Nonaqueous electrolyte for lithium secondary battery and lithium secondary battery containing same
A non-aqueous electrolyte with specific additives addresses decomposition and low-temperature limitations in lithium secondary batteries, improving quick charging and low-temperature performance by forming resistant films that enhance lithium ion mobility and reduce precipitation.
Patent Information
- Application Number
- JP2024519911
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-26
- Filing Date
- 2022-10-25
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2042-10-25
AI Technical Summary
Lithium secondary batteries face issues with irreversible decomposition reactions due to propylene carbonate and limited low-temperature performance due to ethylene carbonate, necessitating an electrolyte that enhances quick charging and low-temperature output characteristics.
A non-aqueous electrolyte comprising specific additives such as compounds represented by chemical formulas 1 and 2, along with vinylene carbonate and/or vinyl ethylene carbonate, to form films with lower resistance and improve electrode durability, allowing for better lithium ion mobility and reduced precipitation during rapid charging.
The electrolyte improves rapid charging performance and capacity retention under low-temperature conditions, enhancing battery life and efficiency.
Smart Images

Figure 2024536292000001 
Figure 2024536292000002 
Figure 2024536292000003
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0143854, filed with the Korean Intellectual Property Office on October 26, 2021, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a non-aqueous electrolyte for a lithium secondary battery and a lithium secondary battery containing the same. [Background technology]
[0003] Lithium secondary batteries can be miniaturized and have high energy density and operating voltage, and therefore are used in a variety of fields such as mobile devices, electronic products, and electric vehicles.
[0004] In general, a lithium secondary battery is manufactured by forming an electrode assembly by interposing a separator between a positive electrode including a positive electrode active material made of a lithium-containing transition metal oxide and a negative electrode including a negative electrode active material capable of storing lithium ions, inserting the electrode assembly into a battery case, injecting a non-aqueous electrolyte solution that serves as a medium for transferring lithium ions, and then sealing the battery case.
[0005] Propylene carbonate has usually been used as the organic solvent for the non-aqueous electrolyte. However, there is a problem that propylene carbonate may cause an irreversible decomposition reaction with the graphite material. To solve this problem, ethylene carbonate has recently been widely used.
[0006] However, ethylene carbonate has a high melting point, which limits the temperature at which it can be used, and there is a further problem that the battery performance may be significantly reduced at low temperatures. Therefore, there is a need to develop an electrolyte for lithium secondary batteries that can be stably operated in various environments by solving such problems.
[0007] In addition, as the fields in which lithium secondary batteries are used become more diverse, a major issue is how to shorten the charging time for the convenience of users. Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made to solve the above problems, and an object of the present invention is to provide a nonaqueous electrolyte for lithium secondary batteries that contains a specific combination of additives and thereby contributes to improving rapid charging performance and low-temperature output characteristics, and a lithium secondary battery containing the same. [Means for solving the problem]
[0009] According to one embodiment, the present invention comprises: An organic solvent; A lithium salt; A first additive which is a compound represented by the following chemical formula 1; A second additive which is a compound represented by the following chemical formula 2; and a third additive which is one or more selected from the group consisting of vinylene carbonate and vinyl ethylene carbonate.
[0010] [Chemical formula 1] P[OSi(R1)3]3
[0011] In the above Chemical Formula 1, R1 is an alkyl group having 1 to 5 carbon atoms; [ka] In the above Chemical Formula 2, n is an integer of 1 or 2.
[0012] According to another embodiment, the present invention provides a lithium secondary battery including a positive electrode including a positive electrode active material, a negative electrode including a negative electrode active material, a separator interposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte for the lithium secondary battery. Effect of the Invention
[0013] The present invention can provide a lithium secondary battery that contains the above-mentioned nonaqueous electrolyte for a lithium secondary battery and that is excellent in capacity retention rate during rapid charging and under low temperature conditions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will now be described in more detail.
[0015] Generally, non-aqueous electrolytes for lithium secondary batteries contain ethylene carbonate as an organic solvent, which has excellent affinity with carbon materials. However, ethylene carbonate has a high melting point, which causes a problem of reduced output characteristics in low temperature environments.
[0016] In addition, lithium secondary batteries using conventional non-aqueous electrolytes have a problem in that lithium ions cannot move freely due to a resistive coating formed during activation, and lithium is precipitated on the surface of the electrode during rapid charging, resulting in a reduction in lifespan due to loss and depletion of lithium.
[0017] Therefore, the present inventors have found a combination of additives for non-aqueous electrolytes that can solve the above problems. Specifically, by combining the effect of forming a coating film having a lower resistance than conventional non-aqueous electrolytes by modifying the coating component of the electrode with a compound represented by the following chemical formula 1, the effect of improving the resistance and durability of the coating film by modifying the coating component of the electrode with a compound represented by the following chemical formula 2, and the effect of improving the durability of the negative electrode coating film by forming a negative electrode protective coating with vinylene carbonate and / or vinyl ethylene carbonate, the effects of improving the resistance and durability of the coating film components are further improved, making the movement of lithium ions easier and reducing the precipitation of lithium during rapid charging, thereby effectively improving the rapid charging life.
[0018] Each component of the present invention will be described in more detail below.
