Lithium secondary battery

A lithium secondary battery using silicon particles with controlled charge and discharge depths addresses the limitations of carbon-based materials, achieving high capacity, rapid charging, and extended lifespan by optimizing electrode loading and prelithiation.

JP2024536254AActive Publication Date: 2024-10-04LG ENERGY SOLUTION LTD

Patent Information

Application Number
JP2024519734
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-05
Filing Date
2022-10-05
Publication Date
2024-10-04
Estimated Expiration
2042-10-05

AI Technical Summary

Technical Problem

Lithium secondary batteries using carbon-based negative electrode active materials face limitations in achieving high capacity and rapid charging performance due to their small capacity and slow reaction rate with lithium, while silicon-based materials offer higher capacity and faster reaction rates but suffer from rapid volume expansion leading to electrode damage and performance deterioration.

Method used

A lithium secondary battery design utilizing silicon particles as the negative electrode active material, with specific charge and discharge depth ratios within a defined range, along with optimized positive electrode loading, negative electrode loading, and prelithiation, to enhance life characteristics and energy density.

Benefits of technology

The battery achieves excellent capacity characteristics, rapid charging performance, and extended lifespan by controlling the Si charging depth and discharge depth within specific ranges, resulting in energy densities of 500 Wh/L or more and 80% life cycles exceeding 450 times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536254000001
    Figure 2024536254000001
  • Figure 2024536254000002
    Figure 2024536254000002
  • Figure 2024536254000003
    Figure 2024536254000003
Patent Text Reader

Abstract

The present invention relates to a lithium secondary battery comprising: a negative electrode containing a negative electrode active material; a positive electrode containing a positive electrode active material; a separator interposed between the negative electrode and the positive electrode; and an electrolyte, wherein the negative electrode active material contains silicon particles, and the Si depth of charge represented by the following formula (1) is 30% to 60%, and the Si depth of discharge represented by the following formula (2) is 10% or more. Formula (1): Si charge depth (%) = {(positive electrode loading amount + negative electrode pre-lithiation capacity) / negative electrode loading amount} × 100 Equation (2): Si discharge depth (%) = {(positive electrode loading amount + negative electrode pre-lithiation capacity - discharge loading amount) / negative electrode loading amount} × 100 In the above formulas (1) and (2), the positive electrode loading amount is the capacity per unit area of ​​the positive electrode (unit: mAh / cm 2 ), and the negative electrode loading is the capacity per unit area of ​​the negative electrode (unit: mAh / cm 2 ), and the prelithiation capacity of the negative electrode is the capacity per unit area of ​​lithium (Li) inserted into the negative electrode by prelithiation (unit: mAh / cm 2 The discharge loading amount is a value obtained by dividing the discharge capacity of the secondary battery at the discharge cut-off voltage by the positive electrode area.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0131946 filed on October 5, 2021 and Korean Patent Application No. 10-2022-0127248 filed on October 5, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated as part of this specification.

[0002] The present invention relates to a lithium secondary battery, and more specifically, to a lithium secondary battery using silicon (Si) particles as a negative electrode active material. [Background technology]

[0003] Recently, lithium secondary batteries have been attracting attention as an energy source for electric vehicles.

[0004] As electric vehicles become more widely used, there is an increasing need for lithium secondary batteries that can provide longer driving distances on a single charge and reduce the time required for rapid charging.

[0005] A lithium secondary battery is generally manufactured by forming an electrode assembly by interposing a separator between a positive electrode including a positive electrode active material made of a transition metal oxide containing lithium and a negative electrode including a negative electrode active material capable of storing lithium ions, inserting the electrode assembly into a battery case, injecting a non-aqueous electrolyte that serves as a medium for transmitting lithium ions, and then sealing the battery case. The non-aqueous electrolyte is generally composed of a lithium salt and an organic solvent capable of dissolving the lithium salt. Conventionally, carbon-based materials such as natural graphite and artificial graphite have been mainly used as negative electrode active materials for lithium secondary batteries. However, such carbon-based negative electrode active materials have a small capacity and a slow reaction rate with lithium, so that secondary batteries using such materials have limitations in achieving high capacity and rapid charging performance.

[0006] For this reason, efforts are being made to develop lithium secondary batteries that use silicon-based anode active materials, which have a theoretical capacity 10 times greater than that of carbon-based materials. Silicon-based anode active materials have the advantage of having a higher theoretical capacity and a faster reaction rate with lithium than carbon-based materials, which can improve capacity characteristics and rapid charging performance. However, they have the problem that their volume expands rapidly during charging, which can damage the anode and break the conductive path, resulting in a rapid deterioration of battery performance.

[0007] Therefore, there is a demand for the development of a lithium secondary battery that uses a silicon-based negative electrode active material and has excellent life characteristics. Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention is intended to solve the above-mentioned problems, and aims to provide a lithium secondary battery that uses silicon (Si) particles as a negative electrode active material to achieve high capacity characteristics and excellent life characteristics. [Means for solving the problem]

[0009] In one aspect, the present invention provides a lithium secondary battery comprising: a negative electrode including a negative electrode active material; a positive electrode including a positive electrode active material; a separator interposed between the negative electrode and the positive electrode; and an electrolyte, wherein the negative electrode active material comprises silicon particles, and the battery has a Si depth of charge represented by the following formula (1) of 30% to 60%, and a Si depth of discharge represented by the following formula (2) of 10% or more. Formula (1): Si charge depth (%) = {(positive electrode loading amount + negative electrode pre-lithiation capacity) / negative electrode loading amount} × 100 In the above formula (1), the positive electrode loading amount is the capacity per unit area of ​​the positive electrode (unit: mAh / cm 2 ), and the negative electrode loading is the capacity per unit area of ​​the negative electrode (unit: mAh / cm 2 ), and the prelithiation capacity of the negative electrode is the capacity per unit area of ​​lithium (Li) inserted into the negative electrode by prelithiation (unit: mAh / cm2 ). Equation (2): Si discharge depth (%) = {(positive electrode loading amount + negative electrode pre-lithiation capacity - discharge loading amount) / negative electrode loading amount} × 100 In the above formula (2), the positive electrode loading amount is the capacity per unit area of ​​the positive electrode (unit: mAh / cm 2 ), and the negative electrode loading is the capacity per unit area of ​​the negative electrode (unit: mAh / cm 2 ), and the prelithiation capacity of the negative electrode is the capacity per unit area of ​​lithium (Li) inserted into the negative electrode by prelithiation (unit: mAh / cm 2 The discharge loading amount is a value obtained by dividing the discharge capacity of the secondary battery at the discharge cut-off voltage by the positive electrode area. Effect of the Invention

