Positive electrode active material, battery, and manufacturing method thereof

The positive electrode active material with controlled morphology and pore structure addresses low-temperature output and energy density issues in lithium-ion batteries, improving performance and stability through optimized manufacturing processes.

JP2024535975AActive Publication Date: 2024-10-04SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD

Patent Information

Application Number
JP2023579467
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-08-23
Filing Date
2022-12-27
Publication Date
2024-10-04
Estimated Expiration
2042-12-27

AI Technical Summary

Technical Problem

Current lithium-ion batteries face issues with insufficient low-temperature output and decreased volumetric energy density, particularly in electric vehicle batteries, due to the use of expensive raw materials and harsh environmental conditions.

Method used

A positive electrode active material with controlled particle morphology, particle size distribution, tap density, and pore structure, optimized through a manufacturing process involving specific sintering and coating, to enhance ion and electron transport and reduce gas generation.

Benefits of technology

The solution improves low-temperature output performance and volumetric energy density while maintaining long-term stability and reducing gas production, enhancing the overall battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024535975000001_ABST
    Figure 2024535975000001_ABST
Patent Text Reader

Abstract

The present application discloses a positive electrode active material, a battery, and a method for manufacturing the same. The positive electrode active material includes porous secondary particles, and the positive electrode active material satisfies the following characteristic: 4≦BET×TD×(Dv90−Dv10)≦14, where BET represents the value of the specific surface area of ​​the positive electrode active material, and is expressed in units of m 2 / g, and TD represents the tap density of the positive electrode active material, expressed in g / cm 3 where Dv90 is the particle diameter value corresponding to the cumulative volume distribution percentage of the positive electrode active material reaching 90%, and the unit is μm, and Dv10 is the particle diameter value corresponding to the cumulative volume distribution percentage of the positive electrode active material reaching 10%, and the unit is μm. The present application realizes improvement of low-temperature output performance by controlling the particle morphology, size and pore structure of the positive electrode active material, and obtains the effect of increasing the volumetric energy density of the battery by rationally controlling the particle morphology, particle size distribution and tap density of the positive electrode active material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the field of new energy technology, and in particular to a positive electrode active material, a battery, and a method for manufacturing the same.

[0002] This application claims priority based on a Chinese patent application filed with the China Patent Office on August 23, 2022, bearing application number 202211010331.4 and entitled "Positive electrode active material, battery, and manufacturing method thereof," the entire contents of which are incorporated herein by reference. [Background technology]

[0003] Batteries such as lithium-ion batteries are widely used in various fields due to their advantages such as high specific energy, good output performance, low self-discharge, and long cycle life. Currently, the positive electrode active materials used in electric vehicle batteries are mainly ternary positive electrode active materials, but their raw materials (such as cobalt sulfate and lithium salt) are expensive. In order to further reduce the cost of electric vehicles, the volumetric energy density of lithium-ion batteries can be increased to reduce the space ratio of the battery module inside the vehicle, which has a positive impact on the weight and cost reduction of new energy vehicles. In addition, the usage environment of electric vehicle batteries is becoming increasingly severe, and cold climates in particular have a serious impact on battery performance, so it is necessary to improve the low-temperature performance of batteries, especially their output performance at low temperatures. Summary of the Invention [Problem to be solved by the invention]

[0004] The present application provides a positive electrode active material, a battery, and a manufacturing method thereof that solve the problems of insufficient low-temperature output and reduced volumetric energy density of batteries manufactured using current positive electrode active materials. [Means for solving the problem]

[0005] According to the positive electrode active material provided in the first aspect of the present application, the positive electrode active material includes secondary particles, the secondary particles have pores, and the positive electrode active material satisfies the following characteristic: 4≦BET×TD×(Dv90−Dv10)≦14, where BET represents the value of the specific surface area of ​​the positive electrode active material, and the unit is m 2 / g, and TD represents the tap density of the positive electrode active material, expressed in g / cm 3 where Dv90 represents the corresponding particle diameter value when the cumulative volume distribution percentage of the positive electrode active material reaches 90%, and the unit is μm, and Dv10 represents the corresponding particle diameter value when the cumulative volume distribution percentage of the positive electrode active material reaches 10%, and the unit is μm.

[0006] Optionally, in other embodiments of the present application, 0.4≦BET≦3.5, 1.2≦TD≦2.6, 4≦Dv90≦18, and 1.5≦Dv10≦6.

[0007] Optionally, in another embodiment of the present application, the maximum pore size of the positive electrode active material is D max nm, 800≦D max <=2200.

[0008] Optionally, in another embodiment of the present application, the half-width of the pore size distribution of the positive electrode active material is D HW nm, 150≦D HW Meet ≦450.

[0009] Optionally, in another embodiment of the present application, the porosity P of the positive electrode active material c 45%≦P c Meet ≦75%.

[0010] Optionally, in another embodiment of the present application, the powder compaction density of the positive electrode active material is P d g / cm 3 and 2.8≦P d <= 3.4.

[0011] Optionally, in other embodiments of the present application, the positive electrode active material has the formula Li x Ni y Co z Me k M pO2, wherein Me is selected from at least one of Mn or Al, and M comprises at least one of Y, Nb, In, La, Zr, Ce, W, Al, Ti, Sr, Mg, Sb, V, Zn, Cu, Cr, or Fe, and 0.8≦x≦1.1, 0.5 <y<1、0<z<1、0<k<1、0≦p≦0.1である。

[0012] Optionally, in another embodiment of the present application, the positive electrode active material includes a lithium nickel cobalt manganese oxide, which contains elemental nickel, elemental cobalt, and elemental manganese, and when the sum of the molar amounts of the elemental nickel, elemental cobalt, and elemental manganese is 1, the content of the elemental nickel is more than 0.3.

