Preparation of Propylimine-Functional Organosilicon Compounds and Primary Aminopropyl-Functional Organosilicon Compounds

The described process addresses the challenges of high cost and instability in amino-functional polyorganosiloxanes by forming propylimine-functional compounds and then converting them to primary aminopropyl-functional compounds, achieving high-purity and cost-effective products for personal care applications.

JP2024536286AActive Publication Date: 2024-10-04DOW GLOBAL TECHNOLOGIES LLC +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024519891
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-04-13
Filing Date
2022-10-06
Publication Date
2024-10-04
Estimated Expiration
2042-10-06

AI Technical Summary

Technical Problem

Existing methods for producing amino-functional polyorganosiloxanes are costly, require expensive starting materials and catalysts, involve multiple steps, and result in products with stability issues such as viscosity changes and ammonia odor, making them unsuitable for personal care applications.

Method used

A process involving the formation of propylimine-functional organosilicon compounds through a propylaldehyde-functional organosilicon compound and subsequent reductive amination with ammonia to produce primary aminopropyl-functional organosilicon compounds, using hydroformylation to introduce the propylaldehyde group and a rhodium/ligand complex catalyst.

Benefits of technology

The process achieves high-purity, selective, and cost-effective production of amino-functional organosilicon compounds suitable for personal care applications without stability issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536286000001
    Figure 2024536286000001
  • Figure 2024536286000002
    Figure 2024536286000002
  • Figure 2024536286000003
    Figure 2024536286000003
Patent Text Reader

Abstract

Organosilicon compounds having primary aminopropyl functionality are prepared. A catalytic reductive amination process for combining a secondary propylimine-functional organosilicon compound with ammonia and hydrogen produces a primary aminopropyl-functional organosilicon compound.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims the benefit under 35 U.S.C. §119(e) of U.S. Provisional Patent Application No. 63 / 252,639, filed October 6, 2021, and U.S. Provisional Patent Application No. 63 / 330,571, filed April 13, 2022. Both U.S. Provisional Patent Application No. 63 / 252,639 and U.S. Provisional Patent Application No. 63 / 330,571 are incorporated herein by reference.

[0002] FIELD OF THEINVENTION A process for preparing propylimine-functional organosilicon compounds and primary aminopropyl-functional organosilicon compounds is disclosed. More specifically, the process includes the protection of the propylaldehyde-functional organosilicon compound by forming a propylimine group from the propylaldehyde group, and then the reductive amination of the propylimine-functional organosilicon compound with ammonia. [Background technology]

[0003] Introduction Certain amino-functional polyorganosiloxanes are useful, for example, in textile and leather treatment applications. Other amino-functional polyorganosiloxanes, such as amine-terminated polydiorganosiloxanes, are useful in personal care applications, such as hair care. Amine-terminated polydiorganosiloxanes can be useful, for example, in hair conditioning applications. Amino-functional polyorganosiloxanes made by condensation can suffer from instability, as indicated by viscosity changes and / or the development of ammonia odor after aging, which is undesirable for personal care applications. Traditionally, amino-functional polyorganosiloxanes are expensive to make by equilibration, as they require expensive starting materials and catalysts and require multiple process steps to complete.

[0004] Another method for making amino-functional polyorganosiloxanes uses allylamines or derivatives that hydrolyze to allylamines, which are used with SiH-functional polymers to perform hydrosilylation chemistry to form amino-functional polyorganosiloxanes; however, this method suffers from the drawback that the amino-functional polyorganosiloxane product may contain at least trace amounts of either SiH or allylamine, either of which must be removed before the product can be used in any personal care application due to the toxicity of allylamine and the reactivity of SiH.

[0005] Another method of making amino-functional polyorganosiloxanes is by ammonolysis of chloropropyl-terminated siloxanes. This expensive multi-step method can suffer from the drawback of leaving residual salts (i.e., ammonium chloride) in the amine-terminated polyorganosiloxane product that may require extensive washing to remove, which is less cost-effective and less sustainable. Also, any residual ammonium chloride may produce a malodor, which is undesirable for personal care applications.

[0006] Thus, there is an unmet need in the organosilicon industry for synthetic methods for preparing a wide range of amino-functional organosilicon compounds with relatively high purity, high selectivity, and / or low cost. Summary of the Invention

[0007] A process for preparing propylaldehyde functional organosilicon compounds is disclosed.Propylimine functional organosilicon compounds can be used to prepare primary aminopropyl functional organosilicon compounds, comprising combining starting materials comprising propylaldehyde functional organosilicon compounds and a primary amine source under conditions that result in a propylimine-forming reaction, thereby forming a reaction product comprising propylimine functional organosilicon compounds and water.The process further comprises forming primary aminopropyl functional organosilicon compounds from propylimine functional organosilicon compounds by reductive amination. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In the process introduced above and detailed below, the propylaldehyde-functional organosilicon compound can be a known propylaldehyde-functional organosilicon compound and can be made by known methods such as those described in U.S. Patent No. 4,424,392 to Petty, U.S. Patent No. 5,021,601 to Frances et al., U.S. Patent No. 5,739,246 to Graiver et al., U.S. Patent No. 7,696,294 to Asirvatham, U.S. Patent No. 7,999,053 to Sutton et al., European Patent Application Publication No. 0392948(A1) to Frances, PCT Patent Application Publication No. 2006027074 to Kuhnle et al., and PCT Patent Application Publication No. 2022081444 to Fisk et al.

[0009] Hydroformylation Alternatively, the propylaldehyde-functional organosilicon compound may be prepared by a hydroformylation process as described in U.S. Provisional Patent Application No. 63 / 330571, filed April 13, 2022, and incorporated herein by reference. The hydroformylation process includes 1) combining starting materials under conditions that catalyze a hydroformylation reaction, the starting materials including (A) a gas containing hydrogen and carbon monoxide, (B) a vinyl-functional organosilicon compound, and (C) a hydroformylation reaction catalyst, such as a rhodium / bisphosphoramidite ligand complex catalyst or a rhodium / tetraphosphoramidite ligand complex catalyst, thereby forming a hydroformylation reaction product including the propylaldehyde-functional organosilicon compound. The starting materials used in the hydroformylation process may optionally further include (D) a solvent.

[0010] (A) Synthetic gas The gas starting material (A) used in the hydroformylation process includes carbon monoxide (CO) and hydrogen gas (H2). For example, the gas can be synthesis gas. As used herein, "syngas" (from synthesis gas) refers to a gas mixture containing various amounts of CO and H2. Production methods are well known and include, for example, (1) steam reforming and partial oxidation of natural gas or liquid hydrocarbons, and (2) gasification of coal and / or biomass. CO and H2 are typically the major components of synthesis gas, but synthesis gas can contain carbon dioxide and inert gases such as CH4, N2, and Ar. The molar ratio of H2 to CO (H2:CO molar ratio) varies widely but can range from 1:100 to 100:1, alternatively 1:10 to 10:1. Synthesis gas is commercially available and is often used as a fuel source or as an intermediate for producing other chemicals. Alternatively, CO and H2 from other sources (i.e., other than syngas) may be used as starting material (A) herein. Alternatively, the H2:CO molar ratio in starting material (A) for use herein may be 3:1 to 1:3, alternatively 2:1 to 1:2, alternatively 1:1.

[0011] (B) Vinyl-functional organosilicon compounds The vinyl-functional organosilicon compound has at least one vinyl group covalently bonded to silicon per molecule. Alternatively, the vinyl-functional organosilicon compound can have two or more vinyl groups covalently bonded to silicon per molecule. The starting material (B) can be one vinyl-functional organosilicon compound. Alternatively, the starting material (B) can include two or more vinyl-functional organosilicon compounds that are different from each other. For example, the vinyl-functional organosilicon compound can include one or both of (B1) silane and (B2) polyorganosiloxane.

[0012] The starting material (B1), a vinyl-functional silane, has the formula (B1-1): A x SiR 4 (4-x) wherein each R A is a vinyl group, and each R 4 is independently selected from the group consisting of alkyl groups of 1 to 18 carbon atoms, aryl groups of 6 to 18 carbon atoms, acyloxy groups of 2 to 18 carbon atoms, and hydrocarbyloxy functional groups of 1 to 18 carbon atoms, and the subscript x is 1 to 4. Alternatively, the subscript x can be 1 or 2, alternatively 2, alternatively 1. Alternatively, each R 4 may be independently selected from the group consisting of an alkyl group of 1 to 18 carbon atoms, an aryl group of 6 to 18 carbon atoms, an acetoxy group of 2 to 18 carbon atoms, and an alkoxy functional group of 1 to 18 carbon atoms. 4 may be independently selected from the group consisting of alkyl groups of 1 to 18 carbon atoms, aryl groups of 6 to 18 carbon atoms, and hydrocarbyloxy functional groups of 1 to 18 carbon atoms. 4 may be independently selected from the group consisting of alkyl groups of 1 to 12 carbon atoms, and aryl groups of 6 to 12 carbon atoms. Alternatively, each R 4may be independently selected from the group consisting of alkyl groups of 1 to 8 carbon atoms and aryl groups of 6 to 8 carbon atoms. 4 may be independently selected from the group consisting of methyl and phenyl.

[0013] R 4 Suitable alkyl groups for may be linear, branched, cyclic, or a combination of two or more thereof. The alkyl groups are exemplified by methyl, ethyl, propyl (including n-propyl and / or isopropyl), butyl (including n-butyl, tert-butyl, sec-butyl, and / or isobutyl), pentyl, hexyl, heptyl, octyl, decyl, dodecyl, undecyl, and octadecyl (and branched isomers having 5 to 18 carbon atoms), and the alkyl groups are further exemplified by cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, and cyclohexyl. Alternatively, R 4 The alkyl group of R may be selected from the group consisting of methyl, ethyl, propyl, and butyl, alternatively methyl, ethyl, and propyl, alternatively methyl or ethyl. 4 The alkyl group in may be methyl.

[0014] R 4 Suitable aryl groups for may be monocyclic or polycyclic and may have pendant hydrocarbyl groups. For example, R 4 Aryl groups of R include phenyl, tolyl, xylyl, and naphthyl, as well as aralkyl groups such as benzyl, 1-phenylethyl, and 2-phenylethyl. 4 The aryl group of R may be monocyclic, such as phenyl, tolyl, or benzyl; alternatively, R 4 The aryl group can be phenyl.

[0015] R 4 Suitable hydrocarbyloxy functional groups for the compound are of the formula -OR 5 Or expression - OR 3 -OR 5 wherein each R 3is an independently selected divalent hydrocarbyl group of 1 to 18 carbon atoms, and each R 5 are independently selected from the group consisting of alkyl groups of 1 to 18 carbon atoms and aryl groups of 6 to 18 carbon atoms, which are 4 As described and exemplified above. 3 Examples of divalent hydrocarbyl groups for are those of the empirical formula -C r H 2r -, where the subscript r is 2 to 8. The alkane-diyl group can be a linear alkane-diyl, for example, -CH2-CH2-, -CH2-CH2-CH2-, -CH2-CH2-CH2-CH2-CH2-, or -CH2-CH2-CH2-CH2-CH2-CH2-CH2-, or a branched alkane-diyl, for example,

[0016] [ka] Alternatively, R 3 is an arylene group such as phenylene, or

[0017] [ka] Alternatively, R may be an alkyl arylene group such as 3 may be a linear alkane-diyl group such as ethylene. Alternatively, the hydrocarbyloxy functionality may be an alkoxy functionality such as methoxy, ethoxy, propoxy, or butoxy, alternatively methoxy or ethoxy, alternatively methoxy.

[0018] R 4 Suitable acyloxy groups for the formula

[0019] [ka] wherein R 5is as described above. Examples of suitable acyloxy groups include acetoxy. Vinyl-functional acyloxysilanes and methods for their preparation are known in the art, for example, U.S. Patent No. 5,387,706 to Rasmussen et al. and U.S. Patent No. 5,902,892 to Larson et al.

[0020] Suitable vinyl-functional silanes are exemplified by vinyl-functional trialkylsilanes such as vinyltrimethylsilane and vinyltriethylsilane, vinyl-functional trialkoxysilanes such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, and vinyltris(methoxyethoxy)silane, vinyl-functional dialkoxysilanes such as vinylphenyldiethoxysilane, vinylmethyldimethoxysilane, and vinylmethyldiethoxysilane, vinyl-functional monoalkoxysilanes such as trivinylmethoxysilane, vinyl-functional triacyloxysilanes such as vinyltriacetoxysilane, and vinyl-functional diacyloxysilanes such as vinylmethyldiacetoxysilane.All of these vinyl-functional silanes are commercially available from Gelest Inc. (Morrisville, Pennsylvania, USA).Furthermore, vinyl-functional silanes can be prepared by known methods such as those disclosed in U.S. Patent No. 4,898,961 to Baile et al. and U.S. Patent No. 5,756,796 to Davern et al.

[0021] Alternatively, (B) the vinyl-functional organosilicon compound may comprise (B2) a vinyl-functional polyorganosiloxane. The polyorganosiloxane may be cyclic, linear, branched, resinous, or a combination of two or more thereof. The polyorganosiloxane may have a unit formula (B2-1): (R 4 3SiO 1 / 2 ) a (R 4 2R A SiO 1 / 2 ) b (R 4 2SiO 2 / 2 ) c (R 4 RA SiO 2 / 2 ) d (R 4 SiO 3 / 2 ) e (R A SiO 3 / 2 ) f (SiO 4 / 2 ) g (ZO 1 / 2 ) h wherein R A and R 4 is as defined above, and each Z is independently selected from a hydrogen atom and R 5 (In the formula, R 5 are as above), and the subscripts a, b, c, d, e, f, and g represent the number of each unit in formula (B2-1), with values ​​such that subscript a≧0, subscript b≧0, subscript c≧0, subscript d≧0, subscript e≧0, subscript f≧0, and subscript g≧0, the quantity (a+b+c+d+e+f+g)≧2, and the quantity (b+d+f)≧1, and the subscript h has a value such that 0≦h / (e+f+g)≦1.5. At the same time, the quantity (a+b+c+d+e+f+g) can be ≦10,000. Alternatively, when e=f=g=0, then h≧0. Alternatively, in formula (B-2-1), each R 4 may be independently selected from the group consisting of a hydrogen atom, an alkyl group of 1 to 18 carbon atoms, and an aryl group of 6 to 18 carbon atoms. 4 may be independently selected from the group consisting of alkyl groups of 1 to 12 carbon atoms, and aryl groups of 6 to 12 carbon atoms. Alternatively, each R 4 may be independently selected from the group consisting of alkyl groups of 1 to 8 carbon atoms, and aryl groups of 6 to 8 carbon atoms. 4 may be independently selected from the group consisting of methyl and phenyl. Alternatively, each Z may be hydrogen or an alkyl group of 1 to 6 carbon atoms. Alternatively, each Z may be hydrogen.

[0022] Alternatively, the vinyl-functional polyorganosiloxane (B2) may comprise a linear polydiorganosiloxane (B2-2) having at least one vinyl group per molecule, alternatively at least two vinyl groups (e.g., when subscripts e=f=g=0 in formula (B2-1) above). For example, the polydiorganosiloxane may have the unit formula (B2-3): (R 4 3SiO 1 / 2 ) a (R A R 4 2SiO 1 / 2 ) b (R 4 2SiO 2 / 2 ) c (R A R 4 SiO 2 / 2 ) d wherein R A and R 4 is as above, subscript a is 0, 1, or 2, subscript b is 0, 1, or 2, subscript c > 0, and subscript d > 0, with the proviso that the quantity (b+d) > 1, the quantity (a+b) = 2, and the quantity (a+b+c+d) > 2. Alternatively, in unit formula (B2-3), the quantity (a+b+c+d) can be at least 3, alternatively at least 4, alternatively > 50. At the same time, in unit formula (B2-3), the quantity (a+b+c+d) can be 10,000 or less, alternatively 4,000 or less, alternatively 2,000 or less, alternatively 1,000 or less, alternatively 500 or less, alternatively 250 or less. Alternatively, in unit formula (B2-3), each R 4 may be independently selected from the group consisting of alkyl and aryl, alternatively methyl and phenyl. Alternatively, each R in the unit formula (B2-3) 4 can be an alkyl group, alternatively, each R 4 can be methyl.

[0023] Alternatively, the polydiorganosiloxane of the unit formula (B2-3) may be a polydiorganosiloxane of the unit formula (B2-4): (R 4 2R A SiO 1 / 2 )2(R 4 2SiO 2 / 2 )m (R 4 R A SiO 2 / 2 ) n , Unit formula (B2-5): (R 4 3SiO 1 / 2 )2(R 4 2SiO 2 / 2 ) o (R 4 R A SiO 2 / 2 ) p or a combination of both (B2-4) and (B2-5).

[0024] In formulas (B2-4) and (B2-5), each R 4 and R A are as above. Subscript m may be 0 or a positive number. Alternatively, subscript m may be at least 2. Alternatively, subscript m may be from 2 to 2,000. Subscript n may be 0 or a positive number. Alternatively, subscript n may be from 0 to 2000. Subscript o may be 0 or a positive number. Alternatively, subscript o may be from 0 to 2000. Subscript p is at least 2. Alternatively, subscript p may be from 2 to 2000.

[0025] The starting material (B2) is a vinyl-functional polydiorganosiloxane, such as i) bis-dimethylvinylsiloxy-terminated polydimethylsiloxane, ii) bis-dimethylvinylsiloxy-terminated poly(dimethylsiloxane / methylvinylsiloxane), iii) bis-dimethylvinylsiloxy-terminated polymethylvinylsiloxane, iv) bis-trimethylsiloxy-terminated poly(dimethylsiloxane / methylvinylsiloxane), v) bis-trimethylsiloxy-terminated polymethylvinylsiloxane, v i) bis-dimethylvinylsiloxy terminated poly(dimethylsiloxane / methylphenylsiloxane / methylvinylsiloxane), vii) bis-dimethylvinylsiloxy terminated poly(dimethylsiloxane / methylphenylsiloxane), viii) bis-dimethylvinylsiloxy terminated poly(dimethylsiloxane / diphenylsiloxane), ix) bis-phenyl,methyl,vinyl-siloxy terminated polydimethylsiloxane, and x) a combination of two or more of i)-ix).

[0026] Methods for preparing the linear vinyl-functional polydiorganosiloxanes described above for starting material (B2), such as the hydrolysis and condensation of the corresponding organohalosilanes and oligomers, or the equilibration of cyclic polydiorganosiloxanes, are known in the art, see, for example, U.S. Pat. Nos. 3,284,406, 4,772,515, 5,169,920, 5,317,072, and 6,956,087, which disclose the preparation of linear polydiorganosiloxanes having vinyl groups. Examples of linear polydiorganosiloxanes having vinyl groups are commercially available, for example, under the trade names DMS-V00, DMS-V03, DMS-V05, DMS-V21, DMS-V22, DMS-V25, DMS-V-31, DMS-V33, DMS-V34, DMS-V35, DMS-V41, DMS-V42, DMS-V43, DMS-V46, DMS-V51, DMS-V52 from Gelest Inc., Morrisville, Pennsylvania, USA.

[0027] Alternatively, the (B2) vinyl-functional polyorganosiloxane may be cyclic, for example, where in the unit formula (B2-1), the subscripts a=b=c=e=f=g=h=0. Cyclic vinyl-functional polydiorganosiloxanes are represented by the unit formula (B2-7): (R 4 R A SiO 2 / 2 ) d wherein R A and R 4 is as above, and subscript d can be 3 to 12, alternatively 3 to 6, alternatively 4 to 5. Examples of cyclic vinyl functional polydiorganosiloxanes include 2,4,6-trimethyl-2,4,6-trivinyl-cyclotrisiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinyl-cyclotetrasiloxane, 2,4,6,8,10-pentamethyl-2,4,6,8,10-pentavinyl-cyclopentasiloxane, and 2,4,6,8,10,12-hexamethyl-2,4,6,8,10,12-hexavinyl-cyclohexasiloxane. These cyclic vinyl functional polydiorganosiloxanes are known in the art and are commercially available, for example, from Sigma-Aldrich (St. Louis, Missouri, USA), Milliken (Spartanburg, South Carolina, USA), and other vendors.

[0028] Alternatively, the cyclic vinyl-functional polydiorganosiloxane may be represented by the unit formula (B2-8): (R 4 2SiO 2 / 2 ) c (R 4 R A SiO 2 / 2 ) d wherein R 4 and R A is as above, and subscript c is >0 to 6, and subscript d is 3 to 12. Alternatively, in formula (B2-8), c can be 3 to 6, and d can be 3 to 6.

[0029] Alternatively, (B2) vinyl-functional polyorganosiloxane may be an oligomer, for example, where the quantity (a+b+c+d+e+f+g) in the above unit formula (B2-1) is ≦50, alternatively ≦40, alternatively ≦30, alternatively ≦25, alternatively ≦20, alternatively ≦10, alternatively ≦5, alternatively ≦4, alternatively ≦3. The oligomer may be cyclic, linear, branched, or a combination thereof. Cyclic oligomers are as described above as starting material (B2-6).

[0030] An example of a linear vinyl-functional polyorganosiloxane oligomer is represented by the formula (B2-10):

[0031] [ka] wherein R 4 is as above, and each R 2 are independently 4 and R A with the proviso that at least one R 2 is R A where the subscript z is 0 to 48. Alternatively, the subscript z can be 0 to 4, alternatively 0 or 1, alternatively 0. Alternatively, when z=0 in formula (B2-10), the vinyl-functional polyorganosiloxane oligomer has the formula (B2-10a):

[0032] [ka] wherein R A is vinyl and R 4Examples of linear vinyl-functional polyorganosiloxane oligomers can include 1,3-divinyl-1,1,3,3-tetramethyldisiloxane, 1,1,1,3,3-pentamethyl-3-vinyl-disiloxane, 1,1,1,3,5,5,5-heptamethyl-3-vinyl-trisiloxane (all of which are commercially available, for example, from Gelest, Inc. (Morrisville, Pennsylvania, USA) or Sigma-Aldrich (St. Louis, Missouri, USA)).

[0033] Alternatively, the vinyl-functional polyorganosiloxane oligomer can be branched. The branched oligomer has the general formula (B2-11): R A SiR 12 3, where R A is vinyl as above, and each R 12 is R 13 and -OSi(R 14 ) 3, wherein each R 13 is a monovalent hydrocarbon group (e.g., R 4 As described and exemplified above for R, each R may be an alkyl group of 1 to 18 carbon atoms or an aryl group of 6 to 18 carbon atoms. 14 is R 13 , -OSi(R 15 )3, and -[OSiR 13 2] ii OSiR 13 3 are selected, and each R 15 is R 13 , -OSi(R 16 )3, and -[OSiR 13 2] ii OSiR 13 3 are selected, and each R 16 is R 13 and -[OSiR 13 2] ii OSiR 13 3, where the subscript ii has a value such that 0≦ii≦100. 12 At least two of -OSi(R 14 ) 3. Alternatively, R12 All three of the -OSi(R 14 )3.

[0034] Alternatively, in formula (B2-11), each R 12 R 13 In the case where the branched polyorganosiloxane oligomer has the following structure (B2-11a):

[0035] [ka] In the formula, R A and R 13 is as defined above. Alternatively, in formula (B2-11a), each R 13 can be methyl.

[0036] Alternatively, in formula (B2-11), each R 12 -OSi(R 14 )3, then each R 14 is -OSi(R) such that the branched polyorganosiloxane oligomer has the following structure (B2-11b): 15 ) three parts,

[0037] [ka] In the formula, R A and R 15 is as described above. Alternatively, each R 15 As above, R 13 Each R 13 can be methyl.

[0038] Alternatively, in formula (B2-11), each R 12 -OSi(R 14 )3, then one R 14 is each R 12 -OSiR 13 (R 14 )2 for each -OSi(R 14 )3 in R 13Alternatively, -OSiR 13 (R 14 )2 R's 14 each of which is a branched polyorganosiloxane oligomer having the following structure (B2-11c):

[0039] [ka] (In the formula, R A , R 13 , and R 15 is as described above) 15 ) 3 moieties. Alternatively, each R 15 is R 13 Each R 13 can be methyl.

