Continuous reaction system, manganese iron phosphate precursor, lithium manganese iron phosphate, and method for producing the same and secondary battery
The continuous reaction system addresses inefficiencies in manganese iron phosphate production by ensuring consistent quality and efficiency, producing precursors with controlled particle size and shape, enhancing the performance of lithium manganese iron phosphate batteries.
Patent Information
- Application Number
- JP2024503350
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-07-15
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-07-15
AI Technical Summary
Current manganese iron phosphate production methods are inefficient, leading to low production efficiency, complicated processes, and inconsistent product quality due to intermittent production, which affects the stability and consistency of lithium manganese iron phosphate batteries.
A continuous reaction system is employed, comprising a series-connected first and second reaction vessels and an aging vessel, with controlled flow rates and temperatures to produce manganese iron phosphate precursors with small particle size, narrow distribution, high crystallinity, and regular shape, using a hydrothermal method with complexing agents and surfactants to enhance uniformity and control.
The method achieves high manufacturing efficiency, energy efficiency, and low labor costs, producing manganese iron phosphate precursors with consistent quality, enabling the production of lithium manganese iron phosphate with improved electrical and chemical properties.
Smart Images

Figure 2024536670000001_ABST
Abstract
Description
[Technical field]
[0001] The present application relates to the field of battery technology, and in particular to a continuous reaction system, a manganese iron phosphate precursor, lithium manganese iron phosphate, and a preparation method thereof and a secondary battery. [Background technology]
[0002] In recent years, secondary batteries have been widely applied in energy storage power systems such as hydroelectric, thermal, wind and solar power stations, as well as in multiple fields such as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and the like. With the application and popularity of secondary batteries, their safety performance has been increasingly focused on. Lithium manganese iron phosphate is one of the most popular positive electrode active materials at present due to its advantages of large capacity, high safety performance, and abundant raw material supply sources. Iron manganese phosphate is one of the important raw materials for producing lithium manganese iron phosphate, and the impact of its performance on lithium manganese iron phosphate and secondary battery performance is extremely important. However, at present, iron manganese phosphate is obtained by using an intermittent production method, which has problems such as low production efficiency, complicated processes, difficulty in controlling the production process, large fluctuations in product quality, and poor stability and consistency of batch production. Summary of the Invention
[0003] The present application aims to provide a continuous reaction system, an iron manganese phosphate precursor, a lithium manganese iron phosphate, and a secondary battery, which are intended to improve the production efficiency of an iron manganese phosphate precursor and obtain an iron manganese phosphate precursor having a small particle size, a narrow particle size distribution, a high crystallinity, single crystallites, a regular shape, a high tap density, and high batch production stability and consistency.
[0004] According to a first aspect of the present application, there is provided a continuous reaction system for producing an iron manganese phosphate precursor, the continuous reaction system comprising a first material melting kettle, a second material melting kettle, a first reaction kettle, a second reaction kettle and an aging kettle, the first reaction kettle, the second reaction kettle and the aging kettle being connected in series in sequence via a pipeline, the first material melting kettle being used for receiving a metal salt solution required for producing the iron manganese phosphate precursor, the second material melting kettle being used for receiving an oxidizing agent and a phosphorus source solution required for producing the iron manganese phosphate precursor, the first reaction kettle having a first supply port and a first overflow port, the first supply port of the first reaction kettle being connected to the first material melting kettle and the second material melting kettle via a first pipeline and a second pipeline respectively, so that the first reaction kettle receives the metal salt solution and the phosphorus source solution, mixes them and reacts them to produce a first reaction liquid, and a first shutoff valve is provided in the first pipeline. and a first metering pump is installed to adjust the flow rate of the metal salt solution; a second shutoff valve and a second metering pump are installed in the second line to adjust the flow rate of the phosphorus source solution; the second reaction kettle has a second inlet and a second overflow port, and the second inlet of the second reaction kettle is connected to the first overflow port of the first reaction kettle through the third line, so that the second reaction kettle receives the first reaction liquid from the first reaction kettle and continuously reacts it to produce a second reaction liquid; the aging kettle includes a third inlet and a third overflow port, and the third inlet of the aging kettle is connected to the second overflow port of the second reaction kettle through the fourth line, so that the aging kettle receives the second reaction liquid from the second reaction kettle and continuously reacts it to produce a third reaction liquid; when the liquid level of the third reaction liquid is higher than the third overflow port of the aging kettle, the third reaction liquid flows out via the third overflow port of the aging kettle.
[0005] According to a second aspect of the present application, there is provided a method for producing an iron manganese phosphate precursor, comprising: at least a first reaction kettle, a second reaction kettle, and an aging kettle, which are connected in series in this order via pipelines; the first reaction kettle has a first supply port and a first overflow port; the first supply port of the first reaction kettle is connected to a first material melting kettle via a first pipeline; the first supply port of the first reaction kettle is connected to a second material melting kettle via a second pipeline; a first shutoff valve and a first metering pump are installed in the first pipeline; a second shutoff valve and a second metering pump are installed in the second pipeline; and the second reaction kettle has a second supply port and a second overflow port. a step S1 in which a metal salt solution required for producing an iron manganese phosphate precursor is added to a first material dissolving pot, an oxidizing agent and a phosphorus source solution required for producing an iron manganese phosphate precursor are added to a second material dissolving pot, and the metal salt solution in the first material dissolving pot is pumped through a first shutoff valve and a first metering pump to the first line. and pumping the phosphorus source solution in the second material dissolution kettle through the second shutoff valve and the second metering pump into the second line, so that the metal salt solution and the phosphorus source solution are mixed and reacted in the first reaction kettle to produce a first reaction liquid; when the liquid level of the first reaction liquid is higher than the first overflow port of the first reaction kettle, the first reaction liquid is automatically transported to the second reaction kettle to continue the reaction to produce a second reaction liquid; when the liquid level of the second reaction liquid is higher than the second overflow port of the second reaction kettle, the second reaction liquid is automatically transported to the aging kettle to continue the reaction to produce a third reaction liquid; when the liquid level of the third reaction liquid is higher than the third overflow port of the aging kettle, the second reaction liquid is automatically transported to the aging kettle to continue the reaction to produce a third reaction liquid; If the temperature is higher than the overflow port, the third reaction liquid will automatically flow out through the third overflow port of the aging kettle; during the reaction process, the first material dissolving kettle, the second material dissolving kettle, the first reaction kettle, the second reaction kettle and the aging kettle are all under a protective gas atmosphere and each kettle is kept in a stirring state, preferably, the protective gas includes nitrogen gas, inert gas or a combination thereof; and step S3, filtering, washing and drying the third reaction liquid obtained from the third overflow port of the aging kettle to obtain a manganese iron phosphate precursor.
[0006] The method for preparing the manganese iron phosphate precursor provided by the present application has the advantages of high production efficiency, high energy efficiency, simple process, easy operation and low labor cost, and is particularly suitable for large-scale industrial production. The method for preparing the manganese iron phosphate precursor provided by the present application is a continuous preparation method, and the manganese iron phosphate precursor obtained by the continuous preparation method provided by the present application has a small particle size, a narrow particle size distribution, a high crystallinity, single crystallites, a regular shape, a high tap density, and high batch production stability and consistency. The method for preparing the manganese iron phosphate precursor provided by the present application can adjust the growth rate of crystal particles and adjust the size and shape of crystal particles, thereby meeting different production requirements and preparing lithium manganese iron phosphate with different particle sizes.
[0007] In any embodiment of the present application, a complexing agent is further added to the first material melting pot, preferably the complexing agent comprises one or more of amino carboxylate, hydroxy carboxylate and organic phosphonate, more preferably comprises one or more of sodium nitrilotriacetate, disodium ethylenediaminetetraacetate, sodium gluconate and sodium citrate, thereby obtaining spherical manganese iron phosphate precursor particles with high purity and uniform distribution of metal elements, which have higher tap density and can realize precise control of metal element content at the same time.
[0008] In any embodiment of the present application, a surfactant is further added to the first material dissolving kettle, preferably the surfactant includes one or more of cetyltrimethylammonium bromide, sodium dodecylsulfonate, and polyvinylpyrrolidone, which helps to better control the shape of the iron manganese phosphate precursor particles.
[0009] In any embodiment of the present application, the reaction temperature of the first reactor is lower than that of the second reactor, and the reaction temperature of the aging reactor is lower than that of the second reactor, which not only can adjust the particle size of the obtained manganese phosphate iron precursor, but also helps to obtain manganese phosphate iron precursor particles with narrow particle size distribution, high crystallinity, single crystallites, regular shape and high tap density.
[0010] In any embodiment of the present application, the reaction temperature of the first reaction vessel is 70°C to 90°C.
[0011] In any embodiment of the present application, the reaction temperature of the second reactor is 150°C to 250°C.
[0012] In any embodiment of the present application, the reaction temperature in the aging tank is 20°C to 30°C.
[0013] In any embodiment of the present application, the flow rate of the metal salt solution in the first pipeline is 0.2 L / min to 2 L / min, and preferably 0.25 L / min to 1 L / min.
[0014] In any embodiment of the present application, the flow rate of the phosphorus source solution in the second pipeline is 0.2 L / min to 2 L / min, and preferably 0.25 L / min to 1 L / min.
[0015] In any embodiment of the present application, the flow rates of the metal salt solution and the phosphorus source solution are the same, which helps to improve the uniformity of the obtained iron manganese phosphate precursor particles.
[0016] In any embodiment of the present application, the residence time of the iron manganese phosphate precursor in the first reaction vessel during the growth process is 1 hour to 4 hours.
[0017] In any embodiment of the present application, the residence time of the iron manganese phosphate precursor in the second reaction vessel during the growth process is 1 h to 16 h, and preferably 4 h to 16 h.