[0019] non-aqueous electrolyte The present invention provides a nonaqueous electrolyte for a lithium secondary battery, which contains an organic solvent, a lithium salt, and the following first to third additives.
[0020] Each component of the nonaqueous electrolyte will be specifically described below.
[0021] (1) First to third additives The non-aqueous electrolyte of the present invention contains a first additive which is a compound represented by the following chemical formula 1.
[0022] [Chemical formula 1] P[OSi(R1)]
[0023] In the above Chemical Formula 1, R1 is an alkyl group having 1 to 5 carbon atoms.
[0024] In one embodiment of the present invention, R1 in the formula 1 may be a methyl group. That is, the first additive may be a compound represented by the following formula 1A:
[0025] [ka]
[0026] In one embodiment of the present invention, the content of the first additive may be 0.1 wt % to 5 wt %, preferably 0.3 wt % to 3 wt %, and more preferably 0.5 wt % to 2 wt %, based on the total weight of the non-aqueous electrolyte.
[0027] When the content of the first additive is 0.1 wt % or more, it is preferable since it can contribute to the formation of an electrode coating, and when the content is 5 wt % or less, it is preferable since it can control aging characteristics and gas generation due to side reactions.
[0028] The non-aqueous electrolyte of the present invention contains a second additive which is a compound represented by the following chemical formula 2.
[0029] [ka]
[0030] In the above Chemical Formula 2, n is an integer of 1 or 2.
[0031] In one embodiment of the present invention, n in the above Chemical Formula 2 may be 1. That is, the second additive may be 1,3-propane sultone (PS).
[0032] In one embodiment of the present invention, the content of the second additive may be 0.1 wt % to 5 wt %, preferably 0.3 wt % to 3 wt %, and more preferably 0.5 wt % to 2 wt %, based on the total weight of the non-aqueous electrolyte.
[0033] When the content of the second additive is 0.1 wt % or more, it is preferable since it can have the effect of forming a coating on the electrode, and when it is 5 wt % or less, it is preferable since there is no risk of performance degradation due to increased resistance.
[0034] The non-aqueous electrolyte of the present invention contains a third additive which is one or more selected from the group consisting of vinylene carbonate (VC) and vinylethylene carbonate (VEC), and preferably contains vinylene carbonate.
[0035] In one embodiment of the present invention, the content of the third additive may be 0.1 wt % to 5 wt %, preferably 0.5 wt % to 4 wt %, and more preferably 1 wt % to 3 wt %, based on the total weight of the non-aqueous electrolyte.
[0036] When the content of the third additive is 0.1 wt % or more, it is preferable because it can form a coating film to protect the negative electrode, and when the content is 5 wt % or less, it is preferable because there is no risk of performance degradation due to increased resistance.
[0037] In one embodiment of the present invention, the weight ratio of the third additive to the first additive may be more than 1, specifically, the weight ratio of the first additive to the third additive may be more than 1:1 and not more than 1:10, more specifically, more than 1:1 and not more than 1:5. It is advantageous for the durability of the negative electrode to be enhanced if the content of the third additive is higher than that of the first additive, but it is preferable that the content of the third additive is 10 times or less in order to obtain the optimal effect of the two additives and prevent an increase in resistance.
[0038] (2) Additives 4 to 6 In an embodiment of the present invention, the non-aqueous electrolyte may further include a fourth additive which is an imidazole-based compound. Specifically, the fourth additive may be propargyl 1H-imidazole-1-carboxylate.
[0039] The fourth additive has the effect of modifying the coating components of the electrode and suppressing lithium precipitation due to its structure that stabilizes the bulk properties of the electrolyte and enables the formation of an electrode coating, and is therefore preferable in that it can improve the durability of the coating and suppress lithium precipitation when used together with the first to third additives.
[0040] In one embodiment of the present invention, the content of the fourth additive may be 0.01 wt % to 3 wt %, preferably 0.05 wt % to 2 wt %, and more preferably 0.1 wt % to 1 wt %, based on the total weight of the non-aqueous electrolyte.
[0041] When the content of the fourth additive is 0.01 wt % or more, it is preferable because it can provide an effect of forming a coating on the negative electrode, and when the content is 3 wt % or less, it is preferable because there is no risk of performance degradation due to an increase in resistance.
[0042] In one embodiment of the present invention, the weight ratio of the first additive to the fourth additive may be more than 1, specifically, the weight ratio of the fourth additive to the first additive may be more than 1:1 and not more than 1:10, more specifically, more than 1:2 and not more than 1:5. It is preferable that the content of the first additive is higher than that of the fourth additive in order to form a coating having a lower resistance on the electrode, but it is preferable that the content of the first additive is 10 times or less in order to obtain the optimal effect of the two additives and to control side reactions and gas generation.
[0043] In one embodiment of the present invention, the non-aqueous electrolyte may further include a fifth additive which is N,N'-dicyclohexylcarbodiimide.
[0044] The fifth additive is preferable because it can stabilize the bulk properties of the electrolyte solution and therefore can improve the stability of the additives against aging when used together with the first to third additives.
[0045] In one embodiment of the present invention, the content of the fifth additive may be 0.01 wt % to 3 wt %, preferably 0.05 wt % to 2 wt %, and more preferably 0.1 wt % to 1 wt %, based on the total weight of the non-aqueous electrolyte.