[0010] The lithium secondary battery according to the present invention is designed so that the Si charge depth and the Si discharge depth satisfy specific ranges, and thus exhibits excellent life characteristics despite the use of Si particles as the negative electrode active material. Meanwhile, the Si particles are not necessarily mixed with the carbon-based negative electrode active material and / or SiO x Since the lithium secondary battery of the present invention using the lithium-based negative electrode active material has superior reactivity with lithium and capacity characteristics compared to the lithium-based negative electrode active material, the lithium secondary battery of the present invention can realize superior capacity characteristics and rapid charging performance. That is, the lithium secondary battery of the present invention has superior capacity characteristics, life characteristics and rapid charging performance.

[0011] In addition, the lithium secondary battery according to the present invention can use, as the positive electrode active material, for example, a lithium nickel-based oxide having a Ni content of 60 mol % or more, and in particular, when the Ni content is 80 mol % or more, the capacity characteristics can be further improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of ​​the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.

[0013] In the present invention, the term "primary particle" refers to a particle unit that does not have grain boundaries when observed at a magnification of 5,000 to 20,000 times using a scanning electron microscope. The term "average particle size of primary particles" refers to the arithmetic average value calculated after measuring the particle sizes of primary particles observed from a scanning electron microscope image.

[0014] In the present invention, the "secondary particles" are particles formed by agglomeration of a plurality of primary particles.

[0015] In the present invention, the "average particle size D 50 " means the particle diameter at 50% of the volume cumulative particle size distribution of the particle powder to be measured (e.g., positive electrode active material powder, negative electrode active material powder, etc.). 50 can be measured using the laser diffraction method. For example, the powder of the particles to be measured is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000), and ultrasonic waves of about 28 kHz are irradiated at an output of 60 W, and a volume cumulative particle size distribution graph is obtained, and the particle diameter corresponding to 50% of the volume cumulative amount is calculated.

[0016] The present invention will be specifically described below.

[0017] Si is used not only in carbon-based negative electrode active materials such as graphite, but also in SiO x, and has excellent capacity characteristics and lithium reactivity, even when compared with silicon-based negative electrode active materials such as SiC. Therefore, when Si is applied as a negative electrode active material, improved energy density and rapid charging performance can be obtained. However, since Si has a significant change in volume during charging and discharging, and the negative electrode rapidly deteriorates during charging and discharging, it has been difficult to achieve satisfactory life characteristics when Si is applied as a negative electrode active material. As a result of intensive research to improve the life characteristics of a lithium secondary battery using Si as a negative electrode active material, the present inventors have found that when a battery is designed so that the Si charge depth and Si discharge depth satisfy a specific range, it is possible to use Si as a negative electrode active material and achieve excellent life characteristics, and have completed the present invention.

[0018] Specifically, the lithium secondary battery according to the present invention is a lithium secondary battery including a negative electrode containing a negative electrode active material, a positive electrode containing a positive electrode active material, a separator interposed between the negative electrode and the positive electrode, and an electrolyte, wherein the negative electrode active material contains silicon (Si), and the Si depth of charge represented by the following formula (1) is 30% to 60%, and the Si depth of discharge represented by the following formula (2) is 10% or more. Preferably, the negative electrode active material does not contain other types of negative electrode active materials and can consist only of silicon.

[0019] Formula (1): Si charge depth (%) = {(positive electrode loading amount + negative electrode pre-lithiation capacity) / negative electrode loading amount} × 100

[0020] In the above formula (1), the positive electrode loading amount is the capacity per unit area of ​​the positive electrode (unit: mAh / cm 2 ), and the negative electrode loading is the capacity per unit area of ​​the negative electrode (unit: mAh / cm 2 ), and the prelithiation capacity of the negative electrode is the capacity per unit area of ​​lithium (Li) inserted into the negative electrode by prelithiation (unit: mAh / cm 2 ).

[0021] Equation (2): Si discharge depth (%) = {(positive electrode loading amount + negative electrode pre-lithiation capacity - discharge loading amount) / negative electrode loading amount} × 100

[0022] In the above formula (2), the positive electrode loading amount is the capacity per unit area of ​​the positive electrode (unit: mAh / cm 2 ), and the negative electrode loading is the capacity per unit area of ​​the negative electrode (unit: mAh / cm 2 ), and the prelithiation capacity of the negative electrode is the capacity per unit area of ​​lithium (Li) inserted into the negative electrode by prelithiation (unit: mAh / cm 2 The discharge loading amount is a value obtained by dividing the discharge capacity of the secondary battery at the discharge cut-off voltage by the positive electrode area.

[0023] The Si charge depth is a value indicating the degree of bonding between Si and Li in a fully charged state (i.e., SOC=100), and according to research by the present inventors, it has been shown that when the Si charge depth exceeds 60% or is less than 30%, the life characteristics are rapidly degraded. Specifically, when the Si charge depth exceeds 60%, the volume expansion of Si occurs rapidly, which results in a decrease in energy density and life characteristics, and when the Si charge depth is less than 30%, reaction non-uniformity becomes severe, resulting in a decrease in life characteristics. Preferably, the Si charge depth can be 40% to 60%, more preferably 50% to 60%.

[0024] The Si charge depth can be adjusted by controlling the positive electrode loading amount, the negative electrode loading amount, and / or the prelithiation degree of the negative electrode, and the positive electrode loading amount and / or the negative electrode loading amount can be set in consideration of the type and content of the active material used, the porosity of the active material layer, and / or the thickness of the active material layer.

