Renewable polymer foam

Thermoreversible crosslinked polymer foams using MAH-g-OBC and secondary alcohol address the issues of melt strength and thermal stability in conventional foams, offering improved mechanical properties and recyclability.

JP2024536058APending Publication Date: 2024-10-04DOW GLOBAL TECHNOLOGIES LLC +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024518349
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-30
Filing Date
2022-09-29
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Conventional polymer foams used in applications like footwear insoles face challenges with high melt strength, thermal stability, and uniform cell structure during the foaming process, often leading to burst cells and poor mechanical properties due to irreversible crosslinking.

Method used

The development of thermoreversible crosslinked polymer foams using a crosslinking reaction product of maleic anhydride grafted olefin block copolymer (MAH-g-OBC) and a secondary alcohol, which allows for higher melt strength, improved processability, and better mechanical properties by dissociating and reassociating crosslinks at elevated and room temperatures.

Benefits of technology

The thermoreversible crosslinked polymer foams provide superior mechanical performance, easier processability, and uniform cell structure, with the ability to be recycled through hot pressing and re-foaming without chemical steps, maintaining high melt strength and thermal stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536058000001_ABST
    Figure 2024536058000001_ABST
Patent Text Reader

Abstract

Embodiments of the present disclosure relate to foams that may include a crosslinked reaction product of maleic anhydride grafted olefin block copolymer (MAH-g-OBC) and a secondary alcohol. The foams may have a density of 0.2 g / cc or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Application No. 63 / 250,256, filed September 30, 2021, the entire disclosure of which is incorporated herein by reference.

[0002] FIELD OF THE DISCLOSURE Embodiments of the present disclosure relate generally to polymers, and more specifically, to polymer foams. [Background technology]

[0003] Polymer foams are widely used in a variety of applications, for example as footwear insole materials. In insole applications, the foam must have high resilience, minimal shrinkage when heated, low density, and high tear strength. To achieve these properties, high melt strength is required. Without high melt strength, the foam cells may burst during the physical foaming that occurs near the melting point of the polymer. Traditionally, this strength is achieved by crosslinking, but crosslinked materials may have thermal stability issues during the foaming process.

[0004] Therefore, there is a need for improved materials that maintain melt strength and thermal stability during and after the physical foaming process.

[0005] The material provides a thermoreversibly crosslinked polymer foam. Summary of the Invention

[0006] The present disclosure addresses this need by providing a thermoreversible crosslinked polymer foam. Thermoreversible crosslinking means that the crosslinks dissociate at high temperature and reassociate at room temperature. Thus, thermoreversible crosslinking can provide high melt strength, easy processability, good mechanical properties, and uniform foam structure compared to irreversibly crosslinked polymer foams.

[0007] In one embodiment, the foam may include a crosslinked reaction product of maleic anhydride grafted olefin block copolymer (MAH-g-OBC) and a secondary alcohol. The foam may have a density of 0.2 g / cc or less.

[0008] According to another embodiment, the foam may be formed by physically foaming the thermoreversibly crosslinkable composition. In such an embodiment, the thermoreversibly crosslinkable composition may include MAH-g-OBC and a secondary alcohol.

[0009] Additional features and advantages of the embodiments will be set forth in the detailed description which follows, and in part will be readily apparent to those skilled in the art from that description, or will be recognized by practice of the embodiments described herein, including the following Detailed Description, the claims, and the accompanying drawings.

[0010] It is to be understood that both the foregoing and the following descriptions are intended to describe various embodiments and provide an overview or framework for understanding the nature and character of the claimed subject matter. The accompanying figures are included to provide a further understanding of the various embodiments, and are incorporated in and constitute a part of this specification. [Brief description of the drawings]

[0011] The following detailed description of certain embodiments of the present disclosure can be best understood when read in conjunction with the following drawings, in which like structure is indicated with like reference numerals and in which: [Figure 1] 1 shows FTIR spectra of Example 1 of the present invention at various temperatures. [Diagram 2] 1 shows the complex viscosity of Inventive Example 1 at various temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present disclosure includes polymer foams and methods for making polymer foams. The polymer foams may be derived from thermoreversibly crosslinkable polymer compositions such as MAH-g-OBC and secondary alcohols. These polymer foams may have superior melt strength, shrinkage, density, and processability compared to conventional foams.

[0013] definition As used herein, the terms "comprising", "including", "having" and their derivatives are not intended to exclude the presence of any additional components, steps, or procedures, whether they are specifically disclosed or not. For the avoidance of any doubt, all compositions claimed through the use of the term "comprising" may include any additional additives, adjuvants, or compounds, whether polymeric or otherwise, unless otherwise stated to the contrary. In contrast, the term "consisting essentially of" excludes from the scope of any succeeding description any other component, step, or procedure, except those that are not essential to operability. The term "consisting of" excludes any component, step, or procedure not specifically delineated or listed.

