Composite material that improves battery performance and its method of manufacture

A carbon-based composite material with a permeable-coating impermeable to liquids addresses the mechanical degradation in lithium-ion batteries by reducing swelling and SEI formation, enhancing electrode stability and performance.

JP2024536290AActive Publication Date: 2024-10-04ASPEN AEROGELS INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024519908
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-12-02
Filing Date
2022-12-09
Publication Date
2024-10-04
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

Lithium-ion batteries experience mechanical degradation due to volumetric expansion of electrode materials during charging and discharging, leading to capacity fade and poor cycle life, particularly with high-capacity materials like silicon, which results in surface cracking and formation of a solid electrolyte interphase (SEI) layer.

Method used

A composite material is developed comprising a carbon-based core with a porous exterior surface coated by a layer that is permeable to metal ions and impermeable to liquids, acting as a barrier to prevent electrolyte penetration and reduce swelling, thereby inhibiting SEI formation and improving electrode stability.

Benefits of technology

The composite material suppresses volumetric expansion, enhances electron transport, and modifies electrode surface chemistry to improve stability and performance, resulting in improved battery capacity, life, and cycling stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536290000006
    Figure 2024536290000006
  • Figure 2024536290000007
    Figure 2024536290000007
  • Figure 2024536290000008
    Figure 2024536290000008
Patent Text Reader

Abstract

Provided herein are composite materials and methods for preparing same for use in electrical energy storage systems (e.g., high capacity batteries). The composite materials of the present disclosure include a carbon-based core having a porous outer surface and a coating on at least a portion of the porous outer surface of the core. Such coating is made of a material that is (i) substantially permeable to at least one metal ion or metal atom and (ii) substantially impermeable to liquids.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to and the benefit of U.S. Provisional Application No. 63 / 287,600, filed December 9, 2021, and No. 63 / 385,845, filed December 2, 2022, entitled "COMPOSITE MATERIALS PROVIDING IMPROVED BATTERY PERFORMANCE AND METHODS OF MANUFACTURE THEREOF," the contents of both applications being incorporated herein by reference in their entirety.

[0002] The present disclosure relates generally to compositions and methods for improving the performance of electrical energy storage systems. In particular, the technology relates to composite materials suitable for use in high capacity battery materials, for example as electrode materials in lithium ion batteries. More specifically, the present disclosure relates to composite materials including a carbon-based core and a coating made of a material that is (i) substantially permeable to at least one metal ion or metal atom and (ii) substantially impermeable to liquids. [Background technology]

[0003] High-capacity battery materials, such as lithium-ion batteries, have a wide range of applications in power drives and energy storage systems. Lithium-ion batteries (LIBs) are widely used in powering portable electronic devices, such as mobile phones, tablets, laptops, power tools, and other high-current devices, such as electric vehicles, due to their high operating voltage, low memory effect, and high energy density compared to conventional batteries.

[0004] The electrochemical cell of a LIB mainly consists of a positive electrode, a negative electrode, an electrolyte capable of conducting lithium ions, a separator that electrically separates the positive electrode and the negative electrode, and a current collector. 0.8Co 0.15 Al 0.05 O2(NCA) and LiNi x Co y Mn z O2 (NMC), ethylene glycol, propylene glycol tetrachloride (PE), propylene glycol tetrachloride (PGTC ... Other novel anode materials, such as titanium-based oxides, alloy / de-alloyed materials, and conversion materials, have also been investigated and have shown excellent electrochemical performance.

[0005] Under normal operation, lithium ions move from one electrode to the other through the electrolyte and separator via diffusion and migration. When a LIB is charged (delithiated), lithium ions in the electrolyte solution move from the cathode, through the separator, and are inserted into the anode. Charge-balancing electrons also move to the anode, but through an external circuit to power a device (computer, cell phone, electric car, etc.). Upon discharge (lithiation), the reverse process occurs, and electrons flow through the device being powered.

[0006] During the lithiation and delithiation process, the anode and cathode undergo dimensional changes during charging and discharging, which can lead to cell expansion. Thus, materials used in the cell (e.g., electrode materials) usually undergo large volume changes during cycling, which can then impart large stresses to the cell. For example, silicon has a typical volume change of up to 300% during lithiation, while graphite has a volume expansion of approximately 10%. The resulting stresses can cause surface and grain boundary cracking of the electrode materials, leading to the crushing of electrode particles and the formation of new surfaces for the formation and growth of solid electrolyte interphase (SEI) layers. As a result, these stresses destroy the integrity of the electrodes, resulting in capacity and power fade, which causes poor cycle life and performance of the battery.

[0007] These mechanical degradation mechanisms are strongly coupled with chemical degradation and are known to have a significant impact on the cycle life of lithium-ion batteries. The effect of swelling becomes increasingly important as higher capacity materials with higher volume expansion (e.g., silicon) are incorporated into battery electrodes. Summary of the Invention

[0008] The embodiments disclosed herein address one or more of the problems and deficiencies identified above by providing improved battery components, improved batteries made therefrom, and methods of making and using the same. However, it is believed that the present disclosure may prove useful in addressing other problems and deficiencies in many areas of technology. Thus, the subject matter recited in the claims should not necessarily be construed as limited to addressing any of the particular problems or deficiencies described herein.

[0009] It is an object of the present disclosure to obviate or mitigate at least one disadvantage of previous methods and materials for improving the performance (e.g., cycling stability, battery life) of large capacity batteries such as lithium ion batteries.

[0010] In one general aspect, the present disclosure provides a composite material for use in an electrical energy storage system, such as a lithium-ion battery. The composite material of the present disclosure advantageously inhibits or reduces the volume expansion (swelling) of the electrode material during charging and discharging, which can improve the performance (e.g., capacity, lifetime, cycling stability, or a combination thereof) of the battery.

[0011] In one general aspect, the composite material disclosed herein comprises a carbon-based core having a porous outer surface and a coating on at least a portion of the porous outer surface of the carbon-based core. The coating of the present disclosure is made of a material that is (i) substantially permeable to at least one metal ion or metal atom and (ii) substantially impermeable to liquid. The coating disclosed herein can act as a barrier to prevent electrolyte of a battery cell (e.g., a Li-ion battery cell) from penetrating the carbon-based core. The carbon-based core can be used as a component of an electrode. The coating (which is substantially impermeable to liquid) inhibits or reduces swelling of the carbon-based core during charging and discharging processes. Without being bound by theory, inhibiting or reducing swelling of the core improves battery performance.

[0012] In another aspect, the coatings of the present disclosure mitigate the continuous formation of a solid electrolyte interphase (SEI) on the porous outer surface of the carbon-based core.

[0013] The composite material of the present technology can improve the performance of lithium-ion batteries compared to lithium-ion batteries having electrodes that do not have the composite material of the present disclosure.

[0014] Carbon-based aerogels can have properties (e.g., pore volume, pore size distribution, morphology, etc.) that can be tuned or modified depending on the precursor materials and / or methods used. In one aspect, the present disclosure uses coated carbon-based aerogels as electrode materials with improved performance for applications in energy storage devices, such as lithium metal anodes for high energy batteries.

[0015] The use of the composites of the present technology in large capacity batteries, such as Li-ion batteries, provides several advantages, including (i) providing volume for active material expansion without electrode swelling during charge / discharge processes, (ii) providing a conductive medium to facilitate electron transport between electrode active particles, (iii) modifying the electrode surface chemistry to alter the electrochemical properties of the electrode surface, improving stability and performance, and (iv) providing a physical protective barrier that inhibits electrolyte reduction and forms an SEI on the core, thereby improving battery performance. Some composites disclosed herein may improve all aspects of performance. Others may improve one or more (but not all) aspects of performance.

[0016] In one aspect, provided herein is a composite material for use in an electrical energy storage system, the composite material comprising a carbon-based core having a porous exterior surface and a coating on at least a portion of the porous exterior surface of the carbon-based core, the coating being (i) substantially permeable to at least one metal ion or metal atom and (ii) substantially impermeable to liquid molecules.

[0017] In some examples, the liquid molecules include an electrolyte solvent. In some examples, the electrolyte solvent is selected from ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), fluoroethylene carbonate (FEC), fluorinated ether (F-EPE), 1,3-dioxolane (DOL), dimethoxyethane (DME), ethyl methyl carbonate (EMC), propylene carbonate (PC), butylene carbonate (BC), ethylene sulfite (ES), propylene sulfite (PS), diethyl sulfite (DES), gamma butyrolactone (BL), dimethyl sulfoxide (DMSO), ethyl acetate (EP), methyl acetate (MA), or a combination thereof.

[0018] In some examples, the at least one metal ion is a lithium ion. In some examples, the at least one metal atom is a lithium atom.

[0019] In some examples, the coating on at least a portion of the porous outer surface of the carbon-based core has a thickness, the thickness being about 2,500 nm or less. In some examples, the coating on at least a portion of the porous outer surface of the carbon-based core is about 100 nm to about 2,000 nm thick, or about 200 nm to 500 nm thick. In some examples, the coating extends into the porous outer surface of the carbon-based core. In some examples, the coating extends into the porous outer surface of the carbon-based core to a depth of about 2,500 nm or less, or about 100 nm to about 2,000 nm, or about 200 nm to 500 nm. In some examples, the coating is uniform on at least a portion of the porous outer surface of the core. In some examples, the coating is continuous on at least a portion of the porous outer surface of the core. In some examples, at least a portion of the porous outer surface of the core is at least 70% of the outer surface, at least 90% of the outer surface, or at least 95% of the outer surface. In some examples, the coating comprises a conductive material. In some examples, the conductive material is formed from a precursor of a non-conductive material. In some examples, the conductive material is carbon. In some examples, the non-conductive material is a polymer. In some examples, the conductive material is formed from a precursor of a first conductive material. In some examples, the first conductive material is selected from a metal or a transition metal. In some examples, the first conductive material is selected from a carbon material. In some examples, the conductive material is pitch-derived carbon, e.g., soft carbon. In some examples, the precursor of the first conductive material includes pitch.

[0020] In some examples, the coating comprises a material selected from an organic molecule, a polymer, a metal, a transition metal, a non-metal, a metal-organic framework (MOF), or a combination thereof. In some examples, the polymer is selected from the group of polyacrylonitrile (PAN), polymethylmethacrylate (PMMA), a polyimide, a polyamide, or a derivative thereof. In a specific example, the coating comprises polyacrylonitrile (PAN). In some examples, the organic molecule, the polymer, or a combination thereof is carbonized. In one example, the coating comprises carbonized polyacrylonitrile (PAN). In some examples, the coating is a carbon-based coating. In some examples, the carbon-based coating is derived from pitch. That is, in some examples, the coating is a pitch-derived carbon coating. In one example, the pitch-derived carbon coating comprises soft carbon.

[0021] In some examples, the coating penetrates into the pores of the carbon-based core. In some examples, the carbon-based core has a low bulk density, the low bulk density being in the range of about 0.25 g / cc to about 1.0 g / cc. In some examples, the carbon-based core has a pore volume of at least 0.3 cc / g. In some examples, the carbon-based core has a porosity of about 10% to about 90% of the volume of the core.

[0022] In some examples, the carbon-based core comprises a skeletal framework. For example, the skeletal framework can comprise carbon nanofibers. In some examples, the skeletal framework comprises an array of interconnected pores.

[0023] In some instances, the carbon-based core is a monolith.

[0024] In some examples, the carbon-based core is in the form of a particle. In some examples, the particle is substantially spherical and has a diameter of about 100 nm to about 4 mm, or about 5 μm to about 4 mm.

[0025] In some examples, the carbon-based core comprises a carbon-based aerogel, a carbon-based xerogel, a carbon-based ambigel, a carbon-based aerogel-xerogel hybrid material, a carbon-based aerogel-ambigel hybrid material, a carbon-based aerogel-ambigel-xerogel hybrid material, or a combination thereof. In some examples, the carbon-based core comprises activated carbon, carbon black, carbon fiber, carbon nanotubes, pyrolytic carbon, graphite, graphene, or a combination thereof.