[0046] When the content of the fifth additive is 0.01 wt % or more, it is preferable since it can stabilize the bulk properties of the electrolyte, and when the content is 3 wt % or less, it is preferable since it does not affect the oxidation stability.
[0047] In one embodiment of the present invention, the weight ratio of the first additive to the fifth additive may be more than 1, specifically, the weight ratio of the fifth additive to the first additive may be more than 1:1 and not more than 1:20, more specifically, more than 1:2 and not more than 1:10. It is preferable that the content of the first additive is higher than that of the fifth additive in terms of stable formation of a coating film.
[0048] In one embodiment of the present invention, the non-aqueous electrolyte may further include a sixth additive as required to prevent the electrolyte from being decomposed in a high voltage environment, which may cause the electrode to collapse, or to further improve low-temperature high-rate discharge characteristics, high-temperature stability, overcharge prevention, and effects of suppressing battery expansion at high temperatures.
[0049] The sixth additive may be at least one selected from carbonate-based compounds, sultone-based compounds, sulfate-based compounds, phosphate-based or phosphite-based compounds, nitrile-based compounds, amine-based compounds, silane-based compounds, benzene-based compounds, lithium salt-based compounds, and ether-based compounds.
[0050] The carbonate compound may be one or more selected from ethylene carbonate (EC), fluoroethylene carbonate (FEC), and methylprop-2-ynyl carbonate.
[0051] The sultone-based compound is a material capable of forming a stable SEI film on the surface of the negative electrode through a reduction reaction, and may be one or more compounds selected from ethene sultone, 1,3-propene sultone (PRS), 1,4-butene sultone, and 1-methyl-1,3-propene sultone.
[0052] The sulfate-based compound is a material that can be electrically decomposed on the surface of the negative electrode to form a stable SEI film that does not crack even when stored at high temperatures, and may be at least one selected from ethylene sulfate (Esa), trimethylene sulfate (TMS), and methyltrimethylene sulfate (MTMS).
[0053] The phosphate or phosphite compound may be one or more selected from lithium difluoro(bisoxalato)phosphate, lithium difluorophosphate, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, tris(2,2,2-trifluoroethyl)phosphate, and tris(trifluoroethyl)phosphite.
[0054] The nitrile compound may be one or more selected from succinonitrile (SN), adiponitrile (ADN), acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, 4-fluorophenylacetonitrile, ethylene glycol bis(propionitrile) ether (ASA3), 1,3,6-hexanetricarbonitrile (HTCN), 1,4-dicyano-2-butene (DCB), and 1,2,3-tris(2-cyanoethyl)propane (TCEP).
[0055] The amine compound may be one or more selected from triethanolamine and ethylenediamine, and the silane compound may be tetravinylsilane.
[0056] The benzene-based compound may be at least one selected from fluorobenzene (FB), difluorobenzene, trifluorobenzene, tetrafluorobenzene, and hexafluorobenzene.
[0057] The lithium salt-based compound is a compound different from the lithium salt contained in the electrolyte, and may be one or more compounds selected from lithium difluorophosphate (LiDFP; LiPO2F2), lithium bis(oxalato)borate (LiBOB; LiB(C2O4)2), lithium tetrafluoroborate (LiBF4), lithium difluoro(oxalato)borate (LiODFB), lithium tetraphenylborate, and lithium difluoro(bis(oxalato)phosphate) (LiDFOP).
[0058] The ether-based compound may be one or more compounds selected from 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethylether, bis(trifluoromethyl)-1,3-dioxolane, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropylether.
[0059] Meanwhile, the content of the sixth additive may be 0.1 wt% to 20 wt% based on the total weight of the nonaqueous electrolyte, and preferably 0.3 wt% to 10 wt%. When the content of the sixth additive is within the above range, a side reaction suppressing effect due to the formation of a coating on the positive electrode and the negative electrode can be obtained.
[0060] (3) Organic Solvent The nonaqueous electrolyte of the present invention contains an organic solvent.
[0061] The organic solvent may be any of various organic solvents commonly used in lithium electrolytes without limitation. For example, the organic solvent may be a cyclic carbonate solvent, a linear carbonate solvent, a linear ester solvent, a cyclic ester solvent, a nitrile solvent, a fluorine solvent, or a mixture thereof.
[0062] In one embodiment of the present invention, the organic solvent may be a mixture of a cyclic carbonate solvent and a linear carbonate solvent. In this case, there is an advantage that an electrolyte solution having high ionic conductivity can be produced.
[0063] The cyclic carbonate solvent is an organic solvent having high viscosity and has the advantage of easily dissociating the lithium salt in the electrolyte due to its high dielectric constant, and may be one or more selected from ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, and vinylene carbonate, and is preferably ethylene carbonate (EC).
[0064] The linear carbonate solvent is an organic solvent having low viscosity and low dielectric constant, and may be one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate, and is preferably dimethyl carbonate (DMC).
[0065] The linear ester solvent may be one or more selected from methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate (EP), propyl propionate (PP), and butyl propionate, and may be preferably ethyl propionate, propyl propionate, or a mixture thereof.
[0066] The cyclic ester solvent may be one or more selected from γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.
[0067] The nitrile solvent may be one or more selected from succinonitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile, and may be preferably succinonitrile.