[0025] On the other hand, the Si depth of discharge indicates the capacity of lithium remaining in the negative electrode at the discharge cut-off voltage. Research by the present inventors has shown that even if the Si depth of charge is 30% to 60%, if the Si depth of discharge is less than 10%, the life characteristics will be rapidly degraded. Preferably, the Si depth of discharge can be 10% to 30%, more preferably 10% to 25%, even more preferably 15% to 25%, and even more preferably 17% to 25%.

[0026] The Si depth of discharge is influenced by a ratio of the negative electrode capacity to the positive electrode capacity (N / P ratio), the operating voltage range of the battery, and the pre-lithiation degree of the negative electrode in a complex manner, and the Si depth of discharge can be adjusted by appropriately controlling these factors.

[0027] On the other hand, the lithium secondary battery of the present invention can be designed so that the Si usage range is 10% to 50%, preferably 20% to 40%, and more preferably about 30% to 40%. The Si usage range means the difference between the Si charge depth and the Si discharge depth, as shown in the following formula (3). If the Si usage range is large, the energy density increases, but the life characteristics are significantly reduced, and if the Si usage range is too small, the energy density decreases.

[0028] Equation (3): Si usage range (%) = Si charge depth - Si discharge depth

[0029] Meanwhile, the lithium secondary battery according to the present invention may have an N / P ratio, which is the percentage of the negative electrode loading amount to the positive electrode loading amount, of 150% to 300%, preferably 180% to 300%, and more preferably 190% to 300%. If the N / P ratio, which is the percentage of the negative electrode loading amount to the positive electrode loading amount, is less than the above range, the Si charge depth may increase and the life may be shortened, and if it exceeds the above range, the Si reaction non-uniformity of the electrode surface portion may become severe, and the life may be shortened.

[0030] The lithium secondary battery according to the present invention, designed to satisfy the above conditions, can realize excellent energy density and rapid charging performance by using Si particles, and also has excellent life characteristics. Specifically, the lithium secondary battery according to the present invention has an energy density of 500 Wh / L or more, preferably 550 Wh / L or more, more preferably 600 Wh / L or more, and even more preferably 650 Wh / L or more, and the number of times to reach 80% life can be 450 times or more, preferably 480 times or more, more preferably 500 times or more, even more preferably 600 times or more, and even more preferably 700 times or more.

[0031] For example, the lithium secondary battery according to the present invention may have a cell energy density of 500 Wh / L or more and a number of times at which 80% life is reached of 450 times or more, a cell energy density of 550 Wh / L or more and a number of times at which 80% life is reached of 480 times or more, a cell energy density of 650 Wh / L or more and a number of times at which 80% life is reached of 480 times or more, or a cell energy density of 550 Wh / L to 600 Wh / L and a number of times at which 80% life is reached of 700 times or more.

[0032] Next, each component of the lithium secondary battery according to the present invention will be specifically described.

[0033] negative electrode The negative electrode according to the present invention may contain silicon (Si) as a negative electrode active material, and preferably, 100% silicon (Si) may be used as the negative electrode active material. The silicon used in the present invention may be pure silicon (Pure Si) that is not bonded with other metals or oxygen. Specifically, the negative electrode according to the present invention includes a negative electrode current collector and a negative electrode active material layer formed on at least one surface of the negative electrode current collector, and the negative electrode active material layer may contain silicon (Si) as a negative electrode active material. Si can be used in carbon-based negative electrode active materials such as graphite as well as SiO xIt has superior capacity characteristics and lithium reactivity compared to silicon-based negative electrode active materials such as SiC. Therefore, when Si is used as a negative electrode active material, improved energy density and fast charging performance can be obtained.

[0034] The average particle size of the silicon (D 50 ) can be 1 μm to 10 μm, specifically 2 μm to 8 μm, and more specifically 3 μm to 7 μm. If the average particle size is less than 1 μm, the specific surface area of ​​the particles increases excessively, and the viscosity of the negative electrode slurry increases excessively. Therefore, the particles constituting the negative electrode slurry are not smoothly dispersed. If the size of the silicon particles is too small, the contact area between the silicon particles and the conductive material is reduced by the complex of the conductive material and the binder in the negative electrode slurry, so that the conductive network is likely to be disconnected and the capacity retention rate is reduced. On the other hand, if the average particle size is more than 10 μm, the silicon particles are too large, and the surface of the negative electrode becomes uneven, so that non-uniform current density occurs during charging and discharging. If the silicon particles are too large, the phase stability of the negative electrode slurry becomes unstable, and the processability is reduced. As a result, the capacity retention rate of the battery is reduced.

[0035] On the other hand, the BET specific surface area of ​​the silicon is preferably 0.01 m 2 / g~150.0m 2 / g, more preferably 0.1m 2 / g~100.0m 2 / g, particularly preferably 0.2m 2 / g~80.0m 2 / g, most preferably 0.2m 2 / g~18.0m 2 / g. The BET surface area can be measured according to DIN 66131 using nitrogen.

[0036] Also, the silicon can exist in crystalline or amorphous form and is preferably not porous. The silicon particles can be spherical or flaky particles, but are not limited thereto, and can also have a fibrous structure or exist in the form of a silicon-containing film or coating.

[0037] Always, the silicon can be contained in an amount of 50% by weight or more, 60% by weight or more, preferably 65% by weight or more, more preferably 70% by weight or more, and can be contained in an amount of 99% by weight or less, preferably 95% by weight or less, more preferably 90% by weight or less, still more preferably 80% by weight or less, based on the total weight of the negative electrode active material layer.

[0038] On the other hand, the negative electrode according to the present invention can further contain other negative electrode active materials other than the silicon, if necessary. The other negative electrode active materials can be, for example, SiO x (where 0 < x < 2), carbon-based negative electrode active materials, and the like. Here, the carbon-based negative electrode active materials can be, for example, artificial graphite, natural graphite, graphitized carbon fiber, amorphous carbon, soft carbon, hard carbon, etc., but are not limited thereto.