[0026] In some examples, the carbon-based core includes one or more additives, the additives being present at a level of at least about 0.1 to 80 weight percent of the carbon-based core. In some examples, the additives include one or more electrochemically active dopants. The one or more electrochemically active dopants are selected from the group consisting of, but not limited to, lithium, sodium, potassium, calcium, magnesium, aluminum, iron, tin, lead, copper, mercury, manganese, vanadium, titanium, molybdenum, niobium, tungsten, zinc, silver, platinum, gold, carbon, boron, gallium, silicon, germanium, phosphorus, and antimony. In one example, the electrochemically active dopant is selected from the group consisting of, but not limited to, silicon, germanium, tin, antimony, gold, silver, zinc, magnesium, platinum, and aluminum.

[0027] In some examples, the coating includes a conductive additive, the conductive additive including carbon, carbon nanotubes, graphene, graphite, a metal, a metal oxide, silicon carbide, or a combination thereof.

[0028] In some examples, the carbon-based core has a capacity of about 200 mAh / g to about 3000 mAh / g. In some examples, the carbon-based core has a conductivity of at least about 1 S / cm. In some examples, the coating has a conductivity of at least about 1 S / cm.

[0029] In some examples, the energy storage system incorporating the composite material of the present technology is a battery. In some examples, the battery is a rechargeable battery. In some examples, the rechargeable battery is a Li-ion battery.

[0030] In one aspect, provided herein is a rechargeable battery comprising the composite material of the present technology disclosed herein.

[0031] In another aspect, provided herein is a method of improving the performance of a rechargeable battery comprising incorporating a composite material disclosed herein into the rechargeable battery.

[0032] In another aspect, provided herein is a method of preparing a composite material of the present disclosure, the method comprising providing a carbon-based core having a porous outer surface and coating at least a portion of the porous outer surface of the core to obtain a composite material.

[0033] In some examples, the method of preparing a composite material of the present disclosure further comprises a subcritical or supercritical drying step prior to the step of coating at least a portion of the porous outer surface of the core. In some examples, the method further comprises a carbonization step between the step of coating at least a portion of the porous outer surface of the core and the step of subcritical or supercritical drying. In one example, the method further comprises a second carbonization step after the step of coating at least a portion of the porous outer surface of the core.

[0034] In some examples, the method of preparing the composite material of the present disclosure further comprises a subcritical or supercritical drying step after the step of coating at least a portion of the porous outer surface of the core, and in some examples, further comprises a carbonization step after the step of subcritical or supercritical drying the composite material.

[0035] In some examples, coating at least a portion of the porous exterior surface of the core comprises a coagulation process. In other examples, coating at least a portion of the porous exterior surface of the core comprises a spray coating process. In some examples, the spray coating process comprises a high speed spray drying method using an atomized feed. In some examples, coating at least a portion of the porous exterior surface of the core comprises a dip coating process.

[0036] In some examples, the step of coating at least a portion of the porous outer surface of the core includes.

[0037] The present technology will be more fully understood from the following detailed description taken in conjunction with the accompanying drawings. [Brief description of the drawings]

[0038] [Figure 1] FIG. 1 illustrates an exemplary bead coating process suitable for application to the carbon-based cores of the present disclosure. [Diagram 2] FIG. 2 shows the preparation scheme for coating C / Si beads with PAN using the solidification process. [Diagram 3] FIG. 3 shows two different routes to apply a PAN coating on the surface of C / Si beads. [Figure 4] Figures 4A and 4B are scanning electron microscope (SEM) photographs of Sample A showing the carbon coating layer on the beads (from PAN coagulation process 1, route 1). Figure 4A shows a portion of the coated bead, and Figure 4B is a higher magnification view of a portion of the coating on the surface of the bead shown in Figure 4A. [Figure 5A] Figure 5A is an SEM image of Sample B (PAN coated aerogel beads using Process 1, Route 2). Image of one of the coated beads (Sample B). [Figure 5B]FIG. 5B is an SEM image of Sample B (PAN coated aerogel beads using Process 1, Route 2). A higher magnification of a portion of the beads in FIG. 5A. [Figure 5C] FIG. 5C is an SEM image of Sample B (PAN coated aerogel beads using Process 1, Route 2) at a higher magnification of a portion of the beads. [Figure 6] FIG. 6 is an SEM image of Sample C (fully PAN coated carbon aerogel beads, coating was formed using Process 2, Route 1). [Figure 7] Figures 7A and 7B are higher magnification images of Sample C. Figure 7A shows two beads connected to each other by a coating, and Figure 7B is a higher magnification of the coating at the neck / junction of the beads. [Figure 8] FIG. 8 is an SEM image of Sample D (fully PAN coated carbon aerogel beads, coating was formed using Process 2, Route 2). [Figure 9] Figures 9A and 9B are higher magnification images of Sample D. Figure 9A shows two beads connected to each other by a coating, and Figure 9B is a higher magnification of the coating at the neck / junction of the beads. [Figure 10A] Figure 10A is an SEM image of Sample D at high magnification showing the PAN coating layer on the fibrous carbon aerogel structure. Figure 10A shows a portion of the coated surface. [Figure 10B] Figure 10B is an SEM image of Sample D at high magnification showing the PAN coating layer on the fibrous carbon aerogel structure. Figure 10B is a higher magnification view of the coating. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0039] As previously mentioned, for certain active materials of interest (e.g., silicon), the storage and release of these ions (e.g., Li ions in Li-ion batteries) results in a substantial change in the volume of the active material. This can lead to irreversible mechanical damage in conventional designs and ultimately to loss of contact between individual electrode particles or between the electrode and the underlying current collector. Furthermore, it can lead to the continued growth of solid electrolyte interphases (SEIs) around such volume-changing particles.

[0040] A composite material is provided to address these aforementioned problems, the composite material including a carbon-based core having an outer surface and a coating, the coating being (i) substantially permeable to at least one metal ion or metal atom and (ii) substantially impermeable to liquid. Without being bound by theory, the carbon-based core structurally supports the active materials, electrically interconnects the active materials, and accommodates the aforementioned changes in volume of the active materials. In general, the composite particles may be able to accommodate changes in volume of the active materials during battery operation.

[0041] Such advantages are obtained for a wide range of high capacity anode and cathode materials. In addition, advantages are particularly obtained for high capacity anode and cathode materials (e.g., greater than about 10%) that exhibit significant volume changes (e.g., greater than about 10%) upon insertion and extraction of ions (e.g., metal ions) (e.g., greater than about 250 mAh / g for Li-ion battery cathodes and greater than about 400 mAh / g for Li-ion battery anodes). With respect to anodes, the composite materials of the present disclosure can be used in metal ion (e.g., Li-ion) batteries. Examples include, without limitation, highly doped, doped, and undoped Si, In, Sn, Sb, Ge, Mg, Pb, their alloys with other metals and metalloids, their mixtures with other metals, metal oxides, metal fluorides, metal oxyfluorides, metal nitrides, metal phosphides, metal sulfides, and semiconductor oxides, and their mixtures with hard carbon, graphite, graphene, and / or other carbon-based materials. With respect to the cathode, the composite materials of the present disclosure can be used in metal ion (e.g., Li-ion) batteries, examples of which include, without limitation, LCO, LFP, LMO, NCA, NMC, metal sulfides, metal fluorides, metal oxyfluorides, and mixtures thereof. In the following description, some examples are provided in the context of aqueous Li-ion batteries due to the current prevalence and popularity of Li-ion technology. However, such examples are provided merely to aid in the understanding and explanation of the underlying techniques, which may also be used in a variety of other metal ion batteries, e.g., Li + , Na + , Mg 2+ , Ca 2+ , and Al 3+ It should be understood that the composite materials of the present disclosure may be similarly applied to other battery chemistries in which the active particles undergo significant volume changes during their operation (e.g., reversible reduction-oxidation reactions), including, for example, aqueous electrolyte-containing batteries.

[0042] definition As used herein, the term "about" means that the numerical value is approximate and that small variations do not significantly affect the practice of the disclosed embodiments. When a numerical limitation is used, unless otherwise indicated by context, "about" means that the numerical value may vary by ±10% and remain within the scope of the disclosed embodiments.

[0043] As used herein, the term "optional" or "optionally" refers to the fact that a described event or circumstance may or may not occur, and the description includes instances where the event or circumstance occurs and instances where the event or circumstance does not occur.

[0044] As used herein, the term "uniform" refers to a variation in thickness of a material (eg, a coating of the present disclosure) of less than about 10%, less than about 5%, or less than about 1%.

[0045] As used herein, the term "continuous" refers to a layer that is free of gaps, holes, or any discontinuities, e.g., a continuous layer that does not contain two (or more) component materials that are physically separated (or spaced apart) within the layer.

[0046] As used herein, in the context of particle size, the term "D50" means that half of the population of particles has a particle size above this point, and half has a particle size below.D90 particle size distribution indicates that 90% of the particles (by number) have a Feret diameter below a certain size measured by scanning electron microscope (SEM) or transmission electron microscope.D10 particle size distribution indicates that 10% of the particles (by number) have a Feret diameter below a certain size measured by scanning electron microscope (SEM) or transmission electron microscope.

[0047] As used herein, the term "pitch" refers to a natural viscoelastic polymer or a viscoelastic polymer that can be produced from petroleum, coal tar, or plants. Pitch is generally obtained as a result of the thermal treatment and subsequent distillation of coal tar or petroleum fractions. It is substantially composed of a mixture of aromatic hydrocarbons. Exemplary pitches include petroleum pitch, coat tar pitch, and chemically treated pitch. Preferred compounds include those that have a high carbon content after pyrolysis, e.g., carbon content ranging from about 1% to about 20%.

[0048] As used herein, the term "xerogel" refers to a gel that has been dried under subcritical conditions, ie, the majority of the solvent is not in a supercritical fluid state under these conditions.

[0049] As used herein, the term "ambigel" refers to a gel dried at atmospheric pressure.

[0050] Carbon-Based Core In some examples, the carbon-based core comprises a carbon-based aerogel, a carbon-based xerogel, a carbon-based ambigel, a carbon-based aerogel-xerogel hybrid material, a carbon-based aerogel-ambigel hybrid material, a carbon-based aerogel-ambigel-xerogel hybrid material, or a combination thereof.

[0051] The aerogels used in the present disclosure may be carbonized to obtain the carbon-based aerogels of the present technology. Carbonization may be performed by pyrolysis at high temperatures in an inert atmosphere. The carbonized forms of the aerogels used in the present disclosure may have a nitrogen content of 0-20%. Typical pyrolysis temperatures range from 500°C to 2000°C. The temperature may be increased to reduce the nitrogen content of the resulting carbon aerogel. Pyrolysis is typically performed in an inert atmosphere (i.e., nitrogen, helium, neon, argon, or some combination).

[0052] The aerogels used in the present disclosure may include a silica component.

[0053] In some examples, the present disclosure includes forming and using carbon-based cores, such as carbon aerogels, as electrode materials in energy storage devices, e.g., as the primary anode material in LIBs. The pores of the porous core are designed, organized, and structured to accommodate, e.g., silicon or other metalloid or metallic particles and to accommodate the expansion of such particles upon lithiation in the LIB. Alternatively, the pores of the porous core may be filled with sulfides, hydrides, any suitable polymer, or other additives, where it is beneficial to contact the additive with a conductive material to provide a more effective electrode.

[0054] Aerogels are solid materials that contain a highly porous network of micro- and meso-sized pores. Depending on the precursor materials used and the processing performed, the pores of an aerogel can occupy more than 90% of the volume when the density of the aerogel is about 0.05 g / cc. Aerogels can be prepared by removing the solvent from the gel (the solid network including the solvent) so that the shrinkage of the gel can be minimized or eliminated by capillary forces at its surface. Methods of solvent removal include, without limitation, supercritical drying (or drying with a supercritical fluid, such that the low surface tension of the supercritical fluid exchanges with the transient solvent in the gel), exchange of the solvent with a supercritical fluid, exchange of the solvent with a fluid that is subsequently converted to a supercritical state, sub- or near-critical drying, and sublimation of the frozen solvent in a freeze-drying process.