[0068] The fluorine-based solvent may be 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether, 2,2-bis(trifluoromethyl)-1,3-dioxolane, 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether, trifluoroethyl phosphate, trifluoroethyl phosphite, ethyl 4,4,4-trifluorobutyrate, 1,2-ethanedisulfonyl difluoride, The fluoroethyl ether may be one or more selected from the group consisting of 1,1,2,2,3,3,4,4-octafluoro-5-(1,1,2,2,-tetrafluoroethoxy)pentane, 1,1,2,2,3,3,4,4-octafluoro-5-(1,1,2,2,-tetrafluoroethoxy)pentane, 1-fluoroethyl methyl carbonate (F-EMC), 2,2,2-trifluoroethyl methyl carbonate (F3-EMC), difluoroethyl acetate, methyl difluoroacetate, ethyl difluoroacetate, and 1,1,2,2,3,3,4,4-octafluoro-5-(1,1,2,2,-tetrafluoroethoxy)pentane.
[0069] In the total weight of the nonaqueous electrolyte solution, the remainder excluding the organic solvent, for example, the first to sixth additives and the lithium salt, is the organic solvent unless otherwise specified.
[0070] (4) Lithium salt The non-aqueous electrolyte of the present invention contains a lithium salt.
[0071] The lithium salt may be any one that is commonly used in electrolytes for lithium secondary batteries, and may be used without limitation. Specifically, the lithium salt may have a cation of Li + and as an anion, F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , B 10 Cl 10 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , (CF3CF2SO2)2N - , (CF3SO2)2N - , (FSO2)2N - , BF2C2O4 - , BC4O8 - , BF2C2O4CHF - , PF4C2O4 - , PF2C4O8 - , PO2F2 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , C4F9SO3 - , CF3CF2SO3 - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CF3(CF2)7SO3 - , and SCN -may include any one or more selected from the following:
[0072] Specifically, the lithium salt may be LiPF6, LiClO4, LiBF4, LiN(FSO2)2 (LiFSI), LiN(CF3SO2)2 (LiTFSI), lithium bis(pentafluoroethanesulfonyl)imide (LiBETI), LiSO3CF3, LiPO2F2, lithium bis(oxalate)borate (LiBOB), lithium difluoro(oxalate)borate (LiODFB), lithium difluoro(bisoxalato)phosphate (LiDFOP), lithium tetrafluoro(oxalate)phosphate (LiTFOP), and lithium fluoromalonato(difluoro)borate (LiTFOP). borate, LiFMDFB), and preferably LiPF6.
[0073] In one embodiment of the present invention, the concentration of the lithium salt in the non-aqueous organic solution containing the lithium salt and the organic solvent may be 0.5 M to 5.0 M, specifically 0.5 M to 3.0 M, more specifically 0.8 M to 2.0 M. When the concentration of the lithium salt satisfies the above range, it is possible to obtain an electrolyte solution having appropriate impregnation properties while sufficiently ensuring the effects of improving low-temperature output and cycle characteristics and preventing the viscosity and surface tension from becoming excessively high.
[0074] Lithium secondary battery Next, the lithium secondary battery according to the present invention will be described.
[0075] The lithium secondary battery according to the present invention includes a positive electrode including a positive electrode active material, a negative electrode including a negative electrode active material, a separator interposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte, the non-aqueous electrolyte being the non-aqueous electrolyte according to the present invention. The non-aqueous electrolyte is as described above, so a description thereof will be omitted, and other components will be described below.
[0076] (1) Positive electrode The positive electrode according to the present invention includes a positive electrode active material, and can be manufactured by coating a positive electrode slurry including a positive electrode active material, a binder, a conductive material, a solvent, etc., on a positive electrode current collector, followed by drying and rolling.
[0077] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, stainless steel; aluminum; nickel; titanium; baked carbon; or aluminum or stainless steel whose surface has been surface-treated with carbon, nickel, titanium, silver, or the like may be used.
[0078] The positive electrode active material is not particularly limited as long as it is a compound capable of reversible intercalation and deintercalation of lithium, and may include, for example, any one or more selected from the group consisting of lithium cobalt-based oxides, lithium nickel-based oxides, lithium nickel cobalt-based oxides, lithium manganese-based oxides, lithium nickel manganese-based oxides, lithium phosphate-based oxides, and lithium nickel cobalt manganese-based oxides.
[0079] More specifically, the positive electrode active material may be a lithium cobalt oxide such as LiCoO2 (LCO); a lithium nickel oxide such as LiNiO2 (LNO); 1-y4 Co y4 Lithium nickel cobalt oxides such as LiO2 (0≦y4<1); Lithium manganese oxides such as LiMnO2 (LMO), LiMnO3, LiMn2O3, and Li2MnO3; Li 1+y1 Mn 2-y1O4(0≦y1≦0.33), LiNi y2 Mn 2-y2 O4(0≦y2≦2), LiNi y3 Mn 2-y3 O2 (0.01≦y3≦0.1), and lithium nickel manganese-based oxides such as Li2NiMn3O8; lithium phosphate-based oxides such as LiFePO4 and LiCoPO4; and lithium nickel cobalt manganese-based oxides represented by the following chemical formula 3, and preferably lithium nickel cobalt manganese-based oxide represented by the following chemical formula 3.