[0039] The other negative electrode active materials can be contained in an amount of 50% by weight or less, preferably 45% by weight or less, more preferably 30% by weight or less, based on the total weight of the negative electrode active material layer.

[0040] On the other hand, the negative electrode active material layer can further contain a conductive material and a binder, if necessary.

[0041] Examples of the conductive material include spherical or flaky graphite; carbonaceous materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, single-walled carbon nanotubes, and multi-walled carbon nanotubes; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and any one of these may be used alone or in combination. The conductive material may be included in an amount of 0.1% by weight to 40% by weight, 1% by weight to 30% by weight, or 5% by weight to 30% by weight based on the total weight of the negative electrode active material layer.

[0042] Preferably, the negative electrode active material layer according to the present invention may contain two or more kinds of conductive materials. In this case, the conductive materials may include dot-shaped conductive materials and plate-shaped conductive materials.

[0043] The dot-shaped conductive material can be used to improve the conductivity of the negative electrode, and is preferably one that does not cause chemical changes and has conductivity.Specifically, the conductive material can be at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, conductive fiber, fluorocarbon, aluminum powder, nickel powder, zinc oxide, potassium titanate, titanium oxide, and polyphenylene derivatives, and preferably can include carbon black in terms of realizing high conductivity and excellent dispersibility.

[0044] The dot-like conductive material has a BET specific surface area of ​​40 m 2 / g or more 70m 2 / g or less, and preferably 45m 2 / g or more 65m 2 / g or less, more preferably 50m 2 / g or more 60m 2 / g or less.

[0045] The dot-like conductive material can satisfy the functional group content (volatile matter) of 0.01% or more and 0.05% or less, preferably 0.01% or more and 0.04% or less, and more preferably 0.01% or more and 0.03% or less.

[0046] The functional group content can be adjusted according to the degree of heat treatment of the dot-shaped conductive material. That is, in the preparation of the dot-shaped conductive material, a high content of functional groups means a large amount of foreign matter, and a low content of functional groups means that more heat treatment processing has been performed. The dot-shaped conductive material according to the present application is characterized in that a predetermined partial heat treatment is performed on the dot-shaped conductive material to satisfy the functional group content range.

[0047] The particle diameter of the dot-like conductive material may be 10 nm to 100 nm, preferably 20 nm to 90 nm, and more preferably 20 nm to 60 nm. The plate-like conductive material can increase the surface contact between silicon particles in the negative electrode to improve conductivity and suppress the disconnection of the conductive path due to volume expansion, and can be expressed as a planar conductive material or a bulk conductive material.

[0048] The plate-shaped conductive material may include at least one selected from the group consisting of plate-shaped graphite, graphene, graphene oxide, and graphite flakes, and may be preferably plate-shaped graphite.

[0049] The average particle size of the plate-shaped conductive material (D 50 ) can be 2 μm to 7 μm, specifically 3 μm to 6 μm, and more specifically 4 μm to 5 μm. When the above range is satisfied, the sufficient particle size does not cause an excessive increase in viscosity of the negative electrode slurry, and dispersion is easy. Therefore, when dispersing using the same equipment and time, the dispersion effect is excellent.

[0050] The plate-shaped conductive material has a BET specific surface area of ​​1 m 2 / g or more 500m 2 / g or less, and preferably 5m 2 / g or more 300m 2 / g or less, more preferably 5m 2 / g or more 300m 2 / g or less.

[0051] Next, examples of the binder include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylic acid, polyacrylamide, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, and various copolymers thereof, and among these, one type alone or a mixture of two or more types can be used. The binder can be included in an amount of 1 wt% to 20 wt%, 2 wt% to 20 wt%, or 2 wt% to 10 wt% based on the total weight of the negative electrode active material layer.

[0052] Meanwhile, the negative electrode may have a single negative electrode active material layer or a multi-layer structure composed of two or more layers. When the negative electrode active material layer has a multi-layer structure composed of two or more layers, each layer may have a different type and / or content of the negative electrode active material, binder, and / or conductive material.

[0053] For example, the anode according to the present invention may have a two-layer structure, and the type of the anode active material of the layer adjacent to the current collector (hereinafter, referred to as the lower layer) and the type of the anode active material of the upper layer formed on the lower layer may be different from each other. Specifically, in the two-layer structure anode, the anode active material of the lower layer is silicon, and the anode active material of the upper layer is SiO. x (where 0 <x<2)であることができる。

[0054] Meanwhile, the negative electrode active material layer may have a porosity of 20% to 70% or 20% to 50%. If the porosity of the negative electrode active material layer is too small, the electrolyte impregnation property may decrease, and the lithium mobility may decrease, whereas if the porosity is too large, the energy density may decrease.

[0055] Meanwhile, in the present invention, the negative electrode may be a prelithiation negative electrode in which lithium is inserted before charging and discharging. The prelithiation of the negative electrode may be performed by a method for prelithiation of a negative electrode well known in the art. For example, the prelithiation of the negative electrode may be performed by a method of pressing or depositing lithium metal on a negative electrode active material layer, a method of inserting lithium into a negative electrode active material layer by an electrochemical method, a method of inserting excess lithium contained in a sacrificial positive electrode material or a positive electrode active material contained in a positive electrode into the negative electrode by an activation process, or a method of providing excess lithium to a positive electrode by an electrochemical method or a method of pressing or depositing lithium metal, and inserting the excess lithium provided to the positive electrode by an activation process into the negative electrode, or a combination of two or more of the above methods.

[0056] As described above, when a pre-lithiated negative electrode is used, deterioration of life characteristics is small even when the battery is discharged to a relatively low cut-off voltage compared to a non-pre-lithiated negative electrode, so that the driving voltage range of the lithium secondary battery can be set to a relatively wide range, and the usable SOC can be increased.

[0057] Preferably, the negative electrode of the present invention has a degree of prelithiation represented by the following formula (4) of 5% to 50%, preferably 5% to 30%, and more preferably 10% to 20%.