[0018] In any embodiment of the present application, the residence time in the aging vessel during the growth process of the iron manganese phosphate precursor is 1 hour to 48 hours, and preferably 12 hours to 48 hours.
[0019] In any embodiment of the present application, the volume of the first reaction kettle is equal to or less than the volume of the second reaction kettle, and preferably, the ratio of the volume of the first reaction kettle to the volume of the second reaction kettle is 1:(1-4), more preferably 1:(2-4), which helps the obtained iron manganese phosphate precursor particles to have a higher crystallinity.
[0020] In any embodiment of the present application, the volume of the first reaction kettle is equal to or less than the volume of the aging kettle, and preferably, the ratio of the volume of the first reaction kettle to the volume of the aging kettle is 1:(1-12), more preferably 1:(4-12), which helps the obtained iron manganese phosphate precursor to have a larger particle size.
[0021] In any embodiment of the present application, the volume of the second reaction kettle is equal to or less than the volume of the aging kettle, and preferably, the ratio of the volume of the second reaction kettle to the volume of the aging kettle is 1:(1-3), more preferably 1:(2-3), which helps the obtained iron manganese phosphate precursor to have a larger particle size.
[0022] In any embodiment of the present application, the metal salts necessary for preparing the iron manganese phosphate precursor include a water-soluble iron salt, a water-soluble manganese salt and preferably a salt of a water-soluble doping element M, where M represents a doping element for the manganese and iron sites and preferably includes one or more of Co, Mg, Zn, Ca, Ti, V, Ni, Cr.
[0023] In any embodiment of the present application, preferably the water soluble iron salt comprises one or more of ferrous chloride, ferrous nitrate, ferrous sulfate, ferrous acetate, ferric chloride, ferric nitrate, ferric sulfate, and ferric acetate.
[0024] In any embodiment of the present application, preferably the water soluble manganese salt comprises one or more of manganous chloride, manganous nitrate, manganous sulfate, manganous acetate.
[0025] In any embodiment of the present application, preferably, the water-soluble salt of doping element M comprises one or more of the hydrochloride, nitrate, sulfate, acetate salt of doping element M.
[0026] In any embodiment of the present application, the phosphorus source required for producing the iron manganese phosphate precursor comprises one or more of phosphoric acid, water soluble phosphate salts, preferably the water soluble phosphate salts comprise one or more of trisodium phosphate, tripotassium phosphate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate, and ammonium phosphate.
[0027] In any embodiment of the present application, the phosphorus source necessary for producing the iron manganese phosphate precursor further comprises a water-soluble source of doping element Q, where Q represents a doping element of phosphorussite and preferably comprises one or more of B, S, Si and N. Preferably, the source of doping element Q comprises one or more of sulfates, borates, nitrates and silicates of doping element Q.
[0028] In any embodiment of the present application, the oxidizing agent comprises one or more of hydrogen peroxide, nitric acid, sodium hypochlorite, potassium hypochlorite, sodium chlorate, potassium chlorate, and preferably hydrogen peroxide.
[0029] In any embodiment of the present application, the molar ratio of the metal salt to the oxidizing agent is 1:(0.1 to 1.2), and preferably 1:(0.5 to 0.6).
[0030] In any embodiment of the present application, the concentration of the metal salt solution is 0.5 mol / L to 2 mol / L, preferably 0.5 mol / L to 1 mol / L.
[0031] In any embodiment of the present application, the concentration of the phosphorus source solution is 0.5 mol / L to 2 mol / L, preferably 0.5 mol / L to 1 mol / L.
[0032] In any embodiment of the present application, the molar ratio of the metal salt to the phosphorus source is 1:1 to 1:3.
[0033] In any embodiment of the present application, the stirring speed of the first material dissolving pot is 100 r / min to 500 r / min.
[0034] In any embodiment of the present application, the stirring speed of the second material dissolving pot is 100 r / min to 500 r / min.
[0035] In any embodiment of the present application, the stirring speed of the first reaction vessel is 100 r / min to 500 r / min.
[0036] In any embodiment of the present application, the stirring speed of the second reaction vessel is 100 r / min to 500 r / min.
[0037] In any embodiment of the present application, the stirring speed of the aging tank is 100 r / min to 500 r / min.
[0038] In any embodiment of the present application, in step S3, the drying temperature is 200°C to 300°C.
[0039] In any embodiment of the present application, in step S3, the drying time is 3 h to 8 h.
[0040] In any embodiment of the present application, in step S3, the dry atmosphere is a protective gas atmosphere, and the protective gas includes nitrogen gas, an inert gas, or a combination thereof.
[0041] According to a third aspect of the present application, there is provided an iron manganese phosphate precursor produced by the method of the second aspect of the present application, the iron manganese phosphate precursor having the chemical formula Fe x Mn y M 1-x-y P1-m Q m It has O4, where 0 < x < 1, preferably 0.2 ≦ x ≦ 0.5; 0 < y < 1, preferably 0.5 ≦ y ≦ 0.8; 0 ≦ 1 - x - y < 1, preferably 0 < 1 - x - y ≦ 0.05; 0 ≦ m ≦ 0.1, preferably 0 < m ≦ 0.05. M represents the doping elements of manganese sites and iron sites, preferably including one or more of Co, Mg, Zn, Ca, Ti, V, Ni, Cr. Q represents the doping elements of phosphate sites, preferably including one or more of B, S, Si, and N, and the manganese iron phosphate precursor is electrically neutral.
[0042] The manganese iron phosphate precursor provided by the present application has the advantages of small particle size, narrow particle size distribution, high crystallinity, single microcrystal, regular shape, high tap density, and high stability and consistency in batch production.
[0043] In any embodiment of the present application, the manganese iron phosphate precursor has a spherical shape.
[0044] In any embodiment of the present application, the manganese iron phosphate precursor is orthorhombic and the space group is pmnb.
[0045] In any embodiment of the present application, the volume-based particle size distribution Dv90 and Dv50 of the manganese iron phosphate precursor satisfy 1 < Dv90 / Dv50 ≦ 2, preferably 1.1 ≦ Dv90 / Dv50 ≦ 1.7.
[0046] In any embodiment of the present application, the volume-based particle size distribution Dv50 of the manganese iron phosphate precursor is 1 μm to 10 μm, preferably 2.5 μm to 6 μm.
[0047] According to the fourth aspect of the present application, a method for manufacturing lithium iron manganese phosphate is provided. At least, a lithium iron manganese phosphate precursor manufactured by the method of the second aspect of the present application or the lithium iron manganese phosphate precursor of the third aspect of the present application, a lithium source, an optional doping element N source, and an optional doping element R source are uniformly mixed at a preset ratio to obtain a mixed raw material. N represents a doping element for lithium sites, preferably including one or more of Zn, Al, Na, K, Mg, Nb, Mo, and W. R represents a doping element for oxygen sites, preferably including one or more of S, F, Cl, and Br. Step S10, and by sintering the mixed raw material obtained in step S10, lithium iron manganese phosphate is obtained. The lithium iron manganese phosphate has the chemical formula Li a N b Fe x Mn y M 1-x-y P 1-m Q m O 4-n R n wherein M represents a doping element for manganese sites and iron sites, preferably including one or more of Co, Mg, Zn, Ca, Ti, V, Ni, and Cr. N represents a doping element for lithium sites, preferably including one or more of Zn, Al, Na, K, Mg, Nb, Mo, and W. Q represents a doping element for phosphorus sites, preferably including one or more of B, S, Si, and N. R represents a doping element for oxygen sites, preferably including one or more of S, F, Cl, and Br. 0.9 ≦ a ≦ 1.1, 0 ≦ b ≦ 0.1, preferably 0 < b ≦ 0.05, 0 < x < 1, preferably 0.2 ≦ x ≦ 0.5, 0 < y < 1, preferably 0.5 ≦ y ≦ 0.8, 0 ≦ 1 - x - y < 1, preferably 0 < 1 - x - y ≦ 0.05, 0 ≦ m ≦ 0.1, preferably 0 < m ≦ 0.05, 0 ≦ n ≦ 0.1, preferably 0 < n ≦ 0.05, and the lithium iron manganese phosphate is electrically neutral. Step S20, and includes.
[0048] The above manufacturing method of the present application helps to obtain spherical lithium iron manganese phosphate with a uniform distribution of each element.
[0049] In any embodiment of the present application, in step S10, a carbon source is further added to the mixed raw material, thereby producing a carbon-coated lithium manganese iron phosphate, which is conducive to forming a complete, uniform and strong carbon coating layer, and improves the electrical conductivity of the obtained lithium manganese iron phosphate.
[0050] According to a fifth aspect of the present application, there is provided lithium manganese iron phosphate which is produced by the production method according to the fourth aspect of the present application and has excellent electrical and chemical properties.
[0051] According to a sixth aspect of the present application, there is provided a secondary battery including the lithium manganese iron phosphate produced by the production method according to the fourth aspect of the present application. [Brief description of the drawings]
[0052] In order to more clearly describe the technical solutions in the embodiments of the present application, the following briefly describes the drawings necessary for the embodiments of the present application. It should be understood that the drawings shown below are only some embodiments of the present application, and those skilled in the art can further obtain other drawings based on the drawings without creative efforts. In the drawings, the drawings are not drawn according to actual scale.