[0014] As used herein, the term "polymer" refers to a polymeric compound prepared by polymerizing monomers, whether of the same or different types. Thus, the term polymer encompasses the term homopolymer (used to refer to a polymer prepared from only one type of monomer, with the understanding that trace amounts of impurities may also be incorporated into the polymer structure), and the terms copolymer or interpolymer. Trace amounts of impurities (e.g., catalyst residues) may be incorporated into and / or within the polymer. The polymer may be a single polymer or a polymer blend.

[0015] "Polyethylene" or "ethylene-based polymer" shall mean a polymer containing more than 50 mole percent units derived from ethylene monomers. This includes ethylene-based homopolymers or copolymers (meaning that the units are derived from two or more comonomers). Common forms of ethylene-based polymers known in the art include, but are not limited to, low density polyethylene (LDPE), linear low density polyethylene (LLDPE), ultra low density polyethylene (ULDPE), very low density polyethylene (VLDPE), single-site catalyzed linear low density polyethylene (m-LLDPE), including both linear and substantially linear low density resins, medium density polyethylene (MDPE), and high density polyethylene (HDPE).

[0016] As used herein, the term "LDPE" or "low density polyethylene" refers to ethylene homopolymers prepared using free radical high pressure (100 MPa or higher (e.g., 100 to 400 MPa)) polymerization. LDPE resins typically have a density of 0.916 to 0.935 g / cm 3 The density is in the range of

[0017] The term "LLDPE" or "linear low density polyethylene" can include resins made using Ziegler-Natta catalyst systems, as well as resins made using single-site catalysts, including but not limited to bis-metallocene catalysts (sometimes referred to as "m-LLDPE"), phosphinimine, and constrained geometry catalysts, and post-metallocene molecular catalysts, including but not limited to bis(biphenylphenoxy) catalysts (also referred to as polyaryloxy ether catalysts). LLDPE includes linear, substantially linear, or heterogeneous ethylene-based copolymers or homopolymers. LLDPE contains less long chain branching than LDPE and includes substantially linear ethylene polymers as further defined in U.S. Patent Nos. 5,272,236, 5,278,272, 5,582,923, and 5,733,155, homogeneously branched linear ethylene polymer compositions such as those in U.S. Patent No. 3,645,992, heterogeneously branched ethylene polymers such as those prepared according to the process disclosed in U.S. Patent No. 4,076,698, and blends thereof (such as those disclosed in U.S. Patent No. 3,914,342 or U.S. Patent No. 5,854,045). LLDPE resins may be made by gas phase, solution phase, or slurry polymerization, or any combination thereof, using any type of reactor or reactor configuration known in the art.

[0018] As used herein, the term "PP" refers to polypropylene. A polypropylene resin may contain at least 50% by weight of propylene monomer. For example, a polypropylene resin may contain at least 60%, at least 70%, at least 80%, at least 90%, at least 95%, at least 99%, or even at least 100% by weight of propylene monomer.

[0019] As used herein, the abbreviation "EVA" refers to ethylene-vinyl acetate. An ethylene-vinyl acetate resin may contain at least 50% by weight of ethylene monomer. For example, an ethylene-vinyl acetate resin may contain at least 60% by weight, at least 70% by weight, or at least 70% by weight of ethylene monomer. Conversely, an ethylene-vinyl acetate resin may contain at least 5% by weight, at least 10% by weight, at least 15% by weight, at least 20% by weight, or at least 25% by weight of vinyl acetate monomer.

[0020] As used herein, the abbreviation "POE" refers to a POE compound having the general formula C n H 2n where n is 2 to 12. The polyolefin elastomer may comprise simple olefins in an amount of at least 50%, at least 60%, at least 70%, at least 80%, at least 90%, at least 95%, at least 99%, or even 100% by weight.

[0021] As used herein, the term "MAH" refers to maleic anhydride.

[0022] As used herein, the term "ASTM" refers to the standards organization ASTM International, formerly known as the American Society for Testing and Materials.

[0023] As used herein, "min." and "mins." mean minutes, "hr." / "hrs." mean hours, "sec." means seconds, "mol." means mole, "mol." means mole percent, "%" means mole percent, "cm" means centimeter, and "cm" means centimeter. -1" means 1 / centimeter, "mm" means millimeter, "kV" means kilovolt, "mA" means milliampere, "℃" means degrees Celsius, "rad / s" means radians per second, "MPA" means megapascal, "g" means gram, and "cc" means cubic centimeter.

[0024] Embodiment The present disclosure relates to reversibly crosslinked polymer foams. These foams are believed to offer superior mechanical performance and processability compared to conventional foams. Furthermore, these foams can be regenerated by hot pressing, compression molding, and physically expanding the foam again, without the need for chemical processes.

[0025] The foams of the present disclosure include a crosslinked reaction product of an MAH-grafted olefin block copolymer ("MAH-g-OBC") and a secondary alcohol. The foams may have a density of 0.2 g / cc or less.