[0055] Upon drying at ambient conditions, gel shrinkage may occur accompanied by solvent evaporation and an ambigel may be formed. Thus, aerogel preparation by sol-gel processes or other polymerization methods may proceed in the following sequence of steps: dissolution of solute in solvent, formation of sol / solution / mixture, formation of gel (which may include further cross-linking), and solvent removal either by supercritical drying techniques or any other method that removes the solvent from the gel with controlled pore collapse.

[0056] Aerogels can be formed from inorganic and / or organic materials, and when formed from organic materials (e.g., phenols, resorcinol formaldehyde (RF), phloroglucinol furfuraldehyde (PF), polyacrylonitrile (PAN), polyimide (PI), polyurethane (PU), polybutadiene, polydicyclopentadiene, and precursors or polymeric derivatives thereof, etc.), the aerogels may be carbonized (e.g., by pyrolysis) to form carbon aerogels.

[0057] Within the context of the present disclosure, the terms "aerogel," "aerogel material," or "aerogel matrix" refer to a gel comprising an interconnected structural framework with a corresponding network of interconnected pores integrated within the framework and containing a gas, such as air, as a dispersed interstitial medium, which exhibits the following physical and structural properties (as determined by nitrogen porosimetry testing) that are attributed to aerogels: (a) an average pore size ranging from about 2 nm to about 100 nm; (b) a porosity of at least 80% or greater; and (c) a surface area of ​​at least about 100 m. 2 / g or more.

[0058] Thus, the aerogel materials of the present disclosure used as the carbon-based core include any aerogel or other open cell material that meets the defining elements set forth in the previous paragraph, including materials that could otherwise be classified as xerogels, cryogels, ambigels, microporous materials, and the like.

[0059] The aerogel material may be further characterized by additional physical properties including: (d) a pore volume of about 2.0 mL / g or more, particularly about 3.0 mL / g or more; (e) a density of about 0.50 g / cc or less, particularly about 0.3 g / cc or less, more particularly about 0.25 g / cc or less; and (f) at least 50% of the total pore volume comprises pores having a pore size between 2 and 50 nm (although, as described in more detail below, embodiments disclosed herein include aerogel frameworks and compositions that include pores having a pore size greater than 50 nm). However, satisfaction of these additional properties is not required to characterize a compound as an aerogel material.

[0060] To further extend in exemplary applications in LIBs, when carbon aerogel materials are used as the primary electrode material (e.g., anode material as in the examples of the present disclosure), the aerogel porous core has a narrow pore size distribution and provides high electrical conductivity, high mechanical strength, and morphology and sufficient pore volume (at final density) corresponding to high weight percentage and expansion of silicon particles.

[0061] In some instances, the surface of the carbon aerogel may be modified via chemical, physical, or mechanical methods to enhance performance via electrochemically active species housed within the pores of the carbon aerogel.

[0062] While this disclosure describes several embodiments that utilize a carbon aerogel-based core, it should be understood that other carbon-based materials can be used instead, for example, other open cell materials such as xerogels, cryogels, ambigels, and microporous materials can be used in place of or in conjunction with aerogels.

[0063] Carbon aerogel itself can act as a current collector due to its electrical conductivity and mechanical strength, thus eliminating the need for a separate current collector on the cathode or anode side (when the cathode or anode, respectively, is formed with carbon aerogel). In the majority of LIBs, aluminum or copper foil needs to be bonded to the cathode or anode, respectively, as its current collector. However, removing one or both of these components leads to additional space for more electrode material, depending on the application of the carbon aerogel, resulting in even greater capacity of the cell / individual electrodes and overall greater energy density of the packaged battery system. However, in some examples, existing current collectors may be integrated with various other example cathode and anode materials to increase the current collection capability or capacity of aluminum and copper foils.

[0064] In some examples, the carbon-based core, specifically carbon aerogel, can be used as a conductive network or current collector on the anode side of the energy storage device. The fully interconnected carbon aerogel network is loaded with electrochemically active species. The electrochemically active species is in direct contact or physically connected to the carbon network. The loading of the electrochemically active species is adjusted to the pore volume and porosity for high and stable capacity and improved safety of the energy storage device. When utilized on the anode side, the electrochemically active species may include, for example, silicon, graphite, lithium, or other metalloids or metals. The anode can include the carbon-based core, and specifically carbon aerogel.

[0065] Within the context of this disclosure, the term "collector-less" refers to the absence of a separate current collector directly connected to the electrode. As mentioned, in conventional LIBs, copper foil is bonded to the anode as its current collector. According to examples of the present disclosure, electrodes formed from carbon-based cores (e.g., carbon aerogel) can be free-standing or otherwise have the ability to be collector-less, since the scaffold or structure itself acts as a current collector due to its high electrical conductivity. In an electrochemical cell, collector-less electrodes can be connected to form a circuit by embedding solid, mesh, woven tabs during the solution step that creates the continuous porous carbon, or by soldering, welding, or metal depositing leads on a portion of the porous carbon surface. Other mechanisms of contacting the carbon to the rest of the system are also contemplated herein. In some examples, the carbon-based scaffold or structure, specifically the carbon aerogel, may be placed on or otherwise in communication with a dedicated current collecting substrate (e.g., copper foil, aluminum foil, etc.). In this scenario, the carbon aerogel can be attached to a solid current collector using a conductive adhesive and can be applied with various amounts of pressure.

[0066] It is further contemplated herein that the carbon-based core, specifically the carbon aerogel, can take the form of a monolithic structure. As essentially monolithic, the carbon aerogel eliminates the need for any binder. In other words, the anode can be binderless. As used herein, the term "monolithic" refers to an aerogel material in which the majority (by weight) of the aerogel contained in the aerogel material or composition is in the form of a single continuous interconnected aerogel nanostructure. Monolithic aerogel materials include aerogel materials that are initially formed with a single interconnected gel or aerogel nanostructure, but may subsequently be cracked, fractured, or segmented into non-single aerogel nanostructures. Monolithic aerogels can take the form of free-standing or reinforced (fiber or foam) materials. In comparison, using silicon lithiation as an example, silicon incorporated within a monolithic aerogel can be more effectively utilized relative to theoretical capacity compared to the same amount of silicon incorporated within a slurry using conventional processes.

[0067] Monolithic aerogel materials are distinguished from particulate aerogel materials. The term "particulate aerogel materials" refers to aerogel materials in which the majority (by weight) of the aerogel contained therein is in the form of particulates, particles, granules, beads, or powders. These can be combined or compressed together (i.e., via a binder, such as a polymeric binder), but lack the interconnected aerogel nanostructure between the individual particles. Collectively, aerogel materials in this form are said to have a powder or particulate form (as opposed to a monolithic form). It should be noted that, despite the individual particles of the powder having a unitary structure, the individual particles are not considered monoliths herein. Integrating aerogel powders into electrochemical cells may typically involve preparation of a paste or slurry from the powder, casting and drying on a substrate, and optionally calendaring.

[0068] Particulate aerogel materials, e.g., aerogel beads, provide certain advantages. For example, particulate matter can be used as a direct replacement for other materials, such as graphite, in LIB anodes and anode manufacturing processes. Particulate matter can also provide improved lithium ion diffusion rates due to shorter diffusion paths within the particulate matter. Particulate matter can also enable electrodes with increased packing density, for example, by tailoring particle size and packing arrangement. Particulate matter can also improve access to silicon due to inter- and intra-particle porosity.

[0069] Carbon-based cores, such as carbon aerogels according to the present disclosure, can be formed from any suitable organic precursor material. Examples of such materials include, without limitation, RF, PF, PI, polyamides, polyacrylates, polymethylmethacrylates, acrylate oligomers, polyoxyalkylenes, polyurethanes, polyphenols, polybutadienes, trialkylsilyl-terminated polydimethylsiloxanes, polystyrenes, polyacrylonitriles, polyfurfurals, melamine-formaldehyde, cresol formaldehyde, phenol-furfurals, polyethers, polyols, polyisocyanates, polyhydroxybenzenes, polyvinyl alcohol dialdehydes, polycyanurates, polyacrylamides, various epoxies, agar, agarose, chitosan, and combinations and derivatives thereof. Any precursor of these materials may be used to form and use the resulting material. In some examples, the carbon aerogels are formed from pyrolyzed / carbonized polyimide-based aerogels, i.e., polymerization of polyimides. Even more specifically, polyimide-based aerogels can be produced using one or more of the methodologies described in U.S. Pat. Nos. 7,071,287 and 7,074,880 (Rhine et al.), for example, by imidizing poly(amide) acids and drying the resulting gel using a supercritical fluid.Other suitable methods for making polyimide aerogels (and carbon aerogels derived therefrom) are also contemplated herein, for example, see U.S. Pat. No. 6,399,669 (Suzuki et al.); U.S. Pat. No. 9,745,198 (Leventis et al.); Leventis et al., Polyimide Aerogels by Ring-Opening Metathesis Polymerization (ROMP), Chem. Mater. 2011, 23, 8, 2250-2261; Leventis et al., Isocyanate-Derived Organic Aerogels: Polyureas, Polyimides, Polyamides, MRS Proceedings, 1306 (2011), Mrsf10-1306-bb03-01. doi:10.1557 / opl.2011.90; Chidambareswarapattar et al., One-step room-temperature synthesis of fibrous polyimide aerogels from anhydrides and isocyanates and conversion to isomorphic carbons, J. Mater.Chem.,2010,20,9666-9678;Guo et al.,Polyimide Aerogels Cross-Linked through Amine Functionalized Polyoligomeric Silsesquioxane,ACS Appl.Mater.Interfaces 2011,3,546-552;Nguyen et al.,Development of High Temperature,Flexible Polyimide Aerogels,American Chemical Society,proceedings published 2011;Meador et al.,Mechanically Strong,Flexible Polyimide Aerogels Cross-Linked with Aromatic Triamine,ACS Appl.Mater.Interfaces,2012,4(2),pp 536-544;Meador et al.,Polyimide Aerogels with Amide Cross-Links:A Low Cost Alternative for Mechanically Strong Polymer Aerogels,ACS Appl.Mater.Interfaces 2015,7,1240-1249; Pei et al., Preparation and Characterization of Highly Cross-Linked Polyimide Aerogels Based on Polyimide Containing Trimethoxysilane Side Groups, Langmuir 2014,30,13375-13383. The resulting polyimide aerogels are then pyrolyzed to form polyimide-derived carbon aerogels.

[0070] Carbon aerogels of the present disclosure, such as polyimide-derived carbon aerogels, can have a residual nitrogen content of at least about 4 wt%. For example, the carbon aerogels can have a residual nitrogen content of at least about 0.1 wt%, at least about 0.5 wt%, at least about 1 wt%, at least about 2 wt%, at least about 3 wt%, at least about 4 wt%, at least about 5 wt%, at least about 6 wt%, at least about 7 wt%, at least about 8 wt%, at least about 9 wt%, at least about 10 wt%, or a range between any two of these values.

[0071] In examples of the present disclosure, the dried polymer aerogel composition can be subjected to a processing temperature of 200° C. or more, 400° C. or more, 600° C. or more, 800° C. or more, 1000° C. or more, 1200° C. or more, 1400° C. or more, 1600° C. or more, 1800° C. or more, 2000° C. or more, 2200° C. or more, 2400° C. or more, 2600° C. or more, 2800° C. or more, or a range between any two of these values, for carbonization of the organic (e.g., polyimide) aerogel. In an exemplary embodiment, the dried polymer aerogel composition can be subjected to a processing temperature in the range of about 1000° C. to about 1100° C., e.g., about 1050° C. Without being bound by theory, it is believed herein that the electrical conductivity of the aerogel composition increases with carbonization temperature.