[0053] [Figure 1] A continuous reaction system for producing iron manganese phosphate precursor. [Diagram 2] 1 is an X-ray diffraction spectrum (XRD) image of the iron manganese phosphate precursor prepared in Example 1. [Diagram 3] 3A and 3B are scanning electron microscope (SEM) images of the iron manganese phosphate precursor produced in Example 1, with FIG. 3(a) at a magnification of 1000 times and FIG. 3(b) at a magnification of 20000 times. [Figure 4] 1 is a scanning electron microscope (SEM) image at 1000x magnification of the iron manganese phosphate precursor produced in Comparative Example 1. [Diagram 5]1 is a scanning electron microscope (SEM) image at 1000x magnification of the iron manganese phosphate precursor produced in Comparative Example 2. [Explanation of symbols]
[0054] 1 First material melting pot 2 Second material melting pot 3. First Reactor 4. Second Reactor 5. Aging kettle 6 1st supply port 7 First overflow port 8. First shutoff valve 9. First metering pump 10. Second shutoff valve 11 second metering pump 12 second supply port 13 Second overflow outlet 14 3rd supply port 15 3rd overflow outlet 16 Third shutoff valve 17 Fourth shutoff valve DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0055] Hereinafter, the continuous reaction system, the iron manganese phosphate precursor, the lithium iron manganese phosphate, and the manufacturing method thereof and the secondary battery of the present application will be described in detail with reference to the drawings as appropriate. However, unnecessary detailed description may be omitted. For example, detailed description of well-known matters and overlapping description of substantially the same structure may be omitted. This is to prevent the following description from becoming unnecessarily redundant and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.
[0056] The "ranges" disclosed herein are defined in the form of lower and upper limits, and a given range is defined by selecting one lower limit and one upper limit, and the selected lower and upper limits define the boundaries of the particular range. Ranges defined in this manner may or may not include the endpoints and may be arbitrarily combined, i.e., any lower limit may be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are recited for a particular parameter, it is understood that ranges of 60-110 and 80-120 are also contemplated. Also, if minimum range values 1 and 2 are recited, and maximum range values 3, 4, and 5 are recited, the ranges 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5 are all contemplated. In this application, unless otherwise stated, the numerical range "a-b" means a shorthand representation of any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are recited herein, and "0-5" is merely a shorthand for combinations of these numerical values. Furthermore, expressing a parameter as an integer ≧2 is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0057] All embodiments and optional embodiments of the present application, unless otherwise specified, can be combined with each other to form new technical solutions, and such technical solutions should be considered as included in the disclosure of the present application.
[0058] All technical features and optional technical features of the present application, unless otherwise specified, can be combined with each other to form new technical solutions, and such technical solutions should be considered as included in the disclosure of the present application.
[0059] All steps in the present application can be performed in sequence or randomly, and are preferably performed in sequence, unless otherwise stated. For example, when the method includes steps S1 and S2, it means that the method may include steps S1 and S2 performed in sequence, or may include steps S2 and S1 performed in sequence. For example, when the method may further include step S3, it means that step S3 may be added to the method in any order, for example, the method may include steps S1, S2, and S3, or may include steps S1, S3, and S2, or may include steps S3, S1, and S2, etc.
[0060] The terms "comprise" and "comprises" referred to in this application refer to both open and closed formats unless otherwise specified. For example, the terms "comprise" and "comprises" can indicate that other elements not listed may also be included or may include, or that only the listed elements may be included or may include.
[0061] In this application, unless otherwise stated, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied by either A being true (or present) and B being false (or absent), or A being false (or absent) and B being true (or present), or both A and B being true (or present).
[0062] Unless otherwise stated, in this application, terms such as "first," "second," and "third" are used to distinguish different objects and are not used to describe a particular order or hierarchical relationship.
[0063] As used herein, the terms "plurality" and "multiple" mean two or more than two.
[0064] A first aspect of an embodiment of the present application provides a continuous reaction system for producing an iron manganese phosphate precursor.
[0065] As shown in FIG. 1, the continuous reaction system includes a first material dissolving pot 1, a second material dissolving pot 2, a first reaction pot 3, a second reaction pot 4, and an aging pot 5. The first reaction pot 3, the second reaction pot 4, and the aging pot 5 are connected in series through a pipeline. The first material dissolving pot 1 is used to receive a metal salt solution required for preparing an iron manganese phosphate precursor, and the second material dissolving pot is used to receive an oxidizing agent and a phosphorus source solution required for preparing an iron manganese phosphate precursor. The first reaction pot 3 has a first supply port 6 and a first overflow port 7. The first supply port 6 of the first reaction pot is connected to the first material dissolving pot 1 and the second material dissolving pot 2 through a first pipeline and a second pipeline, respectively, so that the first reaction pot 3 receives the metal salt solution and the phosphorus source solution, mixes them, and reacts them to produce a first reaction liquid. A first shutoff valve 8 and a first metering pump 9 are installed in the first pipeline to regulate the flow of the metal salt solution. a second shutoff valve 10 and a second metering pump 11 are provided in the second line to adjust the flow rate of the phosphorus source solution; the second reaction kettle 4 has a second supply port 12 and a second overflow port 13, the second supply port 12 of the second reaction kettle is connected to the first overflow port 7 of the first reaction kettle through the third line, so that the second reaction kettle 4 receives the first reaction liquid from the first reaction kettle 3 and continuously reacts it to produce a second reaction liquid; the aging kettle 5 has a third supply port 14 and a third overflow port 15, the third supply port 14 of the aging kettle is connected to the second overflow port 13 of the second reaction kettle through the fourth line, so that the aging kettle 5 receives the second reaction liquid from the second reaction kettle 4 and continuously reacts it to produce a third reaction liquid; when the liquid level of the third reaction liquid is higher than the third overflow port 15 of the aging kettle, the third reaction liquid flows out via the third overflow port 15 of the aging kettle.
[0066] In some embodiments, the first material melting pot 1, the second material melting pot 2, the first reaction pot 3, the second reaction pot 4 and the aging pot 5 are all equipped with stirring devices.
[0067] In some embodiments, the first reaction kettle 3, the second reaction kettle 4 and the aging kettle 5 may further be equipped with a heating device, so as to adjust the reaction temperature of each kettle according to actual needs.
[0068] In some embodiments, a third shutoff valve 16 is further installed in the third line, and a fourth shutoff valve 17 is further installed in the fourth line.
[0069] When producing the manganese ferric phosphate precursor, the first shutoff valve 8, the second shutoff valve 10, the third shutoff valve 16, and the fourth shutoff valve 17 are all kept open, thereby ensuring continuous material supply and continuous discharge, and allowing multiple kettles to react simultaneously.
[0070] A second aspect of the present embodiment provides a method for producing an iron manganese phosphate precursor using the continuous reaction system of the first aspect of the present embodiment. As shown in FIG. 1, the method includes at least: a first reactor 3, a second reactor 4 and an aging reactor 5 are connected in series through pipelines, the first reactor 3 has a first supply port 6 and a first overflow port 7, the first supply port 6 of the first reactor is connected to a first material dissolving reactor 1 through a first pipeline, the first supply port 6 of the first reactor is connected to a second material dissolving reactor 2 through a second pipeline, a first shutoff valve 8 and a first metering pump 9 are installed in the first pipeline, a second shutoff valve 10 and a second metering pump 11 are installed in the second pipeline, the second reactor 4 has a second supply port 12 and a second overflow port 13, the second supply port 12 of the second reactor is connected to the first overflow port 7 of the first reactor through a third pipeline, the aging reactor 5 includes a third supply port 14 and a third overflow port 15, the third supply port 14 of the aging reactor is connected to the second overflow port 13 of the second reactor through a fourth pipeline; A metal salt solution required for producing the manganese iron phosphate precursor is added to a first material dissolving pot 1, an oxidizing agent and a phosphorus source solution required for producing the manganese iron phosphate precursor are added to a second material dissolving pot 2, the metal salt solution in the first material dissolving pot 1 is pumped to a first line through a first shutoff valve 8 and a first metering pump 9, and the phosphorus source solution in the second material dissolving pot 2 is pumped to a second line through a second shutoff valve 10 and a second metering pump 11, so that the metal salt solution and the phosphorus source solution are mixed and reacted in a first reaction pot 3 to produce a first reaction liquid, and when the liquid level of the first reaction liquid is higher than a first overflow port 7 of the first reaction pot, the first reaction liquid is mixed and reacted in a second reaction pot 3 to produce a second reaction liquid. the second reaction liquid is automatically transported to the kettle 4 to continue the reaction and produce a second reaction liquid; when the liquid level of the second reaction liquid is higher than the second overflow port 13 of the second reaction kettle, the second reaction liquid is automatically transported to the aging kettle 5 to continue the reaction and produce a third reaction liquid; when the liquid level of the third reaction liquid is higher than the third overflow port 15 of the aging kettle, the third reaction liquid is automatically discharged through the third overflow port 15 of the aging kettle; during the reaction process, the first material dissolving kettle 1, the second material dissolving kettle 2, the first reaction kettle 3, the second reaction kettle 4 and the aging kettle 5 are all under a protective gas atmosphere, and each kettle is kept in a stirring state in step S2; and step S3 of filtering, washing and drying the third reaction liquid obtained from the third overflow port 15 of the aging kettle to obtain an iron manganese phosphate precursor.
[0071] Most of the conventional reaction systems for producing manganese iron phosphate precursors adopt a single reactor or an intermittent production process in which multiple reactors are connected in parallel, which has the disadvantage of low production efficiency. In addition, when multiple reactors are connected in parallel, it is necessary to switch between different reactors at regular intervals, which makes the production process complicated and increases labor costs.
[0072] The present application employs a continuous reaction system as shown in Fig. 1 to produce manganese phosphate iron precursor, in which the first reaction kettle, the second reaction kettle and the aging kettle are connected in series, thereby ensuring continuous material supply and continuous discharge, and allowing multiple kettle to react simultaneously. Therefore, the method for producing manganese phosphate iron precursor provided by the present application has the advantages of high production efficiency, high energy efficiency, simple process, easy operation, low labor cost, etc., and is particularly suitable for large-scale industrial production.
[0073] The iron manganese phosphate precursor obtained by the conventional intermittent preparation method further has defects such as large particle size, wide particle size distribution, irregular shape and low tap density, which affect the flowability, dispersibility and processability of the product and greatly hinder the practical application of the iron manganese phosphate precursor in lithium iron manganese phosphate.