[0026] The MAH-g-OBC can include a maleic anhydride grafted olefin block copolymer ("olefin block copolymer, OBC"). The MAH can be covalently bonded to the olefin block copolymer.

[0027] The MAH-g-OBC can have a maleic anhydride grafting level of 0.1-2.0 wt.%, for example, the MAH-g-OBC can be 0.1-2.0 wt.%, 0.5-2.0 wt.%, 1.0-2.0 wt.%, 1.5-2.0 wt.%, 0.1-1.5 wt.%, 0.1-1.0 wt.%, 0.1-0.5 wt.%, 0.2-1.8 wt.%, 0.4-1.6 wt.%, 0.6-1.4 wt.%, 0.8-1.2 wt.%, 0.3-0.7 wt.%, 0.4-0.5 wt.%, or any subset thereof, of MAH.

[0028] In various embodiments, the OBC is, for example, an ethylene / alpha-olefin block copolymer. Commercially available examples of ethylene / alpha-olefin block copolymers include resins available under the trade name INFUSE™ available from The Dow Chemical Company (Midland, MI).

[0029] In various embodiments, the ethylene / alpha-olefin copolymer may comprise ethylene in polymerized form and one or more copolymerizable alpha-olefin monomers, characterized by multiple blocks or segments of two or more polymerized monomer units with different chemical or physical properties. In one or more embodiments, the OBC may be represented by the formula (AB)n, where n is an integer of at least 1, preferably greater than 1, such as 2, 3, 4, 5, 10, 15, 20, 30, 40, 50, 60, 70, 80, 90, 100, or more, and "A" represents a hard block and "B" represents a soft block. In embodiments, A and B are linked in a substantially linear fashion, as opposed to a substantially branched or substantially star-shaped fashion. In one or more embodiments, the A and B blocks are randomly distributed along the polymer chain and do not have a structure such as AAA-AA-BBB-BB. In some embodiments, the block copolymer does not have a third type of block that includes a different comonomer. In an embodiment, block A and block B each have monomers or comonomers substantially randomly distributed within the block, such that neither block A nor block B includes two or more subsegments of distinct composition, such as tip segments, that have a substantially different composition than the remainder of the block.

[0030] OBC may contain various amounts of "hard" and "soft" blocks. "Hard" blocks refer to blocks of polymerized units in which ethylene is present in an amount greater than about 95% by weight, preferably greater than about 98% by weight, based on the weight of the polymer. In other words, the comonomer content in the hard blocks, i.e., the content of monomers other than ethylene, is less than about 5% by weight, preferably less than about 2% by weight, based on the weight of the polymer. In one or more embodiments, the hard blocks contain all or substantially all ethylene. On the other hand, "soft" blocks refer to blocks of polymerized units in which the comonomer content, i.e., the content of monomers other than ethylene, is greater than about 5% by weight. For example, the comonomer content may be greater than about 5% by weight, greater than about 8% by weight, greater than about 10% by weight, or greater than about 15% by weight, based on the weight of the polymer. In various embodiments, the comonomer content in the soft blocks can be greater than about 20% by weight, greater than about 25% by weight, greater than about 30% by weight, greater than about 35% by weight, greater than about 40% by weight, greater than about 45% by weight, greater than about 50% by weight, or greater than about 60% by weight based on the weight of the polymer.

[0031] In various embodiments, the soft block is present in the OBC in an amount of about 1% to about 99% by weight of the total weight of the polyolefin elastomer. For example, the soft block may be present in an amount of about 5% to about 95% by weight, about 10% to about 90% by weight, about 15% to about 85% by weight, about 20% to about 80% by weight, about 25% to about 75% by weight, about 30% to about 70% by weight, about 35% to about 65% by weight, about 40% to about 60% by weight, or about 45% to about 55% by weight of the total weight of the OBC. Conversely, the hard flocs may be present in a similar range. The weight percentages of the soft block and the hard block may be calculated based on data obtained from DSC or NMR. Such methods and calculations are disclosed in U.S. Patent Application Publication No. 2006 / 0199930.

[0032] Examples of alpha-olefin comonomers that can be used to form ethylene / alpha-olefin block copolymers include, by way of example and not limitation, propylene, isobutylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, and 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecent, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 4-methyl-1-pentene, 4,6-dimethyle-1-heptene, 4-vinylcyclohexene, vinylcyclohexane, norbornadiene, ethylidenenorbornene, cyclopentene, cyclohexene, dicyclopentadiene, cyclooctene, C4-C6 40 Dienes, other C4-C 40 In further embodiments, the alpha-olefin comonomer may include a C4-C8 comonomer. Comonomer content can be measured using any suitable technique, such as techniques based on nuclear magnetic resonance ("NMR") spectroscopy, for example, as described in U.S. Pat. No. 7,498,282, incorporated herein by reference. 13 It can be measured by C NMR analysis.

