risks, on the other hand, it can omit the tunnel furnace and the second combined process in the traditional battery core production process, further saving production space and production time, reducing energy consumption, obviously improving the production capacity of the battery core production, and at the same time improving the shaping performance, safety performance and dynamic performance of the battery core. In addition, the separator of the present application has a good matching relationship between the adhesive strength F1 and F2 at room temperature and high temperature.

[0263] Examples 20-21 This is the same as Example 16, except that the mass ratio of the organic particles (including the first organic particles and the second organic particles) to the pressure-sensitive adhesive in the coating, and the mass ratio of the first organic particles to the second organic particles based on the dry weight are different. The mass ratio of the organic particles to the pressure-sensitive adhesive in the coating of the separator produced in Example 20 was 85:15 based on the dry weight, and the mass ratio of the first organic particles to the second organic particles in the organic particles was 75:10 based on the dry weight.

[0264] The mass ratio of the organic particles to the pressure-sensitive adhesive in the pressure-sensitive coating of the separator produced in Example 21 was 90:10 based on the dry weight, and the mass ratio of the first organic particles to the second organic particles in the organic particles was 65:25 based on the dry weight.

[0265] The experimental results of Examples 20-21 are shown in Table 3.

[0266] [Table 3]

[0267] As can be seen from Table 3, by adjusting the mass ratio of the first organic particles, the second organic particles, and the pressure-sensitive adhesive, the resistance of the separator can be further reduced and significant deterioration of the cycle performance of the secondary battery can be avoided.

[0268] Examples 22-24 Except for the difference in the graft ratio of the plasticizer in the pressure-sensitive adhesive used, the pressure-sensitive adhesive used in Example 22 was the same as Example 1. Specifically, the graft ratio of the plasticizer in the pressure-sensitive adhesive used in Example 22 was 5 wt%.

[0269] The graft ratio of the plasticizer in the pressure-sensitive adhesive used in Example 23 was 3 wt %.

[0270] The grafting rate of the plasticizer in the pressure-sensitive adhesive used in Example 24 was 0 wt %, that is, the plasticizer was not grafted.

[0271] The experimental results of Examples 22-24 are shown in Table 4.

[0272] [Table 4]

[0273] As can be seen from Table 4, by adjusting the grafting rate of the plasticizer, the resistance of the separator can be further reduced, and the adhesive performance of the separator and the cycle performance of the corresponding battery can be improved.

[0274] Examples 25-29 Except for the different particle size of the first organic particles and the different coating thickness, it is the same as Example 1. Specifically, the Dv50 particle size of the first organic particles used in Example 25 is about 3 μm, and the coating thickness is about 0.8 μm.

[0275] The Dv50 particle size of the first organic particles used in Example 26 is about 5 μm, and the coating thickness is about 2 μm.

[0276] The Dv50 particle size of the first organic particles used in Example 27 is about 20 μm, and the coating thickness is about 15 μm.

[0277] The Dv50 particle size of the first organic particles used in Example 28 is about 30 μm, and the coating thickness is about 20 μm.

[0278] The Dv50 particle size of the first organic particles used in Example 29 is about 36 μm, and the coating thickness is about 22 μm.

[0279] Examples 30-36 Except for the different particle size of the pressure-sensitive adhesive, this is the same as Example 1. Specifically, the Dv50 particle size of the pressure-sensitive adhesive used in Example 30 is about 0.3 μm.

[0280] The pressure sensitive adhesive used in Example 31 has a Dv50 particle size of about 0.5 μm.

[0281] The pressure sensitive adhesive used in Example 32 has a Dv50 particle size of about 0.8 μm.

[0282] The pressure sensitive adhesive used in Example 33 has a Dv50 particle size of about 1.0 μm.

[0283] The pressure sensitive adhesive used in Example 34 has a Dv50 particle size of about 2.0 μm.

[0284] The pressure sensitive adhesive used in Example 35 has a Dv50 particle size of about 3.0 μm.

[0285] The pressure sensitive adhesive used in Example 36 has a Dv50 particle size of about 3.5 μm.

[0286] Examples 37-40 Except for the different particle sizes of the second organic particles used and the different coating thicknesses produced, this is the same as Example 20. Specifically, the Dv50 particle size of the second organic particles used in Example 37 is about 2 μm, and the coating thickness is about 3 μm.

[0287] The Dv50 particle size of the second organic particles used in Example 38 is about 8 μm, and the coating thickness is about 4 μm.

[0288] The Dv50 particle size of the second organic particles used in Example 39 is about 10 μm, and the coating thickness is about 6 μm.

[0289] The Dv50 particle size of the second organic particles used in Example 40 is about 12 μm, and the coating thickness is about 10 μm.

[0290] The experimental results of Examples 25-40 are shown in Table 5.