[0074] The method for preparing the manganese phosphate iron precursor provided by the present application is a continuous preparation method, and in the continuous preparation process, the residence time in the first reaction kettle, the second reaction kettle and the aging kettle during the growth process of the manganese phosphate iron precursor particles is the same. Therefore, compared with the manganese phosphate iron precursor obtained by the conventional intermittent preparation method, the manganese phosphate iron precursor obtained by the continuous preparation method provided by the present application has the advantages of small particle size, narrow particle size distribution, high crystallinity, single crystallites, regular shape, high tap density, and high stability and consistency of batch production.
[0075] The method for preparing the manganese iron phosphate precursor provided by the present application is a hydrothermal method, and the manganese iron phosphate precursor obtained by the method provided by the present application has a regular spherical shape. The spherical shape of the manganese iron phosphate precursor can ensure that lithium ions pass through the pores on the surface of the spherical particles and penetrate into the center of the manganese iron phosphate precursor uniformly and simultaneously from all directions during the subsequent sintering process of lithium manganese iron phosphate, which is helpful in obtaining lithium manganese iron phosphate with a spherical shape and uniform distribution of each element. In addition, compared with the irregular shaped manganese iron phosphate precursor prepared by the prior art, the spherical manganese iron phosphate precursor particles obtained by the continuous preparation method of the present application can form a complete, uniform and strong carbon coating layer during the subsequent sintering process of lithium manganese iron phosphate, which improves the electrical conductivity of the obtained lithium manganese iron phosphate.
[0076] In the preparation method of the iron manganese phosphate precursor provided by the present application, the flow rate of the metal salt solution and the phosphorus source solution, the residence time in each vessel during the growth process of the iron manganese phosphate precursor particles, the reaction temperature of each vessel and other parameters can be precisely adjusted, so that the preparation method provided by the present application has good flexibility in production.
[0077] The residence time in each kettle (first reaction kettle, second reaction kettle and aging kettle) during the growth of the manganese phosphate iron precursor is negatively correlated with the flow rate of the metal salt solution and the phosphorus source solution, and positively correlated with the volume of each kettle. When the flow rate of the metal salt solution and the phosphorus source solution is fast, the residence time of the manganese phosphate iron precursor particles in each kettle is short, and when the flow rate of the metal salt solution and the phosphorus source solution is slow, the residence time of the manganese phosphate iron precursor particles in each kettle is long. When the volume of each kettle is small, the residence time of the manganese phosphate iron precursor particles in each kettle is short, and when the volume of each kettle is large, the residence time of the manganese phosphate iron precursor particles in each kettle is long. Therefore, the particle size of the manganese phosphate iron precursor can be adjusted by adjusting the flow rate of the metal salt solution and the phosphorus source solution, and also the volume of each kettle.
[0078] The reaction temperature also affects the particle size and shape of the obtained manganese ferrous phosphate precursor, so that the reaction temperature of each kettle can be adjusted within different ranges to realize the adjustment of the particle size and shape of the manganese ferrous phosphate precursor.
[0079] Therefore, the method for preparing the lithium manganese iron phosphate precursor provided in the present application can adjust the growth rate of crystal particles and adjust the size and shape of crystal particles, thereby meeting different production requirements and preparing lithium manganese iron phosphate with different particle sizes.
[0080] In some embodiments, a complexing agent is further added to the first material melting pot.
[0081] In the prior art, the manganese phosphate iron precursor is prepared by a general co-precipitation method, but due to the difference in the precipitation speed of different metal ions, uniform co-precipitation cannot be achieved, and at the same time, the molar ratio of each metal element in the obtained manganese phosphate iron precursor particles is significantly different from the molar ratio of each metal element in the raw materials, which affects the performance and consistency of the product.In addition, the manganese phosphate iron precursor particles prepared by the co-precipitation method in the prior art are generally in an irregular sheet or block shape, so that the tap density is low, which affects the fluidity, dispersibility and processability of the product, and greatly hinders the practical application of the manganese phosphate iron precursor in lithium manganese phosphate iron.
[0082] The preparation method of the manganese iron phosphate precursor provided by the present application is a hydrothermal method, and in the preparation method provided by the present application, a complexing agent is further added to the first material melting pot. The complexing agent can achieve the purpose of complexing metal ions and controlling free metal ions, thereby improving the conversion efficiency of metal ions, reducing the difference in reaction rate of different metal ions in the reaction solution, and achieving uniform precipitation and crystallization. Therefore, when a complexing agent is further added to the first material melting pot, the preparation method of the present application can obtain spherical manganese iron phosphate precursor particles with high purity and uniform distribution of metal elements, which have a higher tap density, and at the same time, the difference between the molar ratio of each metal element in the spherical manganese iron phosphate precursor particles obtained by the preparation method of the present application and the molar ratio of each metal element in the raw material is small, so that the metal element content can be accurately controlled.
[0083] Preferably, the complexing agent comprises one or more of an aminocarboxylate, a hydroxycarboxylate and an organic phosphonic acid, more preferably, the complexing agent comprises one or more of sodium nitrilotriacetate, disodium ethylenediaminetetraacetate, sodium gluconate, sodium citrate.
[0084] Preferably, the mass concentration of the complexing agent is 10 wt % or less, more preferably 1 wt % to 10 wt %, based on the total mass of the metal salt solution.
[0085] In some embodiments, a surfactant is further added to the first material melt kettle, which helps to better control the shape of the ferrous manganese phosphate precursor particles.
[0086] Preferably, the surfactant comprises one or more of cetyltrimethylammonium bromide, sodium dodecylsulfonate, polyvinylpyrrolidone.
[0087] Preferably, the mass concentration of the surfactant is 5 wt % or less, preferably 1 wt % to 5 wt %, based on the total mass of the metal salt solution.
[0088] In some embodiments, the reaction temperature of the first reaction kettle is lower than the reaction temperature of the second reaction kettle, and the reaction temperature of the aging kettle is lower than the reaction temperature of the second reaction kettle.
[0089] In the method for preparing the manganese iron phosphate precursor provided by the present application, the first reaction kettle, the second reaction kettle and the aging kettle are connected in series, and the reaction temperatures of the first reaction kettle and the aging kettle are set lower than the reaction temperature of the second reaction kettle, so that each kettle in the continuous reaction system can be given a different main function. Since the reaction temperature of the first reaction kettle is low, the first reaction kettle can realize the pre-mixing of the metal salt solution and the phosphorus source solution and the rapid pre-nucleation, during which the metal ions and phosphate ions (PO4 3- ) tends to form a large amount of crystal nuclei, which is favorable for better crystallization and particle size distribution control in the subsequent second reactor. The second reactor has a high reaction temperature, so that after the reaction liquid flows from the first reactor to the second reactor, the high reaction temperature can provide sufficient energy to promote the growth and crystallization of the crystal nuclei, and can improve the crystallinity of the crystal nuclei under the premise of avoiding the condensation growth of the crystal nuclei. The reaction temperature of the aging vessel is lower than that of the second reactor, so that when the reaction liquid flows from the second reactor to the aging vessel, it can play the role of cooling the reaction liquid, and the raw materials not involved in the reaction in the reaction liquid can continue to crystallize on the surface of the already formed crystal particles, realizing the continuous growth of the crystal particles, increasing the size of the crystal particles, and narrowing the particle size distribution of the crystal particles.
[0090] Therefore, the particle size of the obtained manganese phosphate iron precursor can be adjusted by adjusting the reaction temperature of each kettle, which helps to obtain manganese phosphate iron precursor particles with narrow particle size distribution, high crystallinity, single crystallites, regular shape, and high tap density.
[0091] In some embodiments, the reaction temperature of the first reactor is preferably 70°C to 90°C.
[0092] In some embodiments, the reaction temperature of the second reactor is preferably 150°C to 250°C.
[0093] In some embodiments, the reaction temperature in the aging vessel is preferably 20°C to 30°C.
[0094] In some embodiments, the flow rate of the metal salt solution in the first line (or the pumping speed of the first metering pump) is between 0.2 L / min and 2 L / min, preferably between 0.25 L / min and 1 L / min.
[0095] In some embodiments, the flow rate of the phosphorus source solution in the second line (or the pumping speed of the second metering pump) is 0.2 L / min to 2 L / min, preferably 0.25 L / min to 1 L / min.
[0096] In some embodiments, the flow rates of the metal salt solution and the phosphorus source solution are the same (i.e., the pumping speeds of the first and second metering pumps are the same), which helps improve the consistency of the resulting ferromanganese phosphate precursor particles.
[0097] In some embodiments, the residence time in the first reactor during the growth of the iron manganese phosphate precursor is 1 h to 4 h.
[0098] In some embodiments, the residence time of the iron manganese phosphate precursor in the second reactor during the growth process is 1 h to 16 h, preferably 4 h to 16 h.
[0099] In some embodiments, the residence time of the iron manganese phosphate precursor in the aging vessel during the growth process is 1 h to 48 h, preferably 12 h to 48 h.
[0100] In some embodiments, the volume of the first reactor is equal to or less than the volume of the second reactor, so that the residence time of the iron manganese phosphate precursor in the second reactor during the growth process is long, which helps the particles of the iron manganese phosphate precursor to have a higher crystallinity. Preferably, the ratio of the volume of the first reactor to the volume of the second reactor is 1:(1-4), more preferably 1:(2-4).
[0101] In some embodiments, the volume of the first reaction kettle is equal to or less than the volume of the aging kettle, which allows the iron manganese phosphate precursor to have a longer residence time in the aging kettle during the growth process, and helps the iron manganese phosphate precursor to have a larger particle size. Preferably, the ratio of the volume of the first reaction kettle to the volume of the aging kettle is 1:(1-12), more preferably 1:(4-12).