[0013] A method for producing a positive electrode active material provided in a second aspect of the present application includes: mixing either a manganese source or an aluminum source with a nickel source and a cobalt source, adding a precipitating agent and a complexing agent, and reacting to obtain a ternary material precursor; Mixing a ternary material precursor, an M element source and a lithium source, performing primary sintering, and then cooling and grinding to obtain a material containing an M element; and mixing the material containing the M element with a coating element source, and performing secondary sintering to obtain a positive electrode active material.

[0014] Optionally, in other embodiments of the present application, the positive electrode active material has the formula Li x Ni y Co z Me k M p O2, where Me is selected from at least one of Mn or Al, and M includes at least one of Y, Nb, In, La, Zr, Ce, W, Al, Ti, Sr, Mg, Sb, V, Zn, Cu, Cr, or Fe, and 0.8≦x≦1.1, 0 <y<1、0<z<1、0<k<1、0≦p≦0.1である。

[0015] Optionally, in other embodiments herein, the nickel source includes at least one of nickel sulfate, nickel acetate, or nickel nitrate.

[0016] Optionally, in other embodiments herein, the cobalt source includes at least one of cobalt sulfate, cobalt acetate, or cobalt nitrate.

[0017] Optionally, in other embodiments herein, the manganese source includes at least one of manganese sulfate, manganese acetate, or manganese nitrate.

[0018] Optionally, in other embodiments herein, the aluminum source comprises at least one of aluminum sulfate, aluminum acetate, or aluminum nitrate.

[0019] Optionally, in other embodiments herein, the M element source comprises at least one of zirconium nitrate, tungsten nitrate, aluminum nitrate, titanium nitrate, strontium nitrate, magnesium nitrate, yttrium nitrate, cerium nitrate, indium nitrate, niobium nitrate, lanthanum nitrate, antimony nitrate, vanadium nitrate, zinc nitrate, copper nitrate, chromium nitrate, iron nitrate, tungsten oxide, or zirconium oxide.

[0020] Optionally, in other embodiments herein, the lithium source includes at least one of lithium hydroxide, lithium carbonate, lithium acetate, or lithium nitrate.

[0021] Optionally, in other embodiments herein, the coating element source comprises one or more of aluminum nitrate, titanium nitrate, cobalt nitrate, tungsten nitrate, yttrium nitrate, silicon oxide, boron oxide, phosphorus pentoxide, or aluminum oxide.

[0022] Optionally, in another embodiment of the present application, the mass percentage of the coating element source in the material containing the M element is 0.3wt% to 0.7wt%.

[0023] Optionally, in another embodiment of the present application, the precipitating agent includes sodium hydroxide solution and the complexing agent includes aqueous ammonia.

[0024] Optionally, in another embodiment of the present application, the primary sintering temperature is 600-1000° C., and the primary sintering time is 3-16 hours.

[0025] Optionally, in another embodiment of the present application, the secondary sintering temperature is 400-700° C., and the secondary sintering time is 1-9 hours.

[0026] A battery provided in a third aspect of the present application includes a positive electrode piece including a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, the positive electrode active material layer including the positive electrode active material described above or a positive electrode active material produced by the production method described above.

[0027] Optionally, in another embodiment of the present application, the positive electrode active material layer is (i) The actual active area of ​​the positive electrode active material layer is A cm 2 4 × 10 4 ≦A≦2×10 5 and (ii) Compressed density PD g / cm of the positive electrode active material layer 3 satisfies 2.4≦PD≦3.5, (iii) Porosity P of the positive electrode active material layer s 20%≦P s ≦40% and (iv) When the temperature is −20° C. and the state of charge of the battery is 30%, the discharge power per unit volume of the positive electrode active material layer is PW / cm 3 , 8≦P≦30, P=P0×PD / m, P0W represents the discharge power of the battery under the above conditions, and PD g / cm 3 represents the compressed density of the positive electrode active material layer, and mg represents the weight of the positive electrode active material layer.

[0028] Alternatively, A and P0 satisfy 0.6≦1000P0 / A≦1.

[0029] A fourth aspect of the present application provides an electric device comprising the battery described above. Effect of the Invention

[0030] The positive electrode active material according to the embodiments of the present application has at least the following technical effects.

[0031] 1) By rationally controlling the particle morphology, particle size distribution and tap density of the positive electrode active material, the powder compression density can be effectively increased, thereby improving the compression ability of the pole pieces, and achieving the effect of increasing the battery volumetric energy density without reducing the performance of output, cycle, storage, gas generation, etc.

[0032] 2) By controlling the particle morphology, particle size and pore structure of the positive electrode active material, the specific surface area and porosity of the material are controlled, the effective contact area between the positive electrode active material and the electrolyte is increased, and the ion transport, electron transport and diffusion rate of the electrolyte are optimized, thereby improving the output performance of the battery, especially at low temperatures.

[0033] In order to more clearly describe the technical solutions in the embodiments of the present application, the drawings that need to be used in the description of the embodiments are briefly introduced below. It is obvious that the drawings in the following description are only some embodiments of the present invention, and those skilled in the art can also obtain other drawings based on these drawings without creative efforts. [Brief description of the drawings]

[0034] [Figure 1] 1 is an electron microscope characteristic evaluation test image of the surface morphology of the positive electrode active material obtained in Example 2 of the present application. [Diagram 2] 1 is an electron microscope characteristic evaluation test image of a cross-sectional morphology of a positive electrode active material obtained in Example 2 of the present application. [Diagram 3] 1 is a flowchart of a method for producing a positive electrode active material provided in an embodiment of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] The technical solutions in the embodiments of the present application are clearly and completely described below with reference to the accompanying drawings of the embodiments of the present application, but obviously, the described embodiments are only some, not all, of the embodiments of the present application. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative efforts are included in the scope of protection of the present application.

[0036] In this specification, a numerical range indicated using "~" means a range that includes the numerical values ​​before and after "~" as the lower limit and upper limit, respectively.