[0040] Alternatively, in formula (B2-11), one R 12 is R 13 R 12 Two of them are -OSi(R 14 )3. R 12 Two of them are -OSi(R 14 )3, then one R 14 Each -OSi(R 14 )R in 3 13 and R 12 Two of them are -OSiR 13 (R 14 )2. Alternatively, -OSiR 13 (R 14 )2 in each R 14 is a branched polyorganosiloxane oligomer having the following structure (B2-11d):

[0041] [ka] (In the formula, R A , R 13 , and R 15 is as described above) 15 ) 3. Alternatively, each R 15is R 13 Each R 13 can be methyl. Alternatively, the vinyl functional branched polyorganosiloxane can have 3 to 16 silicon atoms per molecule, alternatively 4 to 16 silicon atoms per molecule, alternatively 4 to 10 silicon atoms per molecule. Examples of vinyl functional branched polyorganosiloxane oligomers include those having the formula:

[0042] [ka] vinyl-tris(trimethylsiloxy)silane having the formula formula

[0043] [ka] Methyl-vinyl-di((1,1,1,3,5,5,5-heptamethyltrisiloxane-3-yl)oxy)-silane having the formula formula

[0044] [ka] The branched vinyl-functional polyorganosiloxane oligomers can be prepared by known methods such as those disclosed in "Testing the Functional Tolerance of the Piers-Rubinsztajn Reaction: A new Strategy for Functional Silicones" by Grande et al., Supplementary Material (ESI) for Chemical Communications, copyright The Royal Society of Chemistry 2010.

[0045] Alternatively, the vinyl-functional polyorganosiloxane (B2) may be branched, such as the branched oligomers described above, and / or branched vinyl-functional polyorganosiloxanes that may have, for example, more vinyl groups and / or more polymer units per molecule than the branched oligomers described above (e.g., in formula (B2-1), the quantity (a+b+c+d+e+f+g)>50). The branched vinyl-functional polyorganosiloxane may have a quantity (e+f+g) sufficient to provide the branched vinyl-functional polyorganosiloxane (in formula (B2-1)) with >0-5 mol% trifunctional and / or tetrafunctional units.

[0046] For example, the branched vinyl-functional polyorganosiloxane may be represented by the unit formula (B2-13): (R 4 3SiO 1 / 2 ) q (R 4 2R A SiO 1 / 2 ) r (R 4 2SiO 2 / 2 ) s (SiO 4 / 2 ) t In one embodiment, the branched polyorganosiloxane may be of the formula: 4 and R A is as above, and the subscripts q, r, s, and t have average values ​​such that 2≧q≧0, 4≧r≧0, 995≧s≧4, t=1, (q+r)=4, and (q+r+s+t) has a value sufficient to impart to the branched polyorganosiloxane a viscosity of >170 mPa·s as measured by a rotational viscometer (described below along with the test method). Alternatively, the viscosity may be >170 mPa·s to 1000 mPa·s, alternatively >170 mPa·s to 500 mPa·s, alternatively 180 mPa·s to 450 mPa·s, alternatively 190 mPa·s to 420 mPa·s. Q-type branched polyorganosiloxanes suitable for the starting material (B2-12) are known in the art and can be made by known methods, exemplified by those disclosed in U.S. Pat. No. 6,806,339 to Cray et al. and U.S. Patent Application Publication No. 2007 / 0289495 to Cray et al.

[0047] Alternatively, the branched vinyl-functional polyorganosiloxane may be represented by the formula (B2-14): [R A R 4 2Si-(O-SiR 4 2) x -O] (4-w) -Si-[O-(R 4 2SiO) v SiR 4 3] w wherein R A and R 4 is as above, and the subscripts v, w, and x have values ​​such that 200 ≧ v ≧ 1, 2 ≧ w ≧ 0, and 200 ≧ x ≧ 1. Alternatively, in this formula (B2-14), each R 4 is independently selected from the group consisting of methyl and phenyl. Suitable branched polyorganosiloxanes for starting material (B2-14) can be prepared by known methods such as by heating a mixture containing a polyorganosilicate resin and a cyclic or linear polydiorganosiloxane in the presence of a catalyst such as an acid or a phosphazene base, followed by neutralization of the catalyst.

[0048] Alternatively, the branched vinyl-functional polyorganosiloxane for the starting material (B2-11) may have the unit formula (B2-15): (R 4 3SiO 1 / 2 ) aa (R A R 4 2SiO 1 / 2 ) bb (R 4 2SiO 2 / 2 ) cc (R A R 4 SiO 2 / 2 ) ee (R 4 SiO 3 / 2 ) dd In the formula, R 4 and R Ais as above, with subscript aa≧0, subscript bb>0, subscript cc is from 15 to 995, subscript dd>0, and subscript ee≧0. Subscript aa may be from 0 to 10. Alternatively, subscript aa may have a value such that 12≧aa≧0, alternatively 10≧aa≧0, alternatively 7≧aa≧0, alternatively 5≧aa≧0, alternatively 3≧aa≧0. Alternatively, subscript bb≧1. Alternatively, subscript bb≧3. Alternatively, subscript bb may have a value such that 12≧bb>0, alternatively 12≧bb≧3, alternatively 10≧bb>0, alternatively 7≧bb>1, alternatively 5≧bb≧2, alternatively 7≧bb≧3. Alternatively, the subscript cc may have a value such that 800≧cc≧15, alternatively 400≧cc≧15. Alternatively, the subscript ee may have a value such that 800≧ee≧0, 800≧ee≧15, alternatively 400≧ee≧15. Alternatively, the subscript ee may be 0. Alternatively, the quantity (cc+ee) may have a value such that 995≧(cc+ee)≧15. Alternatively, the subscript dd≧1. Alternatively, the subscript dd may be 1 to 10. Alternatively, the subscript dd may have a value such that 10≧dd>0, alternatively 5≧dd>0, alternatively dd=1. Alternatively, the subscript dd may be 1 to 10, alternatively the subscript dd may be 1 or 2. Alternatively, when subscript dd=1, subscript bb can be 3 and subscript cc can be 0. The value of subscript bb can be sufficient to provide a silsesquioxane of formula (B2-15) having a vinyl content of 0.1% to 1%, alternatively 0.2% to 0.6%, based on the weight of the silsesquioxane. Suitable T-branched polyorganosiloxanes (silsesquioxanes) for the starting material (B2-15) are exemplified by those disclosed in U.S. Patent No. 4,374,967 to Brown et al., U.S. Patent No. 6,001,943 to Enami et al., U.S. Patent No. 8,546,508 to Nabeta et al., and U.S. Patent No. 10,155,852 to Enami.

[0049] Alternatively, the vinyl-functional polyorganosiloxane (B2) is represented by the formula R M 3SiO 1 / 2 and monofunctional units ("M" units) of formula SiO 4 / 2 wherein each R M are independently selected monovalent hydrocarbon radicals, and each R M are independently R as above 4 and R A Alternatively, each R may be selected from the group consisting of M may be selected from the group consisting of alkyl, vinyl, and aryl. Alternatively, each R M may be selected from methyl, vinyl, and phenyl. Alternatively, R M At least one third, alternatively at least two thirds, of the groups are methyl groups. Alternatively, the M units are (MeSiO 1 / 2 ), (Me2PhSiO 1 / 2 ), and (Me2ViSiO 1 / 2 The polyorganosilicate resins are soluble in solvents such as those described herein as starting material (D), exemplified by liquid hydrocarbons such as benzene, ethylbenzene, toluene, xylene, and heptane, or in liquid non-functional organosilicon compounds such as low viscosity linear and cyclic polydiorganosiloxanes.

[0050] When prepared, the polyorganosilicate resin contains the M and Q units described above, and the polyorganosiloxane contains silicon-bonded hydroxyl groups, and / or the moieties (ZO) described above. 1 / 2 ) and further comprising units having hydrolyzable groups represented by the formula Si(OSiR M 3) may contain 4 neopentamers, where R M is as described above, for example, neopentamer can be tetrakis(trimethylsiloxy)silane. 29 Si NMR and 13C NMR spectroscopy can be used to measure the hydroxyl and alkoxy content, as well as the molar ratio of M and Q units, expressed as {M(resin)} / {Q(resin)}, excluding the M and Q units from the neopentamer. The M / Q ratio represents the molar ratio of the total number of triorganosiloxy groups (M units) in the resinous portion of the polyorganosilicate resin to the total number of silicate groups (Q units) in the resinous portion. The M:Q ratio can be from 0.5 / 1 to 1.5 / 1, alternatively from 0.6 / 1 to 0.9 / 1.

[0051] The Mn of the polyorganosilicate resin is determined by the R M The Mn of the polyorganosilicate resins varies depending on various factors such as the type of hydrocarbon group represented by Mn=Mn+Hn. The Mn of the polyorganosilicate resins refers to the number average molecular weight measured using GPC when the peak representing the neopentamer is excluded from the measurement. The Mn of the polyorganosilicate resins may be 1,500 Da to 30,000 Da, alternatively 1,500 Da to 15,000 Da, alternatively >3,000 Da to 8,000 Da. Alternatively, the Mn of the polyorganosilicate resins may be 3,500 Da to 8,000 Da.

[0052] U.S. Patent No. 8,580,073, column 3, line 5 to column 4, line 31, and U.S. Patent Application Publication No. 2016 / 0376482, paragraphs

[0023] to

[0026] , are incorporated herein by reference to disclose MQ resins, which are suitable polyorganosilicate resins for use as starting material (B2). The polyorganosilicate resins can be prepared by any suitable method, such as cohydrolysis of the corresponding silanes or a silica hydrosol capping method. The polyorganosilicate resins can be prepared by a silica hydrogel capping process, such as those disclosed in U.S. Patent No. 2,676,182 to Daudt et al., U.S. Patent No. 4,611,042 to Rivers-Farrell et al., and U.S. Patent No. 4,774,310 to Butler et al. The method of Daudt et al., supra, involves reacting a silica hydrosol with a hydrolyzable triorganosilane, such as trimethylchlorosilane, a siloxane, such as hexamethyldisiloxane, or mixtures thereof, under acidic conditions, and recovering a copolymer having M and Q units. The resulting copolymer generally contains 2-5 weight percent hydroxyl groups.

[0053] The intermediates used to prepare the polyorganosilicate resins can be triorganosilanes and silanes or alkali metal silicates containing four hydrolyzable substituents. The triorganosilanes are represented by the formula R M 3SiX, where R M is as above, and X represents a hydroxyl group or a hydrolyzable substituent, for example of the formula OZ above. A silane having four hydrolyzable substituents has the formula SiX ’ 4, wherein each X ’ is independently selected from the group consisting of halogen, alkoxy, and hydroxyl. Suitable alkali metal silicates include sodium silicate.

[0054] The polyorganosilicate resins prepared as described above typically have the formula, for example, HOSiO 3 / 2of silicon-bonded hydroxyl groups. The polyorganosilicate resin may contain up to 3.5% silicon-bonded hydroxyl groups as measured by FTIR spectroscopy and / or NMR spectroscopy as described above. In certain applications, it may be desirable for the amount of silicon-bonded hydroxyl groups to be less than 0.7%, alternatively less than 0.3%, alternatively less than 1%, alternatively between 0.3% and 0.8%. The silicon-bonded hydroxyl groups formed during the preparation of the polyorganosilicate resin can be converted to trihydrocarbon siloxane groups or different hydrolyzable groups by reacting the silicone resin with a silane, disiloxane or disilazane containing the appropriate end group. The silane containing the hydrolyzable group can be added in a molar excess over the amount required to react with the silicon-bonded hydroxyl groups in the polyorganosilicate resin.

[0055] Alternatively, the polyorganosilicate resin has no more than 2%, alternatively no more than 0.7%, alternatively no more than 0.3%, alternatively between 0.3% and 0.8% hydroxyl groups, e.g., of the formula XSiO 3 / 2 wherein R M is as above, and X represents a hydrolyzable substituent, such as OH. The concentration of silanol groups (wherein X=OH) present in the polyorganosilicate resin can be determined using FTIR spectroscopy and / or NMR, as described above.

[0056] For use herein, polyorganosilicate resins further comprise one or more vinyl groups per molecule. Polyorganosilicate resins having vinyl groups can be prepared by reacting the product of Daudt et al. with a vinyl-containing endblocking agent and an endblocking agent free of aliphatic unsaturation in an amount sufficient to provide 3 to 30 mole percent vinyl groups in the final product. Examples of endblocking agents include, but are not limited to, silazanes, siloxanes, and silanes. Suitable endblocking agents are known in the art and are exemplified in U.S. Pat. Nos. 4,584,355 to Blizzard et al., 4,591,622 to Blizzard et al., and 4,585,836 to Homan et al. A single endblocking agent or a mixture of such agents can be used to prepare such resins.

[0057] Alternatively, the polyorganosilicate resin may be represented by the unit formula (B2-17): (R 4 3SiO 1 / 2 ) mm (R 4 2R A SiO 1 / 2 ) nn (SiO 4 / 2 ) oo (ZO 1 / 2 ) h wherein Z, R 4 , and R A , and subscript h are as above, and the subscripts mm, nn, and oo have average values ​​such that mm≧0, nn>0, oo>0, and 0.5≦(mm+nn) / oo≦4. Alternatively, 0.6≦(mm+nn) / oo≦4, alternatively, 0.7≦(mm+nn) / oo≦4, alternatively, 0.8≦(mm+nn) / oo≦4.

[0058] Alternatively, the vinyl-functional polyorganosiloxane (B2) may be a vinyl-functional silsesquioxane resin (B2-18), i.e., a polyorganosiloxane having the unit formula: (R 4 3SiO 1 / 2 ) a (R 4 2R A SiO 1 / 2 ) b(R 4 2SiO 2 / 2 ) c (R 4 R A SiO 2 / 2 ) d (R 4 SiO 3 / 2 ) e (R A SiO 3 / 2 ) f (ZO 1 / 2 ) h may contain a resin containing trifunctional (T) units, where R 4 and R A are as defined above, subscript f > 1, 2 < (e + f) < 10,000, 0 < (a + b) / (e + f) < 3, 0 < (c + d) / (e + f) < 3, and 0 < h / (e + f) < 1.5. Alternatively, the vinyl-functional silsesquioxane resin may contain the unit formula (B2-19): (R 4 SiO 3 / 2 ) e (R A SiO 3 / 2 ) f (ZO 1 / 2 ) h where R 4 , R A , Z, and subscripts h, e, and f are as defined above. Alternatively, in addition to the above T units, the vinyl-functional silsesquioxane resin may further contain bifunctional (D) units of the formula R 4 2SiO 2 / 2 ) c (R 4 R A SiO 2 / 2 ) d , i.e., a DT resin, where subscripts c and d are as defined above. Alternatively, the vinyl-functional silsesquioxane resin may further contain monofunctional (M) units of the formula (R 4 3SiO 1 / 2 ) a (R 4 2R A SiO 1 / 2 ) b , i.e., an MDT resin, where subscripts a and b are as defined above for the unit formula (B2-1).

[0059] Vinyl-functional silsesquioxane resins are commercially available, for example, as follows: 1 / 2 ) 25 (PhSiO 3 / 2 ) 75 RMS-310, which contains DSC, is commercially available. Vinyl-functional silsesquioxane resins can be produced by hydrolysis and condensation of trialkoxysilanes or mixtures using methods such as those described in Noll, "Chemistry and Technology of Silicone," Academic Press (1968), Chapter 5, pages 190-245. Alternatively, vinyl-functional silsesquioxane resins can be produced by hydrolysis and condensation of trichlorosilanes using methods described in U.S. Pat. No. 6,281,285 to Becker et al. and U.S. Pat. No. 5,010,159 to Bank et al. Vinyl-functional silsesquioxane resins containing D units can be prepared by known methods such as those disclosed in U.S. Patent Application No. 2020 / 0140619 and WO 2018 / 204068 to Swier et al.

[0060] Alternatively, the vinyl-functional organosilicon compound starting material (B) may include (B3) a vinyl-functional silazane. The vinyl-functional silazane has the formula (B3-1): [(R 1 (3-gg) R A gg Si) ff NH (3-ff) ] hh wherein R A is as above, and each R 1 is independently selected from the group consisting of alkyl groups and aryl groups; each subscript ff is independently 1 or 2; each subscript gg is independently 0, 1, or 2; <hh<10である。R 1 For the alkyl and aryl groups, R 4The alkyl group and aryl group can be as described above. Alternatively, the subscript hh can have a value such that 1 < hh < 6. Examples of vinyl-functional silazanes include MePhViSiNH2, Me2ViSiNH2, (ViMe2Si)2NH, and (MePhViSi)2NH. Vinyl-functional silazanes can be prepared by known methods, for example, reacting a vinyl-functional halosilane with ammonia under anhydrous or substantially anhydrous conditions, and then distilling the resulting reaction mixture to separate the cyclic vinyl-functional silazane and the linear vinyl-functional silazane, which are disclosed in, for example, Haber U.S. Patent No. 2,462,635, Martellock U.S. Patent No. 3,243,404, and Dziark International Publication No. 83 / 02948. Suitable vinyl-functional silazanes are commercially available. For example, 2,4,6-trimethyl-2,4,6-trivinylcyclotrisilazane (MeViSiNH)3 is available from Sigma-Aldrich (St. Louis, MO, USA), sym-tetramethyldivinyldisilazane (ViMe2Si)2NH is available from Alfa Aesar, and 1,3-divinyl-1,3-diphenyl-1,3-dimethyldisilazane (MePhViSi)2NH is available from Gelest, Inc. (Morrisville, Pennsylvania, USA).

[0061] The starting material (B) can be any one of the above vinyl-functional organosilicon compounds. Alternatively, the starting material (B) can contain a mixture of two or more of the vinyl-functional organosilicon compounds.

[0062] (C) Hydroformylation reaction catalyst The hydroformylation catalyst starting material (C) for use herein comprises an active complex of rhodium and a ligand. The ligand may be symmetric or asymmetric. Alternatively, the ligand may be symmetric. The ligand may comprise a bisphosphoramidite ligand, or may be a bisphosphoramidite ligand. Alternatively, the ligand may comprise a tetraphosphoramidite ligand, or may be a tetraphosphoramidite ligand. Alternatively, the ligand may comprise a phosphine amine ligand, or may be a phosphine amine ligand. Alternatively, the ligand may comprise a phosphine ligand, or may be a phosphine ligand. Alternatively, the hydroformylation catalyst starting material (C) may comprise a combination of rhodium / ligand complexes comprising different types of ligands.

[0063] The ligand has the formula (C1), (C2), and / or (C3): Formula (C1) is

[0064] [ka] and Formula (C2) is

[0065] [ka] and Formula (C3) is

[0066] [ka] and In the formula, R 101 ~R 122 are each independently selected from hydrogen, a hydrocarbyl group, a heteroaryl group, a halogen atom, or a heterocarbyl group; R 101 ~R 122 two or more of X may optionally be joined together to provide one or more cyclic moieties; 1~X 4 is independently selected from O, CH, NH, NR, NSO2R, or NSO2A, where each R is an independently selected substituted or unsubstituted alkyl or aryl group, each A is an independently selected aryl or heteroaryl group, and Y 1 ~Y 8 each is an independently selected nitrogen-containing heterocyclic moiety bonded to P through N, wherein each heterocyclic moiety is optionally substituted with one or more groups or atoms selected from alkyl, aryl, heteroaryl, alkoxy, acyl, carboxyl, carboxylate, cyano, -SOH, sulfonate, amino, trifluoromethyl, and halogen.

[0067] The ligand may have the formula (C1): Alternatively, the ligand may have the formula (C2): Alternatively, the ligand may have the formula (C3):

[0068] R 101 ~R 122Suitable hydrocarbyl groups of may be independently linear, branched, cyclic, or combinations thereof. Cyclic hydrocarbyl groups include aryl groups, and saturated or non-conjugated cyclic groups. Cyclic hydrocarbyl groups may be monocyclic or polycyclic. Linear and branched hydrocarbyl groups may be independently saturated or unsaturated. An example of a combination of linear and cyclic hydrocarbyl groups is an aralkyl group. "Substituted" means that one or more hydrogen atoms may be replaced by an atom other than hydrogen (e.g., a halogen atom such as chlorine, fluorine, or bromine). Suitable alkyl groups are exemplified by, but are not limited to, methyl, ethyl, propyl (e.g., iso-propyl and / or n-propyl), butyl (e.g., isobutyl, n-butyl, tert-butyl, and / or sec-butyl), pentyl (e.g., isopentyl, neopentyl, and / or tert-pentyl), hexyl, and branched saturated hydrocarbon groups of 6 carbon atoms. Suitable aryl groups are exemplified by, but are not limited to, phenyl, tolyl, xylyl, naphthyl, benzyl, and dimethylphenyl. Suitable alkenyl groups include vinyl, allyl, propenyl, isopropenyl, butenyl, isobutenyl, pentenyl, heptenyl, hexenyl, and cyclohexenyl. Suitable monovalent halogenated hydrocarbon groups include, but are not limited to, halogenated alkyl groups having 1-6 carbon atoms or halogenated aryl groups having 6-10 carbon atoms. Suitable halogenated alkyl groups are exemplified by, but are not limited to, the above-mentioned alkyl groups in which one or more hydrogen atoms are replaced with a halogen atom such as F or Cl.For example, fluoromethyl, 2-fluoropropyl, 3,3,3-trifluoropropyl, 4,4,4-trifluorobutyl, 4,4,4,3,3-pentafluorobutyl, 5,5,5,4,4,3,3-heptafluoropentyl, 6,6,6,5,5,4,4,3,3-nonafluorohexyl, and 8,8,8,7,7-pentafluorooctyl, 2,2-difluorocyclopropyl, 2,3-difluorocyclobutyl, 3,4-difluorocyclohexyl, and 3,4-difluoro-5-methylcycloheptyl, chloromethyl, chloropropyl, 2-dichlorocyclopropyl, and 2,3-dichlorocyclopentyl are examples of suitable halogenated alkyl groups.Suitable halogenated aryl groups are exemplified by, but not limited to, the above-mentioned aryl groups in which one or more hydrogen atoms are replaced with halogen atoms such as F or Cl.For example, chlorobenzyl and fluorobenzyl are suitable halogenated aryl groups. Suitable heterocarbyl groups include any of the hydrocarbyl groups described above, but containing one or more heteroatoms such as oxygen, sulfur, or nitrogen. Suitable halogen atoms include F, Cl, Br, I, At, and Ts, alternatively F, Cl, and Br, alternatively Cl.

[0069] As mentioned above, R 101 ~R 122 Two or more of R may optionally be joined together to provide one or more cyclic moieties. 101 ~R 122 The cyclic moiety formed by any combination of may be aliphatic or aromatic and may be monocyclic, bicyclic, or polycyclic.

[0070] For example, when the ligand has the formula (C1), R 101 , R 102 , R 107 , and R 108 If each is H, then R 103 and R 104 forms an aliphatic ring, and R 105 and R 106 When taken together to form an aliphatic ring, the ligand of formula (C1) has the following formula (C1-1):

[0071] [ka] In the formula, X 1 , X 2 , and Y 1 ~Y 4 is defined above.

[0072] As another example, when the ligand has the formula (C1), R 101 R 102 , R 107 , and R 108 are H, and R 103 and R 104 forms an aromatic ring, and R 105 and R 106 When taken together to form an aromatic ring, the ligand of formula (C1) can be represented by the following formula (C1-2):

[0073] [ka] In the formula, X 1 , X 2 , and Y 1 ~Y 4 is defined above.

[0074] As yet another example, when the ligand has the formula (C1), R 103 , R 104 , R 105 , and R 106 are H, and R 101 and R 102 forms a bicyclic aromatic ring structure, and R 107 and R 108 When taken together to form a bicyclic aromatic structure, the ligand of formula (C1) may be represented by the following formula (C1-3):

[0075] [ka] In the formula, X 1 , X2 , and Y 1 ~Y 4 is defined above.

[0076] X 1 ~X 4 is independently selected from O, CH, NH, NR, NSO2R, or NSO2A, where each R is an independently selected substituted or unsubstituted alkyl or aryl group, and each A is an independently selected aryl or heteroaryl group. 1 ~X 4 Each of may be O.

[0077] Y 1 ~Y 8 Each of Y is an independently selected nitrogen-containing heterocyclic moiety bonded to P through N, where each heterocyclic moiety is optionally substituted with one or more groups or atoms selected from alkyl, aryl, heteroaryl, alkoxy, acyl, carboxyl, carboxylate, cyano, -SOH, sulfonate, amino, trifluoromethyl, and halogen. 1 ~Y 8 Each of may be independently monocyclic, bicyclic, and / or polycyclic. Illustrative examples of nitrogen-containing heterocyclic groups include indole, isoindole, pyrrole, carbazole, and imidazole groups. As noted above, any of the carbon atoms in these groups may be substituted with one or more groups or atoms selected from alkyl, aryl, heteroaryl, alkoxy, acyl, carboxyl, carboxylate, cyano, -SO3H, sulfonate, amino, trifluoromethyl, and halogen. Alternatively, Y 1 ~Y 8 At least one of Y may be substituted with an alkoxy group having 1 to 8 carbon atoms. 1 ~Y 8 At least one of the is substituted with an alkyl group having 1 to 12 carbon atoms, such as a tert-butyl group.