[0291] [Table 5]

[0292] As can be seen from Table 5, by adjusting the Dv50 particle size of the first organic particles, the pressure-sensitive adhesive and the second organic particles in the coating and the coating thickness, the resistance of the separator can be further reduced, and the adhesive performance of the separator and the cycle performance of the corresponding battery can be improved.

[0293] It should be noted that the present application is not limited to the above-mentioned embodiment. The above-mentioned embodiment is merely an example, and any embodiment having substantially the same configuration as the technical idea and achieving the same effect within the scope of the technical solution of the present application is included in the technical scope of the present application. In addition, various modifications that a person skilled in the art can make to the embodiment and other methods configured by combining some of the components in the embodiment are also included in the scope of the present application, within the scope of the purpose of the present application. [Explanation of symbols]

[0294] The explanation of the symbols is as follows. 1. Battery pack, 2. Upper housing, 3. Lower housing, 4. Battery module, 5. Secondary battery

Claims

1. A separator, A substrate; a coating applied to at least one surface of said substrate; Including, the coating comprises 40-90 wt % first organic particles, 2-15 wt % pressure sensitive adhesive, and optionally 0-50 wt % second organic particles; wherein the first organic particles include an organic polymer and an inorganic substance, and the pressure-sensitive adhesive includes an organic polymer and a plasticizer; Alternatively, the first organic particles have a volume average particle diameter satisfying (Dv90-Dv10) / Dv50≦2.5, optionally ≦2, further optionally ≦1.8, and the first organic particles have a vitrification transition temperature of 20-100° C., optionally 30-80° C.; Optionally, the separator has a density of 0.1 g / m -2 ・Ω -1 ≦ρ / R≦1.0g・m -2 ・Ω -1 , optionally 0.5 g m -2 ・Ω -1 ≦ρ / R≦0.9g・m -2 ・Ω -1 , and more selectively 0.6 g m -2 ・Ω -1 ≦ρ / R≦0.8g・m -2 ・Ω -1 where ρ represents the areal density of the coating on the substrate, and R represents the resistance of the separator at 25° C.

2. The first organic particles are (1) the volume average particle diameter Dv50 of the first organic particles is 3-36 μm, optionally 5-20 μm; (2) the vitrification transition temperature of the first organic particles is 20-100°C, optionally 30-80°C; (3) The weight average molecular weight of the organic polymer in the first organic particles is 500×10 3 g / mol-1000×10 3 g / mol, optionally 800×10 3 g / mol-1000×10 3 g / mol; The separator according to claim 1 , which satisfies one or more of the following conditions.

3. The organic polymer in the first organic particles is at least a first polymerizable monomer having at least one ester bond and selectively one or more of methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, vinyl acetate, trifluoroethyl methacrylate, glycidyl methacrylate, or trimethylolpropane triacrylate, and further selectively one or more of methyl methacrylate, lauryl acrylate, lauryl methacrylate, or trimethylolpropane triacrylate; a second polymerizable monomer having at least one cyano bond and optionally one or more of acrylonitrile, methacrylonitrile, ethacrylonitrile, and further optionally one or more of acrylonitrile, methacrylonitrile; A monomer having at least one amide bond, which is optionally one or more of acrylamide, N-methylolacrylamide, and N-butoxymethacrylamide, and further optionally one or more of acrylamide and N-methylolacrylamide, is polymerized with a third polymerizable monomer, Optionally, the weight ratio of the first polymerizable monomer to the second polymerizable monomer to the third polymerizable monomer is 1:0-0.8:0.05-0.75, and optionally 1:0.1-0.6:0.1-0.

6. The separator according to any one of claims 1 to 2.

4. The content of the organic polymer in the first organic particles is 50-99.9%, alternatively 60-99%, and further alternatively 70-99%, based on the total dry weight of the first organic particles; The separator according to any one of claims 1 to 3, wherein the content of the inorganic matter in the first organic particles is 0.1-50%, alternatively 1-40%, and further alternatively 1-30%, based on the total dry weight of the first organic particles.

5. The separator according to any one of claims 1 to 4, wherein the weight ratio of organic polymer to inorganic matter in the first organic particles is 99:1-1:1, optionally 70:30-1:

1.

6. Based on the total weight of the organic polymer in the first organic particles, The content of the first polymerizable monomer is 35-80% by weight, optionally 45-70% by weight; The content of the second polymerizable monomer is 0-30% by weight, optionally 5-25% by weight; and The separator according to any one of claims 1 to 5, wherein the content of the third polymerizable monomer is 5-40% by weight, and optionally 8-35% by weight.