[0072] Within the context of this disclosure, the term "electrical conductivity" refers to a measurement of the ability of a material to carry electric current or other material to allow the flow of electrons. Electrical conductivity is specifically measured as the electrical conductance / susceptance / admittance of a material per unit size of the material. It is usually recorded as S / m (Siemens / meter) or S / cm (Siemens / centimeter). The electrical conductivity or resistivity of a material may be determined by methods known in the art, including, for example, without limitation, in-line 4-point resistivity (using the dual configuration test method of ASTM F84-99). Within the context of this disclosure, electrical conductivity measurements are obtained according to ASTM F84-resistivity (R) measurements, which are obtained by measuring the voltage (V) divided by the current (I), unless otherwise specified. The aerogel material, e.g., the carbon aerogels or compositions of the present disclosure, can have an electrical conductivity of about 1 S / cm or more, about 5 S / cm or more, about 10 S / cm or more, 20 S / cm or more, 30 S / cm or more, 40 S / cm or more, 50 S / cm or more, 60 S / cm or more, 70 S / cm or more, 80 S / cm or more, or a range between any two of these values.

[0073] Within the context of this disclosure, the term "electrochemically active species" refers to an additive that can be used in small amounts, e.g., as a dopant, and can accept and release ions in an energy storage device. Using a LIB as an example, the electrochemically active species in the anode accepts lithium ions during charging and releases lithium ions during discharging. The electrochemically active species can be stabilized in the anode by having a direct / physical connection with the porous carbon core. The porous carbon network can form an interconnected structure around the electrochemically active species. The electrochemically active species is connected to the porous carbon at multiple points. An example of an electrochemically active species is silicon, which can expand and crack or break upon lithiation. However, because silicon has multiple connection points with the porous carbon (aerogel), the silicon can be retained within the porous structure (e.g., pores) and remain active, or in other cases, be enveloped by the structure even upon breaking or cracking.

[0074] Electrochemically active species can be referred to as electrically active additives and can be used to promote infiltration and plating. For example, silicon doping can be used as a material for Li metal anodes to promote Li infiltration and initiate lithium plating. Besides silicon, other electrically active additives include gold, silver, zinc, magnesium, platinum, aluminum, tin, copper, nickel, and other dopants described herein. In some examples, electrochemically active materials can be used in small amounts as dopants to seed lithium plating within the porosity of carbon nanostructures.

[0075] Within the context of this disclosure, the terms "compressive strength," "flexural strength," and "tensile strength" refer to the resistance of a material to breaking or fracturing under compressive, bending or flexing, and tension or pulling forces, respectively. These strengths are specifically measured as the amount of load / force per unit area resisting the load / force. This can be recorded as pounds per square inch (psi), megapascals (MPa), or gigapascals (GPa). Among other factors, the compressive, flexural, and tensile strengths of a material collectively contribute to the structural integrity of the material, which is useful, for example, to withstand the volumetric expansion of silicon particles during lithiation in LIBs. With specific reference to Young's modulus, which is a measure of mechanical strength, the modulus may be determined by methods known in the art, including, but not limited to, the following Standard Test Practice for Instrumented Indentation Testing (ASTM E2546, ASTM International, West Conshocken, PA); or Standardized Nanoindentation (ISO 14577, International Organization for Standardization, Switzerland). Within the context of the present disclosure, Young's modulus measurements are taken in accordance with ASTM E2546 and ISO 14577 unless otherwise specified. In certain examples, the aerogel material, e.g., the carbon aerogels or compositions of the present disclosure, have a Young's modulus of about 0.2 GPa or more, 0.4 GPa or more, 0.6 GPa or more, 1 GPa or more, 2 GPa or more, 4 GPa or more, 6 GPa or more, 8 GPa or more, or a range between any two of these values.

[0076] Within the context of this disclosure, the term "pore size distribution" refers to the statistical distribution or relative amount of each pore size within a sample volume of a porous material. A narrower pore size distribution refers to a relatively large percentage of pores in a narrow range of pore sizes, thus increasing the amount of pores that can contain electrochemically active species and maximizing the use of pore volume. Conversely, a wider pore size distribution refers to a relatively small percentage of pores in a narrow range of pore sizes. Thus, pore size distribution can be measured as a function of pore volume and recorded as the unit size of the full width at half maximum of the main peak in a pore size distribution chart. The pore size distribution of a porous material may be determined by methods known in the art, including, but not limited to, surface area and porosity analyzers by nitrogen adsorption / desorption, which can calculate the pore size distribution. Within the context of this disclosure, measurements of pore size distribution are obtained according to this method unless otherwise specified. In some examples, the aerogel material, e.g., the carbon aerogels or compositions of the present disclosure, has a relatively narrow pore size distribution (full width at half maximum) of about 50 nm or less, 45 nm or less, 40 nm or less, 35 nm or less, 30 nm or less, 25 nm or less, 20 nm or less, 15 nm or less, 10 nm or less, 5 nm or less, or a range between any two of these values.

[0077] Within the context of the present disclosure, the term "pore volume" refers to the total volume of pores within a sample of a porous material. Pore volume is specifically measured as the volume of voids within a porous material, which voids may be measurable and / or accessible by other materials, e.g., electrochemically active species such as silicon particles. It is expressed in cubic centimeters per gram (cm 3Pore ​​volume of a porous material may be determined by methods known in the art, including, but not limited to, surface area and porosity analyzers by nitrogen adsorption / desorption, which allows pore volume to be calculated. Within the context of the present disclosure, pore volume measurements are taken according to this method unless otherwise indicated. In certain examples, aerogel materials or compositions of the present disclosure (not incorporating electrochemically active species, e.g., silicon particles) have a relatively large pore volume of about 0.5 cc / g or more, 1 cc / g or more, 1.5 cc / g or more, 2 cc / g or more, 2.5 cc / g or more, 3 cc / g or more, 3.5 cc / g or more, 4 cc / g or more, or in a range between any two of these values. In other examples, aerogel materials, e.g., carbon aerogels or compositions of the present disclosure (incorporating electrochemically active species, e.g., silicon particles), have a pore volume of about 0.10 cc / g or more, 0.3 cc / g or more, 0.6 cc / g or more, 0.9 cc / g or more, 1.2 cc / g or more, 1.5 cc / g or more, 1.8 cc / g or more, 2.1 cc / g or more, 2.4 cc / g or more, 2.7 cc / g or more, 3.0 cc / g or more, 3.3 cc / g or more, 3.6 cc / g or more, or a range between any two of these values.

[0078] Within the context of the present disclosure, the term "porosity" refers to the volume fraction of the pores that does not include other materials (e.g., electrochemically active species such as silicon particles) attached to the walls of the pores. For purposes of clarity and explanation, it is noted that within the specific implementation of silicon-doped carbon aerogels as the primary anode material in LIBs, porosity refers to the voids after including the silicon particles. Porosity may be determined by methods known in the art, including, for example and without limitation, the ratio of the pore volume of an aerogel material to its bulk density. Within the context of the present disclosure, porosity measurements are obtained according to this method unless otherwise indicated. In certain examples, the aerogel materials, e.g., carbon aerogels or compositions of the present disclosure, have a porosity of about 90% or less, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or a range between any two of these values.

[0079] It should be noted that pore volume and porosity are different measures for the same property of the pore structure, namely the "empty space" within the pore structure. For example, when silicon is used as the electrochemically active species enclosed within the pores of a nanoporous carbon material, the pore volume and porosity refer to the space that is "empty", i.e., the space that is not utilized by carbon or electrochemically active species. As will be appreciated, densification of the pre-carbonized porous material (e.g., by compression) can have an effect on the pore volume and porosity, among other properties.

[0080] Within the context of this disclosure, the term "pore size at the maximum peak from a distribution" refers to the value at a recognizable peak on a graph illustrating a pore size distribution. The pore size at the maximum peak from a distribution is specifically measured as the pore size at which the largest percentage of pores are formed. It can be recorded as any unit length of pore size, such as μm or nm. The pore size at the maximum peak from a distribution may be determined by methods known in the art, including, but not limited to, surface area and porosity analyzers by nitrogen adsorption / desorption, which can calculate the pore size distribution and determine the pore size at the maximum peak. Within the context of this disclosure, the measurement of the pore size at the maximum peak from a distribution is obtained according to this method, unless otherwise specified. The aerogel material, e.g., the carbon aerogels or compositions of the present disclosure, can have a pore size at the largest peak from the distribution that is about 150 nm or less, 140 nm or less, 130 nm or less, 120 nm or less, 110 nm or less, 100 nm or less, 90 nm or less, 80 nm or less, 70 nm or less, 60 nm or less, 50 nm or less, 40 nm or less, 30 nm or less, 20 nm or less, 10 nm or less, 5 nm or less, 2 nm or less, or a range between any two of these values.

[0081] Within the context of this disclosure, the term "capacity" refers to the amount of specific energy or charge that a battery can store. In some examples, capacity refers to reversible capacity. Capacity is specifically measured as the discharge current that a battery can deliver per unit mass over time. It can be recorded as ampere-hours or milliampere-hours per gram, Ah / g or mAh / g of total electrode mass. The capacity of a battery (particularly the anode) may be determined by methods known in the art, including, for example and without limitation: A constant constant current load is applied to a fully charged cell until the cell voltage reaches an end of discharge voltage value; the time to reach the end of discharge voltage multiplied by the constant current is the discharge capacity; specific and volumetric capacity can be determined by dividing the discharge capacity by the weight of the electrode material or volume. Within the context of this disclosure, capacity measurements are taken according to this method unless otherwise specified. The aerogel material, e.g., the carbon aerogel or composition of the present disclosure, may have an anode capacity of about 100 mAh / g or more, 150 mAh / g or more, 200 mAh / g or more, 300 mAh / g or more, 400 mAh / g or more, 500 mAh / g or more, 600 mAh / g or more, 700 mAh / g or more, 800 mAh / g or more, 900 mAh / g or more, 1000 mAh / g or more, 1100 mAh / g or more, 1200 mAh / g or more, or .... h / g or greater, 1300 mAh / g or greater, 1400 mAh / g or greater, 1500 mAh / g or greater, 1600 mAh / g or greater, 1700 mAh / g or greater, 1800 mAh / g or greater, 1900 mAh / g or greater, 2000 mAh / g or greater, 2500 mAh / g or greater, 3000 mAh / g or greater, or a range between any two of these values, or any intervening value (e.g., 520 mAh / g).

[0082] It is believed herein that the pore size can be adjusted as needed. There are five main ways to adjust the pore size taught herein. First, the amount of solids, specifically the amount of polyimide precursor monomers (e.g., aromatic or aliphatic diamines and aromatic or aliphatic dianhydrides), can adjust the pore size. Smaller pore sizes result from a larger amount of solids per unit volume of fluid, since there is less space available for interconnections to occur more closely. Note that the strut width does not change measurably regardless of the amount of solids used. The amount of solids is more related to how dense the network will be.

[0083] Pore ​​size tuning can be achieved by using radiation (e.g., radio waves, microwaves, infrared, visible light, ultraviolet, x-rays, gamma rays) on the composite in either the polyimide or carbon state. Radiation has an oxidizing effect, resulting in increased surface area, increased pore size, and a broadening of the pore size distribution. Third, pore size is affected by macroscopic compression of the polyimide composite. In some instances, pore size decreases with compression.

[0084] Tuning of the pore size can be achieved by ion bombardment of the composite material in either the polyimide or carbon state. The effect of the ion bombardment depends on the method specified. For example, there is additive ion bombardment (e.g., CVD), where something is added, resulting in a decrease in pore size; there is also destructive ion bombardment, where the pore size increases. Finally, the pore size can be tuned (increased or decreased) by heat treatment in different gas environments, e.g., in the presence of carbon dioxide or carbon monoxide, chemically active environments, hydrogen reducing environments, etc. For example, a carbon dioxide environment is known to create activated carbon, and in the case of activation, mass is removed, pore size increases, and surface area increases.