[0058] Formula (4): Degree of prelithiation (%) = {Capacity per unit area of ​​Li inserted into the negative electrode by prelithiation / Capacity per unit area of ​​Si} × 100

[0059] When the degree of pre-lithiation of the negative electrode satisfies the above range, a lithium secondary battery having excellent capacity and life characteristics can be realized. Specifically, if the degree of pre-lithiation of the negative electrode is too small, the life characteristics may be deteriorated. Although the life characteristics can be improved by controlling the depth of discharge, in this case, it is difficult to ensure the cell energy density. In addition, if the degree of pre-lithiation of the negative electrode is too large, the deterioration of silicon particles in the electrode may be accelerated, and the capacity characteristics may be deteriorated.

[0060] positive electrode The positive electrode according to the present invention includes a positive electrode active material layer. Specifically, the positive electrode according to the present invention may include a positive electrode current collector and a positive electrode active material layer formed on at least one surface of the positive electrode current collector.

[0061] The positive electrode active material layer contains a positive electrode active material, and may further contain a conductive material and / or a binder, if necessary.

[0062] As the positive electrode active material, various positive electrode active materials well known in the art, such as lithium nickel oxide, lithium manganese oxide, and lithium cobalt oxide, can be used. Preferably, the positive electrode active material of the present invention includes a lithium nickel oxide having a molar ratio of nickel of 60 mol% or more, preferably 80 mol% or more, more preferably 83 mol% or more, and even more preferably 85 mol% or more of the total metals other than lithium. Since a lithium nickel oxide containing 60 mol% or more of Ni has a high capacity, when a lithium nickel oxide containing 60 mol% or more of Ni is used as a positive electrode active material and Si is used as a negative electrode active material, a lithium secondary battery having significantly better capacity characteristics than the conventional one can be manufactured.

[0063] The lithium nickel-based oxide may be represented, for example, by the following Formula 1.

[0064] [Chemical formula 1] Li 1+x1 [Ni a1 Co b1 Mn c1 M 1 d1 ]O 2

[0065] In the above Chemical Formula 1, M 1 can be at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr and Zr.

[0066] Meanwhile, 1+x1 represents the molar ratio of lithium in the lithium nickel-based oxide and may be −0.2≦x1≦0.2 or 0≦x1≦0.1.

[0067] The a1 represents a molar ratio of nickel to all metals other than lithium in the lithium nickel-based oxide, and may be 0.6≦a1<1, 0.8≦a1<1, 0.8≦a1≦0.98, 0.82≦a1≦0.98, 0.83≦a1≦0.98, 0.85≦a1≦0.98, 0.88≦a1≦0.98, or 0.90≦a1≦0.98.

[0068] The b1 represents the molar ratio of cobalt to all metals other than lithium in the lithium nickel-based oxide, and is 0 <b1<0.4、0<b1<0.2、0<b1<0.18、0.01≦b1<0.18、0.01≦b1<0.17、0.01≦b1<0.15、0.01≦b1<0.12、または0.01≦b1<0.10であることができる。

[0069] The c1 represents a molar ratio of manganese among all metals other than lithium in the lithium nickel-based oxide, and is 0 <c1<0.4、0<c1<0.2、0<c1<0.18、0.01≦c1<0.18、0.01≦c1<0.17、0.01≦c1<0.15、0.01≦c1<0.12、または0.01≦c1<0.10であることができる。

[0070] The d1 is M out of all metals other than lithium in the lithium nickel-based oxide. 1 and may be 0≦d1<0.2, 0≦d1<0.18, 0≦d1<0.17, 0≦d1<0.15, 0≦d1<0.12, or 0≦d1<0.10.

[0071] Meanwhile, the positive electrode active material may further include a coating layer on the surface of the lithium nickel-based oxide, if necessary.

[0072] The coating layer is a coating element M 2 The coating element M 2may be at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr and Zr. The coating layer may be formed by various coating methods known in the art, such as dry coating, wet coating, chemical vapor deposition (CVD), physical vapor deposition (PVD), atomic layer deposition (ALD), etc.

[0073] The form of the positive electrode active material is not particularly limited, and may be, for example, a secondary particle form in which tens to hundreds of primary particles are aggregated, a single particle form consisting of 10 or less primary particles, or a combination thereof. When the positive electrode active material is in the form of secondary particles, the average particle diameter of the primary particles may be 0.05 μm to 4 μm, specifically, the average particle diameter of the primary particles may be 0.05 μm or more, 0.1 μm or more, and the average particle diameter of the primary particles may be 4 μm or less, 3 μm or less, or 2 μm or less. If the average particle diameter of the primary particles is too large, a rock salt phase may be formed, which may reduce the resistance characteristics and life characteristics, and if the average particle diameter of the primary particles is too small, the contact area with the electrolyte may increase, which may cause rapid deterioration. In addition, the average particle diameter of the secondary particles may be 2 μm to 25 μm, specifically, 2 μm or more, 3 μm or more, or 4 μm or more, and 25 μm or less, 20 μm or less, or 18 μm or less. When the average particle size of the secondary particles is within the above range, it is possible to prevent the positive electrode active material particles from being broken during the rolling process or to prevent the processability from being deteriorated during the preparation of the slurry. 50 Specifically, the average particle diameter D of the single particles can be 2 μm to 10 μm. 50 The average particle diameter D of the single particles can be 2 μm or more, 3 μm or more, 4 μm or more, 5 μm or more, or 6 μm or more, and can be 10 μm or less, 9 μm or less, 8 μm or less, or 7 μm or less. 50If it is too large, the lithium migration path becomes long, the resistance increases, and the output characteristics may decrease, and if it is too small, the specific surface area increases, and the side reaction with the electrolyte may increase. The average particle size of the primary particles constituting the single particle may be 0.5 μm to 4 μm, specifically, 0.5 μm or more, 0.7 μm or more, 1 μm or more, or 1.5 μm or more, and 4 μm or less, 3.5 μm or less, or 3 μm or less. If the average particle size of the primary particles constituting the single particle is too large, the lithium migration path becomes long, the resistance increases, and the output characteristics may decrease, and if it is too small, the specific surface area increases, and the side reaction with the electrolyte may increase.