[0078] Alternatively, the ligand may have the formula (C1), where R101 ~R 108 , X 1 ~X 2 , and Y 1 ~Y 4 is selected such that the ligand is a bisphosphoramidite ligand having one of the following formulas (where Me represents methyl and tBu represents t-butyl):

[0079] [ka] 2,2'-Bis((di(1H-indol-1-yl)phosphanyl)oxy)-5,5',6,6',7,7',8,8'-octahydro-1,1'-binaphthalene

[0080] [ka] 2,2'-Bis((bis(6-(4-methoxyphenyl)-1H-indol-1-yl)phosphanyl)oxy)-5,5',6,6',7,7',8,8'-octahydro-1,1'-binaphthalene

[0081] [ka] 2,2'-Bis((bis(6-(4-methoxyphenyl)-1H-indol-1-yl)phosphanyl)oxy)-5,5',6,6',7,7',8,8'-octahydro-1,1'-binaphthalene

[0082] [ka] 2,2'-Bis((bis(6-(3,5-di-tert-butylphenyl)-1H-indol-1-yl)phosphanyl)oxy)-1,1'-binaphthalene

[0083] [ka] 1,1',1'',1'''-(((4,4',5,5',6,6'-hexamethyl-[1,1'-biphenyl]-2,2'-diyl)bis(oxy))bis(phosphantriyl))tetrakis(6-(3,5-di-tert-butylphenyl)-1H-indole), and

[0084] [ka] 2,2'-Bis((bis(6-(3,5-di-tert-butyl-4-methoxyphenyl)-1H-indol-1-yl)phosphanyl)oxy)-5,5',6,6',7,7',8,8'-octahydro-1,1'-binaphthalene A method for preparing the first ligand structure above in this section for formula (C1) is disclosed in U.S. Pat. No. 9,795,952 to Diebolt et al., which is incorporated herein by reference in its entirety.

[0085] Alternatively, the ligand may have the formula (C2), where R 109 ~R 122 , X 1 ~X 2 , and Y 5 ~Y 8 is selected such that the ligand is a bisphosphoramidite ligand having one of the following formulas: (C2-1):

[0086] [ka] 7,7'-bis((bis(6-(3,5-di-tert-butylphenyl)-1H-indol-1-yl)phosphanyl)oxy)-2,2',3,3'-tetrahydro-1,1'-spirobi[indene] and (C2-2):

[0087] [ka] 7,7'-Bis((di(1H-indol-1-yl)phosphanyl)oxy)-2,2',3,3'-tetrahydro-1,1'-spirobi[indene].

[0088] Alternatively, the ligand may have the formula (C3), where R 101 ~R 106 , X 1 ~X 4 , and Y 1 ~Y 8 may be selected such that the ligand is a tetraphosphoramidite ligand having one of the following formulas: (C3-1)

[0089] [ka] (C3-2)

[0090] [ka] Methods for preparing these ligand structures described above in this section for formula (C3) are disclosed in US Pat. No. 7,531,698 to Zhang et al., which is incorporated herein by reference in its entirety.

[0091] The starting material (C), the rhodium / ligand complex catalyst, may be prepared by methods known in the art, such as those disclosed in U.S. Patent No. 4,769,498 to Billig et al., column 20, line 50 to column 21, line 40, and U.S. Patent No. 10,023,516 to Brammer et al., column 11, line 35 to column 12, line 12, by varying the appropriate starting materials. For example, the rhodium / ligand complex catalyst may be prepared by a process comprising combining a rhodium precursor with the above-described ligand under conditions to form a complex, which may then be introduced into a hydroformylation reaction medium containing one or both of the above-described starting materials (A) and / or (B). Alternatively, the rhodium / ligand complex catalyst may be formed in situ by introducing a rhodium catalyst precursor to the reaction medium and a ligand to the reaction medium (e.g., before, during, and / or after the introduction of the rhodium catalyst precursor) for in situ formation of the rhodium / ligand complex catalyst. The rhodium / ligand complex catalyst may be activated by heating and / or exposure to starting material (A) to form (C) the rhodium / ligand complex catalyst. The rhodium catalyst precursor may be rhodium dicarbonyl acetylacetonate, Rh2O3, Rh4(CO) 12 , Rh6(CO) 16 Further methods for preparing certain ligands are described herein in the accompanying Examples.

[0092] The rhodium precursor, e.g., rhodium dicarbonyl acetylacetonate, optionally the starting material (D), the solvent, and the ligand may be combined by any convenient means, e.g., by mixing. The resulting rhodium / ligand complex catalyst may be introduced into the reactor, optionally with an excess of the ligand. Alternatively, the rhodium precursor, (D) the solvent, and the ligand may be combined with the starting materials (A) and / or (B), the vinyl-functional organosilicon compound, in the reactor, and the rhodium / ligand complex may be formed in situ. The relative amounts of the ligand and the rhodium precursor are sufficient to provide a molar ratio of ligand / Rh of 10 / 1 to 1 / 1, alternatively 5 / 1 to 1 / 1, alternatively 3 / 1 to 1 / 1, alternatively 2.5 / 1 to 1.5 / 1. In addition to the rhodium / ligand complex catalyst, an excess (e.g., uncomplexed) ligand may be present in the reaction mixture. The excess ligand may be the same as the ligand in the rhodium / ligand complex catalyst, or it may be different.

[0093] The amount of (C) rhodium / ligand complex catalyst (catalyst) is sufficient to catalyze the hydroformylation of (B) vinyl-functional organosilicon compound. The exact amount of (C) rhodium / ligand complex catalyst depends on various factors, including the type of vinyl-functional organosilicon compound selected for starting material (B), its exact vinyl content, and reaction conditions such as temperature and pressure of starting material (A). However, the amount of (C) rhodium / ligand complex catalyst may be sufficient to provide a rhodium metal concentration of at least 0.1 ppm, alternatively 0.15 ppm, alternatively 0.2 ppm, alternatively 0.25 ppm, alternatively 0.5 ppm, based on the weight of (B) vinyl-functional organosilicon compound. At the same time, the amount of (C) rhodium / ligand complex catalyst may be sufficient to provide a rhodium metal concentration of up to 300 ppm, alternatively up to 100 ppm, alternatively up to 20 ppm, alternatively up to 5 ppm, based on the same basis. Alternatively, the amount of (C) catalyst may be sufficient to provide from 0.1 ppm to 300 ppm, alternatively from 0.2 ppm to 100 ppm, alternatively from 0.25 ppm to 20 ppm, alternatively from 0.5 ppm to 5 ppm, based on the weight of the (B) vinyl functional organosilicon compound.

[0094] The hydroformylation process reaction may be carried out without additional solvent. Alternatively, the hydroformylation process reaction may be carried out using a solvent to facilitate mixing and / or feeding of one or more of the above starting materials, such as (C) the rhodium / ligand complex catalyst and / or the vinyl-functional organosilicon compound starting material (B), for example, when a vinyl-functional polyorganosilicate resin is selected for the starting material (B). Solvents are exemplified by aliphatic or aromatic hydrocarbons capable of dissolving the starting materials, such as toluene, xylene, benzene, hexane, heptane, decane, cyclohexane, or combinations of two or more of these. Additional solvents include THF, dibutyl ether, diglyme, and texanol. Without wishing to be bound by theory, it is believed that a solvent may be used to reduce the viscosity of the starting materials. The amount of solvent is not critical, but if present, the amount of solvent may be 5% to 70% based on the weight of the vinyl-functional organosilicon compound starting material (B).

[0095] In the hydroformylation process described herein, the hydroformylation reaction of step 1) is carried out at a relatively low temperature. For example, step 1) can be carried out at a temperature of at least 30°C, alternatively at least 50°C, alternatively at least 70°C. At the same time, the temperature in step 1) can be up to 150°C, alternatively up to 100°C, alternatively up to 90°C, alternatively up to 80°C. Without wishing to be bound by theory, it is believed that lower temperatures, for example, 30°C to 90°C, alternatively 40°C to 90°C, alternatively 50°C to 90°C, alternatively 60°C to 90°C, alternatively 70°C to 90°C, alternatively 80°C to 90°C, alternatively 30°C to 60°C, alternatively 50°C to 60°C, may be desirable to obtain high selectivity and ligand stability.

[0096] In the hydroformylation process described herein, step 1) may be carried out at a pressure of at least 101 kPa (ambient pressure), alternatively at least 206 kPa (30 psi), alternatively at least 344 kPa (50 psi). At the same time, the pressure in step 1) may be up to 6,895 kPa (1,000 psi), alternatively up to 1,379 kPa (200 psi), alternatively up to 1000 kPa (145 psi), alternatively up to 689 kPa (100 psi). Alternatively, step 1) may be carried out at 101 kPa to 6,895 kPa, alternatively from 344 kPa to 1,379 kPa, alternatively from 101 kPa to 1000 kPa, alternatively from 344 kPa to 689 kPa. Without wishing to be bound by theory, it is believed that it may be beneficial to use relatively low pressures in the processes herein, e.g., <-6,895 kPa, and the ligands described herein enable low pressure hydroformylation processes, which have the benefits of lower cost and better safety than high pressure hydroformylation processes.

[0097] The hydroformylation process may be carried out in batch, semi-batch, or continuous mode using one or more suitable reactors, such as fixed bed reactors, fluidized bed reactors, continuous stirred tank reactors (CSTRs), or slurry reactors. (B) The choice of vinyl-functional organosilicon compound, (C) the catalyst, and (D) whether a solvent is used may affect the size and type of reactor used. One reactor, or two or more different reactors may be used. The hydroformylation process may be carried out in one or more steps, which may be influenced by balancing capital costs, achieving high catalyst selectivity, activity, life, and ease of operation, as well as the reactivity of the particular starting materials and the reaction conditions selected, and the products desired.

[0098] Alternatively, the hydroformylation process can be carried out in a continuous manner. For example, the process used can be as described in U.S. Patent No. 10,023,516, except that the olefin feed stream and catalyst described therein are replaced with (B) the vinyl-functional organosilicon compound and (C) the rhodium / ligand complex catalyst described herein, respectively.

[0099] Step 1) of the hydroformylation process forms a hydroformylation reaction product comprising a propyl aldehyde functional organosilicon compound. The hydroformylation reaction product may further include additional materials, such as those intentionally used during step 1) of the process or those formed in situ. Examples of such materials that may also be present include unreacted (B) vinyl functional organosilicon compound, unreacted (A) carbon monoxide and hydrogen gas, and / or by-products formed in situ, such as ligand decomposition products and their adducts, and high boiling liquid aldehyde condensation by-products, and (D) solvent, if used. The term "ligand decomposition products" includes, but is not limited to, any and all compounds resulting from one or more chemical transformations of at least one of the ligand molecules used in the process.

[0100] The process may further include one or more additional steps, such as 2) recovering (C) the rhodium / ligand complex catalyst from the reaction fluid containing the propylaldehyde-functional organosilicon compound. Recovering (C) the rhodium / ligand complex catalyst may be carried out by methods known in the art, including, but not limited to, adsorption and / or membrane separation (e.g., nanofiltration). Suitable recovery methods are described, for example, in U.S. Patent No. 5,681,473 to Miller et al., U.S. Patent No. 8,748,643 to Priske et al., and U.S. Patent No. 10,155,200 to Geilen et al.

[0101] However, one benefit of the process described herein is that there is no need to remove and reuse (C) catalyst.Due to the low level of Rh required, it may be more cost-effective not to recover and reuse (C) catalyst, and the propyl aldehyde-functional organosilicon compound produced by the process may be stable even if catalyst is not removed.Therefore, alternatively, the above process may be carried out without step 2).

[0102] Alternatively, the process may further include 3) purification of the hydroformylation reaction product. For example, the propylaldehyde-functional organosilicon compound may be isolated from the additional materials described above by any convenient means, such as stripping and / or distillation, optionally using reduced pressure.

[0103] Propylaldehyde-functional organosilicon compounds The above-mentioned propylaldehyde-functional organosilicon compounds are useful as starting materials in the process for preparing propylimine-functional organosilicon compounds and aminopropyl-functional organosilicon compounds. The starting material (E) is a propylaldehyde-functional organosilicon compound having at least one propylaldehyde functional group covalently bonded to silicon per molecule. Alternatively, the propylaldehyde-functional organosilicon compound may have two or more propylaldehyde functional groups covalently bonded to silicon per molecule. The propylaldehyde functional group covalently bonded to silicon is represented by the formula:

[0104] [ka] where G has the empirical formula -C2H4-. G may be linear (-CH2CH-) or branched.

[0105] [ka] Alternatively, the propylaldehyde-functional organosilicon compound may be a combination of propylaldehyde-functional organosilicon compounds, with some instances of the group G being linear and some being branched. Alternatively, the propylaldehyde-functional organosilicon compound produced by the above hydroformylation process may have most instances of G being linear. The propylaldehyde-functional organosilicon compound may be one propylaldehyde-functional organosilicon compound. Alternatively, two or more different propylaldehyde-functional organosilicon compounds may be used in the process described herein. For example, the propylaldehyde-functional organosilicon compound may include one or both of a propylaldehyde-functional silane and a propylaldehyde-functional polyorganosiloxane.

[0106] The propylaldehyde-functional organosilicon compound is represented by the formula (E1) (E1-1): Ald x SiR 4 (4-x) wherein each R Ald are independently selected expressions

[0107] [ka] where G is as defined above and R 4 and the subscript x is as defined above. Alternatively, each R 4 may be independently selected from the group consisting of alkyl groups of 1 to 18 carbon atoms, and aryl groups of 6 to 18 carbon atoms. Alternatively, the subscript x may be 1 to 4.

[0108] Suitable propylaldehyde-functional silanes are exemplified by propylaldehyde-functional trialkylsilanes such as (propyl-aldehyde)-trimethylsilane and (propyl-aldehyde)-triethylsilane.

[0109] Alternatively, the propylaldehyde-functional organosilicon compound may comprise (E2) a propylaldehyde-functional polyorganosiloxane. The propylaldehyde-functional polyorganosiloxane may be cyclic, linear, branched, resinous, or a combination of two or more thereof. The propylaldehyde-functional polyorganosiloxane may have a unit formula (E2-1): (R 4 3SiO 1 / 2 ) a (R 4 2R Ald SiO 1 / 2 ) b (R 4 2SiO 2 / 2 ) c (R 4 R Ald SiO 2 / 2 ) d (R 4 SiO 3 / 2 ) e (R Ald SiO 3 / 2 ) f (SiO 4 / 2 ) g (ZO 1 / 2 ) h wherein each R Ald is the formula above.

[0110] [ka] and G, R are independently selected propylaldehyde groups. 4 , Z, and subscripts a, b, c, d, e, f, g, and h are as defined above.

[0111] Alternatively, the (E2) propylaldehyde-functional polyorganosiloxane may comprise (E2-2) a linear polydiorganosiloxane having at least one propylaldehyde functional group per molecule, or alternatively at least two propylaldehyde functional groups (e.g., when subscripts e=f=g=0 in formula (E2-1) for the propylaldehyde-functional polyorganosiloxane above). For example, the polydiorganosiloxane may have a unit formula (E2-3): (R4 3SiO 1 / 2 ) a (R Ald R 4 2SiO 1 / 2 ) b (R 4 2SiO 2 / 2 ) c (R Ald R 4 SiO 2 / 2 ) d wherein R Ald and R 4 is as above, subscript a is 0, 1 or 2, subscript b is 0, 1 or 2, subscript c is 0 or more, and subscript d is 0 or more, with the proviso that the quantity (b+d) is 1 or more, the quantity (a+b) is 2, and the quantity (a+b+c+d) is 2 or more. Alternatively, in the above unit formula (E2-3) for the linear propylaldehyde-functional polyorganosiloxane, the quantity (a+b+c+d) can be at least 3, alternatively at least 4, alternatively >50. At the same time, in the formula, the quantity (a+b+c+d) can be 10,000 or less, alternatively 4,000 or less, alternatively 2,000 or less, alternatively 1,000 or less, alternatively 500 or less, alternatively 250 or less. Alternatively, in the unit formula for the linear propylaldehyde-functional polyorganosiloxane, each R 4 may be independently selected from the group consisting of alkyl and aryl, alternatively, methyl and phenyl. Alternatively, each R 4 can be an alkyl group, alternatively, each R 4 can be methyl.

[0112] Alternatively, the linear propylaldehyde-functional polydiorganosiloxane of the unit formula (E2-3) may be represented by the unit formula (E2-4): (R 4 2R Ald SiO 1 / 2 )2(R 4 2SiO 2 / 2 ) m (R 4 R Ald SiO 2 / 2 ) n , Unit formula (E2-5): (R 4 3SiO1 / 2 )2(R 4 2SiO 2 / 2 ) o (R 4 R Ald SiO 2 / 2 ) p or a combination of both (E2-4) and (E2-5).

[0113] In formulae (E2-4) and (E2-5), each R 4 and R Ald are as above. Subscript m may be 0 or a positive number. Alternatively, subscript m may be at least 2. Alternatively, subscript m may be from 2 to 2,000. Subscript n may be 0 or a positive number. Alternatively, subscript n may be from 0 to 2000. Subscript o may be 0 or a positive number. Alternatively, subscript o may be from 0 to 2000. Subscript p is at least 2. Alternatively, subscript p may be from 2 to 2000.

[0114] The starting material (E2) is i) bis-dimethyl(propyl-aldehyde)siloxy terminated polydimethylsiloxane, ii) bis-dimethyl(propyl-aldehyde)siloxy terminated poly(dimethylsiloxane / methyl(propyl-aldehyde)siloxane), iii) bis-dimethyl(propyl-aldehyde)siloxy terminated polymethyl(propyl-aldehyde)siloxane, iv) bis-trimethylsiloxane terminated poly(dimethylsiloxane / methyl(propyl-aldehyde)siloxane), v) bis-trimethylsiloxane terminated polymethyl(propyl-aldehyde)siloxane, vi) bis-dimethyl(propyl- The polydiorganosiloxanes may include propylaldehyde functional polydiorganosiloxanes such as bis-dimethyl(propyl-aldehyde)siloxy terminated poly(dimethylsiloxane / methylphenylsiloxane / methyl(propyl-aldehyde)siloxane), vii) bis-dimethyl(propyl-aldehyde)siloxy terminated poly(dimethylsiloxane / methylphenylsiloxane), viii) bis-dimethyl(propyl-aldehyde)siloxy terminated poly(dimethylsiloxane / diphenylsiloxane), ix) bis-phenyl,methyl,(propyl-aldehyde)-siloxy terminated polydimethylsiloxane, and x) combinations of two or more of i)-ix).

[0115] Alternatively, (E2) the propylaldehyde-functional polyorganosiloxane may be cyclic, for example, in the unit formula (E2-1), the subscripts a=b=c=e=f=g=h=0. (E2-6) The cyclic propylaldehyde-functional polydiorganosiloxane may be represented by the unit formula (E2-7): (R 4 R Ald SiO 2 / 2 ) d wherein R Ald and R 4is as above, and subscript d can be 3 to 12, alternatively 3 to 6, alternatively 4 to 5. Examples of cyclic propylaldehyde functional polydiorganosiloxanes include 2,4,6-trimethyl-2,4,6-tri(propyl-aldehyde)-cyclotrisiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetra(propyl-aldehyde)-cyclotetrasiloxane, 2,4,6,8,10-pentamethyl-2,4,6,8,10-penta(propyl-aldehyde)-cyclopentasiloxane, and 2,4,6,8,10,12-hexamethyl-2,4,6,8,10,12-hexa(propyl-aldehyde)-cyclohexasiloxane.

[0116] Alternatively, the (E2-6) cyclic propylaldehyde-functional polydiorganosiloxane may be represented by the unit formula (E2-8): (R 4 2SiO 2 / 2 ) c (R 4 R Ald SiO 2 / 2 ) d wherein R 4 and R Ald is as above, where subscript c is >0 to 6, and subscript d is 3 to 12. Alternatively, in formula (E2-8), the quantity (c+d) can be 3 to 12. Alternatively, in formula (E2-8), c can be 3 to 6, and d can be 3 to 6.

[0117] Alternatively, (E2) the propylaldehyde-functional polyorganosiloxane may be an (E2-9) oligomer, for example, where the quantity (a+b+c+d+e+f+g) in the above unit formula (E2-1) is ≦50, alternatively ≦40, alternatively ≦30, alternatively ≦25, alternatively ≦20, alternatively ≦10, alternatively ≦5, alternatively ≦4, alternatively ≦3. The oligomer may be cyclic, linear, branched, or a combination thereof. The cyclic oligomer is as described above as the starting material (E2-6).

[0118] An example of a linear propylaldehyde functional polyorganosiloxane oligomer is represented by the formula (E2-10):

[0119] [ka] wherein R 4 is as above, and each R 2’ are independently 4 and R Ald with the proviso that at least one R 2’ But R Ald with the proviso that the subscript z is 0 to 48. Alternatively, the subscript z can be 0 to 4, alternatively 0 to 1, alternatively 0. Alternatively, when z=0 in formula (E2-10), the propylaldehyde-functional polyorganosiloxane oligomer has the formula (E2-10a):

[0120] [ka] wherein R 4 and R Ald Examples of linear propylaldehyde-functional polyorganosiloxane oligomers include 1,3-di(propyl-aldehyde)-1,1,3,3-tetramethyldisiloxane, 1,1,1,3,3-pentamethyl-3-(propyl-aldehyde)-disiloxane, and 1,1,1,3,5,5,5-heptamethyl-3-(propyl-aldehyde)-trisiloxane.

[0121] Alternatively, the propylaldehyde-functional polyorganosiloxane oligomer can be branched. The branched oligomer has the general formula (E2-11): R Ald SiR 12 3, where R Ald is as above, and each R 12 is R 13 and -OSi(R 14 ) 3, each R 13 is a monovalent hydrocarbon group, and each R 14 is R 13, -OSi(R 15 )3, and -[OSiR 13 2] ii OSiR 13 3 are selected, and each R 15 is R 13 , -OSi(R 16 )3, and -[OSiR 13 2] ii OSiR 13 3 are selected, and each R 16 is R 13 and -[OSiR 13 2] ii OSiR 13 3, where the subscript ii has a value such that 0≦ii≦100. 12 At least two of -OSi(R 14 ) 3. Alternatively, R 12 All three of the -OSi(R 14 )3.

[0122] Alternatively, in formula (E2-11), each R 12 R 13 In the case where

[0123] [ka] In the formula, R Ald and R 13 is as defined above. Alternatively, in formula (E2-11a), each R 13 can be methyl.

[0124] Alternatively, in formula (E2-11), each R 12 -OSi(R 14 )3, then each R 14 is -OSi(R ) such that the branched polyorganosiloxane oligomer has the following structure (E2-11b): 15 ) three parts,

[0125] [ka] In the formula, R Ald and R 15 is as described above. Alternatively, each R 15 As above, R 13 Each R 13 can be methyl.

[0126] Alternatively, in formula (E2-11), each R 12 -OSi(R 14 )3, then one R 14 is each R 12 -OSiR 13 (R 14 )2 for each -OSi(R 14 )3 in R 13 Alternatively, -OSiR 13 (R 14 )2 R's 14 each of which is a branched propylaldehyde-functional polyorganosiloxane oligomer having the following structure (E2-11c):

[0127] [ka] -OSi(R 15 ) three parts, In the formula, R Ald , R 13 , and R 15 is as described above. Alternatively, each R 15 is R 13 Each R 13 can be methyl.