[0085] Lithium can be used with carbon aerogels in a variety of ways, including pre-depositing by ex situ lithium plating or melt injection prior to cell assembly. For lithium pre-deposited in carbon aerogels, examples include carbon aerogels that are pre-treated to promote Li permeation, and carbon aerogels pre-doped with Si (a known additive to promote Li permeation). For carbon aerogels that are lithiated (or plated) in situ during formation, examples include providing sufficient Li available in the electrolyte and cathode, such that upon first charge, the carbon aerogel is plated such that no more than 50% of the Li is lost due to SEI formation.

[0086] The lithium in carbon aerogel can have several forms, such as free-standing carbon aerogel monoliths, carbon aerogel on copper current collectors, carbon aerogel on lithium metal, and carbon aerogel beads. Carbon aerogels have high electrical conductivity and can function as current collectors. The beads can be used in standard battery manufacturing slurry / casting methods. Beads of specific size and particle size distribution can be manufactured and then heavily infiltrated with Li metal onto the individual beads and post-cast beads as electrodes.

[0087] In the case of carbon aerogel, lithium infiltration can be achieved via melt injection and electrodeposition. A narrow and controllable particle size distribution helps to provide uniform lithium deposition during charging, which can help to reduce or prevent the formation of dendrites. In one embodiment, when carbon aerogel is present between the lithium metal and the separator, during operation of the battery, the carbon aerogel is reduced upon charging and Li ions (from the Li metal underlayer and electrolyte) are deposited on the surface of the carbon aerogel. Then, upon discharge, the accumulated Li ions in the carbon aerogel are released and the Li metal underlayer can continue to resupply Li ions as needed, but the dendrites cannot propagate. The carbon aerogel moderator / barrier layer is prepared with the desired surface area, pore size, and pore size distribution to achieve high capacity, long cycle life, excellent power characteristics, and improved safety.

[0088] Within the context of this disclosure, the terms "char content" and "char yield" refer to the amount of carbonized organic material present in an organic aerogel after exposing the aerogel to high temperature pyrolysis. The char content of an aerogel can be expressed as a percentage of the amount of organic material present in the aerogel framework after high temperature pyrolysis treatment relative to the total amount of material in the original aerogel framework before the high temperature pyrolysis treatment. This percentage can be measured using thermogravimetric analysis, such as TG-DSC analysis. Specifically, the char yield in an organic aerogel can be correlated to the percentage of weight retained by the organic aerogel material when subjected to high carbonization temperatures during TG-DSC analysis (with weight losses resulting from moisture evaporation, organic outgassing, and other materials lost from the aerogel framework during the high temperature pyrolysis treatment). For purposes of this disclosure, the char yield is correlated to the carbonization exposure temperature up to 1000°C. Preferably, the aerogel materials of the present disclosure that can serve as precursors to carbon-based aerogels can have a char yield of about 50% or greater, about 55% or greater, about 60% or greater, about 65% or greater, or about 70% or greater.

[0089] Coating Materials The coating materials of the present disclosure are used to coat the porous exterior surface of the carbon-based cores disclosed herein.

[0090] Without wishing to be bound by theory, the coatings disclosed herein may act as a barrier to prevent electrolyte in a battery cell (e.g., a Li-ion battery cell) from penetrating into a carbon-based core that may be used as a component of an electrode, thereby inhibiting or mitigating swelling of the carbon-based core during charge / discharge processes. Such coatings may help improve abrasion resistance, chemical resistance, and shape formation for carbon-based cores (e.g., porous carbon-based materials such as aerogels, ambigels, xerogels, cryogels, etc.).

[0091] The coating may be conductive or non-conductive.

[0092] In some examples, the coating may filter the passage of other atoms and / or molecules based on their size. In some examples, the coating is tailored to support size selectivity in ion and molecular diffusion. For example, the coating may allow lithium ions to diffuse freely, while larger cations such as the cathode metal and molecules such as electrolyte species are blocked. In some examples, the coatings disclosed herein can function as metal ion, e.g., Li ion diffusion barriers. Lithium ions have a migration barrier of about 0.7 eV or less through the coating. As used herein, the term "diffusion barrier" refers to the potential that Li ions must overcome as they migrate under the action of a concentration gradient.

[0093] The coating may include a material selected from organic molecules, polymers, metals, transition metals, nonmetals, metal-organic frameworks (MOFs), or combinations thereof. Alternatively, the coating may be formed from a precursor(s) of organic molecules, polymers, metals, transition metals, nonmetals, metal-organic frameworks (MOFs), or combinations thereof. In some examples, the polymer is selected from the group of polyacrylonitrile (PAN), polymethylmethacrylate (PMMA), polyimide, polyamide, or derivatives thereof. In some examples, the organic molecules, polymers, or combinations thereof are carbonized at temperatures >1000°C, 800°C, 700°C, or 650°C. In some examples, the organic molecules, polymers, or combinations thereof are cyclized at temperatures >400°C, 300°C, or 250°C.

[0094] In general, polymers suitable for coating the exterior surface of the carbon-based core include most hydrocarbon-based organic polymers, including thermoplastics and thermosets. Such polymers include, but are not limited to, the following: polyimide, polyamide, polyarylamide, polybenzimidazole, polybutylene, polyurethane, cellulose acetate, cellulose nitrate, ethyl cellulose, ethylene vinyl alcohol, polyperfluoroalkoxyethylene, fluorocarbon, polyketone, polyether ketone, liquid crystal polymer, nylon, polyether, polyetherimide, polyether sulfone, natural rubber, synthetic rubber, acrylic (emulsion or solution), nitrile, ethylene propylene, ethylene propylene diene methylene, polyethylene, chlorosulfonated polyethylene, neoprene, hypalon, ethylene acrylic, Viton, acrylonitrile-butadiene acrylate, acrylonitrile-butadiene styrene terpolymer, acrylonitrile-chlorinated polyethylene styrene terpolymer, acrylate maleic anhydride terpolymer, acrylonitrile-methyl methacrylate, acrylonitrile styrene copolymer, acrylonitrile styrene acrylate, bismaleimide, cellulosic acid acetate, cellulose acetate, cellulose acrylate, cellulose acetate terpolymer ... cellulose acetate butyrate, cellulose acetate propionate, cellulose nitrate, cycloolefin copolymer, chlorinated polyethylene, chlorinated polyvinyl chloride, cellulose triacetate, chlorotrifluoroethylene, diallyl phthalate, ethylene acrylic acid copolymer, ethyl cellulose, ethylene chlorotrifluoroethylene, ethylene-methyl acrylate copolymer, ethylene n-butyl acetate, epoxy, ethylene propylene diene monomer rubber, ethylene propylene copolymer rubber, ethylene propylene rubber, expandable polystyrene, ethylene tetrafluoroethylene, ethylene vinyl acetate, ethylene / vinyl acetate copolymer, ethylene vinyl alcohol, fluorinated ethylene propylene, high density polyethylene, high impact polystyrene, high molecular weight high density polyethylene, low density polyethylene, linear low density polyethylene, linear polyethylene, maleic anhydride, methyl methacrylate / ABS copolymer, methyl methacrylate butadiene styrene terpolymer, medium density polyethylene, melamine formaldehyde,Melamine phenols, nitrile butadiene rubber, olefin modified styrene acrylonitrile, phenolic polymers, polyacetic acid, polyamide-imide, polyaryletherketone, polyester alkyd, polyaniline, polyacrylonitrile, polyarylamide, polyarylsulfone, polybutylene, polybutadiene acrylonitrile, polybutadine, polybenzimidazole, polybutylene naphthalate, polybutadiene styrene, polybutylene terephthalate, polycarbonate, polycarbonate / acrylonitrile butadiene styrene blend, polycaprolactone, polycyclohexylene terephthalate, glycol modified polycyclohexyl terephthalate, polymonochlorotrifluoroethylene, polyethylene, polyether block amide or polyester block amide, polyetheretherketone, polyetherimide, polyetherketone, polyetherketone etherketone ketone, polyetherketone ketone, polyethylene naphthalene, polyethylene oxide, polyethersulfone, polyethylene terephthalate, glycol modified polyethylene terephthalate , perfluoroalkoxy, polyimide, polyisoprene, polyisobutylene, polyisocyanurate, polymethacrylonitrile, polymethyl methacrylate, polymethylpentene, paramethylstyrene, polyoxymethylene, polypropylene, polyphthalamide, chlorinated polypropylene, polyphthalate carbonate, polyphenylene ether, polymeric polyisocyanate, polyphenylene oxide, polypropylene oxide, polyphenylene sulfide, polyphenylene sulfone, polypropylene terephthalate, polystyrene, polystyrene / Polyisoprene block copolymer, polysulfone, polytetrafluoroethylene, polytetramethylene terephthalate, polyurethane, polyvinyl alcohol, polyvinyl acetate, polyvinyl butyryl, polyvinyl chloride, polyvinyl chloride acetate, polyvinylidene acetate, polyvinylidene chloride, polyvinylidene fluoride, polyvinyl fluoride, polyvinyl carbazole, polyvinyl alcohol, polyvinyl pyrrolidone, styrene acrylonitrile, styrene butadiene, styrene butadiene rubber, styrene butadiene styrene block copolymer,The polymer may be selected from styrene-ethylene-butylene-styrene block copolymers, styrene-isoprene-styrene block copolymers, styrene-maleic anhydride copolymers, styrene-methyl methacrylate, styrene / a-methylstyrene, styrene-vinyl acrylonitrile, urea-formaldehyde, ultra-high molecular weight polyethylene, ultra-low density polyethylene, unsaturated polyester, vinyl acetate, vinyl acetate ethylene, ultra-low density polyethylene, expandable polystyrene, derivatives thereof, and copolymers thereof.

[0095] In preferred examples, the coating includes one or more of the following: polyethylene, Kapton, polyurethane, polyester, natural rubber, synthetic rubber, hypalon, plastic alloy, PTFE, polyvinyl halide, polyester, neoprene, acrylic, nitrite, EPDM, EP, Viton, vinyl, vinyl acetate, ethylene vinyl acetate, styrene, styrene-acrylate, styrene-butadiene, polyvinyl alcohol, polyvinyl chloride, acrylamide, phenolic, or combinations thereof.

[0096] In some examples, the coating comprises soft carbon. In one example, the coating is a pitch-derived carbon coating. In one example, the pitch-derived carbon coating comprises soft carbon.

[0097] According to some examples of the present disclosure, the coating comprises pitch-derived carbon. In some examples, the pitch-derived carbon comprises soft carbon. As used herein, the term "soft carbon" refers to amorphous carbon formed by carbonization of pitch. Soft carbon refers to graphitizable non-graphitic carbon with higher electronic conductivity, the degree of graphitization and interlayer distance of which can be adjusted by heat treatment.

[0098] In some examples, the coating is selected from soft carbon derived from pitch, carbon black, and spherical carbon derived from mesitylene.

[0099] Without being bound by theory, the pitch-derived carbon coatings of the present disclosure largely prevent the formation of defects and oxygen-containing groups. The pitch-derived carbon coatings of the present disclosure (e.g., soft carbon) can withstand the severe volume expansion that occurs during Si lithiation due to their high mechanical strength resulting from long-range graphitic ordering (e.g., crystallinity). Exemplary pitch-derived carbon coatings of the present disclosure contain ordered graphitic domains with controllable crystallinity. Without being bound by theory, the controllable crystallinity of the pitch-derived carbon coatings imparts superior electron transport properties and structural elasticity to improve electrochemical performance. The graphitic ordering of the pitch-derived carbon coatings can be adjusted by increasing the heat treatment temperature to the range of 500-1400°C. Staged carbonization can be performed to gradually adjust the crystallinity.

[0100] In the examples of the present disclosure, virtually any method for coating according to the practice of the art may be used. Examples of suitable coating techniques include, but are not limited to, sol-gel coating, such as the solidification process, knife-over-roll coating, dip or saturation coating, reverse roll (all forms) coating, direct roll coating, gravure coating, printing rotary screen coating, curtain coating, die coating or extrusion, spray coating, transfer coating, electrostatic coating, brush coating, vapor deposition, flocking, hot knife or hot melt extrusion, and combinations of the above.