[0074] Meanwhile, examples of the conductive material include spherical or flaky graphite; carbonaceous materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, single-walled carbon nanotubes, and multi-walled carbon nanotubes; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, among which one type alone or a mixture of two or more types can be used. The conductive material can be included in an amount of 0.1% by weight to 20% by weight, 1% by weight to 20% by weight, or 1% by weight to 10% by weight based on the total weight of the positive electrode active material layer.

[0075] Examples of the binder include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, and various copolymers thereof, and among these, one type alone or a mixture of two or more types can be used. The binder can be included in an amount of 1% by weight to 20% by weight, 2% by weight to 20% by weight, or 2% by weight to 10% by weight based on the total weight of the positive electrode active material layer.

[0076] Separator In the lithium secondary battery of the present invention, the separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular restrictions. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent humidification ability of the electrolyte solution is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting point glass fiber, polyethylene terephthalate fiber, etc., can be used. In addition, a coated separator containing a ceramic component or a polymeric substance can be used to ensure heat resistance or mechanical strength, and can be selectively used as a single layer or multilayer structure.

[0077] electrolyte In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.

[0078] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0079] The organic solvent can be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of solvents that can be used include carbonate-based solvents such as polycarbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a straight-chain, branched or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; and sulfolanes.

[0080] The lithium salt can be used without any particular limitation as long as it is a compound that can provide lithium ions used in lithium secondary batteries. Specifically, the anion of the lithium salt is F - , Cl - , Br - , I - , NO 3 - , N(CN) 2 - , B.F. 4 - , C.F. 3 CF 2 SO 3 - , (CF 3 SO 2 ) 2 N - , (FSO 2 ) 2 N - , C.F. 3 CF 2 (CF 3 ) 2 CO - , (CF 3 SO 2 ) 2 CH - ,(SCIENCE FICTION 5 ) 3 C - , (CF 3 SO 2 ) 3 C - , C.F. 3 (CF 2 ) 7 SO 3 - , C.F. 3 CO 2 - , C.H. 3 CO 2 - , SCN - and (CF 3 CF 2 SO 2 ) 2 N - The lithium salt may be at least one selected from the group consisting of LiPF 6 , LiN(FSO2 ) 2 , LiClO 4 , LiAsF 6 , LiBF 4 , LiSbF 6 , LiAl0 4 , LiAlCl 4 , LiCF 3 SO 3 , LiC 4 F 9 SO 3 , LiN(C 2 F 5 SO 3 ) 2 , LiN(C 2 F 5 SO 2 ) 2 , LiN(CF 3 SO 2 ) 2 , LiCl, LiI, or LiB(C 2 O 4 ) 2 The lithium salt may be used at a concentration within the range of 0.1M to 5.0M.

[0081] The electrolyte may contain additives for the purpose of improving the life characteristics of the battery, suppressing the capacity decrease, suppressing gas generation, etc. Examples of the additives include various additives used in the art, such as fluoroethylene carbonate (FEC), vinylene carbonate (VC), vinylethylene carbonate (VEC), ethylene sulfate (ESa), lithium difluorophosphate (LiPO 2 F 2 ), lithium bis(oxalato)borate (LiBOB), lithium tetrafluoroborate (LiBF 4), lithium difluorooxalate borate (LiDFOB), lithium difluorobisoxalate phosphate (LiDFBP), lithium tetrafluorooxalate phosphate (LiTFOP), lithium methyl sulfate (LiMS), lithium ethyl sulfate (LiES), propane sultone (PS), propene sultone (PRS), succinonitrile (SN), adiponitrile (AND), 1,3,6-hexanetricarbonitrile (HTCN), 1,4-dicyano-2-butene (DCB), fluorobenzene (FB), ethyl Di(prop-2-ynyl)phosphate (EDP), 5-methyl-5-propargyloxylcarbonyl-1,3-dioxane-2-one (MPOD), a compound represented by the following chemical formula A (e.g., cyanoethyl polyvinyl alcohol, PVA-CN), a compound represented by the following chemical formula B (e.g., heptafluorobutyl cyanoethyl polyvinyl alcohol, PF-PVA-CN), a compound represented by the following chemical formula C (e.g., propargyl 1H-imidazole-1-carboxylate, PAC), and / or a compound represented by the following chemical formula D (e.g., C 6 H 8 N 2 Aryl imidazoles such as aryl imidazoles can be used.

[0082] [ka]

[0083] In the above chemical formula A, m and n each independently represent an integer of 1-100.

[0084] [ka]

[0085] [ka]

[0086] In the above chemical formula C, R 16is a linear or non-linear alkylene group having 1 to 3 carbon atoms; R 17 ~R 19 are each independently at least one selected from the group consisting of hydrogen, an alkyl group having 1 to 3 carbon atoms, and -CN, and D is CH or N.

[0087] [ka]

[0088] In the above chemical formula D, R 1 , R 2 , R 3 , and R 4 may each independently contain hydrogen; or an alkyl group having 1 to 5 carbon atoms, a cyano group (CN), an allyl group, a propargyl group, an amine group, a phosphate group, an ether group, a benzene group, a cyclohexyl group, a silyl group, an isocyanate group (-NCO), or a fluoro group (-F).

[0089] Preferably, the additive may be a compound that acts as an oxygen scavenger. Phosphite-based structures such as tristri(methylsilyl)phosphite (TMSPi), tristrimethylphosphite (TMPi), and tris(2,2,2-trifluoroethyl)phosphite (TTFP) (see Chemical Formula E); tristri(methylsilyl)phosphate (TMSPa); polyphosphate trimethylsilyl ester (PPSE); tris(pentafluorophenyl)borane (TPFPB); coumarin-3-carbonitrile (CMCN), 7-ethynylcoumarin (ECM), 3-a Compounds containing a coumarin structure (see chemical formula F), such as cetylcoumarin (AcCM), 3-[(trimethylsilyl)oxyl]-2H-1-benzopyran-2-one (TMSOCM), and 3-(trimethylsilyl)coumarin (TMSCM); 3-(2-propyn-1-yloxyl)-2H-1-benzopyran-2-one (POCM), 2-propyn-1-yl-2-iodo-2H-1-benzopyran-3-carboxylate (OBCM), and the like, can be used as compounds that act as oxygen scavengers.