[0128] Alternatively, in formula (B2-11), one R 12 is R 13 R 12 Two of them are -OSi(R 14 )3. R 12 Two of them are -OSi(R 14 )3, then one R 14 Each -OSi(R 14)R in 3 13 and R 12 Two of them are -OSiR 13 (R 14 )2. Alternatively, -OSiR 13 (R 14 ) Each R in 2 14 is a branched polyorganosiloxane oligomer having the following structure (E2-11d):

[0129] [ka] (In the formula, R Ald , R 13 , and R 15 is as described above) 15 ) 3. Alternatively, each R 15 is R 13 Each R 13 can be methyl. Alternatively, the propylaldehyde functional branched polyorganosiloxane can have 3 to 16 silicon atoms per molecule, alternatively 4 to 16 silicon atoms per molecule, alternatively 4 to 10 silicon atoms per molecule. Examples of propylaldehyde functional branched polyorganosiloxane oligomers include those having the formula:

[0130] [ka] 3-(3,3,3-trimethyl-1-lambda 2 -disiloxaneyl)propanal (which may also be referred to as propyl-aldehyde-tris(trimethyl)siloxy)silane), of the formula

[0131] [ka] 3-(1,3,5,5,5-pentamethyl-1λ 3 ,3λ 3-trisiloxaneyl)propanal (which may also be referred to as methyl-(propyl-aldehyde)-di((1,1,1,3,5,5,5-heptamethyltrisiloxane-3-yl)oxy)-silane), and formula

[0132] [ka] 3-(3,5,5,5-tetramethyl-1λ 2 ,3λ 3 -trisiloxaneyl)propanal (which may also be referred to as (propyl-aldehyde)-tris((1,1,1,3,5,5,5-heptamethyltrisiloxane-3-yl)oxy)-silane).

[0133] Alternatively, the (E2) propylaldehyde-functional polyorganosiloxane may be branched, such as the branched oligomers described above, and / or branched propylaldehyde-functional polyorganosiloxanes that may have, for example, more propylaldehyde groups and / or more polymer units per molecule than the branched oligomers described above (e.g., in formula (E2-1), the amount (a+b+c+d+e+f+g)>50). The branched propylaldehyde-functional polyorganosiloxane may have an amount (e+f+g) sufficient to provide the branched propylaldehyde-functional polyorganosiloxane (in formula (E2-1)) with >0-5 mol% trifunctional and / or tetrafunctional units.

[0134] For example, the branched propylaldehyde-functional polyorganosiloxane can be represented by the unit formula (E2-13): 4 3SiO 1 / 2 ) q (R 4 2R Ald SiO 1 / 2 ) r (R 4 2SiO 2 / 2 ) s (SiO 4 / 2 ) t In one embodiment, the branched polyorganosiloxane may be of the formula:4 and R Ald is as above, and the subscripts q, r, s, and t have average values ​​such that 2≧q≧0, 4≧r≧0, 995≧s≧4, t=1, (q+r)=4, and (q+r+s+t) has a value sufficient to impart to the branched polyorganosiloxane a viscosity of >170 mPa·s as measured by a rotational viscometer (described below along with the test method). Alternatively, the viscosity may be >170 mPa·s to 1000 mPa·s, alternatively >170 mPa·s to 500 mPa·s, alternatively 180 mPa·s to 450 mPa·s, alternatively 190 mPa·s to 420 mPa·s.

[0135] Alternatively, the branched propylaldehyde-functional polyorganosiloxane may be represented by the formula (E2-14): [R Ald R 4 2Si-(O-SiR 4 2) x -O] (4-w) -Si-[O-(R 4 2SiO) v SiR 4 3] w wherein R Ald and R 4 is as above, and the subscripts v, w, and x have values ​​such that 200≧v≧1, 2≧w≧0, and 200≧x≧1. Alternatively, in this formula (E2-14), each R 4 is independently selected from the group consisting of methyl and phenyl.

[0136] Alternatively, the branched propylaldehyde-functional polyorganosiloxane for the starting material (E2-11) may have the unit formula (E2-15): (R 4 3SiO 1 / 2 ) aa (R Ald R 4 2SiO 1 / 2 ) bb (R 4 2SiO 2 / 2 ) cc (R Ald R 4 SiO 2 / 2 ) ee (R4 SiO 3 / 2 ) dd In the formula, R 4 and R Ald is as above, with subscript aa≧0, subscript bb>0, subscript cc is from 15 to 995, subscript dd>0, and subscript ee≧0. Subscript aa may be from 0 to 10. Alternatively, subscript aa may have a value such that 12≧aa≧0, alternatively 10≧aa≧0, alternatively 7≧aa≧0, alternatively 5≧aa≧0, alternatively 3≧aa≧0. Alternatively, subscript bb≧1. Alternatively, subscript bb≧3. Alternatively, subscript bb may have a value such that 12≧bb>0, alternatively 12≧bb≧3, alternatively 10≧bb>0, alternatively 7≧bb>1, alternatively 5≧bb≧2, alternatively 7≧bb≧3. Alternatively, the subscript cc may have a value such that 800≧cc≧15, alternatively 400≧cc≧15. Alternatively, the subscript ee may have a value such that 800≧ee≧0, 800≧ee≧15, alternatively 400≧ee≧15. Alternatively, the subscript ee may be 0. Alternatively, the quantity (cc+ee) may have a value such that 995≧(cc+ee)≧15. Alternatively, the subscript dd≧1. Alternatively, the subscript dd may be 1 to 10. Alternatively, the subscript dd may have a value such that 10≧dd>0, alternatively 5≧dd>0, alternatively dd=1. Alternatively, the subscript dd may be 1 to 10, alternatively the subscript dd may be 1 or 2. Alternatively, when subscript dd=1, subscript bb can be 3 and subscript cc can be 0. The value of subscript bb can be sufficient to provide a silsesquioxane of unit formula (E2-15) having an aldehyde content of 0.1% to 1%, alternatively 0.2% to 0.6%, based on the weight of the silsesquioxane.

[0137] Alternatively, (E2) the propylaldehyde-functional polyorganosiloxane may comprise a propylaldehyde-functional polyorganosiloxane resin, such as a propylaldehyde-functional polyorganosilicate resin and / or a propylaldehyde-functional silsesquioxane resin. Such resins may be prepared, for example, by hydroformylating a vinyl-functional polyorganosiloxane resin, as described above. The propylaldehyde-functional polyorganosilicate resin may be represented by the formula R M’ 3SiO 1 / 2 and monofunctional units ("M" units) of formula SiO 4 / 2 "R" is a tetrafunctional silicate unit ("Q" unit) of the formula M’ are independently R as above 4 and R Ald Alternatively, each R M’ may be selected from the group consisting of alkyl groups, propylaldehyde functional groups of the formula shown above, and aryl groups. Alternatively, each R M’ may be selected from methyl, (propyl-aldehyde), and phenyl. Alternatively, R M’ At least one third, alternatively at least two thirds, of the groups are methyl groups. Alternatively, the M' units are (MeSiO 1 / 2 ), (Me2PhSiO 1 / 2 ), and (MeR Ald SiO 1 / 2 The polyorganosilicate resins are soluble in solvents such as those described herein as starting material (D), exemplified by liquid hydrocarbons such as benzene, ethylbenzene, toluene, xylene, and heptane, or in liquid non-functional organosilicon compounds such as low viscosity linear and cyclic polydiorganosiloxanes.

[0138] When prepared, the polyorganosilicate resin contains the M' and Q units described above, and the polyorganosiloxane contains silicon-bonded hydroxyl groups, and / or the moieties (ZO) described above. 1 / 2 ) and further comprising units having hydrolyzable groups represented by the formula Si(OSiR M’ 3) may contain 4 neopentamers, where RM’ is as described above, for example, the neopentamer can be tetrakis(trimethylsiloxy)silane. 29 Si NMR and 13 C NMR spectroscopy can be used to measure the hydroxyl and alkoxy content, as well as the molar ratio of M' and Q units, expressed as {M'(resin)} / {Q(resin)}, excluding the M' and Q units from the neopentamer. The M' / Q ratio represents the molar ratio of the total number of triorganosiloxy groups (M' units) in the resinous portion of the polyorganosilicate resin to the total number of silicate groups (Q units) in the resinous portion. The M' / Q ratio can be from 0.5 / 1 to 1.5 / 1, alternatively from 0.6 / 1 to 0.9 / 1.

[0139] The Mn of the polyorganosilicate resin is determined by the R M’ The Mn of the polyorganosilicate resins varies depending on various factors including the type of hydrocarbon group represented by. The Mn of the polyorganosilicate resins refers to the number average molecular weight measured using GPC when the peak representing the neopentamer is excluded from the measurement. The Mn of the polyorganosilicate resins may be 1,500 Da to 30,000 Da, alternatively 1,500 Da to 15,000 Da, alternatively >3,000 Da to 8,000 Da. Alternatively, the Mn of the polyorganosilicate resins may be 3,500 Da to 8,000 Da.

[0140] Alternatively, the polyorganosilicate resin may be represented by the unit formula (E2-17): (R 4 3SiO 1 / 2 ) mm (R 4 2R Ald SiO 1 / 2 ) nn (SiO 4 / 2 ) oo (ZO 1 / 2 ) h wherein Z, R 4 , and R Aldand the subscript h is as described above, and the subscripts mm, nn, and oo have average values such that mm≧0, nn>0, oo>0, and 0.5≦(mm + nn) / oo≦4. Alternatively, 0.6≦(mm + nn) / oo≦4, alternatively, 0.7≦(mm + nn) / oo≦4, alternatively, 0.8≦(mm + nn) / oo≦4.

[0141] Alternatively, the (E2) propyl aldehyde-functional polyorganosiloxane may include a (E2-18) propyl aldehyde-functional silsesquioxane resin, i.e., the unit formula: (R 4 3SiO 1 / 2 ) a (R 4 2R Ald SiO 1 / 2 ) b (R 4 2SiO 2 / 2 ) c (R 4 R Ald SiO 2 / 2 ) d (R 4 SiO 3 / 2 ) e (R Ald SiO 3 / 2 ) f (ZO 1 / 2 ) h resin containing trifunctional (T’) units of, wherein R 4 and R Ald are as described above, with subscript f>1, 2<(e + f)<10,000, 0<(a + b) / (e + f)<3, 0<(c + d) / (e + f)<3, and 0<h / (e + f)<1.5. Alternatively, the propyl aldehyde-functional silsesquioxane resin may include the unit formula (E2-19): (R 4 SiO 3 / 2 ) e (R Ald SiO 3 / 2 ) f (ZO 1 / 2 ) h and may contain, wherein R 4 , R Ald, Z, and the subscripts h, e, and f are as described above. Alternatively, the propylaldehyde-functional silsesquioxane resin may further include, in addition to the above T units, a difunctional (D’) unit of the formula (R 4 2SiO 2 / 2 ), i.e., a D’T’ resin, where the subscripts c and d are as described above. Alternatively, the propylaldehyde-functional silsesquioxane resin may further include a monofunctional (M’) unit of the formula (R 4 3SiO 1 / 2 ), i.e., an M’D’T’ resin, where the subscripts a and b are as described above for the unit formula (E2-1).

[0142] Alternatively, the starting material (E), the propylaldehyde-functional organosilicon compound, may include the unit formula (E3-1): [(R 1 (3-gg) R Ald gg Si) ff NH (3-ff) hh , where R Ald is a propylaldehyde group as described above, each R 1 is independently selected from the group consisting of alkyl and aryl groups as described above, each subscript ff is independently 1 or 2 as described above, the subscript gg is independently 0, 1, or 2 as described above, and the subscript h has a value such that 1 < hh < 10 as described above.

[0143] ​​​​​​​​​​​​​​​​​​​​​Starting material (E) can be any one of the above-mentioned propylaldehyde-functional organosilicon compounds (whether made via the hydroformylation reaction process described herein or via some other method). Alternatively, starting material (E) can include a mixture of two or more of the propylaldehyde-functional organosilicon compounds.

[0144] Alternatively, in the processes described herein, the starting material (E) can be a hydrolytically unstable propylaldehyde-functional organosilicon compound. A hydrolytically unstable propylaldehyde-functional organosilicon compound is, for example, a compound having at least one R 4 is a hydrocarbyloxy group or an acyloxy group; any (E3) propylaldehyde-functional silazane; or any (E4) propylaldehyde-functional polyorganosiloxane oligomer of the formula (E2-10a) shown above, e.g., 1,3-di(propyl-aldehyde)-1,1,3,3-tetramethyldisiloxane; or (E2-11a), e.g., 1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)-3-vinyltrisiloxane.

[0145] Preparation of Propylimine- and Aminopropyl-Functional Organosilicon Compounds The process for preparing the propylamino-functional organosilicon compound comprises: I) combining starting materials under conditions which result in a dehydration imine formation reaction, the starting materials being: (E) a propylaldehyde-functional organosilicon compound as described above; and (F1) a primary amine source; optionally, (G) a hydrogenation catalyst; and optionally, (J) a solvent; provided that, when (G) a hydrogenation catalyst is present in step I), step I) is carried out in the absence of hydrogen; combining, thereby forming a reaction product comprising (L) a propylimine-functional organosilicon compound and water; Optionally, II) removing water produced by the dehydration imine-producing reaction in step I); and Optionally, the (L) propylimine functional organosilicon compound may be isolated. The propylimine functional organosilicon compound may be isolated by any convenient means, such as stripping and / or distillation of the reaction product, and the propylimine functional organosilicon compound may be used for purposes other than those described below. Alternatively, the (L) propylimine functional organosilicon compound may be used to prepare an aminopropyl functional organosilicon compound, if the process further comprises: III) combining a starting material under conditions to catalyze a reductive amination reaction, the starting material being: (L) a propylimine-functional organosilicon compound as described above; (F2) ammonia, optionally, (G) a hydrogenation catalyst; (H) hydrogen; and optionally, (J) a solvent to form a reaction product comprising an aminopropyl-functional organosilicon compound. With the proviso that (G) a hydrogenation catalyst is added in at least one of steps I) and III).

[0146] The process may optionally further comprise, before step I), 1) combining starting materials under conditions that catalyze hydroformylation reaction, the starting materials comprising (A) a gas comprising hydrogen and carbon monoxide, (B) a vinyl-functional organosilicon compound, and (C) a rhodium / ligand complex catalyst, thereby forming a hydroformylation reaction product comprising a propylaldehyde-functional organosilicon compound as described above. The process may optionally further comprise, before step I) and after step 1), step 2) recovering (C) the rhodium / ligand complex catalyst from the reaction product comprising the propylaldehyde-functional organosilicon compound. However, step 2) is optional and may not be required. For example, when hydroformylation is used to prepare (E) propylaldehyde-functional organosilicon compounds, it may not be necessary to remove the hydroformylation reaction catalyst, since, without wishing to be bound by theory, it is believed that the amount of catalyst is not cost-effective to remove, and / or the selection and amount of catalyst does not adversely affect the dehydration imine formation reaction or the reductive amination reaction.Optionally, the process may further comprise step 3) before step I) and after step 1) or step 2) (if present), purifying the hydroformylation reaction product, thereby isolating (E) propylaldehyde-functional organosilicon compounds from additional materials, as described above.However, this step 3) is optional, and may not be necessary, for example, when a solvent is used in the hydroformylation reaction to prepare (E) propylaldehyde-functional organosilicon compounds, and the same solvent is used in a later step of the process.

[0147] Step I) Protection of the aldehyde In step I) of the above process, a dehydration imine formation reaction occurs to protect the aldehyde group and form an imine group. In step I), the starting materials including (E) the propylaldehyde functional organosilicon compound and (F1) the primary amine source can be combined by any convenient means, such as mixing. The mixing can be carried out by any convenient means, for example, at RT and at ambient pressure and atmosphere. The mixing time is sufficient to form the imine group from the aldehyde group under the selected conditions. Step I) can be carried out in batch or continuous mode. The time is not critical and is sufficient to form the imine group, for example, from 1 second to 1 hour.

[0148] (F) Amine source In the process described herein, (F1) a primary amine source is used in step I). The primary amine source can be any primary amine source that is inexpensive and separable from the aminopropyl-functional organosilicon compound prepared by the process. The primary amine source can be an organic primary amine. The organic primary amine can be represented by the formula: R 18 NH2, where R 18 R is an alkyl group having 1 to 18 carbon atoms or an aryl group having 6 to 18 carbon atoms. 18 Suitable alkyl groups for may be linear, branched, cyclic, or a combination of two or more thereof. Alkyl groups are exemplified by methyl, ethyl, propyl (including n-propyl and / or isopropyl), butyl (including n-butyl, tert-butyl, sec-butyl, and / or isobutyl), pentyl, hexyl, heptyl, octyl, decyl, dodecyl, undecyl, and octadecyl (and branched isomers having 5 to 18 carbon atoms), and alkyl groups are further exemplified by cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, and cyclohexyl. 18 Suitable aryl groups for R can be, for example, phenyl, tolyl, xylyl, phenylethyl, and benzyl. 18 The alkyl group of R may be selected from the group consisting of ethyl, propyl, and butyl, alternatively ethyl or propyl, alternatively propyl and butyl.18 The alkyl group in R can be propyl. 18 can be an aryl group, alternatively, R 18 can be benzyl. Alternatively, the organic primary amine can have two or more primary amine groups per molecule. Organic primary amines are known in the art and are commercially available. For example, ethylamine, propylamine, n-butylamine, isobutylamine, and benzylamine are available from various sources, such as Acros Organics or Sigma Aldrich, Inc. (St. Louis, Missouri, USA). Alternatively, the primary amine source can include a primary amino-functional organosilicon compound. The primary amino-functional organosilicon compound used as the primary amine source in step I) can be any primary amino-functional organosilicon compound, for example, the primary amine source can have the same formula as the primary amino-functional organosilicon compound prepared by this process. For example, the primary amine source can be 2-aminopropyltrimethylsilane, 3,3'-(1,1,3,3,-tetramethyldisiloxane-1,3-diyl)propane-diamine. The formation of imine functional organosilicon compounds using primary amino functional organosilicon compounds as the primary amine source is shown in Scheme 1 below.

[0149] [ka]

[0150] The primary amine source used in step I) may be used in a superstoichiometric amount of amine functionality relative to the aldehyde functionality of the (E) propylaldehyde-functional organosilicon compound. For example, the primary amine source may be used in an amount sufficient to provide a molar ratio of amine groups:aldehyde groups of 10:1 to 1:1.

[0151] Propyl imine functional organosilicon compounds The propylimine-functional organosilicon compound prepared in step I) of the above process has at least one propylimine functional group covalently bonded to silicon per molecule. Alternatively, the propylimine-functional organosilicon compound may have two or more propylimine functional groups covalently bonded to silicon per molecule. This propylimine functional group, R I is the expression:

[0152] [ka] where G is a divalent hydrocarbon group free of aliphatic unsaturation having 2 carbon atoms as described and exemplified above, and R 19 is R 18 (alkyl or aryl groups as described above when an organic primary amine is used as the primary amine source) and an organosilicon moiety (when an amino-functional organosilicon compound is used as the primary amine source). The propylimine-functional organosilicon compound may have any of the formulas described above for the (E) propylaldehyde-functional organosilicon compound, provided that at least one R Ald R I Alternatively, R Ald All or substantially all of the cases are I can be replaced by

[0153] The propylimine-functional organosilicon compound is represented by the formula (L1) (L1-1): R I x SiR 4 (4-x) wherein R I , R 4 , and the subscript x are as above.

[0154] Alternatively, the propylimine-functional organosilicon compound may comprise (L2) a propylimine-functional polyorganosiloxane. The propylimine-functional polyorganosiloxane may be cyclic, linear, branched, resinous, or a combination of two or more thereof. The propylimine-functional polyorganosiloxane may have a unit formula (L2-1): (R 4 3SiO 1 / 2 ) a (R 4 2R I SiO 1 / 2 ) b (R 4 2SiO 2 / 2 ) c (R 4 R I SiO 2 / 2 ) d (R 4 SiO 3 / 2 ) e (R I SiO 3 / 2 ) f (SiO 4 / 2 ) g (ZO 1 / 2 ) h wherein each R I are independently selected imine groups of the formula above, and R 4 , Z, and subscripts a, b, c, d, e, f, g, and h are as defined above for formula (B2-1).

[0155] Alternatively, the (L2) propylimine-functional polyorganosiloxane may comprise a (L2-2) linear polydiorganosiloxane having at least one propylimine functional group, or alternatively at least two propylimine functional groups, per molecule (e.g., when subscripts e=f=g=0 in formula (L2-1) for the propylimine-functional polyorganosiloxane above). For example, the polydiorganosiloxane may have the unit formula (L2-3): (R 4 3SiO 1 / 2 ) a (R I R 4 2SiO 1 / 2 ) b (R 4 2SiO2 / 2 ) c (R I R 4 SiO 2 / 2 ) d wherein R I is as above, and R 4 and the subscripts a, b, c, and d are as defined above for formula (E2-3).

[0156] Alternatively, the linear propylimine-functional polydiorganosiloxane of the unit formula (L2-3) may be represented by the unit formula (L2-4): (R 4 2R I SiO 1 / 2 )2(R 4 2SiO 2 / 2 ) m (R 4 R I SiO 2 / 2 ) n , Unit formula (L2-5): (R 4 3SiO 1 / 2 )2(R 4 2SiO 2 / 2 ) o (R 4 R I SiO 2 / 2 ) p or a combination of both (L2-4) and (L2-5).

[0157] In formulas (L2-4) and (L2-5), R I is as above, and R 4 and the subscripts m, n, o, and p are as defined above for formulas (E2-4) and (E2-5).

[0158] Alternatively, the (L2) propylimine-functional polyorganosiloxane may be cyclic, for example, when in the unit formula (L2-1), the subscripts a=b=c=e=f=g=h=0. The (L2-6) cyclic propylimine-functional polydiorganosiloxane may be represented by the unit formula (L2-7): (R 4 R I SiO 2 / 2 ) d wherein R I and R4 is as above, where subscript d can be 3 to 12, alternatively 3 to 6, alternatively 4 to 5.

[0159] Alternatively, the (L2-6) cyclic imine-functional polydiorganosiloxane may be represented by the unit formula (L2-8): (R 4 2SiO 2 / 2 ) c (R 4 R I SiO 2 / 2 ) d wherein R 4 and R I is as above, where subscript c is >0 to 6, and subscript d is 3 to 12. Alternatively, in formula (L2-8), the quantity (c+d) can be 3 to 12. Alternatively, in formula (L2-8), c can be 3 to 6, and d can be 3 to 6.

[0160] Alternatively, the (L2) imine-functional polyorganosiloxane may be an (L2-9) oligomer, for example, where the quantity (a+b+c+d+e+f+g) in the above unit formula (L2-1) is ≦50, alternatively ≦40, alternatively ≦30, alternatively ≦25, alternatively ≦20, alternatively ≦10, alternatively ≦5, alternatively ≦4, alternatively ≦3. The oligomer may be cyclic, linear, branched, or a combination thereof. The cyclic oligomer is as described above as the starting material (L2-6).

[0161] An example of a linear propylimine-functional polyorganosiloxane oligomer is represented by the formula (L2-10):

[0162] [ka] wherein R 4 is as above, and each R 2’’’ are independently 4 and R I with the proviso that at least one R 2’’’ But R Iwith the proviso that the subscript z is 0 to 48. Alternatively, the subscript z can be 0 to 4, alternatively 0 to 1, alternatively 0. Alternatively, when z=0 in formula (L2-10), the propylimine-functional polyorganosiloxane oligomer has the formula (L2-10a):

[0163] [ka] wherein R 4 and R I is as stated above.

[0164] Alternatively, the propylimine-functional polyorganosiloxane oligomer can be branched. The branched oligomer has the general formula (L2-11): R I SiR 12 3, where R I is as above, and each R 12 is R 13 and -OSi(R 14 ) 3, each R 13 is a monovalent hydrocarbon group, and each R 14 is R 13 , -OSi(R 15 )3, and -[OSiR 13 2] ii OSiR 13 3 are selected, and each R 15 is R 13 , -OSi(R 16 )3, and -[OSiR 13 2] ii OSiR 13 3 are selected, and each R 16 is R 13 and -[OSiR 13 2] ii OSiR 13 3, where the subscript ii has a value such that 0≦ii≦100. 12 At least two of -OSi(R 14 ) 3. Alternatively, R 12 All three of the -OSi(R 14 )3.

[0165] Alternatively, in formula (L2-11), each R 12 R 13 In the case where the branched polyorganosiloxane oligomer has the following structure (L2-11a):

[0166] [ka] In the formula, R I and R 13 is as defined above. Alternatively, in formula (L2-11a), each R 13 can be methyl.

[0167] Alternatively, in formula (L2-11), each R 12 -OSi(R 14 )3, then each R 14 is a branched polyorganosiloxane oligomer having the following structure (L2-11b): -OSi(R 15 ) three parts,

[0168] [ka] In the formula, R I and R 15 is as described above. Alternatively, each R 15 As above, R 13 Each R 13 can be methyl.