[0101] In examples of the present disclosure, a coating can be applied onto the surface of a carbon material (e.g., carbon aerogel beads) or onto the surface of a carbon precursor material (e.g., aerogel, xerogel, cryogel or ambigel materials, such as polyimide beads).

[0102] In certain examples, typical coatings of the present technology (e.g., polymer coatings, pitch coatings, soft carbon coatings, pitch-derived carbon coatings) can be applied onto the surface of the aerogel material (e.g., the precursor of the carbon aerogel material prior to a heat treatment step, e.g., a carbonization step). In one example, application of such coatings can be accomplished by spraying the molten coating material, the coating material in solution, the coating material in suspension, or a combination thereof through a nozzle or similar device. U.S. Patent Nos. 5,180,104, 5,102,484, 5,683,037, 5,478,014, 5,687,906, 6,488,773, and 6,440,218 teach spray nozzles, spray guns, and other devices that can be used in this embodiment, all of which are incorporated herein by reference. In yet another example, the coating is applied via a dip-coating method.

[0103] In another example, a typical coating is applied via a sol-gel process. The coating material dissolved or dispersed in a solution is solidified on the surface of the aerogel material (e.g., aerogel beads) by a coagulant solvent or coagulant. In some examples, the coagulant solvent includes DMF, DMAC, DMSO, methanol, ethanol, isopropyl alcohol, water, or mixtures thereof. In another example, the coagulant solvent includes an aqueous electrolyte solution. A typical bead coating process suitable for application to the surface of the aerogel material (e.g., aerogel beads) of the present disclosure is shown in FIG. 1.

[0104] In one example, an exemplary coating material and an exemplary aerogel material (e.g., aerogel beads) of the present disclosure are dispersed in a carrier fluid (e.g., silicone oil) to prepare an emulsion (e.g., a slurry), and then the emulsion is contacted with a coagulation solvent. Without being bound by theory, when the emulsion is contacted with the coagulation solvent, the coating material coagulates or solidifies almost instantly around the aerogel material, thereby forming a solid coating layer on the surface of the aerogel material. That is, the addition of the coagulation solvent leads to the formation of a coated aerogel material. In one example, the time required to add the coagulation solvent to the emulsion (e.g., a slurry of the coating material and aerogel material in the carrier fluid) is at least 150 seconds, at least 600 seconds, at least 20 minutes, at least 30 minutes, at least 60 minutes, at least 2 hours, at least 3 hours, at least 6 hours, at least 12 hours, at least 24 hours, or at least 48 hours.

[0105] In some instances, the solidification solvent is miscible with the solvent (e.g., carrier fluid) used to prepare the coating aerogel material solution or slurry.

[0106] In certain instances, typical coated aerogel materials of the present technology (e.g., polymer-coated, pitch-coated, carbon-coated aerogel beads) are further subjected to at least one heat treatment step (e.g., softening process, carbonization step).

[0107] As mentioned above, the surface of the typical aerogel material of the present technology can be coated using any method for coating conventionally known in the art (e.g., spray coating, solidification process). The coating of the present technology can also be directly adhered onto the surface of the carbon-based core (e.g., carbon aerogel material). That is, no intermediate layer is deposited or formed between the core and the coating. In some examples, the carbon aerogel material is obtained by processing (e.g., carbonizing) the aerogel material before applying or providing the coating material. As a result, a carbonization step is not necessary after applying the coating material.

[0108] In certain examples, exemplary coatings (e.g., polymer coatings, pitch coatings, soft carbon coatings, pitch-derived carbon coatings) can be applied onto the surface of the carbon aerogel material. That is, any carbonization step on the aerogel was performed prior to applying the exemplary coating. In one example, application of such coatings can be accomplished by spraying molten coating material, coating material in solution, coating material in suspension, or combinations thereof through a nozzle or similar device. U.S. Patent Nos. 5,180,104, 5,102,484, 5,683,037, 5,478,014, 5,687,906, 6,488,773, and 6,440,218 teach spray nozzles, spray guns, and other devices that can be used in this embodiment, all of which are incorporated herein by reference. In yet another example, the coating is applied via a dip coating method.

[0109] In another example, the coating is applied via a sol-gel process. The coating material, dissolved or dispersed in a solution, is solidified on the surface of the carbon aerogel material by a coagulant solvent. In some examples, the coagulant solvent includes DMF, DMAC, DMSO, water, or mixtures thereof. An exemplary bead coating process suitable for application to the carbon-based cores of the present disclosure is shown in FIG. 1.

[0110] The thickness of the coating can vary depending on the end use and the properties of the selected polymer. In one example, the coating thickness is about 2,500 nm or less, or about 100 nm to about 2,000 nm thick, or about 200 nm to 500 nm thick.

[0111] For certain applications, it may be desirable to use a flexible coating so that once coated, the bending modes of the carbon aerogel or aerogel material (or aerogel composite) are not significantly hindered. Thus, polymer coatings with elastic behavior or low stiffness are preferred.

[0112] In another example, the surface of a porous carbon system (e.g., an aerogel material) is modified prior to coating. Surface treatment methods include plasma treatment, corona treatment, or other chemical modifications. This procedure may aid in the deposition of a desired coating, for example, to achieve better deposition of the coating, more uniform thickness, or better adhesion to the core.

[0113] Once applied, the coating along with the composite material may be subjected to other processing steps such as drying, curing, carbonization, and sintering for reasons such as solvent removal, better adhesion to the core, improved mechanical properties, and many others. One non-limiting mode of carrying out the embodiments of the present disclosure includes a motorized conveyor with one or more spray systems and one or more thermal treatment units, preferably ovens, and other mechanical devices that automate the process in an industrial environment. The carbon-based cores are fed into the system through a moving conveyor element that carries the cores to the spray system. The spray system may consist of one or more spray heads that can individually control the spray characteristics. Curing / drying is provided to the coating by a thermal treatment unit such as an infrared or UV oven. The spray and thermal treatment units can be arranged in series or in any combination to provide the desired thickness and finish on the coated core. If a solvent is used in the spray process, appropriate equipment such as a hood and VOC reduction devices may be used.

[0114] In some examples, the coating includes an electrically insulating material (eg, a non-conductive material).

[0115] In some examples, the coating includes a conductive material. The conductive material (e.g., carbon) can be formed from a precursor of a non-conductive material (e.g., a polymer). In another example, the conductive material is formed from a precursor of a first conductive material (e.g., a metal or transition metal).

[0116] The coatings of the present technology are permeable to metal ions and / or metal atoms. The coatings are also impermeable to fluids.

[0117] In some instances, the permeability of the coating depends on the porosity of the coating (eg, pore size, pore volume, or a combination thereof).

[0118] In some designs, the coating may be generally uniform, while in other designs it may have a non-uniform composition that varies gradually with radial distance (e.g., from the inner surface to the outer surface).

[0119] In some examples, the coating may include multiple layers. For example, the multiple layers may include an outer layer formed of an electrical insulator material to prevent electrochemical reduction of the aqueous metal-ion electrolyte on the anode or to prevent electrochemical oxidation of the aqueous metal-ion electrolyte on the cathode. This may be accomplished by an insulating outer layer that corresponds to a portion of the voltage drop between the anode and the cathode, thereby reducing the voltage drop across the aqueous metal-ion electrolyte. In other examples, the multiple layers may include a conductive layer to electrically connect the active material particles, an interfacial layer to improve the uniformity or adhesion of another layer, a mechanically stable layer to improve the mechanical stability of the conformal, metal ion and / or metal atom permeable coating, or an auxiliary protective layer to prevent electrochemical reduction of the aqueous metal-ion electrolyte on the anode or to prevent electrochemical oxidation of the aqueous metal-ion electrolyte on the cathode.

[0120] Lithium-ion battery A basic example of a lithium-ion battery includes a cathode, an anode in electrical communication with the cathode, an electrolyte disposed between the anode and the cathode, and a separator also disposed between the anode and the cathode.

[0121] The electrolyte is an ionically conductive material and may include solvents, ionic liquids, metal salts, ions, such as metal ions or inorganic ions, polymers, ceramics, and other components. The electrolyte may be an organic or inorganic solid or liquid, such as a solvent (e.g., a non-aqueous solvent) containing dissolved salts. Non-aqueous electrolytes may include organic solvents, such as cyclic carbonates, linear carbonates, fluorinated carbonates, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylsulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, and mixtures thereof. Examples of salts that may be included in the electrolyte include lithium salts, such as LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, Li(FSO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y-1 SO2), (χ and y are natural numbers), LiC, LiI, and mixtures thereof. In some examples, the liquid molecules include an electrolyte solvent (electrolyte). The electrolyte solvent of the present disclosure can be selected from any of the suitable electrolytes described above. In particular, the electrolyte is selected from ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), fluoroethylene carbonate (FEC), fluorinated ethers (F-EPE), 1,3-dioxolane (DOL), dimethoxyethane (DME), or combinations thereof.

[0122] The separator is typically a thin, porous or semi-permeable insulating film with high ion permeability. The separator can be made of a polymer, such as an olefin-based polymer (e.g., polyethylene, polypropylene, and / or polyvinylidene fluoride). When a solid polymer electrolyte is used as the electrolyte, the solid polymer electrolyte can also act as the separator.

[0123] The anode is comprised of an active anode material that participates in the electrochemical reaction during operation of the battery. Example anode active materials include elemental materials such as lithium, alloys of Si and Sn or alloys containing other lithium compounds, and intercalation host materials such as graphite. By way of example only, the anode active material may include metals and / or metalloids that are alloyable with lithium, its alloys, or its oxides. Metals and metalloids that can be alloyed with lithium include Si, Sn, Al, Ge, Pb, Bi, and Sb. For example, oxides of metals / metalloids that can be alloyed with lithium include lithium titanate, vanadium oxide, lithium vanadium oxide, SnO2, or SiO x (0 <x<2)であってもよい。

[0124] The cathode is comprised of an active cathode material that participates in the electrochemical reactions during operation of the battery. The active cathode material may be a lithium composite oxide, and may include layered-based materials such as LiCoO2, olivine-type materials such as LiFePO4, spinel-type materials such as LiMn2O4, and similar materials. Spinel-type materials include those having a structure similar to the natural spinel LiMn2O4, which contains small amounts of nickel cations in addition to lithium cations, and optionally anions other than manganate. By way of example, such materials include those of the formula LiNi (0.5-x) Mn 1.5 M x O4 (0≦x≦0.2, M is Mg, Zn, Co, Cu, Fe, Ti, Zr, Ru, or Cr).

[0125] Within the context of this disclosure, the term "cycle life" refers to the number of complete charge / discharge cycles that an anode or battery (e.g., a LIB) can support before its capacity drops below about 80% of its original rated capacity. Cycle life can be affected by various factors, such as the mechanical strength of the underlying substrate (e.g., carbon aerogel) and maintenance of aerogel interconnectivity. It is noted that these factors actually remaining relatively unchanged over time is a surprising aspect of certain examples of the present disclosure. Cycle life may be determined by methods known in the art, including, without limitation, cycle testing. A battery cell is subjected to repeated charge / discharge cycles at a given current rate and operating voltage. Within the context of this disclosure, cycle life measurements are obtained according to this method unless otherwise specified. An energy storage device, such as a battery, or an electrode thereof can have a cycle life of about 25 cycles or more, 50 cycles or more, 75 cycles or more, 100 cycles or more, 200 cycles or more, 300 cycles or more, 500 cycles or more, 1000 cycles or more, or a range between any two of these values.