[0080] [Chemical formula 3] Li 1+x (Ni a Co b Mn c M d )O2
[0081] In the above Chemical Formula 3, M is one or more selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; 1+x, a, b, c, and d are the atomic fractions of each independent element, -0.2≦x≦0.2, 0.50≦a<1, 0 <b≦0.40、0<c≦0.40、0≦d≦0.1、a+b+c+d=1である。
[0082] The 1+x represents the molar ratio of lithium in the lithium nickel cobalt manganese-based oxide, and may be -0.1≦x≦0.2 or 0≦x≦0.2. When the lithium molar ratio satisfies the above range, the crystal structure of the lithium nickel cobalt manganese-based oxide can be stably formed.
[0083] Said a represents the molar ratio of nickel in all metals excluding lithium in the lithium nickel cobalt manganese oxide, and it may be 0.60 ≦ a < 1, 0.70 ≦ a < 1, or 0.80 ≦ a < 1. When the molar ratio of nickel satisfies the above range, it exhibits a high energy density and high capacity can be achieved.
[0084] Said b represents the molar ratio of cobalt in all metals excluding lithium in the lithium nickel cobalt manganese oxide, and it may be 0 < b ≦ 0.30, 0 < b ≦ 0.20, or 0 < b ≦ 0.10. When the molar ratio of cobalt satisfies the above range, good resistance characteristics and output characteristics can be realized.
[0085] Said c represents the molar ratio of manganese in all metals excluding lithium in the lithium nickel cobalt manganese oxide, and it may be 0 < c ≦ 0.30, 0 < c ≦ 0.20, or 0 < c ≦ 0.10. When the molar ratio of manganese satisfies the above range, it has excellent structural stability of the positive electrode active material.
[0086] In one embodiment of the present invention, the lithium nickel cobalt manganese oxide may contain any one or more doping elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo, and preferably may contain Al as the doping element. In other words, said d representing the molar ratio of the doping element in all metals excluding lithium in the lithium composite transition metal oxide may be 0 < d ≦ 0.08, 0 < d ≦ 0.05, or 0 < d ≦ 0.03.
[0087] For example, the lithium nickel cobalt manganese oxide is Li(Ni 0.6 Co 0.2 Mn 0.2 )O2, Li(Ni 0.7 Co 0.15 Mn 0.15 )O2, Li(Ni 0.8 Co 0.1 Mn0.1 )O2, and Li(Ni 0.9 Co 0.05 Mn 0.04 Al 0.01 ) O2.
[0088] In particular, the lithium nickel cobalt manganese oxide may have a nickel content of 85 mol % or more in the total transition metal content, i.e., it may be an ultra-high nickel material in which 0.85≦a<1 in Chemical Formula 3. In this case, b, c, and d are each 0. <b≦0.1、0<c≦0.1、0≦d≦0.03であってもよい。
[0089] A positive electrode active material with a high nickel content may be structurally unstable, which may increase side reactions and gas generation, thereby shortening the battery life. However, when the nonaqueous electrolyte according to the present invention is applied, it has an excellent effect of improving the coating properties of the electrode, thereby solving the problems associated with the application of such a high-nickel positive electrode active material.
[0090] The positive electrode active material may be contained in an amount of 80% by weight to 99% by weight, specifically 90% by weight to 99% by weight, based on the total weight of the solid content in the positive electrode slurry. If the content of the positive electrode active material is less than 80% by weight, the energy density may be reduced, and the capacity may be reduced.
[0091] The binder is a component that assists in binding the active material and conductive material, etc., and binding to the current collector, and may be added in an amount of 1% by weight to 30% by weight based on the total weight of the solid content in the positive electrode slurry. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, or various copolymers thereof.
[0092] The conductive material is a substance that imparts conductivity to the battery without causing any chemical change, and may be added in an amount of 0.5% by weight to 20% by weight based on the total weight of the solid content in the positive electrode slurry.
[0093] The conductive material may be selected from, for example, carbon blacks such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; graphite powders such as natural graphite, artificial graphite, carbon nanotubes, and graphite; conductive fibers such as carbon fibers and metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0094] The solvent for the positive electrode slurry may contain an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a suitable viscosity when containing the positive electrode active material, binder, conductive material, etc. For example, the positive electrode slurry containing the positive electrode active material, binder, and conductive material may be contained so that the solid content concentration is 40% by weight to 90% by weight, preferably 40% by weight to 60% by weight.
[0095] (2) Negative electrode The negative electrode according to the present invention includes a negative electrode active material, and can be manufactured by coating a negative electrode slurry including a negative electrode active material, a binder, a conductive material, a solvent, etc., on a negative electrode current collector, followed by drying and rolling.
[0096] The negative electrode according to the present invention includes a negative electrode active material, and can be manufactured by coating a negative electrode slurry including a negative electrode active material, a binder, a conductive material, a solvent, etc., on a negative electrode current collector, followed by drying and rolling.
[0097] The negative electrode current collector generally has a thickness of 3 μm to 500 μm. Such a negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and for example, copper; stainless steel; aluminum; nickel; titanium; baked carbon; copper or stainless steel surface treated with carbon, nickel, titanium, silver, or the like; or an aluminum-cadmium alloy may be used. In addition, as with the positive electrode current collector, the binding force of the negative electrode active material may be strengthened by forming fine irregularities on the surface, and the negative electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0098] The negative electrode active material may include one or more selected from a carbon material capable of reversibly intercalating / deintercalating lithium ions; a metal or an alloy of such a metal and lithium; a metal composite oxide; a material capable of doping and dedoping lithium; lithium metal; and a transition metal oxide.