[0033] In various embodiments, the OBC has a melt index (I2) of about 0.5 to about 30.0 g / 10 min as determined according to ASTM D1238 (190° C., 2.16 kg). For example, the ethylene / alpha-olefin block copolymer can have a melt index (I2) of 0.5 to 30.0 g / 10 min, 0.5 to 12 g / 10 min, 0.5 g / 10 min to 5.0 g / 10 min, or 3.0 g / 10 min to 7.0 g / 10 min.

[0034] In various embodiments, the OBC has a density from 0.850 g / cc to 0.890 g / cc. All individual values ​​and subranges from 0.850 g / cc to 0.890 g / cc are included herein and disclosed herein, for example, the density of the ethylene / alpha-olefin block copolymer can be from a lower limit of 0.850 g / cc, 0.855 g / cc, 0.860 g / cc, 0.865 g / cc, or 0.870 g / cc to an upper limit of 0.890 g / cc, 0.885 g / cc, 0.880 g / cc, or 0.875 g / cc. In embodiments, the ethylene / alpha-olefin block copolymer has a density from 0.860 g / cc to 0.890 g / cc.

[0035] OBC has a melting temperature (T m ) (DSC). All individual values ​​and subranges from 115°C to 125°C are included herein and disclosed herein, for example, the melting point of the ethylene / alpha-olefin block copolymer can be from a lower limit of 115°C, 116°C, 117°C, 118°C, 119°C, or 120°C to an upper limit of 125°C, 124°C, 123°C, 122°C, or 121°C.

[0036] In some embodiments, the OBC has a molecular weight distribution (MWD) of 3.5 or less. Molecular weight distribution (MWD) is defined as the weight average molecular weight (Mw) divided by the number average molecular weight (Mn). For example, the OBC of some embodiments has an MWD of 2-3. Techniques for determining molecular weight (Mn and Mw) and MWD can be found in U.S. Pat. No. 4,540,753, which is incorporated herein by reference.

[0037] OBCs can be formed using known polymerization processes, such as those described in International Application No. PCT / US2005 / 008915, International Application No. PCT / US2005 / 008916, and International Application No. PCT / US2005 / 008917, each of which is incorporated herein by reference.

[0038] The foam may include a crosslinked reaction product of MAH-g-OBC and a secondary alcohol. As used herein, a "secondary alcohol" is a compound having a hydroxide group bonded to a carbon atom that has two other carbon atoms and a hydrogen bonded to it. A secondary alcohol may consist of carbon, oxygen, and hydrogen.

[0039] The secondary alcohol may be defined by Formula 1:

[0040] [ka]

[0041] Referring to formula 1, R1 and R4 may each independently represent a linear or cyclic alkyl group having 1 to 20 carbon atoms, an alkoxy group, or an aromatic group. For example, R1 may represent a linear or cyclic alkyl group having 1 to 20, 5 to 20, 10 to 20, 15 to 20, 1 to 15, 1 to 10, 1 to 5, 5 to 15, or any subset thereof; an alkoxy group; or an aromatic group. R4 may represent a linear or cyclic alkyl group having 1 to 20, 5 to 20, 10 to 20, 15 to 20, 1 to 15, 1 to 10, 1 to 5, 5 to 15, or any subset thereof; an alkoxy group; or an aromatic group.

[0042] Further referring to formula 1, R2 and R3 may each independently represent a linear or cyclic alkylene group having 1 to 20 carbon atoms, a carbonyl group, an aromatic group, or an oxy group. For example, R2 may represent a linear or cyclic alkylene group having 1 to 20, 5 to 20, 10 to 20, 15 to 20, 1 to 15, 1 to 10, 1 to 5, or 5 to 15 carbon atoms; a carbonyl group; an aromatic group; or an oxy group. R3 may represent a linear or cyclic alkylene group having 1 to 20, 5 to 20, 10 to 20, 15 to 20, 1 to 15, 1 to 10, 1 to 5, or 5 to 15 carbon atoms; a carbonyl group; an aromatic group; or an oxy group.

[0043] Still referring to Formula 1, d can be an integer equal to or greater than 0. For example, d can be 0, 1, 2, 3, 4, 5, or greater than 5. e can be an integer equal to or greater than 0. For example, e can be 0, 1, 2, 3, 4, 5, or greater than 5. f can be an integer equal to or greater than 1. For example, f can be 1, 2, 3, 4, 5, or greater than 5.

[0044] According to some embodiments, the secondary alcohol may include 2,5-hexanediol. For example, the secondary alcohol may include at least 50% by weight, at least 75% by weight, at least 90% by weight, at least 95% by weight, at least 99% by weight, or even at least 99.9% by weight of 2,5-hexanediol. 2,5-hexanediol may be represented by Formula 2:

[0045] [ka]

[0046] The foam may comprise 98% to 99.999% by weight of MAH-g-OBC. For example, the foam may comprise 98-99.99% by weight, 98-99.9% by weight, 98-99.9% by weight, 98-99% by weight, 98.5-99.999% by weight, 98.5-99.99% by weight, 98.5-99.9% by weight, 98.5-99.0% by weight, 99-99.999% by weight, 99-99.99% by weight, 99-99.9% by weight, 99.9-99.999% by weight, or any subset thereof.