[0037] The present application provides a cathode active material, a battery, and a method for manufacturing the same, each of which will be described in detail below. Note that the order of the following description of the examples is not intended to limit the preferred order of the examples.

[0038] A first aspect of the present application provides a positive electrode active material, the positive electrode active material including secondary particles, the secondary particles having pores, and an I value of the positive electrode active material satisfying the following characteristics: 4≦I=BET×TD×(Dv90−Dv10)≦14, where BET represents a value of a specific surface area of ​​the positive electrode active material, and the unit is m 2 / g, and TD represents the tap density of the positive electrode active material, expressed in g / cm 3 where Dv90 is the particle diameter value corresponding to the cumulative volume distribution percentage of the positive active material reaching 90%, in μm, and Dv10 is the particle diameter value corresponding to the cumulative volume distribution percentage of the positive active material reaching 10%, in μm. Since low-temperature discharge power performance is mainly affected by the positive electrode piece of the battery, the present application controls the particle morphology, particle size, particle size distribution, tap density and pore structure of the positive active material to improve the low-temperature output performance and volumetric energy density of the battery manufactured using this positive active material.

[0039] In some embodiments of the present application, I is 4.5≦I≦11.7. For example, I may be 4.5, 4.8, 5.1, 5.6, 6.1, 6.3, 6.9, 7.3, 7.8, 8.1, 8.6, 9.3, 9.7, 10.5, 11.7, or a range consisting of any two of these values. In some embodiments of the present application, I is 5.1≦I≦9.7. In some embodiments of the present application, I is 5.6≦I≦8.6. When the value of I is within this range, the particle morphology, particle size, particle size distribution, tap density, and pore structure of the positive electrode active material are all in good condition, the low-temperature power performance of the battery is further improved, and the volumetric energy density of the battery is further increased.

[0040] At present, from the viewpoint of materials and battery design, the methods for improving the energy density of lithium-ion batteries mainly include increasing the content of nickel element in the ternary material, increasing the upper voltage limit, and improving the compression ability of the pole pieces, etc. The first two solutions can improve the gram capacity of the material, but they will lead to various degrees of deterioration in battery performance, such as reduced thermal stability, increased side reactions with the electrolyte, and increased gas generation; the solution of increasing the compression density of the pole pieces can increase the volumetric energy density of the battery, but it has problems such as particles being easily broken, many interfacial side reactions occurring, large amounts of gas generation, and short long-term life. Therefore, in this application, the particle morphology, particle size, particle size distribution, tap density, and pore structure of the positive electrode active material are controlled to improve the energy density of the battery and improve the low-temperature output performance, while ensuring the reduction of gas generation and the improvement of long-term performance.

[0041] In some embodiments of the present application, 0.4≦BET≦3.5. For example, it may be 0.4, 0.8, 1.1, 1.2, 1.4, 1.8, 2.0, 2.3, 2.8, 3.0, 3.5, or a range consisting of any two values ​​thereof. In some embodiments of the present application, 0.4≦BET≦2.7. By controlling the BET of the positive electrode active material within this range, the effective contact area between the positive electrode active material and the electrolyte can be better controlled, side reactions between the positive electrode active material and the electrolyte can be controlled, and the output performance of the battery can be improved. The BET value can be tested using a specific surface area analyzer (model: Tristar II3020).

[0042] In some embodiments of the present application, 1.2≦TD≦2.6. For example, 1.2, 1.3, 1.4, 1.5, 1.8, 2.1, 2.2, 2.6, or a range consisting of any two values ​​thereof. In some embodiments of the present application, 1.3≦TD≦2.2. In some embodiments of the present application, 1.5≦TD≦2.1. By rationally controlling the tap density of the positive electrode active material, the powder compression density can be effectively increased, thereby improving the compression ability of the positive electrode pieces, and increasing the battery volumetric energy density. For the tap density test, reference can be made to GB / T5162-2021 Measurement of the Tap Density of Metal Powder.

[0043] In some embodiments of the present application, 4≦Dv90≦18, for example, 4.7, 4.8, 4.9, 5.0, 5.2, 5.4, 5.5, 5.8, 10, 15, or a range consisting of any two values ​​thereof. In some embodiments of the present application, 4.9≦Dv90≦15. In some embodiments of the present application, 5.0≦Dv90≦10. 1.5≦Dv10≦6, for example, 1.5, 1.8, 2.1, 2.2, 2.4, 2.5, 2.6, 2.7, 2.8, 5, or a range consisting of any two values ​​thereof. In some embodiments of the present application, 1.5≦Dv10≦5. In some embodiments of the present application, 1.8≦Dv10≦2.8. By controlling the appropriate particle size distribution, the problem of particle breakage during rolling can be reduced and the occurrence of interface side reactions can be reduced. Dv90, Dv50 and Dv10 are tested using a Malvern Laser Particle Sizer.

[0044] In some embodiments of the present application, 2≦Dv50≦8, and Dv50 represents the corresponding particle size value when the cumulative volume distribution percentage of the positive electrode active material reaches 50%, and is expressed in μm.

[0045] In some embodiments of the present application, the maximum pore diameter D of the positive electrode active material max nm is 800≦D max≦2200, and may be, for example, 850, 1100, 1200, 1400, 1500, 1700, 1800, 1900, 2000, or a range consisting of any two values ​​thereof. max In some embodiments of the present application, 1100≦D max ≦1900. When the value of I is within the above range and the maximum pore size of the positive electrode active material satisfies the above condition, the pore structure, particle morphology, particle size, particle size distribution, and tap density of the positive electrode active material are controlled within more appropriate ranges, and the battery has high energy density and excellent low-temperature output performance.