[0102] In some embodiments, the volume of the second reaction kettle is equal to or less than the volume of the aging kettle, which allows the iron manganese phosphate precursor to have a longer residence time in the aging kettle during the growth process, and helps the iron manganese phosphate precursor to have a larger particle size. Preferably, the ratio of the volume of the second reaction kettle to the volume of the aging kettle is 1:(1-3), more preferably 1:(2-3).
[0103] In some embodiments, in step S3, the drying temperature is preferably 200°C to 300°C.
[0104] In some embodiments, in step S3, the drying time is preferably 3 h to 8 h.
[0105] In some embodiments, in step S3, the drying may be performed in a desiccator, and the drying atmosphere may be a protective gas atmosphere, where the protective gas includes nitrogen gas, an inert gas, or a combination thereof. Preferably, the inert gas includes helium gas, argon gas, or a combination thereof.
[0106] In some embodiments, the metal salts necessary to prepare the iron manganese phosphate precursor include a water-soluble iron salt, a water-soluble manganese salt and preferably a salt of a water-soluble doping element M, where M represents a doping element for the manganese and iron sites, preferably including one or more of Co, Mg, Zn, Ca, Ti, V, Ni, Cr.
[0107] The water-soluble iron salt may be a compound containing various iron ions (e.g., ferrous ion, ferric ion) that are soluble in conventional water, and preferably the water-soluble iron salt comprises one or more of ferrous chloride, ferrous nitrate, ferrous sulfate, ferrous acetate, ferric chloride, ferric nitrate, ferric sulfate, and ferric acetate.
[0108] The water-soluble manganese salt may be any conventional water-soluble compound containing manganese ions (e.g., divalent manganese ions), and preferably the water-soluble manganese salt comprises one or more of manganous chloride, manganous nitrate, manganous sulfate, and manganous acetate.
[0109] The water-soluble salt of doping element M may be any conventional water-soluble compound containing M ions, and preferably the water-soluble salt of doping element M comprises one or more of hydrochloride, nitrate, sulfate, acetate of doping element M.
[0110] In some embodiments, the phosphorus source required to produce the iron manganese phosphate precursor comprises one or more of phosphoric acid, water-soluble phosphate salts, preferably one or more of trisodium phosphate, tripotassium phosphate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate, and ammonium phosphate.
[0111] In some embodiments, the phosphorus source necessary for producing the iron manganese phosphate precursor may further comprise a water-soluble source of doping element Q, where Q represents a doping element of phosphorussite and preferably comprises one or more of B, S, Si and N. In some embodiments, preferably, the source of doping element Q comprises one or more of sulfates, borates, nitrates and silicates of doping element Q.
[0112] In some embodiments, the metal salt solution is an aqueous metal salt solution, for example obtained by homogeneously mixing the metal salts required to prepare the iron manganese phosphate precursor with deionized water.
[0113] In some embodiments, the phosphorus source solution is an aqueous phosphorus source solution, for example, obtained by uniformly mixing an oxidizing agent, a phosphorus source, and deionized water.
[0114] In some embodiments, the oxidizing agent comprises one or more of hydrogen peroxide, nitric acid, sodium hypochlorite, potassium hypochlorite, sodium chlorate, potassium chlorate, preferably hydrogen peroxide.
[0115] In some embodiments, the concentration of the metal salt solution is 0.5 mol / L to 2 mol / L, preferably 0.5 mol / L to 1 mol / L.
[0116] In some embodiments, the concentration of the phosphorus source solution is 0.5 mol / L to 2 mol / L, preferably 0.5 mol / L to 1 mol / L.
[0117] The amount of the phosphorus source added may be in excess relative to the metal salt. In some embodiments, the molar ratio of the metal salt to the phosphorus source is 1:1 to 1:3.
[0118] The amount of the oxidizing agent added may be in excess of the amount of the metal salt. In some embodiments, the molar ratio of the metal salt to the oxidizing agent is 1:(0.1 to 1.2), preferably 1:(0.5 to 0.6).
[0119] During the reaction process, the first material dissolution tank, the second material dissolution tank, the first reaction tank, the second reaction tank, and the aging tank all maintain a stirring state. In some embodiments, the stirring speed of the first material dissolution tank is 100 r / min to 500 r / min. In some embodiments, the stirring speed of the second material dissolution tank is 100 r / min to 500 r / min. In some embodiments, the stirring speed of the first reaction tank is 100 r / min to 500 r / min. In some embodiments, the stirring speed of the second reaction tank is 100 r / min to 500 r / min. In some embodiments, the stirring speed of the aging tank is 100 r / min to 500 r / min.
[0120] During the reaction process, protective gas is introduced into the first material dissolution tank, the second material dissolution tank, the first reaction tank, the second reaction tank, and the aging tank. In some embodiments, the protective gas includes nitrogen gas, inert gas, or a combination thereof. Preferably, the inert gas includes helium gas, argon gas, or a combination thereof.
[0121] In the method for producing the manganese iron phosphate precursor provided by the present application, unless otherwise specified, each raw material may be directly purchased.
[0122] According to the third aspect of the embodiment of the present application, a manganese iron phosphate precursor produced by the production method of the second aspect of the embodiment of the present application is provided, and the manganese iron phosphate precursor has the chemical formula Fe x Mn y M 1-x-y P 1-m Q m O4, where 0 < x < 1, 0 < y < 1, 0 ≤ 1 - x - y < 1, 0 ≤ m ≤ 0.1, M represents a doping element for the manganese site and the iron site, preferably including one or more of Co, Mg, Zn, Ca, Ti, V, Ni, Cr, Q represents a doping element for the phosphorus site, preferably including one or more of B, S, Si, and N, and the manganese iron phosphate precursor is electrically neutral.
[0123] The iron manganese phosphate precursor provided by the present application is produced by the method of the second aspect of the embodiment of the present application. Therefore, it has the advantages of small particle size, narrow particle size distribution, high crystallinity, single microcrystal, regular shape, high tap density, and high stability and consistency in batch production.
[0124] In some embodiments, the iron manganese phosphate precursor has a spherical shape.
[0125] In some embodiments, the iron manganese phosphate precursor is orthorhombic and the space group is pmnb.
[0126] In some embodiments, the volume-based particle size distributions Dv90 and Dv50 of the iron manganese phosphate precursor satisfy 1 < Dv90 / Dv50 ≤ 2, and preferably, 1.1 ≤ Dv90 / Dv50 ≤ 1.7.
[0127] In some embodiments, the volume-based particle size distribution Dv50 of the iron manganese phosphate precursor is 1 μm to 10 μm, and preferably, 2.5 μm to 6 μm.
[0128] In some embodiments, 0.2 ≤ x ≤ 0.5.
[0129] In some embodiments, 0.5 ≤ y ≤ 0.8.
[0130] In some embodiments, 1 - x - y = 0, and in another embodiment, 0 < 1 - x - y ≤ 0.05.
[0131] In some embodiments, m = 0, and in another embodiment, 0 < m ≤ 0.05.
[0132] According to a fourth aspect of the embodiment of the present application, a method for manufacturing lithium iron manganese phosphate is provided. At least, a lithium iron manganese phosphate precursor manufactured by the method of the second aspect of the embodiment of the present application or a lithium iron manganese phosphate precursor of the third aspect of the embodiment of the present application, a lithium source, an optional doping element N source, and an optional doping element R source are uniformly mixed at a preset ratio to obtain a mixed raw material. N represents a doping element for lithium sites, preferably including one or more of Zn, Al, Na, K, Mg, Nb, Mo, and W. R represents a doping element for oxygen sites, preferably including one or more of S, F, Cl, and Br. Step S10; by sintering the mixed raw material obtained in step S10, lithium iron manganese phosphate is obtained. The lithium iron manganese phosphate has the chemical formula Li a N b Fe x Mn y M 1-x-y P 1-m Q m O 4-n R n wherein M represents a doping element for manganese sites and iron sites, preferably including one or more of Co, Mg, Zn, Ca, Ti, V, Ni, and Cr. N represents a doping element for lithium sites, preferably including one or more of Zn, Al, Na, K, Mg, Nb, Mo, and W. Q represents a doping element for phosphorus sites, preferably including one or more of B, S, Si, and N. R represents a doping element for oxygen sites, preferably including one or more of S, F, Cl, and Br. 0.9 ≦ a ≦ 1.1, 0 ≦ b ≦ 0.1, preferably 0 < b ≦ 0.05, 0 < x < 1, preferably 0.2 ≦ x ≦ 0.5, 0 < y < 1, preferably 0.5 ≦ y ≦ 0.8, 0 ≦ 1 - x - y < 1, preferably 0 < 1 - x - y ≦ 0.05, 0 ≦ m ≦ 0.1, preferably 0 < m ≦ 0.05, 0 ≦ n ≦ 0.1, preferably 0 < n ≦ 0.05, and the lithium iron manganese phosphate is electrically neutral. Step S20; and includes.
[0133] When the lithium manganese iron phosphate is prepared using the above-mentioned manganese iron phosphate precursor of the present application, during the sintering process, lithium ions can pass through the pores on the surface of the spherical manganese iron phosphate precursor particles and uniformly and simultaneously penetrate into the center of the manganese iron phosphate precursor from all directions, which helps to obtain lithium manganese iron phosphate with a spherical shape and uniform distribution of each element. Therefore, the lithium manganese iron phosphate obtained by the preparation method of the present application has excellent electrical and chemical properties.
[0134] In some embodiments, the lithium source can be any lithium-containing compound known in the art for use in producing lithium manganese iron phosphate active cathode materials, for example, the lithium source can include one or more of Li2CO3, LiOH, Li3PO4, and LiH2PO4.
[0135] In some embodiments, the source of doping element N comprises one or more of hydrochlorides, nitrates, sulfates and acetates of doping element N.
[0136] In some embodiments, the source of doping element R comprises one or more of an elemental form and an ammonium salt of the doping element R.