[0169] Alternatively, in formula (L2-11), each R 12 -OSi(R 14 )3, then one R 14 is each R 12 -OSiR 13 (R 14 )2 for each -OSi(R 14 )3 in R 13 Alternatively, -OSiR 13 (R 14 )2 R's14 each of which is a branched aldehyde-functional polyorganosiloxane oligomer having the following structure (L2-11c):

[0170] [ka] -OSi(R 15 ) three parts, In the formula, R I , R 13 , and R 15 is as described above. Alternatively, each R 15 is R 13 Each R 13 can be methyl.

[0171] Alternatively, in formula (L2-11), one R 12 is R 13 R 12 Two of them are -OSi(R 14 )3. R 12 Two of them are -OSi(R 14 )3, then one R 14 Each -OSi(R 14 )R in 3 13 and R 12 Two of them are -OSiR 13 (R 14 )2. Alternatively, -OSiR 13 (R 14 )2 in each R 14 is a branched polyorganosiloxane oligomer having the following structure (L2-11d):

[0172] [ka] -OSi(R 15 )3, wherein R I , R 13 , and R 15 is as described above. Alternatively, each R 15 is R 13 Each R 13may be methyl. Alternatively, the branched polyorganosiloxane may have 3 to 16 silicon atoms per molecule, alternatively 4 to 16 silicon atoms per molecule, alternatively 4 to 10 silicon atoms per molecule. Examples of imine functional branched polyorganosiloxane oligomers include those having the formula:

[0173] [ka] and (E)-N-butyl-3-(1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)trisiloxane-3-yl)propan-1-imine having the formula formula

[0174] [ka] and (E)-3-(1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)trisiloxane-3-yl)-N-propylpropan-1-imine having the formula:

[0175] Alternatively, the (L2) propylimine-functional polyorganosiloxane may be branched, such as the branched oligomers described above, and / or branched propylimine-functional polyorganosiloxanes that may have, for example, more propylimine groups and / or more polymer units per molecule than the branched oligomers described above (e.g., where the quantity (a+b+c+d+e+f+g) in formula (L2-1) is >50). The branched propylimine-functional polyorganosiloxane may have a quantity (e+f+g) sufficient to provide the branched propylimine-functional polyorganosiloxane (in formula (L2-1)) with >0-5 mol% trifunctional and / or tetrafunctional units.

[0176] For example, the branched propylimine-functional polyorganosiloxane has the unit formula (L2-13): (R 4 3SiO 1 / 2 ) q (R 42R I SiO 1 / 2 ) r (R 4 2SiO 2 / 2 ) s (SiO 4 / 2 ) t In one embodiment, the branched polyorganosiloxane may be of the formula: I is as above, and R 4 and the subscripts q, r, s, and t are as defined above for (E2-13).

[0177] Alternatively, the branched propylimine-functional polyorganosiloxane may be represented by the formula (L2-14): [R I R 4 2Si-(O-SiR 4 2) x -O] (4-w) -Si-[O-(R 4 2SiO) v SiR 4 3] w wherein R I is as above, and R 4 and the subscripts v, w, and x are as defined above for formula (E2-14). Alternatively, in this formula (L2-14), each R 4 is independently selected from the group consisting of methyl and phenyl; I has the formula above, where G has 2, 3, or 6 carbon atoms.

[0178] Alternatively, the branched propylimine-functional polyorganosiloxane for (L2-11) may be represented by the unit formula (L2-15): (R 4 3SiO 1 / 2 ) aa (R I R 4 2SiO 1 / 2 ) bb (R 4 2SiO 2 / 2 ) cc (R I R 4 SiO 2 / 2 ) ee (R 4 SiO 3 / 2 )dd In the formula, R I is as above, and R 4 and the subscripts aa, bb, cc, dd, and ee are as defined above for unit formula (E2-15).

[0179] Alternatively, (L2) the propylimine-functional polyorganosiloxane may comprise a propylimine-functional polyorganosiloxane resin, such as a propylimine-functional polyorganosilicate resin and / or a propylimine-functional silsesquioxane resin. The propylimine-functional polyorganosilicate resin is represented by the formula R M’’’ 3SiO 1 / 2 and a monofunctional unit ("M'' unit) of formula SiO 4 / 2 "R" is a tetrafunctional silicate unit ("Q" unit) of the formula M’’’ are independently R as above 4 and R I Alternatively, each R M’’’ is an alkyl group, R I and aryl groups, propylimine functional groups of the formula: The polyorganosilicate resins are soluble in solvents such as those described herein as starting material (D), exemplified by liquid hydrocarbons such as benzene, ethylbenzene, toluene, xylene, and heptane, or in liquid non-functional organosilicon compounds such as low viscosity linear and cyclic polydiorganosiloxanes.

[0180] The propylimine-functional polyorganosilicate resin comprises M''' and Q units as described above, and the polyorganosilicate resin contains silicon-bonded hydroxyl groups, and / or the moieties (ZO) as described above. 1 / 2 ) and further comprising units having hydrolyzable groups represented by the formula Si(OSiR M’’’ 3) may contain 4 neopentamers, where R M’’’ is as described above, for example, the neopentamer can be tetrakis(trimethylsiloxy)silane. 29 Si NMR and13 C NMR spectroscopy can be used to measure the hydroxyl and alkoxy content, as well as the molar ratio of M''' and Q units, expressed as {M'''(resin)} / {Q(resin)}, excluding the M'' and Q units from the neopentamer. The M'' / Q ratio represents the molar ratio of the total number of triorganosiloxy groups (M'' units) in the resinous portion of the polyorganosilicate resin to the total number of silicate groups (Q units) in the resinous portion. The M'' / Q ratio can be from 0.5 / 1 to 1.5 / 1, alternatively from 0.6 / 1 to 0.9 / 1.

[0181] The Mn of the polyorganosilicate resin is determined by the R M’’’ The Mn of the polyorganosilicate resins varies depending on various factors including the type of hydrocarbon group represented by. The Mn of the polyorganosilicate resins refers to the number average molecular weight measured using GPC when the peak representing the neopentamer is excluded from the measurement. The Mn of the polyorganosilicate resins may be 1,500 Da to 30,000 Da, alternatively 1,500 Da to 15,000 Da, alternatively >3,000 Da to 8,000 Da. Alternatively, the Mn of the polyorganosilicate resins may be 3,500 Da to 8,000 Da.

[0182] Alternatively, the polyorganosilicate resin may be represented by the unit formula (L2-17): (R 4 3SiO 1 / 2 ) mm (R 4 2R I SiO 1 / 2 ) nn (SiO 4 / 2 ) oo (ZO 1 / 2 ) h wherein Z, R 4 , and R I , and subscript h are as above, and the subscripts mm, nn, and oo have average values ​​such that mm≧0, nn>0, oo>0, and 0.5≦(mm+nn) / oo≦4. Alternatively, 0.6≦(mm+nn) / oo≦4, alternatively, 0.7≦(mm+nn) / oo≦4, alternatively, 0.8≦(mm+nn) / oo≦4.

[0183] Alternatively, the (L2) propylimine-functional polyorganosiloxane may include a (L2-18) propylimine-functional silsesquioxane resin, i.e., the unit formula: (R 4 3SiO 1 / 2 ) a (R 4 2R I SiO 1 / 2 ) b (R 4 2SiO 2 / 2 ) c (R 4 R I SiO 2 / 2 ) d (R 4 SiO 3 / 2 ) e (R I SiO 3 / 2 ) f (ZO 1 / 2 ) h containing a trifunctional (T’’’) unit of the formula, wherein R 4 and R I are as described above, the subscript f > 1, 2 < (e + f) < 10,000, 0 < (a + b) / (e + f) < 3, 0 < (c + d) / (e + f) < 3, and 0 < h / (e + f) < 1.5. Alternatively, the propylimine-functional silsesquioxane resin may include the unit formula (L2-19): (R 4 SiO 3 / 2 ) e (R I SiO 3 / 2 ) f (ZO 1 / 2 ) h wherein R 4 , R I , Z, and the subscripts h, e, and f are as described above. Alternatively, the propylimine-functional silsesquioxane resin may further include a difunctional (D’’’) unit, and the imine-functional silsesquioxane resin, in addition to the above T units, has the formula (R 4 2SiO 2 / 2 ) c (R 4 R I SiO 2 / 2 ) dunits, i.e., may contain D’’’T’’’ resin, where the subscripts c and d are as described above. Alternatively, the propylimine-functionalized silsesquioxane resin may further contain a monofunctional (M’’’) unit of the formula (R 4 3SiO 1 / 2 ) a (R 4 2R I SiO 1 / 2 ) b , i.e., may further contain M’’’D’’’T’’’ resin, where the subscripts a and b are as described above for the unit formula (E2-1).

[0184] Alternatively, the (L) propylimine-functionalized organosilicon compound may contain a unit formula (L3-1): [(R 1 (3-gg) R I gg Si) ff NH (3-ff) hh , where R I is a propylimine group as described above, each R 1 is independently selected from the group consisting of an alkyl group and an aryl group as described above, each subscript ff is independently 1 or 2 as described above, the subscript gg is independently 0, 1, or 2 as described above, and the subscript h has a value such that 1 < hh < 10 as described above.

[0185] The propylimine-functionalized organosilicon compound (L) prepared in step I) and used in step III) of the process described herein can be any one of the above propylimine-functionalized organosilicon compounds. Alternatively, the (L) propylimine-functionalized organosilicon compound may contain a mixture of two or more of the propylimine-functionalized organosilicon compounds.

[0186] Alternatively, in the process described herein, the (L) propylimine-functionalized organosilicon compound can be a propylimine-functionalized organosilicon compound that is unstable to hydrolysis. A propylimine-functionalized organosilicon compound that is unstable to hydrolysis is, for example, at least one R 4 ​is a hydrocarbyloxy group or an acyloxy group, any (L3) propylimine-functional silazane, or any propylimine-functional polyorganosiloxane oligomer of formula (L2-10a) or (L2-11a) shown above, such as (E)-N-butyl-3-(1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)trisiloxane-3-yl)propan-1-imine or (E)-3-(1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)trisiloxane-3-yl)-N-propylpropan-1-imine.

[0187] Step II) Drying The above process may optionally further comprise step II) of removing water produced by the dehydration imine-forming reaction in step I). Step II) may be carried out during and / or after step I), during and / or after step III), or a combination thereof. Alternatively, step II) may be present and carried out during and / or after step I), for example, when a hydrolytically unstable propylaldehyde-functional organosilicon compound is used and / or when a hydrolytically unstable propylimine-functional organosilicon compound or a hydrolytically unstable aminopropyl-functional organosilicon compound is formed during the process.

[0188] In step II), water may be removed by any convenient means, such as stripping, distillation, and / or contacting the reaction mixture in step I) and / or the reaction product of step I) with (K) a desiccant. The desiccant may include an adsorbent, which may include inorganic particulates. The adsorbent may have a particle size of 10 micrometers or less, alternatively 5 micrometers or less. The adsorbent may have an average pore size sufficient to adsorb water, for example, 10 Å (angstroms) or less, alternatively 5 Å or less, alternatively 3 Å or less. Examples of adsorbents include zeolites such as chabazite, mordenite, and analcime, alkali metal aluminosilicates, silica gel, silica magnesia gel, activated carbon, activated alumina, calcium oxide, and molecular sieves such as combinations thereof.

[0189] Examples of commercially available adsorbents include dry molecular sieves, such as 3 Å molecular sieves available from Grace Davidson under the trade name SYLOSIV™ and Zeochem (Louisville, Kentucky, USA) under the trade name PURMOL, and 4 Å molecular sieves such as Doucil zeolite 4A available from Ineos Silicas (Warrington, England). Other useful molecular sieves include MOLSIV ADSORBENT TYPES 13X, 3A, 4A and 5A (all available from UOP (Illinois, USA)), SILIPORITE NK 30AP and 65xP (Atofina (Philadelphia, Pennsylvania, USA)), and molecular sieves available from WRGrace (Maryland, USA).

[0190] Alternatively, the desiccant may include chemicals that complex with water, such as calcium chloride (CaCl2), sodium sulfate (Na2SO4), calcium sulfate (CaSO4), or magnesium sulfate (MgSO4), all of which are commercially available.

[0191] The amount of desiccant is not particularly limited and depends on various factors, including the type of desiccant selected. A person skilled in the art will be able to select an appropriate desiccant and conditions for removing water in step II). If a desiccant is used, the process described herein may further include removing the desiccant before step III). The desiccant may then be removed by any convenient means, such as filtration. Alternatively, a desiccant may be used during and / or after step III). The desiccant may then be removed after step III).

[0192] The process for making aminopropyl-functional organosilicon compounds can optionally further comprise an additional step (G) of pretreating the hydrogenation catalyst before step III). Pretreatment can be carried out to activate the catalyst and / or to increase the activity of the catalyst. Pretreatment can be carried out by any convenient means, such as exposing the hydrogenation catalyst to hydrogen before starting the reductive amination reaction in step III). For example, the packed bed of hydrogenation catalyst can be purged with hydrogen before introducing (L) propylimine-functional organosilicon compound and (F2) ammonia.

[0193] In step III) of the process, (F2) ammonia, e.g., anhydrous ammonia, having the formula NH3 is used. Ammonia is known in the art and is commercially available from a variety of sources, including Air Products (Allentown, Pennsylvania, USA). The amount of (F2) ammonia used in step III) can be sufficient to provide a molar ratio of ammonia:imine groups of greater than 1:1, alternatively greater than 5:1, alternatively between 10:1 and 40:1.

[0194] (G) Hydrogenation catalyst The hydrogenation catalyst used in step III) of the process for preparing aminopropyl-functional organosilicon compounds can be a heterogeneous hydrogenation catalyst, a homogeneous hydrogenation catalyst, or a combination thereof. Alternatively, the hydrogenation catalyst can be a heterogeneous hydrogenation catalyst. Suitable heterogeneous hydrogenation catalysts include metals selected from the group consisting of cobalt (Co), copper (Cu), iron (Fe), nickel (Ni), iridium (Ir), palladium (Pd), platinum (Pt), rhodium (Rh), ruthenium (Ru), and combinations of two or more thereof. Alternatively, the hydrogenation catalyst can include Co, Cu, Ni, Pd, Pt, Ru, or combinations of two or more thereof. Alternatively, the hydrogenation catalyst can include Co, Cu, Ni, Pd, or combinations of two or more thereof. Alternatively, the hydrogenation catalyst may include Co, Cu, Ni, or a combination of two or more thereof. The hydrogenation catalyst may include a support such as alumina (Al2O3), silica (SiO2), silicon carbide (SiC), or carbon (C). Alternatively, the hydrogenation catalyst may be selected from the group consisting of Rh / C, Raney nickel, Raney copper, Raney cobalt, Ru / C, Ru / Al2O3, Pd / C, Pd / Al2O3, Pd / CaCO3, Cu / C, Cu / Al2O3, Cu / SiO2, Cu / SiC, Cu / C, nickel catalysts on the above supports, and combinations of two or more thereof.

[0195] Alternatively, the heterogeneous hydrogenation catalyst for the reductive amination of the imine group of the (L) propylimine-functional organosilicon compound may comprise copper, chromium, nickel, rhodium, or a support material to which two or more of these are applied as active components. Exemplary catalysts include 0.3-15% copper, 0.3%-15% nickel, and 0.05%-3.5% chromium. The support material may be, for example, porous silicon dioxide or aluminum oxide. Barium may optionally be added to the support material. Alternatively, a chromium-free hydrogenation catalyst may be used. For example, Ni / Al2O3 or Co / Al2O3, or a copper oxide / zinc oxide-containing catalyst (which may further comprise potassium, nickel, and / or cobalt), in addition to an alkali metal, may be used. Suitable hydrogenation catalysts are disclosed, for example, in U.S. Pat. No. 7,524,997 or U.S. Pat. No. 9,567,276 and references cited therein. Alternatively, heterogeneous hydrogenation catalysts may be commercially available, such as Rh / C catalyst available from Sigma-Aldrich, Ni-5256P available from BASF, and Co-179, which is also commercially available.

[0196] Other examples of heterogeneous hydrogenation catalysts suitable for use herein include Raney nickel, e.g., Raney nickel 2400, Ni-3288, Raney copper, Hysat 401 salt (Cu), ruthenium on carbon (Ru / C), rhodium on carbon (Rh / C), platinum on carbon (Pt / C), copper on silicon carbide (Cu / SiC).

[0197] Alternatively, homogeneous hydrogenation catalysts may be used herein. The homogeneous hydrogenation catalyst may be a metal complex, and the metal may be selected from the group consisting of Co, Fe, Ir, Rh, and Ru. Examples of suitable homogeneous hydrogenation catalysts are [RhCl(PPh3)3] (Wilkinson's catalyst), [Rh(NBD)(PR'3)2]+ClO4- (where R' is an alkyl group, e.g., Et), [RuCl2(diphosphine)(1,2-diamine)] (Noyori's catalyst), RuCl2(TRIPHOS) (where TRIPHOS = PhP[(CH2CH2PPh2)2], Ru(II)(dppp)(glycine) complex (where dppp = 1,3-bis(diphenylphosphino)propane), RuCl2(PPh3), RuCl2(CO)2(PPh3), IrH3(PPh3), [Ir(H2)(CH3COO)(PPh3)], cis-[Ru-Cl2(ampy)(PP)] [where ampy = 2-(aminomethyl)pyridine, and PP = 1,4-bis-(diphenylphosphino)butane, 1,1'-ferrocenediyl-bis(diphenylphosphine)], pincer RuCl(CNNR)(PP) complexes [where PP = 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,1'-ferrocenediyl-bis(diphenylphosphine)] and HCNNR = 4-substituted aminomethyl-benzo[h]quinolines, R = Me, Ph], [RuCl(dppb)(ampy)] (where dppb = 1,4-bis(diphenylphosphino)butane, ampy = 2-aminomethylpyridine), [Fe(PNPMeiPr)(CO)(H)(Br)], [Fe(PNPMe-iPr)(H)2(CO)], and combinations thereof.

[0198] The amount of hydrogenation catalyst used in the process varies depending on various factors including whether the process is run in batch or continuous mode, the type of propylimine-functional organosilicon compound, whether a heterogeneous or homogeneous hydrogenation catalyst is selected, and the reductive amination reaction conditions such as temperature and pressure. However, when the process is run in batch mode, the amount of catalyst can be less than 1% to 50% by weight, alternatively 5% to 30% by weight, based on the weight of the propylimine-functional organosilicon compound. Alternatively, the amount of catalyst can be at least 1, alternatively at least 4, alternatively at least 6.5, alternatively at least 8% by weight, while the amount of catalyst can be up to 50, alternatively up to 20, alternatively up to 14, alternatively up to 13, alternatively up to 10, alternatively up to 9% by weight, on the same basis. Alternatively, when the process is run in continuous mode, for example by filling the reactor with a heterogeneous hydrogenation catalyst, the amount of heterogeneous hydrogenation catalyst can be less than 10% by weight, alternatively 5 ... -1 Reactor volume (filled with hydrogenation catalyst) to achieve a space time of 1 m 2 The catalyst surface area may be sufficient to achieve 10 kg / hr of substrate per hour.

[0199] (H) Hydrogen Hydrogen is known in the art and is commercially available from a variety of sources, such as Air Products. Hydrogen may be used in superstoichiometric amounts relative to the imine groups of the (L) propylimine-functional organosilicon compound to allow for complete reaction.

[0200] (J) Solvent The solvent (J) that may be optionally used in the process for preparing the propylimine-functional organosilicon compound and / or the aminopropyl-functional organosilicon compound may be selected from solvents that are neutral to the dehydration imine-forming reaction when used in step I) above, and / or to the reductive amination reaction when used in step III) of the process. The following are specific examples of such solvents: monohydric alcohols such as methanol, ethanol, and isopropyl alcohol; ethers such as dioxane, THF; aliphatic hydrocarbons such as hexane, heptane, and paraffinic solvents; aromatic hydrocarbons such as benzene, toluene, and xylene; and chlorinated hydrocarbons. These solvents may be used individually or in combination of two or more. The amount of solvent is not critical and may vary depending on various factors such as the type and amount of each starting material used. For example, more solvent may be used if the propylaldehyde-functional organosilicon compound and / or the propylimine-functional organosilicon compound is resinous rather than oligomeric. However, the amount of solvent may be 0-99% based on the total weight of all starting materials used in the process.

[0201] During or after step III) of the process, water removal may be performed as described above for step II). For example, a drying agent such as (K) an adsorbent or water complexing agent may be optionally used to remove water generated as a by-product. Suitable drying agents and their conditions of use are described above. The drying agent selected for use during or after step III) may be the same as or different from the drying agent selected for use during or after step I). Alternatively, if a drying agent is used during or after step I), the drying agent may be omitted during or after step III).

[0202] Step III) Reductive amination reaction The reductive amination reaction in step III) may be carried out using pressurized hydrogen. The hydrogen (gauge) pressure may be from 10 psig (68.9 kPa) to 3000 psig (20,685 kPa), alternatively from 10 psig to 2000 psig (13,790 kPa), alternatively from 10 psig to 1500 psig (10,342 kPa), alternatively from 200 psig (1379 kPa) to 1200 psig (8274 kPa). The reaction may be carried out at a temperature of 0 to 200° C. Alternatively, to shorten the reaction time, a temperature of 50 to 150° C. may be suitable. Alternatively, the hydrogen (gauge) pressure used can be at least 25 psig, alternatively at least 50 psig, alternatively at least 100 psig, alternatively at least 150 psig, alternatively at least 164 psig, while the hydrogen gauge pressure can be up to 800 psig, alternatively up to 400 psig, alternatively up to 300 psig, alternatively up to 200 psig, alternatively up to 194 psig. The temperature for the reaction can be at least 40° C., alternatively at least 50° C., alternatively at least 65° C., alternatively at least 80° C., while the temperature can be up to 200° C., alternatively up to 150° C., alternatively up to 120° C.

[0203] The reductive amination reaction can be carried out in batch mode or continuous mode. In batch mode, the reductive amination reaction time varies depending on various factors including the amount of catalyst and the reductive amination reaction temperature, but step III) of the process for preparing aminopropyl-functional organosilicon compounds can be carried out for 1 minute to 24 hours. Alternatively, the reductive amination reaction can be carried out for at least 1 minute, alternatively at least 2 minutes, alternatively at least 1 hour, alternatively at least 2 hours, alternatively at least 3 hours, alternatively at least 3.3 hours, alternatively at least 3.7 hours, alternatively at least 4 hours, alternatively at least 4.5 hours, alternatively at least 5.5 hours, alternatively at least 6 hours, while the reductive amination reaction can be carried out for up to 24 hours, alternatively up to 23 hours, alternatively up to 22.5 hours, alternatively up to 22 hours, alternatively up to 17.5 hours, alternatively up to 17 hours, alternatively up to 16.5 hours.

[0204] Alternatively, in batch mode, the end point of the reductive amination reaction may be considered to be the time when a decrease in reactor pressure is no longer observed after continuing the reaction for an additional 1-2 hours. If the reactor pressure decreases during the course of the reaction, it may be desirable to repeat the introduction of hydrogen and amine sources and to maintain it under elevated pressure to shorten the reaction time. Alternatively, the reactor can be repressurized with hydrogen and ammonia one or more times to achieve a sufficient supply of hydrogen and ammonia for the reaction of the imine functional group while maintaining a reasonable reactor pressure.

[0205] In continuous mode, the reductive amination reaction can be carried out in a trickle bed reactor. A trickle bed reactor can provide reduced capital investment and / or increased yield in step III) of the process, and / or easier handling for separation of the aminopropyl-functional organosilicon compound from the catalyst after step III) of the process. Alternatively, a high pressure reactor (e.g., as described above, a reactor that can withstand pressures of up to 3000 psig (20,685 kPa)) can be used for the reductive amination reaction in step III), either in batch mode or continuous mode.

[0206] After completion of the reductive amination reaction, (G) the hydrogenation catalyst may be separated by any convenient means, such as filtration or adsorption with, for example, diatomaceous earth or activated carbon, sedimentation, centrifugation, in a pressurized inert (e.g., nitrogen) atmosphere, by maintaining the hydrogenation catalyst in a structured packing or other fixed structure, or by a combination thereof.