[0046] In some embodiments of the present application, the half-width D HW nm is 150≦D HW ≦450, and may be, for example, 160, 200, 300, 400, 450, or a range consisting of any two values ​​thereof. In some embodiments of the present application, 160≦D HW ≦380. In some embodiments of the present application, 160≦D HW <=300.

[0047] In some embodiments of the present application, the porosity P c 45%≦P c ≦75%, for example, 46%, 53%, 54%, 56%, 58%, 62%, 63%, 65%, 66%, 67%, 72%, or a range consisting of any two values ​​thereof. c In some embodiments of the present application, 56%≦P c ≦67%. Positive electrode active material porosity P c When the contact area between the positive electrode active material and the electrolyte is within the above range, the contact area between the positive electrode active material and the electrolyte can be controlled to a more optimal range, resulting in better performance of the entire battery.

[0048] In some embodiments of the present application, the powder compaction density P d g / cm 3 , 2.8≦P d≦3.4, and may be, for example, 2.9, 3.0, 3.1, 3.2, 3.3, or a range consisting of any two values ​​thereof. d ≦3.3.

[0049] Here, the pore size distribution and porosity of the positive electrode active material are measured by mercury intrusion porosimetry. d is tested by compression density meter, and the test process can refer to the national standard GB / T 24533-2019. In this application, by controlling the particle morphology, particle size and pore structure of the material, the specific surface area and porosity of the material are controlled, the effective contact area between the positive electrode active material and the electrolyte is increased, the ion transport, electron transport and diffusion speed of the electrolyte are optimized, and the output performance of the battery, especially the output performance at low temperature, is improved; by controlling the appropriate particle size distribution and compression strength of the positive electrode active material, the problem of particle breakage during rolling can be effectively alleviated, the interfacial side reaction of the battery can be improved, gas generation can be reduced and the long-term service life can be improved.

[0050] In some embodiments of the present application, the positive electrode active material includes nickel element, cobalt element, and Me element, and when the molar amounts of nickel element, cobalt element, and Me element are taken as 1, the content of nickel element is 0.3 or more, and Me is selected from at least one of Mn and Al.

[0051] In some embodiments of the present application, the positive electrode active material includes nickel, cobalt, and Me elements, and when the molar amounts of nickel, cobalt, and Me are taken as 1, the content of nickel element is 0.5 or more, and Me is selected from at least one of Mn and Al.

[0052] In some embodiments of the present application, the positive electrode active material includes nickel, cobalt and Me, and when the molar amounts of nickel, cobalt and Me are 1, the content of nickel is 0.7 or less, where Me is selected from at least one of Mn and Al. When the porous positive electrode active material satisfies 4≦BET×TD×(Dv90−Dv10)≦14, the content of nickel is controlled within the above range, which further improves the stability of the positive electrode active material structure, improves the ion transport and electron transport of the battery, and more effectively alleviates problems such as reduced thermal stability, intensified side reactions with the electrolyte, and increased gas generation, thereby improving the overall performance of the battery.

[0053] In some embodiments of the present application, the positive electrode active material includes an M element, and the M element includes at least one of Y, Nb, In, La, Zr, Ce, W, Al, Ti, Sr, Mg, Sb, V, Zn, Cu, Cr, or Fe.

[0054] In some embodiments of the present application, the positive electrode active material includes an M element, and the M element includes at least one of Y, Nb, In, La, Zr, or Ce, and at least one of W, Al, Ti, Sr, Mg, Sb, V, Zn, Cu, Cr, or Fe.

[0055] In some embodiments of the present application, the positive electrode active material includes an M element, and the M element includes W and at least one of Y, Nb, In, La, Zr, Ce, Al, Ti, Sr, Mg, Sb, V, Zn, Cu, Cr, or Fe.

[0056] Furthermore, the lithium nickel cobalt manganese oxide contains nickel element, cobalt element and manganese element, and when the sum of the molar amounts of nickel element, cobalt element and manganese element is taken as 1, the content of nickel element is more than 0.3.

[0057] In addition, the positive electrode active material has the chemical formula Li x Ni y Co z Me k M pand wherein Me is selected from at least one of Mn or Al, and M comprises at least one of Y, Nb, In, La, Zr, Ce, W, Al, Ti, Sr, Mg, Sb, V, Zn, Cu, Cr, or Fe, and 0.8≦x≦1.1, 0 <y<1、0<z<1、0<k<1、0≦p≦0.1である。

[0058] In some embodiments of the present application, the surface of the positive electrode active material particles further includes a coating material containing at least one coating element selected from Al, Ti, Co, W, Y, Si, B, P, and F. The coating material covers the surface of the positive electrode active material. Specifically, the coating material is coated on the surface of the positive electrode active material by dry coating (high-temperature solid-phase method), and the surface of the positive electrode active material is partially or completely covered with a coating layer formed by the coating material, for example, the contact area between the coating layer and the positive electrode active material occupies 50%, 60%, 70%, 80%, 90%, or 100% of the surface area of ​​the positive electrode active material. The coating material is added to the surface of the positive electrode active material to improve the structural stability and rate performance of the positive electrode active material.

[0059] In some embodiments of the present application, the positive electrode active material particles have a surface region and a central region adjacent to the surface region, the surface region includes at least one of Al, Ti, Co, W, Y, Si, B, P or F, and the central region includes an M element, the M element including Zr and W. While the porous positive electrode active material satisfies 4≦I=BET×TD×(Dv90-Dv10)≦14, the central region of the positive electrode active material includes an M element, and the surface of the positive electrode active material includes a coating element, so that the particle morphology and particle size of the positive electrode active material can be improved when used in a positive electrode piece, so that the positive electrode active material can be better distributed in the positive electrode piece; at the same time, the composition of the M element and the coating element can be adjusted and a better M element and coating element can be selected to improve the structure of the positive electrode active material and improve the overall performance of the battery.