[0047] The foam may contain 0.001 to 2.0% by weight of a secondary alcohol. For example, the foam may contain 0.001 to 1.5% by weight, 0.001 to 1.0% by weight, 0.001 to 0.5% by weight, 0.001 to 0.25% by weight, 0.001 to 0.2% by weight, 0.001 to 0.1% by weight, 0.001 to 0.01% by weight, 0.01 to 2% by weight, 0.01 to 1.5% by weight, 0.01 to 1.0% by weight, 0.01 to 0.5% by weight, 0.01 to 0.25% by weight, 0.01 to 0.2% by weight , 0.01-0.1 wt %, 0.1-2.0 wt %, 0.1-1.5 wt %, 0.1-1.0 wt %, 0.1-0.5 wt %, 0.1-0.25 wt %, 0.1-0.2 wt %, 0.5-2.0 wt %, 0.5-1.5 wt %, 0.5-1.0 wt %, 0.5-0.5 wt %, 1.0-2.0 wt %, 1-1.5 wt %, or any subset thereof of a secondary alcohol.

[0048] The foam may comprise 98-99.999% by weight of MAH-g-OBC and 0.001-2% by weight of secondary alcohol. Thus, at least 98.001% by weight of the foam may be the combined weight of MAH-g-OBC and secondary alcohol. For example, at least 98.01% by weight, at least 98.1% by weight, at least 98.5% by weight, at least 99.0% by weight, at least 99.5% by weight, at least 99.9% by weight, at least 99.99% by weight, at least 99.999% by weight, or even 100% by weight of the foam may be the combined weight of MAH-g-OBC and secondary alcohol.

[0049] The thermoreversible polymer composition contained in the foam and the reactions that make the thermoreversible polymer composition can be represented by Equation 3.

[0050] [ka]

[0051] Referring now to Formula 3, the thermoreversible polymer composition may be represented by the structure on the right, where the structure on the left is MAH-g-OBC and the structure above the line is a secondary alcohol. As in Formula 1, R1 and R4 each independently represent a linear or cyclic alkyl group, alkoxy group, or aromatic group having 1 to 20 carbon atoms. R2 and R3 each independently represent a linear or cyclic alkylene group, carbonyl group, aromatic group, or oxy group having 1 to 20 carbon atoms. d and e are integers of 0 or more. f is an integer of 1 or more.

[0052] The foam may include a blend of MAH-g-OBC with one or more of polyolefin elastomer ("POE"), ethylene vinyl acetate copolymer ("EVA"), and low density polyethylene ("LDPE"). One or more of POE, EVA, and LDPE may be chemically bonded to the MAH-g-OBC or may be blended with the MAH-g-OBC. According to some embodiments, the MAH-g-OBC may be mixed with one or more of POE, EVA, and LDPE prior to the crosslinking reaction with the secondary alcohol. According to other embodiments, the MAH-g-OBC may be mixed with one or more of POE, EVA, and LDPE after the crosslinking reaction with the secondary alcohol.

[0053] According to embodiments in which the foam further comprises one or more of POE, EVA, and LDPE, the foam may comprise at least 0.01 wt.%, at least 0.1 wt.%, at least 0.5 wt.%, at least 1.0 wt.%, at least 5.0 wt.%, at least 10 wt.%, at least 20 wt.%, or even at least 30 wt.% POE, EVA, and LDPE.

[0054] According to embodiments in which the foam further comprises one or more of POE, EVA, and LDPE, the foam may comprise at least 70% by weight of the combined weight of the MAH-g-OBC and the secondary alcohol. For example, the foam may comprise at least 80%, at least 90%, at least 95%, at least 99%, or even at least 99.9% by weight of the combined weight of the MAH-g-OBC and the secondary alcohol.

[0055] According to embodiments in which the foam further comprises one or more of POE, EVA, and LDPE, at least 99% by weight of the foam may be the combined weight of POE, EVA, LDPE, MAH-g-OBC, and secondary alcohol, for example, at least 99.5%, at least 99.9%, at least 99.99%, or even at least 99.999% by weight of the foam may be the combined weight of POE, EVA, LDPE, MAH-g-OBC, and secondary alcohol.

[0056] The foam may include a thermoreversibly crosslinkable polymer composition, such as MAH-g-OBC and a secondary alcohol. As used herein, a thermoreversibly crosslinkable polymer composition is a polymer in which crosslinks exist between units at low temperatures, and at high temperatures these crosslinks break down and reform again when the temperature is reduced. For example, at least 50% of the crosslinks between polymer units may dissolve when the temperature is increased from 25°C to 200°C. At least 90% of the crosslinks broken down at 200°C may reform when the temperature is reduced to 25°C.