[0137] By selecting the source of each doping element, the distribution uniformity of each doping element can be improved, and the electrical and chemical properties of the lithium manganese iron phosphate can be improved.
[0138] In some embodiments, in step S10, a carbon source may be further added to the mixed raw material, thereby producing a carbon-coated lithium manganese iron phosphate. When the lithium manganese iron phosphate is produced using the above-mentioned manganese iron phosphate precursor of the present application, a complete, uniform and strong carbon coating layer can be formed on the surface of the lithium manganese iron phosphate, which improves the electrical conductivity of the obtained lithium manganese iron phosphate.
[0139] In some embodiments, the carbon source comprises one or more of an organic carbon source, an inorganic carbon source, preferably a combination of one or more of glucose, sucrose, starch, fructose, polyvinyl alcohol, polyethylene glycol, and citric acid.
[0140] In the above preparation method, the amount of each of the doping elements N and R sources added depends on the target doping amount, and the amount of the lithium source added is in accordance with the stoichiometric ratio of the lithium manganese iron phosphate. In some embodiments, the amount of the lithium source added may be slightly excess, for example, 100% to 110% of the theoretical mass of the lithium source, where the theoretical mass of the lithium source is the mass of the lithium source calculated based on the stoichiometric ratio of the lithium manganese iron phosphate.
[0141] In the above-mentioned production method, unless otherwise specified, each raw material may be directly purchased.
[0142] According to a fifth aspect of the present embodiment, there is provided lithium manganese iron phosphate produced by the production method according to the fourth aspect of the present embodiment.
[0143] The lithium manganese iron phosphate has the chemical formula Li a N b Fe x Mn y M 1-x-y P 1-m Q m O 4-n R nIt has, where M represents the doping elements of manganese sites and iron sites, preferably including one or more of Co, Mg, Zn, Ca, Ti, V, Ni, Cr; N represents the doping elements of lithium sites, preferably including one or more of Zn, Al, Na, K, Mg, Nb, Mo, and W; Q represents the doping elements of phosphorus sites, preferably including one or more of B, S, Si, and N; R represents the doping elements of oxygen sites, preferably including one or more of S, F, Cl, and Br; 0.9 ≦ a ≦ 1.1, 0 ≦ b ≦ 0.1, preferably 0 < b ≦ 0.05, 0 < x < 1, preferably 0.2 ≦ x ≦ 0.5, 0 < y < 1, preferably 0.5 ≦ y ≦ 0.8, 0 ≦ 1 - x - y < 1, preferably 0 < 1 - x - y ≦ 0.05, 0 ≦ m ≦ 0.1, preferably 0 < m ≦ 0.05, 0 ≦ n ≦ 0.1, preferably 0 < n ≦ 0.05, and the lithium iron manganese phosphate is electrically neutral.
[0144] In some embodiments, the surface of the lithium iron manganese phosphate is coated with carbon, thereby improving the conductivity of the lithium iron manganese phosphate.
[0145] According to the sixth aspect of the embodiments of the present application, a secondary battery including lithium iron manganese phosphate manufactured by the manufacturing method of the fourth aspect of the embodiments of the present application is provided. The lithium iron manganese phosphate can be applied as a positive electrode active material in a secondary battery and is helpful for improving the electrical and chemical properties of the secondary battery.
[0146] Example The following examples more specifically describe the contents disclosed in the present application, but since various modifications and changes made within the scope of the contents disclosed in the present application are obvious to those skilled in the art, these examples are merely illustrative.Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are based on mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without treatment, and all equipment used in the examples are commercially available.
[0147] Example 1 The continuous reaction system shown in Figure 1 is employed to produce the iron manganese phosphate precursor.
[0148] Add water-soluble manganese chloride, water-soluble ferrous chloride, and deionized water to a first material dissolution kettle to prepare a metal salt solution with a concentration of 1 mol / L. In the prepared metal salt solution, the molar ratio of manganese ions to ferrous ions is 5:5. Add hydrogen peroxide as an oxidizer, phosphoric acid as a phosphorus source, and deionized water to a second material dissolution kettle to prepare a phosphorus source solution with a concentration of 1 mol / L, and control the molar ratio of hydrogen peroxide to metal salt to (0.5-0.6):1.
[0149] As shown in Figure 1, nitrogen gas is introduced into the first material melting pot, the second material melting pot, the first reaction pot, the second reaction pot and the aging pot, and the stirring speed of each pot during the reaction is 200r / min. The reaction temperature of the first reaction pot is controlled at 90℃, the reaction temperature of the second reaction pot is controlled at 160℃, and the reaction temperature of the aging pot is controlled at 25℃.
[0150] The metal salt solution and the phosphorus source solution are continuously pumped from the first material dissolving kettle and the second material dissolving kettle to the first reaction kettle through the shutoff valve and the metering pump, respectively, and mixed and reacted to produce the first reaction liquid, and the flow rates of the metal salt solution and the phosphorus source solution are both 0.5L / min.
[0151] After 2 hours of reaction, when the liquid level of the first reaction liquid becomes higher than the first overflow port, the first reaction liquid automatically flows out from the first overflow port into the second reaction vessel to continue the reaction and produce the second reaction liquid.
[0152] After the reaction continues for 8 hours, when the liquid level of the second reaction liquid becomes higher than the second overflow port, the second reaction liquid automatically flows out from the second overflow port into the aging kettle to continue the reaction and produce a third reaction liquid.
[0153] After the reaction has continued for 24 hours, when the liquid level of the third reaction liquid becomes higher than the third overflow port, the third reaction liquid automatically flows out from the third overflow port.
[0154] The obtained third reaction liquid is filtered and washed using a filter press, then transferred to a dryer and dried at 200°C for 6 hours under a nitrogen gas atmosphere to remove water of crystallization, finally obtaining a manganese iron phosphate precursor.
[0155] Example 2 The continuous reaction system shown in Figure 1 is employed to produce the iron manganese phosphate precursor.
[0156] A water-soluble manganese salt, manganous nitrate, a water-soluble iron salt, ferrous nitrate, a complexing agent, sodium nitrilotriacetate, and deionized water are added to a first material dissolution kettle to prepare a metal salt solution with a concentration of 0.5 mol / L. In the prepared metal salt solution, the molar ratio of manganese ions to iron ions is 6:4, and the mass concentration of the complexing agent is 1 wt%. An oxidizing agent, hydrogen peroxide, a phosphorus source, and deionized water are added to a second material dissolution kettle to prepare a phosphorus source solution with a concentration of 0.5 mol / L, and the molar ratio of hydrogen peroxide to metal salt is controlled to (0.5-0.6):1.
[0157] As shown in Figure 1, nitrogen gas is introduced into the first material melting pot, the second material melting pot, the first reaction pot, the second reaction pot and the aging pot, and the stirring speed of each pot during the reaction is 250r / min. The reaction temperature of the first reaction pot is controlled at 80℃, the reaction temperature of the second reaction pot is controlled at 180℃, and the reaction temperature of the aging pot is controlled at 25℃.
[0158] The metal salt solution and the phosphorus source solution are continuously transported from the first material dissolving kettle and the second material dissolving kettle to the first reaction kettle through the shutoff valve and the metering pump, respectively, and mixed and reacted to produce the first reaction liquid, and the flow rates of the metal salt solution and the phosphorus source solution are both 0.25 L / min.
[0159] After 4 hours of reaction, when the liquid level of the first reaction liquid becomes higher than the first overflow port, the first reaction liquid automatically flows out from the first overflow port into the second reaction vessel to continue the reaction and produce the second reaction liquid.
[0160] After the reaction continues for 16 hours, when the liquid level of the second reaction liquid becomes higher than the second overflow port, the second reaction liquid automatically flows out from the second overflow port into the aging kettle to continue the reaction and produce a third reaction liquid.
[0161] After the reaction has continued for 48 hours, when the liquid level of the third reaction liquid becomes higher than the third overflow port, the third reaction liquid automatically flows out from the third overflow port.
[0162] The obtained third reaction liquid is filtered and washed using a filter press, then transferred to a dryer and dried at 200°C for 6 hours under a nitrogen gas atmosphere to remove water of crystallization, finally obtaining a manganese iron phosphate precursor.
[0163] Example 3 The continuous reaction system shown in Figure 1 is employed to produce the iron manganese phosphate precursor.
[0164] A water-soluble manganese salt, manganous nitrate, a water-soluble iron salt, ferrous sulfate, a water-soluble iron chromium salt, chromium sulfate, a complexing agent, disodium ethylenediaminetetraacetate, and deionized water are added to a first material dissolution kettle to prepare a metal salt solution with a concentration of 1 mol / L. In the prepared metal salt solution, the molar ratio of the manganese ions, the iron ions, and the chromium ions is 6.9:3:0.1, and the mass concentration of the complexing agent is 5 wt%. An oxidizing agent, hydrogen peroxide, a phosphorus source, trisodium phosphate, and deionized water are added to a second material dissolution kettle to prepare a phosphorus source solution with a concentration of 1 mol / L, and the molar ratio of the hydrogen peroxide to the metal salt is controlled to (0.5-0.6):1.
[0165] As shown in Figure 1, nitrogen gas is introduced into the first material dissolving kettle, the second material dissolving kettle, the first reaction kettle, the second reaction kettle and the aging kettle, and the stirring speed of each kettle during the reaction is 150r / min. The reaction temperature of the first reaction kettle is controlled at 90℃, the reaction temperature of the second reaction kettle is controlled at 160℃, and the reaction temperature of the aging kettle is controlled at 25℃.
[0166] The metal salt solution and the phosphorus source solution are continuously transported from the first material dissolving kettle and the second material dissolving kettle to the first reaction kettle through the shutoff valve and the metering pump, respectively, and mixed and reacted to produce the first reaction liquid, and the flow rates of the metal salt solution and the phosphorus source solution are both 1L / min.