[0099] The carbonaceous material capable of reversibly intercalating / deintercalating lithium ions may be any carbonaceous negative electrode active material commonly used in lithium ion secondary batteries, and representative examples thereof include crystalline carbon, amorphous carbon, or a combination of both. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite; artificial graphite; double layer graphite; or a mixture thereof, and examples of the amorphous carbon include soft carbon (low-temperature calcined carbon), hard carbon, mesophase pitch carbide, and calcined coke.
[0100] The metal or the alloy of these metals and lithium may be a metal selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn, or an alloy of these metals and lithium.
[0101] Examples of the metal composite oxide include PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, Li x Fe2O3 (0 ≦ x ≦ 1), Li x WO2 (0 ≦ x ≦ 1), and Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, elements of Group 1, Group 2, Group 3 of the periodic table, halogen; 0 < x ≦ 1; 1 ≦ y ≦ 3; 1 ≦ z ≦ 8), and one or more selected from the group consisting thereof can be used.
[0102] Examples of the substance capable of doping and undoping lithium include Si, SiO x (0 < x < 2), Si - Y alloy (wherein Y is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, and combinations thereof, and is not Si), Sn, SnO2, Sn - Y (wherein Y is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, and combinations thereof, and is not Sn), etc. Further, at least one of these and SiO2 may be mixed and used. The element Y may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db (dubnium), Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0103] Examples of the transition metal oxide include lithium - containing titanium composite oxide (LTO), vanadium oxide, lithium vanadium oxide, etc.
[0104] In one embodiment of the present invention, the negative electrode active material may include a blend of natural graphite and artificial graphite; or double layer graphite, which has the advantage of reducing the cost of the battery and improving its performance.
[0105] The negative electrode active material may be included in an amount of 80% by weight to 99% by weight based on the total weight of solids in the negative electrode slurry.
[0106] The binder is a component that assists in bonding between the conductive material, the active material, and the current collector, and may be added in an amount of 1% by weight to 30% by weight based on the total weight of the solid content in the negative electrode slurry. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, and various copolymers thereof.
[0107] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 0.5% by weight to 20% by weight based on the total weight of the solid content in the negative electrode slurry. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and may be selected from, for example, carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; graphite powder such as natural graphite, artificial graphite, carbon nanotube, and graphite; conductive fibers such as carbon fiber and metal fiber; conductive powders such as carbon fluoride powder, aluminum powder, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0108] The solvent for the negative electrode slurry may include water or an organic solvent such as NMP or alcohol, and may be used in an amount that provides a suitable viscosity when containing the negative electrode active material, binder, conductive material, etc. For example, the solvent may be included so that the concentration of solids in the slurry containing the negative electrode active material, binder, and conductive material is 30% by weight to 80% by weight, preferably 40% by weight to 70% by weight.
[0109] (3) Separator The lithium secondary battery according to the present invention includes a separator between the positive electrode and the negative electrode.
[0110] The separator separates the negative electrode and the positive electrode and provides a path for lithium ion migration. Any separator that is typically used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to the migration of ions in the electrolyte and has excellent electrolyte impregnation ability and safety is preferred.
[0111] Specifically, the separator may be a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer; or a laminated structure of two or more layers thereof. In addition, a normal porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, or the like, may be used. In order to ensure heat resistance or mechanical strength, a coated separator containing a ceramic component or a polymeric substance may be used, and may be used as a single layer or a multilayer structure.
[0112] The lithium secondary battery according to the present invention as described above can be usefully used in portable devices such as mobile phones, notebook computers, and digital cameras; and electric vehicles such as hybrid electric vehicles (HEVs).
[0113] According to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.
[0114] The battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, including power tools; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); and power storage systems.
[0115] The external shape of the lithium secondary battery of the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.
[0116] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for small devices, but also suitably as a unit battery in a medium- to large-sized battery module containing a large number of battery cells.
[0117] The present invention will now be described in more detail with reference to specific examples.
[0118] <Examples and Comparative Examples: Manufacture of Lithium Secondary Battery> Example 1. (Production of non-aqueous electrolyte) Ethylene carbonate (EC) and dimethyl carbonate (DMC) were mixed in a volume ratio of 30:70, and LiPF6 was dissolved therein to a concentration of 1.0 M to prepare a non-aqueous organic solution. 1 wt% of the compound represented by Chemical Formula 1A, 1 wt% of 1,3-propane sultone (PS), 2 wt% of vinylene carbonate (VC), 0.3 wt% of 1H-imidazole-1-carboxylate, and the remaining non-aqueous organic solution were mixed to prepare a 100 wt% non-aqueous electrolyte.
[0119] (manufacturing lithium secondary batteries) N-methyl-2-pyrrolidone (NMP) with LiNi as the positive electrode active material 0.9 Co 0.05 Mn 0.04 Al 0.01 A positive electrode slurry (solid content: 50 wt%) was prepared by adding O2, a conductive material (carbon black), and a binder (polyvinylidene fluoride) in a weight ratio of 98:0.5:1.5. The positive electrode slurry was applied to a 15 μm-thick aluminum (Al) thin film, which is a positive electrode current collector, and dried, followed by roll pressing to prepare a positive electrode.