[0090] [ka]

[0091] [ka]

[0092] In the chemical formulas E and F, R1 to R6 may each independently include a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms and a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a cyano group (-CN), a fluoro group (F), an ether group (COC), a carboxyl group (OC=O), a trimethylsilyl group (-TMS), an isocyanate group (-NCO), and / or an isothiocyanate group (-NCS).

[0093] The present invention will now be described in more detail with reference to specific examples.

[0094] Manufacturing Example 1 <Production of positive electrodes> The positive electrode active material, conductive material, and PVDF binder were mixed in a weight ratio of 97.7:0.9:1.4 in N-methylpyrrolidone to prepare a positive electrode slurry. 0.86 Co 0.05 Mn 0.07 Al 0.02 O 2 As the conductive material, CNT was used.

[0095] The positive electrode slurry was applied onto an aluminum collector sheet, dried, and then rolled to obtain a loading capacity of 4.52 mAh / cm 2 A positive electrode having the formula:

[0096] <Production of negative electrodes> A negative electrode slurry was prepared by mixing the negative electrode active material, conductive material, and acrylic binder in a weight ratio of 70:20.3:9.7 in water. Here, Si particles (manufactured by Elkem) with an average particle size of 5 μm were used as the negative electrode active material, and carbon black, graphite, and CNT were mixed in a weight ratio of 9.8:10:0.52 as the conductive material.

[0097] The negative electrode slurry was applied onto a copper current collector sheet, dried, and then rolled to obtain a loading capacity of 8.73 mAh / cm 2 A negative electrode having the formula:

[0098] <Manufacturing lithium secondary batteries> A separator was interposed between the positive electrode and the negative electrode to prepare an electrode assembly. The electrode assembly was inserted into a battery case, and an electrolyte was injected into the battery case to prepare a lithium secondary battery A.

[0099] Manufacturing Example 2 <Production of positive electrodes> The positive electrode active material, conductive material, and PVDF binder were mixed in a weight ratio of 96.25:1.5:2.25 in N-methylpyrrolidone to prepare a positive electrode slurry. 0.83 Co 0.11 Mn 0.06 O 2 As the conductive material, Denka black was used.

[0100] The positive electrode slurry was applied onto an aluminum current collector sheet, dried, and then rolled to obtain a loading capacity of 3.50 mAh / cm 2 A positive electrode having the formula:

[0101] <Production of negative electrodes> A negative electrode slurry was prepared by mixing the negative electrode active material, conductive material, and acrylic binder in a weight ratio of 70:20.3:9.7 in water. Here, Si particles (manufactured by Waker) with an average particle size of 5 μm were used as the negative electrode active material, and carbon black, graphite, and CNT were mixed in a weight ratio of 9.8:10:0.52 as the conductive material.

[0102] The negative electrode slurry was applied onto a copper current collector sheet, dried, and then rolled to obtain a loading capacity of 7.36 mAh / cm 2 A negative electrode having the formula:

[0103] <Manufacturing lithium secondary batteries> A separator was interposed between the positive electrode and the negative electrode to prepare an electrode assembly. The electrode assembly was inserted into a battery case, and an electrolyte was injected into the battery case to prepare a lithium secondary battery B.

[0104] Production Example 3 A lithium secondary battery C was produced in the same manner as in Production Example 2, except that the loading amounts of the positive electrode and the negative electrode were changed as shown in Table 1 below.

[0105] Manufacturing Example 4 to Manufacturing Example 6 Lithium secondary batteries D to F were produced in the same manner as in Production Example 1, except that the loading amounts of the positive electrode and the negative electrode were changed as shown in Table 1 below.

[0106] Production Example 7 A lithium secondary battery G was produced in the same manner as in Production Example 2, except that the loading amounts of the positive electrode and the negative electrode were changed as shown in Table 1 below.

[0107] Production Example 8 <Production of positive electrodes> The positive electrode active material, conductive material, and PVDF binder were mixed in a weight ratio of 97.7:0.9:1.4 in N-methylpyrrolidone to prepare a positive electrode slurry. 0.86 Co 0.05 Mn 0.07 Al 0.02 O 2 As the conductive material, CNT was used.

[0108] The positive electrode slurry was applied onto an aluminum current collector sheet, dried, and then rolled to obtain a loading capacity of 3.03 mAh / cm 2 A positive electrode having the formula:

[0109] <Production of negative electrodes> A negative electrode slurry was prepared by mixing the negative electrode active material, conductive material, and acrylic binder in a weight ratio of 70:20.3:9.7 in water. Here, Si particles (manufactured by Elkem) with an average particle size of 5 μm were used as the negative electrode active material, and carbon black, graphite, and CNT were mixed in a weight ratio of 9.8:10:0.52 as the conductive material.

[0110] The negative electrode slurry was applied onto a copper current collector sheet, dried, and then rolled to obtain a loading capacity of 7.75 mAh / cm 2 A negative electrode having the formula:

[0111] Lithium metal was pressed onto the negative electrode to perform prelithiation, and the degree of prelithiation was 7.38%.

[0112] <Manufacturing lithium secondary batteries> A separator was interposed between the positive electrode and the pre-lithiated negative electrode to prepare an electrode assembly. The electrode assembly was inserted into a battery case, and an electrolyte was injected to prepare a lithium secondary battery H.

[0113] Manufacturing Example 9 to Manufacturing Example 11 Lithium secondary batteries I to K were produced in the same manner as in Production Example 8, except that the loading amount of the positive electrode was changed as shown in Table 1 below.

[0114] Manufacturing Example 12 A lithium secondary battery L was produced in the same manner as in Production Example 8, except that prelithiation was performed so that the degree of prelithiation (%) of the negative electrode was 16.5%.

[0115] The N / P ratios and Si charge depths of the lithium secondary batteries A to L prepared as above are shown in Table 1 below.