[0167] After reacting for 1 hour, when the liquid level of the first reaction liquid becomes higher than the first overflow port, the first reaction liquid automatically flows out from the first overflow port into the second reaction vessel to continue the reaction and produce the second reaction liquid.
[0168] After the reaction continues for 4 hours, when the liquid level of the second reaction liquid becomes higher than the second overflow port, the second reaction liquid automatically flows out from the second overflow port into the aging kettle to continue the reaction and produce a third reaction liquid.
[0169] After the reaction has continued for 12 hours, when the liquid level of the third reaction liquid becomes higher than the third overflow port, the third reaction liquid automatically flows out from the third overflow port.
[0170] The obtained third reaction liquid is filtered and washed using a filter press, then transferred to a dryer and dried at 200°C for 6 hours under a nitrogen gas atmosphere to remove water of crystallization, finally obtaining a manganese iron phosphate precursor.
[0171] Comparative Example 1 A water-soluble manganese salt, manganese nitrate, a water-soluble iron salt, ferrous nitrate, and deionized water are added to a first material dissolution kettle to prepare a metal salt solution with a concentration of 0.5 mol / L. In the prepared metal salt solution, the molar ratio of manganese ions to iron ions is 6:4. An oxidizing agent, hydrogen peroxide, a phosphorus source, and deionized water are added to a second material dissolution kettle to prepare a phosphorus source solution with a concentration of 0.5 mol / L, and the molar ratio of hydrogen peroxide to metal salt is controlled to (0.5-0.6):1.
[0172] The metal salt solution and the phosphorus source solution are pumped into the reactor simultaneously, the pumping speed of the metering pump is 0.25L / min, nitrogen gas is introduced into the reactor, and the stirring is started quickly, the stirring speed is 250r / min, the temperature of the reactor is controlled at 180℃, the reaction time is 20h, and after the reaction is completed, the mixture is cooled naturally from 180℃ to room temperature to obtain a paste. The obtained paste is discharged from the outlet of the reactor, filtered and washed by a filter press, and then transferred to a dryer and dried at 200℃ for 6h under nitrogen gas atmosphere to remove water of crystallization, and finally obtain manganese iron phosphate precursor.
[0173] Comparative Example 2 A water-soluble manganese salt, manganous nitrate, a water-soluble iron salt, ferrous nitrate, a complexing agent, sodium nitrilotriacetate, and deionized water are added to a first material dissolution kettle to prepare a metal salt solution with a concentration of 0.5 mol / L. In the prepared metal salt solution, the molar ratio of manganese ions to iron ions is 6:4, and the mass concentration of the complexing agent is 1 wt%. An oxidizing agent, hydrogen peroxide, a phosphorus source, and deionized water are added to a second material dissolution kettle to prepare a phosphorus source solution with a concentration of 0.5 mol / L, and the molar ratio of hydrogen peroxide to metal salt is controlled to (0.5-0.6):1.
[0174] The metal salt solution and the phosphorus source solution are pumped into the reactor simultaneously, the pumping speed of the metering pump is 0.25L / min, nitrogen gas is introduced into the reactor, and the stirring is started quickly, the stirring speed is 250r / min, the temperature of the reactor is controlled at 180℃, the reaction time is 20h, and after the reaction is completed, the mixture is cooled naturally from 180℃ to room temperature to obtain a paste. The obtained paste is discharged from the outlet of the reactor, filtered and washed by a filter press, and then transferred to a dryer and dried at 200℃ for 6h under nitrogen gas atmosphere to remove water of crystallization, and finally obtain manganese iron phosphate precursor.
[0175] Examination section (1) Particle size measurement The volumetric particle size distribution of the prepared manganese iron phosphate precursor was measured using a Malvern Master Size 3000 laser particle size analyzer. Dv50 and Dv90 are the corresponding particle sizes when the cumulative volume distribution percentage of the material reaches 50% and 90%. GB / T 19077-2016 was used as the basis for the measurement.
[0176] (2) Mn / Fe molar ratio measurement The manganese and iron contents in the manganese iron phosphate precursor prepared above were measured by ICP-OES using a Plasma 3000 inductively coupled plasma optical emission spectrometer, and the molar ratios thereof were calculated.
[0177] [Table 1]
[0178] FIG. 2 is an X-ray diffraction spectrum (XRD) image of the manganese iron phosphate precursor produced in Example 1. FIG. 3 is a scanning electron microscope (SEM) image of the manganese iron phosphate precursor produced in Example 1, where FIG. 3(a) is at a magnification of 1000 times and FIG. 3(b) is at a magnification of 20000 times. FIG. 4 is a scanning electron microscope (SEM) image of the manganese iron phosphate precursor produced in Comparative Example 1 at a magnification of 1000 times. FIG. 5 is a scanning electron microscope (SEM) image of the manganese iron phosphate precursor produced in Comparative Example 2 at a magnification of 1000 times.
[0179] As can be seen from the measurement results in Table 1 and FIGS. 2 and 3 , the iron manganese phosphate precursor produced by the continuous production method provided by the present application has advantages of small particle size, narrow particle size distribution, high crystallinity, single crystallites, and regular shape.
[0180] As can be seen from the measurement results in Table 1 and FIGS. 4 and 5 collectively, the iron manganese phosphate precursor produced by the conventional intermittent production method has a large particle size, a wide particle size distribution, and low shape regularity.
[0181] As can be seen from the measurement results of Example 2, Comparative Example 1 and Comparative Example 2, the difference between the Mn / Fe molar ratio in the iron manganese phosphate precursor particles prepared by the continuous preparation method provided in the present application and the Mn / Fe molar ratio in the metal salt solution is smaller, so that the contents of manganese and iron can be precisely controlled.
[0182] As can be further seen from the measurement results of Example 2, Comparative Example 1 and Comparative Example 2, the complexing agent can help to more accurately control the contents of manganese and iron elements in the prepared manganese iron phosphate precursor particles.
[0183] The present application is not limited to the above-mentioned embodiment. The above-mentioned embodiment is merely an example, and any embodiment that has substantially the same configuration as the technical idea and exhibits the same effect within the scope of the technical solution of the present application is included in the technical scope of the present application. In addition, various modifications that a person skilled in the art can conceive of are added to the embodiment, and other forms constructed by combining some of the components in the embodiment are also included in the scope of the present application, as long as they do not deviate from the gist of the present application.
Claims
1. 1. A continuous reaction system for producing an iron manganese phosphate precursor, comprising: The apparatus includes a first material melting pot, a second material melting pot, a first reaction pot, a second reaction pot, and an aging pot, the first reaction pot, the second reaction pot, and the aging pot being connected in series in order via a pipeline; The first material melting pot is used to accommodate a metal salt solution required for preparing the manganese iron phosphate precursor, and the second material melting pot is used to accommodate an oxidizing agent and a phosphorus source solution required for preparing the manganese iron phosphate precursor; The first reaction kettle has a first supply port and a first overflow port, and the first supply port of the first reaction kettle is connected to the first material dissolving kettle and the second material dissolving kettle through a first pipeline and a second pipeline, respectively, so that the first reaction kettle receives the metal salt solution and the phosphorus source solution, mixes them, and reacts them to produce a first reaction liquid, and a first shutoff valve and a first metering pump are installed in the first pipeline to adjust the flow rate of the metal salt solution, and a second shutoff valve and a second metering pump are installed in the second pipeline to adjust the flow rate of the phosphorus source solution, the second reaction kettle has a second inlet and a second overflow port, the second inlet of the second reaction kettle communicates with the first overflow port of the first reaction kettle through a third pipe, so that the second reaction kettle receives the first reaction liquid from the first reaction kettle and continuously reacts it to produce a second reaction liquid; the aging kettle includes a third supply port and a third overflow port, the third supply port of the aging kettle communicates with the second overflow port of the second reaction kettle through a fourth pipe line, so that the aging kettle receives the second reaction liquid from the second reaction kettle and continuously reacts it to produce a third reaction liquid; When the liquid level of the third reaction liquid is higher than the third overflow port of the aging kettle, the third reaction liquid flows out through the third overflow port of the aging kettle.
2. at least, a step S1 in which the first reaction kettle, the second reaction kettle and the aging kettle are connected in series in order via pipelines, the first reaction kettle has a first supply port and a first overflow port, the first supply port of the first reaction kettle is connected to a first material dissolving kettle via a first pipeline, the first supply port of the first reaction kettle is connected to a second material dissolving kettle via a second pipeline, a first shutoff valve and a first metering pump are installed in the first pipeline, a second shutoff valve and a second metering pump are installed in the second pipeline, the second reaction kettle has a second supply port and a second overflow port, the second supply port of the second reaction kettle is connected to the first overflow port of the first reaction kettle via a third pipeline, the aging kettle includes a third supply port and a third overflow port, and the third supply port of the aging kettle is connected to the second overflow port of the second reaction kettle via a fourth pipeline; A metal salt solution required for producing the manganese iron phosphate precursor is added to a first material dissolving kettle, an oxidizing agent and a phosphorus source solution required for producing the manganese iron phosphate precursor are added to a second material dissolving kettle, the metal salt solution in the first material dissolving kettle is pumped to a first line through a first shutoff valve and a first metering pump, and the phosphorus source solution in the second material dissolving kettle is pumped to a second line through a second shutoff valve and a second metering pump, so that the metal salt solution and the phosphorus source solution are mixed and reacted in the first reaction kettle to produce a first reaction liquid, and when the liquid level of the first reaction liquid is higher than the first overflow port of the first reaction kettle, the first reaction liquid is automatically transported to the second reaction kettle to continue the reaction. Step S2: producing a second reaction liquid, when the level of the second reaction liquid is higher than the second overflow port of the second reaction kettle, the second reaction liquid is automatically transported to the aging kettle to continue the reaction and produce a third reaction liquid, when the level of the third reaction liquid is higher than the third overflow port of the aging kettle, the third reaction liquid is automatically discharged through the third overflow port of the aging kettle, during the reaction process, the first material dissolving kettle, the second material dissolving kettle, the first reaction kettle, the second reaction kettle and the aging kettle are all under a protective gas atmosphere and each kettle is kept in a stirring state, preferably the protective gas includes nitrogen gas, inert gas or a combination thereof; and step S3 of filtering, washing, and drying the third reaction liquid obtained from a third overflow port of the aging kettle to obtain an iron manganese phosphate precursor.