[0126] The present disclosure includes an electrical energy storage device having at least one anode comprising a composite material of the present technology as described herein, at least one cathode, and an electrolyte having lithium ions. The electrical energy storage device can have a first cycle efficiency (i.e., the coulombic efficiency of the cell from the first charge / discharge) of at least 10%, 20%, 30%, 40%, 50%, 60%, 70%, any intervening value (e.g., 65%), or a range between any two of these values ​​(e.g., a range of about 30% to about 50%). As previously described herein, the reversible capacity can be at least 150 mAh / g. The at least one cathode can be selected from the group consisting of conversion cathodes, such as lithium sulfide and lithium air, and intercalation cathodes, such as phosphates and transition metal oxides.

[0127] According to different examples, the composite material of the present disclosure may be applied to both the positive and negative electrodes of an electrochemical energy storage device, or to the electrodes (either the positive or negative electrodes) separately. In various examples, the cathode, anode, or solid electrolyte material is coated with the composite material of the present technology. EXAMPLES

[0128] The following examples are included to demonstrate preferred embodiments of the technology, however, as one of ordinary skill in the art will recognize in light of the present disclosure, many changes can be made in the specific examples disclosed and still obtain a like or similar result without departing from the spirit and scope of the technology.

[0129] Example 1: Polyacrylonitrile (PAN) fiber production by coagulation process To produce PAN fibers, dry spinning or wet spinning processes are typically used. In this example, a wet spinning route was followed, which involves extrusion of a PAN solution into a bath containing a coagulant (e.g., DMSO or DMAC) and a non-solvent (e.g., water).

[0130] In the coagulation bath, the fibers slowly started to coagulate and continued to form a dense structure. The coagulation process depends on two diffusion mechanisms: the diffusion of the solvent from the fiber into the bath and the diffusion of the non-solvent from the bath into the fiber. Both mechanisms occur simultaneously. The balance of these two processes leads to the PAN precipitating into fiber form. Coagulation can be influenced by various reaction parameters such as polymer composition, coagulation bath composition, and coagulation bath temperature.

[0131] Example 2: Preparation of PAN-coated carbon / silicon beads by coagulation In a clean beaker, a slurry of PAN solution and C / Si beads was prepared (Figure 2). Depending on the PAN content (e.g., viscosity) in the solution, the slurry was mixed under a mechanical mixer for 5 minutes to 16 hours. The slurry was then poured into a homogenized dispersant medium (e.g., silicon oil, mineral oil, hydrocarbon) to ensure better dispersion / scattering of the beads in the dispersant medium. In Figure 2, the dispersant medium used was silicon oil. The homogenizer mixer was set at a speed of 3,000 to 9,000 rpm depending on the viscosity of the dispersant medium. Once a good dispersion of the C / Si beads was achieved where the C / Si beads are covered with a layer of PAN solution, the coagulant solvent (aqueous solution, e.g., H2O or EtOH / H2O mixture) was added to the homogenized bath while mixing the solution. When the coagulant solvent comes into contact with the layer of PAN solution covering each C / Si bead, the PAN instantly coagulates or solidifies around the beads, thereby forming a solid PAN coating layer on the C / Si beads.

[0132] Coating of beads (e.g., aerogel beads) by PAN coagulation was performed by two different routes. As shown in Figure 3, Process 1 describes the route for coating wet polyimide / silicon beads (wet beads means freshly prepared by sol-gel process), while Process 2 describes the same route for coating carbonized beads (C / Si beads). Both processes use coagulation in homogenized oil medium to ensure better bead dispersion and avoid bead agglomeration. Finally, the beads are filtered, washed off, dried (dried in supercritical, subcritical, or ambient conditions) and carbonized. The beads in Process 2 underwent two carbonization cycles.

[0133] There are at least two different routes to carbonization of PAN-coated C / Si (or polyimide / Si) beads. Route 1 applies a heat treatment at 300°C in air for 1-6 hours to obtain complete cyclization of the PAN, followed by carbonization at temperatures above 650°C under inert gas for 2-5 hours. Route 2 utilizes direct carbonization at temperatures above 650°C under inert gas for 2-5 hours.

[0134] Example 2.1 Preparation of PAN-coated carbon / silicon beads by coagulation via process 1 Polyimide / silicone beads (silicone available from Evonik Industries AG, North Rhine-West phalia, Germany) were prepared by the sol-gel route using DMAC as the solvent and 100 cSt (centistokes) silicone oil as the dispersant medium for bead fabrication. After multiple washes with ethanol, the cake or bead gel was split into two equal amounts (~75 g each). One portion of the sample was supercritically dried with CO2 (i.e., uncoated beads, uncoated #1) and the other portion (wet bead gel) was coated with PAN using process 1 as previously described and shown in Figure 3.

[0135] A 5% PAN solution was prepared by dissolving 5g of PAN in 95g of DMAC. The solution was then mixed for 6 hours. 75 grams of wet bead gel was then mixed in the PAN solution for 20-30 minutes until a uniform slurry was obtained. The slurry was poured into a silicon oil bath mixed with a homogenizer at 7500 rpm and mixed for 2 minutes. An ethanol solution (50 / 50: EtOH / H2O) was slowly added to the system while mixing. The appearance of the mixture changed from black to gray, indicating solidification of the PAN. Once the beads were coated, they were separated from the oil and washed with ethanol (and heptane to remove residual oil) and filtered. The coated beads were also supercritically dried in the same manner as the uncoated bead gel.

[0136] The resulting PAN-coated aerogel beads were divided into two samples: one sample (sample A) was heat treated in air at 300°C and carbonized under N2 at 650°C, and the other sample (sample B) was directly carbonized under N2 at 1050°C. Table 1 summarizes the carbonization conditions and structural characteristics of the three different beads. [Table 1]

[0137] The coated beads show a reduction in surface area. With reference to Table 1, the surface area of ​​Uncoated #1 is greater than the two coated samples. That is, Samples A and B appear to include a coating that covers at least a portion of the available surface area. For example, Sample B, which underwent path 2, shows a surface area that is approximately 43% less than that of the uncoated sample (Uncoated #1). The data suggests coating of at least a portion of the surface area of ​​the uncoated sample.

[0138] The reduction in the surface area of ​​the beads after coating suggests that the PAN coating may have desirable porosity characteristics with respect to its permeability. For example, when phenolic resin was used as a coating material, the surface area of ​​the system increased, suggesting that phenolic resin may not be desirable as a coating material for fluid impermeability.

[0139] The SEM pictures shown in Figures 4A and 4B and Figures 5A-5C show the presence of a carbon coating layer on the C / Si beads. Thus, the process of PAN coating by solidification appears promising for further improvement and optimization. However, this route (Process 1) shows some imperfections and some uncoated areas on the beads. The carbonization temperature (Route 1: 300°C / air, then 650°C / N2, whereas Route 2: 1050°C / N2) does not seem to affect the quality of the coating. However, the temperature may directly affect the porosity (surface area) and possibly the cell performance.

[0140] Example 2.2 Preparation of PAN-coated carbon / silicon beads by coagulation via process 2 In this example, carbon aerogel beads (uncoated #2) were used. These beads had a diameter of 440 mm. 2 This resulted in a high surface area of ​​1000 nm / g. To coat the beads, 3.53 grams of carbon aerogel (uncoated #2) was mixed with 26 g of PAN solution (5% wtPAN in DMAC) for 20-30 minutes until a uniform slurry was obtained. The slurry was poured into a silicon oil bath mixed with a homogenizer at 7500 rpm and mixed for 2 minutes. An ethanol solution (50 / 50: EtOH / H2O) was slowly added to the system while mixing. The appearance of the mixture changed from black to gray, indicating solidification of the PAN. Once the beads were coated, they were separated from the oil, washed with ethanol (and heptane to remove residual oil), and filtered. The carbon PAN coated beads were supercritically dried. Note that other drying methods can be used in other examples. For example, the beads could be subcritically dried or dried at ambient conditions to obtain a xerogel or ambigel.

[0141] The resulting PAN-coated aerogel beads were divided into two samples: one sample was heat treated in air at 300°C and then carbonized under N2 at 650°C (Sample C), and the other part was directly carbonized under N2 at 1050°C (Sample D). Table 2 summarizes the carbonization conditions and structural properties of the three different beads.

[0142] Since the starting material (carbon aerogel beads) is a silicon-free material, the surface area of ​​the PAN-coated carbon beads is greater than the PAN-coated carbon / silicon beads previously characterized in Process 1. The presence of silicon in the carbon structure contributes significantly to the reduction in surface area of ​​the system; i.e., the higher the silicon content, the lower the surface area. The coated beads show a reduction in surface area. With reference to Table 2, the surface area of ​​Uncoated #2 is greater than the two coated samples; i.e., Samples C and D appear to include a coating that covers at least a portion of the available surface area. For example, Sample C, which underwent Route 2, shows a surface area that is approximately 25% less than that of the uncoated sample (Uncoated #2). The data suggests coating of at least a portion of the surface area of ​​the uncoated sample. [Table 2]

[0143] Increasing the carbonization temperature of the PAN-coated carbon aerogel to 1600–2200 °C could further reduce the surface area of ​​the system through graphitization of the PAN layer.

[0144] The SEM pictures (Figures 6-10B) show fully coated beads (i.e., the entire bead is coated with PAN). Regardless of the temperature profile of carbonization, both samples C and D show a PAN coating on the surface of the entire bead. The presence of the PAN coating is well documented in the high magnification SEM pictures (Figures 7A, 7B, 9A, 9B, 10A, and 10B). Particularly Figures 10A and 10B show a layer of PAN covering the fibrous structure of the carbon aerogel. The coating appears to be free of imperfections.

[0145] Example 3: Solution-based pitch coating directly onto PI (polyimide) beads A solution-based pitch coating was performed on the surface of polyimide (PI) gel beads prepared by emulsion process. After obtaining the PI beads, the PI beads were further polymerized by thermal imidization in a furnace (250-400°C, 2 hours). Without thermal imidization, the dimethylacetamide (DMAC) used in the next step may dissolve the polyamic acid (PAA) present in the PI gel beads. After dissolving the pitch in the DMAC solvent first, the DMAC / pitch slurry was stirred for a few minutes, then stirred while adding the PI gel beads, and stirred at above 100 RPM for 30 minutes. The temperature of the mixture was then increased to 50°C-120°C, and the mixture was stirred overnight under 100 RPM to evaporate the DMAC. Once the solvent (e.g., DMAC) was dried, the pitch-coated PI beads were gently crushed by a mortar and pestle.

[0146] The pitch-coated PI beads were then heated to 250-300°C and maintained at that temperature for 2 hours to undergo a softening process. The softening process allows the solid pitch to be transformed into a viscous liquid, so that the pitch can be coated uniformly. The pitch-coated PI beads were then subjected to a carbonization process at 1050°C for 2 hours. In the carbonization process, the PI beads were transformed into a carbon-based core, and the pitch coating was transformed into a soft carbon coating layer. The graphitization degree and interlayer distance of the pitch coating were adjusted in the carbonization process.

[0147] Example 4: Solution-based pitch coating directly onto carbon beads A solution-based pitch coating was performed on the surface of the carbon beads. After obtaining the PI beads, the PI gel beads were subjected to a carbonization process at 1050°C for 2 hours to obtain carbon-based cores, e.g., carbon beads. First, pitch was dissolved in DMAC solvent to obtain a DMAC / pitch slurry, and then the DMAC / pitch slurry was stirred for a few minutes, and then the carbon beads were added and stirred, and stirred at above 100 RPM for 30 minutes. The temperature of the mixture was then increased to 50°C-120°C, and the mixture was stirred overnight under 100 RPM to evaporate the DMAC. Once the solvent (e.g., DMAC) was dried, the pitch-coated carbon beads were gently crushed with a mortar and pestle.

[0148] The pitch-coated carbon beads were then heated to 250-300°C and maintained at that temperature for 2 hours to undergo a softening process. The softening process allows the solid pitch to be transformed into a viscous liquid, so that the pitch can be coated uniformly. The pitch-coated carbon beads were further subjected to a carbonization process (1050°C for 2 hours) to adjust the graphitization degree and interlayer distance of the pitch coating.