[0207] The reductive amination reaction in step III) may also generate by-products including a primary amine source (as described above for use in (step I)). The primary amine source may be recovered from the reductive amination reaction product produced in step III) by any convenient means, such as stripping and / or distillation. The resulting primary amine source thus recovered may be recycled to the process of step I). An exemplary reaction scheme illustrating the above process is described and illustrated below.

[0208] Exemplary Reaction Schemes In an optional first step, a vinyl-functional organosilicon compound (e.g., 1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)-3-vinyltrisiloxane) undergoes a hydroformylation reaction to form a propylaldehyde-functional organosilicon compound (e.g., 3-(1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)trisiloxan-3-yl)propanal). In step I), a propylaldehyde-functional organosilicon compound (e.g., 3-(1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)trisiloxan-3-yl)propanal) is combined with an organic primary amine (e.g., N-butylamine) to form a propylimine-functional organosilicon compound (e.g., N-butyl-3-(1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)trisiloxan-3-yl)propan-1-imine) and water as a by-product. In step II), water can be removed, and in step III), a propylimine-functional organosilicon compound (e.g., N-butyl-3-(1,1,1,5,5,5,-hexamethyl-3-((trimethylsilyl)oxy)trisiloxane-3-yl)propane-1-imine) can be combined with hydrogen, ammonia, and a hydrogenation catalyst under conditions to catalyze the reductive amination reaction. N-butylamine is formed as a by-product of the reductive amination reaction, and N-butylamine can optionally be recycled back to step I). The desired product, e.g., 3-(1,1,1,5,5,5,-hexamethyl-3-((trimethylsilyl)oxy)trisiloxane-3-yl)propane-1-amine), is also formed in step III).

[0209] Example of Optional Step - Hydroformylation to Form Aldehyde Functional Organosilicon Compounds.

[0210] [ka]

[0211] Step I) - Example of dehydration reaction to form imines

[0212] [ka]

[0213] Step II) removing the water and optionally isolating N-butyl-3-(1,1,1,5,5,5,-hexamethyl-3-((trimethylsilyl)oxy)trisiloxan-3-yl)propan-1-imine.

[0214] Step III) Examples of reductive amination reactions

[0215] [ka]

[0216] Aminopropyl-functional organosilicon compounds The aminopropyl-functional organosilicon compounds prepared as above have at least one primary aminopropyl functional group covalently bonded to silicon per molecule. Alternatively, the aminopropyl-functional organosilicon compounds may have two or more primary aminopropyl functional groups covalently bonded to silicon per molecule. The primary aminopropyl functional group, R N is the expression:

[0217] [ka] where G is a divalent hydrocarbon group free of aliphatic unsaturation having 2 carbon atoms, as described and exemplified above. The aminopropyl-functional organosilicon compound may have at least one R I R N The (L) propylimine-functional organosilicon compound may have any one of the formulas above for the propylimine-functional organosilicon compound, preplaced with

[0218] The aminopropyl-functional organosilicon compound prepared as above can be represented by the formula (N1) (N1-1): N x SiR4 (4-x) wherein R N , R 4 and subscript x are as above. Aminopropyl-functional silanes are exemplified by aminopropyl-functional trialkylsilanes such as (aminopropyl)-trimethylsilane and (aminopropyl)-triethylsilane.

[0219] Alternatively, the aminopropyl-functional organosilicon compound may comprise (N2) an aminopropyl-functional polyorganosiloxane. The aminopropyl-functional polyorganosiloxane may be cyclic, linear, branched, resinous, or a combination of two or more thereof. The aminopropyl-functional polyorganosiloxane may have a unit formula (N2-1): (R 4 3SiO 1 / 2 ) a (R 4 2R N SiO 1 / 2 ) b (R 4 2SiO 2 / 2 ) c (R 4 R N SiO 2 / 2 ) d (R 4 SiO 3 / 2 ) e (R N SiO 3 / 2 ) f (SiO 4 / 2 ) g (ZO 1 / 2 ) h wherein each R N is an independently selected primary aminopropyl functional group of the formula above, R 4 , Z, and subscripts a, b, c, d, e, f, g, and h are as defined above for formula (B2-1).

[0220] Alternatively, the aminopropyl-functional polyorganosiloxane (N2) may comprise a linear polydiorganosiloxane (N2-2) having at least one primary aminopropyl functional group per molecule, or alternatively at least two primary aminopropyl functional groups (e.g., when subscripts e=f=g=0 in formula (N2-1) for the aminopropyl-functional polyorganosiloxane above). For example, the polydiorganosiloxane may have a unit formula (N2-3): (R 4 3SiO 1 / 2 ) a (R N R 4 2SiO 1 / 2 ) b (R 4 2SiO 2 / 2 ) c (R I R 4 SiO 2 / 2 ) d wherein R N is as above, and R 4 and the subscripts a, b, c, and d are as defined above for formula (E2-3).

[0221] Alternatively, the linear aminopropyl-functional polydiorganosiloxane of the unit formula (N2-3) may be represented by the unit formula (N2-4): (R 4 2R N SiO 1 / 2 )2(R 4 2SiO 2 / 2 ) m (R 4 R N SiO 2 / 2 ) n , Unit formula (N2-5): (R 4 3SiO 1 / 2 )2(R 4 2SiO 2 / 2 ) o (R 4 R N SiO 2 / 2 ) p or a combination of both (N2-4) and (N2-5).

[0222] In formulas (N2-4) and (N2-5), RN is as above, and R 4 and the subscripts m, n, o, and p are as defined above for formulas (E2-4) and (E2-5).

[0223] The aminopropyl-functional polyorganosiloxanes (N2) are selected from the group consisting of i) bis-dimethyl(aminopropyl)siloxy-terminated polydimethylsiloxanes, ii) bis-dimethyl(aminopropyl)siloxy-terminated poly(dimethylsiloxane / methyl(aminopropyl)siloxanes), iii) bis-dimethyl(aminopropyl)siloxy-terminated polymethyl(aminopropyl)siloxanes, iv) bis-trimethylsiloxy-terminated poly(dimethylsiloxane / methyl(aminopropyl)siloxanes), v) bis-trimethylsiloxy-terminated polymethyl(aminopropyl)siloxanes, vi) bis-dimethyl( The functional groups may include aminopropyl functional polydiorganosiloxanes such as bis-dimethyl(aminopropyl)siloxy terminated poly(dimethylsiloxane / methylphenylsiloxane / methyl(aminopropyl)siloxane), vii) bis-dimethyl(aminopropyl)siloxy terminated poly(dimethylsiloxane / methylphenylsiloxane), viii) bis-dimethyl(aminopropyl)siloxy terminated poly(dimethylsiloxane / diphenylsiloxane), ix) bis-phenyl,methyl,(aminopropyl)-siloxy terminated polydimethylsiloxane, and x) combinations of two or more of i)-ix).

[0224] Alternatively, (N2) the aminopropyl-functional polyorganosiloxane may be cyclic, for example, if in the unit formula (N2-1), the subscripts a=b=c=e=f=g=h=0. (N2-6) The cyclic aminopropyl-functional polydiorganosiloxane may be represented by the unit formula (N2-7): (R 4 R N SiO 2 / 2 ) d wherein R N and R 4is as above, and subscript d can be 3 to 12, alternatively 3 to 6, alternatively 4 to 5. Examples of cyclic aminopropyl functional polydiorganosiloxanes include 2,4,6-trimethyl-2,4,6-tri(aminopropyl)-cyclotrisiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetra(aminopropyl)-cyclotetrasiloxane, 2,4,6,8,10-pentamethyl-2,4,6,8,10-penta(aminopropyl)-cyclopentasiloxane, and 2,4,6,8,10,12-hexamethyl-2,4,6,8,10,12-hexa(aminopropyl)-cyclohexasiloxane.

[0225] Alternatively, the (N2-6) cyclic aminopropyl-functional polydiorganosiloxane may be represented by the unit formula (N2-8): (R 4 2SiO 2 / 2 ) c (R 4 R N SiO 2 / 2 ) d wherein R 4 and R N is as above, where subscript c is >0 to 6, and subscript d is 3 to 12. Alternatively, in formula (N2-8), the quantity (c+d) can be 3 to 12. Alternatively, in formula (N2-8), c can be 3 to 6, and d can be 3 to 6.

[0226] Alternatively, (N2) aminopropyl-functional polyorganosiloxane may be an (N2-9) oligomer, for example, where the quantity (a+b+c+d+e+f+g) in the above formula (N2-1) is ≦50, alternatively ≦40, alternatively ≦30, alternatively ≦25, alternatively ≦20, alternatively ≦10, alternatively ≦5, alternatively ≦4, alternatively ≦3. The oligomer may be cyclic, linear, branched, or a combination thereof. The cyclic oligomer is as described above as (N2-6).

[0227] An example of a linear aminopropyl-functional polyorganosiloxane oligomer is represented by the formula (N2-10):

[0228] [ka] wherein R 4 is as above, and each R 2’’ are independently 4 and R N with the proviso that at least one R 2’’ But R N with the proviso that the subscript z is 0 to 48. Alternatively, the subscript z can be 0 to 4, alternatively 0 to 1, alternatively 0. Alternatively, when z=0 in formula (N2-10), the aminopropyl-functional polyorganosiloxane oligomer has the formula (N2-10a):

[0229] [ka] wherein R 4 and R N are as described above. Examples of linear aminopropyl-functional polyorganosiloxane oligomers include 1,3-di(aminopropyl)-1,1,3,3-tetramethyldisiloxane, 1,1,1,3,3-pentamethyl-3-(aminopropyl)-disiloxane, and 1,1,1,3,5,5,5-heptamethyl-3-(aminopropyl)-trisiloxane.

[0230] Alternatively, the aminopropyl-functional polyorganosiloxane oligomer can be branched. The branched oligomer has the general formula (N2-11): R N SiR 12 3, where R N is as above, and each R 12 is R 13 and -OSi(R 14 ) 3, each R 13 is a monovalent hydrocarbon group, and each R 14 is R 13 , -OSi(R 15 )3, and -[OSiR 13 2]ii OSiR 13 3 are selected, and each R 15 is R 13 , -OSi(R 16 )3, and -[OSiR 13 2] ii OSiR 13 3 are selected, and each R 16 is R 13 and -[OSiR 13 2] ii OSiR 13 3, where the subscript ii has a value such that 0≦ii≦100. 12 At least two of -OSi(R 14 ) 3. Alternatively, R 12 All three of the -OSi(R 14 )3.

[0231] Alternatively, in formula (L2-11), each R 12 R 13 In the case where the branched polyorganosiloxane oligomer has the following structure (N2-11a):

[0232] [ka] In the formula, R N and R 13 is as defined above. Alternatively, in formula (N2-11a), each R 13 can be methyl.

[0233] Alternatively, in formula (N2-11), each R 12 -OSi(R 14 )3, then each R 14 is -OSi(R) such that the branched polyorganosiloxane oligomer has the following structure (B2-11b): 15 ) three parts,

[0234] [ka] In the formula, RN and R 15 is as described above. Alternatively, each R 15 As above, R 13 Each R 13 can be methyl.

[0235] Alternatively, in formula (N2-11), each R 12 -OSi(R 14 )3, then one R 14 is each R 12 -OSiR 13 (R 14 )2 for each -OSi(R 14 )3 in R 13 Alternatively, -OSiR 13 (R 14 )2 R's 14 each of which is a branched aldehyde-functional polyorganosiloxane oligomer having the following structure (N2-11c):

[0236] [ka] -OSi(R 15 ) three parts, In the formula, R N , R 13 , and R 15 is as described above. Alternatively, each R 15 is R 13 Each R 13 can be methyl.

[0237] Alternatively, in formula (N2-11), one R 12 is R 13 R 12 Two of them are -OSi(R 14 )3. R 12 Two of them are -OSi(R 14 )3, then one R 14 Each -OSi(R 14 )R in 3 13 and R 12 Two of them are -OSiR13 (R 14 )2. Alternatively, -OSiR 13 (R 14 )2 in each R 14 is a branched polyorganosiloxane oligomer having the following structure (N2-11d):

[0238] [ka] -OSi(R 15 )3, wherein R N , R 13 , and R 15 is as described above. Alternatively, each R 15 is R 13 Each R 13 may be methyl. Alternatively, the branched polyorganosiloxane may have 3 to 16 silicon atoms per molecule, alternatively 4 to 16 silicon atoms per molecule, alternatively 4 to 10 silicon atoms per molecule. An example of an aminopropyl-functional branched polyorganosiloxane oligomer includes 3-(3,3,3-trimethyl-112-disiloxaneyl)propan-1-amine, which has the formula

[0239] [ka] has.

[0240] Alternatively, the (N2) aminopropyl-functional polyorganosiloxane may be branched, such as the branched oligomers described above, and / or branched aminopropyl-functional polyorganosiloxanes that may have, for example, more aminopropyl groups and / or more polymer units per molecule than the branched oligomers described above (e.g., where the quantity (a+b+c+d+e+f+g) in formula (N2-1) is >50). The branched aminopropyl-functional polyorganosiloxane may have a quantity (e+f+g) sufficient to provide the branched aminopropyl-functional polyorganosiloxane (in formula (N2-1)) with >0-5 mol% trifunctional and / or tetrafunctional units.

[0241] For example, the branched aminopropyl-functional polyorganosiloxane has the unit formula (N2-13): (R 4 3SiO 1 / 2 ) q (R 4 2R N SiO 1 / 2 ) r (R 4 2SiO 2 / 2 ) s (SiO 4 / 2 ) t In one embodiment, the branched polyorganosiloxane may be of the formula: N is as above, and R 4 and the subscripts q, r, s, and t are as defined above for (E2-13).

[0242] Alternatively, the branched aminopropyl-functional polyorganosiloxane may be represented by the formula (N2-14): [R N R 4 2Si-(O-SiR 4 2) x -O] (4-w) -Si-[O-(R 4 2SiO) v SiR 4 3] w wherein R N is as above, and R 4and the subscripts v, w, and x are as defined above for formula (E2-14). Alternatively, in this formula (N2-14), each R 4 is independently selected from the group consisting of methyl and phenyl.

[0243] Alternatively, the branched aminopropyl-functional polyorganosiloxane for (N2-11) may be represented by the unit formula (N2-15): (R 4 3SiO 1 / 2 ) aa (R N R 4 2SiO 1 / 2 ) bb (R 4 2SiO 2 / 2 ) cc (R N R 4 SiO 2 / 2 ) ee (R 4 SiO 3 / 2 ) dd In the formula, R N is as above, and R 4 and the subscripts aa, bb, cc, dd, and ee are as defined above for unit formula (E2-15).

[0244] Alternatively, (N2) the aminopropyl-functional polyorganosiloxane may comprise an aminopropyl-functional polyorganosiloxane resin, such as an aminopropyl-functional polyorganosilicate resin and / or an aminopropyl-functional silsesquioxane resin. The aminopropyl-functional polyorganosilicate resin may be represented by the formula R M’’ 3SiO 1 / 2 and monofunctional units ("M'' units) of formula SiO 4 / 2 "R" is a tetrafunctional silicate unit ("Q" unit) of the formula M’’ are independently R as above 4 and R N Alternatively, each R may be selected from the group consisting of M’’ is an alkyl group, R Nand an aryl group, an aminopropyl functional group of the formula: M’’ may be selected from methyl, (aminopropyl), (aminobutyl), and phenyl. Alternatively, R M’’ At least one third, alternatively at least two thirds, of the groups are methyl groups. Alternatively, the M″ units are (MeSiO 1 / 2 ), (Me2PhSiO 1 / 2 ), and (MeR N SiO 1 / 2 The polyorganosilicate resins are soluble in solvents such as those described herein as starting material (D), exemplified by liquid hydrocarbons such as benzene, ethylbenzene, toluene, xylene, and heptane, or in liquid non-functional organosilicon compounds such as low viscosity linear and cyclic polydiorganosiloxanes.

[0245] The aminopropyl-functional polyorganosilicate resin comprises the M″ and Q units described above, and the polyorganosilicate resin contains silicon-bonded hydroxyl groups, and / or the moieties (ZO) described above. 1 / 2 ) and further comprising units having hydrolyzable groups represented by the formula Si(OSiR M’’ 3) may contain 4 neopentamers, where R M’’ is as described above, for example, the neopentamer can be tetrakis(trimethylsiloxy)silane. 29 Si NMR and 13 C NMR spectroscopy can be used to measure the hydroxyl and alkoxy content, as well as the molar ratio of M″ and Q units, expressed as {M″(resin)} / {Q(resin)}, excluding the M″ and Q units from the neopentamer. The M″ / Q ratio represents the molar ratio of the total number of triorganosiloxy groups (M″ units) in the resinous portion of the polyorganosilicate resin to the total number of silicate groups (Q units) in the resinous portion. The M″ / Q ratio can be from 0.5 / 1 to 1.5 / 1, alternatively from 0.6 / 1 to 0.9 / 1.

[0246] The Mn of the aminopropyl-functional polyorganosilicate resin is determined by the R M’’ The Mn of the polyorganosilicate resins varies depending on various factors such as the type of hydrocarbon group represented by Mn. The Mn of the polyorganosilicate resins refers to the number average molecular weight measured using GPC when the peak representing the neopentamer is excluded from the measurement. The Mn of the polyorganosilicate resins may be 1,500 Da to 30,000 Da, alternatively 1,500 Da to 15,000 Da, alternatively >3,000 Da to 8,000 Da. Alternatively, the Mn of the polyorganosilicate resins may be 3,500 Da to 8,000 Da.

[0247] Alternatively, the polyorganosilicate resin may be represented by the unit formula (N2-17): (R 4 3SiO 1 / 2 ) mm (R 4 2R N SiO 1 / 2 ) nn (SiO 4 / 2 ) oo (ZO 1 / 2 ) h wherein Z, R 4 , and R N , and subscript h are as above, and the subscripts mm, nn, and oo have average values ​​such that mm≧0, nn>0, oo>0, and 0.5≦(mm+nn) / oo≦4. Alternatively, 0.6≦(mm+nn) / oo≦4, alternatively, 0.7≦(mm+nn) / oo≦4, alternatively, 0.8≦(mm+nn) / oo≦4.

[0248] Alternatively, the (N2) aminopropyl-functional polyorganosiloxane may be an (N2-18) aminopropyl-functional silsesquioxane resin, i.e., a polyorganosiloxane having the unit formula: 4 3SiO 1 / 2 ) a (R 4 2R N SiO 1 / 2 ) b (R 4 2SiO 2 / 2 ) c (R 4 R N SiO2 / 2 ) d (R 4 SiO 3 / 2 ) e (R N SiO 3 / 2 ) f (ZO 1 / 2 ) h may include a resin containing trifunctional (T'') units, where R 4 and R N are as defined above, subscript f > 1, 2 < (e + f) < 10,000, 0 < (a + b) / (e + f) < 3, 0 < (c + d) / (e + f) < 3, and 0 < h / (e + f) < 1.5. Alternatively, the aminopropyl-functional silsesquioxane resin may include the unit formula (N2-19): (R 4 SiO 3 / 2 ) e (R N SiO 3 / 2 ) f (ZO 1 / 2 ) h where R 4 , R N , Z, and subscripts h, e, and f are as defined above. Alternatively, the aminopropyl-functional silsesquioxane resin may further include difunctional (D'') units, and the aminopropyl-functional silsesquioxane resin may, in addition to the above T units, include units of the formula (R 4 2SiO 2 / 2 ) c (R 4 R N SiO 2 / 2 ) d , i.e., a D''T'' resin, where subscripts c and d are as defined above. Alternatively, the aminopropyl-functional silsesquioxane resin may further include monofunctional (M'') units of the formula (R 4 3SiO 1 / 2 ) a (R 4 2R N SiO 1 / 2 ) b , i.e., an M''D''T'' resin, where subscripts a and b are as defined above for the unit formula (E2-1).

[0249] Alternatively, the (N) aminopropyl-functionalized organosilicon compound may have the unit formula (N3-1): [(R 1 (3-gg) R N gg Si) ff NH (3-ff) hh wherein R N is as defined above, each R 1 is independently selected from the group consisting of alkyl and aryl groups as defined above, each subscript ff is independently 1 or 2 as defined above, the subscript gg is independently 0, 1, or 2 as defined above, and the subscript h has a value such that 1 < hh < 10 as defined above.

[0250] The aminopropyl-functionalized organosilicon compound prepared in step III) of the process described herein can be any one of the above aminopropyl-functionalized organosilicon compounds. Alternatively, the reductive amination reaction product can include a mixture of two or more of the aminopropyl-functionalized organosilicon compounds.

[0251] Alternatively, the process described herein can be used to produce an aminopropyl-functionalized organosilicon compound that is unstable to hydrolysis. The aminopropyl-functionalized organosilicon compound that is unstable to hydrolysis can be, for example, any one of the (N1) aminopropyl-functionalized silanes and / or (N2) aminopropyl-functionalized polyorganosiloxanes of the formulas shown above in which at least one R 4 is a hydrocarbon oxy group or an acyloxy group, any (N3) aminopropyl-functionalized silazane, or any aminopropyl-functionalized polyorganosiloxane oligomer of formula (N2-10a) or (N2-11a) as described and exemplified above.

Examples

[0252] ​These examples are provided to illustrate the invention to one of ordinary skill in the art and should not be construed as limiting the scope of the invention as set forth in the claims. The starting materials used in the examples are listed in Table 1 below.

[0253] [Table 1]

[0254] In this Reference Example 1, the formula

[0255] [ka] 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)dipropanal was synthesized as follows: In a nitrogen-filled glovebox, Rh(acac)(CO)2 (25.2 mg), Ligand 1 (150.5 mg), and toluene (17.07 g) were added to a 30 mL glass vial using a magnetic stir bar. The mixture was stirred on a stir plate until a homogenous solution was formed. The catalyst solution was transferred to an airtight syringe equipped with a metal valve and subsequently removed from the glovebox. In a ventilated fume hood, 1,3-divinyltetramethyldisiloxane (1000 g) was charged to a 2 L autoclave reactor. The reactor was sealed and mounted in a holder. The reactor was pressurized to 100 psig (689.5 kPa) with nitrogen via a dip tube and carefully released through a valve connected to the headspace. This process was repeated three times for reactor headspace inerting. The reactor was then pressure tested by pressurizing with nitrogen to 300 psig (2068.4 kPa). After releasing the pressure, the catalyst solution was added to the reactor through the sample loading port. The reactor was pressurized with syngas to 100 psig (689.5 kPa) and then released three times before pressurizing to 80 psig (551.6 kPa) through the dip tube. The reaction temperature was set to 50°C until gas uptake slowed, then the temperature was set to 80°C. The agitation speed was set to 800 RPM. Once the desired temperature was reached, the reactor was connected to an intermediate cylinder containing syngas. The pressure was set to 100 psig (689.5 kPa). The progress of the reaction was monitored by a data logger that measured the pressure in the 300 mL intermediate cylinder as syngas was fed to the reactor through a pressure reducing regulator. A conversion of over 98% was observed after 22.5 hours. The n / i ratio of the final product 1 Determined by 1 H NMR analysis.

[0256] In this Comparative Example 2, 18 g of 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)dipropanal prepared as described in Example 1 was charged to a 300 mL autoclave reactor along with toluene solvent (18 g) and Ni-5256P catalyst (4.1 g). The reactor was sealed and the headspace inerted with nitrogen. Ammonia (74.6 g, 30 equiv.) was added and the reactor was pressurized to 550 psig (3792.1 kPa) with hydrogen. The reactor was heated to 90° C. and hydrogen was added until the pressure was 100 psig (689.5 kPa) higher than the reactor pressure at the reaction temperature. The reaction pressure was observed to be 940 psig (6481.1 kPa). The reductive amination was carried out at 90° C. and 825 RPM for 4 hours. The reactor was cooled and vented. The reaction product was collected, filtered to remove the catalyst, and the solvent was removed using a rotary evaporator to collect 17.0 g of concentrated product, which was 59.7 wt% 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)bis(propan-1-amine) as analyzed using GC-FID.