3. 3. The method according to claim 2, further comprising adding a complexing agent to the first material dissolving kettle, and preferably the complexing agent comprises one or more of an amino carboxylate, a hydroxy carboxylate and an organic phosphonate, more preferably one or more of sodium nitrilotriacetate, disodium ethylenediaminetetraacetate, sodium gluconate and sodium citrate.
4. 4. The method according to claim 2 or 3, further comprising adding a surfactant to the first material dissolving kettle, and preferably the surfactant comprises one or more of cetyltrimethylammonium bromide, sodium dodecylsulfonate, and polyvinylpyrrolidone.
5. The reaction temperature of the first reactor is lower than that of the second reactor, and the reaction temperature of the aging reactor is lower than that of the second reactor; Preferably, the reaction temperature of the first reactor is 70° C. to 90° C.; Preferably, the reaction temperature of the second reactor is 150° C. to 250° C.; The method according to any one of claims 2 to 4, wherein the reaction temperature in the aging tank is preferably 20°C to 30°C.
6. the flow rate of the metal salt solution in the first line is between 0.2 L / min and 2 L / min, preferably between 0.25 L / min and 1 L / min; and / or The flow rate of the phosphorus source solution in the second line is 0.2 L / min to 2 L / min, preferably 0.25 L / min to 1 L / min; and / or The method according to any one of claims 2 to 5, wherein the flow rates of the metal salt solution and the phosphorus source solution are the same.
7. The residence time of the iron manganese phosphate precursor in the first reactor during the growth process is 1 h to 4 h; and / or The residence time of the iron manganese phosphate precursor in the second reactor during the growth process is 1 h to 16 h, preferably 4 h to 16 h, and / or The method according to any one of claims 2 to 6, wherein the residence time of the iron manganese phosphate precursor in the aging vessel during the growth process is 1 to 48 hours, preferably 12 to 48 hours.
8. The volume of the first reactor is equal to or less than the volume of the second reactor, and preferably the ratio of the volume of the first reactor to the volume of the second reactor is 1:(1-4), more preferably 1:(2-4); and / or The volume of the first reaction vessel is equal to or smaller than the volume of the aging vessel, and preferably, the ratio of the volume of the first reaction vessel to the volume of the aging vessel is 1:(1-12), more preferably 1:(4-12); and / or The process according to any one of claims 2 to 7, wherein the volume of the second reaction kettle is equal to or less than the volume of the aging kettle, and preferably, the ratio of the volume of the second reaction kettle to the volume of the aging kettle is 1:(1-3), more preferably 1:(2-3).
9. The metal salts necessary for producing said iron manganese phosphate precursor include water-soluble iron salts, water-soluble manganese salts and preferably salts of water-soluble doping elements M, where M represents a doping element for the manganese and iron sites and preferably includes one or more of Co, Mg, Zn, Ca, Ti, V, Ni, Cr; Preferably, the water soluble iron salt comprises one or more of ferrous chloride, ferrous nitrate, ferrous sulfate, ferrous acetate, ferric chloride, ferric nitrate, ferric sulfate, ferric acetate; Preferably, the water soluble manganese salt comprises one or more of manganous chloride, manganous nitrate, manganous sulfate, manganous acetate; A method according to any one of claims 2 to 8, wherein the water-soluble salt of doping element M comprises one or more of the following salts: hydrochloride, nitrate, sulphate, acetate of doping element M.
10. the phosphorus source required for producing said iron manganese phosphate precursor comprises one or more of phosphoric acid, water-soluble phosphate salts, preferably said water-soluble phosphate salts comprise one or more of trisodium phosphate, tripotassium phosphate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate and ammonium phosphate; 10. The method according to any one of claims 2 to 9, wherein preferably the phosphorus source necessary for producing said iron manganese phosphate precursor further comprises a water soluble source of doping element Q, Q representing a doping element of phosphorussite and preferably comprising one or more of B, S, Si and N, preferably said source of doping element Q comprising one or more of sulfates, borates, nitrates and silicates of doping element Q.
11. The oxidizing agent includes one or more of hydrogen peroxide, nitric acid, sodium hypochlorite, potassium hypochlorite, sodium chlorate, and potassium chlorate, and is preferably hydrogen peroxide; The process according to any one of claims 2 to 10, wherein the molar ratio of said metal salt to said oxidizing agent is 1:(0.1-1.2), preferably 1:(0.5-0.6).
12. The concentration of the metal salt solution is between 0.5 mol / L and 2 mol / L, preferably between 0.5 mol / L and 1 mol / L; and / or The concentration of the phosphorus source solution is 0.5 mol / L to 2 mol / L, preferably 0.5 mol / L to 1 mol / L; and / or The method according to any one of claims 2 to 11, wherein the molar ratio of the metal salt to the phosphorus source is from 1:1 to 1:
3.
13. The stirring speed of the first material dissolving pot is 100 r / min to 500 r / min, and / or The stirring speed of the second material dissolving pot is 100 r / min to 500 r / min, and / or The stirring speed of the first reactor is 100 r / min to 500 r / min, and / or The stirring speed of the second reactor is 100 r / min to 500 r / min, and / or The method according to any one of claims 2 to 12, wherein the stirring speed of the aging tank is 100 r / min to 500 r / min.
14. In step S3, the drying temperature is 200° C. to 300° C.; and / or In step S3, the drying time is 3 h to 8 h, and / or The manufacturing method according to any one of claims 2 to 13, wherein in step S3, the dry atmosphere is a protective gas atmosphere, and the protective gas comprises nitrogen gas, an inert gas, or a combination thereof.
15. A manganese iron phosphate precursor produced by the method according to any one of claims 2 to 14, Chemical formula Fe x Mn y M 1-x-y P 1-m Q m O 4 wherein 0<x<1, preferably 0.2≦x≦0.5, 0<y<1, preferably 0.5≦y≦0.8, 0≦1-x-y<1, preferably 0<1-x-y≦0.05, 0≦m≦0.1, preferably 0<m≦0.05, M represents a doping element for the manganese site and the iron site, preferably comprising one or more of Co, Mg, Zn, Ca, Ti, V, Ni, Cr, Q represents a doping element for the phosphorus site, preferably comprising one or more of B, S, Si and N, and said manganese iron phosphate precursor is electrically neutral.
16. have a spherical shape, and / or 16. The iron manganese phosphate precursor of claim 15, which is orthorhombic and has a space group of pmnb.
17. The volumetric particle size distributions Dv90 and Dv50 satisfy 1<Dv90 / Dv50≦2, preferably 1.1≦Dv90 / Dv50≦1.7, and / or The iron manganese phosphate precursor according to claim 15 or 16, wherein the volumetric particle size distribution Dv50 is 1 μm to 10 μm, preferably 2.5 μm to 6 μm.
18. at least, Step S10 of uniformly mixing the iron manganese phosphate precursor produced by the method according to any one of claims 2 to 14 or the iron manganese phosphate precursor according to any one of claims 15 to 17 with a lithium source, a selectable doping element N source and a selectable doping element R source in a preset ratio to obtain a mixed raw material, N representing a doping element at the lithium site, preferably including one or more of Zn, Al, Na, K, Mg, Nb, Mo and W, and R representing a doping element at the oxygen site, preferably including one or more of S, F, Cl and Br; The mixed raw material obtained in step S10 is sintered to obtain lithium manganese iron phosphate, which has the chemical formula Li a N b Fe x Mn y M 1-x-y P 1-m Q m O 4-n R nM represents a doping element at the manganese site and the iron site, and preferably comprises one or more of Co, Mg, Zn, Ca, Ti, V, Ni, Cr; N represents a doping element at the lithium site, and preferably comprises one or more of Zn, Al, Na, K, Mg, Nb, Mo, and W; Q represents a doping element at the phosphorus site, and preferably comprises one or more of B, S, Si, and N; R represents a doping element at the oxygen site, and preferably comprises one or more of S, F, Cl, and Br; and step S20, wherein a≦a≦1.1, 0≦b≦0.1, preferably 0<b≦0.05, 0<x<1, preferably 0.2≦x≦0.5, 0<y<1, preferably 0.5≦y≦0.8, 0≦1-x-y<1, preferably 0<1-x-y≦0.05, 0≦m≦0.1, preferably 0<m≦0.05, 0≦n≦0.1, preferably 0<n≦0.05, and the lithium manganese iron phosphate is electrically neutral.
19. The method according to claim 18, wherein in step S10, a carbon source is further added to the mixed raw material.
20. 20. Lithium manganese iron phosphate produced by the method according to claim 18 or 19.
21. A secondary battery comprising the lithium manganese iron phosphate produced by the method according to claim 18 or 19.
Citation Information
Patent Citations
Metal / carbon nanotube compound doped phosphate ferromanganese material and preparation method thereof
CN106848309A
Continuous ferric phosphate production system and method
CN107337189A
Continuous production method and device for in-situ doping of high-nickel ternary positive electrode material precursor of lithium ion battery
CN113387400A
Lithium manganese iron phosphate precursor, lithium manganese iron phosphate positive electrode material, preparation method of lithium manganese iron phosphate positive electrode material, electrode material, electrode and lithium ion battery
CN113942990A
Preparation method of lithium manganese iron phosphate, positive electrode material and lithium ion battery
CN114644328A
Cited By
Manganese iron phosphate precursor and its manufacturing method, positive electrode material, positive electrode sheet and secondary battery