[0116] [Table 1]

[0117] Examples and Comparative Examples The number of cycles until the capacity retention rate reached 80% (80% lifespan number) and cell energy density were measured while charging / discharging the lithium secondary batteries A to L. Here, the charging / discharging was performed at 25° C., 1C / 0.5C, CCCV mode, the charge cut-off voltage was set to 4.2V, and the discharge cut-off voltage was set so that the Si depth of discharge had the value shown in [Table 2] below. The measurement results are shown in [Table 2] below. Table 2 also shows the usable SOC within the charge / discharge voltage range of each lithium secondary battery.

[0118] [Table 2]

[0119] As shown in Table 1, in the lithium secondary batteries of Examples 1 to 9, in which the Si depth of charge is 30% to 60% and the Si depth of discharge is 10% to 20%, the number of times to reach 80% life is shown to be high at 480 times or more, even though Si is used as the negative electrode active material. Also, the cell energy density is shown to be good at 500 Wh / L or more. In contrast, in the cases of Comparative Examples 1 to 12, in which either the Si depth of charge or the Si depth of discharge deviates from the range of the present invention, it can be confirmed that although the capacity characteristics are excellent, the number of times to reach 80% life is significantly reduced.

Claims

1. A lithium secondary battery comprising: a negative electrode including a negative electrode active material; a positive electrode including a positive electrode active material; a separator interposed between the negative electrode and the positive electrode; and an electrolyte, the negative electrode active material contains silicon particles, A lithium secondary battery having a Si charge depth represented by the following formula (1) of 30% to 60% and a Si discharge depth represented by the following formula (2) of 10% or more. Formula (1): Si charge depth (%) = {(positive electrode loading amount + negative electrode pre-lithiation capacity) / negative electrode loading amount} × 100 In the above formula (1), the positive electrode loading amount is the capacity per unit area of ​​the positive electrode (unit: mAh / cm 2 ), the negative electrode loading amount is the capacity per unit area of ​​the negative electrode (unit: mAh / cm 2 ), the prelithiation capacity of the negative electrode is the capacity per unit area of ​​lithium (Li) inserted into the negative electrode by prelithiation (unit: mAh / cm 2 ) and Formula (2): Si discharge depth (%) = {(positive electrode loading amount + negative electrode pre-lithiation capacity - discharge loading amount) / negative electrode loading amount} x 100 In the formula (2), the positive electrode loading amount is the capacity per unit area of ​​the positive electrode (unit: mAh / cm 2 ), the negative electrode loading amount is the capacity per unit area of ​​the negative electrode (unit: mAh / cm 2 ), the prelithiation capacity of the negative electrode is the capacity per unit area of ​​lithium (Li) inserted into the negative electrode by prelithiation (unit: mAh / cm 2 ), the discharge loading amount is a value obtained by dividing the discharge capacity of the secondary battery at the discharge cut-off voltage by the positive electrode area.

2. The lithium secondary battery according to claim 1 , wherein the negative electrode active material is made of silicon particles.

3. 2. The lithium secondary battery according to claim 1, wherein the Si charge depth is 40% to 60%.

4. 2. The lithium secondary battery according to claim 1, wherein the Si depth of discharge is 10% to 30%.

5. 2. The lithium secondary battery according to claim 1, wherein the lithium secondary battery has a Si usage range of 10% to 50% as represented by the following formula (3): Formula (3): Si usage range (%) = Si charge depth - Si discharge depth

6. 2. The lithium secondary battery according to claim 1, wherein the N / P ratio, which is a percentage of a negative electrode loading amount to a positive electrode loading amount, is 150% to 300%.

7. 2. The lithium secondary battery according to claim 1, wherein the N / P ratio, which is a percentage of a negative electrode loading amount to a positive electrode loading amount, is 180% to 300%.

8. The negative electrode is a prelithiated negative electrode, and the degree of prelithiation represented by the following formula (4) is 5% to 50%. The lithium secondary battery according to any one of claims 1 to 7. Formula (4): Degree of prelithiation (%)={capacity per unit area of ​​Li inserted into negative electrode by prelithiation / capacity per unit area of ​​Si}×100

9. 9. The lithium secondary battery according to claim 8, wherein the prelithiation degree is 5% to 30%.

10. 2. The lithium secondary battery of claim 1, wherein the positive electrode active material comprises a lithium nickel-based oxide having a nickel content of 60 mol % or more of all metals other than lithium.

11. The lithium secondary battery of claim 10 , wherein the lithium nickel-based oxide is represented by the following Chemical Formula 1: [Chemical formula 1] Li 1+x1 [Ni a1 Co b1 Mn c1 M 1 d1 ]O 2 In the formula 1, −0.2≦x1≦0.2, 0.6≦a1<1, 0<b1<0.4, 0<c1<0.4, and 0≦d1<0.2; M 1 is at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr and Zr.

12. 2. The lithium secondary battery according to claim 1, wherein the lithium secondary battery has a cell energy density of 500 Wh / L or more and an 80% life reaching number of times of 450 or more.

13. 2. The lithium secondary battery according to claim 1, wherein the lithium secondary battery has a cell energy density of 650 Wh / L or more and an 80% life reaching number of times of 480 or more.

14. 2. The lithium secondary battery according to claim 1, wherein the lithium secondary battery has a cell energy density of 550 Wh / L to 600 Wh / L and a number of times at which 80% of the battery life is reached is 700 or more.

Citation Information

Patent Citations

  • Lithium battery

    JP2014137996A

  • Lithium ion secondary battery, and method for manufacturing the same

    JP2016018588A

  • Lithium ion battery and producing method thereof

    US20200036035A1

  • Electrical device

    WO2015111194A1

  • Positive electrode, cell, cell pack, electronic device, electric vehicle, electric storage device, and electric power system

    WO2015198521A1

Cited By

  • Nonaqueous electrolyte containing additive for nonaqueous electrolyte and lithium secondary battery containing the same

    JP2024531441A

  • Nonaqueous electrolyte containing additive for nonaqueous electrolyte and lithium secondary battery containing the same