[0060] Correspondingly, a second aspect of the present application provides a method for producing a positive electrode active material, as shown in FIG. 3, comprising the following steps: S1: Either a manganese source or an aluminum source is mixed with a nickel source and a cobalt source, a precipitating agent and a complexing agent are added, and reacted to obtain a ternary material precursor. S2: The ternary material precursor, the M element source and the lithium source are mixed, and then primary sintering is performed. After cooling and pulverization, a material containing the M element is obtained. S3: A material containing an M element and a coating element source are mixed and then secondary sintering is carried out to obtain a positive electrode active material.

[0061] In the present invention, the crystal nucleation rate and growth rate are optimized by changing process parameters such as pH value, complexing agent concentration and synthesis atmosphere during the precursor manufacturing process. The sintering temperature, sintering time and crushing strength are also controlled in the present invention. Since the control of the pore structure is very sensitive to the above parameters, the above process parameters need to be precisely controlled in multiple stages.

[0062] In addition, the positive electrode active material has the chemical formula Li x Ni y Co z Me k M p O2, wherein Me is selected from at least one of Mn or Al, and M comprises at least one of Y, Nb, In, La, Zr, Ce, W, Al, Ti, Sr, Mg, Sb, V, Zn, Cu, Cr, or Fe, and 0.8≦x≦1.1, 0 <y<1、0<z<1、0<k<1、0≦p≦0.1である。

[0063] In some embodiments of the present application, the nickel source comprises at least one of nickel sulfate, nickel acetate, or nickel nitrate, the cobalt source comprises at least one of cobalt sulfate, cobalt acetate, or cobalt nitrate, the manganese source comprises at least one of manganese sulfate, manganese acetate, or manganese nitrate, the aluminum source comprises at least one of aluminum sulfate, aluminum acetate, or aluminum nitrate, and the M element source comprises zirconium nitrate, tungsten nitrate, aluminum nitrate, titanium nitrate, strontium nitrate, magnesium nitrate. the lithium source comprises at least one of lithium hydroxide, lithium carbonate, lithium acetate, or lithium nitrate; and the coating element source comprises at least one of aluminum nitrate, titanium nitrate, cobalt nitrate, tungsten nitrate, yttrium nitrate, silicon oxide, boron oxide, phosphorus pentoxide, or aluminum oxide.

[0064] In some embodiments of the present application, the precipitating agent includes sodium hydroxide solution and the complexing agent includes aqueous ammonia.

[0065] Furthermore, the ternary precursor, the M element source and the lithium source are mixed and sintered, the sintering temperature may be 600-1000°C, 700-900°C, or 800-880°C, the temperature is increased to this temperature at a rate of 5-50°C / min, and the sintering time may be 3-16 hours, 5-15 hours, or 8-10 hours.

[0066] Furthermore, the material containing the M element and the coating element source are mixed and sintered, and the sintering temperature may be 400 to 700°C, 450 to 600°C, or 500 to 550°C, and the sintering time may be 1 to 9 hours, 2 to 8 hours, or 3 to 7 hours.

[0067] In particular, the method for preparing the positive electrode active material includes the following steps: (1) A nickel source, a cobalt source, a manganese source, or an aluminum source is weighed according to a certain molar ratio and dissolved in deionized water, respectively. A precursor is synthesized by controlling process conditions such as ammonia water concentration, pH value, stirring speed, reaction time, and reaction temperature, and the pH value can be controlled to 10 to 13, for example. (2) The precursor obtained in step (1) is uniformly mixed with an M element source and a lithium source, sintered in an oxygen atmosphere, cooled to room temperature, and then pulverized to obtain a material containing the M element. (3) The material containing the M element and the coating element source are uniformly mixed and sintered in an air atmosphere at 400 to 700° C. for 1 to 9 hours to obtain a positive electrode active material.

[0068] In addition, a third aspect of the present application provides a battery including a positive electrode piece including a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, the positive electrode active material layer including the positive electrode active material described above or a positive electrode active material produced by the production method described above.

[0069] In some embodiments of the present application, the actual active area of ​​the positive electrode active material layer is A cm 2 4 × 10 4 ≦A≦2×10 5 For example, 4.5×10 4 , 6.5×10 4 , 7.6×10 4 , 8×10 4 , 9×10 4 , 1×10 5 , or a range consisting of any two values ​​thereof. In some embodiments of the present application, 4 ≦A≦1×10 5 and in some embodiments of the present application, 7.6×10 4 ≦A≦9×10 4 The actual active area refers to the effective area that can participate in an electrochemical reaction. The actual active area of ​​the positive electrode active material layer is related to the pore structure, pore size distribution, specific surface area, and pressure resistance of the positive electrode active material, and the above material parameters and the compression density of the positive electrode active material layer work together to change the actual active area.

[0070] In some embodiments of the present application, when the temperature is −20° C. and the state of charge (SOC) of the battery is 30%, the discharge power per unit volume of the positive electrode active material layer is PW / cm 3 , 8≦P≦30, and may be, for example, 8.9, 14, 15, 16, 22, 23, 24, 25, 29, or a range consisting of any two values ​​thereof. In some embodiments of the present application, 8.9≦P≦29, and in some embodiments of the present application, 15≦P≦25. The relationship between the low-temperature low-SOC discharge power P0 of the battery and the actual active area A satisfies 0.6≦1000P0 / A≦1, d, P=P0×PD / m, where P0W represents the discharge power of the battery under the above conditions, and PD g / cm 3 represents the compressed density of the positive electrode active material layer, and mg represents the weight of the positive electrode active material layer.

[0071] In some embodiments of the present application, the compressed density of the positive electrode active material layer is PD g / cm 3 and 2.4≦PD≦3.5 is satisfied, and may be, for example, 2.6, 2.8, 3.0, 3.1, 3.3, or a range consisting of any two values ​​thereof. In some embodiments of the present application, 2.6≦P s ≦3.1, and the porosity P s 20%≦P s ≦40%, for example, 22%, 23%, 25%, 26%, 27%, 28%, 30%, 35%, or a range consisting of any two values ​​thereof. s ≦35%, and in some embodiments of the present application, 25%≦P s ≦30%.