[0257] In this Reference Example 3, the DP of 560 and the formula

[0258] [ka] A bis(propylaldehyde-terminated) polydimethylsiloxane having an average of 558 dimethylsiloxy (D) units per molecule (M) was prepared as follows: In a nitrogen-filled glove box, Rh(acac)(CO)2 (90.6 mg, 0.350 mmol), Ligand 1 (550 mg, 0.656 mmol), and toluene (51.43 g, 558 mmol) were added to a 120 mL glass bottle using a magnetic stir bar. The mixture was stirred on a stir plate until a homogenous solution was formed. A portion of this solution (1.45 g) was transferred to an airtight syringe equipped with a metal valve and subsequently removed from the glove box. In a ventilated fume hood, a bis(propylaldehyde-terminated) polydimethylsiloxane having an average of 558 dimethylsiloxy (D) units per molecule (M) was dissolved in 100 mL of water.Vi 2D 558 Bis-dimethylvinylsiloxy terminated polydimethylsiloxane (195.3 g, 4.68 mmol) with dimethylvinylsiloxy was charged into a 300 mL Parr reactor. The reactor was sealed and mounted in a holder. The reactor was pressurized to 100 psi (689.5 kPa) with nitrogen through a dip tube and carefully released three times through the valve connected to the head space. The reactor was then pressure tested by pressurizing to 300 psi (2068.4 kPa) with nitrogen. After releasing the pressure, the catalyst solution was added to the reactor through the sample load port. The reactor was pressurized to 100 psi (689.5 kPa) with syngas and then released three times before pressurizing to 80 psi (551.6 kPa) through a dip tube. The reaction temperature was set to 90° C. The agitation speed was set to 600 RPM. Once the desired temperature was reached, an intermediate cylinder containing syngas was connected to the reactor. The pressure was set at 100 psi (689.5 kPa). The progress of the reaction was monitored by a data logger that measured the pressure in a 300 ml intermediate cylinder as syngas was fed to the reactor through a pressure reducing regulator. The reaction was run for 4 hours. The resulting product contained bis(propylaldehyde terminated) polydimethylsiloxane with a DP of 560. The product was 1 H and 29 It was characterized by Si NMR.

[0259] In this Comparative Example 4, the compound of the formula:

[0260] [ka] A bis(3-aminopropyl) terminated poly(dimethylsiloxane) having a DP of 560 (where the subscript qq was 558) was prepared as follows: In a 2 L autoclave reactor was added 100 mL of dipropionoterminated poly(dimethylsiloxane), (poly[oxy(dimethylsilylene)], α-[dimethyl(3-oxopropyl)silyl]-ω-[[dimethyl(3-oxopropyl)silyl]oxy], or (C2H6OSi) n C 10 H22 Charged with O3Si2 (where n=560) (595 g), toluene (399 g), and 5 wt% Rh / C (36.5 g). The reactor was sealed and the headspace was inerted with nitrogen. The mixture was stirred at 820 rpm, ammonia (44 g) was added, and the mixture was stirred for 18 minutes. The reactor was pressurized to 615 psig (4240.3 kPa) with hydrogen and heated to 60°C. The reactor pressure was 683 psig (4709.1 kPa). The reactor pressure was increased to 795 psig (5481.3 kPa) with hydrogen and the reaction was run for 4 hours with continuous addition of hydrogen. The reactor was cooled and vented. The reaction product was collected, filtered to remove the catalyst, and the solvent was removed by rotary evaporation to collect 595.8 g of product. The product was 29 Characterized by Si analysis, GPC, and viscosity. Octamethylcyclotetrasiloxane content was determined by GC analysis. 29 Si NMR analysis showed 78% -propyl-NH2 end-capped polydimethylsiloxane.

[0261] In this Reference Example 5, 3-1,1,1,3,5,5,5-heptamethyltrisiloxane-3-yl)propanal was prepared as follows. In a nitrogen-filled glove box, Rh(acac)(CO)2 (13.6 mg, 0.0525 mmol), Ligand 1 (84.5 mg, 0.101 mmol), and toluene (10.0 g, 108.5 mmol) were added to a 30 mL glass vial using a magnetic stir bar. The mixture was stirred on a stir plate until a homogeneous solution was formed. The solution was transferred to an airtight syringe equipped with a metal valve and subsequently removed from the glove box. In a ventilated fume hood, vinylmethylbis(trimethylsiloxy)silane (MD ViM) (1000 g, 4.02 mol) was loaded into a 2 L autoclave reactor. The reactor was sealed and mounted in a holder. The reactor was pressurized to 100 psi (689.5 kPa) with nitrogen through a dip tube and carefully released three times through the valve connected to the headspace. The reactor was then pressure tested by pressurizing to 300 psi (2068.4 kPa) with nitrogen. After releasing the pressure, the catalyst solution was added to the reactor through the sample loading port. The reactor was pressurized to 100 psi (689.5 kPa) with syngas and then released three times before pressurizing to 80 psi (551.6 kPa) through a dip tube. The reaction temperature was set to 75° C. The stirring speed was set to 800 RPM. Once the desired temperature was reached, an intermediate cylinder containing syngas was connected to the reactor. The pressure was set to 100 psi (689.5 kPa). The progress of the reaction was monitored by a data logger that measured the pressure in the intermediate cylinder as synthesis gas was fed to the reactor through a pressure reducing regulator. The resulting product was 3-(1,1,1,3,5,5,5-heptamethyltrisiloxane-3-yl)propanal (MD Pr-ald Containing crude 3-(1,1,1,3,5,5,5-heptamethyltrisiloxane-3-yl)propanal (MD Pr-ald A portion of 3-(1,1,1,3,5,5,5-heptamethyltrisiloxane-3-yl)propanal (MD) was purified by vacuum distillation. The vacuum distillation apparatus consisted of a 500 three-neck round bottom flask with a PTFE coated magnetic stir bar, an electric heating mantle with internal temperature controlled by a J-CHEM™ as measured by a thermoprobe, and a 12 inch (30.48 cm) Vigreux column connected to a 250 mL pre-tared collection flask. A vacuum manifold was connected to a system that included a vacuum gauge and a nitrogen line to regulate pressure and break vacuum. Water cooling was used on the distillate condenser, and a dry ice trap was placed between the distillation system and the diaphragm vacuum pump to capture lower boiling components. A thermometer was installed to measure the temperature of the overhead vapors. Crude 3-(1,1,1,3,5,5,5-heptamethyltrisiloxane-3-yl)propanal (MD) was purified by vacuum distillation. Pr-aldDistillation was carried out by charging 341.5 g of 1,1,1,3,5,5,5-heptamethyltrisiloxane-3-yl)propanal (MDM) to a 500 mL reboiler. The distillation was carried out at a pressure of 2 Torr (266.6 Pa). A light cut (13 g) was collected at a pot temperature of 76° C. and an overhead temperature of 66° C. Purified 3-(1,1,1,3,5,5,5-heptamethyltrisiloxane-3-yl)propanal (MDM) was obtained. Pr-ald A main fraction containing 243 g of dimethylformamide (M) was collected at a pot temperature of 80-85° C. and an overhead temperature of 67-69° C. 55 g of bottoms material was also collected.

[0262] In this Comparative Example 6, N-(3-(1,1,1,3,5,5,5-heptamethyltrisiloxan-3-yl)propyl)butan-1-amine was synthesized as follows: A 300 mL autoclave reactor was charged with 12.0 g of 3-(1,1,1,3,5,5,5-heptamethyltrisiloxan-3-yl)propanal prepared as described in Reference Example 5, toluene (48.5 g), n-butylamine (3.8 g), and 5 wt. % Rh / C (1.4 g). The reactor was sealed and the headspace was inerted with nitrogen. The mixture was stirred at 800 rpm for 5 minutes. The reactor was pressurized to 463 psig (3192.3 kPa) with hydrogen and heated to 60° C. The reactor pressure was 452 psig (3116.4 kPa). The reactor pressure was increased to 651 psig (4488.5 kPa) with hydrogen and the reaction was run for 4 hours with continuous addition of hydrogen. The reactor was cooled and vented. The reaction product was collected and the reactor was rinsed with toluene to collect 75.2 g of material. A portion of the material was filtered through a syringe filter, stripped of solvent, and analyzed by gas chromatography as well as HPLC. 1 H and 13 Characterization was by C NMR analysis, which confirmed the presence of N-(3-(1,1,1,3,5,5,5-heptamethyltrisiloxan-3-yl)propyl)butan-1-amine. GC analysis showed the N-(3-(1,1,1,3,5,5,5-heptamethyltrisiloxan-3-yl)propyl)butan-1-amine product to be present at 86 area %.

[0263] In this Example 7, 3-(1,1,1,3,5,5,5-heptamethyltrisiloxan-3-yl)propan-1-amine and N-(3-(1,1,1,3,5,5,5-heptamethyltrisiloxan-3-yl)propyl)butan-1-amine were synthesized as follows: A 300 mL autoclave reactor was charged with 11.7 g of 3-(1,1,1,3,5,5,5-heptamethyltrisiloxan-3-yl)propanal prepared as described in Reference Example 5, toluene (48.4 g), n-butylamine (3.9 g, 1.25 equivalents), and 5 wt.% Rh / C (1.2 g). The reactor was sealed and the headspace was inerted with nitrogen. Ammonia (18.3 g, 25 equivalents) was added to the mixture and the reactor pressure was 114 psig (786 kPa). The mixture was stirred at 800 rpm for 7 minutes. The reactor was charged with hydrogen to 480 psig (3309.5 kPa) and hydrogenation was stopped. The reactor was heated to 60° C. at which point the reaction pressure was 580 psig (3999 kPa). The reactor pressure was increased to 798 psig (5502 kPa) with hydrogen and the reaction was run for 4 hours with continuous addition of hydrogen. The reactor was cooled and vented. The reaction product was collected and the reactor was rinsed with toluene to collect 109.6 g of liquid. A portion of the liquid was filtered through a syringe filter, stripped of solvent, and analyzed by gas chromatography as well as HPLC. 1 H and 13 Characterization was performed using C NMR analysis, which revealed that Showed 67.4 GC / FID area % 3-(1,1,1,3,5,5,5-heptamethyltrisiloxan-3-yl)propan-1-amine and 18.6 GC / FID area % N-(3-(1,1,1,3,5,5,5-heptamethyltrisiloxan-3-yl)propyl)butan-1-amine, which combined is 86 area % product by GC.

[0264] In this Comparative Example 8, 3-(1,1,1,3,5,5,5-heptamethyltrisiloxan-3-yl)propan-1-amine was synthesized as follows: A 300 mL autoclave reactor was charged with 12.1 g of 3-(1,1,1,3,5,5,5-heptamethyltrisiloxan-3-yl)propanal prepared as described in Reference Example 30, toluene (48.4 g), and 5 wt. % Rh / C (1.3 g). The reactor was sealed and the headspace was inerted with nitrogen. Agitation at 800 rpm was started, ammonia (19.9 g, 26.9 equiv.) was added to the mixture, and the reactor pressure was 117 psig (806.7 kPa). The reaction was charged with hydrogen to 444 psig (3061.3 kPa) and the hydrogenation valve was closed. The reactor was heated to 60° C. at which point the reaction pressure was 610 psig (4205.8 kPa). The reactor was pressurized to 463 psig (3192.3 kPa) with hydrogen and heated to 60° C. The reactor pressure was increased to 816 psig (5626.1 kPa) with hydrogen and the reaction was run for 4.5 hours with continuous addition of hydrogen. The reactor was cooled and vented. The desired product was collected to give 60.6 g of liquid. A portion of the liquid was filtered through a syringe filter, stripped of solvent, and analyzed by gas chromatography as well as HPLC. 1 H and 13 Characterization by C NMR and GC / FID analysis confirmed the presence of 3-(1,1,1,3,5,5,5-heptamethyltrisiloxan-3-yl)propan-1-amine in the reaction product. GC analysis showed 79 area % 3-(1,1,1,3,5,5,5-heptamethyltrisiloxan-3-yl)propan-1-amine product.

[0265] Example 7 showed improved yield over Comparative Example 8 using the process of the present invention.

[0266] In this Example 9, a compound of the formula:

[0267] [ka] A bis(3-aminopropyl) terminated poly(dimethylsiloxane) having a DP of 560 (where the subscript qq was 558) was prepared as follows: In a glass container was added 100 mL of dipropionoterminated poly(dimethylsiloxane), (poly[oxy(dimethylsilylene)], α-[dimethyl(3-oxopropyl)silyl]-ω-[[dimethyl(3-oxopropyl)silyl]oxy], or (C2H6OSi) n C 10 H 22 O3Si2 (where n=558) (70.0 g) and toluene (71.0 g) were charged to form a solution. To this solution was charged n-butylamine (0.51 g, 2.1 equiv.) and mixed thoroughly. The mixture became cloudy. MgSO4 (3.0 g) was added, mixed, and the mixture was held for 16 hours. The mixture was filtered to remove the MgSO4, yielding 140 g of a clear liquid. The liquid was 1 Analysis by 1 H NMR confirmed the presence of butylimine.

[0268] In a 300 mL autoclave reactor, add the diimine-terminated siloxane prepared in this Example 9, (poly[oxy(dimethylsilylene)], α-[dimethyl(3-(butylimino)propylsilyl]-ω-[[dimethyl(3-(butylimino)propylsilyl]oxy], or (CHOSi) n C 18 H 40 The reactor was charged with 140 g of O3N2Si2 (where n=558) solution, and 3.5 g of 5 wt.% Rh / C. The reactor was sealed and the headspace was inerted with nitrogen. The mixture was stirred at 800 rpm, ammonia (7.1 g) was added, and the mixture was stirred for 13 minutes. The reactor was pressurized to 259 psig (1785.7 kPa) with hydrogen and heated to 60°C. The reactor pressure was 290 psig (1999.5 kPa). The reactor pressure was increased to 790 psig (5446.9 kPa) with hydrogen and the reaction was run for 4 hours with continuous addition of hydrogen. The reactor was cooled and vented. The reaction product was collected, filtered to remove the catalyst, and the solvent was removed by rotary evaporation to collect 70.7 g of product. The product was 29 Si and1 It was characterized by 1 H NMR analysis. 29 Si NMR analysis showed 91% primary amino functional end-capped polydimethylsiloxane.

[0269] In this Example 10, 50.33 g of 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)dipropanal prepared as described in Example 1 was charged to a 300 mL autoclave reactor along with methanol (15.1 g), Ni-5256P (6.01 g), and n-butylamine (29.7 g). The reactor was sealed, stirring was started at 400 RPM, and the headspace was inerted with nitrogen. The stirring rate was increased to 800 RPM, and ammonia (35.3 g, 10 equiv.) was added. The reactor was pressurized to 505 psig with hydrogen. The reactor was heated to 90° C. and hydrogen was added until the pressure was 805 psig. The reductive amination was carried out at 90° C. for approximately 16 hours. The reactor was cooled and vented. The reaction product was collected, filtered to remove the catalyst, and the solvent was removed using a rotary evaporator to collect 49.8 g of concentrated product, which was 72.4 wt % 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)bis(propan-1-amine) as analyzed using GC-FID.

[0270] In this Example 11, 50.07 g of 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)dipropanal prepared as described in Example 1 was charged to a 300 mL autoclave reactor along with methanol (15.05 g), Ni-5256P (6.02 g), and iso-butylamine (29.72 g). The reactor was sealed, stirring was started at 400 RPM, and the headspace was inerted with nitrogen. The stirring rate was increased to 820 RPM, and ammonia (35.3 g, 10 equiv.) was added. The reactor was pressurized to 506 psig with hydrogen. The reactor was heated to 90° C. and hydrogen was added until the pressure was 802 psig. The reductive amination was carried out at 90° C. for approximately 16 hours. The reactor was cooled and vented. The reaction product was collected, filtered to remove the catalyst, and the solvent was removed using a rotary evaporator to collect 48.7 g of concentrated product, which was 79.2 wt% 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)bis(propan-1-amine) as analyzed using GC-FID.

[0271] In this Example 12, 25.1 g of 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)dipropanal prepared as described in Example 1 was charged to a glass vessel along with methanol (25.1 g) and 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)bis(propan-1-amine) (30.0 g) to form an imine solution. This solution was charged to a 300 mL autoclave reactor and Ni-5256P (2.76 g) was added. The reactor was sealed, stirring was started at 820 RPM, and the headspace was inerted with nitrogen. The stirring rate was continued at 820 RPM and ammonia (37.3 g) was added. The reactor was pressurized to 519 psig with hydrogen. The reactor was heated to 90° C. and hydrogen was added until the pressure reached 773 psig. The reductive amination was carried out at 90° C. for approximately 16 hours. The reactor was cooled and vented. The reaction product was collected, filtered to remove the catalyst, and the solvent was removed using a rotary evaporator to collect 48.7 g of concentrated product. The concentrated product was 79.2 wt % 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)bis(propan-1-amine) as analyzed using GC-FID.

[0272] Hydroformylation of branched organosilicon oligomers to produce aldehydes

[0273] [ka] In this Reference Example 13, 3-(1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)trisiloxane-3-yl)propanal of formula (above) was synthesized as follows: In a nitrogen-filled glove box, Rh(acac)(CO)2 (47.5 mg), Ligand 1 (294 mg), and toluene (60.2 g) were added to a glass bottle using a magnetic stir bar. The mixture was stirred on a stir plate until a homogeneous solution was formed. A portion of this catalyst solution (2.88 g) was transferred to an airtight syringe equipped with a metal valve and subsequently removed from the glove box. In a ventilated fume hood, 1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)-3-vinyltrisiloxane (180 g) was charged to a 300 mL pressure reactor. The reactor was sealed. With stirring at 600 RPM, the reactor was pressurized to 100 psig with nitrogen through a dip tube and carefully released through a valve connected to the headspace. This process was repeated three times for reactor headspace inerting. The reactor was then pressure tested by pressurizing to 300 psig with nitrogen. After releasing the pressure, the catalyst solution was added to the reactor through the sample loading port. The reactor was pressurized to 100 psig with syngas and then released three times before pressurizing to 100 psig through a dip tube. The reaction temperature was set at 80°C. The stirring speed was set at 600 RPM. Once the desired temperature was reached, the reactor was connected to an intermediate cylinder containing syngas. The pressure was set at 100 psig. The progress of the reaction was monitored by a data logger that measured the pressure in the 300 mL intermediate cylinder as syngas was fed to the reactor through a pressure reducing regulator. A conversion rate of over 99% was observed after 16 hours. The n / i ratio was 0.01 to 0.01 for the final product. 1 The ratio was determined to be 7.5 to 1 by 1 H NMR analysis.

[0274] [ka]

[0275] In this Comparative Example 14, 40 g of 3-(1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)trisiloxan-3-yl)propanal prepared as described in Example 13 was charged to a 300 mL autoclave reactor along with THF (40.03 g) and Ni-5256P (3.99 g). The reactor was sealed and the headspace was inerted with nitrogen. Ammonia (29.0 g, 15 equiv.) was added and the reactor was pressurized to 530 psig with hydrogen. The reactor was heated to 100° C. and hydrogen was added until the pressure was 100 psig higher than the reactor pressure at the reaction temperature. The reductive amination was carried out at 100° C., 920 psig, and 800 RPM for 16 hours. The reactor was cooled and vented. The reaction product was collected, filtered to remove the catalyst, and the solvent was removed using a rotary evaporator to collect 33.8 g of concentrated product, which was 44.1 wt% 3-(1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)trisiloxan-3-yl)propan-1-amine as analyzed using GC-FID.

[0276] [ka]

[0277] In this Example 15, 30 g of 3-(1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)trisiloxan-3-yl)propanal prepared as described in Example 13 was charged to a glass round-bottom flask. THF solvent (60 g) was added to form a solution. N-butylamine (6.53 g, 1.05 equiv.) was added to the solution while stirring with a PTFE-coated magnetic stir bar. A mild exotherm was observed. MgSO4 was added to adsorb water from the solution. The MgSO4 was removed by filtration to give 95 g of a solution containing N-butyl-3-(1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)trisiloxan-3-yl)propan-1-imine. The imine-containing solution was charged to a 300 mL autoclave reactor along with Ni-5256P catalyst (3.01 g). The reactor was sealed and the headspace was inerted with nitrogen. Ammonia (21.7 g, 15 equiv.) was added and the reactor was pressurized to 520 psig with hydrogen. The reactor was heated to 100° C. and hydrogen was added until the pressure was 100 psig higher than the reactor pressure at the reaction temperature. The reductive amination was carried out at 100° C., 925 psig, and 800 RPM for 20 hours. The reactor was cooled and vented. The reaction product was collected, filtered to remove the catalyst, and the solvent was removed using a rotary evaporator to collect 25.0 g of concentrated product. The condensed product was 75.9% by weight 3-(1,1,1,5,5,5-hexamethyl-3-((trimethylsilyl)oxy)trisiloxan-3-yl)propan-1-amine as analyzed using GC-FID. This example and the comparative example immediately preceding it demonstrate the dramatic increase in yield using the process of the present invention instead of attempting to form primary amino-functional organosilicon compounds directly from the corresponding aldehyde-functional organosilicon compounds with ammonia.

[0278] In this Reference Example 16, the formula, M 0.24 M プロパナールアルデヒド 0.139 T Ph 0.62T-phenyl resin propanal was synthesized as follows: In a nitrogen filled glove box, Rh(acac)(CO)2 (48.0 mg), Ligand 1 (311.9 mg), and toluene (59.9 g) were combined to form a homogeneous catalyst solution. A portion of this catalyst solution (5.8 g) was transferred to an airtight syringe equipped with a metal valve and subsequently removed from the glove box. In a ventilated fume hood, M dissolved in toluene (90 g) was 0.24 M Vi 0.139 T Ph 0.62 (90 g) was loaded into a 300 mL pressure reactor. The reactor was sealed. With stirring at 600 RPM, the reactor was pressurized to 100 psig with nitrogen through a dip tube and carefully released through a valve connected to the headspace. This process was repeated three times for reactor headspace inerting. The reactor was then pressure tested by pressurizing to 300 psig with nitrogen. After releasing the pressure, the catalyst solution was added to the reactor through the sample loading port. The reactor was pressurized to 100 psig with syngas and then released three times before pressurizing to 100 psig through a dip tube. The reaction temperature was set to 70° C. The stirring speed was set to 600 RPM. Once the desired temperature was reached, the reactor was connected to an intermediate cylinder containing syngas. The pressure was set to 100 psig. The progress of the reaction was monitored by a data logger that measured the pressure in the 300 mL intermediate cylinder as syngas was fed to the reactor through a pressure reducing regulator. The final product 1 Greater than 99% conversion was observed after 16 h as determined by H NMR analysis. The toluene was removed to leave the product as a viscous liquid.

[0279] In this Example 17, 25.8 g of M 0.24 M プロパナールアルデヒド 0.14 T Ph 0.62was charged to a glass round bottom flask. THF solvent (51.6 g) was added to form a solution. N-butylamine (2.55 g, 1.1 equiv.) was added to the solution while stirring with a PTFE coated magnetic stir bar. MgSO4 was added to adsorb water from the solution. The MgSO4 was removed by filtration to give a solution containing the corresponding N-butylimine. The imine-containing solution was charged to a 300 mL autoclave reactor along with 5% Ru / C catalyst (2.6 g). The reactor was sealed and the headspace was inerted with nitrogen. Ammonia (8.3 g, ca. 15 equiv.) was added and the reactor was pressurized with hydrogen to 530 psig. The reactor was heated to 80° C. and hydrogen was added until the pressure was 880 psig. The reductive amination was carried out at 80° C., 880 psig, and 800 RPM for 18.5 hours. The reactor was cooled and vented. The reaction product was collected, filtered to remove the catalyst, and the solvent was removed using a rotary evaporator to collect 27.2 g of concentrated product. 1 H and 13 M as determined by C NMR 0.24 M プロピルアミン 0.139 T Ph 0.52 This Example 17 shows that the process of the present invention can be used to make a primary amino-functional polyorganosiloxane resin.

[0280] In this Example 18, 299.1 g of 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)dipropanal prepared as described in Example 1 was charged into a glass round-bottom flask. Isopropanol solvent (898.1 g) was added to form a solution. Iso-butylamine (196.1 g, 2.1 equivalents) was added to the solution while stirring with a mechanical stirrer. The resulting imine-functional organosilicon compound in isopropanol solution, as well as ammonia and hydrogen, were passed through a continuous tubular (trickle-bed) reactor at flow rates of 0.18 mL / min, 0.036 mL / min, and 8.6 sccm, respectively. The inner diameter of the tubular reactor was 3 mm and contained 6.03 g of Ni-5256E catalyst. The reactor was controlled at 100°C. The reactor effluent was collected and volatiles were removed under vacuum to leave a liquid. The liquid contained more than 50% 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)bis(propan-1-amine) as analyzed using GC-FID. This example demonstrated that the reductive amination reaction of the present invention can be carried out in a continuous mode without plugging.