7. 7. The separator according to claim 1, wherein the inorganic matter in the first organic particles is selected from one or more of oxides of silicon, aluminum, calcium, zinc, magnesium, sodium sulfate, sodium benzoate, calcium carbonate, and modified materials thereof, and is optionally one or more of silicon dioxide, silica sol, aluminum oxide, zinc oxide, magnesium oxide, and sodium benzoate, and further optionally one or more of fumed silicon dioxide, silicon fine powder, aluminum oxide, and sodium benzoate.

8. 8. The separator according to claim 1, wherein the surfaces of the first organic particles are uneven, and inorganic oxide clusters having a particle size of 10 to 200 nm are uniformly distributed thereon.

9. The separator according to any one of claims 1 to 8, wherein the mass ratio of the organic polymer to the plasticizer contained in the pressure-sensitive adhesive is (4-25):1, and optionally (4-11):

1.

10. 10. The separator of claim 1, wherein the pressure sensitive adhesive has a core-shell structure, and the core and the housing of the core-shell structure both comprise an organic polymer and a plasticizer, and wherein the weight ratio of the organic polymer to the plasticizer in the core is (3-4):1, optionally (3.2-3.8):1, and the weight ratio of the organic polymer to the plasticizer in the housing structure is (7-9):1, optionally (7.5-8.5):

1.

11. In the pressure sensitive adhesive, a portion of the plasticizer is grafted to the organic polymer; Optionally, in the pressure sensitive adhesive, at least 5 wt % of the plasticizer, based on the weight of the plasticizer, is grafted to the organic polymer.

12. The separator of any one of claims 1 to 11, wherein the pressure sensitive adhesive has a volume average particle diameter Dv50 of 0.3-3.5 μm, optionally 0.8-2.0 μm, and optionally a glass transition temperature of the pressure sensitive adhesive of -50°C-100°C, optionally -45°C-60°C.

13. In the pressure sensitive adhesive, the organic polymer comprises a copolymer obtained by copolymerizing a mixture of at least one of the following first monomer group, at least one of the following second monomer group, at least one of the following third monomer group, and at least one of the following reactive dispersants, namely: the first monomer group includes acrylic acid, methacrylic acid, methyl methacrylate, tert-butyl methacrylate, isobornyl methacrylate, methylol acrylamide, acrylamide, styrene, and acrylonitrile; The second monomer group is acrylic acid C 4 -C 22 Alkyl esters, such as isobutyl acrylate, isooctyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, ethyl methacrylate, isobutyl methacrylate, 2-ethylhexyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, and benzyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, ethylene urea ethyl methacrylate, dicyclopentenyloxyethyl methacrylate, tetrahydrofuryl methacrylate, trifluoroethyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, acrylic methacrylate, and dicyclopentenyloxyethyl methacrylate; The third monomer group includes 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, glycidyl acrylate, glycidyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, γ-methacryloxypropyltrimethoxysilane, N-methylol acrylamide, N-butoxymethacrylamide, diacetone acrylamide (DAAM), ethyl acetoacetate methacrylate (AAEM), divinylbenzene, an epoxy resin having an epoxy value of 0.35-0.50, and divinylbenzene; and The separator according to claim 1 , wherein the reactive dispersant comprises polyvinyl alcohol, polypropylene alcohol, polypropylene glycol, polyethylene glycol, or polyvinyl alcohol.

14. The plasticizer is glycerol C 4 -C 10 Alkyl diether or monoether, glycerol C 4 -C 10 Carboxylic acid monoester or diester, propylene glycol C 4 -C 10 14. The separator of any one of claims 1 to 13, selected from one or more of an alkyl monoether or glycerol.

15. The separator of any one of claims 1 to 14, wherein the average thickness of the coating is 0.8-22 μm, optionally 2-15 μm.

16. the second organic particles are polymers of one or more monomers containing halogen, phenyl, epoxy, cyano, ester and amide groups; Optionally, the second organic particles are selected from at least one of homopolymers or copolymers of fluorine-containing alkenyl monomer units, homopolymers or copolymers of olefin-based monomer units, homopolymers or copolymers of unsaturated nitrile-based monomer units, homopolymers or copolymers of alkylene oxide-based monomer units, dipolymers, homopolymers or copolymers of monosaccharide monomer units, and modified compounds of each of the homopolymers or copolymers; More preferably, the second organic particles are selected from at least one of polyperfluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polystyrene-co-methyl methacrylate, polystyrene-co-butyl acrylate, styrene-butyl acrylate-isooctyl acrylate, polymethyl methacrylate, polyacrylonitrile, polyvinyl acetate, polyethylene-co-vinyl acetate, polyimide, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, and cyanoethyl sucrose; 16. The separator according to claim 1, further comprising at least one of polyvinylidene fluoride-co-hexafluoropropylene, polystyrene-co-butyl acrylate, styrene-butyl acrylate-isooctyl acrylate, polyperfluoroethylene, polyvinylidene fluoride, and polyvinylidene fluoride-co-trichloroethylene.