[0072] Specifically, the above-mentioned positive electrode active material or the positive electrode active material produced by the above-mentioned method is uniformly mixed with a conductive agent, a binder and a solvent, and the positive electrode pieces are produced through processes such as sieving, coating, rolling, slitting and cutting. By changing the rolling parameters, the corresponding characteristics and parameters of the positive electrode pieces can also be controlled. The positive electrode active material layer of the present application can be controlled to satisfy the above characteristics.

[0073] Specifically, the battery comprises a positive electrode piece, a negative electrode piece, a separator and an electrolyte, and the positive electrode piece is the above-mentioned positive electrode piece. In a specific implementation, the above-mentioned positive electrode piece, negative electrode piece, separator and electrolyte are combined to form a lithium ion battery. Here, the negative electrode material used in the negative electrode piece may be one or more of artificial graphite, natural graphite, mesophase carbon microspheres, amorphous carbon, lithium titanate, or silicon carbon alloy. The negative electrode material also needs to have properties such as high compression density, high mass specific capacity, and high volume specific capacity.

[0074] In some embodiments, the electrolyte includes an organic solvent, and the organic solvent may include a chain ester and a cyclic ester, and the weight percentage of the chain ester is greater than the weight percentage of the cyclic ester. The cyclic ester may include at least one of ethylene carbonate (EC) or propylene carbonate (PP), and the chain ester may include at least one of dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), or diethyl carbonate (DEC). In some embodiments, the solvent of the electrolyte includes EC, EMC, and DEC. In some embodiments, the weight ratio of EC, EMC, and DEC is (10-25):(10-25):(51-75). In some embodiments, the preparation of the electrolyte includes dissolving a completely dried lithium salt in an organic solvent in an argon atmosphere glove box having a moisture content of less than 10 ppm, and mixing the organic solvent uniformly to obtain the electrolyte. Here, the concentration of the lithium salt is 0.8-1.3 mol / L.

[0075] In some embodiments, the lithium salt can be LiPF6 (lithium hexafluorophosphate), LiBF4 (lithium tetrafluoroborate), or the like.

[0076] In some embodiments, the preparation of the separator includes selecting a polypropylene film having a thickness of 9 to 18 μm as the separator. The separator is not particularly limited, and any known separator having a porous structure and electrochemical stability and mechanical stability may be used.

[0077] A fourth aspect of the present application provides an electric device comprising the battery described above.

[0078] In some embodiments, the electric device of the present application may be, but is not limited to, a backup power source, a motor, an electric vehicle, an electric motorcycle, an electric assist bicycle, a bicycle, an electric tool, a large household battery, and the like.

[0079] The following describes specific examples.

[0080] Example 1, This embodiment provides a method for manufacturing a positive electrode active material and a positive electrode piece.

[0081] The preparation of the positive electrode active material includes the following steps. 1) Nickel sulfate, cobalt sulfate and manganese sulfate are weighed according to the element molar ratio Ni:Co:Mn=0.5:0.2:0.3, respectively dissolved in deionized water, each metal solution is transported to a reactor through a pipeline to form a mixed metal solution, nitrogen is introduced as a protective gas, NaOH aqueous solution as a precipitant and ammonia water as a complexing agent are added to the mixed metal solution, the ammonia water concentration of the solution and the pH value of the solution are adjusted stepwise, and the precursor is obtained by reacting for 10 hours. 2) Precursor, lithium carbonate, tungsten oxide and zirconium oxide are mixed uniformly, the lithium ratio is controlled to be 1.1:1, and the weight ratios of tungsten oxide and zirconium oxide to the precursor are 0.6 wt% and 0.37 wt%, respectively. 3) The mixed materials are transferred to the sintering process, which consists of two stages including the first stage sintering at 600℃ for 6 hours and the second stage sintering at 880℃ for 10 hours. 4) The sintered material is crushed, and the crushed material is uniformly mixed with aluminum oxide, and the weight ratio of aluminum oxide to the crushed material is 0.5 wt%. 5) The mixed materials are transferred to the sintering process, where the positive electrode active material is obtained by sintering at a temperature of 450°C for 8 hours. 6) The positive electrode active material, conductive agent, and binder are mixed in a mass ratio of 97:1.5:1.5, and the mixture is uniformly stirred and mixed with a solvent, and then the positive electrode pieces are produced through processes such as sieving, coating, rolling, slitting, and cutting. The obtained positive electrode active material parameters and positive electrode piece parameter values ​​are specifically shown in Tables 1 and 2.

[0082] The manufacturing method of the positive electrode active material and the positive electrode pieces in Examples 2 to 8, 14 to 18 and Comparative Examples 1 to 3 is almost the same as that in Example 1, and the difference is that in Examples 2 to 8 and Comparative Examples 1 to 3, the relevant parameters in the manufacturing step of the positive electrode active material are changed, and in Examples 14 to 18, the nickel-cobalt-manganese ratio, for example, the process parameters such as pH value, ammonia water concentration and synthesis atmosphere are further changed, so that the pore size distribution, porosity and specific surface area of ​​the positive electrode active material can be controlled to obtain a positive electrode active material having a predetermined parameter characteristic, and by manufacturing a positive electrode piece using such a positive electrode active material, a positive electrode piece having a predetermined parameter characteristic can be obtained, and the specific parameters are shown in Tables 1 and 2. Here, Comparative Examples 1 to 3 show the case where the parameters of the specific surface area, pore size and porosity are outside the range of the present application, and the expected actual active area of ​​the positive electrode active material layer cannot be achieved.