[0281] In this Comparative Example 19, 300.0 g of 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)dipropanal prepared as described in Example 1 was charged to a glass round-bottom flask. Isopropanol solvent (1200 g) was added to form a solution. The resulting aldehyde-functional organosilicon compound in isopropanol solution, as well as ammonia and hydrogen, were passed through a continuous tubular (trickle-bed) reactor at flow rates of 0.30 mL / min, 0.056 mL / min, and 14 sccm, respectively. The inner diameter of the tubular reactor was 3 mm and contained 6.0 g of Ni-5256E catalyst. The reactor was controlled at 100° C. The reactor plugged soon after starting the feed flow due to the formation of solids in the reactor, and the reactor effluent was not collected.

[0282] Example 18 shows the advantage of improved processability over Comparative Example 19 when using the process of the present invention.

[0283] In this prophetic Example 20, methanol (30 g) and Ni-5256P (6.0 g) are charged into a 300 mL autoclave reactor and the reactor is inerted with nitrogen. Ammonia (35 g, 10 equivalents) is added. The mixture is heated to 110° C., and then hydrogen is added until the pressure reaches 1000 psig. 50 g of 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)dipropanal prepared as described in Example 1 is pumped into the stirred reaction mixture (800 RPM) over a period of 60 minutes. Hydrogen is fed continuously at 1000 psig during this time. After the addition of 3,3'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)dipropanal is complete, the reaction is continued at 110° C. and 1000 psig for 2 hours. The reactor is cooled and vented. The reaction product is collected, filtered to remove the catalyst, and the solvent is removed using a rotary evaporator to collect the concentrated product.

[0284] Industrial Applicability When carrying out the reductive amination of propylaldehyde-functional organosilicon compounds with ammonia, primary imine-functional organosilicon compounds are first produced, which are converted to the desired primary aminopropyl-functional organosilicon compounds through reductive amination.However, primary imine groups are relatively unstable and can cause the self-condensation of propylimine-functional organosilicon compounds to form higher molecular weight by-products such as triazines and secondary amines, often resulting in significant yield loss.Furthermore, the formation of these by-products often leads to increased product viscosity and / or the formation of solids, which makes catalyst separation difficult and limits the opportunity to carry out reductive amination reactions using continuous reactor equipment.A method for minimizing the formation of these by-products is desirable to improve the yield and process robustness of reductive amination reactions to produce aminopropyl-functional organosilicon compounds.The process described herein addresses this issue by using a primary amine source to produce secondary propylimine-functional organosilicon compounds. The secondary imine is then treated with excess ammonia, hydrogen, and a hydrogenation catalyst to give the primary aminopropyl-functional organosilicon compound, regenerating the primary amine source which can be recycled for use in subsequent dehydration imine formation reactions.

[0285] Furthermore, during the reductive amination reaction of propylaldehyde-functional organosilicon compounds with ammonia, one molar equivalent of water is generated per mole of aldehyde functionality as a by-product of the formation of primary imine groups.Certain aminopropyl-functional organosilicon compounds are unstable to hydrolysis and react with water under the conditions used in this reductive amination reaction, and this instability leads to side reactions that can generate additional undesirable by-products.Alkoxy- or acyloxy-functionalized silanes, silazanes, and branched and linear oligomeric siloxanes, such as the oligomeric aminopropyl-functional siloxanes derived from the branched propylaldehyde-functional siloxane oligomers (E2-10) or (E2-11) mentioned above, are more susceptible to side reactions in the presence of water than other aminopropyl-functional polyorganosiloxanes.

[0286] Without wishing to be bound by theory, it is believed that the ability to remove water in step II) of the process described herein (i.e., after secondary imine group and water formation via dehydration imine formation reaction begins in step I) and before reductive amination reaction in step III) of the process described herein) can improve the yield of primary aminopropyl functional organosilicon compounds as products, even when using hydrolytically unstable propylaldehyde functional organosilicon compounds as starting materials and / or producing hydrolytically unstable propylimine functional organosilicon compounds and hydrolytically unstable aminopropyl functional organosilicon compounds. Furthermore, due to the improved stability of secondary imine groups over primary imine groups, the present invention provides an opportunity to improve the yield and robustness of reductive amination reactions by providing options to address the above problems. Secondary imine groups are less prone to decomposition via self-condensation, which increases the yield of the process while also allowing alternative processing options, such as the use of continuous reactors. In addition, the increased stability of the secondary imine functional organosilicon compound intermediate allows the water generated during secondary imine group formation to be optionally removed using various techniques, including distillation or the use of drying agents.The ability to remove water during the early stages of the process minimizes or eliminates the formation of certain by-products when using organosilicon compounds with lower hydrolytic stability in the process.Finally, the generation of secondary imine functional organosilicon compounds as intermediates protects the aldehyde group (of the aldehyde functional organosilicon compound starting material) from oxidative decomposition.

[0287] Without wishing to be bound by theory, it is believed that the process may also provide less or no salt by-product streams, shorter reaction times, and / or lower production of cyclic siloxane by-products than conventional condensation reaction processes.Furthermore, the hydroformylation and reductive amination may be carried out in one single reactor without the need to isolate intermediates and may have minimal process steps.

[0288] Without wishing to be bound by theory, it is believed that another advantage of the present invention is that the aminopropyl functional organosilicon compound produced has a high proportion of linear aminopropyl functional groups, and this is because the propylaldehyde functional organosilicon compound with branched propylaldehyde moiety reacts and decomposes during the process described herein, so that they can be easily removed.In addition, the aminopropyl functional organosilicon compound produced can have reduced cyclic siloxane (e.g., octamethylcyclotetrasiloxane, D4) content compared to the aminopropyl functional organosilicon compound produced via condensation chemistry using carboxylic acid catalyst or equilibration chemistry using base catalyst.

[0289] Definitions and Use of Terms All amounts, ratios, and percentages are by weight unless otherwise specified. The amounts of all starting materials in the composition total 100% by weight. The Summary and Abstract are incorporated herein by reference. The articles "a," "an," and "the" each refer to one or more, unless otherwise indicated by the context of the specification. The singular includes the plural unless otherwise indicated. The transitional phrases "comprising," "consisting essentially of," and "consisting of" are used as described in Sections §2111.03 I., II., and III of the Manual of Patent Examining Procedure Ninth Edition, Revision 08.2017, Last Revised January 2018. The term "hydrolytically unstable" refers to any organosilicon compound that reacts with water at temperatures below 120°C. The hydrolytically unstable organosilicon compounds herein include any organosilicon compound used or produced that reacts with water at temperatures below 120° C. Examples include any of the (B) alkenyl-functional organosilicon compounds, any of the (E) aldehyde-functional organosilicon compounds, any of the (L) imine-functional organosilicon compounds, and any primary amino-functional organosilicon compounds prepared as described herein that meet one or more of the following criteria: i) one or more R groups per molecule; 4 is acyloxy or hydrocarbyloxy, ii) the organosilicon compound is a silazane, and / or ii) any oligomeric polyorganosiloxane of formula (B2-10a), (E2-10a), (L2-10a), (N2-10a), as shown above, such as 1,3-di(aminopropyl)-1,1,3,3-tetramethyldisiloxane, (B2-11a), (E2-11a), (L2-11a), or (N2-11a), such as 3-(3,3,3-trimethyl-112-disiloxaneyl)propan-1-amine. Abbreviations used herein have the definitions in Table Z.

[0290] [Table 2]

[0291] The following test methods were used herein: FTIR: The concentration of silanol groups present in polyorganosiloxane resins (e.g., polyorganosilicate resins and / or silsesquioxane resins) was determined using FTIR spectroscopy according to ASTM standard E-168-16. GPC: The molecular weight distribution of polyorganosiloxanes was determined by GPC using an Agilent Technologies 1260 Infinity chromatograph and toluene as the solvent. The instrument was equipped with three columns, a PL Gel 5 μm, 7.5×50 mm guard column, and two PL Gel 5 μm, Mixed-C 7.5×300 mm columns. Calibration was performed using polystyrene standards. Samples were made by dissolving polyorganosiloxanes in toluene (approximately 1 mg / mL), and then the solution was immediately analyzed by GPC (flow rate of 1 mL / min, column temperature of 35° C., run time of 25 min). 29 Si NMR: The alkenyl content of the starting material (B) can be measured by the techniques described in "The Analytical Chemistry of Silicones," edited by A. Lee Smith, Vol. 112 of Chemical Analysis, John Wiley & Sons, Inc. (1991). Viscosity: Viscosity can be measured, for example, for polymers (e.g., certain (B2) alkenyl-functional polyorganosiloxanes and (E2) aldehyde-functional polyorganosiloxanes) having a viscosity of 120 mPa·s to 250,000 mPa·s on a Brookfield DV-III cone & plate viscometer equipped with a #CP-52 spindle at 25°C and 0.1 to 50 RPM. Those skilled in the art will recognize that as the viscosity increases, the rotation speed decreases and that appropriate spindles and rotation speeds can be selected.

[0292] The mixture of the aldehyde-functional organosilicon compound and the reductive amination reaction product from the above examples is 1 H,13 C NMR and 29 The conversion and yield in the above examples were mainly analyzed by Si NMR, GC / MS, GPC, and viscosity. 1 The results were based on 1 H NMR data.

[0293] EMBODIMENTS OF THE PRESENT DISCLOSURE In a first embodiment, the process for preparing an imine-functional organosilicon compound comprises: I) combining starting materials under conditions which result in a dehydration imine formation reaction, the starting materials being: (E) a propylaldehyde-functional organosilicon compound; and (F1) a primary amine source; optionally, (G) a hydrogenation catalyst; optionally, (J) a solvent; Optionally, (K) a desiccant; thereby forming a dehydrated imine-producing reaction product comprising (L) a propylimine-functional organosilicon compound and water; and Optionally, II) removing water; and and optionally, (L) isolating the imine-functional organosilicon compound.

[0294] In a second embodiment, a process for making an aminopropyl-functional organosilicon compound comprises carrying out the process of the first embodiment; III) combining a starting material under conditions to catalyze a reductive amination reaction, the starting material being: (L) a propylimine-functional organosilicon compound; (F2) ammonia, optionally, (G) a hydrogenation catalyst; (H) hydrogen; optionally, (J) a solvent; Optionally, (K) a desiccant; provided that (G) a hydrogenation catalyst is combined in at least one of steps I) and III); and combining, thereby forming a reductive amination reaction product comprising an aminopropyl-functional organosilicon compound and a primary amine source.

[0295] In a third embodiment, the process of the first embodiment or the second embodiment further comprises preparing the (E) propylaldehyde functional organosilicon compound by a hydroformylation process, the hydroformylation process comprising: 1) combining starting materials under conditions to catalyze a hydroformylation reaction, the starting materials being: (A) a gas containing hydrogen and carbon monoxide; (B) a vinyl-functional organosilicon compound; and (C) a rhodium / phosphoramidite ligand complex catalyst, thereby forming a hydroformylation reaction product comprising (E) a propylaldehyde-functional organosilicon compound; Optionally, 2) recovering (C) the rhodium / phosphoramidite ligand complex catalyst from the hydroformylation reaction product comprising (E) the propylaldehyde-functional organosilicon compound; and and optionally, 3) isolating the propylaldehyde-functional organosilicon compound.

[0296] In a fourth embodiment, in the process of any one of the first to third embodiments, the propylaldehyde-functional organosilicon compound is hydrolytically unstable, for example, as defined above.

[0297] In a fifth embodiment, in the process of the fourth embodiment, the aldehyde-functional organosilicon compound is represented by the formula

[0298] [ka] wherein each R 4 is independently selected from the group consisting of an alkyl group having 1 to 18 carbon atoms and an aryl group having 6 to 18 carbon atoms; Aldare independently selected expressions

[0299] [ka] where G is a divalent hydrocarbon group free of aliphatic unsaturation having 2 carbon atoms.

[0300] In a sixth embodiment, in the process of the fifth embodiment, each R 4 is methyl, R Ald is a linear propyl aldehyde.

[0301] In a seventh embodiment, in the process of any one of the first to fourth embodiments, the propylaldehyde-functional organosilicon compound is represented by the formula

[0302] [ka] wherein each R 13 is independently selected from the group consisting of an alkyl group having 1 to 18 carbon atoms and an aryl group having 6 to 18 carbon atoms; Ald are independently selected expressions

[0303] [ka] where G is a divalent hydrocarbon group free of aliphatic unsaturation having 2 carbon atoms.

[0304] In an eighth embodiment, in the process of the seventh embodiment, each R 13 is methyl, R Ald is a linear propyl aldehyde.

[0305] In a ninth embodiment, in the process of any one of the first to third embodiments, the propylimine-functional organosilicon compound is hydrolytically unstable, for example as defined above.

[0306] In a tenth embodiment, in the process of the ninth embodiment, the propylimine functional organosilicon compound is represented by the formula

[0307] [ka] wherein each R 4 is independently selected from the group consisting of an alkyl group having 1 to 18 carbon atoms and an aryl group having 6 to 18 carbon atoms; I are independently selected expressions

[0308] [ka] where G is a divalent hydrocarbon radical free of aliphatic unsaturation having 2, and R 19 is selected from alkyl groups of 1 to 18 carbon atoms, aryl groups of 6 to 18 carbon atoms, and organosilicon moieties.

[0309] In an eleventh embodiment, in the process of the tenth embodiment, each R 4 is methyl, G is linear, and each R 19 is an alkyl group of 1 to 4 carbon atoms.

[0310] In a twelfth embodiment, in the process of the eleventh embodiment, the propylimine-functional organosilicon compound is represented by the formula

[0311] [ka] wherein each R 13 is independently selected from the group consisting of alkyl groups of 1 to 18 carbon atoms and aryl groups of 6 to 18 carbon atoms; R I is the formula

[0312] [ka] where G is a divalent hydrocarbon radical free of aliphatic unsaturation having 2 carbon atoms, and R 19 is selected from the group consisting of alkyl groups of 1 to 18 carbon atoms, aryl groups of 6 to 18 carbon atoms, and organosilicon moieties.

[0313] In a thirteenth embodiment, in the process of the twelfth embodiment, each R 13 is methyl, G is linear, and each R 19 is an alkyl group of 1 to 4 carbon atoms.

[0314] In a fourteenth embodiment, in the process of the second embodiment, the aminopropyl-functional organosilicon compound is hydrolytically unstable, for example as defined above.

[0315] In a fifteenth embodiment, in the process of the fourteenth embodiment, the aminopropyl-functional organosilicon compound is represented by the formula

[0316] [ka] wherein each R 4 is independently selected from the group consisting of an alkyl group having 1 to 18 carbon atoms and an aryl group having 6 to 18 carbon atoms; N are independently selected expressions

[0317] [ka] where G is a divalent hydrocarbon group free of aliphatic unsaturation having 2 carbon atoms.

[0318] In a sixteenth embodiment, in the process of the fifteenth embodiment, each R 4 is methyl and G is linear.

[0319] In a seventeenth embodiment, in the process of the fourteenth embodiment, the amino functional organosilicon compound is represented by the formula

[0320] [ka] wherein each R 13 is independently selected from the group consisting of alkyl groups of 1 to 18 carbon atoms and aryl groups of 6 to 18 carbon atoms; R N is the formula

[0321] [ka] where G is a divalent hydrocarbon group free of aliphatic unsaturation having 2 carbon atoms.

[0322] In an eighteenth embodiment, in the process of the seventeenth embodiment, each R 13 is methyl and G is linear.

Claims

1. 1. A process for preparing a propylimine-functional organosilicon compound, said process comprising: I) combining starting materials under conditions which result in a dehydration imine formation reaction, the starting materials being: a propylaldehyde-functional organosilicon compound; A primary amine source; Optionally, a solvent; and optionally a hydrogenation catalyst; thereby forming a reaction product comprising a propylimine-functional organosilicon compound and water; with the proviso that when said hydrogenation catalyst is present in step I), step I) is carried out in the absence of hydrogen; Optionally, II) removing water produced by the dehydration imine production reaction in step I); and and optionally isolating said imine-functional organosilicon compound.

2. 1. A process for preparing an amino-functional organosilicon compound, said process comprising: Preparing the imine-functional organosilicon compound by carrying out the process of claim 1; III) combining starting materials under conditions to catalyze a reductive amination reaction, the starting materials being: the imine-functional organosilicon compound; Ammonia and Hydrogen, Optionally, said hydrogenation catalyst; and optionally said solvent; provided that the hydrogenation catalyst is combined in at least one of steps I) and III); thereby forming a reaction product comprising an aminopropyl-functional organosilicon compound.

3. Prior to step I), the method further comprises forming said propylaldehyde-functional organosilicon compound by a process comprising combining starting materials under conditions to catalyze a hydroformylation reaction, the starting materials being: (A) a gas containing hydrogen and carbon monoxide; (B) an alkenyl-functional organosilicon compound; and (C) a rhodium / ligand complex catalyst, wherein the ligand has the formula (C1), (C2), and / or (C3): Formula (C1) is 【Chemistry 1】 and Formula (C2) is 【Chemistry 2】 and Formula (C3) is 【Chemistry 3】 and During the ceremony, R 101 ~R 122 are each independently selected from hydrogen, a hydrocarbyl group, a heteroaryl group, a halogen atom, or a heterocarbyl group; R 101 ~R 122 two or more of may optionally be joined together to provide one or more cyclic moieties; X 1 ~X 4 Each of is independently O, CH 2 , NH, NR, NSO 2 R or NSO 2 A, wherein each R is an independently selected substituted or unsubstituted alkyl or aryl group and each A is an independently selected aryl or heteroaryl group; Y 1 ~Y 8 each is an independently selected nitrogen-containing heterocyclic moiety attached to P through N, wherein each heterocyclic moiety is an alkyl, aryl, heteroaryl, alkoxy, acyl, carboxyl, carboxylate, cyano, -SO 3 3. The process of claim 1 or 2, optionally substituted with one or more groups or atoms selected from H, sulfonate, amino, trifluoromethyl, and halogen.

4. The process of any one of claims 1 to 3, further comprising recovering the propylaldehyde-functional organosilicon compound prior to step I).

5. the primary amine source being Formula: R 18 N.H. 2 (In the formula, R 18 is an alkyl group of 1 to 18 carbon atoms or an aryl group of 6 to 18 carbon atoms, 5. The process of any one of claims 1 to 4, wherein the organic functional group is selected from the group consisting of:

6. 6. The process of any one of claims 1 to 5, wherein the hydrogenation catalyst is a heterogeneous hydrogenation catalyst comprising a metal selected from the group consisting of Co, Cu, Fe, Ni, Ir, Pd, Pt, Rh, Ru, and combinations of two or more thereof.

7. The process of any one of claims 1 to 6, wherein the amount of the hydrogenation catalyst is from less than 1% to 50% by weight based on the weight of the aldehyde functional organosilicon compound.

8. In step III), one or both of conditions (i) and (ii) are satisfied, and condition (i) is H 2 3. The process of claim 2, wherein the pressure is from 10 psig (68.9 kPa) to 1500 psig (10,342 kPa) and condition (ii) is that the temperature is from 0° C. to 200° C.

9. 9. The process of claim 2 or 8, further comprising pretreating the hydrogenation catalyst prior to step III).

10. 10. The process of any one of claims 2, 8, or 9, further comprising IV) recovering said aminopropyl-functional organosilicon compound from said reaction product during and / or after step III).

11. V) recovering the primary amine source produced in step III) and, optionally, recycling the primary amine source in step I).

12. The process according to any one of claims 2 and 8 to 11, wherein step III) is carried out in a continuous mode, optionally in a trickle bed reactor.

13. The process according to any one of claims 1 to 12, wherein step II) is present and step II) is carried out before and / or during step I).

14. 14. The process of claim 13, wherein the propylaldehyde functional organosilicon compound reacts with water at a temperature less than 120°C.

15. 13. An aminopropyl-functional organosilicon compound prepared by the process of any one of claims 2 and 8-12, wherein the aminopropyl-functional organosilicon compound has the formula: R N x SIR 4 (4-x) wherein each R N are independently selected expressions 【Chemistry 4】 where G is a divalent hydrocarbon radical free of aliphatic unsaturation having 2 carbon atoms.

16. 13. An aminopropyl-functional organosilicon compound prepared by the process of any one of claims 2 and 8 to 12, wherein the aminopropyl-functional organosilicon compound has the unit formula: (R 4 3 SiO 1/2 ) a (R 4 2 R N SiO 1/2 ) b (R 4 2 SiO 2/2 ) c (R 4 R N SiO 2/2 ) d (R 4 SiO 3/2 ) e (R N SiO 3/2 ) f (SiO 4/2 ) g (Z.O. 1/2 ) h wherein each R N are independently selected expressions 【Chemistry 5】 where G is a divalent hydrocarbon radical free of aliphatic unsaturation having 2 carbon atoms.

17. The aminopropyl-functional polyorganosiloxane is (R 4 R N SiO 2/2 ) d (wherein the subscript d is 3 to 12); (R 4 2 SiO 2/2 ) c (R 4 R N SiO 2/2 ) d wherein c is 0 to 6 and d is 3 to 12; Unit formula: (R 4 3 SiO 1/2 ) a (R 4 2 R N SiO 1/2 ) b (R 4 2 SiO 2/2 ) c (R 4 R N SiO 2/2 ) d wherein the quantity (a+b)=2, the quantity (b+d)≧1, and the quantity (a+b+c+d)≧2; Unit formula: (R 4 3 SiO 1/2 ) mm (R 4 2 R N SiO 1/2 ) nn (SiO 4/2 ) oo (Z.O. 1/2 ) h wherein the subscripts mm, nn, and oo represent the mole percentage of each unit in said polyorganosilicate resin, and the subscripts mm, nn, and oo have average values ​​such that mm≧0, nn≧0, oo>0, and 0.5≦(mm+nn) / oo≦4; Unit formula: (R 4 3 SiO 1/2 ) a (R 4 2 R N SiO 1/2 ) b (R 4 2 SiO 2/2 ) c (R 4 R N SiO 2/2 ) d (R 4 SiO 3/2 ) e (R N SiO 3/2 ) f (Z.O. 1/2 ) h wherein f>1, 2<(e+f)<10,000, 0<(a+b) / (e+f)<3, 0<(c+d) / (e+f)<3, and 0<h / (e+f)<1.5; and Unit: R N SIR 12 3 wherein each R 12 is R 13 and -OSi(R 14 ) 3 Each R 13 is a monovalent hydrocarbon group, and each R 14 is R 13 , -OSi(R 15 ) 3 , and -[OSiR 13 2 ] ii OSI R 13 3 Each R 15 is R 13 , -OSi(R 16 ) 3 , and -[OSiR 13 2 ] ii OSI R 13 3 Each R 16 is R 13 and -[OSiR 13 2 ] ii OSI R 13 3 where subscript ii has a value such that 0≦ii≦100, with the proviso that R 12 At least two of the groups are -OSi(R 14 ) 3 17. The amino-functional organosilicon compound of claim 16, selected from the group consisting of branched aminopropyl-functional polyorganosiloxanes, with the proviso that

18. The aminopropyl-functional organosilicon compound has the formula 【Chemistry 6】 wherein each R 4 is independently selected from the group consisting of alkyl groups of 1 to 18 carbon atoms and aryl groups of 6 to 18 carbon atoms; N are independently selected expressions 【Chemistry 7】 18. The aminopropyl-functional organosilicon compound of claim 17, wherein G is a primary amino group of the formula:

19. The aminopropyl-functional organosilicon compound has the formula 【Chemistry 8】 wherein each R 13 is independently selected from the group consisting of alkyl groups of 1 to 18 carbon atoms and aryl groups of 6 to 18 carbon atoms; R N is the formula 【Chemistry 9】 18. The aminopropyl-functional organosilicon compound of claim 17, wherein G is a primary amino group of the formula:

20. 13. An aminopropyl-functional organosilicon compound prepared by the process of any one of claims 2 and 8-12, wherein the aminopropyl-functional organosilicon compound has the formula: [(R 1 (3-gg) R N gg Si) ff N.H. (3-ff) ] hh wherein each R N are independently selected expressions 【Chemistry 10】 where G is a divalent hydrocarbon radical free of aliphatic unsaturation having from 2 to 8 carbon atoms, and each R 1 is independently selected from the group consisting of alkyl groups and aryl groups, each subscript ff is independently 1 or 2, subscript gg is independently 0, 1, or 2, and subscript hh has a value such that 1<hh<10.

Citation Information

Patent Citations

  • Methods for preparing isoquinolines

    WO2013003315A2