[0057] The foam may have a % resilience of 60% or more. For example, the foam may have a % resilience of 62%, 64%, 66%, 68%, 70%, or 71% or more. % resilience or rebound is a measure of the relationship between the storage modulus and loss modulus in a polymer. % resilience may be measured according to ASTM D7121.

[0058] The foam may have a density of 0.2 g / cc or less. For example, the foam may have a density of less than 0.18 g / cc, less than 0.16 g / cc, 0.14 g / cc, 0.12 g / cc, 0.10 g / cc, 0.08 g / cc, or even 0.06 g / cc. The density of the foam may be measured according to ASTM D 792 Method A.

[0059] The foam can be formed by physically foaming the thermoreversibly crosslinkable composition to form the foam. As used herein, "physical foaming" is a process that can convert a polymeric composition into a foam without the use of chemical reactions. The thermoreversibly crosslinkable composition can include at least 50 wt%, at least 75 wt%, at least 90 wt%, at least 95 wt%, at least 99 wt%, or even at least 99.9 wt% MAH-g-OBC and secondary alcohol.

[0060] The thermoreversibly crosslinkable composition may be a virgin material or a recycled material. As used herein, a "virgin material" refers to a polymer composition that has never been foamed. As used herein, a "recycled material" refers to a polymer composition that has previously been foamed at least once.

[0061] The foam can be regenerated, which may include hot pressing the foam to remove air and form a solid film piece, compression molding the solid film piece into one or more plates, and physically expanding the plates to produce the regenerated foam.

[0062] Physical foaming may use a physical blowing agent. The physical blowing agent may include CO2 or N2. As used herein, a "physical blowing agent" may be a substance that can generate a cellular structure in a material. The physical blowing agent may be incorporated into the polymer by diffusion or mechanical mixing.

[0063] The polymer may be foamed by placing it in a high pressure chamber at a physical blowing agent pressure of at least 1 MPA, at least 2 MPA, at least 4 MPA, at least 6 MPA, at least 8 MPA, at least 10 MPA, or at least 12 MPA. The high pressure chamber may be heated to between 60°C and 180°C, between 80°C and 160°C, between 100°C and 140°C, between 110°C and 130°C, or any subset thereof, while the chamber is at the elevated blowing agent pressure.

[0064] The recycled foam may comprise a blend of recycled foam material and virgin foam material. For example, the recycled foam may be at least 10% by weight, at least 20% by weight, at least 30% by weight, at least 40% by weight, at least 50% by weight, at least 60% by weight, at least 70% by weight, at least 80% by weight, or at least 90% by weight recycled foam material. Further, the recycled foam may be at least 10% by weight, at least 20% by weight, at least 30% by weight, at least 40% by weight, at least 50% by weight, at least 60% by weight, at least 70% by weight, at least 80% by weight, or at least 90% by weight virgin foam material.

[0065] Test Method density The density of the foam (with both skins) was measured according to ASTM D 792 Method A by weighing the foam in air and in water.

[0066] Repulsion The rebound of foams (with skin) was measured according to ASTM D7121. An impact head was repeatedly bounced off the foam. The maximum rebound heights obtained for the fourth, fifth, and sixth bounces of the impact head after the first hit were recorded and the average was taken as the rebound of the specimen. Three specimens were tested for each foam sample and the average was reported as the rebound of the foam. As used herein, the rebound test may also be referred to as "resilience" or "rebound resilience."

[0067] Compression set ("Compression Set, C-set") The C-set of the foam (with one side skin) was measured according to ASTM D395 Method B. Each sample was a foam cylinder with a diameter of 2.54 mm and a thickness of 10 mm. Each sample was compressed to 50% of its original size and held at 50° C. for 6 hours. After decompression, each sample was allowed to recover at room temperature for 30 minutes to produce a sample labeled 30 minutes. An additional sample was allowed to rest for 24 hours to produce a "24 hour" sample. The thickness of the final specimen was measured and the compression set was calculated using the following formula: Compression Set (%)=((T o -T f )) / ((T o -T s )) × 100, where To is the original sample thickness and T f is the final sample thickness and T s is the spacer thickness.

[0068] tear strength The tear strength of foams (with one skin) was measured according to ASTM D3574. Foam strips of 25 mm (width) x 100 mm (length) x 10 mm (thickness) were cut. The foam strips were torn at a rate of 50 mm / min. The maximum load recorded divided by the sample width is the tear strength.

[0069] splitting splitting strength The split tear strength of foam (with one skin) was measured according to ASTM D3574. A foam strip of 25 mm (width) x 100 mm (length) x 10 mm (thickness) was cut and scored with a razor to a depth of 15 mm. The two foam strips (each 5 mm thick) formed by the razor cut were torn apart at a rate of 50 mm / min. The maximum load recorded divided by the sample width is the split tear strength.