[0083] Examples 19 to 22 use the same positive electrode active material as Example 1, as well as the same conductive agent and binder. The difference is that Examples 19 to 22 change the rolling parameters in the electrode piece manufacturing process. By controlling the compression density of the positive electrode pieces, the porosity and actual active area of ​​the positive electrode pieces can be controlled, and positive electrode pieces with predetermined parameter characteristics can be obtained. For specific parameters, see Tables 1 and 2.

[0084] Compared with Example 1, the differences between Examples 9 to 13 are the differences in M ​​elements and coating elements, but the pore size distribution, specific surface area and I value of the material are ensured to be within the appropriate range. For specific material parameters and pole piece parameters, please refer to Tables 1 and 2.

[0085] The actual active area A of the positive electrode active material layer was measured in the following manner. 1) Condition the battery to a specified SOC (e.g., 30% SOC). 2) The battery with the adjusted SOC is transferred to a glove box and disassembled. A sample is made by cutting the positive electrode piece using a mold for making a symmetrical battery sample (the size of the positive electrode piece sample is 46x28mm), and an appropriate amount of high-purity anhydrous dimethyl carbonate (DMC) is injected to soak and wash the sample. The DMC is replaced every 8 hours, and the sample is washed three times in a row and dried for 12 hours, after which a symmetrical battery is made from the positive electrode piece. 3) Conduct an EIS test on the symmetrical battery, read the frequency f corresponding to the maximum radius according to the EIS test curve (Nyquist plot), and calculate the ω max = 2πf according to the angular velocity ω max Calculate. 4) Fit the symmetrical cell EIS to obtain the charge transfer impedance R ct Get a specific value of . 5) Formula A=1 / 20ω max R ct to obtain the real active area A of the electrode.

[0086] [Table 1-1]

[0087] [Table 1-2]

[0088] [Table 1-3]

[0089] [Table 2-1]

[0090] [Table 2-2]

[0091] For the lithium ion batteries of Examples 1-22 and Comparative Examples 1-3, low-temperature output test, high-temperature storage test and high-temperature gas generation test were carried out. The process of low-temperature output test is to adjust the battery to 30% SOC, then leave it at a temperature of -20°C to stabilize the battery surface temperature, discharge it at a constant output P0W for 10 seconds, and if the terminal voltage is 2.21-2.26V, the output test is deemed successful, that is, P0W at this time is the low-temperature discharge power of the battery. The process of high-temperature storage test is to charge it to 4.3V, store it in a thermostatic box at 60°C, test the remaining capacity every 30 days, and store it again at full power. The calculation method is to test the initial capacity Q0 before storing it in the furnace, take it out of the thermostatic box every 30 days, test the remaining capacity Q after cooling, and "Q / Q0×100%" is the storage capacity maintenance rate of the battery. The process of high-temperature gas generation test is to take three battery samples, charge them to 4.3V, store them in a constant temperature box at 60℃, and test the battery volume every 15 days using the drainage method. Fully charge them at 1C every 30 days. The calculation method is to test the initial volume V0 using the drainage method, take the battery out of the constant temperature box every 15 days, and test the battery volume V using the drainage method after cooling, and "(V / V0-1)×100%" is the high-temperature storage volume expansion rate.

[0092] The performance data is shown in Table 3.

[0093] [Table 3]

[0094] In Examples 1 to 8 and Comparative Examples 1 to 3, the relevant parameters of materials with different pore size distributions are compared. max increases, and the half-width of the pore size distribution D HW As increases, the porosity P c is increased, and through the same electrode and battery manufacturing process, the actual active area A of the positive electrode active material layer is increased, and the low-temperature output performance of the battery is improved.

[0095] Examples 1, 19 to 22, and 14 to 18 compare the relevant parameters of the positive electrode active material layers having different compressed densities, and the compressed densities of the positive electrode active material layers and the porosity P s When the change in the active area A of the positive electrode active material layer is affected, the low-temperature output of the battery is also affected. This means that the appropriate I value, P s and compressed density.

[0096] Example 1 and Examples 9-10 compare the relevant parameters of materials with different M elements, and show that when the positive electrode active material contains two M elements, especially when it contains W, the overall performance of the battery is better than that when it contains only one M element.

[0097] Example 1 and Examples 11-12 compare the relevant parameters of materials with different coating elements, and the change and replacement of the above coating elements does not significantly affect the pore size distribution and porosity of the positive electrode active material, and does not significantly affect the electrical performance of the battery.

[0098] FIG. 1 shows an electron microscope characteristic evaluation test image of the surface morphology of the positive electrode active material obtained in Example 2 of the present application, and FIG. 2 shows an electron microscope characteristic evaluation test image of the cross-sectional morphology of the positive electrode active material obtained in Example 2 of the present application.

[0099] According to the present application, the actual active area of ​​the positive electrode active material layer is increased without affecting the processing of the slurry and the positive electrode pieces, the effective contact area between the positive electrode active material and the electrolyte is increased, and the ion transport, electron transport, and diffusion rate of the electrolyte are optimized, so that the output performance of the cell, especially the output performance at low temperatures, can be improved. The positive electrode active material produced according to the present application has excellent particle size distribution and compressive strength, which can effectively reduce the problem of particle breakage during rolling, improve the interface side reaction of the battery, reduce gas generation, and improve the long-term life. The positive electrode active material and positive electrode pieces of the present application have excellent compressibility, which can ensure the weight of the active material within a unit volume, and thus ensure the unit volume capacity of the battery.

[0100] The above is a detailed introduction of the positive electrode active material, battery, and its manufacturing method provided in the present application, in which specific examples are used to explain the principles and embodiments of the present application, and the above description of the examples is only used to understand the method and its core idea of ​​the present application. At the same time, those skilled in the art may change the specific embodiment and application scope based on the idea of ​​the present application, and in summary, the contents of this specification should not be understood as limitations on the present application.