[0120] Anode active material (graphite blended with artificial graphite and natural graphite in a weight ratio of 3:7), binder (SBR-CMC), and conductive material (carbon black) were added to the solvent water in a weight ratio of 98:1:1 to prepare anode slurry (solid content: 60wt%). The anode slurry was applied to a copper (Cu) thin film as an anode current collector with a thickness of 6μm, dried, and then roll pressed to prepare the anode.
[0121] The positive electrode, a polyolefin-based porous separator coated with inorganic particles (Al2O3), and a negative electrode were sequentially stacked to prepare an electrode assembly.
[0122] The electrode assembly assembled as described above was placed in a pouch-shaped battery case, and the non-aqueous electrolyte prepared as described above was poured into the case, thereby producing a lithium secondary battery.
[0123] Example 2. A lithium secondary battery was manufactured in the same manner as in Example 1, except that propargyl 1H-imidazole-1-carboxylate was not added during the preparation of the non-aqueous electrolyte.
[0124] Example 3. A lithium secondary battery was manufactured in the same manner as in Example 1, except that 0.1 wt % of N,N'-dicyclohexylcarbodiimide was added as a fifth additive during the preparation of the nonaqueous electrolyte solution.
[0125] Example 4. A lithium secondary battery was produced in the same manner as in Example 2, except that 0.1 wt % of N,N'-dicyclohexylcarbodiimide was added as a fifth additive during the production of the nonaqueous electrolyte solution.
[0126] Comparative Example 1 A lithium secondary battery was manufactured in the same manner as in Example 1, except that the compound represented by Formula 1A was not used in preparing the non-aqueous electrolyte.
[0127] Comparative Example 2 A lithium secondary battery was produced in the same manner as in Example 1, except that 1,3-propane sultone (PS) was not added during the production of the non-aqueous electrolyte solution.
[0128] Comparative Example 3. A lithium secondary battery was produced in the same manner as in Example 1, except that vinylene carbonate (VC) was not added during the production of the non-aqueous electrolyte solution.
[0129] Comparative Example 4. A lithium secondary battery was manufactured in the same manner as in Example 2, except that the compound represented by Formula 1A was not added during the preparation of the non-aqueous electrolyte.
[0130] Comparative Example 5. A lithium secondary battery was produced in the same manner as in Example 2, except that 1,3-propane sultone (PS) was not added during the production of the non-aqueous electrolyte solution.
[0131] Comparative Example 6. A lithium secondary battery was produced in the same manner as in Example 2, except that vinylene carbonate (VC) was not added during the production of the non-aqueous electrolyte solution.
[0132] <Experimental example: Performance evaluation of lithium secondary batteries> Experimental example 1: High temperature quick charging performance evaluation For each of the lithium secondary batteries manufactured in the Examples and Comparative Examples, a lithium secondary battery was prepared with a SOC (State Of Charge) of 3%, and then charged while changing the C-rate according to the SOC state as shown in Table 1 below. The voltage value was checked at an interval of 1 second for each charging section, and a voltage profile was measured.
[0133] [Table 1]
[0134] Then, the end conditions were set based on the voltage values obtained for each section, and the charge amount when charging in CC mode was recorded. Then, further, in CC mode, the battery was discharged at 0.5C to SOC 3%. The above charge and discharge constitute one cycle, and the initial capacity, which is the discharge capacity of the first cycle, was measured at room temperature (25°C), and the discharge capacity after 100 cycles at 45°C was measured. Based on the measured values, the capacity retention rate after rapid charging was calculated using the following formula 1, and the results are shown in Table 2 below.
[0135] [Formula 1] Capacity retention rate (%) = (capacity measured after 100 cycles / initial capacity) x 100
[0136] Experimental example 2: Room temperature resistance evaluation The lithium secondary batteries manufactured in the examples and comparative examples were subjected to electrochemical impedance spectroscopy (EIS) using a VMP-3 model manufactured by Bio-logic Science Instruments. ct Specifically, the charge transfer resistance (R) was measured after two hours while passing an AC current of 10 mV through each battery at 0% and 50% SOC at room temperature (25°C). ct Value confirmed.
[0137] R measured on the battery of Comparative Example 1 ctR of each battery against the value ct The values were calculated according to the following formula 2 and are listed in Table 2 below.
[0138] [Formula 2] Resistance change rate (%) = (R ct -R of the battery of Comparative Example 1 ct ) / (R of the battery of Comparative Example 1 ct ) x 100
[0139] Experimental example 3: Low-temperature rapid discharge output evaluation The lithium secondary batteries prepared in the Examples and Comparative Examples were charged at 25° C. under constant current / constant voltage conditions at a rate of 0.2 C up to 4.2 V, and then a 0.05 C current cut was performed. The discharge capacity after discharging at a rate of 0.2 C up to 2.5 V under constant current conditions was set as the initial discharge capacity.
[0140] Next, the battery was charged at 25° C. under constant current / constant voltage conditions at a rate of 0.2 C up to 4.2 V, and then the current was cut at 0.05 C and the battery was rapidly discharged at a rate of 2 C up to 2.5 V under constant current conditions at 0° C. Based on the discharge capacity measured at this time, the discharge output after rapid discharge was calculated according to the following formula 3, and the results are shown in Table 2 below.