[0070] Contraction The foam sample was marked and the length and width were measured. It was placed in a 70°C oven for 40 minutes, then removed from the oven and allowed to cool overnight. The marked length and width were measured again and the shrinkage was calculated by the following formula: Heat Shrinkage = (1-(L f +W f ) / (L o +W o ))×100. L o is the original length, and W o is the original width, and L f is the final length, and W f is the final width.

[0071] Fourier-Transform Infrared Spectroscopy (FTIR) Characterization A Perkin Elmer Spectrum Spotlight 200 equipped with a Smart DurasampLR Diamond Attenuated Total Reflectance (ATR) was used for ATR-FTIR analysis. The sample to be analyzed was placed on the diamond / ZnSe crystal. Appropriate pressure was applied to ensure optimal contact, and then the 4000 cm -1 ~650cm -1 ATR-FTIR spectra were collected at 100° C. Each sample was scanned eight times.

[0072] Scanning Electron Microscope (SEM) A small piece of sample was cut, mounted on a sample holder, and coated with Ir using an Emitech K575X coater. The current was set to 45 mA and the coating time was set to 15 seconds. The coated sample was immediately imaged in a Nova 630 NanoSEM operating in immersion mode using a through the lens detector (TLD) at an accelerating voltage of 2 kV, a spot size of 2.5, and a working distance of 4 mm.

[0073] Thermal sensitivity assessment by shear rheology Oscillatory frequency sweep tests were performed using a parallel plate rotational rheometer. Characterization was performed with a stress-controlled rheometer. Aluminum parallel plates (25 mm diameter) were used against thin disks of polymer (25 mm diameter, 2 mm thickness). The temperatures were set at 130°C, 150°C, and 180°C, respectively. The angular frequencies were set from 0.1 to 100 rad / s at a strain of 2%.

[0074] Tensile Modulus Oscillatory heating tests were performed using a dynamic mechanical analyzer. Characterization was performed with an RSA-G2 (TA Instruments). A tensile fixture was used to ensure the rectangular shape of the samples (width: approximately 5 mm, thickness: approximately 0.5 mm). The test temperature was set from 80 °C to 200 °C with a heating rate of 3 °C / min. The angular frequency was set to 6.28 rad / s and the auto strain mode was enabled over the entire temperature range.

[0075] hardness Hardness was measured according to ASTM D 2240. EXAMPLES

[0076] Sample foams were prepared by combining various MAH-grafted polymers with crosslinkers. The polymers are specified in Table 1. In the comparative example (CE1), 0.9 wt% Luperox 101 (2,5-bis(tert-butylperoxy)-2,5-dimethylhexane(peroxide) was used as the crosslinker. In the inventive examples (IE1-IE2) and other comparative examples (CE2-CE5), 0.1 wt% 2,5-hexanediol was used as the secondary alcohol crosslinker.

[0077] [Table 1]

[0078] Preparation of MAH-g-OBC resin MAH-grafted olefin polymers IE1-IE2 and CE1-CE5 were prepared by a reactive extrusion process. Specifically, polymer pellets were fed into a twin-screw extruder under nitrogen atmosphere. Downstream of the polymer injection point, a mixture of MAH, peroxide, 2-butanone, and methyl ethyl ketone (MEK) was added to the extruder. Further downstream, MEK, unreacted MAH, and peroxide by-products were removed via a vacuum line trap system. The resulting polymer melt was then extruded through a strand die, quenched in a water bath, and pelletized using a Conair strand pelletizer.

[0079] 1. Preparation of Pellets To prepare the inventive examples, 400 g of MAH-grafted polymer resin was placed in a bottle of 0.1 wt % 2,5-hexanediol and stirred at 60° C. overnight.

[0080] To prepare a comparative example, 400 g of MAH-grafted polymer resin was placed in a bottle of 0.9 wt % Luperox 101 (2,5-bis(tert-butylperoxy)-2,5-dimethylhexane) and stirred at 60° C. overnight.

[0081] The alcohol-soaked resin pellets were then compression molded to form plates. They were compression molded at 150°C for 20 minutes at a pressure of 10 MPA to 12 MPA to obtain a size of 6 mm x 70 mm x 150 mm, and finished at 190°C for 30 minutes.

[0082] Physical foaming The crosslinked and compression molded plates were then physically foamed by placing them in a high pressure chamber. The samples were kept in the CO2 chamber at 121°C and 12 MPA for 180 minutes.

[0083] The samples were tested for density, rebound, C-set, shrinkage, fractional tear, tensile modulus at maximum load, maximum load to tear, and Asker hardness. The results are shown in Table 2. Samples marked N / A were not tested. Sample CE2 did not form a foam and was not tested.

[0084] [Table 2]

[0085] As shown in Table 2, inventive examples IE1-IE2 have improved shrink and tear performance compared to the control.