17. The second organic particles are (1) the volume average particle diameter Dv50 of the second organic particles is 2-20 μm, and optionally 6-15 μm; (2) the melting point of the second organic particles is 130-160°C, optionally 138-150°C; (3) The weight average molecular weight of the second organic particles is 400×10 3 g / mol-1000×10 3 g / mol, and optionally 450×10 3 g / mol-650×10 3 g / mol; The separator according to claim 1 , which satisfies one or more of the following conditions:

18. The separator is (1) the porosity of the substrate is 10-95%; (2) the hole diameter of the substrate is 20-60 nm; (3) the thickness of the substrate is 3-12 μm, optionally 5-9 μm; (4) The substrate is a film or nonwoven fabric selected from one or more of polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyether ether ketone, polyaryl ether ketone, polyether imide, polyamide imide, polybenzimidazole, polyether sulfone, polyphenylene ether, cycloolefin copolymer, polyphenylene sulfide, and polyethylene naphthalene; The separator according to claim 1 , which satisfies one or more of the following conditions:

19. In the separator, The mass ratio of the first organic particles to the second organic particles is 10-100:0-90, optionally 20-90:0-60; Optionally, the ratio of the sum of the mass of the first organic particles and the second organic particles to the mass of the pressure-sensitive adhesive is 20-92:8-20, optionally 60-90:10-15. The separator of any one of claims 1 to 18.

20. A method for producing the separator according to any one of claims 1 to 19, comprising the steps of: Step S1: adding first organic particles and a dispersant to a solvent to form a first polymer solution; Step S2 of adding a pressure sensitive adhesive to the first polymer solution obtained in step S1 and thoroughly mixing to form a second polymer solution; Optionally, step S3 of adding second organic particles to the second polymer solution obtained in step S2 and thoroughly mixing to form a third polymer solution; Step S4) of applying the second polymer solution obtained in step S2 or the third polymer solution obtained in step S3 to at least one surface of a substrate and drying the substrate to obtain a separator; Including, The separator includes a substrate and a coating applied to at least one surface of the substrate; the coating comprises 40-90 wt % first organic particles, 2-15 wt % pressure sensitive adhesive, and optionally 0-50 wt % second organic particles; The first organic particles include an organic polymer and an inorganic material, the pressure sensitive adhesive includes an organic polymer and a plasticizer, and optionally the first organic particles have a volume average particle size satisfying (Dv90-Dv10) / Dv50≦2.5, optionally ≦2, further optionally ≦1.8, and the first organic particles have a vitrification transition temperature of 20-100° C., optionally 30-80° C., and optionally the separator has a mass of 0.1 g m -2 ・Ω -1 ≦ρ / R≦1.0g・m -2 ・Ω -1 , optionally 0.5 g m -2 ・Ω -1 ≦ρ / R≦0.9g・m -2 ・Ω -1 , and more selectively 0.6 g m -2 ・Ω -1 ≦ρ / R≦0.8g・m -2 ・Ω -1 where ρ represents an areal density of the coating on the substrate, and R represents a resistance of the separator at 25° C.

21. 21. A secondary battery comprising: a positive electrode plate; a negative electrode plate; a separator located between the positive electrode plate and the negative electrode plate; and an electrolyte, wherein the separator is the separator according to any one of claims 1 to 19 or a separator produced by the method according to claim 20.

22. The adhesive strength between the positive electrode plate and the separator of the secondary battery satisfies 1.2≦F2 / F1≦4, and optionally 1.5≦F2 / F1≦3.8; 22. The secondary battery of claim 21, wherein F1 represents the adhesive strength between the positive electrode plate and the separator at 25° C. and ≧2 MPa, and F2 represents the adhesive strength between the positive electrode plate and the separator at 95° C. and ≧2 MPa.

23. A battery module comprising the secondary battery according to claim 21 or 22.

24. A battery pack comprising at least one of the secondary battery according to claim 21 or 22 or the battery module according to claim 23.

25. A power consuming device comprising at least one of the secondary battery according to claim 21 or 22, the battery module according to claim 23, or the battery pack according to claim 24.

Citation Information

Patent Citations

  • Porous film

    JP2016031832A

  • Slurry for porous membrane of lithium ion secondary battery and manufacturing method thereof, separator for lithium ion secondary battery, and lithium ion secondary battery

    JP2019140114A

  • Separator for lithium secondary battery, and lithium secondary battery comprising same

    US20220102810A1

  • Slurry for porous membranes of secondary battery separators, porous membrane for secondary battery separators, method for producing porous membrane for secondary battery separators, separator for secondary batteries, and secondary battery

    WO2014136799A1