[0141] [Formula 3] Discharge output (%) = (capacity measured after rapid discharge / initial discharge capacity) x 100
[0142] [Table 2]
[0143] From the results in Table 2, it can be seen that Examples 1 to 4, which use a non-aqueous electrolyte containing any of the first to third additives according to one embodiment of the present invention, show superior results in the rapid charge evaluation, room temperature resistance evaluation, and low temperature rapid discharge evaluation compared to Comparative Examples 1 to 6. In particular, this is significant in that the performance of a battery using an ultra-high nickel cathode material is improved when the battery is subjected to rapid charge and discharge under various temperature conditions.
[0144] Specifically, Comparative Examples 1 to 3 were prepared under the same conditions as Example 1, but with the first additive, the second additive, and the third additive excluded, respectively, from the nonaqueous electrolyte solution, and Comparative Examples 4 to 6 were prepared under the same conditions as Example 2, but with the first additive, the second additive, and the third additive excluded, respectively, from the nonaqueous electrolyte solution. Thus, by comparing the results of Example 1 and Comparative Examples 1 to 3, and the results of Example 2 and Comparative Examples 4 to 6, it can be seen that in order to achieve the effects of the present invention, it is essential to include all of the first to third additives.
Claims
1. An organic solvent; A lithium salt; A first additive which is a compound represented by the following chemical formula 1; A second additive which is a compound represented by the following chemical formula 2; A non-aqueous electrolyte solution for a lithium secondary battery comprising: a third additive which is one or more selected from the group consisting of vinylene carbonate and vinyl ethylene carbonate: [Chemical formula 1] P[OSi(R1) 3 ] 3 (In the above Chemical Formula 1, R1 is an alkyl group having 1 to 5 carbon atoms; 【Chemistry 1】 In the above Chemical Formula 2, n is an integer of 1 or 2.
2. 2. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein R1 in the formula (1) is a methyl group.
3. The nonaqueous electrolyte for a lithium secondary battery according to claim 1 , wherein n in the formula (2) is 1.
4. 2. The non-aqueous electrolyte for a lithium secondary battery according to claim 1, wherein the content of the first additive is 0.1 to 5 wt % based on the total weight of the non-aqueous electrolyte.
5. 2. The non-aqueous electrolyte for a lithium secondary battery according to claim 1, wherein the content of the second additive is 0.1 to 5 wt % based on the total weight of the non-aqueous electrolyte.
6. 2. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein a weight ratio of the third additive to the first additive is greater than 1.
7. 2. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, further comprising a fourth additive which is an imidazole-based compound.
8. 8. The nonaqueous electrolyte for a lithium secondary battery according to claim 7, wherein the fourth additive is propargyl 1H-imidazole-1-carboxylate.
9. 8. The nonaqueous electrolyte for a lithium secondary battery according to claim 7, wherein a weight ratio of the first additive to the fourth additive is greater than 1.
10. 8. The nonaqueous electrolyte for a lithium secondary battery according to claim 7, further comprising a fifth additive which is N,N'-dicyclohexylcarbodiimide.
11. 2. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein the organic solvent comprises a mixture of a cyclic carbonate solvent and a linear carbonate solvent.
12. a positive electrode including a positive electrode active material; a negative electrode including a negative electrode active material; a separator interposed between the positive electrode and the negative electrode; A lithium secondary battery comprising the nonaqueous electrolyte solution according to claim 1 .
13. 13. The lithium secondary battery according to claim 12, wherein the positive electrode active material includes at least one selected from the group consisting of lithium cobalt-based composite oxides, lithium nickel-based composite oxides, lithium nickel cobalt-based composite oxides, lithium manganese-based composite oxides, lithium nickel manganese-based composite oxides, lithium iron phosphate-based composite oxides, and lithium nickel cobalt manganese-based composite oxides.
14. The lithium secondary battery according to claim 13 , wherein the positive electrode active material comprises a lithium nickel cobalt manganese-based oxide represented by the following Chemical Formula 3: [Chemical formula 3] Li 1+x (N a Co b Mn c M d )O 2 (In the above Chemical Formula 3, M is at least one selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; 1+x, a, b, c, and d are each independently the atomic fraction of an element, -0.2≦x≦0.2, 0.50≦a<1, 0<b≦0.40, 0<c≦0.40, 0≦d≦0.1, a+b+c+d=1.)
15. 13. The lithium secondary battery according to claim 12, wherein the negative electrode active material comprises a mixture of natural graphite and artificial graphite, or double-layer graphite.
Citation Information
Patent Citations
High-voltage lithium ion battery electrolyte and lithium ion battery using same
CN111740163A
Non-aqueous electrolyte for lithium battery, preparation method of non-aqueous electrolyte and lithium ion battery
CN113328143A
Method for preparing polymer lithium batteries
JP2013504170A
Device and method for judging fall accidents based on artificial intelligence and providing a notification of the occurrence of a fall to a guardian's terminal
KR1020230024770A
Composition for gel polymer electrolyte, gel polymer electrolyte prepared therefrom, and lithium secondary battery including the same
US20210194052A1