Claims

1. A positive electrode active material comprising secondary particles, the secondary particles having pores, the positive electrode active material comprising: The characteristic of 4≦BET×TD×(Dv90−Dv10)≦14 is satisfied, Here, BET represents the specific surface area of ​​the positive electrode active material, and the unit is m 2 / g, TD represents the tap density of the positive electrode active material, and the unit is g / cm 3 Dv90 represents a corresponding particle diameter value when the cumulative volume distribution percentage of the positive electrode active material reaches 90%, and is expressed in units of μm; and Dv10 represents a corresponding particle diameter value when the cumulative volume distribution percentage of the positive electrode active material reaches 10%, and is expressed in units of μm.

2. 2. The positive electrode active material according to claim 1, wherein 0.4≦BET≦3.5, 1.2≦TD≦2.6, 4≦Dv90≦18, and 1.5≦Dv10≦6.

3. The maximum pore size of the positive electrode active material is D max nm, and 800≦D max 2. The positive electrode active material according to claim 1, wherein the positive electrode active material satisfies a molecular weight of ≦2200.

4. The half-width of the pore size distribution of the positive electrode active material is D HW nm, 150≦D HW 2. The positive electrode active material according to claim 1, wherein the positive electrode active material satisfies a molecular weight of ≦450.

5. The porosity P of the positive electrode active material c 45%≦P c 2. The positive electrode active material according to claim 1, wherein the positive electrode active material satisfies a content of ≦75%.

6. The powder compression density of the positive electrode active material is P d g / cm 3 and 2.8≦P d 2. The positive electrode active material according to claim 1, wherein the positive electrode active material satisfies a ratio of ≦3.

4.

7. The positive electrode active material has the chemical formula Li x Ni y Co z Me k M p O 2 wherein Me is selected from at least one of Mn or Al, M comprises at least one of Y, Nb, In, La, Zr, Ce, W, Al, Ti, Sr, Mg, Sb, V, Zn, Cu, Cr, or Fe, and 0.8≦x≦1.1, 0<y<1, 0<z<1, 0<k<1, and 0≦p≦0.

1.

8. 2. The positive electrode active material according to claim 1, wherein the positive electrode active material contains lithium nickel cobalt manganese oxide, the lithium nickel cobalt manganese oxide contains nickel element, cobalt element, and manganese element, and when a sum of a molar amount of the nickel element, the cobalt element, and the manganese element is taken as 1, a content of the nickel element is more than 0.

3.

9. mixing either a manganese source or an aluminum source with a nickel source and a cobalt source, adding a precipitating agent and a complexing agent, and reacting to obtain a ternary material precursor; mixing the ternary material precursor, the M element source and the lithium source, performing primary sintering, and obtaining a material containing the M element after cooling and pulverizing; and mixing the material containing the M element with a coating element source, and performing secondary sintering to obtain the positive electrode active material.

10. The nickel source includes at least one of nickel sulfate, nickel acetate, or nickel nitrate, the cobalt source includes at least one of cobalt sulfate, cobalt acetate, or cobalt nitrate, the manganese source includes at least one of manganese sulfate, manganese acetate, or manganese nitrate, the aluminum source includes at least one of aluminum sulfate, aluminum acetate, or aluminum nitrate, and the M element source includes at least one of zirconium nitrate, tungsten nitrate, aluminum nitrate, titanium nitrate, strontium nitrate, magnesium nitrate, yttrium nitrate, cerium nitrate, or the like.

10. The method of claim 9, wherein the lithium source comprises at least one of lithium hydroxide, lithium carbonate, lithium acetate, and lithium nitrate, and the coating element source comprises at least one of aluminum nitrate, titanium nitrate, cobalt nitrate, tungsten nitrate, yttrium nitrate, silicon oxide, boron oxide, phosphorus pentoxide, and aluminum oxide.

11. The method for producing a positive electrode active material according to any one of claims 9 to 10, characterized in that the mass percentage of the coating element source in the material containing the M element is 0.3 wt% to 0.7 wt%, the precipitating agent includes a sodium hydroxide solution, and the complexing agent includes an ammonia water.

12. The method for producing a positive electrode active material according to any one of claims 9 to 10, wherein the primary sintering temperature is 600 to 1000 ° C, the primary sintering time is 3 to 16 hours, the secondary sintering temperature is 400 to 700 ° C, and the secondary sintering time is 1 to 9 hours.

13. A battery including a positive electrode piece, the positive electrode piece including a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, the positive electrode active material layer including the positive electrode active material according to any one of claims 1 to 8, or a positive electrode active material produced by the production method according to any one of claims 9 to 12.

14. The positive electrode active material layer is (i) The actual active area of ​​the positive electrode active material layer is A cm 2 4×10 4 ≦A≦2×10 5 and (ii) The compressed density of the positive electrode active material layer is PD g / cm 3 and 2.4≦PD≦3.5 is satisfied; (iii) the porosity P of the positive electrode active material layer s 20%≦P s 14. The battery of claim 13, wherein the battery satisfies at least one of the following characteristics: ≦40%.

15. 15. An electrical device comprising the battery of claim 14.

Citation Information

Patent Citations

  • Positive electrode material for lithium ion secondary battery

    JP2005310421A

  • Lithium transition metal composite oxide, its manufacturing method, cathode for lithium secondary battery using it, and lithium secondary battery using it

    JP2008243447A

  • Lithium secondary battery

    JP2012209161A

  • Positive electrode active material for lithium secondary battery, positive electrode for lithium secondary battery, and lithium secondary battery

    JP2018106892A

  • Lithium transition metal complex oxide powder, nickel-containing transition metal complex hydroxide powder, positive electrode active substance for lithium secondary battery, positive electrode for lithium secondary battery, and lithium secondary battery

    JP2020100549A

Cited By

  • Electrode and lithium ion secondary battery

    JP2026087780A