[0086] Simulated playback FTIR: Sample IE1 was placed in the FTIR so that the height of the ester peak could be observed at multiple temperatures. As shown in Figure 1, the sample was started at room temperature (110), then the sample was ramped to 110°C (120), then the sample was ramped to 150°C (130), and finally the sample was returned to room temperature (140). As can be seen, the 1735 cm- 1 and 1710cm -1 The ester peak at decreases as the temperature is gradually increased. It then returns as the sample cools. This indicates that the ester is present initially, is destroyed as the temperature is increased, and new ester is formed as the sample cools again.

[0087] Complex Viscosity: Plaques of IE1 were prepared by compression molding and subjected to oscillatory frequency sweeps at 130°C (210), 150°C (220), and 180°C (230). As shown in Figure 2, the sample has the lowest complex viscosity at 180°C and the highest complex viscosity at 130°C, indicating that the sample is highly thermoplastic.

[0088] Actual playback The virgin sample IE1 was chopped and hot pressed to remove the air to obtain a solid film sample. The solid film sample was compression molded to obtain a 6 mm thick plate, which was then subjected to the same physical foaming process as the fresh sample. This sample is referred to as RE3 in Table 2.

[0089] In Table 3 the melt index of blends of IE1 and RE3 are compared.

[0090] [Table 3]

[0091] After re-expansion, the foam density was almost the same as when it was new. The density of the new foam was 0.075 g / cm 3 The recycled foam had a density of 0.078 g / cm 3 The density was 1.01 μm.

[0092] All documents cited herein, including any cross-referenced or related patents or applications, if any, and any patent applications or patents to which this application claims priority or the benefit thereof, are incorporated herein by reference in their entirety, unless expressly excluded or otherwise limited. The citation of any document is not an admission that it is prior art with respect to any invention disclosed or claimed herein, or that it alone, or in any combination with any other reference, teaches, suggests, or discloses such invention. Furthermore, to the extent that a meaning or definition of any term in this document conflicts with any meaning or definition of the same term in a document incorporated by reference, the meaning or definition assigned to that term in this document shall govern.

[0093] While particular embodiments of the present invention have been illustrated and described, it would be obvious to those skilled in the art that various other changes and modifications can be made without departing from the spirit and scope of the invention. Therefore, it is intended in the appended claims to cover all such changes and modifications that are within the scope of this invention.

Claims

1. A foam, comprising: Maleic anhydride grafted olefin block copolymer (MAH-g-OBC); A secondary alcohol, The crosslinked reaction product of A foam having a density of 0.2 g / cc or less.

2. 10. The foam of claim 1 comprising a blend of MAH-g-OBC and one or more of a polyolefin elastomer, an ethylene vinyl acetate copolymer, and a low density polyethylene.

3. The secondary alcohol has the formula: [Formula 1] (In the formula, R1 and R4 each independently represent a linear or cyclic alkyl group, alkoxy group, or aromatic group having 1 to 20 carbon atoms, R2 and R3 each independently represent a linear or cyclic alkylene group, carbonyl group, aromatic group, or oxy group having 1 to 20 carbon atoms, d and e each independently represent an integer of 0 or more, and f each independently represent an integer of 1 or more.) 3. The foam of claim 1 or 2, wherein the foam is defined by:

4. The foam of any of claims 1 to 3, wherein the secondary alcohol comprises 2,5-hexanediol.

5. The foam of any one of claims 1 to 4, having a rebound % of 60 or more.

6. The foam according to any one of claims 1 to 5, wherein the foam has a density of 0.1 g / cc or less.

7. 7. The foam of any of claims 1 to 6, wherein the MAH-g-OBC has a grafting level of maleic anhydride of 0.1 to 2.0 wt%.

8. The foam of any of claims 1 to 7, wherein the OBC is an ethylene / alpha-olefin block copolymer.

9. The foam of claim 8, wherein the alpha-olefin is octene.

10. 10. The foam of claim 8 or 9, wherein the ethylene / alpha-olefin block copolymer comprises greater than 50 mole % ethylene monomer.

11. 11. The foam of any of claims 1 to 10, comprising 98 to 99.999 wt. % MAH-g-OBC and 0.001 to 2 wt. % secondary alcohol.

12. 12. A foaming process for forming the foam of any one of claims 1 to 11 by physically foaming a thermoreversibly crosslinkable composition, wherein the thermoreversibly crosslinkable composition comprises the MAH-g-OBC and the secondary alcohol.

13. 13. The foaming process of claim 12, comprising: hot pressing the foam to remove air and form a solid film piece; compression molding said solid film pieces into one or more plates; and physically foaming the plate to produce recycled foam.

14. 14. The foaming process of claim 12 or 13, wherein the recycled foam comprises a blend of recycled and virgin foam materials.

15. The physical foaming uses a physical foaming agent, and the physical foaming agent is CO 2 Or N 2 The foaming process according to any one of claims 12 to 14, comprising:

Citation Information

Patent Citations

  • Polyolefin resin crosslinked foam and its preparation

    JP2001081222A

  • Composition and its use

    JP2005068184A