[0149] Table 3 summarizes the structural characteristics of solution-based pitch-coated carbon beads and the first cycle efficiency (FCE) of the power storage device (e.g., Li-ion battery) in which the pitch-coated PI and carbon beads are applied. [Table 3]

[0150] Solution-based pitch coating was also applied to Si / C composite beads. Pitch-coated Si / C composite beads were obtained using a protocol similar to that in Examples 3 and 4. The effects of the softening and carbonation steps were investigated.

[0151] Table 4 summarizes the structural properties of the solution-based pitch-coated Si / C composite beads as well as the first cycle efficiency (FCE) of the power storage device (e.g., Li-ion battery) in which the pitch-coated Si / C beads are applied.

[0152] The results shown in Table 4 indicate that the pitch-coated Si / C beads give higher FCE and cycling efficiency compared to the pitch-coated carbon beads shown in Table 3. The pitch-coated Si / C composite particles that underwent a softening and carbonization step were found to be more efficient compared to the pitch-coated Si / C composite particles that were not carbonized. It is believed that the softening process contributes to the improvement of the electrochemical performance of the electrode. Without being bound by theory, this may be because the softening process allows for a uniform coating of the beads with pitch. [Table 4]

[0153] Example 5: Spray-drying based pitch coating directly onto PI (polyimide) beads A spray-drying based pitch coating was performed on the surface of polyimide (PI) gel beads prepared by emulsion process. After obtaining the PI beads, the PI beads were further polymerized by thermal imidization in a furnace (250-400 °C, 2 h). Without thermal imidization, the dimethylacetamide (DMAC) used in the next step may dissolve the polyamic acid (PAA) present in the PI gel beads. First, after dissolving the pitch in DMAC solvent, the DMAC / pitch slurry was stirred for a few minutes, then stirred while adding the PI gel beads, and stirred at over 100 RPM for 30 minutes.

[0154] The temperature of the mixture was then increased to 160°C to dry the beads. This spray drying step allows for a uniform pitch coating on the PI beads. The pitch-coated PI beads were then heated to 250-300°C and the temperature was maintained for 2 hours to allow for the softening process (i.e., the process of obtaining soft carbon from the pitch).

[0155] The softening process allows the solid pitch to be transformed into a viscous liquid, allowing the pitch to be coated uniformly. The pitch-coated carbon beads were further subjected to a carbonization process (1050°C for 2 hours) to convert the underlying PI core beads to carbon and the pitch coating to soft carbon.

[0156] Table 5 summarizes the structural characteristics of the spray-based pitch-coated carbon beads as well as the first cycle efficiency (FCE) of the power storage device (e.g., Li-ion battery) to which the pitch-coated Si / C beads were applied. [Table 5]

[0157] As shown in Table 5, the coulombic efficiency from the first charge / discharge (FCE) of the electrode using pitch-coated carbon beads was relatively higher (improved) compared to the electrode using the control beads.

[0158] Example 6: Spray-drying based pitch coating directly onto carbon beads A spray-drying based pitch coating was performed on the surface of the carbon beads. After obtaining the PI beads, the PI gel beads were subjected to a carbonization process at 1050°C for 2 hours to obtain carbon-based cores, e.g., carbon beads. First, pitch was dissolved in DMAC solvent to obtain a DMAC / pitch slurry, and the DMAC / pitch slurry was stirred for a few minutes, then the carbon beads were added and stirred, and stirred at over 100 RPM for 30 minutes.

[0159] The temperature of the mixture was then increased to 160°C to dry the beads. This spray drying step allows for a uniform pitch coating on the carbon beads. The pitch-coated carbon beads were then heated to 250-300°C and the temperature was maintained for 2 hours to allow for a softening process (i.e., a process to obtain soft carbon from the pitch).

[0160] The softening process allows the solid pitch to be transformed into a viscous liquid, so that the pitch can be coated uniformly and the graphitization degree and interlayer distance can be adjusted. The pitch-coated carbon beads were further subjected to a carbonization process (1050°C for 2 hours).

[0161] While the present disclosure has been particularly shown and described with reference to example embodiments thereof, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the scope of the technology encompassed by the appended claims.

Claims

1. 1. A composite material for use in an electrical energy storage system, comprising: a. a carbon-based core having a porous outer surface; b. a coating on at least a portion of the porous exterior surface of the carbon-based core, the coating being (i) substantially permeable to at least one metal ion or metal atom and (ii) substantially impermeable to liquids; The composite material comprising:

2. The composite material of claim 1 , wherein the liquid comprises an electrolyte solvent.

3. 3. The composite material of claim 2, wherein the electrolyte solvent is selected from ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), fluoroethylene carbonate (FEC), fluorinated ethers (F-EPE), 1,3-dioxolane (DOL), dimethoxyethane (DME), or combinations thereof.

4. 2. The composite material of claim 1, wherein the at least one metal ion is a lithium ion.

5. 2. The composite material of claim 1, wherein the at least one metal atom is a lithium atom.

6. 10. The composite of claim 1, wherein the coating is about 2,500 nm or less in thickness, or about 100 nm to about 2,000 nm in thickness, or about 200 nm to 500 nm in thickness.

7. 10. The composite material of claim 1 or claim 6, wherein the coating extends into the porous outer surface of the carbon-based core.

8. 8. The composite material of claim 7, wherein the coating extends into the porous outer surface of the carbon-based core by about 2,500 nm or less, or from about 100 nm to about 2,000 nm, or from about 200 nm to 500 nm.

9. The composite material of claim 1 , wherein the coating is uniform over at least a portion of the porous exterior surface of the carbon-based core.

10. The composite material of claim 1 , wherein the coating is continuous over at least a portion of the porous exterior surface of the core.

11. 2. The composite material of claim 1, wherein at least a portion of the porous exterior surface of the core is at least 70% of the porous exterior surface, at least 90% of the porous exterior surface, or at least 95% of the porous exterior surface.

12. The composite material of claim 1 , wherein the coating comprises an electrically conductive material.

13. The composite material of claim 12 , wherein the conductive material is formed from a precursor of a non-conductive material.

14. 14. The composite material of claim 12 or 13, wherein the conductive material is carbon.

15. The composite material of claim 13 , wherein the non-conductive material is a polymer.

16. The composite material of claim 12 , wherein the conductive material is formed from a precursor of a first conductive material.

17. 17. The composite material of claim 16, wherein the first conductive material is selected from a metal or a transition metal.

18. 10. The composite material of claim 1, wherein the coating comprises a material selected from organic molecules, polymers, metals, transition metals, non-metals, metal-organic frameworks (MOFs), or combinations thereof.

19. 20. The composite material of claim 18, wherein the polymer is selected from the group of polyacrylonitrile (PAN), polymethylmethacrylate (PMMA), polyimide, polyamide, or derivatives thereof.

20. 20. The composite material of claim 18, wherein the coating comprises polyacrylonitrile (PAN).

21. 20. The composite material of claim 18, wherein the organic molecule, the polymer, or the combination thereof is carbonized.

22. 20. The composite material of claim 18, wherein the coating comprises carbonized polyacrylonitrile (PAN).

23. The composite material of claim 1 , wherein the coating is a carbon-based coating.

24. 24. The composite material of claim 23, wherein the carbon-based coating is derived from pitch.

25. The composite material of claim 1 , wherein the coating infiltrates into the pores of the carbon-based core.

26. 10. The composite material of claim 1, wherein the carbon-based core has a low bulk density, the low bulk density ranging from about 0.25 g / cc to about 1.0 g / cc.

27. 10. The composite material of claim 1, wherein the carbon-based core comprises a skeletal framework, the skeletal framework comprising an array of interconnected pores.

28. 10. The composite material of claim 1, wherein the carbon-based core has a pore volume of at least 0.3 cc / g.

29. The composite material of claim 1 , wherein the carbon-based core has a porosity of about 10% to about 90% of the volume of the core.

30. The composite material of claim 1 , wherein the carbon-based core is a monolith.

31. The composite material of claim 1 , wherein the carbon-based core is in the form of particles.

32. 10. The composite material of claim 1, wherein the particles are substantially spherical and have a diameter of from about 100 nm to about 4 mm, or from about 5 μm to about 4 mm.

33. 10. The composite material of claim 1, wherein the carbon-based core comprises a carbon-based aerogel, a carbon-based xerogel, a carbon-based ambigel, a carbon-based aerogel-xerogel hybrid material, a carbon-based aerogel-ambigel hybrid material, a carbon-based aerogel-ambigel-xerogel hybrid material, or a combination thereof.

34. 10. The composite material of claim 1, wherein the carbon-based core comprises activated carbon, carbon black, carbon fiber, carbon nanotubes, pyrolytic carbon, graphite, graphene, or a combination thereof.

35. 10. The composite material of claim 1, wherein the carbon-based core comprises one or more additives, the additives being present at a level of at least about 5-60 weight percent of the composite material.

36. 35. The composite material of claim 34, wherein the additive comprises one or more electrochemically active dopants.

37. 36. The composite material of claim 35, wherein the electrochemically active dopant is selected from the group consisting of silicon, germanium, tin, antimony, gold, silver, zinc, magnesium, platinum, and aluminum.

38. The composite material of claim 1 , wherein the coating comprises a conductive additive.

39. 38. The composite material of claim 37, wherein the conductive additive comprises carbon, carbon nanotubes, graphene, graphite, a metal, a metal oxide, silicon carbide, or a combination thereof.

40. 10. The composite material of claim 1, wherein the carbon-based core has a capacity of about 200 mAh / g to about 3000 mAh / g.

41. 10. The composite material of claim 1, wherein the carbon-based core has an electrical conductivity of at least about 1 S / cm.

42. 10. The composite material of claim 1, wherein the coating has a conductivity of at least about 1 S / cm.

43. 10. The composite material of claim 1, wherein the energy storage system is a battery.

44. 43. The composite material of claim 42, wherein the battery is a rechargeable battery.

45. 44. The composite material of claim 43, wherein the rechargeable battery is a Li-ion battery.

46. A rechargeable battery comprising a composite material according to any one of the preceding claims.

47. 13. A method for improving the performance of a rechargeable battery comprising incorporating into said rechargeable battery a composite material according to any one of the preceding claims.

48. A method for preparing a composite material according to any one of claims 1 to 45, comprising the steps of: a. providing a carbon-based core having an exterior surface; b. Obtaining the composite material by coating at least a portion of the porous exterior surface of the carbon-based core; The method comprising:

49. 48. The method of claim 47, further comprising sub- or supercritical drying prior to coating at least a portion of the porous exterior surface of the core.

50. 48. The method of claim 47, further comprising a step of sub- or supercritical drying after the step of coating at least a portion of the porous exterior surface of the core.

51. 49. The method of claim 48, further comprising a carbonization step between said step of coating at least a portion of said porous exterior surface of said core and said step of sub- or supercritical drying.

52. 51. The method of claim 50, further comprising a second carbonizing step after the step of coating at least a portion of the porous exterior surface of the core.

53. 50. The method of claim 49, further comprising a carbonization step after the subcritical or supercritical drying step of the composite material.

54. 48. The method of claim 47, wherein the step of coating at least a portion of the porous exterior surface of the core comprises a solidification process.

55. 48. The method of claim 47, wherein the step of coating at least a portion of the porous exterior surface of the core comprises a spray coating process.

56. 55. The method of claim 54, wherein the spray coating process comprises a high speed spray drying process using atomized delivery.

57. 48. The method of claim 47, wherein the step of coating at least a portion of the porous exterior surface of the core comprises a dip coating process.

Citation Information

Patent Citations

  • Silicon-carbon composite material for lithium ion battery and preparation method of same

    CN111384373A

  • Novel materials with extremely durable intercalation of lithium and manufacturing methods thereof

    EP3836261A1

  • Carbonaceous coated graphite particle, manufacturing method thereof, lithium ion negative electrode for secondary battery and lithium ion secondary battery

    JP2017117799A

  • Novel material having highly durable lithium insertion and method for manufacturing the same

    JP2018534720A